Purification method for lithium bis(fluorosulfonyl)imide
Bismuth trichloride or antimony trichloride-based purification of LiFSI addresses the challenges of water and chloride ion removal, achieving high-purity LiFSI with enhanced thermal stability and safety for lithium batteries.
Patent Information
- Application Number
- JP2024526826
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-08-31
- Filing Date
- 2023-08-03
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2043-08-03
AI Technical Summary
Existing methods for purifying lithium bis(fluorosulfonyl)imide (LiFSI) are ineffective in removing water and residual chloride ions, leading to poor thermal stability and environmental pollution, which affects the performance and safety of lithium batteries.
Using bismuth trichloride or antimony trichloride as a water removing agent, followed by recrystallization, to achieve a water content of less than 20 ppm and chloride ion content of less than 5 ppm in LiFSI, ensuring high purity and safety.
The method effectively removes water and chloride ions, resulting in high-purity LiFSI with improved thermal stability and reduced environmental impact, enhancing the performance and safety of lithium batteries.
Smart Images

Figure 0007587904000001
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This patent application claims priority to Chinese Patent Application No. CN202211055475.1, filed on August 31, 2022. The entire disclosure of the prior application is incorporated herein by reference.
[0002] The present application relates to the field of purification technology, and in particular to a method for purifying lithium bis(fluorosulfonyl)imide. [Background technology]
[0003] Lithium bis(fluorosulfonyl)imide (LiFSI) has excellent electrochemical stability, thermal stability and low temperature performance, is more compatible with battery positive and negative electrode materials, and is safer. It is an important high-performance electrolyte material in new energy devices such as primary lithium batteries, secondary lithium ion batteries and supercapacitors, and is currently the new lithium salt with the greatest potential for industrialization.
[0004] LiFSI is mainly obtained by the synthetic route of first reacting chlorosulfonic acid, thionyl chloride and sulfamic acid to obtain imidodisulfuryl chloride, or reacting chlorosulfonic acid with chlorosulfonyl isocyanate to obtain imidodisulfuryl chloride, and then reacting imidodisulfuryl chloride with a fluorination reagent to obtain bis(fluorosulfonyl)imide (HFSI) or bis(fluorosulfonyl)imide metal salt, and then reacting HFSI or bis(fluorosulfonyl)imide metal salt with a lithiation reagent (lithium hydroxide or lithium carbonate) to obtain LiFSI. However, the above synthetic route generates water as a by-product, and LiFSI is very prone to water absorption, so water is contained in the LiFSI crude product, and one crystal water is complexed. Research has shown that LiFSI after absorbing water has poor thermal stability and is not suitable for long-term storage, and the more water it contains, the faster its decomposition rate. Therefore, conventional physical methods are basically unable to effectively remove the moisture in the LiFSI crude product, and water removal is often performed by adding a dehydrating agent to cause a chemical reaction with the water in the LiFSI crude product.
[0005] The currently commonly used dehydrating agents are thionyl chloride or other water-sensitive materials, such as acetyl chloride or sulfuryl chloride-based materials, which can achieve excellent dehydration effect, but generate significant chloride ion residue, which seriously affects the performance of lithium batteries, and also generates pollution due to mixed waste gas that is difficult to treat, which increases the stress of environmental protection. Therefore, it is desirable to find a LiFSI purification method that has high dehydration effect, does not generate chloride ion residue, and is safe and environmentally friendly, which is of great significance to guarantee the stability of the electrolyte of lithium batteries and promote the smooth popularization of lithium batteries. Summary of the Invention [Problem to be solved by the invention]
[0006] In order to solve the above problems in the prior art, the object of the present application is to provide a method for purifying lithium bis(fluorosulfonyl)imide, which uses bismuth trichloride or antimony trichloride as a water remover and further obtains high-purity lithium bis(fluorosulfonyl)imide having a water content of only 5 ppm to 20 ppm and no residual chloride ions by recrystallization. [Means for solving the problem]
[0007] In order to achieve the objectives of the above application, the embodiments of the present application adopt the following technical solutions:
[0008] The method for purifying lithium bis(fluorosulfonyl)imide is as follows: Step 1: adding a dehydrating agent to a pretreatment solution containing a lithium bis(fluorosulfonyl)imide crude product, carrying out a dehydration reaction under conditions of 20°C to 40°C, and after no acidic gas is generated in the reaction system, carrying out the reaction for another 1h to 6h, filtering, and obtaining a filtrate, the dehydrating agent being bismuth trichloride or antimony trichloride; and step 2, evaporating and concentrating the filtrate and recrystallizing the concentrate to obtain high-purity lithium bis(fluorosulfonyl)imide.
