Electrolyte solution for lithium secondary battery, secondary battery, and electric device
By adding sulfate ester and difluorophosphate ions to the electrolyte for lithium secondary batteries, the stability and ionic conductivity of the interface film are improved, and the problem of reduced performance after circulation of lithium secondary batteries is solved, achieving better Storage performance and cycle performance.
Patent Information
- Application Number
- PCT/CN2023/097818
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-06-01
- Publication Date
- 2024-12-05
AI Technical Summary
After multiple cycles of existing lithium secondary batteries, the storage performance and circulation performance are significantly reduced, and the DC internal resistance is significantly increased.
An electrolyte for lithium secondary battery is used, which contains sulfate ester and difluorophosphate ions. The molar ratio of sulfate ester to difluorophosphate ions is (0.2-30): 1, and the molar concentration of sulfate ester is 0.04 mol/ L-0.16mol/L, through these ingredients, improves the mechanical and thermal stability of the interface mask, improves ionic conductivity, and reduces DC internal resistance.
It effectively improves the storage performance and circulation performance of lithium secondary batteries, reduces DC internal resistance, and extends the service life of the battery.
Smart Images

Figure CN2023097818_05122024_PF_FP_ABST
Abstract
Description
Electrolyte for lithium secondary batteries, secondary batteries and electrical equipment Technical Field
[0001] The present application relates to the technical field of secondary batteries, and in particular to an electrolyte for a lithium secondary battery, a secondary battery, and an electrical device. Background Art
[0002] Secondary batteries are not only used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, but are also widely used in electric vehicles such as electric bicycles, electric motorcycles, electric cars, as well as in military equipment, aerospace and other fields.
[0003] However, after multiple cycles, the storage performance and cycle performance of existing secondary batteries will be significantly reduced, and the DC internal resistance will also be significantly increased.
[0004] Public content
[0005] In view of the technical problems existing in the background technology, the present application provides an electrolyte for lithium secondary batteries, aiming to solve the problem that the storage performance and cycle performance of secondary batteries containing the electrolyte are significantly reduced and the DC internal resistance is significantly increased after multiple cycles.
[0006] In order to achieve the above-mentioned purpose, the first aspect of the present application provides an electrolyte for a lithium secondary battery, wherein the electrolyte for a lithium secondary battery comprises sulfate and difluorophosphate ions, the molar ratio of the sulfate to the difluorophosphate ions is (0.2-30):1, and the molar concentration of the sulfate is 0.04 mol / L-0.16 mol / L.
[0007] The present application includes at least the following beneficial effects: adding sulfate and difluorophosphate ions to the electrolyte for lithium secondary batteries, and the electrolyte including sulfate and difluorophosphate ions in the above-mentioned ratio, and sulfate at the above-mentioned concentration, can not only improve the mechanical stability of the interface film, but also change the solvation structure of the electrolyte, so that more alkali metal ions participate in film formation, improve the ionic conductivity of the interface film, and furthermore, can also improve the thermal stability of the interface film. Thus, the simultaneous use of sulfate and difluorophosphate ions can reduce the DC internal resistance of the secondary battery and improve the storage performance and cycle performance of the battery.
[0008] In some embodiments of the present application, the molar ratio of the sulfate ester to the difluorophosphate ion is (2.5-10): 1. This can reduce the DC internal resistance of the secondary battery and improve the storage performance and cycle performance of the secondary battery.
[0009] In some embodiments of the present application, the molar concentration of the sulfate ester in the lithium secondary battery electrolyte is 0.05 mol / L-0.1 mol / L. Thus, the molar concentration of the sulfate ester in the electrolyte within the above range can improve the cycle performance of the secondary battery.
[0010] In some embodiments of the present application, the molar concentration of difluorophosphate ions in the lithium secondary battery electrolyte is 0.01 mol / L-0.04 mol / L, and optionally 0.01 mol / L-0.02 mol / L. Thus, a molar concentration of difluorophosphate ions in the electrolyte within the above range can reduce the DC internal resistance of the battery and improve the storage performance of the secondary battery.
[0011] In some embodiments of the present application, the sulfate ester includes at least one of vinyl sulfate, 4-methyl vinyl sulfate, 4-fluorovinyl sulfate, 4-n-propyl vinyl sulfate and 4,4'-disulfate.
[0012] In some embodiments of the present application, the difluorophosphate ion is the following substance: APO2F2, wherein A includes at least one of Li, Na, K and H.
[0013] In some embodiments of the present application, the lithium secondary battery electrolyte further includes a positive electrode film-forming additive, whereby the positive electrode film-forming additive can participate in forming an interface film on the positive electrode surface of the battery, thereby improving the storage performance and cycle performance of the battery.
[0014] In some embodiments of the present application, the cathode film-forming additive includes at least one of fluoroethylene carbonate and 1,3-propane sultone. Thus, the cathode film-forming additive, which includes at least one of the aforementioned substances, can participate in forming an interface film on the surface of the secondary battery's positive electrode, thereby improving the secondary battery's storage performance and cycling performance.
[0015] In some embodiments of the present application, in the lithium secondary battery electrolyte, the ratio of the molar amount of the positive electrode film-forming additive to the sum of the molar amounts of the sulfate ester and difluorophosphate ions is (0.05-0.6):1, and can optionally be (0.1-0.4):1. Thus, when the ratio of the molar amount of the positive electrode film-forming additive to the sum of the molar amounts of the sulfate ester and difluorophosphate ions in the electrolyte is within the above range, the electrolyte can participate in forming an interface film on the surface of the positive electrode of the secondary battery, thereby improving the storage performance and cycle performance of the secondary battery.
[0016] In some embodiments of the present application, the molar concentration of the positive electrode film-forming additive in the lithium secondary battery electrolyte is 0.01 mol / L-0.03 mol / L. Thus, the concentration of the positive electrode film-forming additive in the electrolyte within the above range can participate in the formation of an interface film on the surface of the positive electrode of the secondary battery, thereby improving the storage performance and cycle performance of the secondary battery.
