Sound-absorbing material block and its manufacturing method and related device

By manufacturing sound-absorbing material blocks through a mixture of porous materials and chemical agents, the issues of particle collisions and complex assembly are resolved, resulting in strong, crush-resistant blocks that enhance speaker performance.

JP7573055B2Active Publication Date: 2024-10-24AAC TECHNOLOGIES (NANJING) CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022580464
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-07-04
Filing Date
2022-08-10
Publication Date
2024-10-24
Estimated Expiration
2042-08-10

AI Technical Summary

Technical Problem

Conventional sound-absorbing materials for speakers are prone to particle collisions, leading to performance instability, particle loss, and damage to the loudspeaker, with a complicated filling process and low strength.

Method used

A method involving mixing porous materials, gelling agents, crosslinking agents, adhesives, and foaming agents to create a sound-absorbing material block, which is filled into the speaker back chamber and dried to form a monolithic structure, eliminating the need for cutting and simplifying the filling process.

Benefits of technology

The resulting sound-absorbing material blocks exhibit high strength, are resistant to crushing, and provide improved acoustic performance by stabilizing the speaker's sound quality without the need for complex assembly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573055000002
    Figure 0007573055000002
  • Figure 0007573055000003
    Figure 0007573055000003
  • Figure 0007573055000004
    Figure 0007573055000004
Patent Text Reader

Abstract

The present invention discloses a block of sound absorbing material and a method and associated apparatus for its manufacture. [Solution] The manufacturing method of the sound-absorbing material block includes step S1, mixing raw materials together to manufacture a mixed paste, the raw materials including a porous material, a gelling agent, a crosslinking agent, an adhesive, a foaming agent and a solvent, and step S2, filling the mixed paste into a speaker back chamber of a pre-provided speaker, and then sequentially drying and dehydrating to obtain a sound-absorbing material block. The present invention mixes a porous material, a gelling agent, a crosslinking agent, an adhesive, a foaming agent and a solvent to manufacture a sound-absorbing material block, and the manufactured sound-absorbing material block has high strength, is not easily broken and has good performance, while the mixed paste is filled into the speaker back chamber, and further sequentially drying and dehydrating to directly manufacture and obtain a sound-absorbing material block that fits the speaker back chamber, thereby omitting the steps of cutting and filling, and simplifying the filling process.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of electroacoustic conversion, and in particular to a block of sound-absorbing material and a method and device for producing the same. [Background technology]

[0002] With the development of smart devices, the requirements for sound quality of traditional smart devices are also becoming higher. Generally, the larger the back chamber space of the speaker, the higher the sound quality. However, smart devices such as mobile phones, tablet computers and watches do not have extra space for the back chamber of the speaker. Therefore, how to generate high-quality sound in a limited space becomes a problem to be solved in this field. A common method is to fill the back chamber with sound-absorbing material to virtually increase the space of the back chamber and improve the sound quality.

[0003] At present, the sound absorbing material filled in the back chamber is mainly granular sound absorbing material, but the particle size of the granular sound absorbing material is generally only 200-500 μm. When the diaphragm of the speaker vibrates, the sound absorbing particles vibrate with the air vibration, and at this time, violent collision occurs between different particles, and the phenomenon of powder falling and crushing is very likely to occur during the collision of particles. This reduces the performance of the sound absorbing particles, and the fallen powder further penetrates the screen mesh and enters the speaker, and in serious cases, further damages the speaker. In addition, the sound absorbing particles have difficulty filling the back chamber when filling, and the utilization rate of the back chamber is low. When the speaker is tilted or inverted, the position of the sound absorbing particles in the back chamber also changes accordingly, and the sound absorbing particles in different positions and stacking states cause instability in the acoustic performance of the speaker, and the performance cannot be optimally achieved.

[0004] Therefore, in order to eliminate the defects generated by the sound-absorbing particles, those skilled in the art have tried to manufacture some sound-absorbing material blocks, but these sound-absorbing material blocks still need to be cut and fitted during the filling process, and the shape of the back chamber is complicated, which makes the filling process complicated; at the same time, the strength of these sound-absorbing material blocks is low, and they are prone to fracture, resulting in poor performance.

