Electrophotographic photoreceptor, process cartridge and electrophotographic device

The electrophotographic photoreceptor's protective layer, with niobium-enriched titanium oxide coating and controlled oxygen vacancies, addresses charging ability deterioration, ensuring consistent performance over multiple uses.

JP7587669B2Active Publication Date: 2024-11-20CANON KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023219861
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-12-26
Publication Date
2024-11-20
Estimated Expiration
2040-04-13

AI Technical Summary

Technical Problem

Existing electrophotographic photoreceptors face challenges in maintaining charging ability during repeated use, particularly due to the deterioration of electrical characteristics caused by the presence of niobium and oxygen vacancies in titanium oxide particles.

Method used

The photoreceptor incorporates a protective layer with metal oxide particles containing titanium oxide, where niobium is preferentially present in the coating layer, and the oxygen vacancy rates in the core material and coating layer follow specific ratios to enhance conductivity and prevent charge retention.

Benefits of technology

This configuration maintains good charging ability over repeated use by facilitating easier connection of conductive paths and reducing charge traps, thereby improving the photoreceptor's durability and image quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587669000010
    Figure 0007587669000010
  • Figure 0007587669000001
    Figure 0007587669000001
  • Figure 0007587669000002
    Figure 0007587669000002
Patent Text Reader

Abstract

To provide an electrophotographic photoreceptor that can maintain its electrification capability during repeated use.SOLUTION: An electrophotographic photoreceptor has a support, a conductive layer, a photosensitive layer, and a protective layer in this order. The protective layer contains a binder resin and metal oxide particles. The metal oxide particle has a core material and a coating layer. The core material and the coating layer individually contain titanium oxide. The coating layer further contains niobium.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrophotographic photoreceptor, and a process cartridge and an electrophotographic apparatus each having the electrophotographic photoreceptor. [Background technology]

[0002] It is known that in electrophotographic photoreceptors used in electrophotographic devices, a protective layer is provided to improve mechanical durability (abrasion resistance) in order to extend the life of the electrophotographic photoreceptor and to improve image quality during repeated use.

[0003] In order to improve the electrical characteristics of an electrophotographic photoreceptor using such a protective layer, it is known to add titanium oxide to the protective layer (Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2009-229495 A Summary of the Invention [Problem to be solved by the invention]

[0005] According to the studies of the present inventors, it has been found that the electrophotographic photoreceptor described in Patent Document 1 has room for improvement in terms of maintaining the charging ability during repeated use.

[0006] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide an electrophotographic photoreceptor capable of maintaining its charging ability even when used repeatedly. [Means for solving the problem]

[0007] The above object can be achieved by the present invention described below. That is, the first aspect of the present invention is An electrophotographic photoreceptor having a support, a conductive layer, a photosensitive layer, and a protective layer in this order, the protective layer contains a binder resin and metal oxide particles, the metal oxide particles have a core material containing titanium oxide and a coating layer containing titanium oxide coating the core material, the coating layer further contains niobium, An electrophotographic photoreceptor, wherein the content ratio of niobium in the coating layer relative to the total mass of the core material is higher than the content ratio of niobium in the coating layer relative to the total mass of the core material.

[0008] Moreover, the second aspect of the present invention is An electrophotographic photoreceptor having a support, a conductive layer, a photosensitive layer, and a protective layer in this order, the protective layer contains a binder resin and metal oxide particles, the metal oxide particles have a core material containing titanium oxide and a coating layer containing titanium oxide coating the core material, an electrophotographic photoreceptor characterized in that, when the oxygen deficiency rate of the metal oxide particles is A (%), the oxygen deficiency rate of the core material is B (%), and the oxygen deficiency rate of the coating layer is C (%), the following formulas (1) and (2) are satisfied: A≦2.0 (1) 10×B <C (2) Effect of the Invention

[0009] According to the first or second aspect of the present invention, it is possible to provide an electrophotographic photoreceptor having good charging ability. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic diagram of an electrophotographic apparatus including a process cartridge having an electrophotographic photosensitive member. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below with reference to preferred embodiments. The inventors have conducted research and found that there is room for improvement in maintaining the charging ability of photoreceptors having metal oxide particles containing titanium oxide, which are used in conventional technology, in their protective layers.

[0012] As a result of investigations conducted in order to solve the technical problems occurring in the above-mentioned conventional techniques, it was found that the technical problems can be solved by including niobium in the coating layer of metal oxide particles containing titanium oxide in the core material and coating layer, as shown in the first aspect of the present invention.

[0013] Furthermore, as shown in the second aspect of the present invention, it has been found that when the oxygen deficiency rate has a specific relationship in a metal oxide containing titanium oxide in a core material and a coating layer, the technical problems occurring in the conventional technology can be solved. The reason for this is not clearly understood, but the present inventors believe it to be as follows.

[0014] As in the first embodiment, metal oxide particles containing titanium oxide generally have improved electrical conductivity when they contain niobium, which is an element with a different valence, but the sites where niobium is present are sites with strong polarity, and therefore, if a large amount of niobium is present, it may act as a trap and deteriorate electrical properties such as residual electricity. However, when the protective layer has metal oxide particles in which niobium is preferentially present (the ratio of niobium is higher in the coating layer than in the core material) in the coating layer of the titanium oxide-containing metal oxide particles, the conductive paths in the protective layer are easily connected, and as a result, electric charges are less likely to remain in the protective layer, which prevents a decrease in charging ability.

