Secondary battery, electronic apparatus, and vehicle
The composite positive electrode active material structure in lithium ion secondary batteries addresses the challenge of achieving high capacity and safety by covering the first active material with a more stable second material, reducing thermal runaway and maintaining discharge capacity while enhancing safety and resistance.
Patent Information
- Application Number
- PCT/IB2024/055123
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-03-14
- Filing Date
- 2024-05-27
- Publication Date
- 2024-12-05
AI Technical Summary
Lithium ion secondary batteries face challenges in achieving both high capacity and safety, with positive electrode active materials like lithium cobalt oxide being prone to thermal runaway due to crystal structure instability during charging, leading to potential fires and reduced discharge capacity over charge/discharge cycles.
A secondary battery design featuring a composite positive electrode active material structure where a second, more stable material covers the surface of the first active material, reducing direct contact with the electrolyte and enhancing crystal stability, thereby mitigating electric field stress and improving safety and discharge capacity.
The composite structure enhances the safety and stability of the battery by reducing the risk of thermal runaway and maintaining discharge capacity, while also providing improved fire resistance and heat resistance.
Smart Images

Figure IB2024055123_05122024_PF_FP_ABST
Abstract
Description
Secondary batteries, electronic devices and vehicles
[0001] The present invention relates to a secondary battery, or to an electronic device and a vehicle having a secondary battery.
[0002] The technical field of the present invention is not limited to the above. For example, the present invention relates to a positive electrode active material. Furthermore, the present invention relates to a manufacturing method or production method corresponding to the above technical field.
[0003] In this specification, the term "electronic device" refers to any device having a positive electrode active material or a secondary battery, and typically includes an electro-optical device or an information terminal device.
[0004] In this specification, the term "electricity storage device" refers to elements and devices in general that have an electricity storage function, and representative examples include lithium ion secondary batteries, lithium ion capacitors, and electric double layer capacitors.
[0005] In recent years, various types of power storage devices, such as lithium-ion secondary batteries and lithium-ion capacitors, have been actively developed. In particular, lithium-ion secondary batteries, which have high output and high energy density, are widely used in electronic devices such as mobile phones, smartphones, and notebook computers, and in vehicles such as electric vehicles (EVs), and are indispensable in today's information society as a rechargeable energy source.
[0006] Composite oxides, such as lithium cobalt oxide and lithium nickel-cobalt-manganese oxide, with a layered rock salt structure are widely used as positive electrode active materials for lithium-ion secondary batteries. These materials have useful properties as active materials for energy storage devices, such as high capacity and high discharge voltage. However, to achieve high capacity, the positive electrode must be exposed to a high potential relative to lithium during charging. Under such high potential conditions, significant lithium desorption can reduce the stability of the crystal structure and lead to significant deterioration during charge-discharge cycles. Against this background, efforts have been actively made to improve the positive electrode active materials of secondary battery positive electrodes in order to develop high-capacity, highly stable secondary batteries (e.g., Patent Documents 1 to 3).
[0007] Research into the crystal structure of positive electrode active materials has also been conducted (Non-Patent Documents 1 to 4).
[0008] XRD (X-ray diffraction) is one of the techniques used to analyze the crystalline structure of positive electrode active materials. XRD data can be analyzed using the Inorganic Crystal Structure Database (ICSD) introduced in Non-Patent Document 5. For example, the lattice constant of lithium cobalt oxide described in Non-Patent Document 6 can be referenced from the ICSD. For Rietveld analysis, for example, the analysis program RIETAN-FP (Non-Patent Document 7) can be used.
[0009] Also, as image processing software, for example, ImageJ (Non-Patent Documents 8 to 10) is known. By using this software, for example, the shape of the positive electrode active material can be analyzed.
[0010] Microelectron diffraction is also effective for identifying the crystalline structure of the positive electrode active material, particularly the crystalline structure of the surface layer. For example, the analysis program ReciPro (Non-Patent Document 11) can be used to analyze the electron diffraction pattern.
[0011] Furthermore, fluorides such as fluorite (calcium fluoride) have long been used as fluxes in iron manufacturing and other processes, and their physical properties have been studied (Non-Patent Document 12).
[0012] It is also said that it is difficult to achieve both high capacity and safety in lithium-ion secondary batteries. For example, it is said that positive electrode active materials with a layered rock-salt crystal structure are prone to thermal runaway if too many lithium ions are released during charging, due to the destruction of the crystal structure, which poses safety issues. For example, it is known that lithium-ion secondary batteries can go through several states before thermal runaway occurs when the temperature rises during charging (Non-Patent Document 13). Furthermore, various research and development efforts are being conducted on the reliability and safety of lithium-ion secondary batteries. For example, Non-Patent Document 14 describes the thermal stability of positive electrode active materials and electrolytes.
[0013] For example, Shannon's ionic radius is known from Non-Patent Document 15.
