Magnetic Recording Media

Optimizing the squareness ratio and magnetic force gradient strengths in magnetic recording media with an auxiliary magnetic pole ensures high SNR for servo signals, addressing the SNR degradation from increased tape capacity.

JP7586266B2Active Publication Date: 2024-11-19SONY GROUP CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023183843
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-29
Filing Date
2023-10-26
Publication Date
2024-11-19
Estimated Expiration
2040-03-27

AI Technical Summary

Technical Problem

The increase in magnetic tape capacity leads to narrower servo bandwidth, resulting in decreased signal-to-noise ratio (SNR) of servo playback signals due to increased azimuth loss and demagnetizing fields in perpendicular magnetic recording systems.

Method used

A magnetic recording medium with a magnetic layer having a servo band, where the squareness ratio and peak-to-peak magnetic force gradient strengths are optimized to achieve an index of 0.42 or higher, ensuring high SNR by recording servo signals in saturation.

Benefits of technology

This approach effectively suppresses the deterioration of servo reproduction signals, maintaining high SNR even with increased tape capacity, by using an auxiliary magnetic pole to induce perpendicular magnetization and enhance magnetic susceptibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586266000003
    Figure 0007586266000003
  • Figure 0007586266000004
    Figure 0007586266000004
  • Figure 0007586266000005
    Figure 0007586266000005
Patent Text Reader

Abstract

To provide a magnetic recording medium and a servo signal recording device capable of suppressing deterioration of servo reproduction signals due to increased capacity.SOLUTION: A magnetic recording medium according to one embodiment of the present technology is a tape-shaped magnetic recording medium including a magnetic layer having a servo band on which a servo signal is recorded. An index expressed by Sq×Fact.(p-p) / F0(p-p) is 0.42 or more where Sq is a squareness ratio of the magnetic layer in a perpendicular direction, F0(p-p) is a peak-to-peak value of a first magnetic force gradient strength observed by a magnetic force microscope when a servo signal is saturation-recorded on the magnetic layer, Fact.(p-p) is a peak-to-peak value of a second magnetic force gradient strength for the servo signal recorded on the servo band observed by the magnetic force microscope.SELECTED DRAWING: Figure 19
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present technology relates to a magnetic recording medium on which a servo signal is recorded and a servo signal recording device. [Background technology]

[0002] 2. Description of the Related Art In recent years, magnetic recording media have come into widespread use for purposes such as backing up electronic data, etc. As one type of magnetic recording medium, magnetic tape is widely used.

[0003] A data band including a plurality of recording tracks is provided on the magnetic layer of the magnetic tape, and data is recorded on the recording tracks. In addition, servo bands are provided on the magnetic layer at positions sandwiching the data band in the width direction, and servo signals are recorded on the servo bands. A magnetic head aligns with the recording tracks by reading the servo signals recorded on the servo bands (see, for example, Patent Document 1).

[0004] Known recording methods for magnetic recording media include a horizontal magnetic recording method in which data is recorded by magnetizing magnetic particles in a magnetic layer in a horizontal direction, and a perpendicular magnetic recording method in which data is recorded by magnetizing magnetic particles in a magnetic layer in a vertical direction. The perpendicular magnetic recording method can record data at a higher density than the horizontal magnetic recording method. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2014-199706 A Summary of the Invention [Problem to be solved by the invention]

[0006] With the recent increase in the capacity of magnetic tapes, the servo band width is expected to become narrower. For example, on magnetic tapes in the LTO format, a servo pattern including two different azimuthal slopes is recorded as a servo signal. In this case, in order to accommodate the increase in the capacity of magnetic tapes, it is necessary to increase the inclination angle of the azimuthal slope with respect to the tape width direction. As a result, the azimuth loss with the servo reproducing head increases, and a decrease in the signal-to-noise ratio (SNR) of the servo reproduction signal, which is the reproduction output of the servo signal, is unavoidable. Moreover, in the perpendicular magnetic recording method, there is a problem that the SNR of the servo reproduction signal is easily decreased due to the influence of the demagnetizing field in the perpendicular direction of the magnetic layer.

[0007] In view of the above circumstances, an object of the present technology is to provide a magnetic recording medium and a servo signal recording device that can suppress deterioration of a servo reproduction signal that accompanies an increase in capacity. [Means for solving the problem]

[0008] A magnetic recording medium according to an embodiment of the present technology is a tape-shaped magnetic recording medium having a magnetic layer having a servo band on which a servo signal is recorded. When the squareness ratio in the vertical direction of the magnetic layer is Sq, the peak-to-peak value of the first magnetic force gradient intensity observed with a magnetic force microscope when a servo signal is saturation recorded in the magnetic layer is F0(pp), and the peak-to-peak value of the second magnetic force gradient intensity observed with a magnetic force microscope for the servo signal recorded in the servo band is Fact.(pp), an index expressed by Sq×Fact.(pp) / F0(pp) is 0.42 or more.

[0009] In this technology, the squareness ratio Sq is calculated by multiplying the squareness ratio Sq by the ratio between the peak-to-peak value of the first magnetic field gradient strength and the peak-to-peak value of the second magnetic field gradient strength, and the servo signal is reproduced with a relatively high SNR by setting the squareness ratio Sq to 0.42 or more. This makes it possible to suppress the deterioration of the servo reproduction signal due to the increase in capacity.

[0010] The index may be 0.5 or greater.

[0011] The index may be 0.6 or greater.

[0012] The squareness (Sq) of the magnetic layer in the perpendicular direction may be 0.45 or more.

[0013] The squareness (Sq) of the magnetic layer in the perpendicular direction may be 0.6 or more.

[0014] The ratio of Fact.(pp) to F0(pp) (Fact.(pp) / F0(pp)) may be 0.6 or greater.

[0015] The ratio of Fact.(pp) to F0(pp) (Fact.(pp) / F0(pp)) may be 0.7 or greater.

[0016] The ratio of Fact.(pp) to F0(pp) (Fact.(pp) / F0(pp)) may be 0.8 or greater.

[0017] The remanent magnetization (Mrt) of the magnetic layer may be 0.35 or greater.

[0018] The remanent magnetization (Mrt) of the magnetic layer may be 0.45 or greater.

[0019] The servo signal may be a servo signal recording pattern including a plurality of stripes inclined at a predetermined azimuth angle with respect to the tape width direction.

[0020] The magnetic layer may include magnetic powder of hexagonal ferrite, ε iron oxide, or cobalt ferrite.

[0021] A servo signal recording device according to an embodiment of the present technology is a device that records a servo signal on a tape-shaped magnetic recording medium having a magnetic layer with a servo band, and includes a servo write head and an auxiliary magnetic pole. The servo write head records a servo signal in the servo band. The auxiliary magnetic pole portion is disposed opposite the servo write head with the magnetic layer interposed therebetween, and is made of a soft magnetic material. Effect of the Invention

[0022] According to the present technology, it is possible to suppress the deterioration of servo reproduction signals that accompanies an increase in capacity. Note that the effects described herein are not necessarily limited to those described herein, and may be any of the effects described in this disclosure. [Brief description of the drawings]

[0023] [Figure 1] 1 is a schematic diagram showing a magnetic recording medium according to an embodiment of the present technology as viewed from the side; [Diagram 2] FIG. 2 is a schematic diagram of the magnetic recording medium as viewed from the magnetic layer side. [Diagram 3] 2 is an enlarged view showing a recording track in a data band of the magnetic layer. FIG. [Figure 4] 3 is an enlarged view showing a servo signal recording pattern in a servo band of the magnetic layer. FIG. [Diagram 5] FIG. 1 is a schematic diagram showing a data recording device. [Figure 6] 4 is a bottom view of a head unit in the data recording device. FIG. [Figure 7] FIG. 2 is a diagram showing a state in which recording / reproduction of a data signal is performed in the head unit. [Figure 8] FIG. 2 is a diagram showing two stripes in the servo signal recording pattern. [Figure 9] FIG. 1 is a schematic diagram showing an example of a servo signal recording device. [Figure 10] FIG. 2 is an enlarged view showing a schematic view of a part of the servo signal recording device. [Figure 11] 3A and 3B are diagrams illustrating the reproduced waveform of a servo signal and the magnitude of its output. [Figure 12] FIG. 2 is a diagram for explaining an external magnetic field required to saturate magnetize one stripe in a servo signal recording pattern. [Figure 13] FIG. 2 is an explanatory diagram of a first magnetic force gradient strength for the one stripe. [Figure 14] FIG. 11 is an explanatory diagram of the second magnetic force gradient strength for the one stripe. [Figure 15] FIG. 11 is another explanatory diagram of the second magnetic force gradient strength for the one stripe. [Figure 16] 1 is a schematic diagram showing a main part of a servo signal recording device according to an embodiment of the present technology; [Figure 17] 17 is an enlarged view of a main part of part A in FIG. 16. [Figure 18] FIG. 17 is a schematic plan view of the main part in FIG. [Figure 19] FIG. 1 is a diagram showing the results of an example and a comparative example. [Figure 20] FIG. 2 is an exploded perspective view showing an example of a configuration of a cartridge. [Figure 21] FIG. 2 is a block diagram showing an example of the configuration of a cartridge memory. [Figure 22] FIG. 11 is an exploded perspective view showing another example of the configuration of the cartridge. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Hereinafter, embodiments of the present technology will be described with reference to the drawings.

[0025] [Configuration of magnetic recording medium] First, the basic configuration of the magnetic recording medium will be described. Fig. 1 is a schematic diagram of a magnetic recording medium 1 according to an embodiment of the present technology as viewed from the side, and Fig. 2 is a schematic diagram as viewed from the magnetic layer side.

[0026] 1 and 2, the magnetic recording medium 1 is configured in the shape of a tape that is long in the longitudinal direction (X-axis direction), short in the width direction (Y-axis direction), and thin in the thickness direction (Z-axis direction). Note that in this specification (and the drawings), the coordinate system based on the magnetic recording medium 1 will be represented as an XYZ coordinate system.

[0027] The magnetic recording medium 1 is configured to be capable of recording signals at a shortest recording wavelength of preferably 96 nm or less, more preferably 75 nm or less, even more preferably 60 nm or less, and particularly preferably 50 nm or less. The magnetic recording medium 1 is preferably used in a data recording device equipped with a ring-type head as a recording head.

[0028] 1, the magnetic recording medium 1 includes a tape-shaped substrate 11 that is long in the longitudinal direction (X-axis direction), a nonmagnetic layer 12 provided on one main surface of the substrate 11, a magnetic layer 13 provided on the nonmagnetic layer 12, and a back layer 14 provided on the other main surface of the substrate 11. Note that the back layer 14 may be provided as necessary, and may be omitted.

[0029] Typically, a coating-type magnetic medium of a perpendicular recording system is used for the magnetic layer 13. Details of the magnetic recording medium 1 including the magnetic layer 13 will be described later.

[0030] [Data band and servo band] Fig. 2 is a schematic diagram of the magnetic recording medium 1 as viewed from above. Referring to Fig. 2, the magnetic layer 13 has a plurality of data bands d (data bands d0 to d3) that are long in the longitudinal direction (X-axis direction) in which data signals are written, and a plurality of servo bands s (servo bands s0 to s4) that are long in the longitudinal direction in which servo signals are written. The servo bands s are arranged at positions sandwiching each data band d in the width direction (Y-axis direction).

[0031] In the present technology, the ratio of the area of ​​the servo bands s to the area of ​​the entire surface of the magnetic layer 13 is typically 4.0% or less. The width of the servo bands s is typically 95 μm or less. The ratio of the area of ​​the servo bands s to the area of ​​the entire surface of the magnetic layer 13 can be measured, for example, by developing the magnetic recording medium 1 with a developer such as a ferricolloid developer, and then observing the developed magnetic recording medium 1 with an optical microscope.

[0032] The servo bands s are arranged at positions sandwiching the data bands d, so the number of servo bands s is one more than the number of data bands d. In the example shown in Fig. 2, the number of data bands d is four, and the number of servo bands s is five (this method is generally adopted in existing systems).

[0033] The number of data bands d and the number of servo bands s can be changed as appropriate, and these numbers may even be increased.

[0034] In this case, the number of servo bands s is preferably 5 or more. If the number of servo bands s is 5 or more, the effect of dimensional changes in the width direction of the magnetic recording medium 1 on the accuracy of reading servo signals can be suppressed, and stable recording and reproducing characteristics with little off-track can be ensured.

[0035] Also, the number of data bands d may be 8, 12, ... (i.e., 4n (n is an integer equal to or greater than 2)), and the number of servo bands s may be 9, 13, ... (i.e., 4n+1 (n is an integer equal to or greater than 2)). In this case, it is possible to accommodate changes in the number of data bands d and the number of servo bands s without modifying the existing system.

[0036] The data band d includes a plurality of recording tracks 5 that are long in the longitudinal direction and aligned in the width direction. Data signals are recorded in the recording tracks 5 along the recording tracks 5. In this technology, the length of one bit in the longitudinal direction of the data signals recorded in the data band d is typically 48 nm or less. The servo band s includes a servo signal recording pattern 6 of a predetermined pattern in which servo signals are recorded by a servo signal recording device (not shown).

[0037] 3 is an enlarged view showing the recording tracks 5 in the data band d. As shown in FIG. 3, the recording tracks 5 are long in the longitudinal direction and aligned in the width direction, and each track has a predetermined recording track width Wd in the width direction. This recording track width Wd is typically 2.0 μm or less. Note that such a recording track width Wd can be measured, for example, by developing the magnetic recording medium 1 with a developer such as a ferricolloid developer, and then observing the developed magnetic recording medium 1 with an optical microscope.

[0038] The number of recording tracks 5 included in one data band d is, for example, about 1000 to 2000.

[0039] 4 is an enlarged view showing a servo signal recording pattern 6 in a servo band s. As shown in FIG. 4, the servo signal recording pattern 6 includes a plurality of stripes 7 (azimuthal slope) inclined at a predetermined azimuth angle α with respect to the width direction (Y-axis direction). The azimuth angle is not particularly limited and is appropriately determined depending on the size of the servo band s, for example, 12°. Alternatively, the azimuth angle may be 15°, 18°, 21°, 24°, etc.

[0040] The multiple stripes 7 are classified into a first group of stripes 8 that are inclined clockwise with respect to the width direction (Y-axis direction) and a second group of stripes 9 that are inclined counterclockwise with respect to the width direction. Note that the shape of such stripes 7 can be measured, for example, by developing the magnetic recording medium 1 with a developer such as a ferricolloid developer, and then observing the developed magnetic recording medium 1 with an optical microscope.

