Pleated molded body, dust collector filter and high volume pulse jet type dust collector

The use of spunbond nonwoven fabric with specific curvature and thickness ratios in pleated filters addresses shape retention and air permeability issues, ensuring durable and efficient dust removal under high airflow conditions.

JP7593099B2Active Publication Date: 2024-12-03TORAY INDUSTRIES INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020213302
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-23
Filing Date
2020-12-23
Publication Date
2024-12-03
Estimated Expiration
2040-12-23

AI Technical Summary

Technical Problem

Existing pleated filters face challenges in maintaining shape retention and air permeability due to issues with partial thermocompression bonding and fusion between fibers, leading to decreased durability and increased pressure loss under high airflow conditions.

Method used

A pleated molded body composed of spunbond nonwoven fabric with specific ratios of radius of curvature and thickness, using thermoplastic continuous filaments with high and low melting point components, partially fused to achieve optimal shape retention, air permeability, and dust removal properties.

Benefits of technology

The solution results in a pleated molded body with excellent shape recovery and air permeability, capable of withstanding high airflow and repeated backwashing, maintaining effective dust removal performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593099000004
    Figure 0007593099000004
  • Figure 0007593099000005
    Figure 0007593099000005
  • Figure 0007593099000006
    Figure 0007593099000006
Patent Text Reader

Abstract

To provide a pleat molded article excellent in durability, especially shape retention property and shape-restoring property and also excellent in air permeability and dust removing property.SOLUTION: There is provided a pleat molded article comprising a spun-bonded nonwoven fabric. The spun-bonded nonwoven fabric is composed of a thermoplastic continuous filament comprising a high melting point component and a low melting point component and is formed by partially fusing the thermoplastic continuous filament and satisfies the following formulae (1) and (2). 0.25≤r1 / t≤0.50 ...(1), 0.90≤r2 / r1≤1.00 ...(2). In the formulae, r1 is a radius of curvature (μm) of one apex of the pleat molded article; r2 is a radius of curvature (μm) of the other apex of the pleat molded article; t is a thickness (μm) of the pleat molded article; provided that r1≥r2 is satisfied.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pleated article made of a spunbonded nonwoven fabric, and to a dust collector filter and a large volume pulse jet type dust collector using the pleated article. [Background technology]

[0002] Conventionally, dust collectors have been used to remove and collect dust in working environments where dust is generated. It is known that the filters of these dust collectors are used in a pleated shape, and pleating makes it possible to greatly increase the filtration area, reduce pressure loss, and increase collection efficiency.

[0003] Incidentally, in the pleated filters of such dust collectors, when a certain pressure loss is reached, compressed air or the like is sprayed from the inside to knock off dust adhering to the surface of the filter material, a so-called backwashing is common. In particular, as the process of "dust collection-dust knocking off with backflow air" is repeated, the pleated filter is bent many times at the pleat apexes by the air pressure, so the pleated filter, which is a pleated body, is required to have two properties: the property of retaining a shape with alternating predetermined pleat apexes in succession (hereinafter simply referred to as shape retention), and the property of returning to the original predetermined shape from deformation during backwashing, etc. (hereinafter simply referred to as shape recovery).

[0004] As a nonwoven fabric substrate having durability, for example, Patent Document 1 discloses a nonwoven fabric in which thermoplastic continuous filaments are partially thermocompressed and integrated. Patent Document 2 discloses a nonwoven fabric for filters, which is a spunbonded nonwoven fabric composed of composite fibers composed of a high melting point polymer and a low melting point polymer, and is partially thermocompressed, and the fibers in the surface layer of the nonwoven fabric are fused to each other by melting or softening the low melting point polymer. Patent Document 3 discloses a nonwoven fabric in which a thermoplastic continuous filament of a high melting point component and a thermoplastic continuous filament of a low melting point component are mixed, and a nonwoven fabric made of a multilobal composite fiber composed of a high melting point component and a low melting point component. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 5422874 [Patent Document 2] Patent No. 5298803 [Patent Document 3] Patent No. 4522671 Summary of the Invention [Problem to be solved by the invention]

[0006] As a manufacturing method for pleated bodies used in pleated filters, a reciprocating method is generally adopted in which a base material is repeatedly folded and heat-pressed to process it. However, when a partial heat-pressed portion is provided as disclosed in Patent Documents 1 and 2 in an attempt to improve durability, it is difficult to achieve both breathability and pleat shape retention when the pleated body is used as a pleated filter. On the other hand, in the technology disclosed in Patent Document 3, the fusion between fibers is weak, and the fusion portion breaks during pleating, resulting in a decrease in rigidity of the nonwoven fabric and the generation of fluff. When used as a pleated filter, the pleat shape cannot be maintained under high airflow, and there are problems such as a decrease in breathability and the loss of fluff.

[0007] The present invention has been made in consideration of the above circumstances, and its object is to provide a pleated body which has excellent durability, particularly shape retention and shape recovery properties, and which also has excellent breathability and dust-removal properties. [Means for solving the problem]

[0008] As a result of intensive research into achieving the above-mentioned object, the inventors have discovered that by setting the ratio of the radius of curvature (r1) of one pleat apex of a pleated body divided by the thickness (t) of the pleated body and the radius of curvature (r1) of one pleat apex to the radius of curvature (r2) of the other pleat apex within a specific range, the pleated body will have excellent shape retention and shape recovery properties, as well as excellent breathability and dust removal properties when used as a pleated filter.

[0009] The present invention has been completed based on these findings, and provides the following inventions.

[0010] The pleated body of the present invention is a pleated body made of a spunbonded nonwoven fabric, the spunbonded nonwoven fabric being made of thermoplastic continuous filaments consisting of a high melting point component and a low melting point component, and being partially fused; before The pleated body is The thickness (t) of the pleated body is 500 μm or more and 1210 μm or less, Satisfy the following formulas (1) and (2) 0.25≦r1 / t≦0.50 (1) 0.90≦r2 / r1≦1.00 (2) Here, r1 is the radius of curvature (μm) of one apex of the pleated body, r2 is the radius of curvature (μm) of the other apex of the pleated body, and t is the thickness (μm) of the pleated body, provided that r1≧r2. 。 The radius of curvature (r 1 ) and the radius of curvature (r 2 ) is measured as follows: (i) Ten measurement samples each having a V-shaped cross section of 10 mm in the CD direction, including one apex or the other apex, are cut out from the pleated body. (ii) The measurement sample is fixed in an open state so that the angle of the apex (11) of the pleated body is 45°. (iii) A pleated body in which the apex of the pleats is fixed at an open angle of 45° is used as a test specimen, and observed at 100x magnification using a microscope, and an enlarged photograph is taken. (iv) An imaginary circle (13) is defined, the inner lines of the apexes of the pleated body being tangent to the lines (12a, 12b). (v) The radius (14) of the imaginary circle (13) is measured and this is regarded as the radius of curvature (μm) of the apex of the pleated body. (vi) Calculate the average value (μm) and standard deviation (μm) of the radius of curvature obtained from the measurement sample of one of the apexes, and round off to the first decimal place. (vii) Similarly, calculate the average value (μm) and standard deviation (μm) of the radius of curvature obtained from the measurement sample of the other vertex, and round off to the first decimal place. (viii) The average value obtained in (vi) is compared with the average value obtained in (vii), and the average value of the larger average value is taken as the radius of curvature (r 1 ), the average value of the smaller curvature radius is taken as the curvature radius (r 2 However, if the average value obtained in (vi) is equal to the average value obtained in (vii), the average value of the apex curvature radius of the one having the larger sum of the average value (μm) and the standard deviation (μm) is set as the radius of curvature (r 1 ) shall be stipulated.

[0011] According to a preferred embodiment of the pleated article of the present invention, the CV value of the spunbonded nonwoven fabric is 5% or less.

[0012] According to a preferred embodiment of the pleated article of the present invention, the area ratio of the fused portions of the spunbonded nonwoven fabric is 5% or more and 20% or less.

[0013] According to a preferred embodiment of the pleated article of the present invention, the average single fiber diameter of the thermoplastic continuous filaments is 12 μm or more and 26 μm or less.

[0014] The dust collector filter of the present invention is formed by using the above-mentioned pleated body.

