Electrolyte and method of manufacturing the same, battery and method of manufacturing the same, and vehicle equipped with the battery

The use of compounds represented by general formulas (1) and (2) in the electrolyte forms a mixed film to prevent solvent decomposition, addressing gas generation and maintaining battery performance during high-temperature storage.

KR1020260162289APending Publication Date: 2026-11-10MU IONIC SOLUTIONS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
KR1020267028208
Authority / Receiving Office
KR · KR
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-03-21
Filing Date
2025-01-10
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing non-aqueous electrolyte secondary batteries suffer from gas generation and degradation of battery characteristics during high-temperature storage, which is not adequately addressed by existing electrolytes.

Method used

Incorporation of specific compounds represented by general formulas (1) and (2) into the electrolyte, along with a non-aqueous solvent, to form a mixed film on the electrode surfaces, preventing solvent decomposition and significantly suppressing gas generation.

Benefits of technology

The electrolyte effectively suppresses gas generation after high-temperature storage, maintaining battery integrity and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCT00019_ABST
    Figure PCT00019_ABST
Patent Text Reader

Abstract

The present invention relates to [1] a compound represented by the following general formula (1), a compound represented by the following formula (2), an electrolyte, and an electrolyte comprising a non-aqueous solvent, [2] a method for manufacturing the battery, [3] a battery comprising a positive electrode, a negative electrode, and the electrolyte, [4] a method for manufacturing the battery, and [5] a vehicle equipped with the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to an electrolyte and a method for manufacturing the same, a battery and a method for manufacturing the same, and a vehicle equipped with the battery. Background Technology

[0002] Non-aqueous electrolyte secondary batteries, such as lithium-ion secondary batteries, are being commercialized for a wide range of applications, including power sources for so-called consumer small devices such as smartphones and laptop computers, and onboard power sources for driving electric vehicles.

[0003] As a means to improve the battery characteristics of non-aqueous electrolyte secondary batteries, numerous studies are being conducted in the fields of active materials for the positive or negative electrodes and additives for non-aqueous electrolytes.

[0004] As a non-aqueous electrolyte secondary battery, lithium-ion batteries are recently being used for applications such as power sources for electric vehicles and power sources for mobile phones such as smartphones. Lithium-ion batteries are mainly composed of a positive electrode and a negative electrode containing materials capable of absorbing and releasing lithium, and a non-aqueous electrolyte consisting of a lithium salt and a non-aqueous solvent. Carbonates such as ethylene carbonate (EC) and propylene carbonate (PC) are used as non-aqueous solvents.

[0005] In addition, lithium metal, metal compounds capable of absorbing and releasing lithium (elementary metals, oxides, alloys with lithium, etc.), and carbon materials are known as negative electrodes for lithium secondary batteries. In particular, among carbon materials, non-aqueous electrolyte secondary batteries using carbon materials capable of absorbing and releasing lithium, such as coke and graphite (synthetic graphite, natural graphite), have been widely commercialized. Since the above negative electrode materials store and release lithium and electrons at an extremely low potential equivalent to that of lithium metal, there is a possibility that a large amount of solvent may undergo reductive decomposition, especially under high temperatures. Regardless of the type of negative electrode material, some of the solvent in the electrolyte may undergo reductive decomposition on the negative electrode, and the movement of lithium ions is hindered by the deposition of decomposition products, gas generation, and expansion of the electrode. This has resulted in problems such as degrading battery characteristics, particularly high-temperature retention characteristics under high temperatures, and deformation of the battery due to the expansion of the electrode. In addition, lithium secondary batteries using metal elements or oxides such as lithium metal, its alloys, tin, or silicon as negative electrode materials are known to have problems such as significantly degraded battery performance, particularly at high temperatures, and deformation of the battery due to electrode expansion, because, although the initial capacity is high, pulverization proceeds during the cycle, and the reductive decomposition of non-aqueous solvents occurs more rapidly compared to carbon material negative electrodes.

[0006] Meanwhile, it is known that in lithium secondary batteries using, for example, LiCoO2, LiMn2O4, LiNiO2, LiFePO4, etc. as the positive electrode, deterioration of electrochemical characteristics occurs when used at high temperatures because decomposition products or gases generated by the local oxidative decomposition of the non-aqueous solvent in the non-aqueous electrolyte at the interface between the positive electrode material and the non-aqueous electrolyte during the charged state inhibit the desirable electrochemical reaction of the battery. Furthermore, LiNi 0.5 Mn 1.5O4, LiNi 0.5 Co 0.2 Mn 0.3 Materials capable of absorbing and releasing lithium, such as solid solutions of O2, Li2MnO3 and LiMO2 (M is a transition metal such as silver, Co, Ni, Mn, Fe, etc.), store and release lithium and electrons at higher voltages, and especially under high temperatures, there is a possibility that a large amount of solvent may undergo oxidative decomposition. Regardless of the type of positive electrode material, some of the solvent in the electrolyte on the positive electrode may undergo oxidative decomposition, and the movement of lithium ions is hindered by the deposition of decomposition products or gas generation, which has a problem of degrading battery characteristics such as high-temperature storage characteristics.

[0007] Patent Document 1 describes an electrolyte for a lithium secondary battery containing a non-aqueous organic solvent, a lithium salt, and a specific phosphorus compound, and discloses that the electrolyte suppresses the expansion of the battery, i.e., the generation of gas, after high-temperature storage.

[0008] Patent Document 2 describes a battery comprising a positive electrode, a negative electrode, and a non-aqueous electrolyte, wherein the non-aqueous electrolyte contains a specific cyclic sulfate ester, and when the narrow spectrum of sulfur atoms is measured by X-ray photoelectron spectroscopy on the surface of the negative electrode and peak separation is performed for the S2p orbital, the area ratio of peak 1 observed in the region of 168.4 eV to 171.1 eV to peak 2 observed in the region of 166.3 eV to 169.0 eV is 10 to 150, and the battery is disclosed to be able to suppress the increase in battery resistance after high-temperature storage.

[0009] Patent Document 3 describes an electrolyte for a lithium secondary battery containing a non-aqueous organic solvent, a lithium salt, and a compound having a difluorophosphoric acid structure represented by a specific chemical formula, and discloses that the electrolyte improves battery characteristics.

[0010] Patent Document 4 describes a non-aqueous electrolyte containing a specific cyclic sulfate ester compound, and discloses that the electrolyte has excellent performance in maintaining open-circuit voltage during charge storage of the battery. Prior art literature

[0011] International Publication No. 2018 / 062719 Japanese Published Patent Application No. 2022-169802 European Patent Application Publication No. 3522287 Specification International Publication No. 2012 / 053644 The problem to be solved

[0012] However, in the non-aqueous electrolyte secondary battery using the electrolyte described in Patent Document 1, there is room for improvement regarding gas suppression after high-temperature storage. Furthermore, in the non-aqueous electrolyte secondary batteries using the non-aqueous electrolytes described in Patent Documents 2 and 4, there is no disclosure or indication regarding gas suppression after high-temperature storage. Additionally, according to the inventors' review, the lithium secondary battery using the electrolyte described in Patent Document 3 does not have a sufficient gas generation suppression effect.

[0013] The present invention aims to provide an electrolyte capable of suppressing gas generation after high-temperature storage when used in a battery, a battery using said electrolyte, a method for manufacturing said electrolyte, and a vehicle equipped with said battery. means of solving the problem

[0014] The inventors, as a result of careful consideration to solve the above problem, discovered that gas generation after high-temperature storage can be suppressed when using a compound represented by the following general formula (1), a compound represented by the following formula (2), an electrolyte, and an electrolyte containing a non-aqueous solvent, and thus completed the present invention.

[0015] That is, the gist of the present invention is [1] to

[14] below.

[0016] [1] An electrolyte comprising a compound represented by the following general formula (1), a compound represented by the following formula (2), an electrolyte, and a non-aqueous solvent.

[0017] [Chemical Formula 1]

[0018]

[0019] (L represents a straight-chain or branched alkylene group having 1 to 6 carbon atoms.)

[0020] [Chemical Formula 2]

[0021]

[0022] [2] An electrolyte described in [1] having a content of 0.001 to 10 mass% of the compound represented by the general formula (1) in the above electrolyte.

[0023] [3] An electrolyte described in [1] or [2] having a content of 0.001 to 8.0 mass% of the compound represented by formula (2) in the electrolyte.

[0024] [4] An electrolyte described in any one of [1] to [3], wherein the mass ratio [(1):(2)] of the compound represented by the general formula (1) and the compound represented by the formula (2) in the above electrolyte is 94:6 to 3:97.

[0025] [5] An electrolyte described in any one of [1] to [4], comprising at least one carbonate compound selected from vinylene carbonate and fluoroethylene carbonate.

[0026] [6] The electrolyte described in [5], in which the carbonate compound is vinylene carbonate.

[0027] [7] The electrolyte described in [5] or [6], wherein the total content of the vinylene carbonate and the fluoroethylene carbonate in the electrolyte is 0.001 to 10 mass%.

[0028] [8] An electrolyte described in any one of [5] to [7], wherein the mass ratio of the total content of vinylene carbonate and fluoroethylene carbonate to the content of the compound represented by general formula (1) in the electrolyte (total of vinylene carbonate and fluoroethylene carbonate [g] / compound represented by general formula (1) [g]) is 0.01 to 100.

[0029] [9] An electrolyte described in any one of [1] to [8], in which L in the above general formula (1) is ethylene.

[0030]

[10] An electrolyte described in any one of [1] to [9] comprising at least one anion-containing compound selected from the group consisting of anion-containing compounds having P=O bonds and PF bonds, anion-containing compounds having S=O bonds and SX bonds, wherein X means heteroatom, and oxalate anion-containing compounds.

[0031]

[11] The electrolyte described in

[10] , wherein the anion-containing compound is at least one selected from a compound containing difluorophosphate anion, a compound containing fluorosulfonic acid anion, a compound containing fluorosulfonylimide anion, a compound containing alkylsulfate anion, a compound containing bis(oxalate)borate anion, a compound containing difluorooxalateborate anion, and a compound containing difluorobis(oxalate)phosphate anion.

[0032]

[12] A method for preparing an electrolyte, comprising a process of dissolving a compound represented by the following general formula (1), a compound represented by the following formula (2), and an electrolyte in a non-aqueous solvent.

[0033] [Chemical Formula 3]

[0034]

[0035] (L represents a straight-chain or branched alkylene group having 1 to 6 carbon atoms.)

[0036] [Chemical Formula 4]

[0037]

[0038]

[13] A battery having a positive electrode, a negative electrode, and an electrolyte described in any one of [1] to

[11] .

[0039]

[14] The battery described in

[13] , in which the positive electrode comprises a lithium transition metal compound.

[0040]

[15] A method for manufacturing a battery comprising a process of housing a positive electrode and a negative electrode in a container, and a process of injecting an electrolyte described in any one of [1] to

[11] into the container.

[0041]

[16] A vehicle equipped with the battery described in

[13] or

[14] . Effects of the invention

[0042] According to the electrolyte related to the present invention, an electrolyte capable of suppressing gas generation after high-temperature storage and a battery using said electrolyte can be provided. Specific details for implementing the invention

[0043] The following describes in detail embodiments for carrying out the present invention. However, the description below is merely an example (representative example) of an embodiment of the present invention, and the present invention is not limited to these contents. Furthermore, the present invention may be implemented with arbitrary modifications within the scope of not departing from the gist thereof. In this specification, "α ~ β" refers to a numerical range of α or more and β or less.

[0044] <1. Electrolyte>

[0045] The electrolyte related to the present embodiment contains a compound represented by general formula (1), a compound represented by formula (2), an electrolyte, and a non-aqueous solvent. The electrolyte related to the present embodiment is preferably a non-aqueous electrolyte.

[0046] [Chemical Formula 5]

[0047]

[0048] (L represents a straight-chain or branched alkylene group having 1 to 6 carbon atoms.)

[0049] [Chemical Formula 6]

[0050]

[0051] Below, each component is explained.

[0052] The reason why the electrolyte of the present invention suppresses gas generation after high-temperature storage is not clear, but is thought to be as follows.

[0053] The compound represented by general formula (1) has a fluorinated phosphoric acid structure, and the compound represented by formula (2) has a structure in which two cyclic sulfate esters are bonded. It is believed that the fluorinated phosphoric acid structure and the cyclic sulfate ester of the compound represented by general formula (1) and the compound represented by formula (2), respectively, decompose to form a mixed film on the negative electrode active material. Furthermore, it is inferred that some of these decomposition products reach the positive electrode and form a mixed film on the positive electrode active material as well, thereby preventing the decomposition of non-aqueous solvents on the surface of the negative electrode active material and / or the surface of the positive electrode active material, and significantly suppressing gas generation. The inventors have discovered that this significant suppression of gas generation cannot be achieved by combining the compound represented by general formula (1) with a general monocyclic sulfate ester. That is, the compound represented by formula (2), in which two cyclic sulfate esters, which are one of the components of the present invention, have a structure in which the decomposition product itself is difficult to generate gas because the molecular weight of the decomposition product is large. Also, because it has many active sites such as -OS(=O)2-O- groups or OC bonds compared to monocyclic sulfate ester compounds, it is easy to form a mixed film with the decomposition product of the compound represented by general formula (1) quickly and strongly, thereby suppressing additional solvent decomposition and significantly suppressing gas generation.

[0054] [1-1. Compounds represented by general formula (1)]

[0055] [Chemical Formula 7]

[0056]

[0057] In general formula (1), L represents a straight-chain or branched alkylene group having 1 to 6 carbon atoms.

[0058] The number of carbon atoms in L is more preferably 1 to 4, and even more preferably 2 to 4. It is preferred because the alkylene group described above tends to suppress side reactions on the surface of the electrode active material.

[0059] Specific examples of L-phosphorus alkylene groups include a straight-chain alkylene group selected from methylene group, ethylene group, propane-1,3-diyl group, butane-1,4-diyl group, pentane-1,5-diyl group, and hexane-1,6-diyl group; ethane-1,1-diyl group, propane-1,2-diyl group, butane-1,3-diyl group, butane-1,2-diyl group, butane-2,3-diyl group, pentane-1,4-diyl group, pentane-1,3-diyl group, pentane-1,2-diyl group, pentane-2,3-diyl group, pentane-2,4-diyl group, hexane-1,5-diyl group, hexane-1,4-diyl group, hexane-1,3-diyl group, and hexane-1,2-diyl group. Examples of branched alkylene groups include hexane-2,3-diyl groups, hexane-2,4-diyl groups, hexane-2,5-diyl groups, hexane-3,4-diyl groups, etc.

[0060] Among the alkylene groups described above, methylene groups, ethylene groups, propane-1,3-diyl groups, butane-1,4-diyl groups, pentane-1,5-diyl groups, hexane-1,6-diyl groups, ethane-1,1-diyl groups, propane-1,2-diyl groups, butane-1,3-diyl groups, butane-2,3-diyl groups, and pentane-2,4-diyl groups are preferred, ethylene groups, propane-1,3-diyl groups, butane-1,4-diyl groups, propane-1,2-diyl groups, butane-1,3-diyl groups, and butane-2,3-diyl groups are more preferred, ethylene groups, propane-1,3-diyl groups, and butane-1,4-diyl groups are even more preferred, and ethylene groups are particularly preferred.

[0061] As specific examples of compounds represented by general formula (1), compounds represented by the following formulas (A-1) to (A-23) (referred to as compounds (A-1) to (A-23)) are exemplified below. In addition, compounds represented by general formula (1) are not limited to the examples below.

