Electrolyte, battery cell and preparation method therefor, battery, and electrical apparatus

By using the combination and additives of low-content vinyl carbonate and specific electrolyte salts in the battery, the electrolyte solution is optimized, and the problem of insufficient battery circulation performance at high temperatures is solved, the high-temperature circulation performance and dynamic performance of the battery is improved, and the battery life is extended .

WO2024243811A1PCT designated stage expired Publication Date: 2024-12-05CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/097179
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The existing batteries have insufficient cycling performance and stability under high temperature conditions, especially the thermal stability and cycling stability of the positive electrode active materials with high nickel content, resulting in an increase in side reactions of the batteries at high temperatures and high voltages, affecting their service life.

Method used

Using a combination of low content of vinyl carbonate (EC) with specific first and second electrolyte salts, the content ratio in the electrolyte is adjusted, combining chain carbonate and third and fourth electrolyte salts, and additives such as 1 ,3-propanesulfolide and fluorovinyl carbonate form an optimized electrolyte for use in combination with high nickel content positive electrode active materials.

Benefits of technology

It significantly improves the high-temperature cycling and kinetic performance of the battery, extends the cycle life of the battery, reduces the interface ion impedance and side reactions, and enhances the ionic conductivity of the electrolyte and the flexibility of the interface mask.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023097179_05122024_PF_FP_ABST
    Figure CN2023097179_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided in the present application are an electrolyte, a battery cell and a preparation method therefor, a battery, and an electrical apparatus. The electrolyte comprises a non-aqueous solvent and electrolyte salts. The non-aqueous solvent comprises ethylene carbonate, and the weight content of ethylene carbonate in the non-aqueous solvent is denoted as x, on the basis of the total weight of the non-aqueous solvent. The electrolyte salts comprise a first electrolyte salt represented by formula (1) and a second electrolyte salt represented by formula (2); the weight content of the first electrolyte salt in the electrolyte is denoted as y, and the weight content of the second electrolyte salt is denoted as z, on the basis of the total weight of the electrolyte. R1 and R2 each independently comprises a fluorine atom and a C1-C6 fluoroalkyl group, R3 comprises a fluorine atom and C1-C6 fluoroalkyl, and M1 and M2 each independently comprises one or more of Li, Na and K; 5%≤x≤25%, 0.75≤x / y≤5 and 120≤x / z≤3000.
Need to check novelty before this filing date? Find Prior Art

Description

Electrolyte, battery cell and preparation method thereof, battery and electrical device Technical Field

[0001] The present application relates to an electrolyte, a battery cell and a preparation method thereof, a battery and an electrical device. Background Art

[0002] In recent years, batteries have been widely used in energy storage systems such as hydropower, thermal, wind, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, and other fields. The electrolyte, as a key component of a battery, affects its performance. The above statements are intended only to provide background information related to this application and do not necessarily constitute prior art.

[0003] Summary of the Invention

[0004] The present application provides an electrolyte, a battery cell and a preparation method thereof, a battery and an electrical device, which can improve the high-temperature cycle performance of the battery.

[0005] In a first aspect, the present application provides an electrolyte solution comprising a non-aqueous solvent and an electrolyte salt, wherein the non-aqueous solvent comprises ethylene carbonate, and the weight content of the ethylene carbonate in the non-aqueous solvent is recorded as x, based on the total weight of the non-aqueous solvent; the electrolyte salt comprises a first electrolyte salt represented by formula (1) and a second electrolyte salt represented by formula (2), and the weight content of the first electrolyte salt in the electrolyte solution is recorded as y, and the weight content of the second electrolyte salt is recorded as z, based on the total weight of the electrolyte solution; R1 and R2 independently include fluorine atoms and C1-C6 fluoroalkyl groups, R3 includes fluorine atoms and C1-C6 fluoroalkyl groups, and M1 and M2 independently include one or more of Li, Na, and K; 5%≤x≤25%, 0.75≤x / y≤5, and 120≤x / z≤3000.

[0006] The inventors have found that by combining a low content of EC (5%-25% of the total weight of the non-aqueous solvent) with the first electrolyte salt represented by formula (1) and the second electrolyte salt represented by formula (2), and rationally adjusting the content relationship between the three, the battery can have good high-temperature cycling performance.

[0007] In any embodiment, 8%≤x≤20%, optionally, 10%≤x≤18%. By adjusting the weight content x of EC in the non-aqueous solvent within the above range, the high temperature cycle performance of the battery can be further improved.

[0008] In any embodiment, 0.86≤x / y≤3, optionally, 1≤x / y≤2. Thus, the synergistic effect between EC and the first electrolyte salt can be better exerted, and the high-temperature cycle performance of the battery can be further improved.

[0009] In any embodiment, 160≤x / z≤1500, optionally, 300≤x / z≤1200. Thus, the synergistic effect between EC and the second electrolyte salt can be better exerted, and the high temperature cycle performance of the battery can be further improved.

[0010] In any embodiment, 2.4%≤y≤18%, optionally, 6%≤y≤12%.By adjusting the weight content y of the first electrolyte salt in the electrolyte within the above range, the high temperature cycle performance of the battery can be further improved.

[0011] In any embodiment, 0.004%≤z≤0.10%, optionally, 0.008%≤z≤0.075%.By adjusting the weight content z of the second electrolyte salt in the electrolyte within the above range, the high temperature cycle performance of the battery can be further improved.

[0012] In any embodiment, 10% ≤ x ≤ 18%, 1 ≤ x / y ≤ 2, 300 ≤ x / z ≤ 1200, 6% ≤ y ≤ 12%, and 0.008% ≤ z ≤ 0.075%. This can better utilize the synergistic effect between EC, the first electrolyte salt, and the second electrolyte salt, and can further improve the high-temperature cycle performance of the battery.

[0013] In any embodiment, R1 and R2 independently include fluorine atoms, trifluoromethyl groups, pentafluoroethyl groups, heptafluoropropyl groups, and nonafluorobutyl groups. When R1 and R2 are within the above ranges, it also helps to form a thinner interface film, thereby helping to reduce the interfacial ionic resistance and improve the dynamic performance of the battery.

[0014] In any embodiment, R3 includes a fluorine atom, a trifluoromethyl group, or a pentafluoroethyl group. When R3 is within the above range, it is also helpful to form a thinner interface film, thereby helping to reduce the interface ion resistance and improve the dynamic performance of the battery.

[0015] In any embodiment, the first electrolyte salt includes one or more of the following:

[0016] When the first electrolyte salt is within the above range, it has higher thermal stability and is less prone to hydrolysis, which helps to improve the ionic conductivity of the electrolyte, thereby helping to further improve the high-temperature cycle performance of the battery; in addition, it also helps to form a thinner interface film, thereby helping to reduce the interface ion impedance and improve the battery's kinetic performance.

[0017] In any embodiment, the second electrolyte salt includes one or more of the following:

[0018] When the second electrolyte salt is within the above range, its thermal stability is higher and the content of inorganic and organic components in the interface film can be better adjusted, thereby helping to obtain a thinner and more flexible interface film, thereby helping to further improve the high-temperature cycle performance of the battery. In addition, it also helps to reduce the interfacial ionic impedance and improve the kinetic performance of the battery.