[0015] Furthermore, as in the second aspect, metal oxide particles containing titanium oxide generally have improved conductivity when they have oxygen vacancies in their crystal structure. However, since the sites having oxygen vacancies are sites with strong polarity, if many of them are present, they act as traps, deteriorating electrical properties such as residual charge. However, when the protective layer contains metal oxide particles containing titanium oxide, and metal oxide particles having a specific relationship between the oxygen deficiency rate of the core material and the coating layer thereof, the conductive paths in the protective layer are connected, making it difficult for charges to remain in the protective layer, and thus preventing a decrease in charging ability.

[0016] Furthermore, it is believed that the inclusion of titanium oxide in both the core material and coating layer of the metal oxide particles of the present invention is necessary from the standpoint of the stability and uniformity of the conductive path performance in which each particle acts.

[0017] As explained above, the respective components interact organically in the protective layer containing the binder resin, thereby making it possible to achieve the effects of the present invention.

[0018] [Electrophotographic photoreceptor] The electrophotographic photoreceptor of the present invention is characterized by having a support, a conductive layer, a photosensitive layer, and a protective layer.

[0019] The method for producing the electrophotographic photoreceptor of the present invention includes a method of preparing the coating liquid for each layer described later, coating the layers in the desired order, and drying the liquid. In this case, the coating liquid can be applied by dip coating, spray coating, inkjet coating, roll coating, die coating, blade coating, curtain coating, wire bar coating, ring coating, etc. Among these, dip coating is preferred from the viewpoint of efficiency and productivity. Each layer will be described below.

[0020] <Support> In the present invention, the electrophotographic photoreceptor has a support. In the present invention, the support is preferably a conductive support having electrical conductivity. The shape of the support may be a cylinder, a belt, a sheet, or the like. Among them, a cylindrical support is preferable. The surface of the support may be subjected to electrochemical treatment such as anodization, blasting, cutting, or the like. The support is preferably made of a metal, a resin, or a glass. Examples of the metal include aluminum, iron, nickel, copper, gold, stainless steel, and alloys thereof. Among them, an aluminum support using aluminum is preferable. Furthermore, the resin or glass may be made conductive by a process such as mixing with or coating with a conductive material.

[0021] <Conductive layer> In the present invention, a conductive layer is provided on the support. By providing the conductive layer, scratches and irregularities on the support surface can be concealed and light reflection on the support surface can be controlled. The conductive layer preferably contains conductive particles and a resin.

[0022] The conductive particles may be made of a material such as metal oxide, metal, or carbon black. Examples of metal oxides include zinc oxide, aluminum oxide, indium oxide, silicon oxide, zirconium oxide, tin oxide, titanium oxide, magnesium oxide, antimony oxide, bismuth oxide, etc. Examples of metals include aluminum, nickel, iron, nichrome, copper, zinc, silver, etc. Among these, it is preferable to use metal oxides as the conductive particles, and it is particularly preferable to use titanium oxide, tin oxide, or zinc oxide. When a metal oxide is used as the conductive particles, the surface of the metal oxide may be treated with a silane coupling agent or the like, or the metal oxide may be doped with an element such as phosphorus or aluminum or an oxide thereof. The conductive particles may have a laminated structure having a core particle and a coating layer that covers the core particle. Examples of the core particle include titanium oxide, barium sulfate, zinc oxide, etc. Examples of the coating layer include metal oxides such as tin oxide. Furthermore, when a metal oxide is used as the conductive particles, the volume average particle size is preferably 1 nm or more and 500 nm or less, and more preferably 3 nm or more and 400 nm or less.

[0023] Examples of the resin include polyester resin, polycarbonate resin, polyvinyl acetal resin, acrylic resin, silicone resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, and alkyd resin. The conductive layer may further contain silicone oil, resin particles, a masking agent such as titanium oxide, and the like.

[0024] The average thickness of the conductive layer is preferably from 1 μm to 50 μm, and particularly preferably from 3 μm to 40 μm.

[0025] The conductive layer can be formed by preparing a coating solution for the conductive layer containing the above-mentioned materials and solvent, forming a coating film of this, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, sulfoxide-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. Examples of the dispersion method for dispersing the conductive particles in the coating solution for the conductive layer include a method using a paint shaker, a sand mill, a ball mill, and a liquid collision type high-speed disperser.

[0026] <Undercoat layer> In the present invention, an undercoat layer may be provided on the conductive layer. By providing the undercoat layer, the adhesion between the layers is improved and a charge injection blocking function can be imparted.

[0027] The undercoat layer preferably contains a resin. Alternatively, the undercoat layer may be formed as a cured film by polymerizing a composition containing a monomer having a polymerizable functional group.

[0028] Examples of the resin include polyester resin, polycarbonate resin, polyvinyl acetal resin, acrylic resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, polyvinyl phenol resin, alkyd resin, polyvinyl alcohol resin, polyethylene oxide resin, polypropylene oxide resin, polyamide resin, polyamic acid resin, polyimide resin, polyamideimide resin, and cellulose resin.

[0029] Examples of the polymerizable functional group contained in the monomer having a polymerizable functional group include an isocyanate group, a blocked isocyanate group, a methylol group, an alkylated methylol group, an epoxy group, a metal alkoxide group, a hydroxyl group, an amino group, a carboxyl group, a thiol group, a carboxylic anhydride group, and a carbon-carbon double bond group.

