Cushioning materials for batteries, dustproof cushioning materials, and waterproof cushioning materials
A polyurethane foam composition with controlled compressive load and hysteresis loss rate maintains cushioning properties across temperature variations, addressing the issue of property loss at low temperatures.
Patent Information
- Application Number
- JP2023522292
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-05-21
- Filing Date
- 2022-03-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-03-28
AI Technical Summary
Polyurethane foams used as cushioning materials lose their cushioning properties at low temperatures, posing a challenge for applications requiring wide temperature range performance.
A polyurethane foam composition is formulated with specific ratios of polyols and polyisocyanates, ensuring a compressive load ratio (P2/P1) of 180 or less at 25°C and -30°C, along with a glass transition point of -30°C or lower and a hysteresis loss rate of 15% or less, maintaining cushioning properties across temperature variations.
The foam maintains effective cushioning properties without significant hardness increase at low temperatures, ensuring suitability for applications like automotive batteries and electronic devices.
Smart Images

Figure 0007581504000007 
Figure 0007581504000001 
Figure 0007581504000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to polyurethane foams and cushioning materials. This application is based on Japanese Patent Application No. 2021-085926 filed on May 21, 2021, and claims the benefit of priority thereto, the entire contents of which are incorporated herein by reference. [Background technology]
[0002] Patent Document 1 discloses a cushioning material for batteries. This cushioning material for batteries has a foam obtained by foaming a foamable resin sheet containing an elastomer component and a foaming agent. Patent Document 2 also discloses a cushioning material for a battery. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-050841 A [Patent Document 2] JP 2020-139062 A Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, polyurethane foams are required to have various performance characteristics, and these requirements are becoming stricter. For example, polyurethane foams used as cushioning materials are expected to be used in a wide temperature range depending on the application. There is a demand for polyurethane foams that do not lose their cushioning properties in a wide temperature range, especially at low temperatures. An object of the present disclosure is to provide a polyurethane foam whose cushioning properties are not easily impaired at low temperatures. The present disclosure can be realized in the following forms. [Means for solving the problem]
[0005] [1] A polyurethane foam obtained from a composition containing polyols and polyisocyanates, If the 25% compressive load measured at 25°C is P1 (MPa) and the 25% compressive load measured at -30°C is P2 (MPa), (P2 / P1)×100≦180 Filled with polyurethane foam. Effect of the Invention
[0006] According to the present disclosure, it is possible to provide a polyurethane foam whose cushioning properties are not easily lost at low temperatures. [Brief description of the drawings]
[0007] [Figure 1] FIG. 2 is a diagram illustrating a cushioning material according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Here, a preferred example of the present disclosure is given.
[0009] [2] Polyurethane foam having a glass transition point of -30°C or lower.
[0010] [3] A polyurethane foam having a hysteresis loss rate of 15% or less.
[0011] [4] Regarding A calculated by the following formula (a), 1000≦A Filled with polyurethane foam.
number
[0012] [5] A cushioning material comprising the above-mentioned polyurethane foam.
[0013] The present disclosure will be described in detail below. In this specification, a description using "~" for a numerical range includes the lower limit and the upper limit unless otherwise specified. For example, the description "10 to 20" includes both the lower limit "10" and the upper limit "20". In other words, "10 to 20" has the same meaning as "10 or more and 20 or less".
[0014] 1.Polyurethane foam The polyurethane foam is obtained from a composition containing polyols and polyisocyanates. When a 25% compressive load measured under conditions of 25°C is P1 (MPa) and a 25% compressive load measured under conditions of -30°C is P2 (MPa), the polyurethane foam has the following properties: (P2 / P1)×100≦180 Meet the following.
[0015] [Polyols] The polyols are not particularly limited as long as they satisfy the above conditions. It is preferable that the polyols are a polyether polyol, a polymer polyol, and a polyester polyol.
[0016] The polyether polyol is preferably a polyether polyol having a weight average molecular weight of 1500 to 4500 (preferably 2000 to 4000) and three or two functional groups. The content of the polyether polyol is not particularly limited, and is preferably 30 parts by mass or more and 90 parts by mass or less, and more preferably 40 parts by mass or more and 85 parts by mass or less, relative to 100 parts by mass of the total amount of polyols.
