Laminated Dental Machining Resin Blanks

The laminated resin blank for dental cutting uses a structural color layer and a second layer with controlled color difference to enhance natural tooth color reproduction, addressing the inefficiencies of existing blanks by improving manufacturing efficiency and reducing shade matching efforts.

JP7574999B2Active Publication Date: 2024-10-29TOKUYAMA DENTAL CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020162971
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-29
Publication Date
2024-10-29
Estimated Expiration
2040-09-29

AI Technical Summary

Technical Problem

Existing dental cutting resin blanks struggle to accurately reproduce the color tone of natural teeth, especially in areas where no natural tooth exists, requiring labor-intensive manufacturing and careful shade matching for each patient.

Method used

A laminated resin-based blank with a first layer expressing a structural color and a second layer with a specific color tone difference, achieving a natural gradation effect by controlling the color difference and transparency between layers, reducing the need for extensive labor and shade taking.

Benefits of technology

The laminated structure allows for a more natural color reproduction of teeth, improving manufacturing efficiency and reducing the effort required for shade matching, while maintaining aesthetic compatibility with surrounding environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574999000001
    Figure 0007574999000001
  • Figure 0007574999000002
    Figure 0007574999000002
  • Figure 0007574999000003
    Figure 0007574999000003
Patent Text Reader

Abstract

To provide resin-based dental cutting blanks that can naturally match the color tone of natural teeth of many patients even when a dental prosthesis is made that includes a part where there is no natural tooth in a base in a relatively wide range from the vicinity of the tooth cervix to the cutting-edge part.SOLUTION: A part to be cut of a resin-based dental cutting blank is made up of a hybrid resin laminate having a laminated structure, in which a first layer made of a structural color-based hybrid resin that does not substantially contain a pigment or the like and can be adapted to the surrounding color tone by expressing the structural color of a specific color tone regardless of the incident angle of light and a second layer made of a hybrid resin colored in a different color tone by blending a pigment or the like are joined, the hybrid resin laminate having a color difference between both layers: ΔE* of 2 to 30.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated type dental mill blank for cutting, having a cutting portion made of a laminate in which a plurality of resin-based material layers are laminated. [Background technology]

[0002] In dental treatment, the use of digital technology is progressing in the manufacture of dental restorations (or dental prostheses) such as inlays, onlays, crowns, bridges, and implant superstructures. For example, as disclosed in Patent Document 1, a CAD / CAM system is becoming more and more popular, which uses a CAD / CAM device based on computer-aided design (CAD) and computer-aided manufacturing (CAM) technology to cut a dental blank for machining made of a nonmetallic material to form a dental restoration from an image of the oral cavity. Here, the dental blank for machining means a cut object (also called a mill blank) that can be attached to a cutting machine in a CAD / CAM system, and generally known examples include a (solid) block formed into a rectangular or cylindrical shape, or a (solid) disk formed into a plate or plate shape. In addition, a holding pin for fixing the dental blank for machining to the cutting machine is often joined to the dental blank for machining, and in such a form, the one integrated with the holding pin is sometimes called a dental blank for machining. In the present invention, the dental blank includes the above-mentioned embodiment integrated with the retaining pin. The main body of the workpiece (the dental blank) is sometimes called the part to be cut.

[0003] As the material to be machined of the dental machining blank, various materials such as glass ceramics, zirconia, titanium, resin, etc. Among these, resin-based materials (also called hybrid resins) consisting of a hardened product of a hardening composition containing an inorganic filler such as silica, a polymerizable monomer such as methacrylate resin, and a polymerization initiator, are attracting attention due to their high workability (machinability), high aesthetics, strength, etc.

[0004] In dental treatment, it is required to give an appearance as close as possible to the color tone of natural teeth. In order to meet such aesthetic requirements, various pigment and dye substances have been added in varying types and amounts to adjust the color tone of the single component of a single-layered resin blank for dental cutting, as well as a multi-layered resin blank for dental cutting made by laminating components of different colors.

[0005] For example, Patent Document 2 proposes a dental CAD / CAM resin block in which a dentin restorative resin layer and an enamel restorative resin layer are laminated as a dental cutting resin blank that is highly versatile and productive and has a high reproducibility of the aesthetic appearance of natural teeth, and at least the dentin restorative resin layer contains light diffusing particles and has a specific diffusion ratio. Patent Document 3 also proposes a dental mill blank that can provide a dental prosthesis having a color tone and transparency similar to that of natural teeth by cutting, and the laminate includes at least three layers, a top layer, at least one intermediate layer, and a bottom layer, each layer constituting the laminate includes a filler (A) and a polymer (B), the filler (A) of each layer includes at least one type of inorganic particle (a) and at least one type of pigment (C), and the chromaticity difference ΔE* between the top layer and the bottom layer is 100%. T is 5.0 or more and 15.0 or less, and the transparency difference ΔΔL* between the uppermost layer and the lowermost layer is T is 5.0 or more and 15.0 or less, the chromaticity difference ΔE* of all adjacent layers is 1.0 or more and 5.5 or less, the transparency difference ΔΔL* of all adjacent layers is 1.0 or more and 5.0 or less, and the transparency ΔL* of the uppermost layer is His 13.5 or more and 25.0 or less, and the transparency ΔL* of the lowermost layer L is 7.0 or more and 13.0 or less, a dental mill blank has been proposed.

[0006] Also, in a resin-based blank for dental cutting with a single-layer structure, there are those known that can achieve color harmony with natural teeth without using pigments or the like by expressing so-called structural color. That is, Patent Document 4 discloses "a resin-based block for dental cutting containing a resin matrix (A) and spherical fillers (B) with an average particle diameter in the range of 230 nm to 1000 nm, wherein 90% or more of the individual particles constituting the spherical fillers (B) are present within a range of 5% before and after the average particle diameter, and the measured color values in the Munsell color system of the colored light under a black background and a white background, measured using a color difference meter at a thickness of 10 mm, have a lightness (V) of less than 5.0 and a chroma (C) of less than 2.0, and the measured color values in the Munsell color system of the colored light under a black background, measured using a color difference meter at a thickness of 1 mm, have a lightness (V) of less than 5.0, a chroma (C) of 0.05 or more, and the measured color values in the Munsell color system of the colored light under a white background have a lightness (V) of 6.0 or more and a chroma (C) of less than 2.0. A resin-based block for dental cutting characterized by this". And according to Patent Document 4, in the above resin-based block for dental cutting, 90% or more of the individual particles constituting the spherical fillers (B) are present within a range of 5% before and after the average particle diameter, and the resin matrix (A) and the spherical fillers (B) satisfy the condition of nP < nF when the refractive index of the resin matrix (A) at 25°C is nP and the refractive index of the spherical fillers (B) at 25°C is nF. Thus, depending on the particle size of the spherical fillers (B), colored light of a specific color tone is expressed as structural color, and a unique reflection spectrum is clearly confirmed according to the colored light under a black background, but under a white background, it shows a substantially uniform reflectance over a substantial entire range of the visible spectrum, and the light of the visible spectrum is not confirmed, and it is explained that it exhibits an effect of widely harmonizing with various surrounding environments.

[0007] In addition, it is known that a composite material in which inorganic particles are dispersed in a resin matrix, which corresponds to the hybrid resin that is the cutting portion of the above-mentioned dental cutting resin block shown in Patent Document 4, will produce a structural color of a constant tone that is not affected by changes in the angle of incidence of light when the shape and particle size distribution of the inorganic particles, the relationship between the refractive index of the inorganic particles and the refractive index of the resin matrix, and the dispersion state of the inorganic particles satisfy certain conditions (see Patent Document 5). [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Special Publication No. 2016-535610 [Patent Document 2] JP 2017-213394 A [Patent Document 3] International Publication No. 2018 / 074605 [Patent Document 4] International Publication No. 2019 / 189698 Brochure [Patent Document 5] International Publication No. 2020 / 050123 Brochure Summary of the Invention [Problem to be solved by the invention]

[0009] Natural teeth are opaque and reddish yellow in the cervical area, gradually changing to a white transparent color toward the incisal edge, and not only are the incisal and cervical areas of natural teeth significantly different in color, but the overall color tone (sometimes called shade) of natural teeth varies from person to person. Therefore, in order to reproduce the color tone of natural teeth to a high degree, it is necessary to prepare multi-layered mill blanks (of different colors) (hereinafter also referred to as "multi-layered mill blanks") for each overall color tone (shade) in order to reproduce the color tone change from the cervical area to the incisal edge. Not only is the production laborious, but when using them, it is necessary to carefully check the shade of each patient's teeth and select a multi-layered mill blank that matches it from among many candidates.

[0010] On the other hand, when a dental resin block for cutting (hereinafter also referred to as a "structural color resin blank") having a cutting portion made of a hybrid resin that exhibits structural color, as described in Patent Document 4, is used, the above-mentioned effect makes it possible to harmonize the color tone of the dental prosthesis manufactured using this with the color tone of the underlying natural tooth.

[0011] However, the present inventors conducted various studies on dental prostheses produced using the structurally colored resin blanks described in Patent Document 4, and found that, depending on the form, it may not be possible to perform highly aesthetic restorations. That is, in dental prostheses that include a relatively wide area from the vicinity of the cervical area to the incisal end where no natural teeth exist as a base, such as a front tooth crown, which is a dental prosthesis for restoring a front tooth, it was found that, as in the case of a white background, structural colors may not be observed and color adjustment effects may not be obtained.

[0012] Therefore, the present invention aims to provide a resin-based blank for dental cutting processing that can harmonize with a wide variety of surrounding environments by making the most of the advantages of the color compatibility of structural color resin-based blanks, even when producing a dental prosthesis that includes a portion where no natural teeth exist as a base. [Means for solving the problem]

[0013] The present inventors have conducted research to solve the above problems, and have found that when a colored hybrid resin layer is provided as a lower layer of a layer made of a hybrid resin that exhibits structural color, even when a dental prosthesis is fabricated that includes a portion where no natural teeth exist as a base, the layer made of a hybrid resin that exhibits structural color has the effect of "being able to blend in with a wide variety of surrounding environments," and that when the color difference between the two layers is within a specific range, a natural gradation effect can be obtained, which has led to the completion of the present invention.

[0014] That is, one embodiment of the present invention is a dental resin blank for cutting having a cutting part made of a composite material in which inorganic particles are dispersed in a resin matrix, The composite material has a laminated structure in which a first layer and a second layer are bonded together, the first layer is made of a first composite material that exhibits a structural color of a predetermined color tone independent of the angle of incidence of light, the second layer is made of a second composite material having a color tone different from the color tone of the first composite material; The color tone of a composite material having a single color tone is measured by a spectrophotometer on a sample having a thickness of 1.0 ± 0.1 mm against a white background. * Value, a * value and b * When expressed as a value, The following formula is an index of the difference in color tone between the first composite material and the second composite material: ΔE * ={(L1 * -L2 * ) 2 +(a1 * -a2 * ) 2 +(b1 * -b2 * ) 2} 1 / 2 (In the above formula, L1 * , a1 * and b1 * is L in the first composite material * Value, a * value and b * value, L2 * , a2 * and b2 * is L in the second composite material * Value, a * value and b * value.) Color difference defined as: ΔE * is 2 to 30 the law of nature, the total amount of pigment and colorant in the first composite material is 100 ppm by mass or less with respect to the total mass of the first composite material, and the total amount of pigment and colorant in the second composite material is 500 to 7000 ppm by mass with respect to the total mass of the second composite material; The present invention relates to a laminated resin blank for dental cutting.