[0030] For the purpose of improving electrical properties, the undercoat layer may further contain an electron transporting material, a metal oxide, a metal, a conductive polymer, etc. Among these, it is preferable to use an electron transporting material or a metal oxide. Examples of the electron transport substance include a quinone compound, an imide compound, a benzimidazole compound, a cyclopentadienylidene compound, a fluorenone compound, a xanthone compound, a benzophenone compound, a cyanovinyl compound, an aryl halide compound, a silole compound, a boron-containing compound, etc. An electron transport substance having a polymerizable functional group may be used as the electron transport substance, and the undercoat layer may be formed as a cured film by copolymerizing the electron transport substance with the monomer having the polymerizable functional group described above. Examples of metal oxides include indium tin oxide, tin oxide, indium oxide, titanium oxide, zinc oxide, aluminum oxide, silicon dioxide, etc. Examples of metals include gold, silver, aluminum, etc. The undercoat layer may further contain an additive.

[0031] The average thickness of the undercoat layer is preferably from 0.1 μm to 50 μm, more preferably from 0.2 μm to 40 μm, and particularly preferably from 0.3 μm to 30 μm.

[0032] The undercoat layer can be formed by preparing a coating solution for the undercoat layer containing the above-mentioned materials and solvent, forming a coating film from the coating solution, and drying and / or curing the coating solution. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents.

[0033] <Photosensitive layer> The photosensitive layer of an electrophotographic photoreceptor is mainly classified into (1) a multi-layer type photosensitive layer and (2) a single-layer type photosensitive layer. (1) The multi-layer type photosensitive layer has a charge generation layer containing a charge generation material and a charge transport layer containing a charge transport material. (2) The single-layer type photosensitive layer has a photosensitive layer containing both a charge generation material and a charge transport material.

[0034] (1) Laminated photosensitive layer The laminated type photosensitive layer has a charge generating layer and a charge transport layer.

[0035] (1-1) Charge generation layer The charge generating layer preferably contains a charge generating material and a resin.

[0036] Examples of the charge generating material include azo pigments, perylene pigments, polycyclic quinone pigments, indigo pigments, and phthalocyanine pigments. Among these, azo pigments and phthalocyanine pigments are preferred. Among phthalocyanine pigments, oxytitanium phthalocyanine pigments, chlorogallium phthalocyanine pigments, and hydroxygallium phthalocyanine pigments are preferred.

[0037] The content of the charge generating material in the charge generating layer is preferably from 40% by mass to 85% by mass, and more preferably from 60% by mass to 80% by mass, based on the total mass of the charge generating layer.

[0038] Examples of the resin include polyester resin, polycarbonate resin, polyvinyl acetal resin, polyvinyl butyral resin, acrylic resin, silicone resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, polyvinyl alcohol resin, cellulose resin, polystyrene resin, polyvinyl acetate resin, polyvinyl chloride resin, etc. Among these, polyvinyl butyral resin is more preferable.

[0039] The charge generating layer may further contain additives such as an antioxidant and an ultraviolet absorbing agent, etc. Specific examples of such additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, and benzophenone compounds.

[0040] The average thickness of the charge generating layer is preferably from 0.1 μm to 1 μm, and more preferably from 0.15 μm to 0.4 μm.

[0041] The charge generating layer can be formed by preparing a coating solution for the charge generating layer containing the above-mentioned materials and solvent, forming a coating film of this, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, sulfoxide-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents.

[0042] (1-2) Charge transport layer The charge transport layer preferably contains a charge transport material and a resin.

[0043] Examples of the charge transport material include polycyclic aromatic compounds, heterocyclic compounds, hydrazone compounds, styryl compounds, enamine compounds, benzidine compounds, triarylamine compounds, and resins having groups derived from these materials. Among these, triarylamine compounds and benzidine compounds are preferred. The content of the charge transport material in the charge transport layer is preferably from 25% by weight to 70% by weight, and more preferably from 30% by weight to 55% by weight, based on the total weight of the charge transport layer.

[0044] Examples of the resin include polyester resin, polycarbonate resin, acrylic resin, polystyrene resin, etc. Among these, polycarbonate resin and polyester resin are preferable. As the polyester resin, polyarylate resin is particularly preferable. The content ratio (mass ratio) of the charge transport material to the resin is preferably from 4:10 to 20:10, and more preferably from 5:10 to 12:10.

[0045] The charge transport layer may also contain additives such as antioxidants, ultraviolet absorbers, plasticizers, leveling agents, slipping agents, and abrasion resistance improvers. Specific examples of such additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, benzophenone compounds, siloxane-modified resins, silicone oils, fluororesin particles, polystyrene resin particles, polyethylene resin particles, silica particles, alumina particles, and boron nitride particles.

[0046] The average thickness of the charge transport layer is preferably from 5 μm to 50 μm, more preferably from 8 μm to 40 μm, and particularly preferably from 10 μm to 30 μm.

[0047] The charge transport layer can be formed by preparing a coating solution for the charge transport layer containing the above-mentioned materials and solvent, forming a coating film of this, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. Among these solvents, ether-based solvents or aromatic hydrocarbon-based solvents are preferred.

[0048] (2) Single-layer photosensitive layer The single-layer type photosensitive layer can be formed by preparing a coating solution for the photosensitive layer containing a charge generating material, a charge transporting material, a resin and a solvent, forming a coating film of this, and drying it. The charge generating material, the charge transporting material and the resin are the same as the examples of materials in "(1) Multi-layer type photosensitive layer" above.