[0009] The present application does not particularly limit the form of recrystallization, and any recrystallization method well known to those skilled in the art may be employed, such as crystallization using a poor solvent for lithium bis(fluorosulfonyl)imide (i.e., a solvent having low solubility for lithium bis(fluorosulfonyl)imide).
[0010] The dehydration principle of the bismuth trichloride and antimony trichloride is as follows: SbCl3+H2O→SbOCl↓+2HCl↑ BiCl3+H2O→BiOCl↓+2HCl↑.
[0011] As one embodiment of the present invention, in step 1, the dehydrating agent is added to a pretreatment liquid containing a lithium bis(fluorosulfonyl)imide crude product, and a dehydration reaction is carried out at 30°C to 35°C. After acidic gas is no longer generated in the reaction system, the reaction is continued for another 1 to 2 hours, and then the reaction is filtered to obtain the filtrate.
[0012] The preferred reaction conditions in the above examples are advantageous in promoting the progress of the dehydration reaction, and can effectively remove water and residual chloride ions in the pretreatment liquid.
[0013] As one embodiment of the present application, in step 1, the molar ratio of the water removing agent to H2O in the pretreatment liquid is 1-2:1.
[0014] More optionally, in step 1, the molar ratio of the water removing agent to H2O in the pretreatment liquid is 1.02-1.1:1.
[0015] The present application is not particularly limited to a method for measuring the H2O content in the pretreatment liquid, and any method well known to those skilled in the art, such as Karl Fischer Coulomb method, may be used.
[0016] The preferred amount of water removing agent can not only ensure the complete removal of water from the lithium bis(fluorosulfonyl)imide crude product, but also remove the residual chloride ions from the pretreatment solution, thereby obtaining high-purity lithium bis(fluorosulfonyl)imide.
[0017] As one embodiment of the present application, in step 1, the time for adding the water removing agent is 40 minutes to 60 minutes.
[0018] Since the dehydrating agent may generate heat during the dehydration reaction, the dehydrating agent may be added all at once or may be added in several portions by controlling the addition time of the dehydrating agent in order to ensure that the temperature of the dehydration reaction is ≦40° C. and to avoid causing decomposition of lithium bis(fluorosulfonyl)imide, which would result in a decrease in the yield after purification.
[0019] In one embodiment of the present application, the preparation process of the pre-treatment solution is to dissolve the lithium bis(fluorosulfonyl)imide crude product in an organic solvent, and the organic solvent is at least one of dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, ethylene carbonate, propylene carbonate, ethyl ether, methyl tert-butyl ether, ethylene glycol dimethyl ether, acetonitrile, butyl acetate, or ethyl acetate.
[0020] The present application is not particularly limited to the origin of the lithium bis(fluorosulfonyl)imide crude product, and the lithium bis(fluorosulfonyl)imide crude product may be obtained by a commonly used manufacturing method in this field. In the present application, the water content in the lithium bis(fluorosulfonyl)imide crude product may be >100ppm, and the purity may be <99.9%.
[0021] As one embodiment of the present application, in step 1, the concentration of lithium bis(fluorosulfonyl)imide in the pretreatment liquid is 10 wt % to 25 wt %.
[0022] As one embodiment of the present application, in step 1, the pretreatment liquid is a solution containing a crude lithium bis(fluorosulfonyl)imide product obtained by subjecting bis(fluorosulfonyl)imide to an ion exchange reaction with a lithium reagent and filtering the resultant.
[0023] The pretreatment solution in this application may be a solution containing a crude lithium bis(fluorosulfonyl)imide product obtained by subjecting bis(fluorosulfonyl)imide and a lithium reagent as raw materials to an ion exchange reaction to obtain a mixed solution, which is then filtered. The lithium reagent is selected from reagents capable of causing typical lithium reactions in this field, such as lithium hydroxide or lithium carbonate. The solution is directly purified to simplify the reaction steps, and high-purity lithium bis(fluorosulfonyl)imide with extremely low water content and no residual chloride ions is obtained.
