Zirconia sintered body with high in-line light transmittance
A zirconia sintered body with controlled particle size and composition, sintered under normal pressure, addresses the challenge of achieving high linear light transmittance without HIP devices, providing strong and translucent dental materials.
Patent Information
- Application Number
- JP2022209178
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-06
- Filing Date
- 2022-12-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-03-05
AI Technical Summary
Existing methods for producing zirconia sintered bodies with high linear light transmittance require high-pressure gas production equipment like HIP devices, making it difficult to achieve high transmittance easily.
A zirconia sintered body with specific particle size and composition, including zirconia particles with an average size of 60 nm or less and 0.5% by mass of particles over 100 nm, sintered under normal pressure with a W-B of 5 or more, and optionally containing yttria, fluorescent agents, colorants, and translucency modifiers, to achieve high linear light transmittance without HIP devices.
The solution enables the production of zirconia sintered bodies with excellent strength and translucency, suitable for dental applications, without the need for HIP devices, and maintains high linear light transmittance.
Smart Images

Figure 0007575441000001 
Figure 0007575441000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a zirconia sintered body having high in-line light transmittance. [Background technology]
[0002] In recent years, zirconia sintered bodies containing yttria have been used as dental materials for dental prostheses, etc. In many cases, these dental prostheses are manufactured by press-molding zirconia particles or molding using a slurry or composition containing zirconia particles to form a zirconia molded body having a desired shape such as a disk or a prism, then calcining this to form a calcined body (mill blank), which is cut (milled) into the shape of the intended dental prosthesis, and then sintering it.
[0003] It has been confirmed that the in-line light transmittance can be improved by making the crystal grain size of the zirconia sintered body small and uniform (see, for example, Patent Document 1, etc.). In order to make the crystal grain size of the zirconia sintered body small and uniform, a hot isostatic press (HIP) treatment is required. However, since the HIP apparatus used in the HIP treatment is a special apparatus classified as a high-pressure gas manufacturing device, it is difficult to say that a zirconia sintered body with high in-line light transmittance can be easily obtained. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2008-214168 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a zirconia sintered body that is excellent in both strength and translucency and in straight light transmittance without using a HIP apparatus, a zirconia molded body and a zirconia calcined body that can provide such a zirconia sintered body, and a production method that can simply and easily produce them. [Means for solving the problem]
[0006] As a result of intensive research conducted by the present inventors in order to achieve the above object, it has been discovered that the zirconia particles have an average particle size of 60 nm or less, and the content of particles having a particle size exceeding 100 nm is 0.5 mass % or less, and that the ΔL * It was found that a zirconia sintered body with excellent linear light transmittance can be obtained without using a HIP device by sintering a zirconia molded body having a weight-beam (WB) of 5 or more under normal pressure. It was also found that such a zirconia sintered body is particularly suitable as a dental material for dental prostheses, and is particularly useful not only for dental prostheses used in the cervical region, but also for dental prostheses used in the occlusal surfaces of molars and the incisal ends of anterior teeth. Based on these findings, the present inventors conducted further studies and completed the present invention.
[0007] That is, the present invention relates to the following [1] to
[19] . [1] A zirconia particle containing 2.0 to 9.0 mol% of yttria, having an average primary particle diameter of 60 nm or less, and having 0.5 mass% or less of particles having a particle diameter exceeding 100 nm, and a ΔL * A zirconia molded body having a weight (WB) of 5 or more. [2] The zirconia molded body according to [1], which has a three-point bending strength of 500 MPa or more after sintering at 900 to 1200° C. under normal pressure. [3] The zirconia molded body according to [1] or [2], which has a transmittance of 40% or more for light with a wavelength of 700 nm at a thickness of 0.5 mm after sintering at 900 to 1200° C. under normal pressure. [4] The zirconia molded body according to any one of [1] to [3], which has a ratio of monoclinic to tetragonal and cubic crystals of 5% or less after sintering at 900 to 1200°C under normal pressure and then immersing in hot water at 180°C for 5 hours. [5] ΔL at a thickness of 1.5 mm after sintering at 200 to 800°C * The zirconia molded body according to any one of [1] to [4], wherein (WB) is 5 or more. [6] ΔL at a thickness of 1.5 mm containing 2.0 to 9.0 mol% yttria * (WB) is 5 or more. [7] The zirconia calcined body according to [6], which has a three-point bending strength of 500 MPa or more after sintering at 900 to 1200°C under normal pressure. [8] The zirconia calcined body according to [6] or [7], which has a transmittance of 40% or more for light with a wavelength of 700 nm at a thickness of 0.5 mm after sintering at 900 to 1200° C. under normal pressure. [9] The zirconia calcined body according to any one of [6] to [8], which has a ratio of monoclinic to tetragonal and cubic crystals of 5% or less after sintering at 900 to 1,200°C under normal pressure and then immersing in hot water at 180°C for 5 hours.
[10] A method for producing a calcined zirconia body, using the zirconia molded body according to any one of [1] to [5].
[11] A method for producing a calcined zirconia body according to
[10] , comprising a step of calcining the zirconia molded body according to any one of [1] to [5] at 200 to 800°C.
[12] A zirconia sintered body containing a fluorescent agent and 2.0 to 9.0 mol% yttria, and having an in-line light transmittance of 1% or more at a thickness of 1.0 mm.
[13] The zirconia sintered body according to
[12] , having a three-point bending strength of 500 MPa or more.
[14] The zirconia sintered body according to
[12] or
[13] , having a transmittance of 40% or more for light having a wavelength of 700 nm at a thickness of 0.5 mm.
[15] The zirconia sintered body according to any one of
[12] to
[14] , having a ratio of monoclinic to tetragonal and cubic crystals of 5% or less after immersion in 180°C hot water for 5 hours.
[16] A method for producing a zirconia sintered body, using the zirconia molded body according to any one of [1] to [5].
[17] A method for producing the zirconia sintered body according to
[16] , comprising a step of sintering the zirconia molded body at 900 to 1200°C under normal pressure.
[18] A method for producing a zirconia sintered body, using the zirconia calcined body according to any one of [6] to [9].
[19] A method for producing a zirconia sintered body according to
[18] , comprising a step of sintering the zirconia calcined body at 900 to 1200°C under normal pressure. Effect of the Invention
[0008] According to the present invention, there are provided a zirconia sintered body having excellent strength, translucency and in-line light transmittance without using a HIP apparatus, a zirconia molded body and a zirconia calcined body which can provide such a zirconia sintered body, and a production method which can simply and easily produce them. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention is directed to a method for producing a zirconia composite material comprising: a) a zirconia composite material having a thickness of 1.5 mm, b) a zirconia composite material including 2.0 to 9.0 mol% of yttria (Y2O3), c) an average primary particle size of 60 nm or less, and e) a particle size exceeding 100 nm of 0.5 mass% or less; * The present invention also includes a zirconia molded body having a ΔL (WB) of 5 or more. By using the zirconia molded body, it is possible to obtain a zirconia sintered body having excellent strength and translucency and excellent linear light transmittance. The present invention also includes a zirconia molded body having a ΔL (WB) of 5 or more at a thickness of 1.5 mm, which contains 2.0 to 9.0 mol % of yttria. * The zirconia calcined body includes a zirconia calcined body having a weight-weight ratio (WB) of 5 or more. The zirconia sintered body can also be obtained by using the zirconia calcined body. Hereinafter, as an embodiment of the present invention, the zirconia sintered body will be described first. The zirconia sintered body of the present invention contains a fluorescent agent and 2.0 to 9.0 mol% of yttria, and has a linear light transmittance of 1% or more at a thickness of 1.0 mm. Note that the following description does not limit the present invention.
[0010] [Zirconia sintered body] The zirconia sintered body of the present invention contains a fluorescent agent. The zirconia sintered body has fluorescence by containing a fluorescent agent. There is no particular limitation on the type of fluorescent agent, and one or more of those that can emit fluorescence with light of any wavelength can be used. Such fluorescent agents include those containing metal elements. Examples of the metal elements include Ga, Bi, Ce, Nd, Sm, Eu, Gd, Tb, Dy, and Tm. The fluorescent agent may contain one of these metal elements alone, or may contain two or more of them. Among these metal elements, Ga, Bi, Eu, Gd, and Tm are preferred, and Bi and Eu are more preferred, because the effects of the present invention are more significantly exhibited. Examples of fluorescent agents used in producing the zirconia sintered body of the present invention include oxides, hydroxides, acetates, and nitrates of the above metal elements. The fluorescent agents are Y2SiO5:Ce, Y2SiO5:Tb, (Y,Gd,Eu)BO3, Y2O3:Eu, YAG:Ce, ZnGa2O4:Zn, BaMgAl 10 O 17 :Eu, etc.
[0011] The content of the fluorescent agent in the zirconia sintered body is not particularly limited, and can be appropriately adjusted depending on the type of fluorescent agent and the use of the zirconia sintered body, but from the viewpoint of being preferably usable as a dental prosthesis, the content of the fluorescent agent is preferably 0.001 mass% or more, more preferably 0.005 mass% or more, even more preferably 0.01 mass% or more, and preferably 1 mass% or less, more preferably 0.5 mass% or less, and even more preferably 0.1 mass% or less, in terms of the oxide of the metal element contained in the fluorescent agent relative to the mass of zirconia contained in the zirconia sintered body. When the content is above the lower limit, the fluorescence is not inferior to that of human natural teeth, and when the content is below the upper limit, the decrease in translucency and strength can be suppressed.
[0012] The zirconia sintered body of the present invention may contain a coloring agent. The zirconia sintered body becomes a colored zirconia sintered body by containing a coloring agent. There is no particular limitation on the type of coloring agent, and known pigments commonly used for coloring ceramics and known dental liquid coloring agents can be used. Examples of coloring agents include those containing metal elements, and specifically, oxides, composite oxides, salts, etc. containing metal elements such as iron, vanadium, praseodymium, erbium, chromium, nickel, and manganese. In addition, commercially available coloring agents can be used, such as Prettau Colour Liquid manufactured by Zirkonzahn. The zirconia sintered body may contain one type of coloring agent, or may contain two or more types of coloring agents.
[0013] The content of the colorant in the zirconia sintered body is not particularly limited, and can be appropriately adjusted depending on the type of colorant and the application of the zirconia sintered body. From the viewpoint of favorable use as a dental prosthesis, the content of the colorant, calculated as the oxide of the metal element contained in the colorant, relative to the mass of zirconia contained in the zirconia sintered body, is preferably 0.001 mass% or more, more preferably 0.005 mass% or more, and even more preferably 0.01 mass% or more, and preferably 5 mass% or less, more preferably 1 mass% or less, and even more preferably 0.5 mass% or less, and may be 0.1 mass% or less, or even 0.05 mass% or less.
[0014] According to the present invention, a zirconia sintered body having excellent linear light transmittance can be obtained. In order to adjust the translucency of the zirconia sintered body, the zirconia sintered body of the present invention may contain a translucency regulator. Specific examples of the translucency regulator include aluminum oxide, titanium oxide, silicon dioxide, zircon, lithium silicate, and lithium disilicate. The zirconia sintered body may contain one type of translucency regulator, or may contain two or more types of translucency regulators.
[0015] The content of the translucency adjuster in the zirconia sintered body is not particularly limited and can be appropriately adjusted depending on the type of translucency adjuster and the application of the zirconia sintered body. From the viewpoint of favorable use as a dental prosthesis, however, it is preferably 0.1 mass % or less with respect to the mass of zirconia contained in the zirconia sintered body.
[0016] The zirconia sintered body of the present invention contains 2.0 to 9.0 mol% of yttria. When the content of yttria in the zirconia sintered body is less than 2.0 mol%, sufficient translucency cannot be obtained. When the content of yttria in the zirconia sintered body is more than 9.0 mol%, the strength decreases. Since a zirconia sintered body having excellent translucency and strength can be obtained, the content of yttria in the zirconia sintered body is preferably 3.0 mol% or more, more preferably 4.0 mol% or more, and preferably 8.0 mol% or less, more preferably 7.0 mol% or less. The content of yttria in the zirconia sintered body means the ratio (mol%) of the number of moles of yttria to the total number of moles of zirconia and yttria.
[0017] The crystal grain size in the zirconia sintered body of the present invention is preferably 180 nm or less. If the crystal grain size exceeds 180 nm, sufficient translucency may not be obtained. Since a zirconia sintered body with excellent translucency can be obtained, the crystal grain size is preferably 140 nm or less, more preferably 120 nm or less, further preferably 110 nm or less, and may be 100 nm or less. There is no particular limit to the lower limit of the crystal grain size, but the crystal grain size can be, for example, 50 nm or more, or even 70 nm or more. The crystal grain size in the zirconia sintered body can be obtained by taking a field emission scanning electron microscope (FE-SEM) photograph of the cross section of the zirconia sintered body, selecting any 10 particles in the photographed image, and calculating the average value of the circle equivalent diameters (diameters of perfect circles with the same area) of each of the particles.
[0018] The zirconia sintered body of the present invention has excellent strength. The three-point bending strength of the zirconia sintered body of the present invention is 500 MPa or more, preferably 600 MPa or more, more preferably 650 MPa or more, even more preferably 700 MPa or more, and particularly preferably 800 MPa or more. When the zirconia sintered body of the present invention has such a three-point bending strength, it is possible to suppress fracture in the oral cavity when used as a dental prosthesis, for example. There is no particular limit to the upper limit of the three-point bending strength, but the three-point bending strength can be, for example, 1500 MPa or less, or even 1000 MPa or less. The three-point bending strength of the zirconia sintered body can be measured in accordance with ISO 6872:2015.
[0019] The zirconia sintered body of the present invention has excellent translucency. The zirconia sintered body of the present invention has a transmittance of 40% or more at a wavelength of 700 nm at a thickness of 0.5 mm, more preferably 45% or more, and may be 46% or more, 48% or more, 50% or more, or even 52% or more. When the transmittance is within the above range, for example, when used as a dental prosthesis, the translucency required for the incisal part is easily satisfied. There is no particular limit to the upper limit of the transmittance, but the transmittance can be, for example, 60% or less, or even 57% or less. The transmittance of light at a wavelength of 700 nm at a thickness of 0.5 mm of the zirconia sintered body can be measured using a spectrophotometer, for example, a spectrophotometer (manufactured by Hitachi High-Technologies Corporation, "Hitachi Spectrophotometer U-3900H type") is used to transmit and scatter light generated from a light source through a sample, and the transmittance can be measured using an integrating sphere. In this measurement, the transmittance may be measured in the wavelength region of 300 to 750 nm, and then the transmittance for light with a wavelength of 700 nm may be obtained. As a sample used for the measurement, a disk-shaped zirconia sintered body having a diameter of 15 mm and a thickness of 0.5 mm and having both sides mirror-polished can be used.