[0015] In the laminated resin blank for dental cutting of the above-mentioned form (hereinafter also referred to as "the blank of the present invention"), it is preferable that the first composite material satisfies all of the following conditions (a) to (d). (a) The inorganic particles are composed of an aggregate of inorganic spherical particles having a predetermined average primary particle diameter within a range of 100 nm to 1000 nm, and include one or more groups of uniform-diameter spherical particles (G-PID) in which 90% or more of the total number of particles in the number-based particle size distribution of the aggregate are present within a 5% range around the predetermined average primary particle diameter. (b) The number of the uniform particle diameter spherical particle groups contained in the inorganic particles is defined as a, and each uniform particle diameter spherical particle group is classified into G-PID m (However, m is 1 when a is 1, and is a natural number from 1 to a when a is 2 or more.) When a is 2 or more, each G-PID m The average primary particle sizes of the particles differ from each other by 25 nm or more. (c) The refractive index of the resin matrix at 25° C. for light with a wavelength of 589 nm is n (MX) Then, each G-PID m The refractive index of the inorganic spherical particles constituting the (G-PIDm) When (G-PIDm) Also, n (MX) <n (G-PIDm) The relationship is established. (d) in a first composite material , Ren The function expresses the probability that another inorganic spherical particle is present at a point distant r from the center of any inorganic spherical particle, and is expressed by the following formula (1) based on the average particle density of the inorganic spherical particles in an observation plane determined based on a scanning electron microscope image in which the inner surface of the composite material is the observation plane: <ρ>, the number of inorganic spherical particles present in the region between a circle at a distance r from any inorganic spherical particle in the observation plane and a circle at a distance r+dr: dn, and the area of ​​the region: da (where da = 2πr dr). g(r)={1 / 〈ρ〉}×{dn / da} ···(1) When g(r) is the radial distribution function, the inorganic spherical particles constituting all of the "spherical particles of the same diameter" (G-PID) in the composite material are dispersed in the matrix material so as to have a short-range ordered structure that satisfies the following conditions 1 and 2: [Condition 1]: In a radial distribution function graph showing the relationship between r / r0 and the g(r) corresponding to r at that time, the distance from the center of any inorganic spherical particle dispersed in the composite material: r, is divided by the average particle size r0 of all the inorganic spherical particles dispersed in the composite material to obtain a dimensionless number (r / r0) on the x-axis and the radial distribution function: g(r) on the y-axis, the nearest inter-particle distance: r1, which is defined as the r corresponding to the peak top of the peak closest to the origin among the peaks appearing in the radial distribution function graph, is a value between 1 and 2 times the average particle size r0 of all the inorganic spherical particles dispersed in the composite material. [Condition 2]: When r corresponding to the peak top of the peak that is second closest to the origin among the peaks appearing in the radial distribution function graph is defined as the next nearest interparticle distance: r2, the minimum value of the radial distribution function: g(r) between the nearest interparticle distance: r1 and the next nearest interparticle distance: r2 is a value of 0.56 or more and 1.10 or less.

[0017] Furthermore, the transparency of the composite material was measured by measuring the color difference of a sample with a thickness of 1.0 ± 0.1 mm using a spectrophotometer. The Y value was measured against a white background. W Y value on a black background: Y B / Ratio: Y B / Y W When the value determined as above is expressed as an index of contrast ratio: CR, it is preferable that the contrast ratio: CR1 of the first composite material is 0.28 to 0.46, and the contrast ratio: CR2 of the second composite material is 0.50 to 0.65. Effect of the Invention

[0018] In the laminated dental resin blank of the present invention, even when a dental prosthesis is produced that includes a relatively wide area from the vicinity of the cervical part to the incisal part where no natural tooth exists in the base layer, the incisal part is formed of the first layer and the vicinity of the cervical part is formed of the second layer, so that the gradation of the natural tooth from the cervical part to the incisal part can be expressed to a high degree, and the color tone of the natural tooth can be reproduced more accurately. Moreover, since the first layer is made of a hybrid resin that expresses a structural color, the color tone naturally matches the color tone of the second layer. Therefore, it is only necessary to adjust the color tone using a pigment or dye only for the second layer that is located near the cervical part. Therefore, compared with the method disclosed in Patent Document 3, where the chromaticity difference and transparency difference between the three layers are highly adjusted and laminated, the labor required for adjustment and lamination is greatly reduced, and the manufacturing efficiency is greatly improved. Furthermore, the labor required for shade taking during use can be reduced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] 1. Overview of the Blank of the Present Invention The laminated dental resin blank of the present invention has a machinable portion made of a composite material (corresponding to a hybrid resin) in which inorganic particles are dispersed in a resin matrix. The composite material (hybrid resin) constituting the machinable portion has a laminated structure in which a first layer and a second layer are bonded together, the first layer is made of a first composite material which is a composite material that exhibits a structural color of a predetermined color tone independent of the angle of incidence of light, the second layer is made of a second composite material which is a composite material having a color tone different from that of the first composite material, and has a color difference: ΔE which is an index of the difference in color tone between the first composite material and the second composite material. * The second composite material constituting the second layer of the laminated structure may exhibit a structural color of a predetermined color tone independent of the angle of incidence of light, or may not exhibit such a structural color.

[0020] In addition, in the above laminated structure, because the color tone compatibility resulting from the structural color of the first composite material is remarkable, it is preferable that the contrast ratio: CR1 of the first composite material is 0.28 to 0.46, particularly 0.28 to 0.43, and the contrast ratio: CR2 of the second composite material is 0.50 to 0.65, particularly 0.55 to 0.63.

[0021] The blank of the present invention is not particularly different from a conventional hybrid resin-based dental blank for cutting, except that the part to be cut has the above-mentioned laminated structure, and may have a holding member for fixing to a cutting machine, such as a holding pin, if necessary. The shape and size of the part to be cut are also not particularly limited, and may be a (solid) block formed into a rectangular parallelepiped or cylindrical shape, or a (solid) disk formed into a plate or board shape.

[0022] The cut part of the blank of the present invention may be a two-layer structure consisting of only the first and second layers, or may be a three-layer structure having an additional layer, so long as it has the above-mentioned laminated structure. The thickness of each layer is not particularly limited, but is usually in the range of 1 to 13 mm, preferably 2 to 12 mm.

[0023] When the composite material (hybrid resin) constituting the cut part has a laminated structure of three or more layers, it is preferable that the composite material (hybrid resin) has a three-layer or four-layer structure in which a layer made of another composite material (hybrid resin) is bonded to the side opposite to the side of the first layer bonded to the second layer and / or the side opposite to the side of the second layer bonded to the first layer. In this case, when a layer made of another composite material (hybrid resin) (also called the "first layer side additional layer") is bonded to the side opposite to the side of the first layer bonded to the second layer, it is preferable that the layer is made of a composite material (hybrid resin) that has a contrast ratio lower than CR1 and exhibits a structural color of a predetermined color tone independent of the incident angle of light. In addition, when a layer made of another composite material (hybrid resin) (also called the "second layer side additional layer") is bonded to the side opposite to the side of the second layer bonded to the first layer, it is preferable that the layer is made of a composite material (hybrid resin) that has a contrast ratio higher than the contrast ratio of the second composite material: CR2, particularly a composite material (hybrid resin) that does not exhibit a structural color. Furthermore, the color difference between the second layer and the second layer side additional layer is preferably 1-10, and more preferably 2-8.

[0024] As described above, when a dental prosthesis for cavity repair covering a relatively wide area from the vicinity of the cervical region to the incisal edge is produced using the structural color resin blank described in Patent Document 4, the structural color may not be observed due to the strong influence of transmitted light, as in the case of a white background, and the color adjustment effect may not be obtained. On the other hand, when the cut part has the laminated structure described above, the second layer is colored, so that the influence of transmitted light can be reduced, and the first layer can exhibit the inherent characteristics of the structural color resin blank. Therefore, even when a dental prosthesis including a part where no natural tooth exists in the base layer is produced, the dental prosthesis is produced by forming the vicinity of the cervical region with the second layer and the vicinity of the incisal edge with the first layer, so that the part formed by the first layer can be matched to the surrounding color without performing color adjustment using a pigment or dye. In addition, the color difference between the first layer and the second layer: ΔE * Since this is within a certain range, a natural gradation with a moderate blur can be seen between the two layers.

[0025] The first composite material constituting the first layer, the composite material to be the first layer side additional layer added as necessary, and the second composite material and the composite material to be the second layer side additional layer added as necessary when they express structural colors, and the above composite materials contain inorganic spherical particles having a predetermined average (primary) particle size and a predetermined particle size distribution, similar to the composite material used in the structural color resin blank described in Patent Document 4, and express a predetermined structural color (hereinafter also referred to as "specific structural color") that does not depend on the incident angle of light (depending on the average particle size of the spherical particle group of the same particle size contained). As described above, for composite materials (hybrid resins) that express such specific structural colors, conditions that must be satisfied in order to express the specific structural color are known (see Patent Document 5). As these first composite materials, etc. in the present invention, composite materials that satisfy such conditions, specifically all of the conditions (a) to (d) described below {hybrid resins that satisfy all of the conditions (a) to (d) described below and express a specific structural color are hereinafter also referred to as "structural color hybrid resins".} can be used without any particular restrictions.

[0026] On the other hand, when the second composite material and the composite material to be added as the second layer side additional layer as necessary do not exhibit structural color, a hybrid resin that does not satisfy the above conditions {that is, does not satisfy at least one of the conditions (a) to (d) described below}, or a hybrid resin in which the expression of a specific structural color cannot be visually confirmed due to the incorporation of a large amount of pigment, etc. (hereinafter, collectively referred to as "non-structural color hybrid resin") is used.

[0027] In the blank of the present invention, it is extremely important that the first composite material and the second composite material constituting the first layer and the second layer in the laminate structure each have specific characteristics. Therefore, first, these characteristics, namely, the structural color, the specific structural color, and the conditions for the hybrid resin to exhibit the specific structural color, as well as the contrast ratio and color difference, will be explained. Then, the raw materials of the first composite material, the second composite material, etc. and the preparation method thereof, as well as the manufacturing method of the blank of the present invention will be explained.

[0028] In this specification, unless otherwise specified, the expression "x~y" using the numerical values ​​x and y means "greater than or equal to x and less than or equal to y". In such an expression, when a unit is added only to the numerical value y, the unit is also applied to the numerical value x. In addition, in this specification, the term "(meth)acrylic" means both "acrylic" and "methacrylic". Similarly, the term "(meth)acrylate" means both "acrylate" and "methacrylate", and the term "(meth)acryloyl" means both "acryloyl" and "methacryloyl".

[0029] 2. Structural color and specific structural color Structural color is a phenomenon in which light incident on an object having a fine structure reflects light of a specific wavelength due to interference, diffraction, refraction, etc. of the light caused by the fine structure, and structural colors of different colors are observed depending on the angle of incidence (or viewing angle) of light in opals, oil films, etc. In contrast, the laminated resin-based blank for dental cutting of the present invention utilizes a specific structural color in which a specific color is observed regardless of the angle of incidence of light as described above.

[0030] It is known that the above-mentioned specific structural color is expressed by dispersing fine particles having a uniform particle size so that they have a specific short-range order structure while being amorphous overall, and a resin-based material utilizing the specific structural color has also been developed in dental materials, specifically, a single-layered resin-based block for dental cutting consisting only of a composite material that expresses such a structural color (see Patent Document 4).The conditions necessary for expressing the specific structural color in hybrid resin, which is a resin-based material in which inorganic particles are dispersed in a resin matrix, have been clarified.

[0031] 3. Conditions that structural color hybrid resins must satisfy As disclosed in Patent Document 5, in order for a hybrid resin to exhibit a specific structural color, it is necessary to satisfy all of the following conditions (a) to (d).