[0005] Therefore, there is a need to provide a sound absorbing material block and a manufacturing method thereof and related apparatus to solve the above technical problems. Summary of the Invention [Problem to be solved by the invention]

[0006] The objective of the present invention is to provide a sound-absorbing material block and its manufacturing method and related device, thereby solving the problems of the traditional sound-absorbing material block's complicated filling process, low strength, easy to breakage and poor performance. [Means for solving the problem]

[0007] In a first aspect, the present invention provides a method for producing a block of sound absorbing material, the method comprising the steps of: Step S1: mixing raw materials together to prepare a mixed paste, the raw materials include a porous material, a gelling agent, a cross-linking agent, an adhesive, a foaming agent, and a solvent, the content of the gelling agent is 1-5 wt% of the mass of the porous material, the content of the cross-linking agent is 5-20 wt% of the mass of the gelling agent, the content of the adhesive is 2-10 wt% of the mass of the porous material, and the content of the foaming agent is 1-5 wt% of the mass of the porous material; Step S2 includes first filling the mixed paste into a speaker back chamber of a pre-provided speaker, and then sequentially carrying out drying and dehydration processes to obtain a sound-absorbing material block.

[0008] Preferably, the gelling agent is one or more of sodium carboxymethylcellulose, hydroxypropylmethylcellulose, sodium alginate, chitosan, polyethylene glycol, polyvinyl alcohol and polyacryloyl chloride materials.

[0009] Preferably, the cross-linking agent is one or more of glutaraldehyde, boric acid, calcium chloride and calcium carbonate.

[0010] Preferably, the porous material is a zeolite and / or activated carbon, the zeolite being one or more of the structures of MFI molecular sieves, MEL molecular sieves and FER molecular sieves, and having a particle size smaller than 10 μm.

[0011] Preferably, the adhesive is one or more of polyacrylic ester, styrene butadiene emulsion, polystyrene acrylate, polystyrene acetate, polyurethane resin, polyethylvinyl acetate salt.

[0012] Preferably, the foaming agent is an inorganic foaming agent, and the inorganic foaming agent is one or more of hydrogen peroxide, ammonium bicarbonate, and sodium bicarbonate.

[0013] Preferably, the blowing agent is an organic blowing agent, the organic blowing agent being one or more of azodicarbonamide, polymeric hollow microspheres, polyurethane foam particles, and PE foam particles.

[0014] Preferably, the solvent is one or more of water, methanol, ethanol, butanol and ethyl acetate.

[0015] Preferably, in the step S1, the step of mixing the raw materials together to prepare a mixed paste specifically includes: Step S11: mixing the porous material, the gelling agent, the adhesive, the foaming agent and the solvent together by stirring to obtain a slurry; Step S12 includes the sub-step of adding the cross-linking agent to the slurry and continuously stirring to mix together to obtain the mixed paste.

[0016] Preferably, in step S2, the mixed paste is filled into the speaker back chamber by injection, and the dehydration treatment is to perform a baking dehydration treatment on the speaker back chamber containing the dried mixed paste.

[0017] Preferably, the drying method is any one of low-temperature vacuum freeze drying, microwave drying, supercritical drying, high-temperature heat drying, and vacuum heat drying.

[0018] In a second aspect, the present invention provides a sound-absorbing material block comprising, by mass percentage, a porous material, a gelling agent, a cross-linking agent and an adhesive, wherein the content of the gelling agent is 1-5 wt % of the mass of the porous material, the content of the cross-linking agent is 5-20 wt % of the mass of the gelling agent, and the content of the adhesive is 2-10 wt % of the mass of the porous material.

[0019] Preferably, the structure of the sound absorbing material block is one of a sphere, an ellipsoid, or a polyhedron.

[0020] Preferably, the sound-absorbing material block is manufactured by the above-mentioned method for manufacturing a sound-absorbing material block.

[0021] In a third aspect, the present invention provides a speaker box, comprising: a housing having an accommodation space; and a sound-emitting element and a sound-guiding channel accommodated and fixed in the accommodation space, the housing includes an upper cover and a lower cover fitted to the upper cover, the sound-guiding channel is formed in the upper cover, the sound-emitting element, the upper cover and the lower cover are surrounded together to form a back chamber, the sound-emitting element and the upper cover are installed at a distance from each other and surrounded together to form a front acoustic chamber, the sound-guiding channel communicates the front acoustic chamber with the outside and forms a front chamber together with the front acoustic chamber, and the back chamber is filled with the above-mentioned sound-absorbing material block.