[0019] In any embodiment, M1 includes one or both of Li and Na, and may be Li.

[0020] In any embodiment, M2 includes one or both of Li and Na, and can be Li.

[0021] In any embodiment, the non-aqueous solvent further comprises a chain carbonate ester. The chain carbonate ester can adjust the viscosity of the electrolyte, thereby further improving the ionic conductivity of the electrolyte and contributing to improving the high-temperature cycle performance of the battery.

[0022] In any embodiment, the weight content of the linear carbonate in the non-aqueous solvent is denoted as m, and based on the total weight of the non-aqueous solvent, m is ≥ 70%.

[0023] In any embodiment, the linear carbonate includes one or more of ethyl methyl carbonate, diethyl carbonate, and dimethyl carbonate.

[0024] In any embodiment, the non-aqueous solvent further comprises propylene carbonate.

[0025] In any embodiment, the weight content of the propylene carbonate in the non-aqueous solvent is recorded as n, based on the total weight of the non-aqueous solvent, and 0<n≤5%.

[0026] In any embodiment, the electrolyte further includes a third electrolyte salt represented by formula (3), and M3 includes one or more of Li, Na, and K.

[0027] The third electrolyte salt represented by formula (3) has appropriate solubility, high ionic conductivity, and a wide electrochemical window in the non-aqueous solvent, thereby improving the ionic conductivity of the electrolyte, passivating the positive electrode current collector, and reducing the corrosion of the positive electrode current collector by the first electrolyte salt. Therefore, when the electrolyte further includes the third electrolyte salt represented by formula (3), it helps to further improve the high-temperature cycle performance of the battery.

[0028] In any embodiment, M3 includes one or both of Li and Na, and may be Li.

[0029] In any embodiment, the weight content of the third electrolyte salt in the electrolyte is denoted as p, and based on the total weight of the electrolyte, 10% ≤ y + p ≤ 25%. This can provide the electrolyte with high ionic conductivity and low viscosity, thereby further improving the high-temperature cycling performance of the battery.

[0030] In any embodiment, the electrolyte further includes a fourth electrolyte salt represented by formula (4), and M4 includes one or more of Li, Na, and K.

[0031] The fourth electrolyte salt represented by formula (4) generally decomposes earlier in the electrolyte than the non-aqueous solvent, thereby forming a low-impedance interface film at the positive electrode. This interface film can protect the positive electrode active material, reduce the oxidative decomposition of the electrolyte on the positive electrode surface, reduce the gas production of the battery, improve the high-temperature storage performance of the battery, and also reduce the charge transfer resistance of the positive electrode, thereby improving the kinetic performance of the positive electrode. At the same time, the fourth electrolyte salt represented by formula (4) can also form a low-impedance interface film at the negative electrode, protecting the negative electrode active material and reducing the reductive decomposition of the electrolyte on the negative electrode surface. Therefore, when the electrolyte further includes the fourth electrolyte salt represented by formula (4), the high-temperature storage performance and / or kinetic performance of the battery can also be improved.

[0032] In any embodiment, M4 includes one or both of Li and Na, and may be Li.

[0033] In any embodiment, the weight content of the fourth electrolyte salt in the electrolyte is denoted as q, based on the total weight of the electrolyte, then 0<q≤0.5%, optionally, 0.1%≤q≤0.4%.

[0034] In any embodiment, the electrolyte further includes an additive, wherein the additive includes one or both of 1,3-propane sultone and fluoroethylene carbonate.

[0035] PS and FEC can form an interfacial film at the negative electrode, improve the stability of the negative electrode interfacial film, thereby better protecting the negative electrode active material, reducing the side reaction between the negative electrode active material and the electrolyte, and improving the high-temperature cycle performance of the battery.

[0036] In any embodiment, the weight content of the additive in the electrolyte is denoted as r, based on the total weight of the electrolyte, and 0<r≤3%.

[0037] A second aspect of the present application provides a battery cell comprising a positive electrode sheet, a negative electrode sheet, a separator, and the electrolyte of the first aspect of the present application.

[0038] In any embodiment, the battery cells include lithium secondary battery cells.

[0039] In any embodiment, the positive electrode sheet includes a first positive electrode active material, wherein the first positive electrode active material includes a general formula of Li a Ni b Co c M d O e A f One or more of lithium transition metal oxides and modified compounds thereof, 0.8≤a≤1.2, 0.8≤b<1, 0<c<0.2, 0<d<0.2, 1≤e≤2, 0≤f≤1, M includes one or more of Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti and B, and A includes one or more of N, F, S and Cl. Positive electrode active materials with high nickel content have a high voltage platform and high gram capacity, which is beneficial to improving the energy density of the battery, but their thermal stability and cycle stability are poor. The combined use of positive electrode active materials with high nickel content and the electrolyte provided in the embodiments of the present application can give full play to the advantages of the positive electrode active materials with high nickel content, thereby enabling the battery to have both high energy density and good high temperature cycle performance.

[0040] In any embodiment, the negative electrode plate includes one or more of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials and lithium titanate.

[0041] The third aspect of the present application provides a method for preparing a battery cell, comprising the following steps: providing a battery container comprising a positive electrode sheet, a negative electrode sheet and a separator; injecting the electrolyte of the first aspect of the present application into the battery container to obtain a battery cell.

[0042] A fourth aspect of the present application provides a battery, comprising the battery cell of the second aspect of the present application or the battery cell prepared by the preparation method of the third aspect of the present application.

[0043] A fifth aspect of the present application provides an electrical device comprising the battery of the fourth aspect of the present application.

[0044] The electric device of the present application includes the battery provided by the present application, and thus has at least the same advantages as the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] To more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on the drawings without inventive effort.

[0046] FIG1 is a schematic diagram of a battery cell according to an embodiment of the present application.

[0047] FIG. 2 is an exploded schematic diagram of an embodiment of the battery cell of FIG. 1 .

[0048] FIG3 is a schematic diagram of an embodiment of a battery module of the present application.

[0049] FIG4 is a schematic diagram of an embodiment of a battery pack of the present application.

[0050] FIG. 5 is an exploded schematic diagram of the embodiment of the battery pack shown in FIG. 4 .

[0051] FIG6 is a schematic diagram of an embodiment of an electric device including the battery of the present application as a power source.

[0052] In the accompanying drawings, which are not necessarily drawn to scale, reference numerals are as follows: 1 battery pack, 2 upper housing, 3 lower housing, 4 battery module, 5 battery cell, 51 housing, 52 electrode assembly, 53 cover plate. DETAILED DESCRIPTION

[0053] Below, the embodiments of the electrolyte, battery cells and their preparation methods, batteries and electrical devices of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0054] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0055] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of the present application.

[0056] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of this application.

[0057] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0058] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0059] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0060] Unless otherwise specified, in this application, the terms "first", "second", "third", "fourth", etc. are used to distinguish different objects rather than to describe a specific order or a primary-secondary relationship.

[0061] In this application, the terms "plurality" and "multiple" refer to two or more.

[0062] Unless otherwise specified, the terms used in this application have the common meanings that are commonly understood by those skilled in the art.

[0063] Unless otherwise stated, the numerical values ​​of the various parameters mentioned in this application can be measured using various test methods commonly used in the art, for example, they can be measured according to the test methods given in the examples of this application. Unless otherwise stated, the test temperature of each parameter is 25°C.