[0032] (a) The inorganic particles are composed of an aggregate of inorganic spherical particles having a predetermined average primary particle diameter within a range of 100 nm to 1000 nm, and include one or more groups of uniform-diameter spherical particles (G-PIDs) in which 90% or more of the total number of particles in the number-based particle size distribution of the aggregate are present within a 5% range around the predetermined average primary particle diameter. (b) The number of the uniform particle diameter spherical particle groups contained in the inorganic particles is defined as a, and each uniform particle diameter spherical particle group is classified into G-PID m (However, m is 1 when a is 1, and is a natural number from 1 to a when a is 2 or more.) When a is 2 or more, each G-PID m The average primary particle sizes of the particles differ from each other by 25 nm or more. (c) The refractive index of the resin matrix at 25° C. for light with a wavelength of 589 nm is n (MX) Then, each G-PID m The refractive index of the inorganic spherical particles constituting the ( G-PIDm) When (G-PIDm) For n (MX) <n (G-PIDm) The relationship is established. (d) In its composite material (hybrid resin) , Ren The function expresses the probability that another inorganic spherical particle is present at a point distant r from the center of any inorganic spherical particle, and is expressed by the following formula (1) based on the average particle density of the inorganic spherical particles in the observation plane: <ρ>, which is determined based on a scanning electron microscope image in which the internal surface of the composite material is the observation plane, the number of inorganic spherical particles present in the region between a circle at a distance r from any inorganic spherical particle in the observation plane and a circle at a distance r+dr: dn, and the area of ​​the region: da (where da = 2πr dr). g(r)={1 / <ρ>}×{dn / da} ···(1) When g(r) is the radial distribution function, the inorganic spherical particles constituting all of the "spherical particles of the same diameter" (G-PID) in the composite material are dispersed in the matrix material so as to have a short-range ordered structure that satisfies the following conditions 1 and 2.

[0033] [Condition 1]: In a radial distribution function graph showing the relationship between r / r0 and the g(r) corresponding to r at that time, the distance from the center of any inorganic spherical particle dispersed in the composite material: r, is divided by the average particle size r0 of all the inorganic spherical particles dispersed in the composite material to obtain a dimensionless number (r / r0) on the x-axis and the radial distribution function: g(r) on the y-axis, the nearest inter-particle distance: r1, which is defined as the r corresponding to the peak top of the peak closest to the origin among the peaks appearing in the radial distribution function graph, is a value between 1 and 2 times the average particle size r0 of all the inorganic spherical particles dispersed in the composite material. [Condition 2]: When r corresponding to the peak top of the peak that is second closest to the origin among the peaks appearing in the radial distribution function graph is defined as the next nearest interparticle distance: r2, the minimum value of the radial distribution function: g(r) between the nearest interparticle distance: r1 and the next nearest interparticle distance: r2 is a value of 0.56 or more and 1.10 or less.

[0034] The radial distribution function g(r) is generally represented by a radial distribution function graph in which the distance r is plotted on the x-axis (distance axis) and the value of g(r) at r {the calculation result according to the above formula (1)} is plotted on the y-axis (vertical axis), or by a radial distribution function graph in which the distance axis is plotted as a dimensionless number normalized by dividing the r by the average particle diameter of the particles and the y-axis (vertical axis) is plotted as the value of g(r) at r corresponding to the x-axis value (the calculation result according to the above formula).

[0035] For the reason that <ρ> and dn can be easily and reliably confirmed, it is preferable to adopt <ρ> and dn determined based on a scanning electron microscope image in which the internal surface of the first composite material is used as the observation plane, and g(r) calculated by the above formula (1) based on da (=2πr dr) corresponding to the value of dr adopted when determining the above dn.

[0036] The determination of <ρ>, dn, and da based on a scanning electron microscope image with the inner surface of the first composite material as the observation plane can be performed as follows. That is, first, a composite material is prepared by curing a polymerizable curable composition that is the raw material of the first composite material, and a plane (observation plane) where the dispersion state of the inorganic spherical particles inside the composite material can be observed is exposed on the surface by means of polishing the surface of the obtained composite material. Next, the observation plane is observed with a scanning electron microscope, and a microscopic image of an area containing at least 500 inorganic spherical particles in the plane is obtained. After that, the coordinates of the inorganic spherical particles in the area are obtained using image analysis software (e.g., "Simple Digitizer ver3.2" free software) for the obtained scanning electron microscope image. One coordinate of an arbitrary inorganic spherical particle is selected from the obtained coordinate data, and a circle is drawn with a radius of a distance r that includes at least 200 inorganic spherical particles centered on the selected inorganic spherical particle, and the number of inorganic spherical particles contained in the circle is counted to obtain the average particle density <ρ> (unit: particles / cm 2 ) can be determined.

[0037] In addition, dn can be determined by setting dr such that the length of the inorganic spherical particles is about r0 / 100 to r0 / 10 when the average particle diameter of the inorganic spherical particles is represented by r0, and counting the number of inorganic spherical particles contained within the region between a circle whose radius is the distance r from the center of one arbitrarily selected inorganic spherical particle as the center and a circle whose radius is r+dr and whose center is the same as that of the circle. Furthermore, da, which is the area of ​​the region between the two circles, is determined as 2πr·dr based on the length of dr that is actually set.

[0038] In the first composite material, the x-axis represents a dimensionless number (r / r0) obtained by dividing the distance from the center of any inorganic spherical particle dispersed in the composite material by the average particle size r0 of all inorganic spherical particles dispersed in the composite material, and the y-axis represents a radial distribution function g(r) representing the probability that other inorganic spherical particles are present at a point a distance r away from the center of any inorganic spherical particle. In this graph, the relationship between r / r0 and the g(r) corresponding to r at that time is represented by a radial distribution function graph. The nearest inter-particle distance r1, which is defined as the r corresponding to the peak top of the peak closest to the origin among the peaks appearing in the radial distribution function graph, must be 1 to 2 times the average particle size r0 of all inorganic spherical particles dispersed in the composite material (Condition 1). When r1 is less than 1 time r0 (r1 / r0<1), there is a lot of overlap between particles in the plane, and when r1 is more than twice r0 (r1 / r0>2), there is no particle in the vicinity of the selected central inorganic particle, so that short-range order is lost and structural color is not expressed. In other words, from the viewpoint of maintaining short-range order and facilitating the expression of structural color, r1 / r0 is preferably 1.0 or more and 2.0 or less, particularly 1.0 or more and 1.5 or less.

[0039] In addition, in the first composite material, when the r corresponding to the peak top of the peak that is second closest to the origin among the peaks appearing in the radial distribution function graph is taken as the next closest interparticle distance: r2, the minimum value of the radial distribution function: g(r) between the nearest interparticle distance: r1 and the next closest interparticle distance: r2 must be a value of 0.56 or more and 1.10 or less (condition 2). If the minimum value is less than 0.56, the long-range orderliness of the arrangement structure of the inorganic spherical particles is high, and not only does the dependency of the structural color on the incident angle of light increase, but the saturation of the composite material is high, making it difficult to obtain color compatibility when used as a dental filling material. On the other hand, if the minimum value exceeds 1.10, the arrangement structure of the inorganic spherical particles becomes a random structure, making it difficult to obtain the desired reflective performance and difficult to express the desired structural color. That is, from the viewpoint of expressing a structural color and facilitating obtaining color compatibility as a dental filling material, the minimum value is preferably 0.56 or more and 1.10 or less, and more preferably 0.56 or more and 1.00 or less.

[0040] 3.Color difference:ΔE * About Color difference:ΔE * is an index that indicates the degree of difference between two colors, and the larger the value, the more different the color tones of the two are. * For the two tones to be contrasted, the lightness is L * , hue a * , saturation b * Expressed as L * a * b * The numerical values ​​of each coordinate axis in the color space (color system) (L * Value, a * value and b * Difference (ΔL * , Δa * and Δb * ) using the following formula: ΔE * means. ΔE * = {(ΔL * ) 2 +(Δa * ) 2 +(Δb * )2} 1 / 2 In addition, the L for composite materials (hybrid resins) having a single color tone in this specification * Value, a * value and b * The value is the L value obtained by measuring a sample with a thickness of 1.0 ± 0.1 mm with a spectrophotometer against a white background. * , a * and b * Specifically, the L obtained by measuring the spectral reflectance of a white background (a standard white plate is placed on the cured product to block light) in a 5 mm diameter measurement area using a spectrophotometer (Tokyo Denshoku Corporation, "TC-1800MKII", halogen lamp: 12V100W, measurement wavelength range 380-780nm) and the reflected light 0°d method (JIS Z8722) is * , a * and b * is determined by.

[0041] For example, the color difference between the first composite material and the second composite material: ΔE * The L * , a * and b * L1 * , a1 * and b1 * and L in the second composite material * , a * and b * L2 * , a2 * and b2 * Then, ΔL * =L1 * -L2 * Δa * =a1 * -a2 * Δb * =b1 * -b2 * Therefore, ΔE* ={(L1 * -L2 * ) 2 +(a1 * -a2 * ) 2 +(b1 * -b2 * ) 2} 1 / 2 It becomes.

[0042] The color difference is mainly due to the addition of pigments and dyes to the second composite material (L2 * , a2 * and b2 * In this case, the color tone (L1) can be adjusted by adding pigments and dyes to the second composite material within a range that does not impair the effect of the specific structural color of the first composite material. * , a1 * and b1 * ) may be adjusted. Note that if the difference in color tone is large, ΔE * The thickness increases, the lamination interface between layers becomes clearly visible to the naked eye, and the gradation effect that naturally blurs the boundary tends to decrease.

[0043] The first layer allows the inherent characteristics of the structural color resin blank to be exhibited, and allows for a more natural gradation to be expressed. This is why the color difference between the first composite material and the second composite material: ΔE * must be 2 to 30, preferably 2 to 25, and more preferably 2 to 20.

[0044] 3. Contrast ratio: CR=Y B / Y W About Contrast ratio (CR) is an index of transparency of a composite material (resin-based material) in which inorganic particles are dispersed in a matrix resin. In the present invention, it is defined as the Y value (Y) obtained when a color difference measurement is performed on a sample with a thickness of 1.0±0.1 mm using a spectrophotometer against a white background. W Y value for background color black: Y B / Ratio: Y B / YW The smaller the contrast ratio (CR), the higher the transparency, and the larger the CR, the lower the transparency.

[0045] Specifically, the contrast ratio is determined by measuring the spectral reflectance of a black background (light-shielded state) and a white background (light-shielded state with a standard white plate placed over the cured product) in a measurement area of ​​5 mmφ using the reflected light 0°d method (JIS Z8722) with a spectrophotometer (Tokyo Denshoku Corporation, "TC-1800MKII", halogen lamp: 12V 100W, measurement wavelength range 380-780nm).

[0046] The contrast ratio can be adjusted by adjusting the amount of ultrafine particles (G-SFP) made of inorganic particles with an average primary particle diameter of less than 100 nm, or coloring substances such as pigments and dyes.

[0047] In the laminated dental resin blank of the present invention, the contrast ratios of the first and second composite materials constituting the first and second layers in the laminated structure included in the machining part are preferably within a predetermined range. That is, the contrast ratio CR1 of the first composite material is preferably 0.28 to 0.46, and the contrast ratio CR2 of the second composite material is preferably 0.50 to 0.65. If the CR1 value is outside the above range, it is difficult to observe the specific structural color, and it tends to be difficult to achieve harmony with the surrounding color tone. In addition, if the CR2 value is outside the above range, when a dental prosthesis is manufactured that includes a portion in which no natural teeth are present in the base layer, it tends to be difficult to exhibit the "effect of being able to widely harmonize with various surrounding environments" of the first layer that expresses structural color.