[0020] The zirconia sintered body of the present invention has excellent linear light transmittance. It is important that the zirconia sintered body of the present invention has a linear light transmittance of 1% or more at a thickness of 1.0 mm, preferably 3% or more, more preferably 5% or more, even more preferably 7% or more, and may even be 10% or more. When the linear light transmittance is within the above range, for example, when used as a dental prosthesis, the translucency required for the incisal part is easily satisfied. There is no particular limit to the upper limit of the linear light transmittance, but the linear light transmittance can be, for example, 60% or less, or even 50% or less. The linear light transmittance of the zirconia sintered body at a thickness of 1.0 mm can be measured using a turbidity meter, for example, a turbidity meter (manufactured by Nippon Denshoku Industries Co., Ltd., "Haze Meter NDH 4000") is used to transmit and scatter light generated from a light source through a sample, and the measurement can be performed using an integrating sphere. In this measurement, the in-line light transmittance is preferably measured in accordance with ISO 13468-1: 1996 and JIS K 7361-1: 1997, and the haze is preferably measured in accordance with ISO 14782-1: 1999 and JIS K 7136: 2000. As a sample used for the measurement, a disk-shaped zirconia sintered body having a diameter of 15 mm and a thickness of 1.0 mm and mirror-polished on both sides can be used.
[0021] The main crystal phase of the zirconia sintered body of the present invention may be either tetragonal or cubic, but it is preferable that the proportion of the cubic system is high. In the zirconia sintered body of the present invention, it is preferable that 30% or more of the cubic system is cubic, and more preferably 50% or more of the cubic system. The proportion of the cubic system in the zirconia sintered body can be determined by analyzing the crystal phase. Specifically, X-ray diffraction (XRD) measurement is performed on a mirror-finished portion of the surface of the zirconia sintered body, and the proportion can be determined by the following formula. f c = 100 × I c / (I m +I t +I c ) where f crepresents the percentage of cubic crystals in the zirconia sintered body, and I m represents the height of the peak near 2θ = 28° (peak based on the monoclinic (11-1) plane), and I t represents the height of the peak near 2θ = 30° (the peak based on the (111) plane of the tetragonal crystal system), and I c represents the height of the peak near 2θ=30° (peak based on the (111) plane of the cubic crystal system). If the peak near 2θ=30° appears as a peak based on the mixed phase of the (111) plane of the tetragonal crystal system and the (111) plane of the cubic crystal system, and it is difficult to separate the peak based on the (111) plane of the tetragonal crystal system from the peak based on the (111) plane of the cubic crystal system, the ratio of the tetragonal crystal system to the cubic crystal system is calculated by using the Rietveld method, and this is used as the height of the peak based on the mixed phase (I t+c ) to get I t and I c can be sought.
[0022] In the zirconia sintered body of the present invention, the ratio of monoclinic to tetragonal and cubic crystals after immersion in 180°C hot water for 5 hours is preferably 5% or less, more preferably 3% or less, and even more preferably 1% or less. By having the ratio within the above range, when used, for example, as a dental prosthesis, it is possible to suppress the change in volume over time and prevent breakage. The ratio can be calculated by the following formula after mirror-finishing the surface of the zirconia sintered body and immersing it in 180°C hot water for 5 hours, and then performing X-ray diffraction (XRD) measurement on the above part. f m = 100 × I m / (I t+c ) where f m represents the ratio (%) of monoclinic to tetragonal and cubic crystals in the zirconia sintered body after immersion in 180°C hot water for 5 hours, and I m represents the height of the peak near 2θ = 28° (peak based on the monoclinic (11-1) plane), and I t+crepresents the height of the peak near 2θ=30° (a peak due to the mixed phase of the tetragonal (111) plane and the cubic (111) plane). Note that the peak near 2θ=30° appears separately as a peak due to the tetragonal (111) plane and a peak due to the cubic (111) plane, and the above I t+c If it is difficult to determine the height of the peak based on the (111) plane of the tetragonal crystal system (I t ) and the height of the peak based on the (111) plane of the cubic crystal system (I c ) and the sum of the above I t+c It can be said that:
[0023] The method for producing the zirconia sintered body of the present invention is characterized by using the zirconia molded body of the present invention described later, and the production method preferably includes a step of sintering the zirconia molded body at normal pressure at 900 to 1200° C. Alternatively, the zirconia calcined body of the present invention described later may be used, and the production method preferably includes a step of sintering the zirconia calcined body at normal pressure at 900 to 1200° C. By such a production method, the zirconia sintered body of the present invention, which is excellent in both strength and translucency and in straight light transmittance, can be easily produced.
[0024] [Zirconia Molded Body] The zirconia molded body of the present invention contains 2.0 to 9.0 mol % of yttria, has an average primary particle size of 60 nm or less, and contains 0.5 mass % or less of particles having a particle size exceeding 100 nm. * (WB) is not less than 5. By using the zirconia molded body, it is possible to obtain a zirconia sintered body having excellent strength, translucency, and in-line light transmittance.
[0025] The zirconia molded body of the present invention has high translucency, and it is possible to produce a zirconia sintered body with high linear light transmittance and a zirconia calcined body from which a zirconia sintered body with high linear light transmittance can be produced from such a zirconia molded body. *It is important that (WB) is 5 or more, preferably 8 or more, and may further be 10 or more. * (WB) is the brightness on a white background (L * ) and lightness on a black background (L * ) on a white background. * value (JIS Z 8781-4:2013 Colorimetry-Part 4:CIE 1976 L*a*b* color space) and L on a black background * The white background refers to the white part of the hiding ratio test paper described in JIS K 5600-4-1:1999 Part 4, Section 1, and the black background refers to the black part of the hiding ratio test paper. * By setting (WB) within the above range, a zirconia sintered body with high linear light transmittance can be obtained when sintered under normal pressure. * There is no particular upper limit for (WB), but for example, it may be set to 30 or less, and from the viewpoint of aesthetics, it may be set to 25 or less. * (WB) can be measured using a spectrophotometer, for example, a spectrophotometer (Konica Minolta Japan, Inc., "CM-3610A", geometric condition c (di: 8°, de: 8°), diffuse illumination: 8° receiving light, measurement mode SCI, measurement diameter / illumination diameter = φ8mm / φ11mm) is used, and it can be calculated using the color management software "SpectraMagic NX ver.2.5" manufactured by Konica Minolta, Inc. In this measurement, the light source can be obtained by using F11. As a sample used for the measurement, a disk-shaped zirconia molded body with a diameter of 20 mm and a thickness of 1.5 mm can be used.
[0026] When the zirconia sintered body is to contain a fluorescent agent, it is preferable that the zirconia molded body contains the fluorescent agent. The content of the fluorescent agent in the zirconia molded body of the present invention can be appropriately adjusted according to the content of the fluorescent agent in the obtained zirconia sintered body. The specific content of the fluorescent agent contained in the zirconia molded body is preferably 0.001 mass% or more, more preferably 0.005 mass% or more, and even more preferably 0.01 mass% or more, and is preferably 1 mass% or less, more preferably 0.5 mass% or less, and even more preferably 0.1 mass% or less, in terms of the oxide of the metal element contained in the fluorescent agent, relative to the mass of zirconia contained in the zirconia molded body.
[0027] When the zirconia sintered body is to contain a colorant, it is preferable that the zirconia molded body contains the colorant. The content of the colorant in the zirconia molded body of the present invention can be appropriately adjusted according to the content of the colorant in the obtained zirconia sintered body. The specific content of the colorant contained in the zirconia molded body is preferably 0.001 mass% or more, more preferably 0.005 mass% or more, and even more preferably 0.01 mass% or more, and is preferably 5 mass% or less, more preferably 1 mass% or less, and even more preferably 0.5 mass% or less, and may be 0.1 mass% or less, or even 0.05 mass% or less, in terms of the oxide of the metal element contained in the colorant, relative to the mass of zirconia contained in the zirconia molded body.
[0028] When the zirconia sintered body contains a translucency regulator, it is preferable that the zirconia shaped body contains the translucency regulator. The content of the translucency regulator in the zirconia sintered body of the present invention can be appropriately adjusted according to the content of the translucency regulator in the obtained zirconia sintered body. The specific content of the translucency regulator contained in the zirconia shaped body is preferably 0.1 mass% or less relative to the mass of zirconia contained in the zirconia shaped body.
[0029] The content of yttria contained in the zirconia molded body of the present invention may be within the range of 2.0 to 9.0 mol%, and may be the same as the content of yttria in the obtained zirconia sintered body, and the specific content of yttria in the zirconia molded body is 2.0 mol% or more, preferably 3.0 mol% or more, more preferably 4.0 mol% or more, and 9.0 mol% or less, preferably 8.0 mol% or less, and more preferably 7.0 mol% or less. The content of yttria in the zirconia molded body means the ratio (mol%) of the number of moles of yttria to the total number of moles of zirconia and yttria.
[0030] The density of the zirconia molded body of the present invention is not particularly limited, and varies depending on the manufacturing method of the zirconia molded body, etc., but since a dense zirconia sintered body can be obtained, the density is preferably 3.0 g / cm 3 It is preferable that the content is 3.2 g / cm or more. 3 More preferably, it is 3.4 g / cm or more. 3 There is no particular upper limit to the density, but it is preferably 6.0 g / cm3 or more. 3 Below that, 5.8g / cm 3 It can be as follows:
[0031] The shape of the zirconia molded body of the present invention is not particularly limited, and can be a desired shape depending on the application, but considering the handleability when obtaining a zirconia calcined body to be used as a mill blank for manufacturing dental materials such as dental prostheses, a disk shape, a prism shape (rectangular parallelepiped shape, etc.), etc. are preferable. As described later, in the manufacture of a zirconia molded body, if a stereolithography method or the like is adopted, a shape corresponding to the desired shape of the finally obtained zirconia sintered body can be imparted to the zirconia molded body, and the present invention also includes a zirconia molded body having such a desired shape. In addition, the zirconia molded body may have a single-layer structure, but may also have a multilayer structure. By making it a multilayer structure, the finally obtained zirconia sintered body can be made a multilayer structure, and its physical properties such as translucency can be locally changed.
[0032] The zirconia molded body of the present invention preferably has a biaxial bending strength in the range of 2 to 10 MPa, more preferably in the range of 5 to 8 MPa, from the viewpoint of handleability, etc. The biaxial bending strength of the zirconia molded body can be measured in accordance with JIS T 6526:2018.
[0033] The zirconia molded body of the present invention preferably has a crystal grain size of 180 nm or less after sintering at 900 to 1200 ° C. for 2 hours under normal pressure (after being made into a zirconia sintered body). This makes it possible to easily manufacture the zirconia sintered body of the present invention having excellent translucency. Since a zirconia sintered body having excellent translucency can be obtained, the crystal grain size is more preferably 140 nm or less, even more preferably 120 nm or less, even more preferably 110 nm or less, and may be 100 nm or less. There is no particular limit to the lower limit of the crystal grain size, but the crystal grain size can be, for example, 50 nm or more, or even 70 nm or more. The method for measuring the crystal grain size is as described above in the explanation of the crystal grain size in the zirconia sintered body.
[0034] The zirconia molded body of the present invention preferably has a three-point bending strength of 500 MPa or more after sintering at 900 to 1200 ° C. under normal pressure (after being made into a zirconia sintered body). This makes it possible to easily manufacture the zirconia sintered body of the present invention having excellent strength. Since a zirconia sintered body having excellent strength can be obtained, the three-point bending strength is more preferably 600 MPa or more, even more preferably 650 MPa or more, even more preferably 700 MPa or more, and particularly preferably 800 MPa or more. There is no particular limit to the upper limit of the three-point bending strength, but the three-point bending strength can be, for example, 1500 MPa or less, or even 1000 MPa or less. The method for measuring the three-point bending strength is as described above in the description of the three-point bending strength of the zirconia sintered body.
[0035] The zirconia molded body of the present invention preferably has a transmittance of 40% or more at a wavelength of 700 nm at a thickness of 0.5 mm after sintering at 900 to 1200 ° C. under normal pressure (after being made into a zirconia sintered body). This makes it possible to easily manufacture the zirconia sintered body of the present invention having excellent translucency. Since a zirconia sintered body having excellent translucency can be obtained, the transmittance is more preferably 45% or more, even more preferably 46% or more, even more preferably 48% or more, particularly preferably 50% or more, and may even be 52% or more. There is no particular limit to the upper limit of the transmittance, but the transmittance can be, for example, 60% or less, or even 57% or less. The method for measuring the transmittance is as described above in the explanation of the transmittance of light at a wavelength of 700 nm at a thickness of 0.5 mm in the zirconia sintered body.
[0036] The zirconia molded body of the present invention preferably has a linear light transmittance of 1% or more at a thickness of 1.0 mm after sintering at 900 to 1200 ° C. under normal pressure (after being made into a zirconia sintered body), more preferably 3% or more, even more preferably 5% or more, even more preferably 7% or more, and may even be 10% or more. When the linear light transmittance is within the above range, for example, when used as a dental prosthesis, the translucency required for the incisal part is easily satisfied. There is no particular limit to the upper limit of the linear light transmittance, but the linear light transmittance can be, for example, 60% or less, or even 50% or less. The method for measuring the linear light transmittance is as described above in the explanation of the linear light transmittance at a thickness of 1.0 mm in the zirconia sintered body.
[0037] [Method for producing zirconia molded body] The method for producing the zirconia molded body of the present invention is not particularly limited as long as it exerts the effects of the present invention. However, since it is possible to easily obtain the zirconia sintered body of the present invention which is excellent in both translucency and strength and in linear light transmittance, it is preferable that the method has a molding step of molding zirconia particles.
[0038] The content of yttria contained in the zirconia particles used is preferably the same as the content of yttria in the obtained zirconia molded body, and furthermore in the zirconia calcined body and zirconia sintered body, and the specific content of yttria in the zirconia particles is preferably 2.0 mol% or more, more preferably 3.0 mol% or more, and even more preferably 4.0 mol% or more, and preferably 9.0 mol% or less, more preferably 8.0 mol% or less, and even more preferably 7.0 mol% or less. The content of yttria in the zirconia particles means the ratio (mol%) of the number of moles of yttria to the total number of moles of zirconia and yttria.