[0022] Preferably, the block of sound absorbing material matches some or all of the back chamber.

[0023] Preferably, the block of sound absorbing material has an inner surface partly or wholly applied to the back chamber.

[0024] Preferably, the block of sound absorbing material is a monolithic structure or a plurality of individual block-like structures.

[0025] In a fourth aspect, the present invention provides an electronic device, the electronic device being one of a mobile phone, a watch, a tablet computer, a sound device and a notebook computer, the electronic device being equipped with the above-mentioned speaker box. Effect of the Invention

[0026] Compared with the related art, the present invention uses a porous material, a gelling agent, a cross-linking agent, an adhesive, a foaming agent and a solvent to manufacture a sound-absorbing material block, so that the sound-absorbing material block manufactured thereby has high strength, is not easily broken and has good performance; meanwhile, the mixed paste is filled into the speaker back chamber, and then a sound-absorbing material block that fits the speaker back chamber is directly manufactured through a drying process and a dehydration process in sequence, so that the steps of cutting and filling can be omitted and the filling process is simplified. [Brief description of the drawings]

[0027] In order to more clearly describe the technical solutions in the embodiments of the present invention, the following briefly introduces drawings necessary for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention, and those skilled in the art can further obtain other drawings based on these drawings without any creative work. [Figure 1] 1 is a schematic flow diagram of a method for producing a sound-absorbing material block provided by an embodiment of the present invention. [Diagram 2]FIG. 2 is a schematic flow diagram of sub-steps of step S1 in an embodiment of the present invention. [Diagram 3] FIG. 2 is a SEM image of a cross section of a sound-absorbing material block in an embodiment of the present invention. [Figure 4] FIG. 2 is a cross-sectional view of a speaker box provided by an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] The following clearly and completely describes the technical solutions in the embodiments of the present invention, and obviously, the described embodiments are only some of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments that a person skilled in the art can obtain without creative labor are all included in the protection scope of the present invention.

[0029] Example 1 As shown in FIG. 1, an embodiment of the present invention provides a method for manufacturing a sound-absorbing material block, the method including the following steps:

[0030] Step S1: mixing raw materials together to produce a mixed paste.

[0031] Specifically, the raw materials include a porous material, a gelling agent, a cross-linking agent, an adhesive, a foaming agent, and a solvent.

[0032] The porous material is zeolite and / or activated carbon, the zeolite being one or more of the structures of MFI molecular sieve, MEL molecular sieve and FER molecular sieve, and having a particle size smaller than 10 μm.

[0033] The gelling agent is one or more of sodium carboxymethylcellulose, hydroxypropylmethylcellulose, sodium alginate, chitosan, polyethylene glycol, polyvinyl alcohol and polyacryloyl chloride materials, and the content of the gelling agent is 1 to 5 wt % of the mass of the porous material.

[0034] The crosslinking agent is one or more of glutaraldehyde, boric acid, calcium chloride, and calcium carbonate, and the content of the crosslinking agent is 5 to 20 wt % of the mass of the gelling agent. The mixing ratio of the crosslinking agent is selected according to the mixing ratio of the gelling agent.

[0035] The adhesive is one or more of polyacrylic ester, styrene butadiene emulsion, polystyrene acrylate, polystyrene acetate, polyurethane resin, and polyethylvinyl acetate salt, and the content of the adhesive is 2 to 10 wt % of the mass of the porous material.

[0036] The foaming agent can be selected from inorganic foaming agents or organic foaming agents, the inorganic foaming agent being one or more of hydrogen peroxide, ammonium bicarbonate and sodium bicarbonate, and the organic foaming agent being one or more of azodicarbonamide, polymer hollow microspheres, polyurethane foam particles and PE foam particles. The content of the foaming agent is 1-5 wt% of the mass of the porous material.

[0037] The solvent is one or more of water, methanol, ethanol, butanol, and ethyl acetate, and the content of the solvent is 80 to 120 wt % of the mass of the porous material.