[0062] [Chemical Formula 8]

[0063]

[0064] Among these, compounds with high symmetry are preferred in terms of the decomposition product forming a homogeneous composite film with the compound represented by formula (2), compounds (A-1) to (A-10) and compounds (A-15) are preferred, compounds (A-2) to (A-4) and compounds (A-8) to (A-10) are more preferred in terms of the stability of the film formed, and among these, compounds (A-2) to (A-4) are even more preferred.

[0065] The content of the compound represented by the general formula (1) in the electrolyte is typically 0.001 mass% or more, from the perspective of enabling the desirable formation of a mixed film with the compound represented by the formula (2) in the negative and positive electrodes and the manufacture of a battery with less gas generation after high-temperature storage; preferably 0.01 mass% or more, from the perspective of suppressing gas generation at higher temperatures; more preferably 0.1 mass% or more, from the perspective of rapidly forming a mixed film on the active material in a high-capacity battery to suppress gas generation; and even more preferably 0.2 mass% or more, from the perspective of suppressing gas generation after long-term storage. Additionally, from the perspective of suppressing gas generation by forming a film with high ion conductivity and high durability with the film thickness reduced to the minimum necessary, it is typically 10 mass% or less, preferably 5.0 mass% or less, more preferably 3.0 mass% or less, and even more preferably 1.2 mass% or less. And, the content of the compound represented by general formula (1) is typically 0.001 to 10 mass%, preferably 0.01 to 5.0 mass%, more preferably 0.1 to 3.0 mass%, and even more preferably 0.2 to 1.2 mass%.

[0066] There are no specific restrictions on the method of incorporating the compound represented by general formula (1) into the electrolyte, but methods such as adding the compound represented by general formula (1) to a non-aqueous solvent, etc., may be used.

[0067] The identification and measurement of the content of the compound represented by the general formula (1) are carried out by nuclear magnetic resonance (NMR) spectroscopy, gas chromatography mass spectrometry (GC / MS), etc.

[0068] [1-2. Compounds represented by Formula (2)]

[0069] [Chemical Formula 9]

[0070]

[0071] The content of the compound represented by formula (2) in the electrolyte is typically 0.001 mass% or more, from the perspective of enabling the manufacture of a battery with less gas generation after high-temperature storage by preferably forming a mixed film with the decomposition product of the compound represented by general formula (1) in the negative and positive electrodes, and from the perspective of suppressing gas generation at higher temperatures, preferably 0.01 mass% or more, more preferably 0.1 mass% or more, from the perspective of rapidly forming a mixed film on the active material in a high-capacity battery to suppress gas generation, more preferably 0.5 mass% or more, and also from the perspective of suppressing gas generation by forming a film with high ion conductivity and high durability with the film thickness at the minimum necessary level, typically 8.0 mass% or less, preferably 6.0 mass% or less, more preferably 4.0 mass% or less. And, the content of the compound represented by formula (2) is typically 0.001 to 8.0 mass%, preferably 0.01 to 8.0 mass%, more preferably 0.1 to 6.0 mass%, and even more preferably 0.5 to 4.0 mass%.

[0072] There are no specific limitations on the method of incorporating the compound represented by formula (2) into the electrolyte, but methods such as adding the compound represented by formula (2) to a non-aqueous solvent, etc., may be used.

[0073] The identification of the compound represented by Equation (2) and the measurement of its content are carried out by nuclear magnetic resonance (NMR) spectroscopy, gas chromatography mass spectrometry (GC / MS), etc.

[0074] The content of the compound represented by formula (2) in the electrolyte is more preferably 94:6 or higher in the mass ratio [(1):(2)] of the compound represented by general formula (1) to the compound represented by formula (2), more preferably 80:20 or higher, and particularly preferably 60:40 or higher. In addition, in the mass ratio [(1):(2)] of the compound represented by general formula (1) to the compound represented by formula (2), it is more preferably 3:97 or lower, more preferably 10:90 or lower, and particularly preferably 23:77 or lower. This is because within this range, it is easy to form a mixed film quickly and firmly, and gas generation after high-temperature storage can be suppressed more effectively. Also, the mass ratio [(1):(2)] of the compound represented by general formula (1) to the compound represented by formula (2) is preferably 94:6 to 3:97, more preferably 80:20 to 10:90, and even more preferably 60:40 to 23:77.

[0075] [1-3. Electrolytes]

[0076] As the electrolyte of the electrolyte, it is preferable that it be an alkali metal salt such as lithium, sodium, or potassium. Furthermore, when the electrolyte related to the present embodiment is used in a lithium-ion battery, the counter cation in the electrolyte is preferably a lithium cation. Furthermore, when the electrolyte related to the present embodiment is used in a sodium-ion battery, the counter cation in the electrolyte is preferably a sodium ion. Furthermore, when the electrolyte related to the present embodiment is used in a potassium-ion battery, the counter cation in the electrolyte is preferably a potassium ion.

[0077] In the electrolyte related to the present embodiment, the electrolyte content is typically greater than 5 mass% and is classified into a "main salt" that primarily carries out ion conduction and an "auxiliary agent" whose content is 5 mass% or less. In addition to the main salt, the electrolyte in the electrolyte related to the present embodiment may contain a specific anion-containing compound as an auxiliary agent. When the electrolyte contains a specific anion-containing compound, its content is preferably 5 mass% or less.

[0078] [1-3-1. Main Inflammation]

[0079] The electrolyte in the electrolyte related to the present embodiment varies depending on the type of secondary battery to which the electrolyte is applied, but, for example, lithium salt is preferably cited, and sodium salt or potassium salt is also preferably cited.

[0080] There are no particular restrictions on the lithium salts, but examples include lithium fluoroborate salts, lithium fluorophosphate salts, lithium tungstate salts, lithium carboxylate salts, lithium sulfonate salts, lithium imide salts, lithium methide salts, lithium oxalate salts, and fluorine-containing organic lithium salts.

[0081] Among these, from the perspective of improving low-temperature output characteristics, high-rate charge / discharge characteristics, impedance characteristics, high-temperature storage characteristics, cycle characteristics, etc., LiBF4 as a lithium fluoroborate salt; LiPF6, Li2PO3F, LiPO2F2 as a lithium fluorophosphate salt; LiFSO3, CH3SO3Li as a lithium sulfonate salt; LiN(FSO2)2, LiN(FSO2)(CF3SO2), LiN(CF3SO2)2, LiN(C2F5SO2)2, lithium cyclic 1,2-perfluoroethanedisulfonylimide, lithium cyclic 1,3-perfluoropropanedisulfonylimide as a lithium imide salt; LiC(FSO2)3, LiC(CF3SO2)3, LiC(C2F5SO2)3 as a lithium methide salt; As a lithium oxalate salt, lithium difluorooxalate borate, lithium bis(oxalate)borate, lithium tetrafluorooxalate phosphate, lithium difluorobis(oxalate)phosphate, lithium tris(oxalate)phosphate, etc. are preferred, and one or more selected from LiPF6, LiN(FSO2)2, lithium bis(oxalate)borate and LiFSO3 are more preferred, and LiPF6 is particularly preferred.

[0082] Other compounds that serve as electrolytes may be used as a single type or in combination of two or more types in any proportion.

[0083] There are no particular limitations on the combination of other compounds that serve as two or more types of electrolytes, and examples include the combination of LiPF6 and LiN(FSO2)2, the combination of LiPF6 and LiBF4, the combination of LiPF6 and LiN(CF3SO2)2, the combination of LiBF4 and LiN(FSO2)2, and the combination of LiBF4, LiPF6, and LiN(FSO2)2.

[0084] Among these, the combination of LiPF6 and LiN(FSO2)2, the combination of LiPF6 and LiBF4, and the combination of LiBF4, LiPF6, and LiN(FSO2)2 are preferred.

[0085] There are no particular restrictions on the sodium salts, but examples include sodium fluoroborate salts, sodium fluorophosphate salts, sodium tungstate salts, sodium carboxylate salts, sodium sulfonate salts, sodium imide salts, sodium methide salts, sodium oxalate salts, and fluorine-containing organic sodium salts.

[0086] Among these, from the perspective of improving low-temperature output characteristics, high-rate charge / discharge characteristics, impedance characteristics, high-temperature storage characteristics, cycle characteristics, etc., NaBF4 as sodium fluoroborate salt; NaPF6, Na2PO3F, NaPO2F2 as sodium fluorophosphate salts; NaFSO3, CH3SO3Na as sodium sulfonate salts; NaN(FSO2)2, NaN(FSO2)(CF3SO2), NaN(CF3SO2)2, NaN(C2F5SO2)2, sodium cyclic 1,2-perfluoroethanedisulfonylimide, sodium cyclic 1,3-perfluoropropanedisulfonylimide as sodium imide salts; NaC(FSO2)3, NaC(CF3SO2)3, NaC(C2F5SO2)3 as sodium methide salts; As a sodium oxalate salt, sodium difluorooxalate borate, sodium bis(oxalate)borate, sodium tetrafluorooxalate phosphate, sodium difluorobis(oxalate)phosphate, sodium tris(oxalate)phosphate, etc. are preferred, and one or more selected from NaPF6, NaN(FSO2)2, sodium bis(oxalate)borate, and NaFSO3 are more preferred, and NaPF6 is particularly preferred.

[0087] Other compounds that serve as electrolytes may be used as a single type or in combination of two or more types in any proportion.

[0088] There are no particular limitations on combinations of other compounds that serve as two or more types of electrolytes, and examples include combinations of NaPF6 and NaN(FSO2)2, NaPF6 and NaBF4, NaPF6 and NaN(CF3SO2)2, NaBF4 and NaN(FSO2)2, and combinations of NaBF4, NaPF6 and NaN(FSO2)2.

[0089] Among these, the combination of NaPF6 and NaN(FSO2)2, the combination of NaPF6 and NaBF4, and the combination of NaBF4, NaPF6, and NaN(FSO2)2 are preferred.

[0090] As for potassium salts, examples include those in which Li or Na in the above lithium salts and sodium salts are each replaced with potassium (K).

[0091] In the present embodiment, the total content of the electrolyte is not particularly limited, but from the perspective of ensuring that the electrical conductivity enables proper battery operation and exhibits sufficient output characteristics, it is typically 8 mass% or more, preferably 8.5 mass% or more, more preferably 9 mass% or more with respect to the total amount of the electrolyte, and is also typically 18 mass% or less, preferably 17 mass% or less, more preferably 16 mass% or less. In the electrolyte, it is typically 8 to 18 mass%, preferably 8.5 to 17 mass%, more preferably 9 to 16 mass%.

[0092] However, the content of the compound disclosed in [1-3-2. Specific Anion-Containing Compound] described below is also included in the content of the electrolyte. In addition, if a compound corresponding to [1-5. Auxiliary Agent] described below is included in the electrolyte, the electrolyte must contain an electrolyte other than the electrolyte shown in the main salt corresponding to the auxiliary agent.

[0093] The identification of electrolytes or the measurement of their content is carried out by nuclear magnetic resonance (NMR) spectroscopy.

[0094] [1-3-2. Specific Anion-Containing Compounds]

[0095] The electrolyte in the electrolyte related to the present embodiment may contain a specific anion-containing compound. The specific anion-containing compound is at least one compound selected from the group consisting of anion-containing compounds having P=O bonds and PF bonds, anion-containing compounds having S=O bonds and SX bonds (X represents a heteroatom), and oxalate anion-containing compounds.

[0096] A specific anion-containing compound is typically an acid or a salt, and is preferably a salt. As for the counter cation in the specific anion-containing compound, an alkali metal cation such as lithium, sodium, or potassium is preferred, and a lithium cation is more preferred. Furthermore, when the electrolyte related to the present embodiment is used in a lithium-ion battery, the counter cation is preferably a lithium cation; when used in a sodium-ion battery, the counter cation is preferably a sodium ion; and when used in a potassium-ion battery, the counter cation is preferably a potassium ion.

[0097] There are no specific restrictions on the method of adding a specific anion-containing compound to the electrolyte, but a method of adding a salt of the specific anion-containing compound may be used. It is preferable to add one or more selected from the group consisting of lithium salts, sodium salts, and potassium salts of the specific anion-containing compound, and it is more preferable to add a lithium salt of the specific anion-containing compound. In addition, a method of adding a raw material of the specific anion-containing compound to the electrolyte and generating the specific anion-containing compound in the electrolyte is also preferred.

[0098] At least one specific anion-containing compound selected from the group consisting of anion-containing compounds having P=O bonds and PF bonds, anion-containing compounds having S=O bonds and SX bonds, and oxalate anion-containing compounds may be used alone or in combination of two or more in any proportion.

[0099] [1-3-3. Anion-containing compounds having PF bonds and P=O bonds]

[0100] As an anion-containing compound having PF bonds and P=O bonds, which is one aspect of a specific anion-containing compound in the present embodiment, for example, PO3F - Monofluorophosphate anion of the like, PO2F2 - Examples of compounds containing difluorophosphate anions include the above.

[0101] Among these, a compound containing a difluorophosphate anion is preferred in terms of the balance between the battery's output characteristics and electrode interface protection.

[0102] There are no particular limitations on the method of adding an anion-containing compound having PF bonds and P=O bonds into the electrolyte, but a method of adding a salt of an anion-containing compound having PF bonds and P=O bonds may be used. It is preferable to add one or more selected from lithium monofluorophosphate, lithium difluorophosphate, sodium monofluorophosphate, sodium difluorophosphate, potassium monofluorophosphate, and potassium difluorophosphate, and more preferable to add at least one of lithium monofluorophosphate and lithium difluorophosphate. Additionally, it is also preferable to add a raw material of an anion-containing compound having PF bonds and P=O bonds into the electrolyte and generate an anion-containing compound having PF bonds and P=O bonds in the electrolyte.

[0103] [1-3-4. Anion-containing compounds having S=O and SX bonds]

[0104] Among the anion-containing compounds having S=O and SX bonds, which are one aspect of the specific anion-containing compounds in the present embodiment, X represents a heteroatom. Examples of heteroatoms include oxygen atoms, nitrogen atoms, fluorine atoms, etc. Examples of anion-containing compounds having S=O and SX bonds include FSO3 - Fluorosulfonic acid anions of the like; (FSO2)2N - , (FSO2)(CF3SO2)N - Fluorosulfonylimide anone of the following; (FSO2)3C - Compounds containing fluorosulfonylmethane anions such as; methylsulfate anion (CH3SO4 - ), ethyl sulfate anion (C2H5SO4 - Examples include compounds containing alkyl sulfates, anions, etc.

[0105] Among these, from the perspective of the balance between the output characteristics of the battery and the protection of the electrode interface, a compound containing a fluorosulfonic acid anion, a fluorosulfonylimide anion, or an alkyl sulfate anion is preferred, a compound containing a fluorosulfonic acid anion, a fluorosulfonylimide anion, a methyl sulfate anion, or an ethyl sulfate anion is more preferred, and a compound containing a fluorosulfonic acid anion is even more preferred.

[0106] There are no particular limitations on the method of adding an anion-containing compound having S=O bonds and SX bonds into the electrolyte, but a method of adding a salt of an anion-containing compound having S=O bonds and SX bonds may be used. It is preferable to add one or more selected from lithium fluorosulfonate, lithium fluorosulfonylimide, sodium fluorosulfonate, sodium fluorosulfonylimide, potassium fluorosulfonate, potassium fluorosulfonylimide, lithium methylsulfate, lithium ethylsulfate, sodium methylsulfate, sodium ethylsulfate, potassium methylsulfate, and potassium ethylsulfate, and it is more preferable to add one or more selected from lithium fluorosulfonate, lithium fluorosulfonylimide, lithium methylsulfate, and lithium ethylsulfate. In addition, a method of adding a raw material of an anion-containing compound having S=O and SX bonds to the electrolyte and generating an anion-containing compound having S=O and SX bonds in the electrolyte is also desirable.