[0017] In some embodiments of the present application, the lithium secondary battery electrolyte further comprises tetrafluoroborate ions. Thus, the tetrafluoroborate ions are compatible with the battery electrolyte system, can participate in the formation of the secondary battery negative electrode interface film, and can reduce the DC internal resistance of the secondary battery.
[0018] In some embodiments of the present application, in the lithium secondary battery electrolyte, the ratio of the molar amount of the tetrafluoroborate ion to the sum of the molar amounts of the sulfate and difluorophosphate ions is (0.02-0.17):1, and can optionally be (0.05-0.1):1. Thus, when the ratio of the molar amount of the tetrafluoroborate ion to the sum of the molar amounts of the sulfate and difluorophosphate ions in the electrolyte is within the above range, the electrolyte can participate in the formation of the negative electrode interface film of the secondary battery, reduce the DC internal resistance of the secondary battery, and improve the storage performance and cycle performance of the secondary battery.
[0019] In some embodiments of the present application, the molar concentration of tetrafluoroborate ions in the lithium secondary battery electrolyte is (0.0025-0.02):1, and can optionally be (0.007-0.017):1. Thus, the molar concentration of tetrafluoroborate ions in the electrolyte within the above range can participate in the formation of the secondary battery negative electrode interface film, thereby reducing the DC internal resistance of the secondary battery.
[0020] In some embodiments of the present application, the tetrafluoroborate ions are provided by at least one of the following substances: at least one of tetrafluoroboric acid, sodium tetrafluoroborate, potassium tetrafluoroborate and lithium tetrafluoroborate.
[0021] In some embodiments of the present application, the water content of the lithium secondary battery electrolyte is less than or equal to 20 ppm. Therefore, the water content of the electrolyte within the above range can reduce water damage to the interfacial membrane, especially at high voltages, thereby improving the storage performance and cycle performance of the secondary battery.
[0022] In some embodiments of the present application, the HF content in the lithium secondary battery electrolyte is less than or equal to 150 ppm. Therefore, the HF content in the electrolyte within the above range can reduce HF damage to the interface film, especially at high voltages, thereby improving the storage performance and cycle performance of the secondary battery.
[0023] The second aspect of the present application provides a secondary battery comprising the electrolyte for lithium secondary batteries according to the first aspect of the present application, thereby providing the secondary battery with low DC internal resistance and excellent storage performance and cycle performance.
[0024] In some embodiments of the present application, the secondary battery includes a positive electrode active material, and the positive electrode active material includes Li x Ni (1-y-z) Co y M z O 2-b , wherein M includes at least one of Mn, Al, Fe, Ti, Mg, Cr, Ga, Cu, Zn, Nb and Zr, 0<x≤1.2, 0.05≤y≤0.8, 0.01≤z≤0.5, 0≤b≤0.2.
[0025] In some embodiments of the present application, the BET specific surface area of the positive electrode active material is less than or equal to 3 m 2 / g, optionally, the BET specific surface area of the positive electrode active material is 1m 2 / g-2.5m 2 / g.
[0026] A third aspect of the present application provides an electrical device, which includes the secondary battery described in the second aspect.
[0027] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become obvious from the description below, or will be learned through practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Various other advantages and benefits will become apparent to those skilled in the art upon reading the detailed description of the preferred embodiment below. The accompanying drawings are for illustration purposes only and are not to be considered as limiting the present application. The same reference numerals are used throughout the drawings to represent the same components. In the drawings:
[0029] FIG1 is a schematic structural diagram of a secondary battery according to an embodiment of the present application;
[0030] FIG2 is a schematic structural diagram of a battery module according to an embodiment of the present application;
[0031] FIG3 is a schematic structural diagram of a battery pack according to an embodiment of the present application;
[0032] FIG4 is an exploded view of FIG3 ;
[0033] FIG5 is a schematic diagram of an embodiment of an electric device using a battery as a power source.
[0034] Explanation of reference numerals: 1: secondary battery; 2: battery module; 3: battery pack; 4: upper case; 5: lower case. DETAILED DESCRIPTION
[0035] The following embodiments of the technical solution of the present application are described in detail. The following embodiments are only used to more clearly illustrate the technical solution of the present application and are therefore only used as examples and are not intended to limit the scope of protection of the present application.
[0036] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0037] For the sake of clarity, only some numerical ranges are specifically disclosed herein. However, any lower limit may be combined with any upper limit to form an unspecified range; and any lower limit may be combined with other lower limits to form an unspecified range, and similarly, any upper limit may be combined with any other upper limit to form an unspecified range. In addition, each individually disclosed point or single value may itself serve as a lower limit or upper limit and be combined with any other point or single value, or with other lower limits or upper limits, to form an unspecified range.
[0038] In the description of the embodiments of this application, the term "and / or" is simply a description of the association relationship between associated objects, indicating that three relationships can exist. For example, A and / or B can represent the following three situations: A exists alone, A and B exist simultaneously, and B exists alone. In addition, the character " / " in this document generally indicates that the associated objects are in an "or" relationship.
[0039] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned figure descriptions are intended to cover non-exclusive inclusions.
[0040] Secondary batteries are not only used in energy storage systems such as hydropower, thermal, wind, and solar power plants, but are also widely used in electric vehicles such as electric bicycles, electric motorcycles, and electric cars, as well as in military equipment and aerospace. As the application of power batteries continues to expand, their market demand is also growing.
[0041] During the initial charge and discharge process of a secondary battery, the electrode material (such as the negative electrode active material) reacts with the electrolyte at the solid-liquid interface, forming a passivation layer covering the surface of the electrode material. This passivation layer is an interfacial film that has the characteristics of a solid electrolyte: an electronic insulator but an excellent conductor of alkali metal ions. Alkali metal ions can freely embed and de-embedding through this passivation layer, hence the name "positive-negative electrode interface film."
[0042] However, existing secondary batteries have the following problems: on the one hand, as the secondary battery is charged and discharged, the interface film at the positive and negative electrode interfaces becomes unstable and easily damaged, and the transmission resistance of alkali metal ions also increases, thereby increasing the DC impedance of the secondary battery and deteriorating the storage performance and cycle performance; on the other hand, when the secondary battery is charged and discharged, under high temperature and high pressure, the positive electrode active material has strong oxidizing properties, which will oxidize the electrolyte and react to generate a large amount of gas, causing the loss of electrolyte and positive electrode active material, affecting the storage performance and cycle performance of the secondary battery.
