Thermoelectric element and its manufacturing method
A lithium-doped Mg2Si thermoelectric element with recrystallized and sintered regions and a boron nitride insulating layer addresses the lack of stable p-type elements, achieving p-type performance and thermal stability for efficient power generation.
Patent Information
- Application Number
- JP2020155900
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-16
- Publication Date
- 2024-12-02
- Estimated Expiration
- 2040-09-16
AI Technical Summary
Conventional Mg2Si-based thermoelectric elements primarily exhibit n-type thermoelectric properties with poor thermal stability and lack effective p-type counterparts.
A thermoelectric element composed of magnesium silicide (Mg2Si) doped with lithium, featuring a recrystallized region for n-type properties and a normally sintered region for p-type properties, with an insulating boron nitride layer around the Si-based material during sintering to enhance thermal stability.
The element achieves p-type thermoelectric characteristics with high thermal stability, enabling efficient thermoelectric power generation by suppressing the influence of n-type properties and maintaining performance under varying temperatures.
Smart Images

Figure 0007592282000001 
Figure 0007592282000002 
Figure 0007592282000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermoelectric element and a manufacturing method thereof, and more particularly to an Mg2Si-based thermoelectric element and a manufacturing method thereof. [Background technology]
[0002] Thermoelectric conversion modules for thermoelectric power generation have been known for some time. Such thermoelectric conversion modules are generally composed of a plurality of π-type thermoelectric elements (n-type thermoelectric elements and p-type thermoelectric elements each having one end joined with a metal electrode) arranged in a plate shape, a plurality of metal electrodes for electrically connecting the plurality of π-type thermoelectric elements, and a pair of insulating substrates (e.g., ceramic substrates) that sandwich the plurality of π-type thermoelectric elements and the plurality of metal electrodes.
[0003] In a thermoelectric conversion module for thermoelectric power generation, power is generated by providing a predetermined temperature difference (for example, about 300° C.) between a high-temperature surface (high-temperature insulating substrate) and a low-temperature surface (low-temperature insulating substrate).
[0004] As described above, a thermoelectric conversion module for thermoelectric power generation is composed of n-type and p-type thermoelectric elements, and since a large temperature difference is applied between both ends of each thermoelectric element when used, it is desirable that the n-type and p-type thermoelectric elements constituting the thermoelectric conversion module have approximately the same thermal expansion coefficient. To achieve this, for example, the n-type and p-type thermoelectric elements may be made of the same type of thermoelectric material.
[0005] Meanwhile, magnesium silicide (Mg2Si)-based thermoelectric materials have been known for some time, in which the thermoelectric properties have been improved by incorporating various dopants into magnesium silicide (Mg2Si), and thermoelectric elements using Mg2Si-based thermoelectric materials are known to have relatively high thermoelectric performance (power generation performance).
[0006] However, while most conventional Mg2Si-based thermoelectric elements are n-type (having a negative Seebeck coefficient), there are few p-type elements (having a positive Seebeck coefficient), and in particular, no p-type elements with excellent thermal stability in air are known.
[0007] Incidentally, JP 2011-29632 A discloses a magnesium-silicon composite material that has a dimensionless figure of merit of 0.665 or more at 866 K and that is substantially free of dopant, and a magnesium-silicon composite material that contains 0.10 to 2.00 at% of a dopant in terms of atomic weight ratio, and describes that when Sb is contained as a dopant, a thermoelectric conversion material with excellent durability at high temperatures can be obtained. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2011-29632 A Summary of the Invention [Problem to be solved by the invention]
[0009] An object of the present invention is to provide an Mg2Si-based thermoelectric element having p-type thermoelectric properties (positive Seebeck coefficient) and high thermal stability, and a method for producing the same. [Means for solving the problem]
[0010] The thermoelectric element according to the present invention is a thermoelectric element made of magnesium silicide, contains lithium as a dopant, and is characterized by having a recrystallized region and a normal sintered region.
[0011] In this case, the recrystallized region may exhibit n-type thermoelectric properties, and the normally sintered region may exhibit p-type thermoelectric properties.
[0012] In the above case, the recrystallized region and the normal sintered region may be disposed adjacent to each other.
[0013] In the above case, the recrystallized region may be disposed on one end side, and the normal sintered region may be disposed on the other end side.
[0014] In the above case, the end portion on the recrystallized region side may be the low temperature end, and the end portion on the normal sintered region side may be the high temperature end.
[0015] In the above case, the thermoelectric element may have a columnar (for example, rectangular parallelepiped) shape.