[0107] [1-3-5. Oxalate complex anion-containing compounds]

[0108] The oxalate complex anion-containing compound, which is one aspect of the specific anion-containing compound in the present embodiment, is not particularly limited as long as it is a compound containing an anion having an oxalate complex within the molecule. An oxalate complex anion-containing compound is a compound containing an acid anion that forms a complex by oxalic acid being coordinated or bonded to a central atom, and examples include a boron oxalate complex anion in which oxalic acid is coordinated or bonded to a boron atom, and a phosphorus oxalate complex anion in which oxalic acid is coordinated or bonded to a phosphorus atom.

[0109] Examples of compounds containing boron oxalate complex anions include compounds containing bis(oxalate)borate anion and difluorooxalate borate anion.

[0110] Examples of compounds containing an oxalate complex anion include compounds containing tetrafluorooxalate phosphate anion, difluorobis(oxalate)phosphate anion, tris(oxalate)phosphate anion, etc., and more preferably, compounds containing difluorobis(oxalate)phosphate anion.

[0111] Among these, a compound containing a boron oxalate complex anion is preferred in terms of forming a stable composite film on the surface of an electrode, and a compound containing a bis(oxalate)borate anion is more preferred.

[0112] There are no particular limitations on the method of adding an oxalate complex anion-containing compound to the electrolyte, but a method of adding a salt of an oxalate complex anion-containing compound may be used. It is preferable to add one or more selected from lithium bis(oxalate)borate, lithium difluorooxalate borate, lithium tetrafluorooxalate phosphate, lithium difluorobis(oxalate)phosphate, lithium tris(oxalate)phosphate, sodium bis(oxalate)borate, sodium difluorooxalate borate, sodium tetrafluorooxalate phosphate, sodium difluorobis(oxalate)phosphate, sodium tris(oxalate)phosphate, potassium bis(oxalate)borate, potassium difluorooxalate borate, potassium tetrafluorooxalate phosphate, potassium difluorobis(oxalate)phosphate, and potassium tris(oxalate)phosphate, and lithium bis(oxalate)borate, lithium difluorooxalate borate, A method of adding one or more selected from lithium tetrafluorooxalate phosphate, lithium difluorobis(oxalate)phosphate, and lithium tris(oxalate)phosphate is more preferable. In addition, a method of adding a raw material for an oxalate complex anion-containing compound to the electrolyte and generating an oxalate complex anion-containing compound in the electrolyte is also preferable.

[0113] [Content of specific anion-containing compounds]

[0114] In the case of containing a specific anion-containing compound, the content of the specific anion-containing compound in the electrolyte related to the present embodiment is preferably 0.001 mass% or more, more preferably 0.01 mass% or more, and even more preferably 0.1 mass% or more, from the perspective of further suppressing gas generation after high-temperature storage, particularly regarding battery characteristics, and also preferably 5 mass% or less, more preferably 4 mass% or less, and even more preferably 3 mass% or less. Furthermore, the content of the specific anion-containing compound is preferably 0.001 to 5 mass%, more preferably 0.01 to 4 mass%, and even more preferably 0.1 to 3 mass%. In addition, if two or more types of specific anion-containing compounds are included, the above content refers to the total content thereof.

[0115] By including a specific anion-containing compound in the electrolyte related to the present embodiment, the battery characteristics, particularly gas generation after high-temperature storage, can be further suppressed. Although the reason is not certain, the specific anion-containing compound can minimize side reactions of the electrolyte components on the electrode surface, and it is believed that this effect is more preferably exhibited within the range of the content of the specific anion-containing compound.

[0116] The identification of specific anion-containing compounds and the measurement of their content are carried out by nuclear magnetic resonance (NMR) spectroscopy, ion chromatography (IC), etc.

[0117] [Mass ratio of compounds represented by general formula (1) for specific anion-containing compounds]

[0118] In the case of containing a specific anion-containing compound, the mass ratio of the content of the compound represented by general formula (1) to the content of the specific anion-containing compound, i.e., the mass ratio represented by the compound [g] of general formula (1) / the specific anion-containing compound [g], is typically 0.01 or more, preferably 0.02 or more, more preferably 0.03 or more, even more preferably 0.04 or more, even more preferably 0.05 or more, particularly preferably 0.1 or more, further more preferably 0.3 or more, even more preferably 0.6 or more, particularly preferably 0.7 or more, and also typically 100 or less, preferably 30 or less, more preferably 25 or less, even more preferably 15 or less, particularly preferably 11 or less, even more preferably 10 or less, further more preferably 8 or less, even more preferably 5 or less, even more preferably 4 or less, further more preferably 3 or less, and particularly preferably 2.5 or less. And, the above mass ratio is typically 0.01 to 100, preferably 0.02 to 30, more preferably 0.03 to 25, even more preferably 0.04 to 15, even more preferably 0.05 to 11, particularly preferably 0.1 to 10, further more preferably 0.3 to 8, even more preferably 0.6 to 5, even more preferably 0.7 to 4, even more preferably 0.7 to 3, and particularly preferably 0.7 to 2.5. Also, the content of the compound represented by general formula (1) and the specific anion-containing compound refers to the total content when two or more of them are included.

[0119] If the above mass ratio is within the above range, the battery characteristics, especially gas generation after high-temperature storage, can be further suppressed. Although the reason is not certain, it is thought that by including a compound represented by general formula (1) and a specific anion-containing compound within the above mass ratio range, side reactions of the electrolyte components on the electrode surface can be suppressed to a minimum.

[0120] [Mass ratio of a specific anion-containing compound to the main salt]

[0121] In the case where the electrolyte in the electrolyte related to the present embodiment contains the specific anion-containing compound, the mass ratio of the content of the specific anion-containing compound to the content of the main salt constituting the electrolyte, i.e., the mass ratio expressed as specific anion-containing compound [g] / main salt [g], is typically 0.00005 or more, preferably 0.0005 or more, more preferably 0.001 or more, even more preferably 0.005 or more, even more preferably 0.01 or more, particularly preferably 0.015 or more, and also typically 0.5 or less, preferably 0.45 or less, more preferably 0.4 or less, and even more preferably 0.35 or less. And, the above mass ratio is typically 0.00005 to 0.5, preferably 0.0005 to 0.5, more preferably 0.001 to 0.45, even more preferably 0.005 to 0.4, even more preferably 0.01 to 0.35, and particularly preferably 0.015 to 0.35. Also, the content of a specific anion-containing compound refers to the total content when two or more specific anion-containing compounds are included.

[0122] If the above mass ratio is within the above range, battery characteristics, particularly gas generation after high-temperature storage, can be further suppressed. Although the reason is not certain, it is believed that by including a specific anion-containing compound and a main salt within the above mass ratio range, side reactions of the electrolyte within the battery system can be suppressed to a minimum.

[0123] [1-4. Non-aqueous Solvents]

[0124] The electrolyte related to the present embodiment contains a non-aqueous solvent. The non-aqueous solvent is a component that dissolves the electrolyte described above.

[0125] There are no specific restrictions on non-aqueous solvents, and known organic solvents may be used.

[0126] Examples of organic solvents include saturated cyclic carbonates such as ethylene carbonate, propylene carbonate, and butylene carbonate; chain carbonates such as dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate; chain carboxylic acid esters such as methyl acetate, ethyl acetate, propyl acetate, and butyl acetate; cyclic carboxylic acid esters such as γ-butyrolactone and γ-valerolactone; ether compounds such as dimethoxymethane, diethoxymethane, ethoxymethoxymethane, tetrahydrofuran, 1,3-dioxane, and 1,4-dioxane; and sulfone compounds such as 2-methylsulfolane, 3-methylsulfolane, 2-fluorosulfolane, 3-fluorosulfolane, dimethylsulfone, ethylmethylsulfone, and monofluoromethylmethylsulfone.

[0127] Among these, preferably, saturated cyclic carbonates, chain carbonates, and chain or cyclic carboxylic acid esters, and more preferably, saturated cyclic carbonates and chain carbonates.

[0128] These non-aqueous solvents can be used as a single type or in combination of two or more types.

[0129] As a combination of two or more non-aqueous solvents, there are no particular limitations, but examples include saturated cyclic carbonates and chain-type carboxylic acid esters, cyclic carboxylic acid esters and chain-type carbonates, and saturated cyclic carbonates, chain-type carbonates, and chain-type carboxylic acid esters. Among these, combinations of saturated cyclic carbonates and chain-type carbonates, and saturated cyclic carbonates, chain-type carbonates, and chain-type carboxylic acid esters are preferred.

[0130] [1-4-1. Saturated Cyclic Carbonate]

[0131] As a saturated cyclic carbonate which is one embodiment of the non-aqueous solvent in this embodiment, it typically has an alkylene group having 2 to 4 carbon atoms, and a saturated cyclic carbonate having 2 to 3 carbon atoms is preferably used from the perspective of improving battery characteristics derived from the improvement of the degree of lithium ion dissociation.

[0132] Examples of saturated cyclic carbonates include ethylene carbonate, propylene carbonate, butylene carbonate, etc. Among these, ethylene carbonate and propylene carbonate are preferred, and ethylene carbonate, which is difficult to oxidize or reduce, is more preferred. Saturated cyclic carbonates may be used as a single type, or two or more types may be used in any combination and ratio.

[0133] The content of the saturated cyclic carbonate is not particularly limited and is optional as long as it does not significantly impede the effects of the present invention, but is typically 3 volume% or more, preferably 5 volume% or more, in the non-aqueous solvent of the electrolyte, and is also typically 90 volume% or less, preferably 85 volume% or less, more preferably 80 volume% or less. Furthermore, the content of the saturated cyclic carbonate in the non-aqueous solvent of the electrolyte is typically 3 to 90 volume%, preferably 3 to 85 volume%, and more preferably 5 to 80 volume%. By keeping it within this range, it is easier to avoid a decrease in electrical conductivity resulting from a decrease in the dielectric constant of the electrolyte, and to keep the large current discharge characteristics, stability against the negative electrode, and cycle characteristics of the battery within a good range, and the oxidation and reduction resistance of the electrolyte is improved, and there is a tendency for stability during high-temperature storage to be improved. Also, in this embodiment, volume % means the volume at 25°C and 1 atmosphere.

[0134] [1-4-2. Chain Carbonate]

[0135] As a chain-type carbonate which is one embodiment of the non-aqueous solvent in this embodiment, one having 3 to 7 carbon atoms is typically used, and in order to adjust the viscosity of the electrolyte to an appropriate range, a chain-type carbonate having 3 to 5 carbon atoms is preferably used.

[0136] Examples of chain-type carbonates include, specifically, dimethyl carbonate, diethyl carbonate, di-n-propyl carbonate, diisopropyl carbonate, n-propylisopropyl carbonate, ethylmethyl carbonate, and methyl-n-propyl carbonate. Particularly preferably, they are dimethyl carbonate, diethyl carbonate, and ethylmethyl carbonate.

[0137] In addition, chain-type carbonates having fluorine atoms (hereinafter abbreviated as "fluorinated chain-type carbonates") may also be preferably used. The number of fluorine atoms in the fluorinated chain-type carbonates is not particularly limited as long as it is 1 or more, but is typically 6 or less, and preferably 4 or less. When the fluorinated chain-type carbonates have multiple fluorine atoms, they may be bonded to the same carbon or to different carbons.

[0138] Examples of fluorinated chain-type carbonates include fluorinated dimethyl carbonate derivatives such as fluoromethylmethyl carbonate, fluorinated ethylmethyl carbonate derivatives such as 2-fluoroethylmethyl carbonate, and fluorinated diethyl carbonate derivatives such as ethyl-(2-fluoroethyl)carbonate.

[0139] Chain-type carbonates may be used as a single type, or two or more types may be used in any combination and ratio.

[0140] The content of the chain-type carbonate is not particularly limited, but in the non-aqueous solvent in the electrolyte, it is typically 15 volume% or more, preferably 20 volume% or more, more preferably 25 volume% or more, and also typically 90 volume% or less, preferably 85 volume% or less, more preferably 80 volume% or less. Furthermore, the content of the chain-type carbonate in the non-aqueous solvent in the electrolyte is typically 15 to 90 volume%, preferably 20 to 85 volume%, and more preferably 25 to 80 volume%. By setting the content of the chain-type carbonate to the above range, it becomes easier to set the viscosity of the electrolyte to an appropriate range, suppress the decrease in ion conductivity, and furthermore, to set the output characteristics of the battery to a good range.

[0141] In addition, for a specific chain-type carbonate, by combining ethylene carbonate with a specific content, battery performance can be significantly improved.

[0142] For example, when dimethyl carbonate and ethylmethyl carbonate are selected as specific chain-type carbonates, the content of ethylene carbonate is not particularly limited and is optional as long as it does not significantly impede the effects of the present invention, but is typically 15 volume% or more, preferably 20 volume% or more, and typically 45 volume% or less, preferably 40 volume% or less, in the non-aqueous solvent of the electrolyte. In addition, the content of ethylene carbonate is typically 15 to 45 volume%, and preferably 20 to 40 volume%, in the non-aqueous solvent of the electrolyte. In addition, the content of dimethyl carbonate is typically 20 volume% or more, preferably 30 volume% or more, and typically 50 volume% or less, preferably 45 volume% or less, in the non-aqueous solvent of the electrolyte. In addition, the content of dimethyl carbonate in the non-aqueous solvent of the electrolyte is typically 20 to 50 volume%, and preferably 30 to 45 volume%. Furthermore, the content of ethyl methyl carbonate in the non-aqueous solvent of the electrolyte is typically 20 volume% or more, preferably 30 volume% or more, and typically 50 volume% or less, preferably 45 volume% or less. In addition, the content of ethyl methyl carbonate in the non-aqueous solvent of the electrolyte is typically 20 to 50 volume%, and preferably 30 to 45 volume%.

[0143] By keeping each content within the above range, high-temperature stability is excellent, and gas generation tends to be further suppressed.

[0144] [1-4-3. Chain-type Carboxylic Acid Esters]

[0145] Examples of chain-type carboxylic acid esters that serve as one form of the non-aqueous solvent in the present embodiment include methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, methyl valerate, methyl isobutyrate, ethyl isobutyrate, and methyl pivalate. Among these, methyl acetate, ethyl acetate, propyl acetate, and butyl acetate are preferred from the perspective of improving battery characteristics. Furthermore, chain-type carboxylic acid esters in which some of the hydrogens of each of the chain-type carboxylic acid esters described above are substituted with fluorine may also be preferably used. Examples of such fluorine-substituted chain-type carboxylic acid esters include methyl trifluoroacetate and ethyl trifluoroacetate.

[0146] [1-4-4. Cyclic acid esters]

[0147] Examples of cyclic carboxylic acid esters that are one form of the non-aqueous solvent in the present embodiment include γ-butyrolactone and γ-valerolactone. Among these, γ-butyrolactone is more preferred. Cyclic acid esters in which some of the hydrogens of each of the cyclic carboxylic acid esters described above are substituted with fluorine can also be preferably used.

[0148] [1-4-5. Ether Compounds]

[0149] As an ether-based compound which is one embodiment of a non-aqueous solvent in the present embodiment, chain-type ethers having 3 to 10 carbon atoms, such as dimethoxymethane, diethoxymethane, ethoxymethoxymethane, ethylene glycol di-n-propyl ether, ethylene glycol di-n-butyl ether, and diethylene glycol dimethyl ether, and cyclic ethers having 3 to 6 carbon atoms, such as tetrahydrofuran, 2-methyltetrahydrofuran, 3-methyltetrahydrofuran, 1,3-dioxane, 2-methyl-1,3-dioxane, 4-methyl-1,3-dioxane, and 1,4-dioxane, are preferred.