[0043] In the present application, sulfate and difluorophosphate ions are added to the electrolyte, and the electrolyte includes sulfate and difluorophosphate ions in the above-mentioned proportion, as well as sulfate at the above-mentioned concentration, which can not only improve the mechanical stability of the interface film, but also change the solvation structure of the electrolyte, so that more alkali metal ions participate in film formation, and improve the ionic conductivity of the interface film. In addition, the thermal stability of the interface film can also be improved. In this way, the simultaneous use of sulfate and difluorophosphate ions can reduce the DC internal resistance of the battery and improve the storage performance and cycle performance of the battery. On the other hand, the interface film has thermal stability and mechanical stability, which can reduce the probability of interface film rupture, thereby reducing the reaction between the positive electrode active material and the electrolyte, inhibiting the gas production of the battery, reducing the loss of electrolyte and positive electrode active material, and improving the storage performance and cycle performance of the secondary battery.
[0044] The positive electrode active material disclosed in the embodiments of the present application is suitable for secondary batteries, and the battery disclosed in the embodiments of the present application can be used in electrical devices that use batteries as power sources or various energy storage systems that use batteries as energy storage elements. Electrical devices may include but are not limited to mobile phones, tablets, laptops, electric toys, power tools, battery cars, electric cars, ships, spacecraft, etc. Among them, electric toys may include fixed or mobile electric toys, for example, game consoles, electric car toys, electric ship toys and electric airplane toys, etc., and spacecraft may include airplanes, rockets, space shuttles and spacecraft, etc.
[0045] In a first aspect, the present application provides an electrolyte for a lithium secondary battery, comprising sulfate and difluorophosphate ions, wherein the molar ratio of the sulfate to the difluorophosphate ions is (0.2-30):1, and the molar concentration of the sulfate is 0.04 mol / L-0.16 mol / L.
[0046] The present application includes at least the following beneficial effects: adding sulfate and difluorophosphate ions to the electrolyte, and the electrolyte including sulfate and difluorophosphate ions in the above-mentioned proportion, and sulfate at the above-mentioned concentration, can not only improve the mechanical stability of the interface film, but also change the solvation structure of the electrolyte, so that more alkali metal ions participate in film formation, improve the ionic conductivity of the interface film, and furthermore, can also improve the thermal stability of the interface film. Thus, the simultaneous use of sulfate and difluorophosphate ions can reduce the DC internal resistance of the secondary battery and improve the storage performance and cycle performance of the battery.
[0047] Direct current internal resistance (DCR) refers to the resistance to current flow within a battery cell. After a secondary battery's discharge cycle, polarization causes the battery voltage to rebound. DC impedance technology calculates the battery's internal resistance by measuring the difference between the voltage immediately before the end of intermittent discharge and the voltage after the battery stabilizes.
[0048] In some embodiments of the present application, the sulfate ester may include at least one of vinyl sulfate, 4-methyl vinyl sulfate, 4-fluorovinyl sulfate, 4-n-propyl vinyl sulfate, and 4,4'-vinyl bisulfate. Thus, by using the above-mentioned sulfate esters in the electrolyte of the present application, they can participate in the formation of the positive and negative electrode interface film, making the interface film flexible, adapting to the expansion and contraction of the battery pole pieces during the cycle, improving the mechanical stability of the interface film, and thus improving the cycle performance of the battery. In other embodiments of the present application, the sulfate ester includes 4,4'-vinyl bisulfate.
[0049] In some embodiments of the present application, the difluorophosphate ion is a substance comprising the following: APO2F2, wherein A comprises at least one of Li, Na, K, and H. Specifically, the substance containing difluorophosphate ions can provide difluorophosphate ions, change the solvation structure of the electrolyte, allow more alkali metal ions to participate in film formation, improve the ionic conductivity of the interface film, and improve the transport resistance of the alkali metal ions. In addition, the difluorophosphate ions can also participate in the formation of the positive and negative electrode interface films, enhance the thermal stability of the interface films, thereby reducing the DC impedance of the secondary battery while improving the storage performance of the battery.
[0050] In some embodiments of the present application, the molar ratio of the sulfate ester to the difluorophosphate ion can be (0.2-29):1, (1-28):1, (2-27):1, (3-26):1, (4-25):1, (5-24):1, (6-23):1, (10-20):1, (12-19):1, (15-17):1, etc. In other embodiments of the present application, the molar ratio of the sulfate ester to the difluorophosphate ion is (10-20):1. Specifically, when the molar ratio of the sulfate ester to the difluorophosphate ion is within the above range, the excessive thickness of the interfacial film caused by excessive sulfate ester can be reduced, resulting in deteriorated ion transport, thereby reducing the DC internal resistance of the secondary battery. It can also reduce the defects of insufficient interfacial film formation and poor stability caused by too little sulfate ester, thereby improving the storage performance and cycle performance of the secondary battery.
[0051] In some embodiments of the present application, in the lithium secondary battery electrolyte, the molar concentration of the sulfate ester is 0.04mol / L-0.16mol / L. For example, in the lithium secondary battery electrolyte, the molar concentration of the sulfate ester can be 0.04mol / L-0.15mol / L, 0.05mol / L-0.14mol / L, 0.06mol / L-0.13mol / L, 0.07mol / L-0.12mol / L, 0.08mol / L-0.11mol / L, 0.09mol / L-0.1mol / L, etc. Thus, the molar concentration of the sulfate ester in the electrolyte is within the above range, which can reduce the probability of excessive film formation at the positive and negative electrode interface films, thereby reducing the DC internal resistance of the secondary battery, while being sufficient to improve the mechanical stability of the interface film, thereby improving the cycle performance of the secondary battery. In other embodiments of the present application, in the lithium secondary battery electrolyte, the molar concentration of the sulfate ester is 0.05mol / L-0.1mol / L.
