Pneumatic tires

The tire design with a specific rubber composition and geometric constraints addresses the issues of high rolling resistance and durability by reducing friction and deformation, resulting in improved performance during high-speed running.

JP7595840B2Active Publication Date: 2024-12-09SUMITOMO RUBBER INDUSTRIES LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2020181287
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-29
Publication Date
2024-12-09
Estimated Expiration
2040-07-28

AI Technical Summary

Technical Problem

Conventional pneumatic tires fail to sufficiently reduce rolling resistance during high-speed running and do not provide adequate durability.

Method used

A pneumatic tire design featuring a rubber composition with styrene-butadiene rubber and isoprene rubber, with a loss tangent of 0.14 or less, and specific geometric constraints such as cross-sectional width, outer diameter, and virtual volume ratios, along with circumferential and lateral grooves, to enhance rolling resistance and durability.

Benefits of technology

The tire design achieves significantly reduced rolling resistance and improved durability during high-speed running by minimizing friction and deformation, while maintaining structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595840000001
    Figure 0007595840000001
  • Figure 0007595840000002
    Figure 0007595840000002
  • Figure 0007595840000003
    Figure 0007595840000003
Patent Text Reader

Abstract

To provide a pneumatic tire in which rolling resistance during high-speed running is sufficiently reduced and durability is sufficiently improved. [Solution] A pneumatic tire has a tread portion, and the rubber layer of the tread portion is formed from a rubber composition containing a rubber component containing styrene butadiene rubber and isoprene-based rubber, and has a loss tangent (30°C tanδ) of 0.14 or less when measured under conditions of 30°C, a frequency of 10 Hz, an initial strain of 5%, and a dynamic strain rate of 1%. When mounted on a regular rim and the internal pressure is set to 250 kPa, the cross-sectional width of the tire is Wt (mm), the outer diameter is Dt (mm), and the volume of the space occupied by the tire is a virtual volume V (mm 3 ), a pneumatic tire that satisfies the following (Equation 1) and (Equation 2). 1600≦(Dt 2 ×π / 4) / Wt≦2827.4 (Formula 1) [(V+1.5×10 7 ) / Wt]≦2.88×10 5 ...(Formula 2)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pneumatic tire. [Background technology]

[0002] In recent years, there has been a growing demand for more fuel-efficient automobiles due to growing concerns about environmental issues and economic reasons, and there is also a strong demand for improved fuel efficiency in pneumatic tires (hereinafter simply referred to as "tires") that are fitted to automobiles.

[0003] The fuel efficiency of a tire can be evaluated by its rolling resistance, and it is known that the smaller the rolling resistance, the more fuel efficient the tire.

[0004] Therefore, it has been proposed to reduce the rolling resistance by modifying the compounding of the rubber composition constituting the tread portion of the tire (for example, Patent Documents 1 to 4). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2018-178034 A [Patent Document 2] JP 2019-089911 A [Patent Document 3] WO2018 / 186367 publication [Patent Document 4] JP 2019-206643 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the tires manufactured by the above-mentioned conventional techniques still do not have sufficient reduction in rolling resistance during high-speed running, and further reduction is desired. Furthermore, the durability of these tires is also insufficient.

[0007] Therefore, an object of the present invention is to provide a pneumatic tire in which the rolling resistance during high-speed running is sufficiently reduced and durability is sufficiently improved. [Means for solving the problem]

[0008] The present inventors have conducted extensive research into solving the above problems, and have found that the above problems can be solved by the invention described below, thereby completing the present invention.

[0009] The invention described in claim 1 is A pneumatic tire having a tread portion, the rubber layer of the tread portion is formed from a rubber composition that includes a rubber component containing styrene-butadiene rubber and isoprene-based rubber, and has a loss tangent (30°C tan δ) of 0.14 or less, measured under conditions of 30°C, a frequency of 10 Hz, an initial strain of 5%, and a dynamic strain rate of 1%; When the tire is mounted on a regular rim and the internal pressure is 250 kPa, the cross-sectional width of the tire is Wt (mm), the outer diameter is Dt (mm), and the volume of the space occupied by the tire is the virtual volume V (mm 3 ), the following (Equation 1) and (Equation 4 ) is a pneumatic tire characterized by satisfying the above. 2008≦(Dt 2 ×π / 4) / Wt≦2827.4 (Formula 1) [(V+ 2.5 ×10 7 ) / Wt]≦2.88×10 5 ······(formula 4 )

[0012] Claim 2 The invention described in A pneumatic tire having a tread portion, the rubber layer of the tread portion is formed from a rubber composition that includes a rubber component containing styrene-butadiene rubber and isoprene-based rubber, and has a loss tangent (30°C tan δ) of 0.10 or less, measured under conditions of 30°C, a frequency of 10 Hz, an initial strain of 5%, and a dynamic strain rate of 1%; When the tire is mounted on a regular rim and the internal pressure is 250 kPa, the cross-sectional width of the tire is Wt (mm), the outer diameter is Dt (mm), and the volume of the space occupied by the tire is the virtual volume V (mm 3 ), the following (Equation 1) and (Equation 2) must be satisfied. Features Sky It is a favorite tire 。 2008≦(Dt2 ×π / 4) / Wt≦2827.4 (Formula 1) [(V+1.5×10 7 ) / Wt]≦2.88×10 5 ...(Formula 2)

[0013] Claim 3 The invention described in A pneumatic tire having a tread portion, the rubber layer of the tread portion is formed from a rubber composition that includes a rubber component containing styrene-butadiene rubber and isoprene-based rubber, and has a loss tangent (30°C tan δ) of 0.14 or less, measured under conditions of 30°C, a frequency of 10 Hz, an initial strain of 5%, and a dynamic strain rate of 1%; When the tire is mounted on a regular rim and the internal pressure is 250 kPa, the cross-sectional width of the tire is Wt (mm), the outer diameter is Dt (mm), and the volume of the space occupied by the tire is the virtual volume V (mm 3 ), the following (Equation 1) and (Equation 2) are satisfied: The tire has a circumferential groove in the tread portion that extends continuously in the circumferential direction of the tire. The groove width L of the circumferential groove at the ground contact surface of the tread portion 0 The groove width L at a depth of 80% of the maximum depth of the circumferential groove 80 Ratio (L 80 / L 0 ) is 0.3 to 0.7 The present invention is characterized in that Sky It's a favorite tire. 2008≦(Dt 2 ×π / 4) / Wt≦2827.4 (Formula 1) [(V+1.5×10 7 ) / Wt]≦2.88×10 5 ...(Formula 2)

[0014] Claim 4 The invention described in A pneumatic tire having a tread portion, the rubber layer of the tread portion is formed from a rubber composition that includes a rubber component containing styrene-butadiene rubber and isoprene-based rubber, and has a loss tangent (30°C tan δ) of 0.14 or less, measured under conditions of 30°C, a frequency of 10 Hz, an initial strain of 5%, and a dynamic strain rate of 1%; When the tire is mounted on a regular rim and the internal pressure is 250 kPa, the cross-sectional width of the tire is Wt (mm), the outer diameter is Dt (mm), and the volume of the space occupied by the tire is the virtual volume V (mm 3 ), the following (Equation 1) and (Equation 2) are satisfied: The tire has a plurality of circumferential grooves in the tread portion, the circumferential grooves extending continuously in the tire circumferential direction. The total cross-sectional area of ​​the plurality of circumferential grooves is 10 to 30% of the cross-sectional area of ​​the tread portion. Yes It is characterized by Sky It's a favorite tire. 2008≦(Dt 2 ×π / 4) / Wt≦2827.4 (Formula 1) [(V+1.5×10 7 ) / Wt]≦2.88×10 5 ...(Formula 2)

[0015] Claim 5 The invention described in A pneumatic tire having a tread portion, the rubber layer of the tread portion is formed from a rubber composition that includes a rubber component containing styrene-butadiene rubber and isoprene-based rubber, and has a loss tangent (30°C tan δ) of 0.14 or less, measured under conditions of 30°C, a frequency of 10 Hz, an initial strain of 5%, and a dynamic strain rate of 1%; When the tire is mounted on a regular rim and the internal pressure is 250 kPa, the cross-sectional width of the tire is Wt (mm), the outer diameter is Dt (mm), and the volume of the space occupied by the tire is the virtual volume V (mm 3 ), the following (Equation 1) and (Equation 2) are satisfied: The tire has a plurality of axially extending lateral grooves in the tread portion, The total volume of the plurality of lateral grooves is 2.0 to 5.0% of the volume of the tread portion. The present invention is characterized in that Sky It's a favorite tire. 2008≦(Dt 2 ×π / 4) / Wt≦2827.4 (Formula 1) [(V+1.5×10 7 ) / Wt]≦2.88×10 5 ...(Formula 2)

[0016] Claim 6 The invention described in 4. The present invention is characterized in that at least one of the lateral grooves has a groove width / groove depth ratio of 0.50 to 0.80. 5 The pneumatic tire is as described above.

[0017] Claim 7 The invention described in 2. The method according to claim 1, wherein the 30° C. tan δ is 0.12 or less. ,or Claim 3 or claims 6 13. The pneumatic tire according to claim 12,

[0018] Claim 8 The invention described in When the tire is mounted on a standard rim and the internal pressure is 250 kPa, the tire's outer diameter is Dt (mm) and its cross-sectional height is Ht (mm), (Dt-2 x Ht) is 470 (mm) or more. characterized in that Claims 1 to Claim Any one of 7 The pneumatic tire is as described above.

[0019] Claim 9 The invention described in Aspect ratio is 40% or more Claims 1 to 5 are characterized in that 8 13. The pneumatic tire according to claim 12,

[0020] Claim 10 The invention described in Aspect ratio is 45% or more The present invention is characterized in that 9 The pneumatic tire is as described above.