[0150] Among these, dimethoxymethane, diethoxymethane, and ethoxymethoxymethane are preferred as chain-type ethers having 3 to 10 carbon atoms because they have high solvation ability for lithium ions, improve ion dissociation, and have low viscosity, thereby imparting high ion conductivity, and tetrahydrofuran, 1,3-dioxane, 1,4-dioxane, etc. are preferred as cyclic ethers having 3 to 6 carbon atoms because they impart high ion conductivity.

[0151] The content of the ether-based compound is not particularly limited and is optional as long as it does not significantly impede the effects of the invention related to the present embodiment, but is typically 1 volume% or more, preferably 2 volume% or more, more preferably 3 volume% or more, in the non-aqueous solvent of the electrolyte, and is also typically 30 volume% or less, preferably 25 volume% or less, more preferably 20 volume% or less. Furthermore, the content of the ether-based compound in the non-aqueous solvent of the electrolyte is typically 1 to 30 volume%, preferably 2 to 25 volume%, and more preferably 3 to 20 volume%. If the content of the ether-based compound is within the above range, it is easy to secure the effect of improved ion conductivity resulting from the improvement in the degree of lithium ion dissociation of the ether and the reduction in viscosity. In addition, when the negative electrode active material is a carbon-based material, the phenomenon of chain-type ether co-insertion with lithium ions can be suppressed, so the input / output characteristics or charge / discharge rate characteristics can be set to an appropriate range.

[0152] [1-4-6. Sulfone Compounds]

[0153] As for the sulfone compound which is one aspect of the non-aqueous solvent in the present embodiment, it is not particularly limited to either a cyclic sulfone or a chain sulfone, but in the case of a cyclic sulfone, the number of carbon atoms is typically 3 to 6, preferably 3 to 5. In addition, in the case of a chain sulfone, the number of carbon atoms is typically 2 to 6, preferably 2 to 5. In addition, the number of sulfonyl groups in one molecule of the sulfone compound is not particularly limited, but is typically 1 or 2.

[0154] Examples of cyclic sulfones include monosulfone compounds such as trimethylenesulfones, tetramethylenesulfones, and hexamethylenesulfones; and disulfone compounds such as trimethylenedisulfones, tetramethylenedisulfones, and hexamethylenedisulfones. Among these, in terms of dielectric constant and viscosity, tetramethylenesulfones, tetramethylenedisulfones, hexamethylenesulfones, and hexamethylenedisulfones are more preferred, and tetramethylenesulfones (sulfolanes) are particularly preferred.

[0155] As for sulfolanes, sulfolanes and / or sulfolane derivatives (hereinafter, sulfolanes may also be included and referred to as “sulfolanes”) are preferred. As for sulfolane derivatives, it is preferred that one or more hydrogen atoms bonded to carbon atoms constituting the sulfolane ring are substituted with fluorine atoms or alkyl groups.

[0156] Among them, 2-methylsulfolane, 3-methylsulfolane, 2-fluorosulfolane, 3-fluorosulfolane, 2,3-difluorosulfolane, 2-trifluoromethylsulfolane, 3-trifluoromethylsulfolane, etc. are desirable in that they have high ion conductivity and high input / output.

[0157] In addition, examples of chain-type sulfones include dimethylsulfone, ethylmethylsulfone, diethylsulfone, monofluoromethylmethylsulfone, difluoromethylmethylsulfone, trifluoromethylmethylsulfone, and pentafluoroethylmethylsulfone. Among these, dimethylsulfone, ethylmethylsulfone, and monofluoromethylmethylsulfone are preferred in that they improve the high-temperature storage stability of the electrolyte.

[0158] The content of the sulfone compound is not particularly limited and is optional as long as it does not significantly impede the effects of the invention related to the present embodiment, but is typically 0.3 volume% or more, preferably 0.5 volume% or more, more preferably 1 volume% or more in the non-aqueous solvent in the electrolyte, and is also typically 40 volume% or less, preferably 35 volume% or less, more preferably 30 volume% or less. Furthermore, the content of the sulfone compound in the non-aqueous solvent in the electrolyte is typically 0.3 to 40 volume%, preferably 0.5 to 35 volume%, and more preferably 1 to 30 volume%. When the content of the sulfone compound is within the above range, an electrolyte with excellent high-temperature storage stability tends to be obtained.

[0159] [1-5. Supplements]

[0160] The electrolyte related to this embodiment may contain various auxiliary agents within a range that does not impede the effects of the present invention. As auxiliary agents, conventionally known ones may be used at will. In addition, auxiliary agents may be used as a single type or in combination of two or more types in any ratio.

[0161] Examples of adjuvants include cyclic carbonates having carbon-carbon unsaturated bonds, cyclic carbonates having fluorine atoms, compounds having isocyanate groups, compounds having an isocyanuric acid backbone, sulfur-containing organic compounds, phosphorus-containing organic compounds, silicon-containing compounds, aromatic compounds, organic compounds having cyano groups, fluorine-free carboxylic acid esters, cyclic ether compounds, acid anhydrides, compounds containing triple bonds, phosphazene compounds, etc. Examples include compounds described in International Publication No. 2015 / 111676.

[0162] Among these, at least one carbonate compound selected from the group consisting of cyclic carbonates having carbon-carbon unsaturated bonds and cyclic carbonates having fluorine atoms (hereinafter also referred to as "specific carbonate compounds") is preferred.

[0163] The content of the auxiliary agent is not particularly limited and is optional as long as it does not significantly impede the effects of the present invention, but is typically 0.001 mass% or more, preferably 0.01 mass% or more, more preferably 0.1 mass% or more in the electrolyte, and is also typically 10 mass% or less, preferably 5 mass% or less, more preferably 3 mass% or less, even more preferably 1 mass% or less, and particularly preferably less than 1 mass%. In addition, the content of the auxiliary agent is typically 0.001 to 10 mass%, preferably 0.01 to 5 mass%, more preferably 0.1 to 3 mass%, even more preferably 0.1 to 1 mass%, and particularly preferably 0.1 mass% or more and less than 1 mass% in the electrolyte.

[0164] Here, cyclic ether compounds may be used as auxiliary agents in the electrolyte, and may also be used as non-aqueous solvents as indicated in [1-4. Non-aqueous solvents].

[0165] When using a cyclic ether compound as an auxiliary agent, it is used in an amount of 5 mass% or less in the electrolyte, but it is preferable to use an amount of less than 4 mass%.

[0166] In addition, boric acid anion-containing compounds, oxalate complex anion-containing compounds, monofluorophosphate anion-containing compounds, and difluorophosphate anion-containing compounds may be used as auxiliary agents in the electrolyte, and may also be used as electrolytes as indicated in [1-3. Electrolytes]. When these compounds are used as auxiliary agents, it is preferable to use them in an amount of less than 3 mass% in the electrolyte.

[0167] [1-5-1. Specific Carbonate Compounds]

[0168] The electrolyte related to the present embodiment preferably comprises, as described above, at least one carbonate compound selected from the group consisting of cyclic carbonates having carbon-carbon unsaturated bonds and cyclic carbonates having fluorine atoms as an auxiliary agent. These may be used individually or in combination of two or more in any proportion.

[0169] When using two or more specific carbonate compounds in combination, it is preferable to combine an unsaturated cyclic carbonate and a fluorinated cyclic carbonate, and it is preferable to combine a vinylene carbonate and a fluorinated cyclic carbonate.

[0170] [Content of specific carbonate compounds]

[0171] In the total amount of the electrolyte related to the present embodiment, the content of a specific carbonate compound is typically 0.001 mass% or more, preferably 0.01 mass% or more, more preferably 0.1 mass% or more, and even more preferably 0.5 mass% or more; additionally, it is typically 10 mass% or less, preferably 6 mass% or less, more preferably 5 mass% or less, and even more preferably 4 mass% or less. Furthermore, the content of the specific carbonate compound is typically 0.001 to 10 mass%, preferably 0.01 to 6 mass%, more preferably 0.1 to 5 mass%, and even more preferably 0.5 to 4 mass% of the total amount of the electrolyte. Also, if two or more types of specific carbonate compounds are contained, the content refers to the total content thereof.

[0172] If the content of a specific carbonate compound is within the above range, battery characteristics, particularly durability, can be improved. Although the reason is not certain, it is thought that by including a specific carbonate compound in this ratio, a film is formed on the electrode, thereby minimizing side reactions of the electrolyte components.

[0173] The identification and measurement of the content of specific carbonate compounds are carried out by nuclear magnetic resonance (NMR) spectroscopy.

[0174] [Mass ratio of a specific carbonate compound to a compound represented by general formula (1)]

[0175] In this embodiment, the mass ratio of the content of a specific carbonate compound to the content of a compound represented by general formula (1), that is, the mass ratio represented as specific carbonate compound [g] / compound represented by general formula (1) [g], is typically 0.01 or more, preferably 0.05 or more, more preferably 0.3 or more, and even more preferably 0.5 or more, and is also typically 100 or less, preferably 50 or less, more preferably 20 or less, and even more preferably 15 or less. Furthermore, the above mass ratio is typically 0.01 to 100, preferably 0.05 to 50, more preferably 0.3 to 20, and even more preferably 0.5 to 15. Also, when two or more types of the compound represented by general formula (1) and a specific carbonate compound are each contained, the content refers to the total content of each.

[0176] If the mass ratio is within the above range, the battery characteristics, especially durability, can be improved. Although the reason is not certain, it is thought that by including a specific carbonate compound and a compound represented by general formula (1) within the above range of mass ratio, a film is formed on the electrode, thereby minimizing side reactions of the electrolyte components.

[0177] [Mass ratio of a specific carbonate compound to the main salt]

[0178] In the electrolyte related to the present embodiment, the mass ratio of the content of a specific carbonate compound to the total content of the main salt constituting the electrolyte, i.e., the mass ratio expressed as specific carbonate compound [g] / main salt [g], is typically 0.00005 or more, preferably 0.0005 or more, more preferably 0.001 or more, even more preferably 0.01 or more, even more preferably 0.02 or more, particularly preferably 0.025 or more, and also typically 0.5 or less, preferably 0.45 or less, more preferably 0.4 or less, and even more preferably 0.35 or less. And, the above mass ratio is typically 0.00005 to 0.5, preferably 0.0005 to 0.5, more preferably 0.001 to 0.45, even more preferably 0.01 to 0.4, even more preferably 0.02 to 0.35, and particularly preferably 0.025 to 0.35. Also, when containing two or more types of main salt and specific carbonate compounds, the above content refers to the total content of each.

[0179] If the mass ratio is within the above range, battery characteristics, particularly durability, can be improved. Although the reason is not certain, it is believed that this is because, by including a specific carbonate compound and a main salt within the above range of mass ratios, a film is formed on the electrode, thereby minimizing side reactions of the electrolyte within the battery system.

[0180] [1-5-1-1. Cyclic carbonates with carbon-carbon unsaturated bonds]

[0181] As for the cyclic carbonate having a carbon-carbon unsaturated bond (hereinafter also referred to as "unsaturated cyclic carbonate"), which is one aspect of the specific carbonate compound in this embodiment, there are no particular limitations as long as it is a cyclic carbonate having a carbon-carbon double bond or a carbon-carbon triple bond. Cyclic carbonates having an aromatic ring are also included in unsaturated cyclic carbonates.

[0182] Examples of unsaturated cyclic carbonates include vinylene carbonates, ethylene carbonates substituted with aromatic rings or substituents having carbon-carbon double or carbon-carbon triple bonds, phenyl carbonates, vinyl carbonates, allyl carbonates, catechol carbonates, etc. Among these, vinylene carbonates and ethylene carbonates substituted with aromatic rings or substituents having carbon-carbon double or carbon-carbon triple bonds are preferred.

[0183] Examples of vinylene carbonates include vinylene carbonate, methyl vinylene carbonate, 4,5-dimethyl vinylene carbonate, phenyl vinylene carbonate, 4,5-diphenyl vinylene carbonate, vinyl vinylene carbonate, 4,5-vinyl vinylene carbonate, allyl vinylene carbonate, 4,5-diallyl vinylene carbonate, etc.

[0184] Examples of ethylene carbonates substituted with a substituent having an aromatic ring or a carbon-carbon double bond or a carbon-carbon triple bond include vinylethylene carbonate, 4,5-divinylethylene carbonate, 4-methyl-5-vinylethylene carbonate, 4-allyl-5-vinylethylene carbonate, ethynylethylene carbonate, 4,5-diethynylethylene carbonate, 4-methyl-5-ethynylethylene carbonate, 4-vinyl-5-ethynylethylene carbonate, 4-allyl-5-ethynylethylene carbonate, phenylethylene carbonate, 4,5-diphenylethylene carbonate, 4-phenyl-5-vinylethylene carbonate, 4-allyl-5-phenylethylene carbonate, allylethylene carbonate, 4,5-diallylethylene carbonate, 4-methyl-5-allylethylene carbonate, etc.

[0185] Among these, vinylene carbonate, vinylethylene carbonate, and ethynylethylene carbonate are preferred because they form a more stable composite film on the electrode, one or more selected from vinylene carbonate and vinylethylene carbonate are more preferred, and vinylene carbonate is more preferred.

[0186] Unsaturated cyclic carbonates can be used as a single type or in combination of two or more types in any proportion.

[0187] [1-5-1-2. Cyclic carbonates containing fluorine atoms]

[0188] A cyclic carbonate having a fluorine atom, which is one aspect of a specific carbonate compound in the present embodiment, is not particularly limited as long as it has a cyclic carbonate structure and also contains a fluorine atom.

[0189] Examples of cyclic carbonates having fluorine atoms include fluorides of cyclic carbonates having alkylene groups having 2 to 6 carbon atoms and derivatives thereof; more specifically, examples include fluorides of ethylene carbonates and derivatives thereof, and ethylene carbonates having fluorine-containing groups. In this specification, fluorides of ethylene carbonates and derivatives thereof are collectively referred to as fluoroethylene carbonates.

[0190] Examples of derivatives of ethylene carbonate fluorides include ethylene carbonate fluorides substituted with alkyl groups (e.g., alkyl groups having 1 to 4 carbon atoms).

[0191] Among these, as cyclic carbonates having fluorine atoms, fluoroethylene carbonates having 1 to 8 fluorine atoms and ethylene carbonates having 1 to 8 fluorine-containing groups are preferred.

[0192] As a fluoroethylene carbonate having 1 to 8 fluorine atoms and an ethylene carbonate having 1 to 8 fluorine atoms containing 1 to 8 fluorine groups, the examples include monofluoroethylene carbonate, 4,4-difluoroethylene carbonate, 4,5-difluoroethylene carbonate, 4-fluoro-4-methylethylene carbonate, 4,5-difluoro-4-methylethylene carbonate, 4-fluoro-5-methylethylene carbonate, 4,4-difluoro-5-methylethylene carbonate, 4-(fluoromethyl)-ethylene carbonate, 4-(difluoromethyl)-ethylene carbonate, 4-(trifluoromethyl)-ethylene carbonate, 4-(fluoromethyl)-4-fluoroethylene carbonate, 4-(fluoromethyl)-5-fluoroethylene carbonate, 4-fluoro-4,5-dimethylethylene carbonate, 4,5-difluoro-4,5-dimethylethylene carbonate, Examples include 4,4-difluoro-5,5-dimethylethylene carbonate.

[0193] Among these, one or more selected from monofluoroethylene carbonate, 4,4-difluoroethylene carbonate, and 4,5-difluoroethylene carbonate are preferred in terms of imparting high ionic conductivity to the electrolyte and also making it easier to form a stable interfacial protective film.

[0194] Cyclic carbonates having fluorine atoms can be used as a single type or in combination of two or more types in any proportion.

