3D laminated object modeling device and 3D laminated object modeling method

The three-dimensional laminate manufacturing device improves flow rate controllability by using a linearly moving piston to control molten resin discharge, addressing the limitations of simultaneous extruder and gear pump control, ensuring consistent bead dimensions and efficient resin discharge.

JP7585938B2Active Publication Date: 2024-11-19TOYOTA JIDOSHA KK
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021058212
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-30
Publication Date
2024-11-19
Estimated Expiration
2041-03-30

AI Technical Summary

Technical Problem

Existing devices for controlling the flow rate of molten resin require simultaneous control of both the extruder screw and gear pump, leading to poor controllability.

Method used

A three-dimensional laminate manufacturing device that controls the flow rate of molten resin by using a piston that moves linearly within a cylinder, allowing independent control of the piston's movement based on the speed of the discharge nozzle, thereby simplifying the control process and improving controllability.

Benefits of technology

This approach enhances the controllability of the flow rate of molten resin, ensuring consistent bead dimensions and preventing residual discharge, while eliminating the need for separate mechanisms for plasticization and flow rate control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585938000002
    Figure 0007585938000002
  • Figure 0007585938000003
    Figure 0007585938000003
  • Figure 0007585938000004
    Figure 0007585938000004
Patent Text Reader

Abstract

To provide a three-dimensionally laminated object modeling apparatus and the like, which is capable of improving a control property of a flow rate of a molten resin discharged from a discharging nozzle.SOLUTION: There is provided a three-dimensionally laminated object modeling apparatus that comprises: cylinders 11 and 12 configured to store a molten resin; a discharging nozzle 18 that is connected to the cylinders; and pistons 14 and 15 configured to discharge the molten resin from the discharging nozzle by moving in a direction of approaching the discharging nozzle and by pressurizing the molten resin in the cylinders. The three-dimensionally laminated object modeling apparatus models a three-dimensionally modeled object Ob1 by laminating a resin bead that is the molten resin discharged from the discharging nozzle on a table 4, and comprises: a moving unit configured to relatively move the discharging nozzle with respect to the table; an acquisition unit that acquires a movement speed of the discharging nozzle; and a piston control unit configured to control movement of the pistons, in which the piston control unit controls movement of the piston based on the movement speed of the discharging nozzle.SELECTED DRAWING: Figure 37
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a three-dimensional laminated object modeling apparatus and a three-dimensional laminated object modeling method. [Background technology]

[0002] An apparatus has been proposed that includes an extruder (screw) and a gear pump arranged in series, and controls the flow rate of molten resin discharged from a discharge nozzle by adjusting the molten resin (fluid material) sent from the extruder (screw) located upstream using the gear pump (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] US Patent Application Publication No. 2018 / 0056602 Summary of the Invention [Problem to be solved by the invention]

[0004] However, in the device described in Patent Document 1, in order to control the flow rate of the molten resin, the rotations of both the extruder (screw) and the gear pump must be controlled simultaneously, which poses a problem of poor controllability.

[0005] The present invention has been made to solve these problems, and provides a three-dimensional laminate modeling device and a three-dimensional laminate modeling method that can improve the controllability of the flow rate of molten resin discharged from the discharge nozzle. [Means for solving the problem]

[0006] The three-dimensional laminate modeling apparatus according to the present invention comprises: A cylinder for storing molten resin; A discharge nozzle communicating with the cylinder; a piston that performs linear reciprocating motion within the cylinder, the piston moving in a direction approaching the discharge nozzle to pressurize the molten resin within the cylinder, thereby discharging the molten resin from the discharge nozzle; and a three-dimensional laminated object printing device that forms a three-dimensional object by layering resin beads, which are the molten resin discharged from the discharge nozzle, on a table, the device comprising: a moving unit that moves the discharge nozzle relatively to the table; An acquisition unit that acquires a moving speed of the discharge nozzle; A piston control unit that controls the movement of the piston, The piston control unit controls the movement of the piston based on the movement speed of the discharge nozzle.

[0007] With this configuration, it is possible to improve the controllability of the flow rate of the molten resin discharged from the discharge nozzle.

[0008] This is because the flow rate of the molten resin is controlled by controlling the movement of a piston that moves back and forth in a straight line inside a cylinder in which the molten resin is stored, rather than by controlling the rotation of both the extruder (screw) and the gear pump (simplification of flow rate control).

[0009] The piston control unit may control a moving speed of the piston based on a moving speed of the discharge nozzle so that a size of the resin bead is constant.

[0010] In this way, the dimensions of the resin bead can be controlled to be constant (approximately constant) by controlling the movement speed of the piston that moves back and forth linearly within the cylinder in which the molten resin is stored, based on the movement speed of the discharge nozzle.

[0011] Further, a space in the cylinder on the opposite side of the piston from the discharge nozzle is a resin raw material supply chamber to which the resin raw material is supplied, a space in the cylinder on the discharge nozzle side with respect to the piston is a plasticization chamber that stores the molten resin, The piston may move in a direction away from the discharge nozzle to plasticize the resin raw material supplied to the resin raw material supply chamber and store the molten resin, which is the plasticized resin raw material, in the plasticization chamber, and move in a direction approaching the discharge nozzle to pressurize the molten resin stored in the plasticization chamber, thereby discharging the molten resin stored in the plasticization chamber from the discharge nozzle.

[0012] In this way, the resin raw material is plasticized and stored, and then the stored molten resin is pressurized by a single piston that moves linearly back and forth, thereby discharging the molten resin from the discharge nozzle. This improves controllability compared to Patent Document 1, in which the rotations of both the extruder (screw) and the gear pump are controlled simultaneously. In addition, the plasticization of the resin raw material (generation and storage of molten resin) and the control of the flow rate of the stored molten resin can be performed by a single piston that moves linearly back and forth. In addition, since the plasticization of the resin raw material and the control of the flow rate of the stored molten resin can be performed by a single piston, there is no need to provide a separate mechanism for plasticizing the resin raw material.

[0013] The piston control unit may control the moving speed of the piston so that the flow rate of the molten resin discharged from the discharge nozzle becomes equal to the moving speed of the discharge nozzle multiplied by the cross-sectional area of ​​the resin bead.

[0014] In this way, the size of the resin bead can be controlled to be constant (approximately constant).

[0015] The apparatus may further include a temperature control unit that controls the temperature of the molten resin stored in the cylinder.

[0016] In this way, the temperature of the molten resin stored in the cylinder can be controlled to a temperature suitable for the molten resin (a temperature at which the molten state is maintained without being overheated).

[0017] a flow rate prediction unit that predicts a flow rate of the molten resin discharged from the discharge nozzle; a discharge nozzle control unit for controlling movement of the discharge nozzle, The discharge nozzle control unit may control the moving speed of the discharge nozzle by controlling the moving unit based on the predicted discharge flow rate so that the size of the resin bead is constant.

[0018] In this way, the moving speed of the discharge nozzle can be controlled based on the predicted discharge flow rate, thereby making it possible to control the size of the resin bead to be constant (approximately constant).

[0019] In addition, the discharge nozzle control unit may control the moving speed of the discharge nozzle by controlling the moving unit so that the moving speed of the discharge nozzle becomes the predicted discharge flow rate / cross-sectional area of ​​the resin bead.

[0020] In this way, the size of the resin bead can be controlled to be constant (approximately constant).

[0021] The piston control unit may control the piston so that the piston moves a predetermined amount in a direction away from the discharge nozzle at a predetermined timing.

[0022] In this way, by controlling the piston so that it moves a predetermined amount in a direction away from the discharge nozzle at a predetermined timing, the discharge pressure can be made negative (for example, a pressure lower than the outside air pressure). This makes it possible to prevent the molten resin from being continuously discharged due to residual pressure, gravity, etc. As a result, the dimensions of the resin bead can be controlled to be constant (approximately constant).

[0023] The predetermined timing may be a timing when the moving speed of the discharge nozzle changes from a value other than 0 to 0.

[0024] In this way, the discharge pressure can be made negative (for example, a pressure lower than the outside air pressure) at the timing when the moving speed of the discharge nozzle changes from a speed other than 0 to 0 (at the timing when the moving discharge nozzle stops).

[0025] The predetermined amount may be an amount at which the resin pressure inside the discharge nozzle is lower than the resin pressure outside the discharge nozzle.

[0026] In this way, the resin pressure inside the discharge nozzle becomes lower than the resin pressure outside the discharge nozzle, so that the molten resin can be prevented from continuing to be discharged due to residual pressure, gravity, and the like.

[0027] The predetermined timing may be a timing a predetermined time before the timing at which the movement speed of the discharge nozzle is predicted to change from a speed other than 0 to 0.

[0028] In this way, the discharge pressure can be made negative (e.g., a pressure lower than the outside air pressure) for a predetermined time before the timing when the movement speed of the discharge nozzle is predicted to change from a value other than 0 to 0 (the moving discharge nozzle stops).

[0029] The predetermined amount may be an amount at which the resin pressure inside the discharge nozzle is lower than the resin pressure outside the discharge nozzle.

[0030] In this way, the resin pressure inside the discharge nozzle becomes lower than the resin pressure outside the discharge nozzle, so that the molten resin can be prevented from continuing to be discharged due to residual pressure, gravity, and the like.

[0031] The predetermined time may be a time required for the piston to move the predetermined amount.

[0032] In this way, it is possible to prevent the molten resin from continuing to be discharged due to residual pressure, gravity, etc. at the same timing when the movement speed of the discharge nozzle changes from a non-zero value to 0 (the timing when the moving discharge nozzle stops) (the flow rate of molten resin discharged from the discharge nozzle can be made 0 (zero)).

[0033] The speed at which the piston moves in the direction away from the discharge nozzle may be a speed at which air does not flow from the resin raw material supply chamber into the plasticization chamber.

[0034] This makes it possible to prevent air from entering the plasticizing chamber.

[0035] a check ball disposed between the plasticizing chamber and the discharge nozzle, the check ball being positioned at an open position for opening a flow path of the molten resin that communicates between the plasticizing chamber and the discharge nozzle, or at a closed position for closing the flow path; an elastic member that positions the check ball at the closed position by an elastic force, The check ball may move from the closed position to the open position while elastically deforming the elastic member when the piston moves in a direction approaching the discharge nozzle and the pressure pressurizing the molten resin in the cylinder exceeds a predetermined pressure, and when the piston moves in a direction away from the discharge nozzle, the check ball may move from the open position to the closed position due to a restoring force that returns the elastic member to its shape before elastic deformation.

[0036] In this way, the check ball automatically moves to the open or closed position in response to the movement of the piston reciprocating linearly within the cylinder, thereby connecting the multiple cylinders to the discharge nozzle. When molten resin in one cylinder is discharged from the discharge nozzle, it is possible to prevent the molten resin from flowing back into the other cylinder.

[0037] In addition, the piston control unit may be configured to control the piston to move a predetermined amount in a direction away from the discharge nozzle while the outlet of the discharge nozzle and the three-dimensional object are fluidly connected, thereby sucking up the uncured resin bead from the three-dimensional object.

[0038] This makes it possible to suck up uncured resin beads that have been layered on the three-dimensional object (for example, resin beads in the overlapping portions of resin beads). As a result, the dimensions of the resin beads can be controlled to be constant (approximately constant).

[0039] Also, a plurality of combinations of the cylinder and the piston may be provided.

[0040] In this way, the molten resin can be discharged continuously without interruption.

[0041] In addition, the three-dimensional laminate modeling method according to the present invention includes the steps of: A cylinder for storing molten resin; A discharge nozzle communicating with the cylinder; a piston that performs linear reciprocating motion within the cylinder, the piston moving in a direction approaching the discharge nozzle to pressurize the molten resin within the cylinder, thereby discharging the molten resin from the discharge nozzle, and a three-dimensional object printing method for a three-dimensional laminated object printing device that forms a three-dimensional object by layering resin beads, which are the molten resin discharged from the discharge nozzle, on a table, comprising: The three-dimensional laminate modeling apparatus further includes a moving unit that moves the discharge nozzle relatively to the table, An acquisition step of acquiring a moving speed of the discharge nozzle; A piston control step of controlling the movement of the piston, The piston control step controls the movement of the piston based on a moving speed of the discharge nozzle.

[0042] a flow rate prediction step of predicting a flow rate of the molten resin discharged from the discharge nozzle; A discharge nozzle control step of controlling the movement of the discharge nozzle, The discharge nozzle control step may include controlling a moving speed of the discharge nozzle by controlling the moving unit based on the predicted discharge flow rate so that a diameter of the resin bead is constant.

[0043] The piston control step may include controlling the moving section so that the piston moves a predetermined amount in a direction away from the discharge nozzle at a predetermined timing. Effect of the Invention

[0044] The present invention can provide a three-dimensional laminated object modeling device and a three-dimensional laminated object modeling method that can improve the controllability of the flow rate of molten resin discharged from a discharge nozzle. [Brief description of the drawings]

[0045] [Figure 1] FIG. 1 is a diagram illustrating an injection molding apparatus according to a first embodiment. [Diagram 2] FIG. 2 is a block diagram of a control system of the injection molding apparatus of the first embodiment. [Diagram 3] FIG. 2 is an enlarged view showing a portion on the negative side of the Z axis of the injection molding machine according to the first embodiment. [Figure 4] FIG. 4 is a cross-sectional view taken along line IV-IV of FIG. [Diagram 5] FIG. 2 is a cross-sectional view taken along the line VV in FIG. [Figure 6] 6 is a cross-sectional view taken along the line VI-VI in FIG. [Figure 7] FIG. 2 is a perspective view showing a first piston unit and a second piston unit according to the first embodiment. [Figure 8] FIG. 2 is an exploded view showing a first piston unit and a second piston unit according to the first embodiment. [Figure 9] 5A to 5C are diagrams illustrating the operation of the injection molding apparatus according to the first embodiment. [Figure 10] 5A to 5C are diagrams illustrating the operation of the injection molding apparatus according to the first embodiment. [Figure 11] 5A to 5C are diagrams illustrating the operation of the injection molding apparatus according to the first embodiment. [Figure 12] 5A to 5C are diagrams illustrating the operation of the injection molding apparatus according to the first embodiment. [Figure 13] 5A to 5C are diagrams illustrating the operation of the injection molding apparatus according to the first embodiment. [Figure 14] FIG. 11 is a configuration diagram of an injection molding machine 2A according to a second embodiment. [Figure 15] FIG. 11 is a configuration diagram of a control device 7A according to a second embodiment. [Figure 16] (a) Graph showing the relationship between nozzle movement speed and indicated flow rate (when the nozzle diameter is 1 mm and the cylinder diameter is 20 mm), (b) another graph showing the relationship between nozzle movement speed and indicated flow rate (when the nozzle diameter is 12 mm and the cylinder diameter is 100 mm). [Figure 17] This is an example (representative example) of a power exponent. [Figure 18] (a) is an example of a table of calculated bulk modulus values, and (b) is a graph plotting FIG. 18(a). [Figure 19] This is a concrete example of converting the relationship between pressure and flow rate into the relationship between shear rate and melt viscosity (resin name: ABS, temperature: 210°C). [Figure 20] 20 is a graph plotting "shear rate" and "melt viscosity" in FIG. 19. [Figure 21] 13 is a flowchart of an example of the operation of a target pressure calculation unit 31A. [Figure 22] 13 is a flowchart of an operation example (torpedo movement speed feedforward control) of a movement speed calculation unit 32A. [Diagram 23] FIG. 1 is a schematic diagram illustrating each element of Equation 10. [Figure 24] FIG. 1 is a schematic diagram illustrating each element in formulas 12 to 15. [Diagram 25] 13 is a flowchart of an example of operation from the second cycle onward of ejection. [Figure 26] FIG. 1 is a schematic diagram illustrating each element in formulas 18 and 19. [Figure 27] 1 is a flowchart common to the first and second embodiments of flow rate control. [Figure 28] 1 is a table summarizing the simulation results (1st to 3rd cycles) of Example 1. [Figure 29] 1 is a table summarizing the simulation results (1st to 3rd cycles) of Example 2. [Diagram 30] FIG. 11 is a configuration diagram of a control device 7B according to a third embodiment. [Diagram 31] 13 is a flowchart of an operation example (automatic stop determination and defect occurrence determination logic) of the abnormality detection unit 35A. [Diagram 32] 13 is a flowchart of another operation example (automatic stop determination and defect occurrence determination logic) of the abnormality detection unit 35A. [Diagram 33] 1 is a flowchart of an embodiment of a method for recording predicted positions of modeling defects when used in a 3D printer. [Diagram 34] 1 is a table summarizing the results of Example 3 (cycles 1 to 6). [Diagram 35] 13 is an example of a predicted position of a modeling defect stored in the position storage unit 25 (the nozzle position at the time when the abnormality detection unit 35A detects an abnormality (defect)). [Diagram 36] 1 is a table summarizing the results of Example 4 (cycles 1 to 5). [Figure 37] FIG. 11 is a system configuration diagram of a 3D printer 300 according to a fourth embodiment. [Figure 38] 13A is a graph showing the relationship between the nozzle velocity in the X-axis direction and time, (b) is a graph showing the relationship between the nozzle velocity in the Y-axis direction and time, and (c) is a graph showing the relationship between the magnitude of the nozzle translation velocity and time. [Figure 39] FIG. 3 is a functional block diagram of a 3D printer 300. [Diagram 40] 1 is a flowchart outlining the operation of the 3D printer 300. [Diagram 41] 10 is a detailed flowchart of the operation of the 3D printer 300. [Diagram 42] 13 is a graph showing the relationship between the extrusion flow rate Qi and the translational speed VR of the discharge nozzle 18. [Diagram 43] 42 is an example of a three-dimensional object Ob1 (layered object) formed according to the flowchart of FIG. 41. [Diagram 44] 13 is a detailed flowchart of another operation example 1 of the 3D printer 300. [Diagram 45] 1 is a graph showing the relationship between the translational speed Vi of the discharge nozzle 18 and the predicted discharge flow rate QP (predicted outflow rate). [Diagram 46] 45 is an example of a three-dimensional object Ob2 (layered object) formed according to the flowchart of FIG. 44. [Figure 47] 13 is a detailed flowchart of another operation example 2 of the 3D printer 300. [Figure 48] 2 is an enlarged cross-sectional view of the vicinity of a discharge nozzle 18. FIG. [Figure 49] 13 is a detailed flowchart of another operation example 3 of the 3D printer 300. [Figure 50] 50 is an example of a three-dimensional object Ob3 (layered object) formed according to the flowchart of FIG. 49. [Figure 51] FIG. 13 is a diagram illustrating problem 1 of Comparative Example 6. [Figure 52] FIG. 13 is a diagram illustrating an advantage of the sixth embodiment and problem 1 of the sixth comparative example. [Figure 53] FIG. 1 is a diagram illustrating a fluidly connected state. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0046] Hereinafter, specific embodiments to which the present disclosure is applied will be described in detail with reference to the drawings. However, the present disclosure is not limited to the following embodiments. In addition, the following description and drawings are appropriately simplified for clarity of explanation.

[0047] <Embodiment 1> First, the configuration of the injection molding apparatus of this embodiment will be described. The injection molding apparatus of this embodiment is suitable for additive manufacturing of a workpiece using an injection molding machine. FIG. 1 is a diagram showing the injection molding apparatus of this embodiment. FIG. 2 is a block diagram of a control system of the injection molding apparatus of this embodiment. In the following description, a three-dimensional (XYZ) coordinate system will be used for clarity.

[0048] As shown in Figures 1 and 2, the injection molding apparatus 1 includes an injection molding machine 2, a supplying device 3, a table 4 (hereinafter also referred to as a base plate 4), a moving device 5, a heating device 6, and a control device 7. The injection molding machine 2 is configured to be able to continuously inject molten resin, for example. Figure 3 is an enlarged view of a portion of the negative side of the Z axis of the injection molding machine of this embodiment. Figure 4 is a cross-sectional view taken along the line IV-IV in Figure 3. Figure 5 is a cross-sectional view taken along the line VV in Figure 1. Figure 6 is a cross-sectional view taken along the line VI-VI in Figure 3.

[0049] As shown in Figures 1 to 3, the injection molding machine 2 includes a first cylinder 11, a second cylinder 12, an end plate 13, a first piston unit 14, a second piston unit 15, a first drive unit 16, a second drive unit 17, an injection unit 18, and a first control unit 19.

[0050] 3, the first cylinder 11 extends in the Z-axis direction and has a basic shape of a cylinder with a top that is closed at the end on the Z-axis + side of the first cylinder 11. That is, the first cylinder 11 has a closed portion 11a disposed on the Z-axis + side and a cylindrical side wall portion 11b that is continuous with the peripheral portion of the closed portion 11a and extends from the closed portion 11a to the Z-axis - side, and the end on the Z-axis - side of the first cylinder 11 is open.

[0051] As shown in Fig. 3, a through hole 11c is formed in the closing portion 11a of the first cylinder 11, penetrating the closing portion 11a in the Z-axis direction. Also, as shown in Fig. 3 and Fig. 4, a supply hole 11d through which a resin raw material is supplied is formed in a portion of the side wall portion 11b of the first cylinder 11 on the Z-axis + side. The resin raw material is, for example, resin pellets (plural).

[0052] 3 and 4, the second cylinder 12 extends in the Z-axis direction and is aligned with the first cylinder 11 in the Y-axis direction. The second cylinder 12 has the same configuration as the first cylinder 11, so a duplicated description will be omitted. However, the second cylinder 12 has a blocking portion 12a having a through hole 12c and a side wall portion 12b having a supply hole 12d, and the end of the second cylinder 12 on the negative Z-axis side is open.

[0053] 3, the end plate 13 is fixed to the ends of the first cylinder 11 and the second cylinder 12 on the negative side in the Z axis direction. The end plate 13 includes a main body 13a and a check valve 13b. The main body 13a has, for example, a plate shape as a basic form, and has through holes 13c formed at intervals in the Y axis direction.

[0054] 3, through hole 13c penetrates main body 13a in the Z-axis direction, and includes accommodation portion 13d in which check valve 13b is accommodated at the portion of through hole 13c on the negative Z-axis side. The surface of accommodation portion 13d on the positive Z-axis side is an inclined surface that inclines toward the negative Z-axis side from the center of through hole 13c toward the outside.

[0055] In this case, the portion of through hole 13c on the Z-axis + side has an inclined surface that inclines toward the Z-axis + side as it moves from the center of through hole 13c outward, and the end of the inclined surface on the Z-axis - side is continuous with the end of storage portion 13d on the Z-axis + side.

[0056] The check valve 13b allows the flow of molten resin to the negative side of the Z axis and blocks the flow of molten resin to the positive side of the Z axis. The check valve 13b can be configured, for example, as a check valve, and includes a check ball 13e and a spring 13f as shown in Fig. 3. The elastic force of the spring 13f may be appropriately set so that the check valve 13b opens when a preset pressure acts on the check ball 13e.

[0057] As shown in Figure 3, such an end plate 13 is fixed to the Z-axis -side ends of the first cylinder 11 and the second cylinder 12 via bolts 13h passed through bolt holes 13g formed in the main body 13a so that the end plate 13 covers the Z-axis -side opening of the first cylinder 11 and the Z-axis -side opening of the second cylinder 12.

[0058] At this time, the through hole 13c on the Y-axis negative side of the end plate 13 is positioned on the Z-axis negative side relative to the first cylinder 11, and the through hole 13c on the Y-axis positive side of the end plate 13 is positioned on the Z-axis negative side relative to the second cylinder 12.

[0059] Here, it is preferable that the central axis of the through hole 13c on the Y-axis - side of the end plate 13 and the central axis of the first cylinder 11 are arranged so as to approximately overlap, and that the central axis of the through hole 13c on the Y-axis + side of the end plate 13 and the central axis of the second cylinder 12 are arranged so as to approximately overlap.

[0060] As shown in Fig. 3, the first piston unit 14 is disposed inside the first cylinder 11 so as to be slidable inside the first cylinder 11. Fig. 7 is a perspective view showing the first piston unit and the second piston unit of this embodiment. Fig. 8 is an exploded view showing the first piston unit and the second piston unit of this embodiment.

[0061] 7 and 8, the first piston unit 14 includes a torpedo piston 14a, a check ring 14b, a stopper 14c, a pressurizing piston 14d, and a biasing means 14e. The torpedo piston 14a has a basic shape of a closed cylinder with a closed end at the Z-axis + side, and has an outer circumferential shape that roughly corresponds to the inner circumferential shape of the first cylinder 11. In this case, it is preferable that the surface of the torpedo piston 14a on the Z-axis + side is an inclined surface that inclines toward the Z-axis - side as it moves from the center to the periphery of the torpedo piston 14a.

[0062] Groove portions 14f are formed on the outer circumferential surface of the torpedo piston 14a, as shown in Figures 7 and 8. The groove portions 14f extend in the Z-axis direction and are arranged at approximately equal intervals in the circumferential direction of the torpedo piston 14a.

[0063] However, as described below, groove portion 14f only needs to have a shape and arrangement that allows the resin raw material supplied to the first space S1 on the Z-axis + side of the first piston unit 14 in the first cylinder 11 to be plasticized into molten resin when it passes through groove portion 14f, and that allows the molten resin to flow into the second space S2 on the Z-axis - side of the first piston unit 14 in the first cylinder 11.