[0014] JP 2018-088400 A, WO 2018 / 203168 Pamphlet, JP 2020-140954 A
[0015] Toyoki Okumura et al.,”Correlation of lithium ion distribution and X−ray absorption near−edge structure in O3−and O2−lithium cobalt oxides from first−principle calculation”,Journal of Materials Chemistry,2012,22,p.17340−17348Motohashi,T.et al.,”Electronic phase diagram of the layered cobalt oxide system Li▲x▼CoO▲2▼(0.0≦x≦1.0)”,Physical Review B,80(16);165114Zhaohui Chen et al.,“Staging Phase Transitions in Li▲x▼CoO▲2▼”,Journal of The Electrochemical Society,2002,149(12)A1604−A1609G.G.Amatucci et al.,“CoO▲2▼,The End Member of the Li▲x▼CoO▲2▼ Solid Solution”J.Electrochem.Soc.143(3)1114(1996).Belsky,A.et al.,“New developments in the Inorganic Crystal Structure Database(ICSD):accessibility in support of materials research and design”,Acta Cryst.,(2002)B58 364−369.Akimoto,J.;Gotoh,Y.;Oosawa,Y.“Synthesis and structure refinement of LiCoO▲2▼ single crystals”Journal of Solid State Chemistry(1998)141,p.298−302.F.Izumi and K.Momma,Solid State Phenom.,130,15−20(2007)Rasband,W.S.,ImageJ,U. S. National Institutes of Health, Bethesda, Maryland, USA, http: / / rsb. info. nih. gov / ij / , 1997-2012. Schneider, C. A. , Rasband, W. S. , Eliceiri, K. W. “NIH Image to ImageJ: 25 years of image analysis”, Nature Methods 9, 671-675, 2012. Abramoff, M. D. , Magelhaes, P. J. , Ram, S. J. , “Image Processing with ImageJ”, Biophotonics International, volume 11, issue 7, pp. 36-42, 2004. Seto, Y. & Ohtsuka, M. , “ReciPro: free and open-source multipurpose crystallographic software integrating a crystal model database and “viewer, diffraction and microscopy simulators, and diffraction data analysis tools” (2022) J. Appl. Cryst. ,55. W. E. Counts, R. Roy, and E. F. Osborn, "Fluoride Model Systems: II, The Binary Systems CaF2-BeF2, MgF2-BeF2, and LiF-MgF2", Journal of the American Ceramic Society, 36[1] 12-17 (1953). Nobuo Eda, 2-4 Heat Generation Mechanism: Learning from Data: Li-ion Battery Charging and Discharging Technology, CQ Publishing, April 4, 2020, pp. 68-72; Shinya Kitano et al., GSYuasa Technical Report, Vol. 2, No. 2, December 2015, pp. 18-24; Shannon et al. , Acta A, 32 (1976) 751. ,
[0016] Lithium cobalt oxide (LiCoO 2Lithium-ion secondary batteries (sometimes referred to as LCO) are said to have low thermal stability if too many lithium ions are released during charging. Furthermore, when an internal short circuit occurs in a lithium-ion secondary battery due to a nail penetration test, Joule heat is generated, causing the lithium cobalt oxide to reach a high temperature and release oxygen. The oxygen released from the lithium cobalt oxide reacts with the electrolyte, etc., which can lead to thermal runaway. While the above-mentioned Patent Documents 1 to 3 have actively improved the positive electrode active material, secondary batteries still have room for improvement in various aspects, such as safety, discharge capacity, cycle characteristics, reliability, and cost.
[0017] Therefore, an object of one embodiment of the present invention is to provide a highly safe secondary battery. Another object of one embodiment of the present invention is to provide a secondary battery that is stable in a high potential state and / or a high temperature state. Another object of one embodiment of the present invention is to provide a secondary battery including a positive electrode active material whose crystal structure is not easily deformed even after repeated charge and discharge. Another object of one embodiment of the present invention is to provide a secondary battery including a positive electrode active material with excellent charge and discharge cycle characteristics. Another object of one embodiment of the present invention is to provide a secondary battery including a positive electrode active material with a large discharge capacity.
[0018] Note that the description of these problems does not preclude the existence of other problems. Note that one embodiment of the present invention does not necessarily solve all of these problems. Note that problems other than these can be extracted from the description in the specification, drawings, and claims.
[0019] In view of the above, one embodiment of the present invention is a secondary battery having a cathode active material composite. In this specification and the like, the term "cathode active material composite" refers to a configuration having a first cathode active material and a second cathode active material covering at least a portion of the surface of the first cathode active material, and preferably refers to a structure in which the second cathode active material covers substantially the entire surface of the first cathode active material. Here, "substantially covering the entire surface" refers to a state in which the second cathode active material covers the first cathode active material to an extent that the first cathode active material and the electrolyte do not come into direct contact with each other. For example, if the second cathode active material covers 80% or more, preferably 95% or more, and more preferably 95% or more of the cross-section of the first cathode active material, this can be said to be a state in which the first cathode active material does not come into direct contact with the electrolyte.
[0020] In a preferred embodiment, the particle size (typically, median diameter D50) of the first positive electrode active material is 1 / 10 or less, preferably 1 / 50 or less, and more preferably 1 / 100 or less of the particle size (typically, median diameter D50) of the second positive electrode active material. In this case, a preferred configuration is to prepare 10 or more, preferably 15 or more, and more preferably 20 or more particles of the second positive electrode active material and cover the surface of the first positive electrode active material.
[0021] It is preferable that the interface between the first positive electrode active material and the second positive electrode active material is clear, but the baking step may make the interface difficult to see.
[0022] In a more preferred embodiment, the composition of the first positive electrode active material is different from the composition of the second positive electrode active material. In another preferred embodiment, the second positive electrode active material has a crystal structure that is more stable in a high-voltage charging state than the first positive electrode active material. In another preferred embodiment, the battery characteristics of a secondary battery using only the first positive electrode active material in the positive electrode are different from the battery characteristics of a secondary battery using only the second positive electrode active material in the positive electrode.
