Composite current collector, and manufacturing method therefor and application thereof
By adopting alternately stacked metal layer and intermediate layer structures in the composite fluid, combined with the design of the bonding layer and protective layer, the microcrack spread and large-area fracture of the conductive layer is achieved during the battery needle puncture process, solving the existing technology The problem of limited improvement in battery safety performance has significantly improved the battery safety performance.
Patent Information
- Application Number
- PCT/CN2024/095406
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-05-17
- Filing Date
- 2024-05-27
- Publication Date
- 2024-12-05
AI Technical Summary
The safety performance of existing composite current collectors is limited during the battery acupuncture process, and it is difficult to effectively avoid the positive and negative current collectors conducting to form a closed circuit and the battery thermal runaway.
Using alternate layered metal layers and intermediate layer structures, microcracks are spread during needle puncture, causing the conductive layer to separate from the steel needle, and through the intermediate layer, the metal layer grains are blocked and grains are promoted to renucleation, forming non-penetrating small crystals. The particle, combined with the design of the bonding layer and the protective layer, cooperates to achieve large-area fracture of the conductive layer.
It significantly improves the safety performance of the battery, avoids the conduction of the positive and negative current collector to form a closed circuit and the thermal runaway of the battery, and improves the promotion and application potential of the composite current collector.
Smart Images

Figure CN2024095406_05122024_PF_FP_ABST
Abstract
Description
A composite current collector and its preparation method and application Technical Field
[0001] The present disclosure relates to the field of new energy battery technology, for example, a composite current collector and its preparation method and application. Background Art
[0002] At present, composite current collectors based on polymer films have received widespread attention and application in the new energy industry. The preparation of this composite current collector usually adopts the method of physical vapor deposition (PVD) to deposit a layer of metal on a polymer film (such as polyester, polyolefin, etc.), thereby preparing a composite current collector with good conductivity. Compared with traditional current collectors, composite current collectors based on polymer films have the characteristics of low cost, light weight, and good internal insulation. These characteristics enable the composite current collector to reduce the cost of the battery and improve the energy density and safety of the battery when used in the battery.
[0003] The current composite current collector mainly relies on the insulation and flame retardant properties of the intermediate layer, namely the polymer film layer, to improve the safety of the battery. However, although this improves the safety performance of the battery, the improvement is limited.
[0004] Therefore, providing a current collector structure with high safety performance and without affecting battery performance is a technical problem that needs to be solved urgently.
[0005] Summary of the Invention
[0006] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0007] The present disclosure provides a composite current collector, its preparation method, and application. The composite current collector structure provided by the present disclosure generates microcracks in the conductive layer during the needle puncture process, which rapidly propagate and cause large-scale fractures, thereby separating the conductive layer from the steel needle. This prevents the positive and negative current collectors from conducting to form a closed circuit and the resulting thermal runaway of the battery, thereby significantly improving the safety performance of the battery.
[0008] In a first aspect, the present disclosure provides a composite current collector, comprising a conductive layer, wherein the conductive layer includes alternately stacked metal layers and intermediate layers.
[0009] In some embodiments, microcracks are generated in the conductive layer during the needling process, and the microcracks propagate and cause large-scale fractures, thereby separating the conductive layer from the steel needle.
[0010] The conductive layer disclosed herein may include alternately stacked metal layers and intermediate layers. During the battery puncture test, cracks are prone to form in the intermediate layer and rapidly spread to the surrounding areas, thereby causing large-scale fractures and fragmentation of the adjacent metal layers, thereby achieving separation of the conductive layer from the steel needle, avoiding the formation of a closed loop by the positive and negative current collectors and the resulting thermal runaway of the battery, thereby improving the safety performance of the battery.
[0011] Specifically, the intermediate layer in the present disclosure has the following functions: ① It can block the penetration of grains in adjacent metal layers and promote the re-nucleation and growth of grains, thereby generating non-penetrating and smaller grains. The metal layer composed of non-penetrating and small grains will produce microcracks after a certain deformation during the battery puncture process, and quickly spread to the surrounding area, causing large-scale fracture and fragmentation of the metal layer, thereby realizing the separation of the metal layer and the steel needle, avoiding the positive and negative current collectors from being connected to form a closed loop and the resulting thermal runaway of the battery, thereby improving the safety performance of the battery; ② It can strengthen the strain hardening of the composite current collector and reduce local stress concentration, thereby promoting the cracks generated by the deformation of the metal layer of the composite current collector during the battery puncture process to be transmitted to the surrounding area, continuously promoting large-scale fracture and fragmentation of the metal layer, avoiding the positive and negative current collectors from being connected to form a closed loop and the resulting thermal runaway of the battery, thereby improving the safety performance of the battery.
[0012] In some embodiments, the conductive layer may generate microcracks during the needle puncture process, which may spread rapidly and cause large-scale fractures, thereby separating the conductive layer from the steel needle, avoiding the formation of a closed loop by the positive and negative current collectors and the resulting thermal runaway of the battery, thereby improving the safety performance of the battery and promoting the promotion and application of composite current collectors.
[0013] In some embodiments, the intermediate layer described in the present disclosure is partially crystalline or completely amorphous (amorphous), and the metal layer described in the present disclosure is a crystalline metal layer.
[0014] Optionally, the composite current collector includes a base film and a functional layer located on at least one side of the base film; the functional layer includes a conductive layer; and the conductive layer includes alternately stacked metal layers and intermediate layers.
[0015] The composite current collector structure provided by the present invention can generate microcracks in the conductive layer during the needle puncture process through the coordinated cooperation of various structural layers in the functional layer, and quickly spread to cause large-scale fractures, thereby separating the conductive layer from the steel needle, avoiding the formation of a closed loop by the positive and negative current collectors and the resulting thermal runaway of the battery, thereby improving the safety performance of the battery and promoting the promotion and application of the composite current collector.
[0016] The intermediate layer in the conductive layer inhibits the continuous growth of the metal layer grains, and prepares a conductive layer with non-penetrating, small-sized metal grains, thereby ensuring that the cracks generated in the conductive layer during the puncture process are easy to spread over a large area, thereby causing large-scale fracture of the conductive layer, avoiding the battery safety problems caused by the conduction of the positive and negative current collectors. If the conductive layer only contains a metal layer, the cracks generated during the puncture process cannot spread over a large area; and the intermediate layer and the metal layer are both non-porous structures. If they are connected to each other through pores, the continuous growth of the metal layer grains cannot be inhibited, which is not conducive to improving the safety performance of the battery; the protective layer isolates the direct contact between the electrolyte and the conductive layer, avoiding erosion by the electrolyte.
[0017] The metal layer in the composite current collector disclosed in the present invention can provide conductivity, and the intermediate layer (such as an oxide layer, etc.) can effectively inhibit the corrosion of the metal layer by fluoride ions in the electrolyte, thereby improving the stability of the performance of the composite current collector during the charge and discharge cycle, and thus promoting the promotion and application of the composite current collector. In addition, the presence of the intermediate layer can also improve the elongation at break of the composite current collector. This is because during the stretching process, the amorphous intermediate layer material (such as metal oxide) can promote the slip between the metal layers, and the regular alternating structure of the intermediate layer-metal layer can play a regular role in the transmission of the electron flow, promoting the rapid conduction of the electron flow along the direction parallel to the metal layer. It can be understood that the composite conductive layer can be located on one side of the thickness direction of the polymer film, or on both sides of the thickness direction thereof. In the above-mentioned composite current collector, the innermost layer of the composite conductive layer can be an intermediate layer or a metal layer; the outermost layer of the composite conductive layer can be an intermediate layer or a metal layer.
[0018] In the present application, the outermost layer of the composite conductive layer refers to the surface layer of the composite conductive layer away from the polymer film, and the innermost layer of the composite conductive layer refers to the bottom layer of the composite conductive layer close to the polymer film.
[0019] In some embodiments, the outermost layer of the composite conductive layer is an intermediate layer (e.g., a metal oxide layer). In the composite current collector described above, the outermost intermediate layer (e.g., a metal oxide layer) of the composite conductive layer (i.e., the layer farthest from the polymer film) can further inhibit fluoride ion corrosion of the metal layer and, in addition, prevent the metal layer from being chemically corroded or physically damaged.
[0020] In some embodiments, the innermost layer of the composite conductive layer is an intermediate layer. In the composite current collector, the innermost layer of the composite conductive layer is an intermediate layer, which can improve the adhesion between the composite conductive layer and the polymer film.
[0021] In some embodiments, the thickness of the base film is 1-10 μm. Controlling the thickness of the base film within the above range is conducive to reducing the difficulty and cost of preparing the base film and promoting the application of the composite current collector containing the base film in the battery. Alternatively, the base film can be prepared by a melt-extrusion-biaxial stretching method. It is understood that the thickness of the base film includes but is not limited to: for example, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm, etc.
[0022] In some embodiments, the material of the base film includes any one or a combination of at least two of polyethylene terephthalate (PET), polypropylene (PP), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), polyethylene (PE), polypropylene, polyvinyl chloride (PVC), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyphenylene sulfide (PPS), polyphenylene oxide (PPO), polystyrene (PS) or polyimide (PI).
[0023] The base film materials in the present disclosure are not limited to the types of materials provided above, and the present disclosure is applicable to all base film materials that can be used for current collector structures.
[0024] In some embodiments, an adhesive layer is further provided between the base film and the conductive layer.
[0025] In the present disclosure, an adhesive layer is introduced into the functional layer. The adhesive layer assists in cooperating with the conductive layer. The adhesive layer provides suitable bonding force between the conductive layer of the composite current collector and the polymer film, so that a certain relative movement occurs between the conductive layer and the polymer film during the deformation of the composite current collector, thereby promoting the deformation and fission of the conductive layer, and further improving the safety performance of the battery. If the adhesive layer is missing, the safety performance of the battery will deteriorate.
[0026] Optionally, the bonding force between the bonding layer and the conductive layer is 100-900 N / m, for example, 100 N / m, 150 N / m, 200 N / m, 250 N / m, 300 N / m, 350 N / m, 400 N / m, 450 N / m, 500 N / m, 550 N / m, 600 N / m, 650 N / m, 700 N / m, 750 N / m, 800 N / m, 850 N / m or 900 N / m, etc.
[0027] In the present disclosure, by adjusting the bonding force between the adhesive layer and the conductive layer, the mutual movement between the base film and the conductive layer during the deformation of the composite current collector is adjusted, thereby affecting the deformation and fission behavior of the conductive layer; if the bonding force is too small, the conductive layer is prone to excessive relative movement with the polymer film during the battery puncture process, which is not conducive to providing sufficient force along the surface of the conductive layer, inhibiting the large-scale expansion and spread of cracks in the conductive layer, and weakening the safety performance of the battery; if it is too large, it is difficult to cause local micro-deformation, which is not conducive to the large-scale expansion and spread of cracks in the conductive layer, and will affect the safety performance of the battery.
[0028] In some embodiments, the material of the bonding layer includes any one or a combination of at least two of aluminum oxide, silicon oxide, titanium oxide, nickel, chromium, titanium, nickel-chromium alloy, nickel-chromium-copper alloy, silicon-aluminum alloy, polyacrylic acid, polyacrylate, polyacrylamide or polyurethane.
[0029] In one embodiment, the thickness of the bonding layer is 1-100 nm, for example, it can be 1 nm, 3 nm, 5 nm, 7 nm, 9 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm.
[0030] As an optional technical solution of the present disclosure, the composite current collector further includes a protective layer;
[0031] When the composite conductive layer is provided on one side surface of the polymer base film, the protective layer is provided on one side surface of the composite conductive layer away from the polymer base film and on the other side surface of the polymer base film; or
[0032] When the composite conductive layer is disposed on one side of the polymer base film, the protective layer is disposed on the side of the composite conductive layer away from the polymer base film; or
[0033] When the composite conductive layer is disposed on both side surfaces of the polymer base film, the protective layer is disposed on a side of the composite conductive layer away from the polymer base film.
[0034] In the present disclosure, the protective layer is used to prevent the composite conductive layer from being chemically corroded or physically damaged.
[0035] In some embodiments, the single-sided thickness of the protective layer is 5-100 nm, for example, 5 nm, 10 nm, 20 nm, 40 nm, 60 nm, 80 nm or 100 nm, etc., and can be optionally 10-80 nm.
[0036] In some embodiments, the material of the protective layer includes any one or a combination of at least two of nickel, chromium, nickel-based alloys, copper-based alloys, copper oxide, aluminum oxide, nickel oxide, chromium oxide, cobalt oxide, graphite, carbon black, copper chromate, cuprous chromite, nano quantum dots, carbon nanotubes, carbon nanofibers or graphene.
[0037] The thickness of the conductive layer described in the present disclosure is 500 nm - 2000 nm, such as 500 nm, 600 nm, 800 nm, 900 nm, 1000 nm, 1100 nm, 1200 nm, 1300 nm, 1500 nm, 1800 nm or 2000 nm, etc., and can be optionally 800 nm - 1200 nm.
[0038] In the present disclosure, when the thickness of the conductive layer is within the numerical range of 500 nm - 2000 nm, a current collector structure with good conductive effect can be obtained, and it will not affect the normal performance of the battery energy density. If the composite conductive layer is too thin, the conductivity will be poor; if it is too thick, the prepared composite current collector will be too heavy, which is not conducive to improving the energy density of the battery. Considering the conductivity and兼顾 the improvement of energy density; further adjusted to the thickness range of 800 nm - 1200 nm, which not only ensures that the battery has good conductivity but also兼顾 the improvement of energy density.
[0039] Optionally, the thickness d1 of the metal layer satisfies: 0 < d1 ≤ 300 nm, optionally 0 < d1 ≤ 200 nm, further optionally 20 < d1 ≤ 200 nm, such as 20 nm, 30 nm, 50 nm, 80 nm, 100 nm, 130 nm, 150 nm, 180 nm or 200 nm, etc. In the present disclosure, if the metal layer is too thin, in order to ensure conductivity, the number of layers of the metal layer will be increased, thus affecting the production efficiency of the current collector.
[0040] In some embodiments, the thickness d2 of the intermediate layer satisfies: 0 nm < d2 ≤ 100 nm, optionally 1 nm ≤ d2 ≤ 50 nm, more optionally 2 nm ≤ d2 ≤ 50 nm, further optionally 5 nm ≤ d2 ≤ 20 nm, most optionally 5 nm ≤ d2 ≤ 10 nm, such as 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm or 10 nm, etc. It should be noted that the single-layer thickness of each intermediate layer can be the same or different, and the single-layer thickness of each metal layer can also be the same or different.
[0041] When the intermediate layer is a conductive material, the thickness of the metal layer disclosed in the present invention is 0-300nm, and is not 0, for example, it can be 50nm, 100nm, 150nm, 200nm, 250nm or 300nm, etc., and can further be 50-200nm. Because when the intermediate layer is a conductive material, increasing the thickness of the intermediate layer will not affect the overall conductive properties of the composite current collector, the thickness of the intermediate layer d2 does not need to meet the following conditions: the thickness of the intermediate layer d2 is less than or equal to one tenth of the thickness of the metal layer d1. Optionally, the thickness of the intermediate layer is 0-100nm, and is not 0, for example, it can be 10nm, 30nm, 50nm, 70nm or 90nm, etc., and can further be 20-80nm. Optionally, the intermediate layer is carbon or copper, and more optionally, the intermediate layer is partially crystalline or amorphous (amorphous) carbon or copper. In the present disclosure, if the thickness of the amorphous intermediate layer is too thin, the preparation efficiency will be affected and the effect will not be obvious; if the thickness of the amorphous intermediate layer is too thick, the amorphous intermediate layer material will transform into a crystalline state during the preparation process, which is not conducive to improving the safety performance of the battery, and too thick will affect the mechanical properties of the composite copper current collector, resulting in poor mechanical properties.
[0042] In some embodiments, the thickness of the intermediate layer d2 is less than or equal to one tenth of the thickness of the metal layer d1. In the present disclosure, the thickness of the intermediate layer d2 is less than or equal to one tenth of the thickness of the metal layer d1, which is more conducive to maintaining good conductivity of the composite current collector.
