Electrolyte for rechargeable lithium battery and rechargeable lithium battery including the same

The electrolyte with imide cesium salt and crown ether compounds forms a stable SEI film, addressing the lithium dendrite issue in lithium secondary batteries, enhancing rapid charging performance and maintaining lifespan.

KR103047644B1Active Publication Date: 2026-11-11SAMSUNG SDI CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
KR1020230073471
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-06-08
Publication Date
2026-11-11
Estimated Expiration
2043-06-08

AI Technical Summary

Technical Problem

Lithium secondary batteries experience deteriorated lifespan characteristics during rapid charging due to the precipitation of lithium dendrites on the negative electrode surface.

Method used

An electrolyte comprising a non-aqueous organic solvent, a lithium salt, and an additive composed of an imide cesium salt compound and a crown ether compound is used, which forms a stable Solid Electrolyte Interface (SEI) film on the cathode, improving rapid charging performance and maintaining lifespan characteristics.

Benefits of technology

The combination of the imide cesium salt and crown ether compounds enhances rapid charging capabilities while ensuring the battery's lifespan by suppressing side reactions between lithium ions and the electrolyte, even under rapid charging conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023062993963-PAT00023_ABST
    Figure 112023062993963-PAT00023_ABST
Patent Text Reader

Abstract

The present invention provides an electrolyte for a lithium secondary battery comprising a non-aqueous organic solvent, a lithium salt, and an additive, wherein the additive is a composition comprising a first compound and a second compound, the first compound is an imide cesium salt compound represented by Formula 1, and the second compound is a crown ether compound represented by Formula 2, and a lithium secondary battery comprising the same. Details regarding Formulas 1 and 2 are as described in the specification.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to an electrolyte for a lithium secondary battery and a lithium secondary battery containing the same. Background Technology

[0002] Lithium secondary batteries are rechargeable and have an energy density more than three times higher per unit weight than conventional lead-acid batteries, nickel-cadmium batteries, nickel-hydrogen batteries, and nickel-zinc batteries, and can be fast-charged. As a result, they are being commercialized for laptops, mobile phones, power tools, and electric bicycles, and research and development to further improve energy density is actively underway.

[0003] These lithium secondary batteries are used by injecting an electrolyte into a battery cell comprising a positive electrode containing a positive electrode active material capable of intercalating and deintercalating lithium, and a negative electrode containing a negative electrode active material capable of intercalating and deintercalating lithium.

[0004] One of the recent development directions for lithium secondary batteries is rapid charging. However, when lithium secondary batteries are rapidly charged, lithium dendrites are precipitated on the surface of the negative electrode, and there is a problem in that the lifespan characteristics of the lithium secondary battery deteriorate due to the precipitates on the surface of the negative electrode. The problem to be solved

[0006] One embodiment provides an electrolyte for a lithium secondary battery that improves rapid charging performance while also enhancing lifespan characteristics even during rapid charging.

[0007] Another embodiment provides a lithium secondary battery with improved lifespan characteristics even during rapid charging by applying the above-mentioned electrolyte. means of solving the problem

[0009] The present invention provides an electrolyte for a lithium secondary battery comprising a non-aqueous organic solvent, a lithium salt, and an additive, wherein the additive is a composition comprising a first compound and a second compound, the first compound is an imide cesium salt compound represented by the following chemical formula 1, and the second compound is a crown ether compound represented by the following chemical formula 2, and a lithium secondary battery comprising the same:

[0010] [Chemical Formula 1]

[0011]

[0012] [Chemical Formula 2]

[0013] . Effects of the invention

[0015] One embodiment combines compound 1, which improves the rapid charging characteristics of a lithium secondary battery, and compound 2, which increases the solubility of compound 1, in a specific weight ratio, thereby improving the rapid charging performance of the lithium secondary battery while ensuring lifespan characteristics even during rapid charging. Brief explanation of the drawing

[0017] FIG. 1 is a schematic diagram illustrating a lithium secondary battery according to one embodiment of the present invention. Specific details for implementing the invention

[0018] Hereinafter, a lithium secondary battery according to one embodiment of the present invention will be described in detail with reference to the attached drawings. However, this is presented as an example and the present invention is not limited thereby, and the present invention is defined only by the scope of the claims set forth below.

[0019] In this specification, "substitution" means that, unless otherwise defined, at least one hydrogen of a substituent or compound is substituted with a deuterium, a halogen group, a hydroxyl group, an amino group, a substituted or unsubstituted C1 to C30 amine group, a nitro group, a substituted or unsubstituted C1 to C40 silyl group, a C1 to C30 alkyl group, a C1 to C10 alkylsilyl group, a C6 to C30 arylsilyl group, a C3 to C30 cycloalkyl group, a C3 to C30 heterocycloalkyl group, a C6 to C30 aryl group, a C2 to C30 heteroaryl group, a C1 to C20 alkoxy group, a C1 to C10 fluoroalkyl group, a cyano group, or a combination thereof.

[0020] In one example of the present invention, "substitution" means that at least one hydrogen in a substituent or compound is substituted with deuterium, a halogen group, a C1 to C30 alkyl group, a C1 to C10 alkylsilyl group, a C6 to C30 arylsilyl group, a C3 to C30 cycloalkyl group, a C3 to C30 heterocycloalkyl group, a C6 to C30 aryl group, a C2 to C30 heteroaryl group, a C1 to C10 fluoroalkyl group, or a cyano group. Furthermore, in a specific example of the present invention, "substitution" means that at least one hydrogen in a substituent or compound is substituted with deuterium, a halogen group, a C1 to C20 alkyl group, a C6 to C30 aryl group, a C1 to C10 fluoroalkyl group, or a cyano group. In addition, in a specific example of the present invention, "substitution" means that at least one hydrogen in the substituent or compound is substituted with deuterium, a halogen group, a C1 to C5 alkyl group, a C6 to C18 aryl group, a C1 to C5 fluoroalkyl group, or a cyano group. In addition, in a specific example of the present invention, "substitution" means that at least one hydrogen in the substituent or compound is substituted with deuterium, a cyano group, a halogen group, a methyl group, an ethyl group, a propyl group, a butyl group, a phenyl group, a biphenyl group, a terphenyl group, a trifluoromethyl group, or a naphthyl group.