[0041] 4, dashed lines indicate servo trace lines T that are lines traced by a servo read head on the servo signal recording pattern 6. The servo trace lines T are set along the longitudinal direction (X-axis direction) and are set at a predetermined interval Ps in the width direction.

[0042] The number of servo trace lines T per servo band s is, for example, about 30 to 200.

[0043] The interval Ps between two adjacent servo trace lines T is the same as the value of the recording track width Wd, and is, for example, 2.0 μm or less, or 1.5 μm or less. Here, the interval Ps between two adjacent servo trace lines T is a value that determines the recording track width Wd. In other words, when the interval Ps between the servo trace lines T is narrowed, the recording track width Wd is narrowed and the number of recording tracks 5 included in one data band d increases. As a result, the data recording capacity increases (and vice versa when the interval Ps is widened). Therefore, in order to increase the recording capacity, it is necessary to reduce the recording track width Wd, but as a result of the interval Ps between the servo trace lines T also being narrowed, it becomes difficult to accurately trace the adjacent servo trace lines. Therefore, in this embodiment, as described later, the reading accuracy of the servo signal recording pattern 6 is improved, so that it is possible to cope with the narrowing of the interval Ps.

[0044] [Data recording device] Next, we will explain the data recording device 20 that records and reproduces data signals on the magnetic recording medium 1. Figure 5 is a schematic diagram showing the data recording device 20. In this specification (and the drawings), the coordinate system based on the data recording device 20 will be represented as an X'Y'Z' coordinate system.

[0045] The data recording device 20 is configured so that a cartridge 21 containing a magnetic recording medium 1 can be loaded therein. For ease of explanation, a case will be described here where the data recording device 20 is configured so that one cartridge 21 can be loaded therein, but the data recording device 20 may be configured so that a plurality of cartridges 21 can be loaded therein. The details of the configuration of the cartridge 21 will be described later.

[0046] As shown in FIG. 5, the data recording device 20 includes a spindle 27, a reel 22, a spindle drive device 23, a reel drive device 24, a plurality of guide rollers 25, a head unit 30, and a control device .

[0047] The spindle 27 is configured to be able to load the cartridge 21. The cartridge 21 is compliant with the LTO (Linear Tape Open) standard, and accommodates the wound magnetic recording medium 1 in a rotatable manner inside the case. The reel 22 is configured to be able to fix the tip side of the magnetic recording medium 1 pulled out from the cartridge 21.

[0048] The spindle drive device 23 rotates the spindle 27 in response to a command from the control device 26. The reel drive device 24 rotates the reel 22 in response to a command from the control device 26. When recording / reproducing a data signal on / from the magnetic recording medium 1, the spindle 27 and the reel 22 are rotated by the spindle drive device 23 and the reel drive device 24, causing the magnetic recording medium 1 to run. The guide roller 25 is a roller for guiding the running of the magnetic recording medium 1.

[0049] The control device 26 includes, for example, a control unit, a storage unit, a communication unit, etc. The control unit is configured, for example, by a CPU (Central Processing Unit) etc., and performs overall control of each unit of the data recording device 20 according to a program stored in the storage unit.

[0050] The storage unit includes a non-volatile memory in which various data and various programs are recorded, and a volatile memory used as a working area for the control unit. The various programs may be read from a portable recording medium such as an optical disk or a semiconductor memory, or may be downloaded from a server device on a network. The communication unit is configured to be capable of communicating with other devices such as a PC (Personal Computer) or a server device.

[0051] The head unit 30 is configured to be capable of recording a data signal on the magnetic recording medium 1 in response to a command from the control device 26. The head unit 30 is also configured to be capable of reproducing data written on the magnetic recording medium 1 in response to a command from the control device 26.

[0052] Fig. 6 is a view of the head unit 30 as seen from below. As shown in Fig. 6, the head unit 30 includes a first head unit 30a and a second head unit 30b. The first head unit 30a and the second head unit 30b are configured symmetrically in the X'-axis direction (the running direction of the magnetic recording medium 1). The first head unit 30a and the second head unit 30b are configured to be movable in the width direction (Y'-axis direction).

[0053] The first head unit 30a is a head that is used when the magnetic recording medium 1 runs in the forward direction (the direction in which it flows from the cartridge 21 side to the device 20 side). On the other hand, the second head unit 30b is a head that is used when the magnetic recording medium 1 runs in the reverse direction (the direction in which it flows from the device 20 side to the cartridge 21 side).

[0054] Since the first head unit 30a and the second head unit 30b basically have the same configuration, the first head unit 30a will be representatively described.

[0055] The first head unit 30 a has a unit body 31 , two servo read heads 32 , and a plurality of data write / read heads 33 .

[0056] The servo read head 32 is configured to be able to reproduce a servo signal by reading a magnetic flux generated from magnetic information recorded on the magnetic recording medium 1 (servo band s) using an MR element (MR: Magneto Resistive) or the like. That is, the servo read head 32 reproduces a servo signal by reading a servo signal recording pattern 6 recorded on the servo band s. One servo read head 32 is provided on each end side in the width direction (Y'-axis direction) of the unit body 31. The interval between the two servo read heads 32 in the width direction (Y'-axis direction) is approximately the same as the distance between adjacent servo bands s on the magnetic recording medium 1.

[0057] The data write / read heads 33 are disposed at equal intervals along the width direction (Y-axis direction). Moreover, the data write / read heads 33 are disposed at positions sandwiched between two servo read heads 32. The number of data write / read heads 33 is, for example, about 20 to 40, but is not particularly limited to this number.

[0058] The data write / read head 33 includes a data write head 34 and a data read head 35. The data write head 34 is configured to be capable of recording a data signal on the magnetic recording medium 1 by a magnetic field generated from a magnetic gap. The data read head 35 is configured to be capable of reproducing the data signal by reading a magnetic field generated from magnetic information recorded on the magnetic recording medium 1 (data band d) by an MR element (MR: Magneto Resistive) or the like.

[0059] In the first head unit 30a, the data write head 34 is disposed on the left side of the data read head 35 (upstream side when the magnetic recording medium 1 flows in the forward direction). On the other hand, in the second head unit 30b, the data write head 34 is disposed on the right side of the data read head 35 (upstream side when the magnetic recording medium 1 flows in the reverse direction). The data read head 35 is capable of reproducing a data signal immediately after the data write head 34 writes the data signal to the magnetic recording medium 1.

[0060] Fig. 7 is a diagram showing a state where the first head unit 30a is recording / reproducing a data signal. Note that the example shown in Fig. 7 shows a state where the magnetic recording medium 1 is traveling in the forward direction (the direction from the cartridge 21 side to the device 20 side).

[0061] As shown in FIG. 7, when the first head unit 30a records / plays back a data signal, one of the two servo read heads 32 is positioned on one of two adjacent servo bands s and reads the servo signal on this servo band s.

[0062] Moreover, the other of the two servo read heads 32 is positioned on the other of the two adjacent servo bands s, and reads the servo signal on this servo band s.

[0063] At this time, the control device 26 judges, based on the reproduced waveform of the servo signal recording pattern 6, whether the servo read head 32 is accurately tracing the intended servo trace line T (see FIG. 4).

[0064] This principle will be explained. As shown in Fig. 4, the first stripe group 8 and the second stripe group 9 in the servo signal recording pattern 6 are inclined in opposite directions with respect to the width direction (Y-axis direction). Therefore, on the upper servo trace line T, the distance in the longitudinal direction (X-axis direction) between the first stripe group 8 and the second stripe group 9 is relatively narrow. On the other hand, on the lower servo trace line T, the distance in the longitudinal direction (X-axis direction) between the first stripe group 8 and the second stripe group 9 is relatively wide.

[0065] Therefore, by calculating the difference between the time when the reproduced waveform of the first group of stripes 8 is detected and the time when the reproduced waveform of the second group of stripes 9 is detected, the current position of the servo read head 32 in the width direction (Y-axis direction) relative to the magnetic recording medium 1 can be determined.

[0066] Therefore, the control device 26 can determine, based on the reproduced waveform of the servo signal, whether the servo read head 32 is accurately tracing the target servo trace line T. If the servo read head 32 is not accurately tracing the target servo trace line T, the control device 26 moves the head unit 30 in the width direction (Y'-axis direction) to adjust the position of the head unit 30.

[0067] Returning to FIG. 7, the data write / read head 33 records a data signal within the recording track 5 while moving along the recording track 5, with its position in the width direction being adjusted (if misaligned).

[0068] When the magnetic recording medium 1 is completely pulled out from the cartridge 21, the magnetic recording medium 1 then runs in the opposite direction (from the device 20 to the cartridge 21). At this time, the second head unit 30b is used as the head unit 30.

[0069] At this time, the servo trace line T used is the servo trace line T adjacent to the previous servo trace line T. In this case, the head unit 30 is moved in the width direction (Y'-axis direction) by the interval Ps between the servo trace lines T (=the recording track width Wd).

[0070] In this case, the data signal is recorded on the recording track 5 adjacent to the recording track 5 on which the data signal has just been recorded.

[0071] In this manner, the magnetic recording medium 1 travels back and forth many times with the running direction changed between the forward and reverse directions, while a data signal is recorded on the recording track 5.

[0072] Here, for example, assume that the number of servo trace lines T is 50, and the number of data write / read heads 33 included in the first head unit 30a (or the second head unit 30b) is 32. In this case, the number of recording tracks 5 included in one data band d is 50×32=1600, and in order to record data signals on all of these recording tracks 5, the magnetic recording medium 1 needs to make 25 round trips.

[0073] FIG. 8 is a diagram showing two stripes 7 in a servo signal recording pattern 6. As shown in FIG.

[0074] 8, among the plurality of stripes 7 included in the first stripe group 8 of the servo signal recording pattern 6, an arbitrary stripe 7 is designated as a first stripe 7a. Moreover, among the plurality of stripes 7 included in the second stripe group 9 of the servo signal recording pattern 6, an arbitrary stripe 7 is designated as a second stripe 7b.

[0075] An arbitrary servo trace line T among the plurality of servo trace lines T is defined as a first servo trace line T1, and a servo trace line T adjacent to the first servo trace line T1 is defined as a second servo trace line T2.

[0076] The intersection point between the first stripe 7a and the first servo trace line T1 is defined as P1. Note that, regarding this P1, any point on the first stripe 7a may be defined as P1.

[0077] The intersection of the first stripe 7a and the second servo trace line T2 is defined as P2. Alternatively, P2 may be a point on the first stripe 7a that is spaced apart from P1 by an interval Ps (i.e., the recording track width Wd) in the width direction (Y-axis direction).

[0078] The distance between P1 and P2 in the longitudinal direction (X-axis direction) is set to a distance D. The distance D corresponds to the amount of deviation between adjacent tracks in the longitudinal direction.

[0079] The intersection of the second stripe 7b and the first servo trace line T1 is designated as P3, and the intersection of the second stripe 7b and the second servo trace line T2 is designated as P4.

[0080] When the first servo trace line T1 is being traced, it is necessary to determine the difference between the time when the reproduced waveform is detected at P1 and the time when the reproduced waveform is detected at P3. This difference is defined as the first period.

[0081] Similarly, when the second trace line T is being traced, it is necessary to determine the difference between the time when the reconstructed waveform is detected at P2 and the time when the reconstructed waveform is detected at P4. This difference is referred to as the second period.

[0082] Next, consider the difference between the first period and the second period. Here, assume that the interval Ps of the servo trace lines T and the recording track width Wd are 1.56 μm, and the azimuth angle α is 12 degrees. In this case, the distance D is 1.56×tan12°, or 0.33 μm. The difference between the distance between P1 and P3 and the distance between P2 and P4 is twice the distance D, so it is 0.66 μm. At this time, if the running speed of the magnetic recording medium 1 is 5 m / s, it is 0.66 / 5000000, or 0.13 μs. This is the difference between the first period and the second period.

[0083] However, if the reproduction output of the servo signal is insufficient, such a small difference cannot be accurately determined. In particular, if the recording track width Wd is reduced and the interval Ps of the servo trace lines T is reduced in order to increase the number of recording tracks 5, the distance D becomes narrower and the difference between the first period and the second period becomes smaller.

[0084] Furthermore, with the recent increase in the capacity of magnetic tapes, the servo band width is expected to become narrower. In this case, in order to accommodate the increase in the capacity of magnetic tapes, it is necessary to increase the inclination angle of the azimuth angle with respect to the tape width direction. As a result, the azimuth loss with the servo read head increases, and a decrease in the signal-to-noise ratio (SNR) of the servo reproduction signal, which is the reproduction output of the servo signal, is unavoidable. Moreover, in the perpendicular magnetic recording method, there is a problem that the SNR of the servo reproduction signal is easily decreased due to the influence of the demagnetizing field in the perpendicular direction of the magnetic layer.

[0085] [Servo signal recording device] Next, a servo signal recording device will be described. Fig. 9 is a front view showing a typical servo signal recording device 100, and Fig. 10 is a partially enlarged view showing a part of it.

[0086] 9 and 10, the servo signal recording device 100 includes, in order from the upstream side in the transport direction of the magnetic recording medium 1, a feed roller 111, a pre-processing unit 112, a servo write head 113, a reproducing head unit 114, and a take-up roller 115. The servo signal recording device 100 also includes a drive unit 120 that drives the servo write head 113, and a controller 130 that performs overall control of the servo signal recording device 100. The controller 130 includes a control unit that performs overall control of each unit of the servo pattern recording device 100, a recording unit that stores various programs and data required for processing by the control unit, a display unit that displays data, an input unit that inputs data, and the like.

[0087] The feed roller 111 is capable of rotatably supporting the roll-shaped magnetic recording medium 1 before a servo signal is recorded thereon. The feed roller 111 is rotated in response to the driving of a driving source such as a motor, and feeds out the magnetic recording medium 1 downstream in response to the rotation.

[0088] The winding roller 115 rotates in synchronization with the delivery roller 111 in response to the drive of a drive source such as a motor, and winds up the magnetic recording medium 1 on which the servo signal is recorded in response to the rotation. The delivery roller 111 and the winding roller 115 are capable of moving the magnetic recording medium 1 at a constant speed within the transport path.

[0089] The servo write head 113 is disposed, for example, above (on the magnetic layer 13 side) of the magnetic recording medium 1. The servo write head 113 may be disposed below (on the substrate 11 side) of the magnetic recording medium 1. The servo write head 113 generates a magnetic field at a predetermined timing in response to a square wave pulse signal, and applies the magnetic field to a part of the magnetic layer 13 (after pretreatment) of the magnetic recording medium 1.

[0090] As a result, the servo write head 113 magnetizes a part of the magnetic layer 13 in a first direction to record a servo signal (hereinafter also referred to as a servo signal recording pattern 6) in the magnetic layer 13 (see the black arrow in FIG. 10 for the magnetization direction). The servo write head 113 is capable of recording the servo signal recording pattern 6 in each of the five servo bands s0 to s4 when the magnetic layer 13 passes below the servo write head 113.