[0048] From the viewpoint of effectiveness, it is preferable that CR1 is 0.28 to 0.46, particularly 0.28 to 0.43, and CR2 is 0.50 to 0.65, particularly 0.55 to 0.63. In addition, the difference from the contrast ratio: CR2-CR1=ΔCR=ΔY B / Y W is preferably 0.10 or more, and particularly preferably 0.12 to 0.27.

[0049] 5. Raw materials and manufacturing methods for structural color hybrid resins As described above, the first composite material constituting the first layer, the composite material which becomes the first layer side additional layer added as necessary, and the second composite material and the composite material which becomes the second layer side additional layer added as necessary when they exhibit structural color are structural color hybrid resins, and the second composite material and the composite material which becomes the second layer side additional layer added as necessary when the second composite material does not exhibit structural color are non-structural color hybrid resins.

[0050] The structural color hybrid resin used in the present invention is not particularly different from the composite material described in claim 1 of Patent Document 5, except that it does not require ultrafine particles (G-SFP) from inorganic particles with an average primary particle diameter of 100 nm. The raw materials and preparation method are also not particularly different from the raw materials and preparation method described in claim 9 of Patent Document 5, except for the above points.

[0051] That is, a curable composition containing a polymerizable monomer, inorganic particles that satisfy certain conditions, and a polymerization initiator is used as a raw material composition (hereinafter referred to as "structural color raw material composition"). The inorganic particles in the structural color raw material composition are made to have a specific dispersion state, and then the composition is cured, thereby producing a structural color hybrid resin such as a first composite material.

[0052] Here, the conditions that the inorganic particles must satisfy are the following (i) to (iii). (i) The particle is composed of an aggregate of inorganic spherical particles having a predetermined average primary particle diameter within a range of 100 nm to 1000 nm, and in a number-based particle size distribution of the aggregate, 90% or more of the total number of particles include uniform spherical particle groups (G-PID) existing within a 5% range around the predetermined average primary particle diameter, and the number of uniform spherical particle groups is one or more. (ii) The number of the uniform particle diameter spherical particle groups contained in the inorganic particles is defined as a, and each uniform particle diameter spherical particle group is classified into G-PID m (However, m is 1 when a is 1, and is a natural number from 1 to a when a is 2 or more.) m The average primary particle sizes of the particles differ from each other by 25 nm or more. (iii) The refractive index of the cured product of the polymerizable monomer at 25° C. is n (MX) Then, each G-PID m The refractive index of the inorganic spherical particles at 25°C is n (G-PIDm) When (G-PIDm) Also, n (MX) <n (G-PIDm) The relationship is established.

[0053] The conditions for the dispersion state that the structural color raw material composition should satisfy are as shown in the following (I) and (II). (I) In a radial distribution function graph showing the relationship between r / r0 and g(r) corresponding to r at that time, the x-axis is a dimensionless number (r / r0) obtained by dividing the distance r from the center of any inorganic spherical particle dispersed in the hardened body of the structural color raw material composition by the average particle diameter r0 of all inorganic spherical particles dispersed in the hardened body of the raw material composition, and the y-axis is a radial distribution function g(r) representing the probability that other inorganic spherical particles exist at a point distant r from the center of the any inorganic spherical particle. The nearest inter-particle distance r1, defined as the r corresponding to the peak top of the peak closest to the origin among the peaks appearing in the radial distribution function graph, is 1 to 2 times the average particle diameter r0 of all inorganic spherical particles dispersed in the hardened body of the mixture. (II) When r corresponding to the peak top of the peak that is second closest to the origin among the peaks appearing in the radial distribution function graph is defined as the next nearest interparticle distance r2, the minimum value of the radial distribution function g(r) between the nearest interparticle distance r1 and the next nearest interparticle distance r2 is a value of 0.56 to 1.10.

[0054] The above conditions (i) to (iii) correspond to the conditions (a) to (c) that the structural color hybrid resin must satisfy, and the hardened polymerizable monomer contained in the structural color raw material composition corresponds to the resin matrix of the structural color hybrid resin (e.g., the resin matrix in the first composite material), and the inorganic particles contained in the structural color raw material composition correspond to the inorganic particles dispersed in the resin matrix of the structural color hybrid resin (e.g., the inorganic particles dispersed in the resin matrix in the first composite material). Regarding the above condition (iii), from the viewpoint of the visibility and clarity of the structural color and the color compatibility when used as a dental cutting blank, n (G-PIDm) and (MX) The difference between (G-PIDm) -n (MX) ) is preferably 0.001 or more and 0.1 or less, more preferably 0.002 or more and 0.1 or less, and most preferably 0.005 or more and 0.05 or less.

[0055] Furthermore, satisfying the above conditions (I) and (II) corresponds to the condition (a) that a structural color hybrid resin must satisfy.

[0056] Below, the raw materials of the structural color raw material composition that serves as the raw material for the structural color hybrid resin such as the first composite material (in other words, the hardened body thereof becomes the structural color hybrid resin such as the first composite material) will be described.

[0057] 5-1. Polymerizable monomers that are the raw materials for structural color raw material compositions The polymerizable monomer in the structural color raw material composition is a monomer whose hardened form becomes the resin matrix of the structural color hybrid resin. As the polymerizable monomer, a radically polymerizable monomer can be suitably used. The radically polymerizable monomer is not particularly limited, and can be appropriately selected from (meth)acrylic compounds, cationic polymerizable monomers such as epoxies and oxetanes, and the like. For example, in order to obtain a dental polymerizable hardening composition, it is preferable to use a (meth)acrylic compound. Examples of (meth)acrylic compounds that can be suitably used include methyl (meth)acrylate, ethyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, (meth)acrylic acid, N-(meth)acryloylglycine, p-vinylbenzoic acid, 2-(meth)acryloyloxybenzoic acid, 6-(meth)acryloyloxyethylnaphthalene-1,2,6-tricarboxylic acid anhydride, 13-(meth)acryloyloxytridecane-1,1-dicarboxylic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, N-hydroxypropyl (meth)acrylate, 1 ... Examples of the copolymer include ethyl (meth)acrylamide, N,N-(dihydroxyethyl)(meth)acrylamide, 2,2-bis(methacryloyloxyphenyl)propane, 2,2-bis[(3-methacryloyloxy-2-hydroxypropyloxy)phenyl]propane, ethylene glycol dimethacrylate, triethylene glycol dimethacrylate, 1,6-bis(methacrylethyloxycarbonylamino)trimethylhexane, trimethylolpropane trimethacrylate, pentaerythritol tetramethacrylate, neopentyl glycol dimethacrylate, and 4,4-diphenylmethane diisocyanate.

[0058] A plurality of types of these (meth)acrylate polymerizable monomers may be used in combination as necessary.

[0059] As the polymerizable monomer, a plurality of polymerizable monomers are generally used to adjust the physical properties (mechanical properties and adhesiveness to tooth structure in dental applications) of the hardened body that becomes the resin matrix of the structural color hybrid resin. In this case, it is desirable to set the type and amount of the polymerizable monomer so that the refractive index of the polymerizable monomer composition (mixture) at 25°C is in the range of 1.38 to 1.55, from the viewpoint of easily satisfying the above-mentioned condition regarding the refractive index. That is, when a silica-titanium group element oxide-based composite oxide, which is easy to adjust the refractive index, is used as the inorganic spherical particle, the refractive index at 25°C is in the range of about 1.45 to 1.58 depending on the content of silica, but by setting the refractive index of the polymerizable monomer composition in the range of 1.38 to 1.55, the refractive index of the obtained hardened body can be adjusted to about 1.40 to 1.57, making it easy to satisfy the above-mentioned condition. The refractive index of the polymerizable monomer and the hardened body of the polymerizable monomer can be determined at 25°C using an Abbe refractometer.

[0060] 5-2. Inorganic particles as raw materials for structural color raw material composition The structural color raw material composition contains inorganic particles in an amount of usually 100 to 900 parts by weight, preferably 150 to 700 parts by weight, based on 100 parts by weight of the polymerizable monomer. The inorganic particles contained in the structural color raw material composition are also inorganic particles dispersed in the resin matrix of the structural color hybrid resin, and contain one or more "spherical particles of the same particle size" (G-PID). In order for the inorganic spherical particles constituting the G-PID to be dispersed in the matrix material so as to have a short-range ordered structure that satisfies the above conditions, it is preferable that the inorganic particles do not contain inorganic particles (regardless of their shape) having an average primary particle size in the range of 100 to 1000 nm other than the G-PID. However, the ultrafine particle group (G-SFP) with an average primary particle diameter of less than 100 nm is unlikely to affect the short-range ordered structure, and has the function of controlling the viscosity of the structural color raw material composition and the contrast ratio of the structural color hybrid resin depending on the amount of the ultrafine particle group (G-SFP), so it is preferable to mix it in the range of 0.1 to 40 parts by mass, especially 0.2 to 30 parts by mass, per 100 parts by mass of the polymerizable monomer.

[0061] When the structural color raw material composition is substantially free of coloring substances such as dyes and pigments (for example, when the concentration of the coloring substances is 100 mass ppm or less, preferably 50 mass ppm or less), and the amount of G-SFP is within this range, the contrast ratio of the resulting structural color hybrid resin can be set to 0.28 to 0.46.

[0062] The amount of the spherical particles of the same particle size: G-PID is usually 100 to 900 parts by mass relative to 100 parts by mass of the polymerizable monomer, which is the total amount of all G-PIDs contained (i.e., the total amount of inorganic spherical particles). Since the structural color hybrid resin has moderate transparency and has a high effect of expressing structural color, the amount of G-PID is preferably 100 to 900 parts by mass, and more preferably 150 to 700 parts by mass, relative to 100 parts by mass of the polymerizable monomer, when the structural color raw material composition does not contain ultrafine particles (G-SFP). In addition, when G-SFP is contained, it is preferable to subtract the amount of G-SFP from the above amount.

[0063] In addition, when multiple types of G-PID are included, the amount of each G-PID should be appropriately allocated so that the total amount is within the above range, taking into consideration the color tone of the structural color of each G-PID and the desired color tone of the dental cutting blank.

[0064] The inorganic spherical particles, G-PID, G-SFP, and the like constituting the inorganic particles will be described in detail below.

[0065] (1) Inorganic spherical particles The inorganic spherical particles constituting the G-PID are not particularly limited as long as they satisfy the above-mentioned conditions for constituting the G-PID. Examples of materials that can be suitably used include amorphous silica, silica-titanium group element oxide composite oxide particles (silica-zirconia, silica-titania, etc.), quartz, alumina, barium glass, strontium glass, lanthanum glass, fluoroaluminosilicate glass, ytterbium fluoride, zirconia, titania, colloidal silica, etc. Among these, it is preferable to use particles made of silica-titanium group element oxide composite oxide, which is a composite oxide of silica and titanium group element (group 4 element of the periodic table) oxide, because the refractive index can be easily adjusted. In the silica-titanium group element oxide composite oxide, the refractive index at 25°C can be changed in the range of about 1.45 to 1.58 depending on the silica content. Specific examples of silica-titanium group element oxide composite oxide particles include silica-titania, silica-zirconia, and silica-titania-zirconia.

[0066] The inorganic spherical particles may be surface-treated with a silane coupling agent.

[0067] (2) Group of spherical particles with the same particle size: G-PID The term "spherical particle group of uniform size (G-PID)" refers to an aggregate of inorganic spherical particles having a predetermined average primary particle size within the range of 100 to 1000 nm, in which the individual inorganic spherical particles constituting the aggregate are substantially composed of the same substance, and in the number-based particle size distribution of the aggregate, 90% or more of the total number of particles are present within a range of 5% around the predetermined average primary particle size.