[0016] The method for manufacturing a thermoelectric element according to the present invention includes a step of preparing an Mg2Si-based thermoelectric material containing lithium as a dopant, and a step of sintering the Mg2Si-based thermoelectric material, and is characterized in that in the sintering step, an insulating layer is provided around the Mg2Si-based thermoelectric material before sintering, and sintering is performed in a state in which the insulating layer is provided around the Mg2Si-based thermoelectric material.
[0017] In this case, the insulating layer may be made of boron nitride.
[0018] In the above cases, the method may further include a processing step of processing the sintered body obtained in the sintering step, and in the processing step, a thermoelectric element may be cut out so as to include both the recrystallized region and the normal sintered region of the sintered body.
[0019] In the above case, the step of preparing the Mg2Si-based thermoelectric material may include a lithium addition step of adding lithium as a dopant to raw materials used in the synthesis of the Mg2Si-based thermoelectric material, and a synthesis step of synthesizing the Mg2Si-based thermoelectric material by heat treating the raw materials to which lithium has been added in the lithium addition step.
[0020] In this case, the raw materials may be magnesium and silicon.
[0021] In the above case, the method may further include a molding step of pressure-molding raw materials used in the synthesis of the Mg2Si-based thermoelectric material, and the synthesis step may include heat-treating the synthesis greenbody formed in the molding step to synthesize the Mg2Si-based thermoelectric material.
[0022] In the above cases, a lithium compound (for example, lithium carbonate or lithium acetate) may be used as a lithium source for the dopant.
[0023] In the above case, the sintering step may be performed by pressure sintering using a spark plasma sintering method. Effect of the Invention
[0024] According to the present invention, it is possible to provide a thermoelectric element having p-type thermoelectric properties (positive Seebeck coefficient) and high thermal stability. [Brief description of the drawings]
[0025] [Figure 1] 4A to 4C are diagrams illustrating a method for manufacturing a thermoelectric element according to the present invention. [Diagram 2] FIG. 2 is a cross-sectional view for explaining the configuration of a sintering jig used in a sintering step. [Diagram 3] 3A to 3C are diagrams for explaining the structure of a sintered body obtained by a sintering step. [Figure 4] 1A to 1C are diagrams for explaining a processing method in a processing step. [Diagram 5] 1 is a photograph (a photograph substituting a drawing) of the sintered body of Example 1. [Figure 6] 1 is a table showing the evaluation results of each thermoelectric element. [Figure 7] 1 is a table showing the evaluation results of the thermal durability of each thermoelectric element. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings.
[0027] The method for manufacturing a thermoelectric element according to the present invention is for manufacturing a Mg2Si-based thermoelectric element, and uses lithium (Li) as a dopant.
[0028] 1 is a diagram for explaining a method for manufacturing a thermoelectric element according to the present invention. In this embodiment, lithium is added as a dopant in the first weighing step. In this embodiment, lithium carbonate (Li2CO3), which is chemically stable and easy to handle compared to pure lithium, which is chemically active, is used as a lithium source for the dopant.
[0029] As shown in the figure, first, the raw materials are weighed (S1). For example, magnesium (Mg) powder and silicon (Si) powder as the main raw materials, and lithium carbonate (Li2CO3) powder as the lithium source of the dopant are weighed.
[0030] Next, the raw material powders are mixed so that the raw material powders weighed in the weighing step S1 become uniform (S2). For example, the raw material powders are mixed using a mixer or the like.
[0031] Next, the raw material powders uniformly mixed in the mixing step S2 are pressure-molded to produce a green body for synthesis (S3). For example, the green body for synthesis is produced by cold uniaxial pressing at an appropriate surface pressure (for example, about 12 MPa).
[0032] Next, the synthetic green body produced in the molding step S3 is subjected to a heat treatment to synthesize an Mg2Si-based thermoelectric material (S4). For example, the synthetic green body is placed in a semi-closeable container (e.g., a carbon container), and then placed in an electric furnace and kept at a temperature of 650°C to 800°C (e.g., 700°C) in an argon (Ar) atmosphere for about 1 to 4 hours to synthesize an Mg2Si-based thermoelectric material.
[0033] Next, the Mg2Si-based thermoelectric material synthesized in the synthesis step S4 is pulverized (S5) into a desired particle size (for example, 38 μm or less) using, for example, an automatic mortar or a ball mill.