[0043] In some embodiments, the total thickness of the intermediate layers accounts for ≤10% of the thickness of the composite conductive layer. The total thickness of the intermediate layers refers to the sum of the thicknesses of all intermediate layers in the composite conductive layer. If the total thickness of the intermediate layers accounts for a high percentage of the thickness of the composite conductive layer, the conductivity of the composite current collector is poor.
[0044] In some embodiments, when the intermediate layer is a non-conductive material, the thickness relationship between adjacent intermediate layers and metal layers can be selected so that the thickness of the intermediate layer d3 is less than or equal to one tenth of the thickness of the metal layer d4. By controlling the thickness of the intermediate layer, it is more conducive to the composite current collector maintaining good conductivity.
[0045] In some embodiments, the number of metal layers in the conductive layer is n, the number of intermediate layers is n, n+1 or n-1, and n satisfies: 2≤n≤50, optionally 5≤n≤40, and more optionally 2≤n≤10, for example, 5, 8, 10, 13, 15, 18, 20, 23, 25, 28, 30, 33, 35, 38 or 40, etc.
[0046] In some embodiments, both the intermediate layer and the metal layer are non-porous structures.
[0047] In the conductive layer mentioned in the present disclosure, the layered structure closer to the bonding layer and the protective layer can be a metal layer or an intermediate layer. Optionally, the metal layer structure is in direct contact with the bonding layer and the protective layer. This stacked structure can better achieve the improvement of battery safety performance; and further, if the number of metal layers is too small, the prepared composite current collector will have a worse effect on improving battery safety; and if the number of metal layers is too large, not only will the battery safety performance fail to be further improved, but it will also easily lead to lower production efficiency and increased production difficulty.
[0048] The metal layer described in the present disclosure may be a crystalline metal layer, and the crystalline state refers to the dominant form of a solid object in which atoms are arranged in a regular pattern. The intermediate layer described in the present disclosure may be an amorphous conductive material, and the "amorphous" or "non-crystalline state" described in the present disclosure refers to the structure of some non-completely crystalline amorphous regions (non-crystalline regions) or the composition of some amorphous solids (non-crystalline). The intermediate layer described in the present disclosure may be any one or a combination of at least two of partially crystalline or amorphous oxides, alloys, nitrides, carbides, sulfides, fluorides, silicides or phosphides, and may be any one or a combination of at least two of carbides, silicides or fluorides.
[0049] In some embodiments, the metal layer is a crystalline metal layer, in which the average particle size of the metal grains is 0-200 nm and is not 0, for example, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 130 nm, 150 nm, 180 nm or 200 nm, etc., and can be optionally 10-100 nm.
[0050] In the present disclosure, the metal grains are columnar, and the average grain size is the diameter of the columnar crystals, not the average grain size of the length. The average grain size of the metal grains in the metal layer affects the generation of microcracks in the conductive layer. If the average grain size is too large, the plasticity of the metal layer will increase, which is not conducive to the large-scale fission of the metal layer during the needle puncture process, thereby reducing the safety improvement effect of the prepared composite current collector on the battery. Further regulation to 10-100nm can achieve the generation of microcracks in the conductive layer without increasing the difficulty of preparation, thereby significantly improving the safety performance of the composite current collector.
[0051] The metal in the metal layer described in the present disclosure includes any one or a combination of at least two of aluminum, copper, gold, silver, nickel, or zinc, and alloys thereof. More optionally, the metal layer is a crystalline copper layer. In some embodiments, the metal layer is an aluminum metal layer, optionally a crystalline aluminum metal layer.
[0052] In some embodiments, the material of the intermediate layer includes any one or a combination of at least two of a fluorocarbon material, oxide, alloy, nitride, carbide, sulfide, fluoride, silicide, or phosphide. These materials offer excellent barrier and tolerance to electrolytes, providing layer-by-layer protection for the metal layer, thereby improving the cyclic charge-discharge performance of batteries based on this composite copper current collector. Carbide, silicide, or fluoride, or a combination of at least two, may be selected.
[0053] In some embodiments, the intermediate layer comprises a fluorocarbon material.
[0054] In some embodiments, the fluorocarbon material is a fluorocarbon polymer.
[0055] In some embodiments, the fluorocarbon polymer is a polymer material containing fluorine and carbon elements.
[0056] In some embodiments, the fluorocarbon polymer is a polymer material composed of fluorine and carbon elements.
[0057] In some embodiments, the fluorocarbon material is a polymer in which some or all of the CH bonds are replaced by CF bonds.
[0058] In some embodiments, the chemical composition of the fluorocarbon polymer is C x F y , where 0.6≤x / y≤10, for example, it can be 0.6, 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10, etc.
[0059] In the present disclosure, if x / y is too low, that is, the carbon content is too low, the conductivity of the intermediate layer will deteriorate, thereby causing the conductivity of the prepared composite current collector to deteriorate, resulting in poor cycle performance of the battery; if x / y is too high, that is, the carbon content is too high, the flexibility of the intermediate layer will deteriorate, defects will easily occur, and the cycle performance of the battery will deteriorate.
[0060] In some embodiments, the weight average molecular weight of the fluorocarbon polymer is 10-100 kDa, for example, 10 kDa, 30 kDa, 50 kDa, 70 kDa, 90 kDa or 100 kDa, etc., and can be optionally 10-60 kDa.
[0061] In some embodiments, the fluorocarbon polymer has a crystallinity ranging from 20% to 80%, for example, 20%, 30%, 40%, 50%, 60%, 70% or 80%.
[0062] In the present disclosure, improving the crystallinity can improve the tolerance of the fluorocarbon layer to the electrolyte, promote its protective effect on the metal layer, and thus promote the improvement of the battery cycle performance. However, the crystallinity should not be too high. Too high crystallinity will lead to increased brittleness of the fluorocarbon layer, resulting in defects easily generated during the production of battery pole pieces, causing the battery cycle performance to deteriorate. According to the present disclosure, compared with carbon materials, fluorocarbon materials are more brittle, which means that the intermediate layer formed by carbon materials is more likely to break when subjected to stress or force. Therefore, in the production process, the requirements for making the carbon layer are higher, the materials and processes required for preparing the carbon layer are more complex and sophisticated, and the production process requires stricter control and monitoring.
[0063] In some embodiments, the oxide in the intermediate layer includes one or more of a metal oxide and a non-metal oxide. Optionally, the metal oxide in the metal oxide layer includes one or more of aluminum oxide (Al2O3), titanium oxide (TiO2), copper oxide (CuO), nickel oxide (NiO), chromium oxide (Cr2O3), zinc oxide (ZnO), magnesium oxide (MgO), cobalt oxide (CoO), zirconium oxide (ZrO2), tin oxide (SnO2), and indium tin oxide (In2O3·SnO2). The above-mentioned metal oxides have the advantages of easy availability of raw materials and good stability. In some embodiments, the non-metal oxide is silicon oxide. In some optional embodiments, the oxide in the intermediate layer includes one or more of aluminum oxide, silicon oxide, and titanium oxide.
[0064] In some embodiments, the alloy in the intermediate layer includes any one of nickel-chromium alloy, nickel-chromium-copper alloy, nickel-chromium-silicon alloy, nickel-chromium-cobalt alloy, silicon-aluminum alloy, aluminum-silicon-copper alloy, copper-nickel alloy, copper-nickel-titanium alloy, copper-gallium alloy, copper-indium alloy, copper-indium-gallium alloy, aluminum-tin-copper alloy, aluminum-chromium alloy, tungsten-titanium alloy, molybdenum-copper alloy, molybdenum-niobium alloy, molybdenum-tantalum alloy, molybdenum-zirconium-titanium alloy or molybdenum-lanthanum alloy, or a combination of at least two thereof.
[0065] In some embodiments, the nitride includes any one or a combination of at least two of aluminum nitride, boron nitride, chromium nitride, titanium nitride, silicon nitride, niobium nitride, zirconium nitride, hafnium nitride, tantalum nitride, vanadium nitride, or aluminum titanium nitride.
[0066] In some embodiments, the carbide includes any one or a combination of at least two of aluminum carbide, boron carbide, chromium carbide, nickel carbide, tungsten carbide, titanium carbide, hafnium carbide, zirconium carbide, tantalum carbide, lanthanum carbide, molybdenum carbide, niobium carbide, silicon carbide, titanium carbide or vanadium carbide.
[0067] In some embodiments, the sulfide includes any one or a combination of at least two of copper sulfide, tin sulfide, zinc sulfide, tungsten sulfide, molybdenum sulfide, iron sulfide, antimony sulfide, chromium sulfide, nickel sulfide, titanium sulfide, aluminum copper sulfide, or iron copper sulfide.
[0068] In some embodiments, the fluoride includes any one or a combination of at least two of iridium fluoride, magnesium fluoride, calcium fluoride, lithium fluoride, aluminum fluoride, barium fluoride, samarium fluoride, cerium fluoride, yttrium fluoride, or scandium fluoride.
[0069] In some embodiments, the silicide includes any one or a combination of at least two of cobalt silicide, chromium silicide, nickel silicide, titanium silicide, hafnium silicide, molybdenum silicide, niobium silicide, tantalum silicide, vanadium silicide, tungsten silicide, or zirconium silicide.
[0070] In some embodiments, the phosphide is any one of aluminum phosphide, boron phosphide, copper phosphide, nickel phosphide, silicon phosphide, tungsten phosphide, gallium phosphide, germanium phosphide, indium phosphide, molybdenum phosphide, niobium phosphide or tantalum phosphide, or a combination of at least two thereof.
[0071] In some embodiments, a protective layer is further provided on the surface of the conductive layer away from the base film. The purpose of providing the protective layer in the present disclosure is to prevent the conductive layer from being chemically corroded or physically damaged.
[0072] In some embodiments, the thickness of the protective layer is 5-100 nm, optionally 10-100 nm, for example, 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm, etc., optionally 20-80 nm.
[0073] In some embodiments, the material of the protective layer includes any one or a combination of at least two of nickel, chromium, nickel-based alloys, copper-based alloys, copper oxide, aluminum oxide, nickel oxide, chromium oxide, cobalt oxide, copper-chromium oxide, graphite, carbon black, carbon nano-quantum dots, carbon nanotubes, carbon nanofibers, graphene or graphene oxide.
[0074] In some embodiments, the area density of the intermediate layer on the side close to the electrolyte is greater than the area density of the intermediate layer on the side close to the polymer-based film.
[0075] In some embodiments, the crystallinity of the intermediate layer is in the range of 20%-80%, for example, 20%, 30%, 40%, 50%, 60%, 70% or 80%.
[0076] In a second aspect, the present disclosure provides a method for preparing the composite current collector according to the first aspect, the preparation method comprising the following steps:
[0077] A conductive layer is composited on the surface of at least one side of the base film; wherein the conductive layer comprises metal layers and intermediate layers stacked alternately.
[0078] In some embodiments, an adhesive layer is further provided between the base film and the conductive layer. Optionally, the adhesive layer is formed by a composite method comprising physical vapor deposition or coating. In some specific embodiments, the physical vapor deposition method comprises one or more of evaporation and magnetron sputtering.
[0079] In some specific embodiments, when the intermediate layer is directly laminated on the base film, the intermediate layer is a bonding layer.
[0080] Optionally, the composite preparation method of the metal layer includes one or more of electroplating, chemical plating, evaporation and / or magnetron sputtering.
[0081] In one embodiment, in the electroplating method, the components of the electroplating solution include copper sulfate, sulfuric acid, hydrochloric acid, a brightener, a leveler, and a wetting agent.
[0082] In one embodiment, the concentration of the copper sulfate is 80-130 g / L, for example, 80 g / L, 90 g / L, 100 g / L, 110 g / L, 120 g / L or 130 g / L, the concentration of the sulfuric acid is 80-160 g / L, for example, 80 g / L, 100 g / L, 120 g / L, 140 g / L or 160 g / L, and the concentration of the chloride ion is 20-80 mg / L, for example, 20 mg / L, 40mg / L, 60mg / L or 80mg / L, etc., the concentration of the brightener is 5-20ppm, for example, 5ppm, 10ppm, 15ppm or 20ppm, etc., the concentration of the leveler is 1-5ppm, for example, 1ppm, 3ppm or 5ppm, etc., the concentration of the wetting agent is 20-200ppm, for example, 20ppm, 50ppm, 100ppm, 150ppm or 200ppm, etc.
[0083] In one embodiment, the brightener includes any one of sodium polydisulfide propane sulfonate, sodium 3-mercapto-1-propane sulfonate, or sodium N,N-dimethyldithiocarboxamide propane sulfonate, or a combination of at least two thereof.
[0084] In one embodiment, the leveler includes any one of N,N-diethylthiourea, 2-mercaptopyridine, or Janus Green, or a combination of at least two thereof.
[0085] In one embodiment, the wetting agent includes any one of polyethylene glycol, polypropylene glycol, or polyoxyethylene ether, or a combination of at least two thereof.
[0086] In one embodiment, the specific process parameters of the electroplating method include: an average cathode current density of 1-3A / dm 2 , for example, it can be 1A / dm 2, 2A / dm 2 or 3A / dm 2 The plating solution temperature is 15-35°C, for example, 15°C, 20°C, 25°C, 30°C or 35°C, and the electroplating time is 1-90s, for example, 1s, 10s, 30s, 60s or 90s.
[0087] In some embodiments, the intermediate layer is prepared by physical vapor deposition or chemical vapor deposition. In some specific embodiments, the physical vapor deposition method includes one or more of evaporation and magnetron sputtering. In some embodiments, the intermediate layer can be prepared by magnetron sputtering.
[0088] In some embodiments, the specific process parameters of the vapor deposition method include: a heating evaporation temperature of 1400-1600°C, for example, 1400°C, 1500°C or 1600°C, etc., a coating vacuum degree of <0.1Pa, for example, 0.08Pa, 0.06Pa or 0.04Pa, etc., a coating main roller cooling temperature of -30°C--10°C, for example, -30°C, -20°C or -10°C, etc., a coating time of 0.1s-10s, for example, 0.1s, 1s, 5s or 10s, etc.
[0089] In some embodiments, the specific process parameters of the magnetron sputtering method include: target power of 1-10kW, such as 1kW, 3kW, 5kW, 7kW, 9kW or 10kW, etc., which can be 2-6kW, such as 2kW, 4kW or 6kW, etc.; the vacuum degree in the chamber during coating is ≤0.1Pa, such as 0.1Pa, 0.08Pa or 0.05Pa, etc.; the flow rate of the gas source is 10-500mL / min, such as 10mL / min, 20mL / min. min, 50mL / min, 100mL / min, 200mL / min, 300mL / min, 400mL / min or 500mL / min, etc., and can be optionally 20-200mL / min, for example, 20mL / min, 50mL / min, 100mL / min, 150mL / min or 200mL / min, etc., and the coating time is 0.1s-60s, for example, 1s, 5s, 10s, 30s or 60s, etc.
[0090] In some embodiments, the gas source may be argon.
[0091] In some embodiments, the target material is selected based on the material of the deposited intermediate layer. For example, when the intermediate layer is a fluorocarbon material, the target material is a mixture of a carbon material and a fluorine-containing material. The carbon material includes graphite. In some embodiments, the fluorine material includes polytetrafluoroethylene. For example, when the intermediate layer is an alloy, nitride, sulfide, fluoride, silicide, or phosphide, the target material is the aforementioned alloy, nitride, sulfide, fluoride, silicide, or phosphide.
[0092] In some embodiments, after the conductive layer is obtained by composite, a protective layer is further provided on the surface of the conductive layer away from the base film. Optionally, the composite preparation method of the protective layer includes any one of physical vapor deposition, chemical vapor deposition, in-situ forming, or coating, or a combination of at least two thereof.
[0093] In some embodiments, the chemical vapor deposition method includes atmospheric pressure chemical vapor deposition or plasma enhanced chemical vapor deposition.
[0094] In some embodiments, the specific steps of the in-situ forming method include: in-situ forming a metal oxide passivation layer on the surface of the metal layer.
[0095] In some embodiments, the coating method includes die coating, knife coating, or extrusion coating.