[0024] In the present application, the solvent for the bis(fluorosulfonyl)imide and the lithium reagent is limited to the same solvent, and the same solvent includes, but is not limited to, ethyl ether, methyl tert-butyl ether, isopropyl ether, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, etc. In addition, the present application does not particularly limit the reaction process using the bis(fluorosulfonyl)imide and the lithium reagent as raw materials, and a production method well known to those skilled in the art may be used.
[0025] As one embodiment of the present application, in step 1, the stirring speed of the dehydration reaction is 60 rpm to 300 rpm.
[0026] The preferred stirring speed in the above embodiment can ensure uniform mixing of each component in the system and promote the smooth progress of the dehydration reaction.
[0027] In one embodiment of the present application, in step 1, the acid gas is recovered using an alkaline solution.
[0028] In the present invention, bismuth trichloride or antimony trichloride is used as a water removing agent, and the generated hydrogen chloride gas is a single by-product, which can be easily recovered and utilized by using an alkaline solution, thereby avoiding the occurrence of pollution caused by mixed waste gases and reducing the stress on environmental protection.
[0029] The present application is not particularly limited to the alkaline solution, and may be a NaOH solution, a KOH solution, a sodium carbonate solution, or the like.
[0030] In some embodiments, the acid gases can be collected in an alkaline solution after passing through a bubbler, with no more bubbles in the bubbler indicating no more acid gas is being generated.
[0031] As one embodiment of the present application, in step 2, the conditions of evaporation and concentration are a temperature of 10° C. to 40° C. and a degree of vacuum of 100 Pa to 600 Pa.
[0032] As one embodiment of the present application, in step 2, the filtrate is evaporated and concentrated until the concentration of lithium bis(fluorosulfonyl)imide in the filtrate reaches 30 wt % to 40 wt %.
[0033] The preferred evaporation conditions in the above examples are favorable for removing a portion of the solvent in the filtrate, which favors the progress of the subsequent recrystallization process.
[0034] In one embodiment of the present application, in step 1, the filtration is performed in a glove box where the moisture content is less than 10 ppm.
[0035] After the above pretreatment liquid undergoes the dehydration reaction, the water content in the reaction system is very low, basically less than 20 ppm, so it needs to be filtered in a glove box, otherwise the reaction system after dehydration will reabsorb moisture in the environment, which will affect the dehydration effect.
[0036] The present invention uses bismuth trichloride or antimony trichloride as a water remover, and utilizes its hydrolysis to remove water from the lithium bis(fluorosulfonyl)imide crude product, producing an oxychloride that is poorly soluble in both organic solvents and water, and then filtering to remove the poorly soluble oxychloride, thereby avoiding the residual chloride ions. Moreover, the anion volume of bis(fluorosulfonyl)imide is large, and bismuth or antimony is unlikely to form a salt with bis(fluorosulfonyl)imide, thus avoiding the generation of new impurities. In addition, the metal ion M 3+ (Sb 3+ Or Bi 3+ ) is Cl under acidic conditions. - It can combine with fluorine to form the sparingly soluble oxychloride MOCl, which helps to remove chloride ions in the solution, and obtain high-purity lithium bis(fluorosulfonyl)imide with high purity, extremely low water content, and no residual chloride ions.