[0021] Lithium secondary batteries can be classified into lithium-ion batteries, lithium-ion polymer batteries, and lithium polymer batteries depending on the type of separator and electrolyte used; classified into cylindrical, prismatic, coin, and pouch types depending on their shape; and divided into bulk and thin-film types depending on their size. Since the structures and manufacturing methods of these batteries are widely known in this field, a detailed description is omitted.

[0022] Here, a cylindrical lithium secondary battery is described as an example of a lithium secondary battery. FIG. 1 schematically shows the structure of a lithium secondary battery according to one embodiment. Referring to FIG. 1, a lithium secondary battery (100) according to one embodiment includes a battery cell comprising a positive electrode (114), a negative electrode (112) positioned opposite to the positive electrode (114), a separator (113) disposed between the positive electrode (114) and the negative electrode (112), and an electrolyte (not shown) impregnating the positive electrode (114), the negative electrode (112), and the separator (113); a battery container (120) containing the battery cell; and a sealing member (140) sealing the battery container (120).

[0024] Below, a more detailed configuration of a lithium secondary battery (100) according to one embodiment of the present invention will be described.

[0025] A lithium secondary battery according to one embodiment of the present invention comprises an electrolyte, a positive electrode, and a negative electrode.

[0026] The above electrolyte comprises a non-aqueous organic solvent, a lithium salt, and an additive, wherein the additive is a composition comprising a first compound and a second compound, the first compound is an imide cesium salt compound represented by the following chemical formula 1, and the second compound is a crown ether compound represented by the following chemical formula 2.

[0027] [Chemical Formula 1]

[0028]

[0029] In the above chemical formula 1, R 1 and R 2 Each is a fluoro group, or a C1 to C3 fluoroalkyl group substituted with at least one fluoro group; and R 1 and R 2 At least one of them is a fluorogroup;

[0030] [Chemical Formula 2]

[0031]

[0032] In the above chemical formula 2, Z is O or NH; x and y are each independently integers of 0 or 1; and m and n are each independently integers of 1 to 3.

[0034] The first compound above is an imide cesium salt compound represented by the chemical formula 1 above, and by being reduced and decomposed before the carbonate-based solvent contained in the non-aqueous organic solvent to form a SEI film (Solid Electrolyte Interface) on the cathode, it prevents the decomposition of the electrolyte and the resulting decomposition reaction of the electrode, thereby particularly improving rapid charging performance.

[0035] However, since the above-mentioned first compound is in the form of a salt, its solubility decreases rapidly when the concentration in the electrolyte exceeds a certain level, which may slightly reduce the aforementioned effect of improving high-temperature characteristics.

[0037] The second compound is a crown ether compound represented by the chemical formula 2 above, and the combined use of the second compound contributes to improving the solubility of the first compound, thereby activating a mechanism in which the first compound is reduced and decomposed to form an SEI film on the cathode, and accordingly, life characteristics can be secured even during rapid charging of the lithium secondary battery.

[0039] However, the above composition comprises the first compound and the second compound in a weight ratio of 1:4 to 1:10.

[0040] Specifically, when the second compound is included in a small amount below the above range, the first compound is not dissolved, and when the second compound is included in an excess amount above the above range, the first compound is included in a small amount rather than being rapidly charged.

[0041] In one embodiment, the composition may include the first compound and the second compound in a weight ratio of 1:4 to 1:10, 1:4 to 1:9, or 1:4 to 1:8. Only within this range can the degree of improvement in rapid charging characteristics due to the synergistic effect of the first compound and the second compound be maximized.

[0043] In summary, by combining compound 1, which improves the rapid charging characteristics of a lithium secondary battery, and compound 2, which increases the solubility of compound 1, in a specific weight ratio, a more stable negative electrode SEI can be formed. Accordingly, side reactions between lithium ions intercalated in the negative electrode and the electrolyte can be effectively suppressed even under rapid charging conditions, thereby improving the rapid charging performance of the lithium secondary battery while ensuring lifespan characteristics even during rapid charging.

[0044] The above electrolyte for a lithium secondary battery is described in more detail below.

[0046] In the imide cesium salt compound represented by the above chemical formula 1 (hereinafter referred to as the "first compound"), the effect of improving rapid charging characteristics can be significantly improved by forming a stable SEI film with a fluoro group directly connected to a sulfone.

[0047] Specifically, the above R 1 can be a fluorogroup; and the above R 2 It may be a fluoro group, a C1 fluoroalkyl group substituted with three fluoro groups, a C2 fluoroalkyl group substituted with five fluoro groups, or a C3 fluoroalkyl group substituted with seven fluoroalkyl groups.

[0048] Representative examples of the above-mentioned first compound are as follows:

[0049] [Chemical Formula 1-1]

[0050]

[0051] [Chemical Formula 1-2]

[0052]

[0053] [Chemical Formula 1-3]

[0054]

[0055] [Chemical Formula 1-4]

[0056] .

[0057] Among the compounds exemplified above, cesium bis(fluorosulfonyl)imide (CsFSI: Cs + (FSO2)2N - In the case of ), since fluoro groups directly connected to sulfone are present on both sides, the effect of improving rapid charging characteristics can be expressed more effectively.

[0059] Meanwhile, the second compound acts as a cation receptor for the first compound, contributing to the improvement of solubility.