[0091] The first direction, which is the magnetization direction of the servo signal recording pattern 6, includes a perpendicular component perpendicular to the top surface of the magnetic layer 13. That is, in this embodiment, since the magnetic layer 13 contains perpendicularly oriented magnetic powder, the servo signal recording pattern 6 recorded in the magnetic layer 13 includes a perpendicular magnetization component.

[0092] The pre-treatment unit 112 is disposed, for example, upstream of the servo write head 113 and below the magnetic recording medium 1 (on the substrate 11 side). The pre-treatment unit 112 may be disposed above the magnetic recording medium 1 (on the magnetic layer 13 side). The pre-treatment unit 112 includes a permanent magnet 112a that can rotate around the Y-axis direction (width direction of the magnetic recording medium 1) as the central axis of rotation. The shape of the permanent magnet 12a is, for example, a cylindrical shape or a polygonal prism shape, but is not limited thereto.

[0093] Before the servo pattern 6 is recorded by the servo write head 13, the permanent magnet 12a applies a magnetic field to the entire magnetic layer 4 using a DC magnetic field, thereby demagnetizing the entire magnetic layer 4. This allows the permanent magnet 112a to magnetize the magnetic layer 4 in advance in a second direction opposite to the magnetization direction of the servo pattern 6 (see the white arrow in FIG. 10). By thus making the two magnetization directions opposite to each other, the reproduced waveform of the servo signal obtained by reading the servo signal recording pattern 6 can be made symmetrical in the up-down direction (±).

[0094] The reproducing head section 114 is disposed on the upper side (magnetic layer 13 side) of the magnetic recording medium 1, downstream of the servo write head 113. The reproducing head section 114 reads the servo signal recording pattern 6 from the magnetic layer 13 of the magnetic recording medium 1 that has been preprocessed by the preprocessing section 112 and on which the servo signal recording pattern 6 has been recorded by the servo write head 113. Typically, the reproducing head section 114 detects magnetic flux generated from the surface of the servo band s when the magnetic layer 13 passes below the reproducing head section 114. The magnetic flux detected at this time becomes the reproduced waveform of the servo signal.

[0095] The servo read head 32 in the head unit 30 of the data recording device 20 described above also reproduces the servo signals recorded on the magnetic recording medium 1 using a similar principle.

[0096] [Servo signal playback output] 11 is a diagram illustrating the reproduced waveform of a servo signal and its output magnitude. (a) shows a first group of stripes 8 in a servo signal recording pattern 6 recorded on a magnetic layer 13, and (b) shows the magnitude of magnetization of each stripe 7 constituting the first group of stripes 7.

[0097] As shown in Fig. 11(b), the magnitude of the DC level of the residual magnetization of the magnetic layer 13 after the demagnetization process by the permanent magnet 12a is +Mr. When the servo write head 113 records the servo recording pattern 6 on the magnetic layer 13, the residual magnetization M of the area corresponding to each stripe 7 changes from the +Mr level to the -Mr level. As shown in Fig. 11(c), +Mr and -Mr correspond to the magnetization levels in the positive and negative directions of the residual magnetization M in the MH curve (hysteresis) of the magnetic layer 13 when the external magnetic field H is zero. In the figure, Hc is the coercive force.

[0098] The reproduction output of the servo signal is proportional to the absolute value of ΔMr, which corresponds to the difference in level of residual magnetization (the difference between +Mr and -Mr) in the magnetic layer 13 before and after recording the servo signal recording pattern 6. In other words, the larger ΔMr is, the larger the reproduction output of the servo reproduction signal is, resulting in a high SNR. Maximizing ΔMr is achieved by saturating recording the servo signal recording pattern 6.

[0099] 12, a recording current capable of generating an external magnetic field (-Hs) at which the magnetization of the magnetic layer 13 reaches saturation is supplied from the driving unit 120 to the servo write head 113 as a head magnetic field required for saturating the servo signal recording pattern 6. The magnitude of the recording current is determined by the magnetic properties of the magnetic layer 13 (residual magnetization, squareness ratio, degree of perpendicular orientation, etc.).

[0100] On the other hand, the perpendicular magnetic recording method is affected by the perpendicular demagnetizing field of the magnetic layer 13, so even if a head magnetic field that reaches saturation recording is generated, the servo signal recording pattern 6 may not be recorded at saturation. For this reason, a method is required to check whether the servo signal recording pattern 6 has been written properly.

[0101] Furthermore, to accommodate the increasing capacity of magnetic tapes, it is necessary to increase the azimuth angle α (see FIG. 11(a)) of each stripe 7 recorded as a servo signal. As a result, the azimuth loss with the reproducing head portion 114 increases, and the distance Δx (see FIG. 11(b)) of the reproducing head portion 114 passing through each stripe 7 becomes longer. As a result, the output waveform of the reproduced signal becomes elongated, and the output level tends to decrease during the signal processing process including averaging. From this perspective, too, there is an increasing need to saturate record the servo signal recording pattern 6.

[0102] Therefore, in this embodiment, in order to properly manage the magnetization level of the servo signal recorded in the magnetic layer 13, a unique index is defined, and a technology is developed to stably provide magnetic recording media that can suppress the deterioration of the servo playback signal that accompanies increased capacity.

[0103] That is, in this technology, assuming that the squareness ratio in the perpendicular direction of the magnetic layer is Sq, the peak-to-peak value of the first magnetic force gradient intensity observed by a magnetic force microscope when a servo signal is saturation recorded in the magnetic layer is F0(pp), and the peak-to-peak value of the second magnetic force gradient intensity observed by a magnetic force microscope for the servo signal recorded in the servo band is Fact.(pp), Sq×Fact.(pp) / F0(pp) The servo signal is recorded so that the index (Q) represented by the following formula is equal to or greater than a predetermined value.

[0104] The value of the index (Q) is 0.42 or more, preferably 0.45 or more, more preferably 0.5 or more, and further preferably 0.6 or more. By making the index (Q) 0.42 or more, it is possible to increase the SNR of the servo reproduction signal, as described later.

[0105] The squareness ratio (Sq) of the magnetic layer in the perpendicular direction is the ratio of the residual magnetization to the saturation magnetization in the perpendicular direction of the magnetic layer. The squareness ratio S typically depends on the residual magnetization (Mrt) and the perpendicular orientation of the magnetic particles that make up the magnetic layer.

[0106] The squareness ratio (Sq) is preferably 0.5 or more, more preferably 0.6 or more, more preferably 0.65 or more, and even more preferably 0.7 or more, which can improve the value of the index (Q).

[0107] The peak-to-peak value of the first magnetic force gradient strength (F0(pp)) is the peak-to-peak value of the magnetic force gradient strength observed by a magnetic force microscope when a servo signal is recorded to saturation in the servo band of the magnetic layer. The first magnetic force gradient strength corresponds to an ideal value in which the servo signal is recorded without being affected by demagnetization due to a demagnetizing field during recording. The first magnetic force gradient strength will be described below with reference to FIG. 13.

[0108] FIG. 13 is an explanatory diagram of the first magnetic force gradient intensity, in which (a) shows the recording magnetization level of one stripe 7 (see FIG. 11(a)) constituting part of the servo signal, (b) shows its MFM (magnetic force microscope) image, and (c) shows the peak value of the magnetic force gradient observed from the MFM image.

[0109] A magnetic force microscope is a device that visualizes the magnetic domain structure by utilizing the magnetic interaction between a magnetic sample and a magnetic probe, and is used to analyze the magnetization state of a magnetic sample. The magnetic probe is scanned in a direction perpendicular to the stripe 7. In an ideal state where the servo signal is saturated and recorded, the MFM image clearly shows two boundary images of the magnetized and non-magnetized regions, which correspond to the magnetization reversal parts, as shown in FIG. 13(b). As a result, as shown in FIG. 13(c), the two peak values ​​of the magnetic force gradient at each of the above-mentioned boundaries are maximum. The magnitude of the magnetic force gradient between these two peaks is defined as the peak-to-peak value (F0(pp)) of the first magnetic force gradient strength.

[0110] On the other hand, the peak-to-peak value of the second magnetic force gradient intensity (Fact.(pp)) is the peak-to-peak value of the magnetic force gradient intensity observed by a magnetic force microscope for a servo signal actually recorded on a servo band using the servo signal recording device 100 or the like. The second magnetic force gradient intensity is typically the magnetic force gradient intensity observed by a magnetic force microscope for a servo signal that is not saturation recorded, and is often lower than the first magnetic force gradient intensity due to the effect of demagnetization caused by a demagnetizing field when recording the servo signal.

[0111] Figures 14 and 15 are explanatory diagrams of the second magnetic force gradient strength (Fact.(pp)), where (a) shows the recording magnetization level of one stripe 7 (see Figure 11(a)) that constitutes part of the servo signal, (b) shows its MFM (magnetic force microscope) image, and (c) shows the peak value of the magnetic force gradient observed from the MFM image.

[0112] The servo signal written in the magnetic layer is usually affected by demagnetization due to the demagnetizing field of the magnetic layer during recording, as shown by symbol D1 in Fig. 14(a), and the residual magnetization (-Mr) of the servo signal does not reach the level of the residual magnetization during saturation recording. Also, as shown in Fig. 14(b), the MFM image shows two boundary images corresponding to the magnetization reversal parts blurred, and as a result, the peak value of the magnetic force gradient at each of the above-mentioned boundaries decreases, as shown in Fig. 14(c). The magnitude (peak-to-peak value) of the magnetic force gradient between these two peaks is defined as the peak-to-peak value (Fact.(pp)) of the second magnetic force gradient strength.

[0113] 14(a)-(c) show the state when the residual magnetization level (demagnetization level) of the magnetic layer before the servo signal is recorded reaches saturation. In contrast, FIG. 15(a)-(c) show the state when the residual magnetization level (demagnetization level) of the magnetic layer before the servo signal is recorded does not reach saturation. In this case, as shown in FIG. 15(a), the recording magnetization of the servo signal may be affected not only by the demagnetization caused by the demagnetization field during servo recording as shown by the symbol D1, but also by the demagnetization caused by the demagnetization field during demagnetization as shown by the symbol D2. In this case, as shown in FIG. 15(b) and (c), the MFM image may show another image around the two boundary images corresponding to the magnetization reversal portion, causing the waveform of the magnetic force gradient to be distorted. In such a case, the magnitude (peak-to-peak value) of the magnetic force gradient between the highest peaks in the waveform of the magnetic force gradient is defined as the second magnetic force gradient intensity peak-to-peak value (Fact.(pp)).

[0114] The ratio of Fact.(pp) to F0(pp) (Fact.(pp) / F0(pp)) is preferably 0.6 or more, more preferably 0.7 or more, and even more preferably 0.8 or more.

[0115] [Servo signal recording device for saturation recording] 16 is a partial schematic diagram showing a configuration of a servo signal recording device 200 according to an embodiment of the present technology. This servo signal recording device 200 is a novel device suitable for saturation recording of a servo signal.

[0116] As shown in Fig. 16, the servo signal recording device 200 includes a servo write head 210 and an auxiliary magnetic pole 220. Other configurations are similar to those of the servo signal recording device 100 described with reference to Fig. 9, so description thereof will be omitted.

[0117] The servo write head 210 has a magnetic core 213 and a coil 214 wound around the magnetic core 213. The magnetic core 213 has a gap portion 213G for recording a servo signal. The magnetic core 213 is made of a magnetic material having soft magnetic properties. The coil 214 magnetizes the magnetic core 213 by applying a recording current supplied from the driving unit 120 (see FIGS. 9 and 10).

[0118] Fig. 17 is an enlarged view of a main portion of part A in Fig. 16. Fig. 18 is a schematic plan view showing a partial region of the servo band s in the magnetic layer 13 of the magnetic recording medium 1.

[0119] The soft magnetic material constituting the magnetic core 213 is not particularly limited, and typically, an Fe (iron)-Ni (nickel) based or Co (cobalt) based metallic magnetic material such as permalloy is used. Alternatively, as shown in FIG. 17, the main body of the magnetic core 213 may be made of permalloy, and the vicinity of the gap portion 213F may be made of a CoFe based high magnetic permeability material. An example of a CoFe based material is Co 1-x Fe x (0.6≦x≦0.8) based materials.

[0120] As shown in Fig. 18, the gap portion 213G is formed in the magnetic core 213 with a " / " shaped groove and a "\" shaped groove spaced apart from each other in the running direction of the magnetic recording medium 1, and the magnetic layer 13 of the magnetic recording medium 1 running directly under the servo write head 210 is magnetized into each of the shapes by a leakage magnetic field (head magnetic field) from the gap portion 213G. The current applied to the coil 214 is typically a pulse current, and by controlling the timing of supplying the current, the servo signal recording pattern 6 consisting of a series of stripe groups 8 and 9 shown in Fig. 2 or 4 is formed. The azimuth angle α is adjusted by the inclination of each groove constituting the gap portion 213G.

[0121] The auxiliary magnetic pole 220 is composed of a pair of metal pieces 220a arranged facing the servo write head 210 with the magnetic layer 13 of the magnetic recording medium 1 in between. As shown in Fig. 18, each metal piece 220a is arranged tilted about the Z axis so as to face the gap portion 213G of the magnetic core 213 in the Z axis direction. The auxiliary magnetic pole 220 is typically arranged in a non-contact manner on the rear surface (support 11 or back layer 14) of the magnetic recording medium 1, and the shorter the facing distance to the gap portion 213G, the better.

[0122] Each metal piece 220a constituting the auxiliary magnetic pole 220 is made of a high magnetic permeability material, such as the above-mentioned CoFe-based material. The auxiliary magnetic pole 220 may include a base portion (not shown) that commonly supports each metal piece 220a in order to improve the ease of handling.

[0123] In the servo signal recording device 200 configured as above, a servo signal is recorded on the magnetic layer 13 while the magnetic recording medium 1 is running between the servo write head 210 and the auxiliary magnetic pole 220. At this time, the auxiliary magnetic pole 220 forms a magnetic path through which the leakage magnetic field (magnetic flux) from the gap portion 213G passes. As a result, the leakage magnetic field from the gap portion 213G is induced to penetrate the magnetic recording medium 1 in the thickness direction, so that the magnetic layer 13 can be easily magnetized in the vertical direction. Therefore, according to the servo signal recording device 200, the servo signal can be recorded in a saturation recording or a state close to it for the following reasons.