[0039] It is important that the zirconia particles used have an average primary particle diameter of 60 nm or less, and that the zirconia particles having a particle diameter exceeding 100 nm are 0.5 mass% or less with respect to the total amount of zirconia particles in terms of particle size distribution. This makes it possible to easily obtain the zirconia molded body of the present invention, and in turn the zirconia calcined body and zirconia sintered body of the present invention. From the viewpoint of ease of production of the zirconia molded body of the present invention, and in turn the zirconia calcined body and zirconia sintered body of the present invention, the average primary particle diameter of the zirconia particles contained in the obtained zirconia molded body is preferably 50 nm or less, more preferably 30 nm or less, even more preferably 20 nm or less, and may be 10 nm or less, and is preferably 1 nm or more, and more preferably 5 nm or more. From the viewpoints of ease of production of the zirconia molded body of the present invention, and furthermore, of the zirconia calcined body and zirconia sintered body of the present invention, and of easily obtaining a desired linear light transmittance, the content of zirconia particles having a particle size exceeding 100 nm is more preferably 0.3% by mass or less, further preferably 0.1% by mass or less, and may be 0.05% by mass or less. The average primary particle size of zirconia particles can be determined, for example, by photographing zirconia particles (primary particles) with a transmission electron microscope (TEM), measuring the particle size (maximum diameter) of each of 100 arbitrary particles on the obtained image, and calculating the average value thereof. The content of zirconia particles having a particle size exceeding 100 nm can be measured, for example, by a zeta potential measuring device (for example, a real-time zeta potential / nanoparticle size measuring device (manufactured by Beckman Coulter, Inc., product name "DelsaMax PRO"), a zeta potential / particle size / molecular weight measuring system (manufactured by Otsuka Electronics Co., Ltd., product name "ELSZ-2000ZS"), etc. For example, the amount of zirconia particles is measured both before and after particle classification, and the difference between the measured values (mass %) corresponds to zirconia particles having a particle size exceeding 100 nm.
[0040] There is no particular limitation on the method for preparing zirconia particles, and for example, a breakdown process in which coarse particles are pulverized into fine powder, a building-up process in which atoms or ions are synthesized through a nucleation and growth process, etc., can be used. Among these, the building-up process is preferred in order to obtain fine zirconia particles of high purity.
[0041] The breakdown process can be carried out by pulverizing the powder using, for example, a ball mill or a bead mill. In this case, it is preferable to use a fine pulverizing medium, for example, a pulverizing medium of 100 μm or less. In addition, the desired ΔL * In order to obtain the desired WB and linear light transmittance, it is preferable to classify the obtained zirconia particles after crushing the coarse particles. For classification, known methods and devices can be used, such as a porous membrane (membrane filter having a pore size of 100 nm, etc.), a classification device (wet classification device, dry classification device), etc.
[0042] On the other hand, examples of building-up processes include a gas-phase pyrolysis method in which an oxide is precipitated by thermally decomposing an oxyacid salt of a metal ion having a high vapor pressure or an organometallic compound while vaporizing it; a gas-phase reaction method in which synthesis is carried out by a gas-phase chemical reaction between a gas of a metal compound having a high vapor pressure and a reactant gas; an evaporation concentration method in which the raw material is heated and vaporized, and then rapidly cooled in an inert gas at a specified pressure to condense the vapor into fine particles; a melt method in which a molten liquid is cooled into small droplets and solidified into a powder; a solvent evaporation method in which a solvent is evaporated to increase the concentration in the liquid and cause it to precipitate in a supersaturated state; and a precipitation method in which the solute concentration is made supersaturated by reaction with a precipitant or hydrolysis, and sparingly soluble compounds such as oxides and hydroxides are precipitated through a nucleation and growth process.
[0043] Precipitation methods are further classified into homogeneous precipitation methods, in which a precipitant is produced in the solution by a chemical reaction, eliminating localized unevenness in the precipitant concentration; coprecipitation methods, in which multiple metal ions coexisting in a liquid are precipitated simultaneously by adding a precipitant; hydrolysis methods, in which an oxide or hydroxide is obtained by hydrolysis from a metal salt solution or an alcohol solution of a metal alkoxide, etc.; and solvothermal synthesis methods, in which an oxide or hydroxide is obtained from a high-temperature, high-pressure fluid. The solvothermal synthesis methods are further classified into hydrothermal synthesis methods, in which water is used as a solvent, and supercritical synthesis methods, in which a supercritical fluid such as water or carbon dioxide is used as a solvent.
[0044] For any build-up process, it is preferable to increase the precipitation rate in order to obtain finer zirconia particles. * In order to obtain the desired WB and linear light transmittance, it is preferable to classify the obtained zirconia particles. For classification, known methods and devices can be used, such as a porous membrane (membrane filter having a pore size of 100 nm, etc.), a classification device (wet classification device, dry classification device), etc.
[0045] As the zirconium source in the building-up process, for example, nitrates, acetates, chlorides, alkoxides, etc. can be used, and specifically, zirconium oxychloride, zirconium acetate, zirconyl nitrate, etc. can be used.
[0046] In order to adjust the content of yttria in the zirconia particles to the above range, yttria can be blended during the production process of the zirconia particles, for example, yttria may be dissolved in the zirconia particles. As the yttrium source, for example, nitrates, acetates, chlorides, alkoxides, etc. can be used, and specifically, yttrium chloride, yttrium acetate, yttrium nitrate, etc. can be used.
[0047] The zirconia particles may be surface-treated in advance with a known surface treatment agent, such as an organic compound having an acidic group; a fatty acid amide such as saturated fatty acid amide, unsaturated fatty acid amide, saturated fatty acid bisamide, unsaturated fatty acid bisamide; a silane coupling agent (organosilicon compound), an organic titanium compound, an organic zirconium compound, an organic aluminum compound, etc., if necessary. By surface-treating the zirconia particles, when a powder containing zirconia particles and a fluorescent agent is prepared using a slurry containing a liquid whose surface tension at 25°C is 50mN / m or less as a dispersion medium as described below, the miscibility with such a liquid can be adjusted, and when a zirconia molded body is produced by a method having a step of polymerizing a composition containing zirconia particles, a fluorescent agent, and a polymerizable monomer as described below, the miscibility between the zirconia particles and a polymerizable monomer can be adjusted. Among the above surface treatment agents, organic compounds having an acidic group are preferred because they have excellent miscibility with liquids having a surface tension of 50 mN / m or less at 25° C. and can improve the strength of the resulting zirconia molded body by increasing the chemical bonding strength between the zirconia particles and the polymerizable monomer.
[0048] Examples of organic compounds having an acidic group include organic compounds having at least one acidic group such as a phosphoric acid group, a carboxylic acid group, a pyrophosphoric acid group, a thiophosphoric acid group, a phosphonic acid group, and a sulfonic acid group. Among these, a phosphoric acid group-containing organic compound having at least one phosphoric acid group and a carboxylic acid group-containing organic compound having at least one carboxylic acid group are preferred, and a phosphoric acid group-containing organic compound is more preferred. The zirconia particles may be surface-treated with one type of surface treatment agent, or may be surface-treated with two or more types of surface treatment agents. When the zirconia particles are surface-treated with two or more types of surface treatment agents, the resulting surface treatment layer may be a surface treatment layer of a mixture of two or more types of surface treatment agents, or may be a surface treatment layer of a multi-layer structure in which a plurality of surface treatment layers are laminated.
[0049] Examples of the phosphoric acid group-containing organic compound include 2-ethylhexyl acid phosphate, stearyl acid phosphate, 2-(meth)acryloyloxyethyl dihydrogen phosphate, 3-(meth)acryloyloxypropyl dihydrogen phosphate, 4-(meth)acryloyloxybutyl dihydrogen phosphate, 5-(meth)acryloyloxypentyl dihydrogen phosphate, 6-(meth)acryloyloxyhexyl dihydrogen phosphate, 7-(meth)acryloyloxyhexyl dihydrogen phosphate, and 8-(meth)acryloyloxyhexyl dihydrogen phosphate. Acryloyloxyheptyl dihydrogen phosphate, 8-(meth)acryloyloxyoctyl dihydrogen phosphate, 9-(meth)acryloyloxynonyl dihydrogen phosphate, 10-(meth)acryloyloxydecyl dihydrogen phosphate, 11-(meth)acryloyloxyundecyl dihydrogen phosphate, 12-(meth)acryloyloxydodecyl dihydrogen phosphate, 16-(meth)acryloyloxyhexadecyl dihydrogen Phosphate, 20-(meth)acryloyloxyicosyl dihydrogen phosphate, bis[2-(meth)acryloyloxyethyl]hydrogen phosphate, bis[4-(meth)acryloyloxybutyl]hydrogen phosphate, bis[6-(meth)acryloyloxyhexyl]hydrogen phosphate, bis[8-(meth)acryloyloxyoctyl]hydrogen phosphate, bis[9-(meth)acryloyloxynonyl]hydrogen phosphate, bis[10- [(meth)acryloyloxydecyl]hydrogen phosphate, 1,3-di(meth)acryloyloxypropyl dihydrogen phosphate, 2-(meth)acryloyloxyethyl phenyl hydrogen phosphate, 2-(meth)acryloyloxyethyl-2-bromoethyl hydrogen phosphate, bis[2-(meth)acryloyloxy-(1-hydroxymethyl)ethyl]hydrogen phosphate, and acid chlorides, alkali metal salts, and ammonium salts thereof.
[0050] Examples of the carboxylic acid group-containing organic compound include succinic acid, oxalic acid, octanoic acid, decanoic acid, stearic acid, polyacrylic acid, 4-methyloctanoic acid, neodecanoic acid, pivalic acid, 2,2-dimethylbutyric acid, 3,3-dimethylbutyric acid, 2,2-dimethylvaleric acid, 2,2-diethylbutyric acid, 3,3-diethylbutyric acid, naphthenic acid, cyclohexanedicarboxylic acid, (meth)acrylic acid, N-(meth)acryloylglycine, N-(meth)acryloylaspartic acid, O-(meth)acryloyltyrosine, N-(meth)acryloyltyrosine, N-(meth)acryloyl p-aminobenzoic acid, N-(meth)acryloyl-o-aminobenzoic acid, p-vinylbenzoic acid, 2-(meth)acryloyloxybenzoic acid, 3-(meth)acryloyloxybenzoic acid, 4-(meth)acryloyloxybenzoic acid, N-(meth)acryloyl-5-aminosalicylic acid, N-(meth)acryloyl-4-aminosalicylic acid, 2-(meth)acryloyloxyethyl hydrogen succinate, 2-(meth)acryloyloxyethyl hydrogen phthalate, 2-(meth)acryloyloxyethyl hydrogen maleate, 2-[ 2-(2-Methoxyethoxy)ethoxy]acetic acid (commonly known as "MEEAA"), 2-(2-Methoxyethoxy)acetic acid (commonly known as "MEAA"), succinic acid mono[2-(2-methoxyethoxy)ethyl]ester, maleic acid mono[2-(2-methoxyethoxy)ethyl]ester, glutaric acid mono[2-(2-methoxyethoxy)ethyl]ester, malonic acid, glutaric acid, 6-(meth)acryloyloxyhexane-1,1-dicarboxylic acid, 9-(meth)acryloyloxynonane-1,1-dicarboxylic acid, 10-(meth)acryloyloxydecane-1,1-dicarboxylic acid carboxylic acid, 11-(meth)acryloyloxyundecane-1,1-dicarboxylic acid, 12-(meth)acryloyloxydodecane-1,1-dicarboxylic acid, 13-(meth)acryloyloxytridecane-1,1-dicarboxylic acid, 4-(meth)acryloyloxyethyl trimellitate, 4-(meth)acryloyloxybutyl trimellitate, 4-(meth)acryloyloxyhexyl trimellitate, 4-(meth)acryloyloxydecyl trimellitate, 2-(meth)acryloyloxyethyl-3'-(meth)acryloyloxy-2'-(3,4-dicarboxybenzoyloxy)propyl succinate, and their acid anhydrides, acid halides, alkali metal salts, ammonium salts, etc.
[0051] In addition, examples of organic compounds having at least one acidic group other than the above, such as a pyrophosphate group, a thiophosphate group, a phosphonic acid group, or a sulfonic acid group, include those described in International Publication No. 2012 / 042911.
[0052] Examples of saturated fatty acid amides include palmitic acid amide, stearic acid amide, and behenic acid amide. Examples of unsaturated fatty acid amides include oleic acid amide and erucic acid amide. Examples of saturated fatty acid bisamides include ethylene bispalmitic acid amide, ethylene bisstearic acid amide, and hexamethylene bisstearic acid amide. Examples of unsaturated fatty acid bisamides include ethylene bisoleic acid amide, hexamethylene bisoleic acid amide, and N,N'-dioleylsebacic acid amide.
[0053] Examples of silane coupling agents (organic silicon compounds) include R 1 n Six 4-n (wherein R 1 is a substituted or unsubstituted hydrocarbon group having 1 to 12 carbon atoms, X is an alkoxy group having 1 to 4 carbon atoms, a hydroxyl group, a halogen atom or a hydrogen atom, and n is an integer of 0 to 3, with the proviso that R 1 and when there are multiple X's, they may be the same or different.
[0054] Specific examples of silane coupling agents (organic silicon compounds) include, for example, methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, diphenyldiethoxysilane, isobutyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(β-methoxyethoxy)silane, and 3,3,3-trifluoropropyltrimethoxysilane. , methyl-3,3,3-trifluoropropyldimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-methacryloyloxypropylmethyldimethoxysilane, γ-methacryloyloxypropylmethyldiethoxysilane, N-(β-aminoethyl)γ-aminopropylmethyldimethoxysilane, N-(β-aminoethyl) N-(β-aminoethyl)γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, trimethylsilanol, methyltrichlorosilane, methyldichlorosilane, dimethyldichlorosilane, trimethylchlorosilane, phenyltrichlorosilane, diphenyldichlorosilane, vinyltrichlorosilane Silane, trimethylbromosilane, diethylsilane, vinyltriacetoxysilane, ω-(meth)acryloyloxyalkyltrimethoxysilane [carbon number between (meth)acryloyloxy group and silicon atom: 3 to 12, e.g., γ-methacryloyloxypropyltrimethoxysilane, etc.], ω-(meth)acryloyloxyalkyltriethoxysilane [carbon number between (meth)acryloyloxy group and silicon atom: 3 to 12, e.g., γ-methacryloyloxypropyltriethoxysilane, etc.], etc. In the present specification, the term "(meth)acryloyl" is used to include both methacryloyl and acryloyl.