[0064] 5, 7 and 8, the check ring 14b is annular in shape with an outer circumferential shape substantially equal to the inner circumferential shape of the first cylinder 11, and is disposed on the negative side of the Z axis with respect to the torpedo piston 14a. The stopper 14c holds the check ring 14b at the end of the torpedo piston 14a on the negative side of the Z axis.

[0065] The stopper 14c includes a ring portion 14g and a hook portion 14h, as shown in Fig. 8. The ring portion 14g has an outer peripheral shape that is substantially the same as the inner peripheral shape of the torpedo piston 14a. The hook portion 14h is substantially L-shaped when viewed from a direction perpendicular to the Z axis, and the end of the vertical portion of the hook portion 14h on the Z axis + side is fixed to the ring portion 14g.

[0066] The horizontal portion of the hook portion 14h protrudes from the end of the vertical portion of the hook portion 14h on the negative side of the Z axis toward the outside of the ring portion 14g as shown in Fig. 8. The hook portions 14h are arranged at approximately equal intervals in the circumferential direction of the ring portion 14g.

[0067] With the ring portion 14g and the vertical portion of the hook portion 14h passing through the through hole of the check ring 14b, the ring portion 14g is fitted into the opening at the end portion on the negative side of the Z axis of the torpedo piston 14a. As a result, the check ring 14b is held at the end portion on the negative side of the Z axis of the torpedo piston 14a via the stopper 14c.

[0068] At this time, the length of the vertical portion of the hook portion 14h in the Z-axis direction is longer than the thickness of the check ring 14b in the Z-axis direction. This allows the check ring 14b to move in the Z-axis direction between the end of the first cylinder 11 on the negative Z-axis side and the horizontal portion of the hook portion 14h. However, it is sufficient that the stopper 14c is configured to hold the check ring 14b at the end of the first cylinder 11 on the negative Z-axis side so as to be able to move in the Z-axis direction.

[0069] 7 and 8, the pressurizing piston 14d has a bottomed cylindrical shape with a closed end on the negative side of the Z axis, and for example, the end face on the negative side of the Z axis of the pressurizing piston 14d is a substantially flat surface parallel to the XY plane. The outer peripheral shape of the pressurizing piston 14d is substantially the same as the inner peripheral shape of the torpedo piston 14a.

[0070] As shown in FIG. 3, the pressurizing piston 14d is slidably inserted inside the torpedo piston 14a with a seal member 14i sealing the gap between the inner peripheral surface of the torpedo piston 14a and the outer peripheral surface of the pressurizing piston 14d.

[0071] That is, the inside of the torpedo piston 14a functions as a sliding portion for the pressurizing piston 14d, and the pressurizing piston 14d slides in the Z-axis direction relative to the torpedo piston 14a, changing the amount of protrusion of the first cylinder 11 into the second space S2 relative to the torpedo piston 14a. The area of ​​the region surrounded by the outer periphery of the pressurizing piston 14d, the maximum amount of movement, and the like will be described later.

[0072] At this time, although the detailed function will be described later, it is preferable that an intrusion portion 14j into which the molten resin intrudes is formed on the end face on the Z-axis negative side of the pressure piston 14d as shown in Figures 7 and 8. The intrusion portion 14j is, for example, a groove portion formed on the end face on the Z-axis negative side of the pressure piston 14d, and extends in a direction perpendicular to the Z axis.

[0073] However, the penetration portion 14j only needs to have a shape that allows molten resin to penetrate between the Z-axis negative end face of the pressure piston 14d and the Z-axis positive end face of the end plate 13 when the Z-axis negative end face of the pressure piston 14d is in contact with the Z-axis positive end face of the end plate 13.

[0074] The biasing means 14e biases the pressurizing piston 14d relative to the torpedo piston 14a toward the second space S2 of the first cylinder 11. The biasing means 14e is, for example, an elastic member such as a coil spring as shown in FIG.

[0075] The biasing means 14e is disposed inside the pressurizing piston 14d with the Z-axis positive end of the biasing means 14e in contact with the Z-axis positive end of the torpedo piston 14a and the Z-axis negative end of the biasing means 14e in contact with the Z-axis negative end of the pressurizing piston 14d. The biasing force of the biasing means 14e will be described later.

[0076] As shown in Fig. 3, the second piston unit 15 is disposed inside the second cylinder 12 so as to be slidable inside the second cylinder 12. The second piston unit 15 has the same configuration as the first piston unit 14, and therefore a duplicated description will be omitted, but as shown in Figs. 5, 7 and 8, the second piston unit 15 includes a torpedo piston 15a having a groove portion 15f formed on the outer circumferential surface, a check ring 15b, a stopper 15c having a ring portion 15g and a hook portion 15h, a pressure piston 15d and a biasing means 15e.

[0077] 3, the pressure applying piston 15d is slidably inserted into the torpedo piston 15a with the gap between the inner peripheral surface of the torpedo piston 15a and the outer peripheral surface of the pressure applying piston 15d sealed with a seal member 15i. At this time, as shown in Fig. 5, Fig. 7 and Fig. 8, an intrusion portion 15j into which the molten resin intrudes may be formed also on the end face of the pressure applying piston 15d on the negative side of the Z axis.

[0078] The first driving unit 16 drives the first piston unit 14 in the Z-axis direction. As shown in Fig. 3, the first driving unit 16 includes a motor 16a, a screw shaft 16b, a slider 16c, a rod 16d, and a case 16e. The motor 16a is, for example, a servo motor, and is fixed to the end of the case 16e on the Z-axis + side. The rotation angle of the output shaft of the motor 16a is detected by an encoder 16f (see Fig. 2).

[0079] 3, the screw shaft 16b extends in the Z-axis direction and is rotatably supported inside the case 16e via a bearing 16g. The end of the screw shaft 16b on the Z-axis positive side is passed through a through hole 16h formed in the end of the case 16e on the Z-axis positive side and is connected to the output shaft of the motor 16a so as to transmit a driving force from the output shaft.

[0080] The slider 16c has a screw hole, and the screw hole of the slider 16c is engaged with the screw shaft 16b so that the slider 16c moves along the screw shaft 16b inside the case 16e. The screw shaft 16b and the slider 16c form a ball screw and are housed inside the case 16e.

[0081] 3, the rod 16d extends in the Z-axis direction and passes through a through-hole 16i formed in the end of the case 16e on the negative side of the Z-axis and a through-hole 11c of the first cylinder 11. The end of the rod 16d on the positive side of the Z-axis is fixed to the slider 16c, and the end of the rod 16d on the negative side of the Z-axis is fixed to the end of the torpedo piston 14a of the first piston unit 14 on the positive side of the Z-axis.

[0082] As shown in Fig. 3, the case 16e supports the motor 16a, the screw shaft 16b, the slider 16c, and the rod 16d. The case 16e is, for example, box-shaped, and forms an enclosed space inside the case 16e. The closing part 11a of the first cylinder 11 is fixed to the end of the case 16e on the negative side of the Z axis.

[0083] The second driving unit 17 drives the second piston unit 15 in the Z-axis direction. The second driving unit 17 has substantially the same configuration as the first driving unit 16, and therefore will not be described again, but includes a motor 17a, a screw shaft 17b, a slider 17c, a rod 17d, and a case 17e, as shown in FIG.

[0084] That is, the motor 17a is fixed to the end of the case 17e on the Z-axis + side, and the rotation angle of the output shaft of the motor 17a is detected by an encoder 17f (see FIG. 2). As shown in FIG. 3, the screw shaft 17b is supported inside the case 17e via a bearing 17g, and the end of the screw shaft 17b on the Z-axis + side is connected to the output shaft of the motor 17a with the screw shaft 17b passing through a through hole 17h formed in the end of the case 17e on the Z-axis + side.

[0085] The screw hole of the slider 17c is engaged with the screw shaft 17b so that the slider 17c moves along the screw shaft 17b inside the case 17e. The rod 17d passes through a through hole 17i formed in the end of the case 17e on the negative side of the Z axis and through a through hole 12c of the second cylinder 12. The end of the rod 17d on the positive side of the Z axis is fixed to the slider 17c, and the end of the rod 17d on the negative side of the Z axis is fixed to the end of the torpedo piston 15a of the second piston unit 15 on the positive side of the Z axis.

[0086] 3, the case 17e supports the motor 17a, the screw shaft 17b, the slider 17c, and the rod 17d, and forms an enclosed space inside the case 17e. The closing part 12a of the second cylinder 12 is fixed to the end of the case 17e on the negative side of the Z axis.

[0087] 1 and 3, in this embodiment, the case 17e is formed integrally with the case 16e of the first drive unit 16, forming a common sealed space. Therefore, in the following description, when the case 16e of the first drive unit 16 is shown, the case 17e of the second drive unit 17 may also be shown. However, the case 17e may be formed of a separate member from the case 16e of the first drive unit 16.

[0088] The injection section 18 is disposed on the negative side of the Z axis with respect to the end plate 13 so as to be able to inject the molten resin extruded from the first cylinder 11 and the second cylinder 12. As shown in Fig. 3, the injection section 18 is provided with an injection port 18a (a resin discharge hole, which corresponds to the discharge nozzle of the present invention, hereinafter also referred to as discharge nozzle 18a or nozzle 18a) for injecting the molten resin, a first branch path 18b extending from the injection port 18a on the positive side of the Z axis and towards the negative side of the Y axis, and a second branch path 18c extending from the injection port 18a on the positive side of the Z axis and towards the positive side of the Y axis. Here, it is preferable that the injection port 18a has a shape that is narrowed as it approaches the negative side of the Z axis.

[0089] 3, the injection section 18 is fixed to the end plate 13 via a retaining nut 18d. At this time, the end portion on the Z-axis + side of the first branch passage 18b communicates with the through hole 13c on the Y-axis - side of the end plate 13, and the end portion on the Z-axis + side of the second branch passage 18c communicates with the through hole 13c on the Y-axis + side of the end plate 13.

[0090] The ejection section 18 is divided into a first plate 18e in which the ejection port 18a is formed, and a second plate 18f in which the first branch passage 18b and the second branch passage 18c are formed, and although detailed functions will be described later, it is preferable that at least one of the first plate 18e and the second plate 18f is made of a ceramic plate. Here, the ejection section 18 can be formed with a housing portion for housing a part of the check valve 13b.

[0091] The first control unit 19, the details of which will be described later, controls the motor 16a of the first driving unit 16 and the motor 17a of the second driving unit 17 based on the detection results of the encoders 16f and 17f.

[0092] The supply device 3 supplies the resin raw material to the first cylinder 11 and the second cylinder 12. As shown in Fig. 1 to Fig. 3, the supply device 3 includes an exhaust unit 31, a hopper 32, a pressurizing unit 33, and a second control unit 34. The exhaust unit 31 exhausts gas from the first space S1 of the first cylinder 11, the first space S3 on the Z-axis + side of the second piston unit 15 in the second cylinder 12, and the space surrounded by the torpedo pistons 14a, 15a and the pressurizing pistons 14d, 15d.

[0093] In detail, exhaust section 31 includes exhaust passage 31a, exhaust hole 31b, and exhaust valve 31c. As shown in Fig. 3, exhaust passage 31a is formed in rod 16d and torpedo piston 14a of first drive section 16, and in rod 17d and torpedo piston 15a of second drive section 17. Exhaust passage 31a passes through the insides of rods 16d, 17d, penetrates the ends of torpedo pistons 14a, 15a on the Z-axis + side, and extends in the Z-axis direction.

[0094] The end of exhaust passage 31a on the negative side of the Z axis branches out and reaches the peripheral surfaces of the ends of rods 16d, 17d on the negative side of the Z axis as well as the space surrounded by torpedo pistons 14a, 15a and pressure pistons 14d, 15d, and the end of exhaust passage 31a on the positive side of the Z axis reaches the end faces of rods 16d, 17d on the positive side of the Z axis.

[0095] Therefore, the end of exhaust passage 31a on the Z-axis - side is connected to the space surrounded by the first space S1 of the first cylinder 11 and the torpedo piston 14a and the pressurizing piston 15d, or the space surrounded by the first space S3 of the second cylinder 12 and the torpedo piston 15a and the pressurizing piston 15d, and the end of exhaust passage 31a on the Z-axis + side is disposed inside the case 16e of the first drive unit 16.

[0096] The exhaust hole 31b is formed in the case 16e of the first drive unit 16. However, if the case 16e of the first drive unit 16 and the case 17e of the second drive unit 17 are configured from separate members, the exhaust hole 31b is formed in each of the cases 16e and 17e. The exhaust valve 31c is connected to the exhaust hole 31b via an exhaust pipe 35. The exhaust valve 31c is, for example, an electromagnetic valve.

[0097] The hoppers 32 accommodate the resin raw material M to be supplied to the first space S1 of the first cylinder 11 and the first space S3 of the second cylinder 12. In this embodiment, as shown in Fig. 1, the hoppers 32 include a first hopper 32a and a second hopper 32b.

[0098] The first hopper 32a is configured so that the inside of the first hopper 32a can be sealed, and is connected to the supply hole 11d of the first cylinder 11 via a first supply pipe 36. The second hopper 32b is configured so that the inside of the second hopper 32b can be sealed, and is connected to the supply hole 12d of the second cylinder 12 via a second supply pipe 37.

[0099] The first hopper 32a and the second hopper 32b may be configured to keep the resin raw material M dry by the residual heater. This makes it possible to suppress molding defects caused by water vapor generated when the resin raw material M is plasticized.

[0100] The inner diameters of the supply hole 11d of the first cylinder 11, the supply hole 12d of the second cylinder 12, the first supply pipe 36 and the second supply pipe 37 are preferably equal to or smaller than twice the diagonal of the resin pellets which are the resin raw material M.

[0101] This prevents the resin raw material M from lining up and forming a bridge in the supply hole 11d of the first cylinder 11, the supply hole 12d of the second cylinder 12, the first supply pipe 36, and the second supply pipe 37, thereby preventing the inside of each from becoming clogged.

[0102] The pressurizing unit 33 is an air pump that applies gas pressure to the inside of the hopper 32. In this embodiment, as shown in Fig. 1, the pressurizing unit 33 is connected to the first hopper 32a via a first connecting pipe 38, and is connected to the second hopper 32b via a second connecting pipe 39.

[0103] The pressurizing unit 33, for example, constantly pressurizes the inside of the hopper 32. Therefore, when the exhaust valve 31c and the check valve 13b of the end plate 13 are in a closed state, the sealed space formed by the space surrounded by the first cylinder 11, the second cylinder 12, the torpedo pistons 14a, 15a and the pressurizing pistons 14d, 15d, and the case 16e of the first drive unit 16 is maintained at a high pressure relative to the outside of the case 16e.

[0104] The second control unit 34 controls the exhaust valve 31c to exhaust gas from the first space S1 of the first cylinder 11 or the first space S3 of the second cylinder 12 at a desired timing, which will be described later.

[0105] As shown in FIG. 1, the table 4 is disposed on the negative side of the Z axis with respect to the injection molding machine 2, and is a molding table for laminating molten resin injected from the injection port 18a of the injection molding machine 2 to mold a workpiece. The molten resin injected (discharged) from this injection port 18a is called a resin bead (molten resin discharged from the injection port 18a that has solidified into a thread-like shape). Here, the table 4 may be configured to be heatable, for example. The moving device 5 moves the injection molding machine 2 and the table 4 to mold the workpiece. The moving device 5 includes, for example, a gantry device 51, a lifting device 52, and a third control unit 53, as shown in FIG. 1 and FIG. 2.

[0106] The gantry device 51 moves the injection molding machine 2 in the X-axis direction and the Y-axis direction. A typical gantry device can be used as the gantry device 51, and for example, as shown in Fig. 37, can be configured by combining a slide rail 51a extending in the X-axis direction and a slide rail 51b extending in the Y-axis direction. Note that the gantry device 51 may be one that moves the injection molding machine 2 in the X-axis direction, the Y-axis direction, and the Z-axis direction.

[0107] The lifting device 52 raises and lowers the table 4 in the Z-axis direction. As the lifting device 52, for example, a general lifting device can be used, and it can be configured with a ball screw. The third control unit 53 controls the gantry device 51 and the lifting device 52 to laminate the molten resin injected from the injection molding machine 2 to mold a desired workpiece.

[0108] 1 to 3, the heating device 6 includes a first heating section 61, a second heating section 62, a temperature detection section 63, and a fourth control section 64. The first heating section 61 keeps the plasticized molten resin warm.

[0109] The first heating section 61 can be configured, for example, by a sheet heater surrounding the negative Z-axis side portions of the first cylinder 11 and the second cylinder 12. However, the first heating section 61 only needs to be able to keep the plasticized molten resin warm, and the configuration and arrangement of the first heating section 61 are not limited.

[0110] The second heating section 62 heats the molten resin to a desired temperature. The second heating section 62 includes a sheet heater 62a and a heat transfer member 62b, for example, as shown in Fig. 3 and Fig. 6. The sheet heater 62a is arranged at approximately equal intervals around the injection port 18a of the injection section 18 as viewed from the Z-axis direction. The heat transfer member 62b is disc-shaped with a through hole formed in approximately the center of the heat transfer member 62b, and is made of a ceramic plate.

[0111] The heat transfer member 62b is disposed between the first plate 18e and the second plate 18f. At this time, the seat heater 62a is disposed between the heat transfer member 62b and the first plate 18e or between the heat transfer member 62b and the second plate 18f. This allows the heat of the seat heater 62a to be transferred satisfactorily to the first plate 18e or the second plate 18f.

[0112] Here, when the first plate 18e and the second plate 18f are made of ceramic plates as described above, the ceramic plates have a smaller heat capacity than metal, and therefore the heat of the second heating part 62 can be efficiently transferred to the molten resin. Furthermore, if the second heating part 62 is damaged, the second heating part 62 can be easily replaced by loosening the retaining nut 18d.

[0113] The temperature detection unit 63 detects the temperature of the molten resin. The temperature detection unit 63 is provided, for example, in the injection unit 18. In this case, the temperature detection unit 63 is preferably provided on the first plate 18e or the second plate 18f on the side formed of the ceramic plate. This makes it possible to detect the temperature of the molten resin with high accuracy.

[0114] The fourth control unit 64 controls the first heating unit 61 and the second heating unit 62 so that the temperature of the molten resin falls within a preset range, based on the detection result of the temperature detection unit 63. If the first cylinder 11 and the second cylinder 12 are configured to be able to keep the molten resin R warm, the heating device 6 may be omitted.

[0115] As shown in FIG. 2, the control device 7 has a first control unit 19, a second control unit 34, a third control unit 53, and a fourth control unit 64, and controls the first control unit 19, the second control unit 34, the third control unit 53, and the fourth control unit 64 in order to form the workpiece.

[0116] Next, in the injection molding apparatus 1 of this embodiment, when plasticizing the resin raw material M supplied to the first space S1 of the first cylinder 11 or the first space S3 of the second cylinder 12 and flowing molten resin into the second space S2 of the first cylinder 11 or the second space S4 on the Z-axis -side of the second piston unit 15 in the second cylinder 12, preferred conditions for suppressing the inflow of gas into the second space S2 of the first cylinder 11 or the second space S4 of the second cylinder 12 will be described.

[0117] First, the area of ​​the region surrounded by the outer periphery in the XY cross section of the pressurizing piston 14d of the first piston unit 14 should be equal to or larger than the area of ​​the region surrounded by the outer periphery in the XY cross section of the rod 16d. Similarly, the area of ​​the region surrounded by the outer periphery in the XY cross section of the pressurizing piston 15d of the second piston unit 15 should be equal to or larger than the area of ​​the region surrounded by the outer periphery in the XY cross section of the rod 17d.

[0118] Furthermore, when the torpedo piston 14a is positioned furthest on the Z axis + side to inject molten resin and the pressurizing piston 14d is positioned in the second space S2 of the first cylinder 11, the volume of the second space S2 should be equal to or less than the volume of the first space S1 when the torpedo piston 14a is positioned furthest on the Z axis - side to plasticize the resin raw material M and the rod 16d is positioned in the first space S1 of the first cylinder 11.

[0119] Similarly, when the torpedo piston 15a is positioned furthest on the Z axis + side to inject molten resin and the pressurizing piston 15d is positioned in the second space S4 of the second cylinder 12, the volume of the second space S4 should be equal to or less than the volume of the first space S3 when the torpedo piston 15a is positioned furthest on the Z axis - side to plasticize the resin raw material M and the rod 17d is positioned in the first space S3 of the second cylinder 12.

[0120] It is preferable that the following formulas 1 to 3 are further satisfied. <Formula 1> (π×(Dc 2 -Dr2 )×Lr×γ) / 4≧(π×(Dc 2 -Dp 2 )×Lr) / 4 <Formula 2> π×Lr×{(Dc 2 -Dr 2 )×γ-(Dc 2 -Dp 2 )} / 4≦π×Dp 2 ×Lp / 4 <Expression 3> (Dc 2 -Dp 2 ) / (Dc 2 -Dr 2 )≦γ≦Dp 2 / (Dc 2 -Dr 2 ) × Lp / Lr + (Dc 2 -Dp 2 ) / (Dc 2 -Dr 2 )

[0121] Here, Dc is the inner diameter of the first cylinder 11 and the second cylinder 12, Dp is the outer diameter of the pressure pistons 14d, 15d, Dr is the outer diameter of the rods 16d, 17d, Lp is the maximum stroke amount (maximum movement amount) of the pressure pistons 14d, 15d, Lr is the maximum stroke amount (maximum movement amount) of the torpedo pistons 14a, 15a, and γ is the filling rate of the resin raw material M.

[0122] As shown in <Formula 1>, it is preferable that the volume of the resin raw material M supplied to the first space S1 of the first cylinder 11 or the first space S3 of the second cylinder 12 is equal to or greater than the increase in the volume of the second space S2 of the first cylinder 11 or the second space S4 of the second cylinder 12 when the resin raw material M is plasticized.

[0123] Here, the volume of the resin raw material M is approximately equal to the volume of the molten resin. Therefore, in other words, the volume of the molten resin flowing into the second space S2 of the first cylinder 11 or the second space S4 of the second cylinder 12 should be equal to or greater than the increase in the volume of the second space S2 of the first cylinder 11 or the second space S4 of the second cylinder 12 when the molten resin flows in.

[0124] As shown in <Equation 2>, it is preferable that the difference obtained by subtracting the increase in the volume of the second space S2 of the first cylinder 11 or the second space S4 of the second cylinder 12 from the volume of the molten resin be equal to or greater than the amount by which the volume of the second space S2 of the first cylinder 11 or the second space S4 of the second cylinder 12 can be increased by moving the pressurizing pistons 14d, 15d from a state in which they are positioned furthest toward the Z axis + side.

[0125] As a result, the amount of molten resin obtained by subtracting the increase in the volume of the second space S2 of the first cylinder 11 or the increase in the volume of the second space S4 of the second cylinder 12 from the volume of the molten resin according to <Equation 1> can be absorbed by the pressurizing pistons 14d, 15d moving toward the Z-axis + side.

[0126] <Equation 3> is obtained by solving <Equation 1> and <Equation 2> for the filling rate of the resin raw material M. Even if the type of resin raw material M is different, by satisfying <Equation 3>, the inflow of gas into the second space S2 of the first cylinder 11 or the second space S4 of the second cylinder 12 can be suppressed.

[0127] Next, a flow of molding a workpiece using the injection molding apparatus 1 of this embodiment will be described. Figures 9 to 13 are diagrams showing the operation of the injection molding apparatus of this embodiment. In Figures 9 to 13, the upper part shows the operation of the injection molding machine 2, and the lower part shows the timing of plasticizing the resin raw material M in the first cylinder 11 and the second cylinder 12 and injecting the molten resin R, etc.

[0128] Here, in the state shown in Figure 9(a), the supply of resin raw material M from the first hopper 32a of the supply device 3 to the first space S1 of the first cylinder 11 is completed, and the first piston unit 14 moves to the Z-axis - side to inject the molten resin R that has flowed into the second space S2 of the first cylinder 11.

[0129] Meanwhile, the second piston unit 15 moves to the negative side of the Z axis and starts injecting the molten resin R from the second space S4 of the second cylinder 12. At this time, it is assumed that the pressurizing piston 15d of the second piston unit 15 is disposed closest to the positive side of the Z axis. Also, it is assumed that the exhaust valve 31c of the exhaust section 31 is closed.

[0130] From this state, the first control unit 19 controls the motor 16a to continue moving the first piston unit 14 on the - side of the Z axis to continue injecting the molten resin R, while controlling the motor 17a to continue moving the second piston unit 15 on the - side of the Z axis to continue injecting the molten resin R.

[0131] Next, when the first control unit 19 confirms by referring to the detection result of the encoder 16f that the first piston unit 14 has reached the furthest side of the Z axis (bottom dead center), it controls the motor 16a to start moving the first piston unit 14 toward the + side of the Z axis, as shown in Figure 9(b) → Figure 9(c) → Figure 10(a).

[0132] In this way, during the period from when the injection of molten resin R from the second cylinder 12 begins to when the injection of molten resin R from the first cylinder 11 is stopped, the molten resin R is injected from the first cylinder 11 and the second cylinder 12.

[0133] Therefore, the period during which the molten resin R is injected from the second cylinder 12 can be made to overlap with the period during which the molten resin R is injected from the first cylinder 11 and the preset first period. Thus, the molten resin R can be injected continuously from the first cylinder 11 and the second cylinder 12.