[0124] When performing saturation recording on a perpendicularly oriented film, it is necessary to apply a recording magnetic field exceeding Hs=Hc+4πMs due to the influence of the demagnetizing field (4πMs). For example, when the coercive force Hc is 3000 Oe and the saturation magnetization Ms is 300 emu / cm 3In the case of a magnetic field strength of 1.25 nm (the value for a typical vertically oriented barium ferrite), Hs=Hc+4πMs=6768 Oe, so a recording magnetic field of at least twice Hc is required. Furthermore, it is generally said that a magnetic field in the recording head gap of at least three times Hs is required to perform saturation recording. Therefore, if the recording head material is Ni45Fe55, which is commonly used in current magnetic tape drives, the magnetic field in the gap will be around 16,000 Oe, making saturation recording difficult on media with Hs=6768 Oe. However, when the auxiliary pole 220 is provided, the surface magnetization induced on the magnetic film surface is suppressed, and the demagnetizing field of 4πMs is cancelled out, so that Hs=Hc and saturation recording becomes possible. EXAMPLES

[0125] Next, various examples and comparative examples of the present technology will be described.

[0126] Example 1 Contains barium ferrite as magnetic powder, with a residual magnetization (Mrt) of 0.55 memu / cm 2 A magnetic recording medium was fabricated having a magnetic layer of 80 nm thickness with a squareness (Sq) of 0.7 (70%) in the perpendicular direction. While the fabricated magnetic recording medium was running at 5 m / s, a servo signal consisting of a servo signal recording pattern with an azimuth angle of 12° was recorded on the magnetic layer using a first servo signal recording device (see FIG. 16) equipped with an auxiliary pole (CoFe system, the same below). The servo write head was made of permalloy (Ni45Fe55), and the recording signal was a step signal with a recording current of 100%. A recording current of 100% refers to the recording current value at which the reproduction signal voltage is maximum when the reproduction signal voltage is monitored while changing the recording current.

[0127] The servo signal recorded by the above method can be considered to be saturation recorded in the magnetic layer due to the action of the above auxiliary magnetic pole. Therefore, in this embodiment, the peak-to-peak value of the magnetic force gradient intensity obtained from the MFM image of the magnetic layer on which the servo signal is recorded is set to the peak-to-peak value (F0(pp)) of the first magnetic force gradient intensity obtained when the servo signal is saturation recorded.

[0128] Next, using a second servo signal recording device that does not have an auxiliary magnetic pole, a servo signal with an azimuth angle of 12° was recorded by applying a step signal of 100% recording current to the servo write head while running the magnetic recording medium in the tape longitudinal direction at 5 m / s. The second servo signal recording device has the same configuration as the first servo signal recording device, except that it does not have an auxiliary magnetic pole.

[0129] Then, an MFM image of the magnetic layer on which the servo signal was recorded under the above conditions was obtained, and the peak-to-peak value (Fact.(pp)) of the second magnetic force gradient intensity, which is the magnetic force gradient intensity of the servo signal, was measured from the obtained MFM image.

[0130] For the measurements of F0(pp) and Fact.(pp), a magnetic force microscope "NanoScope III A D3100" manufactured by Bruker was used. The measurement conditions are as follows. Measurement mode: Phase Mode Scanning speed: 1.0Hz Number of data points: 512 x 512 The probe used was MFMR manufactured by Nanoworld.

[0131] Next, the ratio of Fact.(pp) to F0(pp), Fact.(pp) / F0(pp), was calculated from the measured Fact.(pp) value, and the value was 0.7. The index (Q), which is the product of this ratio and the squareness ratio (Sq) of the magnetic layer, was 0.49.

[0132] Next, the servo signal of the magnetic recording medium used for measuring Fact.(pp) was reproduced and its SNR was measured. For the measurement, a signal from a reproducing head part installed in a servo signal recording device was used. The measured value was a relative value when the SNR of the servo reproduction signal of a commercially available LTO7 format magnetic tape was set to 0 dB. As a result of the measurement, the SNR was 2.0 dB.

[0133] Example 2 A servo signal was recorded on the magnetic layer of a magnetic recording medium made of the same material as in Example 1, using a second servo signal recording device not equipped with an auxiliary pole, under the same conditions as in Example 1, except that the recording current was set to 90%. An MFM image of the recorded servo signal was obtained, and the peak-to-peak value of the magnetic force gradient intensity of the servo signal was measured from the MFM image, and this was taken as the peak-to-peak value (Fact.(pp)) of the second magnetic force gradient intensity of the servo signal in the magnetic recording medium.

[0134] The ratio of the Fact.(pp) of the servo signal to the F0(pp) measured in Example 1, Fact.(pp) / F0(pp), was calculated to be 0.65, and the index (Q), which is the product of the ratio and the squareness ratio (Sq) of the magnetic layer, was 0.455. Furthermore, the servo signal was reproduced under the same conditions as in Example 1 to measure the SNR, which was 1.0 dB.

[0135] Example 3 A servo signal was recorded on the magnetic layer of a magnetic recording medium made of the same material as in Example 1, using a second servo signal recording device not equipped with an auxiliary pole, under the same conditions as in Example 1, except that the recording current was set to 80%. An MFM image of the recorded servo signal was obtained, and the peak-to-peak value of the magnetic force gradient strength of the servo signal was measured from the MFM image, and this was taken as the peak-to-peak value (Fact.(pp)) of the second magnetic force gradient strength of the servo signal.

[0136] The ratio of Fact.(pp) / F0(pp) of the servo signal to F0(pp) measured in Example 1 was calculated to be 0.6, and the index (Q) value, which is the product of the ratio and the squareness ratio (Sq) of the magnetic layer, was 0.42. Furthermore, the servo signal was reproduced under the same conditions as in Example 1 to measure the SNR, which was 0.0 dB.

[0137] Example 4 Contains barium ferrite as magnetic powder, with a residual magnetization (Mrt) of 0.45 memu / cm 2 A magnetic recording medium was fabricated having a magnetic layer of 80 nm thickness with a squareness (Sq) of 0.6 (60%) in the perpendicular direction. While the fabricated magnetic recording medium was running at 5 m / s, a servo signal consisting of a servo signal recording pattern with an azimuth angle of 12° was recorded on the magnetic layer using a first servo signal recording device equipped with an auxiliary pole. The servo write head was made of permalloy, and the recording signal was a step signal with a recording current of 100%.

[0138] The servo signal recorded by the above method can be considered to be saturation recorded in the magnetic layer due to the action of the above auxiliary magnetic pole. Therefore, in this embodiment, the peak-to-peak value of the magnetic force gradient intensity obtained from the MFM image of the magnetic layer on which the servo signal is recorded is set to the peak-to-peak value (F0(pp)) of the first magnetic force gradient intensity obtained when the servo signal is saturation recorded.

[0139] Next, using a second servo signal recording device that did not have an auxiliary magnetic pole, the magnetic recording medium was run in the longitudinal direction of the tape at 5 m / s while a step signal of 100% recording current was applied to the servo write head to record a servo signal with an azimuth angle of 12°.

[0140] Then, an MFM image of the magnetic layer on which the servo signal was recorded under the above conditions was obtained, and the peak-to-peak value (Fact.(pp)) of the second magnetic force gradient intensity, which is the magnetic force gradient intensity of the servo signal, was measured from the obtained MFM image.

[0141] Next, the ratio of Fact.(pp) to F0(pp) was calculated from the measured Fact.(pp) value, Fact.(pp) / F0(pp), and the value was 0.7, and the index (Q), which is the product of the ratio and the squareness ratio (Sq) of the magnetic layer, was 0.42. Furthermore, the servo signal was reproduced under the same conditions as in Example 1, and the SNR was measured, and was 0.0 dB.

[0142] Example 5 Contains barium ferrite as magnetic powder, with a residual magnetization (Mrt) of 0.39 memu / cm 2 A magnetic recording medium was fabricated having a magnetic layer of 80 nm thickness with a squareness (Sq) of 0.5 (50%) in the perpendicular direction. While the fabricated magnetic recording medium was running at 5 m / s, a servo signal consisting of a servo signal recording pattern with an azimuth angle of 12° was recorded on the magnetic layer using a first servo signal recording device equipped with an auxiliary magnetic pole. The servo write head was made of permalloy, and the recording signal was a step signal with a recording current of 100%.

[0143] The servo signal recorded by the above method can be considered to be saturation recorded in the magnetic layer due to the action of the above auxiliary magnetic pole. Therefore, in this embodiment, the peak-to-peak value of the magnetic force gradient intensity obtained from the MFM image of the magnetic layer on which the servo signal is recorded is set to the peak-to-peak value (F0(pp)) of the first magnetic force gradient intensity obtained when the servo signal is saturation recorded.

[0144] Next, using a first servo signal recording device equipped with an auxiliary magnetic pole, the magnetic recording medium was run in the longitudinal direction of the tape at 5 m / s while a step signal of 90% of the recording current was applied to the servo write head to record a servo signal with an azimuth angle of 12°.

[0145] Then, an MFM image of the magnetic layer on which the servo signal was recorded under the above conditions was obtained, and the peak-to-peak value (Fact.(pp)) of the second magnetic force gradient intensity, which is the magnetic force gradient intensity of the servo signal, was measured from the obtained MFM image.

[0146] Next, the ratio of Fact.(pp) to F0(pp) was calculated from the measured Fact.(pp) value, Fact.(pp) / F0(pp), and the value was 0.9, and the value of the index (Q), which is the product of the ratio and the squareness ratio (Sq) of the magnetic layer, was 0.45.Furthermore, the servo signal was reproduced under the same conditions as in Example 1, and the SNR was measured, and was 0.8 dB.

[0147] Comparative Example 1 A servo signal was recorded on the magnetic layer of a magnetic recording medium made of the same material as in Example 1, using a second servo signal recording device not equipped with an auxiliary pole, under the same conditions as in Example 1, except that the recording current was set to 70%. An MFM image of the recorded servo signal was obtained, and the peak-to-peak value of the magnetic force gradient intensity of the servo signal was measured from the MFM image, and this was taken as the peak-to-peak value (Fact.(pp)) of the second magnetic force gradient intensity of the servo signal in the magnetic recording medium.

[0148] The ratio of Fact.(pp) / F0(pp) of the servo signal to F0(pp) measured in Example 1 was calculated to be 0.5, and the index (Q) value, which is the product of the ratio and the squareness ratio (Sq) of the magnetic layer, was 0.35. Furthermore, the servo signal was reproduced under the same conditions as in Example 1 to measure the SNR, which was -2.0 dB.

[0149] Comparative Example 2 A servo signal was recorded on the magnetic layer of a magnetic recording medium made of the same material as in Example 5, using a first servo signal recording device equipped with an auxiliary pole, under the same conditions as in Example 5, except that the recording current was set to 80%. An MFM image of the recorded servo signal was obtained, and the peak-to-peak value of the magnetic force gradient intensity of the servo signal was measured from the MFM image, and this was taken as the peak-to-peak value (Fact.(pp)) of the second magnetic force gradient intensity of the servo signal in the magnetic recording medium.

[0150] The ratio of Fact.(pp) / F0(pp) of the servo signal to F0(pp) measured in Example 5 was calculated to be 0.8, and the index (Q) value, which is the product of the ratio and the squareness ratio (Sq) of the magnetic layer, was 0.4. Furthermore, the servo signal was reproduced under the same conditions as in Example 1 to measure the SNR, which was -0.5 dB.

[0151] Comparative Example 3 A servo signal was recorded on the magnetic layer of a magnetic recording medium made of the same material as in Example 5, using a second servo signal recording device not equipped with an auxiliary pole, under the same conditions as in Example 5, except that the recording current was set to 100%. An MFM image of the recorded servo signal was obtained, and the peak-to-peak value of the magnetic force gradient intensity of the servo signal was measured from the MFM image, and this was taken as the peak-to-peak value (Fact.(pp)) of the second magnetic force gradient intensity of the servo signal in the magnetic recording medium.

[0152] The ratio of Fact.(pp) / F0(pp) of the servo signal to F0(pp) measured in Example 5 was calculated to be 0.7, and the index (Q) value, which is the product of the ratio and the squareness ratio (Sq) of the magnetic layer, was 0.35. Furthermore, the servo signal was reproduced under the same conditions as in Example 1 to measure the SNR, which was -2.0 dB.

[0153] Comparative Example 4 Contains barium ferrite as magnetic powder, with a residual magnetization (Mrt) of 0.35 memu / cm 2 A magnetic recording medium was fabricated having a magnetic layer of 80 nm thickness with a squareness (Sq) of 0.45 (45%) in the perpendicular direction. While running the fabricated magnetic recording medium at 5 m / s, a servo signal consisting of a servo signal recording pattern with an azimuth angle of 12° was recorded on the magnetic layer using a first servo signal recording device equipped with an auxiliary magnetic pole. The servo write head was made of permalloy, and the recording signal was a step signal with a recording current of 100%.

[0154] The servo signal recorded by the above method can be considered to be saturation recorded in the magnetic layer due to the action of the above auxiliary magnetic pole. Therefore, in this embodiment, the peak-to-peak value of the magnetic force gradient intensity obtained from the MFM image of the magnetic layer on which the servo signal is recorded is set to the peak-to-peak value (F0(pp)) of the first magnetic force gradient intensity obtained when the servo signal is saturation recorded.

[0155] Next, using a second servo signal recording device that did not have an auxiliary magnetic pole, the magnetic recording medium was run in the longitudinal direction of the tape at 5 m / s while a step signal of 100% recording current was applied to the servo write head to record a servo signal with an azimuth angle of 12°.

[0156] Then, an MFM image of the magnetic layer on which the servo signal was recorded under the above conditions was obtained, and the peak-to-peak value (Fact.(pp)) of the second magnetic force gradient intensity, which is the magnetic force gradient intensity of the servo signal, was measured from the obtained MFM image.

[0157] Next, the ratio of Fact.(pp) to F0(pp) was calculated from the measured Fact.(pp) value, Fact.(pp) / F0(pp), and the value was 0.7, and the value of the index (Q), which is the product of the ratio and the squareness ratio (Sq) of the magnetic layer, was 0.315.Furthermore, the servo signal was reproduced under the same conditions as in Example 1, and the SNR was measured, which was -2.5 dB.

[0158] The conditions and results of Examples 1 to 5 and Comparative Examples 1 to 3 are summarized in Table 1.

[0159] [Table 1]

[0160] As shown in Table 1, the SNR of the servo reproduction signal in Examples 1 to 5, in which the value of index Q, which is the product of the perpendicular squareness ratio (Sq) of the magnetic layer and the ratio of the magnetic force gradient strength of the servo signal (Fact.(pp) / F0(pp)), is 0.42 or more, is 0 dB or more, and the results are equal to or better than the SNR of the servo reproduction signal of the magnetic recording medium adopted in LTO7. Figure 19 shows the relationship between the SNR and index Q.