[0195] In the case where the electrolyte related to the present embodiment includes a specific carbonate, it is preferable to include at least one selected from vinylene carbonate and fluoroethylene carbonate in order to impart higher ionic conductivity to the electrolyte and to make it easier to form a stable interfacial protective film, and it is more preferable that the specific carbonate is vinylene carbonate in order to make it easier to form a more stable interfacial protective film.

[0196] When the electrolyte related to the present embodiment comprises at least one selected from vinylene carbonate and fluoroethylene carbonate, the total content of vinylene carbonate and fluoroethylene carbonate in the total amount of the electrolyte related to the present embodiment is typically 0.001 mass% or more, preferably 0.01 mass% or more, more preferably 0.1 mass% or more, and even more preferably 0.5 mass% or more, and is also typically 10 mass% or less, preferably 6 mass% or less, more preferably 5 mass% or less, and even more preferably 4 mass% or less. Furthermore, the total content of vinylene carbonate and fluoroethylene carbonate is typically 0.001 to 10 mass%, preferably 0.01 to 6 mass%, more preferably 0.1 to 5 mass%, and even more preferably 0.5 to 4 mass% in the total amount of the electrolyte. In addition, when two or more specific carbonate compounds are contained, the content refers to the total content thereof.

[0197] If the total content of vinylene carbonate and fluoroethylene carbonate is within the above range, battery characteristics, particularly durability, can be improved. Although the reason is not certain, it is thought that by including at least one selected from vinylene carbonate and fluoroethylene carbonate in this ratio, a film is formed on the electrode, thereby minimizing side reactions of the electrolyte components.

[0198] The identification and measurement of the content of vinylene carbonate and fluoroethylene carbonate are carried out by nuclear magnetic resonance (NMR) spectroscopy.

[0199] When the electrolyte related to the present embodiment comprises at least one selected from vinylene carbonate and fluoroethylene carbonate, the mass ratio of the total content of vinylene carbonate and fluoroethylene carbonate to the content of the compound represented by general formula (1), i.e., the mass ratio represented as the total [g] of vinylene carbonate and fluoroethylene carbonate / the compound represented by general formula (1) [g], is typically 0.01 or more, preferably 0.05 or more, more preferably 0.3 or more, and even more preferably 0.5 or more, and is also typically 100 or less, preferably 50 or less, more preferably 20 or less, and even more preferably 15 or less. And, the mass ratio is typically 0.01 to 100, preferably 0.05 to 50, more preferably 0.3 to 20, and even more preferably 0.5 to 15. Also, when two or more types of compounds represented by general formula (1) and fluoroethylene carbonate are each contained, the content refers to the total content of each.

[0200] If the mass ratio is within the above range, the battery characteristics, especially durability, can be improved. Although the reason is not certain, it is thought that by including vinylene carbonate and fluoroethylene carbonate and a compound represented by general formula (1) within the above range of mass ratio, a film is formed on the electrode, thereby minimizing side reactions of the electrolyte components.

[0201] In the case where the electrolyte related to the present embodiment contains at least one selected from vinylene carbonate and fluoroethylene carbonate, the mass ratio of the total content of vinylene carbonate and fluoroethylene carbonate to the total content of the main salt constituting the electrolyte, i.e., the mass ratio expressed as the total content of vinylene carbonate and fluoroethylene carbonate [g] / main salt [g], is typically 0.00005 or more, preferably 0.0005 or more, more preferably 0.001 or more, even more preferably 0.01 or more, even more preferably 0.02 or more, particularly preferably 0.025 or more, and also typically 0.5 or less, preferably 0.45 or less, more preferably 0.4 or less, and even more preferably 0.35 or less. And, the above mass ratio is typically 0.00005 to 0.5, preferably 0.0005 to 0.5, more preferably 0.001 to 0.45, even more preferably 0.01 to 0.4, even more preferably 0.02 to 0.35, and particularly preferably 0.025 to 0.35. Also, when two or more types of main salt and fluoroethylene carbonate are each contained, the above content refers to the total content of each.

[0202] If the mass ratio is within the above range, the battery characteristics, especially durability, can be improved. Although the reason is not certain, it is thought that by including vinylene carbonate and fluoroethylene carbonate and a compound represented by general formula (1) within the above range of mass ratio, a film is formed on the electrode, thereby minimizing side reactions of the electrolyte in the battery system.

[0203] [1-5-2. Organic compounds having isocyanate groups]

[0204] As for the organic compound having an isocyanate group, which is one embodiment of the auxiliary agent in the present embodiment, it is not particularly limited as long as it is an organic compound having at least one isocyanate group in a molecule. The number of isocyanate groups in one molecule is preferably 1 to 4, more preferably 2 or 3, and even more preferably 2.

[0205] Examples of organic compounds having an isocyanate group include monoisocyanate compounds such as methyl isocyanate, ethyl isocyanate, butyl isocyanate, vinyl isocyanate, propargyl isocyanate, cyclohexyl isocyanate, phenyl isocyanate, 2-isocyanatoethyl acrylate, 2-isocyanatoethyl methacrylate; diisocyanate compounds such as monomethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, octamethylene diisocyanate, 1,4-phenylene diisocyanate, 1,3-diisocyanatopropane, 1,3-bis(isocyanatomethyl)cyclohexane, carbonyl diisocyanate, 1,4-diisocyanato-2-fluorobutane; etc.

[0206] In particular, from the perspective of forming a stable interfacial protective film, an organic compound having at least two isocyanate groups is preferred, hexamethylene diisocyanate and 1,3-bis(isocyanatomethyl)cyclohexane are more preferred, and 1,3-bis(isocyanatomethyl)cyclohexane is even more preferred.

[0207] [1-5-3. Organic compounds with an isocyanuric acid backbone]

[0208] As for the organic compound having an isocyanuric acid backbone (hereinafter also referred to as "isocyanurate compound") which is one embodiment of the auxiliary agent in the present embodiment, it is not particularly limited as long as it is an organic compound having at least one isocyanuric acid backbone in its molecule. Examples of organic compounds having an isocyanuric acid backbone include the following compounds.

[0209] [Chemical Formula 10]

[0210]

[0211] As an isocyanurate compound, particularly in terms of forming a stable interfacial protective film, an isocyanurate compound having a saturated or unsaturated aliphatic hydrocarbon group that may have a halogen atom is preferred, an isocyanurate compound having an unsaturated aliphatic hydrocarbon group containing a carbon-carbon unsaturated bond at the terminal is more preferred, and trialyl isocyanurate is even more preferred.

[0212] [1-5-4. Sulfur-containing organic compounds]

[0213] As for the sulfur-containing organic compound which is one aspect of the auxiliary agent in this embodiment, it is not particularly limited to any organic compound having at least one sulfur atom (S) in the molecule, but does not include the compound represented by Formula (2) of the present invention. Preferably, the sulfur-containing organic compound is an organic compound having at least one S=O bond, and more preferably, ester compounds having an S=O bond, such as chain-type sulfonic acid esters and cyclic sulfonic acid esters, may be examples.

[0214] However, an anion-containing compound having S=O bonds and SX bonds is not a "sulfur-containing organic compound" and is included in the "anion-containing compound having S=O bonds and SX bonds" mentioned above.

[0215] As sulfur-containing organic compounds, for example, chain-type sulfonic acid esters such as alkyl disulfonic acid esters including methyl fluorosulfonate, methyl methanesulfonate, ethyl methanesulfonate, busulpan, methyl methanesulfonyloxyacetate, methyl vinylsulfonate, allyl vinylsulfonate, propargyl allylsulfonic acid, methoxycarbonylmethyl methanedisulfonate, ethoxycarbonylmethyl methanedisulfonate, methoxycarbonylmethyl 1,3-butanedisulfonate, ethoxycarbonylmethyl 1,3-butanedisulfonate, 1-methoxycarbonylethyl 1,3-butanedisulfonate, 1-ethoxycarbonylethyl 1,3-butanedisulfonate, butane-2,3-diyl dimethanesulfonate, butane-1,4-diyl dimethanesulfonate; Cyclic acid esters such as 1,3-propanesulfone, 1-fluoro-1,3-propanesulfone, 1-methyl-1,3-propanesulfone, 1-propene-1,3-sulfone, 2-propene-1,3-sulfone, 1-fluoro-1-propene-1,3-sulfone, 1-methyl-1-propene-1,3-sulfone, 1,3-butanesulfone, 2,4-butanesulfone, 1,4-butanesulfone, 1,5-pentanesulfone, methylenemethanedisulfonate, ethylenemethanedisulfonate, 2,2-dioxide-1,2-oxathiolan-4-yl acetate; Examples include cyclic sulfones such as 1,1-dioxide-tetrahydrothiophene-3-yl methanesulfonate and 1,1-dioxide-2,3-dihydrothiophene-3-yl methanesulfonate; and vinylsulfone compounds such as divinylsulfone, 1,2-bis(vinylsulfonyl)ethane and bis(2-vinylsulfonylethyl)ether.

[0216] In particular, from the perspective of forming a stable interfacial protective film, chain-type or cyclic sulfonic acid esters are more preferable, cyclic sulfonic acid esters are particularly preferable, and 1,3-propanesulfone and methylenemethanedisulfonate are most preferable.

[0217] [1-5-5. Phosphorus-containing organic compounds]

[0218] As for the phosphorus-containing organic compound which is one aspect of the auxiliary agent in this embodiment, it is not particularly limited to any compound having at least one phosphorus atom in its molecule. However, the compound represented by the general formula (1) of the present invention is not included in the “phosphorus-containing organic compound.” Furthermore, an anion-containing compound having a P=O bond and a PF bond is not considered a “phosphorus-containing organic compound,” but is included in the “anion-containing compound having a P=O bond and a PF bond” as a specific anion-containing compound.

[0219] Examples of phosphorus-containing organic compounds include trimethyl phosphate, tributyl phosphate, trioctyl phosphate, tris(2,2,2-trifluoroethyl phosphate), ethyl-2-(diethoxyphosphoryl)acetate and 2-propynyl-2-(diethoxyphosphoryl)acetate.

[0220] In particular, ethyl 2-(diethoxyphosphoryl)acetate or 2-propynyl-2-(diethoxyphosphoryl)acetate is preferred, and 2-propynyl-2-(diethoxyphosphoryl)acetate is more preferred.

[0221] [1-5-6. Silicon-containing compounds]

[0222] As for the silicon-containing compound which is one embodiment of the auxiliary agent in this embodiment, it is not particularly limited as long as it is a compound having at least one silicon atom in the molecule.

[0223] Silicon-containing compounds include, for example, boric acid compounds such as tris(trimethylsilyl), tris(trimethoxysilyl), tris(triethylsilyl), and tris(dimethylvinylsilyl); phosphate compounds such as tris(trimethylsilyl), tris(triethylsilyl), tris(triphenylsilyl), tris(trimethoxysilyl), and tris(dimethylvinylsilyl); phosphite compounds such as tris(trimethylsilyl), tris(triethylsilyl), tris(triphenylsilyl), tris(trimethoxysilyl), and tris(dimethylvinylsilyl); and sulfonic acid compounds such as trimethylsilyl methanesulfonic acid and trimethylsilyl tetrafluoromethanesulfonic acid. Silane compounds such as tetramethylsilane, trimethylvinylsilane, dimethyldivinylsilane, methyltrivinylsilane, tetravinylsilane, etc.; disilane compounds such as hexamethyldisilane, hexaethyldisilane, 1,1,2,2-tetramethyldisilane, 1,2-diphenyltetramethyldisilane, etc.; disiloxane compounds such as hexamethyldisiloxane, 1,3-divinyltetramethyldisiloxane, 1,1,3,3-tetramethyl-1,3-diphenyldisiloxane, etc.

[0224] In particular, from the perspective of forming a stable interfacial protective film, disilane compounds and disiloxane compounds are preferred, disiloxane compounds are more preferred, hexamethyldisiloxane and 1,3-divinyltetramethyldisiloxane are even more preferred, and 1,3-divinyltetramethyldisiloxane is particularly preferred.

[0225] [1-5-7. Aromatic Compounds]

[0226] As an aromatic compound which is one aspect of the auxiliary agent in the present embodiment, it is not particularly limited as long as it is a compound having an aromatic group within the molecule. Examples of aromatic compounds include aromatic compounds having branched alkyl groups such as cyclohexylbenzene, tert-butylbenzene, tert-amylbenzene, 1-fluoro-4-tert-butylbenzene; aromatic compounds such as biphenyl, terphenyl (o-, m-, p-), fluorobenzene, methylphenyl carbonate, ethylphenyl carbonate, diphenyl carbonate; etc.

[0227] In particular, biphenyl, terphenyl (o-, m-, p-type), fluorobenzene, cyclohexylbenzene, tert-butylbenzene, and tert-amylbenzene are more preferred, and biphenyl, o-terphenyl, fluorobenzene, cyclohexylbenzene, and tert-amylbenzene are more preferred.

[0228] [1-5-8. Organic compounds containing cyano groups]

[0229] As for the organic compound having a cyano group, which is one embodiment of the auxiliary agent in this embodiment, it is not particularly limited as long as it is an organic compound having at least one cyano group in its molecule.

[0230] Organic compounds having a cyano group include, for example, organic compounds having one cyano group in their molecule such as acetonitrile, propionitrile, butyronitrile, pentanitrile, hexanitrile, decanitrile, undecanenitrile, dodecanenitrile, cyclohexanecarbonitrile, acrylonitrile, methacrylonitrile, crotononitrile, etc.; organic compounds having two cyano groups in their molecule such as succinonitrile, glutaronitrile, adiponitrile, pimelonitrile, suberonitrile, sebaconitrile, methylmalononitrile, ethylmalononitrile, bicyclohexyl-1,1-dicarbonitrile, 1,4-dicyanopentan, 1,2-dicyanobenzene, etc. Examples include organic compounds having three cyano groups within the molecule, such as 1,2,3-propanetricarbonitrile, 1,2,3-tris(2-cyanoethoxy)propane, 1,3,5-cyclohexanetricarbonitrile, and 1,3,5-benzenetricarbonitrile.

[0231] In particular, organic compounds having two cyano groups are preferred for the formation of a stable interfacial protective film, succinonitrile and adiponitrile are more preferred, and adiponitrile is even more preferred.

[0232] [1-5-9. Fluoride-free carboxylic acid esters]

[0233] The fluorine-free carboxylic acid ester, which is one aspect of the auxiliary agent in the present embodiment, is not particularly limited as long as it is a carboxylic acid ester that does not have a fluorine atom in its molecule.

[0234] Preferably, it is a fluorine-free chain-type carboxylic acid ester, and more preferably, a fluorine-free saturated chain-type carboxylic acid ester.

[0235] The total number of carbon atoms in the fluorine-free chain-type carboxylic acid ester is preferably 3 or more, more preferably 4 or more, preferably 7 or less, more preferably 6 or less, and even more preferably 5 or less. And, the total number of carbon atoms in the fluorine-free chain-type carboxylic acid ester is preferably 3 to 7, more preferably 3 to 6, and even more preferably 4 to 5.

[0236] Examples of chain-type carboxylic acid esters include methyl acetate, ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, methyl propionate, ethyl propionate, n-propyl propionate, isopropyl propionate, n-butyl propionate, methyl pivalate, ethyl pivalate, n-propyl pivalate, isopropyl pivalate, n-butyl pivalate, methyl acrylate, ethyl acrylate, methyl methacrylate, ethyl methacrylate, methyl crotonicate, ethyl crotonicate, 2-methyl propinate, etc.

[0237] In particular, from the perspective of improving the output characteristics of the battery, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, and n-propyl propionate are preferred, and methyl propionate is more preferred.

[0238] [1-5-10. Cyclic Ether Compounds]

[0239] As a cyclic ether compound which is one aspect of the auxiliary agent in the present embodiment, it is not particularly limited as long as it is a compound having one or more ether bonds within the molecule. Examples of cyclic ether compounds include, for instance, cyclic acetal compounds such as 1,3-dioxolane, 1,3-dioxane, or 1,3,5-trioxane.