[0055] Among these, silane coupling agents having a functional group are preferred, and ω-(meth)acryloyloxyalkyltrimethoxysilane [number of carbon atoms between the (meth)acryloyloxy group and the silicon atom: 3 to 12], ω-(meth)acryloyloxyalkyltriethoxysilane [number of carbon atoms between the (meth)acryloyloxy group and the silicon atom: 3 to 12], vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriacetoxysilane, and γ-glycidoxypropyltrimethoxysilane are more preferred.
[0056] Examples of the organic titanium compound include tetramethyl titanate, tetraisopropyl titanate, tetra-n-butyl titanate, butyl titanate dimer, and tetra(2-ethylhexyl) titanate.
[0057] Examples of the organic zirconium compound include zirconium isopropoxide, zirconium n-butoxide, zirconium acetylacetonate, and zirconyl acetate.
[0058] Examples of the organoaluminum compound include aluminum acetylacetonate and aluminum organic acid salt chelate compounds.
[0059] The specific method of surface treatment is not particularly limited, and known methods can be used, such as a method of spraying the above-mentioned surface treatment agent while vigorously stirring the zirconia particles, or a method of dispersing or dissolving the zirconia particles and the above-mentioned surface treatment agent in a suitable solvent and then removing the solvent. The solvent may be a dispersion medium containing a liquid having a surface tension of 50 mN / m or less at 25°C, as described below. In addition, after dispersing or dissolving the zirconia particles and the above-mentioned surface treatment agent, reflux or high-temperature and high-pressure treatment (autoclave treatment, etc.) may be performed.
[0060] In the present invention, when a zirconia molded body is produced by a method having a molding step of molding zirconia particles, the type of the molding step is not particularly limited. However, since the zirconia molded body of the present invention, and further the zirconia calcined body and zirconia sintered body of the present invention can be easily obtained, the molding step is preferably: (i) slip casting a slurry containing zirconia particles; (ii) gel casting a slurry containing zirconia particles; (iii) press-molding the powder containing zirconia particles; (iv) forming a composition comprising zirconia particles and a resin; and (v) polymerizing the composition comprising the zirconia particles and the polymerizable monomer; It is preferable that at least one of the above is used.
[0061] Slurry containing zirconia particles There is no particular limitation on the method for preparing the slurry containing zirconia particles. For example, it may be one obtained through the above-mentioned breakdown process or building-up process, or it may be a commercially available product.
[0062] When the zirconia molded body, and in turn the zirconia calcined body and zirconia sintered body, contain a colorant and / or a translucency adjuster, the slurry containing the zirconia particles and the fluorescent agent may contain such a colorant and / or a translucency adjuster. In this case, the colorant and / or the translucency adjuster are preferably mixed in a liquid state such as a solution or dispersion with the slurry containing the zirconia particles.
[0063] Powder containing zirconia particles There is no particular limitation on the method for preparing the powder containing zirconia particles, and it is preferable to prepare the powder by drying the above-mentioned slurry containing zirconia particles, since it is possible to obtain a more uniform zirconia sintered body having excellent physical properties, etc. The slurry to be dried here may further contain a fluorescent agent and / or a colorant and / or a translucency adjuster.
[0064] The drying method is not particularly limited, and for example, spray drying, supercritical drying, freeze drying, hot air drying, reduced pressure drying, etc. can be adopted. Among these, any of spray drying, supercritical drying, and freeze drying is preferable, any of spray drying and supercritical drying is more preferable, and spray drying is further preferable, because it is possible to suppress aggregation of particles during drying and obtain a denser zirconia sintered body.
[0065] The slurry containing zirconia particles to be dried may be a slurry in which the dispersion medium is water. However, it is preferable that the slurry be a slurry in which the dispersion medium is other than water, such as an organic solvent, because this makes it possible to suppress aggregation of particles during drying and obtain a denser zirconia sintered body.
[0066] Examples of organic solvents include alcohols such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-2-propanol, 2-methoxyethanol, 2-ethoxyethanol, 2-(2-ethoxyethoxy)ethanol, diethylene glycol monobutyl ether, and glycerin; ketones such as acetone and methyl ethyl ketone; ethers such as tetrahydrofuran, diethyl ether, diisopropyl ether, 1,4-dioxane, and dimethoxyethane (including modified ethers such as propylene glycol monomethyl ether acetate (commonly known as "PGMEA") (preferably ether-modified ethers and / or ester-modified ethers, more preferably ether-modified alkylene glycols and / or ester-modified alkylene glycols)); esters such as ethyl acetate and butyl acetate; hydrocarbons such as hexane and toluene; and halogenated hydrocarbons such as chloroform and carbon tetrachloride. These organic solvents may be used alone or in combination of two or more. Among these, taking into consideration both safety to the living body and ease of removal, the organic solvent is preferably a water-soluble organic solvent, and specifically, ethanol, 2-propanol, 2-methyl-2-propanol, 2-ethoxyethanol, 2-(2-ethoxyethoxy)ethanol, propylene glycol monomethyl ether acetate, acetone, and tetrahydrofuran are more preferred.
[0067] In particular, when spray drying is employed, it is preferable that the dispersion medium of the slurry containing zirconia particles and a fluorescent agent to be dried contains a liquid having a surface tension of 50 mN / m or less at 25° C., since this can suppress the aggregation of particles during drying and allows the production of a denser zirconia sintered body. From this viewpoint, the surface tension of the liquid is preferably 40 mN / m or less, and more preferably 30 mN / m or less.
[0068] The surface tension at 25°C can be, for example, the value described in the Handbook of Chemistry and phisics, and for liquids not described therein, the value described in International Publication No. 2014 / 126034 can be used. For liquids not described in any of these, it can be determined by a known measurement method, for example, the hanging ring method, the Wilhelmy method, etc. The surface tension at 25°C is preferably measured using an automatic surface tensiometer "CBVP-Z" manufactured by Kyowa Interface Science Co., Ltd., or "SIGMA702" manufactured by KSV INSTRUMENTS LTD.
[0069] As the liquid, an organic solvent having the above surface tension can be used. As the organic solvent, any of the above-mentioned organic solvents having the above surface tension can be used, but at least one selected from the group consisting of methanol, ethanol, 2-methoxyethanol, 1,4-dioxane, 2-ethoxyethanol, and 2-(2-ethoxyethoxy)ethanol is preferable, since it is possible to suppress the aggregation of particles during drying and obtain a denser zirconia sintered body, and at least one selected from the group consisting of methanol, ethanol, 2-ethoxyethanol, and 2-(2-ethoxyethoxy)ethanol is more preferable.
[0070] The content of the above liquid in the dispersion medium is preferably 50% by mass or more, more preferably 80% by mass or more, even more preferably 95% by mass or more, and particularly preferably 99% by mass or more, because this makes it possible to suppress aggregation of particles during drying and obtain a denser zirconia sintered body.
[0071] A slurry of a dispersion medium other than water can be obtained by replacing the dispersion medium of a slurry whose dispersion medium is water. There is no particular limitation on the method of replacing the dispersion medium, and for example, a method of adding a dispersion medium other than water (such as an organic solvent) to a slurry whose dispersion medium is water, and then distilling off the water can be adopted. In distilling off the water, a part or all of the dispersion medium other than water may be distilled off together. The addition of the dispersion medium other than water and the distillation off of the water may be repeated multiple times. In addition, a method of adding a dispersion medium other than water to a slurry whose dispersion medium is water, and then precipitating the dispersoids can be adopted. Furthermore, for a slurry whose dispersion medium is water, the dispersion medium may be replaced with a specific organic solvent, and then further replaced with another organic solvent. The fluorescent agent may be added after replacing the dispersion medium, but is preferably added before replacing the dispersion medium, because a more uniform and excellent zirconia sintered body can be obtained. Similarly, when a colorant and / or a translucency regulator is contained in the slurry, the fluorescent agent may be added after replacing the dispersion medium, but is preferably added before replacing the dispersion medium, because a more uniform and excellent zirconia sintered body can be obtained.
[0072] The slurry containing zirconia particles to be dried may be one that has been subjected to a dispersion treatment using heat or pressure, such as reflux treatment or hydrothermal treatment. The slurry containing zirconia particles to be dried may be one that has been subjected to a mechanical dispersion treatment using a roll mill, colloid mill, high-pressure jet disperser, ultrasonic disperser, vibration mill, planetary mill, bead mill, etc. Only one of the above treatments may be used, or two or more of them may be used.
[0073] The slurry containing zirconia particles to be dried may further contain one or more of other components such as a binder, a plasticizer, a dispersant, an emulsifier, an antifoaming agent, a pH adjuster, a lubricant, etc. By containing such other components (particularly a binder, a dispersant, an antifoaming agent, etc.), it may be possible to suppress the aggregation of particles during drying, and to obtain a denser zirconia sintered body.
[0074] Examples of the binder include polyvinyl alcohol, methyl cellulose, carboxymethyl cellulose, acrylic binders, wax binders, polyvinyl butyral, polymethyl methacrylate, and ethyl cellulose.
[0075] Examples of the plasticizer include polyethylene glycol, glycerin, propylene glycol, and dibutyl phthalate.
[0076] Examples of dispersants include ammonium polycarboxylate (e.g., triammonium citrate), ammonium polyacrylate, acrylic copolymer resin, acrylic acid ester copolymer, polyacrylic acid, bentonite, carboxymethyl cellulose, anionic surfactants (e.g., polyoxyethylene alkyl ether phosphate esters such as polyoxyethylene lauryl ether phosphate esters), nonionic surfactants, olein glycerides, amine salt surfactants, and oligosaccharide alcohols.
[0077] Examples of the emulsifier include alkyl ethers, phenyl ethers, sorbitan derivatives, and ammonium salts.
[0078] Examples of the defoaming agent include alcohol, polyether, polyethylene glycol, silicone, and wax.
[0079] Examples of pH adjusters include ammonia, ammonium salts (including ammonium hydroxides such as tetramethylammonium hydroxide), alkali metal salts, and alkaline earth metal salts.
[0080] Examples of the lubricant include polyoxyethylene alkylate ether and wax.
[0081] The water content in the slurry containing zirconia particles to be dried is preferably 3% by mass or less, more preferably 1% by mass or less, and even more preferably 0.1% by mass or less, because it is possible to suppress the aggregation of particles during drying and obtain a denser zirconia sintered body. The water content can be measured using a Karl Fischer moisture meter.
[0082] The drying conditions in each of the above drying methods are not particularly limited, and known drying conditions can be appropriately adopted. When an organic solvent is used as a dispersion medium, it is preferable to perform drying in the presence of a non-flammable gas, and more preferably to perform drying in the presence of nitrogen, in order to reduce the risk of explosion during drying.
[0083] The supercritical fluid used in supercritical drying is not particularly limited, and for example, water, carbon dioxide, etc. can be used. However, it is preferable that the supercritical fluid is carbon dioxide, since it is possible to suppress aggregation of particles and obtain a denser zirconia sintered body.
[0084] A composition comprising zirconia particles and a resin There is no particular limitation on the method for preparing the composition containing zirconia particles and a resin. For example, the composition can be obtained by mixing the above-mentioned powder containing zirconia particles with a resin.
[0085] A composition comprising zirconia particles and a polymerizable monomer There is no particular limitation on the method for preparing the composition containing zirconia particles and a polymerizable monomer. For example, the composition can be obtained by mixing the above-mentioned powder containing zirconia particles with a polymerizable monomer.
[0086] (i) Slip casting When a zirconia molded body is produced by a method having a step of slip casting a slurry containing zirconia particles, the specific method of slip casting is not particularly limited, and for example, a method can be adopted in which a slurry containing zirconia particles is poured into a mold and then dried.
[0087] The content of the dispersion medium in the slurry containing the zirconia particles used is preferably 80 mass % or less, more preferably 50 mass % or less, and even more preferably 20 mass % or less, because this makes it easy to pour the slurry into a mold, prevents a long drying time from being required, and enables the mold to be used more frequently.
[0088] The slurry may be poured into the mold under normal pressure, but it is preferable to pour the slurry into the mold under pressurized conditions from the viewpoint of production efficiency. There is no particular limitation on the type of mold used in slip casting, and for example, a porous mold made of gypsum, resin, ceramics, etc. can be used. Porous molds made of resin or ceramics are excellent in terms of durability.
[0089] The slurry containing the zirconia particles used in slip casting may further contain one or more of the other components such as the binder, plasticizer, dispersant, emulsifier, antifoaming agent, pH adjuster, and lubricant as described above.
[0090] (ii) Gel casting When a zirconia molded body is produced by a method having a step of gel-casting a slurry containing zirconia particles, the specific method of gel-casting is not particularly limited. For example, a method can be employed in which a shaped wet body is obtained by gelling a slurry containing zirconia particles and a fluorescent agent in a mold, and then this is dried.
[0091] The content of the dispersion medium in the slurry containing the zirconia particles used is preferably 80 mass % or less, more preferably 50 mass % or less, and even more preferably 20 mass % or less, because this can prevent the drying process from taking a long time and can also suppress the occurrence of cracks during drying.
[0092] The gelation may be performed, for example, by adding a gelling agent, or by adding a polymerizable monomer and then polymerizing it. There is no particular limitation on the type of mold used, and for example, a porous mold made of gypsum, resin, ceramics, etc., or a non-porous mold made of metal, resin, etc. can be used.
[0093] There is no limitation on the type of gelling agent, and for example, a water-soluble gelling agent can be used, and specifically, agarose, gelatin, etc. can be preferably used. One type of gelling agent may be used alone, or two or more types may be used in combination. From the viewpoint of suppressing crack generation during sintering, the amount of gelling agent used is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less based on the mass of the slurry after the gelling agent is mixed, based on the mass of the slurry after the gelling agent is mixed, from the viewpoint of suppressing crack generation during sintering.