[0049] <Protective layer> In the present invention, a protective layer is provided on the photosensitive layer. The protective layer has a binder resin and the metal oxide particles according to the first or second aspect of the present invention. More preferably, it is the second aspect, in which the coating layer of the metal oxide particles further contains niobium.

[0050] In the first embodiment of the present invention, the coating layer must contain niobium. The core material of the metal oxide particles does not need to contain niobium, and if niobium is evenly present throughout the metal oxide particles, it acts as a charge trap and reduces the charging ability. Therefore, the niobium content ratio to the total mass of the coating layer must be higher than the niobium content ratio to the total mass of the core material. In this case, the niobium content ratio to the total mass of the coating layer is preferably 10 times or more than the niobium content ratio to the total mass of the core material. The content is preferably 0.5% by mass or more, more preferably 2.0% by mass or more, based on the total mass of the coating layer. It is more preferably 5.0% by mass or more and 15.0% by mass or less.

[0051] The niobium content of the metal oxide particles is preferably 2.6% by weight or more, more preferably 2.6% by weight or more and 10.0% by weight or less, based on the total mass of the metal oxide particles.

[0052] In the case of particles satisfying the above formulae (1) and (2), in the present invention, the oxygen deficiency rate A of the entire metal oxide particles is more preferably 1.0% or less, and even more preferably 0.5% or less.

[0053] In the metal oxide particles of the present invention, a higher oxygen deficiency rate of the coating layer, that is, a larger C / B value, indicates that the coating layer is more selectively oxygen deficient.

[0054] Considering that oxygen deficiencies present evenly throughout the metal oxide particle act as charge traps and reduce charging ability, in order to exert the effects of the present invention, C / B must be greater than 10, and preferably greater than or equal to 20. The core material of the metal oxide particle does not need to be completely oxygen deficient.

[0055] In the present invention, the niobium content in the coating layer of the metal oxide particle and the ratio of the oxygen deficiency rate of the core material of the metal oxide particle to the oxygen deficiency rate of the coating layer can be measured by energy dispersive X-ray analysis (EDX).

[0056] In the present invention, the niobium content in the coating layer of the metal oxide particle and the ratio of the oxygen deficiency rate of the core material of the metal oxide particle to the oxygen deficiency rate of the coating layer were measured by SEM-EDX analysis of the cross section of the metal oxide particle.

[0057] In the present invention, the oxygen deficiency rate of the metal oxide particles can be determined by thermogravimetry (TG). When the metal oxide particles of the present invention are heated in an oxygen atmosphere, the mass decreases immediately after the start of heating due to the desorption of moisture and the like adsorbed on the metal oxide particle surface, and then increases from a certain temperature. The mass at the point where the mass changes from decreasing to increasing is taken as the minimum mass, and the difference between this and the maximum mass during subsequent heating is obtained. This difference is due to the oxygen deficiency sites of the titanium oxide particles bonding with oxygen.

[0058] In the present invention, the oxygen deficiency rate of the metal oxide particles was measured using a thermogravimetric analyzer (product name: Q5000IR, manufactured by TA Instruments). The temperature rise rate during the measurement was 10°C / min, and the measurement was performed under oxygen flow. The mass at the temperature at which the mass started to increase in the range of 300°C to 900°C was taken as the minimum mass, and the oxygen deficiency rate A was calculated from the minimum mass and the maximum mass during subsequent heating.

[0059] The percentage (mass%) of titanium contained in the core material of the metal oxide particles can also be determined by performing ICP emission spectrometry on a powder of the same material as the particles used for the core material. This material is dissolved in an acid such as sulfuric acid, and the resulting solution is measured.

[0060] In the present invention, the core material of the metal oxide particles can be of various shapes such as sphere, polyhedron, ellipsoid, flake, and needle. Among these, it is preferable to use a core material of a sphere, polyhedron, or ellipsoid from the viewpoint of reducing image defects such as black spots. Furthermore, it is more preferable that the core material is a sphere or a polyhedron close to a sphere. Titanium oxide particles can be preferably used as the core material of the metal oxide particles.

[0061] In the present invention, the core material and the coating layer preferably contain anatase type titanium oxide or rutile type titanium oxide. Furthermore, the core material and the coating layer more preferably contain anatase type titanium oxide, and particularly preferably are composed of anatase type titanium oxide. By using anatase type titanium oxide, fluctuations in the bright area potential are less likely to occur.

[0062] In the present invention, the average primary particle size of the metal oxide particles is preferably 30 nm or more and 500 nm or less. If the average primary particle size of the metal oxide particles is 30 nm or more, re-aggregation of the particles is unlikely to occur after the preparation of the coating solution for the protective layer. If re-aggregation of the particles occurs, the stability of the coating solution for the protective layer decreases, and cracks are likely to occur on the surface of the protective layer formed. If the average primary particle size of the metal oxide particles is 500 nm or less, the surface of the protective layer is unlikely to become rough. If the surface of the protective layer becomes rough, the image exposure is scattered, and the image quality is likely to deteriorate.

[0063] Furthermore, in the present invention, the average primary particle size of the metal oxide particles is more preferably 30 nm or more and 400 nm or less.