[0015] The large volume pulse jet type dust collector of the present invention uses the above-mentioned dust collector filter. Effect of the Invention

[0016] According to the present invention, by setting the value obtained by dividing the radius of curvature of one pleat apex of a pleated body by the thickness and the ratio of the radius of curvature of one pleat apex to the radius of curvature of the other pleat apex within specific ranges, a pleated body having excellent breathability, shape retention and dust removability can be obtained. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic perspective view illustrating an example of a pleated body of the present invention. [Diagram 2] FIG. 2 is a schematic top view illustrating a method for measuring the radius of curvature (r) of the pleat apex of the pleated article of the present invention. [Diagram 3] FIG. 3 is a diagram for explaining the configuration of a test system for carrying out a pleat shape stability test according to an embodiment of the present invention. [Figure 4] FIG. 4 is a diagram for explaining a measuring unit U in a pleat shape stability test according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The pleated body of the present invention is a pleated body made of a nonwoven fabric, The nonwoven fabric is composed of thermoplastic continuous filaments consisting of a high melting point component and a low melting point component, and is partially fused, and satisfies the following formulas (1) and (2): 0.25≦r1 / t≦0.50 (1) 0.90≦r2 / r1≦1.00 (2) Here, r1 is the radius of curvature (μm) of one apex of the pleated body, r2 is the radius of curvature (μm) of the other apex of the pleated body, and t is the thickness (μm) of the pleated body, provided that r1≧r2. The components will be described in detail below, but the present invention is not limited to the scope described below as long as it does not deviate from the gist of the invention.

[0019] (Thermoplastic continuous filament) The spunbond nonwoven fabric constituting the pleated body of the present invention is composed of thermoplastic continuous filaments. As the thermoplastic resin that is the raw material of the thermoplastic continuous filaments, polyester is particularly preferably used. Polyester is a polymer having an acid component and an alcohol component as monomers. As the acid component, aromatic carboxylic acids such as phthalic acid (ortho form), isophthalic acid, and terephthalic acid, aliphatic dicarboxylic acids such as adipic acid and sebacic acid, and alicyclic dicarboxylic acids such as cyclohexane carboxylic acid can be used. As the alcohol component, ethylene glycol, diethylene glycol, polyethylene glycol, and the like can be used.

[0020] Examples of polyesters include polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polyethylene naphthalate, polylactic acid, polybutylene succinate, etc. As the polyester used as the high melting point polymer described later, PET is most preferably used because it has a high melting point, excellent heat resistance, and excellent rigidity.

[0021] In addition, additives such as crystal nucleating agents, matting agents, pigments, mildewproofing agents, antibacterial agents, flame retardants, metal oxides, aliphatic bisamides and / or aliphatic monoamides, and hydrophilic agents can be added to these polyester raw materials within the scope of the present invention. Among them, metal oxides such as titanium oxide have the effect of improving spinnability by reducing surface friction of fibers and preventing fusion between fibers, and also of improving the fusion property of nonwoven fabrics by increasing thermal conductivity during fusion molding of nonwoven fabrics with heated rolls. In addition, aliphatic bisamides such as ethylene bisstearic acid amide and / or alkyl-substituted aliphatic monoamides have the effect of increasing the releasability between the heated roll and the nonwoven fabric web, improving transportability.

[0022] Next, the thermoplastic continuous filaments constituting the spunbonded nonwoven fabric are composed of a high melting point component and a low melting point component. The thermoplastic continuous filaments are preferably composite filaments in which a polyester-based low melting point polymer, which is a low melting point component having a melting point 10°C to 140°C lower than the melting point of the polyester-based high melting point polymer, is arranged around the polyester-based high melting point polymer, which is a high melting point component. In this way, when the spunbonded nonwoven fabric is formed by fusion, the composite polyester fibers (filaments) constituting the spunbonded nonwoven fabric are firmly fused to each other, so that the spunbonded nonwoven fabric has excellent mechanical strength and can fully withstand dust processing under a high air volume.

[0023] The melting point of the polyester-based low melting point polymer in the present invention can be made 10° C. or more, more preferably 20° C. or more, and even more preferably 30° C. or more lower than the melting point of the polyester-based high melting point polymer to ensure the desired fusion properties. On the other hand, the melting point of the polyester-based low melting point polymer can be made 140° C. or less, more preferably 120° C. or less, and even more preferably 100° C. or less lower than the melting point of the polyester-based high melting point polymer to prevent a decrease in heat resistance.

[0024] The melting point of the polyester-based high melting point polymer in the present invention is preferably in the range of 200° C. or more and 320° C. or less. By setting the melting point of the polyester-based high melting point polymer to preferably 200° C. or more, more preferably 210° C. or more, and even more preferably 220° C. or more, a filter having excellent heat resistance can be obtained. On the other hand, by setting the melting point of the polyester-based high melting point polymer to preferably 320° C. or less, more preferably 300° C. or less, and even more preferably 280° C. or less, a large consumption of thermal energy for melting during the production of the nonwoven fabric and a decrease in productivity can be suppressed.

[0025] On the other hand, the melting point of the polyester-based low melting point polymer is preferably in the range of 160° C. or more and 250° C. or less. By setting the melting point of the polyester-based low melting point polymer to preferably 160° C. or more, more preferably 170° C. or more, and even more preferably 180° C. or more, the shape retention is excellent even if the pleated filter is passed through a process in which heat is applied during production, such as heat setting during pleating. On the other hand, by setting the melting point of the polyester-based low melting point polymer to preferably 250° C. or less, more preferably 240° C. or less, a filter having excellent fusion properties during nonwoven fabric production and excellent mechanical strength can be obtained.

[0026] In the present invention, the melting point of a thermoplastic resin is measured using a differential scanning calorimeter (for example, "DSC-2" model manufactured by PerkinElmer Japan Co., Ltd.) at a heating rate of 20°C / min and a measurement temperature range of 30°C to 300°C, and the temperature at which the obtained melting endothermic curve gives an extreme value is defined as the melting point of the thermoplastic resin. For resins whose melting endothermic curve does not show an extreme value in the differential scanning calorimeter, the resin is heated on a hot plate, and the temperature at which the resin melts under a microscope is defined as the melting point.

[0027] When the thermoplastic resin is polyester, examples of the combination of a polyester-based high melting point polymer and a polyester-based low melting point polymer (hereinafter, the combinations may be described in the order of polyester-based high melting point polymer / polyester-based low melting point polymer) include PET / PBT, PET / PTT, PET / polylactic acid, and PET / copolymerized PET, among which the combination of PET / copolymerized PET is preferably used because of its excellent spinnability. As the copolymerization component of the copolymerized PET, isophthalic acid copolymerized PET is preferably used because of its excellent spinnability.

[0028] The composite filament may have a composite form, for example, a concentric sheath-core type, an eccentric sheath-core type, or an island-in-the-sea type, among which the concentric sheath-core type is preferred because it can fuse the filaments uniformly and firmly. The cross-sectional shape of the composite filament may be a circular cross-section, a flat cross-section, a polygonal cross-section, a multi-lobal cross-section, a hollow cross-section, or the like. Among these, a preferred embodiment is one in which the filament has a circular cross-sectional shape.

[0029] Incidentally, the form of the above-mentioned composite filament can be, for example, a method of blending fibers made of a polyester-based high melting point polymer with fibers made of a polyester-based low melting point polymer, but in the case of blending, uniform fusion is difficult, and for example, fusion is weak in a portion where the fibers made of the polyester-based high melting point polymer are densely packed, resulting in poor mechanical strength and rigidity, and thus unsuitable for a spunbonded nonwoven fabric. On the other hand, there is also a method of applying a low melting point polymer to fibers made of a polyester-based high melting point polymer by immersion or spraying, but in either case, it is difficult to apply the low melting point polymer uniformly on the surface layer or in the thickness direction, and the mechanical strength and rigidity are poor, making the nonwoven fabric unsuitable for a spunbonded nonwoven fabric.

[0030] The content ratio of the polyester-based high melting point polymer and the polyester-based low melting point polymer in the thermoplastic continuous filaments is preferably in the range of 90:10 to 60:40 by mass ratio, and more preferably in the range of 85:15 to 70:30. By making the polyester-based high melting point polymer 60% by mass or more and 90% by mass or less, the rigidity and heat resistance of the spunbonded nonwoven fabric can be excellent. On the other hand, by making the polyester-based low melting point polymer 10% by mass or more and 40% by mass or less, when the spunbonded nonwoven fabric is formed by fusion and used, the composite filaments constituting the spunbonded nonwoven fabric can be firmly fused to each other, the mechanical strength is excellent, and the fabric can sufficiently withstand dust collection under a large air volume.