[0094] The type of polymerizable monomer is not particularly limited, and examples thereof include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, propylene glycol mono(meth)acrylate, glycerol mono(meth)acrylate, erythritol mono(meth)acrylate, N-methylol (meth)acrylamide, N-hydroxyethyl (meth)acrylamide, N,N-bis(2-hydroxyethyl) (meth)acrylamide, etc. The polymerizable monomer may be used alone or in combination of two or more kinds.
[0095] From the viewpoint of suppressing the occurrence of cracks during sintering, the amount of the polymerizable monomer used is preferably 10 mass % or less, more preferably 5 mass % or less, and even more preferably 1 mass % or less, based on the mass of the slurry after the polymerizable monomer is blended.
[0096] When gelation is performed by polymerization of a polymerizable monomer, the polymerization is preferably performed using a polymerization initiator. There is no particular limitation on the type of polymerization initiator, but a photopolymerization initiator is particularly preferred. The photopolymerization initiator can be appropriately selected from photopolymerization initiators used in general industry, and photopolymerization initiators used for dental purposes are particularly preferred.
[0097] Specific examples of photopolymerization initiators include (bis)acylphosphine oxides (including salts), thioxanthones (including salts such as quaternary ammonium salts), ketals, α-diketones, coumarins, anthraquinones, benzoin alkyl ether compounds, and α-aminoketone compounds. The photopolymerization initiator may be used alone or in combination of two or more. Among these photopolymerization initiators, it is preferable to use at least one selected from the group consisting of (bis)acylphosphine oxides and α-diketones. This allows polymerization (gelation) to be performed in both the ultraviolet region (including the near ultraviolet region) and the visible light region, and in particular, polymerization (gelation) can be sufficiently performed using any light source such as a laser such as an Ar laser or a He-Cd laser; a halogen lamp, a xenon lamp, a metal halide lamp, a light-emitting diode (LED), a mercury lamp, or a fluorescent lamp.
[0098] Of the above (bis)acylphosphine oxides, examples of the acylphosphine oxides include 2,4,6-trimethylbenzoyldiphenylphosphine oxide (commonly known as "TPO"), 2,6-dimethoxybenzoyldiphenylphosphine oxide, 2,6-dichlorobenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoylmethoxyphenylphosphine oxide, 2,4,6-trimethylbenzoylethoxyphenylphosphine oxide, 2,3,5,6-tetramethylbenzoyldiphenylphosphine oxide, benzoyldi(2,6-dimethylphenyl)phosphonate, sodium salt of 2,4,6-trimethylbenzoylphenylphosphine oxide, potassium salt of 2,4,6-trimethylbenzoylphenylphosphine oxide, and ammonium salt of 2,4,6-trimethylbenzoylphenylphosphine oxide.
[0099] Of the above (bis)acylphosphine oxides, examples of the bisacylphosphine oxides include bis(2,6-dichlorobenzoyl)phenylphosphine oxide, bis(2,6-dichlorobenzoyl)-2,5-dimethylphenylphosphine oxide, bis(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, bis(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide, bis(2,6-dimethoxybenzoyl)phenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,5-dimethylphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, and bis(2,3,6-trimethylbenzoyl)-2,4,4-trimethylpentylphosphine oxide. Furthermore, compounds described in JP-A-2000-159621 can also be used.
[0100] Among these (bis)acylphosphine oxides, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoylmethoxyphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, and the sodium salt of 2,4,6-trimethylbenzoylphenylphosphine oxide are preferred.
[0101] Examples of α-diketones include diacetyl, benzyl, camphorquinone, 2,3-pentadione, 2,3-octadione, 9,10-phenanthrenequinone, 4,4′-oxybenzyl, acenaphthenequinone, etc. Among these, camphorquinone is preferred, particularly when a light source in the visible light region is used.
[0102] The slurry containing the above-mentioned zirconia particles used in gel casting may further contain one or more of the other components such as the binder, plasticizer, dispersant, emulsifier, antifoaming agent, pH adjuster, and lubricant as described above, in the same manner as the slurry used in slip casting.
[0103] The drying method for drying the shaped wet body is not particularly limited, and examples thereof include natural drying, hot air drying, vacuum drying, dielectric heating drying, induction heating drying, constant temperature and humidity drying, etc. Only one of these may be used, or two or more may be used. Among these, natural drying, dielectric heating drying, induction heating drying, and constant temperature and humidity drying are preferred because they can suppress the occurrence of cracks during drying.
[0104] (iii) Press molding In the case of producing a zirconia molded body by a method having a step of press-molding a powder containing zirconia particles, the specific method of press molding is not particularly limited, and can be performed using a known press molding machine. Specific examples of the press molding method include uniaxial pressing. In addition, in order to increase the density of the obtained zirconia molded body, it is preferable to further perform cold isostatic pressing (CIP) treatment after uniaxial pressing.
[0105] The powder containing the zirconia particles used in the press molding may further contain one or more of the above-mentioned other components such as binders, plasticizers, dispersants, emulsifiers, antifoaming agents, pH adjusters, lubricants, etc. These components may be mixed when preparing the powder.
[0106] (iv) Molding of a composition containing a resin In the case of producing a zirconia molded body by a method having a step of molding a composition containing zirconia particles and a resin, the specific method for molding the composition is not particularly limited, and for example, injection molding, cast molding, extrusion molding, etc. can be adopted. In addition, a method of molding the composition by a thermal fusion method (FDM), an inkjet method, a powder / binder lamination method, and other additive manufacturing methods (3D printing, etc.) may be adopted. Among these molding methods, injection molding and cast molding are preferred, and injection molding is more preferred.
[0107] The type of the resin is not particularly limited, and one that functions as a binder can be preferably used. Specific examples of the resin include paraffin wax, polyvinyl alcohol, polyethylene, polypropylene, ethylene-vinyl acetate copolymer, polystyrene, atactic polypropylene, methacrylic resin, and fatty acids such as stearic acid. These resins may be used alone or in combination of two or more.
[0108] The composition containing the zirconia particles and the resin may further contain one or more of the other components such as the plasticizer, dispersant, emulsifier, antifoaming agent, pH adjuster, and lubricant as described above.
[0109] (v) Polymerization of a composition containing a polymerizable monomer By polymerizing a composition containing zirconia particles and a polymerizable monomer, the polymerizable monomer in the composition can be polymerized to harden the composition. When a zirconia molded body is manufactured by a method having a polymerization step, the specific method is not particularly limited, and for example, (a) a method of polymerizing a composition containing zirconia particles and a polymerizable monomer in a mold; (b) a stereolithography (SLA) method using a composition containing zirconia particles and a polymerizable monomer, etc. can be adopted. Among these, the stereolithography method (b) is preferable. According to the stereolithography method, a shape corresponding to the desired shape of the finally obtained zirconia sintered body can be imparted at the time of manufacturing the zirconia molded body. Therefore, the stereolithography method may be preferable, especially when the zirconia sintered body of the present invention is used as a dental material such as a dental prosthesis.
[0110] The type of polymerizable monomer in the composition containing the zirconia particles and the polymerizable monomer is not particularly limited, and may be any of monofunctional polymerizable monomers such as monofunctional (meth)acrylates and monofunctional (meth)acrylamides, and polyfunctional polymerizable monomers such as bifunctional aromatic compounds, bifunctional aliphatic compounds, and trifunctional or higher compounds. The polymerizable monomer may be used alone or in combination of two or more kinds. Among these, it is preferable to use a polyfunctional polymerizable monomer, particularly when a stereolithography method is adopted.
[0111] Examples of the monofunctional (meth)acrylate include (meth)acrylates having a hydroxyl group such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, propylene glycol mono(meth)acrylate, glycerol mono(meth)acrylate, and erythritol mono(meth)acrylate; methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, and sec-butyl (meth)acrylate. Examples of the acrylate include alkyl (meth)acrylates such as acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-hexyl (meth)acrylate, lauryl (meth)acrylate, cetyl (meth)acrylate, and stearyl (meth)acrylate; alicyclic (meth)acrylates such as cyclohexyl (meth)acrylate and isobornyl (meth)acrylate; aromatic group-containing (meth)acrylates such as benzyl (meth)acrylate and phenyl (meth)acrylate; and (meth)acrylates having functional groups such as 2,3-dibromopropyl (meth)acrylate, 3-(meth)acryloyloxypropyltrimethoxysilane, and 11-(meth)acryloyloxyundecyltrimethoxysilane.
[0112] Examples of monofunctional (meth)acrylamides include (meth)acrylamide, N-(meth)acryloylmorpholine, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-di-n-propyl(meth)acrylamide, N,N-di-n-butyl(meth)acrylamide, N,N-di-n-hexyl(meth)acrylamide, N,N-di-n-octyl(meth)acrylamide, N,N-di-2-ethylhexyl(meth)acrylamide, N-hydroxyethyl(meth)acrylamide, and N,N-di(hydroxyethyl)(meth)acrylamide.
[0113] Among these monofunctional polymerizable monomers, (meth)acrylamide is preferred because of its excellent polymerizability, and N-(meth)acryloylmorpholine, N,N-dimethyl(meth)acrylamide, and N,N-diethyl(meth)acrylamide are more preferred.
[0114] Examples of bifunctional aromatic compounds include 2,2-bis((meth)acryloyloxyphenyl)propane, 2,2-bis[4-(3-(meth)acryloyloxy-2-hydroxypropoxy)phenyl]propane, 2,2-bis[4-(3-methacryloyloxy-2-hydroxypropoxy)phenyl]propane (commonly known as "Bis-GMA"), 2,2-bis(4-(meth)acryloyloxyethoxyphenyl)propane, 2,2-bis(4-(meth)acryloyloxypolyethoxyphenyl)propane, 2,2-bis(4-(meth)acryloyloxydiethoxyphenyl)propane, 2,2-bis(4-(meth)acryloyloxytetraethoxyphenyl)propane, and 2,2-bis(4-(meth)acryloyloxypentaethoxyphenyl)propane. , 2,2-bis(4-(meth)acryloyloxydipropoxyphenyl)propane, 2-(4-(meth)acryloyloxydiethoxyphenyl)-2-(4-(meth)acryloyloxyethoxyphenyl)propane, 2-(4-(meth)acryloyloxydiethoxyphenyl)-2-(4-(meth)acryloyloxytriethoxyphenyl)propane, 2-(4-(meth)acryloyloxydipropoxyphenyl)-2-(4-(meth)acryloyloxytriethoxyphenyl)propane, 2,2-bis(4-(meth)acryloyloxypropoxyphenyl)propane, 2,2-bis(4-(meth)acryloyloxyisopropoxyphenyl)propane, 1,4-bis(2-(meth)acryloyloxyethyl)pyromellitate, and the like. Among these, 2,2-bis[4-(3-methacryloyloxy-2-hydroxypropoxy)phenyl]propane (commonly known as "Bis-GMA") and 2,2-bis(4-(meth)acryloyloxypolyethoxyphenyl)propane are preferred because of their excellent polymerizability and the strength of the resulting zirconia molded body. Among 2,2-bis(4-(meth)acryloyloxypolyethoxyphenyl)propane, 2,2-bis(4-methacryloyloxypolyethoxyphenyl)propane (a compound having an average added mole number of ethoxy groups of 2.6 (commonly known as "D-2.6E")) is preferred.
[0115] Examples of the bifunctional aliphatic compounds include glycerol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,4- Examples of the dimethacrylate include butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 2-ethyl-1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, 1,2-bis(3-methacryloyloxy-2-hydroxypropoxy)ethane, 2,2,4-trimethylhexamethylene bis(2-carbamoyloxyethyl)dimethacrylate (commonly known as "UDMA"). Among these, triethylene glycol dimethacrylate (commonly known as "TEGDMA") and 2,2,4-trimethylhexamethylene bis(2-carbamoyloxyethyl)dimethacrylate are preferred because of their excellent polymerizability and the strength of the resulting zirconia molded body.
[0116] Examples of trifunctional or higher compounds include trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, trimethylolmethane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, N,N-(2,2,4-trimethylhexamethylene)bis[2-(aminocarboxy)propane-1,3-diol]tetra(meth)acrylate, and 1,7-diacryloyloxy-2,2,6,6-tetra(meth)acryloyloxymethyl-4-oxaheptane. Among these, N,N-(2,2,4-trimethylhexamethylene)bis[2-(aminocarboxy)propane-1,3-diol]tetramethacrylate and 1,7-diacryloyloxy-2,2,6,6-tetraacryloyloxymethyl-4-oxaheptane are preferred because of their excellent polymerizability and the strength of the resulting zirconia molded body.
[0117] In both the above methods (a) and (b), the polymerization of the composition is preferably carried out using a polymerization initiator, and the composition preferably further contains a polymerization initiator. There is no particular limitation on the type of polymerization initiator, but a photopolymerization initiator is particularly preferred. The photopolymerization initiator can be appropriately selected from photopolymerization initiators used in general industry, and among them, photopolymerization initiators used for dental purposes are preferred. Specific examples of photopolymerization initiators are the same as those described above in the explanation of gel casting, and overlapping explanations will be omitted here.
[0118] The composition containing the zirconia particles and the polymerizable monomer may further contain one or more of the other components such as the plasticizer, dispersant, emulsifier, antifoaming agent, pH adjuster, and lubricant as described above.
[0119] In the case of producing a zirconia molded body by stereolithography using a composition containing zirconia particles and a polymerizable monomer, the specific method of stereolithography is not particularly limited, and a known method can be appropriately adopted for stereolithography. For example, a method can be adopted in which a liquid composition is photopolymerized with ultraviolet light, a laser, or the like using a stereolithography device to sequentially form layers having a desired shape to obtain the desired zirconia molded body.
[0120] When a zirconia molded body is obtained by stereolithography, the content of zirconia particles in a composition containing zirconia particles and a polymerizable monomer is preferably as high as possible from the viewpoint of subsequent sintering, specifically, it is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and particularly preferably 50% by mass or more. On the other hand, in the stereolithography, from the principle of lamination molding, it is desirable that the viscosity of the composition is within a certain range, and therefore the content of zirconia particles in the composition is preferably 90% by mass or less, more preferably 80% by mass or less, even more preferably 70% by mass or less, and particularly preferably 60% by mass or less. When performing a controlled liquid level method in which a zirconia molded body is formed one by one by irradiating light from the bottom of a container through the bottom surface of the container to harden the layers, the adjustment of the viscosity of the composition may be particularly important in order to raise the hardened layer by one layer and smoothly flow the composition for forming the next layer between the bottom surface of the hardened layer and the bottom surface of the container.