[0161] In particular, in Examples 1, 2, and 5, in which the value of index Q is 0.45 (rounded to one decimal place) or more, an SNR of 0.8 dB or more is obtained, and it is expected that a good SNR can be ensured even when the azimuth angle of the servo signal increases due to the increased capacity of magnetic recording media.

[0162] Furthermore, by using the first servo signal recording device equipped with an auxiliary magnetic pole for recording the servo signal, it is possible to increase the index Q compared to using the second servo signal recording device equipped with no auxiliary magnetic pole. This is believed to be because the magnetic susceptibility in the perpendicular direction of the magnetic layer is further increased by the magnetic flux induction effect of the auxiliary magnetic pole, resulting in the realization of saturation magnetization of the servo signal or a state close to it, which leads to an increase in the index Q.

[0163] As described above, by referring to the index Q, which is the product of the perpendicular squareness (Sq) of the magnetic layer and the ratio of the magnetic force gradient strength of the servo signal (Fact.(pp) / F0(pp)), it is possible to estimate the magnetization state of the servo signal of the magnetic recording medium and the SNR of the reproduced signal. This makes it easier to manage the magnetic recording medium, and makes it possible to provide a magnetic recording medium that can achieve a high SNR of the servo reproduced signal. It is also possible to suppress the deterioration of the SNR of the servo reproduced signal due to the increased capacity of the magnetic recording medium.

[0164] <Details of magnetic recording media> Next, the magnetic recording medium 1 will be described in detail.

[0165] [Base material] The substrate 11 is a non-magnetic support that supports the non-magnetic layer 12 and the magnetic layer 13. The substrate 11 has a long film shape. The upper limit of the average thickness of the substrate 11 is 4.0 μm, preferably 4.2 μm, more preferably 3.8 μm, and even more preferably 3.4 μm. When the upper limit of the average thickness of the substrate 11 is 4.2 μm or less, the recording capacity that can be recorded in one cartridge 21 (see FIG. 5) can be made higher than that of a general magnetic recording medium.

[0166] The average thickness of the substrate 11 is obtained as follows. First, a magnetic recording medium 1 with a width of 1 / 2 inch is prepared and cut to a length of 250 mm to prepare a sample. Next, layers other than the substrate 11 of the sample (i.e., the nonmagnetic layer 12, the magnetic layer 13, and the back layer 14) are removed with a solvent such as MEK (methyl ethyl ketone) or dilute hydrochloric acid. Next, the thickness of the sample (substrate 11) is measured at five or more positions using a Mitutoyo laser hologram as a measuring device, and the measured values ​​are simply averaged (arithmetic average) to calculate the average thickness of the substrate 11. Note that the measurement positions are selected randomly from the sample.

[0167] The substrate 11 includes at least one of polyesters, polyolefins, cellulose derivatives, vinyl resins, and other polymer resins, for example. When the substrate 11 includes two or more of the above materials, the two or more materials may be mixed, copolymerized, or laminated.

[0168] The polyesters include, for example, at least one of PET (polyethylene terephthalate), PEN (polyethylene naphthalate), PBT (polybutylene terephthalate), PBN (polybutylene naphthalate), PCT (polycyclohexylene dimethylene terephthalate), PEB (polyethylene-p-oxybenzoate), and polyethylene bisphenoxycarboxylate.

[0169] The polyolefins include, for example, at least one of PE (polyethylene) and PP (polypropylene). The cellulose derivatives include, for example, at least one of cellulose diacetate, cellulose triacetate, CAB (cellulose acetate butyrate) and CAP (cellulose acetate propionate). The vinyl resins include, for example, at least one of PVC (polyvinyl chloride) and PVDC (polyvinylidene chloride).

[0170] Other polymer resins include, for example, at least one of PA (polyamide, nylon), aromatic PA (aromatic polyamide, aramid), PI (polyimide), aromatic PI (aromatic polyimide), PAI (polyamideimide), aromatic PAI (aromatic polyamideimide), PBO (polybenzoxazole, such as Zylon (registered trademark)), polyether, PEK (polyetherketone), PEEK (polyetheretherketone), polyetherester, PES (polyethersulfone), PEI (polyetherimide), PSF (polysulfone), PPS (polyphenylene sulfide), PC (polycarbonate), PAR (polyarylate), and PU (polyurethane).

[0171] [Magnetic layer] The magnetic layer 13 is a recording layer for recording data signals. It contains magnetic powder, a binder, conductive particles, etc. The magnetic layer 13 may further contain additives such as a lubricant, an abrasive, and an anti-rust agent, as necessary. The magnetic layer 13 has a surface provided with a large number of holes. A lubricant is stored in these holes. The large number of holes are preferably extended in a direction perpendicular to the surface of the magnetic layer.

[0172] The thickness of the magnetic layer 13 is typically 35 nm or more and 90 nm or less. In this way, by making the thickness of the magnetic layer 13 35 nm or more and 90 nm or less, it is possible to improve the electromagnetic conversion characteristics. Furthermore, from the viewpoint of the half-width of an isolated waveform in the reproduced waveform of a servo signal, the thickness of the magnetic layer 13 is preferably 90 nm or less, more preferably 80 nm or less, more preferably 60 nm or less, more preferably 50 nm or less, and even more preferably 40 nm or less. By making the thickness of the magnetic layer 13 90 nm or less, it is possible to narrow the half-width of an isolated waveform in the reproduced waveform of a servo signal (195 nm or less), and make the peak of the reproduced waveform of the servo signal sharp. This improves the reading accuracy of the servo signal, so that the number of recording tracks can be increased and the recording density of data can be improved.

[0173] The thickness of the magnetic layer 13 can be determined, for example, as follows: First, the magnetic recording medium 1 is thinned perpendicularly to its main surface to prepare a test piece, and the cross section of the test piece is observed with a transmission electron microscope (TEM) under the following conditions. Equipment: TEM (Hitachi H9000NAR) Acceleration voltage: 300 kV Magnification: 100,000x

[0174] Next, using the obtained TEM image, the thickness of magnetic layer 13 is measured at at least 10 or more positions in the longitudinal direction of magnetic recording medium 10, and then these measured values ​​are simply averaged (arithmetic mean) to determine the thickness of magnetic layer 13. Note that the measurement positions are selected at random from the test piece.

[0175] (magnetic powder) The magnetic powder includes a powder of nanoparticles containing ε-iron oxide (hereinafter referred to as "ε-iron oxide particles"). Even fine particles of ε-iron oxide particles can obtain high coercivity. It is preferable that the ε-iron oxide contained in the ε-iron oxide particles has a crystal orientation preferentially in the thickness direction (perpendicular direction) of the magnetic recording medium 1.

[0176] The ε-iron oxide particles are spherical or nearly spherical, or cubic or nearly cubic. Because the ε-iron oxide particles have the above-mentioned shapes, when the ε-iron oxide particles are used as the magnetic particles, the contact area between the particles in the thickness direction of the magnetic recording medium 1 can be reduced and the aggregation between the particles can be suppressed, compared to when hexagonal plate-shaped barium ferrite particles are used as the magnetic particles. Therefore, the dispersibility of the magnetic powder can be improved, and a better SNR (Signal-to-Noise Ratio) can be obtained.

[0177] The ε-iron oxide particles have a core-shell structure. Specifically, the ε-iron oxide particles have a core and a two-layered shell portion provided around the core. The two-layered shell portion has a first shell portion provided on the core and a second shell portion provided on the first shell portion.

[0178] The core portion contains ε-iron oxide. The ε-iron oxide contained in the core portion preferably has ε-Fe2O3 crystals as a main phase, and more preferably is made of single-phase ε-Fe2O3.

[0179] The first shell portion covers at least a part of the periphery of the core portion. Specifically, the first shell portion may cover a part of the periphery of the core portion, or may cover the entire periphery of the core portion. From the viewpoint of ensuring sufficient exchange coupling between the core portion and the first shell portion and improving magnetic properties, it is preferable that the first shell portion covers the entire surface of the core portion 21.

[0180] The first shell portion is a so-called soft magnetic layer, and includes a soft magnetic material such as α-Fe, a Ni-Fe alloy, an Fe-Si-Al alloy, etc. The α-Fe may be obtained by reducing ε-iron oxide included in the core portion 21.

[0181] The second shell portion is an oxide coating serving as an anti-oxidation layer. The second shell portion includes α-iron oxide, aluminum oxide, or silicon oxide. The α-iron oxide includes at least one type of iron oxide, for example, Fe3O4, Fe2O3, and FeO. When the first shell portion includes α-Fe (soft magnetic material), the α-iron oxide may be obtained by oxidizing the α-Fe included in the first shell portion 22a.

[0182] By having the first shell portion as described above, the coercivity Hc of the ε iron oxide particles as a whole (core-shell particles) can be adjusted to a coercivity Hc suitable for recording while maintaining a high coercivity Hc of the core portion alone to ensure thermal stability. Furthermore, by having the second shell portion as described above, it is possible to prevent the ε iron oxide particles from being exposed to air during and before the manufacturing process of the magnetic recording medium, which would cause rust or the like on the particle surface, and thus to prevent deterioration of the properties of the ε iron oxide particles. Therefore, deterioration of the properties of the magnetic recording medium 1 can be prevented.

[0183] The average particle size (average maximum particle size) of the magnetic powder is preferably 22 nm or less, more preferably 8 nm or more and 22 nm or less, and even more preferably 12 nm or more and 22 nm or less.

[0184] The average aspect ratio of the magnetic powder is preferably 1 or more and 2.5 or less, more preferably 1 or more and 2.1 or less, and even more preferably 1 or more and 1.8 or less. When the average aspect ratio of the magnetic powder is within the range of 1 or more and 2.5 or less, aggregation of the magnetic powder can be suppressed, and the resistance applied to the magnetic powder when the magnetic powder is vertically oriented in the process of forming the magnetic layer 13 can be suppressed. Therefore, the vertical orientation of the magnetic powder can be improved.

[0185] The average volume Vave (particle volume) of the magnetic powder is preferably 2300 nm 3 Less than or equal to 2200 nm, preferably 3 Less than or equal to 2100 nm, preferably 3 Less than or equal to 1950 nm, more preferably 3Less than or equal to 1600 nm, more preferably 3 Below 1300 nm, and even more preferably below 1300 nm 3 The average volume of the magnetic powder is 2300 nm 3 If it is less than this, the half-width of the isolated waveform in the reproduced waveform of the servo signal can be narrowed (195 nm or less), and the peak of the reproduced waveform of the servo signal can be made sharper. This improves the accuracy of reading the servo signal, so the number of recording tracks can be increased and the data recording density can be improved (details will be described later). Note that the smaller the average volume Vave of the magnetic powder, the better, so there is no particular limit to the volume, but the lower limit can be set to 1000 nm, for example. 3 That is all.

[0186] The average particle size, average aspect ratio and average volume Vave of the magnetic powder are obtained as follows (for example, when the magnetic powder has a shape such as a sphere like ε iron oxide particles). First, the magnetic recording medium 1 to be measured is processed by a FIB (Focused Ion Beam) method or the like to prepare a thin piece, and the cross section of the thin piece is observed by a TEM. Next, 50 magnetic powders are randomly selected from the TEM photograph, and the long axis length DL and short axis length DS of each magnetic powder are measured. Here, the long axis length DL means the maximum distance between two parallel lines drawn from all angles so as to be tangent to the outline of the magnetic powder (so-called maximum Feret diameter). On the other hand, the short axis length DS means the maximum length of the magnetic powder in the direction perpendicular to the long axis of the magnetic powder.

[0187] Next, the long axis lengths DL of the 50 measured magnetic powder particles are simply averaged (arithmetic mean) to determine the average long axis length DLave. The average long axis length DLave thus determined is the average particle size of the magnetic powder. The short axis lengths DS of the 50 measured magnetic powder particles are also simply averaged (arithmetic mean) to determine the average short axis length DSave. Next, the average aspect ratio of the magnetic powder (DLave / DSave) is determined from the average long axis length DLave and the average short axis length DSave.

[0188] Next, the average volume Vave (particle volume) of the magnetic powder is calculated using the average major axis length DLave from the following formula. Vave = π / 6 × DLave 3

[0189] In the above description, the ε-iron oxide particles have a shell part with a two-layer structure, but the ε-iron oxide particles may have a shell part with a single-layer structure. In this case, the shell part has the same configuration as the first shell part. However, from the viewpoint of suppressing deterioration of the properties of the ε-iron oxide particles, it is preferable that the ε-iron oxide particles have a shell part with a two-layer structure, as described above.

[0190] In the above description, the ε iron oxide particles have a core-shell structure, but the ε iron oxide particles may contain an additive instead of the core-shell structure, or may have a core-shell structure and contain an additive. In this case, part of the Fe in the ε iron oxide particles is substituted with the additive. By containing an additive in the ε iron oxide particles, the coercive force Hc of the ε iron oxide particles as a whole can be adjusted to a coercive force Hc suitable for recording, thereby improving ease of recording. The additive is a metal element other than iron, preferably a trivalent metal element, more preferably at least one of Al, Ga and In, and even more preferably at least one of Al and Ga.

[0191] Specifically, ε-iron oxide containing additives is ε-Fe 2-x M x O3 crystal (wherein M is a metal element other than iron, preferably a trivalent metal element, more preferably at least one of Al, Ga and In, and even more preferably at least one of Al and Ga. x is, for example, 0 <x<1である。)である。

[0192] The magnetic powder may include a powder of nanoparticles containing hexagonal ferrite (hereinafter referred to as "hexagonal ferrite particles"). The hexagonal ferrite particles have, for example, a hexagonal plate shape or a nearly hexagonal plate shape. The hexagonal ferrite preferably includes at least one of Ba, Sr, Pb, and Ca, more preferably at least one of Ba and Sr. The hexagonal ferrite may specifically be, for example, barium ferrite or strontium ferrite. The barium ferrite may further include at least one of Sr, Pb, and Ca in addition to Ba. The strontium ferrite may further include at least one of Ba, Pb, and Ca in addition to Sr.

[0193] More specifically, hexagonal ferrite has the general formula MFe 12 O 19 The average composition is represented by the formula: where M is, for example, at least one metal selected from Ba, Sr, Pb, and Ca, and preferably at least one metal selected from Ba and Sr. M may be a combination of Ba and at least one metal selected from the group consisting of Sr, Pb, and Ca. M may also be a combination of Sr and at least one metal selected from the group consisting of Ba, Pb, and Ca. In the above general formula, a part of Fe may be substituted with another metal element.