[0017] The polymer polyol is more preferably a polymer polyol having a weight average molecular weight of 1500 to 4500 (preferably 2000 to 4000) and a functional number of 2 or 3. As the polymer polyol, for example, a polymer polyol obtained by graft copolymerizing a vinyl monomer such as acrylonitrile and styrene in a polyether polyol having a functional number of 2 or 3 as a base polyol can be suitably used. The weight average molecular weight of the polymer polyol means the weight average molecular weight of the base polyol.
[0018] The polymer content of the polymer polyol (the mass ratio of the portion other than the base polyol to the entire polymer polyol) is preferably 10 to 40 mass%, more preferably 15 to 30 mass%. From the viewpoint of improving the strength of the polyurethane foam, a larger polymer content is preferable, but if the polymer content is too large, the viscosity may increase and the workability may decrease. As the polymer polyol, only one type of polymer polyol may be contained, or two or more types of polymer polyols having different weight average molecular weights, polymer contents, functional groups, etc. may be used in combination. By using the polymer polyol, the hardness of the polyurethane foam can be improved.
[0019] The content of the polymer polyol is not particularly limited, and is preferably 5 parts by mass or more and 60 parts by mass or less, and more preferably 25 parts by mass or more and 45 parts by mass or less, based on 100 parts by mass of the total amount of polyols.
[0020] The polyester polyol is more preferably a polyester polyol having two functional groups. The weight average molecular weight of the polyester polyol is preferably in the range of 200 to 2500, preferably in the range of 250 to 1500, and more preferably in the range of 300 to 800. For example, polycaprolactone-based polyester polyols, adipate-based polyester polyols, etc. can be used as the polyester polyol. For example, polycaprolactone-based polyester polyols include polyester polyols obtained by ring-opening addition polymerization of lactones such as ε-caprolactone. For example, adipate-based polyester polyols include polyester polyols obtained by polycondensation of polyfunctional carboxylic acid and polyfunctional hydroxy compound. The strength of polyurethane foam can be improved by using polyester polyol. In addition, polyester polyols also have the effect of making the cells of polyurethane foam finer and more uniform.
[0021] The content of the polyester polyol is not particularly limited. The content of the polyester polyol is preferably 1 part by mass or more and 20 parts by mass or less, and more preferably 5 parts by mass or more and 15 parts by mass or less, based on 100 parts by mass of the total amount of polyols.
[0022] The polyol may contain other polyols in addition to the above polyols. The other polyols may be any polyol that is generally used in polyurethane foams without any particular limitation. In the present disclosure, when low molecular weight polyhydric alcohols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, 1,3-butanediol, 1,4-butanediol, glycerin, trimethylolpropane, pentaerythritol, and sorbitol are used, these polyhydric alcohols are also included in the polyols.
[0023] [Polyisocyanates] Polyisocyanates are compounds having a plurality of isocyanate groups, and examples thereof include aromatic isocyanates such as 4,4-diphenylmethane diisocyanate (MDI), tolylene diisocyanate (TDI), 1,5-naphthalene diisocyanate (NDI), triphenylmethane triisocyanate, and xylylene diisocyanate (XDI), alicyclic isocyanates such as isophorone diisocyanate (IPDI), and dicyclohexylmethane diisocyanate, and aliphatic isocyanates such as hexamethylene diisocyanate (HDI), and free isocyanate prepolymers obtained by reacting these with polyols, and modified isocyanates such as carbodiimide-modified isocyanates. These polyisocyanates may be contained alone or in combination of two or more.