[0121] The specific viscosity of the composition is preferably 20,000 mPa·s or less, more preferably 10,000 mPa·s or less, even more preferably 5,000 mPa·s or less, and preferably 100 mPa·s or more, as measured at 25°C. Since the viscosity of the composition tends to increase as the content of zirconia particles increases, it is preferable to appropriately adjust the balance between the content of zirconia particles and the viscosity of the composition in accordance with the performance of the stereolithography device used, while taking into account the balance between the speed of stereolithography and the accuracy of the obtained zirconia molded body. The viscosity can be measured using an E-type viscometer.
[0122] In the method for producing a zirconia molded body of the present invention, in order to further improve the density of the zirconia molded body, the zirconia molded body may be subjected to a humidification treatment and then a CIP treatment. When press molding is performed, the powder containing zirconia particles before press molding may be subjected to a humidification treatment and then press molding. The humidification treatment may be performed by any known method without any restrictions, and may be performed by spraying water with a sprayer or using a hygrostat or a thermo-hygrostat. The increase in moisture due to the humidification treatment depends on the particle size of the zirconia particles contained, and is preferably more than 2 mass% of the mass of the pre-wet powder and the molded body, more preferably more than 3 mass%, even more preferably more than 4 mass%, particularly preferably more than 5 mass%, and is preferably 15 mass% or less, more preferably 13 mass% or less, and even more preferably 11 mass% or less. The increase in moisture due to the humidification treatment can be calculated as a percentage by dividing the value obtained by subtracting the mass of the pre-wet powder and the molded body from the mass of the pre-wet powder and the molded body by the mass of the pre-wet powder and the molded body.
[0123] [Zirconia calcined body] The zirconia calcined body of the present invention contains 2.0 to 9.0 mol % of yttria and has a ΔL *(WB) is not less than 5. By using the calcined zirconia body, it is possible to obtain a zirconia sintered body having excellent strength, translucency, and in-line light transmittance.
[0124] When the zirconia sintered body of the present invention contains a fluorescent agent, it is preferable that the zirconia calcined body contains such a fluorescent agent. The content of the fluorescent agent in the zirconia calcined body of the present invention can be appropriately adjusted according to the content of the fluorescent agent in the obtained zirconia sintered body. The specific content of the fluorescent agent contained in the zirconia calcined body is preferably 0.001 mass% or more, more preferably 0.005 mass% or more, and even more preferably 0.01 mass% or more, and is preferably 1 mass% or less, more preferably 0.5 mass% or less, and even more preferably 0.1 mass% or less, in terms of the oxide of the metal element contained in the fluorescent agent, relative to the mass of zirconia contained in the zirconia calcined body.
[0125] When the zirconia sintered body contains a colorant, it is preferable that the zirconia calcined body contains such a colorant. The content of the colorant in the zirconia calcined body of the present invention can be appropriately adjusted according to the content of the colorant in the obtained zirconia sintered body. The specific content of the colorant contained in the zirconia calcined body is preferably 0.001 mass% or more, more preferably 0.005 mass% or more, and even more preferably 0.01 mass% or more, and is preferably 5 mass% or less, more preferably 1 mass% or less, and even more preferably 0.5 mass% or less, and may be 0.1 mass% or less, or even 0.05 mass% or less, in terms of the oxide of the metal element contained in the colorant, relative to the mass of zirconia contained in the zirconia calcined body.
[0126] When the zirconia sintered body contains a translucency regulator, it is preferable that the zirconia calcined body contains such a translucency regulator. The content of the translucency regulator in the zirconia calcined body of the present invention can be appropriately adjusted according to the content of the translucency regulator in the obtained zirconia sintered body. The specific content of the translucency regulator contained in the zirconia calcined body is preferably 0.1 mass% or less relative to the mass of zirconia contained in the zirconia calcined body.
[0127] The content of yttria contained in the zirconia calcined body of the present invention may be within the range of 2.0 to 9.0 mol%, and may be the same as the content of yttria in the obtained zirconia sintered body, and the specific content of yttria in the zirconia calcined body is 2.0 mol% or more, preferably 3.0 mol% or more, more preferably 4.0 mol% or more, and 9.0 mol% or less, preferably 8.0 mol% or less, and more preferably 7.0 mol% or less. The content of yttria in the zirconia calcined body means the ratio (mol%) of the number of moles of yttria to the total number of moles of zirconia and yttria.
[0128] The density of the zirconia calcined body of the present invention is not particularly limited, and varies depending on the method for producing the zirconia molded body used, but is preferably 3.0 to 6.0 g / m 3 It is preferable that the range is 3.2 to 5.8 g / m 3 It is more preferable that the range is within the range.
[0129] The shape of the zirconia calcined body of the present invention is not particularly limited, and can be a desired shape depending on the application, but considering the handleability when used as a mill blank for manufacturing dental materials such as dental prostheses, a disk shape, a prism shape (rectangular parallelepiped shape, etc.), etc. are preferable. As described below, the zirconia calcined body can be cut (milled) to a desired shape depending on the application before being made into a zirconia sintered body, and the present invention also includes the zirconia calcined body having the desired shape after such cutting (milling). In addition, the zirconia calcined body may have a single-layer structure, but may also have a multi-layer structure. By making it into a multi-layer structure, the zirconia sintered body finally obtained can have a multi-layer structure, and its physical properties such as translucency can be locally changed.
[0130] The three-point bending strength of the zirconia calcined body of the present invention is preferably within the range of 10 to 70 MPa, and more preferably within the range of 20 to 60 MPa, from the viewpoints of being able to maintain the shape of the workpiece during processing using a cutting machine, and being able to easily perform the cutting itself, etc. The three-point bending strength of the zirconia calcined body can be measured for a sample of 5 mm x 40 mm x 10 mm using a universal testing machine under conditions of a span length (distance between supports) of 30 mm and a crosshead speed of 0.5 mm / min.
[0131] The zirconia calcined body of the present invention preferably has a crystal grain size of 180 nm or less after sintering at 900 to 1200 ° C. for 2 hours under normal pressure (after being made into a zirconia sintered body). This makes it possible to easily manufacture the zirconia sintered body of the present invention having excellent translucency. Since a zirconia sintered body having excellent translucency can be obtained, the crystal grain size is more preferably 140 nm or less, even more preferably 120 nm or less, and even more preferably 115 nm or less, and may be 110 nm or less. There is no particular restriction on the lower limit of the crystal grain size, but the crystal grain size can be, for example, 50 nm or more, or even 100 nm or more. The method for measuring the crystal grain size is as described above in the explanation of the crystal grain size in the zirconia sintered body.
[0132] The zirconia calcined body of the present invention has a ΔL * (WB) is 5 or more, preferably 7 or more, and may be 10 or more. * By setting (WB) within the above range, a zirconia sintered body with high linear light transmittance can be obtained when sintered under normal pressure. * There is no particular upper limit to (WB), but it can be, for example, 30 or less, or even 25 or less. * (WB) may be measured using a spectrophotometer, for example, a spectrophotometer (manufactured by Konica Minolta Japan, Inc., "CM-3610A") may be used. In this measurement, F11 is used as a light source, and the reflected light is measured to obtain the value. As a sample used for the measurement, a disk-shaped calcined zirconia body having a diameter of 20 mm and a thickness of 1.5 mm may be used.
[0133] The zirconia calcined body of the present invention preferably has a three-point bending strength of 500 MPa or more after sintering at 900 to 1200 ° C. under normal pressure (after being made into a zirconia sintered body). This makes it possible to easily manufacture the zirconia sintered body of the present invention having excellent strength. Since a zirconia sintered body having excellent strength can be obtained, the three-point bending strength is more preferably 600 MPa or more, even more preferably 650 MPa or more, even more preferably 700 MPa or more, and particularly preferably 800 MPa or more. There is no particular limit to the upper limit of the three-point bending strength, but the three-point bending strength can be, for example, 1500 MPa or less, or even 1000 MPa or less. The method for measuring the three-point bending strength is as described above in the description of the three-point bending strength of the zirconia sintered body.
[0134] The zirconia calcined body of the present invention preferably has a transmittance of 40% or more at a wavelength of 700 nm at a thickness of 0.5 mm after sintering at 900 to 1200 ° C. under normal pressure (after being made into a zirconia sintered body). This makes it possible to easily manufacture the zirconia sintered body of the present invention having excellent translucency. Since a zirconia sintered body having excellent translucency can be obtained, the transmittance is more preferably 45% or more, even more preferably 46% or more, even more preferably 48% or more, particularly preferably 50% or more, and may even be 52% or more. There is no particular limit to the upper limit of the transmittance, but the transmittance can be, for example, 60% or less, or even 57% or less. The method for measuring the transmittance is as described above in the explanation of the transmittance of light at a wavelength of 700 nm at a thickness of 0.5 mm in the zirconia sintered body.
[0135] The zirconia calcined body of the present invention preferably has a linear light transmittance of 1% or more at a thickness of 1.0 mm after sintering at 900 to 1200 ° C. under normal pressure (after being made into a zirconia sintered body), more preferably 3% or more, even more preferably 5% or more, even more preferably 7% or more, and may even be 10% or more. When the linear light transmittance is within the above range, for example, when used as a dental prosthesis, the translucency required for the incisal part is easily satisfied. There is no particular limit to the upper limit of the linear light transmittance, but the linear light transmittance can be, for example, 60% or less, or even 50% or less. The method for measuring the linear light transmittance is as described above in the explanation of the linear light transmittance at a thickness of 1.0 mm in the zirconia sintered body.
[0136] [Method for producing zirconia calcined body] The method for producing the zirconia calcined body of the present invention is preferably characterized by using the zirconia molded body of the present invention, and includes a step of calcining the zirconia molded body at 200 to 800°C. From the viewpoint of easily obtaining the desired zirconia calcined body, the calcination temperature is preferably 200°C or higher, more preferably 250°C or higher, and even more preferably 300°C or higher, and is preferably 800°C or lower, more preferably 700°C or lower, and even more preferably 600°C or lower. By setting the calcination temperature to the above lower limit or higher, it is possible to effectively suppress the generation of organic residues. In addition, by setting the calcination temperature to the above upper limit or lower, it is possible to suppress the excessive progression of sintering, which makes cutting (milling) with a cutting machine difficult.
[0137] The heating rate during calcination of the zirconia molded body of the present invention is not particularly limited, but is preferably 0.1° C. / min or more, more preferably 0.2° C. / min or more, even more preferably 0.5° C. / min or more, and is preferably 50° C. / min or less, more preferably 30° C. / min or less, and even more preferably 20° C. / min or less. When the heating rate is equal to or higher than the lower limit, productivity is improved. When the heating rate is equal to or lower than the upper limit, the volume difference between the inside and the outside of the zirconia molded body or the zirconia calcined body can be suppressed, and when the zirconia molded body contains an organic substance, the organic substance can be prevented from being rapidly decomposed, thereby preventing cracks and breakage.
[0138] There is no particular restriction on the calcination time when the zirconia molded body of the present invention is calcined. However, in order to efficiently and stably obtain the desired zirconia calcined body with good productivity, the calcination time is preferably 0.5 hours or more, more preferably 1 hour or more, and even more preferably 2 hours or more, and is preferably 10 hours or less, more preferably 8 hours or less, and even more preferably 6 hours or less.
[0139] The calcination in the present invention can be carried out using a calcination furnace. There is no particular limitation on the type of the calcination furnace, and for example, an electric furnace or a degreasing furnace generally used in industry can be used.
[0140] The zirconia calcined body of the present invention can be cut (milled) into a desired shape according to the application before being made into a zirconia sintered body. In particular, the zirconia sintered body of the present invention is particularly suitable as a dental material such as a dental prosthesis, since it has excellent translucency and strength despite containing a fluorescent agent, and in order to obtain a zirconia sintered body to be used for such an application, the zirconia calcined body can be cut (milled) into a shape corresponding to the application. There is no particular limitation on the method of cutting (milling), and it can be performed, for example, using a known milling device.
[0141] [Method for producing zirconia sintered body] As described above, the zirconia sintered body of the present invention can be produced by sintering the zirconia molded body of the present invention under normal pressure, and can also be produced by sintering the zirconia calcined body of the present invention under normal pressure.
[0142] In both the case of sintering the zirconia molded body of the present invention and the case of sintering the zirconia calcined body of the present invention, the sintering temperature is preferably 900°C or higher, more preferably 1000°C or higher, and even more preferably 1050°C or higher, from the viewpoint of easily obtaining the desired zirconia sintered body, and is preferably 1200°C or lower, more preferably 1150°C or lower, and even more preferably 1120°C or lower, from the viewpoint of easily obtaining the desired zirconia sintered body. By setting the sintering temperature to the above lower limit or higher, sintering can be sufficiently advanced, and a dense sintered body can be easily obtained. In addition, by setting the sintering temperature to the above upper limit or lower, a zirconia sintered body having a crystal grain size within the preferred range of the present invention can be easily obtained, and deactivation of the fluorescent agent can be suppressed.
[0143] In both cases of sintering the zirconia molded body of the present invention and sintering the zirconia calcined body of the present invention, there are no particular limitations on the sintering time, but in order to enable the desired zirconia sintered body to be obtained efficiently and stably with good productivity, the sintering time is preferably 5 minutes or more, more preferably 15 minutes or more, and even more preferably 30 minutes or more, and is preferably 6 hours or less, more preferably 4 hours or less, and even more preferably 2 hours or less.
[0144] The sintering in the present invention can be carried out using a sintering furnace. There is no particular limitation on the type of sintering furnace, and for example, electric furnaces and degreasing furnaces used in general industry can be used. In particular, when used for dental material applications, in addition to conventional sintering furnaces for dental zirconia, dental porcelain furnaces with relatively low sintering temperatures can also be used.
[0145] The zirconia sintered body of the present invention can be easily produced without HIP treatment, but by carrying out HIP treatment after the above-mentioned sintering under normal pressure, it is possible to further improve the translucency and strength.
[0146] [Uses of zirconia sintered body] Although there is no particular limitation on the use of the zirconia sintered body of the present invention, the zirconia sintered body of the present invention is particularly suitable as a dental material such as a dental prosthesis, since it has excellent translucency and strength and excellent linear light transmittance, and is particularly useful not only as a dental prosthesis used in the cervical region, but also as a dental prosthesis used in the occlusal surface of a molar or the incisal edge of an anterior tooth. The zirconia sintered body of the present invention is preferably used as a dental prosthesis used in the incisal edge of an anterior tooth. EXAMPLES
[0147] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these examples, etc. The methods for measuring each physical property are as follows.