[0134] Here, the preset first period can be appropriately set according to the moving speed of each of the piston units 14, 15. Then, the first control unit 19 controls the motors 16a, 17a to adjust the moving speed of each of the piston units 14, 15 so that the injection amount of the molten resin R injected from the injection unit 18 becomes the target injection amount, whereby the desired workpiece can be molded with high precision.

[0135] When the first piston unit 14 starts to move toward the + side of the Z axis, the resin raw material M is compressed by the first piston unit 14, the blocking portion 11a of the first cylinder 11, and the side wall portion 11b of the first cylinder 11, and the resin raw material M plasticizes as it passes through the groove portion 14f of the torpedo piston 14a of the first piston unit 14, becoming molten resin R, and flows into the second space S2 of the first cylinder 11.

[0136] At this time, the supply hole 11d is formed in the side wall portion 11b of the first cylinder 11, so that the resin raw material M is unlikely to leak out from the supply hole 11d. Moreover, the force on the Z-axis + side acting when the resin raw material M is plasticized by the first piston unit 14 can be received by the closing portion 11a of the first cylinder 11.

[0137] Furthermore, if the surface on the Z-axis + side of the torpedo piston 14a of the first piston unit 14 is formed as an inclined surface that slopes toward the Z-axis - side as it moves from the center of the torpedo piston 14a toward the peripheral edge, the resin raw material M can be effectively guided into the groove portion 14f of the torpedo piston 14a of the first piston unit 14 when the first piston unit 14 moves toward the Z-axis + side.

[0138] When the first piston unit 14 moves toward the + side of the Z axis, the check ring 14b of the first piston unit 14 is pushed toward the - side of the Z axis, allowing the molten resin R to flow smoothly through the gap between the torpedo piston 14a and the check ring 14b and through the through hole of the check ring 14b into the second space S2 of the first cylinder 11.

[0139] When the first piston unit 14 moves toward the + side of the Z axis in this manner, the pressing piston 14d protrudes toward the - side of the Z axis relative to the torpedo piston 14a due to the biasing force of the biasing means 14e so that the end of the pressing piston 14d on the - side of the Z axis remains in contact with the end plate 13.

[0140] In this embodiment, the area of ​​the region surrounded by the outer peripheral edge of the pressurizing piston 14d in the XY cross section is greater than or equal to the area of ​​the region surrounded by the outer peripheral edge of the rod 16d in the XY cross section, and the volume of the second space S2 when the torpedo piston 14a is positioned furthest on the Z axis + side to inject the molten resin R and the pressurizing piston 14d is positioned in the second space S2 of the first cylinder 11 is less than or equal to the volume of the first space S1 when the torpedo piston 14a is positioned furthest on the Z axis - side to plasticize the resin raw material M and the rod 16d is positioned in the first space S1 of the first cylinder 11.

[0141] Therefore, the pressurizing piston 14d is biased by the biasing means 14e so that the increase in volume of the second space S2 of the first cylinder 11 when the torpedo piston 14a moves toward the Z-axis + side is less than or equal to the decrease in volume of the first space S1 of the first cylinder 11, thereby suppressing the inflow of gas when the molten resin R flows into the second space S2 of the first cylinder 11.

[0142] Meanwhile, the first control unit 19 controls the motor 17a while referring to the detection result of the encoder 17f, and continues to move the second piston unit 15 toward the Z-axis negative side. As a result, the molten resin R is injected through the through hole 13c on the Y-axis positive side, the second branch passage 18c of the injection unit 18, and the injection port 18a while pushing the check valve 13b on the Y-axis positive side of the end plate 13 toward the Z-axis negative side. At this time, the check valve 13b on the Y-axis negative side blocks the flow of the molten resin R toward the Z-axis positive side due to the pressure of the molten resin R injected from the second cylinder 12.

[0143] When the second piston unit 15 moves toward the negative side of the Z axis, the check ring 15b of the second piston unit 15 is pushed toward the positive side of the Z axis, and the groove portion 15f of the torpedo piston 15a is blocked by the check ring 15b, thereby preventing the molten resin R from flowing back into the first space S3 of the second cylinder 12 through the groove portion 15f of the torpedo piston 15a.

[0144] Next, when the first control unit 19 confirms with reference to the encoder 16f that the first piston unit 14 has reached the furthest position on the Z axis + side, it controls the motor 16a to start moving the first piston unit 14 toward the Z axis - side, as shown in Fig. 10(b). Meanwhile, the first control unit 19 controls the motor 17a with reference to the encoder 17f to continue moving the second piston unit 15 toward the Z axis - side.

[0145] At this time, the pressurizing piston 14d of the first piston unit 14 is in a state where it protrudes most toward the Z-axis - side from the torpedo piston 14a, and as the first piston unit 14 moves toward the Z-axis - side, the pressure of the molten resin R in the second space S2 of the first cylinder 11 increases.

[0146] Then, as the molten resin R in the second space S2 of the first cylinder 11 enters the entering portion 14j of the pressurizing piston 14d, the force due to the pressure of the molten resin R exceeds the biasing force of the biasing means 14e, and the pressurizing piston 14d is pushed toward the negative side of the Z axis as shown in Figure 10(c) -> Figure 11(a) -> Figure 11(b). At this time, the gas in the space surrounded by the torpedo piston 14a and the pressurizing piston 14d is exhausted from the exhaust path 31a into the case 16e by the amount corresponding to the reduction in the volume of the space.

[0147] On the other hand, when the first control unit 19 refers to the encoder 17f and confirms that the second piston unit 15 has reached a preset position in the Z-axis direction, the second control unit 34 controls the exhaust valve 31c of the exhaust unit 31 to open the exhaust valve 31c.

[0148] As a result, the gas in the first space S3 of the second cylinder 12 passes through the exhaust passage 31a of the rod 17d, enters the inside of the case 16e, and is discharged through the exhaust hole 31b and the exhaust valve 31c. As a result, a flow of gas flows from the second hopper 32b into the first space S3 of the second cylinder 12, and the resin raw material M is pushed by the gas from the second hopper 32b and is supplied to the first space S3 of the second cylinder 12 through the supply hole 12d of the second cylinder 12, as shown in Fig. 10(c) → Fig. 11(a) → Fig. 11(b).

[0149] At this time, since the supply hole 12d is formed in the side wall portion 12b of the second cylinder 12, the resin raw material M falls to the negative side of the Z axis while swirling together with the gas. Therefore, the resin raw material M can be supplied approximately uniformly into the first space S3 of the second cylinder 12.

[0150] Next, when the pressurizing piston 14d reaches the furthest side of the Z axis + side (for example, the Z axis + side end of the pressurizing piston 14d comes into contact with the Z axis + side end of the torpedo piston 14a) and the pressure pushing the molten resin R toward the Z axis - side at the Z axis - side end of the first piston unit 14 reaches a preset pressure, the check valve 13b on the Y axis - side of the end plate 13 opens.

[0151] As a result, the molten resin R is injected through the Y-axis -side through hole 13c, the first branch passage 18b of the injection section 18, and the injection port 18a while pushing the check valve 13b on the Y-axis -side of the end plate 13 toward the Z-axis -side.

[0152] At this time, when the first piston unit 14 moves toward the negative side of the Z axis, the check ring 14b of the first piston unit 14 is pushed toward the positive side of the Z axis, and the groove portion 14f of the torpedo piston 14a is blocked by the check ring 14b, thereby preventing the molten resin R from flowing back into the first space S1 of the first cylinder 11 through the groove portion 14f of the torpedo piston 14a.

[0153] On the other hand, when the first control unit 19 confirms with reference to the encoder 17f that the second piston unit 15 has reached the closest position to the negative side of the Z axis, the second control unit 34 controls and closes the exhaust valve 31c of the exhaust unit 31. At this time, the first space S3 of the second cylinder 12 is filled with the resin raw material M.

[0154] That is, by simply opening the exhaust valve 31c of the exhaust section 31, the resin raw material M can be automatically supplied to the first space S3 of the second cylinder 12. At this time, since the resin raw material M is supplied to the first space S3 of the second cylinder 12 during the period from when the second piston unit 15 reaches a preset position in the Z axis direction until when it reaches the closest position to the negative side of the Z axis, the resin raw material M can be supplied to the second cylinder 12 quantitatively.

[0155] Then, the period during which the resin raw material M is supplied to the first space S3 of the second cylinder 12 and the period during which the molten resin R is injected from the second cylinder 12 can be made to overlap with a preset second period.

[0156] Therefore, it is possible to efficiently repeat the injection of the molten resin R from the second cylinder 12 and the supply of the raw resin material M to the second cylinder 12. Here, the preset second period can be appropriately set according to the moving speed of the second piston unit 15, the timing of opening the exhaust valve 31c of the exhaust section 31, and the like.

[0157] Next, when the first control unit 19 confirms with reference to the encoder 17f that the second piston unit 15 has reached the furthest Z-axis negative side (bottom dead center), it controls the motor 17a to start moving the second piston unit 15 to the Z-axis positive side, as shown in Fig. 11(c) → Fig. 12(a) → Fig. 12(b). At this time, the check valve 13b on the Y-axis positive side blocks the flow of the molten resin R to the Z-axis positive side due to the pressure of the molten resin R injected from the first cylinder 11.

[0158] As a result, the resin raw material M is compressed by the second piston unit 15, the blocking portion 12a of the second cylinder 12, and the side wall portion 12b of the second cylinder 12, and the resin raw material M is plasticized as it passes through the groove portion 15f of the torpedo piston 15a of the second piston unit 15, becoming molten resin R, and flows into the second space S4 of the second cylinder 12.

[0159] At this time, the supply hole 12d is formed in the side wall portion 12b of the second cylinder 12, so that the resin raw material M is unlikely to leak out from the supply hole 12d. Moreover, the force on the Z-axis + side acting when the resin raw material M is plasticized by the second piston unit 15 can be received by the closing portion 12a of the second cylinder 12.

[0160] Furthermore, if the surface on the Z-axis + side of the torpedo piston 15a of the second piston unit 15 is formed as an inclined surface that slopes toward the Z-axis - side as it moves from the center of the torpedo piston 15a toward the peripheral edge, the resin raw material M can be effectively guided into the groove portion 15f of the torpedo piston 15a of the second piston unit 15 when the second piston unit 15 moves toward the Z-axis + side.

[0161] When the second piston unit 15 moves toward the + side of the Z axis, the check ring 15b of the second piston unit 15 is pushed toward the - side of the Z axis, allowing the molten resin R to flow smoothly through the gap between the torpedo piston 15a and the check ring 15b and the through hole of the check ring 15b into the second space S4 of the second cylinder 12.

[0162] When the second piston unit 15 moves toward the + side of the Z axis in this manner, the biasing force of the biasing means 15e causes the pressurizing piston 15d to protrude toward the - side of the Z axis relative to the torpedo piston 15a so that the end of the pressurizing piston 15d on the - side of the Z axis remains in contact with the end plate 13.

[0163] In this embodiment, the area of ​​the region surrounded by the outer peripheral edge of the pressurizing piston 15d in the XY cross section is greater than or equal to the area of ​​the region surrounded by the outer peripheral edge of the rod 17d in the XY cross section, and the volume of the second space S4 when the torpedo piston 15a is positioned furthest on the Z axis + side to inject the molten resin R and the pressurizing piston 15d is positioned in the second space S4 of the second cylinder 12 is less than or equal to the volume of the first space S3 when the torpedo piston 15a is positioned furthest on the Z axis - side to plasticize the resin raw material M and the rod 17d is positioned in the first space S3 of the second cylinder 12.

[0164] Therefore, when the torpedo piston 15a moves toward the Z-axis + side, the pressurizing piston 15d is biased by the biasing means 15e so that the increase in volume of the second space S4 of the second cylinder 12 is equal to or less than the decrease in volume of the first space S3 of the second cylinder 12, thereby suppressing the inflow of gas when the molten resin R flows into the second space S4 of the second cylinder 12.

[0165] Meanwhile, the first control unit 19 controls the motor 16a while referring to the detection result of the encoder 16f to continue the movement of the first piston unit 14 toward the negative side of the Z axis. As a result, the molten resin R is injected from the first cylinder 11 and the second cylinder 12 during the period from when the injection of the molten resin R from the first cylinder 11 starts to when the injection of the molten resin R from the second cylinder 12 stops.

[0166] Therefore, the period during which the molten resin R is injected from the first cylinder 11 can be made to overlap with a preset first period during which the molten resin R is injected from the second cylinder 12. Thus, the molten resin R can be injected from the first cylinder 11 and the second cylinder 12 continuously.

[0167] Then, the first control unit 19 controls the motors 16a, 17a to adjust the movement speeds of the piston units 14, 15 so that the amount of molten resin R injected from the injection unit 18 becomes the target injection amount, thereby enabling the desired workpiece to be molded with high precision.

[0168] 12(c), when the first control unit 19 confirms with reference to the encoder 17f that the second piston unit 15 has reached the furthest position on the Z axis + side, it controls the motor 17a to start moving the second piston unit 15 toward the Z axis - side. Meanwhile, the first control unit 19 controls the motor 16a with reference to the encoder 16f to continue moving the first piston unit 14 toward the Z axis - side.

[0169] At this time, the pressurizing piston 15d of the second piston unit 15 is in a state where it protrudes most toward the Z-axis - side from the torpedo piston 15a, and as the second piston unit 15 moves toward the Z-axis - side, the pressure of the molten resin R in the second space S4 of the second cylinder 12 increases.

[0170] Then, as the molten resin R in the second space S4 of the second cylinder 12 enters the entering portion 15j of the pressurizing piston 15d, the force due to the pressure of the molten resin R exceeds the biasing force of the biasing means 15e, and the pressurizing piston 15d is pushed toward the negative side of the Z axis, as shown in Fig. 13(a). At this time, the gas in the space surrounded by the torpedo piston 15a and the pressurizing piston 15d is exhausted from the exhaust path 31a into the case 16e by the amount corresponding to the reduction in the volume of the space.

[0171] On the other hand, when the first control unit 19 refers to the encoder 16f and confirms that the first piston unit 14 has reached a preset position in the Z-axis direction, the second control unit 34 controls the exhaust valve 31c of the exhaust unit 31 to open the exhaust valve 31c.

[0172] As a result, the gas in the first space S1 of the first cylinder 11 passes through the exhaust passage 31a of the rod 16d, enters the inside of the case 16e, and is discharged through the exhaust hole 31b and the exhaust valve 31c. As a result, a flow of gas flows from the first hopper 32a into the first space S1 of the first cylinder 11, and the resin raw material M is pushed by the gas from the first hopper 32a and supplied to the first space S1 of the first cylinder 11 through the supply hole 11d of the first cylinder 11.

[0173] At this time, since the supply hole 11d is formed in the side wall portion 11b of the first cylinder 11, the resin raw material M falls to the Z-axis negative side while swirling together with the gas. Therefore, the resin raw material M can be supplied approximately uniformly into the first space S1 of the first cylinder 11.

[0174] 13(b), when the first control unit 19 confirms with reference to the encoder 16f that the first piston unit 14 has reached the closest position to the negative side of the Z axis, the second control unit 34 controls and closes the exhaust valve 31c of the exhaust unit 31. At this time, the first space S1 of the first cylinder 11 is filled with the resin raw material M.

[0175] That is, by simply opening the exhaust valve 31c of the exhaust section 31, the resin raw material M can be automatically supplied to the first space S1 of the first cylinder 11. At this time, since the resin raw material M is supplied to the first space S1 of the first cylinder 11 during the period from when the first piston unit 14 reaches a preset position in the Z axis direction to when it reaches the closest position to the negative side of the Z axis, the resin raw material M can be supplied to the first cylinder 11 quantitatively.

[0176] Then, the period during which the resin raw material M is supplied to the first space S1 of the first cylinder 11 and the period during which the molten resin R is injected from the first cylinder 11 can be made to overlap with a preset second period.

[0177] Therefore, it is possible to efficiently repeat the injection of the molten resin R from the first cylinder 11 and the supply of the raw resin material M to the first cylinder 11. Here, the preset second period can be appropriately set according to the moving speed of the first piston unit 14, the timing of opening the exhaust valve 31c of the exhaust section 31, and the like.

[0178] Next, the first control unit 19 controls the motor 16a to continue moving the first piston unit 14 toward the negative side of the Z axis, and controls the motor 17a to continue moving the second piston unit 15 toward the negative side of the Z axis.

[0179] Then, as shown in Figure 13(c), the state transitions to that of Figure 9(a), and the pressurizing piston 15d reaches the furthest side of the Z axis + side (for example, the Z axis + side end of the pressurizing piston 15d comes into contact with the Z axis + side end of the torpedo piston 15a), and when the pressure pushing the molten resin R toward the Z axis - side at the Z axis - side end of the second piston unit 15 reaches a preset pressure, the check valve 13b on the Y axis + side of the end plate 13 opens.

[0180] As a result, the molten resin R is injected through the through hole 13c on the Y-axis + side, the second branch passage 18c of the injection section 18, and the injection port 18a while pushing the check valve 13b on the Y-axis + side of the end plate 13 toward the Z-axis - side.

[0181] In this way, the first control unit 19 controls the motors 16a, 17a to continuously inject molten resin R from the first cylinder 11 and the second cylinder 12, while the third control unit 53 controls the gantry device 51 and the lifting device 52 so that the desired workpiece is additively manufactured on the Z-axis + side surface of the table 4 by the injected molten resin R, thereby molding the workpiece.

[0182] At this time, the fourth control unit 64 controls the first heating unit 61 and the second heating unit 62 so that the temperature of the injected molten resin R falls within a preset range based on the detection result of the temperature detection unit 63. This allows the molten resin R to be injected in a stable state.

[0183] The injection molding apparatus 1, injection molding machine 2, and injection molding method of this embodiment are equipped with pressure pistons 14d, 15d that are slidable in the Z-axis direction, and biasing means 14e, 15e that bias the pressure pistons 14d, 15d toward the negative side of the Z-axis relative to the torpedo pistons 14a, 15a so that the amount of protrusion of the first and second cylinders 11, 12 into the second spaces S2, S4 relative to the torpedo pistons 14a, 15a changes.

[0184] Therefore, the volumes of the second spaces S2, S4 of the first and second cylinders 11, 12 can be reduced when the molten resin R flows into the second spaces S2, S4, and the inflow of gas into the second spaces S2, S4 can be suppressed when the molten resin R is caused to flow into the second spaces S2, S4. Therefore, the injection molding apparatus 1, the injection molding machine 2, and the injection molding method of the present embodiment can suppress the inflow of gas into the molten resin R when the molten resin R is injected, and can contribute to improving the quality of the workpiece.

[0185] In particular, in the injection molding apparatus 1, injection molding machine 2, and injection molding method of this embodiment, the biasing means 14e, 15e bias the pressurizing pistons 14d, 15d so that the increase in volume of the second spaces S2, S4 of the first and second cylinders 11, 12 when the torpedo pistons 14a, 15a move toward the Z-axis + side is less than the decrease in volume of the first spaces S1, S3 of the first and second cylinders 11, 12, thereby suppressing the inflow of gas when the molten resin R flows into the second spaces S2, S4 of the first and second cylinders 11, 12.

[0186] Moreover, in the injection molding apparatus 1, the injection molding machine 2, and the injection molding method of the present embodiment, the period during which the molten resin R is injected from the first cylinder 11 and the period during which the molten resin R is injected from the second cylinder 12 partially overlap each other. This makes it possible to continuously inject the molten resin R from the first cylinder 11 and the second cylinder 12.

[0187] Furthermore, the injection molding apparatus 1, the injection molding machine 2, and the injection molding method of the present embodiment can automatically supply the resin raw material M to the first and second cylinders 11, 12 simply by controlling the exhaust valve 31c of the exhaust section 31. That is, the supply device 3 of the present embodiment can function as an automatic supply device for the resin raw material M. Therefore, the resin raw material M can be supplied with a simple configuration.

[0188] In addition, since the resin raw material M is supplied to the first cylinder 11 or the second cylinder 12 from when the first piston unit 14 or the second piston unit 15 reaches a preset position in the Z axis direction until it reaches the closest position to the negative side of the Z axis, the resin raw material M can be supplied quantitatively to the first cylinder 11 and the second cylinder 12. Therefore, a meter for the resin raw material M can be omitted.

[0189] The pre-installed position in the Z-axis direction may be set so that the first space S1 of the first cylinder 11 or the first space S3 of the second cylinder 12 is filled with the resin raw material M by the time the first piston unit 14 or the second piston unit 15 reaches the closest position to the negative side of the Z-axis.

[0190] Here, since the end portion on the negative Z-axis side of the first cylinder 11 is open, the first piston unit 14 and the rod 16d of the first driving unit 16 can be inserted from the opening on the negative Z-axis side of the first cylinder 11. Similarly, since the end portion on the negative Z-axis side of the second cylinder 12 is open, the second piston unit 15 and the rod 17d of the second driving unit 17 can be inserted from the opening on the negative Z-axis side of the second cylinder 12. Therefore, a plunger such as that provided in the injection molding apparatus of Patent Document 1 can be omitted.

[0191] 3, the injection molding machine 2 may include a cooling unit 8 between the case 16e of the first driving unit 16 and the first and second cylinders 11 and 12. The cooling unit 8 has, for example, a ring shape as a basic form, and a through hole 8a through which the rod 16d or 17d passes is formed so as to penetrate the cooling unit 8 in the Z-axis direction. A cooling passage 8b through which a cooling medium flows is formed in the cooling unit 8 so as to surround the through hole 8a.

[0192] With this configuration, when a cooling medium is flowed through the cooling passage 8b of the cooling unit 8 during molding of a workpiece with the injection molding apparatus 1, heat from the first cylinder 11 and the second cylinder 12 is not easily transferred to the bearing 16g of the first driving unit 16 and the bearing 17g of the second driving unit 17. This makes it possible to suppress temperature changes in the bearings 16g and 17g, and to suppress malfunctions of the bearings 16g and 17g. As a result, the workpiece can be molded with high precision.

[0193] <Embodiment 2> Next, the configuration of an injection molding machine 2A according to the second embodiment will be described.

[0194] FIG. 14 is a configuration diagram of an injection molding machine 2A according to the second embodiment.

[0195] The configuration of an injection molding machine 2A of the second embodiment is similar to the configuration of the injection molding machine 2 of the first embodiment described above, but differs in the following respects.

[0196] As shown in FIG. 14, a first pressure detection unit 65 and a second pressure detection unit 66 are added to the injection molding machine 2A of the second embodiment. The first pressure detection unit 65 is a pressure detection sensor that detects the pressure applied to the molten resin housed (stored) in the first cylinder 11, and is, for example, a strain gauge. The strain gauge detects the pressure from the strain of the outer wall of the first cylinder 11 due to the pressure applied to the molten resin housed (stored) in the first cylinder 11. The first pressure detection unit 65 is, for example, attached (for example, pasted) to a portion of the outer circumferential surface of the first cylinder 11 that corresponds to the portion where the molten resin is housed. The second pressure detection unit 66 is a pressure detection sensor that detects the pressure applied to the molten resin housed (stored) in the second cylinder 12, and is, for example, a strain gauge. The strain gauge detects the pressure from the strain of the outer wall of the second cylinder 12 due to the pressure applied to the molten resin housed (stored) in the second cylinder 12. The second pressure detection unit 66 is attached (eg, affixed) to a location on the outer circumferential surface of the second cylinder 12 that corresponds to a portion in which the molten resin is accommodated.

[0197] In the second embodiment, potentiometers are used instead of the encoders 16f and 17f. Hereinafter, they are referred to as potentiometers 16f and 17f. The potentiometer 16f is a position detection means for the motor 16a (servomotor). The position of the first torpedo 14 can be detected by the position detection value of the potentiometer 16f. Similarly, the potentiometer 17f is a position detection means for the motor 17a (servomotor). The position of the second torpedo 15 can be detected by the position detection value of the potentiometer 17f. In addition, a ceramic heater is used instead of the seat heater 62a. Hereinafter, they are referred to as ceramic heater 62a.

[0198] In the second embodiment, a thermocouple is used as the temperature detection unit 63 (means for detecting the temperature of the molten resin contained in the first cylinder 11 and the second cylinder 12).

[0199] Next, a control device 7A according to the second embodiment will be described.

[0200] FIG. 15 is a configuration diagram of a control device 7A according to the second embodiment.

[0201] As shown in FIG. 15, the control device 7A includes a storage unit 20, a control unit 30A, and a memory .

[0202] The storage unit 20 is, for example, a non-volatile storage unit such as a hard disk device or a ROM. A k data table 21, an n data table 22, and a K data table 23 are stored in the storage unit 20. The storage unit 20 also stores dimensions 24 of the discharge nozzle (for example, nozzle diameter, nozzle length). The storage unit 20 also stores a predetermined program (not shown) executed by the control unit 30A.

[0203] The k data table 21 stores in advance the pseudoplastic viscosity k for each type of resin and temperature. The pseudoplastic viscosity k will be described later. The n data table 22 stores in advance the power exponent n for each type of resin. The power exponent n will be described later. The K data table 23 stores in advance the bulk modulus K for each type of resin. The bulk modulus K will be described later. The control unit 30A includes a processor (not shown). The processor is, for example, a CPU (Central Processing Unit). There may be one processor or multiple processors. The processor executes a predetermined program loaded from the storage unit 20 into a memory 40 (for example, a RAM) to function mainly as a target pressure calculation unit 31A, a movement speed calculation unit 32A, a movement speed control unit 33A, and a corrected bulk modulus calculation unit 34A. Some or all of these may be realized by hardware.