[0021] Claim 11 The invention described in Aspect ratio is 47.5% or more The present invention is characterized in that to 10 The pneumatic tire is as described above.

[0022] Claim 12 The invention described in Aspect ratio is 50% or more The present invention is characterized in that to 11 The pneumatic tire is as described above.

[0023] Claim 13 The invention described in 30℃tanδ×Wt≦30.0 Claims 1 to 5 are characterized in that 12 13. The pneumatic tire according to claim 12,

[0024] Claim 14 The invention described in 30℃tanδ×Wt≦25.0 The present invention is characterized in that 13 The pneumatic tire is as described above.

[0025] Claim 15 The invention described in Claims 1 to 5, characterized in that when the tire is mounted on a regular rim and the internal pressure is 250 kPa, the outer diameter of the tire is Dt (mm) and Dt is less than 685 (mm). 14 13. The pneumatic tire according to claim 12,

[0026] Claim 16 The invention described in 1 to 3, characterized in that the cross-sectional width Wt (mm) is less than 205 mm. 15 13. The pneumatic tire according to claim 12,

[0027] Claim 17 The invention described in 3. The cross-sectional width Wt (mm) is less than 200 mm. 16 The pneumatic tire is as described above. Effect of the Invention

[0028] According to the present invention, it is possible to provide a pneumatic tire in which the rolling resistance during high-speed running is sufficiently reduced and durability is sufficiently improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] [1] Characteristics of the tire according to the present invention First, the features of the tire according to the present invention will be described.

[0030] 1. Overview The tire according to the present invention is characterized in that the rubber layer of the tread portion is formed from a rubber composition that includes a rubber component containing styrene-butadiene rubber (SBR) and an isoprene-based rubber, and has a loss tangent (30°C tan δ) of 0.14 or less, measured under conditions of 30°C, a frequency of 10 Hz, an initial strain of 5%, and a dynamic strain rate of 1%.

[0031] The tire according to the present invention is further defined as a virtual volume V (mm) when the tire cross-sectional width is Wt (mm), the outer diameter is Dt (mm) and the volume of the space occupied by the tire is V (mm) when the tire is mounted on a regular rim and the internal pressure is 250 kPa. 3 ), it is also characterized in that the following (Equation 1) and (Equation 2) are satisfied. 2008 ≦(Dt 2 ×π / 4) / Wt≦2827.4 (Formula 1) [(V+1.5×10 7 ) / Wt]≦2.88×10 5 ...(Formula 2)

[0032] By providing the above-mentioned characteristics for the physical properties of the rubber composition forming the tread portion and the tire shape, it is possible to provide a tire with sufficiently reduced rolling resistance during high-speed running and sufficiently improved durability.

[0033] In the above description, the term "genuine rim" refers to a rim that is specified for each tire by the standard system that includes the standard on which the tire is based. For example, in the case of JATMA (Japan Automobile Tire Manufacturers Association), it is the standard rim for the applicable size listed in the "JATMA YEAR BOOK", and in the case of ETRTO (The European Tyre and Rim Manufacturers Association), it is the standard rim for the applicable size listed in the "JATMA YEAR BOOK". For tires not specified by a standard, it refers to the rim with the smallest rim diameter and the next narrowest rim width that can be mounted on a rim and can hold internal pressure, that is, that does not cause air leakage between the rim and tire.

[0034] In the above description, the outer diameter Dt of the tire refers to the outer diameter of the tire when it is mounted on a standard rim, with the internal pressure set to 250 kPa and no load applied, and the cross-sectional width Wt of the tire refers to the width obtained by excluding the patterns, letters, etc. on the side of the tire from the straight-line distance between the sidewalls (total width of the tire) including all patterns, letters, etc. on the side of the tire when the tire is mounted on a standard rim, with the internal pressure set to 250 kPa and no load applied.

[0035] In addition, the virtual volume of the tire V (mm 3Specifically, the tire cross-sectional width (Wt) can be calculated by the following formula based on the tire outer diameter Dt (mm), tire cross-sectional height (the distance from the bottom of the bead to the outermost surface of the tread, which is half the difference between the tire outer diameter and the nominal rim diameter) Ht (mm), and tire cross-sectional width Wt (mm) when the tire is mounted on a regular rim and the internal pressure is set to 250 kPa with no load applied. V = [(Dt / 2) 2 -{(Dt / 2)-Ht} 2 ]×π×Wt

[0036] 2. Mechanism of effect manifestation in the tire according to the present invention The mechanism by which the effects of the tire according to the present invention are manifested, that is, the mechanism by which the rolling resistance during high-speed running is sufficiently reduced and the durability is sufficiently improved, is presumed to be as follows.

[0037] (1) Tire shape As described above, in the present invention, the tire section width Wt (mm) and the outer diameter Dt (mm) are 2008 ≦(Dt 2 ×π / 4) / Wt≦2827.4 (Equation 1) is satisfied.

[0038] The above formula (1) is the area of ​​the tire when viewed from the side with respect to the cross-sectional width Wt [(Dt / 2) 2 ×π)=(Dt 2 × π / 4) to satisfy the numerical range defined in Equation 1, it is believed that the friction between the tread portion and the road surface can be reduced, thereby achieving low rolling resistance. do.

[0039] However, such narrow tires are subject to large centrifugal forces when traveling at high speeds, which can cause the tire radius to grow significantly while rolling or the tread to become rounded and undergo large deformation.

[0040] Furthermore, as the outside diameter grows, the tread portion may become stretched and weakened, or the amount of deformation of the tread portion may increase as the outside diameter grows, which may result in damage to the tread portion.

[0041] Therefore, in the present invention, the virtual volume V (mm 3 ) and cross-sectional width Wt (mm) are [(V+1.5×10 7 ) / Wt]≦2.88×10 5 It is designed to satisfy (Equation 2).

[0042] In this way, by reducing the virtual volume V of the tire in accordance with the reduction in the tire cross-sectional width Wt and reducing the volume of the tire itself, it is possible to suppress the growth of the outer diameter caused by the expansion of the air inside, reduce the deformation of the tread portion, and reduce heat generation. In addition, since the growth of the outer diameter can be suppressed, it is thought that the tread is less likely to become weak and its ability to withstand damage is enhanced.

[0043] In this case, [(V+2.0×10 7 ) / Wt]≦2.88×10 5 It is more preferable that (Formula 3) is [(V+2.5×10 7 ) / Wt]≦2.88×10 5 It is more preferable that the formula is (Formula 4).

[0044] (2) Rubber composition forming the tread portion In the present invention, the tread portion is further formed of a rubber composition containing a rubber component containing styrene-butadiene rubber and isoprene-based rubber, whereby the styrene-butadiene rubber phase and the isoprene-based rubber phase can be phase-separated and entangled with each other, thereby reducing distortion inside the rubber.

[0045] Furthermore, by setting the loss tangent (30°C tan δ) of the rubber composition measured under conditions of 30°C, a frequency of 10 Hz, an initial strain of 5%, and a dynamic strain rate of 1% to 0.14 or less, heat generation in the tread portion can be reduced. This, together with the ability to reduce the strain inside the rubber as described above, suppresses the rise in tire temperature, suppresses the decrease in durability of the rubber composition itself and the growth in outer diameter associated with temperature rise, and prevents damage to the tire and increases its durability.

[0046] The 30° C. tan δ is more preferably 0.12 or less, and even more preferably 0.10 or less.

[0047] The 30° C. tan δ can be measured, for example, by using a viscoelasticity measuring device, “IPLEXER (registered trademark)” manufactured by GABO.

[0048] [2] More preferred embodiments of the tire according to the present invention The tire according to the present invention can achieve even greater effects by adopting the following aspects.

[0049] 1. Flatness The tire according to the present invention is preferably a tire with an aspect ratio of 40% or more, which increases the height of the side portions of the tire, reduces the contribution of heat generation in the tread portion, and makes the deformation of the tire uniform throughout, thereby sufficiently reducing the total heat generation of the tire. As a result, the rolling resistance during high-speed driving can be further reduced, and the durability of the tire can be further increased.

[0050] The above aspect ratio (%) can be calculated by the following formula using the tire section height Ht (mm) and section width Wt (mm) when the internal pressure is set to 250 kPa. (Ht / Wt) x 100(%)

[0051] The above-mentioned aspect ratio is more preferably 45% or more, even more preferably 47.5% or more, still more preferably 50% or more, particularly preferably 52.5% or more, and most preferably 55% or more.

[0052] 2. Relationship between loss tangent (30℃ tanδ) and cross-sectional width Wt (mm) As the cross-sectional width Wt increases, the contribution of heat generation in the tread increases, making it difficult to control heat generation. Therefore, we investigated the relationship between the loss tangent (30°C tan δ) and the cross-sectional width Wt (mm) and found that if 30°C tan δ × Wt ≦ 30.0 is satisfied, heat generation can be controlled according to the width, further reducing rolling resistance during high-speed driving and further improving the durability of the tire.

[0053] It was also found that 30° C. tan δ×Wt≦25.0 was more preferable.

[0054] 3. Tread grooves The tire according to the present invention has a circumferential groove in the tread portion that extends continuously in the tire circumferential direction, and the groove width L of the circumferential groove in the contact surface of the tread portion is 0 Groove width L at 80% of the maximum depth of the circumferential groove 80 Ratio (L 80 / L 0 ) is preferably 0.3 to 0.7. This makes it possible to suppress the movement of the entire land portion at the bottom surface of the land portion of the tread portion, thereby sufficiently suppressing uneven wear of the tread portion during high-speed running and improving durability. It is more preferably 0.35 to 0.65, even more preferably 0.40 to 0.60, and particularly preferably 0.45 to 0.55.