[0023] According to one embodiment of the present invention described above, it is expected that the potential of the surface of the first positive electrode active material can be reduced. In this specification and the like, reducing the voltage of the surface of the first positive electrode active material is sometimes referred to as mitigating the electric field to the positive electrode active material. In other words, by covering at least a portion of the first positive electrode active material with the second positive electrode active material, the function of mitigating the electric field can be expected, and a highly safe secondary battery can be provided.
[0024] Furthermore, according to the above-described embodiment of the present invention, the area where the first positive electrode active material is in direct contact with the electrolyte is reduced or there is no area where the first positive electrode active material is in contact with the electrolyte. Therefore, even when the first positive electrode active material is exposed to a high-voltage charging state, it is possible to suppress the detachment of a transition metal element and / or oxygen from the first positive electrode active material, and therefore it is possible to suppress a decrease in discharge capacity due to repeated charging and discharging.
[0025] Furthermore, by covering the first positive electrode active material with a second positive electrode active material having a more stable crystal structure, a secondary battery with improved stability at high temperatures or improved fire resistance can be provided. In particular, by using a material with a stable crystal structure for the first positive electrode active material, specifically, lithium cobalt oxide with added magnesium and fluorine, lithium cobalt oxide with added magnesium, fluorine, aluminum, and nickel, or lithium nickel-cobalt-manganese oxide (preferably in a ratio of nickel:cobalt:manganese = 8:1:1 or nickel:cobalt:manganese = 9:0.5:0.5, etc.), a secondary battery with even more improved stability at high temperatures or improved fire resistance can be provided. The lithium nickel-cobalt-manganese oxide is preferably in the form of secondary particles. Furthermore, the lithium nickel-cobalt-manganese oxide is preferably coated with aluminum oxide. In this specification and the like, secondary particles coated with a specific oxide are sometimes referred to as metal oxide-coated composite oxides. Materials applicable to the first positive electrode active material described above have excellent stability in a high-voltage charging state, making it possible to provide a secondary battery with improved heat resistance and / or fire resistance. Lithium cobalt oxide to which magnesium, fluorine, aluminum, and nickel have been added will be described later. This lithium cobalt oxide is unique in that magnesium, fluorine, and aluminum are distributed in greater amounts in the surface layer of the positive electrode active material, and nickel is widely distributed throughout the particles. Such unique lithium cobalt oxide is particularly preferred as the first positive electrode active material.
[0026] LiM2PO as the second positive electrode active material 4 (M2 is one or more selected from Fe, Ni, Co, and Mn) is preferably used. 4(M2 is one or more selected from Fe, Ni, Co, and Mn) has high stability, particularly at high temperatures, and further has a stable crystal structure even in a high-voltage charging state. Therefore, the higher the mixing ratio of the second positive electrode active material in the positive electrode of one embodiment of the present invention, the more the fire resistance and heat resistance of the secondary battery can be improved. Preferred examples of the mixing ratio include a ratio of the first positive electrode active material to the second positive electrode active material of 7:3, 8:2, or 9:1. Even when the mixing ratio of the second positive electrode active material is reduced, a secondary battery using the second positive electrode active material can have higher fire resistance than a secondary battery not using the second positive electrode active material.
[0027] The above LiM2PO 4 (M2 is one or more selected from Fe, Ni, Co, and Mn) may be coated with carbon. The carbon coating layer may be referred to as a carbon layer in this specification.
[0028] The positive electrode of the present invention may have a carbon layer, such as a carbon coating layer, between the first positive electrode active material and the second positive electrode active material, i.e., at a position corresponding to the interface between them. The carbon layer may be a layer containing a conductive material such as carbon nanotubes (CNT), a graphene compound, or acetylene black (AB). A binder may be included in addition to or instead of the carbon layer. Even in a configuration in which a carbon layer and / or a binder is located between the first positive electrode active material and the second positive electrode active material, it is sufficient that the contact area between the first positive electrode active material and the electrolyte is reduced by the second positive electrode active material.
[0029] One aspect of the present invention includes a positive electrode, a negative electrode, and an electrolyte. The positive electrode includes a first positive electrode active material and a second positive electrode active material. The first positive electrode active material is LiMO. 2 (M1 represents one or more selected from Fe, Ni, Co, Mn, and Al), and the second positive electrode active material is represented by LiM2PO 4(M2 represents one or more selected from Fe, Ni, Co, and Mn), the first positive electrode active material has an additive element X (X represents one or more selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic) in a surface layer portion, the negative electrode has graphite, and the graphite has a specific surface area of 0.8 m as measured by a BET method. 2 / g or more 8m 2 / g.
[0030] Another aspect of the present invention is a battery comprising a positive electrode, a negative electrode, and an electrolyte. The positive electrode comprises a first positive electrode active material and a second positive electrode active material, and the first positive electrode active material is LiMO. 2 (M1 represents one or more selected from Fe, Ni, Co, Mn, and Al), and the second positive electrode active material is represented by LiM2PO 4 (M2 represents one or more selected from Fe, Ni, Co, and Mn), the first positive electrode active material has an additive element X (X represents one or more selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic) in a surface layer portion, and the negative electrode has graphite, the graphite having a median diameter (D50) measured by a laser diffraction method of 3 μm or more and 50 μm or less.