[0024] The polyisocyanates may be any of aromatic, alicyclic, and aliphatic isocyanates, and may also be bifunctional isocyanates having two isocyanate groups in one molecule, or trifunctional or higher isocyanates having three or more isocyanate groups in one molecule, and these may be used alone or in combination. For example, bifunctional isocyanates include 2,4-tolylene diisocyanate (TDI), 2,6-tolylene diisocyanate (TDI), m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate (MDI), 2,4'-diphenylmethane diisocyanate (MDI), 2,2'-diphenylmethane diisocyanate (MDI), xylylene diisocyanate, 3,3'-dimethyl-4,4'-biphenylene diisocyanate, 3,4'-diphenylmethane diisocyanate, 3,5'-diphenylmethane diisocyanate, 3,6'-diphenylmethane diisocyanate, 3,7'-diphenylmethane diisocyanate, 3,8'-diphenylmethane diisocyanate, 3,9'-diphenylmethane diisocyanate, 3,10'-diphenylmethane diisocyanate, 3,11'-diphenylmethane diisocyanate, 3,12'-diphenylmethane diisocyanate, 3,13'-diphenylmethane diisocyanate, 3,14'-diphenylmethane diisocyanate, 3,15'-diphenylmethane diisocyanate, 3,16'-diphenylmethane diisocyanate, 3,17'-diphenylmethane diisocyanate, 3,18'-diphenylmethane diisocyanate, 3,19'-diphenylmethane diisocyanate, 3,20'-diphenylmethane diisocyanate, 3,21'-diphenylmethane diisocyanate, 3,22'-diphenylmethane diisocyanate, 3,23'-diphenylmethane diisocyanate, 3,24'-diphenylmethane diisocyanate, 3,25'-di Examples of the isocyanate include aromatic isocyanates such as 1,3'-dimethoxy-4,4'-biphenylene diisocyanate, alicyclic isocyanates such as cyclohexane-1,4-diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, and methylcyclohexane diisocyanate, and aliphatic isocyanates such as butane-1,4-diisocyanate, hexamethylene diisocyanate, isopropylene diisocyanate, methylene diisocyanate, and lysine isocyanate. Also, an example of a bifunctional or higher isocyanate is polymethylene polyphenylisocyanate (polymeric MDI). Examples of tri- or higher functional isocyanates include 1-methylbenzene-2,4,6-triisocyanate, 1,3,5-trimethylbenzene-2,4,6-triisocyanate, biphenyl-2,4,4'-triisocyanate, diphenylmethane-2,4,4'-triisocyanate, methyldiphenylmethane-4,6,4'-triisocyanate, 4,4'-dimethyldiphenylmethane-2,2',5,5'tetraisocyanate, and triphenylmethane-4,4',4"-triisocyanate. The number of isocyanates is not limited to one, and may be one or more. For example, one type of aliphatic isocyanate and two types of aromatic isocyanate may be used in combination. From the viewpoints of hardness and resilience, the number of functional groups of the polyisocyanates is preferably in the range of 2.0 to 2.8.
[0025] The isocyanate index (INDEX) of the polyisocyanates is preferably in the range of 90 to 110. The isocyanate index is the equivalent ratio of the isocyanate groups of the polyisocyanates to the reactive groups such as hydroxyl groups in the polyols that can react with isocyanate. Therefore, when the value is less than 100, it means that the reactive groups such as hydroxyl groups are in excess of the isocyanate groups, and when it exceeds 100, it means that the isocyanate groups are in excess of the reactive groups such as hydroxyl groups. When the isocyanate index is less than 90, there is a risk that the polyols will not be able to react sufficiently with the polyisocyanates. On the other hand, when the isocyanate index is more than 110, there is a risk that low resilience will be exhibited.
[0026] [Foam stabilizer] The foam stabilizer is used to facilitate the foaming of the composition, and the composition preferably contains the foam stabilizer. As the foam stabilizer, a known foam stabilizer that is usually used when the mechanical froth method is adopted, for example, a silicone-based foam stabilizer, can be used. Since such a foam stabilizer has a high viscosity, it is usually blended into the composition in a state diluted with a solvent such as alkylbenzene.
[0027] The content of the foam stabilizer in the composition is preferably 3 to 6 parts by mass per 100 parts by mass of polyols. If the content is 3 parts by mass or more, it can contribute to improving the uniformity of the cells and reducing the density of the polyurethane foam. Furthermore, even if the content exceeds 6 parts by mass, no significant improvement in foam stabilization can be expected. Furthermore, when the foam stabilizer is diluted with a solvent, the mass ratio (foam stabilizer:solvent) is preferably in the range of 25:75 to 75:25.
[0028] [catalyst] The catalyst is mainly for accelerating the urethane reaction between polyols and polyisocyanates, and the composition preferably contains a catalyst. As the catalyst, a known catalyst usually used in polyurethane foams, for example, tertiary amines such as triethylenediamine, dimethylethanolamine, and N,N',N'-trimethylaminoethylpiperazine, organometallic compounds such as stannous octoate and stannous octoate (tin octoate), acetates, and alkali metal alcoholates can be used.
[0029] The content of the catalyst in the composition is preferably 0.1 to 5.0 parts by mass relative to 100 parts by mass of the polyols. If the content is 0.1 parts by mass or more, the urethane reaction can be sufficiently promoted. If the content is 5.0 parts by mass or less, the formation of a cell structure that is not uniform due to excessive promotion of the urethane reaction can be suppressed.