[0052] In some embodiments of the present application, in the electrolyte for the lithium secondary battery, the molar concentration of the difluorophosphate ions is 0.01mol / L-0.04mol / L. For example, the molar concentration of the difluorophosphate ions in the electrolyte can be 0.01mol / L-0.03mol / L, 0.01mol / L-0.02mol / L, 0.02mol / L-0.03mol / L, etc. Specifically, the molar concentration of the difluorophosphate ions in the electrolyte is within the above range, which can reduce the problem of increased viscosity of the electrolyte caused by the addition of substances containing difluorophosphate ions, thereby reducing the DC internal resistance of the secondary battery, while being sufficient to improve the thermal stability of the interface film and improve the storage performance of the secondary battery. In other embodiments of the present application, in the electrolyte for the lithium secondary battery, the molar concentration of the difluorophosphate ions is 0.01mol / L-0.02mol / L.
[0053] In some embodiments of the present application, the lithium secondary battery electrolyte may further include a positive electrode film-forming additive. Specifically, the positive electrode film-forming additive may promote the formation of a stable interface film on the positive electrode surface of the battery, reduce the DC impedance of the battery, and improve the cycle performance of the secondary battery.
[0054] In some embodiments of the present application, the cathode film-forming additive may include at least one of fluoroethylene carbonate and 1,3-propane sultone. Specifically, the cathode interface film formed with fluoroethylene carbonate and 1,3-propane sultone exhibits excellent performance, forming a tight interface film without increasing impedance. This interface film can prevent electrolyte decomposition, reduce the battery's DC internal resistance, and improve the storage and cycling performance of the secondary battery.
[0055] In some embodiments of the present application, in the electrolyte for the lithium secondary battery, the ratio of the molar amount of the positive electrode film-forming additive to the sum of the molar amounts of the sulfate and difluorophosphate ions is (0.05-0.6):1. For example, the ratio of the molar amount of the positive electrode film-forming additive to the sum of the molar amounts of the sulfate and difluorophosphate ions can be (0.05-0.55):1, (0.1-0.5):1, (0.15-0.45):1, (0.2-0.4):1, (0.25-0.35):1, (0.3-0.32):1, etc. Thus, the ratio of the molar amount of the positive electrode film-forming additive to the sum of the molar amounts of sulfate and difluorophosphate ions in the lithium secondary battery electrolyte is within the above range, which not only reduces the effect of the excess amount of the positive electrode film-forming additive on the sulfate and difluorophosphate ions, thereby increasing the DC impedance of the battery, but also reduces the effect of the positive electrode film-forming additive being unable to participate in the positive electrode film formation due to the excess amount of the positive electrode film-forming additive. This can reduce the DC internal resistance of the secondary battery and improve the storage performance and cycle performance of the secondary battery. In other embodiments of the present application, in the lithium secondary battery electrolyte, the ratio of the molar amount of the positive electrode film-forming additive to the sum of the molar amounts of sulfate and difluorophosphate ions is (0.1-0.4):1.
[0056] In some embodiments of the present application, in the electrolyte for lithium secondary batteries, the molar concentration of the positive electrode film-forming additive is 0.01mol / L-0.03mol / L. For example, in the electrolyte for lithium secondary batteries, the molar concentration of the positive electrode film-forming additive may be 0.01mol / L-0.025mol / L, 0.013mol / L-0.024mol / L, 0.015mol / L-0.023mol / L, 0.018mol / L-0.02mol / L, etc. Thus, when the concentration of the positive electrode film-forming additive in the electrolyte is within the above range, the increase in the DC impedance of the secondary battery caused by an excessive amount of the positive electrode film-forming additive is reduced, and the inability of the positive electrode film-forming additive to participate in the positive electrode film formation due to an insufficient amount of the positive electrode film-forming additive is reduced, thereby reducing the DC internal resistance of the secondary battery and improving the storage performance and cycle performance of the secondary battery.
[0057] In some embodiments of the present application, the lithium secondary battery electrolyte further comprises tetrafluoroborate ions. Tetrafluoroborate ions are compatible with the lithium secondary battery electrolyte system and can participate in forming the negative electrode interface film of the battery, opening up ion channels and reducing the DC internal resistance of the secondary battery.
[0058] In some embodiments of the present application, the substance containing the tetrafluoroborate ion may be at least one of tetrafluoroboric acid, sodium tetrafluoroborate, potassium tetrafluoroborate and lithium tetrafluoroborate.
[0059] In some embodiments of the present application, in the lithium secondary battery electrolyte, the ratio of the molar amount of the tetrafluoroborate ion to the sum of the molar amounts of the sulfate and difluorophosphate ions is (0.0025-0.02):1. For example, the ratio of the molar amount of the tetrafluoroborate ion to the sum of the molar amounts of the sulfate and difluorophosphate ions can be (0.0025-0.019):1, (0.005-0.015):1, (0.008-0.014):1, (0.01-0.013):1, (0.011-0.012):1, etc. Thus, the ratio of the molar amount of tetrafluoroborate ions to the molar amount of sulfate and difluorophosphate ions in the lithium secondary battery electrolyte is within the above range, which not only reduces the effect of excessive tetrafluoroborate ions on sulfate and difluorophosphate ions, thereby increasing the DC impedance of the secondary battery, but also reduces the effect of too little tetrafluoroborate ions on the negative electrode film formation, thereby reducing the DC internal resistance of the battery and improving the storage performance and cycle performance of the secondary battery. In other embodiments of the present application, in the lithium secondary battery electrolyte, the ratio of the molar amount of tetrafluoroborate ions to the molar amount of sulfate and difluorophosphate ions is (0.007-0.017):1.
[0060] In some embodiments of the present application, in the lithium secondary battery electrolyte, the molar concentration of the tetrafluoroborate ion is 0.0005mol / L-0.001mol / L, for example, in the electrolyte, the molar concentration of the tetrafluoroborate ion can be 0.0005mol / L-0.0009mol / L, 0.0006mol / L-0.0008mol / L, 0.0007mol / L-0.0008mol / L, etc. Thus, the molar concentration of the tetrafluoroborate ion in the electrolyte is within the above range, which reduces the deterioration of the battery DC impedance caused by excessive tetrafluoroborate ions, while allowing the tetrafluoroborate ions to play a role in participating in the negative electrode film formation, thereby reducing the DC internal resistance of the secondary battery and improving the storage performance and cycle performance of the secondary battery. In other embodiments of the present application, in the lithium secondary battery electrolyte, the molar concentration of the tetrafluoroborate ion is 0.0008mol / L-0.001mol / L.