[0068] The average primary particle diameter of the inorganic spherical particles referred to here means the average value obtained by taking a photograph of the G-PID with a scanning electron microscope, selecting 30 or more particles observed within a unit visual field of the photograph, and determining the primary particle diameter (maximum diameter) of each of them. In addition, the spherical shape may be approximately spherical, and does not necessarily have to be a perfect sphere. A photograph of the G-PID is taken with a scanning electron microscope, and the maximum diameter of each particle (30 or more) within the unit visual field is measured. The average uniformity obtained by dividing the particle diameter in the direction perpendicular to the maximum diameter by the maximum diameter is 0.6 or more, more preferably 0.8 or more.

[0069] In structural color hybrid resins such as the first composite material, the constituent inorganic particles of G-PID, which is an aggregate of inorganic particles with a spherical shape and a narrow particle size distribution (number-based particle size distribution), have a specific short-range order structure and are dispersed in a resin matrix, causing diffraction interference according to the Bragg condition, emphasizing light of a specific wavelength and generating colored light of a color tone according to the average primary particle diameter (structural color is expressed). In other words, in order to express structural color, 90% (by number) or more of the inorganic spherical particles constituting G-PID must be present within a range of 5% around the average primary particle diameter. In addition, in order to express structural color with a specific color tone within a wide range of blue to yellow to red, the average primary particle diameter of the inorganic spherical particles constituting G-PID must be within the range of 100 to 1000 nm. When the average primary particle diameter is 230 to 800 nm, a yellow to red structural color (colored light) is likely to be expressed, and when the average primary particle diameter is less than 150 nm to 230 nm, a blue structural color (colored light) is likely to be expressed.

[0070] The average primary particle size of G-PID is preferably 230 to 800 nm, more preferably 240 to 500 nm, and particularly preferably 260 to 350 nm, because it expresses a yellow to red structural color (colored light) that is preferable for restoring natural teeth. When G-PID having an average primary particle size in the range of 230 nm to 260 nm is used, the obtained colored light is yellowish, which is useful for restoring teeth in the category of B (reddish yellow) in the shade guide ("VITA Classical", manufactured by VITA Co., Ltd.). When G-PID having an average primary particle size in the range of 260 nm to 350 nm is used, the obtained colored light is redish, which is useful for restoring teeth in the category of A (reddish brown) in the shade guide ("VITA Classical", manufactured by VITA Co., Ltd.). Since the hue of dentin is often reddish, the embodiment using only G-PID with an average primary particle size of 260 nm to 350 nm is the most preferable because it has a wide compatibility with various colors of restored teeth. On the other hand, when only G-PID with a particle size of less than 150 nm to 230 nm is used, the colored light obtained is blueish as described above, and the color compatibility with the tooth tissue is likely to be poor for cavities formed from the enamel to the dentin, but it is useful for restoring enamel, especially for restoring the incisal edge.

[0071] The G-PID contained in the inorganic particles contained in the structural color raw material composition (dispersed in the resin matrix in the structural color hybrid resin such as the first composite material) may be one or more types. The number of G-PIDs contained: a is preferably 1 to 5, particularly preferably 1 to 3, and most preferably 1 or 2.

[0072] However, if the inorganic particles contain multiple types of G-PID, each G-PID m The average primary particle diameters of the G-PIDs must differ from each other by 25 nm or more. In other words, when the number of G-PIDs contained in the inorganic particles is "a" (for example, "3"), the G-PIDs are sorted in order of the smallest average primary particle diameter. m(However, m is 1 when a is 1, and is a natural number from 1 to a when a is 2 or more.) m (For example, G-PID1, G-PID2, and G-PID3 when a = 3) may have different materials constituting individual particles. m The average primary particle diameter of each m Then, for each d m must differ from each other by 25 nm or more (for example, when a=3, |d1-d2|≧25 nm, |d2-d3|≧25 nm, and of course |d1-d3|≧25 nm). By satisfying this condition, for example, each G-PID can be dispersed in the form of an aggregate of a small number of inorganic spherical particles, not exceeding about 20, which is aggregated with a very loose binding force, and it is believed that this is because it becomes possible to disperse with a short-range order structure that can express a structural color for each G-PID, and as a result, it becomes possible to express a unique structural color (according to the average primary particle size) for each G-PID. On the other hand, if this condition is not satisfied, the particle size distribution of the inorganic spherical particles as a whole becomes broad, and probably the inorganic spherical particles constituting each G-PID are dispersed by mutual substitution, and it becomes difficult to express a structural color, which is believed to be due to the same phenomenon that occurs when an aggregate of a single inorganic spherical particle that does not satisfy the condition of the number-based particle size distribution is used.

[0073] When multiple G-PIDs are used, each G-PID m Average primary particle diameter d m are different from each other by more than 30 nm, especially more than 40 nm (i.e., d m and d m―1 The difference between the thickness and the thickness is preferably 30 nm or more, and more preferably 40 nm or more. m and d m―1 The difference between them is preferably 100 nm or less, and more preferably 60 nm or less.

[0074] In addition, when a structural color raw material composition, and in turn a structural color hybrid resin such as the first composite material, contains multiple G-PIDs, each G-PID has a very sharp particle size distribution, and since there is a difference in the average primary particle diameter as described above, the particle size distributions of each G-PID are unlikely to overlap, and even if they overlap in part, it is possible to confirm the particle size distribution of each G-PID. That is, the particle size distribution of inorganic particles, the particle size distribution of each G-PID, has the same number of independent peaks as the number of G-PIDs contained in the range of 100 nm to 1000 nm, and even if each peak overlaps in part, the average primary particle diameter and number-based particle size distribution of each G-PID can be confirmed by performing waveform processing. In addition, the particle size distribution of inorganic particles contained in a structural color hybrid resin such as the first composite material can be confirmed, for example, by image processing an electron microscope photograph of its internal surface.

[0075] (3) Organic-inorganic composite filler At least a part of the one or more "same-sized spherical particle groups" (G-PID) comprises one type of "same-sized spherical particle groups" (G-PID) and a resin whose refractive index at 25°C is smaller than that of the inorganic spherical particles constituting the one type of "same-sized spherical particle groups" (G-PID), and is preferably blended as an organic-inorganic hybrid filler that does not contain any "same-sized spherical particle groups" (G-PID) other than the one type of "same-sized spherical particle groups" (G-PID), in other words, an "organic-inorganic hybrid filler that contains only a single G-PID." Here, the organic-inorganic hybrid filler is a composite consisting of an inorganic filler dispersed in an (organic) resin matrix. powder The term "filler" refers to a filler consisting of an aggregate in which primary particles of an inorganic filler are bound together with an (organic) resin.

[0076] For example, three types of G- PIDThat is, when G-PID1, G-PID2, and G-PID3 are included, it is preferable to mix all or a part of at least one of them as an "organic-inorganic composite filler containing only a single G-PID". When all of G-PID1 is mixed into the structural color raw material composition as an organic-inorganic composite filler (composite filler 1) containing only G-PID1, only G-PID1 is included in the composite filler 1, so that the short-range order structure that expresses the structural color of G-PID1 is realized, and the structural color of G-PID1 is surely expressed in the structural color hybrid resin such as the first composite material obtained by curing the structural color raw material composition. From the viewpoint of expecting such an effect and further facilitating the adjustment of the viscosity of the structural color raw material composition, it is preferable to mix 10% to 90%, particularly 20% to 80%, and further 30% to 70% of each G-PID as an "organic-inorganic composite filler containing only a single G-PID".

[0077] In addition, when G-PID is mixed in a form other than "organic-inorganic composite filler containing only a single G-PID", powder It is common to compound the G-PID in the form of a solid (G-PID itself as an aggregate of inorganic spherical particles), but it is also possible to compound it as an organic-inorganic composite filler containing multiple types of G-PID.

[0078] When blended as an organic-inorganic composite filler, it is important that the refractive index at 25°C of the resin constituting the (organic) resin matrix is ​​smaller than that of the inorganic spherical particles contained in the organic-inorganic composite filler. The resin is not particularly limited as long as it satisfies these conditions, but it is preferably a hardened product of the polymerizable monomer in the raw material composition. In this case, it is not necessary for the resin to have exactly the same composition as the polymerizable monomer component of the raw material composition, but it is preferable to use one whose refractive index at 25°C is equivalent to that of the polymerizable monomer component at 25°C. In addition, the refractive index of the resin at 25°C is set to n (R) The refractive index of the inorganic spherical particles at 25° C. is n (F)In this case, in any organic-inorganic composite filler, n (R) <n (F) The relationship must be satisfied. When the organic-inorganic composite filler contains inorganic spherical particles having different refractive indices at 25° C., this relationship must be satisfied for all inorganic spherical particles. (F) and (R) The difference between Δn(=n (F) -n (R) ) is preferably 0.001 or more and 0.01 or less, and more preferably 0.001 or more and 0.005 or less.

[0079] The average particle size of the organic-inorganic composite filler is not particularly limited, but from the viewpoint of improving the mechanical strength of the cured body and the handleability of the curable paste, it is preferably 2 to 100 μm, more preferably 5 to 50 μm, and particularly preferably 5 to 30 μm.

[0080] The amount of the organic-inorganic composite filler in the raw material composition may be determined by converting the amount of the inorganic spherical particles contained in the organic-inorganic composite filler into the amount of G-PID, a group of spherical particles having the same particle size that is not formed into an organic-inorganic composite filler and is contained in the raw material composition, so that the total amount of all G-PID contained (i.e., the total amount of inorganic spherical particles) is the amount described above.

[0081] (4) Ultrafine particle group: G-SFP The ultrafine particle group (G-SFP), which may be contained in the inorganic particles, is a particle aggregate consisting of inorganic particles having an average primary particle diameter of less than 100 nm, and is blended for the purpose of adjusting the viscosity of the hardenable composition that is the precursor of the first composite material (a material for obtaining a dental cutting blank by hardening), or for the purpose of adjusting the contrast ratio of the dental cutting blank. However, the average primary particle diameter of G-SFP must be 25 nm or more smaller than the average primary particle diameter (d1) of G-PID1, which has the smallest average primary particle diameter among the G-PIDs blended with the inorganic particles. If such conditions are not satisfied, the dispersion state of the inorganic spherical particles is adversely affected, making it difficult to express the specific structural color. The shape of the inorganic particles constituting the G-SFP is not particularly limited, and may be either amorphous or spherical. The lower limit of the average primary particle diameter is usually 2 nm.

[0082] The average primary particle size of G-SFP is preferably 3 nm to 75 nm, particularly 5 nm to 50 nm, because it has little effect on the expression of structural color. For the same reason, it is preferably 30 nm or more, particularly 40 nm or more smaller than the average primary particle size (d1) of G-PID1.

[0083] The material of the inorganic particles constituting G-SFP can be the same as that of the inorganic spherical particles without any particular limitation. Also, surface treatment can be performed with a silane coupling agent in the same manner as that of the inorganic spherical particles. The preferred embodiment is also basically the same as that of the inorganic spherical particles, except for the average primary particle size and shape.

[0084] 5-3. Polymerization initiators as raw materials for structural color raw material compositions The polymerization initiator, which is a raw material of the structural color raw material composition, is not particularly limited as long as it has the function of polymerizing and curing the polymerizable monomer. The polymerization method of the curable composition may be a reaction by light energy such as ultraviolet light or visible light (hereinafter referred to as photopolymerization), a chemical reaction between a peroxide and an accelerator, or a method by heat energy (hereinafter referred to as thermal polymerization). Photopolymerization and thermal polymerization are preferred because the timing of polymerization can be freely selected by external energy such as light or heat, and the operation is simple. Thermal polymerization is particularly preferred because it is less likely to cause polymerization unevenness due to light irradiation and can carry out the polymerization reaction uniformly.