[0031] The average single fiber diameter of the thermoplastic continuous filaments constituting the spunbonded nonwoven fabric is preferably in the range of 12 μm or more and 26 μm or less. By making the average single fiber diameter of the thermoplastic continuous filaments 12 μm or more, preferably 13 μm or more, more preferably 14 μm or more, the breathability of the spunbonded nonwoven fabric can be improved and the pressure loss can be reduced. In addition, the number of thread breaks during the formation of the thermoplastic continuous filaments can be reduced, and the stability during production can be improved. On the other hand, by making the average single fiber diameter of the thermoplastic continuous filaments 26 μm or less, preferably 25 μm or less, more preferably 24 μm or less, the uniformity of the spunbonded nonwoven fabric can be improved, the surface of the nonwoven fabric can be made dense, and the collection performance can be improved, such as making it easier to filter dust at the surface layer.

[0032] In the present invention, the average single fiber diameter (μm) of the spunbonded nonwoven fabric is determined by the following method. (i) Ten small samples are randomly taken from the spunbond nonwoven fabric. (ii) Take photographs of the surface of the collected small sample using a scanning electron microscope or similar device at magnifications of 500 to 2000 times, which allows the thickness of the fibers to be measured. (iii) From the photographs of each small sample, 10 fibers are randomly selected (100 fibers in total) and their diameters are measured. The fibers are assumed to have a circular cross section, and the diameter is taken as the single fiber diameter. (iv) The arithmetic mean value was rounded off to one decimal place to obtain the average single fiber diameter.

[0033] (Manufacturing method of spunbond nonwoven fabric) Next, a method for producing the spunbonded nonwoven fabric according to the present invention will be described. The spunbonded nonwoven fabric according to the present invention is produced by sequentially carrying out the following steps (a) to (c). (a) A process in which a thermoplastic polymer is molten and extruded from a spinneret, and then pulled and drawn by an air sucker to obtain a thermoplastic continuous filament. (b) A process in which the obtained filaments are deposited on a moving net conveyor while regulating the fiber arrangement with a fiber-spreading plate to form a fiber web. (c) subjecting the resulting fibrous web to partial fusion bonding.

[0034] Each of the above steps will now be described in more detail.

[0035] (a) Thermoplastic continuous filament forming process First, a thermoplastic polymer is melt-extruded from a spinneret. In particular, when a composite filament in which a polyester-based low-melting point polymer having a melting point lower than that of a polyester-based high-melting point polymer is used as a thermoplastic continuous filament, the polyester-based high-melting point polymer and the polyester-based low-melting point polymer are melted at a temperature higher than the melting point and lower than the melting point +70°C, respectively, and a composite filament in which a polyester-based low-melting point polymer having a melting point lower than that of the polyester-based high-melting point polymer is disposed around the polyester-based high-melting point polymer by spun out from a fine hole with a spinneret temperature higher than the melting point and lower than the melting point +70°C, and then pulled and stretched by an air sucker at a spinning speed of 4000m / min to 6000m / min to spin a filament having a circular cross-sectional shape.

[0036] (b) Fiber web forming process The nonwoven fabric according to the present invention is a so-called spunbonded nonwoven fabric, and includes a process in which spun thermoplastic continuous filaments are sucked by an ejector, ejected from a fiber-spreading plate having a slit at the bottom of the ejector, and deposited on a moving net conveyor to obtain a fiber web.

[0037] Even when composite polyester fibers are used, it is important that the spunbonded nonwoven fabric is made of the filaments (long fibers). This makes it possible to increase the rigidity and mechanical strength compared to the case of a short fiber nonwoven fabric made of discontinuous fibers, and makes it preferable as a pleated filter. In the manufacturing method of the spunbonded nonwoven fabric according to the present invention, it is also a preferred embodiment to temporarily fuse the fiber web collected on the net conveyer. For the temporary fusion, a method is preferably used in which the collected fiber web is fused with a pair of flat rolls, or a flat roll is placed on the net conveyer and fused between the net conveyer and the flat roll.

[0038] (c) Partial fusion process The spunbonded nonwoven fabric according to the present invention is partially fused, but the method of partially fusion is not particularly limited. Here, the fused portion of the spunbonded nonwoven fabric is called the fused portion, and the other unfused portion is called the nonfused portion. Fusion by a hot embossing roll or a combination of an ultrasonic oscillator and an embossing roll is preferred. In particular, fusion by an embossing roll is most preferred from the viewpoint of improving the strength of the nonwoven fabric. The partial fusion step is preferably processed continuously from the web forming step. By processing continuously from the web forming step, the density of the fused portion is increased, and a nonwoven fabric having excellent waist strength and excellent pleat formability as a spunbonded nonwoven fabric can be obtained. The temperature of fusion by a hot embossing roll is preferably 5°C to 60°C lower than the melting point of the polymer with the lowest melting point present on the fiber surface of the nonwoven fabric, and more preferably 10°C to 50°C lower. Excessive fusion can be prevented by setting the temperature difference between the melting points of the polymers with the lowest melting points present on the fiber surfaces of the nonwoven fabric by the hot embossing roll to 5° C. or more, more preferably 10° C. or more. On the other hand, uniform fusion can be achieved within the nonwoven fabric by setting the temperature difference to 60° C. or less, more preferably 50° C. or less.

[0039] The line pressure for fusion is preferably 30 kg / cm or more and 90 kg / cm or less. By setting the line pressure for fusion to 30 kg / cm or more, more preferably 40 kg / cm or more, the strength required for pleating when used as a spunbonded nonwoven fabric can be imparted to the nonwoven fabric. By setting the line pressure for fusion to 90 kg / cm or less, more preferably 80 kg / cm or less, excessive fusion can be prevented.

[0040] The fusion area ratio of the partial fusion of the spunbonded nonwoven fabric according to the present invention is the ratio of the fusion part to the total area of ​​the nonwoven fabric, and is preferably in the range of 5% to 20% of the total area of ​​the nonwoven fabric. If the fusion area ratio is 5% or more, more preferably 6% or more, and even more preferably 8% or more, the nonwoven fabric has sufficient mechanical strength and the surface does not easily become fuzzed. On the other hand, if the fusion area ratio is 20% or less, more preferably 18% or less, and even more preferably 15% or less, the gap between the fibers is reduced, so that the pressure loss does not increase and the collection performance does not decrease.

[0041] The fused portion forms a depression, and is formed by fusing the thermoplastic continuous filaments constituting the nonwoven fabric together by heat and pressure. That is, the fused portion is the portion where the thermoplastic continuous filaments are fused and aggregated compared to other portions. When fusing by a thermal embossing roll is adopted as the fusing method, the portion where the thermoplastic continuous filaments are fused and aggregated by the convex portion of the embossing roll becomes the fused portion. For example, when a roll having a predetermined pattern of unevenness only on the upper or lower side is used, and the other roll is a flat roll without unevenness, the fused portion refers to the portion where the thermoplastic continuous filaments of the nonwoven fabric are fused by the convex portion of the roll having unevenness and the flat roll and aggregated. In addition, for example, when an embossing roll is used, which is composed of a pair of upper and lower rolls having a plurality of linear grooves arranged in parallel on the surface, and is arranged so that the grooves of the upper roll and the grooves of the lower roll cross at a certain angle, the fused portion refers to the portion where the thermoplastic continuous filaments of the nonwoven fabric are fused by the convex portion of the upper roll and the convex portion of the lower roll and aggregated. In this case, the portion fused between the upper convex portion and the lower concave portion or between the upper concave portion and the lower convex portion is not included in the fused portion referred to here.

[0042] The area of ​​each fused part is 0.3 mm 2 More than 5.0mm 2 Less than 0.3mm is preferred. 2 By setting the thickness to 5.0 mm or more, sufficient mechanical strength as a spunbond nonwoven fabric can be obtained, and fuzzing on the surface of the nonwoven fabric can be suppressed. 2 By setting the thickness below, the mechanical strength of the spunbonded nonwoven fabric as well as the breathability can be maintained, and sufficient collection performance can be obtained.

[0043] The fusion area ratio of the spunbonded nonwoven fabric is measured using a digital microscope (for example, "VHX-5000" manufactured by Keyence Corporation) and 100 rectangular frames of 1.0 cm x 1.0 cm parallel to the longitudinal and transverse directions of the nonwoven fabric are taken from any part of the spunbonded nonwoven fabric at a magnification of 20 times using the microscope. The area of ​​the fusion part within the rectangular frame is measured for each of the 100 points and the average value is calculated as a percentage and rounded off to the first decimal place to obtain the fusion area ratio (%). When not expressed as a percentage, the area (cm2) of the fusion part within the rectangular frame is used. 2 ) to the area of ​​the rectangular frame, 1.0 cm 2 Then, the fused area ratio can be calculated by rounding off to two decimal places.