[0064] In the present invention, the average primary particle size D1 of metal oxide particles was determined using a scanning electron microscope as follows. The particles to be measured were observed using a scanning electron microscope S-4800 manufactured by Hitachi, Ltd., and the particle sizes of 100 particles were measured from the images obtained by the observation, and the arithmetic average was calculated to obtain the average primary particle size D1. The particle size of each particle was determined as (a+b) / 2, where a is the longest side of the primary particle and b is the shortest side. For needle-like metal oxide particles or flaky titanium oxide particles, the average particle size was calculated for each of the major axis diameter and minor axis diameter to obtain the average primary particle size.

[0065] In the present invention, the surfaces of the metal oxide particles may be treated with a silane coupling agent or the like.

[0066] In the present invention, the content of the metal oxide particles in the total volume of the protective layer is preferably 33% by volume or more, and more preferably 50% by volume or more. If these ranges are satisfied, the probability of contact between metal oxide particles in the protective layer increases, so that conductive paths due to niobium or oxygen deficiency in the coating layer become more easily connected, improving the effect of preventing charge retention.

[0067] The protective layer may contain a charge transport material, and examples of the charge transport material include polycyclic aromatic compounds, heterocyclic compounds, hydrazone compounds, styryl compounds, enamine compounds, benzidine compounds, triarylamine compounds, and resins having groups derived from these materials. Among these, triarylamine compounds and benzidine compounds are preferred.

[0068] Examples of the binder resin include polyester resin, acrylic resin, phenoxy resin, polycarbonate resin, polystyrene resin, phenol resin, melamine resin, epoxy resin, etc. Among them, polycarbonate resin, polyester resin, and acrylic resin are preferable.

[0069] The protective layer may be formed as a cured film by polymerizing a composition containing a monomer having a polymerizable functional group. Examples of the reaction include thermal polymerization, photopolymerization, and radiation polymerization. Examples of the polymerizable functional group of the monomer having a polymerizable functional group include an acrylic group and a methacrylic group. A material having a charge transport function may be used as the monomer having a polymerizable functional group.

[0070] The protective layer may contain additives such as antioxidants, ultraviolet absorbers, plasticizers, leveling agents, slipping agents, abrasion resistance improvers, etc. Specific examples of such additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, benzophenone compounds, siloxane-modified resins, silicone oils, fluororesin particles, polystyrene resin particles, polyethylene resin particles, silica particles, alumina particles, and boron nitride particles.

[0071] The average thickness of the protective layer is preferably from 0.3 μm to 10 μm, and more preferably from 0.5 μm to 7 μm.

[0072] The protective layer can be formed by preparing a coating solution for the protective layer containing the above-mentioned materials and solvent, forming a coating film from the coating solution, and drying and / or curing the coating solution. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, sulfoxide-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents.

[0073] [Process cartridges, electrophotographic devices] The process cartridge of the present invention is characterized in that it integrally supports the electrophotographic photosensitive member described above and at least one means selected from the group consisting of a charging means, a developing means, a transfer means and a cleaning means, and is detachably mountable to the main body of the electrophotographic apparatus.

[0074] The electrophotographic apparatus of the present invention is characterized by having the electrophotographic photosensitive member, charging means, exposure means, developing means and transfer means described above.

[0075] FIG. 1 shows an example of a schematic configuration of an electrophotographic apparatus having a process cartridge equipped with an electrophotographic photosensitive member. Reference numeral 1 denotes a cylindrical electrophotographic photoreceptor, which is driven to rotate around an axis 2 in the direction of the arrow at a predetermined peripheral speed. The surface of the electrophotographic photoreceptor 1 is charged to a predetermined positive or negative potential by a charging means 3. Although the figure shows a roller charging method using a roller-type charging member, a corona charging method, a proximity charging method, an injection charging method, or other charging methods may be adopted. Exposure light 4 is irradiated from an exposure means (not shown) onto the charged surface of the electrophotographic photoreceptor 1, and an electrostatic latent image corresponding to the target image information is formed. The electrostatic latent image formed on the surface of the electrophotographic photoreceptor 1 is developed with toner contained in a developing means 5, and a toner image is formed on the surface of the electrophotographic photoreceptor 1. The toner image formed on the surface of the electrophotographic photoreceptor 1 is transferred to a transfer material 7 by a transfer means 6. The transfer material 7 to which the toner image has been transferred is conveyed to a fixing means 8, where the toner image is fixed, and the material is printed out outside the electrophotographic device. The electrophotographic device may have a cleaning means 9 for removing deposits such as toner remaining on the surface of the electrophotographic photoreceptor 1 after transfer. Also, a so-called cleanerless system may be used in which the deposits are removed by a developing means or the like without providing a separate cleaning means. The electrophotographic apparatus may have a charge eliminating mechanism that eliminates charge on the surface of the electrophotographic photoreceptor 1 by pre-exposure light 10 from a pre-exposure means (not shown). Also, in order to mount and remove the process cartridge of the present invention to and from the main body of the electrophotographic apparatus, a guide means 12 such as a rail may be provided.

[0076] The electrophotographic photoreceptor of the present invention can be used in laser beam printers, LED printers, copiers, facsimiles, and combination machines thereof. EXAMPLES

[0077] The present invention will be described in more detail below using examples and comparative examples. The present invention is not limited to the following examples without departing from the gist of the present invention. In the following description of the examples, "parts" are by mass unless otherwise specified. Moreover, Examples 14 to 23 and 27 are reference examples.