[0061] In some embodiments of the present application, the water content in the electrolyte for the lithium secondary battery is less than or equal to 20 ppm. For example, the water content in the electrolyte can be 1 ppm-19 ppm, 2 ppm-18 ppm, 3 ppm-17 ppm, 4 ppm-16 ppm, 5 ppm-15 ppm, 6 ppm-14 ppm, 7 ppm-13 ppm, 8 ppm-12 ppm, 9 ppm-11 ppm, etc. Therefore, when the water content in the electrolyte is within the above range, it can reduce the damage of water to the battery interface membrane, especially at high voltage, which can reduce the DC internal resistance of the secondary battery and improve the storage performance and cycle performance of the secondary battery.
[0062] In some embodiments of the present application, the HF content in the lithium secondary battery electrolyte is less than or equal to 150 ppm. For example, the HF content in the electrolyte can be 10 ppm-140 ppm, 20 ppm-130 ppm, 30 ppm-120 ppm, 40 ppm-110 ppm, 50 ppm-100 ppm, 60 ppm-90 ppm, 70 ppm-80 ppm, etc. Therefore, when the HF content in the electrolyte is within the above range, the damage caused by HF to the battery interface film can be reduced, especially at high voltage, which can reduce the DC internal resistance of the secondary battery and improve the storage performance and cycle performance of the secondary battery.
[0063] It is understandable that the control of the water content and HF content in the electrolyte for lithium secondary batteries can be achieved by removing water using molecular sieves. Specifically, molecular sieves can be added to the electrolyte for lithium secondary batteries to ensure full contact between the molecular sieve and the electrolyte, thereby adsorbing water and HF in the electrolyte. The molecular sieve and the electrolyte can then be separated by filtration, centrifugation, etc.
[0064] It is understood that the water content and HF content in the electrolyte can be measured by the following method:
[0065] Testing of water content in electrolyte for lithium secondary batteries
[0066] The electrolyte is injected into the electrolytic cell to reach equilibrium. After the indicator electrode detects H2O, electrode oxidation occurs. - I2 is a quantitative chemical reaction between I2 and H2O, so the water content is calculated. According to HG / T4067-2015 Determination of Water in Hexafluorophosphate Electrolyte 5.9, the quantitative reaction formula of I2 and H2O is: H2O+I2+SO2+3C5H5N=2C5H5N·HI+C5H5N·SO3. The amount of water is calculated by the amount of iodine consumed.
[0067] Test of hydrofluoric acid content in electrolyte
[0068] In a dry environment, the free acid in the electrolyte is titrated with a standard triethylamine solution and calculated based on the HF content;
[0069] HG / T4067-2015 Lithium hexafluorophosphate electrolyte 5.10 Determination of free acid content;
[0070] HF(ppm)=(V2-V1) / 1000×C×20 / m×1000000=(V2-V1)×C / m×20000;
[0071] Where: 0.01——concentration of standard solution, 0.02mol / L;
[0072] V1 - the volume reading of the burette before starting the titration, ml;
[0073] V2——The volume reading of the burette after adding the electrolyte sample and titrating to the endpoint, ml;
[0074] 20 – molar molecular weight of HF, g / mol;
[0075] m——the amount of electrolyte weighed, g;
[0076] 20000——The coefficient for conversion to ug / g.
[0077] In some embodiments of the present application, the electrolyte for a lithium secondary battery may further include an electrolyte salt and a solvent.
[0078] As an example, the electrolyte salt may include at least one of lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium bisoxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobisoxalatophosphate (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).
[0079] As an example, the solvent may include at least one of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).
[0080] In some embodiments, the electrolyte for lithium secondary batteries may further include additives. For example, the additives may include additives that can improve certain battery properties, such as additives that improve the secondary battery's overcharge performance, additives that improve the battery's high-temperature performance, and additives that improve the secondary battery's low-temperature performance.
[0081] The second aspect of the present application provides a secondary battery comprising the electrolyte for lithium secondary batteries according to the first aspect of the present application, thereby providing the secondary battery with low DC internal resistance, excellent storage performance and cycle performance.
[0082] A battery is a battery that can be recharged to activate the active materials after discharge and continue to be used.
[0083] Typically, a battery consists of a positive electrode, a negative electrode, a separator, and an electrolyte. During the battery's charge and discharge processes, active ions (alkali metal ions) are inserted and removed between the positive and negative electrodes. The separator is placed between the positive and negative electrodes to isolate them. The electrolyte conducts ions between the positive and negative electrodes.
[0084] In an embodiment of the present application, the battery includes a lithium-ion battery.
[0085] [Positive electrode]
[0086] In a battery, the positive electrode sheet generally includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, wherein the positive electrode active material layer includes a positive electrode active material.
[0087] The positive electrode current collector may be a conventional metal foil or a composite current collector (a metal material may be disposed on a polymer substrate to form a composite current collector). As an example, the positive electrode current collector may be an aluminum foil.
[0088] The specific type of the positive electrode active material is not limited, and any active material known in the art that can be used for a positive electrode of a battery can be used, and those skilled in the art can select it according to actual needs.
[0089] The positive electrode active material may include, but is not limited to, at least one of a lithium transition metal oxide, an olivine-structured lithium-containing phosphate, and their respective modified compounds. Examples of lithium transition metal oxides may include, but are not limited to, at least one of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, a composite material of lithium iron manganese phosphate and carbon, and their modified compounds. These materials can all be obtained through commercial channels.
[0090] In some embodiments of the present application, the positive electrode active material includes Li x Ni (1-y-z) Co y M z O 2-b , wherein M includes at least one of Mn, Al, Fe, Ti, Mg, Cr, Ga, Cu, Zn, Nb and Zr, 0<x≤1.2, 0.05≤y≤0.8, 0.01≤z≤0.5, 0≤b≤0.2.