[0030] [Other ingredients] The composition may contain other components other than those described above as necessary. Examples of other components include antioxidants, ultraviolet absorbers, thickeners, plasticizers, antibacterial agents, and colorants. Examples of antioxidants include dibutylhydroxytoluene and hindered phenol-based antioxidants, and from the viewpoint of reducing the content of volatile organic compounds, it is particularly preferable to use hindered phenol-based antioxidants with a molecular weight of 300 or more. Examples of thickeners include calcium carbonate, aluminum hydroxide, and magnesium hydroxide.
[0031] 2. Requirements for weight average molecular weight per hydroxyl group in polyols The polyurethane foam preferably satisfies 1000≦A, where A is calculated by the above formula (a). The polyurethane foam more preferably satisfies 1100≦A, and further preferably satisfies 1150≦A. The upper limit of A is not particularly limited. The polyurethane foam may, for example, satisfy A≦2300, where A is calculated by the above formula (a).
[0032] A calculated by formula (a) represents the weight average molecular weight per hydroxyl group in the polyols. When the polyols contain one type of polyol, the weight average molecular weight can be calculated by dividing the weight average molecular weight of the polyol by the number of hydroxyl groups per molecule of the polyol. When the polyols contain multiple types of polyols, the weight average molecular weight can be calculated by multiplying the weight average molecular weight of each polyol divided by the number of hydroxyl groups per molecule of each polyol by the content (mass%) of each polyol, and adding them together.
[0033] For example, in Example 2 (n=12) described later, A is calculated as 1194 from the following formula (a-1).
number
[0034] More preferably, the polyurethane foam satisfies 2400≦A×B, where A calculated by the above formula (a) and B calculated by the following formula (b).
number
[0035] B calculated by formula (b) represents the average number of functional groups of the polyisocyanates. When the polyisocyanates contain one type of polyisocyanate, it can be calculated as the number of functional groups of that type. When the polyisocyanates contain multiple types of polyisocyanates, it can be calculated by multiplying the number of functional groups of each polyisocyanate by the content (mass%) of each polyisocyanate and adding these together.
[0036] For example, in Example 2 (m=2) described later, B is calculated to be 2.4 from the following formula (b-1).
number
[0037] Multiplying A and B gives the weight average molecular weight of the polyols per one isocyanate molecule. A×B being equal to or greater than a predetermined value is an indicator that the weight average molecular weight of the polyols per one isocyanate molecule is equal to or greater than a predetermined value. If the weight average molecular weight of the polyols per one isocyanate molecule is equal to or greater than a predetermined value, the cushioning properties at low temperatures can be favorably maintained. For example, in Example 2 described below, the value of A×B is calculated as 2866 from the formula 1194×2.4.
[0038] The value of A×B may be 2500 or more, 2600 or more, or 2700 or more. The value of A×B is usually 5000 or less, and may be 4500 or less, 4000 or less, or 3500 or less.
[0039] 3. Physical properties of polyurethane foam For polyurethane foam, the 25% compressive load measured at 25°C is P1 (MPa), and the 25% compressive load measured at -30°C is P2 (MPa). (P2 / P1)×100≦180 Meet the following.
[0040] The compressive load under each temperature condition can be measured as follows, based on JIS K 6254:2010. [Measurement method] The test piece is cylindrical with a diameter of 50 mm. There are three test pieces. For the measurement, a compression tester is used in which the CLD (Compression-Load-Deflection) measuring jig attached to the test piece contacts the test piece, and at the same time, the load cell detects the rebound force from the compressed test piece and records it continuously. The test piece is compressed at a rate of 1.0 mm / min until it reaches 30% strain, and the relationship between the compression force and deflection (compression force-deformation curve) is recorded. From the recorded compression force-deformation curve, the compression force at which the deflection is 25% (25% compression force) is determined relative to the thickness of the test piece before compression. The 25% compression load is calculated using the following formula. 25% compressive load [MPa] = 25% compressive force [N] / test piece area [mm 2 ]
[0041] The above P2 / P1 value is an index that indicates the rate of increase in the hardness of a polyurethane foam when it is cooled from room temperature to -30° C. A P2 / P1 value of 100 means that the 25% compressive load is the same at 25° C. (room temperature) and -30° C., meaning that the hardness does not increase at low temperatures. The value of P2 / P1 may be 160 or less, 140 or less, 120 or less, or 110 or less. The value of P2 / P1 is usually 95 or more, and may be 98 or more, or 100 or more.