[0204] Motors 16a, 17a, potentiometers 16f, 17f, a temperature detector 63, a first pressure detector 65, a second pressure detector 66, an XY-axis driver 50, a Z-axis driver 60, and the like are electrically connected to the controller 7A.

[0205] The XY-axis driving device 50 drives the injection molding machine 2A (discharge nozzle 18a) in the X and Y axes by a mechanism not shown. The Z-axis driving device 60 drives the base plate 4 in the Z axis by a mechanism not shown.

[0206] The injection molding apparatus configured as described above functions as a 3D printer (one example of an additive manufacturing apparatus of the present invention) that forms resin beads on a base plate 4 that can be driven in the Z axis using molten resin discharged (injected) from an injection molding machine 2A (discharge nozzle 18a) that drives in the XY axes, and sequentially layers the resin beads to form a three-dimensional object (additive manufactured body).

[0207] Next, an outline of the operation of the injection molding machine 2A of the embodiment 2 will be described. The following processing is realized by the control unit 30A (processor) executing a predetermined program read from the storage unit 20 to the memory 40 (for example, RAM).

[0208] The base plate 4 is placed directly under the resin discharge hole of the discharge nozzle 18a, and the discharge nozzle 18a is moved along the modeling trajectory that will be the first layer of the layered object by the XY-axis driving device 50. At that time, the moving speed of the discharge nozzle 18a is input to the control device 7A, which outputs drive command values ​​to the motors 16a and 17a according to the flowchart of FIG.

[0209] The control device 7A calculates the target pressure to obtain the command flow rate according to the flowchart of FIG. 21 from the position (position detection value), pressure (pressure detection value), temperature (temperature detection value) and values ​​(pseudoplastic viscosity, power exponent, bulk modulus, nozzle dimensions) stored in the memory unit (data tables 21-23). ​​At that time, in the first cycle, the command movement speed is calculated according to the flowchart of FIG. 22, and a drive command value based on the calculated speed is output to the motor 16a or 17a. From the second cycle, the control device 7A calculates the corrected bulk modulus K' according to the flowchart of FIG. 25, calculates the command movement speed using the corrected bulk modulus, and outputs a drive command value based on the calculated speed to the motor 16a or 17a.

[0210] <Terminology> The "instructed flow rate" is a target value (target flow rate) of the flow rate of the molten resin discharged from the discharge nozzle 18a, and refers to the flow rate of the molten resin discharged from the nozzle 18a per unit time. The instructed flow rate Q is expressed by the following formula 4.

[0211] Q = Cross-sectional area of ​​resin bead (= Cross-sectional area of ​​nozzle) × Nozzle moving speed (Equation 4)

[0212] Figure 16(a) is a graph showing the relationship between the nozzle movement speed and the indicated flow rate (when the nozzle diameter is 1 mm and the cylinder diameter is 20 mm). Note that in the region where the movement speed is close to zero, when it is below the minimum controllable flow rate (7.85 in Figure 16(a)), the indicated flow rate may be set to zero. Figure 16(b) is another graph showing the relationship between the nozzle movement speed and the indicated flow rate (when the nozzle diameter is 12 mm and the cylinder diameter is 100 mm). Note that in the region where the movement speed is close to zero, when it is below the minimum controllable flow rate (1,131 in Figure 16(b)), the indicated flow rate may be set to zero.

[0213] "Power exponent" refers to a constant determined for each resin.

[0214] Fig. 17 shows an example (representative example) of the power index. As the power index, a known one (for example, see "Plastic Product Design Method" by Seiichi Homma, published by Nikkan Kogyo Shimbun, 2011, p. 9) may be used.

[0215] "Pseudoplastic viscosity" refers to a constant that is determined by temperature for each resin. An example of calculating pseudoplastic viscosity will be described below.

[0216] Fig. 19 is a specific example of converting the relationship between pressure and flow rate into the relationship between shear rate and melt viscosity (resin name: ABS, temperature: 210°C). Fig. 20 is a graph plotting "shear rate" and "melt viscosity" in Fig. 19.

[0217] From the experimental results in Figure 19, the relationship between the measured pressure and flow rate was converted into the relationship between the shear rate and melt viscosity, and plotted on a double logarithmic graph as shown in Figure 20. The power approximation equation (y = kx (n-1)) using the least squares method, y=42500x -0.75 This gives a pseudoplastic viscosity k of 42,500. The pseudoplastic viscosity can be calculated in the same manner for resins and temperatures other than ABS and 210°C.

[0218] "Bulk modulus" refers to a constant determined by the properties of molten resin. Figure 18(a) shows an example of a table of calculated bulk modulus values, and Figure 18(b) is a graph plotting Figure 18(a).

[0219] The "target pressure" refers to the pressure applied to the molten resin contained (stored) in the cylinder 11 or 12 in order to make the flow rate of the molten resin discharged from the discharge nozzle 18a equal to the designated flow rate.

[0220] The "predicted outflow amount" refers to the outflow amount of molten resin predicted to be discharged from the nozzle 18a per Δt (control time interval).

[0221] The "instructed movement speed" refers to the speed at which the first piston unit 14 or the second piston unit 15 is moved in order to set the flow rate of the molten resin discharged from the nozzle 18a to the instructed flow rate. The first piston unit 14 or the second piston unit 15 is an example of the piston of the present invention. Hereinafter, the first piston unit 14 or the second piston unit 15 will also be referred to as the first torpedo 14 or the second torpedo 15. "Operating the injection molding machine" means ejecting resin (molten resin).

[0222] <Example of Operation of Target Pressure Calculation Unit 31A> Next, an example of the operation of the target pressure calculation unit 31A will be described.

[0223] The target pressure calculation unit 31A calculates the "target pressure" based on the command flow rate, the temperature of the molten resin, the pseudoplastic viscosity, and the dimensions of the discharge nozzle 18a.

[0224] FIG. 21 is a flowchart of an operation example of the target pressure calculation unit 31A.

[0225] First, the command flow rate Q is input (acquired) (step S10).

[0226] Next, for the command flow rate Q, the shear rate D is calculated by the following formula 5 (step S11). D = 32Q / (πd n 3 )...(Formula 5)

[0227] However, d n is the equivalent value of the diameter of the minimum cross-sectional area of ​​the discharge nozzle 18a (nozzle diameter). π is the ratio of the circumference of a circle to its diameter. n can be obtained from the storage unit.

[0228] Next, the temperature T of the molten resin immediately before being discharged is detected (step S12). The temperature T may be a temperature (temperature detection value) directly detected by the temperature detection unit 63 (thermocouple) or may be an estimated temperature. Step S12 is an example of the temperature acquisition unit of the present invention.

[0229] Next, the pseudoplastic viscosity k determined by the temperature T is calculated (step S13). The pseudoplastic viscosity k corresponding to the type of resin (molten resin) and the temperature (temperature T detected in step S12) can be acquired from the k data table 21. The type of resin (molten resin) is input by, for example, a user. Step S13 is an example of the pseudoplastic viscosity acquisition unit of the present invention.

[0230] Next, the melt viscosity η is calculated by the following formula 6 (step S14).

[0231] η = kD n-1 ...(Formula 6) Here, n is an index that should correspond to the type of resin (molten resin). The index n that should correspond to the type of resin (molten resin) can be acquired from the n data table 22. The type of resin (molten resin) is input by, for example, the user.

[0232] Next, the shear stress τ is calculated by the following formula 7 (step S15).

[0233] τ = ηD (equation 7)

[0234] Next, the target pressure Pt is calculated by the following formula 8 (step S16) and output (step S17). Note that the target pressure Pt is a relative pressure with the pressure outside the discharge nozzle 18a set to atmospheric pressure (zero).

[0235] P t = τ4L n / d n ...(Formula 8) However, L n The discharge nozzle 18a (diameter d n ) (nozzle length). Nozzle length L n can be obtained from the storage unit 20.

[0236] <Example of Operation of the Movement Speed ​​Calculation Unit 32A (Torpedo Movement Speed ​​Feedforward Control)> Next, an operation example (torpedo movement speed feedforward control) of the movement speed calculation unit 32A will be described.

[0237] The movement speed calculation unit 32A calculates the "instruction movement speed (first cycle of ejection)".

[0238] FIG. 22 is a flowchart of an operation example (torpedo movement speed feedforward control) of the movement speed calculation unit 32A.

[0239] First, the target pressure Pt calculated in step S16 and output in step S17 is input (acquired) (step S20).

[0240] Next, the measured pressure Pr is detected (step S21). The measured pressure Pr refers to the detection value (pressure detection value) of the first pressure detection unit 65 and the second pressure detection unit 66.

[0241] Next, the amount of pressurization ΔP that will result in the target pressure Pt is calculated by the following equation 9 (step S22).

[0242] ΔP=Pt-Pr (Formula 9)

[0243] Next, the actual position X r is detected (step S23). r refers to the detection values ​​(position detection values) of the potentiometers 16f and 17f.

[0244] Next, the bulk modulus K corresponding to the type of resin (molten resin) is set (step S24). For example, in the first cycle of discharge, the bulk modulus K corresponding to the type of resin (molten resin) is obtained from the K data table 23. Note that the type of resin (molten resin) is input by, for example, the user.

[0245] Next, the pressure component of the movement speed of the first torpedo 14 (or the second torpedo 15) is V rp is calculated by the following formula 10 (step S25). Note that in the following formula 10, the outflow (discharge) of the molten resin due to the application of pressure is not taken into consideration.

number

[0246] Next, the predicted runoff volume Q p is calculated by the following formula 11 (step S26).

[0247] Q p =πd n 3 / 32×{P r d n / (4kL n )} 1 / n ×Δt...(Equation 11)

[0248] Equation 11 is derived as follows. First, the above formula 5 is transformed into the following formula 12. Q p =Dπd n 3 / 32...(Formula 12)

[0249] Next, substituting the above formulas 6 and 7 into formula 8 gives the following formula 13. P r =kD n 4L n / d n ...(Equation 13)

[0250] This formula 13 is transformed into the following formula 14. D=(P r d n / 4kL n ) 1 / n ...(Formula 14)

[0251] Substituting the above formula 14 into the above formula 12 gives the following formula 15. Q p =πd n 3 / 32×{P r d n / (4kL n )} 1 / n ...(Equation 15)

[0252] Multiplying the right hand side of this formula 15 by Δt results in the above formula 11. Each element in the above formulas 12 to 15 can be illustrated as in Fig. 24. Fig. 24 is a schematic diagram illustrating each element in formulas 12 to 15.

[0253] Next, the flow rate portion of the moving speed of the first torpedo 14 (or the second torpedo 15) is Vrq is calculated by the following equation 16 (step S27). V rq =Q p / Δt / S...(Equation 16)

[0254] Next, the command movement speed V r The pressure increase amount and the flow rate amount are added together, calculated using the following formula 17, and output (step S28). V r =V rp +V rq ...(Formula 17)

[0255] <Example of operation from the second discharge cycle onwards (method to improve accuracy of torpedo movement speed prediction)>

[0256] Next, an example of operation from the second cycle of discharge onwards (method of improving accuracy in predicting the torpedo movement speed) will be described.

[0257] From the second cycle of discharge onwards, the movement speed calculation unit 32A calculates the "instructed movement speed (from the second cycle of discharge onwards)". At that time, the pressure change amount resulting from the movement of the first torpedo 14 (or the second torpedo 15) is calculated from the measured pressure, the volume change amount due to the movement of the first torpedo 14 (or the second torpedo 15) and the outflow amount calculated by the above formula 11 using the measured pressure are subtracted from the volume change amount to calculate the "effective pressurized volume", and a corrected bulk modulus is calculated from the pressure change amount and the "effective pressurized volume", which is used to calculate the instructed movement speed (see steps S32 and S33 described later). This makes it possible to use a predicted value (corrected bulk modulus) reflecting the volume modulus according to the state of air entrainment in the molten resin, thereby improving accuracy.

[0258] FIG. 25 is a flowchart of an example of operation from the second cycle of ejection onward.

[0259] First, the measured pressure Pr is detected (step S30). The measured pressure Pr refers to the detection value (pressure detection value) of the first pressure detection unit 65 and the second pressure detection unit 66.

[0260] Next, the corrected bulk modulus calculation unit 34A calculates the corrected bulk modulus K' by the following formula 18 (step S31). K´=(P r -P r-1 ) / (ΔV p / V)...(Formula 18) However, P r is the actual pressure when calculating the corrected bulk modulus when the control time step width is Δt. P r-1 is the actual pressure measured Δt time ago. ΔV p is the "effective pressurized volume" obtained by subtracting the outflow volume from the volume that is reduced by the movement of the first torpedo 14 (or the second torpedo 15) in time Δt.

[0261] ΔV p is calculated using the following formula 19. ΔV p =V r ×Δt×SQ p ...(Formula 19) Each element in the above formulas 18 to 19 can be illustrated as in Fig. 26. Fig. 26 is a schematic diagram illustrating each element in the formulas 18 to 19.

[0262] Next, the moving speed calculation unit 32A sets the corrected bulk modulus K' as the bulk modulus K' in the second cycle (step S32). Next, the movement speed calculation unit 32A calculates and outputs the command movement speed Vr in the same manner as in the first cycle (steps S25 to S28) (step S33).

[0263] <Example of Operation of the Movement Speed ​​Control Unit 33A> The moving speed control unit 33A calculates the moving speed of the first torpedo 14 (or the second torpedo 15) in step S28 and outputs the instructed moving speed V r Specifically, the movement speed control unit 33A controls the motor 16a or 17a so that the movement speed of the first torpedo 14 (or the second torpedo 15) is equal to or greater than the designated movement speed V rIn addition, the movement speed control unit 33A outputs a drive command value to the motor 16a or 17a so that the movement speed of the first torpedo 14 (or the second torpedo 15) is calculated and output in step S33. r Specifically, the movement speed control unit 33A controls the motor 16a or 17a so that the movement speed of the first torpedo 14 (or the second torpedo 15) is equal to or faster than the designated movement speed V r A drive command value is output to the motor 16a or 17a so as to satisfy the following.

[0264] <Flow rate control example 1> Next, a first embodiment of flow rate control will be described.

[0265] Example 1 is an example of ejection control for printing small objects with high resolution. In Example 1, the nozzle diameter is as small as φ1 mm (cylinder diameter d t This section describes the flow rate control and the method of controlling the nozzle 18a when the nozzle 18a, whose nozzle diameter is φ1 mm, is driven at a steady speed (the maximum speed normally used) of 160 mm / s in order to linearly form an ABS resin bead having a circular cross section of φ1 mm (diameter of the nozzle 18a).

[0266] Fig. 27 is a flowchart of flow rate control common to Example 1 and Example 2. Fig. 28 is a table summarizing the simulation results (1st to 3rd cycles) of Example 1.

[0267] In the following description, it is assumed that first torpedo 14 and second torpedo 15 alternately pressurize the molten resin in cylinders 11 and 12 (see FIGS. 9 to 13), thereby causing the molten resin to be continuously discharged from discharge nozzle 18a.

[0268] Each cycle in FIG. 27 corresponds to Δt (control time step size).

[0269] First, the first cycle of processing of the first torpedo 14 (steps S40 to S47) will be described.

[0270] First, the nozzle movement speed is input (step S40). Here, it is assumed that the movement speed of the nozzle 18a is detected as 160 mm / s by the XY-axis driving device 50 and input to the control device 7A.

[0271] Next, the command flow rate Q is calculated (step S41). Here, the command flow rate Q is calculated by the above-mentioned formula 4 as follows: Command flow rate Q=cross-sectional area of ​​resin bead (=cross-sectional area of ​​nozzle 18a)×nozzle moving speed=π / 4×1 2 mm 2 ×160 mm / s=125.6 mm 3 / s is assumed to have been calculated.

[0272] Next, the target pressure Pt is calculated (step S42). Specifically, the process shown in FIG. 21 (steps S11 to S17) is executed.

[0273] First, the shear rate D is calculated (step S11). Here, the shear rate D=32Q / (πd n 3 )=32×125.6mm 3 / s / (3.14×(1mm) 3 ) = 1,280 / s is calculated. Note that Q = 125.6 mm 3 / s, d n =1mm.

[0274] Next, the temperature T of the molten resin immediately before being discharged is detected (step S12). Here, it is assumed that the temperature T detected is 210° C.

[0275] Next, the pseudoplastic viscosity k determined by the temperature T is calculated (step S13). Here, the pseudoplastic viscosity k of ABS resin at 210°C is 42,500 [kg / (m s 2-n )] is assumed to be calculated (see FIG. 20).

[0276] Next, the melt viscosity η is calculated (step S14). Here, the melt viscosity η=kD n-1 =42,500 kg / (m s 2-0.25 )×1,2800.25-1 / s 0.25-1 = 199 kg / (m s) = 199 Pa s is calculated. In the case of ABS resin, n = 0.25 (see Figure 17).

[0277] Next, the shear stress τ is calculated (step S15). Here, it is assumed that the shear stress τ = ηD = 199 Pa·s × 1,280 / s = 254,720 Pa = 0.25 MPa is calculated by the above formula 7. Here, η = 199 Pa·s, and D = 1,280 / s.

[0278] Next, the target pressure Pt is calculated (step S16). Here, the target pressure Pt=τ4L / d n = 0.25MPa × 4 × 2mm / 1mm = 2.0MPa is calculated. Note that τ = 0.25MPa, L = 2mm, d n = 1 mm. This target pressure Pt (2.0 MPa) is output to the control device 7A (step S17).

[0279] 27, the actual pressure Pr is detected (step S43). Here, it is assumed that the actual pressure Pr=0.0 MPa is detected.

[0280] Next, the amount of pressurization ΔP is calculated. Here, it is assumed that the amount of pressurization ΔP=Pt−Pr=2.0 MPa−0.0 MPa=2.0 MPa is calculated using the above formula 9.

[0281] Next, the actual position X r is detected (step S44). In this example, it is assumed that the actual position Xr=25 mm is detected.

[0282] Next, the bulk modulus K is set (step S45). Here, it is assumed that the bulk modulus K is set to 834 MPa (see FIG. 18(a)).

[0283] Next, the command movement speed V r (Step S46) Specifically, the process shown in FIG. 22 (Steps S25 to S28) is executed.

[0284] First, the moving speed (pressurization) V of the first torpedo 14 rp (Step S25). Here, the moving speed (pressure) Vrp = (2.0 MPa / 834 MPa) (628 mm 3 +314mm 2 ×25mm) / 0.1s / 314mm 2 = 0.647 mm / s is calculated. Note that V0 = 628 mm 3 , S = π / 4 × d t =314mm 2 (d t = 20 mm), and Δt = 0.1 sec. Note that Δt is not limited to 0.1 sec and may be another value.

[0285] Next, the predicted runoff volume Q p Here, the predicted outflow amount Qp=πd is calculated by the above formula 11 (step S26). n 3 / 32×{P r d n / (4kL n )} 1 / n ×Δt=0mm 3 is calculated. Note that P r = 0.0 MPa.

[0286] Next, the moving speed (flow rate) V of the first torpedo 14 rq (Step S27). Here, it is assumed that the moving speed (flow rate) Vrq=Qp / Δt / S=0 mm / s is calculated by the above formula 16. p =0mm 3 It is.

[0287] Next, the command movement speed V r Here, the command movement speed V is calculated and outputted by the above formula 17. r =V rp +V rq =0.647mm / s+0mm / s=0.647mm / s is calculated and output.

[0288] Next, the movement speed of the first torpedo 14 is set to the instructed movement speed V calculated in step S46 (step S27). r A drive command value is output to the motor 16a so as to satisfy the following condition (step S47).

[0289] Next, the processing from the second cycle onwards of the first torpedo 14 (torpedo movement speed feedback control; steps S48 to S52) will be described.

[0290] First, the nozzle movement speed is input (step S48). Here, it is assumed that the movement speed of the nozzle 18a is detected as 160 mm / s from the XY-axis drive device and input to the control device 7A.

[0291] Next, the same processes as those in steps S41 to S44 above are executed.

[0292] Here, it is assumed that the measured pressure Pr=1.45 MPa is detected in step S43.

[0293] Next, the corrected bulk modulus K' is calculated (step S49). Here, the corrected bulk modulus K'=(P r -P r-1 ) / (ΔV p / V)ΔV p =V r ×Δt×SQ p =(1.45MPa-0MPa) / (20.33 mm 3 / 8,478 mm 3 ) = 604.6MPa is calculated. Note that ΔVp = 0.647mm / s × 0.1s × 314mm 2 -0mm 3 =20.33mm 3 , P r = 1.45MPa, P r-1 = 0MPa, V = 628mm 3 +π / 4×202mm 2 ×25mm=8,478mm 3 It is. Next, the corrected bulk modulus K' is set as the bulk modulus K' in the second cycle (step S50).

[0294] Next, the calculation of the command movement speed Vr is performed in the same manner as in the first cycle (step S46) (step S51). Here, the command movement speed V r =V rp +V rq = 0.245mm / s + 0.103mm / s = 0.348 mm / s is calculated. Note that ΔP = Pt - Pr = 2.0MPa - 1.45MPa = 0.55MPa, Xr = 24.94mm, Vrp = (0.55MPa / 604.6MPa) (628mm 3 +314mm 2 ×24.94mm) / 0.1s / 314mm 2 = 0.245 mm / s, Qp = π × (1 mm) 3 / 32×{1.45MPa×1mm / (4×42,500kg / (m·s 2-0.25 )×2mm)} 1 / 0.25 ×0.1s=3.25mm 3 , Vrq=3.25mm 3 / 0.1s / 314mm 2 =0.103mm / s.

[0295] Next, the moving speed of the first torpedo 14 is set to the instructed moving speed V calculated in step S51. r A drive command value is output to the motor 16a so as to satisfy the following equation (step S52).

[0296] From the second cycle onwards, the above steps S48 to S52 are repeatedly executed until it is determined that the cycle is the final one (step S53: YES), that is, until it is determined that the first torpedo 14 has reached the bottom dead center. Whether or not the first torpedo 14 has reached the bottom dead center can be determined based on the detection value (position detection value) of the potentiometer 16f.

[0297] Next, the same processes as steps S40 to S52 are executed until the second torpedo 15 moves toward the Z-axis + side and reaches the Z-axis - side (bottom dead center) (step S54; YES).

[0298] <Flow rate control example 2> Next, a second embodiment of the flow rate control will be described.

[0299] Example 2 is an example of ejection control for printing a large object the size of a car in a short time. In Example 2, the nozzle diameter is as large as φ12 mm (cylinder diameter d t This section describes the flow rate control and the method of controlling the nozzle 18a when the nozzle 18a, whose nozzle diameter is φ12 mm, is driven at a steady speed (the maximum speed normally used) of 160 mm / s in order to linearly form an ABS resin bead having a circular cross section of φ12 mm (diameter = 100 mm).

[0300] Fig. 27 is a flowchart of flow rate control common to Example 1 and Example 2. Fig. 29 is a table summarizing the simulation results (1st to 3rd cycles) of Example 2.

[0301] In the following description, it is assumed that first torpedo 14 and second torpedo 15 alternately pressurize the molten resin in cylinders 11 and 12 (see FIGS. 9 to 13), thereby causing the molten resin to be continuously discharged from discharge nozzle 18a.

[0302] Each cycle in FIG. 27 corresponds to Δt (control time step size).

[0303] First, the first cycle of processing of the first torpedo 14 (steps S40 to S47) will be described.

[0304] First, the nozzle movement speed is input (step S40). Here, it is assumed that the movement speed of the nozzle 18a is detected as 160 mm / s by the XY-axis driving device 50 and input to the control device 7A.

[0305] Next, the command flow rate Q is calculated (step S41). Here, the command flow rate Q is calculated by the above-mentioned formula 4 as follows: Command flow rate Q=cross-sectional area of ​​resin bead (=cross-sectional area of ​​nozzle 18a)×nozzle moving speed=π / 4×122 mm 2 ×160 mm / s=18,096 mm 3 / s is assumed to have been calculated.

[0306] Next, the target pressure Pt is calculated (step S42). Specifically, the process shown in FIG. 21 (steps S11 to S17) is executed.

[0307] First, the shear rate D is calculated (step S11). Here, the shear rate D is calculated by the above formula 5 as follows: D = 32 × 18,096 mm 3 / s / (3.14×(12mm) 3 ) = 106.7 / s is calculated. Note that Q = 18,096 mm 3 / s, dn=12mm.

[0308] Next, the temperature T of the molten resin immediately before being discharged is detected (step S12). Here, it is assumed that the temperature T detected is 210° C.

[0309] Next, the pseudoplastic viscosity k determined by the temperature T is calculated (step S13). Here, the pseudoplastic viscosity k of ABS resin at 210°C is 42,500 [kg / (m s 2-n )] is assumed to be calculated (see FIG. 20).

[0310] Next, the melt viscosity η is calculated (step S14). Here, the melt viscosity η is calculated as 42,500 kg / (m s 2-0.25 ) x 106.7 0.25-1 / s 0.25-1 = 1,280 kg / (m s) = 1,280 Pa s is calculated. In the case of ABS resin, n = 0.25 (see Figure 17).

[0311] Next, the shear stress τ is calculated (step S15). Here, it is assumed that the shear stress τ = 1,280 Pa·s × 106.7 / s = 136,576 Pa = 0.14 MPa is calculated by the above formula 7. Note that η = 1,280 Pa·s, and D = 106.7 / s.