[0031] In the present invention, the electrolyte preferably contains a fluorinated cyclic carbonate and a fluorinated chain carbonate as a solvent.
[0032] In the present invention, the electrolyte contains fluoroethylene carbonate and methyl trifluoropropionate as solvents, and when the total volume of fluoroethylene carbonate and methyl trifluoropropionate is 100 vol%, the volume ratio of fluoroethylene carbonate to methyl trifluoropropionate is preferably y:100-y (where 5≦y≦30).
[0033] In the present invention, the additional element X preferably contains at least magnesium and fluorine, and when a cross section of the first positive electrode active material is subjected to STEM-EDX ray analysis, the fluorine concentration peak is preferably located closer to the surface than the magnesium concentration peak.
[0034] Another embodiment of the present invention is a vehicle or electronic device having a secondary battery.
[0035] According to one embodiment of the present invention, a highly safe secondary battery can be provided. According to another embodiment of the present invention, a secondary battery that is stable at a high potential and / or at a high temperature can be provided. According to another embodiment of the present invention, a secondary battery including a positive electrode active material whose crystal structure is not easily degraded even after repeated charge and discharge can be provided. According to another embodiment of the present invention, a secondary battery including a positive electrode active material with excellent charge and discharge cycle characteristics can be provided. According to another embodiment of the present invention, a secondary battery including a positive electrode active material with a large discharge capacity can be provided.
[0036] Note that the description of these effects does not preclude the existence of other effects. Note that one embodiment of the present invention does not necessarily have all of these effects. Note that effects other than these will become apparent from the description in the specification, drawings, claims, etc., and it is possible to extract other effects from the description in the specification, drawings, claims, etc.
[0037] FIGS. 1A and 1B are cross-sectional views illustrating a cathode active material composite according to one embodiment of the present invention. FIGS. 2A and 2B are cross-sectional views illustrating a cathode active material composite according to one embodiment of the present invention. FIGS. 3A and 3B are cross-sectional views illustrating a cathode active material composite according to one embodiment of the present invention. FIGS. 4A and 4B are views illustrating a method for fabricating a cathode active material composite according to one embodiment of the present invention. FIGS. 5A to 5C are views illustrating a method for fabricating a cathode active material composite according to one embodiment of the present invention. FIGS. 6A and 6B are views illustrating a nail penetration test. FIG. 7 is a view illustrating the nail penetration operation. FIG. 8 is a graph showing changes in the internal temperature of a secondary battery in which an internal short circuit has occurred as the internal temperature increases. FIG. 9 is a graph showing changes in the internal temperature of a secondary battery as the internal temperature increases. FIG. 10 is a view illustrating the crystalline structure of a cathode active material according to one embodiment of the present invention. FIG. 11 is a view illustrating the state of charge and the crystalline structure of a cathode active material. FIG. 12 is an XRD pattern calculated from the crystalline structure. FIG. 13 is an XRD pattern calculated from the crystalline structure. FIGS. 14A and 14B are XRD patterns calculated from the crystal structure. FIGS. 15A and 15B are diagrams illustrating the distribution of added elements. FIGS. 16A to 16C are diagrams illustrating an example of a method for manufacturing a positive electrode active material. FIGS. 17A to 17C are diagrams illustrating an example of a method for manufacturing a positive electrode active material. FIG. 18 is a diagram illustrating an example of a method for manufacturing a positive electrode active material. FIGS. 19A to 19C are diagrams illustrating an example of a method for manufacturing a positive electrode active material. FIG. 20A is an exploded perspective view of a coin-type secondary battery, FIG. 20B is an external view of the coin-type secondary battery, and FIG. 20C is a cross-sectional perspective view thereof. FIG. 21A shows an example of a cylindrical secondary battery. FIG. 21B shows an example of a cylindrical secondary battery. FIG. 21C shows an example of an energy storage system having multiple cylindrical secondary batteries. FIG. 21D shows an example of an energy storage system having multiple cylindrical secondary batteries. FIGS. 22A and 22B are diagrams illustrating an example of a secondary battery, and FIG. 22C shows the internal appearance of the secondary battery. 23A to 23C are diagrams illustrating an example of a secondary battery. FIGS. 24A and 24B are diagrams illustrating the appearance of a secondary battery. FIGS. 25A to 25C are diagrams illustrating a secondary battery and a method for manufacturing the secondary battery. FIGS. 26A to 26C are diagrams illustrating an example of the configuration of a battery pack.FIGS. 27A and 27B are diagrams illustrating an example of a secondary battery. FIGS. 28A to 28C are diagrams illustrating an example of a secondary battery. FIGS. 29A and 29B are diagrams illustrating an example of a secondary battery. FIG. 30A is a perspective view of a battery pack illustrating one embodiment of the present invention, FIG. 30B is a block diagram of the battery pack, and FIG. 30C is a block diagram of a vehicle having a motor. FIGS. 31A to 31D are diagrams illustrating an example of a transportation vehicle. FIGS. 32A and 32B are diagrams illustrating a power storage device according to one embodiment of the present invention. FIG. 33A is a diagram illustrating an electric bicycle, FIG. 33B is a diagram illustrating a secondary battery for the electric bicycle, and FIG. 33C is a diagram illustrating an electric motorcycle. FIGS. 34A to 34D are diagrams illustrating an example of an electronic device. FIG. 35A illustrates an example of a wearable device, FIG. 35B is a perspective view of a wristwatch-type device, and FIG. 35C is a diagram illustrating a side view of the wristwatch-type device. FIG. 35D is a diagram illustrating an example of a wireless earphone. FIG. 36 is a graph of DSC measurement results. Figures 37A and 37B are graphs of charge / discharge curves. Figures 38A and 38B are graphs of cycle tests. Figures 39A and 39B are photographs of nail penetration tests. Figure 40 is a graph of DSC measurement results.