[0096] As an optional technical solution of the present application, the preparation method comprises the following steps:
[0097] (1) preparing a polymer base film with a thickness of 1-10 μm by a melt-extrusion-biaxial stretching method;
[0098] (2) depositing a bonding layer with a thickness of 1-100 nm on each side of the polymer by physical vapor deposition or coating to obtain a composite film having a bonding layer on the surface;
[0099] (3) alternately depositing an intermediate layer material (such as an amorphous copper layer, a fluorocarbon material layer, an amorphous carbon layer, an oxide layer, an alloy layer, a nitride layer, a carbide layer, a sulfide layer, a fluoride layer, a silicide layer, or a phosphide layer) and a metal layer (such as aluminum, copper, gold, silver, nickel, zinc, and optionally a crystalline copper layer) on both sides of the composite film, wherein the number of layers of the intermediate layer and the metal layer is ≥2, to obtain a composite film containing a conductive layer and an adhesive layer;
[0100] (4) A protective layer with a thickness of 5-100 nm is deposited on both sides of the composite film containing the conductive layer and the adhesive layer by physical vapor deposition, chemical vapor deposition, in-situ forming or coating.
[0101] In some embodiments, the metal layer is prepared by physical vapor deposition, and specific process parameters include:
[0102] The target material is any one of a copper target, an aluminum target or a copper-aluminum alloy target, the target power is 10-14kW (for example, it can be 10kW, 11kW, 12kW, 13kW or 14kW, etc.), the gas flow rate is 20-500mL / min (for example, it can be 20mL / min, 40mL / min, 45mL / min, 50mL / min, 55mL / min or 60mL / min, etc.), the vacuum degree is ≤0.1Pa (for example, it can be 0.1Pa, 0.08Pa, 0.05Pa or 0.03Pa, etc.), and the coating time of a single metal layer is 5s-20s (for example, it can be 5s, 10s, 15s or 20s, etc.).
[0103] In some embodiments, the specific process parameters of the magnetron sputtering are selected based on whether the intermediate layer contains amorphous material and the mass ratio of the amorphous material in the intermediate layer, such as reducing the target power, gas flow rate, and / or reducing the cooling temperature of the coating main roller.
[0104] In one embodiment, the middle layer is an amorphous copper layer, which is prepared by magnetron sputtering. The preparation process parameters include: using a copper target as the target material, the target power is 2-6kW, the vacuum degree in the chamber during coating is ≤0.1Pa, the flow rate of the gas source is 10-200mL / min, the coating time is 0.1s-60s, and the cooling temperature of the coating main roller is -30℃-0℃.
[0105] In one embodiment, the metal layer is a crystalline copper layer, which is prepared by electroplating. The preparation process parameters include: an average cathode current density of 1-3A / dm 2 , the plating solution temperature is 15℃-35℃, and the electroplating time is 1s-90s.
[0106] In some more specific embodiments, the metal layer is formed by evaporation. Specifically, the process conditions for preparing the metal layer include: the raw material is any one of copper, aluminum or copper-aluminum alloy, and high-purity aluminum wire (purity ≥99.9%) can be selected; the heating temperature is greater than the melting point of the aluminum wire; the vacuum degree of the vacuum chamber is ≤0.1 Pa; and each deposition time is 0.5s-40s. The process conditions for controlling the aluminum metal layer include the above-mentioned process parameters, which can improve the uniformity, density and integrity of the prepared aluminum metal layer, thereby improving the conductivity of the aluminum metal layer. It is understood that the vacuum degree of the vacuum chamber includes but is not limited to: 0.05Pa, 0.06Pa, 0.07Pa, 0.08Pa, 0.09Pa, or 0.1Pa; each deposition time includes but is not limited to: 0.5s, 2s, 5s, 8s, 10s, 12s, 15s, 18s, 20s, 22s, 25s, 28s, 30s, 32s, 35s, 38s, or 40s.
[0107] In some more specific embodiments, the metal layer is formed by magnetron sputtering. Specifically, the process conditions for preparing the metal layer include: the target material is any one of a copper target, an aluminum target, or a copper-aluminum alloy target, and a high-purity aluminum target (purity ≥ 99.9%) can be selected; the target power supply is a DC power supply with a power density of 10W / cm 2 -150W / cm 2 The vacuum degree of the vacuum chamber is ≤0.5Pa, the gas source is argon, the flow rate of argon is 10mL / min-500mL / min, and the deposition time each time is 1s-60s.
[0108] It should be noted that the process conditions for controlling the aluminum metal layer, including the above process parameters, can improve the uniformity, density and integrity of the prepared aluminum metal layer, thereby improving the conductivity of the aluminum metal layer. It is understood that the power density includes but is not limited to: 10W / cm 2 、30W / cm 2 , 50W / cm 2 , 70W / cm 2 , 90W / cm 2 、110W / cm 2 、130W / cm 2 , or 150W / cm 2 ; The vacuum degree of the vacuum chamber includes but is not limited to: 0.1Pa, 0.2Pa, 0.3Pa, 0.4Pa, or 0.5Pa; the flow rate of argon gas includes but is not limited to: 10mL / min, 50mL / min, 100mL / min, 150mL / min, 200mL / min, 250mL / min, 300mL / min, 350mL / min, 400mL / min, 450mL / min, or 500mL / min; the deposition time for each time includes but is not limited to: 1s, 5s, 10s, 15s, 20s, 25s, 30s, 35s, 40s, 45s, 50s, 55s, or 60s.
[0109] In some more specific embodiments, the intermediate layer (such as an oxide layer, in particular a metal oxide layer) is formed by evaporation. Specifically, the preparation process conditions include: the raw material is a high-purity metal wire (purity ≥99.9%), the heating temperature during the evaporation process is greater than the melting point of the metal wire, the gas source is oxygen, the oxygen flow rate is 10mL / min-500mL / min, the vacuum degree of the vacuum chamber is ≤0.5Pa, and the deposition time for each deposition is 0.1s-10s. The process conditions for controlling the metal oxide layer include the above-mentioned process parameters, which can improve the uniformity, density and integrity of the prepared metal oxide layer, thereby improving the corrosion resistance of the composite current collector (mainly resistance to fluoride ion corrosion). It is understood that the vacuum degree of the vacuum chamber includes but is not limited to: 0.1Pa, 0.2Pa, 0.3Pa, 0.4Pa, or 0.5Pa; the deposition time for each deposition includes but is not limited to: 0.1s, 1s, 2s, 3s, 4s, 5s, 6s, 7s, 8s, 9s, or 10s.
[0110] In some more specific embodiments, the intermediate layer (e.g., oxide layer, particularly metal oxide layer) is formed by magnetron sputtering. Specifically, the process conditions for preparing the metal oxide layer include: the target material is a high-purity metal oxide target material (purity ≥ 99.9%), the target power supply is a DC power supply, and the power density is 10W / cm 2 -150W / cm 2 The vacuum degree of the vacuum chamber is ≤0.5Pa, the gas source is argon, the flow rate of argon is 10mL / min-500mL / min, and the deposition time each time is 0.5s-30s.
[0111] It should be noted that controlling the process conditions of the intermediate layer (such as the oxide layer, especially the metal oxide layer) including the above process parameters can improve the uniformity, density and integrity of the prepared intermediate layer, thereby improving the corrosion resistance of the composite current collector (mainly resistance to fluoride ion corrosion). It is understood that the power density includes but is not limited to: 10W / cm 2 、30W / cm 2 , 50W / cm 2 , 70W / cm 2 , 90W / cm 2 、110W / cm 2 、130W / cm 2 , or 150W / cm 2; The vacuum degree of the vacuum chamber includes but is not limited to: 0.1Pa, 0.2Pa, 0.3Pa, 0.4Pa, or 0.5Pa; the flow rate of argon gas includes but is not limited to: 10mL / min, 50mL / min, 100mL / min, 150mL / min, 200mL / min, 250mL / min, 300mL / min, 350mL / min, 400mL / min, 450mL / min, or 500mL / min; each deposition time includes but is not limited to: 0.5s, 5s, 10s, 15s, 20s, 25s, or 30s.
[0112] In some more specific embodiments, the metal layer is made by evaporation, and the conditions for preparing the metal layer are: the raw material is high-purity metal wire (purity ≥99.9%), the heating temperature is greater than the melting point of the metal wire, the vacuum degree of the vacuum chamber is less than or equal to 0.05 Pa, the coating time each time is 0.5-100s, and the cooling temperature of the main roller is: -30℃-10℃.
[0113] In some more specific embodiments, the metal layer is made by magnetron sputtering, and the conditions for preparing the metal layer are: the target material is a target material of the metal layer material (purity ≥99.9%), the target power supply is a DC power supply, the target power is 5-20kW, the vacuum degree of the vacuum chamber is less than or equal to 0.1Pa, the gas source is argon, the argon flow rate is 20-500mL / min, the coating time for each time is 0.1-120s, and the cooling temperature of the main roller is: -20℃-30℃.
[0114] In some more specific embodiments, the intermediate layer (e.g., alloy, nitride, sulfide, fluoride, silicide, or phosphide) is formed by magnetron sputtering. Specifically, the process conditions for preparing the intermediate layer include: For magnetron sputtering, the target material is a high-purity target material (purity ≥ 99.9%), such as the alloy, nitride, sulfide, fluoride, silicide, or phosphide described above. The target power supply has a target power of 1-10 kW, the vacuum chamber has a vacuum level of 0.1 Pa or less, the gas source is argon, the argon flow rate is 10-500 mL / min, and each deposition time is 0.1-10 seconds.
[0115] In the preparation method of the composite current collector provided in the present disclosure, the preparation process is all conventional technical means, and those skilled in the art can adapt the preparation method and adjust the parameters according to actual needs.
[0116] In the third aspect, the present disclosure further provides an electrode plate, including the above-mentioned composite current collector or the composite current collector prepared by the above-mentioned preparation method. It should be noted that the electrode plate of the present disclosure can be, for example, formed into a slurry by mixing positive electrode active material / negative electrode active material, a conductive agent, a binder and a solvent, and the slurry is coated on the composite current collector of the present application using a method for preparing electrode plates well known to those skilled in the art. Depending on the active material, the electrode plate can be divided into a positive electrode plate and a negative electrode plate. The present disclosure has no special restrictions on the preparation method of the electrode plate, and the above-mentioned preparation method can be a preparation method well known to those skilled in the art. The above-mentioned electrode plate can be a positive electrode plate or a negative electrode plate.
[0117] The present disclosure also provides a battery, which includes the composite current collector as described in the first aspect. The above-mentioned battery may, for example, include a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator. The separator is arranged between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. During the charge and discharge process of the battery, lithium ions are embedded and extracted back and forth between the positive electrode sheet and the negative electrode sheet. The above-mentioned positive electrode sheet and / or negative electrode sheet can adopt the electrode sheet disclosed in the present disclosure.
[0118] The batteries provided in the present disclosure include lithium-ion batteries and / or sodium-ion batteries. Except for the composite current collector provided in the present disclosure, the remaining materials, structures and preparation methods are all selected from conventional technologies.
[0119] Optionally, the composite current collector is used in an electrode plate of the battery.
[0120] The composite current collector provided in the present disclosure can be used in both positive and negative electrode sheets, and those skilled in the art can make an adaptive selection based on their needs.
[0121] Another embodiment of the present disclosure further provides an electrical device comprising the above-mentioned battery. The above-mentioned battery can be used as a power source or energy storage unit in the above-mentioned electrical device, including but not limited to electric vehicles, smart home appliances, computers, tablets, mobile phones, digital cameras, etc.
[0122] Compared with the related art, the present disclosure has the following beneficial effects:
[0123] The composite current collector structure provided by the present invention can generate microcracks in the conductive layer during the needle puncture process through the coordinated cooperation of various structural layers in the functional layer, and quickly spread to cause large-scale fractures, thereby separating the conductive layer from the steel needle, avoiding the formation of a closed loop by the positive and negative current collectors and the resulting thermal runaway of the battery, thereby improving the safety performance of the battery and promoting the promotion and application of the composite current collector.
[0124] Still other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0125] The accompanying drawings are used to provide a further understanding of the technical solution of this article and constitute a part of the specification. Together with the embodiments of this application, they are used to explain the technical solution of this article and do not constitute a limitation on the technical solution of this article.
[0126] Figure 1 is a schematic diagram of the structure of the composite current collector provided in Example 1. 1-base film, 2-adhesive layer, 3-conductive layer, 4-protective layer.
[0127] Figure 2 is the overall morphology of the composite current collector prepared in Example 32.
[0128] Figure 3 is a partial morphology of the composite current collector prepared in Example 32. In addition, an elemental surface scan was performed on the composite current collector in Figure 3. The test results show that aluminum oxide (metal oxide layer) and aluminum (metal layer) in the composite current collector in Figure 3 are alternately stacked.
[0129] FIG4 is an X-ray diffraction pattern of a composite copper layer and an amorphous copper layer prepared in a specific embodiment of the present disclosure. DETAILED DESCRIPTION
[0130] The technical solution of the present disclosure is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present disclosure and should not be regarded as specific limitations of the present disclosure.
[0131] In one embodiment, the present disclosure provides a method for preparing a composite current collector, the method comprising the following steps:
[0132] (1) placing the base film in a magnetron sputtering machine, using the material of the bonding layer as a target material, adjusting the power, gas flow, vacuum degree and time during the sputtering process, and depositing the bonding layer on the surface of the base film;
[0133] (2) Compounding a conductive layer on the surface of the adhesive layer is performed according to the stacking order of the conductive layer (i.e., the number and alternating order of the metal layer and the intermediate layer):
[0134] The preparation of the metal layer includes:
[0135] a. Evaporation method: the conditions for preparing the metal layer are: the raw material is high-purity metal wire (purity ≥ 99.9%), the heating temperature is greater than the melting point of the metal wire, the vacuum degree of the vacuum chamber is less than or equal to 0.1Pa, and can be less than or equal to 0.05Pa, each coating time is 0.5s-100s, and can be selected from 0.5s-40s, and the main roller cooling temperature is: -30℃-10℃;
[0136] b. Magnetron sputtering method: For magnetron sputtering, the conditions for preparing the metal layer are: the target material is a target material of the metal layer material (purity ≥99.9%), the target power supply is a DC power supply, the target power is 5-20kW, the vacuum degree of the vacuum chamber is less than or equal to 0.1Pa, the gas source is argon, the argon flow rate is 10-500mL / min, and 20-500mL / min is optional. The coating time for each time is 0.1s-120s, and 1s-60s is optional. The cooling temperature of the main roller is: -20℃-30℃;
[0137] c. Electroplating method: The specific process parameters of the electroplating method include: average cathode current density of 1~3A / dm 2 , for example, it can be 1A / dm 2 , 2A / dm 2 or 3A / dm 2 The plating solution temperature is 15°C-35°C, for example, 15°C, 20°C, 25°C, 30°C or 35°C, and the electroplating time is 1s-90s, for example, 1s, 10s, 30s, 60s or 90s.
[0138] The preparation of the middle layer includes:
[0139] a. Magnetron sputtering: The target material is a high-purity target material (purity ≥ 99.9%), and the material is the alloy, nitride, sulfide, fluoride, silicide, phosphide, etc. The target power of the target power supply is 1-10kW, the vacuum degree of the vacuum chamber is less than or equal to 0.1Pa, the gas source is argon, and the argon flow rate is 10-500mL / min. The coating time per deposition is 0.1-30s, and 0.5s-10s is optional.
[0140] b. Evaporation method: The specific process parameters of the evaporation method include: heating evaporation temperature of 1400~1600℃, for example, it can be 1400℃, 1500℃ or 1600℃, etc., coating vacuum degree is less than 0.1Pa, for example, it can be 0.08Pa, 0.06Pa or 0.04Pa, etc., the cooling temperature of the coating main roller is -30~-10℃, for example, it can be -30℃, -20℃ or -10℃, etc., the coating time is 0.1~10s, for example, it can be 0.1s, 1s, 5s or 10s, etc.
[0141] (3) A composite protective layer is formed on the surface of the conductive layer.
[0142] The following examples and comparative examples are all prepared based on the above-mentioned specific preparation methods.