[0060] In this regard, the solubility of the first compound can be more effectively improved when the second compound has a structure containing at least five ether groups. If the second compound contains fewer than five ether groups, the solubility of the first compound cannot be effectively improved, and accordingly, it may be difficult to expect an improved rapid charging effect.

[0061] Specifically, the second compound may be a crown ether compound represented by any one of the following chemical formulas 2-1 to 2-3:

[0062] [Chemical Formula 2-1]

[0063]

[0064] [Chemical Formula 2-2]

[0065]

[0066] [Chemical Formula 2-3]

[0067]

[0068] In the above chemical formulas 2-1 to 2-3, m and n are each independently one of integers 1 to 3.

[0069] More specifically, the second compound may be at least one selected from 15-crown-5, 18-crown-6, 21-crown-7, 24-crown-8, dibenzo-15-crown-5, dibenzo-18-crown-6, dibenzo-21-crown-7, dibenzo-24-crown-8, 1-aza-15-crown-5, 1-aza-18-crown-6, 1-aza-21-crown-7, and 1-aza-24-crown-8.

[0070] Among the compounds exemplified above, in the case of 18-crown-6 in which m and n of the chemical formula 2-1 are 1 and 2, respectively, the size of the crown is suitable for trapping the cation of the first compound, so the first compound can be dissolved more effectively.

[0072] Meanwhile, the first compound may be included in an amount of 0.1 to 2.0 weight% with respect to 100 weight% of the total electrolyte for a lithium secondary battery, for example, 0.5 to 2.0 weight%, 0.5 to 1.5 weight%, or 0.7 to 2.0 weight%, or 0.7 to 1.0 weight%.

[0073] In addition, the second compound may be included in an amount of less than 0.1 to 10 weight% with respect to 100 weight% of the total electrolyte for a lithium secondary battery, for example, 0.1 to 8.0 weight%, 0.5 to 8.0 weight%, 1.0 to 8.0 weight%, 2.8 to 8 weight%, or 4.0 to 8.0 weight%.

[0074] The composition comprising the first compound and the second compound may be included in an amount of less than 0.5 to 10 weight% with respect to 100 weight% of the total electrolyte for a lithium secondary battery, for example, less than 1.0 to 10 weight%, less than 2.0 to 10 weight%, or less than 2.5 to 10 weight%.

[0075] In a more specific embodiment, the composition comprises the first compound and the second compound in a weight ratio of 1:4 to 1:10, wherein within the above range, the first compound is included in an amount of 0.7 to 2.0 weight% with respect to 100 weight% of the total electrolyte for a lithium secondary battery, and the second compound is included in an amount of 2.8 to 8 weight% with respect to 100 weight% of the total electrolyte for a lithium secondary battery.

[0076] In a more specific embodiment, the composition comprises the first compound and the second compound in a weight ratio of 1:4 to 1:18, wherein within the above range, the first compound is included in an amount of 0.7 to 1.0 weight% with respect to 100 weight% of the total electrolyte for a lithium secondary battery, and the second compound is included in an amount of 4 to 8 weight% with respect to 100 weight% of the total electrolyte for a lithium secondary battery.

[0077] When the content of the composition and the content of each component within the composition are within the above range, a lithium secondary battery with improved resistance characteristics during high-temperature storage can be realized.

[0079] The above lithium salt is a material that dissolves in a non-aqueous organic solvent and acts as a source of lithium ions within the battery, enabling the operation of a basic lithium secondary battery and facilitating the movement of lithium ions between the anode and cathode. Representative examples of such lithium salts include LiPF6, LiBF4, LiDFOP, LiDFOB, LiPO2F2, LiSbF6, LiAsF6, LiN(SO2C2F5)2, Li(CF3SO2)2N, LiN(SO3C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide (LiFSI), LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiN(C p F 2p+1 SO2)(C q F 2q+1 One or more selected from the group consisting of SO2)(where p and q are each independently integers from 1 to 20), LiCl, LiI, and LiB(C2O4)2 (lithium bis(oxalato) borate: LiBOB). It is preferable to use a lithium salt concentration within the range of 0.1 M to 2.0 M. When the lithium salt concentration falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and lithium ions can move effectively.

[0081] The above-mentioned non-aqueous organic solvent serves as a medium through which ions involved in the electrochemical reaction of the battery can move.

[0082] The above-mentioned non-aqueous organic solvent may be a carbonate-based, ester-based, ether-based, ketone-based, alcohol-based, or aprotic solvent.

[0083] The above carbonate-based solvents may include ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. The above ester-based solvents may include methyl acetate, ethyl acetate, n-propyl acetate, t-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, decanolide, mevalonolactone, caprolactone, etc. The above ether-based solvent may include dibutyl ether, tetraglame, diglame, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, etc. Additionally, the above ketone-based solvent may include cyclohexanone, etc. Additionally, the above alcohol-based solvent may include ethyl alcohol, isopropyl alcohol, etc., and the above aprotic solvent may include nitriles such as R-CN (where R is a straight-chain, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms and may include a double bond, a directional ring, or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, sulfolanes, etc.

[0084] The above-mentioned non-aqueous organic solvents may be used alone or in a mixture of one or more. When used in a mixture of one or more, the mixing ratio can be appropriately adjusted according to the desired battery performance, which is widely understood by those working in the field.

[0085] In addition, for the above carbonate-based solvent, it is preferable to use a mixture of cyclic carbonates and chain carbonates. In this case, using a mixture of cyclic carbonates and chain carbonates in a volume ratio of 5:95 to 50:50 can result in excellent performance of the electrolyte.

[0086] Specifically, ethylene carbonate (EC) and propylene carbonate (PC) may be used as the cyclic carbonates, and propyl propionate (PP) may be used as the linear carbonates.