[0064] In the present application, "fluoroalkyl" may be a partially fluorinated alkyl or a fully fluorinated alkyl, and includes fluorinated straight-chain alkyl and fluorinated branched-chain alkyl.

[0065] In various embodiments, the C1-C6 fluoroalkyl group, ie, the fluoroalkyl group, may contain 1-6 carbon atoms.

[0066] Throughout this specification, substituents of compounds are disclosed in groups or ranges. It is expressly intended that this description includes each individual subcombination of members of these groups and ranges. For example, it is expressly intended that the term "C1-C6 fluoroalkyl" individually discloses C1, C2, C3, C4, C5, C6, C1-C6, C1-C5, C1-C4, C1-C3, C1-C2, C2-C6, C2-C5, C2-C4, C2-C3, C3-C6, C3-C5, C3-C4, C4-C6, C4-C5, C5-C6 fluoroalkyl.

[0067] The battery mentioned in the embodiments of the present application may be a single physical module including one or more battery cells to provide higher voltage and capacity. For example, the battery mentioned in the present application may include a battery cell, a battery module, or a battery pack.

[0068] A battery cell is the smallest unit of a battery, independently capable of charging and discharging. A battery cell can be cylindrical, rectangular, or have other shapes, though this is not a limitation in the present invention. Figure 1 shows a battery cell 5 with a rectangular structure as an example.

[0069] When there are multiple battery cells, the multiple battery cells are connected in series, in parallel, or in mixed series via a busbar. In some embodiments, the battery may be a battery module; when there are multiple battery cells, the multiple battery cells are arranged and fixed to form a battery module. In some embodiments, the battery may be a battery pack, which includes a housing and battery cells, with the battery cells or battery modules housed in the housing. In some embodiments, the housing may serve as part of the vehicle's chassis structure. For example, a portion of the housing may form at least a portion of the vehicle's floor, or a portion of the housing may form at least a portion of the vehicle's crossbeam or longitudinal beam.

[0070] In some embodiments, the battery may be an energy storage device, including an energy storage container, an energy storage cabinet, and the like.

[0071] A battery cell generally includes an electrode assembly and an electrolyte. The electrode assembly generally includes a positive electrode sheet and a negative electrode sheet. The electrode assembly can be a wound structure or a laminated structure, which is not limited in the present embodiment.

[0072] The battery cell may also include an outer packaging, which can be used to encapsulate the electrode assembly and electrolyte. The outer packaging can be a hard shell, such as a hard plastic shell, aluminum shell, steel shell, etc. The outer packaging can also be a soft package, such as a bag-type soft package. The soft package can be made of plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).

[0073] In some embodiments, as shown in Figure 2, the outer packaging may include a housing 51 and a cover plate 53. The housing 51 may include a base plate and side plates connected to the base plate, which together form a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover plate 53 is used to cover the opening, thereby sealing the receiving cavity. The electrode assembly 52 is enclosed in the receiving cavity. The number of electrode assemblies 52 contained in a battery cell 5 can be one or more, and can be adjusted according to needs.

[0074] In some embodiments, battery cells can be assembled into a battery module. The number of battery cells contained in a battery module can be multiple, and the specific number can be adjusted according to the application and capacity of the battery module. Figure 3 is a schematic diagram of a battery module 4 as an example. As shown in Figure 3, in the battery module 4, multiple battery cells 5 can be arranged in sequence along the length of the battery module 4. Of course, they can also be arranged in any other manner. The multiple battery cells 5 can further be fixed by fasteners.

[0075] Optionally, the battery module 4 may further include a housing having an accommodation space, and the plurality of battery cells 5 are accommodated in the accommodation space.

[0076] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0077] Figures 4 and 5 are schematic diagrams of an exemplary battery pack 1. As shown in Figures 4 and 5, the battery pack 1 may include a housing and multiple battery modules 4 disposed within the housing. The housing comprises an upper housing 2 and a lower housing 3. The upper housing 2 covers the lower housing 3 and forms an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 may be arranged in any manner within the housing.

[0078] The electrolyte is one of the key factors affecting battery performance. As demand for battery energy density continues to increase, ternary materials, especially high-nickel ternary materials, have attracted widespread attention due to their high voltage platform and high gram capacity. However, the thermal and cycling stability of ternary materials are not excellent. Furthermore, side reactions between the electrolyte and the cathode active material increase at high temperatures and high voltages, thus affecting battery performance.

[0079] In view of this, the inventors improved the electrolyte.

[0080] The electrolyte provided in the embodiments of the present application can be used in a battery cell, which can be a lithium secondary battery cell.

[0081] The electrolyte includes a non-aqueous solvent and an electrolyte salt. The non-aqueous solvent includes ethylene carbonate (EC), and the weight content of ethylene carbonate in the non-aqueous solvent is recorded as x, based on the total weight of the non-aqueous solvent; the electrolyte salt includes a first electrolyte salt represented by formula (1) and a second electrolyte salt represented by formula (2), and the weight content of the first electrolyte salt in the electrolyte is recorded as y, and the weight content of the second electrolyte salt is recorded as z, based on the total weight of the electrolyte; R1 and R2 independently include fluorine atoms and C1-C6 fluoroalkyl groups, R3 includes fluorine atoms and C1-C6 fluoroalkyl groups, M1 and M2 independently include one or more of Li, Na, and K; 5%≤x≤25%, 0.75≤x / y≤5, and 120≤x / z≤3000.

[0082] EC is widely used as a non-aqueous solvent in electrolytes due to its high dielectric constant. Current commercial battery electrolytes typically contain over 30% EC by weight, resulting in high ionic conductivity. However, EC is unstable at high temperatures, and high EC content can affect the battery's high-temperature performance.

[0083] The inventors have found that by combining a low content of EC (5%-25% of the total weight of the non-aqueous solvent) with the first electrolyte salt represented by formula (1) and the second electrolyte salt represented by formula (2), and rationally adjusting the content relationship between the three, the battery can have good high-temperature cycling performance.

[0084] Compared with the electrolytes of current commercial batteries, the electrolyte provided in the embodiments of the present application has a lower EC content, which is 5%-25% of the total weight of the non-aqueous solvent, thereby reducing the adverse effects of high EC content on the high-temperature performance of the battery.

[0085] The first electrolyte salt shown in formula (1) has the characteristics of high thermal stability and non-hydrolysis, which helps to form an interface film with high thermal stability on the surface of the negative electrode active material, thereby reducing the side reaction between the negative electrode active material and the electrolyte. In addition, the anion of the first electrolyte salt is a weakly coordinated anion centered on N, containing a conjugated group and a strongly charge-absorbing fluorine atom and / or a fluoroalkyl group. The anion charge is highly delocalized, and the interaction force between the anion and the metal M1 ion is weak. Therefore, the first electrolyte salt also has a low lattice energy and is easy to dissociate, which also helps to improve the ionic conductivity of the electrolyte and reduce the viscosity of the electrolyte.

[0086] However, the first electrolyte salt easily corrodes the positive electrode current collector (eg, aluminum foil), thereby increasing the side reaction between the positive electrode active material and the electrolyte, and thus easily affecting the high-temperature cycle performance of the battery.