[0143] Example 1
[0144] This embodiment provides a composite current collector, as shown in FIG1 , wherein the composite current collector includes a base film 1
[0145] (PET film) and functional layers located on both sides of the base film 1 (i.e., functional layers are provided on both sides of the base film); along the direction from close to the base film 1 to away from the base film 1, the functional layers include an adhesive layer 2 (nickel-chromium alloy), a conductive layer 3 (1030 nm thick), and a protective layer 4 (copper-chromium oxide) stacked in sequence; the conductive layer 3 includes alternating metal layers (copper) and intermediate layers (nickel-chromium-copper layers), with the number of metal layers being 9 and the number of intermediate layers being 8, i.e., the metal layer in the conductive layer 4 is in direct contact with the adhesive layer and the protective layer;
[0146] The preparation method of the composite current collector is as follows, based on the preparation method provided in one of the above specific embodiments:
[0147] (1) Preparing an adhesive layer: a biaxially oriented PET film with a thickness of 6 μm was placed in a magnetron sputtering machine, and a nickel-chromium alloy target was used as the target material to deposit a 5 nm adhesive layer on each side of the PET film. The specific process conditions were: a nickel-chromium target (purity: 99.99%) was used as the target material, a target power of 5.0 kW, an argon gas flow rate of 50 mL / min, a coating vacuum of 0.08 Pa, and a coating time of 1 s, thereby preparing a PET composite film with an adhesive layer on the surface;
[0148] (2) Prepare a conductive layer (metal layer and intermediate layer are arranged alternately), place the PET composite film with the adhesive layer prepared above in a magnetron sputtering machine, and deposit copper and nickel-chromium-copper on the surface of the composite film in sequence, wherein: ① Metal layer: The metal layer is a copper layer with a thickness of 110 nm, the number of layers is 9, and the average size of the copper grains in the metal layer is 30 nm. The preparation conditions of each layer are: a copper target (purity: 99.99%) is used as the target material, the target power is 12.0 kW, the argon flow rate is 50 mL / min, and the coating vacuum is 0.08Pa, the cooling temperature of the main roller during the coating process was -10°C, and the coating time was 11s; ② Intermediate layer: The intermediate layer was a nickel-chromium-copper layer with a thickness of 5nm and 8 layers. The preparation conditions of each layer were: a nickel-chromium-copper target (purity: 99.99%) was used as the target material, the target power was 4.5kW, the argon flow rate was 50mL / min, the coating vacuum was 0.08Pa, the cooling temperature of the main roller during the coating process was -20°C, and the coating time was 1s, thus preparing a PET composite film including an adhesive layer and a conductive layer;
[0149] (3) Prepare a protective layer, place the PET composite film containing the adhesive layer and the conductive layer prepared above in a 0.5g / L chromic anhydride aqueous solution (25°C) and soak it for 20s. After the treatment, wash it in a pure water tank. After washing, place it in a 60°C oven for drying to obtain a finished composite current collector. The bonding strength between the conductive layer and the base film in the prepared composite current collector is 500N / m.
[0150] Example 2
[0151] This embodiment differs from Example 1 in that the intermediate layer in this embodiment is made of aluminum nitride. The intermediate layer preparation process is as follows: an aluminum nitride target (purity: 99.99%) is used as the target material, the target power is 6.0 kW, the argon flow rate is 50 mL / min, the coating vacuum is 0.08 Pa, the coating time is 1 second, and the main roller cooling temperature during the coating process is -20°C.
[0152] The rest of the structure and preparation process are consistent with those in Example 1.
[0153] Example 3
[0154] This embodiment differs from Example 1 in that the intermediate layer in this embodiment is made of chromium carbide. The intermediate layer preparation process is as follows: a chromium carbide target (purity: 99.99%) is used as the target material, the target power is 5.6 kW, the argon flow rate is 50 mL / min, the coating vacuum is 0.08 Pa, the coating time is 1 second, and the main roller cooling temperature during the coating process is -20°C.
[0155] The rest of the structure and preparation process are consistent with those in Example 1.
[0156] Example 4
[0157] This embodiment differs from Example 1 in that the intermediate layer in this embodiment is made of magnesium fluoride. The intermediate layer preparation process is as follows: a magnesium fluoride target (purity: 99.99%) is used as the target material, the target power is 6.5 kW, the argon flow rate is 50 mL / min, the coating vacuum is 0.08 Pa, the coating time is 1 second, and the main roller cooling temperature during the coating process is -20°C.
[0158] The rest of the structure and preparation process are consistent with those in Example 1.
[0159] Example 5
[0160] The difference between this embodiment and embodiment 1 is that the material of the intermediate layer in this embodiment is nickel silicide. The preparation process of the intermediate layer is as follows: a nickel silicide target (purity: 99.99%) is used as the target material, the target power is 5.8kW, the argon flow rate is 50mL / min, the coating vacuum is 0.08Pa, the coating time is 1s, and the main roller cooling temperature during the coating process is -20°C.
[0161] The rest of the structure and preparation process are consistent with those in Example 1.
[0162] Example 6
[0163] This embodiment differs from Example 1 in that the intermediate layer in this embodiment is made of aluminum phosphide. The intermediate layer preparation process is as follows: an aluminum phosphide target (purity: 99.99%) is used as the target material, the target power is 7.0 kW, the argon flow rate is 50 mL / min, the coating vacuum is 0.08 Pa, the coating time is 1 second, and the main roller cooling temperature during the coating process is -20°C.
[0164] The rest of the structure and preparation process are consistent with those in Example 1.
[0165] Example 7
[0166] The difference between this embodiment and embodiment 1 is that the material of the intermediate layer in this embodiment is a mixture of nickel-chromium-copper and aluminum nitride.
[0167] The preparation process of the intermediate layer is as follows: a nickel-chromium-copper and aluminum nitride mixture target (purity: 99.99%) is used as the target material, the target power is 5.0kW, the argon flow rate is 50mL / min, the coating vacuum is 0.08Pa, the coating time is 1s, and the main roller cooling temperature during the coating process is -20°C.
[0168] The rest of the structure and preparation process are consistent with those in Example 1.
[0169] Example 8
[0170] The difference between this embodiment and embodiment 1 is that the material of the intermediate layer in this embodiment is a mixture of magnesium fluoride and chromium carbide.
[0171] The preparation process of the intermediate layer is as follows: using a mixture target of magnesium fluoride and chromium carbide (purity: 99.99%) as the target material, the target power is 6.2kW, the argon flow rate is 50mL / min, the coating vacuum is 0.08Pa, the coating time is 1s, and the cooling temperature of the main roller during the coating process is -20°C.
[0172] The rest of the structure and preparation process are consistent with those in Example 1.
[0173] Example 9
[0174] The difference between this embodiment and embodiment 1 is that the material of the intermediate layer in this embodiment is a mixture of aluminum nitride and chromium carbide.
[0175] The preparation process of the intermediate layer is as follows: using aluminum nitride and chromium carbide mixture target (purity: 99.99%) as the target material, the target power is 6.0kW, the argon flow rate is 50mL / min, the coating vacuum is 0.08Pa, the coating time is 1s, and the main roller cooling temperature during the coating process is -20℃.
[0176] The rest of the structure and preparation process are consistent with those in Example 1.
[0177] Example 10
[0178] The difference between this embodiment and embodiment 1 is that the material of the metal layer in this embodiment is metal aluminum.
[0179] The preparation process of the metal layer is as follows: aluminum target (purity: 99.99%) is used as the target material, the target power is 10.0kW, the argon flow rate is 50mL / min, the coating vacuum is 0.08Pa, the coating time is 10s, and the main roller cooling temperature during the coating process is -10℃.
[0180] The rest of the structure and preparation process are consistent with those in Example 1.
[0181] Example 11
[0182] The difference between this embodiment and embodiment 1 is that the thickness of the metal layer in this embodiment is 60 nm, and the thickness of the conductive layer is 580 nm.
[0183] The preparation process of the metal layer is as follows: copper target (purity: 99.99%) is used as the target material, the target power is 12kW, the argon flow rate is 50mL / min, the coating vacuum is 0.08Pa, the coating time is 6s, and the main roller cooling temperature during the coating process is -10℃.
[0184] The rest of the structure and preparation process are consistent with those in Example 1.
[0185] Example 12
[0186] The difference between this embodiment and embodiment 1 is that the thickness of the metal layer in this embodiment is 200 nm, and the thickness of the conductive layer is 1840 nm.
[0187] The preparation process of the metal layer is as follows: copper target (purity: 99.99%) is used as the target material, the target power is 12kW, the argon flow rate is 50mL / min, the coating vacuum is 0.08Pa, the coating time is 20s, and the main roller cooling temperature during the coating process is -10℃.
[0188] The rest of the structure and preparation process are consistent with those in Example 1.
[0189] Example 13
[0190] The difference between this embodiment and embodiment 1 is that in this embodiment, the thickness of the metal layer is 220 nm, the number of layers is 5, the number of the intermediate layer is 4, and the thickness of the conductive layer is 1120 nm.
[0191] The preparation process of the metal layer is as follows: copper target (purity: 99.99%) is used as the target material, the target power is 12kW, the argon flow rate is 50mL / min, the coating vacuum is 0.08Pa, the coating time is 22s, and the main roller cooling temperature during the coating process is -10℃.
[0192] The rest of the structure and preparation process are consistent with those in Example 1.
[0193] Example 14
[0194] The difference between this embodiment and embodiment 1 is that the average particle size of the metal grains in the metal layer in this embodiment is 100 nm.
[0195] The preparation process of the metal layer is as follows: copper target (purity: 99.99%) is used as the target material, the target power is 10.0kW, the argon flow rate is 50mL / min, the coating vacuum is 0.08Pa, the coating time is 14s, and the main roller cooling temperature during the coating process is 1°C.
[0196] The rest of the structure and preparation process are consistent with those in Example 1.
[0197] Example 15
[0198] The difference between this embodiment and embodiment 1 is that the average particle size of the metal grains in the metal layer in this embodiment is 200 nm.
[0199] The preparation process of the metal layer is as follows: copper target (purity: 99.99%) is used as the target material, the target power is 8.0kW, the argon flow rate is 50mL / min, the coating vacuum is 0.08Pa, the coating time is 17s, and the main roller cooling temperature during the coating process is 10°C.
[0200] The rest of the structure and preparation process are consistent with those in Example 1.
[0201] Example 16
[0202] The difference between this embodiment and embodiment 1 is that the average particle size of the metal grains in the metal layer in this embodiment is 220 nm.
[0203] The preparation process of the metal layer is as follows: copper target (purity: 99.99%) is used as the target material, the target power is 7.0kW, the argon flow rate is 50mL / min, the coating vacuum is 0.08Pa, the coating time is 19s, and the main roller cooling temperature during the coating process is 12°C.
[0204] The rest of the structure and preparation process are consistent with those in Example 1.
[0205] Example 17
[0206] The difference between this embodiment and embodiment 1 is that in the conductive layer of this embodiment, the number of intermediate layers is 9.
[0207] The number of metal layers is 8, that is, the middle layer in the conductive layer is in direct contact with the bonding layer and the protective layer, and the thickness of the conductive layer is 925 nm.
[0208] During the preparation process, the intermediate layer is first deposited on the surface of the adhesive layer. The rest of the structure and preparation process are consistent with Example 1.
[0209] Example 18
[0210] The difference between this embodiment and embodiment 1 is that in the conductive layer of this embodiment, there are 5 metal layers, 4 intermediate layers, and the thickness of the conductive layer is 570 nm.
[0211] The rest of the structure and preparation process are consistent with those in Example 1.
[0212] Example 19
[0213] The difference between this embodiment and embodiment 11 is that in the conductive layer of this embodiment, the metal layer has 20 layers with a thickness of 60 nm, the intermediate layer has 19 layers with a thickness of 5 nm, and the conductive layer has a thickness of 1295 nm.
[0214] The rest of the structure and preparation process are consistent with Example 11.
[0215] Example 20
[0216] The difference between this embodiment and embodiment 1 is that in the conductive layer of this embodiment, there are 40 metal layers and 39 intermediate layers. The thickness of the metal layer is 20 nm, the thickness of the intermediate layer is 2 nm, and the thickness of the conductive layer is 878 nm.
[0217] The preparation conditions of the metal layer are as follows: copper target (purity: 99.99%) as the target material, target power of 12.0 kW, argon flow rate of 50 mL / min, coating vacuum of 0.08 Pa, coating time of 2.0 s, and the temperature of the main roller during the coating process is -10 °C.
[0218] The intermediate layer preparation conditions are as follows: a nickel-chromium-copper target (purity: 99.99%) is used as the target material, the target power is 2.0 kW, the argon flow rate is 50 mL / min, the coating vacuum is 0.08 Pa, the main roller cooling temperature during the coating process is -10°C, and the coating time is 1 second. A PET composite film including an adhesive layer and a conductive layer is thus prepared.
[0219] The rest of the structure and preparation process are consistent with those in Example 1.
[0220] Example 21
[0221] The difference between this embodiment and embodiment 20 is that in the conductive layer of this embodiment, the metal layer is 45 layers, the intermediate layer is 44 layers, and the thickness of the conductive layer is 988 nm.
[0222] The rest of the structure and preparation process are consistent with Example 20.
[0223] Example 22
[0224] The difference between this embodiment and embodiment 12 is that in the conductive layer of this embodiment, there are 4 metal layers, 3 intermediate layers, and the thickness of the conductive layer is 815 nm.
[0225] The rest of the structure and preparation process are consistent with Example 12.
[0226] Example 23
[0227] The difference between this embodiment and embodiment 1 is that in the conductive layer of this embodiment, the thickness of the intermediate layer is 0.5 nm.
[0228] The preparation process of the intermediate layer is as follows: nickel-chromium-copper target (purity: 99.99%) is used as the target material, the target power is 2.0kW, the argon flow rate is 50mL / min, the coating vacuum is 0.08Pa, the coating time is 0.25s, and the main roller cooling temperature during the coating process is -20℃.
[0229] The rest of the structure and preparation process are consistent with those in Example 1.
[0230] Example 24
[0231] This embodiment differs from Example 1 in that the conductive layer in this embodiment has an intermediate layer thickness of 1 nm. The intermediate layer preparation process is as follows: a nickel-chromium-copper target (purity: 99.99%) is used as the target material, the target power is 2.0 kW, the argon flow rate is 50 mL / min, the coating vacuum is 0.08 Pa, the coating time is 0.5 s, and the main roller cooling temperature during the coating process is -20°C.
[0232] The rest of the structure and preparation process are consistent with those in Example 1.
[0233] Example 25
[0234] The difference between this embodiment and embodiment 1 is that in the conductive layer of this embodiment, the thickness of the intermediate layer is 10 nm.
[0235] The preparation process of the intermediate layer is as follows: nickel-chromium-copper target (purity: 99.99%) is used as the target material, the target power is 4.5kW, the argon flow rate is 50mL / min, the coating vacuum is 0.08Pa, the coating time is 2s, and the main roller cooling temperature during the coating process is -20°C.
[0236] The rest of the structure and preparation process are consistent with those in Example 1.
[0237] Example 26
[0238] The difference between this embodiment and embodiment 1 is that the bonding layer in this embodiment is titanium.
[0239] The bonding layer preparation process was as follows: a titanium target (purity: 99.99%) was used as the target material, the target power was 4.8 kW, the argon flow rate was 50 mL / min, the coating vacuum was 0.08 Pa, the coating time was 1 s, and the main roller cooling temperature during the coating process was -20°C. The bonding strength between the conductive layer and the base film in the prepared composite current collector was 100 N / m. The remaining structure and preparation process were consistent with Example 1.
[0240] Example 27
[0241] The difference between this embodiment and embodiment 1 is that the bonding layer in this embodiment is silicon oxide.
[0242] The bonding layer preparation process uses a silicon oxide target (99.99% purity) as the target material, a target power of 6 kW, an argon flow rate of 50 mL / min, a coating vacuum of 0.08 Pa, a coating time of 1 second, and a main roller cooling temperature of -20°C. The resulting composite current collector exhibits a bonding strength of 900 N / m between the conductive layer and the base film.
[0243] The rest of the structure and preparation process are consistent with those in Example 1.
[0244] Example 28
[0245] The difference between this embodiment and embodiment 1 is that a porous PET film (average pore size of 0.2 μm) is used in this embodiment, and the bonding force between the conductive layer and the base film in the prepared composite current collector is 1000 N / m.
[0246] The rest of the structure and preparation process are consistent with those in Example 1.
[0247] Example 29
[0248] The difference between this embodiment and embodiment 1 is that the functional layer structure in this embodiment is located on one side surface of the base film.