[0034] Next, the Mg2Si-based thermoelectric material pulverized in the pulverization step S5 is sintered (S6). In this embodiment, pressure sintering is performed by spark plasma sintering (SPS). Furthermore, in this embodiment, a specific sintering method is adopted in the sintering step S6, so that a part of the Mg2Si-based thermoelectric material is recrystallized during sintering, and the finally obtained sintered body includes a recrystallized region (recrystallized region) and a non-recrystallized region (normal sintered region) (see FIG. 5). The sintering method in the sintering step S6 will be described in detail later.
[0035] Next, the sintered body obtained in the sintering step S6 is processed to have a predetermined shape (S7). For example, the sintered body is cut with a cutting device such as a wire cutter so as to obtain a plurality of rectangular parallelepiped elements. In this embodiment, the sintered body is cut so that each thermoelectric element includes both a recrystallized region and a normal sintered region.
[0036] The thermoelectric element manufactured through the above steps S1 to S7 has p-type thermoelectric properties (positive Seebeck coefficient) as a whole, and has high thermal stability.
[0037] Next, the sintering method in the sintering step S6 will be described in detail.
[0038] 2 is a diagram for explaining the sintering method in the sintering step S6. More specifically, the diagram shows a cross-sectional view for explaining the configuration of a sintering jig used in the sintering step.
[0039] As shown in the figure, the sintering jig 200 includes a cylindrical carbon die 211 and a pair of cylindrical carbon punches 212, 213, and an Mg2Si-based thermoelectric material 201 is filled in a cylindrical space formed by the cylindrical die 211 and the cylindrical punches 212, 213 inserted from above and below into the through holes of the die 211.
[0040] As shown in the figure, the sintering jig 200 includes a cylindrical carbon paper 221 arranged along the inner peripheral surface of the die 211, and disk-shaped carbon papers 222, 223 arranged between each punch 212, 213 and the Mg2Si-based thermoelectric material 201.
[0041] The carbon papers 221-223 are intended to prevent the Mg2Si-based thermoelectric material 201 from adhering to the die 211 and the punches 212, 213. Each of the carbon papers 221-223 is produced, for example, by cutting a sheet of carbon paper into a predetermined shape.
[0042] Furthermore, as shown in the figure, BN coating layers 231-233 are formed on the inside of the cylindrical carbon paper 221 (the side in contact with the punches 212, 213 and the Mg2Si-based thermoelectric material 201) and on the outside of the disk-shaped carbon papers 222, 223 (the side in contact with the punches 212, 213).
[0043] The BN coated layers 231-233 are insulating layers for electrically insulating the die 211 and punches 212, 213 from the Mg2Si-based thermoelectric material 201, and in this embodiment, are formed by applying boron nitride to each of the carbon papers 221-223. The BN coated layers 231-233 are formed to have a certain thickness (for example, a thickness of 100 μm or more) so as to obtain a certain level of electrical insulation. The size of the recrystallized region changes depending on the thickness of the BN coated layers 231-233. For example, increasing the thickness of the BN coated layers 231-233 results in an expansion of the recrystallized region.
[0044] Next, a preparation procedure for the sintering jig 200 shown in FIG. 2 will be described.
[0045] First, BN coating layers 231-233 are formed on one side of the carbon paper constituting the cylindrical carbon paper 221 and the disk-shaped carbon papers 222 and 223. The BN coating layers 231-233 are formed, for example, by applying a BN spray (manufactured by Fine Chemical Japan Co., Ltd.) to one side of the carbon paper.
[0046] Next, the carbon paper constituting the cylindrical carbon paper 221 is placed in the die 211 so that the surface on which the BN coating layer 231 is formed faces inward (toward the punches 212 and 213), and then the lower punch 213 is inserted.
[0047] Next, the carbon paper constituting the lower circular carbon paper 223 is placed on the lower punch 213 so that the surface on which the BN coating layer 233 is formed is on the outer side (the punch 213 side), and then the Mg2Si-based thermoelectric material 201 is filled in.
[0048] Next, the carbon paper constituting the upper circular carbon paper 222 is placed on the Mg2Si-based thermoelectric material 201 so that the surface on which the BN coating layer 232 is formed is on the outer side (the punch 212 side), and then the upper punch 212 is inserted.
[0049] In this manner, preparation of the sintering jig 200 to be used in the sintering step S6 is completed.
[0050] Using a sintering jig having the above-mentioned configuration, a BN coating layer (insulating layer) is provided around the Mg2Si-based thermoelectric material, and then pressure sintering is performed by spark plasma sintering (SPS), resulting in a sintered body having a partial recrystallized region (recrystallized region).