[0087] The inventors have discovered that by making the electrolyte contain the first electrolyte salt represented by formula (1) and adjusting the relationship between the weight content x of EC in the non-aqueous solvent and the weight content y of the first electrolyte salt in the electrolyte so that it satisfies 0.75≤x / y≤5, the synergistic effect of EC and the first electrolyte salt can be fully exerted. By using the first electrolyte salt in the electrolyte, the thermal stability of the electrolyte can be improved, the hydrolysis of the electrolyte can be reduced, and the deficiency of low EC content in the electrolyte ion conductivity can be supplemented; EC and the anions of the first electrolyte salt have a certain binding force, thereby reducing the corrosion of the first electrolyte salt on the positive electrode current collector, and further reducing the side reactions between the positive electrode active material and the electrolyte. Therefore, by adjusting 0.75≤x / y≤5, the battery can have good high-temperature cycle performance.

[0088] When x / y is less than 0.75, the content of EC in the non-aqueous solvent is relatively small and the content of the first electrolyte salt in the electrolyte is relatively large. At this time, some anions of the first electrolyte salt cannot combine with EC molecules, resulting in more serious corrosion of the positive electrode current collector by the anions of the first electrolyte salt under high temperature and high voltage, which in turn deteriorates the high-temperature cycle performance of the battery.

[0089] When x / y is greater than 5, the content of EC in the non-aqueous solvent is relatively high while the content of the first electrolyte salt in the electrolyte is relatively low. At this time, there are more free EC molecules in the electrolyte, which will also deteriorate the high-temperature cycle performance of the battery.

[0090] In some embodiments, optionally, 0.86≤x / y≤3, 1≤x / y≤2. Thus, the synergistic effect between EC and the first electrolyte salt can be better exerted, and the high-temperature cycle performance of the battery can be further improved.

[0091] The second electrolyte salt represented by formula (2) has high thermal stability and can improve the charge-discharge characteristics of the battery at high temperatures. Furthermore, the second electrolyte salt can form a film on the surface of the negative electrode active material or the positive electrode active material, and can also adjust the composition of the interface film, thereby reducing side reactions between the negative electrode active material and the electrolyte, as well as between the positive electrode active material and the electrolyte. However, the second electrolyte salt has low ionic conductivity, and when the second electrolyte salt content is too high, the content of inorganic components in the interface film increases, thereby reducing the flexibility of the interface film. After repeated charge and discharge, the interface film is prone to cracking, which in turn deteriorates the high-temperature cycle performance of the battery.

[0092] The inventors have found that by making the electrolyte contain a second electrolyte salt represented by formula (2) and adjusting the relationship between the weight content x of EC in the non-aqueous solvent and the weight content z of the second electrolyte salt in the electrolyte so that it satisfies 120≤x / z≤3000, the synergistic effect of EC and the second electrolyte salt can be fully exerted. By adopting a suitable content of the second electrolyte salt, the composition of the interface film can be adjusted so that the interface film has a suitable content of inorganic components and a suitable content of organic components, thereby obtaining a dense, uniform and flexible interface film, which can play the role of long-term protection of the active material by the interface film and reduce the side reactions between the negative electrode active material and the electrolyte and the side reactions between the positive electrode active material and the electrolyte. Therefore, by adjusting 120≤x / z≤3000, the cycle stability of the battery can be improved, and the battery can have a longer high-temperature cycle life.

[0093] When x / z is less than 120, the content of EC in the non-aqueous solvent is relatively small and the content of the second electrolyte salt in the electrolyte is relatively large. At this time, the content of inorganic components in the interface film formed on the surface of the negative electrode active material is high. The inorganic components are usually more rigid, which leads to poor elasticity and flexibility of the interface film, thereby deteriorating the high-temperature cycle performance of the battery.

[0094] When x / y is greater than 3000, the content of EC in the non-aqueous solvent is relatively high and the content of the second electrolyte salt in the electrolyte is relatively low. At this time, the content of organic components in the interface film formed on the surface of the negative electrode active material is high. At high temperatures, the organic components in the interface film are more easily dissolved into the electrolyte, which will also deteriorate the high-temperature cycle performance of the battery.

[0095] In some embodiments, optionally, 160≤x / z≤1500, 300≤x / z≤1200, 400≤x / z≤1000, and 400≤x / z≤800. In this way, the synergistic effect between EC and the second electrolyte salt can be better exerted, and the high temperature cycle performance of the battery can be further improved.

[0096] In some embodiments, optionally, 8%≤x≤20%, 10%≤x≤18%.By adjusting the weight content x of EC in the non-aqueous solvent within the above range, the high temperature cycle performance of the battery can be further improved.

[0097] In some embodiments, optionally, 2.4%≤y≤18%, 4%≤y≤15%, 6%≤y≤12%, and 6%≤y≤10%. By adjusting the weight content y of the first electrolyte salt in the electrolyte within the above range, the high-temperature cycle performance of the battery can be further improved.

[0098] In some embodiments, optionally, 0.004%≤z≤0.10%, 0.008%≤z≤0.075%, 0.01%≤z≤0.06%, and 0.01%≤z≤0.04%. By adjusting the weight content z of the second electrolyte salt in the electrolyte within the above range, the high-temperature cycle performance of the battery can be further improved.

[0099] In some embodiments, 10% ≤ x ≤ 18%, 1 ≤ x / y ≤ 2, 300 ≤ x / z ≤ 1200, 6% ≤ y ≤ 12%, and 0.008% ≤ z ≤ 0.075%. Thus, the synergistic effect between EC, the first electrolyte salt, and the second electrolyte salt can be better utilized, and the high-temperature cycling performance of the battery can be further improved.

[0100] M1 includes one or more of Li, Na, and K. In some embodiments, M1 may include one or both of Li and Na, and may be Li.

[0101] M2 includes one or more of Li, Na, and K. In some embodiments, M2 may include one or both of Li and Na, and may be Li.

[0102] In some embodiments, R1 and R2 may independently include a fluorine atom, a trifluoromethyl group, a pentafluoroethyl group, a heptafluoropropyl group, or a nonafluorobutyl group. When R1 and R2 are within the above ranges, they can also help form a thinner interfacial film, thereby reducing interfacial ionic resistance and improving the kinetic performance of the battery.

[0103] In some embodiments, the first electrolyte salt may include one or more of the following:

[0104] In some embodiments, the first electrolyte salt may include one or more of A1 to A7:

[0105] When the first electrolyte salt is within the above range, it has higher thermal stability and is less prone to hydrolysis, which helps to improve the ionic conductivity of the electrolyte, thereby helping to further improve the high-temperature cycle performance of the battery; in addition, it also helps to form a thinner interface film, thereby helping to reduce the interface ion impedance and improve the battery's kinetic performance.

[0106] In some embodiments, R3 may include a fluorine atom, a trifluoromethyl group, or a pentafluoroethyl group. When R3 is within the above range, it is also helpful to form a thinner interface film, thereby helping to reduce the interface ion impedance and improve the kinetic performance of the battery.