[0249] The rest of the structure and preparation process are consistent with those in Example 1.
[0250] Example 30
[0251] The difference between this embodiment and Example 1 is that no adhesive layer is provided in this comparative example, and the adhesive force between the conductive layer and the base film is 50 N / m.
[0252] The rest of the structure and preparation process are consistent with those in Example 1.
[0253] Example 31
[0254] Prepare the composite current collector as follows:
[0255] A 6μm thick biaxially oriented PET film was placed in a vacuum evaporation machine, and metal oxide layers and aluminum metal layers were alternately deposited on both sides of the biaxially oriented PET film in the thickness direction. The specific process conditions were as follows:
[0256] (a) Preparation of aluminum metal layer: The raw material is high-purity aluminum wire (purity: 99.93%), the heating temperature is 1200°C, the vacuum degree of the vacuum chamber is 0.1 Pa, and the deposition time is 20 s per deposition.
[0257] (b) Preparation of the metal oxide layer: The starting material was a high-purity metal wire (99.93%). During the evaporation process, the heating temperature was greater than the melting point of the metal wire. The gas source was oxygen at a flow rate of 100 mL / min. The vacuum level of the vacuum chamber was 0.3 Pa, and each deposition time was 0.3 s.
[0258] A multi-layer composite current collector was prepared according to the above-mentioned process conditions, wherein both sides of the PET film in the thickness direction had two aluminum metal layers and three aluminum oxide layers (metal oxide layers), and one side of the PET film in the thickness direction had a structure in which a metal oxide layer, an aluminum metal layer, a metal oxide layer, an aluminum metal layer, and a metal oxide layer were stacked in sequence, with each aluminum metal layer having a thickness of 500 nm and each metal oxide layer having a thickness of 5 nm.
[0259] Example 32
[0260] The preparation method of the composite current collector in this embodiment is the same as that in Example 31, with the following difference: in the process condition (a) for preparing the aluminum metal layer, the deposition time for each deposition is 2.1s; in the prepared composite current collector, both sides of the PET film in the thickness direction have 19 aluminum metal layers and 20 aluminum oxide layers, and the thickness of each aluminum metal layer is 53nm.
[0261] Example 33
[0262] The preparation method of the composite current collector in this embodiment is the same as that in Example 31, with the following differences: in the process conditions (a) for preparing the aluminum metal layer, the deposition time for each time is 0.8 s; in the process conditions (b) for preparing the metal oxide layer, the deposition time for each time is 0.1 s; in the prepared composite current collector, both sides of the PET film in the thickness direction have 50 aluminum metal layers and 51 aluminum oxide layers, the thickness of each aluminum metal layer is 20 nm, and the thickness of each metal oxide layer is 1.9 nm.
[0263] Example 34
[0264] Prepare the composite current collector as follows:
[0265] A 6μm thick biaxially oriented PET film was placed in a vacuum evaporation machine, and metal oxide layers and aluminum metal layers were alternately deposited on both sides of the biaxially oriented PET film in the thickness direction. The specific process conditions were as follows:
[0266] (a) Preparation of aluminum metal layer: The raw material is high-purity aluminum wire (purity: 99.93%), the heating temperature is 1200°C, the vacuum degree of the vacuum chamber is 0.1 Pa, and the deposition time is 2.1 s per deposition.
[0267] (b) Preparation of metal oxide layer: The target material was silicon oxide (99.95% purity), the target power supply was a DC power supply with a power density of 50 W / cm2, the vacuum degree of the vacuum chamber was 0.1 Pa, the gas source was argon with an argon flow rate of 60 mL / min, and each deposition time was 1.0 s;
[0268] A multi-layer composite current collector was prepared according to the above process conditions, in which both sides of the PET film in the thickness direction had 19 aluminum metal layers and 20 silicon oxide layers (metal oxide layers), the thickness of each aluminum metal layer was 53 nm, and the thickness of each metal oxide layer was 5 nm.
[0269] Example 35
[0270] Prepare the composite current collector as follows:
[0271] A 6μm thick biaxially oriented PET film was placed in a vacuum evaporation machine, and metal oxide layers and aluminum metal layers were alternately deposited on both sides of the biaxially oriented PET film in the thickness direction. The specific process conditions were as follows:
[0272] (a) Preparation of aluminum metal layer: The raw material is high-purity aluminum wire (purity: 99.93%), the heating temperature is 1200°C, the vacuum degree of the vacuum chamber is 0.1 Pa, and the deposition time is 2.1 s per deposition.
[0273] (b) Preparation of metal oxide layer: The target material was titanium oxide (99.95% purity), the target power supply was a DC power supply with a power density of 50 W / cm2, the vacuum degree of the vacuum chamber was 0.1 Pa, the gas source was argon with an argon flow rate of 60 mL / min, and the deposition time was 1.2 s per deposition.
[0274] A multi-layer composite current collector was prepared according to the above process conditions, in which both sides of the PET film in the thickness direction had 19 aluminum metal layers and 20 titanium oxide layers (metal oxide layers), the thickness of each aluminum metal layer was 53 nm, and the thickness of each metal oxide layer was 5 nm.
[0275] Example 36
[0276] Prepare the composite current collector as follows:
[0277] A 6μm thick biaxially oriented PET film was placed in a vacuum evaporation machine, and metal oxide layers and aluminum metal layers were alternately deposited on both sides of the biaxially oriented PET film in the thickness direction. The specific process conditions were as follows:
[0278] (a) Preparation of aluminum metal layer: The raw material is high-purity aluminum wire (purity: 99.93%), the heating temperature is 1200°C, the vacuum degree of the vacuum chamber is 0.1 Pa, and the deposition time is 2.1 s per deposition.
[0279] (b) Preparation of metal oxide layer: The target material was copper oxide (99.95% purity), the target power supply was a DC power supply with a power density of 50 W / cm2, the vacuum degree of the vacuum chamber was 0.1 Pa, the gas source was argon with an argon flow rate of 60 mL / min, and the deposition time was 1.5 s per deposition.
[0280] A multi-layer composite current collector was prepared according to the above process conditions, in which both sides of the PET film in the thickness direction had 19 aluminum metal layers and 20 copper oxide layers (metal oxide layers), the thickness of each aluminum metal layer was 53 nm, and the thickness of each metal oxide layer was 5 nm.
[0281] Example 37
[0282] Prepare the composite current collector as follows:
[0283] A 6μm thick biaxially oriented PET film was placed in a vacuum evaporation machine, and metal oxide layers and aluminum metal layers were alternately deposited on both sides of the biaxially oriented PET film in the thickness direction. The specific process conditions were as follows:
[0284] (a) Preparation of aluminum metal layer: The raw material is high-purity aluminum wire (purity: 99.93%), the heating temperature is 1200°C, the vacuum degree of the vacuum chamber is 0.1 Pa, and the deposition time is 2.1 s per deposition.
[0285] (b) Preparation of metal oxide layer: nickel oxide target (purity 99.95%), target power supply is a DC power supply with a power density of 50 W / cm2, vacuum chamber vacuum is 0.1 Pa, argon gas source is argon gas flow rate of 60 mL / min, and each deposition time is 1.3 s;
[0286] A multi-layer composite current collector was prepared according to the above process conditions, in which both sides of the PET film in the thickness direction had 19 aluminum metal layers and 20 copper oxide layers (metal oxide layers), the thickness of each aluminum metal layer was 53 nm, and the thickness of each metal oxide layer was 5 nm.
[0287] Example 38
[0288] The preparation method of the composite current collector in this embodiment is the same as that in Example 31, except that the PET film is replaced by a PEN film.
[0289] Example 39
[0290] The preparation method of the composite current collector in this embodiment is the same as that in Example 31, except that the PET film is replaced by a PP film.
[0291] Example 40
[0292] The preparation method of the composite current collector in this embodiment is the same as that in Example 31, except that the PET film is replaced by a PPS film.
[0293] Example 41
[0294] The preparation method of the composite current collector of this embodiment is the same as that of Example 31, except that: in the process condition (a) for preparing the aluminum metal layer, the deposition time is 10s each time; and in the prepared composite current collector, the thickness of each aluminum metal layer is 250nm.
[0295] Example 42
[0296] The preparation method of the composite current collector in this embodiment is the same as that in Example 31, except that: in the process condition (a) for preparing the aluminum metal layer, the deposition time is 40s each time; and in the prepared composite current collector, the thickness of each aluminum metal layer is 1000nm.
[0297] Example 43
[0298] The preparation method of the composite current collector in this embodiment is the same as that in Example 31, except that: in the process condition (a) for preparing the aluminum metal layer, the deposition time is 8s each time; and in the prepared composite current collector, the thickness of each aluminum metal layer is 200nm.
[0299] Example 44
[0300] The preparation method of the composite current collector of this embodiment is the same as that of Example 31, except that: in the process condition (b) for preparing the metal oxide layer, the deposition time for each deposition is 1.2 s; and in the prepared composite current collector, the thickness of each metal oxide layer is 20 nm.
[0301] Example 45
[0302] The preparation method of the composite current collector of this embodiment is the same as that of Example 31, except that: in the process condition (b) for preparing the metal oxide layer, the deposition time is 2.0 s each time; and in the prepared composite current collector, the thickness of each metal oxide layer is 33 nm.
[0303] Example 46
[0304] The preparation method of the composite current collector of this embodiment is the same as that of Example 31, except that: in the process condition (b) for preparing the metal oxide layer, the deposition time is 2.4s each time; and in the prepared composite current collector, the thickness of each metal oxide layer is 40nm.
[0305] Example 47
[0306] The preparation method of the composite current collector of this embodiment is the same as that of Example 31, except that the composite current collector of this embodiment has one aluminum metal layer and two aluminum oxide layers.
[0307] Example 48
[0308] The preparation method of the composite current collector of this embodiment is the same as that of Example 31, with the difference that: metal oxide layers and aluminum metal layers are alternately deposited on one side of the thickness direction of the biaxially oriented PET film. The composite current collector has 2 layers of aluminum metal layers and 3 layers of aluminum oxide layers. It is a structure in which PET film, metal oxide layer, aluminum metal layer, metal oxide layer, aluminum metal layer, and metal oxide layer are stacked in sequence. The thickness of each aluminum metal layer is 500 nm, and the thickness of each metal oxide layer is 5 nm.
[0309] Example 49
[0310] The preparation method of the composite current collector of this embodiment is the same as that of Example 31, except that:
[0311] In the prepared multilayer composite current collector, both sides of the PET film in the thickness direction have two aluminum metal layers and two aluminum oxide layers (metal oxide layers). One side of the PET film in the thickness direction is a structure in which aluminum metal layer, metal oxide layer, aluminum metal layer, and metal oxide layer are stacked in sequence. The thickness of each aluminum metal layer is 500 nm, and the thickness of each metal oxide layer is 5 nm.
[0312] Example 50
[0313] This embodiment provides a composite copper current collector, comprising:
[0314] Polymer base film, made of PET, with a thickness of 4.5 μm;
[0315] The bonding layers provided on both surfaces of the polymer base film are made of nickel-chromium alloy, have a thickness of 5 nm on a single side, and include a first bonding layer and a second bonding layer;
[0316] a composite copper layer disposed on a surface of the bonding layer on a side relatively far from the polymer base film, having a single-side thickness of 750 nm and comprising a first composite copper layer and a second composite copper layer, wherein the composite copper layer is formed by alternating amorphous copper layers and crystalline copper layers, wherein the side of the composite copper layer close to the bonding layer is the amorphous copper layer, and the side of the composite copper layer away from the bonding layer is the crystalline copper layer, wherein the number of amorphous copper layers is 5, each layer having a thickness of 50 nm, and the number of crystalline copper layers is 5, each layer having a thickness of 100 nm;
[0317] The protective layer disposed on the surface of the composite copper layer on the side relatively far from the polymer base film is made of carbon nanotubes, has a single-side thickness of 12 nm, and includes a first protective layer and a second protective layer.
[0318] This embodiment also provides a method for preparing the composite copper current collector, which comprises the following steps:
[0319] (1) PET film was prepared by melt-extrusion-biaxial stretching method;
[0320] (2) placing the PET film in a magnetron sputtering machine, and depositing a bonding layer on each side of the PET film. The specific process conditions are: using a nickel-chromium target (purity: 99.99%) as the target material, a target power of 5.0 kW, an argon flow rate of 50 mL / min, a coating vacuum of 0.08 Pa, a coating time of 1 s, and a main roller temperature of 0° C. during the coating process, to obtain a PET composite film having a bonding layer on the surface;
[0321] (3) The PET composite film containing the bonding layer on the surface is placed in a magnetron sputtering machine, and amorphous copper layers and crystalline copper layers are alternately deposited on both sides of the composite film to obtain a PET film containing a composite copper layer and a bonding layer; wherein, ① the number of amorphous copper layers is 5, and the preparation process conditions of each layer are as follows: a copper target (purity: 99.99%) is used as the target material, the target power is 5 kW, the gas source is argon, the argon flow rate is 60 mL / min, the coating vacuum is 0.09 Pa, the coating time is 15 s, and the cooling temperature of the main roller during the coating process is -30°C; ② the number of crystalline copper layers is 5, and the preparation process conditions of each layer are as follows: the electroplating solution components include 100 g / L copper sulfate, 120 g / L sulfuric acid, 50 mg / L chloride ion, 10 ppm sodium polydisulfide dipropane sulfonate, 2 ppm N,N-diethylthiourea and 100 ppm polyoxyethylene ether, and the average cathode current density is 1.7 A / dm 2 , the plating solution temperature is 25℃, and the plating time is 30s;
[0322] (4) 1.5 g of carbon nanotubes were uniformly dispersed in 998.5 g of nitrogen methyl pyrrolidone (NMP) solution by ultrasonic dispersion to prepare a coating solution with a solid content of 0.15 wt.%, and then the coating solution was uniformly coated on the surface of the PET film containing the composite copper layer and the adhesive layer by a die coating process. Finally, the film was dried at 100° C. to obtain a protective layer with a thickness of 12 nm, thereby obtaining the composite copper current collector.
[0323] Furthermore, to demonstrate that the composite copper layer of this embodiment comprises a laminated structure of an amorphous copper layer and a crystalline copper layer, two samples were first prepared according to the preparation method of this embodiment: a layer of amorphous copper was prepared on the surface of a PET film according to the preparation method for amorphous copper in this embodiment, namely, Sample 1; and a layer of crystalline copper was prepared on the surface of Sample 1 according to the preparation method for crystalline copper in this embodiment, namely, Sample 2. The samples were then prepared according to the requirements of an X-ray diffractometer and placed in an X-ray diffractometer (Bruker D8 ADVANCE) using copper as the target, with a scanning speed of 2.0000 deg / min and a scanning range of 30° to 80°. The test results are shown in Figure 4. As can be seen from the figure, no diffraction peak of copper was found in the diffraction pattern of sample 1, while diffraction peaks of copper (111), (200), (220) and other crystal plane orientations were found in sample 2. This shows that according to the preparation method of this embodiment, an amorphous copper layer and a crystalline copper layer can be prepared, that is, the composite copper layer prepared in this embodiment is a stacked structure of an amorphous copper layer and a crystalline copper layer.
[0324] Example 51
[0325] The difference between this embodiment and Example 50 is that the thickness of the amorphous copper layer is 20 nm, and the preparation process conditions of each layer are: using a copper target (purity: 99.99%) as the target material, the target power is 5 kW, the gas source is argon, the argon flow rate is 60 mL / min, the coating vacuum is 0.09 Pa, the coating time is 6 s, and the cooling temperature of the main roller during the coating process is -30°C.
[0326] The remaining preparation methods and parameters remained consistent with those in Example 50.
[0327] Example 52
[0328] The difference between this embodiment and Example 50 is that the thickness of the amorphous copper layer is 80 nm, and the preparation process conditions of each layer are: using a copper target (purity: 99.99%) as the target material, the target power is 5 kW, the gas source is argon, the argon flow rate is 60 mL / min, the coating vacuum is 0.09 Pa, the coating time is 24 s, and the cooling temperature of the main roller during the coating process is -30°C.
[0329] The remaining preparation methods and parameters remained consistent with those in Example 50.