[0240] As for the cyclic ether compound, a cyclic acetal compound is particularly preferred, 1,3-dioxolane or 1,3-dioxane is preferred, and 1,3-dioxane is more preferred.

[0241] [1-5-11. Acid Anhydride]

[0242] As for the acid anhydride which is one aspect of the auxiliary agent in the present embodiment, it is not particularly limited as long as it is an acid anhydride having a “C(=O)-OC(=O) group,” a “C(=O)-OS(=O)2 group,” or an “S(=O)2-OS(=O)2 group” within the molecule.

[0243] Examples of acid anhydrides include, for instance, chain-type carboxylic acid anhydrides such as acetic anhydride, acrylic anhydride, methacrylic anhydride, cyclohexanecarboxylic anhydride, propinic anhydride, benzoic anhydride, fluoroacetic anhydride, 4-fluorobenzoic anhydride, and acetic acid propionic anhydride; succinic anhydride, maleic anhydride, citraconic anhydride, glutaric anhydride, itaconic anhydride, fluorosuccinic anhydride, allylsuccinic anhydride, 1,2-oxathiolan-5-one 2,2-dioxide, 1,2,6-oxaditian 2,2,6,6-tetraoxide, etc.

[0244] In particular, regarding the formation of a stable interfacial protective film, methacrylic anhydride, succinic anhydride, maleic anhydride, and allyl succinic anhydride are preferred, and succinic anhydride or allyl succinic anhydride is more preferred.

[0245] [1-5-12. Compounds Containing Triple Bonds]

[0246] As a compound containing a triple bond, which is one embodiment of the auxiliary agent in the present embodiment, it is not particularly limited as long as it is a compound having at least one triple bond within the molecule. Examples of compounds containing a triple bond include 2-propynylmethyl carbonate, 2-propynyl acetate, 2-propynyl formic acid, 2-propynyl methacrylate, 2-propynyl methanesulfonic acid, 2-propynyl vinylsulfonic acid, 2-(methanesulfonyloxy)propionic acid, di(2-propynyl)oxalate, 2-butin-1,4-diyldimethansulfonate, and 2-butin-1,4-diyldiformate.

[0247] In particular, 2-propynylmethyl carbonate, 2-propynyl methacrylate, 2-propynyl methanesulfonic acid, 2-propynyl vinylsulfonic acid, di(2-propynyl)oxalate and 2-butin-1,4-diyldimethanesulfonate are preferred, and 2-propynyl methanesulfonic acid, 2-propynyl vinylsulfonic acid, di(2-propynyl)oxalate and 2-butin-1,4-diyldimethanesulfonate are more preferred.

[0248] [1-5-13. Phospazene Compounds]

[0249] As for the phosphazene compound which is one aspect of the auxiliary agent in the present embodiment, it is not particularly limited as long as it is a compound having an "N=PN group" in its molecule. Examples of phosphazene compounds include cyclic phosphazene compounds such as methoxypentafluorocyclotriphosphazene, ethoxypentafluorocyclotriphosphazene, phenoxypentafluorocyclotriphosphazene, or ethoxyheptafluorocyclotetraphosphazene.

[0250] In particular, cyclic phosphazene compounds such as methoxypentafluorocyclotriphosphazene, ethoxypentafluorocyclotriphosphazene, or phenoxypentafluorocyclotriphosphazene are preferred, and methoxypentafluorocyclotriphosphazene or ethoxypentafluorocyclotriphosphazene is even more preferred.

[0251] [Mass ratio of main salt and auxiliary agent]

[0252] In the case where the electrolyte related to the present embodiment includes an auxiliary agent other than a specific carbonate compound as an auxiliary agent, the mass ratio of the content of the auxiliary agent to the content of the main salt contained in the electrolyte in the electrolyte, i.e., the mass ratio expressed as auxiliary agent [g] / main salt [g], is typically 0.00005 or more, preferably 0.0001 or more, more preferably 0.001 or more, even more preferably 0.01 or more, even more preferably 0.02 or more, particularly preferably 0.025 or more, and also typically 0.5 or less, preferably 0.45 or less, more preferably 0.4 or less, and even more preferably 0.35 or less. In addition, the above mass ratio is typically 0.00005 to 0.5, preferably 0.0001 to 0.5, more preferably 0.001 to 0.45, even more preferably 0.01 to 0.4, even more preferably 0.02 to 0.4, and particularly preferably 0.025 to 0.35. Furthermore, the content of the main salt and auxiliary agent refers to the total content of the main salt and auxiliary agent when two or more types of the main salt and auxiliary agent are each contained. Additionally, depending on the content of a specific anion-containing compound, the content of the specific anion-containing compound is also included in the main salt or auxiliary agent.

[0253] If the above mass ratio is within the above range, the battery characteristics, particularly the rate of increase in internal resistance, can be suppressed. Although the reason is not certain, it is believed that by including the auxiliary agent and the main salt within the above range of mass ratio, a film is formed on the electrode, thereby minimizing side reactions of the electrolyte within the battery system.

[0254] [1-6. Method for preparing electrolyte]

[0255] The method for preparing the electrolyte of the present invention includes a process of dissolving the compound represented by the general formula (1), the compound represented by the formula (2), and the electrolyte in the non-aqueous solvent.

[0256] <2. Battery>

[0257] The battery related to the present embodiment is a battery comprising a positive electrode and a negative electrode capable of absorbing and releasing metal ions, and an electrolyte, wherein the electrolyte is the electrolyte described in <1. Electrolyte>. The battery is preferably a non-aqueous electrolyte battery, and more preferably a non-aqueous electrolyte secondary battery.

[0258] Regarding the components of the battery other than the above-mentioned electrolyte, a lithium-ion secondary battery is described below as an example. Furthermore, a lithium-ion secondary battery is a secondary battery comprising a positive electrode capable of absorbing and releasing lithium ions, a negative electrode capable of absorbing and releasing lithium ions, and a lithium salt as the main salt of the electrolyte contained in the above-mentioned electrolyte.

[0259] [2-1. Straight Drama]

[0260] The positive electrode has a positive electrode active material capable of absorbing and releasing lithium ions on at least a portion of the surface of the current collector.

[0261] [2-1-1. Positive Electrode Active Material]

[0262] The positive electrode active material used for the positive electrode is not particularly limited as long as it is capable of electrochemically absorbing and releasing metal ions, but examples include lithium transition metal-based compounds.

[0263] The following describes the positive electrode active material (lithium transition metal-based compound) used in the positive electrode.

[0264] [2-1-1-1. Lithium Transition Metal Compounds]

[0265] A lithium transition metal compound is a compound having a structure capable of extracting and inserting lithium ions, and examples include sulfides, phosphate compounds, silicate compounds, boric acid compounds, and lithium transition metal complex oxides. Among these, phosphate compounds and lithium transition metal complex oxides are preferred, and lithium transition metal complex oxides are more preferred.

[0266] Examples of lithium transition metal composite oxides include spinel structures and olivine structures that enable three-dimensional diffusion of lithium ions, or layered structures that enable two-dimensional diffusion of lithium ions. Among these, lithium transition metal composite oxides having a layered structure are preferred from the perspective of improving battery capacity.

[0267] Lithium transition metal composite oxides having a spinel structure are generally represented by the following composition formula (1).

[0268] Li x' M' y' O4··· (1)

[0269] (In Equation (1), 0.8≤x'≤1.5 and 1.9≤y'≤2.1, and M' contains at least one transition metal element.)

[0270] As a lithium transition metal composite oxide having a spinel structure, specifically LiMn2O4, LiCoMnO4, and LiNi 0.5 Mn 1.5 Examples include O4, LiCoVO4, etc.

[0271] Lithium transition metal composite oxides having an olivine structure are generally represented by the following composition formula (2).

[0272] Li x" M" y" PO4··· (2)

[0273] (In Equation (2), 0.8≤x"≤1.5 and 0.9≤y"≤1.1, and M" contains at least one transition metal element.)

[0274] Examples of M" include Fe, Ni, Co, Mn, etc.

[0275] Lithium transition metal composite oxides having an olivine structure, specifically LiFePO4, can be cited.

[0276] Lithium transition metal composite oxides having a layered structure are generally represented by the following composition formula (3).

[0277] Li 1+x M y O2··· (3)

[0278] (In Equation (3), -0.2≤x≤0.5, 0.5≤y≤1.1, and M contains at least one transition metal element.)

[0279] As a lithium transition metal composite oxide having a layered structure, specifically LiCoO2, LiNiO2, and LiNi 0.90 Co 0.05 Mn 0.05 O2, LiNi 0.85 Co 0.10 Al 0.05 O2, LiNi 0.80 Co 0.15 Al 0.05 O2, LiNi 0.33 Co 0.33 Mn 0.33 O2, Li 1.05 Ni 0.33 Co 0.33 Mn 0.33 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, Li 1.05 Ni 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, Li 1.0 Ni 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.91 Co 0.06 Mn 0.03 O2, LiNi 0.91 Co 0.06 Al 0.03 O2, LiNi 0.90 Co 0.03 Al 0.07 O2, Li 1.00 Ni 0.61 Co 0.2 0Mn 0.19O2, Li[Li 1 / 3 Mn 2 / 3 Examples include O2, and their solid solutions.

[0280] Among lithium transition metal composite oxides having a layered structure, it is preferable to have a lithium transition metal composite oxide represented by the following composition formula (4) in terms of high capacity.

[0281] Li 1+y M1O2 (4)

[0282] (In Equation (4), ―0.2≤y≤0.5, M1 represents a plurality of elements including at least Ni, and the molar ratio of the content of Ni to the content of all elements contained in M1 (Ni / M1) is 0.30 to 1.0.)

[0283] In the above composition formula (4), the molar ratio (Ni / M1) is 0.30 or higher, preferably 0.40 or higher, more preferably 0.50 or higher, and also preferably 1.0 or lower, more preferably 0.90 or lower. And, the molar ratio (Ni / M1) is 0.30 to 1.0, preferably 0.40 to 0.90, more preferably 0.50 to 0.90.

[0284] If the molar ratio (Ni / M1) is in this range, the compound represented by general formula (1) is more likely to form a film on the positive electrode, and by suppressing side reactions between the positive electrode and the electrolyte, the rate of increase in internal resistance after high-temperature storage of the battery can be suppressed.

[0285] Specific examples of lithium transition metal oxides having a layered structure represented by formula (4) include LiNiO2 and LiNi 0.90 Co 0.05 Mn 0.05 O2, LiNi 0.85 Co 0.10 Al 0.05 O2, LiNi 0.80 Co 0.15 Al 0.05 O2, LiNi0.33 Co 0.33 Mn 0.33 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, Li 1.05 Ni 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, Li 1.0 Ni 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.91 Co 0.06 Mn 0.03 O2, LiNi 0.91 Co 0.06 Al 0.03 O2, LiNi 0.90 Co 0.03 Al 0.07 O2, Li 1.00 Ni 0.61 Co 0.2 0Mn 0.19 Examples include O2.

[0286] Among lithium transition metal compounds, a lithium transition metal composite oxide having a layered structure is preferred for improving battery capacity, and a lithium transition metal composite oxide represented by the following composition formula (5) is more preferred.

[0287] Li a1 Ni b1 M2 c1 O2 (5)

[0288] (In Equation (5), M2 represents at least one element selected from the group consisting of Co, Mn, Al, Mg, Zr, Fe, Ti, and Er, 0.80≤a1≤1.10, 0.30≤b1≤0.98, 0.00≤c1≤0.70, and 0.90≤b1+c1≤1.10.)

[0289] In the composition formula (5), b1 is 0.30 or higher, preferably 0.40 or higher, more preferably 0.45 or higher, even more preferably 0.50 or higher, and also 0.98 or lower. In addition, in the composition formula (5), b1 is preferably 0.40 to 0.98, more preferably 0.45 to 0.98, and even more preferably 0.50 to 0.98.

[0290] A specific example of a lithium transition metal oxide having a layered structure represented by the composition formula (5) is LiNi 0.90 Co 0.05 Mn 0.05 O2, LiNi 0.85 Co 0.10 Al 0.05 O2, LiNi 0.80 Co 0.15 Al 0.05 O2, LiNi 0.33 Co 0.33 Mn 0.33 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, Li 1.05 Ni 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, Li 1.0 Ni 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.91 Co 0.06 Mn 0.03 O2, LiNi 0.91 Co 0.06 Al 0.03 O2, LiNi 0.90 Co 0.03 Al 0.07 O2, Li 1.00 Ni 0.61 Co 0.2 0Mn 0.19 Examples include O2.

[0291] In particular, from the perspective of structural stability of the lithium transition metal composite oxide, it is preferable to have a lithium transition metal composite oxide represented by the following composition formula (6).

[0292] Li a2 Ni b2 Co c2 M3 d2 O2 (6)

[0293] (In Equation (6), M3 represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti and Er, 0.80≤a2≤1.10, 0.30≤b2≤0.98, 0.01≤c2≤0.70, and 0.01≤d2≤0.60, and 0.90≤b2+c2+d2≤1.10.)

[0294] In the composition formula (6), b2 is preferably 0.40 or higher, more preferably 0.45 or higher, and even more preferably 0.50 or higher. Also, in the composition formula (6), b2 is 0.30 to 0.98, 0.40 to 0.98 is preferable, 0.45 to 0.98 is more preferable, and 0.50 to 0.98 is even more preferable.

[0295] In addition, among the composition formula (6), d2 is preferably 0.01 or more, more preferably 0.10 or more, and more preferably 0.60 or less. Also, among the composition formula (6), d2 is preferably 0.01 to 0.60, and more preferably 0.10 to 0.60.

[0296] Suitable examples of the lithium transition metal composite oxide represented by the above composition formula (6) include LiNi 0.90 Co 0.05 Mn 0.05 O2, LiNi 0.85 Co 0.10 Al 0.05 O2, LiNi 0.80 Co 0.15 Al 0.05 O2, LiNi 0.33 Co 0.33 Mn0.33 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, Li 1.05 Ni 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, Li 1.0 Ni 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.91 Co 0.06 Mn 0.03 O2, LiNi 0.91 Co 0.06 Al 0.03 O2, LiNi 0.90 Co 0.03 Al 0.07 O2, Li 1.00 Ni 0.61 Co 0.2 0Mn 0.19 Examples include O2.

[0297] Among the above composition formulas (4) or (5), in order to increase the structural stability of the lithium transition metal oxide and suppress structural degradation when repeatedly charged and discharged, it is preferable that M1 or M2 include Mn or Al, and more preferable that it include Mn.

[0298] Among the above composition formula (6), in order to increase the structural stability of the lithium transition metal composite oxide and suppress structural degradation when repeatedly charged and discharged, it is preferable that M3 contains Mn or Al, and more preferable that it contains Mn.

[0299] Identification of the positive electrode active material and measurement of its content are performed by ICP emission spectroscopy after wet digestion of the sample.

[0300] [2-1-1-2. Introduction of Different Elements]

[0301] The lithium transition metal oxide may additionally contain an element (a dielement) other than the element contained in any one of the composition formulas (1) to (6).

[0302] [2-1-1-3. Surface Coating]

[0303] As a positive electrode, a material having a composition different from that of the positive electrode active material (surface-attached material) may be used, provided that the surface of the positive electrode active material is attached thereto.

[0304] Examples of surface-attached materials include oxides such as aluminum oxide, sulfates such as lithium sulfate, and carbonates such as lithium carbonate. These surface-attached materials can be attached to the surface of the positive electrode active material by, for example, by dissolving or suspending them in a solvent, impregnating and adding them to the positive electrode active material, or by drying.