[0085] Examples of photopolymerization initiators include benzoin alkyl ethers such as benzoin methyl ether, benzoin ethyl ether, and benzoin isopropyl ether; benzil ketals such as benzil dimethyl ketal and benzil diethyl ketal; benzophenones such as benzophenone, 4,4'-dimethylbenzophenone, and 4-methacryloxybenzophenone; α-diketones such as diacetyl, 2,3-pentanedione benzyl, camphorquinone, 9,10-phenanthraquinone, and 9,10-anthraquinone; 2,4-diethoxythioxanthone; Examples of the thioxanthone compounds that can be used include thioxanthone compounds such as 2-chlorothioxanthone and methylthioxanthone; and bisacylphosphine oxides such as bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide.

[0086] Incidentally, a reducing agent is often added to the photopolymerization initiator. Examples of such a reducing agent include tertiary amines such as 2-(dimethylamino)ethyl methacrylate, ethyl 4-dimethylaminobenzoate, and N-methyldiethanolamine; aldehydes such as lauryl aldehyde, dimethylaminobenzaldehyde, and terephthalaldehyde; and sulfur-containing compounds such as 2-mercaptobenzoxazole, 1-decanethiol, thiosalicylic acid, and thiobenzoic acid.

[0087] Furthermore, in addition to the above-mentioned photopolymerization initiator and reducing compound, a photoacid generator is often used. Examples of such photoacid generators include diaryliodonium salt compounds, sulfonium salt compounds, sulfonate compounds, halomethyl-substituted S-triazine derivatives, and pyridinium salt compounds.

[0088] Examples of the thermal polymerization initiator include peroxides such as benzoyl peroxide, p-chlorobenzoyl peroxide, tert-butylperoxy-2-ethylhexanoate, tert-butylperoxydicarbonate, and diisopropylperoxydicarbonate; azo compounds such as azobisisobutyronitrile; boron compounds such as tributylborane, tributylborane partial oxide, sodium tetraphenylborate, sodium tetrakis(p-fluorophenyl)borate, and triethanolamine tetraphenylborate; barbituric acids such as 5-butylbarbituric acid and 1-benzyl-5-phenylbarbituric acid; and sulfinic acid salts such as sodium benzenesulfinate and sodium p-toluenesulfinate.

[0089] These polymerization initiators may be used alone or in combination of two or more. It is also possible to combine a plurality of initiators which use different polymerization methods.

[0090] The amount of the polymerization initiator to be added may be selected according to the purpose, and is usually 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, per 100 parts by mass of the polymerizable monomer.

[0091] The polymerization temperature when using a thermal polymerization initiator is preferably 60 to 200°C, more preferably 70 to 150°C, and even more preferably 80 to 130°C. If polymerization is performed at a temperature below 60°C, the polymerization reaction becomes insufficient, the strength of the dental cutting blank is weakened, and cracks occur. On the other hand, if polymerization is performed at a temperature above 200°C, the structural color hybrid resin is exposed to high temperatures during production, causing discoloration of the resin component, making it difficult to achieve the effect of the present invention of matching color with natural teeth.

[0092] 5-4. Other additives that are used as raw materials for structural color raw material compositions The structural color raw material composition may contain other additives such as polymerization inhibitors and ultraviolet absorbers within the range that does not impair the effect of the composition.

[0093] The hardened product of the structural color raw material composition, including the first composite material, becomes a structural color hybrid resin, and as described above, it expresses a specific structural color without using a coloring substance such as a pigment. Therefore, there is no particular need to blend coloring substances such as dyes and pigments that may discolor over time into the structural color hybrid resin, and it is preferable not to include coloring substances from the viewpoint of preventing discoloration and transparency. However, the blending of these coloring substances is not excluded, and they can be blended within a range that does not hinder the effect of the specific structural color. Depending on the amount of inorganic particles and the like contained in the structural color raw material composition that is the raw material of the first composite material, the (allowable) blending amount of the coloring substance based on the total mass of the structural color raw material composition (which is also the total mass of the first composite material) is usually 100 mass ppm or less, preferably 50 mass ppm or less. However, with regard to the structural color raw material composition that is the raw material of the composite material that becomes the second composite material and the second layer side additional layer formed as necessary, the effect of coloring takes precedence over the effect of the specific structural color, so it is necessary to blend the coloring substance so that the color difference from the first composite material is within a predetermined range, as described below.

[0094] 5-5. Method for preparing raw material composition The raw material composition can be prepared by kneading and defoaming predetermined amounts of each of the above components. In order to reliably satisfy the conditions (I) and (II) for the dispersion state, it is preferable to adjust as follows. That is, as for the kneading method, it is preferable to knead using a kneading device such as a planetary motion stirrer, because it is possible to satisfy the above dispersion conditions in a short time and scale-up production is easy. In addition, as for the defoaming treatment, it is preferable to adopt a method of defoaming under reduced pressure, because it is possible to remove air bubbles in a short time even from a highly viscous composition.

[0095] In this method, the kneading and degassing treatments need to be performed under kneading and degassing treatment conditions that have been confirmed to result in a dispersion state of the inorganic particles (b) in a hardened body obtained by hardening the resulting kneaded product satisfying the conditions (I) and (II).

[0096] Such conditions are preferably (1) prepared in advance by changing the kneading conditions and degassing conditions in a plurality of ways using a curable composition having the same or substantially the same composition as the raw material composition to be actually produced, and determining the conditions that satisfy the conditions (I) and (II) by examining the radial-radial distribution function: g(r) of the cured product of the curable composition prepared under each condition, and adopting the same conditions as the determined conditions. Since the target first polymerizable curable composition can be reliably produced simply by setting the predetermined kneading conditions, it is not necessary to change the conditions each time when producing the same first polymerizable curable composition (same composition and same amount) every time, and excessive kneading (kneading for an unnecessarily long time) can be prevented, which improves the efficiency of the work.

[0097] 6. Non-structural color hybrid resins and their raw materials A non-structural color hybrid resin is a hybrid resin that does not satisfy at least one of the above conditions (a) to (d), or a hybrid resin in which the expression of a specific structural color cannot be visually confirmed due to the incorporation of a large amount of pigment, etc., and is used as a composite material when the second composite material and the composite material that becomes the second layer side additional layer, which is added as necessary, do not express a structural color.

[0098] As described above, the second composite material has a different color tone from the first composite material, and the color difference must be within a specific range. The contrast ratio: CR2 of the second composite material is preferably 0.50 to 0.65. Since the first composite material is not usually colored by adding a coloring material such as a dye or pigment in order to obtain an effect due to a specific structural color, a coloring substance is usually blended into the second composite material and the raw material composition that is the raw material thereof. This point is also true for the composite material that becomes the second layer side additional layer that is added as necessary, and the raw material composition thereof.

[0099] That is, the non-structural color hybrid resin, which is a composite material that becomes the second composite material and the second layer side additional layer added as necessary, is a composite material in which inorganic particles are dispersed in a resin matrix, and a coloring material such as a dye or pigment is added so that the color difference from the first composite material is within a specific range, and is obtained by curing a polymerizable curable composition (hereinafter also referred to as "non-structural color raw material composition") containing a polymerizable monomer, inorganic particles, a polymerization initiator, and a coloring material. The non-structural color raw material composition may be a structural color raw material composition to which a coloring material is added (in an amount such that the specific structural color cannot be visually confirmed), and the same polymerizable monomer and polymerization initiator as those in the structural color raw material composition can be used. There are no particular restrictions on the inorganic particles as in the structural color raw material composition, and those that are considered to be usable in conventional dental cutting resin blanks can be used without particular restrictions. The total amount of inorganic particles is usually 100 to 900 parts by weight, preferably 150 to 700 parts by weight, relative to 100 parts by weight of the polymerizable monomer. The amount of the coloring substance contained in the non-structural color raw material composition is usually 500 to 7000 mass ppm, preferably 600 to 6500 mass ppm, based on the total mass of the non-structural color raw material composition (which is also the total mass of the composite material that is the cured product thereof). In addition, the composition may contain other additives such as ultrafine particle group (G-SFP) for adjusting the color tone and contrast ratio of the cured product, polymerization inhibitors, and ultraviolet absorbers.

[0100] In the blank of the present invention, the second composite material and the non-structural color hybrid resin which forms the second layer side additional layer added as necessary are often materials which constitute the vicinity of the cervical part of the tooth in a dental prosthesis. Furthermore, there are large individual differences in the color tone of the cervical part of the tooth, and it is necessary to prepare a color tone that suits each individual patient. However, by adding a coloring substance, it is possible to meet such requirements.

[0101] The coloring material (colorant) may be a pigment or a dye. The pigment is typically an inorganic pigment, and examples of such inorganic pigments include titanium oxide, zinc oxide, zirconium oxide, zinc sulfide, aluminum silicate, calcium silicate, carbon black, iron oxide, copper chromite black, chromium oxide green, chrome green, violet, chrome yellow, lead chromate, lead molybdate, cadmium titanate, nickel titanium yellow, ultramarine blue, cobalt blue, bismuth vanadate, cadmium yellow, and cadmium red. In the present invention, the inorganic pigment also corresponds to an inorganic filler. In addition, organic pigments such as monoazo pigments, diazo pigments, diazo condensation pigments, perylene pigments, and anthraquinone pigments can also be used. Examples of dyes include red dyes such as KAYASET RED G (Nippon Kayaku) and KAYASET REDB (Nippon Kayaku), yellow dyes such as KAYASET Yellow 2G and KAYASET Yellow GN, and blue dyes such as KAYASET Blue N, KAYASET Blue G and KAYASET Blue B. Considering color stability in the oral cavity, it is preferable to use water-insoluble pigments rather than water-soluble dyes.

[0102] 7. Method for producing the blank of the present invention The blank of the present invention can be produced by appropriately processing a laminate of the hybrid resin having the above-mentioned laminate structure into a part to be machined.

[0103] The hybrid resin laminate can be suitably manufactured by casting polymerization using a curable raw material composition that is the raw material of the hybrid resin (composite) that constitutes each layer. Here, casting polymerization means that a mold of a predetermined shape is filled with a polymerizable curable composition and then polymerized and cured. The volume of the mold may be appropriately selected according to the desired shape. Similarly, the shape of the mold may be a rectangular column, a cylindrical column, a square plate, a disk, or other irregular shape, and is not particularly limited. During polymerization, pressure may be applied with an inert gas such as nitrogen, as necessary. A mold having the same or substantially the same shape as the part to be cut is prepared, and the curable raw material composition that will be each layer is filled in sequence to a predetermined thickness inside the mold, and then polymerized and cured, and the obtained bulk body (hybrid resin laminate) may be used as the part to be cut as it is, or a bulk body may be manufactured by filling a mold having a larger size, and the bulk body may be punched or cut to be the part to be cut. The filling method can be a known technique and is not particularly limited, but for example, the mold can be filled by injection, extrusion, pressing, etc.

[0104] The material of the mold may be metal, ceramic, resin, etc., depending on the purpose, and it is preferable to use a material that has a higher heat resistance than the polymerization temperature to be carried out. Examples of the material of the mold include SUS, high-speed tool steel, aluminum alloy, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polystyrene (PS), etc.

[0105] In addition, the obtained bulk body can be subjected to post-processing such as heat treatment, polishing, cutting, attachment of a holder, printing, etc., as necessary. Furthermore, a holding pin for fixing the dental cutting blank to a cutting machine can be joined as necessary. The shape of the holding pin is not particularly limited as long as it can fix the dental cutting blank to the cutting machine, and may not be provided depending on the shape of the dental cutting blank and the requirements of the processing machine. Examples of materials for the holding pin include stainless steel, brass, aluminum, etc. The method of fixing the holding pin to the part to be cut (dental cutting blank body) is not limited to adhesion, and may be a method such as fitting or screwing. There is also no particular limitation on the adhesion method, and various commercially available adhesives such as isocyanate-based, epoxy-based, urethane-based, silicone-based, and acrylic-based adhesives can be used. EXAMPLES

[0106] Next, the multilayer mill blank of the present invention will be specifically described by examples. In each of the examples and comparative examples described below, various structural color raw material compositions and non-structural color raw material compositions are prepared, and the obtained compositions and their cured bodies are evaluated. In addition, these compositions are laminated in a predetermined combination and then cured to obtain a hybrid resin laminate that will be the cutting part of the dental cutting blank, and the evaluation is performed.