[0087] More specifically, the above-mentioned non-aqueous organic solvent may include a carbonate-based solvent mixed with ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC). For example, the performance of the electrolyte may be excellent when the above-mentioned carbonate-based solvent mixed with ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) is mixed and used in a volume ratio of EC:EMC:DMC = 1:0.5:5 to 5:3:10.

[0088] The above-mentioned non-aqueous organic solvent may further include an aromatic hydrocarbon organic solvent in addition to the carbonate-based solvent. In this case, the carbonate-based solvent and the aromatic hydrocarbon solvent may be mixed in a volume ratio of 1:1 to 30:1.

[0089] As the above aromatic hydrocarbon solvent, an aromatic hydrocarbon compound of the following chemical formula 3 may be used.

[0090] [Chemical Formula 3]

[0091]

[0092] In the above chemical formula 3, R 201 to R 206 The groups are identical or different and are selected from the group consisting of hydrogen, halogen, alkyl groups having 1 to 10 carbon atoms, haloalkyl groups, and combinations thereof.

[0093] Specific examples of the above aromatic hydrocarbon solvents include benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, fluorotoluene, 2,3-difluorotoluene, 2,4-difluorotoluene. It is selected from the group consisting of 2,5-difluorotoluene, 2,3,4-trifluorotoluene, 2,3,5-trifluorotoluene, chlorotoluene, 2,3-dichlorotoluene, 2,4-dichlorotoluene, 2,5-dichlorotoluene, 2,3,4-trichlorotoluene, 2,3,5-trichlorotoluene, iodotoluene, 2,3-diiodotoluene, 2,4-diiodotoluene, 2,5-diiodotoluene, 2,3,4-triiodotoluene, 2,3,5-triiodotoluene, xylene, and combinations thereof.

[0094] The above electrolyte may further include vinylene carbonate, vinyl ethylene carbonate, or an ethylene-based carbonate compound of the following chemical formula 4 as a life-enhancing additive to improve battery life.

[0095] [Chemical Formula 4]

[0096]

[0097] In the above chemical formula 4, R 207 and R 208 The groups are identical or different from each other and are selected from the group consisting of hydrogen, halogen groups, cyano groups (CN), nitro groups (NO2), and fluorinated alkyl groups having 1 to 5 carbon atoms, and the R 207 and R 208At least one of the groups is selected from the group consisting of a halogen group, a cyano group (CN), a nitro group (NO2), and a fluorinated alkyl group having 1 to 5 carbon atoms, provided that R 207 and R 208 Not all of it is hydrogen.

[0098] Representative examples of the above-mentioned ethylene-based carbonate compounds include difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, or fluoroethylene carbonate. When using more of these lifespan-enhancing additives, the amount used can be appropriately controlled.

[0100] Another embodiment of the present invention provides a lithium secondary battery comprising: a positive electrode comprising a positive active material; a negative electrode comprising a negative active material; and the aforementioned electrolyte.

[0101] The above positive electrode comprises a positive current collector and a positive active material layer located on the positive current collector, and the positive active material layer comprises a positive active material.

[0102] As the above-mentioned positive electrode active material, a compound capable of reversible intercalation and deintercalation of lithium (a lithated intercalation compound) may be used.

[0103] Specifically, at least one type of composite oxide of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof may be used.

[0104] Of course, a coating layer on the surface of the above-mentioned composite oxide may be used, or a mixture of the above-mentioned composite oxide and the composite oxide having a coating layer may be used. This coating layer may include at least one coating element compound selected from the group consisting of oxides of coating elements, hydroxides of coating elements, oxyhydroxides of coating elements, oxycarbonates of coating elements, and hydroxycarbonates of coating elements. The compounds forming these coating layers may be amorphous or crystalline. As coating elements included in the above-mentioned coating layer, Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or mixtures thereof may be used. For the coating layer formation process, any coating method may be used as long as the compound can be coated using these elements in a way that does not adversely affect the physical properties of the cathode active material (e.g., spray coating, immersion method, etc.). Since this is a matter that is well understood by those engaged in the relevant field, a detailed explanation will be omitted.

[0105] Specifically, the positive electrode active material may include lithium cobalt oxide.

[0106] The above lithium cobalt oxide has low wettability compared to other cathode active materials and may impair the high-temperature storage characteristics of a lithium secondary battery containing it. However, in one embodiment, by combining the electrolyte additive and the cathode conductive material, even when using lithium cobalt oxide as the cathode active material, the increase in initial resistance and resistance during high-temperature storage can be more effectively suppressed while improving the high-temperature storage characteristics of the lithium secondary battery.

[0107] More specifically, the positive electrode active material may include lithium cobalt oxide represented by the following chemical formula 2:

[0108] [Chemical Formula 2]

[0109] Li a11Co x11 M 11 y11 O2

[0110] In the above chemical formula 2, 0.9≤a11≤1.8, 0.9≤x11≤1, 0≤y11≤0.1, x11+y11=1, and M 11 It is selected from Al, B, Ce, Cr, F, Mg, Mn, Mo, Nb, P, S, Si, Sr, Ti, V, W, Zr and combinations thereof.

[0111] For example, the above positive active material may be LiCoO2.

[0113] In the positive electrode of one embodiment, the content of the positive electrode active material may be 50% to 99% by weight, 60% to 99% by weight, 70% to 99% by weight, 80% to 99% by weight, or 90% to 99% by weight based on the total weight of the positive electrode active material layer.

[0114] In one embodiment of the present invention, the positive active material layer may optionally include a conductive material and a binder. In this case, the content of the conductive material and the binder may each be 1.0 weight% to 5.0 weight% with respect to the total weight of the positive active material layer.

[0115] The above conductive material is used to impart conductivity to the positive electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed. Examples include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, and carbon fibers; metal-based materials such as metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; or conductive materials including mixtures thereof.