[0051] 3A to 3C are diagrams for explaining the configuration of the sintered body obtained in the sintering step S6, in which (a) shows a plan view, (b) shows a front view, and (c) shows a bottom view.
[0052] In the example shown in the figure, the sintered body 300 has a short cylindrical shape and is composed of a recrystallized region 310 and a normal sintered region 320. In the figure (and FIG. 4), the recrystallized region 310 is hatched (with parallel oblique lines).
[0053] The recrystallized region 310 is a region formed by recrystallization of the Mg2Si-based thermoelectric material during sintering, and is a region exhibiting n-type thermoelectric properties, and in this embodiment, as shown in the figure, is formed in the center part of the sintered body 300. The recrystallized region 310 has a cylindrical shape with a smaller diameter than the sintered body 300, and is formed continuously from the top surface to the bottom surface of the sintered body 300.
[0054] The normal sintered region 320 is a region formed by normal sintering of the Mg2Si-based thermoelectric material during sintering, and is a region exhibiting p-type thermoelectric characteristics. In this embodiment, as shown in the figure, it is formed around the recrystallized region 310.
[0055] The sintered body having the above-mentioned configuration is cut appropriately in processing step S7 and used as a thermoelectric element. In this embodiment, the sintered body is cut so that each thermoelectric element includes both the recrystallized region 310 and the normal sintered region 320.
[0056] Next, the processing method in processing step S7 will be described in detail.
[0057] FIG. 4 is a diagram for explaining the processing method in processing step S7.
[0058] Fig. 4(a) shows a plan view of the sintered body 400, with the cut portions indicated by two-dot chain lines. Fig. 4(a) also shows the dimensions of the cut portions used in the examples described below. Fig. 4(b) to (e) show the shapes of the thermoelectric elements obtained by cutting at the cut portions shown in Fig. 4(a), with Fig. 4(b) showing a front view, Fig. 4(c) showing a right side view, Fig. 4(d) showing a rear view, and Fig. 4(e) showing a bottom view.
[0059] In the example shown in the same figure, multiple (specifically, four) thermoelectric elements having the same shape are cut out from one sintered body 400, and each thermoelectric element 430 is cut out to have a columnar (specifically, rectangular) shape.
[0060] Furthermore, in the example shown in the figure, each thermoelectric element 430 is cut out so that the recrystallized region 410 and the normal sintered region 420 have approximately the same size, that is, the size ratio (volume ratio) of the two regions is approximately 1:1.
[0061] By carrying out the above-mentioned processing in processing step S7, a thermoelectric element 430 including both the recrystallized region 410 and the normal sintered region 420 is obtained.
[0062] As shown in (b) to (d) of the same figure, in each processed thermoelectric element 430, the recrystallized region 410 is arranged on one end side (lower side in the same figure), and the normal sintered region 420 is arranged on the other end side (upper side in the same figure). In other words, the recrystallized region 410 and the normal sintered region 420 are arranged side by side adjacent to each other from one end to the other end.
[0063] As described above, the recrystallized region 410 exhibits n-type thermoelectric properties, and the normal sintered region 420 exhibits p-type thermoelectric properties. The thermoelectric element 430 includes the recrystallized region 410 exhibiting n-type thermoelectric properties and the normal sintered region 432 exhibiting p-type thermoelectric properties, so that the element as a whole exhibits p-type thermoelectric properties and has high thermal stability.
[0064] When the thermoelectric element 430 having the above configuration is used for thermoelectric power generation, the end 431 on the recrystallized region 410 side is usually used as the low temperature end and the end 432 on the normal sintered region 420 side is used as the high temperature end so as to obtain higher thermoelectric performance as a p-type thermoelectric element. By using the end 431 on the recrystallized region 410 side as the low temperature end and the end 432 on the normal sintered region 420 side as the high temperature end, it becomes possible to relatively suppress the influence of the recrystallized region 410 which exhibits n-type thermoelectric properties.
[0065] Although the embodiments of the present invention have been described above, it is to be understood that the embodiments of the present invention are not limited to the above. For example, in the above-mentioned embodiment, lithium carbonate is used as the lithium source of the dopant, but it is also possible to use pure lithium or other lithium compounds (e.g., lithium acetate (C2H3LiO2)) as the lithium source of the dopant.
[0066] In addition, in the above-described embodiment, lithium is added as a dopant in the initial weighing step, but it may be added at another timing (for example, between the grinding step and the sintering step).