[0107] 1. Raw materials for structural color raw material composition and non-structural color raw material composition The raw materials of the structural color raw material compositions and non-structural color raw material compositions used in the examples and comparative examples, as well as their physical properties, will be described below.

[0108] 1-1. Polymerizable monomer components As the polymerizable monomer component in the structural color raw material composition and the non-structural color raw material composition, a polymerizable monomer mixture M1 having the composition shown in Table 1 was used. The abbreviations in the polymerizable monomer column in Table 1 represent the compounds shown below, and the numbers in parentheses after the abbreviations represent the parts by mass used. UDMA: 1,6-bis(methacryloyloxycarbonylamino)trimethylhexane 3G: Triethylene glycol dimethacrylate The viscosity of M1 and the refractive index of M1 (before curing) and its cured body were measured as follows. The results are shown in Table 1. That is, the viscosity was measured in a thermostatic chamber at 25°C using an E-type viscometer (Tokyo Seiki: VISCONIC ELD). The refractive index of M1 (before curing) and its cured body was measured in a thermostatic chamber at 25°C using an Abbe refractometer (Atago Co., Ltd.). At this time, the cured body sample was prepared by adding 0.2 mass% of camphorquinone (CQ), 0.3 mass% of ethyl pN,N-dimethylaminobenzoate (DMBE), and 0.15 mass% of hydroquinone monomethyl ether (HQME) (as photopolymerization initiators) per 100 mass parts of polymerizable monomer, mixing them uniformly, placing them in a mold with a through hole of 7 mmφ×0.5 mm, pressing polyester films on both sides, and then irradiating the mixture with a light intensity of 500 mW / cm. 2 The specimen was then cured by irradiating it with light for 30 seconds using a halogen-type dental light irradiator (Demetron LC, manufactured by Cybron) and then removed from the mold. When the cured specimen was set in the Abbe refractometer, bromonaphthalene, a solvent that does not dissolve the specimen and has a higher refractive index than the specimen, was dropped onto the specimen in order to bring the cured specimen into close contact with the measurement surface.

[0109] [Table 1]

[0110] 1-2. Group of spherical particles with the same particle size: G-PID As the G-PID, G-PID1 and G-PID2 shown in Table 2 were used. Note that G-PID1 and G-PID2 were prepared in the same manner as the method (sol-gel method) disclosed in Patent Document 5, and both were surface-treated with γ-methacryloyloxypropyltrimethoxysilane. In addition, for G-PID1 and G-PID2, the average primary particle size, the ±5% particle ratio [the ratio (%) of the number of particles present in the range of 5% around the average primary particle size in the number-based particle size distribution to the total number of particles], the average uniformity, and the refractive index were measured as follows, in the same manner as the method described in the examples of Patent Document 5. The results are also shown in Table 2. As shown in Table 2, it can be said that both G-PID1 and G-PID2 are spherical particles of the same particle size that satisfy the above condition (a).

[0111] (1) Average primary particle diameter Photographs of the powder were taken at magnifications of 5,000 to 100,000 times using a scanning electron microscope (Philips, "XL-30S"), and the images were processed using image analysis software ("IP-1000PC", product name; Asahi Kasei Engineering Corporation). The number of particles observed within a unit field of view of the photograph (30 or more) and the primary particle diameter (maximum diameter) were measured, and the number average primary particle diameter was calculated based on the measured values ​​(the sum of the measurements divided by the number of particles).

[0112] (2) Particle ratio within ±5% Of all particles (30 or more) in the unit field of view of the photograph, the number of particles having a primary particle diameter (maximum diameter) outside the particle diameter range of 5% around the average primary particle diameter obtained above was counted, and this value was subtracted from the total number of particles to obtain the number of particles within the particle diameter range of 5% around the average primary particle diameter in the unit field of view of the photograph, and calculated according to the following formula.

[0113] Percentage of particles within ±5% (%) = [(Number of particles within a particle size range of 5% around the average primary particle size in a unit field of view of a scanning electron microscope photograph) / (Total number of particles in a unit field of view of a scanning electron microscope photograph)] × 100

[0114] (3) Average symmetry A photograph of the powder was taken with a scanning electron microscope, and the number (n: 30 or more) of spherical particles of the same diameter (G-PID) observed within a unit field of view of the photograph was determined, and the ratio (Bi / Li) of the maximum diameter of the particle (long diameter (Li)) to the diameter in the direction perpendicular to the long diameter (Bi) was calculated. The sum of these ratios was divided by the number of particles to obtain the average uniformity.

[0115] (4) Refractive index The measurement was performed by the immersion method using an Abbe refractometer (manufactured by Atago Co., Ltd.). That is, in a thermostatic room at 25°C, a group of spherical particles of the same particle size (G-PID) was dispersed in 50 ml of anhydrous toluene in a 100 ml sample bottle. While stirring this dispersion with a stirrer, 1-bromotoluene was added dropwise little by little, and the refractive index of the dispersion at the point when the dispersion became most transparent was measured, and the obtained value was taken as the refractive index of the group of spherical particles of the same particle size (G-PID).

[0116] [Table 2]

[0117] 1-3. Organic-inorganic composite filler (CF) The organic-inorganic composite filler (CF) was also prepared as follows, using G-PID2 shown in Table 2, in the same manner as in the examples of Patent Document 5. That is, first, a dispersion in which 100 g of G-PID2 was dispersed in 200 g of water was obtained using a circulation type grinder SC Mill (manufactured by Nippon Coke Engineering Co., Ltd.). Next, a mixed solution (pH 4) of 4 g of γ-methacryloyloxypropyltrimethoxysilane, 0.003 g of acetic acid, and 80 g of water, which had been separately prepared, was added to the dispersion and mixed until uniform. After that, the dispersion was lightly mixed and supplied onto a disk rotating at high speed to be granulated by a spray drying method, and then vacuum dried at 60° C. to obtain an aggregate having a roughly spherical shape. Then, 50 g of the above aggregates were immersed in a polymerizable monomer solution containing 10 g of polymerizable monomer component M1, 0.025 g of azobisisobutyronitrile (AIBN) as a thermal polymerization initiator, and 5.0 g of methanol as an organic solvent. After thorough stirring, the organic solvent was removed, and the mixture was heated for 1 hour under conditions of a reduced pressure of 10 hectopascals and 100°C to polymerize and harden the above polymerizable monomer component, thereby obtaining an organic-inorganic composite filler (CF) with a roughly spherical shape and an average particle size of 12 μm.

[0118] 1-4. Ultrafine particles (G-SFP) As the G-SFP, Rheolosil QS-102 (average primary particle diameter 12 nm, manufactured by Tokuyama Corporation) was used.

[0119] 1-5. Polymerization initiator A thermal polymerization initiator made of benzoyl peroxide (BPO) was used.

[0120] 1-6.Pigments · Red pigment (Pigment Red 166) Yellow pigment (Pigment Yellow 95) ·Blue pigment (Pigment Blue 60).

[0121] 2. Preparation of structural color raw material composition and non-structural color raw material composition and evaluation of the hardened bodies 2-1. Preparation of structural color raw material compositions (P1 to P6) The structural color raw material composition: P1 was prepared as shown below. That is, after mixing 100 parts by mass of M1 and 1.0 parts by mass of BPO, G-PID1 and G-SFP were added so that the mass ratio of the two was G-PID1:G-SFP=95:5, and the inorganic filling rate, defined as the ratio of the mass of the total inorganic particles to the mass of the total structural color raw material composition, was 72% by mass, and the mixture was mixed until uniform using a planetary mixer to form a paste, thereby preparing the structural color raw material composition: P1.

[0122] In addition, structural color raw material compositions P2 to P6 were prepared in the same manner as above, except that the inorganic filling rate was set to the inorganic filling rate shown in Table 3.

[0123] The refractive index of the hardened body of M1 is: n (MX) is 1.509, and the refractive index of G-PID1 is n(G-PID1) = 1.515, respectively. (MX) Since the value is larger than the above, the condition (c) is satisfied. Therefore, it can be said that the hybrid resins made of the cured bodies of these structural color raw material compositions: P1 to P6 all satisfy the above conditions (a) to (c) {P1 to P6 contain one type of G-PID, and also satisfy the above condition (b).}

[0124] [Table 3]

[0125] 2-2. Preparation of non-structural color raw material compositions (L1 to L6) After mixing 100 parts by mass of M1 and 1.0 part by mass of BPO, a mixture of 50% by mass of G-PID2 and 50% by mass of CF (organic-inorganic composite filler) was added so that the inorganic filling rate was 76%. In addition, various pigments were added in the amounts shown in Table 4. The non-structural color raw material compositions: L1 to L6 were prepared in the same manner as in the preparation of P1.

[0126] [Table 4]

[0127] 2-3. Evaluation of hardened bodies of each raw material composition 2-3-1. Confirmation that the hardened bodies of the structural color raw material compositions (P1-P6) are structural color hybrid resins According to the method described in Patent Document 5, the cured products of each structural color raw material composition (P1 to P6) were visually evaluated for coloring light, measured for peak wavelength of coloring light, and evaluated for radial distribution function of inorganic spherical particles by the following methods (1) to (3). The results are shown in Table 5.

[0128] (1) Visual evaluation method for colored light The structural color raw material compositions (P1 to P6) were vacuum degassed, filled into a 10 mm x 12 mm x 14 mm mold, and the top surface was smoothed. After that, using a heating and pressure polymerization apparatus, heating and pressure polymerization was performed under nitrogen pressure at a pressure of 0.4 MPa, 100°C, and 12 hours. Solid samples of 1 mm x 12 mm x 14 mm were cut out from the removed hardened body and polished to a glossy finish to prepare solid samples for colored light measurement. Each solid sample for colored light measurement was placed perpendicular to the adhesive surface of a 10 mm square black tape (carbon tape), and the color tone of the colored light was evaluated visually.

[0129] (2) Measurement method for peak wavelength of colored light For the solid sample for colored light measurement with black tape attached, prepared in the same manner as in (1), the spectral reflectance was measured against a black background using a spectrophotometer (Tokyo Denshoku Corporation, "TC-1800MKII", halogen lamp: 12V100W, measurement wavelength range 380-780nm), and the maximum point of reflectance was taken as the wavelength of the colored light.

[0130] (3) Radial distribution function evaluation method for inorganic spherical particles A hardened body was prepared in the same manner as in (1) except that the structural color raw material compositions (P1 to P6) were filled into a mold of 5 mmφ×10 mm, and the dispersion state of the spherical particles in the hardened body was observed with a scanning electron microscope (Philips, "XL-30S") to obtain the radial distribution function and perform evaluation. Specifically, the cross-section of the hardened body was milled using an ion milling device (Hitachi, Ltd., "IM4000") at 2 kV for 20 minutes to obtain an observation plane. A microscopic image of an area containing 1000 spherical particles in the plane of the observation plane was obtained using a scanning electron microscope, and the obtained scanning electron microscope image was analyzed using image analysis software ("Simple Digitizer ver3.2" free software) to obtain the coordinates of the spherical particles in the above area. From the obtained coordinate data, the coordinates of any one spherical particle are selected, and a circle is drawn with a radius of distance r that contains at least 200 spherical particles centered on the selected spherical particle, and the number of spherical particles contained within the circle is calculated to obtain the average particle density <ρ> (unit: particles / cm 2 ) was calculated. dr is a value of about r0 / 100 to r0 / 10 (r0 indicates the average particle diameter of the spherical particles). The number of particles dn contained in the region between the circle at the distance r from the central spherical particle and the circle at the distance r + dr, and the area da of the above region (where da = 2πr dr) were calculated. Using the values ​​of <ρ>, dn, and da calculated in this way, Formula: g(r) = {1 / <ρ>} × {dn / da} The radial distribution function g(r) defined as follows was calculated. A graph was then created showing the relationship between the radial distribution function and r / r0 (r indicates an arbitrary distance from the center of the circle, and r0 indicates the average particle diameter of the spherical particles), and the radial distribution function was evaluated for condition 1 and condition 2, with those that satisfied the conditions being given an "S" and those that did not being given an "N."