[0078] [Production of metal oxide particles] (Production Example 1) (Metal oxide particles A1) The titanium dioxide core material can be produced by the known sulfuric acid method, in which a solution containing titanium sulfate and titanyl sulfate is heated and hydrolyzed to produce a metatitanic acid slurry, which is then dehydrated and fired. The core particles used were anatase-type titanium oxide particles with an average primary particle size of 150 nm, in which no niobium was detected. 100 g of this core material was dispersed in water to prepare a 1 L water suspension, which was then heated to 60°C. Niobium pentachloride (NbCl 5 A niobium solution in which 3.1 g of titanium dioxide was dissolved in 100 mL of 11.4 mol / L hydrochloric acid was mixed with 600 mL of titanium sulfate solution containing 33.7 g of Ti to form a titanium niobate solution, and a 10.7 mol / L sodium hydroxide solution were simultaneously added dropwise (parallel addition) over a period of 3 hours so that the pH of the suspension was 2 to 3. After the dropwise addition was completed, the pH was adjusted to approximately neutral, and a flocculant was added to cause the solid matter to settle. The supernatant was removed, the remainder was filtered, the residue was washed, and dried at 110°C to obtain an intermediate containing 0.1 wt% of organic matter derived from the flocculant in terms of C. This intermediate was heated at 800°C in nitrogen gas to produce metal oxide particles A1 with an average primary particle size of 190 nm.

[0079] (Metal oxide particles A2~A9, B1~B6, C1~C6) Titanium oxide-containing metal oxide particles A2 to A9, B1 to B6, and C1 to C6 were produced in the same manner as in Production Example 1, except that in the production of metal oxide particles 1, the core material used and the coating conditions were changed.

[0080] (Comparative Manufacturing Example 1) With reference to JP 2007-334334 A, a powder of particles R1 containing titanium oxide, which is rutile-type titanium oxide particles having an average primary particle size of 200 nm, was obtained.

[0081] Comparative Production Example 2 With reference to JP-A-2005-17470, a powder of titanium oxide-containing particles R2 was obtained, which were anatase-type titanium oxide particles having an average primary particle size of 180 nm and a niobium content of 1.0 wt %.

[0082] [Table 1]

[0083] [Production of protective layer coating solution] (Protective layer coating solution 1) 22 parts of a compound represented by the following structural formula (1) was mixed with a mixed solvent of 144 parts of 2-propanol and 16 parts of tetrahydrofuran, and 100 parts of metal oxide particles A1 were added to this solution and stirred. These were placed in a vertical sand mill using 200 parts of glass beads with an average particle size of 1.0 mm, and dispersed for 2 hours at a dispersion temperature of 23±3° C. and a rotation speed of 1500 rpm (circumferential speed 5.5 m / s) to obtain a dispersion. The glass beads were removed from this dispersion using a mesh, and the resulting dispersion was pressure filtered using PTFE filter paper (product name: PF060, manufactured by Advantec Toyo) to prepare protective layer coating solution A1. [ka]

[0084] (Protective layer coating solutions A2 to A13, B1 to B10, C1 to C10 and R1 to R2) Protective layer coating solutions A2 to A13, B1 to B10, C1 to C10 and R1 to R2 were prepared in the same manner as protective layer coating solution 1, except that the type and mass (parts) of metal oxide particles used in preparing protective layer coating solution 1 were as shown in Table 2.

[0085] (Protective layer coating solution A14) Protective layer coating solution A14 was prepared by dispersing 22 parts of the acrylic monomer represented by the above structural formula (1), 7 parts of 2-methylthioxanthone as a photoinitiator, 100 parts of metal oxide particles A1, and 160 parts of ethanol in the same manner as in protective layer coating solution 1.

[0086] [Table 2]

[0087] [Manufacturing of electrophotographic photoreceptors] (Electrophotographic Photoreceptor 1) An aluminum cylinder (JIS-A3003, aluminum alloy) having a diameter of 24 mm and a length of 257.5 mm was used as a support (conductive support). An aluminum cylinder (JIS-A3003, aluminum alloy) having a length of 260.5 mm and a diameter of 30 mm was used as a support (conductive support).

[0088] Next, 50 parts of titanium oxide particles coated with oxygen-deficient tin oxide (powder resistivity: 120 Ω cm, tin oxide coverage: 40%), 40 parts of phenolic resin (Plyofen J-325, Dainippon Ink and Chemicals, Inc., resin solids content: 60%), and 55 parts of methoxypropanol were placed in a sand mill using glass beads with a diameter of 1 mm and dispersed for 3 hours to prepare a coating solution for the conductive layer. The average particle size of the titanium oxide particles coated with oxygen-deficient tin oxide in this conductive layer coating liquid was measured by centrifugal sedimentation method using a particle size distribution meter (product name: CAPA700) manufactured by Horiba, Ltd., tetrahydrofuran as a dispersion medium, and a rotation speed of 5000 rpm. As a result, the average particle size was 0.30 μm. This conductive layer coating liquid was dip-coated onto a support, and the resulting coating film was dried at 160° C. for 30 minutes to form a conductive layer having a thickness of 30 μm.