[0044] The shape of the fused portion is not particularly specified, and even when a roll having a predetermined pattern of unevenness only on the upper or lower side is used and the other roll is a flat roll without unevenness, or when an embossing roll is composed of a pair of upper and lower rolls having a plurality of parallel linear grooves formed on the surface, and the grooves of the upper roll and the grooves of the lower roll are arranged so as to intersect at a certain angle, and the convex portions of the upper roll and the convex portions of the lower roll are fused, the shape of the fused portion may be a circle, a triangle, a rectangle, a parallelogram, an ellipse, a rhombus, or the like. The arrangement of these fused portions is not particularly specified, and they may be arranged regularly at equal intervals, randomly, or a mixture of different shapes. Among them, it is preferable that the fused portions are arranged at equal intervals from the viewpoint of uniformity of the nonwoven fabric. Furthermore, in terms of achieving partial fusion without peeling off the nonwoven fabric, it is preferable to use an embossing roll consisting of a pair of upper and lower rolls having a plurality of parallel linear grooves formed on the surface thereof, in which the grooves of the upper roll and the grooves of the lower roll are arranged so as to intersect at a certain angle, and to form a parallelogram-shaped fused portion formed by fusion between the convex portions of the upper roll and the convex portions of the lower roll.

[0045] (Spunbond nonwoven fabric) The spunbond nonwoven fabric according to the present invention has a bending resistance in the MD direction (Br MD) is 40mN or more and 80mN or less. MD When the tension is 40 mN or more, more preferably 45 mN or more, and even more preferably 50 mN or more, the strength and shape retention of the nonwoven fabric can be maintained while pleating is performed. On the other hand, when the tension is 80 mN or less, more preferably 75 mN or less, and even more preferably 70 mN or less, the folding resistance during pleating is reduced, and the apexes of the pleats are finished at acute angles.

[0046] In the present invention, the MD direction refers to the sheet conveying direction during the production of the spunbonded nonwoven fabric, i.e., the winding direction of the nonwoven fabric roll, and the CD direction refers to the direction perpendicular to the sheet conveying direction, i.e., the winding direction of the nonwoven fabric roll. When the spunbonded nonwoven fabric is not in a rolled state, for example, because it is cut, the MD direction and CD direction are determined by the following procedure. (a) Within the plane of the spunbond nonwoven fabric, select one arbitrary direction and take a test piece 38.1 mm long and 25.4 mm wide along that direction. (b) Similarly, test pieces measuring 38.1 mm in length and 25.4 mm in width are taken at angles rotated 30 degrees, 60 degrees, and 90 degrees from the direction in which the test piece was taken. (c) For each test piece in each direction, the bending resistance of each test piece is measured based on the method for measuring the bending resistance of spunbond nonwoven fabric described below. (d) The direction in which the measured value is highest is the MD direction of the spunbond nonwoven fabric, and the direction perpendicular to this is the CD direction.

[0047] In addition, when determining the MD and CD directions from a pleated body as exemplified in FIG. 1, the direction parallel to the ridge line of the apex of the pleat is the CD direction, and the direction perpendicular to the CD direction is the MD direction.

[0048] The bending resistance (Br MD) is the value obtained as follows in accordance with "6.7.4 Gurley method (JIS method)" in "6.7 Bending resistance (JIS method and ISO method)" of JIS L1913:2010 "General nonwoven fabric testing methods". (i) Test pieces measuring 38.1 mm in length (effective sample length L = 25.4 mm) along the MD direction of the spunbond nonwoven fabric and 25.4 mm in width d = 25.4 mm along the CD direction are taken from any five points on the sample. (ii) Attach each sampled test piece to a chuck and fix the chuck so that it is aligned with the 1-1 / 2" (1.5 inches = 38.1 mm) scale on the movable arm A. In this case, 1 / 2" (0.5 inches = 12.7 mm) of the sample length is applied to the chuck by 1 / 4" (0.25 inches = 6.35 mm), and 1 / 4" (0.25 inches = 6.35 mm) is applied to the tip of the pendulum at the free end of the sample, so the effective sample length L for measurement is the test piece length minus 1 / 2" (0.5 inches = 12.7 mm). (iii) Next, insert a suitable weight W from the fulcrum of the pendulum B to the lower weight mounting holes a, b, and c (mm). a , W b , W c (g) is attached to the movable arm A, and the movable arm A is rotated at a constant speed, and the scale RG (mgf) is read when the test piece separates from the pendulum B. The scale is read to the first decimal place. The weight to be attached to the weight attachment hole can be selected appropriately, but it is preferable to set the scale RG to 4 to 6. (iv) Measurements are performed on five test pieces, five times on each side, for a total of 50 times. (v) From the obtained scale RG value, the bending resistance value is calculated by using the following formula and rounding off to the first decimal place. The average value of 50 measurements is rounded off to the first decimal place to calculate the bending resistance in the MD direction (Br MD ) was decided.

[0049]

number

[0050] The basis weight of the spunbond nonwoven fabric of the present invention is 150 g / m 2More than 300g / m 2 The following range is preferable: Weight per unit area is 150 g / m 2 If the weight is more than 300 g / m, the necessary rigidity for the pleats can be obtained, which is preferable. 2 Less than 270 g / m 2 Less than 260 g / m 2 If it is equal to or less than this, an increase in pressure loss can be suppressed, and it is also preferable in terms of cost.

[0051] The basis weight of the spunbond nonwoven fabric mentioned here is calculated by taking three samples of 50 cm in MD x 50 cm in CD, measuring the mass of each, and calculating the average value (g) per unit area (1 m 2 ) and round off to the first decimal place.

[0052] The CV value of the spunbonded nonwoven fabric according to the present invention is preferably 5% or less. More preferably, it is 4.5% or less, and even more preferably, it is 4% or less, because the nonwoven fabric can be made dense with improved uniformity of the nonwoven fabric, which makes it easier to improve the collection efficiency and to obtain a satisfactory filter life. On the other hand, when the spunbonded nonwoven fabric according to the present invention is used in a filter, the CV value of the spunbonded nonwoven fabric is more preferably 1% or more, because the life of the spunbonded nonwoven fabric is extended by ensuring a certain amount of air permeability and reducing pressure loss.

[0053] In the present invention, the basis weight CV value (%) of the spunbond nonwoven fabric is determined as follows. (i) Take 100 small pieces of 5 cm x 5 cm from the spunbond nonwoven fabric. (ii) Measure the mass (g) of each piece and calculate the unit area (1 m 2 ) per unit. (iii) The average value of the conversion in (ii) (W ave ), standard deviation (W sdv ) are calculated respectively. (iv) Calculate the basis weight CV value (%) using the following formula and round off to the first decimal place. Weight CV value (%) = W sdv / W ave x100.

[0054] The apparent density of the spunbond nonwoven fabric according to the present invention is 0.25 g / cm 3 More than 0.40g / cm 3 It is preferable that the apparent density is 0.25 g / cm or less. 3 More than 0.40g / cm 3 If the apparent density is less than 0.26 g / cm, the spunbond nonwoven fabric has a dense structure, which makes it difficult for dust to get inside, and the dust can be easily removed. A more preferable apparent density range is 0.26 g / cm. 3 More than 0.38g / cm 3 The range is as follows:

[0055] In the present invention, the apparent density (g / cm 3 ) shall be measured and calculated as follows: (i) Using a thickness meter (for example, "TECLOCK" (registered trademark) SM-114 manufactured by Teclock Corporation), the thickness of the spunbond nonwoven fabric is measured at 10 equally spaced points in the CD direction. (ii) The thickness (μm) of the spunbond nonwoven fabric is calculated by rounding off the three decimal places from the arithmetic average value. (iii) The basis weight (g / m2) of the spunbond nonwoven fabric 2 ) and the thickness (μm) calculated using the following formula, rounded off to two decimal places to obtain the apparent density. Apparent density (g / cm 3 )=Weight (g / m 2 ) / Thickness(μm) / 10 6 .

[0056] The air permeability of the spunbond nonwoven fabric of the present invention is 10 (cm 3 / (cm 2 ·sec)) or more 130(cm) 3 / (cm 2It is preferable that the ventilation rate is 10 (cm 2 sec) or less. 3 / (cm 2 sec) or more, preferably 13 (cm 3 / (cm 2 When the air flow rate per unit area is 130 (cm 2 sec) or more, the pressure loss can be suppressed from increasing. 3 / (cm 2 ·sec) or less, preferably 105 (cm 3 / (cm 2 If the time t1 is less than 1.0 s, dust is less likely to remain inside the filter, and the filter has good collection performance.