[0330] Example 53
[0331] The difference between this embodiment and Example 50 is that the thickness of the amorphous copper layer is 100 nm, and the preparation process conditions of each layer are: using a copper target (purity: 99.99%) as the target material, the target power is 5 kW, the gas source is argon, the argon flow rate is 60 mL / min, the coating vacuum is 0.09 Pa, the coating time is 30 s, and the cooling temperature of the main roller during the coating process is -30°C.
[0332] The remaining preparation methods and parameters remained consistent with those in Example 50.
[0333] Example 54
[0334] The difference between this embodiment and embodiment 50 is that the thickness of the crystalline copper layer is 50 nm, and the preparation process conditions of each layer are as follows: the electroplating solution components include 100 g / L copper sulfate, 120 g / L sulfuric acid, 50 mg / L chloride ion, 10 ppm sodium polydisulfide propane sulfonate, 2 ppm N,N-diethylthiourea and 100 ppm polyoxyethylene ether, and the average cathode current density is 1.7 A / dm 2 , the plating solution temperature is 25℃, and the plating time is 15s;
[0335] The remaining preparation methods and parameters remained consistent with those in Example 50.
[0336] Example 55
[0337] The difference between this embodiment and embodiment 50 is that the thickness of the crystalline copper layer is 200 nm, and the preparation process conditions of each layer are as follows: the electroplating solution components include 100 g / L copper sulfate, 120 g / L sulfuric acid, 50 mg / L chloride ion, 10 ppm sodium polydisulfide propane sulfonate, 2 ppm N,N-diethylthiourea and 100 ppm polyoxyethylene ether, and the average cathode current density is 1.7 A / dm 2 , the plating solution temperature is 25℃, and the plating time is 60s;
[0338] The remaining preparation methods and parameters remained consistent with those in Example 50.
[0339] Example 56
[0340] The difference between this embodiment and embodiment 50 is that the thickness of the crystalline copper layer is 300 nm, and the preparation process conditions of each layer are as follows: the electroplating solution components include 100 g / L copper sulfate, 120 g / L sulfuric acid, 50 mg / L chloride ion, 10 ppm sodium polydisulfide propane sulfonate, 2 ppm N,N-diethylthiourea and 100 ppm polyoxyethylene ether, and the average cathode current density is 1.7 A / dm 2 , the plating solution temperature is 25℃, and the plating time is 90s;
[0341] The remaining preparation methods and parameters remained consistent with those in Example 50.
[0342] Example 57
[0343] The difference between this embodiment and embodiment 56 is that the number of layers of the amorphous copper layer and the crystalline copper layer are both 2.
[0344] The rest of the preparation methods and parameters remained the same as in Example 56.
[0345] Example 58
[0346] The difference between this embodiment and embodiment 50 is that the number of layers of the amorphous copper layer and the crystalline copper layer are both 10.
[0347] The remaining preparation methods and parameters remained consistent with those in Example 50.
[0348] Example 59
[0349] The difference between this embodiment and Example 50 is that the amorphous copper layer is prepared by vapor deposition, and the preparation process conditions of each layer are: copper wire (purity 99.99%) is used as the copper source, the heating evaporation temperature is 1500°C, the coating vacuum is 0.05Pa, the cooling temperature of the coating main roller is -30°C, and the coating time is 1.5s.
[0350] The remaining preparation methods and parameters remained consistent with those in Example 50.
[0351] Example 60
[0352] The difference between this embodiment and Example 50 is that the amorphous copper layer is prepared in two steps of magnetron sputtering and evaporation, and the preparation process conditions of each layer are as follows: ① Preparation of 20nm amorphous copper by magnetron sputtering: using a copper target (purity: 99.99%) as the target material, the target power is 5kW, the gas source is argon, the argon flow rate is 60mL / min, the coating vacuum is 0.09Pa, the coating time is 6s, and the temperature of the main roller during the coating process is -30℃; ② Preparation of 30nm amorphous copper by evaporation: using copper wire (purity 99.99%) as the copper source, the heating evaporation temperature is 1500℃, the coating vacuum is 0.05Pa, the coating main roller cooling temperature is -30℃, and the coating time is 0.9s.
[0353] The remaining preparation methods and parameters remained consistent with those in Example 50.
[0354] Example 61
[0355] The difference between this embodiment and embodiment 50 is that the number of layers of the amorphous copper layer and the crystalline copper layer is 1, and the thickness of the amorphous copper layer in the conductive layer is 100 nm, and the thickness of the crystalline copper layer is 300 nm. The preparation process conditions of the amorphous copper layer are as follows: a copper target (purity: 99.99%) is used as the target material, the target power is 5 kW, the gas source is argon gas with an argon gas flow rate of 60 mL / min, the coating vacuum is 0.09 Pa, the coating time is 30 s, and the cooling temperature of the main roller during the coating process is -30°C. The preparation process conditions of the crystalline copper layer are as follows: the electroplating solution composition includes 100 g / L copper sulfate, 120 g / L sulfuric acid, 50 mg / L chloride ion, 10 ppm sodium polydisulfide dipropane sulfonate, 2 ppm N,N-diethylthiourea, and 100 ppm polyoxyethylene ether, the average cathode current density is 1.7 A / dm2, the plating solution temperature is 25°C, and the electroplating time is 90 s.
[0356] The remaining preparation methods and parameters remained consistent with those in Example 50.
[0357] Example 62
[0358] The difference between this embodiment and Example 50 is that the thickness of the amorphous copper layer is 120 nm, and the preparation process conditions of each layer are: using a copper target (purity: 99.99%) as the target material, the target power is 5 kW, the gas source is argon, the argon flow rate is 60 mL / min, the coating vacuum is 0.09 Pa, the coating time is 36 s, and the cooling temperature of the main roller during the coating process is -30°C.
[0359] The remaining preparation methods and parameters remained consistent with those in Example 50.
[0360] Example 63
[0361] The difference between this embodiment and embodiment 50 is that the thickness of the crystalline copper layer is 320 nm, and the preparation process conditions of each layer are as follows: the electroplating solution components include 100 g / L copper sulfate, 120 g / L sulfuric acid, 50 mg / L chloride ion, 10 ppm sodium polydisulfide propane sulfonate, 2 ppm N,N-diethylthiourea and 100 ppm polyoxyethylene ether, and the average cathode current density is 1.7 A / dm 2 , the bath temperature is 25°C, and the plating time is 96s;
[0362] The remaining preparation methods and parameters remained consistent with those in Example 50.
[0363] Example 64
[0364] This embodiment provides a composite current collector, which includes a polymer base film and a composite conductive layer provided on both sides of the polymer base film.
[0365] The composite conductive layer includes an intermediate layer and a metal layer alternately stacked, the intermediate layer includes a fluorocarbon material, and the fluorocarbon material is a fluorocarbon polymer;
[0366] The chemical composition of the fluorocarbon polymer is C x F y , wherein x / y=5, and the weight average molecular weight of the fluorocarbon polymer is 32000 Da;
[0367] The number of the intermediate layers is 10, the thickness of a single intermediate layer is 5 nm, the number of the metal layers is 10, the material of the metal layers is copper, and the thickness of a single metal layer is 50 nm;
[0368] The thickness of the composite conductive layer provided on one surface of the polymer base film is 550 nm;
[0369] The thickness of the polymer base film is 4.5 μm and the material is PET;
[0370] A protective layer is provided on the surface of the composite conductive layer away from the polymer base film, wherein the thickness of the protective layer is 5 nm and the material is graphene;
[0371] The thickness of the composite current collector is 5.61 μm.
[0372] This embodiment also provides a method for preparing the composite current collector, which comprises the following steps:
[0373] (1) placing a PET film prepared by a melt-extrusion-biaxial stretching method in a magnetron sputtering machine, and alternately depositing an intermediate layer and a copper layer on both sides of the PET film, wherein the number of intermediate layers is 10 and the number of copper layers is 10, to obtain a PET composite film containing a composite conductive layer;
[0374] The process parameters for preparing a single layer of the intermediate layer include: using a graphite-polytetrafluoroethylene mixture target (the mass ratio of graphite to polytetrafluoroethylene is 2.16:1) as the target material, a target power of 3 kW, an argon flow rate of 50 mL / min, a coating vacuum of 0.08 Pa, a coating time of 1 s, and a main roller temperature of 0°C during the coating process;
[0375] The process parameters for preparing a single layer of copper include: using a copper target (purity of 99.99%) as the target material, a target power of 12 kW, an argon flow rate of 50 mL / min, a coating vacuum of 0.08 Pa, a coating time of 5 s, and a main roller temperature of 2°C during the coating process;
[0376] (2) The PET composite film prepared above is placed in a coating device, and a graphene solution with a solid content of 0.1 wt.% (the solvent is nitrogen methyl pyrrolidone) is used as the coating liquid. The coating liquid is then evenly coated on both sides of the PET composite film through a die coating process, and finally dried at 70°C to obtain a protective layer with a single-sided thickness of 5 nm, and finally the composite current collector is obtained.
[0377] Example 65
[0378] The difference between this embodiment and Example 64 is that the thickness of the single layer of the metal layer in the composite conductive layer is 100 nm, and the coating time in the preparation process parameters of the single layer is adjusted to 10 s.
[0379] The rest of the preparation methods and parameters remained the same as in Example 64.
[0380] Example 66
[0381] The difference between this embodiment and Example 64 is that the thickness of the single layer of the metal layer in the composite conductive layer is 150 nm, and the coating time in the preparation process parameters of the single layer is adjusted to 15 s.
[0382] The rest of the preparation methods and parameters remained the same as in Example 64.
[0383] Example 67
[0384] The difference between this embodiment and Example 64 is that the thickness of the single layer of the metal layer in the composite conductive layer is 200 nm, and the coating time in the preparation process parameters of the single layer is adjusted to 20 s.
[0385] The rest of the preparation methods and parameters remained the same as in Example 64.
[0386] Example 68
[0387] The difference between this embodiment and Example 65 is that the single layer thickness of the middle layer in the composite conductive layer is 2 nm, and the coating time in the preparation process parameters of the single layer is adjusted to 0.4 s.
[0388] The rest of the preparation methods and parameters remained the same as in Example 65.
[0389] Example 69
[0390] The difference between this embodiment and Example 65 is that the single layer thickness of the middle layer in the composite conductive layer is 20 nm, and the coating time in the preparation process parameters of the single layer is adjusted to 4 s.
[0391] The rest of the preparation methods and parameters remained the same as in Example 65.
[0392] Example 70
[0393] The difference between this embodiment and Example 65 is that the single layer thickness of the middle layer in the composite conductive layer is 50 nm, and the coating time in the preparation process parameters of the single layer is adjusted to 10 s.
[0394] The rest of the preparation methods and parameters remained the same as in Example 65.
[0395] Example 71
[0396] The difference between this embodiment and Example 65 is that the number of layers of the intermediate layer and the metal layer are both 3, and the single layer thickness of the metal layer is 200nm. At the same time, the coating time in the single layer preparation process parameters is adjusted to 20s.
[0397] The rest of the preparation methods and parameters remained the same as in Example 65.
[0398] Example 72
[0399] The difference between this embodiment and embodiment 65 is that the number of layers of the intermediate layer and the metal layer are both 5.
[0400] The rest of the preparation methods and parameters remained the same as in Example 65.
[0401] Example 73
[0402] The difference between this embodiment and embodiment 65 is that the number of layers of the intermediate layer and the metal layer are both 15.
[0403] The rest of the preparation methods and parameters remained the same as in Example 65.
[0404] Example 74
[0405] The difference between this embodiment and Example 64 is that the material of the metal layer is aluminum. At the same time, in the preparation process parameters of the single layer, the target material is adjusted to an aluminum target with a purity of 99.99%, the target power is adjusted to 10kW, the coating vacuum is adjusted to 0.07Pa, and the temperature of the main roller during the coating process is adjusted to 0°C.
[0406] The rest of the preparation methods and parameters remained the same as in Example 64.
[0407] Example 75
[0408] The difference between this embodiment and Example 64 is that the material of the polymer base film is adjusted to PP.
[0409] The rest of the preparation methods and parameters remained consistent with those in Example 64.
[0410] Example 76
[0411] The difference between this embodiment and embodiment 64 is that the chemical composition of the fluorocarbon polymer in the middle layer is C xF y , where x / y = 0.6. Meanwhile, in the single-layer preparation process parameters, the mass ratio of graphite to polytetrafluoroethylene in the target material is adjusted to 0.048:1, and the target power is adjusted to 5 kW.
[0412] The rest of the preparation methods and parameters remained consistent with those in Example 64.
[0413] Example 77
[0414] The difference between this embodiment and embodiment 64 is that the chemical composition of the fluorocarbon polymer in the middle layer is C x F y , where x / y=10. At the same time, in the single-layer preparation process parameters, the mass ratio of graphite to polytetrafluoroethylene in the target material is adjusted to 4.56:1, and the target power is adjusted to 5kW.
[0415] The rest of the preparation methods and parameters remained consistent with those in Example 64.
[0416] Example 78
[0417] The difference between this embodiment and Example 64 is that the thickness of the single layer of the metal layer in the composite conductive layer is 220 nm, and the coating time in the preparation process parameters of the single layer is adjusted to 22 s.
[0418] The rest of the preparation methods and parameters remained consistent with those in Example 64.
[0419] Example 79
[0420] The difference between this embodiment and Example 65 is that the single layer thickness of the middle layer in the composite conductive layer is 55 nm, and the coating time in the preparation process parameters of the single layer is adjusted to 11 s.
[0421] The rest of the preparation methods and parameters remained the same as in Example 65.
[0422] Example 80
[0423] The difference between this embodiment and Example 65 is that the single layer thickness of the middle layer in the composite conductive layer is 1 nm, and the coating time in the preparation process parameters of the single layer is adjusted to 0.2 s.
[0424] The rest of the preparation methods and parameters remained the same as in Example 65.
[0425] Example 81
[0426] The difference between this embodiment and embodiment 65 is that the number of layers of the intermediate layer and the metal layer are both 16.
[0427] The rest of the preparation methods and parameters remained the same as in Example 65.
[0428] Example 82
[0429] The difference between this embodiment and embodiment 71 is that the number of layers of the intermediate layer and the metal layer are both 2.
[0430] The rest of the preparation methods and parameters remained consistent with Example 71.
[0431] Example 83
[0432] The difference between this embodiment and embodiment 64 is that the chemical composition of the fluorocarbon polymer in the middle layer is C x F y , where x / y = 0.55. At the same time, in the preparation process parameters of the single layer, the mass ratio of graphite to polytetrafluoroethylene in the target material is adjusted to 0.024:1, and the target power is adjusted to 6 kW.
[0433] The rest of the preparation methods and parameters remained the same as in Example 64.
[0434] Example 84
[0435] The difference between this embodiment and embodiment 64 is that the chemical composition of the fluorocarbon polymer in the middle layer is C x F y , where x / y=11. Meanwhile, in the single-layer preparation process parameters, the mass ratio of graphite to polytetrafluoroethylene in the target material is adjusted to 5.04:1, and the target power is adjusted to 6 kW.
[0436] The rest of the preparation methods and parameters remained the same as in Example 64.
[0437] Comparative Example 1
[0438] The difference between this comparative example and Example 1 is that the conductive layer in this comparative example does not contain an intermediate layer (ie, the conductive layer is a pure metal layer), and the thickness of the metal layer is 1030 nm.
[0439] The metal layer was prepared using a copper target (purity: 99.99%) as the target material, a target power of 12.0 kW, an argon flow rate of 50 mL / min, a coating vacuum of 0.08 Pa, a coating time of 103 s, and a main roller temperature of -10°C during the coating process. The remaining structure and preparation process remained consistent with Example 1.
[0440] Comparative Example 2
[0441] The preparation method of the composite current collector of Comparative Example 2 is the same as that of Example 31, with the difference that a layer of aluminum metal is deposited on both sides of the thickness direction of the biaxially oriented PET film, the deposition time is 40s, and the thickness of the aluminum metal layer on one side of the PET film is 1000nm.
[0442] Comparative Example 3
[0443] The difference between this comparative example and Example 50 is that the composite copper layer is a single-layer copper layer, and the specific preparation process is: using a copper target (purity: 99.99%) as the target material, the target power is 12kW, the argon flow rate is 50mL / min, the coating vacuum is 0.08Pa, the coating time is 100s, and the temperature of the main roller during the coating process is 2°C.