[0194] When the magnetic powder contains hexagonal ferrite particles, the average particle size of the magnetic powder is preferably 50 nm or less, more preferably 10 nm to 40 nm, and even more preferably 15 nm to 30 nm. When the magnetic powder contains hexagonal ferrite particles, the average aspect ratio and the average volume Vave of the magnetic powder are as described above.

[0195] The average particle size, average aspect ratio, and average volume Vave of the magnetic powder are obtained as follows (for example, when the magnetic powder has a plate-like shape such as hexagonal ferrite). First, the magnetic recording medium 1 to be measured is processed by the FIB method or the like to prepare a thin piece, and the cross section of the thin piece is observed by TEM. Next, 50 magnetic powder particles oriented at an angle of 75 degrees or more to the horizontal direction are randomly selected from the TEM photograph, and the maximum plate thickness DA of each magnetic powder is measured. Next, the maximum plate thicknesses DA of the 50 measured magnetic powder particles are simply averaged (arithmetic mean) to obtain the average maximum plate thickness DAave.

[0196] Next, the surface of the magnetic layer 13 of the magnetic recording medium 1 is observed by TEM. Next, 50 magnetic powder particles are randomly selected from the TEM photograph, and the maximum plate diameter DB of each magnetic powder particle is measured. Here, the maximum plate diameter DB means the maximum distance between two parallel lines drawn from all angles so as to be tangent to the outline of the magnetic powder particle (so-called maximum Feret diameter). Next, the maximum plate diameters DB of the 50 measured magnetic powder particles are simply averaged (arithmetic mean) to obtain the average maximum plate diameter DBave. The average maximum plate diameter DBave thus obtained is then regarded as the average particle size of the magnetic powder particle. Next, the average aspect ratio (DBave / DAave) of the magnetic powder particle is obtained from the average maximum plate thickness DAave and the average maximum plate diameter DBave.

[0197] Next, the average maximum plate thickness DAave and the average maximum plate diameter DBave are used to calculate the average volume Vave (particle volume) of the magnetic powder according to the following formula.

number

[0198] The magnetic powder may contain a powder of nanoparticles containing Co-containing spinel ferrite (hereinafter referred to as "cobalt ferrite particles"). The cobalt ferrite particles preferably have uniaxial anisotropy. The cobalt ferrite particles have, for example, a cubic or nearly cubic shape. The Co-containing spinel ferrite may further contain at least one of Ni, Mn, Al, Cu, and Zn in addition to Co.

[0199] The Co-containing spinel ferrite has, for example, an average composition represented by the following formula (1). Co x M y FeO Z (1) (In formula (1), M is, for example, at least one metal selected from the group consisting of Ni, Mn, Al, Cu, and Zn. x is a value within the range of 0.4≦x≦1.0. y is a value within the range of 0≦y≦0.3. However, x and y satisfy the relationship of (x+y)≦1.0. z is a value within the range of 3≦z≦4. A part of Fe may be substituted with another metal element.)

[0200] When the magnetic powder contains cobalt ferrite particles, the average particle size of the magnetic powder is preferably 25 nm or less, more preferably 23 nm or less. When the magnetic powder contains cobalt ferrite particles, the average aspect ratio of the magnetic powder is determined by the above method, and the average volume Vave of the magnetic powder is determined by the following method.

[0201] When the magnetic powder has a cubic shape like cobalt ferrite particles, the average volume Vave (particle volume) of the magnetic powder can be calculated as follows. First, the surface of the magnetic layer 13 of the magnetic recording medium 1 is observed by TEM, and then 50 magnetic powder particles are randomly selected from the TEM photograph, and the side length DC of each magnetic powder is measured. Next, the side lengths DC of the measured 50 magnetic powder particles are simply averaged (arithmetic mean) to calculate the average side length DCave. Next, the average volume Vave (particle volume) of the magnetic powder is calculated from the following formula using the average side length DCave. Vave=DCave 3

[0202] (Binding agent) As the binder, a resin having a structure in which a crosslinking reaction is given to a polyurethane resin, a vinyl chloride resin, or the like is preferable. However, the binder is not limited to these, and other resins may be appropriately blended depending on the physical properties required for the magnetic recording medium 1. There is no particular limitation on the resin to be blended, so long as it is a resin that is generally used in coating-type magnetic recording media 1.

[0203] Examples of the polymer include polyvinyl chloride, polyvinyl acetate, vinyl chloride-vinyl acetate copolymer, vinyl chloride-vinylidene chloride copolymer, vinyl chloride-acrylonitrile copolymer, acrylic acid ester-acrylonitrile copolymer, acrylic acid ester-vinyl chloride-vinylidene chloride copolymer, vinyl chloride-acrylonitrile copolymer, acrylic acid ester-acrylonitrile copolymer, acrylic acid ester-vinylidene chloride copolymer, methacrylic acid ester-vinylidene chloride copolymer, methacrylic acid ester-vinyl chloride copolymer, methacrylic acid ester-ethylene copolymer, polyvinyl fluoride, vinylidene chloride-acrylonitrile copolymer, acrylonitrile-butadiene copolymer, polyamide resin, polyvinyl butyral, cellulose derivatives (cellulose acetate butyrate, cellulose diacetate, cellulose triacetate, cellulose propionate, nitrocellulose), styrene-butadiene copolymer, polyester resin, amino resin, and synthetic rubber.

[0204] Examples of the thermosetting resin or reactive resin include phenol resin, epoxy resin, urea resin, melamine resin, alkyd resin, silicone resin, polyamine resin, and urea formaldehyde resin.

[0205] Furthermore, in order to improve the dispersibility of the magnetic powder, polar functional groups such as -SO3M, -OSO3M, -COOM, and P=O(OM)2 may be introduced into each of the above-mentioned binders, where M is a hydrogen atom or an alkali metal such as lithium, potassium, or sodium.

[0206] Furthermore, the polar functional group is -NR1R2, -NR1R2R3 + X - Side chain type with terminal group of >NR1R2 + X - In the formula, R1, R2, and R3 are hydrogen atoms or hydrocarbon groups, and X - is a halogen element ion such as fluorine, chlorine, bromine, or iodine, or an inorganic or organic ion. Examples of the polar functional group include -OH, -SH, -CN, and an epoxy group.

[0207] (Lubricant) The lubricant preferably contains a compound represented by the following general formula (1) and a compound represented by the following general formula (2). When the lubricant contains these compounds, the dynamic friction coefficient of the surface of the magnetic layer 13 can be particularly reduced. Therefore, the running properties of the magnetic recording medium 1 can be further improved. CH3(CH2) n COOH (1) (In the general formula (1), n ​​is an integer selected from the range of 14 to 22.) CH3(CH2) p COO(CH2) q CH3···(2) (In the general formula (2), p is an integer selected from the range of 14 to 22, and q is an integer selected from the range of 2 to 5.)

[0208] (Additives) The magnetic layer 13 may further contain non-magnetic reinforcing particles such as aluminum oxide (α, β or γ alumina), chromium oxide, silicon oxide, diamond, garnet, emery, boron nitride, titanium carbide, silicon carbide, titanium carbide, titanium oxide (rutile or anatase titanium oxide), etc.

[0209] [Nonmagnetic layer 12] The non-magnetic layer 12 contains a non-magnetic powder and a binder. The non-magnetic layer 12 may contain additives such as conductive particles, a lubricant, a hardener, and an anti-rust material, as necessary.

[0210] The thickness of the nonmagnetic layer 12 is preferably 0.6 μm to 2.0 μm, more preferably 0.6 μm to 1.4 μm, more preferably 0.8 μm to 1.4 μm, and more preferably 0.6 μm to 1.0 μm. The thickness of the nonmagnetic layer 12 can be determined by the same method (e.g., TEM) as that for determining the thickness of the magnetic layer 13. The magnification of the TEM image is appropriately adjusted according to the thickness of the nonmagnetic layer 12.

[0211] (Non-magnetic powder) The non-magnetic powder includes at least one of inorganic particle powder and organic particle powder. The non-magnetic powder may also include a carbon material such as carbon black. One type of non-magnetic powder may be used alone, or two or more types of non-magnetic powder may be used in combination. The inorganic particles include, for example, metals, metal oxides, metal carbonates, metal sulfates, metal nitrides, metal carbides, or metal sulfides. The shape of the non-magnetic powder may be, for example, various shapes such as needles, spheres, cubes, and plates, but is not limited thereto.

[0212] (Binding agent) The binder is the same as that used in the magnetic layer 13 described above.

[0213] [Back layer 14] The back layer 14 contains a nonmagnetic powder and a binder. The back layer 14 may contain additives such as a lubricant, a hardener, and an antistatic agent, as necessary. The nonmagnetic powder and the binder may be the same materials as those used for the nonmagnetic layer 12 described above.

[0214] (Non-magnetic powder) The average particle size of the non-magnetic powder is preferably 10 nm or more and 150 nm or less, more preferably 15 nm or more and 110 nm or less. The average particle size of the non-magnetic powder is determined in the same manner as the average particle size D of the magnetic powder described above. The non-magnetic powder may contain non-magnetic powder having two or more particle size distributions.

[0215] The upper limit of the average thickness of the back layer 14 is preferably 0.6 μm or less, more preferably 0.5 μm or less, and even more preferably 0.4 μm or less. If the upper limit of the average thickness of the back layer 14 is 0.6 μm or less, the thickness of the nonmagnetic layer 12 and the substrate 11 can be kept thick even when the average thickness of the magnetic recording medium 1 is 5.6 μm, so that the running stability of the magnetic recording medium 1 in a recording and reproducing device can be maintained. The lower limit of the average thickness of the back layer 14 is not particularly limited, but is, for example, 0.2 μm or more.

[0216] The average thickness of the back layer 14 is obtained as follows. First, a magnetic recording medium 1 having a width of 1 / 2 inch is prepared, and then cut into a length of 250 mm to prepare a sample. Next, the thickness of the sample is measured at five or more points using a Mitutoyo laser hologram as a measuring device, and the measured values ​​are simply averaged (arithmetic average) to obtain the average thickness t of the magnetic recording medium 1. T [μm] is calculated. The measurement positions are selected randomly from the sample. Next, the back layer 14 of the sample is removed with a solvent such as MEK (methyl ethyl ketone) or dilute hydrochloric acid. After that, the thickness of the sample is measured again at five or more points using the above-mentioned laser hologram, and the measured values ​​are simply averaged (arithmetic average) to obtain the average thickness t of the magnetic recording medium 1 from which the back layer 14 has been removed. B [μm] is calculated. The measurement positions are selected randomly from the sample. Then, the average thickness t of the back layer 14 is calculated from the following formula: b Calculate [μm]. t b [μm]=t T [μm]-t B [μm]

[0217] The back layer 14 has a surface on which a large number of protrusions are provided. The large number of protrusions are intended to form a large number of holes in the surface of the magnetic layer 13 when the magnetic recording medium 1 is wound in a roll. The large number of holes are composed of, for example, a large number of non-magnetic particles protruding from the surface of the back layer 14.

[0218] In the explanation given here, a large number of protrusions provided on the surface of the back layer 14 are transferred to the surface of the magnetic layer 13 to form a large number of holes in the surface of the magnetic layer 13, but the method of forming a large number of holes is not limited to this. For example, a large number of holes may be formed in the surface of the magnetic layer 13 by adjusting the type of solvent contained in the paint for forming the magnetic layer and the drying conditions of the paint for forming the magnetic layer.

[0219] [Average thickness of magnetic recording media] The upper limit of the average thickness (average total thickness) of the magnetic recording medium 1 is preferably 5.6 μm or less, more preferably 5.4 μm or less, more preferably 5.2 μm or less, more preferably 5.0 μm or less, more preferably 4.8 μm or less, more preferably 4.6 μm or less, and even more preferably 4.4 μm or less. When the average thickness of the magnetic recording medium 1 is 5.6 μm or less, the recording capacity that can be recorded in the cartridge 21 can be increased compared to that of a general magnetic recording medium. The lower limit of the average thickness of the magnetic recording medium 1 is not particularly limited, but is, for example, 3.5 μm or more.

[0220] The average thickness of the magnetic recording medium 1 is determined by the procedure explained above for determining the average thickness of the back layer 14.

[0221] (Coercive force Hc) The upper limit of the coercive force Hc of the magnetic recording medium 1 in the longitudinal direction is, for example, 2500 or less, preferably 2000 Oe or less, more preferably 1900 Oe or less, and even more preferably 1800 Oe or less.

[0222] If the lower limit of the coercive force Hc measured in the longitudinal direction of the magnetic recording medium 1 is preferably 1000 Oe or more, demagnetization due to leakage flux from the recording head can be suppressed.

[0223] The coercive force Hc is obtained as follows. First, three magnetic recording media 1 are stacked with double-sided tape, and then punched out with a φ6.39 mm punch to prepare a measurement sample. Then, a vibrating sample magnetometer (VSM) is used to measure the MH loop of the measurement sample (whole magnetic recording medium 1) corresponding to the longitudinal direction of the magnetic recording medium 1 (the running direction of the magnetic recording medium 1). Next, acetone or ethanol is used to wipe off the coating film (non-magnetic layer 12, magnetic layer 13, back layer 14, etc.) and only the substrate 11 is left. Then, three obtained substrates 11 are stacked with double-sided tape, and then punched out with a φ6.39 mm punch to prepare a sample for background correction (hereinafter simply referred to as a correction sample). Then, a VSM is used to measure the MH loop of the correction sample (substrate 11) corresponding to the longitudinal direction of the substrate 11 (the running direction of the magnetic recording medium 1).

[0224] The MH loop of the measurement sample (whole magnetic recording medium 1) and the MH loop of the correction sample (substrate 11) are measured using a high-sensitivity vibration sample magnetometer "VSM-P7-15 type" manufactured by Toei Industry Co., Ltd. The measurement conditions are as follows: measurement mode: full loop, maximum magnetic field: 15 kOe, magnetic field step: 40 bits, time constant of locking amp: 0.3 sec, waiting time: 1 sec, number of MH averages: 20.

[0225] After the two MH loops are obtained, background correction is performed by subtracting the MH loop of the correction sample (substrate 11) from the MH loop of the measurement sample (whole magnetic recording medium 1), and the MH loop after background correction is obtained. The measurement and analysis program attached to the "VSM-P7-15" is used for the calculation of this background correction.

[0226] The coercive force Hc is obtained from the obtained MH loop after background correction. For this calculation, a measurement and analysis program attached to the "VSM-P7-15 type" is used. All of the above MH loop measurements are performed at 25°C. Furthermore, no "demagnetizing field correction" is performed when measuring the MH loop in the longitudinal direction of the magnetic recording medium 1.