[0148] (1) Average primary particle size of zirconia particles The zirconia particles were photographed using a transmission electron microscope (TEM), and the particle diameter (maximum diameter) of each of 100 randomly selected particles on the obtained image was measured, and the average value thereof was taken as the average primary particle diameter of the zirconia particles.
[0149] (2) Proportion of particles with a diameter exceeding 100 nm Zirconia particles were dispersed in methanol and measured using a laser diffraction / scattering type particle size distribution measuring device (LA-950, manufactured by Horiba, Ltd.).
[0150] (3) Crystal grain size The crystal grain size in the zirconia sintered body was determined by taking a field emission scanning electron microscope (FE-SEM) photograph of the cross section of the zirconia sintered body, arbitrarily selecting 10 particles from the photographed image, and calculating the average of their circle equivalent diameters (diameters of perfect circles with the same area).
[0151] (4) Three-point bending strength The three-point bending strength of the zirconia sintered body was measured in accordance with ISO 6872:2015. Samples of 4 mm × 1.2 mm × 15 mm were prepared from the plate-shaped zirconia sintered bodies of each Example and Comparative Example, and measurements were performed on the samples using a universal testing machine under conditions of a support distance of 12 mm and a crosshead speed of 0.5 mm / min.
[0152] (5) Light transmittance (wavelength 700 nm, thickness 0.5 mm) The transmittance of light with a wavelength of 700 nm at a thickness of 0.5 mm of the zirconia sintered body was measured using a spectrophotometer (Hitachi High-Technologies Corporation, "Hitachi Spectrophotometer U-3900H"), in which light generated from a light source was transmitted through and scattered by the sample, and an integrating sphere was used. In this measurement, the transmittance was first measured in the wavelength range of 300 to 750 nm, and then the transmittance for light with a wavelength of 700 nm was obtained. For the measurement, a disk-shaped zirconia sintered body with a diameter of 15 mm and a thickness of 0.5 mm, both sides of which were mirror-polished, was used as the sample.
[0153] (6)Linear light transmittance (1.0mm thickness) The linear light transmittance of the zirconia sintered body at a thickness of 1.0 mm was measured using a turbidity meter (manufactured by Nippon Denshoku Industries Co., Ltd., "Haze Meter NDH 4000") by transmitting and scattering light generated from a light source through the sample and using an integrating sphere. In this measurement, the linear light transmittance was measured in accordance with ISO 13468-1:1996 and JIS K 7361-1:1997, and the haze was measured in accordance with ISO 14782-1:1999 and JIS K 7136:2000 to measure the linear light transmittance. For the measurement, a disk-shaped zirconia sintered body with a diameter of 15 mm and a thickness of 1.0 mm, both sides of which were mirror-polished, was used as the sample.
[0154] (7) Proportion of cubic crystals The proportion of cubic crystals in the zirconia sintered body was determined by analyzing the crystal phase. Specifically, X-ray diffraction (XRD) measurements were performed on the mirror-finished surface of the zirconia sintered body, and the proportion was calculated from the following formula. f c = 100 × I c / (I m +I t +I c ) where f c represents the percentage of cubic crystals in the zirconia sintered body, and I m represents the height of the peak near 2θ = 28° (peak based on the monoclinic (11-1) plane), and I t represents the height of the peak near 2θ = 30° (the peak based on the (111) plane of the tetragonal crystal system), and I c represents the height of the peak near 2θ=30° (peak based on the (111) plane of the cubic crystal system). For the measurement, disk-shaped zirconia sintered bodies of each of the examples and comparative examples were used as samples.
[0155] (8) Proportion of monoclinic crystals after hot water treatment The ratio of monoclinic to tetragonal and cubic crystals of the zirconia sintered body after immersion in 180°C hot water for 5 hours was calculated by mirror-finishing the surface of the zirconia sintered body, immersing it in 180°C hot water for 5 hours, and then performing X-ray diffraction (XRD) measurement on the above part, and calculating it from the following formula. f m = 100 × I m / (I t+c ) where f m represents the ratio (%) of monoclinic to tetragonal and cubic crystals in the zirconia sintered body after immersion in 180°C hot water for 5 hours, and I m represents the height of the peak near 2θ = 28° (peak based on the monoclinic (11-1) plane), and I t+c represents the height of the peak near 2θ=30° (a peak based on a mixed phase of the (111) plane of the tetragonal crystal system and the (111) plane of the cubic crystal system). For the measurement, the disk-shaped zirconia sintered bodies of each of the examples and comparative examples were used as samples.
[0156] (9) Appearance of zirconia sintered body The appearance (color) of the zirconia sintered body was evaluated visually.
[0157] (10) Fluorescence of zirconia sintered body The fluorescence of the zirconia sintered body was evaluated by visually observing the presence or absence of fluorescence under UV light.
[0158] (11) ΔL of zirconia compact and zirconia calcined body * (WB) ΔL at 1.5 mm thickness for zirconia compact and zirconia calcined body * (WB) was measured using a spectrophotometer. Specifically, it was measured using a spectrophotometer (Konica Minolta Japan, Inc., "CM-3610A") and calculated using Konica Minolta, Inc.'s color management software "SpectraMagic NX ver.2.5". In this measurement, F11 was used as the light source, and the reflected light was measured. For the measurement, a disk-shaped zirconia compact and a zirconia calcined body with a diameter of 20 mm and a thickness of 1.5 mm were used as samples.
[0159] [Example 1] 1.0 L of a mixed aqueous solution containing 0.62 mol / L of zirconium oxychloride and 0.038 mol / L of yttrium chloride, and 0.5 L of a 1.9 mol / L aqueous sodium hydroxide solution were prepared. 1.0L of pure water was poured into the precipitation tank, and the mixed aqueous solution and the sodium hydroxide aqueous solution were poured in at the same time to co-precipitate zirconium oxychloride and yttrium chloride to obtain a slurry. After filtering and washing, 22.2g of acetic acid was added to the slurry, and the slurry was hydrothermally treated at 200°C for 3 hours. The obtained slurry was centrifuged through a membrane filter having a pore size of 100nm, and pure water was added so that the solid concentration (zirconia and yttria concentration) was 5.0 mass%, to produce a zirconia slurry from which coarse particles had been removed. The average primary particle diameter of the zirconia particles contained in this zirconia slurry was 17nm, and no zirconia particles having a particle diameter exceeding 100nm were confirmed. The zirconia slurry was poured into a plaster mold as a molding slurry, left at room temperature for 2 weeks, and then subjected to cold isostatic pressing (CIP) (pressure 170 MPa) to increase the density and obtain a zirconia molded body. The plaster mold was made so that the molded body shape before CIP was a plate shape of 25 mm x 25 mm x 5 mm and a disk shape of 20 mm in diameter x 2.5 mm in thickness. The plaster mold was made by mixing plaster ("Noritake Dental Plaster", manufactured by Kuraray Noritake Dental Co., Ltd.) with water at a water mixing ratio of 50 mass%. The zirconia molded body was calcined at 500°C for 2 hours under normal pressure to obtain a zirconia calcined body. Furthermore, the zirconia calcined body was sintered at 1100°C for 2 hours under normal pressure to obtain a zirconia sintered body containing 3 mol% yttria. The obtained zirconia sintered body was white. The measurement results are shown in Table 1. In addition, the zirconia calcined bodies prepared in the same manner as described above were cut using a milling device ("Katana H-18", manufactured by Kuraray Noritake Dental Co., Ltd.) into zirconia calcined bodies having a single crown shape for a maxillary central incisor and a single crown shape for a mandibular first molar, and these were sintered at 1100°C for 2 hours under normal pressure to obtain dental prostheses having a crown shape.
[0160] [Example 2] A zirconia slurry was prepared in the same manner as in Example 1, except for using 1.0 L of a mixed aqueous solution containing 0.62 mol / L zirconium oxychloride and 0.066 mol / L yttrium chloride. The average primary particle size of the zirconia particles contained in the zirconia slurry was 18 nm, and the content of zirconia particles having a particle size exceeding 100 nm was 0.35 mass%. A zirconia compact, a zirconia calcined body, and a zirconia sintered body each containing 5 mol% of yttria were obtained in the same manner as in Example 1, except that the slurry obtained above was used as a molding slurry. The obtained zirconia sintered body was white. The measurement results are shown in Table 1.
[0161] [Example 3] A zirconia slurry was prepared in the same manner as in Example 1, except for using 1.0 L of a mixed aqueous solution containing 0.62 mol / L zirconium oxychloride and 0.108 mol / L yttrium chloride. The average primary particle size of the zirconia particles contained in the zirconia slurry was 17 nm, and the content of zirconia particles having a particle size exceeding 100 nm was 0.15 mass%. A zirconia compact, a zirconia calcined body, and a zirconia sintered body each containing 8 mol% of yttria were obtained in the same manner as in Example 1, except that the slurry obtained above was used as a molding slurry. The obtained zirconia sintered body was white. The measurement results are shown in Table 1.
[0162] [Example 4] A dilute nitric acid solution of bismuth nitrate was added to the zirconia slurry prepared in Example 2 (average primary particle size: 18 nm, zirconia particles having a particle size exceeding 100 nm were 0.35% by mass) so that the content of bismuth, calculated as bismuth oxide (Bi2O3), relative to the mass of zirconia was 0.02% by mass, to prepare a molding slurry containing zirconia particles and a fluorescent agent. A zirconia compact, a zirconia calcined body, and a zirconia sintered body each containing 5 mol% of yttria were obtained in the same manner as in Example 1, except that the slurry obtained above was used as the molding slurry. The obtained zirconia sintered body was white and had fluorescence. The measurement results are shown in Table 1.
[0163] [Example 5] A nickel (II) nitrate aqueous solution was added to the zirconia slurry prepared in Example 2 (average primary particle size: 18 nm, zirconia particles having a particle size exceeding 100 nm: 0.35% by mass) so that the content of nickel (II) converted to oxide (NiO) relative to the mass of zirconia was 0.02% by mass, thereby preparing a molding slurry containing zirconia particles and a colorant. A zirconia compact, a zirconia calcined body, and a zirconia sintered body each containing 5 mol% of yttria were obtained in the same manner as in Example 1, except that the slurry obtained above was used as the molding slurry. The obtained zirconia sintered body was colored red. The measurement results are shown in Table 1.
[0164] [Comparative Example 1] Zirconia particle powder "TZ-3Y" (manufactured by Tosoh Corporation, yttria content: 3 mol%, average primary particle diameter: 30 nm) was molded into a plate shape of 25 mm × 25 mm × 5 mm and a disk shape of 20 mm diameter × 2.5 mm thickness by a uniaxial press, and these were subjected to cold isostatic pressing (CIP) treatment (pressure 170 MPa) to increase the density and obtain zirconia molded bodies. These zirconia molded bodies were calcined at 500 ° C under normal pressure for 2 hours to obtain zirconia calcined bodies. Furthermore, these zirconia calcined bodies were sintered at 1100 ° C under normal pressure for 2 hours to obtain zirconia sintered bodies containing 3 mol% yttria. The obtained zirconia sintered bodies were white. The measurement results are shown in Table 1.
[0165] [Comparative Example 2] The zirconia compacts produced in Comparative Example 1 were calcined at 500°C under normal pressure for 2 hours to obtain calcined zirconia bodies. These calcined zirconia bodies were then sintered at 1500°C under normal pressure for 2 hours to obtain zirconia sintered bodies containing 3 mol% yttria. The obtained zirconia sintered bodies were white in color. The measurement results are shown in Table 1.
[0166] [Comparative Example 3] Zirconia particle powder "TZ-8YS" (manufactured by Tosoh Corporation, yttria content: 8 mol%, average primary particle diameter: 300 nm) was molded into a plate shape of 25 mm × 25 mm × 5 mm and a disk shape of 20 mm diameter × 2.5 mm thickness by a uniaxial press, and these were subjected to cold isostatic pressing (CIP) treatment (pressure 170 MPa) to increase the density and obtain zirconia molded bodies. These zirconia molded bodies were calcined at 500 ° C under normal pressure for 2 hours to obtain zirconia calcined bodies. Furthermore, these zirconia calcined bodies were sintered at 1500 ° C under normal pressure for 2 hours to obtain zirconia sintered bodies containing 8 mol% yttria. The obtained zirconia sintered bodies were white. The measurement results are shown in Table 1.
[0167] [Comparative Example 4] 1.0 L of a mixed aqueous solution containing 0.62 mol / L of zirconium oxychloride and 0.066 mol / L of yttrium chloride, and 0.5 L of a 1.9 mol / L aqueous sodium hydroxide solution were prepared. 1.0 L of pure water was poured into a precipitation tank, and the above mixed aqueous solution and an aqueous sodium hydroxide solution were further poured in at the same time to co-precipitate zirconium oxychloride and yttrium chloride, thereby obtaining a slurry. After filtering and washing, 22.2 g of acetic acid was added to the slurry, which was then hydrothermally treated at 200° C. for 3 hours, and pure water was added to give a solids concentration (zirconia and yttria concentration) of 5.0 mass % to produce a zirconia slurry. The average primary particle size of the zirconia particles contained in this zirconia slurry was 19 nm, and zirconia particles having a particle size exceeding 100 nm accounted for 5.3 mass %. A zirconia compact, a zirconia calcined body, and a zirconia sintered body each containing 5 mol% of yttria were obtained in the same manner as in Example 1, except that the zirconia slurry obtained above was used as a molding slurry. The obtained zirconia sintered body was white. The measurement results are shown in Table 1.
[0168] [Table 1]
[0169] [Example 6] Tetramethylammonium hydroxide was added as a pH adjuster and triammonium citrate was added as a dispersant to the zirconia slurry (average primary particle size: 18 nm, zirconia particles having a particle size exceeding 100 nm: 0.35% by mass) prepared in Example 2. Agarose was added as a gelling agent while heating and stirring this mixture to prepare a molding slurry containing zirconia particles, a pH adjuster, a dispersing agent and a gelling agent. The molding slurry was poured into a polypropylene mold and dried at room temperature for 16 days to obtain a zirconia molded body. The zirconia molded body was calcined at 500°C under normal pressure for 2 hours to obtain a zirconia calcined body. The zirconia calcined body was further sintered at 1100°C under normal pressure for 2 hours to obtain a zirconia sintered body containing 5 mol% yttria. The obtained zirconia sintered body was white. The measurement results are shown in Table 2.