[0042] The 25% compressive load P1 measured under the condition of 25° C. is preferably 0.005 MPa or more and 1 MPa or less, more preferably 0.01 MPa or more and 0.75 MPa or less, and further preferably 0.1 MPa or more and 0.5 MPa or less. The 25% compressive load P2 measured under conditions of -30°C is preferably 0.005 MPa or more and 1 MPa or less, more preferably 0.01 MPa or more and 0.75 MPa or less, and further preferably 0.1 MPa or more and 0.5 MPa or less.
[0043] In addition to the above, the physical properties of the polyurethane foam can be appropriately set depending on the application, etc. The polyurethane foam preferably has the following physical properties.
[0044] The glass transition point of the polyurethane foam is preferably −25° C. or lower, more preferably −30° C. or lower, and more preferably −35° C. or lower. The lower limit of the glass transition point of the polyurethane foam is not particularly limited, but is usually −100° C. or higher. In the present disclosure, the glass transition point is defined as the temperature at which a peak value of tan δ is obtained when viscoelasticity is measured under conditions of a frequency of 1 Hz and a temperature rise rate of 3° C. / min.
[0045] The hysteresis loss rate of the polyurethane foam, when measured by the following measurement method, is preferably 15% or less, more preferably 10% or less, and even more preferably 8% or less. The lower limit of the hysteresis loss rate is not particularly limited, but is usually 1% or more.
[0046] The hysteresis loss rate can be measured as follows based on JIS K 6254:2010. [Measurement method] The test piece shall be cylindrical with a diameter of 50 mm. There shall be three test pieces. For the measurement, a compression tester shall be used in which the CLD measurement tool attached to the test piece contacts the test piece, and at the same time, the load cell detects the rebound force from the compressed test piece and records it continuously. The test piece is compressed at a speed of 1.0 mm / min until it reaches 50% strain, and then the jig is returned at the same speed of 1.0 mm / min until the test piece returns to 0% strain. The relationship between the compression force and the deflection (compression force-deformation curve) is recorded. The hysteresis loss rate is calculated from the recorded compression force-deformation curve using the same calculation method as JIS K 6400-2.
[0047] The apparent density of polyurethane foam (JIS K7222) is 100kg / m 3 ~900kg / m 3 is preferred, and 200 kg / m 3 ~800kg / m3 More preferably, 300 kg / m 3 ~700kg / m 3 If the apparent density is within the above range, suitable cushioning properties can be ensured when used as the cushioning material 10 described below.
[0048] The average cell diameter of the polyurethane foam is preferably 50 μm to 300 μm, more preferably 50 μm to 200 μm, and even more preferably 50 μm to 100 μm. If the cell diameter is within the above range, suitable cushioning properties can be ensured, and it is also preferable in terms of heat insulation. The average cell diameter of a polyurethane foam can be calculated by dividing the cumulative cell diameters of cells that contact a 25 mm straight line when the cross section of the polyurethane foam is observed under a scanning electron microscope (SEM) at a magnification of 200 times by the number of cells.
[0049] 4. Manufacturing method of polyurethane foam The polyurethane foam can be produced by a general polyurethane foam production method used when the mechanical froth method is adopted. For example, the above composition is charged into a mixing head, and then stirred and mixed to homogeneity while mixing inert gas. The composition mixed in the mixing head is then heated and cured on a release paper or in a predetermined mold to obtain a polyurethane foam. In order to form a foam of a desired density, the amount of inert gas stirred into the composition is controlled by a gas flow meter. Increasing the amount of cell-forming inert gas decreases the density, and decreasing the amount of inert gas increases the density. As the inert gas, a gas that is a gas under ambient conditions and is substantially inert or does not react at all with any component in the liquid phase can be used as necessary. Examples include nitrogen, carbon dioxide, and dry air, which is a dried normal gas.
[0050] 5. Cushioning material 10 Polyurethane foam is suitable as a cushioning material because it has moderate flexibility and a low hysteresis loss rate. Polyurethane foam is particularly suitable as a cushioning material used for vehicle-mounted parts, for example, a cushioning material for batteries such as lithium-ion batteries, because its cushioning properties are not easily lost at low temperatures. In addition, polyurethane foam is suitable as a cushioning material used in electronic devices and sensor parts because it has small changes in properties such as hardness over a wide temperature range from low to high temperatures and has high responsiveness. Note that high responsiveness can be achieved, for example, by reducing the hysteresis loss rate.