[0057] In the present invention, the air permeability (cm 3 / (cm 2 For the air permeability (sec), the value measured based on 6.8.1 "Fragile method" in 6.8 "Air permeability (JIS method)" of JIS L1913:2010 "Test methods for general nonwoven fabrics" shall be adopted as follows. (i) Ten test pieces measuring 150 mm in MD x 150 mm in CD are taken at equal intervals from the spunbond nonwoven fabric. (ii) After attaching a test specimen to one end of the cylinder of the testing machine, adjust the suction fan and air hole so that the inclined barometer indicates a pressure of 125 Pa using the lower limit resistor, and measure the pressure indicated by the vertical barometer at that time. (iii) From the measured pressure and the type of air hole used, calculate the volume of air (cm3) passing through the test piece using the conversion table attached to the test machine. 3 / (cm 2 100 seconds) (iv) The average value of the air permeability of the 10 test pieces is rounded off to the nearest tenth and used as the air permeability (cm 3 / (cm 2 · seconds).

[0058] (Pleated body) The pleated article of the present invention is made of the above-mentioned spunbonded nonwoven fabric.

[0059] The thickness (t) of the pleated body in the present invention is preferably 500 μm or more and 800 μm or less. By making the thickness 500 μm or more, more preferably 510 μm or more, it is possible to improve the rigidity and obtain a spunbonded nonwoven fabric suitable for forming a pleated body. In addition, by making the thickness 800 μm or less, more preferably 780 μm or less, it is possible to obtain a spunbonded nonwoven fabric having excellent handling properties and processability as a pleated body.

[0060] In the present invention, the thickness (μm) of the pleated body is determined by the following method. (i) Using a thickness meter (for example, "TECLOCK" (registered trademark) SM-114 manufactured by Teclock Corporation), the thickness of the pleated body is measured at 10 equally spaced points in the CD direction. (ii) The above arithmetic mean value is rounded off to the first decimal place to obtain the thickness (μm) of the pleated body.

[0061] The pleated body of the present invention satisfies the following formulas (1) and (2): 0.25≦r1 / t≦0.50 (1) 0.90≦r2 / r1≦1.00 (2) Here, r1 is the radius of curvature (μm) of one apex of the pleated body, r2 is the radius of curvature (μm) of the other apex of the pleated body, and t is the thickness (μm) of the pleated body, where r1≧r2. These will be explained in more detail below.

[0062] (1) Equation (1) (ratio of radius of curvature at one pleat apex of a pleated body to thickness) In the pleated body of the present invention, the ratio (r1 / t) of the radius of curvature (r1) (μm) of one of the pleat apexes to the thickness (t) (μm) of the pleated body is 0.25 or more and 0.50 or less. When this ratio is 0.25 or more, preferably 0.26 or more, more preferably 0.27 or more, the pleat shape has an acute angle, and when used as a filter, the pleat shape has excellent breathability even under a high air volume. On the other hand, when the ratio is 0.50 or less, preferably 0.49 or less, more preferably 0.48 or less, the pleat shape can be given rigidity, and when used as a filter, the pleat shape can have excellent shape retention even under a high air volume.

[0063] (2) Equation (2) (ratio of the radius of curvature of one apex of the pleated body to the radius of curvature of the other apex of the pleated body) In the pleated body of the present invention, the ratio (r2 / r1) of the radius of curvature (r1) (μm) of one of the pleat apexes of the pleats of the pleated body to the radius of curvature (r2) (μm) of the other of the pleat apexes of the pleated body is 0.90 or more and 1.00 or less. When this ratio is 0.90 or more, preferably 0.91 or more, more preferably 0.92 or more, when the pleated body is used as a pleated filter for a dust collector, deformation of the pleat shape due to compressed air during backwashing can be prevented. On the other hand, when the ratio is 1.00 or less, preferably 0.99 or less, more preferably 0.98 or less, a difference in the strength of the pleats can be imparted between the front and back, and when the pleated body is used as a pleated filter for a dust collector, the pleat shape can be maintained excellently under a large air volume, and the pleat apexes can be vibrated during backwashing to provide excellent dust removal properties.

[0064] Here, the radius of curvature (r1) of one pleat apex and the radius of curvature (r2) of the other pleat apex of the pleated body of the present invention, which are used in calculating the above formulas (1) and (2), are measured as follows. (i) Ten measurement samples each having a V-shaped cross section of 10 mm in the CD direction, including one apex or the other apex, are cut out from the pleated body. (ii) As shown in FIG. 2, the measurement sample is fixed in an open state so that the angle of the apex (11) of the pleated body is 45°. (iii) A pleated body in which the apex of the pleats is fixed at an open angle of 45° is used as a test specimen, and observed at 100x magnification using a microscope, and an enlarged photograph is taken. (iv) An imaginary circle (13) is defined, the inner lines of the apexes of the pleated body being tangent to the lines (12a, 12b). (v) The radius (14) of the imaginary circle (13) is measured and this is regarded as the radius of curvature (μm) of the apex of the pleated body. (vi) Calculate the average value (μm) and standard deviation (μm) of the radius of curvature obtained from the measurement sample of one of the apexes, and round off to the first decimal place. (vii) Similarly, calculate the average value (μm) and standard deviation (μm) of the radius of curvature obtained from the measurement sample of the other vertex, and round off to the first decimal place. (viii) The average values ​​obtained in (vi) and (vii) are compared, and the average value of the larger radius of curvature is determined to be the "radius of curvature of one apex (r1)" of the pleated body, and the average value of the smaller radius of curvature is determined to be the "radius of curvature of the other apex (r2)". However, if the average values ​​obtained in (vi) and (vii) are equal, the average value of the radius of curvature of the apex with the larger sum of the average value (μm) and standard deviation (μm) is determined to be the "radius of curvature of one apex (r1)".

[0065] The pleated body of the present invention can be suitably used as a dust collector filter, since the spunbonded nonwoven fabric constituting the pleated body has a balance between dust collection performance and breathability. In particular, the pleated shape retention required for the nonwoven fabric alone to withstand dust collection under a large air flow rate of more than 300 L / min and repeated backwashing is particularly suitable for use as a filter material for pleated filters for large air volume pulse jet type dust collectors, in which the spunbonded nonwoven fabric alone is used as a filter without being bonded to a substrate such as a PTFE membrane that is likely to peel off, and a large air volume pulse jet type dust collector filter. Such a pleated body can be, for example, a cylindrical dust collector filter in which the entire pleated body is made cylindrical and then the upper and lower ends of the cylinder are fixed, or a panel type dust collector filter in which the ends of the pleated body are fixed to the inner wall of a frame material such as a square or round frame made of a metal material or a polymer resin material.

[0066] The pulse jet type dust collector may use the dust collector filter, and may be particularly suitable for use as a high-volume pulse jet type dust collector that performs dust collection and repeated backwashing under a high air volume of more than 300 L / min. In this high-volume pulse jet type dust collector, the dust collector filter is used in an atmosphere where the flow rate per dust collector filter is 3.0 L / min to 5.0 L / min and the pressure of the processing air acting on each dust collector filter is 0.5 MPa to 0.7 MPa.

[0067] The pulse jet type dust collector includes at least one dust collector filter that filters dust from the equipment to be collected, and a pulse jet mechanism that sprays compressed air in a pulsed manner onto the inner surface of the dust collector filter to remove dust adhering to the outer surface of the filter. This pulse jet mechanism may be an online pulse mechanism that can operate while the dust collector blower motor is operating, or an offline pulse mechanism that can operate while dust collection is suspended.

[0068] Alternatively, the pleated product of the present invention is preferably used as a bellows because it is resistant to tearing even when repeatedly folded and has excellent durability. Such bellows can be freely bent in the direction of the ridges and is made of a stretchable and flexible material, and is therefore used for air ducts used for air conditioning, ventilation, exhaust, etc. in buildings, pipes for draining waste liquids discharged from factories, and car through-holes at the coupling parts of train cars, or is used as a substrate by coating a foam such as neoprene rubber or polyurethane rubber on the surface of a nonwoven fabric.

[0069] (Method for manufacturing pleated body) The pleated body of the present invention can be obtained by pleating the spunbonded nonwoven fabric. For this pleating, a reciprocating folding machine having a mechanism for alternately folding the spunbonded nonwoven fabric up and down by moving upper and lower teeth back and forth, or a rotary folding machine having a mechanism for pressing rolls with folding teeth against the spunbonded nonwoven fabric from above and below to create ridges and fold the fabric can be used. In particular, a reciprocating folding machine is preferably used because the width of the pleats can be freely adjusted.