[0038] The various materials in the raw materials can be blended according to actual needs, so as to obtain a sound-absorbing material block with high strength, resistance to shattering and good performance.

[0039] Specifically, as shown in FIG. 2, step S1 specifically includes the following sub-steps: Step S11: mixing the porous material, the gelling agent, the adhesive, the foaming agent and the solvent together by stirring to obtain a slurry; Step S12 includes the sub-step of adding the cross-linking agent to the slurry and continuously stirring to mix together to obtain the mixed paste.

[0040] The time of stirring and mixing together in step S11 and step S12 is set according to actual demand.

[0041] The mixed paste does not undergo settling even after standing for 24 hours, and can be industrially applied to manufacture sound-absorbing material blocks.

[0042] In step S2, the mixed paste is first filled into a speaker back chamber of a pre-prepared speaker, and then dried and dehydrated in order to obtain a sound-absorbing material block.

[0043] Specifically, when filling the speaker back chamber with the mixed paste, it is necessary to ensure that the back chamber of the speaker is filled with the mixed paste.

[0044] The mixed paste is filled into the speaker back chamber by injection, and the drying method is one of low-temperature vacuum freeze drying, microwave drying, supercritical drying, high-temperature heating drying, and vacuum heating drying. The dehydration is performed by baking the speaker back chamber containing the dried mixed paste, i.e., the speaker back chamber that has been dried is directly baked and dehydrated, and the speaker back chamber contains the dried mixed paste.

[0045] The drying process is carried out directly on the speaker back chamber filled with the mixed paste.

[0046] After the drying and dehydration processes are completed, the solvent and the foaming agent in the mixed paste are completely removed, that is, the obtained sound-absorbing material block does not contain the solvent and the foaming agent.

[0047] FIG. 3 is a SEM (scanning electron microscope) view of a cross section of the sound absorbing material block, from which its internal structure can be clearly seen.

[0048] Compared with the related art, this embodiment uses a porous material, a gelling agent, a cross-linking agent, an adhesive, a foaming agent and a solvent to manufacture a sound-absorbing material block, so that the sound-absorbing material block manufactured thereby has high strength, is not easily broken and has good performance; meanwhile, the mixed paste is filled into the speaker back chamber, and then a sound-absorbing material block that fits the speaker back chamber is directly manufactured through a drying process and a dehydration process in sequence, so that the steps of cutting and filling can be omitted and the filling process is simplified.

[0049] Example 2 An embodiment of the present invention provides a sound-absorbing material block, comprising, by mass percentage, a porous material, a gelling agent, a cross-linking agent and an adhesive, wherein the content of the gelling agent is 1-5 wt% of the mass of the porous material, the content of the cross-linking agent is 5-20 wt% of the mass of the gelling agent, and the content of the adhesive is 2-10 wt% of the mass of the porous material.

[0050] In the sound-absorbing material block of this embodiment, the solvent and the foaming agent are released during the drying and dehydration processes, so the sound-absorbing material block does not contain the solvent and the foaming agent in the first embodiment.

[0051] Specifically, the structure of the sound-absorbing material block is one of a sphere, an ellipsoid, a tetrahedron, a trapezoid, a rectangular parallelepiped, and a square. Of course, the structure may be a complex polyhedral structure according to actual needs. When the sound-absorbing material block is a plurality of independent block structures, the plurality of independent block structures may be the same, for example, the sound-absorbing material block may be formed by combining one of a plurality of spheres, a plurality of trapezoids, and a plurality of rectangular parallelepipeds. The plurality of independent block structures may be different, for example, the sound-absorbing material block may be formed by combining a plurality of block structures among a sphere block structure, an ellipsoid block structure, a tetrahedron block structure, a trapezoid block structure, and a square block structure.

[0052] Specifically, the sound-absorbing material block is manufactured by the method for manufacturing the sound-absorbing material block in the first embodiment, and the sound-absorbing material block is used to fill a speaker back chamber.

[0053] Since the sound-absorbing material block in this embodiment is manufactured by the manufacturing method of the sound-absorbing material block in Example 1, the sound-absorbing material block in this embodiment can achieve the technical effects achieved by the manufacturing method of the sound-absorbing material block in Example 1, and they will not be described repeatedly here.