[0055] The above L 0 and L 80 is the linear distance (L) between the ends of the circumferential grooves on the tread surface of a tire mounted on a regular rim, with an internal pressure of 250 kPa and no load applied. 0), and the minimum distance of the groove wall at 80% of the groove depth (L 80 ) and can be calculated simply by cutting a section of the tire 2 to 4 cm wide in the radial direction and pressing the space between the beads to match the width of the rim.

[0056] It is preferable that the tread portion has a plurality of circumferential grooves, and the total cross-sectional area of ​​the plurality of circumferential grooves is 10 to 30% of the cross-sectional area of ​​the tread portion. This makes it possible to suppress the movement of the tread portion, sufficiently suppress uneven wear of the tread portion during high-speed running, and sufficiently improve durability. It is more preferable that it is 15 to 27%, even more preferable that it is 18 to 25%, and particularly preferable that it is 21 to 23%.

[0057] The cross-sectional area of ​​the circumferential grooves mentioned above refers to the total area defined by the straight line connecting the ends of the tread circumferential grooves and the groove walls when the tire is mounted on a regular rim, the internal pressure is 250 kPa, and the tire is in an unloaded state. In simple terms, the cross-sectional area can be determined by cutting the tire in a radial direction with a width of 2 to 4 cm and pressing the space between the bead portions to match the width of the rim.

[0058] It is also preferable that the tread portion has a plurality of lateral grooves extending in the tire axial direction, and the total volume of the plurality of lateral grooves is 2.0 to 5.0% of the volume of the tread portion. This makes it possible to suppress the movement of the tread portion, sufficiently suppress uneven wear of the tread portion, and improve durability. It is more preferable that it is 2.2 to 4.0%, even more preferable that it is 2.5 to 3.5%, and particularly preferable that it is 2.7 to 3.0%.

[0059] The volume of the lateral grooves mentioned above refers to the total volume of the surfaces connecting the ends of the lateral grooves and the groove walls in a tire mounted on a regular rim with an internal pressure of 250 kPa and no load, and can be calculated simply by calculating the volume of each lateral groove in a state where the tire is cut out in a radial direction with a width of 2 to 4 cm and pressed down between the beads to match the rim width, and multiplying the volume by the number of grooves. The volume of the tread portion can be calculated by calculating the area of ​​the part of the tread portion not including the lateral grooves from the section, multiplying it by the outer diameter, and calculating the difference between the volume of the lateral grooves.

[0060] In order to suppress uneven wear of the tread portion and further improve durability, at least one of these lateral grooves has a ratio of groove width Gw to groove depth Gd (Gw / Gd) of preferably 0.50 to 0.80, more preferably 0.53 to 0.77, even more preferably 0.55 to 0.75, and particularly preferably 0.60 to 0.70.

[0061] The groove width and groove depth of the lateral grooves mentioned above refer to the maximum straight line connecting the tread surface ends of the lateral grooves that is perpendicular to the groove direction and the maximum depth of the lateral grooves when the tire is under no load and the internal pressure is 250 kPa. Simply put, these can be calculated from the state in which the space between the bead portions of a section 2 to 4 cm wide cut out of the tire in the radial direction is pressed down to match the rim width.

[0062] 4. Tire shape In the tire according to the present invention, when the tire is mounted on a regular rim and the internal pressure is set to 250 kPa, the specific outer diameter Dt (mm) is, for example, preferably 515 mm or more, more preferably 558 mm or more, even more preferably 585 mm or more, particularly preferably 658 mm or more, and most preferably 673 mm or more. On the other hand, it is preferably less than 843 mm, more preferably less than 725 mm, even more preferably less than 707 mm, particularly preferably less than 685 mm, and most preferably less than 655 mm.

[0063] The specific cross-sectional width Wt (mm) is, for example, preferably 115 mm or more, more preferably 130 mm or more, even more preferably 150 mm or more, even more preferably 170 mm or more, particularly preferably 185 mm or more, and most preferably 193 mm or more. On the other hand, it is preferably less than 305 mm, more preferably less than 245 mm, even more preferably less than 210 mm, particularly preferably less than 205 mm, and most preferably less than 200 mm.

[0064] Specifically, the cross-sectional height Ht (mm) is, for example, preferably 37 mm or more, more preferably 87 mm or more, and even more preferably 95 mm or more, while it is preferably less than 180 mm, more preferably less than 112 mm, and even more preferably less than 101 mm.

[0065] A specific virtual volume V is, for example, 13,000,000 mm 3 It is preferable that the length is 29,000,000 mm or more. 3 More preferably, it is 36,000,000 mm or more. 3 More preferably, the thickness is 66,000,000 mm or more. 3 Preferably less than 44,000,000 mm 3 Preferably less than 38,800,000 mm 3 It is even more preferable that it is less than 1000 .mu.m.

[0066] In the present invention, in consideration of the stability of the ride comfort during running, (Dt-2×Ht) is preferably 450 (mm) or more, more preferably 470 (mm) or more, and even more preferably 480 (mm) or more. On the other hand, in consideration of the deformation of the tread portion, it is preferably less than 560 (mm), more preferably less than 530 (mm), and even more preferably less than 510 (mm).

[0067] [3] Implementation form Hereinafter, the present invention will be described in detail based on the embodiments.

[0068] 1. Rubber composition forming the tread portion The rubber composition forming the tread portion of the tire according to the present invention can be obtained from the rubber component and other compounding materials described below.

[0069] (1) Rubber component In the present embodiment, the rubber component may be a rubber (polymer) that is generally used in the manufacture of tires, such as styrene-butadiene rubber (SBR), isoprene-based rubber, butadiene rubber (BR), or nitrile rubber (NBR). Among these, it is preferable that the rubber contains styrene-butadiene rubber (SBR) and isoprene-based rubber.

[0070] (a) SBR The content of SBR in 100 parts by mass of the rubber component is, for example, preferably more than 5 parts by mass, more preferably more than 10 parts by mass, from the viewpoint of wet grip performance. On the other hand, from the viewpoint of heat generation during high-speed driving, it is preferably less than 100 parts by mass, more preferably less than 65 parts by mass, even more preferably less than 55 parts by mass, and particularly preferably less than 45 parts by mass. The weight average molecular weight of SBR is, for example, more than 100,000 and less than 2,000,000. For example, from the viewpoint of obtaining good wet grip performance, the styrene content of SBR is preferably more than 5% by mass, more preferably more than 10% by mass, and even more preferably more than 20% by mass. On the other hand, from the viewpoint of heat generation during high-speed driving and durability performance, it is preferably less than 50% by mass, more preferably less than 40% by mass, and even more preferably less than 35% by mass. The vinyl bond amount (1,2-bonded butadiene unit amount) of SBR is, for example, more than 5% by mass and less than 70% by mass. The structure of SBR can be identified (measurement of styrene content and vinyl bond amount) using, for example, a JNM-ECA series device manufactured by JEOL Ltd.

[0071] There are no particular limitations on the SBR, and for example, emulsion-polymerized styrene-butadiene rubber (E-SBR), solution-polymerized styrene-butadiene rubber (S-SBR), etc. may be used. The SBR may be either unmodified SBR or modified SBR.

[0072] The modified SBR may be any SBR having a functional group that interacts with a filler such as silica, and examples thereof include terminal-modified SBR in which at least one end of SBR has been modified with a compound (modifying agent) having the above-mentioned functional group (terminal-modified SBR having the above-mentioned functional group at the end), main-chain-modified SBR in which the main chain has the above-mentioned functional group, main-chain-terminal-modified SBR in which the main chain and at least one end are modified with the above-mentioned modifier, and terminal-modified SBR modified (coupled) with a polyfunctional compound having two or more epoxy groups in the molecule and having a hydroxyl group or epoxy group introduced therein.

[0073] Examples of the functional group include an amino group, an amide group, a silyl group, an alkoxysilyl group, an isocyanate group, an imino group, an imidazole group, a urea group, an ether group, a carbonyl group, an oxycarbonyl group, a mercapto group, a sulfide group, a disulfide group, a sulfonyl group, a sulfinyl group, a thiocarbonyl group, an ammonium group, an imide group, a hydrazo group, an azo group, a diazo group, a carboxyl group, a nitrile group, a pyridyl group, an alkoxy group, a hydroxyl group, an oxy group, an epoxy group, etc. These functional groups may have a substituent.

[0074] Furthermore, as the modified SBR, for example, SBR modified with a compound (modifying agent) represented by the following formula can be used.

[0075] [ka]

[0076] In the formula, R1, R2, and R3 are the same or different and represent an alkyl group, an alkoxy group, a silyloxy group, an acetal group, a carboxyl group (-COOH), a mercapto group (-SH), or a derivative thereof. R4 and R5 are the same or different and represent a hydrogen atom or an alkyl group. R4 and R5 may be bonded to form a ring structure together with the nitrogen atom. n represents an integer.

[0077] As the modified SBR modified with a compound (modifier) ​​represented by the above formula, SBR in which the polymerization terminals (active terminals) of solution-polymerized styrene-butadiene rubber (S-SBR) have been modified with a compound represented by the above formula (such as the modified SBR described in JP 2010-111753 A).

[0078] R1, R2, and R3 are preferably alkoxy groups (preferably alkoxy groups having 1 to 8 carbon atoms, more preferably alkoxy groups having 1 to 4 carbon atoms). R4 and R5 are preferably alkyl groups (preferably alkyl groups having 1 to 3 carbon atoms). n is preferably 1 to 5, more preferably 2 to 4, and even more preferably 3. In addition, when R4 and R5 combine to form a ring structure together with the nitrogen atom, it is preferably a 4- to 8-membered ring. The alkoxy group also includes cycloalkoxy groups (cyclohexyloxy group, etc.) and aryloxy groups (phenoxy group, benzyloxy group, etc.).