[0070] In the manufacturing method of the pleated body of the present invention, it is preferable to heat the upper and lower teeth of the reciprocating folder or the rolls of the rotary folder when folding the pleats during pleating. By heating and folding the spunbonded nonwoven fabric, the angles of the apexes of the pleats of the pleated body are sharp, and the pleated body has excellent breathability when used as a filter.

[0071] The temperature of the upper and lower teeth of the reciprocating folder or the roll of the rotary folder during pleating is preferably in the range of 50° C. to 250° C. If the heating temperature during pleating is 50° C. or higher, preferably 60° C. or higher, more preferably 70° C. or higher, the low melting point components of the thermoplastic continuous filaments constituting the spunbonded nonwoven fabric are softened, and the spunbonded nonwoven fabric can be given a softness suitable for forming the pleat apex of the pleated body. On the other hand, by setting the temperature to 250° C. or lower, preferably 230° C. or lower, more preferably 210° C. or lower, deformation of the pleat apex during pleating due to excessive softening of the entire spunbonded nonwoven fabric can be prevented, and the pleat shape can be maintained excellent against repeated backwashing when used as a filter.

[0072] The humidity during pleating is preferably in the range of 45% to 80%. By keeping the humidity during pleating at 45% or more, preferably 47% or more, and more preferably 50% or more, it is possible to prevent static electricity from being generated between the teeth and the nonwoven fabric when forming the pleating ridges. By keeping the humidity during pleating at 80% or less, preferably 75% or less, and more preferably 70% or less, it is possible to suppress a decrease in the mechanical strength of the nonwoven fabric after pleating. EXAMPLES

[0073] Next, the present invention will be specifically described based on examples. However, the present invention is not limited to these examples. In addition, in the measurement of each physical property, unless otherwise specified, the measurement was performed based on the above-mentioned method.

[0074] [Measurement method] (1) Melting point of thermoplastic resin (℃) The measurement was performed using a differential scanning calorimeter "DSC-2" manufactured by PerkinElmer Japan Co., Ltd., at a temperature rise rate of 20°C / min, and the temperature giving the extreme value in the obtained melting endothermic curve was taken as the melting point.

[0075] (2) Intrinsic viscosity (IV) of thermoplastic resin The intrinsic viscosity (IV) of the thermoplastic resin was measured by the following method.

[0076] Dissolve 8 g of sample in 100 mL of orthochlorophenol, and measure the relative viscosity η using an Ostwald viscometer at 25°C. r was calculated using the following formula: η r =η / η0=(t×d) / (t0×d0) (Here, η is the viscosity of the polymer solution, η0 is the viscosity of orthochlorophenol, t is the drop time of the solution (sec), and d is the density of the solution (g / cm 3 ), t0 is the fall time of orthochlorophenol (sec), and d0 is the density of orthochlorophenol (g / cm 3 ) and the relative viscosity η r The intrinsic viscosity (IV) was calculated from the following formula: Intrinsic viscosity (IV)=0.0242η r +0.2634.

[0077] (3) Thickness of the pleated body (μm) The thickness was measured by the above-mentioned method using a "TECLOCK" (registered trademark) SM-114 manufactured by TECLOCK Corporation as a thickness gauge.

[0078] (4) Weight of spunbond nonwoven fabric (g / m 2 ) First, the ridges of both apexes of the pleated body were spread and an iron heated to 100° C. was applied to flatten the pleated body. Three samples measuring 50 cm in length in the MD and 50 cm in length in the CD were then taken from the flattened pleated body, and the samples were evaluated in the same manner as in the measurement of basis weight of the spunbonded nonwoven fabric described above.

[0079] (5) CV value of spunbond nonwoven fabric (%) First, the ridges of both apexes of the pleated body were spread and an iron heated to 100° C. was applied to flatten the pleated body. Then, 100 samples measuring 5 cm in length in the MD and 5 cm in length in the CD were taken from the flattened pleated body, and the samples were evaluated in the same manner as in the measurement of basis weight of the spunbonded nonwoven fabric described above.

[0080] (6) Apparent density of spunbond nonwoven fabric (g / cm 3 ) The apparent density of spunbond nonwoven fabric is defined as "(4) Basis weight of spunbond nonwoven fabric (g / m 2 The thickness of the pleated body obtained in "(3) Thickness (μm) of the pleated body" was calculated using the method described above.

[0081] (7) Bending resistance of spunbond nonwoven fabric (mN) The bending resistance of the spunbond nonwoven fabric was measured and calculated using the Gurley flexibility tester "GAS-10" manufactured by Daiei Seiki Seisakusho Co., Ltd., in the manner described above.

[0082] (8) Air permeability of spunbond nonwoven fabric (cm 3 / (cm 2 ·sec)) The air permeability of the spunbond nonwoven fabric was measured using the air permeability tester "FX3300-III" manufactured by Textest, Switzerland.

[0083] (9) Ratio of the radius of curvature of one apex of the pleat-formed body to the thickness (r1 / t), and ratio of the radius of curvature of one apex of the pleat-formed body to the radius of curvature of the other apex of the pleat-formed body (r2 / r1) The radii of curvature (r1, r2) of the pleat apexes of the pleated body were calculated by the method described above. The ratio of the radius of curvature of one pleat apex of the pleated body to the thickness (r1 / t) and the ratio of the radius of curvature of one apex of the pleated body to the radius of curvature of the other apex of the pleated body (r2 / r1) were calculated by the method described above.

[0084] (10) Initial pressure loss of pleated body (Pa) (i) The following measurement samples were taken from a pleated product in which the distance from the ridgeline of one pleat apex to the ridgeline of the other pleat apex was 35 mm. CD dimension: 515mm MD dimension: The length that includes 45 apexes on one side of the pleated body (35mm x (45+1) = 1610mm) (ii) A total of five pieces of (i) were collected and five cylindrical cartridge filters were made. (iii) The cylindrical cartridge filter thus prepared was set in a multi-pass tester, and the air velocity was 3.2 m / min and the dust concentration was 5.0 g / m 3 The pressure loss was measured after 15 types of JIS standard powders were poured in for 5 minutes. (iv) The average pressure loss obtained from the test was rounded off to the first decimal place, and this value was regarded as the initial pressure loss (Pa) of the pleated body.

[0085] (11) Dust removal ability of pleated body (i) The following measurement samples were taken from a pleated product in which the distance from the ridgeline of one pleat apex to the ridgeline of the other pleat apex was 35 mm. CD dimension: 515mm MD dimension: The length that includes 45 apexes on one side of the pleated body (35mm x (45+1) = 1610mm) (ii) A total of five pieces of (i) were collected and five cylindrical cartridge filters were made. (iii) The cylindrical cartridge filter thus prepared was set in a multi-pass tester, and the air velocity was 3.2 m / min and the dust concentration was 5.0 g / m 3 We supplied 15 types of JIS standard powders. (iv) When the pressure loss of the cartridge filter reached 1000 Pa, compressed air at 0.5 MPa was sprayed from the pulse jet device for 0.1 seconds to remove the dust adhering to the cartridge filter. The operation time (seconds) required for (v) and (iv) to reach 200 brush strokes was measured. (vi) The average operating time obtained from the test was rounded off to the first decimal place, and this value was regarded as the dust-removability of the pleated body.

[0086] (12) Shape retention of pleated body The shape retention of the pleated article was evaluated using the cylindrical cartridge filter used in the above "(11) Dust removal ability of the pleated article". (i) After the evaluation of "(11) Dust-removing ability of pleated article" was performed, the cylindrical cartridge filter was removed from the pulse jet device. (ii) Twenty panelists visually inspected the appearance of the cylindrical cartridge filter removed from the pulse jet device and judged the shape retention of the pleated body on a 5-point scale according to the following criteria. The total score was therefore calculated from a minimum of 0 points to a maximum of 100 points, with a score of 80 points or more being considered a pass. 5 points: Very good (There is no contact between the pleats or distortion in the shape of the pleats, and adjacent pleats are aligned in parallel lines.) 4 points: Good (Between 5 and 3) 3 points (The pleats are not touching each other, but the shape of the pleats is distorted.) 2 points (Between 3 and 2) 1 point (The pleats are distorted and the pleats are touching each other.) (12) Shape stability of pleated body Fig. 3 is a diagram for explaining the configuration of a test system for carrying out a pleat shape stability test according to an embodiment of the present invention. The test system 31 shown in Fig. 3 includes a sample holder 32 for setting a test sample, a pressure gauge 33, a flow meter 34, a flow control valve 35, and a blower 36. The flow meter 34, the flow control valve 35, and the blower 36 are connected to the sample holder 32. In this test system 31, air is sent by the blower 36, and the air is discharged from an air outlet 37 in the direction indicated by 38.