[0227] (Orientation degree (square ratio)) The degree of perpendicular orientation is obtained as follows. First, three magnetic recording media 1 are stacked with double-sided tape, and then punched out with a φ6.39 mm punch to prepare a measurement sample. Then, the MH loop of the measurement sample (whole magnetic recording medium 1) corresponding to the perpendicular direction (thickness direction) of the magnetic recording medium 1 is measured using a VSM. Next, the coating film (non-magnetic layer 12, magnetic layer 13, back layer 14, etc.) is wiped off using acetone or ethanol, etc., and only the substrate 11 is left. Then, three obtained substrates 11 are stacked with double-sided tape, and then punched out with a φ6.39 mm punch to prepare a sample for background correction (hereinafter, simply referred to as a correction sample). Then, the MH loop of the correction sample (substrate 11) corresponding to the perpendicular direction of the substrate 11 (perpendicular direction of the magnetic recording medium 1) is measured using a VSM.

[0228] The MH loop of the measurement sample (whole magnetic recording medium 1) and the MH loop of the correction sample (substrate 11) are measured using a high-sensitivity vibration sample magnetometer "VSM-P7-15 type" manufactured by Toei Industry Co., Ltd. The measurement conditions are as follows: measurement mode: full loop, maximum magnetic field: 15 kOe, magnetic field step: 40 bits, time constant of locking amp: 0.3 sec, waiting time: 1 sec, number of MH averages: 20.

[0229] After the two MH loops are obtained, background correction is performed by subtracting the MH loop of the correction sample (substrate 11) from the MH loop of the measurement sample (whole magnetic recording medium 1), and the MH loop after background correction is obtained. The measurement and analysis program attached to the "VSM-P7-15" is used for the calculation of this background correction.

[0230] The saturation magnetization Ms(emu) and residual magnetization Mr(emu) of the MH loop after background correction are substituted into the following formula to calculate the degree of perpendicular orientation (%). Note that all of the above MH loop measurements are performed at 25°C. Also, no "demagnetizing field correction" is performed when measuring the MH loop in the perpendicular direction to the magnetic recording medium 1. Note that a measurement and analysis program provided with the "VSM-P7-15" is used for this calculation. Vertical orientation degree (%)=(Mr / Ms)×100

[0231] The degree of orientation (longitudinal orientation) in the longitudinal direction (running direction) of the magnetic recording medium 1 is preferably 35% or less, more preferably 30% or less, and even more preferably 25% or less. If the degree of longitudinal orientation is 35% or less, the magnetic powder will have a sufficiently high perpendicular orientation, making it possible to obtain a better SNR.

[0232] The degree of longitudinal orientation is determined in the same manner as the degree of perpendicular orientation, except that the MH loop is measured in the longitudinal direction (running direction) of the magnetic recording medium 1 and the substrate 11.

[0233] (Kinematic friction coefficient) The coefficient of dynamic friction μ between the surface of the magnetic layer 13 and the magnetic head when the tension applied to the magnetic recording medium 1 is 1.2 N. A and the coefficient of dynamic friction μ between the surface of the magnetic layer 13 and the magnetic head when the tension applied to the magnetic recording medium 1 is 0.4 N. B Ratio to (μ B / μ A) is preferably 1.0 or more and 2.0 or less, the change in the coefficient of friction due to the fluctuation in tension during running can be reduced, so that the running of the tape can be stabilized.

[0234] The coefficient of dynamic friction μ between the surface of the magnetic layer 13 and the magnetic head when the tension applied to the magnetic recording medium 1 is 0.6 N. A is the ratio between the value μ5 of the 5th run and the value μ1000 of the 1000th run (μ 1000 / μ5) is preferably 1.0 or more and 2.0 or less, more preferably 1.0 or more and 1.5 or less. B / μ A When the coefficient of friction is 1.0 or more and 2.0 or less, the change in coefficient of friction due to multiple runs can be reduced, and the tape running can be stabilized.

[0235] <Method of manufacturing magnetic recording medium> Next, a method for manufacturing the magnetic recording medium 1 will be described. First, a paint for forming a non-magnetic layer is prepared by kneading and dispersing non-magnetic powder, binder, lubricant, etc. in a solvent. Next, a paint for forming a magnetic layer is prepared by kneading and dispersing magnetic powder, binder, lubricant, etc. in a solvent. Next, a paint for forming a back layer is prepared by kneading and dispersing binder, non-magnetic powder, etc. in a solvent. For example, the following solvents, dispersing devices, and kneading devices can be used to prepare the paint for forming a magnetic layer, the paint for forming a non-magnetic layer, and the paint for forming a back layer.

[0236] Examples of the solvent used in preparing the coating material include ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, alcohol-based solvents such as methanol, ethanol, and propanol, ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, propyl acetate, ethyl lactate, and ethylene glycol acetate, ether-based solvents such as diethylene glycol dimethyl ether, 2-ethoxyethanol, tetrahydrofuran, and dioxane, aromatic hydrocarbon-based solvents such as benzene, toluene, and xylene, and halogenated hydrocarbon-based solvents such as methylene chloride, ethylene chloride, carbon tetrachloride, chloroform, and chlorobenzene. These may be used alone or in appropriate mixture.

[0237] Examples of the kneading device used in the preparation of the above-mentioned coating material include, but are not limited to, a continuous twin-screw kneader, a continuous twin-screw kneader capable of diluting in multiple stages, a kneader, a pressure kneader, a roll kneader, etc. Examples of the dispersing device used in the preparation of the above-mentioned coating material include, but are not limited to, a roll mill, a ball mill, a horizontal sand mill, a vertical sand mill, a spike mill, a pin mill, a tower mill, a pearl mill (for example, "DCP Mill" manufactured by Eirich Co., Ltd.), a homogenizer, an ultrasonic dispersing machine, etc.

[0238] Next, a paint for forming a non-magnetic layer is applied to one main surface of the substrate 11 and dried to form a non-magnetic layer 12. Next, a paint for forming a magnetic layer is applied to the non-magnetic layer 12 and dried to form a magnetic layer 13 on the non-magnetic layer 12. During drying, it is preferable to magnetically orient the magnetic powder in the thickness direction of the substrate 11, for example, by a solenoid coil. Also, during drying, the magnetic powder may be magnetically oriented in the running direction (longitudinal direction) of the substrate 11, for example, by a solenoid coil, and then magnetically oriented in the thickness direction of the substrate 11. After the magnetic layer 13 is formed, a paint for forming a back layer is applied to the other main surface of the substrate 11 and dried to form a back layer 14. This results in a magnetic recording medium 1 being obtained.

[0239] The obtained magnetic recording medium 1 is then subjected to a calendaring process to smooth the surface of the magnetic layer 13. Next, the calendared magnetic recording medium 1 is wound into a roll, and in this state, the magnetic recording medium 1 is subjected to a heat treatment to transfer the numerous protrusions 14A on the surface of the back layer 14 to the surface of the magnetic layer 13. As a result, numerous holes 13A are formed in the surface of the magnetic layer 13.

[0240] The heat treatment temperature is preferably 55°C or higher and 75°C or lower. When the heat treatment temperature is 55°C or higher, good transferability can be obtained. On the other hand, when the heat treatment temperature is 75°C or higher, the amount of pores becomes too large, resulting in an excess of lubricant on the surface. Here, the heat treatment temperature is the temperature of the atmosphere in which the magnetic recording medium 1 is held.

[0241] The heat treatment time is preferably 15 hours or more and 40 hours or less. When the heat treatment time is 15 hours or more, good transferability can be obtained. On the other hand, when the heat treatment time is 40 hours or less, a decrease in productivity can be suppressed.

[0242] Finally, the magnetic recording medium 1 is cut to a predetermined width (for example, 1 / 2 inch width). Through the above steps, the desired magnetic recording medium 1 is obtained.

[0243] [Preparation process of paint for forming magnetic layer] Next, the preparation process of the coating material for forming the magnetic layer will be described. First, the first composition having the following composition was kneaded with an extruder. Next, the kneaded first composition and the second composition having the following composition were added to a stirring tank equipped with a disperser and premixed. Next, further sand mill mixing was performed and filtering was performed to prepare the coating material for forming the magnetic layer.

[0244] (First composition) Barium ferrite (BaFe 12 O 19 ) Particle powder (hexagonal plate shape, aspect ratio 2.8, particle volume 1950nm 3 ):100 parts by mass Vinyl chloride resin (cyclohexanone solution 30% by mass): 51.3 parts by mass (including solution) (Degree of polymerization: 300, Mn=10,000, contains polar groups OSO3K=0.07mmol / g and secondary OH=0.3mmol / g.) Aluminum oxide powder: 5 parts by weight (α-Al2O3, average particle size 0.2μm) Carbon black: 2 parts by weight (Manufactured by Tokai Carbon Co., Ltd., product name: Seast TA)

[0245] (Second composition) Vinyl chloride resin: 1.1 parts by mass (Resin solution: resin 30% by mass, cyclohexanone 70% by mass) n-Butyl stearate: 2 parts by weight Methyl ethyl ketone: 121.3 parts by mass Toluene: 121.3 parts by mass Cyclohexanone: 60.7 parts by mass

[0246] Finally, 4 parts by mass of polyisocyanate (product name: Coronate L, manufactured by Nippon Polyurethane Industries, Ltd.) and 2 parts by mass of myristic acid were added as a curing agent to the magnetic layer-forming coating material prepared as described above.

[0247] [Preparation process of paint for forming non-magnetic layer] Next, the preparation process of the paint for forming the nonmagnetic layer will be described. First, the third composition having the following composition was kneaded with an extruder. Next, the kneaded third composition and the fourth composition having the following composition were added to a stirring tank equipped with a disperser and premixed. Next, further sand mill mixing was performed and filtering was performed to prepare the paint for forming the nonmagnetic layer.

[0248] (Third composition) Acicular iron oxide powder: 100 parts by weight (α-Fe2O3, average major axis length 0.15μm) Vinyl chloride resin: 55.6 parts by mass (Resin solution: resin 30% by mass, cyclohexanone 70% by mass) Carbon black: 10 parts by weight (Average particle size 20nm)

[0249] (4th composition) Polyurethane resin UR8200 (manufactured by Toyobo): 18.5 parts by weight n-Butyl stearate: 2 parts by weight Methyl ethyl ketone: 108.2 parts by mass Toluene: 108.2 parts by mass Cyclohexanone: 18.5 parts by mass

[0250] Finally, 4 parts by mass of polyisocyanate (product name: Coronate L, manufactured by Nippon Polyurethane Industries, Ltd.) and 2 parts by mass of myristic acid were added as a curing agent to the coating material for forming the nonmagnetic layer prepared as described above.

[0251] [Preparation process of paint for forming back layer] Next, the process for preparing the paint for forming the back layer will be described. The following raw materials were mixed in a stirring tank equipped with a disperser, and the mixture was filtered to prepare the paint for forming the back layer. Carbon black particle powder (average particle size 20 nm): 90 parts by mass Carbon black particle powder (average particle size 270 nm): 10 parts by mass Polyester polyurethane: 100 parts by weight (Manufactured by Nippon Polyurethane Co., Ltd., product name: N-2304) Methyl ethyl ketone: 500 parts by weight Toluene: 400 parts by mass Cyclohexanone: 100 parts by mass

[0252] The type and amount of inorganic particles may be changed as follows. Carbon black particle powder (average particle size 20 nm): 80 parts by mass Carbon black particle powder (average particle size 270 nm): 20 parts by mass

[0253] The type and amount of inorganic particles may be changed as follows. Carbon black particle powder (average particle size 20 nm): 100 parts by mass

[0254] [Coating process] Using the magnetic layer-forming paint and non-magnetic layer-forming paint prepared as described above, a non-magnetic layer with an average thickness of 1.0 to 1.1 μm and a magnetic layer with an average thickness of 40 to 100 nm were formed on one main surface of a long polyethylene naphthalate film (hereinafter referred to as "PEN film") (for example, average thickness 4.0 μm) serving as a non-magnetic support, as follows. First, the non-magnetic layer-forming paint was applied to one main surface of the PEN film and dried to form a non-magnetic layer. Next, the magnetic layer was formed by applying the magnetic layer-forming paint on the non-magnetic layer and drying it. Note that, when the magnetic layer-forming paint was dried, the magnetic powder was magnetically oriented in the thickness direction of the film by a solenoid coil. The degree of orientation in the thickness direction (vertical direction) and the degree of orientation in the longitudinal direction of the magnetic recording medium were set to a predetermined value by adjusting the strength of the magnetic field from the solenoid coil (2 to 3 times the holding power of the magnetic powder), adjusting the solid content of the paint for forming the magnetic layer, and adjusting the drying conditions (drying temperature and drying time) of the paint for forming the magnetic layer to adjust the conditions for orienting the magnetic powder in the magnetic field. Next, the paint for forming the back layer was applied to the other main surface of the PEN film and dried to form a non-magnetic layer. This resulted in the magnetic recording medium. In order to increase the degree of orientation, it is necessary to improve the dispersion state of the paint for forming the magnetic layer. Furthermore, in order to increase the degree of vertical orientation, it is also effective to magnetize the magnetic powder in advance before the magnetic recording medium enters the orientation device.

[0255] [Calendar process, transfer process] Then, a calendar treatment was performed to smooth the surface of the magnetic layer. Next, the obtained magnetic recording medium was wound into a roll, and in this state, the magnetic recording medium was subjected to a heat treatment at 60°C for 10 hours twice. As a result, many protrusions on the surface of the back layer were transferred to the surface of the magnetic layer, and many holes were formed on the surface of the magnetic layer.

[0256] [Cutting process] The magnetic recording medium obtained as described above was cut into a width of 1 / 2 inch (12.65 mm), thereby obtaining the desired long magnetic recording medium.

[0257] <Cartridge details> Next, the cartridge 21 will be described in detail.

[0258] [Cartridge configuration example 1] 20 is an exploded perspective view showing an example of the configuration of the cartridge 21. The cartridge 21 includes a reel 313 around which a tape-like magnetic recording medium (hereinafter referred to as "magnetic tape") MT is wound, a reel lock 314 and a reel spring 315 for locking the rotation of the reel 313, a spider 316 for unlocking the locked state of the reel 313, a slide door 317 for opening and closing a tape outlet 312C provided in the cartridge case 312 across the lower shell 312A and the upper shell 312B, a door spring 318 for biasing the slide door 317 to a closed position of the tape outlet 312C, a write protector 319 for preventing erroneous erasure, and a cartridge memory 311, all of which are arranged inside a cartridge case 312 consisting of a lower shell 312A and an upper shell 312B. The reel 313 is substantially disk-shaped with an opening in the center, and is composed of a reel hub 313A and a flange 313B made of a hard material such as plastic. One end of the magnetic tape MT is provided with a leader pin 320. The magnetic tape MT corresponds to the magnetic recording medium 1 according to the embodiment described above.