[0051] FIG. 1 illustrates a cushioning material 10 with polyurethane foam. The cushioning material 10 is disposed between a plurality of cells C, C stacked together. Although FIG. 1 illustrates two cells C, C and one cushioning material 10, the number of cells and cushioning materials is arbitrary. Each cell C may expand and contract when the battery is charged and discharged. The cushioning material 10 of this embodiment has high responsiveness, and can be compressed with the expansion of the cell C and restored with the contraction of the cell C. The cushioning material 10 follows the expansion and contraction of the cells C, C and fixes the cells C, C so that they do not move within the battery housing. Batteries, particularly batteries (e.g., lithium ion batteries) mounted on vehicles are expected to be used in a wide temperature range (e.g., -30°C to 60°C), and the cushioning material 10 is also required to have characteristics such as hardness that are unlikely to change over a wide temperature range. The polyurethane foam of the present disclosure has a 25% compressive load that does not change significantly between 25°C and -30°C, and therefore can fix each cell C, C by following the expansion and contraction of cells C, C even in a low temperature environment, for example.
[0052] The thickness of the cushioning material 10 is not particularly limited. From the viewpoint of conformity to the cells C, C, the thickness of the cushioning material 10 is preferably 0.5 mm to 6 mm, more preferably 1 mm to 5 mm, and even more preferably 2 mm to 3 mm. From the viewpoint of controlling the surface pressure of the block-shaped cells C, C, the size of the cushioning material 10 is preferably approximately the same as or slightly smaller than the opposing surfaces of the adjacent cells C, C. From the viewpoint of formability, the cushion material 10 can be obtained by punching out a polyurethane foam molded into a sheet in the thickness direction.
[0053] The polyurethane foam can be used for various purposes, not limited to cushioning materials, such as electronic device parts for mobile phones, cameras, televisions, etc., vehicle-mounted parts for batteries, vehicle lighting devices, vehicle display devices, etc., waterproof and dustproof sealants for toner cartridges, etc.
[0054] 6. Functions and Effects of the Present Embodiment In recent years, polyurethane foams are required to have various performance characteristics, and these requirements are becoming stricter. For example, the battery cushioning material 10 is required to be able to follow the expansion and contraction of cells over a wide temperature range from low to high. In particular, polyurethane foams that can maintain their cushioning properties (following properties) at low temperatures are required.
[0055] The polyurethane foam of this embodiment is less likely to lose its cushioning properties at low temperatures. Unlike this embodiment, conventional cushioning materials using polyurethane foam have a high glass transition point and therefore cannot ensure cushioning properties in a low-temperature environment. On the other hand, the cushioning material 10 using the polyurethane foam of this embodiment shows only a small increase in hardness even in a low-temperature environment. Therefore, the cushioning material 10 can ensure cushioning properties in a low-temperature environment.
[0056] The polyurethane foam of the present embodiment has a small hysteresis loss rate, and therefore can adequately follow the displacement of the surrounding members such as the cells C and exhibit suitable cushioning properties. EXAMPLES
[0057] Next, the above embodiment will be described more specifically with reference to examples and comparative examples. 