[0054] Example 3 As shown in FIG. 4, an embodiment of the present invention provides a speaker box, which includes a housing 1 having an accommodation space, a sound-generating element 2 accommodated and fixed in the accommodation space, and a sound-guiding channel 3. The housing 1 includes an upper cover 11 and a lower cover 12 covered by the upper cover 11. The sound-guiding channel 3 is formed in the upper cover 11. The sound-generating element 2, the upper cover 11 and the lower cover 12 are surrounded together to form a back chamber 10. The sound-generating element 2 and the upper cover 11 are spaced apart and surrounded together to form a front sound chamber 201. The sound-guiding channel 3 connects the front sound chamber 201 to the outside, and forms a front chamber 20 together with the front sound chamber 201. A sound-absorbing material block 4 is filled in the back chamber 10.

[0055] The sound absorbing material block 4 in this embodiment is the sound absorbing material block in the second embodiment.

[0056] Specifically, the speaker back chamber 10 in the first embodiment is the same as or similar to the back chamber 10 of the speaker box in this embodiment.

[0057] Specifically, the sound-absorbing material block can match some or all of the chambers of the back chamber, i.e., can partially or completely fill the speaker back chamber, the sound-absorbing material block has an inner surface that is partially or completely coated on the back chamber, and the sound-absorbing material block is a monolith structure or a multiple single block-like structure.

[0058] The sound-absorbing material block 4 filled in the back chamber 10 of the speaker box in this embodiment is the sound-absorbing material block in Example 2, so the sound-absorbing material block 4 in this embodiment can achieve the technical effects achieved by the sound-absorbing material block in Example 2, and will not be described again here.

[0059] Example 4 An embodiment of the present invention provides an electronic device, in which the speaker box of the third embodiment is installed.

[0060] The electronic device is one of the following devices: mobile phone, watch, tablet computer, audio device, notebook computer, etc. Of course, according to actual needs, the electronic device may also be a device with a speaker box structure, such as a portable game machine or a radio.

[0061] Since the electronic device in this embodiment is installed with the speaker box of Example 3, the electronic device in this embodiment can achieve the technical effects achieved by the speaker box in Example 3, which will not be described again here.

[0062] Example 5 An embodiment of the present invention provides a method for manufacturing a block of sound absorbing material, the method comprising the following steps.

[0063] In step S101, 1 wt% sodium alginate is weighed out and added to 43 wt% water and stirred for 20 minutes to form a uniform and transparent sodium alginate solution, and then 50 wt% zeolite, 4 wt% polystyrene acrylate and 2 wt% hydrogen peroxide are added to the sodium alginate solution and stirred for 30 minutes to form a mixed slurry.

[0064] In step S102, a 1% calcium chloride aqueous solution is prepared, and then a 5 wt % calcium chloride aqueous solution is mixed into the slurry by dropping the calcium chloride aqueous solution while stirring. After the dropping is completed, the mixture is stirred for 20 minutes and then aged for 2 hours to obtain a gel-like mixed paste.

[0065] The materials in step S101 and step S102 are weighed by mass ratio, and the content of the slurry accounts for 97 wt% of the mass of the mixed paste.

[0066] Step S103: use a syringe to suck up a certain amount of the mixed paste, then inject it into the speaker back chamber, and fill the speaker back chamber with the mixed paste. Then, the speaker back chamber is freeze-dried. After the drying process is completed, the speaker back chamber is further baked in an 80°C environment for 2 hours to perform dehydration, and finally a sound-absorbing material block is obtained.

[0067] Example 6 An embodiment of the present invention provides a method for manufacturing a block of sound absorbing material, the method comprising the following steps.

[0068] In step S201, 1 wt% sodium alginate is weighed and added to 43 wt% water and stirred for 20 minutes to form a uniform and transparent sodium alginate solution, and then 50 wt% zeolite, 4 wt% styrene butadiene emulsion and 2 wt% azodicarbonamide are added to the sodium alginate solution, followed by stirring for 30 minutes to form a mixed slurry.

[0069] In step S202, 0.04 wt% calcium chloride powder is added to the slurry, stirred for 30 minutes until a gel is formed, and then aged for 4 hours to obtain a gel-like mixed paste.