[0116] The above binder serves to adhere the positive active material particles well to each other and also to adhere the positive active material well to the current collector. Representative examples include polyvinyl alcohol, carboxymethylcellulose, hydroxypropylcellulose, diacetylcellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc., but are not limited thereto.

[0118] Al may be used as the anode current collector, but is not limited thereto.

[0120] The above cathode includes a cathode active material layer comprising a cathode current collector and a cathode active material formed on the cathode current collector.

[0121] The above-mentioned negative electrode active material includes a material capable of reversibly intercalating / deintercalating lithium ions, lithium metal, an alloy of lithium metal, a material capable of doping and dedoping lithium, or a transition metal oxide.

[0122] As a material capable of reversibly intercalating / deintercalating the above lithium ions, any carbon-based negative electrode active material commonly used in lithium secondary batteries can be used, and representative examples include crystalline carbon, amorphous carbon, or a combination thereof. Examples of the above crystalline carbon include graphite such as amorphous, plate-like, flake-like, spherical, or fibrous natural graphite or artificial graphite, and examples of the above amorphous carbon include soft carbon or hard carbon, mesophase pitch carbide, calcined coke, etc.

[0123] As the above lithium metal alloy, an alloy of a metal selected from the group consisting of lithium, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn may be used.

[0124] Materials capable of doping and undoping the above lithium include Si, Si-C composites, SiOx (0 < x < 2), Si-Q alloys (wherein Q is an element selected from the group consisting of alkali metals, alkaline earth metals, group 13 elements, group 14 elements, group 15 elements, group 16 elements, transition metals, rare earth elements, and combinations thereof, and is not Si), Sn, SnO2, Sn-R (wherein R is an element selected from the group consisting of alkali metals, alkaline earth metals, group 13 elements, group 14 elements, group 15 elements, group 16 elements, transition metals, rare earth elements, and combinations thereof, and is not Sn), and at least one of these may also be mixed with SiO2.

[0125] The above elements Q and R may be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.

[0126] Examples of the above transition metal oxides include vanadium oxide, lithium vanadium oxide, or lithium titanium oxide.

[0127] In one embodiment, the negative electrode active material may include at least one of graphite and Si composites.

[0128] The above Si composite comprises a core containing Si particles and amorphous carbon, for example, the Si particles are a Si-C composite, SiO x It may include one or more of (0 < x ≤ 2) and Si alloys.

[0129] For example, the above Si-C composite may include a core containing Si particles and amorphous carbon.

[0130] The core may include a void in the center, and the radius of the center may correspond to 30% to 50% of the radius of the Si-C composite.

[0131] The average particle size of the above Si particles may be 10 nm to 200 nm.

[0132] In this specification, the average particle size may be the particle size (D50) at 50% by volume ratio in the cumulative size-distribution curve.

[0133] If the average particle size of the above Si particles falls within the above range, volume expansion occurring during charging and discharging can be suppressed, and the disruption of the conductive path due to particle fragmentation during charging and discharging can be prevented.

[0134] The above Si particles may be included in an amount of 1 to 60 weight% with respect to the total weight of the Si-C composite, for example, 3 It may be included in an amount of up to 60 weight%.

[0135] The above central part does not contain amorphous carbon, and amorphous carbon may exist only on the surface of the negative electrode active material.

[0136] In this case, the surface region refers to the area from the center to the outermost surface of the cathode active material.

[0137] In addition, Si particles are incorporated substantially uniformly throughout the cathode active material, that is, they can exist at a substantially uniform concentration in the center and on the surface.

[0138] The above amorphous carbon may be soft carbon, hard carbon, mesophase pitch carbide, calcined coke, or a combination thereof.

[0139] The above-mentioned cathode active material may further include crystalline carbon.

[0140] When the above-mentioned cathode active material includes a Si-C composite and crystalline carbon together, the Si-C composite and crystalline carbon may be included in the form of a mixture, in which case the Si-C composite and crystalline carbon may be included in a weight ratio of 1:99 to 50:50. More specifically, the Si-C composite and crystalline carbon may be included in a weight ratio of 3:97 to 20:80 or a weight ratio of 5:95 to 20:80.

[0141] The above crystalline carbon may be, for example, graphite, and more specifically may include natural graphite, artificial graphite, or a mixture thereof.

[0142] The average particle size of the crystalline carbon above may be 5 μm to 30 μm.

[0143] As the above amorphous carbon precursor, coal-based pitch, mesophase pitch, petroleum-based pitch, coal-based oil, petroleum-based heavy oil, or polymer resins such as phenolic resin, furan resin, and polyimide resin may be used.

[0144] The content of the negative electrode active material in the above negative electrode active material layer may be 95% to 99% by weight with respect to the total weight of the negative electrode active material layer.

[0145] In one embodiment of the present invention, the negative electrode active material layer comprises a binder and may optionally further comprise a conductive material. The content of the binder in the negative electrode active material layer may be 1% to 5% by weight with respect to the total weight of the negative electrode active material layer. Additionally, when further comprising a conductive material, the negative electrode active material may be used in an amount of 90% to 98% by weight, the binder in an amount of 1% to 5% by weight, and the conductive material in an amount of 1% to 5% by weight.

[0146] The above binder serves to effectively bond the negative electrode active material particles to each other and also to effectively bond the negative electrode active material to the current collector. As the binder, a water-insoluble binder, a water-soluble binder, or a combination thereof may be used.

[0147] Examples of the above-mentioned water-insoluble binders include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or combinations thereof.

[0148] Examples of the above water-soluble binders include rubber-based binders or polymer resin binders. The above rubber-based binder may be selected from styrene-butadiene rubber, acrylated styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, and combinations thereof. The above polymer resin binder may be selected from polytetrafluoroethylene, ethylene-propylene copolymer, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polystyrene, ethylene-propylene-diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, and combinations thereof.