[0091] For example, x can satisfy: 0.2≤x≤1.2, 0.4≤x≤1.1, 0.5≤x≤1.0, 0.6≤x≤0.9, 0.7≤x≤0.8, etc.; y can satisfy: 0.05≤y≤0.7, 0.1≤y≤0.6, 0.2≤y≤0.5, 0.3≤y≤0.4, etc.; z can satisfy: 0.01≤z≤0.45, 0.1≤z≤0.4, 0.2≤z≤0.3, etc.; b can satisfy: 0≤b≤0.15, 0.02≤b≤0.13, 0.05≤b≤0.1, 0.07≤b≤0.09, etc.
[0092] It should be noted that in the positive electrode sheet, battery, or electrical device, lithium ions are consumed during the battery formation and cycling processes, so the measured lithium content x in the positive electrode active material may be less than 1. Furthermore, if a lithium supplement is used in the positive and negative electrode sheets, the measured lithium content x in the positive electrode active material may be greater than 1 after the battery formation and cycling processes.
[0093] In addition, as the battery undergoes processes such as formation and cycling, the positive electrode active material may release oxygen from the lattice, causing oxygen loss. Therefore, the oxygen content in the positive electrode active material may be less than 2.
[0094] In some embodiments of the present application, the BET specific surface area of the positive electrode active material is less than or equal to 3 m 2 / g, for example, the BET specific surface area of the positive electrode active material can be 0.3 m 2 / g-3m 2 / g,1m 2 / g-2.5m 2 / g,1.2m 2 / g-2.3m 2 / g,1.5m 2 / g-2m 2 / g, etc. Specifically, the BET specific surface area of the positive electrode active material is within the above range, which can reduce the side reaction of the positive electrode active material under high voltage and improve the storage performance and cycle performance of the battery. In other embodiments of the present application, the BET specific surface area of the positive electrode active material is 1m 2 / g-2.5m 2 / g.
[0095] It can be understood that the BET specific surface area of the positive electrode active material can be tested by referring to the following method: using the American Micrometer multi-station fully automatic specific surface area and pore analyzer GeminiVII2390, take about 7g of sample and put it into a 9cc long tube with a bulb, degas at 200℃ for 2h, and then put it into the host to test to obtain the BET (specific surface area) data of the positive electrode active material.
[0096] The positive electrode active material layer may also optionally include a binder, a conductive agent, and other optional auxiliary agents.
[0097] As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, Super P (SP), graphene, and carbon nanofibers.
[0098] As an example, the binder may include at least one of styrene-butadiene rubber (SBR), water-based acrylic resin, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyacrylic acid (PAA), carboxymethyl cellulose (CMC), polyvinyl alcohol (PVA), and polyvinyl butyral (PVB).
[0099] [Negative electrode]
[0100] In a battery, the negative electrode sheet generally includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, wherein the negative electrode active material layer includes a negative electrode active material.
[0101] The negative electrode current collector may be a conventional metal foil or a composite current collector (for example, a metal material may be disposed on a polymer substrate to form a composite current collector). As an example, the negative electrode current collector may be a copper foil.
[0102] The specific type of the negative electrode active material is not limited, and active materials that can be used for the negative electrode of the battery known in the art can be used, and those skilled in the art can choose according to actual needs. As an example, the negative electrode active material may include but is not limited to at least one of artificial graphite, natural graphite, hard carbon, soft carbon, silicon-based materials and tin-based materials. The silicon-based material may include at least one of elemental silicon, silicon oxide (such as silicon monoxide), silicon-carbon composite, silicon-nitrogen composite, and silicon alloy. The tin-based material may include at least one of elemental tin, tin oxide, and tin alloy. These materials can be obtained through commercial channels.
[0103] In some embodiments, to further improve the energy density of the battery, the negative electrode active material may include a silicon-based material.
[0104] The negative electrode active material layer may also optionally include a binder, a conductive agent, and other optional auxiliary agents.
[0105] As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0106] As an example, the binder may include at least one of styrene-butadiene rubber (SBR), water-based acrylic resin, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyvinyl alcohol (PVA), and polyvinyl butyral (PVB).
[0107] As examples, other optional additives may include thickening and dispersing agents (eg, sodium carboxymethyl cellulose CMC-Na), and PTC thermistor materials.
[0108] As the above-mentioned isolation membrane, the present application has no special restrictions and any known porous structure isolation membrane with electrochemical stability and mechanical stability can be selected according to actual needs. For example, it can include a single-layer or multi-layer film containing at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride.
[0109] The embodiment of the present application has no particular limitation on the shape of the battery, which can be cylindrical, square or any other shape. FIG1 shows a square battery 1 as an example.
[0110] In some embodiments, the battery may include an outer packaging for encapsulating the positive electrode sheet, the negative electrode sheet, and the electrolyte.
[0111] In some embodiments, the outer packaging may include a housing and a cover. The housing may include a bottom plate and side plates connected to the bottom plate, with the bottom plate and side plates enclosing a receiving cavity. The housing may have an opening communicating with the receiving cavity, and the cover may be positioned over the opening to seal the receiving cavity.
[0112] The positive electrode sheet, negative electrode sheet, and separator can be wound or laminated to form an electrode assembly. The electrode assembly is encapsulated in the housing. The number of electrode assemblies in a battery can be one or more, adjustable based on demand.
[0113] In some embodiments, the outer packaging of the battery may be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell.
[0114] The outer packaging of the battery may also be a soft bag, such as a bag-type soft bag. The material of the soft bag may be plastic, such as at least one of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0115] In some embodiments, batteries may be assembled into a battery module. The battery module may contain multiple batteries, and the specific number may be adjusted according to the application and capacity of the battery module.
[0116] Figure 2 shows an example battery module 2. Referring to Figure 2 , within the battery module 2, multiple batteries 1 may be arranged sequentially along the length of the battery module 2. Of course, any other arrangement is also possible. Furthermore, the multiple batteries 1 may be secured together using fasteners.