[0037] In this application, the water contained in the crude product is removed using bismuth trichloride or antimony trichloride as a water remover, and then some of the organic solvent is removed by evaporation and concentration, and finally recrystallization is performed to obtain lithium bis(fluorosulfonyl)imide with a high purity of 99.95% or more, a chloride ion content of <5 ppm, and a water content of <20 ppm. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0038] In order to make the objectives, technical solutions and advantages of the present application clearer, the present application will be described in more detail below with reference to the embodiments. It should be understood that the specific embodiments described herein are only used to interpret the present application, and do not limit the present application. EXAMPLES
[0039] The present application provides a method for purifying lithium bis(fluorosulfonyl)imide, 37.4 g (0.2 mol) of lithium bis(fluorosulfonyl)imide crude product (purity 98.5%, water content 5000 ppm) was dissolved in 200 g of dimethyl carbonate to form a pretreatment solution; Step 1: Add 3.47g of bismuth trichloride to the pretreatment solution in several portions within 40 minutes at 35°C to carry out a dehydration reaction, and after the acid gas generated in the reaction system passes through a bubbler and is absorbed by the NaOH solution, the reaction is continued for another 2 hours after the acid gas is no longer generated in the reaction system, and the solution is filtered in a glove box where the moisture content is less than 10ppm to obtain a filtrate; and step 2, evaporating and concentrating the filtrate under conditions of a vacuum degree of 600 Pa and a temperature of 10° C. until the concentration of lithium bis(fluorosulfonyl)imide in the filtrate becomes 30 wt %, and then recrystallizing and vacuum drying the concentrate to obtain 35.63 g of high-purity lithium bis(fluorosulfonyl)imide with a purity of 99.97% and a yield of 96.7%. EXAMPLES
[0040] The present application provides a method for purifying lithium bis(fluorosulfonyl)imide, 37.4 g (0.2 mol) of lithium bis(fluorosulfonyl)imide crude product (purity 98.2%, water content 6000 ppm) was dissolved in 300 g of propylene carbonate to form a pretreatment solution; Step 1: Add 5.4g of bismuth trichloride to the pretreatment solution in several portions within 50 minutes at 20°C to carry out a dehydration reaction, and after the acid gas generated in the reaction system passes through a bubbler and is absorbed by the NaOH solution, the reaction is continued for another 5.5 hours after the acid gas is no longer generated in the reaction system, and the solution is filtered in a glove box where the moisture content is less than 10ppm to obtain a filtrate; and step 2, evaporating and concentrating the filtrate under conditions of a vacuum degree of 350 Pa and a temperature of 25° C. until the concentration of lithium bis(fluorosulfonyl)imide in the filtrate is 35 wt %, and then recrystallizing and vacuum drying the concentrate to obtain 35.46 g of high-purity lithium bis(fluorosulfonyl)imide with a purity of 99.96% and a yield of 96.5%. EXAMPLES
[0041] The present application provides a method for purifying lithium bis(fluorosulfonyl)imide, 37.4 g (0.2 mol) of lithium bis(fluorosulfonyl)imide crude product (purity 98.1%, water content 6800 ppm) was dissolved in 115 g of methyl tert-butyl ether to form a pretreatment solution; Step 1: Add 4.5g of bismuth trichloride to the pretreatment solution in several portions within 60 minutes at 40°C to carry out a dehydration reaction, and after the acid gas generated in the reaction system passes through a bubbler and is absorbed by the NaOH solution, the reaction is continued for another 3 hours after the acid gas is no longer generated in the reaction system, and the solution is filtered in a glove box where the moisture content is less than 10ppm to obtain a filtrate; and step 2, evaporating and concentrating the filtrate under conditions of a vacuum degree of 100 Pa and a temperature of 40° C. until the concentration of lithium bis(fluorosulfonyl)imide in the filtrate becomes 40 wt %, and then recrystallizing and vacuum drying the concentrate to obtain 35.53 g of high-purity lithium bis(fluorosulfonyl)imide with a purity of 99.96% and a yield of 96.8%.
[0042] In order to better illustrate the technical solution of the present application, the following Comparative Examples are further compared with the Examples of the present application. Comparative Example 1
[0043] This comparative example provides a method for purifying lithium bis(fluorosulfonyl)imide. Different from Example 1, in step 1, 3.47g of bismuth trichloride is replaced with 1.78g of anhydrous ferric chloride (the molar ratio of dehydrating agent and H2O content is the same as in Example 1), and 30.99g of lithium bis(fluorosulfonyl)imide is obtained with a purity of 93.5% and a yield of 78.4%. Comparative Example 2
[0044] This comparative example provides a method for purifying lithium bis(fluorosulfonyl)imide. Different from Example 1, in step 1, 3.47g of bismuth trichloride is replaced with 1.47g of aluminum trichloride (the molar ratio of water remover and HO content is the same as in Example 1), and 33.05g of lithium bis(fluorosulfonyl)imide is obtained with a purity of 95.2% and a yield of 85.4%.