[0170] [Example 7] To the zirconia slurry prepared in Example 2 (average primary particle size: 18 nm, zirconia particles having a particle size exceeding 100 nm: 0.35% by mass), 50 parts by mass of 2-ethoxyethanol was added as a dispersion medium replacement operation, and the mixture was concentrated to a total amount of 100 parts by mass using a rotary evaporator. The above dispersion medium replacement operation was repeated four times to obtain a 2-ethoxyethanol-substituted slurry. The residual moisture content of this 2-ethoxyethanol-substituted slurry was measured using a Karl Fischer moisture meter and found to be 0.05% by mass. This 2-ethoxyethanol substituted slurry was dried using a spray dryer (B-290, manufactured by Nippon Buchi Co., Ltd.) under conditions of a feed rate of 5 mL / min, an inlet temperature of 150° C., and an outlet temperature of 100° C., to obtain a powder containing zirconia particles.
[0171] The obtained powder was molded into a plate shape of 25 mm x 25 mm x 5 mm and a disk shape of 20 mm diameter x 2.5 mm thickness by a uniaxial press, and these were subjected to cold isostatic pressing (CIP) treatment (pressure 170 MPa) to increase the density and obtain zirconia molded bodies. These zirconia molded bodies were calcined at 500°C under normal pressure for 2 hours to obtain zirconia calcined bodies. Furthermore, these zirconia calcined bodies were sintered at 1100°C under normal pressure for 2 hours to obtain zirconia sintered bodies containing 5 mol% yttria. The obtained zirconia sintered bodies were white. The measurement results are shown in Table 2. In addition, the zirconia calcined bodies prepared in the same manner as described above were cut using a milling device ("Katana H-18", manufactured by Kuraray Noritake Dental Co., Ltd.) into zirconia calcined bodies having a single crown shape for a maxillary central incisor and a single crown shape for a mandibular first molar, and these were sintered at 1100°C for 2 hours under normal pressure to obtain dental prostheses having a crown shape.
[0172] [Example 8] To the zirconia slurry prepared in Example 2 (average primary particle diameter: 18 nm, zirconia particles having a particle diameter exceeding 100 nm: 0.35% by mass), isopropanol was added in an amount 9 times the volume of the zirconia slurry, which was then placed in a centrifuge tube and mixed thoroughly, followed by centrifugation at 4000 rpm for 10 minutes. After confirming the precipitation of white matter, the supernatant was removed, and isopropanol was added again, mixed thoroughly, and centrifuged at 4000 rpm for 10 minutes. After confirming the precipitation of white matter, the supernatant was removed, and methanol was added to the mixture to make it the same volume as the zirconia slurry used, and further mixed thoroughly to obtain a methanol-substituted slurry. The remaining moisture content of this methanol-substituted slurry was measured using a Karl Fischer moisture meter and found to be 0.08% by mass. The obtained methanol-substituted slurry was supercritically dried using a supercritical drying apparatus according to the following procedure. That is, the methanol-substituted slurry was placed in a pressure vessel, the pressure vessel was connected to a supercritical carbon dioxide extraction apparatus, and it was confirmed that there was no pressure leakage. Then, the pressure vessel and the preheating tube were immersed in a water bath heated to 60°C, and the temperature was raised to 80°C, and the pressure was increased to 25 MPa, and the mixture was left to stand for 10 minutes for stabilization. Next, carbon dioxide and methanol as an entrainer were introduced under the specified conditions (temperature: 80°C, pressure: 25 MPa, flow rate of carbon dioxide: 10 mL / min, flow rate of entrainer (methanol): 1.5 mL / min), and the introduction of methanol was stopped after 2 hours had elapsed, and the introduction of only carbon dioxide was continued. After 2 hours of the introduction of only carbon dioxide, the delivery of carbon dioxide was stopped, and the pressure was gradually reduced from 25 MPa over about 20 minutes while maintaining the temperature at 80°C, and returned to normal pressure. The pressure vessel was removed from the water bath and cooled to normal temperature, opened, and the treated sample was collected, and a powder containing zirconia particles was obtained. A zirconia compact, a zirconia calcined body, and a zirconia sintered body each containing 5 mol% of yttria were obtained in the same manner as in Example 7, except that the powder obtained above was used. The obtained zirconia sintered body was white. The measurement results are shown in Table 2.
[0173] [Example 9] To the zirconia slurry prepared in Example 2 (average primary particle diameter: 18 nm, zirconia particles having a particle diameter exceeding 100 nm: 0.35% by mass), isopropanol was added in an amount 9 times the volume of the zirconia slurry, which was then placed in a centrifuge tube and mixed thoroughly, followed by centrifugation at 4000 rpm for 10 minutes. After confirming the precipitation of white matter, the supernatant was removed, and isopropanol was added again to the mixture, mixed thoroughly, and centrifuged at 4000 rpm for 10 minutes. After confirming the precipitation of white matter, the supernatant was removed, and tert-butyl alcohol was added to the mixture to make the volume the same as that of the zirconia slurry used, and further mixed thoroughly to obtain a tert-butyl alcohol-substituted slurry. The residual moisture content of the tert-butyl alcohol-substituted slurry was measured using a Karl Fischer moisture meter and found to be 0.05% by mass.
[0174] The obtained tert-butyl alcohol-substituted slurry was transferred to an aluminum tray and immersed in liquid nitrogen in a separately prepared Dewar vessel to freeze the tert-butyl alcohol-substituted slurry. The frozen tert-butyl alcohol-substituted slurry was placed in a freeze-dryer pre-cooled to -40°C, and the freeze-dryer was depressurized to 130 Pa or less using a vacuum pump, and the temperature inside the freeze-dryer was changed to -10°C. The internal temperature of the freeze-dryer was confirmed by inserting a temperature sensor inside and outside the aluminum tray. 72 hours after the temperature inside the freeze-dryer stabilized at -10°C, it was confirmed that the temperature difference inside and outside the aluminum tray was within 5°C, the temperature inside the freeze-dryer was changed to 30°C, and after leaving it for 24 hours, the reduced pressure inside the freeze-dryer was released, and a powder containing zirconia particles was obtained. A zirconia compact, a zirconia calcined body, and a zirconia sintered body each containing 5 mol% of yttria were obtained in the same manner as in Example 7, except that the powder obtained above was used. The obtained zirconia sintered body was white. The measurement results are shown in Table 2.
[0175] [Example 10] A dilute nitric acid solution of bismuth nitrate was added to the zirconia slurry prepared in Example 1 (average primary particle size: 17 nm; no zirconia particles having a particle size exceeding 100 nm were confirmed) so that the content of bismuth, calculated as bismuth oxide (Bi2O3), relative to the mass of zirconia was 0.02 mass%, to prepare a molding slurry containing zirconia particles and a fluorescent agent. A zirconia compact, a zirconia calcined body, and a zirconia sintered body each containing 3 mol% of yttria were obtained in the same manner as in Example 1, except that the slurry obtained above was used as the molding slurry. The obtained zirconia sintered body was white and had fluorescence. The measurement results are shown in Table 2.
[0176] [Example 11] A dilute nitric acid solution of bismuth nitrate was added to the zirconia slurry prepared in Example 3 (average primary particle size: 17 nm, zirconia particles having a particle size exceeding 100 nm were 0.15% by mass) so that the content of bismuth, calculated as bismuth oxide (Bi2O3), relative to the mass of zirconia was 0.02% by mass, to prepare a molding slurry containing zirconia particles and a fluorescent agent. A zirconia compact, a zirconia calcined body, and a zirconia sintered body each containing 8 mol% of yttria were obtained in the same manner as in Example 3, except that the slurry obtained above was used as the molding slurry. The obtained zirconia sintered body was white and had fluorescence. The measurement results are shown in Table 2.
[0177] [Example 12] Tetramethylammonium hydroxide was added as a pH adjuster to the zirconia slurry prepared in Example 4 (average primary particle size: 18 nm, zirconia particles with a particle size exceeding 100 nm were 0.35 mass%, and a dilute nitric acid solution of bismuth was added so that the content of bismuth in terms of oxide (Bi2O3) relative to the mass of zirconia was 0.02 mass%), and triammonium citrate was added as a dispersant. Agarose was added as a gelling agent while heating and stirring this mixture, to prepare a molding slurry containing zirconia particles, a fluorescent agent, a pH adjuster, a dispersant, and a gelling agent. A zirconia compact, a zirconia calcined body, and a zirconia sintered body each containing 5 mol% of yttria were obtained in the same manner as in Example 6, except that the slurry obtained above was used as the molding slurry. The obtained zirconia sintered body was white and had fluorescence. The measurement results are shown in Table 2.
[0178] [Example 13] To the zirconia slurry prepared in Example 4 (average primary particle size: 18 nm, zirconia particles having a particle size exceeding 100 nm: 0.35 mass%, dilute bismuth nitric acid solution was added so that the content of bismuth oxide (Bi2O3) relative to the mass of zirconia was 0.02 mass%), 50 mass parts of 2-ethoxyethanol was added as a dispersion medium replacement operation, and the mixture was concentrated to a total amount of 100 mass parts using a rotary evaporator. The above dispersion medium replacement operation was repeated four times to obtain a 2-ethoxyethanol-substituted slurry. The residual moisture content of this 2-ethoxyethanol-substituted slurry was measured using a Karl Fischer moisture meter and found to be 0.07 mass%. This 2-ethoxyethanol substituted slurry was dried using a spray dryer (B-290, manufactured by Nippon Buchi Co., Ltd.) under conditions of a feed rate of 5 mL / min, an inlet temperature of 150°C, and an outlet temperature of 100°C, to obtain a powder containing zirconia particles and a fluorescent agent.
[0179] A zirconia compact, a zirconia calcined body, and a zirconia sintered body each containing 5 mol% of yttria were obtained in the same manner as in Example 7, except that the above powder was used as the obtained powder. The obtained zirconia sintered body was white and had fluorescence. The measurement results are shown in Table 2. In addition, the zirconia calcined bodies prepared in the same manner as above were cut into single-crown zirconia bodies for the upper central incisor and the lower first molar, using a milling machine ("Katana H-18", manufactured by Kuraray Noritake Dental Co., Ltd.), and these were sintered at 1100°C for 2 hours under normal pressure to obtain dental prostheses in the shape of crowns. The obtained zirconia sintered bodies in the shape of crowns had fluorescence.
[0180] [Example 14] To the zirconia slurry prepared in Example 4 (average primary particle size: 18 nm, zirconia particles having a particle size exceeding 100 nm: 0.35 mass%, bismuth oxide (Bi2O3) content relative to the mass of zirconia: 0.02 mass%), isopropanol was added in an amount 9 times the volume of the zirconia slurry, which was then placed in a centrifuge tube and mixed thoroughly, then centrifuged at 4000 rpm for 10 minutes. After confirming the precipitation of white matter, the supernatant was removed, isopropanol was added again, mixed thoroughly, and centrifuged at 4000 rpm for 10 minutes. After confirming the precipitation of white matter, the supernatant was removed, and methanol was added to the mixture to make it the same volume as the zirconia slurry used, and the mixture was further mixed thoroughly to obtain a methanol-substituted slurry. The remaining water content of this methanol-substituted slurry was measured using a Karl Fischer moisture meter and found to be 0.06 mass%. A powder containing zirconia particles and a fluorescent agent was obtained in the same manner as in Example 8, except that the above methanol-substituted slurry was used.
[0181] A zirconia compact, a zirconia calcined body, and a zirconia sintered body each containing 5 mol% of yttria were obtained in the same manner as in Example 8, except that the above powder was used as the obtained powder. The obtained zirconia sintered body was white and had fluorescence. The measurement results are shown in Table 2. In addition, the zirconia calcined bodies prepared in the same manner as above were cut into single-crown zirconia bodies for the upper central incisor and the lower first molar, using a milling machine ("Katana H-18", manufactured by Kuraray Noritake Dental Co., Ltd.), and these were sintered at 1100°C for 2 hours under normal pressure to obtain dental prostheses in the shape of crowns. The obtained zirconia sintered bodies in the shape of crowns had fluorescence.
[0182] [Table 2]
Claims
1. The zirconia particles contain 2.0 to 9.0 mol % of yttria, have an average primary particle size of 5 nm or more and 30 nm or less, and contain 0.35 mass % or less of particles having a particle size exceeding 100 nm, The total content of polymerizable monomers and their polymers is 5% by mass or less, and ΔL at a thickness of 1.5 mm * A zirconia molded body, wherein (W−B) is 5 or more.
2. 2. The zirconia molded body according to claim 1, having a three-point bending strength of 500 MPa or more after sintering at 900 to 1200° C. under normal pressure.
3. 3. The zirconia molded body according to claim 1, which has a transmittance of 40% or more for light with a wavelength of 700 nm at a thickness of 0.5 mm after sintering at 900 to 1200° C. under normal pressure.
4. The zirconia molded body according to any one of claims 1 to 3, wherein the ratio of monoclinic to tetragonal and cubic crystals is 5% or less after sintering at 900 to 1200°C under normal pressure and then immersing in hot water at 180°C for 5 hours.
5. ΔL at a thickness of 1.5 mm after sintering at 200 to 800° C. * The zirconia molded body according to any one of claims 1 to 4, wherein (W-B) is 5 or more.
6. A method for producing a calcined zirconia body, using the zirconia molded body according to any one of claims 1 to 5.
7. A method for producing the zirconia calcined body according to claim 6, comprising a step of calcining the zirconia molded body according to any one of claims 1 to 5 at 200 to 800°C.
8. A method for producing a zirconia sintered body using the zirconia molded body according to any one of claims 1 to 5.
9. The method for producing a zirconia sintered body according to claim 8, comprising a step of sintering the zirconia molded body at normal pressure at 900 to 1200 ° C.
Citation Information
Patent Citations
Light-transmitting zirconia sintered compact and its production method
JP2008214168A
Light-transmitting zirconia sintered compact, method for producing the same and use thereof
JP2010150064A
Sintered body of zirconia and method for manufacturing the same
JP2011073907A
Zirconia composition, zirconia calcinated body, zirconia sintered body and manufacturing zirconia sintered body and dental product
JP2016117618A
Method for producing zirconia molded body
JP2019026594A