[0067] Furthermore, in the above-described embodiment, the sintered body is cut (cut into elements) so that the recrystallized region and the normal sintered region have approximately the same size (volume), but it is also conceivable to cut the sintered body (cut into elements) so that the recrystallized region and the normal sintered region have different sizes (volumes). EXAMPLES
[0068] Next, examples of the thermoelectric element and the manufacturing method thereof according to the present invention will be described.
[0069] First, a number of types of thermoelectric elements made of magnesium silicide doped with lithium as a dopant element were produced by changing the amount of lithium added and the type of lithium compound serving as the lithium source, as described below.
[0070] Example 1 First, the stoichiometric ratio is Mg 1.96 Si1Li 0.04 Magnesium (Mg) powder (manufactured by High Purity Chemical Laboratory Co., Ltd.) with a purity of 99.5% and a particle size of 180 μm, silicon (Si) powder (manufactured by High Purity Chemical Laboratory Co., Ltd.) with a purity of 99.9% and a particle size of 150 μm, and lithium carbonate (Li2CO3) powder (99% purity, 300 μm particle size lithium carbonate powder (manufactured by High Purity Chemical Laboratory Co., Ltd.) that was previously crushed) with a purity of 99% and a particle size of approximately 10 μm were weighed out so that the above values were obtained.
[0071] Next, the raw material powders were mixed in a mortar until they were uniform. The raw material powders were then placed in a 30φ super steel die and pressed at a pressure of 12 MPa using a press (NT-50H, manufactured by NPA Systems Co., Ltd.) to obtain a cylindrical synthetic compact measuring 30φ x 10 mm.
[0072] Next, the obtained synthetic green body was placed in a semi-closeable carbon container with a lid, then placed in an electric furnace and heat-treated at 700°C for 1 hour in an argon atmosphere to obtain granules of Mg2Si-based thermoelectric material.
[0073] Next, the obtained aggregates were coarsely crushed in a mortar to a size of 1 mm or less, and then finely crushed in an automatic mortar to a particle size of 38 μm or less.
[0074] Next, the obtained Mg2Si-based thermoelectric material powder was filled in a sintering jig as shown in FIG. 2. More specifically, first, a carbon sheet (manufactured by NJS Co., Ltd.) having a thickness of 0.2 mm was cut into a predetermined shape to prepare carbon paper constituting the cylindrical carbon paper 221 and the disk-shaped carbon papers 222 and 223. Next, BN spray (manufactured by Fine Chemical Japan Co., Ltd.) was applied to one side of the carbon paper constituting the cylindrical carbon paper 221 and the disk-shaped carbon papers 222 and 223 to form BN coating layers 231 to 233 having a thickness of about 100 μm. Next, the carbon paper constituting the cylindrical carbon paper 221 was placed in a 30φ carbon die 211 so that the surface on which the BN coating layer 231 was formed was facing inward, and then the lower carbon punch 213 was inserted. Next, the carbon paper constituting the lower circular carbon paper 223 was placed on the lower carbon punch 213 so that the surface on which the BN coating layer 233 was formed was facing outward (lower), and then filled with the Mg2Si-based thermoelectric material powder 201. Next, the carbon paper constituting the upper circular carbon paper 222 was placed on the Mg2Si-based thermoelectric material 201 so that the surface on which the BN coating layer 232 was formed was facing outward (upper), and then the upper carbon punch 212 was inserted.
[0075] The sintering tool prepared as described above was placed in a spark plasma sintering apparatus (LABOX-1575, manufactured by Sinterland Co., Ltd.) and sintering was performed under conditions of a sintering temperature of 850°C, a sintering time of 5 minutes, and a vacuum degree of 6 Pa, obtaining a sintered body (30φ, height 3 mm).
[0076] Fig. 5 shows a photograph of the obtained sintered body. As shown in the figure, the central part exhibits a recrystallized pattern. Note that in Examples 2 to 4 described later, similar recrystallized patterns were also observed in the central part. On the other hand, in Comparative Examples 1 to 5 described later, no recrystallized patterns were observed.
[0077] Next, the obtained sintered body was cut using a micro cutter (MC-201N, manufactured by Maruto Co., Ltd.) to cut out rectangular sintered body pieces of 6 mm x 2 mm x 3 mm from the recrystallized region near the center and the normal sintered region near the periphery. That is, a sintered body piece consisting of only the recrystallized region and a sintered body piece consisting of only the normal sintered region were obtained.
[0078] XRD analysis was performed on each sintered piece using an X-ray diffractometer (MiniFlex, manufactured by Rigaku Corporation). The X-ray diffraction pattern of the sintered piece consisting only of recrystallized regions showed missing diffraction lines compared to the X-ray diffraction pattern of the sintered piece consisting only of normally sintered regions, and it was confirmed that the crystal orientation of the recrystallized regions was more aligned than that of the normally sintered regions.