[0079] Specific examples of the modifying agent include 2-dimethylaminoethyltrimethoxysilane, 3-dimethylaminopropyltrimethoxysilane, 2-dimethylaminoethyltriethoxysilane, 3-dimethylaminopropyltriethoxysilane, 2-diethylaminoethyltrimethoxysilane, 3-diethylaminopropyltrimethoxysilane, 2-diethylaminoethyltriethoxysilane, 3-diethylaminopropyltriethoxysilane, etc. These may be used alone or in combination of two or more.

[0080] In addition, modified SBR modified with the following compounds (modifiers) can also be used as the modified SBR. Examples of the modifiers include polyglycidyl ethers of polyhydric alcohols such as ethylene glycol diglycidyl ether, glycerin triglycidyl ether, trimethylolethane triglycidyl ether, and trimethylolpropane triglycidyl ether; polyglycidyl ethers of aromatic compounds having two or more phenol groups such as diglycidylated bisphenol A; polyepoxy compounds such as 1,4-diglycidylbenzene, 1,3,5-triglycidylbenzene, and polyepoxidized liquid polybutadiene; epoxy group-containing tertiary amines such as 4,4'-diglycidyl-diphenylmethylamine and 4,4'-diglycidyl-dibenzylmethylamine; diglycidylaniline, N,N'-diglycidyl-4-glycidyloxyaniline, Diglycidyl amino compounds such as diglycidyl orthotoluidine, tetraglycidyl meta-xylylenediamine, tetraglycidyl aminodiphenylmethane, tetraglycidyl-p-phenylenediamine, diglycidyl aminomethylcyclohexane, and tetraglycidyl-1,3-bisaminomethylcyclohexane; amino group-containing acid chlorides such as bis-(1-methylpropyl)carbamic acid chloride, 4-morpholinecarbonyl chloride, 1-pyrrolidinecarbonyl chloride, N,N-dimethylcarbamic acid chloride, and N,N-diethylcarbamic acid chloride; epoxy group-containing silane compounds such as 1,3-bis-(glycidyloxypropyl)-tetramethyldisiloxane and (3-glycidyloxypropyl)-pentamethyldisiloxane;(Trimethylsilyl)[3-(trimethoxysilyl)propyl]sulfide, (trimethylsilyl)[3-(triethoxysilyl)propyl]sulfide, (trimethylsilyl)[3-(trippropoxysilyl)propyl]sulfide, (trimethylsilyl)[3-(tributoxysilyl)propyl]sulfide, (trimethylsilyl)[3-(methyldimethoxysilyl)propyl]sulfide, (trimethylsilyl)[3-(methyldiethoxysilyl)propyl]sulfide, (trimethylsilyl)[3-(methyldipropoxy sulfide group-containing silane compounds such as (trimethylsilyl)[3-(methyldibutoxysilyl)propyl]sulfide and (trimethylsilyl)[3-(methyldibutoxysilyl)propyl]sulfide; N-substituted aziridine compounds such as ethyleneimine and propyleneimine; methyltriethoxysilane, N,N-bis(trimethylsilyl)-3-aminopropyltrimethoxysilane, N,N-bis(trimethylsilyl)-3-aminopropyltriethoxysilane, N,N-bis(trimethylsilyl)aminoethyltrimethoxysilane, N,N-bis(trimethylsilyl)aminoethyltrimethoxysilane, Alkoxysilanes such as thyltriethoxysilane; (thio)benzophenone compounds having amino groups and / or substituted amino groups, such as 4-N,N-dimethylaminobenzophenone, 4-N,N-di-t-butylaminobenzophenone, 4-N,N-diphenylaminobenzophenone, 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, 4,4'-bis(diphenylamino)benzophenone, and N,N,N',N'-bis-(tetraethylamino)benzophenone; Benzaldehyde compounds having an amino group and / or a substituted amino group, such as dimethylaminobenzaldehyde, 4-N,N-diphenylaminobenzaldehyde, 4-N,N-divinylaminobenzaldehyde, etc.; N-substituted pyrrolidones, such as N-methyl-2-pyrrolidone, N-vinyl-2-pyrrolidone, N-phenyl-2-pyrrolidone, Nt-butyl-2-pyrrolidone, N-methyl-5-methyl-2-pyrrolidone, etc.; N-substituted piperidones, such as N-methyl-2-piperidone, N-vinyl-2-piperidone, N-phenyl-2-piperidone, etc.;N-substituted lactams such as N-methyl-ε-caprolactam, N-phenyl-ε-caprolactam, N-methyl-ω-laurylolactam, N-vinyl-ω-laurylolactam, N-methyl-β-propiolactam, and N-phenyl-β-propiolactam; as well as N,N-bis-(2,3-epoxypropoxy)-aniline, 4,4-methylene-bis-(N,N-glycidylaniline), and tris-(2,3-epoxypropyl)-1,3,5-triazine-2,4,6-trione. , N,N-diethylacetamide, N-methylmaleimide, N,N-diethylurea, 1,3-dimethylethyleneurea, 1,3-divinylethyleneurea, 1,3-diethyl-2-imidazolidinone, 1-methyl-3-ethyl-2-imidazolidinone, 4-N,N-dimethylaminoacetophene, 4-N,N-diethylaminoacetophenone, 1,3-bis(diphenylamino)-2-propanone, 1,7-bis(methylethylamino)-4-heptanone, etc. Modification with the above compounds (modifiers) can be carried out by known methods.

[0081] As the SBR, for example, SBR manufactured and sold by Sumitomo Chemical Co., Ltd., JSR Corporation, Asahi Kasei Corporation, Zeon Corporation, etc. can be used. The SBR may be used alone or in combination of two or more kinds.

[0082] (b) Isoprene rubber The content (total content) of isoprene-based rubber in 100 parts by mass of the rubber component is preferably more than 5 parts by mass, more preferably more than 25 parts by mass, even more preferably more than 35 parts by mass, and particularly preferably more than 50 parts by mass, from the viewpoint of obtaining good low heat generation properties and durability during high-speed driving. On the other hand, the upper limit of the content of isoprene-based rubber is not particularly limited, but is preferably less than 100 parts by mass, more preferably less than 80 parts by mass, from the viewpoint of wet grip performance. Examples of isoprene-based rubber include natural rubber (NR), isoprene rubber (IR), modified NR, modified NR, and modified IR.

[0083] As the NR, for example, SIR20, RSS♯3, TSR20, etc., which are common in the tire industry, can be used. As the IR, there is no particular limitation, and for example, IR2200, etc., which are common in the tire industry can be used. As the modified NR, deproteinized natural rubber (DPNR), highly purified natural rubber (UPNR), etc. can be used. As the modified NR, epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), grafted natural rubber, etc. can be used. As the modified IR, epoxidized isoprene rubber, hydrogenated isoprene rubber, grafted isoprene rubber, etc. can be used. These may be used alone or in combination of two or more kinds.

[0084] (c)BR The rubber composition may further contain BR, if necessary. In this case, the content of BR in 100 parts by mass of the rubber component is preferably more than 5 parts by mass, for example, from the viewpoint of wear resistance. On the other hand, from the viewpoint of rolling resistance during high-speed running, it is preferably less than 100 parts by mass, more preferably less than 30 parts by mass, and even more preferably less than 20 parts by mass. The weight average molecular weight of BR is, for example, more than 100,000 and less than 2,000,000. The vinyl bond amount of BR is, for example, more than 1% by mass and less than 30% by mass. The cis amount of BR is, for example, more than 1% by mass and less than 98% by mass. The trans amount of BR is, for example, more than 1% by mass and less than 60% by mass.

[0085] The BR is not particularly limited, and BR with a high cis content (cis content of 90% or more), BR with a low cis content, BR containing syndiotactic polybutadiene crystals, etc. can be used. The BR may be either unmodified BR or modified BR, and the modified BR may be modified BR into which the above-mentioned functional groups have been introduced. These may be used alone or in combination of two or more. The cis content can be measured by infrared absorption spectroscopy.

[0086] As the BR, for example, products from Ube Industries, Ltd., JSR Corporation, Asahi Kasei Corporation, Zeon Corporation, etc. can be used.

[0087] (d) Other rubber components The rubber composition may also contain, as another rubber component, a rubber (polymer) that is generally used in the manufacture of tires, such as nitrile rubber (NBR).

[0088] (2) Compounding materials other than rubber components (a) Filler In the present embodiment, the rubber composition preferably contains a filler. Specific examples of the filler include silica, carbon black, calcium carbonate, talc, alumina, clay, aluminum hydroxide, and mica. Among these, silica and carbon black are preferably used as reinforcing agents. When silica is used, it is preferable to use it in combination with a silane coupling agent.

[0089] (a) Silica The rubber composition preferably contains silica. The BET specific surface area of ​​the silica is preferably 140 m from the viewpoint of obtaining good durability. 2 / g or more is preferable, and 160m 2 On the other hand, from the viewpoint of obtaining good rolling resistance during high-speed driving, a tire having a rolling resistance of 250 m 2 / g or less is preferable, and 220m 2 The BET specific surface area is preferably less than N / g. 2 This is the SA value.

[0090] When silica is used as a reinforcing filler, the content of silica per 100 parts by mass of the rubber component is preferably more than 35 parts by mass, more preferably more than 40 parts by mass, from the viewpoint of obtaining good durability performance, while being preferably less than 70 parts by mass, more preferably less than 65 parts by mass, and even more preferably less than 60 parts by mass, from the viewpoint of obtaining good rolling resistance during high-speed running.

[0091] Examples of silica include dry process silica (anhydrous silica), wet process silica (hydrated silica), etc. Among these, wet process silica is preferred because it has a large number of silanol groups.

[0092] As the silica, for example, products manufactured by Degussa, Rhodia, Tosoh Silica Co., Ltd., Solvay Japan Co., Ltd., Tokuyama Corporation, etc. can be used.