1. Polyurethane foam production First, the raw material components of the compositions used in the polyurethane foams of each Example and Comparative Example are shown below. Polymer polyol 1: Polymer polyol having a weight average molecular weight of 3,000, functionality of 3, hydroxyl value of 42 mgKOH / g, polymer content of 22.9% by mass, EO content of 0%, and PO content of 100%. Polymer polyol 2: Polymer polyol having a weight average molecular weight of 3,000, functionality of 2, hydroxyl value of 28.6 mgKOH / g, polymer content of 20.0 mass%, EO content of 10%, and PO content of 90%. Polyether polyol 1: Polyether polyol having a weight average molecular weight of 3,000, functionality of 2, hydroxyl value of 37.4 mg KOH / g, EO content of 10%, and PO content of 90%. Polyether polyol 2: Polyether polyol having a weight average molecular weight of 3,000, functionality of 3, hydroxyl value of 56.1 mgKOH / g, EO content of 0%, and PO content of 100%. Polyether polyol 3: Polyether polyol having a weight average molecular weight of 3,000, functionality of 3, hydroxyl value of 56.1 mgKOH / g, EO content of 0%, and PO content of 100%. Polyether polyol 4: Polyether polyol having a weight average molecular weight of 3,000, functionality of 3, hydroxyl value of 56.1 mgKOH / g, EO content of 7%, and PO content of 93%. Polyether polyol 5: Polyether polyol having a weight average molecular weight of 3,400, functionality of 3, hydroxyl value of 50.3 mgKOH / g, EO content of 80%, and PO content of 20%. Polyether polyol 6: Polyether polyol having a weight average molecular weight of 2000, functionality of 2, hydroxyl value of 56.1 mgKOH / g, EO content of 0%, and PO content of 100%. Polyether polyol 7: Polyether polyol having a weight average molecular weight of 400, functionality of 2, hydroxyl value of 280.5 mg KOH / g, EO content of 0%, and PO content of 100%. Polyester polyol: polycaprolactone diol having a weight average molecular weight of 529, a functionality of 2, and a hydroxyl value of 212 mgKOH / g. The EO content and PO content are 0%. Other polyols 1: Dipropylene glycol having a molecular weight of 134, a functionality of 2, and a hydroxyl value of 837 mg KOH / g. The EO content and PO content are 0%. Other polyols 2: 2-methyl-1,3-propanediol having a molecular weight of 90, a functionality of 2, and a hydroxyl value of 1245 mg KOH / g. The EO content and PO content are 0%. Aluminum hydroxide (Sumitomo Chemical Co., Ltd., CW-325LV) Foam stabilizer: Silicone foam stabilizer (Toray Dow Corning, SZ-1952) Catalyst 1: Iron catalyst (manufactured by Nippon Chemical Industries, Ltd., FIN-P1) Catalyst 2: Nickel catalyst (Momentive Performance Materials Japan, LC-5615) Antioxidant: Hindered phenol-based antioxidant (BASF Japan, IRGANOX 1135) Moisture absorbent: Zeolite (Molecular sieve 3APOWDER, manufactured by Union Showa Co., Ltd.) Isocyanate 1: Polymeric MDI with molecular weight of 320, functionality of 2.4, and NCO% of 31.5% Isocyanate 2: Carbodiimide-modified MDI with molecular weight of 292, functionality of 2, and NCO% of 30.88% The numerical values of each component in Tables 1 and 2 represent parts by mass. The "F" column in Tables 1 and 2 indicates the number of hydroxyl groups for polyols and the number of isocyanate groups for polyisocyanates. The "Mw" column in Tables 1 and 2 indicates the weight average molecular weight.
[0058] The above components were mixed in the proportions shown in Tables 1 and 2 below to obtain compositions for each Example and Comparative Example. The composition was then placed in a mixing head and stirred to homogenize while mixing in an inert gas (nitrogen) in the range of 69 to 77% by volume. The mixed composition was then fed onto a continuously fed film of a given thickness and heat cured at 120 to 200°C to obtain a sheet-like polyurethane foam.
[0059] [Table 1]
[0060] 2. Observation of polyurethane foam The cross section of the sheet of each of the Examples and Comparative Examples was observed using an SEM. The average cell diameter of the polyurethane foam of each of the Examples was 50 μm or more and 300 μm or less.
[0061] 3. Evaluation Next, the polyurethane foams obtained in each of the Examples and Comparative Examples were evaluated as follows.
[0062] [Weight average molecular weight per hydroxyl group in polyol: A] In this example, 10 types of polyols were used, and "n=12" in the above formula (a) including the two types used only in the comparative example. A was calculated based on the above formula (a). The results are shown in the "Average molecular weight per hydroxyl group in polyol: A" column in Table 2. [Weight average molecular weight of polyols per isocyanate molecule: A x B] In this example, two types of polyisocyanates are used, and "m=2" in the above formula (b). B was calculated based on the above formula (b). In Comparative Example 1, B is 2. In Comparative Examples 2 to 4 and the Example, B is 2.4. A and B were multiplied to calculate the value of A×B. The results are shown in the "Average molecular weight per isocyanate molecule" column in Table 2.