[0149] When a water-soluble binder is used as the above-mentioned cathode binder, a cellulose-based compound capable of imparting viscosity may be further included as a thickener. As this cellulose-based compound, one or more types such as carboxymethyl cellulose, hydroxypropylmethyl cellulose, methyl cellulose, or alkali metal salts thereof may be mixed and used. Na, K, or Li may be used as the alkali metal. The content of such a thickener may be 0.1% to 3% by weight relative to 100% by weight of the cathode active material.

[0150] The above conductive material is used to impart conductivity to the electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed. Examples include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, and carbon fibers; metal-based materials such as metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; or conductive materials comprising a mixture thereof.

[0152] The above-mentioned cathode current collector may be selected from the group consisting of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.

[0154] Depending on the type of lithium secondary battery, a separator may be present between the positive and negative electrodes. Such a separator may be a porous substrate; or a composite porous substrate.

[0155] The porous substrate is a substrate containing pores through which lithium ions can move. The porous substrate may be, for example, polyethylene, polypropylene, polyvinylidene fluoride, or a multilayer film of two or more layers thereof, and of course, a mixed multilayer film such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, or a polypropylene / polyethylene / polypropylene three-layer separator may be used.

[0156] The above composite porous substrate may be in the form of a porous substrate and a functional layer located on the porous substrate. From the perspective of enabling the addition of additional functions, the functional layer may be, for example, at least one of a heat-resistant layer and an adhesive layer, and for example, the heat-resistant layer may include a heat-resistant resin and optionally a filler.

[0157] In addition, the adhesive layer may include an adhesive resin and optionally a filler.

[0158] The above filler may be an organic filler or an inorganic filler.

[0159] Referring to FIG. 1, a lithium secondary battery (100) according to one embodiment comprises a battery cell comprising a negative electrode (112), a positive electrode (114) positioned opposite to the negative electrode (112), a separator (113) disposed between the negative electrode (112) and the positive electrode (114), and an electrolyte (not shown) impregnating the negative electrode (112), the positive electrode (114), and the separator (113), a battery container (120) containing the battery cell, and a sealing member (140) sealing the battery container (120).

[0161] Examples and comparative examples of the present invention are described below. The following examples are merely embodiments of the present invention, and the present invention is not limited to the following examples.

[0163] (Preparation of electrolyte)

[0164] Example 1

[0165] In a non-aqueous organic solvent in which ethylene carbonate:propylene carbonate:propyl propionate (EC:PC:PP) is mixed in a volume ratio of 10:15:75, 1.3 M LiPF6 was dissolved, and a composition containing the first compound and the second compound in a weight ratio of 1:4 was added.

[0166] The first compound mentioned above is cesium bis(fluorosulfonyl)imide (CsFSI: Cs + (FSO2)2N - ) was used, and 18-Crown-6 was used as the second compound.

[0167] In addition, the composition containing the first compound and the second compound in a weight ratio of 1:4 was included in an amount of 3.5 weight% relative to 100 weight% of the total electrolyte for a lithium secondary battery.

[0168] (However, in the above electrolyte composition, “weight%” refers to the relative weight of the additive to 100 weight% of the total electrolyte (lithium salt + non-aqueous organic solvent + additive).)

[0169] Example 2

[0170] An electrolyte was prepared in the same manner as in Example 1, except that a composition comprising the first compound and the second compound in a weight ratio of 1:4 was included in an amount of 5% by weight relative to 100% by weight of the total electrolyte for a lithium secondary battery.

[0171] Example 3

[0172] An electrolyte was prepared in the same manner as in Example 1, except that a composition comprising the first compound and the second compound in a weight ratio of 1:4 was included at 10% by weight relative to 100% by weight of the total electrolyte for a lithium secondary battery.

[0173] Example 4

[0174] An electrolyte was prepared in the same manner as in Example 1, except that a composition comprising the first compound and the second compound in a weight ratio of 1:8 was included at 9% by weight relative to 100% by weight of the total electrolyte for a lithium secondary battery.

[0175] Example 5

[0176] An electrolyte was prepared in the same manner as in Example 1, except that a composition comprising the first compound and the second compound in a weight ratio of 1:10 was included at 7.7 weight% with respect to 100 weight% of the total electrolyte for a lithium secondary battery.

[0177] Comparative Example 1

[0178] The electrolyte was prepared in the same manner as in Example 1, except that the first compound and the second compound were not used at all.

[0179] Comparative Example 2

[0180] The electrolyte was prepared in the same manner as in Example 1, except that only the first compound was included at 0.5% by weight relative to 100% by weight of the total electrolyte for a lithium secondary battery.

[0181] Comparative Example 3

[0182] The electrolyte was prepared in the same manner as in Example 1, except that only the first compound was included at 0.7% by weight relative to 100% by weight of the total electrolyte for a lithium secondary battery.

[0183] Comparative Example 4

[0184] The electrolyte was prepared in the same manner as in Example 1, except that only the second compound was included at 5% by weight relative to 100% by weight of the total electrolyte for a lithium secondary battery.

[0185] Comparative Example 5

[0186] The electrolyte was prepared in the same manner as in Example 1, except that only the second compound was included in an amount of 105% by weight relative to 100% by weight of the total electrolyte for a lithium secondary battery.

[0187] Comparative Example 6

[0188] An electrolyte was prepared in the same manner as in Example 1, except that a composition comprising the first compound and the second compound in a weight ratio of 1:2 was included at 2.1 weight% with respect to 100 weight% of the total electrolyte for a lithium secondary battery.