[0312] Next, the target pressure Pt is calculated (step S16). Here, it is assumed that the target pressure Pt = 0.14 MPa x 4 x 2 mm / 12 mm = 0.09 MPa is calculated by the above formula 8. Note that τ = 0.14 MPa, L = 2 mm, and dn = 12 mm. This target pressure Pt (0.09 MPa) is output to the control device 7A (step S17).

[0313] 27, the actual pressure Pr is detected (step S43). Here, it is assumed that the actual pressure Pr=0.0 MPa is detected.

[0314] Next, the amount of pressurization ΔP is calculated. Here, it is assumed that the amount of pressurization ΔP=Pt−Pr=0.09MPa−0.0MPa=0.09MPa is calculated using the above formula 9.

[0315] Next, the actual position X r is detected (step S44). In this example, it is assumed that the actual position Xr=25 mm is detected.

[0316] Next, the bulk modulus K is set (step S45). Here, it is assumed that the bulk modulus K is set to 834 MPa (see FIG. 18(a)).

[0317] Next, the command movement speed V r (Step S46) Specifically, the process shown in FIG. 22 (Steps S25 to S28) is executed.

[0318] First, the moving speed (pressurization) V of the first torpedo 14 rp Here, the moving speed (pressure) Vrp = (0.09 MPa / 834 MPa) (15,700 mm3 +7,854mm 2 ×25mm) / 0.1s / 7,854mm 2 = 0.029 mm / s is calculated. Note that V0 = 15,700 mm 3 , S=7,854mm 2 (d t = 100 mm), and Δt = 0.1 sec. Note that Δt is not limited to 0.1 sec and may be another value.

[0319] Next, the predicted runoff volume Q p Here, the predicted outflow amount Qp=πd is calculated by the above formula 11 (step S26). n 3 / 32×{P r d n / (4kL n )} 1 / n ×Δt=0mm 3 is calculated. Note that P r = 0.0 MPa.

[0320] Next, the moving speed (flow rate) V of the first torpedo 14 rq (Step S27). Here, it is assumed that the moving speed (flow rate) Vrq=Qp / Δt / S=0 mm / s is calculated by the above formula 16. p =0mm 3 It is.

[0321] Next, the command movement speed V r Here, the command movement speed V is calculated and outputted by the above formula 17. r =V rp +V rq =0.029 mm / s+0 mm / s =0.029 mm / s is calculated and output.

[0322] Next, the movement speed of the first torpedo 14 is set to the instructed movement speed V calculated in step S46 (step S27). r A drive command value is output to the motor 16a so as to satisfy the following condition (step S47).

[0323] Next, the processing from the second cycle onwards of the first torpedo 14 (torpedo movement speed feedback control; steps S48 to S52) will be described.

[0324] First, the nozzle movement speed is input (step S48). In this case, it is assumed that the movement speed of the nozzle 18a is 160 mm / s, which is detected from the XY-axis drive device and input to the control device.

[0325] Next, the same processes as those in steps S41 to S44 above are executed.

[0326] Here, it is assumed that the measured pressure Pr=0.046 MPa is detected in step S43.

[0327] Next, the corrected bulk modulus K' is calculated (step S49). Here, the corrected bulk modulus K'=(P r -P r-1 ) / (ΔV p / V)ΔV p =V r ×Δt×SQ p =(0.046 MPa-0 MPa) / (22.88 mm 3 / 212,049mm 3 ) = 426.3MPa is calculated. Note that ΔVp = 0.029mm / s × 0.1s × 7,854mm 2 -0mm 3 =22.88mm 3 , P r =0.046MPa P r-1 = 0MPa, V = 15,700mm 3 +π / 4×1002mm 2 ×25mm=212,049mm 3 It is.

[0328] Next, the corrected bulk modulus K' is set as the bulk modulus K' in the second cycle (step S50).

[0329] Next, the calculation of the command movement speed Vr is performed in the same manner as in the first cycle (step S46) (step S51). Here, the command movement speed V r =V rp +V rq = 0.028mm / s + 0.150mm / s = 0.178mm / s. Note that ΔP = Pt - Pr = 0.09MPa - 0.046MPa = 0.044MPa, Xr = 24.98mm, Vrp = (0.044MPa / 426.3MPa) (15,700mm 3 +7,854mm 2 ×24.98mm) / 0.1s / 7,854mm 2 = 0.028 mm / s, Qp = π × (12 mm) 3 / 32×{0.046MPa×12mm / (4×42,500kg / (m s 2-0.25 )×2mm)} 1 / 0.25 ×0.1s=117.86mm 3 , Vrq=117.86mm 3 / 0.1s / 7,854mm 2 =0.150mm / s.

[0330] Next, the moving speed of the first torpedo 14 is set to the instructed moving speed V calculated in step S51. r A drive command value is output to the motor 16a so as to satisfy the following equation (step S52).

[0331] From the second cycle onwards, the above steps S48 to S52 are repeatedly executed until it is determined that the cycle is the final one (step S53: YES), that is, until it is determined that the first torpedo 14 has reached the bottom dead center. Whether or not the first torpedo 14 has reached the bottom dead center can be determined based on the detection value (position detection value) of the potentiometer 16f.

[0332] Next, the same processes as steps S40 to S52 are executed until the second torpedo 15 moves toward the Z-axis + side and reaches the Z-axis - side (bottom dead center) (step S54: YES).

[0333] As described above, according to the second embodiment, it is possible to provide an injection molding machine that can optimally control the discharge amount while operating.

[0334] This is because the device is equipped with a movement speed control unit 33A that controls the movement speed of the piston so that it becomes the commanded movement speed (the commanded movement speed which is the sum of the pressure component of the movement speed of the piston (first torpedo 14 or second torpedo 15), where the pressure applied to the molten resin in the cylinder becomes the target pressure, and the flow rate component of the movement speed of the piston, where the flow rate of the molten resin discharged from the discharge nozzle 18a per unit time becomes the predicted outflow volume).

[0335] Furthermore, according to embodiment 2, the predicted outflow rate is calculated from the actually measured pressure, and the target moving speed of the piston (first torpedo 14 or second torpedo 15) is calculated, thereby making it possible to control the discharge flow rate without measuring the actual outflow rate, and therefore it is possible to control the discharge flow rate while operating the injection molding machine 2A.

[0336] Furthermore, according to the second embodiment, in the initial cycle of discharge (for example, the first cycle of the first torpedo in FIG. 27), the target command flow rate can be quickly reached by using the pre-stored bulk modulus.

[0337] Moreover, according to the second embodiment, it is possible to adjust the flow rate with high accuracy according to the state in which air is entrained in the molten resin.

[0338] Moreover, according to the second embodiment, the target pressure can be calculated in consideration of the type (material type) of the molten resin, the temperature, and the nozzle dimensions, and the discharge flow rate can be controlled.

[0339] This is because the device is provided with a movement speed control section (one example of the pressure control section of the present invention) that controls the pressure of the molten resin inside the cylinder so as to reach the target pressure.

[0340] Moreover, according to the second embodiment, the target pressure of the molten resin is calculated using the pseudoplastic viscosity that varies with temperature, thereby enabling accurate control of the resin discharge flow rate.

[0341] Furthermore, according to the second embodiment, even when a plurality of resin material types are used, the target pressure of the molten resin can be calculated using the pseudoplastic viscosity that differs depending on the resin material type, thereby enabling accurate control of the resin discharge flow rate.

[0342] According to the second embodiment, the pseudoplastic viscosity for each type of resin and each temperature is stored in advance, so that the calculation load for calculating the target pressure can be reduced. Also, the target command flow rate can be quickly achieved from the first cycle of discharge.

[0343] Furthermore, according to embodiment 2, the movement speed control unit 33A can more accurately control the movement speed of the piston (first torpedo 14 or second torpedo 15) to the target pressure by feedforward control using the bulk modulus of the molten resin.

[0344] Furthermore, according to the second embodiment, the predicted outflow rate is calculated from the actually measured pressure, and the instructed moving speed of the piston (first torpedo 14 or second torpedo 15) is calculated, thereby making it possible to control the discharge flow rate without measuring the actual outflow rate, and therefore it is possible to control the discharge flow rate while the injection molding machine is operating.

[0345] Moreover, according to the second embodiment, a corrected bulk modulus calculation unit 34A is provided which corrects the bulk modulus based on the amount of pressure change calculated from the actual pressure measurement and the substantial pressurized volume, so that a highly accurate flow rate can be obtained according to the degree of air entrainment in the molten resin.

[0346] Furthermore, according to the second embodiment, the modified bulk modulus calculation unit 34A modifies the bulk modulus only when the difference between the measured pressure and the target pressure is equal to or greater than a predetermined value, so that modification can be performed only when the value of the bulk modulus needs to be corrected.

[0347] Moreover, according to the second embodiment, the following effects are achieved.

[0348] The flow rate control of the resin discharge nozzle 18a described in the second embodiment is preferably applied to a 3D printer that forms and layers resin beads (molten resin discharged from the nozzle 18a that solidifies into a thread-like shape) from resin pellet material (which is usually distributed in large quantities industrially and is therefore much cheaper than the filaments used in conventional 3D printers such as those made by Stratasys, for example).

[0349] The reason for this is that it has the potential to solve the following four problems:

[0350] <Assignment 1> In a 3D printer (injection molding machine 2A or injection molding device 1 equipped with it), it is required to be able to form resin beads of uniform thickness even if the moving speed of nozzle 18a changes. In other words, it is required to detect the moving speed and quickly respond to the flow rate according to it.

[0351] <Task 2> It is difficult to measure the actual flow rate of the resin discharge nozzle while operating the 3D printer with the resin nozzle assumed in this invention. For this reason, a method of controlling the flow rate based on the measured value of the resin discharge pressure is generally adopted.

[0352] <Assignment 3> However, the inventor found that the actual flow rate varies considerably even at the same pressure depending on the type of resin material, the temperature of the molten resin, and the diameter of the discharge hole. At high temperatures, the melt viscosity decreases, so the flow rate is likely to increase relative to the pressure. In addition, the larger the nozzle diameter, the smaller the range affected by wall friction, so the apparent viscosity decreases and the flow rate is likely to increase relative to the pressure. In addition, since the molten resin is a non-Newtonian fluid, the larger the flow rate, the lower the apparent viscosity and the larger the flow rate is. It is desirable for a single 3D printer to be able to handle various resin types, various molten resin temperatures, and diameters from extremely small diameters (e.g., φ0.5 mm) to large discharge hole diameters (e.g., φ12 mm). (For example, when comparing the production of a small object such as a pen case with a large object such as a minivan, the time required for one layer of additive manufacturing changes, so it is necessary to change the temperature of the resin and the nozzle diameter depending on the amount of heat dissipated until the next layer is stacked.)

[0353] <Task 4> The inventors have found the following. That is, one of the problems with using resin pellet materials is that the plasticization process differs for each stroke depending on the filling condition of the pellets. As a result, even with the same compressed volume, the actual pressure rise differs (this is due to differences in bulk modulus) depending on the melting condition (degree of air entrapment), and as a result, the flow rate also differs.

[0354] In the second embodiment, in order to solve the above problems 1 to 4, material property values ​​for various resin types and various molten resin temperatures are stored in advance as constants in data tables 21 to 23, the type of resin to be filled is input, the temperature of the molten resin is measured, and the corresponding constants and the diameter of the attached discharge hole (nozzle diameter) are input to calculate the target pressure for discharging the designated flow rate calculated from the moving speed. This solves the above problems 1 and 3.

[0355] Next, to reach the target pressure, the moving speed of the torpedo (first torpedo 14 or second torpedo 15) that generates the pressurized amount calculated from the difference with the actual measured pressure is controlled by the sum of the moving speed of the torpedo that generates the pressurized amount and the moving speed of the torpedo that corresponds to the outflow amount while the torpedo is moving. Since it is difficult to directly measure the outflow amount, a flow rate predicted from the actual measured pressure is used. When calculating the moving speed of the torpedo that generates the pressurized amount, in the first cycle of discharge (for example, the first cycle of the first torpedo in Figure 27), feedforward control is performed by using the corresponding bulk modulus in the data table, and the target indicated flow rate is quickly reached. This solves the above problem 2.

[0356] In subsequent cycles (for example, the second cycle of the first torpedo in Fig. 27 and thereafter), the pressure change resulting from the movement of the torpedo is actually measured, the volume change calculated from the torpedo position detection result and the "effective pressurized volume" is calculated by subtracting the outflow volume calculated by the above formula 11 from the actual measured pressure, and the corrected bulk modulus is calculated from the pressure change and the "effective pressurized volume," which is then used to calculate the indicated movement speed, thereby making it possible to obtain a highly accurate flow rate according to the degree of air entrainment in the molten resin. This solves the above problem 4.

[0357] Next, the advantages of the second embodiment will be further described in comparison with the first to third comparative examples.

[0358] <Comparative Example 1> In Comparative Example 1 (Patent No. 5920859), the flow rate of the resin plasticized by the screw is adjusted by a gear pump placed immediately afterwards.

[0359] The advantages of embodiment 2 over comparative example 1 are as follows: In other words, in embodiment 2, instead of adjusting the flow rate of the resin plasticized by the screw with a gear pump located immediately behind it, the resin plasticized by the torpedo is temporarily stored in a plasticization chamber, and the flow rate is controlled by the moving speed of the torpedo controlled by an actuator during discharge, so that the gear pump at the tip of the nozzle in comparative example 1 and a piston member that can move back and forth to change the volume of the internal space of the nozzle are not required, and there is an advantage that the structure can be simplified and made small.

[0360] <Comparative Example 2> In Comparative Example 2 (Patent No. 4166746), when it is desired to control the outflow amount of molten resin by pressure and temperature, the nozzle is kept in a closed state and the change characteristics of the compression ratio C(P, T) are obtained. The advantages of the second embodiment over the second comparative example are as follows: That is, the second embodiment has an advantage that a process of measuring characteristic values ​​before the injection process is not required, since the material property values ​​required for calculating the instruction value for driving the actuator that controls the torpedo moving speed from the instruction flow rate (target flow rate) are stored as constants in a data table in the device.

[0361] <Comparative Example 3> In Comparative Example 3 (JP Patent Publication No. 16195), it is assumed that the bulk modulus of the molding material changes depending on the position of the plunger, and the actual injection flow rate value of the molding material injected from the nozzle is calculated. The advantages of the second embodiment over the third comparative example are as follows. That is, the second embodiment has the advantage that the process of measuring the constant ABC that determines the bulk modulus before the injection process required in the third comparative example is not required. The reason for this is that the second embodiment uses the bulk modulus in the data table only in the first cycle (for example, the first cycle of the first torpedo in FIG. 27), but from the second cycle (for example, the second cycle of the first torpedo in FIG. 27 onwards), the corrected bulk modulus can be calculated for each cycle while performing the injection process, so that the value takes into account the degree of entrapment of air, and an effect equivalent to that of the third comparative example can be obtained.

[0362] The difference between the feedback control of Comparative Example 3 and the second embodiment will be described in the following I, and the reason why the second embodiment can obtain the corrected bulk modulus while performing the injection process will be described in the following II.

[0363] I: In Comparative Example 3, the "actual flow rate" (as it is called in Comparative Example 3) is calculated from the results of pressure and position measurements, and feedback control is performed based on the difference from the target flow rate. However, the nozzle assumed in embodiment 2 does not have a means for measuring the true actual flow rate. For this reason, embodiment 2 (the technical concept of the present invention) uses open-loop control for the flow rate even from the second cycle onwards. In other words, the present invention is to use the actually measured pressure to determine the corrected bulk modulus, and to improve the prediction accuracy of the torpedo movement speed to obtain the indicated flow rate (target flow rate).

[0364] II: The reason why the second embodiment can calculate the corrected bulk modulus while performing the injection process is that the volume change due to the movement of the torpedo is regarded as the sum of the "actual pressurized volume" (the compressed volume that contributes to increasing the pressure) and the amount equivalent to the outflow, and the outflow amount is treated as the "predicted outflow amount" calculated with high accuracy from the actual measured pressure using the above equation 11. By doing so, the volume change due to the movement of the torpedo is also treated as a highly accurate value compared to the actual position that can be measured by the position sensor (potentiometers 16f, 17f), and the "actual pressurized volume", which is the difference between the latter and the former, can be calculated with high accuracy while performing the injection process (= while moving the torpedo and allowing the resin to flow without closing the nozzle).

[0365] In the second embodiment, the corrected bulk modulus is calculated using the measured pressure, the volume change due to the movement of the torpedo, and the "predicted outflow volume," but as shown in the above formula 11, the measured pressure is used to calculate the "predicted outflow volume," but the bulk modulus is not used. Therefore, the corrected bulk modulus can be calculated independently of the bulk modulus.

[0366] On the other hand, in Comparative Example 3, the bulk modulus K(z) is used in addition to the measured pressure P° to calculate the "actual flow rate q°" (as it is called in Comparative Example 3). Therefore, even if the "effective pressurized volume" in embodiment 2 is calculated by subtracting the "actual flow rate q°" from the volume change As·Z° due to the movement of the torpedo and an attempt is made to calculate the corrected bulk modulus from this and the measured pressure P°, the predicted value (corrected bulk modulus) is used in the calculation process of the predicted value (corrected bulk modulus), which results in what is called a circular reference in Excel and makes it impossible to perform the calculation.

[0367] Moreover, in the second embodiment, a target pressure for a desired indicated flow rate is calculated from a theoretical formula that determines the flow rate from viscosity and pressure (using the power law of non-Newtonian fluids in pseudoplastic flow, taking into account the shear rate dependency and temperature dependency of melt viscosity) using a value that takes into account the change in viscosity with respect to the temperature and flow rate of the molten resin, and is used for control, so that prediction accuracy is superior and the indicated flow rate (target flow rate) is reached quickly. Also, by preparing the power exponent n for various resins in a data table and preparing k obtained in advance for each temperature, accurate flow control of various resins is possible.

[0368] <Embodiment 3> Next, as a third embodiment, a method for automatically stopping a 3D printer when a modeling defect occurs and recording the defect position will be described.

[0369] The configuration of the injection molding machine 2B of the third embodiment is similar to the configuration of the injection molding machine 2A of the second embodiment (see FIG. 14), and therefore a description thereof will be omitted.

[0370] FIG. 30 is a configuration diagram of a control device 7B according to the third embodiment.

[0371] The configuration of the control device 7B of embodiment 3 is similar to the configuration of the control device 7A of embodiment 2 above (see FIG. 15). However, as shown in FIG. 30, the control device 7B of embodiment 3 additionally includes a position memory unit 25, an abnormality detection unit 35A, and an abnormality notification unit 70.

[0372] The position storage unit 25 is provided in, for example, the storage unit 20. The position storage unit 25 stores the nozzle position at the time when the abnormality detection unit 35A detects an abnormality (defect) (the operating position of the 3D printer from which the position of the nozzle 18a at the time when the abnormality (defect) is detected is known). FIG. 35 shows an example of the position of the nozzle 18a stored in the position storage unit 25.

[0373] The abnormality detection unit 35A is realized by the control unit 30 (processor) executing a predetermined program read from the storage unit 20 to the memory 40 (for example, RAM). The abnormality detection unit 35A may be realized by hardware. An example of the operation of the abnormality detection unit 35A will be described later.

[0374] The abnormality notification unit 70 is a display that displays the abnormality detected by the abnormality detection unit 35A or a speaker that outputs the abnormality detected by the abnormality detection unit 35A by voice.

[0375] <Example of operation of the abnormality detection unit 35A> Next, an example of the operation of the abnormality detection unit 35A (automatic stop determination and defect occurrence determination logic) will be described.

[0376] Fig. 31 is a flowchart of an operation example (automatic stop determination and defect occurrence determination logic) of the abnormality detection unit 35A. In Fig. 31, the area surrounded by a dotted line is the operation example (automatic stop determination and defect occurrence determination logic) of the abnormality detection unit 35A.

[0377] First, the target pressure Pt is determined (step S60). Specifically, the target pressure Pt of the molten resin upstream of the discharge hole is determined so as to obtain a flow rate calculated from the moving speed of the discharge nozzle 18a so as to form a resin bead of a certain thickness. The target pressure Pt can be determined, for example, by the target pressure calculation unit 31A described in the second embodiment.

[0378] Next, the measured pressure Pr is detected (step S61). The measured pressure Pr can be directly detected by a pressure sensor or the like, or can be estimated from a value (pressure detection value) of the pressure detection unit 65 or 66 (e.g., a strain gauge) attached to the outer circumferential surface of the first cylinder 11 or the outer circumferential surface of the second cylinder 12.

[0379] Next, the pressure difference ΔP is calculated by the following equation 20 (step S62). ΔP=Pr-Pt (Formula 20) Here, Pr is the measured pressure and Pt is the target pressure.

[0380] Next, similarly to step S47, a drive command value is output to the motor 16a (step S63).

[0381] Next, it is determined whether ΔP satisfies a predetermined standard ST1 or standard ST2 (step S64).

[0382] The criterion ST1 is, for example, ΔP>threshold Pmax. The threshold Pmax is a positive value, and is, for example, a relatively large value that can be determined in advance by an experiment. The criterion ST1 (threshold Pmax, etc.) is, for example, stored in the memory unit 20. The criterion ST1 is satisfied when the actual flow rate Q becomes smaller than the target flow rate (instructed flow rate) due to clogging of the discharge nozzle 18a (discharge hole) with unmelted resin pieces or dust. The reason for this is that if the actual flow rate Q is smaller than the target flow rate, the compression amount of the resin in the cylinder 11 becomes larger than expected, and the internal pressure rises, so that the actual pressure Pr becomes larger than the target pressure Pt.

[0383] The standard ST2 is, for example, ΔP<threshold Pmin. The threshold Pmin is a negative value, and is, for example, a relatively small value that can be determined in advance by an experiment. The standard ST2 (threshold Pmin, etc.) is stored, for example, in the storage unit 20. The standard ST2 is satisfied when the bulk modulus K of the molten resin becomes smaller than that without air mixing. The reason for this is that air is mixed into the molten resin when a bridge is caused to clog the supply pipe and the amount of resin pellets supplied is insufficient, when the filling rate to the nozzle 18a is low due to the pellet shape or the influence of static electricity, or when the amount of plasticized resin is below the volume of the first cylinder 11. The resin bead formed in this state contains a cavity defect caused by the expansion of the mixed air, which leads to a deterioration in the quality of the molded object.

[0384] If ΔP satisfies the standard ST1 (step S64: YES), it is determined that a modeling malfunction has occurred due to clogging of the discharge nozzle 18a, and modeling is automatically stopped (step S65). Stopping refers to stopping the discharge nozzle 18a (stopping the actuator (here, the motor 16a or 17a)) and stopping the gantry device 51. In this case (step S64: YES), the abnormality notification unit 70 may display the fact that the discharge nozzle 18a is clogged on a display or may output it by voice.

[0385] On the other hand, if ΔP satisfies the standard ST2 (step S64: YES), it is determined that the entrapment of air into the molten resin is excessive, and a molding defect occurs, and the molding is automatically stopped (step S65). In this case (step S64: YES), the abnormality notification unit 70 may display on a display or output by voice that the entrapment of air into the molten resin is excessive.

[0386] On the other hand, if it is determined in step S64 that ΔP does not satisfy the criteria ST1 and ST2 (step S64: NO), it is determined whether ΔP satisfies a predetermined criterion DF1 (step S66). The criterion DF1 is, for example, ΔP<threshold P DF The threshold P DF is a negative value and is greater than the threshold Pmin. DFcan be determined in advance, for example, through experiments. DF etc.) are stored in the storage unit 20, for example.

[0387] If ΔP satisfies the criterion DF1 (step S66: YES), it is considered that there is a somewhat large amount of air entrapment in the molten resin (void defect) (however, the additively manufactured object can be used as a product), so the nozzle position (the operating position of the 3D printer at which the position of the nozzle 18a at the time the abnormality (defect) was detected is known) is recorded in the position memory unit 25 so that the location of the void defect can be confirmed later (step S67). In this case, the abnormality notification unit 70 may display on the display that there is a somewhat large amount of air entrapment in the molten resin (and the nozzle position), or may output this by voice.

[0388] On the other hand, if it is determined in step S66 that ΔP does not satisfy the criterion DF1 (step S66: NO), it is determined whether the number of occurrences of DF1 satisfies a criterion ST3 (step S68). DF The predetermined number of times is determined in advance as a total cumulative number of times or a cumulative number of times within a predetermined period of time. The standard ST3 (predetermined number of times, etc.) is stored in the storage unit 20, for example.

[0389] If the number of occurrences of DF1 satisfies the standard ST3 (step S68: YES), it is determined that a molding defect has occurred (frequent occurrence of void defects), and the molding is automatically stopped (step S69). In this case, the abnormality notification unit 70 may display the fact that void defects occur frequently on a display or may output the same by voice.

[0390] On the other hand, if it is determined in step S68 that the number of occurrences of DF1 does not satisfy the standard ST3 (step S68: NO), the process returns to step S60 and the processes from step S60 onwards are repeatedly executed.

[0391] <Other Operation Examples of the Abnormality Detection Unit 35A> Next, another operation example (automatic stop determination and defect occurrence determination logic) of the abnormality detection unit 35A will be described.

[0392] Fig. 32 is a flowchart of another operation example (automatic stop determination and defect occurrence determination logic) of the abnormality detection unit 35A. In Fig. 32, the area surrounded by a dotted line is another operation example (automatic stop determination and defect occurrence determination logic) of the abnormality detection unit 35A.