[0089] Next, the following materials were mixed with 50 parts of 1-methoxy-2-propanol and 5 parts of tetrahydrofuran. 0 parts of the mixed solvent. Compound represented by formula (2) 3.36 parts Styrene-acrylic resin as polyolefin resin (product name: UC-3920, Toa Goh Manufactured by Sei Co., Ltd.) 0.35 parts As an isocyanate compound, a blocked isocyanate compound (product name: SBB- 70P, Asahi Kasei Corporation) 6.40 parts This solution was mixed with silica slurry dispersed in isopropyl alcohol (product name: IPA-S T-UP, manufactured by Nissan Chemical Industries, Ltd., solid content concentration: 15% by mass, viscosity: 9mPa·s)1. 8 parts of polytetrafluoroethylene (Advantec) was added and stirred for 1 hour. The mixture was pressure filtered using a filter manufactured by Epson (product name: PF020). The thus obtained coating liquid for forming an undercoat layer was dip-coated onto the conductive layer, and the obtained coating film was heated at 170° C. for 40 minutes to be cured (polymerized) to form an undercoat layer with a thickness of 0.7 μm. [ka]

[0090] Next, a hydroxygallium phthalocyanine crystal (charge generating material) having peaks at Bragg angles (2θ±0.2°) of 7.5°, 9.9°, 12.5°, 16.3°, 18.6°, 25.1°, and 28.3° in CuKα characteristic X-ray diffraction was prepared. 8 parts of this hydroxygallium phthalocyanine crystal, 4 parts of polyvinyl butyral (product name: S-LEC BX-1, manufactured by Sekisui Chemical Co., Ltd.), and 250 parts of cyclohexanone were placed in a sand mill using glass beads with a diameter of 1 mm, and dispersed for 2 hours. Next, 250 parts of ethyl acetate were added to this to prepare a coating solution for charge generating layer. This charge generating layer coating liquid was dip coated onto the undercoat layer to form a coating film, and the resulting coating film was dried at 95° C. for 10 minutes to form a charge generating layer having a thickness of 0.2 μm.

[0091] Next, 6 parts of an amine compound (hole transport material) represented by the following formula (3), 2 parts of an amine compound (hole transport material) represented by the following formula (4), and 10 parts of a polyester resin having a weight average molecular weight (Mw) of 100,000 and having structural units represented by the following formulas (5) and (6) in a 5 / 5 ratio were dissolved in a mixed solvent of 40 parts of dimethoxymethane and 60 parts of chlorobenzene to prepare a coating solution for the charge transport layer. [ka] [ka] [ka] [ka] This charge transport layer coating liquid was dip-coated onto the charge generating layer, and the resulting coating was dried at 120° C. for 40 minutes to form a charge transport layer having a thickness of 22 μm.

[0092] Next, the protective layer coating solution A1 was applied on the charge transport layer by dip coating to form a coating film, and the obtained coating film was dried at 50°C for 6 minutes. Thereafter, under a nitrogen atmosphere, the support (irradiated body) was rotated at a speed of 300 rpm under conditions of an acceleration voltage of 70 kV and a beam current of 2.0 mA, and the coating film was irradiated with an electron beam for 1.6 seconds. The oxygen concentration during electron beam irradiation was 810 ppm. Next, the coating film was naturally cooled in the atmosphere until the temperature reached 25°C, and then heat-treated for 1 hour under conditions that the temperature of the coating film reached 120°C, forming a protective layer with a thickness of 3 μm. In this way, a cylindrical (drum-shaped) electrophotographic photoreceptor having the protective layer of Example 1 was produced.

[0093] (Electrophotographic photoreceptors 2 to 33, electrophotographic photoreceptors R1 to R2) An electrophotographic photoreceptor was produced in the same manner as in Example 1, except that the protective layer coating liquid used in the production of the electrophotographic photoreceptor was changed from protective layer coating liquid 1 to protective layer coating liquids A2 to A14, B1 to B10, C1 to C10, and R1 to R2, respectively.

[0094] (Electrophotographic photoreceptor 34) The protective layer coating solution 34 is used, and this is dip-coated on the charge transport layer, dried, and then irradiated with a high-pressure mercury lamp at 250 W / cm 2 An electrophotographic photoreceptor was produced in the same manner as in Example 1, except that the photoreceptor was irradiated with ultraviolet light at a light intensity of 100 nm for 60 seconds, and then dried with hot air at 120° C. for 2 hours to form a protective layer having a thickness of 3 μm.

[0095] (Analysis of Protective Layer of Electrophotographic Photoreceptor) Five pieces each having a size of 5 mm square were cut out from the electrophotographic photoreceptor produced as described above, and five sample pieces for observation were prepared for each electrophotographic photoreceptor. First, for each electrophotographic photoreceptor, one sample piece was used, and the protective layer was sliced ​​to a thickness of 150 nm by the FIB-μ sampling method using a focused ion beam processing and observation device (product name: FB-2000A, manufactured by Hitachi High-Tech Manufacturing & Services). The composition of the protective layer was analyzed using a field emission electron microscope (HRTEM) (product name: JEM-2100F, manufactured by JEOL Ltd.) and an energy dispersive X-ray analyzer (EDX) (product name: JED-2300T, manufactured by JEOL Ltd.). The measurement conditions for EDX were an acceleration voltage of 200 kV and a beam diameter of 1.0 nm.

[0096] From the EDX images obtained, the core diameter and coating layer thickness were determined for each of the 100 metal oxide particles, and the ratio of the average primary particle diameter of the core material to the average layer thickness of the coating layer was calculated from the arithmetic average of these. Therefore, the average primary particle diameter of metal oxide particles with an average coating layer thickness of 20 nm and an average primary particle diameter of the core material of 150 nm is 190 nm.