[0070] The materials in step S201 and step S202 are weighed by mass ratio, and the content of the slurry accounts for 97 wt% of the mass of the mixed paste.

[0071] Step S203: Using a syringe to suck up a certain amount of the mixed paste, then injecting it into a speaker back chamber, and filling the speaker back chamber with the mixed paste. Then, the speaker back chamber is subjected to a supercritical freeze-drying process. After the drying process is completed, the speaker back chamber is further placed in an environment of 100° C. and baked for 1 hour. Then, a dehydration treatment is performed to finally obtain a sound-absorbing material block.

[0072] Example 7 An embodiment of the present invention provides a method for manufacturing a block of sound absorbing material, the method comprising the following steps.

[0073] In step S301, 2 wt% polyvinyl alcohol is weighed and added to 42 wt% water and stirred for 20 minutes to form a homogeneous polyvinyl alcohol aqueous solution, and then 50 wt% zeolite, 5 wt% polyethylvinylacetate salt and 1 wt% ammonium bicarbonate are added to the polyvinyl alcohol aqueous solution, followed by stirring for 30 minutes to form a mixed slurry.

[0074] In step S302, a 5% boric acid solution is prepared, and then 2 wt % of the boric acid solution is mixed into the above slurry by dripping while stirring. After the dripping is completed, the mixture is stirred for 20 minutes and then aged for 6 hours to obtain a gel-like mixed paste.

[0075] The materials in steps S301 and S302 are measured in mass ratio.

[0076] In step S303, a certain amount of the mixed paste is sucked up using a syringe, and then injected into the speaker back chamber, and the speaker back chamber is filled with the mixed paste, after which the speaker back chamber is freeze-dried, and after the drying process is completed, the speaker back chamber is further placed in an 80°C environment and baked for 2 hours to perform dehydration, and finally a sound-absorbing material block is obtained.

[0077] Example 8 An embodiment of the present invention provides a method for manufacturing a block of sound absorbing material, the method comprising the following steps.

[0078] In step S401, 2.5 wt% polyacryloyl chloride is weighed and added to 42 wt% water and stirred for 20 minutes to form a uniform polyacryloyl chloride aqueous solution; then, 50 wt% zeolite, 3 wt% polyethylvinylacetate salt and 2 wt% azodicarbonamide are added to the polyacryloyl chloride aqueous solution, and stirred for 30 minutes to form a mixed slurry.

[0079] In step S402, 0.2 wt% glutaraldehyde is added to the above slurry, stirred for 30 minutes, and then aged for 4 hours to obtain a gel-like mixed paste.

[0080] The materials in steps S401 and S402 are measured in mass ratio.

[0081] In step S403, a certain amount of the mixed paste is sucked up using a syringe, and then injected into the speaker back chamber, and the speaker back chamber is filled with the mixed paste, after which the speaker back chamber is subjected to a freeze-drying process, and after the drying process is completed, the speaker back chamber is further placed in an environment of 110°C and baked for 1 hour to perform a dehydration process, and finally a sound-absorbing material block is obtained.

[0082] Comparative Example 1 An embodiment of the present invention provides a method for manufacturing a block of sound absorbing material, the method comprising the following steps.

[0083] In step S501, 41 wt% water is weighed out, and 50 wt% zeolite, 4 wt% polystyrene acrylate and 5 wt% hydrogen peroxide are added thereto, and stirred for 30 minutes to form a mixed slurry.

[0084] The materials in step S501 are measured by mass ratio.

[0085] In step S502, a certain amount of the slurry is sucked up using a syringe, and then injected into a speaker back chamber, and the speaker back chamber is filled with the mixed paste, after which the speaker back chamber is subjected to a freeze-drying process, and after the drying process is completed, the speaker back chamber is further placed in an environment of 100°C and baked for 2 hours to perform a dehydration process, and finally a sound-absorbing material block is obtained.

[0086] Comparative Example 2 An embodiment of the present invention provides a method for manufacturing a block of sound absorbing material, the method comprising the following steps.