[0107] In some embodiments, the second electrolyte salt may include one or more of the following:

[0108] In some embodiments, the second electrolyte salt may include one or more of B1 to B6:

[0109] When the second electrolyte salt is within the above range, its thermal stability is higher and the content of inorganic and organic components in the interface film can be better adjusted, thereby helping to obtain a thinner and more flexible interface film, thereby helping to further improve the high-temperature cycle performance of the battery. In addition, it also helps to reduce the interfacial ionic impedance and improve the kinetic performance of the battery.

[0110] In some embodiments, the non-aqueous solvent may further include a chain carbonate ester, which can adjust the viscosity of the electrolyte, thereby further improving the ionic conductivity of the electrolyte and helping to improve the high-temperature cycle performance of the battery.

[0111] In some embodiments, the weight content of the linear carbonate in the non-aqueous solvent is denoted as m. Based on the total weight of the non-aqueous solvent, m ≥ 70%. For example, m can be 75%, 78%, 80%, 82%, 85%, 88%, 90%, 95%, or any range thereof. Alternatively, 70% ≤ m ≤ 95%, 75% ≤ m ≤ 95%, 75% ≤ m ≤ 90%, 80% ≤ m ≤ 90%, and 82% ≤ m ≤ 88%.

[0112] In some embodiments, the linear carbonate may include one or more of ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), and ethyl propyl carbonate (EPC). Alternatively, the linear carbonate may include one or more of ethyl methyl carbonate (EMC), diethyl carbonate (DEC), and dimethyl carbonate (DMC).

[0113] In some embodiments, the non-aqueous solvent may further include propylene carbonate. Optionally, the weight content of propylene carbonate in the non-aqueous solvent is recorded as n, based on the total weight of the non-aqueous solvent, then 0<n≤5%.

[0114] In some embodiments, the non-aqueous solvent may further include other solvents, for example, methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), cyclopentane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS) and diethyl sulfone (ESE) One or more of the present application embodiment is not limited to this.

[0115] In some embodiments, the electrolyte may further include a third electrolyte salt represented by formula (3), wherein M3 includes one or more of Li, Na, and K. Alternatively, M3 includes one or both of Li and Na, and more preferably, Li.

[0116] The third electrolyte salt represented by formula (3) has appropriate solubility, high ionic conductivity, and a wide electrochemical window in the non-aqueous solvent, thereby improving the ionic conductivity of the electrolyte, passivating the positive electrode current collector, and reducing the corrosion of the positive electrode current collector by the first electrolyte salt. Therefore, when the electrolyte further includes the third electrolyte salt represented by formula (3), it helps to further improve the high-temperature cycle performance of the battery.

[0117] In some embodiments, the weight content of the third electrolyte salt in the electrolyte is denoted as p, and based on the total weight of the electrolyte, 10% ≤ y + p ≤ 25%, and optionally, 12% ≤ y + p ≤ 20%. This can provide the electrolyte with high ionic conductivity and low viscosity, thereby further improving the high-temperature cycling performance of the battery.

[0118] In some embodiments, the electrolyte may further include a fourth electrolyte salt represented by formula (4), wherein M4 includes one or more of Li, Na, and K. Alternatively, M4 includes one or both of Li and Na, and more preferably, Li.

[0119] The fourth electrolyte salt represented by formula (4) generally decomposes earlier in the electrolyte than the non-aqueous solvent, thereby forming a low-impedance interface film at the positive electrode. This interface film can protect the positive electrode active material, reduce the oxidative decomposition of the electrolyte on the positive electrode surface, reduce the gas production of the battery, improve the high-temperature storage performance of the battery, and also reduce the charge transfer resistance of the positive electrode, thereby improving the kinetic performance of the positive electrode. At the same time, the fourth electrolyte salt represented by formula (4) can also form a low-impedance interface film at the negative electrode, protecting the negative electrode active material and reducing the reductive decomposition of the electrolyte on the negative electrode surface. Therefore, when the electrolyte further includes the fourth electrolyte salt represented by formula (4), the high-temperature storage performance and / or kinetic performance of the battery can also be improved.

[0120] In some embodiments, the weight content of the fourth electrolyte salt in the electrolyte is denoted as q, based on the total weight of the electrolyte, then 0<q≤0.5%, optionally, 0.1%≤q≤0.4%.

[0121] In some embodiments, the electrolyte may further include other electrolyte salts. For example, the anions of the electrolyte salt may further include perchlorate anions (ClO4 - ), hexafluoroarsenate anion (AsF6 - ), difluorooxalatoborate anion (DFOB - ), dioxalatoborate anion (BOB - ), difluorobis(oxaloyl)phosphate anion (DFOP - ) and tetrafluorooxalophosphate anion (TFOP - ) in one or more; the cation of the electrolyte salt may include Li + 、Na + , K + One or more of, optionally including Li + 、Na + One or two of the following, preferably Li + .

[0122] In some embodiments, the electrolyte may further include an additive, and the additive may include one or both of 1,3-propane sultone (PS) and fluoroethylene carbonate (FEC).

[0123] PS and FEC can form an interfacial film at the negative electrode, improve the stability of the negative electrode interfacial film, thereby better protecting the negative electrode active material, reducing the side reaction between the negative electrode active material and the electrolyte, and improving the high-temperature cycle performance of the battery.

[0124] PS can also improve the flexibility of the positive electrode interface film, allowing the battery to remain stable during long-term cycling; PS can also reduce the gas production of the battery and improve the high-temperature storage performance of the battery.

[0125] The LUMO energy of FEC is much lower than that of EC, so its decomposition in the electrolyte is usually earlier than that of non-aqueous solvents, which can reduce the decomposition of the electrolyte, reduce the gas production of the battery, and improve the high-temperature storage performance of the battery; FEC can also increase the content of inorganic components in the negative electrode interface film, thereby improving the mechanical strength of the negative electrode interface film, thereby improving the cycle stability of the negative electrode interface film; FEC also helps to form a thin and stable interface film at the negative electrode, reduce the diffusion impedance of ions, and help reduce the low-temperature impedance of the negative electrode interface film, thereby improving the low-temperature performance of the battery.

[0126] In some embodiments, the weight content of the additive in the electrolyte is denoted as r, based on the total weight of the electrolyte, and 0<r≤3%.

[0127] In some embodiments, the electrolyte may further include other additives, for example, additives for improving the overcharge performance of the battery, additives for improving the low-temperature power performance of the battery, etc., which are not limited in the embodiments of the present application.

[0128] The electrolyte provided in the embodiments of the present application can be prepared according to conventional methods in the art. For example, the non-aqueous solvent, electrolyte salt, optional additives, and other components can be mixed uniformly to obtain the electrolyte. The order of adding the materials is not particularly limited. For example, the electrolyte salt, optional additives, and other components can be added to the non-aqueous solvent and mixed uniformly to obtain the electrolyte.

[0129] The components and their contents in the electrolyte can be determined by methods known in the art, for example, by gas chromatography-mass spectrometry (GC-MS), ion chromatography (IC), liquid chromatography (LC), nuclear magnetic resonance spectroscopy (NMR), and the like.

[0130] [Positive electrode]

[0131] The battery cell also includes a positive electrode plate.

[0132] The positive electrode sheet includes a positive electrode current collector and a positive electrode film disposed on at least one surface of the positive electrode current collector. For example, the positive electrode current collector has two surfaces that face each other in the thickness direction, and the positive electrode film is disposed on either or both of the two opposing surfaces of the positive electrode current collector.