[0038] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to the following description, and it will be readily understood by those skilled in the art that various modifications can be made to the embodiments and details. Furthermore, the present invention should not be interpreted as being limited to the description of the embodiments shown below.
[0039] A secondary battery has, for example, a positive electrode and a negative electrode. A material constituting the positive electrode is a positive electrode active material. The positive electrode active material is, for example, a substance that undergoes a reaction that contributes to the charge / discharge capacity. Note that the positive electrode active material may contain a substance that does not contribute to the charge / discharge capacity.
[0040] In this specification and the like, the positive electrode active material of one embodiment of the present invention may be referred to as a positive electrode material, a positive electrode material for a secondary battery, a composite oxide, or the like. Furthermore, in this specification and the like, the positive electrode active material of one embodiment of the present invention preferably includes a compound. Furthermore, in this specification and the like, the positive electrode active material of one embodiment of the present invention preferably includes a composition. Furthermore, in this specification and the like, the positive electrode active material of one embodiment of the present invention preferably includes a composite.
[0041] Furthermore, in this specification and the like, the term "particle" is not limited to referring only to spherical shapes (having a circular cross-sectional shape), and examples of the cross-sectional shape of individual particles include ellipsoids, rectangles, trapezoids, cones, squares with rounded corners, and asymmetric shapes, and further, individual particles may have an irregular shape.
[0042] The particle size can be measured, for example, by laser diffraction particle size distribution measurement, and the D50 value can be used for comparison. Here, D50 refers to the particle size when the cumulative amount in the cumulative curve of the particle size distribution measurement results accounts for 50%, i.e., the median diameter. The measurement of particle size is not limited to laser diffraction particle size distribution measurement, and when the particle size is below the lower measurement limit of laser diffraction particle size distribution measurement, the major axis of the particle cross section may be measured by analysis using a scanning electron microscope (SEM) or a transmission electron microscope (TEM).
[0043] Furthermore, in this specification and the like, Miller indices are used to represent crystal planes and directions. Individual planes indicating crystal planes are represented in parentheses. In crystallography, crystal planes, directions, and space groups are represented by adding a superscript bar to the numbers, but in this specification and the like, due to restrictions on notation in applications, numbers may be represented by adding a - (minus sign) before them instead of adding a bar above them.
[0044] In addition, in this specification, the layered rock-salt type crystal structure of a composite oxide containing lithium and a transition metal refers to a crystal structure having a rock-salt type ion arrangement in which cations and anions are alternately arranged, and in which the transition metal and lithium are regularly arranged to form a two-dimensional plane, allowing two-dimensional diffusion of lithium. Defects such as cation or anion deficiencies may also be present. Furthermore, strictly speaking, the layered rock-salt type crystal structure may have a distorted rock-salt type crystal lattice structure, which may result in a lower symmetry than the rock-salt type crystal structure.
[0045] In this specification and the like, the rock salt type crystal structure refers to a structure in which cations and anions are arranged alternately. Note that the crystal structure may have a deficiency of cations or anions in part.
[0046] In this specification, the theoretical capacity of a positive electrode active material refers to the amount of electricity when all of the intercalable and deintercalable lithium contained in the positive electrode active material is deintercalated. For example, LiFePO 4 The theoretical capacity of LiCoO is 170 mAh / g per active material weight. 2 The theoretical capacity of LiNiO is 274 mAh / g per active material weight. 2 The theoretical capacity of LiMn is 275 mAh / g per active material weight. 2 O 4 The theoretical capacity of the active material is 148 mAh / g.
[0047] In this specification and the like, the depth of charge when all intercalable and deintercalable lithium is intercalated is defined as 0, and the depth of charge when all intercalable and deintercalable lithium contained in the positive electrode active material is deintercalated is defined as 1.
[0048] Although the present specification and the like may illustrate examples of secondary batteries using lithium metal as the counter electrode in the positive electrode and positive electrode active material of one embodiment of the present invention, the secondary battery of one embodiment of the present invention is not limited thereto. Other materials, such as graphite and lithium titanate, may also be used for the negative electrode. The positive electrode and positive electrode active material of one embodiment of the present invention have properties such as a crystalline structure that is not easily broken even after repeated charge and discharge, and good cycle characteristics, which are not affected by the material of the negative electrode. Furthermore, the secondary battery of one embodiment of the present invention is expected to have improved cycle characteristics due to a synergistic effect between the positive electrode active material and the negative electrode active material.
[0049] In this specification, ignition in a nail penetration test refers to the observation of a flame outside the exterior body within one minute of the nail being inserted, or the occurrence of thermal runaway in the secondary battery. For example, thermal runaway is said to have occurred if, after the completion of the nail penetration test, thermal decomposition products of the positive electrode and / or negative electrode are observed at a location 2 cm or more away from the insertion point. Examples of thermal decomposition products of the positive electrode and / or negative electrode include aluminum oxide, which is oxidized aluminum from the positive electrode current collector, and copper oxide, which is oxidized copper from the negative electrode current collector.