[0189] Comparative Example 7

[0190] An electrolyte was prepared in the same manner as in Example 1, except that a composition comprising the first compound and the second compound in a weight ratio of 1:3 was included at 4% by weight relative to 100% by weight of the total electrolyte for a lithium secondary battery.

[0191] Comparative Example 8

[0192] An electrolyte was prepared in the same manner as in Example 1, except that a composition comprising the first compound and the second compound in a weight ratio of 1:15 was included in an amount of 11.2% by weight relative to 100% by weight of the total electrolyte for a lithium secondary battery.

[0193] Comparative Example 9

[0194] As the first compound above, cesium bis(trifluoromethanesulfonyl)imide (CsTFSI: Cs + (CF3SO2)2N - Except for the use of ), the electrolyte was prepared in the same manner as in Example 1 above.

[0196] For reference, the composition of each additive in the examples and comparative examples is summarized in Table 1 below.

[0198] 1st compound Content of Compound 1 in Electrolyte (Weight%) Content of Compound 2 in Electrolyte (Weight%) Mixing ratio of 1st compound to 2nd compound (w:w) Example 1 CsFSI 0.7 2.8 1:4 Example 2 CsFSI 1 4 1:4 Example 3 CsFSI 2 8 1:4 Example 4 CsFSI 1 8 1:8 Example 5 CsFSI 0.7 7 1:10 Comparative Example 1 CsFSI - - - Comparative Example 2 CsFSI 0.5 - - Comparative Example 3 CsFSI 0.7 - - Comparative Example 4 CsFSI - 5 - Comparative Example 5 CsFSI - 10 - Comparative Example 6 CsFSI 0.7 1.4 1:2 Comparative Example 7 CsFSI 1 3 1:3 Comparative Example 8 CsTFSI 0.7 10.5 1:15

[0199] Evaluation 1: Evaluation of additive dissolution in the electrolyte

[0200] For each electrolyte of Examples 1 to 5 and Comparative Examples 1 to 8, the dissolution of the additive was checked and recorded in Table 2 below.

[0201] Specifically, after adding the first and second compounds to the base electrolyte and stirring for at least one day, the presence of residue was checked. If there was no residue, it was indicated as O (dissolved), and if there was residue, it was indicated as X (not dissolved).

[0202] Whether additives in the electrolyte are dissolved Example 1 O Example 2 O Example 3 O Example 4 O Example 5 O Comparative Example 1 (No additives) Comparative Example 2 O Comparative Example 3 X Comparative Example 4 O Comparative Example 5 X Comparative Example 6 X Comparative Example 7 X Comparative Example 8 X

[0203] According to Table 2 above, in Examples 1 to 5, all additives in the electrolyte are dissolved, but in Comparative Examples 1 to 8, there are cases where additives in the electrolyte are not dissolved.

[0204] Specifically, looking at Comparative Examples 2 to 5, when only one of the above compound 1 and the above compound 2 is used, only a small amount is used to dissolve in the electrolyte.

[0205] Meanwhile, looking at Examples 1 to 5 and Comparative Examples 6 to 8, it can be seen that when the weight ratio of the compound 1 and the compound 2 is controlled within the range of 1:4 to 1:10, the additive dissolves well in the electrolyte.

[0207] Evaluation 2: Evaluation of Room Temperature Rapid Life Characteristics of Lithium Secondary Batteries

[0208] LiCoO2 as the positive active material, polyvinylidene fluoride as the binder, and Ketjen black as the conductive material are mixed in a weight ratio of 97:2:1, respectively. N - A positive electrode active material slurry was prepared by dispersing in methylpyrrolidone.

[0209] The above positive active material slurry was coated onto an Al foil with a thickness of 15 μm, dried at 100°C, and then pressed to produce a positive electrode.

[0210] A mixture of artificial graphite and a Si-C composite mixed in a weight ratio of 93:7 was used as the negative electrode active material, and a negative electrode active material slurry was prepared by mixing the negative electrode active material, a styrene-butadiene rubber binder as a binder, and carboxymethylcellulose as a thickener in a weight ratio of 97:1:2, respectively, and dispersing them in distilled water.

[0211] The above Si-C composite is in the form of a core containing artificial graphite and silicon particles and a coal-based pitch coated on the surface of the core.

[0212] The above cathode active material slurry was coated onto a 10㎛ thick Cu foil, dried at 100℃, and then pressed to manufacture a cathode.

[0213] An electrode assembly was manufactured by assembling the above-manufactured positive and negative electrodes with a polyethylene separator having a thickness of 25 μm, and a lithium secondary battery was manufactured by injecting the electrolytes of Examples 1 to 5 and Comparative Examples 1, 2, and 4.

[0214] For each lithium secondary battery of Examples 1 to 5 and Comparative Examples 1, 2, and 4, room temperature rapid life characteristics were evaluated and listed in Table 3 below.

[0215] Specifically, the capacity retention rate was measured by performing 200 charge-discharge cycles in a 25℃ constant temperature chamber with a charge CC-CV of 3.0C and 4.5V and a 1.0C cut-off, and a discharge CV of 1.0C and 3.0V cut-off.

[0217] Room temperature rapid life characteristics (capacity retention rate @ 200 cy, 2 5℃) Example 1 85 % Example 2 88 % Example 3 91 % Example 4 87 % Example 5 83 % Comparative Example 1 73 % Comparative Example 2 81 % Comparative Example 4 79 %

[0218] According to Table 3 above, the lithium secondary batteries of Examples 1 to 5 can improve the rapid charging performance of the lithium secondary battery and secure lifespan characteristics even during rapid charging by combining Compound 1, which improves the rapid charging characteristics of the lithium secondary battery, and Compound 2, which increases the solubility of Compound 1, in a specific weight ratio.