[0305] The amount of surface-attached material is preferably 1 μmol / g or more with respect to the positive electrode active material, more preferably 10 μmol / g or more, and also typically preferably 1 mmol / g or less. Furthermore, the amount of surface-attached material is preferably 1 μmol / g to 1 mmol / g with respect to the positive electrode active material, and more preferably 10 μmol / g to 1 mmol / g.

[0306] In this specification, a surface-attached material attached to the surface of a positive electrode active material is also referred to as a "positive electrode active material."

[0307] [2-1-1-4. Blend]

[0308] The positive electrode active material can be used as a single type or in combination of two or more types in any ratio.

[0309] [2-1-2. Composition and Manufacturing Method of the Pole]

[0310] The manufacture of a positive electrode having the above positive electrode active material can be carried out by conventional methods. That is, a positive electrode can be obtained by a method in which a positive electrode active material, a binder, and, if necessary, a conductive material and a thickener are dry-mixed to form a sheet and then pressed onto a positive electrode current collector, or by a coating method in which these materials are dissolved or dispersed in a liquid medium such as an aqueous solvent or an organic solvent to form a slurry, which is then applied to a positive electrode current collector and dried to form a layer of positive electrode active material on the current collector. In addition, for example, the positive electrode active material may be roll-molded to form a sheet electrode or compression-molded to form a pellet electrode.

[0311] Below, a case in which a slurry is sequentially applied and dried on a positive electrode current collector is described.

[0312] [2-1-2-1. Content of Positive Electrode Active Material]

[0313] The positive electrode consists of a current collector and a positive electrode active material layer comprising a positive electrode active material formed on the current collector. The content of the positive electrode active material in the positive electrode active material layer is typically 80 to 99.5 mass%.

[0314] [2-1-2-2. Electrode Density]

[0315] The positive electrode active material layer obtained by coating and drying the positive electrode active material together with a binder, conductive material, etc., is preferably compacted by a hand press, roller press, etc., in order to increase the packing density of the positive electrode active material.

[0316] Although the electrode structure when the positive electrode active material is electroded is not particularly limited, the density of the positive electrode active material layer existing on the current collector is typically 1.5 to 4.5 g / cm³ 3 am.

[0317] [2-1-2-3. Binding Agent]

[0318] As for the binder, if it is a material that dissolves or disperses in a liquid medium for a slurry when forming a positive electrode active material layer by a coating method, the type thereof is not particularly limited.

[0319] For example, fluorine-based resins such as polyvinyl fluoride, polyvinylidene fluoride, and polytetrafluoroethylene are preferred in terms of weather resistance, chemical resistance, heat resistance, flame retardancy, etc.; and CN group-containing polymers such as polyacrylonitrile and polyvinylidene cyanide are preferred.

[0320] In addition, mixtures, modifieds, derivatives, random copolymers, alternating copolymers, graft copolymers, block copolymers, etc. of the above polymers may also be used. Furthermore, the binder may be used as a single type or in combination of two or more types in any ratio.

[0321] When a resin is used as a binder, the weight-average molecular weight of the resin is optional as long as it does not impede the effects of the present invention, and is typically 10,000 to 3 million. If the molecular weight is within this range, the strength of the electrode is improved, and the formation of the electrode can be carried out preferably.

[0322] The content of the binder in the positive electrode active material layer is typically 0.1 to 20 mass%.

[0323] [2-1-2-4. Challenge Material]

[0324] As for challenge materials, any announced challenge material may be used at will.

[0325] Specific examples include metallic materials such as copper and nickel; graphite such as natural graphite and artificial graphite; carbon black such as acetylene black; carbon-based materials such as amorphous carbon such as needle coke; etc. The conductive material may be used as a single type or in combination of two or more types in any ratio.

[0326] The conductive material is typically used to be contained in the positive electrode active material layer in an amount of 0.01 to 20 mass%.

[0327] [2-1-2-5. Entire House]

[0328] The material of the current collector holding the positive electrode active material is not particularly limited and any known material may be used at will. Specific examples include metal materials such as aluminum, stainless steel, nickel plating, titanium, and tantalum, and aluminum is preferred.

[0329] Examples of shapes for the current collector include metal foil, metal cylinder, metal coil, metal plate, metal thin film, expanded metal, punched metal, foamed metal, etc. Among these, metal foil or metal thin film is preferred. In addition, the metal thin film may be formed into a mesh shape as appropriate.

[0330] When the shape of the current collector of the positive electrode is plate-like or film-like, the thickness of the current collector is arbitrary, but is typically 1 μm to 1 mm.

[0331] [2-1-2-6. Thickness of the positive plate]

[0332] The thickness of the positive electrode (positive electrode plate) is not particularly limited, but from the perspective of high capacity and high output, the thickness of the positive electrode active material layer, which is the thickness of the positive electrode plate minus the thickness of the current collector, is typically 10 to 500 μm for one side of the current collector. The positive electrode active material layer may be formed on one surface of the current collector or on both surfaces.

[0333] [2-1-2-7. Surface Coating of Positive Plate]

[0334] The positive electrode plate may be used with a material having a composition different from that of the positive electrode active material attached to its surface, and the material used may be the same as the surface-attached material that may be attached to the surface of the positive electrode active material.

[0335] [2-2. Pole]

[0336] The negative electrode has a negative electrode active material capable of absorbing and releasing lithium ions on at least a portion of the current collector surface.

[0337] [2-2-1. Negative Electrode Active Material]

[0338] As for the negative electrode active material used for the negative electrode, there are no particular restrictions as long as it is capable of electrochemically absorbing and releasing metal ions.

[0339] Specific examples include (i) carbon-based materials, (ii) materials containing metal elements and / or metalloid elements capable of alloying with Li, (iii) lithium-containing metal composite oxide materials, and (iv) mixtures of (i) to (iii).

[0340] Among these, (i) a carbon-based material, (ii) a material containing a metal element and / or a metal element capable of alloying with Li, and (iv) a mixture of (i) to (iii) are preferred in that they have good cycle characteristics and safety and also excellent continuous charging characteristics, and (iv) a mixture of a material containing a metal element and / or a metal element capable of alloying with Li and graphite is more preferred.

[0341] These can be used as a single type or in combination of two or more types in any ratio.

[0342] [2-2-1-1. Carbon-based Materials]

[0343] (i) Examples of carbon-based materials include natural graphite, artificial graphite, amorphous carbon, carbon-coated graphite, graphite-coated graphite, and resin-coated graphite. Among these, natural graphite is preferred. Carbon-based materials may be used as a single type or in combination of two or more types in any proportion.

[0344] Examples of natural graphite include scaly graphite, flake-like graphite, and / or graphite particles obtained by treating these graphites with spheroidization or densification. Among these, spherical or ellipsoidal graphite particles obtained by spheroidization treatment are preferred from the perspective of particle filling ability or charge / discharge rate characteristics.

[0345] The average particle size (d50) of graphite particles is typically 1 to 100 μm. Here, the average particle size (d50) is the volume-based average particle size (median diameter) obtained by laser diffraction and scattering.

[0346] [2-2-1-2. Physical Properties of Carbon-based Materials]

[0347] It is preferable that the carbon-based material used as the negative electrode active material satisfies at least one of the physical properties and shape characteristics shown in (1) to (4) below, and it is more preferable that it satisfies multiple items simultaneously.

[0348] (1) X-ray diffraction parameters

[0349] The d value (interlayer distance) of the lattice plane (002 plane) obtained from X-ray diffraction by the Gakushin method of carbon-based materials is typically 0.335 to 0.360 nm. In addition, the crystallite size (Lc) of the carbon-based material obtained from X-ray diffraction by the Gakushin method is 1.0 nm or greater.

[0350] (2) Average particle size based on volume

[0351] The volume-based average particle size of carbon-based materials is the volume-based average particle size (median diameter) obtained by the laser diffraction and scattering method, and is typically 1 to 100 μm.

[0352] (3) Raman R value, Raman half-length

[0353] The Raman R value of carbon-based materials is a value measured using the argon ion laser Raman spectroscopy, and is typically 0.01 to 1.5.

[0354] In addition, 1580 cm of carbon-based materials -1 The Raman halfway width in this area is not specifically limited, but is typically 10 to 100 cm -1 am.

[0355] (4) BET specific surface area

[0356] The BET specific surface area of ​​carbon-based materials is the value of the specific surface area measured using the BET method, typically ranging from 0.1 to 100 m². 2 ·g -1 am.

[0357] The negative electrode active material may contain two or more types of carbon-based materials with different properties. The properties mentioned here refer to one or more characteristics selected from the group of X-ray diffraction parameters, volume-based average particle size, Raman R value, Raman full width at half maximum, and BET specific surface area as shown in (1) to (4) above.

[0358] Examples of containing two or more types of carbon-based materials with different properties include the fact that the volume-based particle size distribution is not symmetrical with respect to the median diameter, the fact that two or more types of carbon-based materials with different Raman R values ​​are contained, and the fact that the X-ray diffraction parameters are different.

[0359] [2-2-1-3. Materials containing metallic elements and / or metalloid elements capable of alloying with Li]

[0360] (ii) Any previously known material containing a metallic element and / or a metalloid element capable of alloying with Li may be used.

[0361] In terms of capacity and cycle life, it is preferable that the material be a metal or metalloid selected from the group consisting of, for example, Sb, Si, Sn, Al, As, and Zn. Additionally, if a material containing a metal element and / or metalloid element capable of alloying with Li contains two or more types of metals, the material may be an alloy material made of an alloy of these metals.

[0362] In addition, materials containing metal elements and / or metalloid elements capable of alloying with Li may include oxides, nitrides, carbides, etc. of metals and / or metalloids. The material may contain two or more types of metals capable of alloying with Li. Among these, a material containing the element Si is preferred, and metallic Si (hereinafter also referred to as "Si") or Si-containing inorganic compounds are more preferred from the perspective of high capacity. In this specification, Si or Si-containing inorganic compounds are collectively referred to as "Si compounds."

[0363] It is preferable that the content of the material containing a metal element and / or metal element capable of alloying with Li be 0.1 to 25 mass% relative to the total mass of the negative electrode active material.

[0364] In addition, a material containing a metal element and / or metal element capable of alloying with Li may already be alloyed with Li at the time of manufacturing the negative electrode described below, and as such a material, a Si compound is preferred from the perspective of high capacity.

[0365] Si compounds are SiO₂ as Si-containing inorganic compounds. x Examples include (0≤x≤2).

[0366] As metal compounds alloyed with Li, Li y Si (0<y≤4.4), Li 2z SiO 2+z Examples include (0<z≤2).

[0367] As for Si compounds, Si oxide (SiO x1 , 0<x1≤2) is desirable in that it has a larger theoretical capacity compared to graphite, and also, amorphous Si or nano-sized Si crystals are desirable in that it is possible to obtain a high capacity because alkali ions such as lithium ions can easily enter and exit.

[0368] When a material containing a metal element and / or metal element capable of alloying with Li is in particulate form, the average particle size (d50) of the particles is typically 0.01 to 10 μm in terms of cycle life.

[0369] [2-2-1-4. Lithium-containing metal composite oxide materials]

[0370] (iii) As for the lithium-containing metal composite oxide material, it is not particularly limited as long as it is capable of absorbing and releasing lithium ions.

[0371] Specifically, from the perspective of high current density charge / discharge characteristics, a lithium-containing metal composite oxide material containing titanium is preferred, a composite oxide of lithium and titanium (hereinafter also referred to as "lithium titanium composite oxide") is more preferred, and a lithium titanium composite oxide having a spinel structure is even more preferred as it significantly reduces output resistance.

[0372] In addition, the lithium and / or titanium of the lithium titanium composite oxide may be substituted with at least one element selected from the group consisting of other metal elements, for example, Al, Ga, Cu, and Zn.

[0373] As a lithium titanium composite oxide, Li 4 / 3 Ti 5 / 3 O4, Li1Ti2O4 and Li 4 / 5 Ti 11 / 5 O4 is preferred. In addition, as a lithium titanium composite oxide in which a portion of the lithium and / or titanium is substituted with other elements, for example, Li 4 / 3 Ti 4 / 3 Al 1 / 3 O4 is also desirable.

[0374] [2-2-1-5. Mixtures of graphite and materials containing metallic and / or metalloid elements capable of alloying with Li]

[0375] (iv) is a mixture of the above (i) carbon-based material, (ii) a material containing a metal element and / or metal element capable of alloying with Li, and (iii) a lithium-containing metal composite oxide material. Among these, a mixture of a material containing a metal element and / or metal element capable of alloying with Li and graphite is preferred.

[0376] The mixture of graphite and a material containing a metal element and / or a metal element capable of alloying with Li may be a mixture in which the material containing the metal element and / or a metal element capable of alloying with Li and the graphite are mixed in the state of independent particles, or it may be a composite in which the material containing the metal element and / or a metal element capable of alloying with Li exists on the surface or inside of the graphite particles.

[0377] The content ratio of the material containing the metal element and / or metal element capable of alloying with Li to the total of the material containing the metal element and / or metal element capable of alloying with Li and graphite is typically 1 to 99 mass%.

[0378] The identification and content measurement of the negative electrode active material are performed by ICP emission spectroscopy after alkaline melting of the sample.

[0379] [2-2-2. Composition and Manufacturing Method of the Negative Electrode]

[0380] Any known method may be used for manufacturing the negative electrode, as long as it does not impede the effects of the present invention.

[0381] For example, a negative electrode active material can be manufactured by adding a binder, a liquid medium such as an aqueous solvent or an organic solvent, and, if necessary, a thickener, a conductive material, a filler, etc. to the negative electrode active material to form a slurry, coating this onto a current collector, drying it, and then pressing it to form a negative electrode active material layer.

[0382] [2-2-2-1. Content of negative electrode active material]

[0383] The negative electrode consists of a current collector and a negative electrode active material layer comprising a negative electrode active material formed on the current collector. The content of the negative electrode active material in the negative electrode active material layer is typically 80 to 99.5 mass%.

[0384] [2-2-2-2. Electrode Density]

[0385] The negative electrode active material layer obtained by coating and drying the negative electrode active material together with a binder, a thickener, etc., is preferably compacted by a hand press, a roller press, etc., in order to increase the packing density of the negative electrode active material.

[0386] Although the electrode structure when the negative electrode active material is electroded is not particularly limited, the density of the negative electrode active material layer existing on the current collector is typically 1 to 2.2 g / cm³ 3 am.

[0387] [2-2-2-3. Binding Agent]

[0388] As for the binder, any material that is stable with respect to the electrolyte or the liquid medium used in the manufacture of the electrode is sufficient and is not particularly limited.

[0389] Specific examples include rubbery polymers such as styrene-butadiene rubber (SBR), isoprene rubber, butadiene rubber, fluororubber, acrylonitrile-butadiene rubber (NBR), and ethylene-propylene rubber, as well as fluorinated polymers such as polyvinylidene fluoride, polytetrafluoroethylene, fluorinated polyvinylidene fluoride, and tetrafluoroethylene-ethylene copolymer. These can be used individually or in combination of two or more types in any proportion.

[0390] The content of the binder in the negative electrode active material layer is typically 0.1 to 20 mass%. In particular, when the binder contains a rubbery polymer, such as SBR, as a main component, the content of the binder in the negative electrode active material layer is typically 0.1 to 5 mass%.

[0391] In addition, when the binder contains a fluorine-based polymer, such as polyvinylidene fluoride, as a main component, the content of the binder in the negative electrode active material layer is typically 1 to 15 mass%.

[0392] [2-2-2-4. Thickeners]

[0393] Thickeners are typically used to adjust the viscosity of a slurry.