[0050] For example, the positive electrode active material is layered rock salt type LiCoO 2 In the case of using LiCoO, the atomic ratio of O to Co is theoretically 2. 2 When oxygen is released from the nail, the O / Co ratio decreases. Therefore, for example, after the completion of a nail penetration test, if the O / Co ratio in energy dispersive X-ray spectroscopy (EDX) analysis at a location 2 cm or more away from the puncture site is less than 1.3, it is said that thermal runaway has occurred. Conversely, if the O / Co ratio in EDX analysis at a location 2 cm or more away from the puncture site is 1.3 or more, it can be said that thermal runaway has not occurred.
[0051] On the other hand, even if a flame, spark, and / or smoke is observed in the nail penetration test, if the flame remains at the point of penetration, i.e., the fire does not spread and the secondary battery does not go into thermal runaway, it is not considered to have ignited. For example, if a secondary battery is subjected to a nail penetration test and the above-mentioned ignition does not occur, it can be said to be a non-igniting secondary battery.
[0052] Unless otherwise specified, the materials (positive electrode active material, negative electrode active material, electrolyte, separator, etc.) contained in the secondary battery are described in their pre-degradation state. A decrease in discharge capacity due to aging and burn-in treatments during secondary battery manufacturing is not considered to be degradation. For example, a secondary battery consisting of a single cell or a battery pack can be said to be in its pre-degradation state if it has a discharge capacity of 97% or more of its rated capacity. For secondary batteries for portable devices, the rated capacity conforms to JIS C 8711:2019. For other secondary batteries, the rated capacity conforms to not only the above JIS standard but also various JIS and IEC standards for electric vehicle propulsion, industrial use, etc.
[0053] In this specification and the like, the state of the materials of a secondary battery before deterioration is sometimes referred to as an initial product or initial state, and the state after deterioration (the state when the secondary battery has a discharge capacity of less than 97% of the rated capacity) is sometimes referred to as a product in use or a state in use, or a used product or a used state.
[0054] In this specification, a lithium ion secondary battery refers to a battery that uses lithium ions as carrier ions, but the carrier ions of the present invention are not limited to lithium ions. For example, alkali metal ions or alkaline earth metal ions can be used as carrier ions of the present invention, and specifically, sodium ions can be used. In this case, the present invention can be understood by replacing lithium ions with sodium ions. Furthermore, when there is no limitation on the carrier ions, the battery may be referred to as a secondary battery.
[0055] In this specification, the (001) plane, the (003) plane, and the like may be collectively referred to as the (00l) plane. In this specification, the (00l) plane may also be referred to as the C plane, the basal plane, and the like. In addition, in lithium cobalt oxide, lithium has a two-dimensional diffusion path. In other words, it can be said that the lithium diffusion path exists along the plane. In this specification, a plane on which the lithium diffusion path is exposed, that is, a plane other than the plane where lithium is inserted and extracted (specifically, the (00l) plane), may be referred to as an edge plane.
[0056] In this specification, the term "loading amount" refers to the weight of the active material per unit surface area of the current collector. The loading amount of the negative electrode active material can be adjusted according to the capacity of the positive electrode. In the case of double-sided coating, in which a slurry containing the active material is applied to both sides of the current collector, the loading amount is preferably set to one side. If the loading amount is small, the discharge capacity will be small. Therefore, the loading amount of the positive electrode active material is set to 8.0 mg / cm. 2 The above is preferable.
[0057] In this specification, etc., secondary particles refer to particles formed by aggregation of primary particles. Also, in this specification, etc., single particles are synonymous with primary particles. Also, in this specification, etc., single crystal particles refer to crystalline particles in which there are no grain boundaries inside the particle, and polycrystalline particles refer to crystalline particles in which there are grain boundaries inside the particle. Polycrystalline particles may be referred to as an aggregate of multiple crystallites, and grain boundaries may be referred to as the interface existing between two or more crystallites.
[0058] In this specification and the like, carbonate refers to an organic compound having at least one carbonate ester in its molecular structure, and includes cyclic carbonates and chain carbonates unless otherwise specified. Furthermore, chain carbonates include both linear and branched chain carbonates.
[0059] In this specification etc., the term "A and / or B" may be used, but this is an example of the description including only A, only B, and both A and B.
[0060] In this embodiment, a positive electrode active material according to one embodiment of the present invention will be described. A layer including a positive electrode active material is referred to as a positive electrode active material layer, and the positive electrode active material layer contains at least a conductive material and / or a binder. In this specification and the like, a positive electrode active material layer and a positive electrode current collector are collectively referred to as a positive electrode.
[0061] A cathode active material layer according to one embodiment of the present invention includes a cathode active material composite 100α as shown in FIG. 1A . The cathode active material composite 100α includes a first cathode active material 100x and a second cathode active material 100y. Note that the bonding state between the first cathode active material 100x and the second cathode active material 100y is not limited in any way in the present invention. That is, the cathode active material composite 100α includes a state in which the first cathode active material 100x is attached to the second cathode active material 100y, and also includes a state in which the first cathode active material 100x is fixed to the second cathode active material 100y. Note that the fixed state includes a sintered state.