[0133] The positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0134] The positive electrode film typically contains a positive electrode active material, an optional binder, and an optional conductive agent. The positive electrode film is typically formed by coating a positive electrode slurry onto a positive electrode current collector, followed by drying and cold pressing. The positive electrode slurry is typically formed by dispersing the positive electrode active material, an optional binder, an optional conductive agent, and any other components in a solvent and stirring until uniformly mixed.

[0135] The solvent may be N-methylpyrrolidone (NMP), but is not limited thereto.

[0136] As an example, the binder for the positive electrode film layer may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.

[0137] As an example, the conductive agent used for the positive electrode film layer may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0138] In some embodiments, the positive electrode active material may include a first positive electrode active material. The first positive electrode active material may include a general formula of Li a Ni b Co c M d O e A fOne or more lithium transition metal oxides and modified compounds thereof. 0.8≤a≤1.2, 0.5≤b<1, 0<c<1, 0<d<1, 1≤e≤2, 0≤f≤1, M includes one or more of Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti and B, and A includes one or more of N, F, S and Cl.

[0139] Optionally, 0.8≤b<1, 0<c<0.2, 0<d<0.2. Positive electrode active materials with high nickel content have a high voltage platform and high gram capacity, which is beneficial to improving the energy density of the battery, but their thermal stability and cycle stability are poor. The use of positive electrode active materials with high nickel content in combination with the electrolyte provided in the embodiments of the present application can give full play to the advantages of the positive electrode active materials with high nickel content, thereby enabling the battery to have both high energy density and good high temperature cycle performance.

[0140] As an example, the first positive active material may include LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM333),LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM523),LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM622),LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM811), LiNi 0.85 Co 0.15 Al 0.05 O2, and one or more of their respective modified compounds.

[0141] The modifying compounds of each of the above-mentioned positive electrode active materials may be doped and / or surface-coated to modify the positive electrode active materials. For example, the coating layer may be a carbon coating layer. The carbon coating layer helps stabilize the surface of the positive electrode active material, further reduces the charge transfer resistance of the positive electrode active material, and improves the kinetic properties of the positive electrode active material. Optionally, the carbon coating layer includes amorphous carbon, such as soft carbon, hard carbon, or a combination thereof.

[0142] Li a Ni b Co c M d O e A fIt can be prepared according to conventional methods in the art. An exemplary preparation method is as follows: a lithium source, a nickel source, a cobalt source, an M element precursor, and an optional A element precursor are mixed and sintered to obtain the obtained product. The sintering atmosphere may be an oxygen-containing atmosphere, for example, an air atmosphere or an oxygen atmosphere. The O2 concentration of the sintering atmosphere is, for example, 70% to 100%. The sintering temperature and sintering time may be adjusted according to actual conditions. As an example, the lithium source includes but is not limited to one or more of lithium oxide (Li2O), lithium phosphate (Li3PO4), lithium dihydrogen phosphate (LiH2PO4), lithium acetate (CH3COOLi), lithium hydroxide (LiOH), lithium carbonate (Li2CO3) and lithium nitrate (LiNO3). As an example, the nickel source includes but is not limited to one or more of nickel sulfate, nickel nitrate, nickel chloride, nickel oxalate and nickel acetate. As an example, the cobalt source includes but is not limited to one or more of cobalt sulfate, cobalt nitrate, cobalt chloride, cobalt oxalate and cobalt acetate. As an example, the M element precursor includes but is not limited to one or more of the oxide, nitric acid compound, carbonate compound, hydroxide and acetic acid compound of the M element. As an example, the precursor of element A includes but is not limited to one or more of ammonium fluoride, lithium fluoride, hydrogen fluoride, ammonium chloride, lithium chloride, hydrogen chloride, ammonium nitrate, ammonium nitrite, ammonium carbonate, ammonium bicarbonate, ammonium phosphate, phosphoric acid, ammonium sulfate, ammonium bisulfate, ammonium bisulfite, ammonium sulfite, ammonium bisulfide, hydrogen sulfide, lithium sulfide, ammonium sulfide and elemental sulfur.

[0143] In some embodiments, the positive electrode active material does not exclude the following: a Ni b Co c M d O e A f The positive electrode active material may further include components other than the lithium transition metal oxide and its modified compounds. For example, the positive electrode active material may further include a second positive electrode active material, and the second positive electrode active material may include one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium-containing phosphate, and their respective modified compounds. As an example, the lithium-containing phosphate may include one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, a composite material of lithium iron manganese phosphate and carbon, and their respective modified compounds.

[0144] In some embodiments, the weight percentage of the first positive electrode active material may be 80% to 99%, based on the total weight of the positive electrode film layer. For example, the weight percentage of the first positive electrode active material may be 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99% or any range consisting of the above values. Alternatively, the weight percentage of the first positive electrode active material may be 85% to 99%, 90% to 99%, 95% to 99%, 80% to 98%, 85% to 98%, 90% to 98%, 95% to 98%, 80% to 97%, 85% to 97%, 90% to 97% or 95% to 97%.

[0145] In some embodiments, the specific surface area of ​​the positive electrode active material can be 0.3-3 m 2 When the specific surface area of ​​the positive electrode active material is within the above range, the positive electrode active material can have good kinetic properties and can also reduce side reactions at high temperatures of the battery, thereby enabling the battery to have good high-temperature cycle performance and kinetic performance.

[0146] The specific surface area of ​​a positive electrode active material is well known in the art and can be measured using instruments and methods known in the art. For example, it can be measured using the nitrogen adsorption specific surface area analysis method in accordance with GB / T 19587-2017 and calculated using the BET (Brunauer Emmett Teller) method. The testing instrument can be a Micromeritics Tri-Star 3020 Specific Surface Area Pore Size Analyzer.

[0147] In some embodiments, the compaction density of the positive electrode sheet can be 2.9-3.6 g / cm 3 When the compaction density of the positive electrode sheet is within the above range, the positive electrode sheet can have good conductivity and good electrolyte wettability, thereby enabling the battery to have good high-temperature cycle performance and dynamic performance.

[0148] The compacted density of the positive electrode sheet is a well-known meaning in the art and can be measured using instruments and methods known in the art. The compacted density of the positive electrode sheet = the surface density of the positive electrode film layer / the thickness of the positive electrode film layer. The thickness of the positive electrode film layer is a well-known meaning in the art and can be measured using instruments and methods known in the art, such as testing with a micrometer. The surface density of the positive electrode film layer is a well-known meaning in the art and can be measured using instruments and methods known in the art. For example, a single-sided coated and cold-pressed positive electrode sheet can be taken (if it is a double-sided coated positive electrode sheet, the positive electrode film layer on one side can be wiped off first), punched into small discs with an area of ​​S1, weighed, and recorded as M1; then the positive electrode film layer of the weighed positive electrode sheet is wiped off, and the weight of the positive electrode current collector is weighed and recorded as M0; the surface density of the positive electrode sheet = (M1-M0) / S1.

[0149] [Negative electrode]

[0150] The battery cell includes a negative electrode plate.