[0131] As shown in Table 5, the cured products of the structural color raw material compositions (P1 to P6) inorganic spherical It was confirmed that the dispersion state of the particles satisfied the above condition (d) and exhibited a specific structural color.

[0132] [Table 5]

[0133] 2-3-2. The brightness of each raw material composition hardened body is L * , hue a * and saturation b * and contrast ratio (CR) evaluation The cured products of the structural color raw material compositions (P1 to P6) and the non-structural color raw material compositions (L1 to L6) were subjected to the following methods (4) and (5). * , a * and b * The results are shown in Table 6.

[0134] (4) Lightness to L * , hue a * and saturation b * Measurement Each raw material composition was vacuum degassed, filled and packed into a 10 mm x 12 mm x 14 mm mold, and the upper surface was smoothed. After that, using a heating and pressure polymerization apparatus, heating and pressure polymerization was performed under nitrogen pressure at a pressure of 0.4 MPa, 100°C, and 12 hours. A solid sample of 14 mm x 12 mm x 1 mm was cut out from the removed cured body to prepare a solid sample for color difference measurement. For this solid sample, the spectral reflectance of the background color black (light shielding state) and the background color white (light shielding state with a standard white plate overlapping the cured body) in a measurement area of ​​5 mmφ was measured by the reflected light 0°d method (JIS Z8722) using a spectrophotometer (Tokyo Denshoku Co., Ltd., "TC-1800MKII", halogen lamp: 12V100W, measurement wavelength range 380 to 780nm) to measure the L * Value, a * value and b * The value was calculated.

[0135] (5) Contrast ratio (CR) measurement The above sample was measured using the above color difference meter, and the Y value for the black background was measured. B and Y value for white background W Based on the contrast ratio CR=Y B / Y W was calculated.

[0136] [Table 6]

[0137] 3. Examples and Comparative Examples The above P1-6 and L1-6 pastes were used in the combinations shown in Table 7 to produce a machined part consisting of a two-layer hybrid resin laminate in which a hybrid resin layer made of a hardened product of the raw material composition for the first layer and a hybrid resin layer made of a hardened product of the raw material composition for the second layer were bonded together at the same layer thickness as described below.

[0138] That is, the raw material composition for the first layer is filled into the mold up to half the height (5 mm) of the mold and left to stand until the surface becomes flat, and then the raw material composition for the second layer is filled into the mold while being careful not to disturb the interface. * , a * and b * Hardening was carried out in the same manner as in the preparation of the measurement sample, and the above-mentioned machined portion was prepared.

[0139] The lamination interface of the obtained machined part was evaluated, and a retaining pin was attached to the machined part to make a resin blank for dental machining. The state of the lamination interface of the dental restoration (crown) made using this was evaluated, as well as the approximation to a natural tooth. The specific evaluation method is shown below. The evaluation results were also evaluated in terms of the color difference between the first and second layers: ΔE * The contrast ratio difference: ΔCR (=CR2-CR1) is also shown in Table 7.

[0140] (1) Evaluation of laminated interfaces The laminate was visually observed to confirm whether the laminate interface was visible. The evaluation criteria are as follows: 5: The interface between the upper and lower layers is completely invisible. 4: The interface between the upper and lower layers is not visible. 3: The interface between the upper and lower layers is barely visible. 2: The interface between the upper and lower layers is barely visible. 1: The interface between the upper and lower layers is clearly visible.

[0141] (2) Evaluation of laminate interfaces in simulated dental restorations The crown of the upper right first tooth was machined using a milling machine (Roland, "DWX-50") to create a dental restoration (restoration), which was then bonded to a resin abutment (equivalent to A3 color) using Esthecem II (Tokuyama Dental, adhesive resin cement), polished, and a mock restoration was performed. The condition of the laminate interface after restoration was visually confirmed. The evaluation criteria are as follows: 5: The interface between the upper and lower layers is completely invisible, and the color is natural. 4: The interface between the upper and lower layers is barely visible, and the color is natural. 3: The interface between the upper and lower layers is difficult to see. 2: The interface between the upper and lower layers is faintly visible. 1: The interface between the upper and lower layers is clearly visible and has an unnatural color tone.

[0142] (3) Evaluation of the similarity of dental restorations to natural teeth (2) The simulated restorations were visually inspected to see whether the color tone from the cervical area to the incisal area was close to that of natural teeth. The evaluation criteria are as follows: 5: Natural color, like natural teeth. 4: The color tone is close to that of natural teeth. 3: The color is somewhat similar to that of natural teeth. 2: The color is not very similar to natural teeth and feels a little strange. 1: The color is unnatural and not at all similar to natural teeth.

[0143] [Table 7]

[0144] As shown in Table 7, the "evaluation of natural tooth similarity" of Comparative Example 1, which is a single-layer structural color resin blank (of P1 hardened body), and Comparative Example 2, which is a single-layer non-structural color resin blank (of L1 hardened body), is "1". That is, in Comparative Example 1, although the color tone of the cervical part being dark and the incisal part being light and transparent was reproduced, the color of the crown was white, so it was rated low in the visual evaluation of similarity to natural teeth. In addition, in Comparative Example 2, since the entire crown is non-structural color, the color tone of the cervical part being dark and the incisal part being light was not reproduced, so it was rated low in the visual evaluation of similarity to natural teeth. In contrast, the "evaluation of natural tooth similarity" of Examples 1 to 11, although to a certain extent, are all rated higher than the evaluations of Comparative Examples 1 and 2. In particular, ΔE * , CR1, CR2 and ΔCR are all within a suitable range (ΔE * For Examples 1, 2, and 8 to 10, in which the experimental results were as follows: CR1=2 to 20, CR1=0.28 to 0.43, CR1=0.55 to 0.63, ΔCR=0.12 to 0.27), the evaluations of "evaluation of the laminate interface," "evaluation of the laminate interface of the dental simulation restoration," and "evaluation of similarity to a natural tooth" were all rated as "4" or higher.

Claims

1. A dental resin blank for machining having a machining part made of a composite material in which inorganic particles are dispersed in a resin matrix, The composite material has a laminated structure in which a first layer and a second layer are bonded together, the first layer is made of a first composite material that exhibits a structural color of a predetermined color tone independent of the angle of incidence of light, the second layer is made of a second composite material having a color tone different from the color tone of the first composite material; The color tone of a composite material having a single color tone is measured by measuring a sample having a thickness of 1.0±0.1 mm against a white background using a spectrophotometer. * Value, a * Value and b * When expressed as a value, The following formula is an index of the difference in color tone between the first composite material and the second composite material: ΔE * = {(L1 * -L2 * ) 2 + (a1 * -a2 * ) 2 + (b1 * -b2 * ) 2} 1/2 (In the above formula, L1 * , a1 * and b1 * is the L in the first composite material * Value, a * Value and b * value, and L2 * , a2 * and b2 * is the L in the second composite material * Value, a * Value and b * value.) Color difference defined as: ΔE * is 2 to 30, the total amount of pigment and colorant in the first composite material is 100 ppm by mass or less relative to the total mass of the first composite material, and the total amount of pigment and colorant in the second composite material is 500 to 7000 ppm by mass relative to the total mass of the second composite material; A laminated resin-based blank for dental cutting, characterized in that

2. 2. The laminated resin-based blank for dental cutting according to claim 1, characterized in that the first composite material satisfies all of the following conditions (a) to (d): (a) The inorganic particles are composed of an aggregate of inorganic spherical particles having a predetermined average primary particle diameter within a range of 100 nm to 1000 nm, and include one or more groups of uniform-diameter spherical particles (G-PID) in which 90% or more of the total number of particles in a number-based particle size distribution of the aggregate are present within a 5% range around the predetermined average primary particle diameter. (b) When the number of the uniform particle groups contained in the inorganic particles is a, and each uniform particle group is expressed as G-PIDm (where m is 1 when a is 1, and is a natural number from 1 to a when a is 2 or more) in ascending order of average primary particle diameter, the average primary particle diameters of each G-PIDm when a is 2 or more differ from each other by 25 nm or more. (c) The refractive index of the resin matrix at 25° C. for light having a wavelength of 589 nm is n(MX), and the refractive index of the inorganic spherical particles constituting each G-PIDm at 25° C. for light having a wavelength of 589 nm is n(G-PIDm), for each n(G-PIDm): n(MX)<n(G-PIDm) The relationship is established. (d) A function expressing the probability that other inorganic spherical particles are present at a point distant r from the center of any inorganic spherical particle in the first composite material, which is determined based on a scanning electron microscope image in which the inner surface of the composite material is used as an observation plane, and is expressed by the following formula (1) based on the average particle density of the inorganic spherical particles in the observation plane: <ρ>, the number of inorganic spherical particles present in the region between a circle at a distance r from any inorganic spherical particle in the observation plane and a circle at a distance r + dr: dn, and the area of ​​the region: da (where da = 2πr dr): g(r)={1 / <ρ>}×{dn / da}...(1) When g(r) is a radial distribution function, the inorganic spherical particles constituting the group of uniform particle diameter spherical particles (G-PID) in the composite material are dispersed in the matrix material so as to have a short-range ordered structure that satisfies the following condition 1 and the following condition 2: [Condition 1]: The distance from the center of any inorganic spherical particle dispersed in the composite material: r is set to the average particle diameter of all inorganic spherical particles dispersed in the composite material: r 0 The dimensionless number (r / r 0 ) on the x-axis, the radial distribution function: g(r) on the y-axis, and the r / r 0 and the g(r) corresponding to r at that time, the nearest interparticle distance is defined as r corresponding to the peak top of the peak that is closest to the origin among the peaks that appear in the radial distribution function graph: r 1 is the average particle size of all inorganic spherical particles dispersed in the composite material: r 0 The value is between 1 and 2 times the value. [Condition 2]: Among the peaks appearing in the radial distribution function graph, the r corresponding to the peak top of the second closest peak from the origin is defined as the next nearest particle distance: r 2 When the distance between the nearest particles is r 1 and the distance between the next nearest neighboring particles: r 2 The minimum value of the radial distribution function g(r) between is 0.56 or more and 1.10 or less.

3. The transparency of the composite material is measured by measuring the color difference of a sample having a thickness of 1.0±0.1 mm using a spectrophotometer. The Y value is measured against a white background. W Y value on a black background: Y B / Ratio: Y B / Y W When the value determined as above is expressed as an index of contrast ratio: CR, The first composite material has a contrast ratio CR1 of 0.28 to 0.46, and the second composite material has a contrast ratio CR2 of 0.50 to 0.

65. A laminated resin-based blank for dental machining according to claim 1 or 2.

Citation Information

Patent Citations

  • dental mill blank

    JP2016535610A

  • Resin material for multi-layer dental cutting

    JP2017105764A

  • Method for producing dental mill blank

    JP2017113224A

  • Resin block for dental CAD / cam

    JP2017213394A

  • Composite material

    JP2020037534A