[0087] First, the spunbond nonwoven fabric is pleated to a pleat height of 48 mm. Next, as shown in FIG. 4, the pleated substrate is surrounded by a frame material having a unit length of 30 cm, a unit width of 30 cm, and a unit height of 48 mm so that the pleat pitch is 1.3 mm and the number of pleats is 23, to prepare three measurement units U. There is no particular requirement for the frame material as long as it is made of a material that does not leak air during measurement. Next, the prepared measurement units U are set in the sample holder 32. Air volumes are set to 2.0, 4.0, 5.0, 6.0, and 7.0 m 3 The flow rate was adjusted with the flow rate adjustment valve 35 so that the flow rate was 1 / min (a total of five points), and the pressure loss at each flow rate was measured. The average value of the pressure loss measurement results for the three units was calculated, and a graph was created with the wind speed on the horizontal axis and the pressure loss on the vertical axis, and the coefficient of determination (R 2 ) was calculated and evaluated according to the following criteria. Pleats shape retention A: R 2 >0.995 Pleats shape retention B: 0.990≦R 2 ≦0.995 Pleats shape retention C: R 2 <0.990 In nonwoven fabrics with high pleat shape stability, the pleats do not deform and the filtration area does not decrease even under high airflow, so the pressure loss increases linearly with the increase in airflow. Therefore, the coefficient of determination (R 2 ) is close to 1. On the other hand, for nonwoven fabrics with low pleat shape stability, as the air volume increases the pleats are crushed by the wind pressure, reducing the effective filtration area and increasing the pressure loss, so the coefficient of determination does not increase linearly and becomes low.

[0088] [Resin used] Next, the resins used in the examples and comparative examples will be described in detail. Polyester resin A: Polyethylene terephthalate (PET) dried to a moisture content of 50 ppm by mass or less, with an intrinsic viscosity (IV) of 0.65 and a melting point of 260°C. Polyester resin B: Copolymerized polyethylene terephthalate (CO-PET) dried to a moisture content of 50 mass ppm or less, with an intrinsic viscosity (IV) of 0.64, an isophthalic acid copolymerization rate of 11 mol%, and a melting point of 230°C. [Example 1] The polyester resin A and the polyester resin B were melted at temperatures of 295°C and 280°C, respectively. Then, the polyester resin A was used as the core component and the polyester resin B was used as the sheath component, and the core:sheath = 80:20 mass ratio was spun from the pores at a spinneret temperature of 295°C, and then a filament having a circular cross section was spun at a spinning speed of 4900m / min by an air sucker, and the fiber arrangement was regulated by a fiber spreader plate and deposited on a moving net conveyor, and a fiber web consisting of fibers with a single fiber diameter of 14.8μm was collected. The collected fiber web was temporarily fused by a calendar roll consisting of a pair of flat rolls at a temperature of 140°C and a linear pressure of 50kg / cm. Further, the fused area ratio was 10%, and the area per fused portion was 1.6mm. 2 The fibers were fused using a pair of embossing rolls consisting of an engraved roll with a temperature of 200°C for both the upper and lower embossing rolls, and a linear pressure of 70 kg / cm was applied to the fiber web to obtain a spunbonded nonwoven fabric. The spunbonded nonwoven fabric was cut to a width of 515 mm, and pleated while being heated and compressed at a temperature of 150°C so that the distance from the ridgeline of one pleat apex to the ridgeline of the other pleat apex was 35 mm, and the fabric had a basis weight of 260 g / m2. 2 The pleated body thus obtained had a CV value of 3.3%, a thickness of 730 μm, a radius of curvature per unit thickness at the apex of the pleats of 0.45, and a ratio of the radii of curvature at the apex of the pleats of 0.98. The results are shown in Table 1.

[0089] [Example 2] The temperatures of the upper and lower embossing rolls were changed from 200°C to 210°C and 180°C, respectively, and fusion was performed to obtain a spunbonded nonwoven fabric having a basis weight of 260 g / m under the same conditions as in Example 1. 2The pleated body thus obtained had a CV value of 3.4%, a thickness of 910 μm, a radius of curvature per unit thickness at the apex of the pleats of 0.46, and a ratio of the radii of curvature at the apex of the pleats of 0.90. The results are shown in Table 1.

[0090] [Example 3] The temperatures of the upper and lower embossing rolls were changed from 200°C to 180°C and 210°C, respectively, and fusion was performed to obtain a spunbonded nonwoven fabric having a basis weight of 260 g / m under the same conditions as in Example 1. 2 The pleated body thus obtained had a CV value of 3.3%, a thickness of 690 μm, a radius of curvature per unit thickness at the apex of the pleats of 0.46, and a ratio of the radii of curvature at the apex of the pleats of 0.95. The results are shown in Table 1.

[0091] [Example 4] The upper and lower embossing rolls are set to a fusion area ratio of 10% and the area of ​​each fusion part is 1.6 mm 2 The fusion area ratio is 6%, and the area of ​​each fusion part is 1.6 mm. 2 The same conditions as in Example 1 were used to obtain a spunbond nonwoven fabric having a basis weight of 260 g / m. 2 The pleated body thus obtained had a CV value of 3.5%, a thickness of 1210 μm, a radius of curvature per unit thickness at the apex of the pleats of 0.47, and a ratio of the radii of curvature at the apex of the pleats of 0.93. The results are shown in Table 1.

[0092] [Example 5] The upper and lower embossing rolls are set to a fusion area ratio of 10% and the area of ​​each fusion part is 1.6 mm 2 The fusion area ratio is 13%, and the area of ​​each fusion part is 1.6 mm. 2 The same conditions as in Example 1 were used to obtain a spunbond nonwoven fabric having a basis weight of 260 g / m. 2The pleated body thus obtained had a CV value of 3.2%, a thickness of 700 μm, a radius of curvature per unit thickness at the apex of the pleats of 0.36, and a ratio of the radii of curvature at the apex of the pleats of 0.92. The results are shown in Table 1.

[0093] [Example 6] The spinning speed was changed so that the average single fiber diameter was 24.6 μm, while the speed of the net conveyer was changed so that the basis weight was the same as in Example 1. Other than that, a spunbond nonwoven fabric was obtained with a basis weight of 260 g / m under the same conditions as in Example 1. 2 The pleated body thus obtained had a CV value of 4.3%, a thickness of 890 μm, a radius of curvature per unit thickness at the apex of the pleats of 0.48, and a ratio of the radii of curvature at the apex of the pleats of 0.93. The results are shown in Table 1.

[0094] [Table 1]

[0095] The properties of the obtained pleated body are as shown in Table 1. The pleated bodies of Examples 1 to 6 all had a basis weight CV value of 5% or less, excellent basis weight uniformity and pleat shape retention, and showed good properties as pleated bodies. The dust brushing ability of the pleated bodies was 970 Pa or less and 5,800 seconds or more, and the pleat shape retention was also good, with 88 points or more and pleat shape stability B or more.

[0096] [Comparative Example 1] In the manufacturing process of Example 1, a step was added between the step of pre-fusing the collected fiber web and the step of fusing using an embossing roll, in which the sheet obtained in the pre-fusing step was once wound up and cooled to room temperature, and then this sheet was sent to the embossing roll. In other words, the step of fusing using an embossing roll was not performed subsequent to the pre-fusing step, and a spunbonded nonwoven fabric having a basis weight of 260 g / m was obtained in the same manner as in Example 1. 2The pleated body thus obtained had a CV value of 3.4%, a thickness of 700 μm, a radius of curvature per unit thickness at the apex of the pleats of 0.65, and a ratio of the radii of curvature at the apex of the pleats of 0.94. The results are shown in Table 2.

[0097] [Comparative Example 2] The upper and lower embossing rolls are set to a fusion area ratio of 10% and the area of ​​each fusion part is 1.6 mm 2 The fusion area ratio is 15% and the area of ​​each fusion part is 1.6 mm from an embossing roll consisting of a pair of engraved rolls. 2 The same procedure as in Example 1 was repeated except that a spunbonded nonwoven fabric having a basis weight of 260 g / m was obtained by fusing the embossed rolls instead of the embossed rolls consisting of an engraved roll and a flat roll. 2 The pleated body thus obtained had a CV value of 5.9%, a thickness of 620 μm, a radius of curvature per unit thickness at the apex of the pleats of 0.55, and a ratio of the radii of curvature at the apex of the pleats of 0.80. The results are shown in Table 2.