[0151] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode film disposed on at least one surface of the negative electrode current collector. For example, the negative electrode current collector has two opposing surfaces in the thickness direction of the negative electrode current collector, and the negative electrode film is disposed on either or both of the two opposing surfaces of the negative electrode current collector.

[0152] The negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, copper foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0153] The negative electrode film typically contains a negative electrode active material, an optional binder, an optional conductive agent, and other optional additives. The negative electrode film is typically formed by coating a negative electrode slurry onto a negative electrode current collector, followed by drying and cold pressing. The negative electrode slurry is typically formed by dispersing the negative electrode active material, an optional conductive agent, an optional binder, and other optional additives in a solvent and stirring them uniformly.

[0154] The solvent may be N-methylpyrrolidone (NMP) or deionized water, but is not limited thereto.

[0155] As an example, the binder for the negative electrode film layer may include one or more of styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, aqueous acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA) and carboxymethyl chitosan (CMCS).

[0156] As an example, the conductive agent for the negative electrode film layer may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. Other optional additives may include thickeners (e.g., sodium carboxymethyl cellulose CMC-Na), PTC thermistor materials, etc.

[0157] The negative electrode active material may be a material known in the art. As an example, the negative electrode active material may include one or more of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials and lithium titanate. Silicon-based materials may include one or more of elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite and silicon alloy materials. Tin-based materials may include one or more of elemental tin, tin oxide and tin alloy materials. The present application is not limited to these materials, and other conventionally known materials that can be used as negative electrode active materials may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0158] [Isolation film]

[0159] The battery cell also includes a separator.

[0160] The separator is provided between the positive electrode and the negative electrode to isolate the electrodes. The present application does not particularly limit the type of separator, and any known porous structure membrane with good chemical and mechanical stability can be selected.

[0161] In some embodiments, the material of the isolation membrane can include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different.

[0162] Preparation method

[0163] The embodiments of the present application also provide a method for preparing a battery cell.

[0164] The method comprises the following steps: providing a battery container comprising a positive electrode sheet, a negative electrode sheet and a separator; and injecting the electrolyte provided in an embodiment of the present application into the battery container comprising the positive electrode sheet, the negative electrode sheet and the separator.

[0165] In some embodiments, the method may further include the following steps: forming an electrode assembly by winding the positive electrode sheet, the separator and the negative electrode sheet through a winding process and / or a lamination process, and placing the electrode assembly in a battery container.

[0166] The battery container can be an outer packaging. The outer packaging can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. The outer packaging can also be a soft package, such as a bag-type soft package. The soft package can be made of plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).

[0167] Multiple battery cells can be further connected in series, parallel, or hybrid to form a battery module. Multiple battery modules can also be connected in series, parallel, or hybrid to form a battery pack. In some embodiments, multiple battery cells can also be directly connected to form a battery pack.

[0168] Electrical devices

[0169] The present application also provides an electrical device, which includes a battery provided in the present application. The battery can be used as a power source for the electrical device or as an energy storage unit for the electrical device. The electrical device can be, but is not limited to, a mobile device (such as a mobile phone, a tablet computer, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship, a satellite, an energy storage system, etc.

[0170] The electrical device can select the type of battery according to its usage requirements, such as a battery cell, a battery module or a battery pack.

[0171] Figure 6 is a schematic diagram of an exemplary electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of this device, a battery pack or battery module may be used.

[0172] As another example, an electric device may be a mobile phone, a tablet computer, a laptop computer, etc. Such an electric device is usually required to be lightweight and thin, and may use a battery cell as a power source.

[0173] Example

[0174] The following examples describe the present disclosure in more detail and are intended to be illustrative only, as various modifications and variations within the scope of the present disclosure will be apparent to those skilled in the art. Unless otherwise indicated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and used directly without further processing, and all instruments used in the examples are commercially available.

[0175] Examples 1-26 and Comparative Examples 1-7 were prepared according to the following method.

[0176] Preparation of positive electrode

[0177] The positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1 O2, conductive agent carbon black, and binder polyvinylidene fluoride (PVDF) are fully stirred and mixed in an appropriate amount of solvent NMP in a weight ratio of 97.5:1.4:1.1 to form a uniform positive electrode slurry; the positive electrode slurry is evenly coated on the surface of the positive electrode current collector aluminum foil, and after drying and cold pressing, the positive electrode sheet is obtained.

[0178] Preparation of negative electrode sheet

[0179] The negative electrode active material graphite, binder styrene-butadiene rubber (SBR), thickener sodium carboxymethyl cellulose (CMC-Na), and conductive agent carbon black (Super P) are fully stirred and mixed in an appropriate amount of solvent deionized water in a weight ratio of 96.2:1.8:1.2:0.8 to form a uniform negative electrode slurry; the negative electrode slurry is evenly coated on the surface of the negative electrode current collector copper foil, and after drying and cold pressing, the negative electrode sheet is obtained.

[0180] Isolation film

[0181] A porous polyethylene (PE) film is used as the separator.

[0182] Preparation of electrolyte

[0183] Ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were uniformly mixed according to the weight contents shown in Table 1 to obtain a non-aqueous solvent. The electrolyte salts shown in Table 1 were dissolved in the non-aqueous solvent according to the weight contents shown in Table 1, and stirred to obtain an electrolyte solution.

[0184] In Table 1, the weight content of EC is recorded as x, the weight content of PC is recorded as n, and the sum of the weight contents of EMC and DEC is recorded as m, all of which are based on the total weight of the non-aqueous solvent, and the weight ratio of EMC to DEC is 1:1.

[0185] In Table 1, the weight content of the first electrolyte salt is recorded as y, the weight content of the second electrolyte salt is recorded as z, and the weight content of the third electrolyte salt is recorded as p, all based on the total weight of the electrolyte.

[0186] In Table 1, “ / ” indicates that the corresponding component was not added to the electrolyte.

[0187] Battery preparation

[0188] The positive electrode sheet, separator, and negative electrode sheet are stacked and wound in order to obtain an electrode assembly; the electrode assembly is placed in an outer package, injected with the above-mentioned electrolyte, and after packaging, standing, formation and other processes, a battery is obtained.

[0189] Test section

[0190] (1) High temperature cycle performance test

[0191] At 45°C, charge the battery at a constant current of 1C to 4.3V. Continue constant voltage charging until the current reaches 0.05C. At this point, the battery is fully charged. Record the charge capacity at this point, which is the charge capacity of the first cycle. After the battery rests for 5 minutes, discharge it at a constant current of 1C to 2.8V. This constitutes one charge-discharge cycle. Record the discharge capacity at this point, which is the discharge capacity of the first cycle. Perform the battery cyclic charge-discharge test as described above, and record the discharge capacity after each cycle. Capacity retention (%) of the battery after 600 cycles at 45°C = discharge capacity after 600 cycles / discharge capacity after the first cycle × 100%.

[0192] (2) Battery high temperature storage performance test

[0193] At 60°C, charge the battery at a constant current of 1C to 4.3V. Continue constant voltage charging until the current reaches 0.05C. At this point, measure the battery volume using the water displacement method and record it as V0. Place the battery in a 60°C incubator and store it for 30 days. After removal, measure the battery volume using the water displacement method and record it as V1. The volume expansion rate (%) of the battery after 30 days of storage at 60°C = [(V1 - V0) / V0] × 100%.