[0062] The first positive electrode active material 100x preferably has an average particle size of 9 μm or more and less than 20 μm, and a maximum particle size of less than 30 μm, and satisfies the large diameter (also referred to as the large particle size). Secondary particles may be used for the first positive electrode active material 100x, and the secondary particles preferably have an average particle size of 9 μm or more and less than 20 μm, and a maximum particle size of less than 30 μm. Lithium cobalt oxide may be used for the first positive electrode active material 100x. The second positive electrode active material 100y preferably has an average particle size of 5 μm or less, 0.1 μm or more and 5 μm or less, and a maximum particle size of less than 9 μm, and satisfies the small diameter (also referred to as the small particle size). Lithium iron phosphate may be used for the second positive electrode active material 100y. In this specification and the like, the average particle size may be the median diameter (D50). Furthermore, in this specification and the like, the maximum particle size may be the particle size observed in a cross section of a 100 μm square positive electrode.
[0063] The first positive electrode active material 100x preferably has a surface layer portion 100xa and an interior portion 100xb. In FIG. 1A, the interface between the surface layer portion 100xa and the interior portion 100xb is indicated by a dashed line. As will be described later, a composite oxide having a unique layered rock-salt crystal structure containing an additive element X such as magnesium, typically lithium cobalt oxide, may be used for the first positive electrode active material 100x. Although FIG. 1A shows a second positive electrode active material 100y that does not have a surface layer portion and an interior portion, the second positive electrode active material 100y may also have a surface layer portion and an interior portion.
[0064] In this specification, the surface layer of the positive electrode active material refers to a region having a depth of 100 nm or less, preferably a region having a depth of 50 nm or less. The surface layer is synonymous with the near-surface and near-surface region. The depth refers to the distance from the surface of the positive electrode active material toward the interior, and is the distance in a direction perpendicular or approximately perpendicular to the surface. "Almost perpendicular to the surface" refers to an angle with the surface of 80° or more and 100° or less (excluding 90°). The region deeper than the surface layer of the positive electrode active material is referred to as the "interior." The "interior" is synonymous with the bulk or core.
[0065] The positive electrode active material layer of one embodiment of the present invention includes the second positive electrode active material 100y in addition to the first positive electrode active material 100x, whereby a highly safe positive electrode can be provided. For example, when a material having an olivine-type crystal structure, typically lithium iron phosphate, is used for the second positive electrode active material 100y, the olivine-type crystal structure has PO adjacent to the lithium site. 4 Due to the presence of this structure, the crystalline structure can be maintained even when lithium ions are desorbed, resulting in high safety. Adding such a second cathode active material 100y to the first cathode active material 100x is expected to improve the safety of secondary batteries. Furthermore, when the second cathode active material 100y is present around the first cathode active material 100x, it is possible to suppress the elution of oxygen and / or cobalt from the first cathode active material 100x, thereby improving the safety of secondary batteries. Alternatively, by including the second cathode active material 100y in addition to the first cathode active material 100x, the cathode active material layer can increase the electrode density of the positive electrode, i.e., the weight of the positive electrode active material (including the first cathode active material and the second cathode active material) per unit area or unit volume. Furthermore, because the second cathode active material 100y has a small particle size, it is extremely unlikely to cleave, even when the press pressure during positive electrode production is increased. Therefore, a positive electrode having the second positive electrode active material 100y can be pressed at a higher pressure than a positive electrode not having the second positive electrode active material 100y, and the electrode density can be increased while suppressing cleavage. In other words, the electrode density of the positive electrode can be increased by adding the second positive electrode active material 100y to the positive electrode active material layer.
[0066] <Pressing Pressure> The above-mentioned pressing refers to a process in which the positive electrode slurry is applied to a positive electrode current collector and then pressed with a press. Pressing can sometimes cause cracks in the positive electrode active material, but the second positive electrode active material 100y has a small particle size, making such cracks less likely to occur. Such a positive electrode active material composite 100α can also be used in a high-pressure pressing process and / or a multi-stage pressing process. A high pressure typically refers to a linear pressure of the press machine of 1000 kN / m or more to 2000 kN / m or less, preferably 1200 kN / m or more to 1500 kN / m or less. This pressing process may be performed in two or more steps. When pressing in two or more steps, it is preferable to set the linear pressure in any number of pressing steps to 1000 kN / m or more to 2000 kN / m or less, preferably 1200 kN / m or more to 1500 kN / m or less. For example, when two pressings are performed, the second pressing is preferably performed at 1000 kN / m or more and 2000 kN / m or less, preferably 1200 kN / m or more and 1500 kN / m or less. Furthermore, it is preferable to set the linear pressure of the first pressing lower than that of the second pressing, since this can suppress the occurrence of cracks. The linear pressure of the first pressing is preferably 100 kN / m or more and 300 kN / m or less, preferably 180 kN / m or more and 250 kN / m or less. Even when pressing is performed using only such a low linear pressure, the electrode density of the positive electrode active material composite 100α can be increased.
[0067] <Electrode density> The electrode density of the positive electrode was 2.9 g / cm 3 4.5g / cm or more 3 Preferably 3.5 g / cm or less 3 4.3g / cm or more 3 It is preferable that the electrode density is within the above range when the linear pressure described above is satisfied. Alternatively, when manufacturing the cathode active material composite 100α, a heating step may be performed to sinter the first cathode active material 100x and the second cathode active material 100y, and it is considered that the electrode density falls within the above range after the sintering. Generally, a high electrode density can be expected to result in a lack of safety, but the application of the cathode active material composite 100α in the present invention makes it possible to achieve both high electrode density and safety.