[0079] Next, the thermoelectric properties of each sintered piece were measured. First, the temperature difference between both ends of each sintered piece and the output voltage were measured while heating one end of each sintered piece with a heater, and the Seebeck coefficient was calculated based on the measurement results. In addition, the resistivity was measured by the four-probe method.
[0080] As a result, the Seebeck coefficient and resistivity of the sintered piece consisting only of the recrystallized region were -50μV / K and 70μΩm, respectively. On the other hand, the Seebeck coefficient and resistivity of the sintered piece consisting only of the normal sintered region were 290μV / K and 195μΩm, respectively. In other words, it was confirmed that the recrystallized region exhibits n-type thermoelectric properties, while the normal sintered region exhibits p-type thermoelectric properties. Furthermore, when comparing the absolute values of the Seebeck coefficients of both, the normal sintered region, which exhibits p-type thermoelectric properties, is sufficiently larger, more than five times, compared to the recrystallized region, which exhibits n-type thermoelectric properties.
[0081] Next, a sintered body was prepared again using the method described above, and the prepared sintered body (30φ, height 3 mm) was cut using the microcutter described above as shown in Figure 4 to cut out rectangular sintered body pieces measuring 10 mm x 5 mm x 3 mm to form the final thermoelectric element.
[0082] Example 2 First, the stoichiometric ratio is Mg 1.98 Si1Li 0.02 The magnesium (Mg) powder, the silicon (Si) powder, and the lithium carbonate (Li2CO3) powder were weighed out so that the following weight ratios were obtained:
[0083] Thereafter, a thermoelectric element was produced in the same manner as in Example 1 described above.
[0084] Example 3 First, the stoichiometric ratio is Mg 1.99 Si1Li 0.01 The magnesium (Mg) powder, the silicon (Si) powder, and the lithium carbonate (Li2CO3) powder were weighed out so that the following weight ratios were obtained:
[0085] Thereafter, a thermoelectric element was produced in the same manner as in Example 1 described above.
[0086] Example 4 First, the stoichiometric ratio is Mg 1.99 Si1Li 0.01 The magnesium (Mg) powder, the silicon (Si) powder, and lithium acetate (C2H3LiO2) powder with a purity of 99.5% and a particle size of about 10 μm (lithium acetate powder (manufactured by Kanto Chemical Co., Ltd.) with a purity of 99.5% and a particle size of 180 μm that was previously crushed) were weighed so that the weight ratio was 1:1.
[0087] Thereafter, a thermoelectric element was produced in the same manner as in Example 1 described above.
[0088] Furthermore, a plurality of types of thermoelectric elements were produced using a sintering tool different from that used in the above Examples 1 to 4, as described below.
[0089] Comparative Example 1 A thermoelectric element was produced in the same manner as in Example 1 described above, except that in preparing the sintering jig, cylindrical carbon paper 221 and disk-shaped carbon papers 222, 223 that had not been sprayed with BN were used, i.e., the sintering process was carried out using a sintering jig on which BN coating layers 231-233 (insulating layers) were not formed.
[0090] Comparative Example 2 A thermoelectric element was produced in the same manner as in Example 2 described above, except that in preparing the sintering jig, cylindrical carbon paper 221 and disk-shaped carbon papers 222, 223 that had not been sprayed with BN were used, i.e., the sintering process was carried out using a sintering jig on which BN coating layers 231-233 (insulating layers) were not formed.
[0091] Comparative Example 3 A thermoelectric element was produced in the same manner as in Example 3 described above, except that in preparing the sintering jig, cylindrical carbon paper 221 and disk-shaped carbon papers 222, 223 that had not been sprayed with BN were used, i.e., the sintering process was carried out using a sintering jig on which BN coating layers 231-233 (insulating layers) were not formed.
[0092] Comparative Example 4 A thermoelectric element was produced in the same manner as in Example 4 described above, except that in preparing the sintering jig, cylindrical carbon paper 221 and disk-shaped carbon papers 222, 223 that had not been sprayed with BN were used, i.e., the sintering process was carried out using a sintering jig on which BN coating layers 231-233 (insulating layers) were not formed.
[0093] Moreover, a thermoelectric element made of magnesium silicide not containing added lithium was produced as follows, using a sintering tool on which the BN coating layers 231-233 (insulating layers) were not formed, as in Comparative Examples 1-4 above.