[0093] (b) Silane coupling agent The rubber composition preferably contains a silane coupling agent together with silica. The silane coupling agent is not particularly limited, and examples thereof include bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)disulfide, bis(4-triethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamoyl silane, and the like. Examples of the silyl silane include sulfide-based silanes such as rubamoyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, and 3-triethoxysilylpropyl methacrylate monosulfide; mercapto-based silanes such as 3-mercaptopropyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, and NXT and NXT-Z manufactured by Momentive; vinyl-based silanes such as vinyltriethoxysilane and vinyltrimethoxysilane; amino-based silanes such as 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane; glycidoxy-based silanes such as γ-glycidoxypropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; nitro-based silanes such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; and chloro-based silanes such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane. These may be used alone or in combination of two or more.

[0094] As the silane coupling agent, for example, products available from Degussa, Momentive, Shin-Etsu Silicones, Tokyo Chemical Industry, Azumax, Dow Corning Toray, etc. can be used.

[0095] The content of the silane coupling agent is, for example, more than 3 parts by mass and less than 25 parts by mass relative to 100 parts by mass of silica.

[0096] (c) Carbon black The rubber composition preferably contains carbon black. The amount of carbon black is, for example, more than 1 part by mass and less than 200 parts by mass per 100 parts by mass of the rubber component.

[0097] The carbon black is not particularly limited, and examples thereof include furnace black (furnace carbon black) such as SAF, ISAF, HAF, MAF, FEF, SRF, GPF, APF, FF, CF, SCF and ECF; acetylene black (acetylene carbon black); thermal black (thermal carbon black) such as FT and MT; channel black (channel carbon black) such as EPC, MPC and CC; graphite, etc. These may be used alone or in combination of two or more.

[0098] The nitrogen adsorption specific surface area of ​​carbon black (N 2 SA) is, for example, 30m 2 / g over 250m 2 The carbon black has a dibutyl phthalate (DBP) absorption of, for example, more than 50 ml / 100 g and less than 250 ml / 100 g. The nitrogen adsorption specific surface area of ​​the carbon black is measured according to ASTM D4820-93, and the DBP absorption is measured according to ASTM D2414-93.

[0099] Specific carbon black is not particularly limited, and examples thereof include N134, N110, N220, N234, N219, N339, N330, N326, N351, N550, and N762. Commercially available products include those from Asahi Carbon Co., Ltd., Cabot Japan Co., Ltd., Tokai Carbon Co., Ltd., Mitsubishi Chemical Co., Ltd., Lion Co., Ltd., Shin-Nichika Carbon Co., Ltd., Columbia Carbon Co., Ltd., and the like. These may be used alone or in combination of two or more kinds.

[0100] (D) Other fillers In addition to the above-mentioned carbon black and silica, the rubber composition may further contain fillers commonly used in the tire industry, such as calcium carbonate, talc, alumina, clay, aluminum hydroxide, mica, etc. The content of these fillers is, for example, more than 0.1 parts by mass and less than 200 parts by mass per 100 parts by mass of the rubber component.

[0101] (b) Softener The rubber composition may contain oil (including extender oil) or liquid rubber as a softener. The total content of these is preferably more than 5 parts by mass, more preferably more than 10 parts by mass, per 100 parts by mass of the rubber component. On the other hand, it is preferably less than 70 parts by mass, more preferably less than 50 parts by mass, and even more preferably less than 30 parts by mass. The oil content includes the amount of oil contained in the rubber (oil-extended rubber).

[0102] Examples of oils include mineral oils (generally called process oils), vegetable oils, and mixtures thereof. Examples of mineral oils (process oils) that can be used include paraffin-based process oils, aromatic process oils, and naphthenic process oils. Examples of vegetable oils include castor oil, cottonseed oil, linseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, peanut oil, rosin, pine oil, pine tar, tall oil, corn oil, rice oil, safflower oil, sesame oil, olive oil, sunflower oil, palm kernel oil, camellia oil, jojoba oil, macadamia nut oil, and tung oil. These may be used alone or in combination of two or more.

[0103] Specific examples of process oils (mineral oils) that can be used include products from Idemitsu Kosan Co., Ltd., Sankyo Yuka Kogyo Co., Ltd., Japan Energy Co., Ltd., Orisoi Co., Ltd., H&R Co., Ltd., Toyokuni Oil Mills Co., Ltd., Showa Shell Sekiyu K.K., Fuji Kosan Co., Ltd., and the like.

[0104] The liquid rubbers mentioned as softeners are polymers that are in a liquid state at room temperature (25° C.) and contain the same monomers as solid rubbers. Examples of liquid rubbers include farnesene-based polymers, liquid diene-based polymers, and hydrogenated products thereof.

[0105] Farnesene polymers are polymers obtained by polymerizing farnesene and contain structural units based on farnesene. Farnesene has isomers such as α-farnesene ((3E,7E)-3,7,11-trimethyl-1,3,6,10-dodecatetraene) and β-farnesene (7,11-dimethyl-3-methylene-1,6,10-dodecatriene).

[0106] The farnesene-based polymer may be a homopolymer of farnesene (farnesene homopolymer) or a copolymer of farnesene and a vinyl monomer (farnesene-vinyl monomer copolymer).

[0107] Examples of liquid diene polymers include liquid styrene-butadiene copolymer (liquid SBR), liquid butadiene polymer (liquid BR), liquid isoprene polymer (liquid IR), and liquid styrene-isoprene copolymer (liquid SIR).

[0108] The liquid diene polymer has a weight average molecular weight (Mw) of, for example, 1.0×10 3 Super, 2.0×10 5 In this specification, the Mw of the liquid diene polymer is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).

[0109] The amount of the liquid rubber (total amount of the liquid farnesene polymer, the liquid diene polymer, etc.) is, for example, more than 1 part by mass and less than 100 parts by mass per 100 parts by mass of the rubber component.

[0110] As the liquid rubber, for example, products of Kuraray Co., Ltd., Cray Valley Co., Ltd., etc. can be used.

[0111] (c) Resin component In addition, the rubber composition preferably contains a resin component as necessary. The resin component may be solid or liquid at room temperature, and specific examples of the resin component include styrene resin, coumarone resin, terpene resin, C5 resin, C9 resin, C5C9 resin, acrylic resin, etc., and two or more of them may be used in combination. The content of the resin component is preferably more than 2 parts by mass and less than 45 parts by mass, more preferably less than 30 parts by mass, based on 100 parts by mass of the rubber component.

[0112] The styrene resin is a polymer using a styrene monomer as a constituent monomer, and examples thereof include polymers polymerized with a styrene monomer as the main component (50% by mass or more).Specific examples thereof include homopolymers obtained by polymerizing each of the styrene monomers (styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, p-methoxystyrene, p-tert-butylstyrene, p-phenylstyrene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, etc.) alone, copolymers obtained by copolymerizing two or more kinds of styrene monomers, and copolymers of a styrene monomer and another monomer that can be copolymerized therewith.

[0113] Examples of the other monomer include acrylonitriles such as acrylonitrile and methacrylonitrile, unsaturated carboxylic acids such as acrylics and methacrylic acid, unsaturated carboxylic acid esters such as methyl acrylate and methyl methacrylate, dienes such as chloroprene and butadiene-isoprene, olefins such as 1-butene and 1-pentene, α,β-unsaturated carboxylic acids such as maleic anhydride, or acid anhydrides thereof.

[0114] As the coumarone resin, coumarone-indene resin is preferably used. Coumarone-indene resin is a resin containing coumarone and indene as monomer components constituting the skeleton (main chain) of the resin. Other monomer components contained in the skeleton besides coumarone and indene include styrene, α-methylstyrene, methylindene, vinyltoluene, etc.

[0115] The amount of the coumarone-indene resin per 100 parts by mass of the rubber component is, for example, more than 1.0 part by mass and less than 50.0 parts by mass.

[0116] The hydroxyl value (OH value) of the coumarone-indene resin is, for example, more than 15 mgKOH / g and less than 150 mgKOH / g. The OH value is the amount of potassium hydroxide required to neutralize acetic acid bonded to hydroxyl groups when acetylating 1 g of the resin, expressed in milligrams, and is a value measured by potentiometric titration (JIS K 0070:1992).

[0117] The softening point of the coumarone-indene resin is, for example, more than 30° C. and less than 160° C. The softening point is the temperature at which the ball drops when the softening point specified in JIS K 6220-1:2001 is measured using a ring and ball softening point tester.

[0118] Terpene resins include polyterpene, terpene phenol, and aromatic modified terpene resins. Polyterpenes are resins obtained by polymerizing terpene compounds and their hydrogenated products. Terpene compounds are (C 5 H 8 ) n The hydrocarbons and their oxygen-containing derivatives are represented by the following composition: Monoterpenes (C 10 H 16 ), sesquiterpenes (C 15 H 24 ), diterpenes (C 20 H 32), and examples thereof include α-pinene, β-pinene, dipentene, limonene, myrcene, alloocimene, ocimene, α-phellandrene, α-terpinene, γ-terpinene, terpinolene, 1,8-cineole, 1,4-cineole, α-terpineol, β-terpineol, and γ-terpineol.

[0119] Examples of polyterpenes include terpene resins such as α-pinene resin, β-pinene resin, limonene resin, dipentene resin, and β-pinene / limonene resin, which are made from the above-mentioned terpene compounds, as well as hydrogenated terpene resins obtained by hydrogenating the terpene resins. Examples of terpene phenols include resins obtained by copolymerizing the above-mentioned terpene compounds with phenolic compounds, and resins obtained by hydrogenating the above-mentioned resins, and specifically include resins obtained by condensing the above-mentioned terpene compounds, phenolic compounds, and formalin. Examples of phenolic compounds include, for example, phenol, bisphenol A, cresol, and xylenol. Examples of aromatic modified terpene resins include resins obtained by modifying terpene resins with aromatic compounds, and resins obtained by hydrogenating the above-mentioned resins. The aromatic compound is not particularly limited as long as it is a compound having an aromatic ring, and examples thereof include phenolic compounds such as phenol, alkylphenols, alkoxyphenols, and phenols containing an unsaturated hydrocarbon group; naphthol compounds such as naphthol, alkylnaphthols, alkoxynaphthols, and naphthols containing an unsaturated hydrocarbon group; styrene derivatives such as styrene, alkylstyrenes, alkoxystyrenes, and styrenes containing an unsaturated hydrocarbon group; coumarone, indene, and the like.