[0444] The remaining preparation methods and parameters remained consistent with those in Example 50.
[0445] Comparative Example 4
[0446] The difference between this comparative example and Example 64 is that the composite conductive layer does not contain an intermediate layer, that is, it only contains a metal layer with a single-sided thickness of 500 nm, and the coating time in the preparation process parameters is adjusted to 50s.
[0447] The rest of the preparation methods and parameters remained consistent with those in Example 64.
[0448] Comparative Example 5
[0449] The difference between this comparative example and Example 64 is that the middle layer is replaced by a carbon layer, and the target material in the single-layer preparation process parameters is adjusted to a graphite target material.
[0450] The rest of the preparation methods and parameters remained consistent with those in Example 64.
[0451] The performance of the composite current collectors provided in the examples and comparative examples was tested:
[0452] 1. Square resistance: Place the prepared flat composite current collector sample on the sample stage and use a four-probe square resistance meter to test the square resistance of the sample.
[0453] 2. Safety performance:
[0454] ①Battery assembly:
[0455] i. For lithium-ion battery assembly based on composite aluminum current collector: For the positive electrode, the positive electrode current collector adopts the composite aluminum (i.e., the metal element in the metal layer is aluminum) current collector prepared in the present disclosure (e.g., Example 11, Example 74, etc.), and the positive electrode material adopts LiNi 0.6 Mn 0.2 Co 0.2 O2 (NCM622); for the negative electrode: the negative electrode current collector uses traditional copper foil (thickness of 6 microns), and the negative electrode material uses artificial graphite; for the diaphragm, alumina ceramic coated polyethylene diaphragm (thickness of 25 microns) is used; for the electrolyte, a 1 mol / L LiPF6 carbonate solution is used, and the carbonates are propylene carbonate, ethylene carbonate, and ethyl methyl carbonate, and the mass ratio of the three is 1:1:1; use the above materials to assemble the lithium-ion battery according to the relevant process.
[0456] ii. For lithium-ion battery assembly based on composite copper current collector (i.e. the metal element in the metal layer is copper): for the positive electrode, the positive electrode current collector adopts a traditional aluminum current collector (thickness of 13 microns), and the positive electrode material adopts LiNi 0.6 Mn 0.2 Co 0.2 O2 (NCM622); for the negative electrode: the negative electrode current collector adopts the composite copper current collector prepared by the present invention (for example, the composite current collector provided in Examples 64-73, Examples 75-84 and Comparative Examples 4-5), and the negative electrode material adopts artificial graphite; for the diaphragm, an alumina ceramic-coated polyethylene diaphragm (thickness 25 microns) is adopted; for the electrolyte, a 1 mol / L LiPF6 carbonate solution is adopted, and the carbonates are propylene carbonate, ethylene carbonate, and ethyl methyl carbonate, and the mass ratio of the three is 1:1:1; the above materials are used to assemble a lithium-ion battery according to the relevant process.
[0457] ② Safety Performance Test: A needle penetration test was performed to verify the battery's safety performance. Specifically, the prepared battery was placed in a needle penetration test apparatus with a 3mm diameter needle, a penetration speed of 10mm / s, a sampling interval of 100ms, and a sampling time of 15 minutes. The maximum temperature of the battery after the penetration process and the battery voltage after the penetration were recorded to indicate the battery's safety performance. The lower the maximum temperature and the higher the battery voltage after the penetration, the better the battery's safety performance.
[0458] ③ Needle puncture pass rate test: A needle puncture test is used to verify the safety performance of the battery, as follows: 100 batteries prepared as described above are taken and placed in a needle puncture test device, wherein the diameter of the steel needle is 3mm and the puncture speed is 10mm / s. If the battery does not explode, catch fire or smoke during the puncture, it passes; otherwise, it fails. The number of batteries that pass and fail is recorded, and the battery needle puncture pass rate can be obtained, that is, the number of batteries that pass / the total number of batteries × 100%.
[0459] 3. Tensile strength and elongation at break: The tensile strength and elongation at break of the prepared composite current collector were tested with reference to GB / T 1040.3-2006.
[0460] 4. Thermal shrinkage: The thermal shrinkage of the prepared composite current collector was tested with reference to GB / T 10003-2008, with the heat treatment condition being 150°C for 30 min.
[0461] 5. The overall morphology and local morphology of the composite current collectors prepared in Example 32 and Comparative Example 2 were observed using a transmission electron microscope. The results are shown in Figures 2-3.
[0462] 6. Electrochemical performance test
[0463] (6.1) Assembly of lithium-ion batteries
[0464] Preparation of positive electrode sheet: The positive electrode current collector adopts the composite current collector prepared in each embodiment and comparative example, and the positive electrode active material is LiNi 0.6 Mn 0.2 Co 0.2 O2 (NCM622), the conductive agent is carbon nanotubes, the binder is polyvinylidene fluoride (PVDF), and the solvent is N-methylpyrrolidone (NMP). The above-mentioned positive electrode active material, conductive agent, binder and solvent are prepared into a positive electrode slurry with a certain fluidity according to the mass ratio of 67.2%:9.4%:1.1%:22.3% (the mass of the positive electrode slurry is 100%), coated on the positive electrode current collector, and dried to form a positive electrode sheet;
[0465] Preparation of negative electrode sheet: The negative electrode current collector uses traditional copper foil (thickness of 6 μm), the negative electrode active material uses artificial graphite, the conductive agent is carbon nanotubes, the binder is sodium carboxymethyl cellulose (CMC), and the solvent is pure water. The above negative electrode active material, conductive agent, binder and solvent are prepared in a mass ratio of 48.0%:5.0%:19.4%:27.6% to form a negative electrode slurry with a certain fluidity (the mass of the negative electrode slurry is 100%), which is coated on the negative electrode current collector and dried to form a negative electrode sheet;
[0466] The positive and negative electrode sheets were prepared into lithium-ion batteries through rolling, slicing, assembly, injection, and packaging. The separator used a polyethylene diaphragm coated with alumina ceramic (thickness 25 μm), and the electrolyte used was 1 mol·L -1 The carbonate solution of LiPF6, the carbonates are propylene carbonate, ethylene carbonate, and ethyl methyl carbonate, and the mass ratio of the three is 1:1:1.
[0467] (6.2) Cycle the assembled lithium-ion battery for 600 cycles at a charge / discharge rate of 1C, and record the battery capacity retention rate after the cycle. The voltage range of the cycle charge and discharge is 3.0V-4.2V. The capacity retention rate (%) of the battery after 600 cycles = the battery's 600th discharge capacity / the battery's 600th charge capacity × 100%. Alternatively, cycle the battery for 2000 cycles at a charge / discharge rate of 1C, and record the battery capacity retention rate after 2000 cycles, i.e., the battery capacity after 2000 cycles / the battery's initial capacity × 100%.
[0468] Table 1 shows the specific test results of the above safety tests.
[0469] Table 1
[0470] The results of acupuncture penetration rate are shown in Table 2
[0471] Table 2
[0472] From the test results of Examples 1-29 and Comparative Example 1, it can be seen that compared with the traditional composite current collector, the safety performance of the battery based on the composite current collector proposed in the present disclosure is significantly improved.
[0473] From the test results of Examples 1-9, it can be seen that compared with the composite current collector with a single material as the intermediate layer, the composite current collector with a combined material as the intermediate layer has a better effect on improving the battery safety performance.
[0474] From the test results of Examples 1 and 11-13, it can be seen that with the increase in the thickness of the metal layer, the safety performance of the battery based on the prepared composite current collector first increases and then decreases. However, when the thickness exceeds a certain range, the safety performance deteriorates significantly. This is because the metal layer is too thick, resulting in the length of the columnar crystals in the layer being too long, and cracks are not easily propagated during the needle puncture process.
[0475] From the test results of Example 1 and Examples 14-16, it can be seen that the larger the average particle size of the metal grains in the metal layer, the greater the maximum temperature rise of the battery during the needling process and the greater the drop in the battery voltage after needling, that is, the battery safety performance deteriorates. This is because the smaller the grains, the more they can promote the propagation of microcracks generated in the metal layer during the needling process, and cause large-scale fractures, thereby separating the metal layer from the steel needle; while if the grains are too large, the plasticity of the metal layer will become stronger, which is not conducive to the large-scale fission of the metal layer during the needling process, thereby making the prepared composite current collector less effective in improving the safety of the battery.
[0476] Compared with Example 1, the maximum temperature rise during the needling process in Example 17 reached 128°C, and the battery voltage was 0.9 after 300 seconds of needling, indicating a serious deterioration in safety performance. This is because when the intermediate layer is in direct contact with the adhesive layer, the adhesion between the metal layer and the polymer film is too high, making it difficult for local micro-deformation to occur during the needling process.
[0477] This is detrimental to the diffusion of microcracks, thus failing to improve safety performance. The test results of Examples 1 and 18-22 show that if the number of metal layers is too small, less than 5, the maximum temperature rise during the needle puncture process increases significantly, and the voltage after the needle puncture decreases significantly, seriously deteriorating the safety improvement effect. If the number of metal layers exceeds 40, the battery safety performance cannot be further improved, and production efficiency is affected, increasing production difficulty. Therefore, the optional number of layers ranges from 5 to 40.
[0478] From the test results of Example 1 and Examples 23-25, it can be seen that: within the appropriate range, the thickness of the intermediate layer has little effect on the change in resistance, that is, it has little effect on the conductivity of the composite current collector. This shows that if the thickness of the intermediate layer is well controlled, the alternating stacking structure formed by the metal layer and the intermediate layer will not significantly affect the conductivity of the composite current collector. The thicker the intermediate layer, the better the safety performance of the battery based on the prepared composite current collector. This is because the thicker the intermediate layer is within the appropriate range, the better the effect of inhibiting the continuous growth of the metal layer grains, and the more effectively it can block the connection between different metal layers. When the intermediate layer is too thin, it cannot effectively inhibit the continuous growth of the metal layer grains, resulting in partial penetration of the grains of adjacent metal layers, causing the safety performance of the battery to deteriorate sharply.
[0479] The test results of Examples 1, 26-28, and 30 show that as the bonding strength between the conductive layer and the base film increases, the safety performance of the battery based on the prepared composite current collector first improves and then decreases. This is because if the bonding strength is too low, the conductive layer is prone to excessive relative movement with the polymer film during the battery needle puncture process, which is not conducive to providing sufficient force along the surface of the conductive layer to inhibit the large-scale expansion and propagation of cracks in the conductive layer, thereby weakening the battery's safety performance. If the bonding strength is too high, local micro-deformation is difficult to occur, which is not conducive to the large-scale expansion and propagation of cracks in the conductive layer, affecting the improvement of battery safety performance. Furthermore, if the composite current collector does not have an adhesive layer, it is not conducive to a significant improvement in battery safety performance.
[0480] From the data results of Example 1 and Comparative Example 1, it can be seen that the composite current collector structure provided by the present invention and the structures in the functional layer must cooperate with each other to ultimately achieve the separation of the conductive layer and the steel needle during the needling process, avoid the positive and negative current collectors from being turned on to form a closed loop and the resulting thermal runaway of the battery, thereby greatly improving the safety performance of the battery.
[0481] It can be seen from Examples 50-63 and Comparative Example 3 that, compared with the traditional composite copper current collector, the composite copper current collector prepared in the present application has improved tensile strength (mechanical properties), and the puncture pass rate of the battery based on the prepared composite current collector is improved, that is, the safety performance is improved, which is due to the stacked structure of amorphous copper and crystalline copper in the conductive layer.
[0482] It can be seen from Examples 50-53 and Example 62 that as the thickness of the amorphous copper in the conductive layer increases, the tensile strength of the composite current collector first increases and then decreases. This is because the introduction of thinner amorphous copper can provide a buffer for the movement of the crystalline copper during the stretching process, thereby improving the tensile strength of the composite current collector. However, if the thickness is too high and the thickness ratio of the amorphous copper to the crystalline copper is too high, the conductive layer will exhibit certain characteristics of amorphous copper, resulting in a decrease in tensile strength. As the thickness of the amorphous copper in the conductive layer increases, the needle penetration rate of the battery based on the prepared composite current collector shows an upward trend, while if the thickness is too high, the needle penetration rate decreases. This is because as the thickness of the amorphous copper increases, the amorphous copper layer is prone to cracking during needle penetration deformation, and the cracks generated are more likely to spread rapidly to the surrounding area, thereby more likely to cause large-scale fractures in the adjacent crystalline copper layer, thereby improving the safety performance of the battery. However, when the thickness is too high, amorphous copper will transform into crystalline copper during the preparation process, which makes it difficult for cracks to form during the needle puncture process and for the cracks to spread to the surrounding areas, thereby reducing the safety performance of the battery.
[0483] It can be seen from Examples 50, 54-56 and 63 that as the thickness of the crystalline copper in the conductive layer increases, the tensile strength of the composite copper current collector and the needle penetration rate of the battery based on the composite copper current collector both show a downward trend. This is because with the increase in the thickness of the crystalline copper, the size of the copper grains along the thickness square becomes larger, resulting in a decrease in the tensile strength of the composite copper current collector, and the grain size becomes larger, which is not conducive to the amorphous copper driving the crystalline copper to produce large-area cracks, resulting in a decrease in the needle penetration rate and poor safety performance.
[0484] It can be seen from Examples 50, 57, 58 and 61 that with the increase in the number of amorphous copper and crystalline copper layers in the conductive layer, the tensile strength of the prepared composite current collector first increases and then decreases, while the needle penetration rate of the battery based on the composite copper current collector shows an increasing trend. This is because the increase in the number of layers can promote the generation of cracks in the conductive layer during the needle penetration process and quickly spread to the surrounding area, thereby improving the safety performance of the battery.
[0485] It can be seen from Example 50, Example 59 and Example 60 that the composite copper current collector prepared by the amorphous copper layer prepared by the combination of magnetron sputtering and evaporation has a better effect on improving the safety performance of the battery.
[0486] Table 3 shows the test results of mechanical properties and electrochemical properties
[0487] Table 3
[0488] It can be seen from Table 3 that compared with Comparative Example 2, the tensile strength, elongation at break and cycle performance of the composite current collectors prepared in Examples 31-49 are significantly improved, indicating that the provided metal oxide layer improves the elongation at break and tensile strength of the composite current collector, while inhibiting the corrosion of the composite current collector by the electrolyte to a certain extent, thereby improving the stability of the composite current collector.
[0489] By comparing the square resistance data of Examples 31-40, Example 44, Example 45, and Comparative Example 2, it can be found that when the total thickness of the metal layer in the composite current collector is basically the same, the alternating stacking structure formed by the metal layer and the metal oxide layer in Examples 31-40, Example 44, and Example 45 will not significantly affect the conductivity of the composite current collector. Since the total thickness of the metal layer of the composite current collector of Examples 41-43 and Example 47 is quite different from the total thickness of the metal layer of Example 31, the square resistance of the composite current collector of Examples 41-43 changes greatly accordingly. Compared with Example 31, the square resistance of the composite current collector of Example 46 is higher, which is caused by the higher proportion of the thickness of the metal oxide layer therein. Compared with Example 31, the thermal shrinkage rate of the composite current collector of Example 43 is higher, which is due to the large difference in the total thickness of the metal layer in the current collector of Example 43 and the total thickness of the metal layer in the current collector of Example 31. In addition, although the square resistance or thermal shrinkage of the composite current collectors of Examples 41-43 and Example 47 changed, the capacity retention rate of the batteries of Examples 41-43 and Example 47 was still significantly higher than the capacity retention rate of the battery of Comparative Example 2.
[0490] Table 4 shows the battery capacity retention and needle penetration rate of some examples after 2000 cycles
[0491] Table 4
[0492] In addition, the elongation at break of Example 64 and Comparative Example 5 was also tested. The testing method for the elongation at break was as follows: sampling was performed longitudinally along the prepared composite current collector, and then the elongation at break was tested in accordance with the national standard GB / T 1040.3-2006.
[0493] The test results are shown in Table 5.