[0259] The cartridge 21 may be a magnetic tape cartridge that complies with the LTO (Linear Tape-Open) standard, or may be a magnetic tape cartridge that complies with a standard other than the LTO standard.

[0260] The cartridge memory 311 is provided near one corner of the cartridge 21. When the cartridge 21 is loaded into the data recording device 20 (FIG. 5), the cartridge memory 311 faces a reader / writer of the data recording device 20. The cartridge memory 311 communicates with the data recording device 20, specifically, with its reader / writer, using a wireless communication standard that complies with the LTO standard.

[0261] 21 is a block diagram showing an example of the configuration of the cartridge memory 311. The cartridge memory 311 includes an antenna coil (communication unit) 431 that communicates with a reader / writer using a specified communication standard, a rectification / power circuit 432 that generates power from radio waves received by the antenna coil 431 using induced electromotive force and rectifies the power to generate power, a clock circuit 433 that generates a clock from the radio waves received by the antenna coil 431 using induced electromotive force, a detection / modulation circuit 434 that detects the radio waves received by the antenna coil 431 and modulates the signal to be transmitted by the antenna coil 431, a controller (control unit) 435 consisting of a logic circuit or the like for determining commands and data from the digital signal extracted from the detection / modulation circuit 434 and processing the same, and a memory (storage unit) 436 that stores information. The cartridge memory 311 also includes a capacitor 437 connected in parallel to the antenna coil 431, and the antenna coil 431 and the capacitor 437 form a resonant circuit.

[0262] The memory 436 stores information related to the cartridge 21. The memory 436 is a non-volatile memory (NVM). The memory capacity of the memory 436 is preferably about 32 KB or more.

[0263] The memory 436 has a first memory area 436A and a second memory area 436B. The first memory area 436A corresponds to the memory area of ​​a cartridge memory (hereinafter referred to as a "conventional cartridge memory") of the LTO standard before LTO8, for example, and is an area for storing information conforming to the LTO standard before LTO8. The information conforming to the LTO standard before LTO8 is, for example, manufacturing information (for example, a unique number of the cartridge 21, etc.), usage history (for example, the number of times the tape has been pulled out (Thread Count), etc.), etc.

[0264] The second memory area 436B corresponds to an extended memory area for the memory area of ​​a conventional cartridge memory. The second memory area 436B is an area for storing additional information. Here, the additional information means, for example, information related to the cartridge 21 that is not specified in the LTO standard before LTO8. Examples of the additional information include tension adjustment information, management ledger data, index information, or thumbnail information of a video stored on the magnetic tape MT, but are not limited to these data. The tension adjustment information is information for adjusting the tension applied in the longitudinal direction of the magnetic tape MT. The tension adjustment information includes the distance between adjacent servo bands (the distance between servo patterns recorded on adjacent servo bands) when data is recorded on the magnetic tape MT. The distance between adjacent servo bands is an example of width-related information related to the width of the magnetic tape MT. In the following description, the information stored in the first memory area 436A may be referred to as "first information," and the information stored in the second memory area 436B may be referred to as "second information."

[0265] The memory 436 may have a plurality of banks. In this case, some of the plurality of banks may constitute a first storage area 436A, and the remaining banks may constitute a second storage area 436B.

[0266] The antenna coil 431 induces an induced voltage by electromagnetic induction. The controller 435 communicates with the data recording device 20 in accordance with a prescribed communication standard via the antenna coil 431. Specifically, for example, mutual authentication, sending and receiving commands, or data exchange is performed.

[0267] The controller 435 stores information received from the data recording device 20 via the antenna coil 431 in the memory 436. For example, the controller 435 stores tension adjustment information received from the data recording device 20 via the antenna coil 431 in the second storage area 436B of the memory 436. In response to a request from the data recording device 20, the controller 435 reads information from the memory 436 and transmits the information to the data recording device 20 via the antenna coil 431. For example, in response to a request from the data recording device 20, the controller 435 reads tension adjustment information from the second storage area 436B of the memory 436 and transmits the information to the data recording device 20 via the antenna coil 431.

[0268] [Cartridge configuration example 2] 22 is an exploded perspective view showing an example of the configuration of a two-reel type cartridge 521. The cartridge 521 includes an upper half 502 made of synthetic resin, a transparent window member 523 fitted and fixed to a window portion 502a opened in the upper surface of the upper half 502, a reel holder 522 fixed to the inside of the upper half 502 to prevent the reels 506 and 507 from floating up, a lower half 505 corresponding to the upper half 502, the reels 506 and 507 stored in a space formed by combining the upper half 502 and the lower half 505, a magnetic tape MT1 wound around the reels 506 and 507, a front lid 509 that closes a front opening formed by combining the upper half 502 and the lower half 505, and a back lid 509A that protects the magnetic tape MT1 exposed at the front opening.

[0269] The reel 506 includes a lower flange 506b having a cylindrical hub portion 506a around which the magnetic tape MT1 is wound in the center, an upper flange 506c having approximately the same size as the lower flange 506b, and a reel plate 511 sandwiched between the hub portion 506a and the upper flange 506c. The reel 507 has a similar configuration to the reel 506.

[0270] The window member 523 has mounting holes 523a for mounting reel holders 522, which are reel holding means for preventing the reels from floating up, at positions corresponding to the reels 506 and 507. The magnetic tape MT1 has the same structure as the magnetic recording medium 1 of the above-described embodiment.

[0271] The present technology can also be configured as follows. (1) A tape-shaped magnetic recording medium having a magnetic layer having a servo band on which a servo signal is recorded, Let Sq be the squareness ratio in the perpendicular direction of the magnetic layer, F0(pp) be the peak-to-peak value of the first magnetic force gradient intensity observed by a magnetic force microscope when a servo signal is saturation recorded on the magnetic layer, and Fact.(pp) be the peak-to-peak value of the second magnetic force gradient intensity observed by a magnetic force microscope for the servo signal recorded on the servo band, Sq×Fact.(pp) / F0(pp) The index represented by is 0.42 or higher. Magnetic recording media. (2) The magnetic recording medium according to (1), The index is 0.45 or more. Magnetic recording media. (3) The magnetic recording medium according to (1), The squareness (Sq) of the magnetic layer in the perpendicular direction is 0.5 or more. Magnetic recording media. (4) The magnetic recording medium according to (3), The squareness (Sq) of the magnetic layer in the perpendicular direction is 0.6 or more. Magnetic recording media. (5) The magnetic recording medium according to (1), The ratio of Fact.(pp) to F0(pp) (Fact.(pp) / F0(pp)) is 0.6 or more. Magnetic recording media. (6) The magnetic recording medium according to (5) above, The ratio of Fact.(pp) to F0(pp) (Fact.(pp) / F0(pp)) is 0.7 or more. Magnetic recording media. (7) The magnetic recording medium according to (1), The residual magnetization (Mrt) of the magnetic layer is 0.39 or more. Magnetic recording media. (8) The magnetic recording medium according to (7), The residual magnetization (Mrt) of the magnetic layer is 0.45 or more. Magnetic recording media. (9) The magnetic recording medium according to any one of (1) to (8), The servo signal is a servo signal recording pattern including a plurality of stripes inclined at a predetermined azimuth angle with respect to the tape width direction. Magnetic recording media. (10) The magnetic recording medium according to any one of (1) to (9), The magnetic layer contains one of the following magnetic powders: hexagonal ferrite, ε iron oxide, or cobalt ferrite. Magnetic recording media. (11) The magnetic recording medium according to any one of (1) to (10) above, The magnetic recording medium further includes a substrate supporting the magnetic layer, and a non-magnetic layer provided between one main surface of the substrate and the magnetic layer. Magnetic recording media. (12) The magnetic recording medium according to any one of (1) to (11) above, Further comprising a back layer provided on the other main surface of the substrate. Magnetic recording media. (13) The magnetic recording medium according to any one of (1) to (12) above, The average thickness of the magnetic recording medium is 5.6 μm or less. Magnetic recording media. (14) The magnetic recording medium according to any one of (1) to (13) above, The average thickness of the magnetic recording medium is 5.4 μm or less. Magnetic recording media. (15) The magnetic recording medium according to any one of (1) to (14) above, The average thickness of the magnetic recording medium is 5.2 μm or less. Magnetic recording media. (16) The magnetic recording medium according to any one of (1) to (15) above, The average thickness of the magnetic recording medium is 5.0 μm or less. Magnetic recording media. (17) The magnetic recording medium according to any one of (1) to (16) above, The average thickness of the nonmagnetic layer is 0.6 μm or more and 2.0 μm or less. Magnetic recording media. (18) An apparatus for recording a servo signal on a tape-shaped magnetic recording medium having a magnetic layer with a servo band, comprising: a servo write head for recording a servo signal on the servo band; an auxiliary pole made of a soft magnetic material and disposed opposite the servo write head with the magnetic layer therebetween; A servo signal recording device comprising: (19) A tape-shaped magnetic recording medium having a magnetic layer with a servo band on which a servo signal is recorded, Let Sq be the squareness ratio in the perpendicular direction of the magnetic layer, F0(pp) be the peak-to-peak value of the first magnetic force gradient intensity observed by a magnetic force microscope when a servo signal is saturation recorded on the magnetic layer, and Fact.(pp) be the peak-to-peak value of the second magnetic force gradient intensity observed by a magnetic force microscope for the servo signal recorded on the servo band, Sq×Fact.(pp) / F0(pp) The index represented by is 0.42 or higher. cartridge. [Explanation of symbols]

[0272] 1...Magnetic recording medium 5…Recording track 6...Servo signal recording pattern 7…Stripes 11...Base material 12...Nonmagnetic layer 13...Magnetic layer 14…Back layer 200...Servo signal recording device 210...Servo light head 220…Auxiliary magnetic pole d...Data band s...Servo band

Claims

1. A tape-shaped magnetic recording medium comprising a substrate, a non-magnetic layer provided on one main surface of the substrate, and a magnetic layer including magnetic powder provided on the non-magnetic layer, the magnetic layer has a servo band in which a servo signal is recorded; Let Sq be the squareness ratio in the perpendicular direction of the magnetic layer, F0(pp) be the peak-to-peak value of the first magnetic force gradient intensity observed by a magnetic force microscope when a servo signal is saturation recorded on the magnetic layer, and Fact.(pp) be the peak-to-peak value of the second magnetic force gradient intensity observed by a magnetic force microscope for the servo signal recorded on the servo band, Sq×Fact.(p-p) / F0(p-p) The index represented by is 0.42 or more. Magnetic recording media.

2. The magnetic recording medium according to claim 1, The magnetic powder includes a powder of ε iron oxide particles or a powder of hexagonal ferrite. Magnetic recording media.

3. The magnetic recording medium according to claim 2, The hexagonal ferrite contains at least one of Ba, Sr, Pb, and Ca. Magnetic recording media.

4. The magnetic recording medium according to claim 2, The hexagonal ferrite is strontium ferrite. Magnetic recording media.

5. A magnetic recording medium according to any one of claims 1 to 4, The thickness of the substrate is 3.4 μm or more and 4.2 μm or less. Magnetic recording media.

6. A magnetic recording medium according to any one of claims 1 to 4, The substrate includes at least one of PET (polyethylene terephthalate), PEN (polyethylene naphthalate), PBT (polybutylene terephthalate), PBN (polybutylene naphthalate), PCT (polycyclohexylene dimethylene terephthalate), PEB (polyethylene-p-oxybenzoate), and polyethylene bisphenoxycarboxylate. Magnetic recording media.

7. The magnetic recording medium according to claim 1, The substrate includes at least one of PA (polyamide, nylon), aromatic PA (aromatic polyamide, aramid), PI (polyimide), aromatic PI (aromatic polyimide), PAI (polyamideimide), aromatic PAI (aromatic polyamideimide), PBO (polybenzoxazole), polyether, PEK (polyetherketone), PEEK (polyetheretherketone), polyetherester, PES (polyethersulfone), PEI (polyetherimide), PSF (polysulfone), PPS (polyphenylene sulfide), PC (polycarbonate), PAR (polyarylate), and PU (polyurethane). Magnetic recording media.

8. The magnetic recording medium according to claim 3 or 4, The average aspect ratio of the magnetic powder is 1 or more and 2.5 or less. Magnetic recording media.

9. The magnetic recording medium according to claim 3 or 4, The average aspect ratio of the magnetic powder is 1 or more and 2.1 or less. Magnetic recording media.

10. The magnetic recording medium according to claim 1, The average thickness of the magnetic recording medium is 5.4 μm or less. Magnetic recording media.

11. The magnetic recording medium according to claim 1, The average thickness of the magnetic recording medium is 5.2 μm or less. Magnetic recording media.

12. The magnetic recording medium according to claim 1, The average thickness of the magnetic recording medium is 5.0 μm or less. Magnetic recording media.

13. The magnetic recording medium according to claim 1, The average thickness of the magnetic recording medium is 4.8 μm or less. Magnetic recording media.

14. The magnetic recording medium according to any one of claims 1 to 13, The index is 0.45 or more. Magnetic recording media.

15. The magnetic recording medium according to any one of claims 1 to 13, The squareness (Sq) of the magnetic layer in the perpendicular direction is 0.5 or more. Magnetic recording media.

16. The magnetic recording medium according to any one of claims 1 to 13, The squareness (Sq) of the magnetic layer in the perpendicular direction is 0.6 or more. Magnetic recording media.

17. The magnetic recording medium according to any one of claims 1 to 13, The ratio of Fact.(pp) to F0(pp) (Fact.(pp) / F0(pp)) is 0.6 or more. Magnetic recording media.

18. The magnetic recording medium according to any one of claims 1 to 13, The ratio of Fact.(pp) to F0(pp) (Fact.(pp) / F0(pp)) is 0.7 or more. Magnetic recording media.

19. The magnetic recording medium according to any one of claims 1 to 13, The residual magnetization (Mrt) of the magnetic layer is 0.39 or more. Magnetic recording media.

20. The magnetic recording medium according to any one of claims 1 to 13, The residual magnetization (Mrt) of the magnetic layer is 0.45 or more. Magnetic recording media.

Citation Information

Patent Citations

  • Magnetic recording medium

    JP2009037700A

  • Magnetic recording medium, servo signal recording apparatus and method of producing magnetic recording medium

    JP2014199706A

  • Magnetic tape and magnetic tape device

    JP2017224365A

  • Magnetic record medium, servo signal storage unit and manufacturing method of magnetic record medium

    JP2018005970A

  • Servo writing of magnetic recording medium having vertical anisotropy

    JP2018073454A