[0094] Comparative Example 5 First, the magnesium (Mg) powder (manufactured by Kojundo Chemical Laboratory Co., Ltd.) and the silicon (Si) powder were weighed out so that the stoichiometric ratio was Mg2Si1.
[0095] Thereafter, a thermoelectric element was produced in the same manner as in Comparative Example 1 described above.
[0096] Next, each thermoelectric element was evaluated as follows.
[0097] First, while one end (outer circumference side) of each thermoelectric element was heated by a heater, the temperature difference between both ends of each thermoelectric element and the output voltage were measured, and the Seebeck coefficient was calculated based on the measurement results. In addition, the resistivity was measured by the four-probe method. Furthermore, the power factor was calculated based on the obtained Seebeck coefficient and resistivity.
[0098] Figure 6 is a table showing the evaluation results of each thermoelectric element. In the figure, α is the Seebeck coefficient (unit: μV / K), ρ is the resistivity (unit: μΩm), and PF is the power factor (unit: μW / mK 2 )
[0099] First, when focusing on the Seebeck coefficient α, as shown in the figure, all of Examples 1 to 4 and Comparative Examples 1 to 4 have positive values, indicating that they are p-type thermoelectric elements (p-type semiconductor elements). On the other hand, Comparative Example 5 has a negative value, indicating that it is an n-type thermoelectric element (n-type semiconductor element).
[0100] As for the resistivity ρ, when Examples 1 to 4 are compared with Comparative Examples 1 to 4 (when comparing the same amount of lithium added and the same lithium source, such as Example 1 and Comparative Example 1, Example 2 and Comparative Example 2, etc.), Examples 1 to 4 have lower resistivity. That is, the resistivity is lower when the sintering jig on which the BN coating layers 231 to 233 (insulating layers) are formed is used.
[0101] Moreover, when focusing on the power factor PF, as shown in the figure, the largest power factor is obtained in Example 1. Comparing Example 1 and Comparative Example 1, the Seebeck coefficients of both are approximately the same, but the resistivity of Example 1 is much smaller (1 / 10 or less) than that of Comparative Example 1, and as a result, a much larger power factor (10 times or more) is obtained compared to Comparative Example 1.
[0102] Furthermore, for Examples 1 to 4 and Comparative Examples 1 to 4, the thermal durability was evaluated as follows.
[0103] First, each thermoelectric element was placed in an electric furnace and heat-treated in air at a temperature of 350° C. for a certain period of time (24 hours and 48 hours). After that, it was naturally cooled to room temperature, and then the Seebeck coefficient was calculated, the resistivity was measured, and the power factor was calculated in the same manner as described above.
[0104] Figure 7 is a table showing the evaluation results of the thermal durability of each thermoelectric element. In the figure, α is the Seebeck coefficient (unit: μV / K), ρ is the resistivity (unit: μΩm), and PF is the power factor (unit: μW / mK 2 )
[0105] As shown in the figure, in all of Examples 1 to 4, even when heat-treated in air at 350°C for 48 hours, the Seebeck coefficient and resistivity did not change significantly, and it was confirmed that the samples had stable p-type thermoelectric properties. On the other hand, in all of Comparative Examples 1 to 4, the Seebeck coefficient did not change significantly, but the resistivity increased as the heat treatment time increased. As a result, when Examples 1 to 4 and Comparative Examples 1 to 4 are compared, the power factors after 48 hours of heat treatment are lower in Comparative Examples 1 to 4.
[0106] In Examples 1 to 4, the recrystallized region was formed because the temperature of the Mg2Si-based thermoelectric material during sintering was higher when pressure sintering was performed by the spark plasma sintering method with a BN coating layer (insulating layer) provided around the Mg2Si-based thermoelectric material than when pressure sintering was performed by the normal spark plasma sintering method (without an insulating layer), and as a result, part of the Mg2Si-based thermoelectric material was melted. It has been confirmed that when the thickness of the BN coating layer is increased, the recrystallized region expands toward the outer periphery and the normal sintered region shrinks.