[0063] [Glass transition temperature] The glass transition temperature (° C.) was measured by the method described in the embodiment. The measurement results are shown in the “Glass transition temperature” column of Table 2. [density] According to JIS K7222, apparent density (kg / m 3 The measurement results are shown in the "Density" column of Table 2. [Amount of inert gas mixed into the composition] The amount of inert gas (volume %) was calculated assuming that the specific gravity of the composition was 1 and the total volume of the composition and the volume of the mixed inert gas was 100 volume %. For example, in Example 5, the amount of inert gas mixed into the composition of 35 volume % indicates that 35 mL of inert gas was mixed into 65 g of the composition prepared at the blending ratio shown in Table 1. The calculation results are shown in the column of "Amount of inert gas mixed into the composition" in Table 2. [25% compression load at 25℃: P1] Using the method described in the embodiment, the 25% compressive load (MPa) was measured at 25° C. The measurement results are shown in the column of "25% compressive load at 25° C." [25% compression load at -30℃: P2] Using the method described in the embodiment, the 25% compressive load (MPa) was measured at −30° C. The measurement results are shown in the column of “25% compressive load at −30° C.” in Table 2. [Hardness increase rate: P2 / P1×100] The hardness increase rate P2 / P1×100(%) was calculated based on the 25% compressive load P1 at 25° C. and the 25% compressive load P2 at −30° C. The measurement results are shown in the “Hardness increase rate” column in Table 2 and were evaluated according to the following criteria. "A": P2 / P1×100≦180 "B": 180 <P2 / P1×100≦250 "C": 250 <P2 / P1×100 [Hysteresis loss rate] The hysteresis loss rate (%) was measured by the method described in the embodiment. The measurement results are shown in the "Hysteresis loss rate" column in Table 2, and were evaluated according to the following criteria. "A": Hysteresis loss rate is 15% or less "B": Hysteresis loss rate is greater than 15%
[0064] [comprehensive evaluation] "A": The hardness increase rate is rated as A, and the hysteresis loss rate is rated as A. "B": The hardness increase rate is rated as B or C, or the hysteresis loss rate is rated as B.
[0065] [Table 2]
[0066] 4.Results In Examples 1 to 4, the hardness increase rate was rated A, and P2 / P1×100≦180 was satisfied. In Comparative Examples 1 to 4, the hardness increase rate was rated B or C, and P2 / P1×100≦180 was not satisfied. Examples 1 to 4 had a higher overall rating than Comparative Examples 1 to 4. In Examples 1 to 4, cushioning properties were less likely to be impaired at low temperatures. In Examples 1 to 4, the hysteresis loss rate was evaluated as A, and compared with Comparative Examples 1, 2 and 4, the cushioning property (conformity) was good.
[0067] The following invention can also be understood from the above examples and comparative examples. The above descriptions are appropriately cited in the following description of the specific aspects of the invention. A polyurethane foam obtained from a composition containing polyols and polyisocyanates, the polyurethane foam satisfying the following conditions: Regarding A calculated by the above formula (a) and B calculated by the above formula (b), Satisfy 2400≦A×B.
[0068] 5. Effects of the embodiment According to the above-mentioned examples, a polyurethane foam whose cushioning properties are not easily lost at low temperatures can be provided.
[0069] The present disclosure is not limited to the above-described embodiments, and various modifications and variations are possible within the scope of the claims of the present disclosure. [Explanation of symbols]
[0070] 10: Cushioning material C: Cell
Claims
1. The 25% compressive load measured under conditions of 25°C is P1 (MPa), When the 25% compressive load measured under conditions of -30 ° C is P2 (MPa), (P2 / P1)×100≦180 Cushioning for batteries with polyurethane foam that fills the space.
2. The 25% compressive load measured under conditions of 25°C is P1 (MPa), When the 25% compressive load measured under conditions of -30 ° C is P2 (MPa), (P2 / P1)×100≦180 Dust-proof cushioning with polyurethane foam that fills the space.
3. The 25% compressive load measured under conditions of 25°C is P1 (MPa), When the 25% compressive load measured under conditions of -30 ° C is P2 (MPa), (P2 / P1)×100≦180 Fulfilling The apparent density is 100 kg / m 3 or more and 900 kg / m 3 or less. Water-stopping cushioning material made of polyurethane foam.
Citation Information
Patent Citations
Production of sheet cushion material for snow mobile
JP1997176274A
Speaker edge made of foamed polyurethane
JP1999008897A
Method for producing low resilience polyurethane foam
JP2004300352A
Composition for polyurethane foam, polyurethane foam obtained from the composition and its application
JP2006002145A
Polyurethane foam
JP2006124578A