[0087] In step S601, 2 wt% sodium carboxymethylcellulose is weighed out and added to 38 wt% water and stirred for 20 minutes to form a uniform and transparent sodium carboxymethylcellulose aqueous solution, and then 50 wt% zeolite, 5 wt% polyacrylic acid ester, and 5 wt% ammonium hydrogen carbonate are added to the sodium carboxymethylcellulose aqueous solution, and stirred for 30 minutes to form a mixed slurry.

[0088] The materials in step S601 are measured by mass ratio.

[0089] In step S602, a certain amount of the slurry is sucked up using a syringe, and then injected into a speaker back chamber, and the speaker back chamber is filled with the mixed paste, after which the speaker back chamber is subjected to a freeze-drying process, and after the drying process is completed, the speaker back chamber is further placed in an 80°C environment and baked for 2 hours to perform a dehydration process, and finally a sound-absorbing material block is obtained.

[0090] In order to easily evaluate the performance of the sound-absorbing material blocks in the embodiments of the present invention, acoustic performance tests are carried out on the sound-absorbing material blocks in the embodiments 5 to 8 and the conventional sound-absorbing particles. In order to facilitate comparison, the sound-absorbing material blocks in the embodiments 5 to 8 are manufactured into cubes with a volume of 10mm*12mm*2mm / 0.24ml, while the volume of the general sound-absorbing particles with excellent performance in this field is also 0.24ml, and the speaker back chambers of the test tool are all 0.4ml in volume. At the same time, drop performance tests are carried out on different embodiments and comparative examples, and the test results are shown in Table 1.

[0091] [Table 1]

[0092] As can be seen from the above table, the performance of the sound-absorbing material blocks manufactured in Examples 5, 6 and 8 is all superior to that of the conventional sound-absorbing particles, and the performance of Examples 5 and 6 is significantly superior to that of the conventional sound-absorbing particles. In addition, the gel performance unique to the sound-absorbing material block of the present invention has a wider range of application, a longer memory time, and can be directly injected into the back chamber of the speaker, making full use of the space of the speaker back chamber and improving the acoustic performance of the speaker box.

[0093] In addition, the performance of Comparative Example 1 is poorer than that of Examples 5 to 8, and the sound-absorbing material block structure produced is loose, has low strength, and is seriously broken, which is due to the lack of support from the gel material cross-linking agent. At the same time, the slurry is prone to sedimentation during the production process of the material, which is not suitable for industrialized production.

[0094] The above description is only an embodiment of the present invention, and does not limit the patent scope of the present invention. Any equivalent structure or equivalent flow conversion made by using the contents of the specification and drawings of the present invention, or any direct or indirect application to other related technical fields, is also included in the patent protection scope of the present invention. [Explanation of symbols]

[0095] 1-Housing 11-Top cover 12-Lower cover 2-Phonetic unit 3-sound conducting channel 4-Sound absorbing material blocks 10-Back Chamber 20-Front chamber 201-Front Acoustic Chamber

Claims

1. A method for producing a sound absorbing material block, comprising the steps of: Step S1: mixing raw materials together to prepare a mixed paste, the raw materials include a porous material, a gelling agent, a cross-linking agent, an adhesive, a foaming agent, and a solvent, the content of the gelling agent is 1-5 wt % of the mass of the porous material, the content of the cross-linking agent is 5-20 wt % of the mass of the gelling agent, the content of the adhesive is 2-10 wt % of the mass of the porous material, and the content of the foaming agent is 1-5 wt % of the mass of the porous material; Step S2: First, the mixed paste is filled into a speaker back chamber of a speaker provided in advance, and then the mixed paste is dried and dehydrated to obtain a sound-absorbing material block.

2. 2. The method for producing a sound-absorbing material block according to claim 1, wherein the gelling agent is one or more of sodium carboxymethylcellulose, hydroxypropylmethylcellulose, sodium alginate, chitosan, polyethylene glycol, polyvinyl alcohol and polyacryloyl chloride materials.

3. 2. The method for producing a sound-absorbing material block according to claim 1, wherein the cross-linking agent is one or more of glutaraldehyde, boric acid, calcium chloride, and calcium carbonate.