[0393] FIG. 32 is a flowchart common to an example of operation of the first torpedo 14 in the first cycle and the second cycle and thereafter, and an example of operation of the second torpedo 15 in the first cycle and the second cycle and thereafter.

[0394] Below, an example of the operation of the first cycle (S70-S73) and the second and subsequent cycles (S74-S88) of the first torpedo will be described as representative examples. The example of the operation of the first cycle (S70-S73) and the second and subsequent cycles (S74-S88) of the second torpedo are similar to the example of the operation of the first cycle and the second and subsequent cycles of the first torpedo, so description thereof will be omitted.

[0395] First, an example of the operation of the first cycle of the first torpedo 14 (S70 to S73) will be described.

[0396] First, the target pressure Pt is determined (calculated) (step S70).

[0397] Next, the measured pressure Pr is detected (step S71).

[0398] Next, similarly to step S45 above, the bulk modulus K is set (step S72).

[0399] Next, similarly to step S47, a drive command value is output to the motor 16a (step S73).

[0400] Next, an example of the operation from the second cycle onwards (S74 to S101) will be described.

[0401] First, the target pressure Pt is determined (calculated) (step S74).

[0402] Next, the measured pressure Pr is detected (step S75).

[0403] Next, the pressure difference ΔP is calculated by the above formula 20 (step S76).

[0404] Next, the actual position X r is detected (step S77).

[0405] Next, similarly to step S31 above, the corrected bulk modulus K' is calculated by the above formula 18 (step S78).

[0406] Next, the difference ΔK in bulk modulus is calculated by the following formula 21 (step S79). ΔK=K´-K···(Formula 21) where K' is the modified bulk modulus and K is the bulk modulus.

[0407] Next, similarly to step S73, a drive command value is output to the motor 16a (step S80).

[0408] Next, it is determined whether ΔP satisfies a predetermined standard ST4 (step S81). The standard ST4 is, for example, ΔP>threshold Pmax. The threshold Pmax is a positive value, and is, for example, a relatively large value that can be determined in advance by an experiment. The standard ST4 (threshold Pmax, etc.) is, for example, stored in the storage unit 20.

[0409] The criterion ST4 is satisfied when the actual flow rate Q becomes smaller than the target flow rate (instructed flow rate) due to clogging of the discharge nozzle 18a (discharge hole) with unmelted resin pieces or dust, etc. The reason is that when the actual flow rate Q is smaller than the target flow rate, the compression amount of the resin in the molten resin storage chamber becomes larger than expected, the internal pressure rises, and the actual measured pressure Pr becomes larger than the target pressure Pt.

[0410] If ΔP satisfies the standard ST4 (step S81: YES), it is determined that a modeling defect has occurred due to clogging of the discharge nozzle 18a, and modeling is automatically stopped (step S82). Stopping refers to stopping the discharge nozzle 18a (stopping the actuator (here, the motor 16a or 17a)) and stopping the gantry device 51. In this case (step S81: YES), the abnormality notification unit 70 may display the fact that the discharge nozzle 18a is clogged on a display or may output it by voice.

[0411] On the other hand, if the result of the determination in step S81 is that ΔP does not satisfy the criterion ST4 (step S81: NO), it is determined whether ΔK satisfies a predetermined criterion ST5 (step S83). The criterion ST5 is, for example, ΔK<threshold Kmin. The threshold Kmin is a negative value, for example, a relatively small value that can be determined in advance by experiment. The criterion ST5 (threshold Kmin, etc.) is stored in, for example, the storage unit 20.

[0412] If ΔK satisfies the standard ST5 (step S83: YES), it is determined that a molding defect has occurred due to excessive air entrapment in the molten resin, and the molding is automatically stopped (step S84). In this case (step S83: YES), the abnormality notification unit 70 may display on a display or output by voice that excessive air is entrapped in the molten resin.

[0413] On the other hand, if it is determined in step S83 that ΔK does not satisfy the criterion ST5 (step S83: NO), it is determined whether ΔK satisfies a predetermined criterion DF2 (step S85). The criterion DF2 is, for example, ΔK<threshold K DF The threshold K DF is a negative value and is greater than the threshold Kmin. DF can be determined in advance, for example, by experiment. DF etc.) are stored in the storage unit 20, for example.

[0414] If ΔK satisfies the criterion DF2 (step S85: YES), it is considered that there is a somewhat large amount of air entrapment in the molten resin (void defect) (however, the additively manufactured object can be used as a product), so the nozzle position (the operating position of the 3D printer at which the position of the nozzle 18a at the time the abnormality (defect) was detected is known) is recorded in the position memory unit 25 so that the location of the void defect can be confirmed later (step S86). In this case, the abnormality notification unit 70 may display on the display that there is a somewhat large amount of air entrapment in the molten resin (and the nozzle position), or may output this by voice.

[0415] On the other hand, if it is determined in step S85 that ΔK does not satisfy the criterion DF2 (step S85: NO), it is determined whether the number of occurrences of DF2 satisfies a criterion ST6 (step S87). DF The predetermined number of times is determined in advance as a total cumulative number of times or a cumulative number of times within a predetermined period of time. The standard ST6 (predetermined number of times, etc.) is stored in the storage unit 20, for example.

[0416] If the number of occurrences of DF2 satisfies the criterion ST6 (Step S87: YES), it is determined that a molding defect has occurred (frequent occurrence of void defects), and the molding is automatically stopped (Step S88). In this case, the abnormality notification unit 70 may display the occurrence of a molding defect (frequent occurrence of void defects) on a display or may output it by voice.

[0417] On the other hand, if it is determined in step S87 that the number of occurrences of DF2 does not satisfy the criterion ST6 (step S87: NO), the process returns to step S74 and the processes from step S74 onwards are repeatedly executed.

[0418] <Example of a method for recording predicted positions of molding defects when used with a 3D printer> Next, an embodiment (hereinafter, referred to as embodiment 3) of a method for recording predicted positions of modeling defects when used in a 3D printer will be described.

[0419] FIG. 33 is a flowchart of an embodiment of a method for recording predicted positions of modeling defects when used in a 3D printer.

[0420] Fig. 33 corresponds to Fig. 27 with the addition of "automatic stop judgment and defect occurrence judgment logic (steps S64-S69; see the dotted line in Fig. 31)" and "automatic stop judgment and defect occurrence judgment logic (steps S81-S88; see the dotted line in Fig. 32)". The processing of each step in Fig. 33 has already been explained, so the explanation will be omitted.

[0421] Fig. 34 is a table summarizing the results (cycles 1 to 6) of Example 3. Specifically, Fig. 34 is a table summarizing the results when the processes of steps S40 to S47 in Fig. 33 were repeated once, and the processes of steps S48 to S52 were repeated five times.

[0422] In Figure 34, after cycle 4, ΔK(=K´-K)<threshold K DF (=-500), that is, it indicates that the standard DF2 has been satisfied. This is considered to be because there is a somewhat large amount of air entrapment in the molten resin (void defect), so in order to be able to check the location of the void defect later, the nozzle position (the operating position of the 3D printer at which the position of the nozzle 18a at the time when the abnormality (defect) was detected is known) is recorded in the position memory unit 25 (step S86). For example, it is recorded as shown in FIG. 35. FIG. 35 is an example of the predicted position of a modeling defect (the nozzle position at the time when the abnormality detection unit 35A detected the abnormality (defect)) stored in the position memory unit 25.

[0423] <Example of modeling stop due to nozzle clogging> Next, an embodiment of stopping modeling due to nozzle clogging (hereinafter, referred to as embodiment 4) will be described.

[0424] Fig. 36 is a table summarizing the results (cycles 1 to 5) of Example 4. Specifically, Fig. 36 is a table summarizing the results when the processes of steps S40 to S47 in Fig. 33 were repeated once, and the processes of steps S48 to S52 were repeated four times.

[0425] 36 shows that in cycle 5, ΔP>threshold Pmax (=2.0 MPa), i.e., criterion ST4 is met. This is thought to be because the flow rate decreased due to clogging of the nozzle 18a (discharge hole) with unmelted resin or dust, and the compressed volume increased, causing the pressure to suddenly rise. Since there is a risk of damaging the nozzle 18a if modeling is continued in this state, for example, a stop signal ST1 is output to automatically stop modeling (step S65).

[0426] As described above, according to embodiment 3, it is possible to provide an injection molding machine 7B that can detect the occurrence of an abnormality, such as when the discharge nozzle 18a (discharge hole) is clogged with unmelted resin pieces or when the discharged resin contains air.

[0427] This is because the abnormality detection unit 35A that detects an abnormality based on the target pressure and the actually measured pressure is provided.

[0428] Furthermore, according to the third embodiment, since it is possible to detect abnormalities as described above, it is possible to prevent the continuous production of additive manufacturing objects with many defects without human supervision, such as during autonomous driving.

[0429] Furthermore, if nozzle 18a continues to operate in an attempt to eject resin without noticing that it is clogged, the internal pressure will rise, which may result in damage to cylinders 11, 12 or the actuators (here, motors 16a, 17a). However, according to embodiment 3, when the pressure difference ΔP exceeds a threshold value or when the difference in bulk modulus exceeds a threshold value, modeling is stopped (steps S65, S82, S84), thereby preventing damage to cylinders 11, 12 or the actuators (here, motors 16a, 17a).

[0430] Furthermore, according to the third embodiment, since the abnormality notification section 70 is provided to notify the abnormality when the abnormality detection section 35A detects the abnormality, the occurrence of the abnormality can be easily grasped.

[0431] Furthermore, according to the third embodiment, when the abnormality detection unit 35A detects an abnormality, the position memory unit 25 is provided which stores the coordinates of the discharge nozzle 18a at the time the abnormality was detected. Therefore, by referring to the coordinates, it is possible to easily determine whether or not the abnormality (defect position) is at an acceptable level when inspecting the completed additive manufacturing body (three-dimensional model).

[0432] According to the third embodiment, when the difference (ΔP) between the target pressure and the measured pressure satisfies a first predetermined criterion (for example, criterion ST2: ΔP<threshold Pmin), the abnormality detection unit 35A detects a first abnormality (excessive air entrapment in the molten resin) and stops the discharge nozzle 18a (step S65). On the other hand, when the difference (ΔP) between the target pressure and the measured pressure satisfies a second predetermined criterion (for example, criterion DF1: ΔP<threshold P DF ) is satisfied, the abnormality detection unit 35A detects a second abnormality (a somewhat large amount of air entrapment in the molten resin (a void defect)), and stores the coordinates of the discharge nozzle 18a at the time the second abnormality was detected in the position memory unit 25 (step S67).

[0433] This allows, for example, that if the difference (ΔP) is large, the equipment will be stopped because it will break down if it is not stopped, but if the difference is within a certain degree of size, molding can continue and later inspection can be made to see if any defects have occurred.

[0434] Furthermore, according to the third embodiment, the abnormality detected by the abnormality detection section 35A when the target pressure is higher than the actual measured pressure and the abnormality detected by the abnormality detection section 35A when the target pressure is lower than the actual measured pressure may be different from each other.

[0435] In this way, it is possible to determine whether the abnormality is caused by air intrusion or by clogging with resin pieces, for example. <Fourth embodiment> Next, a 3D printer 300 will be described as a fourth embodiment.

[0436] <System configuration of 3D Printer 300 (overview)> FIG. 37 is a system configuration diagram of a 3D printer 300 according to the fourth embodiment.

[0437] As shown in Fig. 37, the 3D printer 300 of the fourth embodiment is a three-dimensional layered object modeling device that models a three-dimensional object (for example, a three-dimensional object indicated by the symbol Ob1 in Fig. 37) by stacking a resin bead RB, which is molten resin discharged from a discharge nozzle 18, on a base plate 4 (an example of a table of the present invention). The 3D printer 300 includes cylinders 11 and 12 that store molten resin, a discharge nozzle 18 that communicates with the cylinders 11 and 12, and a first piston unit 14 (and a second piston unit 15). Although not shown, a robot that moves in the Z-axis direction in addition to the X-axis and Y-axis directions, and a fixed base plate may also be used.

[0438] Hereinafter, the first piston unit 14 and the second piston unit 15 are also referred to as the first piston 14 and the second piston 15. The first piston 14 and the second piston 15 are examples of the pistons of the present invention. The first piston 14 and the second piston 15 are pistons that perform linear reciprocating motion within the cylinders 11 and 12, and move in a direction approaching the discharge nozzle 18 (downward in FIG. 37) to pressurize the molten resin within the cylinders 11 and 12, thereby discharging the molten resin from the discharge nozzle 18.

[0439] <3D Printer 300 System Configuration (Hardware Configuration)> As shown in Fig. 37, the 3D printer 300 includes the injection molding machine 2A of the second embodiment, a control device 7A, an XY-axis drive device 50 (gantry drive device), and a Z-axis drive device 60. The XY-axis drive device 50 is an example of a moving unit of the present invention. These have already been described in the above-mentioned second embodiment, and so description thereof will be omitted.

[0440] The first pressure detection unit 65 and the second pressure detection unit 66 may be means (e.g., pressure sensors) capable of measuring or estimating the pressure of the molten resin somewhere between the plasticizing chambers S2, S4 and the discharge nozzle 18 (resin discharge hole). The temperature detection unit 63 may be means (e.g., thermocouples) capable of measuring or estimating the temperature of the molten resin somewhere between the plasticizing chambers S2, S4 and the discharge nozzle 18 (resin discharge hole).

[0441] In FIG. 37, “constants due to resin” correspond to the data tables 21 to 23 in FIG. 15, and “nozzle diameter, nozzle length” correspond to the nozzle dimensions 24 in FIG.

[0442] Furthermore, the 3D printer 300 includes a modeling trajectory generating unit 80 and a piston linear actuator driving device 81.

[0443] The modeling trajectory generating unit 80 generates a modeling trajectory (hereinafter also referred to as a 3D print trajectory) by executing a predetermined process on the modeling model MD (e.g., 3D data describing a target three-dimensional object in STL (Standard Triangulated Language)). The modeling trajectory generating unit 80 is realized by, for example, executing a well-known software (program) called a slicer by an information processing device such as a personal computer (not shown).

[0444] The 3D printing trajectory is data for controlling the 3D printer 300 so that a desired three-dimensional object is formed (laminate), for example, a G-code. The G-code is data for controlling the 3D printer 300 to form a desired three-dimensional object for each layer divided (sliced) in the lamination direction (Z-axis direction), and includes, for example, a movement target position (XY coordinates) of the discharge nozzle 18.

[0445] For example, as shown in FIG. 37, assume that a three-dimensional object Ob1 (layered object) passing through a start point A, a reversal point B, and a midway point C is to be printed. In this case, a 3D print trajectory is generated that has the relationship between speed and time shown in FIG. 38(a) to FIG. 38(c). FIG. 38(a) is a graph showing the relationship between the nozzle speed in the X-axis direction and time, FIG. 38(b) is a graph showing the relationship between the nozzle speed in the Y-axis direction and time, and FIG. 38(c) is a graph showing the relationship between the magnitude of the nozzle translation speed and time. A, B, and C in FIG. 38 correspond to A, B, and C in FIG. 37. In FIG. 38(c), the "magnitude of the nozzle translation speed" refers to the magnitude of the speed vector calculated as a combination of the movement speeds of the X-axis and Y-axis (or the X-axis, Y-axis, and Z-axis).

[0446] The modeling trajectory generating unit 80 may generate all movement target positions between the start point and the end point as the 3D printing trajectory, or may generate only a movement target position at least one position ahead of the current position (the current position of the discharge nozzle 18). In the fourth embodiment, the latter is taken as an example. The piston linear actuator driving device 81 controls the motors 16a and 17a in accordance with the control from the control device 7A (based on the drive command value output from the control device 7A).

[0447] <Functional configuration of 3D printer 300> FIG. 39 is a functional block diagram of the 3D printer 300. The control unit 30A (processor) of the control device 7A executes a predetermined program read from the storage unit 20 into the memory 40 (e.g., RAM), and thereby functions mainly as an acquisition unit 30a, a piston control unit 30b, a temperature control unit 30c, a flow rate prediction unit 30d, and a discharge nozzle control unit 30e, as shown in Fig. 39. Some or all of these may be realized by hardware.

[0448] The acquisition unit 30a acquires the movement speed (translation speed) of the discharge nozzle 18.

[0449] The piston control unit 30b controls the movement (movement direction, movement speed) of the first piston 14 (or the second piston 15). Specifically, the piston control unit 30b controls the movement of the first piston 14 (or the second piston 15) based on the movement speed (translation speed) of the discharge nozzle 18. In particular, the piston control unit 30b controls the movement speed of the first piston 14 (or the second piston 15) by controlling the piston linear actuator driving device 81 so that the dimensions of the resin bead RB are constant.

[0450] The temperature control unit 30c controls the temperature of the molten resin stored in the cylinders 11 and 12 (plasticization chambers S2 and S4). The flow rate prediction unit 30d predicts the flow rate of the molten resin discharged from the discharge nozzle 18. The discharge nozzle control unit 30e controls the movement of the discharge nozzle 18. For example, the discharge nozzle control unit 30e controls the moving speed (translation speed) of the discharge nozzle 18 by controlling the XY-axis driving device 50 (an example of a moving unit of the present invention) based on the predicted discharge flow rate so that the dimensions of the resin bead RB are constant.

[0451] <Outline of operation of 3D printer 300> Next, an outline of the operation of the 3D printer 300 according to the fourth embodiment will be described. 40 is a flowchart showing the outline of the operation of the 3D printer 300. The following processing is realized by the control unit 30A (processor) executing a predetermined program read from the storage unit 20 into the memory 40 (for example, RAM).

[0452] First, a 3D printing trajectory is generated (Step S90). The 3D printing trajectory is generated by the printing trajectory generating unit 80 executing a predetermined process on the printing model MD.

[0453] Next, the discharge nozzle 18 is moved in the XY axis directions (step S91). This is realized by the control device 7A (discharge nozzle control unit 30e) outputting drive command values ​​for moving the injection molding machine 2A (discharge nozzle 18) along the 3D printing trajectory (modeling trajectory) to the XY axis drive device 50 (gantry drive device), and the XY axis drive device 50 moves the injection molding machine 2A (discharge nozzle 18) in the XY axis directions according to the control from the control device 7A (based on the drive command values ​​output from the control device 7A).

[0454] The process of step S91 is executed until the printing of one layer of the 3D printing trajectory (printing trajectory) is completed (step S92: YES).

[0455] Next, when the printing of the 3D print trajectory (printing trajectory) of one layer is completed (step S92: YES), the base plate 4 is moved a predetermined amount in the Z-axis direction (upward in FIG. 37) in order to print the 3D print trajectory of the next layer (step S93). This is realized by the control device 7A outputting a drive command value for moving the base plate 4 a predetermined amount in the Z-axis direction to the Z-axis drive device 60, and the Z-axis drive device 60 moving the base plate 4 a predetermined amount in the Z-axis direction (upward in FIG. 37) in accordance with the control from the control device 7A (based on the drive command value output from the control device 7A).

[0456] The above steps S91 to S93 are repeatedly executed until the desired three-dimensional object is completed.

[0457] In the above steps S91 to S93, the first piston 14 moves in a direction away from the discharge nozzle 18 (upward in FIG. 14), whereby the resin raw material M (resin pellets (plural)) supplied to the resin raw material supply chamber S1 (first space S1 in the cylinder 11) is plasticized, and the molten resin that is the plasticized resin raw material M is stored in the plasticization chamber S2 (second space S2 in the cylinder 11). The resin raw material supply chamber S1 is provided on the opposite side of the first piston 14 from the discharge nozzle 18 side (upper side in FIG. 14), and the plasticization chamber S2 is provided on the discharge nozzle 18 side of the first piston 14 (lower side in FIG. 14).

[0458] That is, a plurality of grooves 14f (hereinafter referred to as torpedo grooves 14f) extending linearly in the Z-axis direction are formed on the outer circumferential surface of the first piston 14 (see FIG. 7), and as the first piston 14 with the torpedo grooves 14f formed therein moves in a direction away from the discharge nozzle 18, the resin raw material M (resin pellets) is melted by friction when passing through the torpedo grooves 14f, and is stored as molten resin in the plasticization chamber S2 below. The molten resin stored in the plasticization chamber S2 is controlled to a temperature suitable for the molten resin stored in the plasticization chamber S2 (a temperature at which the molten state is maintained without being overheated) by the temperature control unit 30c controlling the first heating unit 61.

[0459] Similarly, in steps S91 to S93, the second piston 15 moves in a direction away from the discharge nozzle 18 (upward in FIG. 14), whereby the resin raw material M (resin pellets (plural)) supplied to the resin raw material supply chamber S3 (first space S3 in the cylinder 12) is plasticized, and the molten resin that is the plasticized resin raw material M is stored in the plasticization chamber S4 (second space S4 in the cylinder 12). The resin raw material supply chamber S3 is provided on the opposite side of the discharge nozzle 18 with respect to the second piston 15 (upper side in FIG. 14), and the plasticization chamber S4 is provided on the discharge nozzle 18 side with respect to the second piston 15 (lower side in FIG. 14).

[0460] That is, a plurality of grooves 15f (hereinafter referred to as torpedo grooves 15f) extending linearly in the Z-axis direction are formed on the outer circumferential surface of the second piston 15 (see FIG. 7), and as the second piston 15 with the torpedo grooves 15f formed therein moves in a direction away from the discharge nozzle 18, the resin raw material M (resin pellets) is melted by friction when passing through the torpedo grooves 15f, and is stored as molten resin in the plasticization chamber S4 below. The molten resin stored in the plasticization chamber S4 is controlled to a temperature suitable for the molten resin stored in the plasticization chamber S4 (a temperature at which the molten state is maintained without being overheated) by the temperature control unit 30c controlling the second heating unit 62.

[0461] In addition, in the above steps S91 to S93, the first piston 14 moves in a direction approaching the discharge nozzle 18 (downward in Figure 14) to pressurize the molten resin stored in the plasticization chamber S2, thereby discharging the molten resin stored in the plasticization chamber S2 from the discharge nozzle 18.

[0462] At this time, since the first piston 14 is provided with a backflow prevention function (check ring 14b; see Figures 7, 14, etc.), the molten resin in the plasticization chamber S2 does not flow back into the resin raw material supply chamber S1, and the molten resin stored in the plasticization chamber S2 can be pressurized.

[0463] Similarly, in steps S91 to S93, the second piston 15 moves in a direction approaching the discharge nozzle 18 (downward in Figure 14) to pressurize the molten resin stored in the plasticization chamber S4, thereby discharging the molten resin stored in the plasticization chamber S4 from the discharge nozzle 18.

[0464] At this time, since the second piston 15 is provided with a backflow prevention function (check ring 15b; see Figures 7, 14, etc.), the molten resin in the plasticization chamber S4 does not flow back into the resin raw material supply chamber S3, and the molten resin stored in the plasticization chamber S4 can be pressurized.

[0465] The first piston 14 and the second piston 15 move alternately (i.e., in opposite phases) in a direction approaching the discharge nozzle 18 to pressurize the molten resin stored in the plasticization chambers S2 and S4. At that time, the discharge periods overlap (overlap). Therefore, the molten resin stored in the plasticization chambers S2 and S4 can be discharged continuously from the discharge nozzle 18a without interruption.

[0466] <Details of 3D Printer 300 operation> Next, the operation of the 3D printer 300 according to the fourth embodiment will be described in detail.

[0467] 41 is a detailed flowchart of the operation of the 3D printer 300. The following processing is realized by the control unit 30A (processor) executing a predetermined program read from the storage unit 20 to the memory 40 (for example, RAM).

[0468] First, a 3D printing trajectory is generated (Step S100). The 3D printing trajectory is generated by the printing trajectory generating unit 80 executing a predetermined process on the printing model MD. Next, a drive instruction value is output to a device (XY-axis drive device 50) that moves the discharge nozzle (step S101). Specifically, the control device 7A (discharge nozzle control unit 30e) outputs a drive command value to the XY-axis drive device 50 (gantry drive device) for moving the injection molding machine 2A (discharge nozzle 18) along the 3D printing trajectory (modeling trajectory). The moving speed of the discharge nozzle 18 is input (step S40) and calculated (step S46) according to the flowchart of FIG. 27, for example. The moving speed of the discharge nozzle 18 (moving speed at the start of movement) may be input as an initial value or may be stored in a storage unit such as a data table.

[0469] This causes the discharge nozzle 18 to move (step S102). Specifically, the XY-axis drive device 50 moves the injection molding machine 2A (discharge nozzle 18) in the X and Y-axis directions in accordance with the control of the control device 7A (based on the drive command value output from the control device 7A).

[0470] Next, the translational speed V of the discharge nozzle 18 R (Step S103). The translational speed V R may be calculated (measured) using a laser measuring device or the like, or may be calculated by other methods. For example, it may be calculated by the discharge nozzle movement distance / discharge nozzle movement time between two different points. The acquisition unit 30a acquires the calculated movement speed (translation speed V R ) is acquired. Note that the moving speed of the discharge nozzle 18 (translational speed V R ) may be obtained from a controller (not shown) of the XY-axis drive unit 50 (gantry drive unit).

[0471] Next, the flow rate Q i (Step S104) The amount of flow Q i The flow rate Q is a flow rate (indicated flow rate) at which the size (e.g., diameter) of the resin bead RB extruded from the extrusion nozzle 18 becomes constant. i can be calculated, for example, by the following formula 22.