[0107] In addition, when evaluating each thermoelectric element, the end on the outer periphery of each thermoelectric element, i.e., the end on the normal sintering region side in the case of Examples 1 to 4, was heated by a heater, in order to obtain a larger temperature difference in the normal sintering region that exhibits p-type thermoelectric properties. Note that, for Examples 1 to 4, evaluation was also performed when the end on the recrystallized region side of each thermoelectric element was heated, and by comparing the two, it was confirmed that a relatively higher thermoelectric performance (power factor) was obtained when the end on the normal sintering region side was the high temperature end (the end on the recrystallized region side was the low temperature end) compared to when the end on the recrystallized region side was the high temperature end (the end on the normal sintering region side was the low temperature end). [Explanation of symbols]
[0108] S1 Weighing process S2 mixing process S3 Molding process S4 Synthesis process S5 Crushing process S6 Sintering process S7 Processing process 200 Sintering fixture 201 Mg2Si thermoelectric materials 211 Dice 212,213 punch 221 Cylindrical carbon paper 222,223 Carbon paper disc 231~233 BN coating layer 300 Sintered body 310 Recrystallization region 320 Normal sintering area 400 Sintered body 410 Recrystallization region 420 Normal sintering area 430 Thermoelectric elements 431,432 End
Claims
1. A thermoelectric element made of magnesium silicide, It contains lithium as a dopant. Recrystallized region and normal sintered region Equipped with The recrystallized region exhibits n-type thermoelectric properties, The normally sintered region exhibits p-type thermoelectric properties. A thermoelectric element characterized by:
2. The recrystallized region and the normal sintered region are disposed adjacent to each other.
2. The thermoelectric element according to claim 1 .
3. The recrystallized region is located at one end and the normal sintered region is located at the other end.
3. A thermoelectric element according to claim 1 or 2.
4. The end on the recrystallized region side becomes the low temperature end, The end on the normal sintering region side becomes the high temperature end.
4. The thermoelectric element according to claim 1, wherein the thermoelectric element is a thermoelectric element having a thickness of 100 nm or less.
5. The thermoelectric element has a columnar shape.
5. The thermoelectric element according to claim 1, wherein the thermoelectric element is a thermoelectric element.
6. A method for producing a thermoelectric element according to any one of claims 1 to 5, comprising the steps of: Mg containing lithium as a dopant 2 preparing a Si-based thermoelectric material; The Mg 2 a sintering step of sintering the Si-based thermoelectric material; Equipped with In the sintering step, before sintering, the Mg 2 An insulating layer is provided around the Si-based thermoelectric material, and the Mg 2 Sintering is performed with the insulating layer provided around the Si-based thermoelectric material. A method for manufacturing a thermoelectric element comprising the steps of:
7. The insulating layer is made of boron nitride. The method for manufacturing a thermoelectric element according to claim 6 .
8. The method further includes a processing step of processing the sintered body obtained in the sintering step, and in the processing step, a thermoelectric element is cut out so as to include both the recrystallized region and the normal sintered region of the sintered body. The method for manufacturing a thermoelectric element according to claim 6 or 7.
9. The Mg 2 The step of preparing a Si-based thermoelectric material includes: Mg 2 A lithium doping step of adding lithium as a dopant to raw materials used in the synthesis of a Si-based thermoelectric material; The raw material to which lithium has been added in the lithium addition step is subjected to heat treatment to obtain Mg 2 A synthesis step of synthesizing a Si-based thermoelectric material; The method for manufacturing a thermoelectric element according to any one of claims 6 to 8, comprising:
10. The raw materials are magnesium and silicon. The method for manufacturing a thermoelectric element according to claim 9 .
11. The Mg 2 The method further includes a molding step of pressure-molding raw materials used in the synthesis of the Si-based thermoelectric material, The synthesis step is a step of heat-treating the synthetic green body formed in the molding step to obtain Mg 2 Synthesizing Si-based thermoelectric materials The method for manufacturing a thermoelectric element according to claim 9 or 10.
12. Use of lithium compounds as lithium sources for dopants The method for manufacturing a thermoelectric element according to any one of claims 6 to 11.
13. In the sintering step, pressure sintering is performed by a spark plasma sintering method. The method for manufacturing a thermoelectric element according to any one of claims 6 to 12.
Citation Information
Patent Citations
Magnesium-silicon composite material and process for producing same, and thermoelectric conversion material, thermoelectric conversion element and thermoelectric conversion module each comprising or including the composite material
JP2011029632A
Method of manufacturing magnesium-based thermoelectric conversion material, method of manufacturing magnesium-based thermoelectric conversion element, magnesium-based thermoelectric conversion material, magnesium-based thermoelectric conversion element, and thermoelectric converter
JP2017152691A
Thermoelectric conversion material, thermoelectric conversion module, and method of manufacturing thermoelectric conversion material
JP2019012828A
Magnesium-based thermoelectric conversion material, magnesium-based thermoelectric conversion element, and, manufacturing method of magnesium-based thermoelectric conversion material
JP2019036623A
Thermoelectric conversion device and method for manufacturing the same
WO2019170826A1