[0120] "C5 resin" refers to a resin obtained by polymerizing a C5 fraction. Examples of C5 fractions include petroleum fractions having 4 to 5 carbon atoms, such as cyclopentadiene, pentene, pentadiene, and isoprene. As a C5 petroleum resin, dicyclopentadiene resin (DCPD resin) is preferably used.

[0121] The term "C9 resin" refers to a resin obtained by polymerizing a C9 fraction, and may be a resin obtained by hydrogenating or modifying the resin. Examples of C9 fractions include petroleum fractions having 8 to 10 carbon atoms, such as vinyltoluene, alkylstyrene, indene, and methylindene. Specific examples of suitable resins include coumarone-indene resins, coumarone resins, indene resins, and aromatic vinyl resins. As aromatic vinyl resins, homopolymers of α-methylstyrene or styrene or copolymers of α-methylstyrene and styrene are preferred, and copolymers of α-methylstyrene and styrene are more preferred, because they are economical, easy to process, and have excellent heat generation properties. As aromatic vinyl resins, for example, those commercially available from Kraton, Eastman Chemical, etc. can be used.

[0122] The term "C5C9 resin" refers to a resin obtained by copolymerizing the C5 fraction and the C9 fraction, and may be a hydrogenated or modified resin. Examples of the C5 fraction and the C9 fraction include the petroleum fractions. As the C5C9 resin, for example, those commercially available from Tosoh Corporation, LUHUA, etc. can be used.

[0123] The acrylic resin is not particularly limited, but for example, a solventless acrylic resin can be used.

[0124] Examples of the solvent-free acrylic resin include (meth)acrylic resins (polymers) synthesized by high-temperature continuous polymerization (high-temperature continuous bulk polymerization) (methods described in U.S. Pat. No. 4,414,370, JP-A-59-6207, JP-B-5-58005, JP-A-1-313522, U.S. Pat. No. 5,010,166, and Toa Gosei Kenkyuu Nenpo TREND 2000 Vol. 3, p. 42-45, etc.) using as little secondary raw material as possible, such as polymerization initiators, chain transfer agents, and organic solvents. In the present invention, (meth)acrylic means methacryl and acrylic.

[0125] Examples of monomer components constituting the acrylic resin include (meth)acrylic acid, (meth)acrylic acid esters (alkyl esters, aryl esters, aralkyl esters, etc.), (meth)acrylamide, and (meth)acrylic acid derivatives such as (meth)acrylamide derivatives.

[0126] In addition, aromatic vinyls such as styrene, α-methylstyrene, vinyltoluene, vinylnaphthalene, divinylbenzene, trivinylbenzene, and divinylnaphthalene may be used together with (meth)acrylic acid or a (meth)acrylic acid derivative as a monomer component constituting the acrylic resin.

[0127] The acrylic resin may be a resin composed only of a (meth)acrylic component, or a resin containing components other than the (meth)acrylic component as constituent elements. The acrylic resin may have a hydroxyl group, a carboxyl group, a silanol group, or the like.

[0128] Examples of the resin component that can be used include products from Maruzen Petrochemical Co., Ltd., Sumitomo Bakelite Co., Ltd., Yasuhara Chemical Co., Ltd., Tosoh Corporation, Rutgers Chemicals, BASF, Arizona Chemical Company, Nippon Paint Chemical Co., Ltd., Nippon Shokubai Co., Ltd., JX Energy Corporation, Arakawa Chemical Industries, Ltd., and Taoka Chemical Co., Ltd.

[0129] (d) Antioxidants The rubber composition preferably contains an antioxidant. The content of the antioxidant is, for example, more than 1 part by mass and less than 10 parts by mass per 100 parts by mass of the rubber component.

[0130] Examples of the antioxidant include naphthylamine-based antioxidants such as phenyl-α-naphthylamine; diphenylamine-based antioxidants such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, and N,N'-di-2-naphthyl-p-phenylenediamine. p-phenylenediamine-based antioxidants such as quinolinone, quinoline-based antioxidants such as polymers of 2,2,4-trimethyl-1,2-dihydroquinoline, monophenol-based antioxidants such as 2,6-di-t-butyl-4-methylphenol and styrenated phenol, and bis-, tris-, and polyphenol-based antioxidants such as tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane. These may be used alone or in combination of two or more.

[0131] As the antioxidant, for example, products available from Seiko Chemical Co., Ltd., Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Industry Co., Ltd., Flexis, etc. can be used.

[0132] (e) Stearic acid The rubber composition may contain stearic acid. The content of stearic acid is, for example, more than 0.5 parts by mass and less than 10.0 parts by mass with respect to 100 parts by mass of the rubber component. As the stearic acid, a conventionally known product can be used, for example, a product from NOF Corporation, NOF Corporation, Kao Corporation, FUJIFILM Wako Pure Chemical Industries, Ltd., Chiba Fatty Acid Co., Ltd., etc. can be used.

[0133] (f) Zinc oxide The rubber composition may contain zinc oxide. The content of zinc oxide is, for example, more than 0.5 parts by mass and less than 10 parts by mass with respect to 100 parts by mass of the rubber component. As the zinc oxide, a conventionally known product can be used, for example, a product of Mitsui Mining & Smelting Co., Ltd., Toho Zinc Co., Ltd., Hakusui Tech Co., Ltd., Seido Chemical Industry Co., Ltd., Sakai Chemical Industry Co., Ltd., etc. can be used.

[0134] (g) Wax The rubber composition preferably contains wax. The content of the wax per 100 parts by mass of the rubber component is, for example, 0.5 to 20 parts by mass, preferably 1.0 to 15 parts by mass, and more preferably 1.5 to 10 parts by mass.

[0135] The wax is not particularly limited, and examples thereof include petroleum waxes such as paraffin wax and microcrystalline wax, natural waxes such as vegetable wax and animal wax, synthetic waxes such as polymers of ethylene, propylene, etc. These may be used alone or in combination of two or more kinds.

[0136] As the wax, for example, products from Ouchi Shinko Chemical Industry Co., Ltd., Nippon Seiro Co., Ltd., Seiko Chemical Co., Ltd., etc. can be used.

[0137] (h) Crosslinking agents and vulcanization accelerators The rubber composition preferably contains a crosslinking agent such as sulfur, etc. The content of the crosslinking agent is, for example, more than 0.1 parts by mass and less than 10.0 parts by mass per 100 parts by mass of the rubber component.

[0138] Examples of sulfur include powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, soluble sulfur, etc., which are commonly used in the rubber industry. These may be used alone or in combination of two or more kinds.

[0139] As sulfur, for example, products from Tsurumi Chemical Industry Co., Ltd., Karuizawa Sulfur Co., Ltd., Shikoku Chemical Industry Co., Ltd., Flexis Corporation, Nippon Kanritsu Kogyo Co., Ltd., Hosoi Chemical Industry Co., Ltd., etc. can be used.

[0140] Examples of crosslinking agents other than sulfur include vulcanizing agents containing sulfur atoms, such as TACKIROL V200 manufactured by Taoka Chemical Co., Ltd., DURALINK HTS (sodium 1,6-hexamethylenedithiosulfate dihydrate) manufactured by Flexsys, and KA9188 (1,6-bis(N,N'-dibenzylthiocarbamoyldithio)hexane) manufactured by LANXESS, as well as organic peroxides such as dicumyl peroxide.

[0141] The rubber composition preferably contains a vulcanization accelerator. The content of the vulcanization accelerator is, for example, more than 0.3 parts by mass and less than 10.0 parts by mass per 100 parts by mass of the rubber component.

[0142] Examples of the vulcanization accelerator include thiazole-based vulcanization accelerators such as 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, and N-cyclohexyl-2-benzothiazyl sulfenamide; thiuram-based vulcanization accelerators such as tetramethylthiuram disulfide (TMTD), tetrabenzylthiuram disulfide (TBzTD), and tetrakis(2-ethylhexyl)thiuram disulfide (TOT-N); sulfenamide-based vulcanization accelerators such as N-cyclohexyl-2-benzothiazole sulfenamide, Nt-butyl-2-benzothiazolyl sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, and N,N'-diisopropyl-2-benzothiazole sulfenamide; and guanidine-based vulcanization accelerators such as diphenyl guanidine, di-orthotolyl guanidine, and orthotolyl biguanidine. These may be used alone or in combination of two or more kinds.

[0143] (i) Other In addition to the above components, the rubber composition may further contain additives commonly used in the tire industry, such as fatty acid metal salts, carboxylate metal salts, organic peroxides, etc. The content of these additives is, for example, more than 0.1 parts by mass and less than 200 parts by mass per 100 parts by mass of the rubber component.

[0144] 2. Preparation of tread rubber composition The rubber composition is produced by a general method, for example, a manufacturing method including a base kneading step of kneading a rubber component with a filler such as silica or carbon black, and a finish kneading step of kneading the kneaded product obtained in the base kneading step with a crosslinking agent.

[0145] The kneading can be carried out using a known (internal) kneading machine such as a Banbury mixer, a kneader, or an open roll.

[0146] The kneading temperature in the base kneading step is, for example, more than 50° C. and less than 200° C., and the kneading time is, for example, more than 30 seconds and less than 30 minutes. In the base kneading step, in addition to the above-mentioned components, compounding agents conventionally used in the rubber industry, for example, softeners such as oil, stearic acid, zinc oxide, antioxidants, waxes, vulcanization accelerators, etc., may be appropriately added and kneaded as necessary.