[0098] [Comparative Example 3] The upper and lower embossing rolls are set to a fusion area ratio of 10% and the area of ​​each fusion part is 1.6 mm 2 The fusion area ratio is 3%, and the area of ​​each fusion part is 1.6 mm. 2 A spunbond nonwoven fabric having a basis weight of 260 g / m was obtained in the same manner as in Example 1, except that a pair of engraved rolls having the same structure was used instead of the embossing roll having the same structure as in Example 1. 2 The pleated body thus obtained had a CV value of 3.5%, a thickness of 1290 μm, a radius of curvature per unit thickness at the apex of the pleats of 0.55, and a ratio of the radii of curvature at the apex of the pleats of 0.90. The results are shown in Table 2.

[0099] [Comparative Example 4] The upper and lower embossing rolls are set to a fusion area ratio of 10% and the area of ​​each fusion part is 1.6 mm 2 The fusion area ratio is 24%, and the area of ​​each fusion part is 1.6 mm. 2A spunbond nonwoven fabric having a basis weight of 260 g / m was obtained in the same manner as in Example 1, except that a pair of engraved rolls having the same structure was used instead of the embossing roll having the same structure as in Example 1. 2 The pleated body thus obtained had a CV value of 3.2%, a thickness of 600 μm, a radius of curvature per unit thickness at the apex of the pleats of 0.57, and a ratio of the radii of curvature at the apex of the pleats of 0.94. The results are shown in Table 2.

[0100] [Comparative Example 5] The spinning speed was changed so that the average single fiber diameter was 29.2 μm, while the speed of the net conveyer was changed so that the basis weight was the same as in Example 1. A spunbond nonwoven fabric was obtained under the same conditions as in Example 1, except that the basis weight was 260 g / m 2 The pleated body thus obtained had a CV value of 5.2%, a thickness of 1010 μm, a radius of curvature per unit thickness at the apex of the pleats of 0.52, and a ratio of the radii of curvature at the apex of the pleats of 0.96. The results are shown in Table 2.

[0101] [Comparative Example 6] The spinning speed was changed so that the average single fiber diameter was 11.2 μm, while the speed of the net conveyer was changed so that the basis weight was the same as in Example 1. Other than that, a spunbond nonwoven fabric was obtained with a basis weight of 260 g / m under the same conditions as in Example 1. 2 The pleated body thus obtained had a CV value of 2.6%, a thickness of 490 μm, a radius of curvature per unit thickness at the apex of the pleats of 0.54, and a ratio of the radii of curvature at the apex of the pleats of 0.95. The results are shown in Table 2.

[0102] [Comparative Example 7] The polyester resin A and the polyester resin B were melted at temperatures of 295°C and 280°C, respectively. Then, the polyester resin A was used as the core component and the polyester resin B was used as the sheath component, and the core:sheath = 80:20 mass ratio was spun out from the fine holes at a spinneret temperature of 300°C, and then a filament having a circular cross section was spun at a spinning speed of 4400 m / min by an air sucker. The filament was collided with a metal collision plate installed at the outlet of the air sucker, and the fibers were charged and opened by frictional charging, and the fiber web consisting of fibers with an average single fiber diameter of 14.8 μm was collected on a moving net conveyor. Subsequently, a fusion area ratio of 18% and an area per fusion part of 0.7 mm were obtained. 2 The fibers were fused using a pair of embossing rolls consisting of an engraved roll with a temperature of 205°C for both the upper and lower embossing rolls and a linear pressure of 70 kg / cm to obtain a spunbonded nonwoven fabric. The obtained spunbonded nonwoven fabric was pleated in the same manner as in Example 1 to obtain a fabric with a basis weight of 260 g / m. 2 The pleated body thus obtained had a CV value of 10.5%, a thickness of 620 μm, a radius of curvature per unit thickness at the apex of the pleats of 0.55, and a ratio of the radii of curvature at the apex of the pleats of 0.89. The results are shown in Table 2.

[0103] [Table 2]

[0104] The properties of the obtained nonwoven fabric are as shown in Table 2. Comparative Examples 1 to 7 had a high radius of curvature per unit thickness, and the angle of the pleat apex relative to the thickness of the pleated body was obtuse, the durability of the pleat apex was reduced, and the pleat shape could not be maintained against the compressed air from the pulse jet device, resulting in poor dust removal properties and poor pleat shape stability. Comparative Example 4 had poor initial pressure loss due to a decrease in the filtration area caused by an increase in the fusion rate between fibers. Comparative Example 5, which had a thicker average single fiber diameter, had a basis weight CV value of 5% or more and an increased thickness, which caused pleat contact in the pleated body, resulting in poor initial pressure loss. Comparative Example 6, which had a thin average single fiber diameter, had poor initial pressure loss and pleat shape stability due to a decrease in durability of the pleat apex and a densified sheet. [Explanation of symbols]

[0105] 1: Pleated body 2: Pleats apex A 3: Pleats apex B 4: MD direction arrow 5: CD direction arrow 21: Apex of the pleated body 22a, 22b: Tangent 23: Virtual circle 24: Radius of virtual circle 31: Pleats shape retention test system 32: Sample holder 33: Pressure gauge 34:Flow meter 35: Flow control valve 36: Blois 37: Air outlet 38: Air blowing direction U: unit of measurement 41: Mountain Pitch 42: Unit length 43: Unit width 44: Unit height 45: Frame material

Claims

1. A pleated body made of a spunbond nonwoven fabric, The spunbond nonwoven fabric is composed of thermoplastic continuous filaments consisting of a high melting point component and a low melting point component, and is partially fused; The pleated body is The thickness (t) of the pleated body is 500 μm or more and 1210 μm or less, A pleated body satisfying the following formulas (1) and (2). 0.25≦r 1 / t≦0.50 ・・・(1) 0.90≦r 2 / r 1 ≦1.00 ・・・(2) Here, r 1 is the radius of curvature of one apex of the pleated body (μm), r 2 is the radius of curvature (μm) of the other apex of the pleated body, and t is the thickness (μm) of the pleated body. 1 ≧r 2 It is. The radii of curvature (r 1 ) and (r 2 ) used in the calculation of the formulas (1) and (2) are measured as follows. (i) Ten measurement samples each having a V-shaped cross section of 10 mm in the CD direction including one apex or the other apex are cut out from the pleated body. (ii) The measurement sample is fixed in an open state so that the angle of the apex (11) of the pleated body is 45°. (iii) A pleated body in which the apexes of the pleats are fixed in an open state at an angle of 45° is used as a test piece, and observed at 100 times using a microscope, and an enlarged photograph is taken. (iv) An imaginary circle (13) is defined to which the inner lines of the apexes of the pleated body are tangent to the lines (12a, 12b). (v) The radius (14) of the imaginary circle (13) is measured and this is regarded as the radius of curvature (μm) of the apex of the pleated body. (vi) The average value (μm) and standard deviation (μm) of the radius of curvature obtained from the measurement sample of one of the apexes are calculated, and the values ​​are rounded off to the first decimal place. (vii) Similarly, the average value (μm) and standard deviation (μm) of the radius of curvature obtained from the measurement sample of the other apex portion are calculated, and the values ​​are rounded off to the first decimal place. (viii) The average values ​​obtained in (vi) and (vii) are compared, and the average value of the larger radius of curvature is determined to be the radius of curvature (r1), and the average value of the smaller radius of curvature is determined to be the radius of curvature (r2). However, if the average values ​​obtained in (vi) and (vii) are equal, the average value of the radius of curvature of the apex part having the larger sum of the average value (μm) and the standard deviation (μm) is determined to be the radius of curvature (r1).

2. The pleated body according to claim 1 , wherein the spunbonded nonwoven fabric has a basis weight CV value of 5% or less.

3. 3. The pleated body according to claim 1 or 2, wherein the area ratio of the fused portions of the spunbonded nonwoven fabric is 5% or more and 20% or less.

4. The pleated body according to any one of claims 1 to 3, wherein the average single fiber diameter of the thermoplastic continuous filaments is 12 µm or more and 26 µm or less.

5. A dust collector filter comprising the pleated article according to any one of claims 1 to 4.

6. A high volume pulse jet type dust collector using the dust collector filter according to claim 5.

Citation Information

Patent Citations

  • Chemical cleaning for forced onceethrough boiler

    JP1977098803A

  • Angle sensor

    JP1979022874A

  • Socket

    JP1994036843A

  • Composite filament nonwoven fabric and filter obtained therefrom

    JP2001248056A

  • Nonwoven fabric for filter

    JP2007237167A