[0472] Q i =V R ×S...(Formula 22) However, V R is the translational speed of the discharge nozzle 18 calculated and acquired in step S103, and S is the cross-sectional area of ​​the resin bead RB discharged from the discharge nozzle 18. i and the translational velocity V of the discharge nozzle 18 R 4 is a graph showing the relationship between

[0473] Next, the velocity V of the linear motion of the first piston 14 (or the second piston 15) r (Step S105). The velocity V of the linear motion of the first piston 14 (or the second piston 15) is calculated. r The flow rate of the molten resin discharged from the discharge nozzle 18 is the flow rate Q iThe velocity of the first piston 14 (or the second piston 15) to achieve the specified flow rate (specified flow rate), i.e., the specified movement velocity. The velocity V of the linear movement of the first piston 14 (or the second piston 15) r The (instructed movement speed) can be calculated by the above formula 17.

[0474] Next, a drive command value is output to the actuator that moves the first piston 14 (or the second piston 15) (step S106). Specifically, the control device 7A (piston control unit 30b) sets the moving speed of the first piston 14 (or the second piston 15) to the command moving speed V calculated in step S105. r A drive command value for achieving this is output to the piston linear movement actuator drive device 81, and the piston linear movement actuator drive device 81 controls the motor 16a (or motor 17a) in accordance with the control from the control device 7A (based on the drive command value output from the control device 7A).

[0475] Next, the molten resin is discharged from the discharge nozzle 18 (step S107). Specifically, the piston linear actuator driving device 81 controls the motor 16a (or motor 17a) in accordance with the control from the control device 7A (based on the drive command value output from the control device 7A), so that the first piston 14 (or the second piston 15) moves in a direction approaching the discharge nozzle 18 (downward in FIG. 14), and pressurizes the molten resin stored in the plasticization chamber S2 (or plasticization chamber S4). As a result, the molten resin (extrusion flow rate Q i 1000 molten resin) is extruded.

[0476] The processes in steps S101 to S107 are repeatedly executed until the target three-dimensional object is completed. For example, the processes are executed at predetermined time intervals (for example, 0.1 seconds). As a result, the size of the resin bead RB discharged from the discharge nozzle 18 is controlled to a constant size.

[0477] As described above, the moving speed of the discharge nozzle 18 (translational speed V R), the speed V of the linear motion of the first piston 14 (or the second piston 15) which reciprocates linearly in the cylinder 11 (or the cylinder 12) in which the molten resin is stored is calculated based on the above. r By controlling the above, the size of the resin bead RB can be controlled to be constant (approximately constant).

[0478] <Examples of sculpture> Next, a specific example of shaping will be described. Fig. 43 shows an example of a three-dimensional object Ob1 (layered object) formed according to the flowchart of Fig. 41. A, B, and C in Fig. 43 correspond to A, B, and C in Figs. 37 and 38.

[0479] Referring to Figure 43, it can be seen that the dimensions of the resin bead RB are thinner than the desired thickness in the portion where the discharge nozzle 18 starts to move and accelerates (see feature 1 in Figure 43), and are thicker than the desired thickness in the U-turn portion where the discharge nozzle 18 decelerates and then accelerates (see feature 3 in Figure 43), but reach the desired thickness in the portion where the discharge nozzle 18 moves at a constant speed (see feature 2 in Figure 43).

[0480] Next, the advantages of the fourth embodiment will be further described in comparison with the fourth and fifth comparative examples.

[0481] <Comparative Example 4> Comparative Example 4 (US Patent Application Publication No. 2018 / 0056602) has the following problems.

[0482] <Assignment 1> In order to stabilize the dimensions of the resin bead, both the rotation speed of the extruder screw and the rotation speed of the gear pump gear must be adjusted based on the increase or decrease in the translation speed of the applicator head. Since there are two controlled targets, the adjustment is complicated and requires labor and costs. In addition, there may be an area where there is a limit to the adjustment in order to maintain a constant resin bead size.

[0483] The reason why problem 1 occurs is as follows. This is due to the following two structural features: First, plasticization by the screw and flow rate adjustment by the gear pump are carried out simultaneously. Second, the screw and gear pump are connected in series by a single flow path.

[0484] Since the gear pump and the screw are connected by a single flow path, the molten resin coming out of the screw must be adjusted immediately by the gear pump, and there may be an adjustment limit even if the flow rate is controlled by the rotation speed of both. For example, when the translation speed of the applicator head is very slow, the rotation speed of the gear pump is adjusted to a small value, and the rotation speed of the screw located upstream is also set to a small value. If it is too small, "since most of the melting energy is generated by the rotation of the extruder screw" (see paragraph 5 of the detailed explanation of Comparative Example 4), the material will not melt sufficiently, and the outflow will be insufficient, resulting in a thin resin bead.

[0485] <Task 2> There is a problem that the temperature of the molten resin rises (in the area where the flow rate is extremely high). This causes the resin to denature, resulting in defective molding, or it takes longer for the resin bead to solidify, making it necessary to extend the time until the next layer is molded, which results in longer molding times.

[0486] The reason why problem 2 occurs is as follows. In other words, when the translation speed of the applicator head is high, a large flow rate is also required, but "since most of the melting energy is generated by the rotation of the extruder screw" (see paragraph 5 of the detailed explanation of Comparative Example 4), "it also changes the amount of thermal energy generated to melt a flowable material such as a thermoplastic resin, resulting in an increase in temperature..." (see paragraph 5 of the detailed explanation of Comparative Example 4).

[0487] <Assignment 3> In areas where the rate of change of the nozzle translational speed is large (high acceleration), a delay occurs in the rise of the flow rate, and compensation must be made using a pressure sensor to keep the dimensions of the resin bead constant, complicating control (see claims 14 to 16 of Comparative Example 4).

[0488] The reason why problem 3 occurs is as follows. That is, a rapid change in the rotational speed of the extruder screw does not immediately result in a rapid change in the flow rate of the molten flowable material. There is a substantial delay between the change in the extruder screw speed and the resulting change in the flow rate of the molten material (see paragraph 5 of the detailed description of Comparative Example 4).

[0489] The advantages of the fourth embodiment over the fourth comparative example are as follows. That is, in the fourth embodiment, the timing of plasticization and flow rate adjustment are controlled to be shifted, and to achieve this, a gear pump and a screw are not connected in series with one flow path, and a molten resin is formed from the resin raw material M (resin pellets) and the flow rate is adjusted and discharged by a method that does not use a gear pump and a screw. Also, the molten resin can be temporarily stored and the temperature adjusted. This solves the above problems 1 and 2.

[0490] Moreover, in the fourth embodiment, the moving speed (translational speed) of the discharge nozzle 18 is controlled based on the actual discharge flow rate of the molten resin, thereby solving the above-mentioned problem 3.

[0491] <Comparative Example 5> Comparative Example 5 (JP 2020-82558 A) has the following problems. <Assignment 1> There are many components required for the suction operation, which complicates control, resulting in increased costs for the device.

[0492] The reason why problem 1 occurs is as follows. That is, the following two elements are necessary to perform the suction operation: First, butterfly valve 72 is closed, and second, suction portion 75 is controlled to be pulled.

[0493] <Task 2> The need for three actuators makes control more complicated, which results in increased costs for the device.

[0494] The reason why problem 2 occurs is as follows. That is, actuators are required for driving the screw, the butterfly valve, and the suction portion 75.

[0495] <Assignment 3> If the screw continues to turn with the butterfly valve 72 closed, the resin may overflow or the pressure may increase too much, causing more resin than necessary to come out of the discharge hole the next time the butterfly valve 72 is opened.

[0496] <Task 4> If you tighten the screw to avoid problem 3 above, the next time you want to take it out it won't come out right away.

[0497] The reasons why problems 3 and 4 above occur are as follows. That is, this is because the extruder (plasticization section) and the gear pump (flow rate control section) are arranged in series.

[0498] The advantages of the fourth embodiment over the fifth comparative example are as follows. That is, in the fourth embodiment, the plasticizing section and the flow rate control section are configured with the same members (first piston 14, second piston 15), the molten resin is discharged by the forward movement of the pistons 14, 15, the flow rate is controlled by the speed, and the molten resin is sucked in by the backward movement. This solves the above problems 1 and 2. In the fourth embodiment, the plasticizing section and the flow rate control section are configured with the same members (first piston 14, second piston 15), and the plasticizing and discharging are staggered in time (the molten resin is plasticized first, and then temporarily stored and discharged later). This solves the above problems 3 and 4.

[0499] As described above, according to the fourth embodiment, the controllability of the flow rate of the molten resin discharged from the discharge nozzle 18 can be improved.

[0500] This is because the flow rate of the molten resin is controlled by controlling the movement of the first piston 14 (or the second piston 15) which moves back and forth in a straight line within the cylinder 11 (or the cylinder 12) in which the molten resin is stored, rather than by controlling the rotation of both the extruder (screw) and the gear pump (simplification of flow rate control).

[0501] According to the fourth embodiment, the speed V of the linear motion of the first piston 14 (or the second piston 15) that reciprocates linearly in the cylinder 11 (or the cylinder 12) in which the molten resin is stored is calculated based on the moving speed (translational speed) of the discharge nozzle 18. r By controlling the above, the size of the resin bead RB can be controlled to be constant (approximately constant).

[0502] According to the fourth embodiment, the resin raw material M is plasticized and stored, and then the stored molten resin is pressurized by the first piston 14 (or the second piston 15) that moves linearly back and forth, so that the molten resin can be discharged from the discharge nozzle 18. This improves controllability compared to the above-mentioned Patent Document 1, in which the rotations of both the extruder (screw) and the gear pump are controlled simultaneously. In addition, the first piston 14 (or the second piston 15) that moves linearly back and forth can plasticize the resin raw material M (generate and store the molten resin) and control the flow rate of the stored molten resin. In addition, since the first piston 14 (or the second piston 15) can plasticize the resin raw material M and control the flow rate of the stored molten resin, there is no need to provide a separate mechanism for plasticizing the resin raw material M.

[0503] Furthermore, according to the fourth embodiment, the temperature of the molten resin stored in cylinder 11 (or cylinder 12) can be controlled to a temperature suitable for the molten resin (a temperature at which the molten state is maintained without being overheated).

[0504] Furthermore, according to embodiment 4, since there are multiple combinations of cylinders and pistons (for example, a combination of cylinder 11 and first piston 14, and a combination of cylinder 12 and second piston 15), molten resin can be ejected continuously without interruption. Furthermore, according to the fourth embodiment, a 3D printer 300 can be provided that has a simpler nozzle structure and a simpler control method, and that can obtain stable dimensions for the resin bead RB, within a range in which the rate of change of the movement speed (translational speed) of the discharge nozzle 18 is not excessively large.

[0505] <Embodiment 5> Next, another operation example 1 of the 3D printer 300 according to the fourth embodiment will be described as a fifth embodiment.

[0506] <Another operation example 1 of 3D printer 300> 44 is a detailed flowchart of another operation example 1 of the 3D printer 300. The following processing is realized by the control unit 30A (processor) executing a predetermined program read from the storage unit 20 to the memory 40 (for example, RAM).

[0507] First, a 3D printing trajectory is generated (Step S110). The 3D printing trajectory is generated by the printing trajectory generating unit 80 executing a predetermined process on the printing model MD. Next, a drive command value is output to a device (XY-axis drive device 50) that moves the discharge nozzle (step S111). Specifically, the control device 7A (discharge nozzle control unit 30e) outputs a drive command value to the XY-axis drive device 50 (gantry drive device) for moving the injection molding machine 2A (discharge nozzle 18) along the 3D printing trajectory (modeling trajectory).

[0508] This causes the discharge nozzle 18 to move (step S112). Specifically, the XY-axis drive device 50 moves the injection molding machine 2A (discharge nozzle 18) in the X and Y-axis directions in accordance with the control of the control device 7A (based on the drive command value output from the control device 7A).

[0509] Next, the translational speed V of the discharge nozzle 18 R (Step S113). The translational speed V of the discharge nozzle 18 is calculated. R may be calculated (measured) using a laser measuring device or the like, or may be calculated by other methods. For example, it may be calculated by the discharge nozzle movement distance / discharge nozzle movement time between two different points. The acquisition unit 30a acquires the calculated movement speed (translation speed V R ) is acquired. Note that the moving speed of the discharge nozzle 18 (translational speed V R ) may be obtained from a controller (not shown) of the XY-axis drive unit 50 (gantry drive unit).

[0510] Next, the flow rate Q i (Step S114) The amount of the extrusion Q i The flow rate Q is a flow rate (indicated flow rate) at which the size (e.g., diameter) of the resin bead RB extruded from the extrusion nozzle 18 becomes constant. i can be calculated, for example, by the following formula 22.

[0511] Q i =V R ×S...(Formula 22) However, V R is the translational speed of the discharge nozzle 18 calculated and acquired in step S113, and S is the cross-sectional area of ​​the resin bead RB discharged from the discharge nozzle 18. i and the translational velocity V of the discharge nozzle 18 R 4 is a graph showing the relationship between

[0512] Next, the velocity V of the linear motion of the first piston 14 (or the second piston 15) r (Step S115). The velocity V of the linear motion of the first piston 14 (or the second piston 15) is calculated. r The flow rate of the molten resin discharged from the discharge nozzle 18 is the flow rate Q iThe velocity of the first piston 14 (or the second piston 15) to achieve the specified flow rate (specified flow rate), i.e., the specified movement velocity. The velocity V of the linear movement of the first piston 14 (or the second piston 15) r The (instructed movement speed) can be calculated by the above formula 17.

[0513] Next, a drive command value is output to the actuator that moves the first piston 14 (or the second piston 15) (step S116). Specifically, the control device 7A (piston control unit 30b) sets the moving speed of the first piston 14 (or the second piston 15) to the command moving speed V calculated in step S115. r A drive command value for achieving this is output to the piston linear movement actuator drive device 81, and the piston linear movement actuator drive device 81 controls the motor 16a (or motor 17a) in accordance with the control from the control device 7A (based on the drive command value output from the control device 7A).

[0514] Next, the discharge pressure P r The discharge pressure P r is detected by the first pressure detection unit 65 and the second pressure detection unit 66.

[0515] Next, the discharge flow rate (predicted discharge volume Q P ) is predicted (step S118). P ) is predicted (calculated) by the flow rate prediction unit 30d. P can be calculated by the above formula 11.

[0516] Next, the molten resin is discharged from the discharge nozzle 18 (step S119). Specifically, the piston linear actuator driving device 81 controls the motor 16a (or motor 17a) in accordance with the control from the control device 7A (based on the drive command value output from the control device 7A), so that the first piston 14 (or the second piston 15) moves in a direction approaching the discharge nozzle 18 (downward in FIG. 14), and pressurizes the molten resin stored in the plasticization chamber S2 (or plasticization chamber S4). As a result, the molten resin (extrusion flow rate Q i 1000 molten resin) is extruded.

[0517] Next, the predicted discharge flow rate (predicted discharge Q P ) based on the translational velocity V of the discharge nozzle 18 i (Step S120). The translational speed V i The translational speed V of the discharge nozzle 18 is a speed at which the size (e.g., diameter) of the resin bead RB discharged from the discharge nozzle 18 becomes constant. i can be calculated, for example, by the following formula 23.

[0518] V i =Q P / S...(Formula 23) However, Q P is the discharge flow rate (estimated outflow rate) predicted in step S118, and S is the cross-sectional area of ​​the resin bead RB discharged from the discharge nozzle 18. i and the predicted discharge flow rate Q P 13 is a graph showing the relationship between the amount of water discharged and the predicted outflow amount.

[0519] Next, a drive instruction value is output to the device (XY-axis drive device 50) that moves the discharge nozzle (step S121). Specifically, the control device 7A (discharge nozzle control unit 30e) moves the injection molding machine 2A (discharge nozzle 18) at the translational speed V i The control unit 50 outputs drive command values ​​for moving the XY-axis drive unit 50 (gantry drive unit) in the XY-axis direction.

[0520] This causes the discharge nozzle 18 to move (step S122). Specifically, the XY-axis drive device 50 moves the injection molding machine 2A (discharge nozzle 18) in the X and Y-axis directions in accordance with the control of the control device 7A (based on the drive command value output from the control device 7A).

[0521] The processes in steps S113 to S122 are repeatedly executed until the target three-dimensional object is completed. For example, the processes are executed at predetermined time intervals (for example, 0.1 seconds). As a result, the size of the resin bead RB discharged from the discharge nozzle 18 is controlled to a constant size.

[0522] As described above, the moving speed (translational speed) of the discharge nozzle 18 on the 3D printer 300 is controlled. At that time, the flow rate Q of the discharge nozzle 18 is i is determined based on the moving speed (translational speed) of the target discharge nozzle 18, and then the linear motion speed V of the first piston 14 (or the second piston 15) is determined. r The resulting pressure P of the molten resin immediately before it comes out of the discharge nozzle 18 (discharge hole) is controlled. r Detect the pressure P r The actual discharge flow rate Q is calculated from the temperature of the molten resin and other constants. P and the predicted runoff volume Q P Based on this, the moving speed (translation speed) of the discharge nozzle 18 on the 3D printer 300 is controlled so that the dimensions of the resin bead RB are constant. P By controlling the moving speed (translational speed) of the discharge nozzle 18 based on the (predicted outflow amount), the size of the resin bead RB can be controlled to be constant (approximately constant).

[0523] <Examples of sculpture> Next, a specific example of shaping will be described. Fig. 46 shows an example of a three-dimensional object Ob2 (layered object) formed according to the flowchart of Fig. 44. A, B, and C in Fig. 46 correspond to A, B, and C in Figs. 37 and 38.

[0524] Referring to Figure 46, it can be seen that the dimensions of the resin bead RB are slightly thicker than the desired thickness at the U-turn portion where the discharge nozzle 18 decelerates and accelerates (see feature 2 in Figure 46), but that they reach the desired thickness at the portion where the discharge nozzle 18 accelerates at the start of its movement (see feature 1 in Figure 46), and that at the U-turn portion where the discharge nozzle 18 decelerates and accelerates (see feature 2 in Figure 46), they are thinner than the U-turn portion of embodiment 4 (see symbol Ob1 in Figure 46).

[0525] As described above, according to the fifth embodiment, it is possible to improve the controllability of the flow rate of molten resin discharged from the discharge nozzle 18. Also, when the nozzle is accelerated or decelerated, a difference may occur between the command flow rate and the actual discharge flow rate, but even in this case, the moving speed (translational speed) of the discharge nozzle 18 is controlled based on the actual discharge flow rate, so that it is possible to provide a 3D printer 300 that always provides stable dimensions for the resin bead RB. Additionally, according to the fifth embodiment, it is possible to achieve the same effects as those of the fourth embodiment.

[0526] Furthermore, according to the fifth embodiment, the moving speed of the discharge nozzle 18 is controlled based on the predicted discharge flow rate, thereby making it possible to control the size of the resin bead RB to be constant (approximately constant).

[0527] <Sixth embodiment> Next, another operation example 2 of the 3D printer 300 according to the fourth embodiment will be described as a sixth embodiment.

[0528] <Another operation example 2 of 3D printer 300> 47 is a detailed flowchart of another operation example 2 of the 3D printer 300. The following processing is realized by the control unit 30A (processor) executing a predetermined program read from the storage unit 20 to the memory 40 (for example, RAM).

[0529] First, a 3D object forming process is executed (step S130). The 3D object forming process is a process for forming a target 3D object by the 3D printer 300, and is, for example, the process of the flowchart in FIG. 27, the process of the flowchart in FIG. 41, or the process of the flowchart in FIG.

[0530] Following this 3D object formation process, it is determined whether it is a predetermined timing (step S131). The predetermined timing will be described later in specific examples 1 and 2 of the predetermined timing. If it is determined in step S131 that it is the predetermined timing (step S131: YES), leakage prevention process is executed (step S132). <Leak prevention treatment> The leakage suppression process is a process of moving the first piston 14 (or the second piston 15) a predetermined amount in a pullback direction (a direction in which the first piston 14 (or the second piston 15) moves away from the discharge nozzle 18). The amount of pullback movement (predetermined amount) will be described later in specific examples 1 and 2 of the predetermined timing.

[0531] The processes of steps S130 to S132 are repeatedly executed until the 3D object formation process ends (step S133: YES).

[0532] <Specific example of specified timing 1> A first specific example of the specified timing is the timing when the movement speed (translation speed) of the discharge nozzle 18 moving in the XY axis directions while discharging molten resin changes from non-zero to 0 (the timing when the moving discharge nozzle 18 stops).

[0533] <Example of pullback movement amount> It is desirable that the amount of pullback movement X (mm) of the first piston 14 (or the second piston 15) is a value that satisfies the following formula 24.

[0534] P t ×V0 / K / S < X ≦ (P t +0.1)×V0 / K / S (Formula 24) However, P t(relative to atmospheric pressure, unit MPa) is the pressure of the molten resin just before it is pulled back, V0 (mm 3 ) is the volume of the plasticization chamber, K (MPa) is the bulk modulus of the molten resin, and S (mm 2 ) is the cross-sectional area of ​​the first piston 14 (or the second piston 15), and 0.1 (MPa) is the atmospheric pressure.

[0535] This equation 24 is derived from the following two equations 25 and 26. ΔV=X×S (Formula 25) P t +0.1=ΔV / V0×K (Formula 26) According to the specific example 1 of the predetermined timing, the movement amount X (one example of the predetermined amount of the present invention) of the first piston 14 (or the second piston 15) in the pullback direction in step S132 is “P t By satisfying "×V0 / K / S < X", the pressure of the molten resin inside the discharge nozzle 18 (discharge hole) becomes lower than the pressure outside the discharge nozzle 18 (resin pressure; atmospheric pressure), so that the molten resin is pushed by the atmospheric pressure and retracted into the discharge nozzle 18 (discharge hole), thereby suppressing leakage of the molten resin from the discharge nozzle 18 (discharge hole). This makes it possible to suppress (suppress leakage) the molten resin from continuing to be discharged due to residual pressure, gravity, etc. As a result, the dimensions of the resin bead RB can be controlled to be constant (approximately constant).

[0536] On the other hand, the amount of movement X of the first piston 14 (or the second piston 15) in the pull-back direction in step S132 is equal to or less than "X ≦ (P t By satisfying "+0.1) × V0 / K / S", the pressure of the molten resin inside the discharge nozzle 18 (discharge hole) or inside the plasticization chamber S2 (or plasticization chamber S4) will not fall below (atmospheric pressure -0.1 MPa), i.e., an absolute vacuum, thereby preventing air from being entrained inside the plasticization chamber S2 (or plasticization chamber S4) or bubbles from being generated, thereby preventing defects from occurring at the timing of the next molding. That is, by preventing the differential pressure (pressure outside the discharge nozzle 18-pressure inside the discharge nozzle 18) that occurs when the first piston 14 (or the second piston 15) is moved in the retracting direction by the amount X from exceeding atmospheric pressure (e.g., 0.1 MPa), it is possible to prevent air from being entrained in the plasticization chamber S2 (or the plasticization chamber S4) or the generation of air bubbles. This is a condition empirically discovered by the present inventor for preventing air from being entrained in the plasticization chamber S2 (or the plasticization chamber S4) or the generation of air bubbles.

[0537] In addition, when calculating the movement amount X (mm), the pressure Pt of the molten resin immediately before being pulled back may be a value calculated by the pressure detection units 65, 66 (pressure sensors), may be an approximate value of the target pressure for obtaining the flow rate, or may be a target pressure calculated each time.

[0538] In addition, the volume of the plasticization chamber S2 (or the plasticization chamber S4) can be calculated from a value obtained from a position detection means such as a potentiometer attached to the actuator that drives the first piston 14 (or the second piston 15), the dead volume, and the cross-sectional area of ​​the first piston 14 (or the second piston 15).

[0539] The bulk modulus of the molten resin may be the value of the corresponding resin in the data table, or may be a general value representative of a general resin. The atmospheric pressure may be 0.1 MPa regardless of the weather. According to the specific example 1 of the pullback movement amount, it is possible to prevent the molten resin from being continuously discharged due to residual pressure, gravity, etc. As a result, the size of the resin bead RB can be controlled to be constant (approximately constant).

[0540] <Specific example of specified timing 2> A second specific example of the specified timing is a timing a specified time before the timing at which the movement speed (translation speed) of the discharge nozzle 18 moving in the XY axis direction while discharging molten resin is predicted to change from a value other than 0 (zero) to 0 (the moving discharge nozzle 18 stops).

[0541] The timing at which the movement speed of the discharge nozzle 18 is predicted to change from a value other than 0 to 0 is, for example, the timing at which the movement speed (translational speed) of the discharge nozzle 18, which is acquired in advance from the modeling trajectory generating unit 80 or the like, becomes 0. The first piston 14 (or the second piston 15) starts to be pulled back a predetermined time before that timing. The predetermined time is the time required to move the pullback movement amount X (mm) calculated by the above formula 24. According to the specific example 2 of the predetermined timing, it is possible to prevent the molten resin from continuing to be discharged due to residual pressure, gravity, etc. (the flow rate of the molten resin discharged from the discharge nozzle 18 can be set to 0 (zero)) at the same timing as the timing when the moving speed (translational speed) of the discharge nozzle 18 changes from a speed other than 0 to 0 (the timing when the moving discharge nozzle 18 stops). As a result, for example, it is possible to prevent the resin bead RB from becoming thicker than the target dimension at the end point.