[0045] In order to better illustrate the characteristics of the purification method of lithium bis(fluorosulfonyl)imide provided in the examples of the present application, the water content and residual chloride ions in the lithium bis(fluorosulfonyl)imides prepared in the following Examples 1 to 3 and Comparative Examples 1 and 2 were detected, and the detection results are shown in Table 1 below.
[0046] [Table 1]
[0047] The water content and chloride ion content in the lithium bis(fluorosulfonyl)imide were both detected according to the method in the People's Republic of China Chemical Industry Standard HG / T4066-2015 Lithium Hexafluorophosphate.
[0048] As can be seen from Table 1, the present invention uses bismuth trichloride or antimony trichloride as a water remover, which can not only significantly remove water contained in the crude product, but also remove the residual chloride ions, thereby obtaining lithium bis(fluorosulfonyl)imide with a water content of less than 20 ppm, a chloride ion content of less than 5 ppm, and a high purity of 99.95% or more.
[0049] The above are merely preferred embodiments of the present application, and do not limit the present application. Any modifications, equivalent replacements or improvements made within the spirit and principle of the present application should be included within the protection scope of the present application.
Claims
1. Step 1: adding a dehydrating agent to a pretreatment solution containing a lithium bis(fluorosulfonyl)imide crude product, carrying out a dehydration reaction under conditions of 20°C to 40°C, and after no acidic gas is generated in the reaction system, carrying out the reaction for another 1h to 6h, filtering, and obtaining a filtrate, the dehydrating agent being bismuth trichloride or antimony trichloride; Step 2: evaporating and concentrating the filtrate and recrystallizing the concentrate to obtain high-purity lithium bis(fluorosulfonyl)imide; In step 1, the water removing agent and the H in the pretreatment liquid 2 The molar ratio of O is 1 to 2:1, In step 1, the pretreatment solution comprises a lithium bis(fluorosulfonyl)imide crude product and an organic solvent, and the organic solvent is at least one of dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, ethylene carbonate, propylene carbonate, ethyl ether, methyl tert-butyl ether, ethylene glycol dimethyl ether, acetonitrile, butyl acetate, or ethyl acetate; In step 2, the evaporation and concentration conditions are a temperature of 10°C to 40°C and a vacuum degree of 100 Pa to 600 Pa.
1. A method for purifying lithium bis(fluorosulfonyl)imide, comprising:
2. In step 1, the water removing agent and the H in the pretreatment liquid 2 The method for purifying lithium bis(fluorosulfonyl)imide according to claim 1, characterized in that the molar ratio of lithium bis(fluorosulfonyl)imide to O is 1.02-1.1:
1.
3. The method for purifying lithium bis(fluorosulfonyl)imide according to claim 1, characterized in that in step 1, the addition time of the water removing agent is 40 min to 60 min.
4. 2. The method for purifying lithium bis(fluorosulfonyl)imide according to claim 1, wherein in step 1, the concentration of lithium bis(fluorosulfonyl)imide in the pretreatment solution is 10 wt % to 25 wt %.
5. 2. The method for purifying lithium bis(fluorosulfonyl)imide according to claim 1, wherein in step 1, the pretreatment solution is a solution containing a lithium bis(fluorosulfonyl)imide crude product obtained by subjecting bis(fluorosulfonyl)imide to an ion exchange reaction with a lithium reagent and filtering the resultant solution, and the lithium reagent is lithium hydroxide or lithium carbonate.
6. The method for purifying lithium bis(fluorosulfonyl)imide according to claim 1, characterized in that in step 1, the stirring speed of the dehydration reaction is 60 rpm to 300 rpm.
7. 2. The method for purifying lithium bis(fluorosulfonyl)imide according to claim 1, wherein in step 1, the acid gas is recovered using an alkaline solution.
8. The method for purifying lithium bis(fluorosulfonyl)imide according to claim 1, characterized in that in step 2, after evaporation and concentration, the concentration of lithium bis(fluorosulfonyl)imide in the filtrate is 30 wt% to 40 wt%.
Citation Information
Patent Citations
Purification method of bis(fluorosulfonyl)imide
CN113912028A
Synthesis of bis(fluorosulfonyl)imides
JP2015531744A
Purified lithium bis(fluorosulfonyl)imide (LIFSI) product, method for purifying crude LIFSI, and uses of purified LIFSI product