[0194] Table 1 gives the test results of Examples 1-26 and Comparative Examples 1-7.

[0195] Table 1

[0196] It can be seen from the test results in Table 1 that by using a low content of EC in combination with the first electrolyte salt represented by formula (1) and the second electrolyte salt represented by formula (2), and reasonably adjusting the content relationship between the three so that they satisfy 0.75≤x / y≤5 and 120≤x / z≤3000, the battery can have good high-temperature cycle performance.

[0197] Examples 27-29

[0198] The battery preparation method is similar to that of Example 4, except for the preparation of the electrolyte. In Table 2, the weight content of the fourth electrolyte salt is denoted as q, and the weight content of the additive is denoted as r, both based on the total weight of the electrolyte. " / " indicates that the corresponding component was not added to the electrolyte.

[0199] In Example 27, 0.2% LiPO2F2 was added to the electrolyte provided in Example 4.

[0200] In Example 28, 0.2% LiPO2F2 and 1% PS were added to the electrolyte provided in Example 4.

[0201] In Example 29, 0.2% LiPO2F2 and 1% FEC were added to the electrolyte provided in Example 4.

[0202] Table 2

[0203] It can be seen from the test results in Table 2 that when a suitable content of the fourth electrolyte salt and / or additive is further added to the electrolyte, the high-temperature cycle performance of the battery can be further improved, and the high-temperature storage performance of the battery can also be further improved.

[0204] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. An electrolyte solution comprising a non-aqueous solvent and an electrolyte salt, wherein: The non-aqueous solvent includes ethylene carbonate, and the weight content of the ethylene carbonate in the non-aqueous solvent is recorded as x, based on the total weight of the non-aqueous solvent; The electrolyte salt comprises a first electrolyte salt represented by formula (1) and a second electrolyte salt represented by formula (2), and the weight content of the first electrolyte salt in the electrolyte is denoted by y, and the weight content of the second electrolyte salt is denoted by z, based on the total weight of the electrolyte; R1 and R2 each independently include a fluorine atom or a C1-C6 fluoroalkyl group, R3 includes a fluorine atom or a C1-C6 fluoroalkyl group, and M1 and M2 each independently include one or more of Li, Na, and K; Among them, 5%≤x≤25%, 0.75≤x / y≤5 and 120≤x / z≤3000.

2. The electrolyte according to claim 1, wherein 8%≤x≤20%, optionally, 10%≤x≤18%; and / or, 0.86≤x / y≤3, optionally, 1≤x / y≤2; and / or, 160≤x / z≤1500, optionally, 300≤x / z≤1200.

3. The electrolyte according to claim 2, wherein 2.4%≤y≤18%, optionally, 6%≤y≤12%; and / or, 0.004%≤z≤0.10%, optionally, 0.008%≤z≤0.075%.

4. The electrolyte according to claim 1, wherein 10%≤x≤18%, 1≤x / y≤2, 300≤x / z≤1200, 6%≤y≤12%, and 0.008%≤z≤0.075%.

5. The electrolyte according to any one of claims 1 to 4, wherein R1 and R2 independently include fluorine atoms, trifluoromethyl, pentafluoroethyl, heptafluoropropyl, and nonafluorobutyl; and / or, R3 includes a fluorine atom, a trifluoromethyl group, and a pentafluoroethyl group.

6. The electrolyte according to any one of claims 1 to 5, wherein The first electrolyte salt includes one or more of the following: and / or, The second electrolyte salt includes one or more of the following:

7. The electrolyte according to any one of claims 1 to 6, wherein: M1 includes one or both of Li and Na, and can be selected from Li; and / or, M2 includes one or both of Li and Na, and can be Li.

8. The electrolyte according to any one of claims 1 to 7, wherein: The non-aqueous solvent also includes a chain carbonate; Optionally, the weight content of the linear carbonate in the non-aqueous solvent is denoted as m, and based on the total weight of the non-aqueous solvent, m≥70%; and / or, Optionally, the linear carbonate includes one or more of ethyl methyl carbonate, diethyl carbonate, and dimethyl carbonate.

9. The electrolyte according to any one of claims 1 to 8, wherein: The non-aqueous solvent also includes propylene carbonate, Optionally, the weight content of the propylene carbonate in the non-aqueous solvent is recorded as n, based on the total weight of the non-aqueous solvent, and 0<n≤5%.

10. The electrolyte according to any one of claims 1 to 9, wherein: The electrolyte further comprises a third electrolyte salt represented by formula (3), M3 includes one or more of Li, Na, and K; Optionally, M3 includes one or both of Li and Na, and more preferably Li; and / or, Optionally, the weight content of the third electrolyte salt in the electrolyte is denoted as p, and based on the total weight of the electrolyte, 10%≤y+p≤25%.

11. The electrolyte according to any one of claims 1 to 10, wherein: The electrolyte further comprises a fourth electrolyte salt represented by formula (4), M4 includes one or more of Li, Na, and K; Optionally, M4 includes one or both of Li and Na, and more preferably Li; and / or, Optionally, the weight content of the fourth electrolyte salt in the electrolyte is denoted as q, based on the total weight of the electrolyte, then 0<q≤0.5%, optionally, 0.1%≤q≤0.4%.

12. The electrolyte according to any one of claims 1 to 11, wherein: The electrolyte further comprises an additive, wherein the additive comprises one or two of 1,3-propane sultone and fluoroethylene carbonate. Optionally, the weight content of the additive in the electrolyte is denoted as r, based on the total weight of the electrolyte, then 0<r≤3%.

13. A battery cell comprising a positive electrode sheet, a negative electrode sheet, a separator and the electrolyte according to any one of claims 1 to 12.

14. The battery cell according to claim 13, wherein: The battery cell includes a lithium secondary battery cell.

15. The battery cell according to claim 13 or 14, wherein: The positive electrode sheet includes a first positive electrode active material, the first positive electrode active material includes a general formula of Li a Ni b Co c M d O e A f One or more of lithium transition metal oxides and modified compounds thereof, 0.8≤a≤1.2, 0.8≤b<1, 0<c<0.2, 0<d<0.2, 1≤e≤2, 0≤f≤1, M includes one or more of Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti and B, and A includes one or more of N, F, S and Cl; and / or, The negative electrode plate includes one or more of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials and lithium titanate.

16. A method for preparing a battery cell, comprising the following steps: Providing a battery container including a positive electrode sheet, a negative electrode sheet and a separator; The electrolyte according to any one of claims 1 to 12 is injected into the battery container to obtain a battery cell.

17. A battery, comprising the battery cell according to any one of claims 13 to 15 or the battery cell prepared by the preparation method according to claim 16.

18. An electrical device comprising the battery according to claim 16.

Citation Information

Patent Citations

  • Lithium ion secondary battery

    CN110265721A

  • Lithium ion secondary battery and electronic product comprising same, electric vehicle and mechanical equipment

    CN112909319A

  • Electrolyte, secondary battery and electric equipment

    CN115411363A

  • Lithium ion secondary battery, battery module, battery pack, and electric device

    CN115699388A

  • Non-aqueous electrolyte for high-nickel ternary lithium ion battery and lithium ion battery containing electrolyte

    CN115775918A