[0147] In the final kneading step, the kneaded product obtained in the base kneading step is kneaded with a crosslinking agent. The kneading temperature in the final kneading step is, for example, higher than room temperature and lower than 80° C., and the kneading time is, for example, longer than 1 minute and shorter than 15 minutes. In the final kneading step, in addition to the above components, a vulcanization accelerator, zinc oxide, etc. may be appropriately added and kneaded as necessary.

[0148] 3. Tire manufacturing The tire of the present invention is manufactured by a conventional method using the unvulcanized rubber composition obtained through the above-mentioned finish mixing step. That is, the unvulcanized rubber composition is extruded to match the shape of the tread, and molded together with other tire components in a tire building machine by a conventional method to produce an unvulcanized tire.

[0149] Specifically, an inner liner as a member for ensuring the airtightness of the tire, a carcass as a member for enduring the load, impact, and filled air pressure received by the tire, and a belt as a member for tightly fastening the carcass and increasing the rigidity of the tread are wound around a molding drum, and both ends of the carcass are fixed to both side edges, and bead portions as members for fixing the tire to the rim are arranged. After molding into a toroidal shape, the tread is attached to the center of the outer periphery, and sidewall portions as members for protecting the carcass and enduring bending are attached to the radially outer side, to produce an unvulcanized tire.

[0150] In this embodiment, it is preferable to provide an inclined belt layer extending at an angle of 15° to 30° with respect to the tire circumferential direction as the belt, which ensures the durability of the tire and can sufficiently maintain the rigidity of the tread. In addition, since the tire can be restrained in the circumferential direction, it is easy to suppress the growth of the outer diameter.

[0151] The unvulcanized tire thus produced is then heated and pressurized in a vulcanizer to obtain a tire. The vulcanization step can be carried out by applying a known vulcanization method. The vulcanization temperature is, for example, more than 120°C and less than 200°C, and the vulcanization time is, for example, more than 5 minutes and less than 15 minutes.

[0152] At this time, the tire is molded into a shape that satisfies the above-mentioned (Equation 1) and (Equation 2) when mounted on a regular rim and the internal pressure is set to 250 kPa.

[0153] Specific examples of tires that can satisfy the above (Formula 1) and (Formula 2) include tires with size descriptions such as 145 / 60R18, 145 / 60R19, 155 / 55R18, 155 / 55R19, 155 / 70R17, 155 / 70R19, 165 / 55R20, 165 / 55R21, 165 / 60R19, 165 / 65R19, 165 / 70R18, 175 / 55R19, 175 / 55R20, 175 / 55R22, 175 / 60R18, 185 / 55R19, 185 / 60R20, 195 / 50R20, and 195 / 55R20.

[0154] In the present embodiment, among tires that can satisfy (Equation 1) and (Equation 2), it is preferable to apply the present invention to pneumatic tires for passenger cars, and by satisfying these equations, the rolling resistance during high-speed driving is sufficiently reduced, and the present invention can more suitably contribute to solving the problem of the present invention, which is to provide a pneumatic tire with sufficiently improved durability. EXAMPLES

[0155] The present invention will now be described more specifically with reference to examples.

[0156] [Experiment 1] In this experiment, a tire of size 175 was produced and evaluated.

[0157] 1. Production of rubber composition for tread First, a rubber composition for a tread was produced.

[0158] (1) Compounding materials First, the following blended materials were prepared.

[0159] (a) Rubber component (a) NR:TSR20 (b) SBR: Modified solution-polymerized SBR prepared according to the method described in the next paragraph. (Styrene content: 30% by mass, vinyl bond content: 52% by mass, Mw: 250,000) (c) BR: UBEPOL-BR150 manufactured by Ube Industries, Ltd.

[0160] The above SBR was prepared according to the procedure shown below. First, cyclohexane, tetrahydrofuran, styrene, and 1,3-butadiene were charged into a nitrogen-substituted autoclave reactor. After adjusting the temperature of the reactor contents to 20°C, n-butyllithium was added to start polymerization. Polymerization was carried out under adiabatic conditions, and the maximum temperature reached 85°C. When the polymerization conversion rate reached 99%, 1,3-butadiene was added, and polymerization was continued for another 5 minutes, after which N,N-bis(trimethylsilyl)-3-aminopropyltriethoxysilane was added as a modifier to carry out the reaction. After the polymerization reaction was completed, 2,6-di-tert-butyl-p-cresol was added. Next, the solvent was removed by steam stripping, and the mixture was dried with a heated roll adjusted to 110°C to obtain SBR.

[0161] (b) Compounding materials other than rubber components (a) Carbon black: Diablack N220 manufactured by Mitsubishi Chemical Corporation (b) Silica: Ultrasil VN3 manufactured by Evonik (BET specific surface area: 165m 2 / g) (c) Silane coupling agent: Degussa Si266 (Bis(3-triethoxysilylpropyl) disulfide) (d) Oil: Process X-140 manufactured by Japan Energy Co., Ltd. (E) Resin (polymer component): SA85 manufactured by Arizona Chemical Company (α-methylstyrene resin) (F) Wax: Ozoace 0355 manufactured by Nippon Seiro Co., Ltd. (G) Anti-aging agent-1: Nocrac 6C manufactured by Ouchi Shinko Chemical Industry Co., Ltd. (N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine) (H) Anti-aging agent-2: Nocrac 224 manufactured by Ouchi Shinko Chemical Industry Co., Ltd. (2,2,4-trimethyl-1,2-dihydroquinoline polymer) (i) Zinc oxide: Zinc oxide No. 1 manufactured by Mitsui Mining & Smelting Co., Ltd. (J) Stearic acid: NOF Corp.'s "Tsubaki" stearic acid (K) Crosslinking agents and vulcanization accelerators Sulfur: Powdered sulfur manufactured by Tsurumi Chemical Industry Co., Ltd. Vulcanization accelerator-1: Noccela CZ-G (CBS) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. (N-cyclohexyl-2-benzothiazolyl sulfenamide) Vulcanization accelerator-2: Noccela D (DPG) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. (1,3-Diphenylguanidine)

[0162] (2) Production of Rubber Composition According to the composition shown in Tables 1 and 2, materials other than sulfur and vulcanization accelerator were kneaded for 5 minutes at 150°C using a Banbury mixer to obtain a kneaded mixture. Each compounding amount is in parts by mass.

[0163] 2. Tire manufacturing Next, sulfur and a vulcanization accelerator were added to the obtained kneaded product, and the mixture was kneaded for 5 minutes at 80°C using an open roll to obtain a tread rubber composition. A tread was formed using the obtained tread rubber composition, and the tread was laminated together with other tire components to form an unvulcanized tire, which was press-vulcanized for 10 minutes at 170°C to produce each test tire of size 175 type (Examples 1-1 to 1-5 and Comparative Examples 1-1 to 1-7).

[0164] In addition, for each test tire, the above-mentioned (L 80 / L 0 ) was 0.5, the total cross-sectional area of ​​the circumferential grooves was 22% of the cross-sectional area of ​​the tread portion, and the total volume of the lateral grooves, including lateral grooves with a groove width / groove depth ratio of 0.65, was 3.5% of the volume of the tread portion.

[0165] 3. Calculation of parameters After that, the outer diameter Dt (mm), section width Wt (mm), section height Ht (mm), and aspect ratio (%) of each test tire were obtained, and the virtual volume V (mm 3 ) was obtained. In addition, rubber test pieces for viscoelasticity measurement were prepared by cutting out a length of 20 mm, width of 4 mm, and thickness of 2 mm from the rubber layer of the tread portion of each test tire, with the long side in the tire circumferential direction. For each rubber test piece, tan δ (30°C tan δ) was measured using an Iplexer series manufactured by GABO under the conditions of 30°C, a frequency of 10 Hz, an initial strain of 5%, and a dynamic strain of 1%. The results are shown in Tables 1 and 2.

[0166] And then, (Dt-2×Ht), (Dt 2 ×π / 4) / Wt, (V+1.5×10 7 ) / Wt, (V+2.0×10 7 ) / Wt, (V+2.5×10 7 ) / Wt and 30°C tan δ×Wt were calculated. The results are shown in Tables 1 and 2.

[0167] 4.Performance evaluation test (1) Evaluation of rolling resistance during high-speed driving Each test tire was fitted to all wheels of a vehicle (a domestically produced FF vehicle with an engine displacement of 2000cc) and filled with air to an internal pressure of 250kPa. The vehicle was then driven around a test course on a dry surface for 10km at a speed of 100km / h, after which the accelerator was released and the distance from when the accelerator was turned off until the vehicle came to a halt was measured as the rolling resistance during high-speed driving.

[0168] Next, the rolling resistance during high-speed driving was relatively evaluated by indexing the results of Comparative Examples 1-7, which were set at 100, according to the following formula. The larger the value, the longer the distance from when the accelerator was released until the vehicle stopped, the smaller the rolling resistance in the steady state, and the more excellent the fuel economy. Rolling resistance = [(measurement result of test tire) / (measurement result of comparative example 1-7)] x 100

[0169] (2) Evaluation of durability Each test tire was fitted to all wheels of a vehicle (domestic FF vehicle, 2000cc displacement) and filled with air to an internal pressure of 250kPa. The vehicle was then overloaded and driven around a test course on a dry road surface at a speed of 50km / h for 10 laps, and then repeatedly driven over uneven surfaces at a speed of 80km / h. The vehicle then went around again at a speed of 50km / h, and the speed was gradually increased, and the speed at which the driver felt something was wrong was measured.

[0170] Next, the results of Comparative Examples 1-7 were set as 100, and the durability was relatively evaluated by indexing it according to the following formula. A larger value indicates better durability. Durability = [(Test tire measurement results) / (Comparative example 1-7 measurement results)] x 100

[0171] (3) Overall evaluation The results of the evaluations (1) and (2) above were summed up to determine the overall evaluation.