[0117] The battery module 2 may further include a housing having a housing space, wherein the housing space accommodates a plurality of secondary batteries 1. In some embodiments, the battery modules may be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0118] Figures 3 and 4 illustrate an example battery pack 3. Referring to Figures 3 and 4 , the battery pack 3 may include a battery box and multiple battery modules 2 disposed within the battery box. The battery box comprises an upper case 4 and a lower case 5. The upper case 4 can be placed over the lower case 5 to form an enclosed space for accommodating the battery modules 2. The multiple battery modules 2 can be arranged in any manner within the battery box.
[0119] In a third aspect, the present application provides an electrical device comprising the secondary battery described in the second aspect. Specifically, the secondary battery can serve as a power source for the electrical device or as an energy storage unit for the electrical device. The electrical device may include, but is not limited to, mobile devices (e.g., mobile phones, laptops), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks), electric trains, ships, satellites, and energy storage systems.
[0120] FIG5 shows an example of an electric device, which includes a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle.
[0121] As another example, electric devices may include mobile phones, tablet computers, and laptop computers. These electric devices are generally required to be lightweight and thin, and may use batteries as power sources.
[0122] In order to make the technical problems, technical solutions and beneficial effects solved by the embodiments of the present application clearer, the following will be further described in detail with reference to the embodiments and drawings. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is in no way intended to limit the present application and its applications. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0123] Example 1
[0124] Preparation of secondary battery containing electrolyte for lithium secondary battery
[0125] 1. Preparation of electrolyte for lithium secondary batteries
[0126] Ethylene carbonate (EC) and ethyl methyl carbonate (EMC) are mixed in a mass ratio of 30:70 to obtain an organic solvent, and fully dried electrolyte salt LiPF6, sulfate, lithium difluorophosphate, positive electrode film-forming additive and lithium tetrafluoroborate are dissolved in the above solvent, and the electrolyte is obtained after mixing evenly.
[0127] Molecular sieves are added to the electrolyte for lithium secondary batteries to allow the molecular sieves to fully contact the electrolyte and adsorb water and HF in the electrolyte. The molecular sieves are then filtered to separate the molecular sieves and the electrolyte, removing water and HF in the electrolyte.
[0128] 2. Preparation of secondary batteries
[0129] Preparation of positive electrode
[0130] The positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811), conductive agent carbon black (Super P), and binder polyvinylidene fluoride (PVDF) are mixed evenly in an appropriate amount of solvent N-methylpyrrolidone (NMP) in a mass ratio of 96.2:2.7:1.1 to obtain a positive electrode slurry. The positive electrode slurry is coated on the positive electrode current collector aluminum foil, and the positive electrode sheet is obtained through drying, cold pressing, slitting, and cutting processes.
[0131] Preparation of negative electrode sheet
[0132] The negative electrode active material artificial graphite, conductive agent carbon black (Super P), binder styrene-butadiene rubber (SBR) and sodium carboxymethyl cellulose (CMC-Na) are mixed evenly in a proper amount of solvent deionized water at a mass ratio of 96.4:0.7:1.8:1.1 to obtain a negative electrode slurry. The negative electrode slurry is coated on the negative electrode current collector copper foil, and the negative electrode sheet is obtained through the processes of drying, cold pressing, slitting and cutting.
[0133] The isolation film is made of polyethylene film.
[0134] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator placed between the positive and negative electrode sheets to serve as an isolation, and then wound to obtain an electrode assembly; the electrode assembly is placed in an outer package, and the above-mentioned electrolyte is injected into the dried battery. After vacuum packaging, standing, formation, and shaping processes, a secondary battery is obtained.
[0135] The secondary batteries of Examples 2-39 and Comparative Examples 1-2 are the same as those of Example 1 except for the different parameters (see Table 1).
[0136] The compositions of the electrolytes for lithium secondary batteries in the secondary batteries of Examples 1-39 and Comparative Examples 1-2 of the present application are shown in Table 1.
[0137] Table 1
[0138] In Table 1, “ / ” means no addition, that is, the addition amount is 0.
[0139] Secondary battery performance test:
[0140] 1. Secondary battery cycle performance
[0141] Taking Example 1 as an example, at 25°C, the secondary battery was charged at a constant current rate of 0.5C to a charge cutoff voltage of 4.2V. It was then charged at a constant voltage to a current of ≤0.05C and allowed to stand for 5 minutes. The battery was then discharged at a constant current rate of 0.33C to a discharge cutoff voltage of 2.8V and allowed to stand for 5 minutes. The discharge capacity (C0) at this point was recorded as the initial capacity of the battery. This method was used to cycle the battery 200 times. The discharge capacity after 200 cycles was recorded as C1, which was the capacity of the battery after 200 cycles.
[0142] Cycle capacity retention rate of secondary battery = C1 / C0×100%
[0143] The test process of the capacity of the secondary batteries of Example 2-39 and Comparative Example 1-2 is the same as above.
[0144] 2. Secondary battery DC internal resistance
[0145] Taking Example 1 as an example, the secondary battery was charged to 4.15 V at a constant current of 1 C at 25° C., then charged at a constant voltage of 4.15 V until the current dropped to 0.05 C, and then discharged to 2.5 V at a constant current of 1 C. After standing for 5 minutes (stabilization time), the next cycle was continued. In each cycle, the battery voltage before discharge termination and the battery voltage after stabilization were recorded, and then the DC impedance R = ΔU / I (where: ΔU is the voltage difference, R is the DC resistance, and I is the discharge current) was calculated using the following formula.
[0146] Battery internal resistance growth rate = (battery internal resistance after 200 cycles - battery initial internal resistance) / battery initial internal resistance × 100%
[0147] The testing process of the DC internal resistance of the secondary batteries of Example 2-39 and Comparative Example 1-2 is the same as above.
[0148] 3. Secondary battery storage performance
[0149] Taking Example 1 as an example, at 25°C, the secondary battery was charged at a constant current rate of 0.5C to a charge cut-off voltage of 4.2V, then charged at a constant voltage to a current ≤ 0.05C, allowed to stand for 5 minutes, and then discharged at a constant current rate of 0.33C to a discharge cut-off voltage of 2.8V, allowed to stand for 5 minutes. The battery discharge capacity C0 at this time was recorded, which was the initial capacity of the battery.