[0220] Although preferred embodiments of the present invention have been described above, the present invention is not limited thereto and can be implemented with various modifications within the scope of the claims, the detailed description of the invention, and the attached drawings, and it is obvious that such modifications also fall within the scope of the present invention. Explanation of the symbols

[0222] 100: Lithium secondary battery 112: Cathode 113: Separator 114: Bipolar 120: Battery container 140: Encapsulated member

Claims

Claim 1 Electrolyte for a lithium secondary battery comprising a non-aqueous organic solvent, a lithium salt, and an additive, wherein the additive is a composition comprising a first compound and a second compound, wherein the first compound is an imide cesium salt compound represented by the following Chemical Formula 1, and the second compound is a crown ether compound represented by the following Chemical Formula 2-1, and the composition comprises the first compound and the second compound in a weight ratio of 1:4 to 1:10: [Chemical Formula 1] In the above chemical formula 1, R 1 and R 2 Each is a fluoro group, or a C1 to C3 fluoroalkyl group substituted with at least one fluoro group; and R 1 and R 2 At least one of them is a fluorogroup; [Chemical Formula 2-1] In the above chemical formula 2-1, m and n are each independently one of integers from 1 to 3. Claim 2 In paragraph 1, the above R 1 is a fluorogroup; and the above R 2 An electrolyte for a lithium secondary battery, wherein is a fluoro group, a C1 fluoroalkyl group substituted with three fluoro groups, a C2 fluoroalkyl group substituted with five fluoro groups, or a C3 fluoroalkyl group substituted with seven fluoroalkyl groups. Claim 3 In claim 1, the first compound is an electrolyte for a lithium secondary battery represented by any one of the following chemical formulas 1-1 to 1-4: [Chemical Formula 1-1] [Chemical Formula 1-2] [Chemical Formula 1-3] [Chemical Formula 1-4] . Claim 4 delete Claim 5 An electrolyte for a lithium secondary battery according to claim 1, wherein the second compound is at least one selected from 15-Crown-5, 18-Crown-6, 21-Crown-7, and 24-Crown-8. Claim 6 An electrolyte for a lithium secondary battery according to claim 1, wherein the first compound is included in an amount of 0.1 to 2.0 weight% based on 100 weight% of the total electrolyte for a lithium secondary battery. Claim 7 An electrolyte for a lithium secondary battery according to claim 1, wherein the second compound is included in an amount of 0.1 to 10 weight% based on 100 weight% of the total electrolyte for a lithium secondary battery. Claim 8 An electrolyte for a lithium secondary battery according to claim 1, wherein the composition comprising the first compound and the second compound is included in an amount of 0.5 to 10 weight% based on 100 weight% of the total electrolyte for a lithium secondary battery. Claim 9 In claim 1, the non-aqueous organic solvent comprises a carbonate-based, ester-based, ether-based, ketone-based, alcohol-based, or aprotic solvent, for an electrolyte for a lithium secondary battery. Claim 10 In claim 9, the above-mentioned non-aqueous organic solvent is an electrolyte for a lithium secondary battery comprising a carbonate-based solvent and an ester-based solvent. Claim 11 An electrolyte for a lithium secondary battery according to claim 10, comprising ethylene carbonate (EC) and propylene carbonate (PC) as the carbonate-based solvents and propylpropionate (PP) as the ester-based solvent. Claim 12 In claim 1, the lithium salt is LiPF6, LiBF4, LiDFOP, LiDFOB, LiPO2F2, LiSbF6, LiAsF6, LiN(SO2C2F5)2, Li(CF3SO2)2N, LiN(SO3C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide (LiFSI), LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiN(C p F 2p+1 SO2)(C q F 2q+1 Electrolyte for a lithium secondary battery comprising one or more selected from the group consisting of SO2)(where p and q are each independently integers from 1 to 20), LiCl, LiI and LiB(C2O4)2 (lithium bis(oxalato) borate (LiBOB). Claim 13 In claim 12, the lithium secondary battery electrolyte in which the concentration of the lithium salt in the lithium secondary battery electrolyte is 1.0M to 2.0M. Claim 14 A lithium secondary battery comprising: a positive electrode comprising a positive active material; a negative electrode comprising a negative active material; and an electrolyte for a lithium secondary battery according to any one of claims 1 to 3 and claims 5 to 13. Claim 15 In claim 14, the positive electrode active material is a lithium secondary battery represented by the following chemical formula 2: [Chemical Formula 2]Li a11 Co x11 M 11 y11 In the above chemical formula 2, O2, 0.9≤a11≤1.8, 0.9≤x11≤1, 0≤y11≤0.1, x11+y11=1, and M 11 It is selected from Al, B, Ce, Cr, F, Mg, Mn, Mo, Nb, P, S, Si, Sr, Ti, V, W, Zr and combinations thereof. Claim 16 In claim 14, the negative electrode active material comprises at least one of graphite and Si composites, in a lithium secondary battery. Claim 17 In paragraph 16, the above Si composite is a lithium secondary battery comprising a core containing Si particles and amorphous carbon. Claim 18 In paragraph 17, the core containing the above Si particles is a Si-C composite, SiO x A lithium secondary battery comprising one or more of (0 < x ≤ 2) and Si alloys. Claim 19 In claim 18, the above Si-C composite is a lithium secondary battery comprising a core containing Si particles and amorphous carbon as internal components. Claim 20 In paragraph 16, the above negative electrode active material is a lithium secondary battery further comprising crystalline carbon.

Citation Information

Patent Citations

  • Electrolyte for secondary battery

    JP2017117592A

  • Electrolyte agent and lithium secondary battery comprising the same

    KR1020180027996A

  • Lithium ion battery

    US20170365883A1

  • Silicon-based energy storage devices with electrolyte containing crown ether based compounds

    US20210226251A1

  • Electrolyte for rechargeable lithium battery and rechargeable lithium battery including same

    WO2023003133A1