[0172] (4) Evaluation results The results of each evaluation are shown in Tables 1 and 2.

[0173] [Table 1]

[0174] [Table 2]

[0175] [Experiment 2] In this experiment, a tire of size 195 was produced and evaluated.

[0176] In the same manner as in Experiment 1, the test tires of Examples 2-1 to 2-5 and Comparative Examples 2-1 to 2-7 shown in Tables 3 and 4 were manufactured, and then the parameters were determined in the same manner. Then, the performance evaluation test was conducted and evaluated in the same manner. In this experiment, the result of Comparative Example 2-7 was set as 100 and the evaluation was performed. The results of each evaluation are shown in Tables 3 and 4.

[0177] [Table 3]

[0178] [Table 4]

[0179] [Experiment 3] In this experiment, a 225 size tire was produced and evaluated.

[0180] In the same manner as in Experiment 1, the test tires of Examples 3-1 to 3-5 and Comparative Examples 3-1 to 3-7 shown in Tables 5 and 6 were manufactured, and then the parameters were determined in the same manner. Then, the performance evaluation test was carried out in the same manner. In this experiment, the result of Comparative Example 3-7 was set as 100 and the evaluation was carried out. The results of each evaluation are shown in Tables 5 and 6.

[0181] [Table 5]

[0182] [Table 6]

[0183] [Summary of Experiments 1-3] The results of Experiments 1 to 3 (Tables 1 to 6) show that, regardless of the tire size, 175 size, 195 size, or 225 size, when the above-mentioned (Equation 1) and (Equation 2) are satisfied, a pneumatic tire can be provided in which the rolling resistance during high-speed driving is sufficiently reduced and durability is sufficiently improved.

[0184] It can also be seen that by satisfying the requirements set forth in claim 2 and onwards, a tire can be provided which has further improved rolling resistance and durability during high-speed running.

[0185] On the other hand, if either (Formula 1) or (Formula 2) is not satisfied, it is not possible to sufficiently reduce the rolling resistance during high-speed running, and it is also not possible to sufficiently improve durability.

[0186] [Experiment 4] Next, three types of tires (Example 4-1 to Example 4-3) that have no significant difference in the relationship between the virtual volume V and the cross-sectional width Wt were manufactured with the same compounding and evaluated in the same manner. Here, the result of the tire of Example 4-3 was set to 100. The results of each evaluation are shown in Table 7.

[0187] [Table 7]

[0188] From Table 7, it can be seen that when there is no significant difference in the relationship between the virtual volume V and the cross-sectional width Wt, as the cross-sectional width Wt becomes smaller, such as less than 205 mm or less than 200 mm, and as the aspect ratio becomes higher, both the rolling resistance and durability during high-speed driving are improved, resulting in a significant effect.

[0189] Although the present invention has been described above based on the embodiment, the present invention is not limited to the above embodiment. Various modifications can be made to the above embodiment within the same and equivalent scope of the present invention.

Claims

1. A pneumatic tire having a tread portion, the rubber layer of the tread portion is formed from a rubber composition that includes a rubber component containing a styrene-butadiene rubber and an isoprene-based rubber, and has a loss tangent (30°C tan δ) of 0.14 or less, measured under conditions of 30°C, a frequency of 10 Hz, an initial strain of 5%, and a dynamic strain rate of 1%; When the tire is mounted on a regular rim and the internal pressure is set to 250 kPa, the cross-sectional width of the tire is Wt (mm), the outer diameter is Dt (mm), and the volume of the space occupied by the tire is the virtual volume V (mm 3 ), the following (Formula 1) and (Formula 4) are satisfied: 2008≦(Dt 2 ×π / 4) / Wt≦2827.4 (Formula 1) [(V+2.5×10 7 ) / Wt]≦2.88×10 5 ・・・・・・(Formula 4)

2. A pneumatic tire having a tread portion, the rubber layer of the tread portion is formed from a rubber composition containing a rubber component including a styrene-butadiene rubber and an isoprene-based rubber, and having a loss tangent (30°C tan δ) of 0.10 or less measured under conditions of 30°C, a frequency of 10 Hz, an initial strain of 5%, and a dynamic strain rate of 1%, A pneumatic tire characterized by satisfying the following (Equation 1) and (Equation 2), where the cross-sectional width of the tire when mounted on a regular rim and the internal pressure is 250 kPa is Wt (mm), the outer diameter is Dt (mm), and the volume of the space occupied by the tire is a virtual volume V (mm3). 2008≦(Dt 2 ×π / 4) / Wt≦2827.4 (Formula 1) [(V+1.5×10 7 ) / Wt]≦2.88×10 5 (Formula 2)

3. A pneumatic tire having a tread portion, the rubber layer of the tread portion is formed from a rubber composition that includes a rubber component containing a styrene-butadiene rubber and an isoprene-based rubber, and has a loss tangent (30°C tan δ) of 0.14 or less, measured under conditions of 30°C, a frequency of 10 Hz, an initial strain of 5%, and a dynamic strain rate of 1%; When the tire is mounted on a regular rim and the internal pressure is set to 250 kPa, the tire cross-sectional width is Wt (mm), the outer diameter is Dt (mm), and the volume of the space occupied by the tire is a virtual volume V (mm3). The following formulas (1) and (2) are satisfied: The tire has a circumferential groove in the tread portion that extends continuously in the circumferential direction of the tire. A groove width L of the circumferential groove at the ground contact surface of the tread portion 0 The groove width L at a depth of 80% of the maximum depth of the circumferential groove 80 The ratio (L 80 / L 0 ) is 0.3 to 0.

7. 2008≦(Dt 2 ×π / 4) / Wt≦2827.4 (Formula 1) [(V+1.5×10 7 ) / Wt]≦2.88×10 5 (Formula 2)

4. A pneumatic tire having a tread portion, the rubber layer of the tread portion is formed from a rubber composition that includes a rubber component containing a styrene-butadiene rubber and an isoprene-based rubber, and has a loss tangent (30°C tan δ) of 0.14 or less, measured under conditions of 30°C, a frequency of 10 Hz, an initial strain of 5%, and a dynamic strain rate of 1%; When the tire is mounted on a regular rim and the internal pressure is set to 250 kPa, the tire cross-sectional width is Wt (mm), the outer diameter is Dt (mm), and the volume of the space occupied by the tire is a virtual volume V (mm3). The following formulas (1) and (2) are satisfied: The tire has a plurality of circumferential grooves in the tread portion, the circumferential grooves extending continuously in the tire circumferential direction. A pneumatic tire characterized in that a total cross-sectional area of ​​the plurality of circumferential grooves is 10 to 30% of a cross-sectional area of ​​the tread portion. 2008≦(Dt 2 ×π / 4) / Wt≦2827.4 (Formula 1) [(V+1.5×10 7 ) / Wt]≦2.88×10 5 (Formula 2)

5. A pneumatic tire having a tread portion, the rubber layer of the tread portion is formed from a rubber composition that includes a rubber component containing a styrene-butadiene rubber and an isoprene-based rubber, and has a loss tangent (30°C tan δ) of 0.14 or less, measured under conditions of 30°C, a frequency of 10 Hz, an initial strain of 5%, and a dynamic strain rate of 1%; When the tire is mounted on a regular rim and the internal pressure is set to 250 kPa, the tire cross-sectional width is Wt (mm), the outer diameter is Dt (mm), and the volume of the space occupied by the tire is a virtual volume V (mm3). The following formulas (1) and (2) are satisfied: The tire has a plurality of axially extending lateral grooves in the tread portion, A pneumatic tire characterized in that a total volume of the plurality of lateral grooves is 2.0 to 5.0% of a volume of the tread portion. 2008≦(Dt 2 ×π / 4) / Wt≦2827.4 (Formula 1) [(V+1.5×10 7 ) / Wt]≦2.88×10 5 (Formula 2)

6. 6. The pneumatic tire according to claim 5, wherein at least one of the lateral grooves has a groove width / groove depth ratio of 0.50 to 0.

80.

7. 7. The pneumatic tire according to claim 1, wherein the 30° C. tan δ is 0.12 or less.

8. The pneumatic tire according to any one of claims 1 to 7, characterized in that, when the outer diameter of the tire is Dt (mm) and the cross-sectional height of the tire is Ht (mm) when the tire is mounted on a regular rim and the internal pressure is 250 kPa, (Dt - 2 x Ht) is 470 (mm) or more.

9. 9. The pneumatic tire according to claim 1, wherein an aspect ratio is 40% or more.

10. 10. The pneumatic tire according to claim 9, wherein the aspect ratio is 45% or more.

11. 11. The pneumatic tire according to claim 10, wherein the aspect ratio is 47.5% or more.

12. 12. The pneumatic tire according to claim 11, wherein the aspect ratio is 50% or more.

13. The pneumatic tire according to any one of claims 1 to 12, characterized in that 30°C tan δ × Wt ≦ 30.

0.

14. The pneumatic tire according to claim 13, characterized in that 30° C. tan δ×Wt≦25.

0.

15. 15. The pneumatic tire according to claim 1, wherein when the outer diameter of the tire is Dt (mm) when mounted on a regular rim and the internal pressure is set to 250 kPa, Dt is less than 685 (mm).

16. 16. The pneumatic tire according to claim 1, wherein the cross-sectional width Wt (mm) is less than 205 mm.

17. 17. The pneumatic tire according to claim 16, wherein the cross-sectional width Wt (mm) is less than 200 mm.

Citation Information

Patent Citations

  • Pneumatic tire

    JP2011225084A

  • Pneumatic tire

    JP2016041583A

  • Run flat tire

    JP2016074282A

  • Pneumatic tire for vehicle

    JP2016074408A

  • Pneumatic tire and design method therefor

    JP2017013693A