[0150] The test process of the storage performance of the secondary batteries of Examples 2-39 and Comparative Examples 1-2 is the same as above.
[0151] The performance test results of the secondary batteries of various embodiments and comparative examples are shown in Table 2.
[0152] Table 2
[0153] As can be seen from Table 2, in Examples 1-39 of the present application, sulfate and difluorophosphate ions are added to the lithium secondary battery electrolyte, and the electrolyte includes sulfate and difluorophosphate ions in the above ratios and the above concentrations. The simultaneous use of sulfate and difluorophosphate ions can reduce the DC internal resistance of the battery and improve the battery's storage performance and cycle performance. Compared to Examples 1-39, the molar ratio of sulfate to difluorophosphate ions in Comparative Examples 1 and 2 is not within the scope of this application, and the battery's storage performance and cycle performance are significantly reduced, and the DC internal resistance is significantly increased.
[0154] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. An electrolyte for a lithium secondary battery, wherein: The electrolyte for lithium secondary batteries includes sulfate and difluorophosphate ions, the molar ratio of the sulfate to the difluorophosphate ions is (0.2-30):1, and the molar concentration of the sulfate is 0.04 mol / L-0.16 mol / L.
2. The electrolyte for lithium secondary battery according to claim 1, wherein The molar ratio of the sulfate ester to the difluorophosphate ion is (2.5-10):
1.
3. The electrolyte for lithium secondary battery according to claim 1 or 2, wherein In the electrolyte for lithium secondary batteries, the molar concentration of the sulfate ester is 0.05 mol / L-0.1 mol / L.
4. The electrolyte for lithium secondary battery according to any one of claims 1 to 3, wherein In the electrolyte for lithium secondary batteries, the molar concentration of difluorophosphate ions is 0.01 mol / L-0.04 mol / L, and can be optionally 0.01 mol / L-0.02 mol / L.
5. The electrolyte for lithium secondary battery according to any one of claims 1 to 4, wherein The sulfate ester includes at least one of vinyl sulfate, 4-methyl-vinyl sulfate, 4-fluorovinyl sulfate, 4-n-propyl vinyl sulfate, and 4,4'-bis-vinyl sulfate.
6. The electrolyte for lithium secondary battery according to any one of claims 1 to 5, wherein The difluorophosphate ion adopts the following substance: APO2F2, wherein A includes at least one of Li, Na, K and H.
7. The electrolyte for lithium secondary battery according to any one of claims 1 to 6, wherein The electrolyte for lithium secondary batteries further includes a positive electrode film-forming additive.
8. The electrolyte for lithium secondary battery according to claim 7, wherein The positive electrode film-forming additive includes at least one of fluoroethylene carbonate and 1,3-propane sultone.
9. The electrolyte for lithium secondary battery according to claim 7 or 8, wherein In the electrolyte for lithium secondary batteries, the ratio of the molar amount of the positive electrode film-forming additive to the sum of the molar amounts of the sulfate and difluorophosphate ions is (0.05-0.6):1, and can be optionally (0.1-0.4):
1.
10. The electrolyte for lithium secondary battery according to any one of claims 7 to 9, wherein In the electrolyte for lithium secondary batteries, the molar concentration of the positive electrode film-forming additive is 0.01 mol / L-0.03 mol / L.
11. The electrolyte for lithium secondary battery according to any one of claims 1 to 10, wherein The electrolyte for lithium secondary batteries also includes tetrafluoroborate ions.
12. The electrolyte for lithium secondary battery according to claim 11, wherein In the electrolyte for lithium secondary batteries, the ratio of the molar amount of the tetrafluoroborate ions to the sum of the molar amounts of the sulfate and difluorophosphate ions is (0.0025-0.02):1, and can be optionally (0.007-0.017):
1.
13. The electrolyte for lithium secondary battery according to claim 11 or 12, wherein In the electrolyte for lithium secondary batteries, the molar concentration of tetrafluoroborate ions is 0.0005 mol / L-0.001 mol / L, and can be optionally 0.0008 mol / L-0.001 mol / L.
14. The electrolyte for lithium secondary battery according to any one of claims 11 to 13, wherein The tetrafluoroborate ions are provided by at least one of the following substances: at least one of tetrafluoroboric acid, sodium tetrafluoroborate, potassium tetrafluoroborate and lithium tetrafluoroborate.
15. The electrolyte for lithium secondary battery according to any one of claims 1 to 14, wherein The lithium secondary battery electrolyte satisfies at least one of the following conditions: The water content of the electrolyte for lithium secondary battery is less than or equal to 20 ppm; The HF content in the electrolyte for lithium secondary batteries is less than or equal to 150 ppm.
16. A secondary battery, wherein: The secondary battery comprises the electrolyte for a lithium secondary battery according to any one of claims 1 to 15.
17. The secondary battery according to claim 16, wherein The secondary battery includes a positive electrode active material, wherein the positive electrode active material includes Li x Ni (1-y-z) Co y M z O 2-b , wherein M includes at least one of Mn, Al, Fe, Ti, Mg, Cr, Ga, Cu, Zn, Nb and Zr, 0<x≤1.2, 0.05≤y≤0.8, 0.01≤z≤0.5, 0≤b≤0.
2.
18. The secondary battery according to claim 17, wherein The BET specific surface area of the positive electrode active material is less than or equal to 3 m 2 / g, optionally, the BET specific surface area of the positive electrode active material is 1m 2 / g-2.5m 2 / g.
19. An electrical device comprising the secondary battery according to any one of claims 16 to 18.
Citation Information
Patent Citations
High-nickel ternary lithium ion power battery electrolyte and high-nickel ternary lithium ion power battery
CN106058316A
Lithium secondary battery electrolyte and lithium secondary battery
CN107369849A
Electrolyte of lithium ion battery and lithium ion battery
CN111653827A
Lithium ion battery electrolytic solution and lithium ion battery
CN111653829A
Lithium ion battery electrolyte and fast-charging lithium ion battery
CN113036222A