[0494] Table 5
[0495] It can be seen from Tables 4 and 5 above that, compared with traditional composite current collectors, due to the introduction of the intermediate layer, the prepared composite current collector can improve the capacity retention rate and needle penetration rate of the battery, that is, improve the cycle charge and discharge performance and safety performance of the battery.
[0496] As shown in Examples 64-67 and 78, increasing the thickness of the metal layer leads to an initial increase and then a decrease in the cycle charge-discharge performance and safety performance of batteries based on composite copper current collectors. This is likely because changes in the thickness of the metal layer affect the size of the grains along the thickness direction within the metal layer, which in turn affects the fracture behavior of the metal layer during needle penetration, resulting in changes in safety performance. Furthermore, changes in the grain size along the thickness direction also affect the conduction resistance of electrons during the battery's charge and discharge process, thereby affecting the battery's cycle charge-discharge performance.
[0497] As shown in Examples 65, 68-70, and 79-80, increasing the thickness of the intermediate layer improves the cyclic charge-discharge performance of batteries based on composite copper current collectors. However, exceeding a certain thickness deteriorates the cyclic charge-discharge performance. This may be because increasing the thickness of the intermediate layer improves the barrier and tolerance of the intermediate layer to the electrolyte, thereby promoting the improvement of the cyclic charge-discharge performance of batteries based on the composite copper current collector. However, excessive thickness of the intermediate layer affects the conductivity of the conductive layer, causing the cyclic charge-discharge performance of batteries based on the composite copper current collector to deteriorate. Increasing the thickness of the intermediate layer also shows a trend of first improving and then remaining unchanged in the safety performance of batteries based on the composite copper current collector. This may be because increasing the thickness of the intermediate layer promotes large-scale fission of the conductive layer during the needle puncture process, making it easier for the conductive layer to disconnect from the steel needle, thereby promoting the improvement of the safety performance of batteries based on the composite copper current collector. However, when the thickness exceeds a certain value, this effect is no longer further promoted, resulting in unchanged safety performance.
[0498] As can be seen from Example 65, Examples 71-73, Examples 81-82, and Comparative Example 4, increasing the number of metal layers and intermediate layers shows an improvement in the cycle charge and discharge performance and safety performance of the battery based on the composite copper current collector. This may be because increasing the number of layers can, on the one hand, improve the multi-layer alternating structure of the intermediate layer and the metal layer, promote layer-by-layer protection of the metal layer, and thus promote the improvement of the cycle charge and discharge performance of the battery; on the other hand, increasing the number of layers can promote the conductive layer to be more prone to large-scale fission during the needle puncture process, thereby causing the conductive layer to be more easily disconnected from the steel needle, thereby promoting the improvement of the safety performance of the battery based on the composite copper current collector. However, when the number of layers exceeds 15 layers, the performance improvement is not obvious. Considering the preparation efficiency of the composite current collector, the optional number of layers is 5-15 layers.
[0499] It can be seen from Examples 64, 76-77 and 83-84 that the chemical composition of the fluorocarbon polymer in the intermediate layer is CxFy. If x / y is too low, the carbon content is too low, resulting in poor conductivity of the intermediate layer, thereby causing the conductivity of the prepared composite current collector to deteriorate, resulting in poor cycle performance of the battery; if x / y is too high, the carbon content is too high, the flexibility of the intermediate layer deteriorates, and defects are easily generated, resulting in poor cycle performance of the battery.
[0500] As shown in Example 64 and Comparative Example 5, replacing the fluorocarbon layer with a carbon layer improves the overall performance of the conventional composite current collector, such as increasing corrosion resistance. However, the addition of the carbon layer also reduces the material's elongation at break, making it more susceptible to breakage during the electrode preparation process, resulting in a lower yield rate for the prepared battery electrode. This is because the carbon layer is more brittle than the fluorocarbon polymer, and its presence increases the brittleness of the overall material.
[0501] In summary, the composite current collector structure provided by the present invention, through the coordinated cooperation of various structural layers in the functional layer, can achieve the generation of microcracks in the conductive layer during the needling process, and quickly spread to cause large-scale fractures, thereby achieving separation of the conductive layer and the steel needle, avoiding the formation of a closed loop by the positive and negative current collectors and the resulting thermal runaway of the battery, thereby improving the safety performance of the battery and promoting the promotion and application of the composite current collector.
[0502] The applicant declares that the above is only a specific embodiment of the present disclosure, but the protection scope of the present disclosure is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed in the present disclosure fall within the protection scope and disclosure scope of the present disclosure.
Claims
1. A composite current collector, wherein: The composite current collector includes a conductive layer, and the conductive layer includes alternately stacked metal layers and intermediate layers.
2. The composite current collector according to claim 1, wherein: The composite current collector includes a base film and a functional layer located on at least one side of the base film; the functional layer includes the conductive layer.
3. The composite current collector according to claim 1 or 2, wherein: The thickness of the base film is 1 - 10 μm; optionally, the material of the base film includes any one or a combination of at least two of polyethylene terephthalate, polypropylene, polybutylene terephthalate, polyethylene naphthalate, polyethylene, polypropylene, polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, polyphenylene sulfide, polyphenylene ether, polystyrene, or polyimide.
4. The composite current collector according to any one of claims 1 to 3, wherein: A bonding layer is further provided between the base film and the conductive layer; Optionally, the adhesion between the bonding layer and the conductive layer is 100 N / m - 900 N / m; Optionally, the material of the bonding layer includes any one or a combination of at least two of aluminum oxide, silicon oxide, titanium oxide, nickel, chromium, titanium, nickel-chromium alloy, nickel-chromium-copper alloy, silicon-aluminum alloy, polyacrylic acid, polyacrylate, polyacrylamide, or polyurethane.
5. The composite current collector according to any one of claims 1 to 4, wherein: The metal in the metal layer includes any one or a combination of at least two of aluminum, copper, gold, silver, nickel, or zinc and their alloys.
6. The composite current collector according to any one of claims 1 to 5, wherein: The material of the intermediate layer includes an amorphous conductive material.
7. The composite current collector according to claim 6, wherein: The amorphous conductive material is amorphous copper.
8. The composite current collector according to claim 6 or 7, wherein: The thickness d1 of the metal layer satisfies: 0 nm < d1 ≤ 300 nm; optionally, the thickness d1 of the metal layer satisfies: 50 nm < d1 ≤ 200 nm; the thickness d2 of the intermediate layer satisfies: 0 nm < d2 ≤ 100 nm; optionally, the thickness d2 of the intermediate layer satisfies: 20 nm < d2 ≤ 80 nm.
9. The composite current collector according to any one of claims 1 to 5, wherein: The material of the intermediate layer includes any one or a combination of at least two of fluorocarbon materials, oxides, alloys, nitrides, carbides, sulfides, fluorides, silicides, or phosphides, and can be any one or a combination of at least two of carbides, silicides, or fluorides.
10. The composite current collector according to claim 9, wherein, The fluorocarbon material in the middle layer includes a fluorocarbon polymer. Optionally, the chemical composition of the fluorocarbon polymer is C x F y , where 0.6≤x / y≤10; The oxides in the intermediate layer include one or more of metal oxides and non-metal oxides. Optionally, the metal oxides are selected from one or more of aluminum oxide, titanium oxide, copper oxide, nickel oxide, chromium oxide, zinc oxide, magnesium oxide, cobalt oxide, zirconium oxide, tin oxide, and indium tin oxide, and the non-metal oxide is silicon oxide; The alloys in the intermediate layer include any one or a combination of at least two of nickel-chromium alloy, nickel-chromium-copper alloy, nickel-chromium-silicon alloy, nickel-chromium-cobalt alloy, silicon-aluminum alloy, aluminum-silicon-copper alloy, copper-nickel alloy, copper-nickel-titanium alloy, copper-gallium alloy, copper-indium alloy, copper-indium-gallium alloy, aluminum-tin-copper alloy, aluminum-chromium alloy, tungsten-titanium alloy, molybdenum-copper alloy, molybdenum-niobium alloy, molybdenum-tantalum alloy, molybdenum-zirconium-titanium alloy, or molybdenum-lanthanum alloy; The nitrides include any one or a combination of at least two of aluminum nitride, boron nitride, chromium nitride, titanium nitride, silicon nitride, niobium nitride, zirconium nitride, hafnium nitride, tantalum nitride, vanadium nitride, or aluminum titanium nitride; The carbide includes any one or a combination of at least two of aluminum carbide, boron carbide, chromium carbide, nickel carbide, tungsten carbide, titanium carbide, hafnium carbide, zirconium carbide, tantalum carbide, lanthanum carbide, molybdenum carbide, niobium carbide, silicon carbide, titanium carbide or vanadium carbide; The sulfide includes any one or a combination of at least two of copper sulfide, tin sulfide, zinc sulfide, tungsten sulfide, molybdenum sulfide, iron sulfide, antimony sulfide, chromium sulfide, nickel sulfide, titanium sulfide, aluminum copper sulfide or iron copper sulfide; The fluoride includes any one or a combination of at least two of iridium fluoride, magnesium fluoride, calcium fluoride, lithium fluoride, aluminum fluoride, barium fluoride, samarium fluoride, cerium fluoride, yttrium fluoride or scandium fluoride; The silicide includes any one or a combination of at least two of cobalt silicide, chromium silicide, nickel silicide, titanium silicide, hafnium silicide, molybdenum silicide, niobium silicide, tantalum silicide, vanadium silicide, tungsten silicide or zirconium silicide; The phosphide includes any one or a combination of at least two of aluminum phosphide, boron phosphide, copper phosphide, nickel phosphide, silicon phosphide, tungsten phosphide, gallium phosphide, germanium phosphide, indium phosphide, molybdenum phosphide, niobium phosphide or tantalum phosphide.
11. The composite current collector according to claim 9 or 10, wherein: The thickness d1 of the metal layer satisfies: 0 < d1 ≤ 200 nm; Optionally, the thickness d2 of the intermediate layer satisfies: 1 nm ≤ d2 ≤ 50 nm, optionally 2 nm ≤ d2 ≤ 50 nm, more optionally 5 nm ≤ d2 ≤ 20 nm, further optionally 10 nm ≤ d2 ≤ 20 nm; Optionally, the thickness of the intermediate layer d2 is less than or equal to one-tenth of the thickness of the metal layer d1.
12. The composite current collector according to any one of claims 9 to 11, wherein: The intermediate layer material is amorphous (non-crystalline) or partially crystalline.
13. The composite current collector according to any one of claims 1 to 12, wherein: The thickness of the conductive layer provided on one surface of the polymer-based film is 500 - 2000 nm, optionally 800 - 1200 nm; Optionally, the number of metal layers in the conductive layer is n, and the number of intermediate layers is n, n - 1 or n + 1, and n satisfies: 2 ≤ n ≤ 50, optionally 2 ≤ n ≤ 15, more optionally 5 ≤ n ≤ 10.
14. The composite current collector according to any one of claims 1 - 13, wherein, The intermediate layer and the metal layer have a pore-free structure.
15. The composite current collector according to any one of claims 1 - 14, wherein, The metal in the metal layer is crystalline, and the average grain size of the grains is 0 - 200 nm, not 0, optionally 10 - 100 nm.
16. The composite current collector according to any one of claims 1 to 15, wherein: A protective layer is further provided on the surface of the conductive layer away from the base film; Optionally, when the composite conductive layer is provided on one surface of the polymer-based film, the protective layer is provided on the surface of the composite conductive layer away from the polymer-based film and the other surface of the polymer-based film; or, When the composite conductive layer is provided on one surface of the polymer-based film, the protective layer is provided on the surface of the composite conductive layer away from the polymer-based film; or, When the composite conductive layer is provided on both surfaces of the polymer-based film, the protective layer is provided on the surface of the composite conductive layer away from the polymer-based film; Optionally, the thickness of the protective layer is 5 nm - 100 nm, optionally 20 nm - 80 nm; Optionally, the material of the protective layer includes any one of nickel, chromium, nickel-based alloy, copper-based alloy, copper oxide, aluminum oxide, nickel oxide, chromium oxide, cobalt oxide, copper chromium oxide, graphite, carbon black, copper chromate, copper chromite, carbon nano-quantum dots, carbon nanotubes, carbon nanofibers, graphene or graphene oxide, or a combination of at least two of them.
17. The composite current collector according to any one of claims 1 to 16, wherein: The conductive layer will produce micro cracks during the needling process, and the micro cracks will spread and cause large-area fractures, thereby separating the conductive layer from the steel needle.
18. A method for preparing the composite current collector according to any one of claims 1 to 17, comprising the following steps: A composite conductive layer is prepared on the surface of at least one side of the base film; wherein the conductive layer comprises alternately stacked metal layers and intermediate layers.
19. The method for preparing a composite current collector according to claim 18, wherein: An adhesive layer is also provided between the base film and the conductive layer; Optionally, the bonding layer is composited by a method including magnetron sputtering, evaporation or coating; Optionally, the composite preparation method of the metal layer includes electroplating, chemical plating, evaporation and / or magnetron sputtering; Optionally, the preparation method of the intermediate layer includes chemical vapor deposition, evaporation or magnetron sputtering; Optionally, after the conductive layer is obtained by composite, a protective layer is further provided on the surface of the conductive layer away from the base film; optionally, the composite preparation method of the protective layer includes any one of physical vapor deposition, chemical vapor deposition, in-situ forming or coating methods, or a combination of at least two of them.
20. The method for preparing a composite current collector according to claim 18 or 19, wherein: The preparation method comprises the following steps: The intermediate layer and the metal layer are alternately deposited on both sides of the polymer base film to form a composite conductive layer; The preparation method of the intermediate layer is magnetron sputtering, chemical vapor deposition or evaporation; Optionally, the specific process parameters of the magnetron sputtering method include: target power of 1-10kW, vacuum degree ≤0.5Pa, gas flow rate of 10mL / min-500mL / min, and coating time of a single intermediate layer of 0.1s-60s; Optionally, the specific process parameters of the evaporation method include: vacuum degree <0.5Pa, gas flow rate of 10mL / min-500mL / min, and each deposition time of 0.1 to 10s; The metal layer is prepared by evaporation, magnetron sputtering or electroplating, and the specific process parameters include: Optionally, the magnetron sputtering target is any one of a copper target, an aluminum target or a copper-aluminum alloy target, the target power is 5-20 kW, the gas flow rate is 10-500 mL / min, the vacuum degree is ≤0.5 Pa, and the coating time of a single metal layer is 0.1s-120s; or Optionally, the average cathode current density of the electroplating method is 1 to 3 A / dm 2 , the plating solution temperature is 15~35℃, and the plating time is 1~90s. Optionally, the raw material for the evaporation method is high-purity metal wire (purity ≥ 99.9%), the heating temperature is greater than the melting point of the metal wire, the vacuum degree of the vacuum chamber is less than or equal to 0.1 Pa, the coating time each time is 0.5-100s, and the main roller cooling temperature is: -30℃-10℃.
21. The method for preparing a composite current collector according to claim 20, wherein: The preparation method further comprises the following steps The protective layer is deposited on the surface of the composite conductive layer away from the polymer base film by a coating method, and the specific process steps include: The coating liquid of the protective layer is coated on the surface of the composite conductive layer, and the protective layer is obtained after drying.
22. A battery, wherein: The battery comprises the composite current collector according to any one of claims 1 to 17 or the composite current collector prepared by the method for preparing the composite current collector according to any one of claims 18 to 21; Optionally, the composite current collector is used in an electrode plate of the battery.
Citation Information
Patent Citations
Current collector with multi-layer structure, preparation method of current collector, battery with current collector and object
CN112670519A
Multilayer structure current collector and preparation method thereof
CN114824289A
Positive pole piece of lithium ion battery
CN115332479A
Current collector and preparation method thereof, negative electrode and electrochemical energy storage device
CN115440986A
High-strength polyester-based film, preparation method thereof and application of high-strength polyester-based film in composite current collector
CN115926389A
Cited By
Functional copper foil current collector and preparation method and application thereof
CN119695168A
Plastic mobile phone frame manufacturing method and plastic mobile phone frame
CN119928136A
Preparation method and application of flexible three-dimensional current collector with functional ion self-release characteristic
CN120006266A
Preparation method and application of flexible three-dimensional current collector with functional ion self-release property
CN120006266B
Multilayer current collector and preparation method and application thereof
CN120149423A