4. 2. The method for producing a sound-absorbing material block according to claim 1, wherein the porous material is zeolite and / or activated carbon, the zeolite has one or more structures selected from the group consisting of MFI molecular sieve, MEL molecular sieve and FER molecular sieve, and has a particle size smaller than 10 μm.

5. 2. The method for producing a sound-absorbing material block according to claim 1, wherein the adhesive is one or more of polyacrylic ester, styrene butadiene emulsion, polystyrene acrylate, polystyrene acetate, polyurethane resin, and polyethylvinyl acetate salt.

6. 2. The method for manufacturing a sound-absorbing material block according to claim 1, wherein the foaming agent is an inorganic foaming agent, and the inorganic foaming agent is one or more of hydrogen peroxide, ammonium bicarbonate, and sodium bicarbonate.

7. 2. The method for producing a sound-absorbing material block according to claim 1, wherein the foaming agent is an organic foaming agent, and the organic foaming agent is one or more of azodicarbonamide, polymer hollow microspheres, polyurethane foam particles, and PE foam particles.

8. 2. The method for producing a sound-absorbing material block according to claim 1, wherein the solvent is one or more of water, methanol, ethanol, butanol, and ethyl acetate.

9. In step S1, the step of mixing the raw materials together to prepare a mixed paste is specifically as follows: Step S11: mixing the porous material, the gelling agent, the adhesive, the foaming agent and the solvent together by stirring to obtain a slurry; 2. The method for producing a sound-absorbing material block according to claim 1, further comprising: a step S12 of adding the cross-linking agent to the slurry, and subsequently stirring and mixing them together to obtain the mixed paste.

10. 2. The method for manufacturing a sound-absorbing material block according to claim 1, wherein in step S2, the mixed paste is filled into the speaker back chamber by injection, and the dehydration treatment is a baking dehydration treatment of the speaker back chamber containing the dried mixed paste.

11. 2. The method for producing a sound-absorbing material block according to claim 1, wherein the drying method is any one of low-temperature vacuum freeze drying, microwave drying, supercritical drying, high-temperature heating drying and vacuum heating drying.

12. 1. A sound-absorbing material block, the sound-absorbing material block being manufactured by the method for manufacturing a sound-absorbing material block as described in claim 1, and comprising, by mass percentage, a porous material, a gelling agent, a crosslinking agent, and an adhesive, the gelling agent content being 1 to 5 wt % of the mass of the porous material, the crosslinking agent content being 5 to 20 wt % of the mass of the gelling agent, and the adhesive content being 2 to 10 wt % of the mass of the porous material.

13. 13. The sound absorbing material block according to claim 12, wherein the structure of the sound absorbing material block is one of a sphere, an ellipsoid, and a polyhedron.

14. 13. A speaker box comprising: a housing having an accommodation space; and a sound-emitting element and a sound-guiding channel accommodated and fixed in the accommodation space, the housing comprising an upper cover and a lower cover fitted to the upper cover, the sound-guiding channel being formed in the upper cover, the sound-emitting element, the upper cover and the lower cover surrounding each other to form a back chamber, the sound-emitting element and the upper cover being installed at a distance from each other and surrounding each other to form a front acoustic chamber, the sound-guiding channel communicating the front acoustic chamber with the outside and forming a front chamber together with the front acoustic chamber, the back chamber being filled with the sound-absorbing material block according to claim 12.

15. 15. The speaker box according to claim 14, wherein the sound absorbing material block matches a part or all of the back chamber.

16. 15. The speaker box according to claim 14, wherein the sound absorbing material block has an inner surface that is partially or completely applied to the back chamber.

17. 15. The speaker box according to claim 14, wherein the sound absorbing material block is a monolithic structure or a plurality of single block-like structures.

18. An electronic device, the electronic device being one of a mobile phone, a wristwatch, a tablet computer, a sound device, and a notebook computer, the electronic device being equipped with the speaker box according to claim 14.

Citation Information

Patent Citations

  • Sound-absorbing material block, preparation method thereof and loudspeaker box using sound-absorbing material block

    CN114495883A

  • Core-shell molecular sieve and preparation method thereof, sound absorption material and loudspeaker

    CN114684832A

  • Polyurethane foam cabinets

    US20040069561A1

  • Porous sound absorbing material, method for producing same and sound absorption method

    WO2020116577A1