[0097] Next, for each electrophotographic photoreceptor, the remaining four sample pieces were used to perform three-dimensional processing of the protective layer at 2 μm×2 μm×2 μm using FIB-SEM Slice&View. The particle content in the total volume of the protective layer was calculated from the difference in contrast of FIB-SEM Slice&View. In this embodiment, the conditions for Slice&View were as follows: Sample processing for analysis: FIB method Processing and observation equipment: SII / Zeiss NVision40 Slice spacing: 10 nm Observation conditions: Acceleration voltage: 1.0 kV Sample tilt: 54° WD: 5mm Detector: BSE detector Perforator: 60μm, high current ABC:ON Image resolution: 1.25nm / pixel

[0098] The analysis area was 2 μm long x 2 μm wide, and the information for each cross section was integrated to obtain a 2 μm long x 2 μm wide x 2 μm thick (8 μm 3 The measurement environment is temperature: 23°C, pressure: 1×10 -4 Pa. As a processing and observation device, a Strata400S (sample tilt: 52°) manufactured by FEI can also be used. Information for each cross section was obtained by image analysis of the area of ​​the specified titanium oxide particles of the present invention or the titanium oxide particles used in the comparative examples. The image analysis was performed using image processing software: Image-Pro Plus manufactured by Media Cybernetics. Based on the obtained information, a volume of 2 μm × 2 μm × 2 μm (unit volume: 8 μm 3 The volume V of the titanium oxide particles of the present invention or the titanium oxide particles used in the comparative example in the sample was determined. 3 / 8μm 3 × 100) was calculated. 3 / 8μm 3 × 100) was taken as the content [volume %] of the titanium oxide particles of the present invention or the titanium oxide particles used in the comparative example in the protective layer relative to the total volume of the protective layer. The results are shown in Table 3.

[0099] <Evaluation> First, the electrophotographic photoreceptors 1 to 34 and R1 to R2 thus produced were used to evaluate the charging ability during repeated use under the following conditions. When the charging ability deteriorates, the dark potential (Vd) decreases and fog increases. The electrophotographic apparatus used was a modified version of a laser beam printer, product name HP LaserJet Enterprise Color M553dn, manufactured by Hewlett-Packard Co. The electrophotographic apparatus used for the evaluation was modified so that the image exposure amount and the developing bias could be adjusted and measured. First, the amount of exposure was adjusted so that the light area potential of the electrophotographic photosensitive members of the Examples and Comparative Examples became −180 V, and then the dark area potential (Vd) was measured. Thereafter, the developing bias Vdc was adjusted to -450 V, and the toner was attached to a cyan cartridge of an electrophotographic apparatus. Thereafter, a solid white image was output in cyan on an A4-size plain paper in an environment of 23° C. temperature and 50% relative humidity. The fogging evaluation was performed by measuring the reflectance of the white part of the image and the unused paper using a white light meter (product name: REFLECTMETER TC-6DS / A, manufactured by Tokyo Denshoku), and the difference between the two was taken as the fogging. Reflectance of unused paper - reflectance of the white part of the image = fogging%, and fogging of 2.0% or more was evaluated as NG. The results are shown in Table 3.

[0100] [Table 3] [Explanation of symbols]

[0101] 1. Electrophotographic photoreceptor 2-axis 3. Charging means 4 Exposure light 5. Developing method 6 Transfer Method 7 Transfer material 8 Fixing Method 9 Cleaning Method 10 Pre-exposure light 11 Process cartridge 12 Guidance means

Claims

1. An electrophotographic photoreceptor having a support, a conductive layer, a photosensitive layer, and a protective layer in this order, the protective layer contains a binder resin and metal oxide particles, The metal oxide particles have a core material containing titanium oxide and a coating layer containing titanium oxide that coats the core material, an electrophotographic photoreceptor, characterized in that the oxygen deficiency rate of the metal oxide particles is A (%), the oxygen deficiency rate of the core material is B (%), and the oxygen deficiency rate of the coating layer is C (%), thereby satisfying the following formulas (1) and (2): A≦2.0 (1) 10 × B < C (2)

2. 2. The electrophotographic photoreceptor according to claim 1, wherein the coating layer further contains niobium.

3. 3. The electrophotographic photoreceptor according to claim 2, wherein the content of said niobium in said metal oxide particles is 2.6% by weight or more based on the total mass of said metal oxide particles.

4. 4. The electrophotographic photoreceptor according to claim 1, wherein the titanium oxide contained in the core material is anatase type titanium oxide or rutile type titanium oxide.

5. 5. The electrophotographic photoreceptor according to claim 1, wherein a content of the metal oxide particles in the total volume of the protective layer is 33 volume % or more.

6. 6. A process cartridge which integrally supports the electrophotographic photosensitive member according to any one of claims 1 to 5 and at least one means selected from the group consisting of a charging means, a developing means and a cleaning means, and is detachably mountable to a main body of an electrophotographic apparatus.

7. 6. An electrophotographic apparatus comprising the electrophotographic photoreceptor according to claim 1, a charging means, an exposure means, a developing means and a transfer means.

Citation Information

Patent Citations

  • Electrophotographic photoreceptor, image forming method and image forming apparatus

    JP2009229495A

  • Electrophotographic photoreceptor and image forming apparatus

    JP2015022297A

  • Electrophotographic photosensitive member, process cartridge, and electrophotographic apparatus

    JP2018141974A

  • Manufacturing method for electrophotographic photoreceptor

    JP2020030384A

  • Electrophotographic photoreceptor, process cartridge, and electrophotographic device

    JP2020034903A