[0394] As for thickeners, there are no particular limitations, but specifically, examples include carboxymethylcellulose and its salts, methylcellulose, hydroxymethylcellulose, ethylcellulose, polyvinyl alcohol, etc. These may be used individually or in combination of two or more types in any proportion.

[0395] When a thickener is used, the content of the thickener in the negative electrode active material layer is typically 0.01 to 5 mass%.

[0396] [2-2-2-5. Entire House]

[0397] As a current collector holding the negative electrode active material, any known material may be used. As a current collector for the negative electrode, metal materials such as aluminum, copper, nickel, stainless steel, and nickel-plated steel may be used, but copper is particularly preferred from the perspective of ease of processing and cost.

[0398] Examples of shapes for the current collector of the negative electrode include metal foil, metal cylinder, metal coil, metal plate, metal thin film, expanded metal, punched metal, foamed metal, etc. Among these, metal foil or metal thin film is preferred. In addition, the metal thin film may be formed into a mesh shape as appropriate.

[0399] When the shape of the current collector of the negative electrode is plate-like or film-like, the thickness of the current collector is arbitrary, but is typically 1 μm to 1 mm.

[0400] [2-2-2-6. Thickness of the negative electrode plate]

[0401] The thickness of the negative electrode (negative electrode plate) is designed to match the positive electrode (positive electrode plate) used and is not specifically limited, but the thickness of the negative electrode active material layer, which is the thickness of the negative electrode material minus the thickness of the current collector, is typically 15 to 1300 μm.

[0402] [2-2-2-7. Surface Coating of the Negative Plate]

[0403] The negative electrode plate may be used with a surface-attached material having a composition different from that of the negative electrode active material. Examples of surface-attached materials include oxides such as aluminum oxide, sulfates such as lithium sulfate, and carbonates such as lithium carbonate.

[0404] [2-3. Separator]

[0405] A separator is typically interposed between the positive and negative electrodes to prevent short circuits. In this case, the electrolyte is usually impregnated into this separator for use.

[0406] The material or shape of the separator is not particularly limited, and known materials may be adopted at will as long as they do not impede the effects of the present invention.

[0407] [2-4. Battery Design]

[0408] [2-4-1. Electrode Group]

[0409] The electrode group may be either a laminated structure in which the positive electrode plate and the negative electrode plate are formed with the separator interposed, or a structure in which the positive electrode plate and the negative electrode plate are wound in a vortex shape with the separator interposed.

[0410] The proportion of the electrode group volume in the battery volume (electrode group share) is typically 40 to 90 percent.

[0411] [2-4-2. Household Structure]

[0412] In the case where the electrode group has the aforementioned laminated structure, a structure formed by gathering the metal core portions of each electrode layer into one and welding them to a terminal is preferably used. A structure that reduces resistance by forming multiple terminals within the electrode is also suitably used. In the case where the electrode group has the aforementioned wound structure, the internal resistance can be lowered by forming multiple lead structures on the positive and negative electrodes, respectively, and gathering them into a single terminal.

[0413] [2-4-3. Protection Elements]

[0414] As a protection element, a PTC (Positive Temperature Coefficient) element, which increases resistance along with heat generation due to overcurrent, etc., a temperature fuse, a thermistor, and a valve (current cutoff valve) that cuts off the current flowing through the circuit due to a rapid rise in internal pressure or internal temperature of the battery in the event of abnormal heat generation can be used.

[0415] It is preferable to select the above-mentioned protection element that does not operate under normal high-current usage, and it is even more preferable to design it so that abnormal heating or thermal runaway does not occur even without the protection element.

[0416] [2-4-4. Exterior Body]

[0417] The battery is typically configured by housing the electrolyte, negative electrode, positive electrode, separator, etc., related to the present embodiment within an outer body (outer case). There are no limitations on this outer body, and any known one may be adopted as long as it does not impede the effects of the present invention.

[0418] The material of the outer casing should be a material that is stable with respect to the electrolyte used and is not particularly limited; however, from the perspective of weight reduction and cost, metals such as iron, aluminum, or aluminum alloys, or laminate films are preferably used. In particular, iron is preferred from the perspective of pressure resistance for operating the current cutoff valve.

[0419] Examples of exterior cases using the above metals include those in which the metals are welded together by laser welding, resistance welding, or ultrasonic welding to form a sealed, airtight structure, or those in which the metals are used to form a caulking structure with a resin gasket interposed therein.

[0420] [2-4-5. Shape]

[0421] The shape of the battery's outer casing is also arbitrary and may be any of the following: cylindrical, prismatic, laminated, coin-shaped, large, etc.

[0422] [2-5. Method of manufacturing a battery]

[0423] A method for manufacturing a battery related to the present embodiment includes a process of housing the positive electrode and the negative electrode in the container, and a process of injecting the electrolyte into the container.

[0424] In addition, the electrolyte may be injected into the container containing the positive electrode and / or negative electrode, or the positive electrode and / or negative electrode may be contained in the container into which the electrolyte has been injected.

[0425] [2-6. Uses of Batteries]

[0426] The battery related to the present embodiment can be used for various known applications. Specific examples of applications include, for instance, notebook computers, pen input personal computers, mobile personal computers, e-book players, mobile phones, mobile fax machines, portable copiers, portable printers, portable audio players, small video cameras, headphone stereos, video movies, liquid crystal televisions, hand cleaners, portable CDs, minidiscs, transceivers, electronic notebooks, electronic desktop calculators, memory cards, portable tape recorders, radios, backup power supplies, motors, automobiles, motorcycles, motorized bicycles, bicycles, lighting fixtures, toys, game devices, watches, power tools, strobes, cameras, home backup power supplies, business office backup power supplies, power supplies for load leveling, natural energy storage power supplies, etc.

[0427] In particular, the battery related to the present embodiment is preferably mounted and used in vehicles such as automobiles, motorcycles, motorized bicycles, and bicycles.

[0428] Examples

[0429] The present invention will be described more specifically below by listing examples and comparative examples, but the present invention is not limited to these examples as long as it does not exceed the gist thereof.

[0430] Each compound used in the examples and comparative examples is shown below.

[0431] ·1,2-Bis(difluorophosphanilloxy)ethane (Compound A-2)

[0432] [Chemical Formula 11]

[0433]

[0434] ·4,4'-bi(1,3,2-dioxathiolan)-2,2,2',2'-tetraoxide (compound B)

[0435] [Chemical Formula 12]

[0436]

[0437] ·1,3,2-dioxathiolan-2,2,-dioxide (Compound C)

[0438] [Chemical Formula 13]

[0439]

[0440] <Examples 1–4, Comparative Examples 1–4>

[0441] [Manufacturing of the Straight Pole]

[0442] Lithium-nickel-cobalt-manganese composite oxide (Li) as a positive electrode active material 1.0 Ni 0.8 Co 0.1 Mn 0.190 parts by mass of O2, 7 parts by mass of acetylene black as a conductive material, and 3 parts by mass of polyvinylidene fluoride (PVdF) as a binder were mixed in an N-methylpyrrolidone solvent using a disperser to form a slurry. This was uniformly coated on both sides of a 15 μm thick aluminum foil serving as a current collector, dried, and then pressed to form a positive electrode.

[0443] [Manufacturing of the negative pole]

[0444] To 98 parts by mass of graphite powder, 1 part by mass of an aqueous dispersion of sodium carboxymethylcellulose (concentration of sodium carboxymethylcellulose 1% by mass) as a thickener and 1 part by mass of an aqueous dispersion of styrene-butadiene rubber (concentration of styrene-butadiene rubber 50% by mass) as a binder were added and mixed with a disperser to form a slurry. The obtained slurry was applied to one side of a copper foil with a thickness of 10 μm, which served as a current collector, dried, and then pressed to form a negative electrode.

[0445] [Preparation of Non-Aqueous Electrolytes]

[0446] Reference electrolyte 1 was prepared by dissolving sufficiently dried LiPF6 as an electrolyte in a mixture of ethylene carbonate (EC), ethylmethyl carbonate (EMC), and dimethyl carbonate (DMC) (volume ratio EC:EMC:DMC = 3:4:3) under a dry argon atmosphere at 1.0 mol / L (12.3 mass%, as a concentration in a non-aqueous electrolyte).

[0447] Each compound was added to the standard electrolyte 1 in the amounts listed in Table 1 below, and additionally, vinylene carbonate was added in such a way that the content was 1 part by mass, thereby preparing the non-aqueous electrolytes of Examples 1 to 4 and Comparative Examples 1 to 4. In addition, "content" here refers to the content (mass%) when the total non-aqueous electrolyte is 100 parts by mass. Also, "-" in Table 1 indicates that it was not added.

[0448] [Manufacture of Non-Aqueous Electrolyte Batteries]

[0449] A battery element was manufactured by stacking the above positive electrode, negative electrode, and polyolefin separator in the order of negative electrode, separator, positive electrode, separator, and negative electrode. This battery element was inserted into a pouch made of a laminate film in which both sides of aluminum (thickness 40 μm) were coated with a resin layer, such that the terminals of the positive electrode and negative electrode were installed protrudingly. Then, each non-aqueous electrolyte prepared above was injected into the pouch, and vacuum sealing was performed to manufacture a laminate-type non-aqueous electrolyte battery. The volume of the non-aqueous electrolyte battery was measured by immersing it in a water bath. This non-aqueous electrolyte battery is a secondary battery.

[0450] <Evaluation of Non-Aqueous Electrolyte Batteries>

[0451] [Initial Conditioning]

[0452] In a constant temperature bath at 25°C, a non-aqueous electrolyte battery prepared by the above method was charged at a constant current of 0.05 C (the current value for discharging the rated capacity by the discharge capacity at a 1-hour rate for 1 hour is defined as 1 C. The same applies hereinafter) to 3.7 V, and then discharged at a constant current of 0.2 C to 2.8 V.

[0453] In addition, the non-aqueous electrolyte battery was stabilized by charging at a constant current and constant voltage of 0.2 C to 4.1 V and then storing at a high temperature of 60 ℃ for 24 hours. After that, it was discharged at a constant current of 0.2 C to 2.8 V at 25 ℃, followed by charging at a constant current and constant voltage of 0.2 C to a voltage of 4.25 V and discharging at a constant current of 0.2 C to 2.8 V.

[0454] [High-temperature charging preservation test]

[0455] After initial conditioning, the non-aqueous electrolyte battery was charged with a constant current and constant voltage to 4.25 V at 0.2 C, and then stored at a high temperature of 60 ℃ for 4 weeks. After that, the non-aqueous electrolyte battery was cooled to 25 ℃ and then discharged with a constant current to 2.8 V at 0.2 C.

[0456] [Evaluation of Gas Generation After High-Temperature Charging and Preservation]

[0457] The volume before and after the high-temperature filling storage test was measured by the Archimedes method, and the change in volume was defined as the amount of gas generated after high-temperature filling storage. Table 1 shows the relative amount of gas generated when the amount of gas generated in Comparative Example 1 is set to 100%.

[0458]

[0459] From Table 1, it can be seen that a non-aqueous electrolyte battery having a non-aqueous electrolyte (Examples 1 to 4) containing a compound represented by general formula (1) and a compound represented by formula (2) can suppress the amount of gas generated after high-temperature storage. This can be confirmed by comparing a non-aqueous electrolyte containing only one type of compound represented by general formula (1) and a compound represented by formula (2) (Comparative Examples 1 and 2) and a non-aqueous electrolyte that does not contain any of the above compounds (Comparative Example 4).

[0460] In addition, a non-aqueous electrolyte battery having a non-aqueous electrolyte (Comparative Example 3) in which a compound C, which is different from the compound represented by Formula (2), is mixed with the compound represented by General Formula (1) could not significantly suppress the amount of gas generated. In this regard, it is presumed that the non-aqueous electrolyte of the present invention forms a rapid and robust mixed film on the negative and positive electrodes, and it was found that the effect of significantly suppressing gas generation is a unique effect when containing General Formula (1) and Formula (2) of the present invention.

[0461] Industrial applicability

[0462] The electrolyte related to this embodiment can suppress gas after high-temperature charging and storage of the battery by using it in a battery. Therefore, the battery of the present invention can be suitably utilized in all fields, such as electronic devices where conventional batteries are used.

[0463] In addition, the battery related to the present embodiment can be used for various known applications. Specific examples of applications include, for instance, notebook computers, pen input personal computers, mobile personal computers, e-book players, mobile phones, mobile fax machines, portable copiers, portable printers, portable audio players, small video cameras, headphone stereos, video movies, liquid crystal televisions, hand cleaners, portable CDs, minidiscs, transceivers, electronic notebooks, electronic desktop calculators, memory cards, portable tape recorders, radios, backup power supplies, motors, automobiles, motorcycles, motorized bicycles, bicycles, lighting fixtures, toys, game devices, watches, power tools, strobes, cameras, home backup power supplies, business office backup power supplies, power supplies for load leveling, natural energy storage power supplies, etc.

Claims

Claim 1 An electrolyte comprising a compound represented by the following general formula (1), a compound represented by the following formula (2), an electrolyte, and a non-aqueous solvent. (L represents a straight-chain or branched alkylene group having 1 to 6 carbon atoms.) Claim 2 An electrolyte according to claim 1, wherein the content of the compound represented by the general formula (1) in the electrolyte is 0.001 to 10 mass%. Claim 3 An electrolyte according to claim 1, wherein the content of the compound represented by formula (2) in the electrolyte is 0.001 to 8.0 mass%. Claim 4 An electrolyte according to claim 1, wherein the mass ratio [(1):(2)] of the compound represented by the general formula (1) and the compound represented by the formula (2) in the electrolyte is 94:6 to 3:

97. Claim 5 The electrolyte according to claim 1, further comprising at least one carbonate compound selected from vinylene carbonate and fluoroethylene carbonate. Claim 6 In claim 5, the electrolyte in which the carbonate compound is vinylene carbonate. Claim 7 In claim 5, the electrolyte having a total content of the vinylene carbonate and the fluoroethylene carbonate in the electrolyte of 0.001 to 10 mass%. Claim 8 In claim 5, the electrolyte is such that the mass ratio of the total content of the vinylene carbonate and the fluoroethylene carbonate to the content of the compound represented by general formula (1) in the electrolyte (total of vinylene carbonate and fluoroethylene carbonate [g] / compound represented by general formula (1) [g]) is 0.01 to 100. Claim 9 In claim 1, the electrolyte in which L in the above general formula (1) is ethylene. Claim 10 An electrolyte comprising at least one anion-containing compound selected from the group consisting of an anion-containing compound having P=O bonds and PF bonds, an anion-containing compound having S=O bonds and SX bonds, wherein X means a heteroatom, and an oxalate anion-containing compound. Claim 11 An electrolyte according to claim 10, wherein the anion-containing compound is at least one selected from a compound containing a difluorophosphate anion, a compound containing a fluorosulfonic acid anion, a compound containing a fluorosulfonylimide anion, a compound containing an alkylsulfate anion, a compound containing a bis(oxalate)borate anion, a compound containing a difluorooxalate borate anion, and a compound containing a difluorobis(oxalate)phosphate anion. Claim 12 A method for preparing an electrolyte, comprising a process of dissolving a compound represented by the following general formula (1), a compound represented by the following formula (2), and an electrolyte in a non-aqueous solvent. (L represents a straight-chain or branched alkylene group having 1 to 6 carbon atoms.) Claim 13 A battery comprising a positive electrode, a negative electrode, and an electrolyte described in any one of claims 1 to 11. Claim 14 A battery according to claim 13, wherein the positive electrode comprises a lithium transition metal-based compound. Claim 15 A method for manufacturing a battery, comprising a process of housing a positive electrode and a negative electrode in a container, and a process of injecting an electrolyte described in any one of claims 1 to 11 into the container. Claim 16 A vehicle equipped with the battery described in Clause 13.