[0542] <Speed ​​of the Pull-Back Movement of the First Piston 14 (or the Second Piston 15)> In the specific examples 1 and 2 of the above-mentioned predetermined timing, it is desirable to make the speed of the retraction operation of the first piston 14 (or the second piston 15) sufficiently fast. Here, "sufficiently" means a degree to which air does not enter the plasticization chamber S2 (or the plasticization chamber S4) from the resin raw material receiving chamber S1 (or the resin raw material receiving chamber S3) during the retraction operation through the part (non-return ring 14b, 15b, see Figures 7, 14, etc.) that is provided on the first piston 14 (or the second piston 15) and has a function of preventing backflow of the molten resin. This "degree" may be calculated from the viscosity of the molten resin and the gap or moment of inertia of the parts that constitute the function of preventing backflow, or may be obtained by a plasticization experiment, etc. In this way, it is possible to prevent air from being entrained in the plasticization chamber S2 (or the plasticization chamber S4) or air bubbles from being generated, which would cause defects at the timing of the next modeling.

[0543] <Check valve 13b> FIG. 48 is an enlarged cross-sectional view of the vicinity of the discharge nozzle 18. As shown in FIG. 48, in the resin discharge unit (first piston 14 or second piston 15), a check valve 13b is provided between the plasticizing chambers S2, S4 and the discharge nozzle 18 (discharge hole).

[0544] The check valve 13b is composed of a seal surface 13k, a check ball 13e that comes into close contact with the seal surface 13k to close the flow path of the molten resin, and a spring 13f (one example of the elastic member of the present invention) that presses the check ball 13e against the seal surface 13k. When the difference between the pressure in the plasticizing chamber S2 (or the plasticizing chamber S4) and the pressure before the discharge nozzle 18 (discharge hole) exceeds the valve opening pressure, the check ball 13e is pushed toward the spring 13f and strokes (see symbol S in Figure 48), and is positioned at the open position (see the position of the check ball 13e on the left side in Figure 48) where the flow path of the molten resin is open.

[0545] When the first piston 14 (or the second piston 15) moves in a direction approaching the discharge nozzle 18 and the pressure applying pressure to the molten resin in the cylinder 11 (or cylinder 12) exceeds a predetermined pressure, the check ball 13e elastically deforms the spring 13f and moves from a closed position in which the flow path of the molten resin is closed to an open position in which the flow path of the molten resin is open (see the position of the check ball 13e on the left in Figure 48), and when the first piston 14 (or the second piston 15) moves in a direction away from the discharge nozzle 18, the spring 13f moves from the open position to the closed position (see the position of the check ball 13e on the right in Figure 48) due to a restoring force that returns it to its shape before elastic deformation.

[0546] The stroke S of the check ball 13e is determined so as to satisfy the following formula 27. (S×π / 4×Dc 2 ) / Vd×K>Pt...(Formula 27) where Dc is the diameter of the check ball, Vd is the dead volume, and K is the bulk modulus of the molten resin.

[0547] In order to make the check ball 13e function more effectively, a throttle 13m is provided between the upstream and downstream of the check ball 13e (see FIG. 48). The throttle 13m is a portion between the upper portion 13d1 and the lower portion 13d2 of the upstream and downstream (the accommodation portion 13d in which the check valve 13b is accommodated), and the cross-sectional area S 13d (and the cross-sectional area S of the lower part 13d2 13d ) compared to the cross-sectional area S 13m This refers to a part with a small cross-sectional area (on a plane parallel to the XY plane).

[0548] The check valve 13b having the above-described configuration provides the following advantageous effects. When the first piston 14 (or the second piston 15) is pulled back, if the pressure in the plasticization chamber S2 (or the plasticization chamber S4) drops, the check ball 13e moves upward due to the pressure difference between it and the discharge nozzle 18 (discharge hole), and when it hits the seal surface 13k, that is, when the check ball 13e is in the closed position where it closes the flow path of the molten resin (see the position of the check ball 13e on the left side in Figure 48), the molten resin is not sucked out from there, so thereafter, the pressure in the vicinity just before the outlet of the discharge nozzle 18 (discharge hole) does not change. If the stroke S of the check ball 13e is too small, it closes immediately, and the pressure in the vicinity of the discharge nozzle 18 (discharge hole) does not drop as intended, and there is a risk that the molten resin will leak out due to residual pressure.

[0549] Considering the mechanism that determines the pressure immediately before the outlet of the discharge nozzle 18 (discharge hole) when the first piston 14 (or second piston 15) is pulled back, the amount of pressure drop ΔP is determined by two factors: the amount of sucked out fluid Q that moves to the plasticizing chamber S2 (or plasticizing chamber S4) side before the check ball 13e closes, and the increase in volume ΔV caused by the check ball 13e moving upward by the stroke S. The relationship is shown in the following equation 28.

[0550] ΔP = (Q+ ΔV ) / Vd×K (Equation 28) ΔV = S×π / 4×Dc 2 ...(Formula 29) Here, Q is an amount that is determined in the moment before the check ball 13e is activated, and since it is difficult to calculate the value, let it be 0 (zero) assuming the worst case. When ΔP is calculated using the above formula 29, the following formula 30 is obtained.

[0551] ΔP = (S × π / 4 × Dc 2 ) / Vd×K (Formula 30) Unless the amount of pressure drop ΔP is made larger than the pressure Pt immediately before the outlet of the discharge hole, residual pressure will remain, and the relationship of the following equation 31 will be satisfied. ΔP>Pt...(Formula 31) From the above formulas 30 and 31, the above formula 27 can be obtained.

[0552] Next, the advantages of the sixth embodiment will be further described in comparison with the sixth comparative example.

[0553] <Comparative Example 6> Comparative Example 6 (US Patent Application Publication No. 2019 / 0322044) has the following problems.

[0554] <Assignment 1> The resulting object has some protruding parts compared to the intended outer shape. By adjusting the speed of the screw and gear pump in accordance with the translation speed of the nozzle, the dimensions of the resin bead can be stabilized and the desired overlap amount can be obtained within the range indicated by reference numeral 101 in Fig. 6 of Comparative Example 6 (see "Detailed Description"

[0066] of Comparative Example 6). However, at the end point and the reversal point of the resin bead (which always exists in 3D printing), the resin bead overlaps excessively, resulting in a protruding portion. Figure 51 is a diagram illustrating problem 1 of Comparative Example 6. In Figure 51, the dashed arrow AR2 indicates the trajectory of the discharge nozzle. Also, the hatched area HA2 indicates the overlapping portion of the resin bead RB.

[0555] The reason why problem 1 occurs is as follows. That is, the nozzle speed becomes 0 (zero) at the reversal point and the end point, but although it is desired to make the discharge flow rate of the molten resin 0 the moment it stops, this is not possible with the nozzle structure of Comparative Example 6, and the resin continues to come out for a while. This is because, as shown in Fig. 2 of Comparative Example 6, the molten resin sent from the screw 60 is adjusted by the gear pump 74, sent through the conduit 52 to the applicator head 43, and becomes a resin bead. That is, even if the nozzle speed corresponds to 0 and the rotation of the gear pump is stopped, a considerable amount continues to come out due to the residual pressure remaining in the conduit and the weight of the molten resin itself.

[0556] The advantages of the sixth embodiment over the sixth comparative example are as follows. That is, in the sixth embodiment, the discharge nozzle 18 (see FIG. 48) is structured so that the molten resin can be pushed out by the first piston 14 (or the second piston 15) to adjust the discharge and flow rate, and when the moving speed (translational speed) of the discharge nozzle 18 is 0, the first piston 14 (or the second piston 15) is pulled back so that the discharge pressure becomes negative (pressure smaller than the outside air pressure) in order to immediately make the flow rate 0. This solves the above-mentioned problem 1.

[0557] FIG. 52 is a diagram illustrating the advantage of the sixth embodiment and problem 1 of the sixth comparative example. In the sixth embodiment, the piston (first piston 14 or second piston 15) that was performing the discharge operation is controlled to be pulled back from a point where the moving speed (translational speed) becomes 0 (zero), such as the reversal point or end point shown in FIG. 52, and the amount of movement back is set so that the pressure of the molten resin just before the discharge nozzle (discharge hole) is smaller than the pressure outside the discharge nozzle and does not become lower than atmospheric pressure. Therefore, the molten resin is pushed back by the atmospheric pressure and does not leak, and air is not entrained in the plasticization chambers S2 and S4, or bubbles are generated, which causes defects at the timing of the next modeling. In addition, at the overlapping portion of the geometric resin bead RB, the resin bead RB that was once layered is sucked up, so that it does not protrude. Referring to FIG. 52, it can be seen that the outer shape of the three-dimensionally shaped object of the sixth embodiment almost matches the targeted outer shape.

[0558] In contrast, in Comparative Example 6, as shown in Figure 52, the resin bead overlaps excessively at the end point and the reversal point, resulting in a portion that protrudes from the intended outline (see the hatched area indicated by the symbol HA3 in Figure 52).

[0559] As described above, according to the sixth embodiment, it is possible to improve the controllability of the flow rate of the molten resin discharged from the discharge nozzle 18. In addition, according to the sixth embodiment, it is possible to achieve the same effects as those of the fourth and fifth embodiments.

[0560] Furthermore, according to the sixth embodiment, the discharge pressure can be made negative (for example, a pressure lower than the outside air pressure) by controlling the first piston 14 (or the second piston 15) so that the first piston 14 (or the second piston 15) moves a predetermined amount in a direction away from the discharge nozzle 18 at a predetermined timing. This makes it possible to prevent the molten resin from being continuously discharged due to residual pressure, gravity, etc. As a result, the dimensions of the resin bead RB can be controlled to be constant (approximately constant).

[0561] Furthermore, according to embodiment 6, the discharge pressure can be made negative (e.g., a pressure lower than the outside air pressure) at the timing when the movement speed (translational speed) of the discharge nozzle 18 changes from a value other than 0 to 0 (at the timing when the moving discharge nozzle stops).

[0562] Furthermore, according to the sixth embodiment, the resin pressure inside the discharge nozzle 18 becomes lower than the resin pressure outside the discharge nozzle 18, thereby making it possible to prevent the molten resin from continuing to be discharged due to residual pressure, gravity, etc. Also, by making the differential pressure (pressure outside the discharge nozzle 18-pressure inside the discharge nozzle 18) generated when the first piston 14 (or the second piston 15) is moved in the retracting direction by the movement amount X not exceed atmospheric pressure (for example, 0.1 MPa), it is possible to prevent air from being entrained in the plasticization chamber S2 (or the plasticization chamber S4) or bubbles from being generated.

[0563] Furthermore, according to embodiment 6, the discharge pressure can be made negative (e.g., a pressure lower than the outside air pressure) for a predetermined time before the timing when the movement speed (translational speed) of the discharge nozzle 18 is predicted to change from a value other than 0 to 0 (when the moving discharge nozzle 18 stops).

[0564] Furthermore, according to embodiment 6, at the same timing when the moving speed (translational speed) of the discharge nozzle 18 changes from a speed other than 0 to 0 (the timing when the moving discharge nozzle 18 stops), it is possible to prevent the molten resin from continuing to be discharged due to residual pressure, gravity, etc. (the flow rate of the molten resin discharged from the discharge nozzle 18 can be made 0 (zero)).

[0565] According to the sixth embodiment, the moving speed of the first piston 14 (or the second piston 15) in the direction away from the discharge nozzle 18 is set to a speed at which air does not flow from the resin raw material supply chamber S1 (or the resin raw material supply chamber S3) to the plasticization chamber S2 (plasticization chamber S4). It is possible to prevent air from entering the plasticization chamber S2 (plasticization chamber S4).

[0566] Furthermore, according to the sixth embodiment (as well as the other embodiments), the check ball 13e automatically moves to the open or closed position in response to the movement of the first piston 14 (or the second piston 15) that makes a linear reciprocating motion inside the cylinder 11 (or the cylinder 12), thereby making it possible to control the flow rate of the molten resin discharged from the discharge nozzle 18. This also makes it possible to improve the controllability of the flow rate of the molten resin discharged from the discharge nozzle 18.

[0567] <Embodiment 7> Next, another operation example 3 of the 3D printer 300 according to the fourth embodiment will be described as a seventh embodiment.

[0568] <Details of other operation example 3 of 3D printer 300> 49 is a detailed flowchart of another operation example 3 of the 3D printer 300. The following processing is realized by the control unit 30A (processor) executing a predetermined program read from the storage unit 20 to the memory 40 (for example, RAM).

[0569] First, a 3D object forming process is executed (step S140). The 3D object forming process is a process for forming a target 3D object by the 3D printer 300, and is, for example, the process of the flowchart in FIG. 27, the process of the flowchart in FIG. 41, or the process of the flowchart in FIG. Here, as shown in Fig. 50, a three-dimensional object Ob3 (layered object) is formed by a resin bead RB passing through a start point P1, reversal points P2a, P2a, and an end point P3. Fig. 50 shows an example of a three-dimensional object Ob3 (layered object) formed according to the flowchart of Fig. 49. In Fig. 50, a dashed arrow AR1 indicates the trajectory of the discharge nozzle 18. Also, a hatched area HA1 indicates the portion where the resin beads RB overlap.

[0570] Following this 3D object formation process, it is determined whether the current position of the discharge nozzle 18, which is moving in the XY axis direction while discharging molten resin, is a reversal point (or end point) (step S141). If the current position of the discharge nozzle 18 is a reversal point (or end point) as a result of the determination in step S141 (step S141: YES), a resin bead suction process is executed (step S142).

[0571] <Resin bead suction treatment> The resin bead suction process is a process for suctioning uncured resin beads RB that have been layered on the three-dimensional object (for example, resin beads RB in the portion where resin beads RB overlap). This is achieved by the piston control unit 30b controlling the first piston 14 (or the second piston 15) so that the first piston 14 (or the second piston 15) moves a predetermined amount (movement amount X that satisfies the following formula 32) in a direction away from the discharge nozzle 18 (pullback direction) while the outlet of the discharge nozzle 18 and the three-dimensional object are fluidly connected.

[0572] As a premise, the outlet of the discharge nozzle 18 (discharge hole) and the three-dimensional model (laminated object) are positioned close enough to be fluidly connected. This is achieved, for example, by the discharge nozzle control unit 30e controlling the XY-axis drive device 50 (gantry drive device) to move the discharge nozzle 18 relatively to the base plate 4 so that the outlet of the discharge nozzle 18 and the three-dimensional model are fluidly connected. A fluidically connected state refers to a state in which they are connected by molten resin before solidification. For example, in FIG. 53, the molten resin RB within a range close to the discharge nozzle 18 (discharge hole 18a) (see the range indicated by the symbol L1 in FIG. 53) L1 On the other hand, the molten resin RB in the area far from the discharge nozzle 18 (discharge hole 18a) (see the area indicated by the symbol L2 in FIG. 53) is not solidified and is in a fluid connected state. L2 is solidified and is not in a fluidly connected state. Figure 53 is a diagram explaining a fluidly connected state.

[0573] <Example of pullback movement amount> It is desirable that the amount of pullback movement X (mm) of the first piston 14 (or the second piston 15) is a value that satisfies the following formula 32. X ≧ (P t +0.1)×V0 / K / S...(Formula 32)

[0574] The processes of steps S140 to S142 are repeatedly executed until the 3D object formation process ends (step S143: YES). This makes it possible to prevent the resin bead RB from protruding or the modeling height from increasing at locations such as the reversal points P2a and P2b where overlapping of the resin bead RB is geometrically unavoidable.

[0575] Also, at a portion such as the end point P3 where the discharge nozzle 18 stops, it is possible to provide a shape that is thinner than a normal portion (improved freedom of molding shape).

[0576] As described above, according to the seventh embodiment, it is possible to improve the controllability of the flow rate of the molten resin discharged from the discharge nozzle 18. In addition, according to the sixth embodiment, it is possible to achieve the same effects as those of the fourth and fifth embodiments.

[0577] Moreover, according to the seventh embodiment, it is possible to suck in the uncured resin beads RB once layered in the three-dimensional object (for example, the resin beads RB in the portion where the resin beads RB overlap each other). As a result, it is possible to control the size of the resin beads RB to be constant (approximately constant).

[0578] <Modification> Next, a modified example will be described.

[0579] In the above fourth to seventh embodiments, an example has been described in which the three-dimensional laminate modeling apparatus of the present invention is applied to a 3D printer equipped with an injection molding machine 2A equipped with a plurality of combinations of a cylinder and a piston (torpedo) (cylinder 11, first piston 14, and cylinder 12, second piston 15), but the present invention is not limited thereto. For example, the three-dimensional laminate modeling apparatus of the present invention may be applied to a 3D printer (not shown) equipped with an injection molding machine equipped with one combination of a cylinder and a piston (torpedo). In other words, the three-dimensional laminate modeling apparatus of the present invention does not particularly limit the number of combinations of a cylinder and a piston (torpedo).

[0580] In the above embodiment, the present invention has been described as a hardware configuration, but the present invention is not limited to this. Any process of the present invention can be realized by causing a CPU (Central Processing Unit) to execute a computer program.

[0581] The program can be stored and provided to the computer using various types of non-transitory computer readable media. The non-transitory computer readable media includes various types of tangible storage media. Examples of the non-transitory computer readable media include magnetic recording media (e.g., flexible disks, magnetic tapes, hard disk drives), magneto-optical recording media (e.g., magneto-optical disks), CD-ROM (Read Only Memory), CD-R, CD-R / W, and semiconductor memory (e.g., mask ROM, PROM (Programmable ROM), EPROM (Erasable PROM), flash ROM, RAM (random access memory)). The program may also be provided to the computer by various types of transitory computer readable media. Examples of the transitory computer readable media include electric signals, optical signals, and electromagnetic waves. The transitory computer readable media can provide the program to the computer via a wired communication path such as an electric wire and an optical fiber, or via a wireless communication path. [Explanation of symbols]

[0582] 1 Injection molding equipment 2 Injection molding machine 3 Feeding device 31 exhaust part, 31a exhaust passage, 31b exhaust hole, 31c exhaust valve 32 Hopper (32a first hopper, 32b second hopper) 33 Pressurizing section 34 Second control section 35 Exhaust pipe 36 First supply pipe 37 Second Supply Pipe 38 First connecting pipe 39 Second connecting pipe 4 Tables 5. Mobile Devices 51 Gantry device 52 Lifting device 53 Third Control Section 6 Heating device 61 First heating section 62 Second heating section 62a Seat heater 62b Heat transfer material 63 Temperature detection unit 64 Fourth Control Section 7 Control device 8 Cooling section, 8a through hole, 8b cooling path 11 first cylinder, 11a closing portion, 11b side wall portion, 11c through hole, 11d supply hole 12 second cylinder, 12a closing portion, 12b side wall portion, 12c through hole, 12d supply hole 13 End Plate 13a Main body 13b check valve, 13e check ball, 13f spring 13c through hole 13d Storage section 13g Bolt hole 13h Volt 14 First piston unit 14a Torpedo Piston 14b Check ring 14c stopper, 14g ring, 14h hook 14d Pressure piston 14e Biasing means 14f Groove 14i Sealing material 14j Intrusion part 15 Second piston unit 15a Torpedo Piston 15b Check ring 15c stopper, 15g ring, 15h hook 15d Pressure piston 15e Biasing means 15f Groove 15i Sealing material 15j Intrusion part 16 first drive unit, 16a motor, 16b screw shaft, 16c slider, 16d rod, 16e case, 16f encoder, 16h, 16i through hole 17 second drive unit, 17a motor, 17b screw shaft, 17c slider, 17d rod, 17e case, 17f encoder, 17h, 17i through hole 18 injection portion, 18a injection port, 18b first branch passage, 18c second branch passage, 18d retaining nut, 18e first plate, 18f second plate 19 First control section M Resin raw material R Molten resin S1 First space of first cylinder S2 Second space of first cylinder S3 First space of second cylinder S4 Second space of second cylinder

Claims

1. A cylinder for storing molten resin; A discharge nozzle communicating with the cylinder; a piston that performs a reciprocating linear motion within the cylinder, the piston moving in a direction approaching the discharge nozzle to pressurize the molten resin within the cylinder, thereby discharging the molten resin from the discharge nozzle; and a three-dimensional layered object fabrication device that forms a three-dimensional object by layering resin beads, which are the molten resin discharged from the discharge nozzle, on a table, the three-dimensional layered object fabrication device comprising: a moving unit that moves the discharge nozzle relatively to the table; An acquisition unit that acquires a moving speed of the discharge nozzle; A piston control unit that controls the movement of the piston, The piston control unit controls the movement of the piston based on a moving speed of the discharge nozzle, a flow rate prediction unit that predicts a flow rate of the molten resin discharged from the discharge nozzle; a discharge nozzle control unit for controlling movement of the discharge nozzle, The discharge nozzle control unit controls the movement speed of the discharge nozzle by controlling the movement unit based on the predicted discharge flow rate so that the dimensions of the resin bead are constant.

2. The three-dimensional layered object manufacturing apparatus according to claim 1 , wherein the piston control unit controls a moving speed of the piston based on a moving speed of the discharge nozzle so that a size of the resin bead is constant.

3. a space in the cylinder on the opposite side of the piston from the discharge nozzle is a resin raw material supply chamber to which a resin raw material is supplied, a space in the cylinder on the discharge nozzle side with respect to the piston is a plasticization chamber that stores the molten resin, The three-dimensional laminated object manufacturing device of claim 1 or 2, wherein the piston moves in a direction away from the discharge nozzle to plasticize the resin raw material supplied to the resin raw material supply chamber and store the molten resin, which is the plasticized resin raw material, in the plasticization chamber, and moves in a direction approaching the discharge nozzle to pressurize the molten resin stored in the plasticization chamber, thereby discharging the molten resin stored in the plasticization chamber from the discharge nozzle.

4. The three-dimensional laminated object manufacturing device according to any one of claims 1 to 3, wherein the piston control unit controls the moving speed of the piston so that the flow rate of the molten resin discharged from the discharge nozzle becomes the moving speed of the discharge nozzle multiplied by the cross-sectional area of ​​the resin bead.

5. The three-dimensional layered object manufacturing apparatus according to claim 1 , further comprising a temperature control unit that controls a temperature of the molten resin stored in the cylinder.

6. The three-dimensional layered object manufacturing device according to claim 1 , wherein the discharge nozzle control unit controls the moving speed of the discharge nozzle by controlling the moving unit so that the moving speed of the discharge nozzle becomes the predicted discharge flow rate / cross-sectional area of ​​the resin bead.

7. The three-dimensional layered object manufacturing apparatus according to claim 1 , wherein the piston control unit controls the piston so that the piston moves a predetermined amount in a direction away from the discharge nozzle at a predetermined timing.

8. The three-dimensional layered object fabrication apparatus according to claim 7 , wherein the predetermined timing is a timing at which a moving speed of the discharge nozzle changes from a speed other than 0 to 0.

9. The three-dimensional layered object modeling apparatus according to claim 8 , wherein the predetermined amount is an amount at which a resin pressure inside the discharge nozzle is lower than a resin pressure outside the discharge nozzle.

10. The three-dimensional layered object fabrication apparatus according to claim 7 , wherein the predetermined timing is a timing a predetermined time before a timing at which the moving speed of the discharge nozzle is predicted to change from a speed other than 0 to 0.

11. The three-dimensional layered object modeling apparatus according to claim 10 , wherein the predetermined amount is an amount at which a resin pressure inside the discharge nozzle is lower than a resin pressure outside the discharge nozzle.

12. The three-dimensional layered object fabrication apparatus according to claim 10 or 11, wherein the predetermined time is a time required for the piston to move the predetermined amount.

13. A cylinder for storing molten resin; A discharge nozzle communicating with the cylinder; a piston that performs linear reciprocating motion within the cylinder, the piston moving in a direction approaching the discharge nozzle to pressurize the molten resin within the cylinder, thereby discharging the molten resin from the discharge nozzle, and a three-dimensional object printing method for a three-dimensional laminated object printing device that forms a three-dimensional object by stacking resin beads, which are the molten resin discharged from the discharge nozzle, on a table, comprising: The three-dimensional laminate modeling apparatus further includes a moving unit that moves the discharge nozzle relatively to the table, An acquisition step of acquiring a moving speed of the discharge nozzle; A piston control step of controlling the movement of the piston, the piston control step controls movement of the piston based on a movement speed of the discharge nozzle; a flow rate prediction step of predicting a flow rate of the molten resin discharged from the discharge nozzle; and a discharge nozzle control step of controlling movement of the discharge nozzle, The discharge nozzle control step is a three-dimensional layered object manufacturing method in which the discharge nozzle movement speed is controlled by controlling the moving unit so that the diameter of the resin bead is constant based on the predicted discharge flow rate.

14. The three-dimensional laminated object manufacturing method according to claim 13 , wherein the piston control step controls the piston so that the piston moves a predetermined amount in a direction away from the discharge nozzle at a predetermined timing.

Citation Information

Patent Citations

  • Device and method for creating three-dimensional object

    JP1991158228A

  • Manufacturing device and manufacturing method of three-dimensional object

    JP2015168135A

  • Method and device for manufacturing an object by using a 3D printing device

    JP2019500251A

  • Additively manufactured objects

    JP2020508909A

  • Methods and apparatus for processing and dispensing material during additive manufacturing