[0068] Furthermore, while it is difficult to achieve a configuration in which the first cathode active material 100x does not contact the electrolyte in the cathode active material layer, the presence of the second cathode active material 100y can reduce the area in contact with the electrolyte of the first cathode active material 100x. Therefore, a safer cathode can be provided. A decomposition product of the electrolyte may be attached to a small area where the first cathode active material 100x contacts the electrolyte, i.e., a portion of the surface of the first cathode active material 100x. Furthermore, a decomposition product of the electrolyte may be attached to the entire surface or a portion of the surface of the second cathode active material 100y. The decomposition product of the electrolyte can be interpreted as a decomposition product of the electrolyte solution. The decomposition product is believed to be able to suppress excessive reaction with the electrolyte, thereby providing a safer cathode. Therefore, a decomposition product may be attached to the cathode active material of the cathode active material composite 100α, which is one embodiment of the present invention.
[0069] Furthermore, the presence of the second positive electrode active material 100y is expected to lower the potential applied to the first positive electrode active material 100x. Therefore, even when the first positive electrode active material 100x is exposed to a high voltage, the voltage on the surface of the first positive electrode active material 100x is reduced, thereby suppressing electrolyte decomposition and providing a safer positive electrode. Although a reduction in voltage can be a concern, the present invention can increase the electrode density as described above, thereby eliminating the reduction in discharge capacity. Furthermore, since the second positive electrode active material 100y is also an active material capable of absorbing and releasing carrier ions, the reduction in discharge capacity can be eliminated.
[0070] <Smooth Surface of Positive Electrode Active Material> The surface shape of the positive electrode active material of the positive electrode active material composite 100α will be described. The positive electrode active material should be smooth overall. In other words, the surface of the positive electrode active material should be glossy overall. Such a positive electrode active material can be said to be rounded or have no corners. It is desirable that the surface be smooth overall even when the first positive electrode active material 100x and the second positive electrode active material 100y are sintered.
[0071] To satisfy the above-mentioned requirement, it is preferable that at least the first positive electrode active material 100x has no or very few ultrafine particles attached to its surface in a powder evaluation. In this specification, ultrafine particles refer to metal oxide particles having a particle size of 0.001 μm or more and 0.1 μm or less. The ultrafine particles may be fragments of the positive electrode active material and / or unreacted starting material (additive element source) for the additive element X.
[0072] The particle diameter of the ultrafine particles is the Feret diameter or the projected circle equivalent diameter measured from a surface SEM (Scanning Electron Microscope) image. For example, when the ultrafine particles are 10 particles / cm in a surface SEM image, 2 Preferably 5 or less per cm 2 If the number is below this, it can be said that there are no or very few microparticles.
[0073] The surface smoothness can be quantified from a cross-sectional SEM image of the first positive electrode active material 100x. First, the first positive electrode active material 100x is processed using an FIB or the like to expose the cross section. At this time, it is preferable to cover the first positive electrode active material 100x with a protective film, protective agent, or the like. Next, an SEM image of the interface between the protective film or the like and the first positive electrode active material 100x is taken. Noise processing is performed on the SEM image using image processing software. For example, Gaussian blurring (σ = 2) is performed, followed by binarization. Furthermore, interface extraction is performed using image processing software. Furthermore, the interface line between the protective film or the like and the first positive electrode active material 100x is selected using a magic hand tool or the like, and the data is extracted into spreadsheet software or the like. Note that the image processing software used for noise processing, interface extraction, etc. is not particularly limited, but for example, "ImageJ" can be used.
[0074] Next, using a function of a spreadsheet software or the like, correction is performed from the regression curve (quadratic regression), and roughness calculation parameters are obtained from the data after the slope correction, and the root mean square surface roughness (RMS) is calculated by calculating the standard deviation. The spreadsheet software or the like is not particularly limited, but for example, Microsoft Office Excel can be used. The surface roughness thus obtained is the surface roughness at 400 nm from the outer periphery of the first positive electrode active material 100x.
[0075] The particle surfaces of the first positive electrode active material 100x preferably have a root mean square (RMS) surface roughness, which is an index of roughness, of less than 3 nm, preferably less than 1 nm, and more preferably less than 0.5 nm.
[0076] The smooth surface has been explained using the powder evaluation of the first positive electrode active material 100x, but it is preferable that the powder evaluation of the second positive electrode active material 100y and other positive electrode active materials contained in the positive electrode active material composite 100α also have a similar state to that of the first positive electrode active material 100x.
[0077] <Crystallinity> The crystallinity of the positive electrode active material of the positive electrode active material composite 100α will be described. High crystallinity is preferable, and single crystal or polycrystalline is more preferable. In particular, if the positive electrode active material is single crystal, cracks are less likely to occur even if volume changes occur in the positive electrode active material due to charge and discharge, which is preferable. Furthermore, if the positive electrode active material is single crystal, secondary batteries using the positive electrode active material are highly safe, which is preferable.
[0078] To satisfy the above requirement, it is desirable that at least first positive electrode active material 100x exhibits single crystal or polycrystal in powder evaluation. It is also desirable that second positive electrode active material 100y and other positive electrode active materials contained in positive electrode active material composite 100α exhibit single crystal or polycrystal in powder evaluation, similar to first positive electrode active material 100x.
[0079] <Dislocations> The first positive electrode active material 100x, particularly the inner portion 100xb, preferably has few defects including dislocations. Dislocations are a type of crystal defect and are different from point defects. Such dislocations can be observed, for example, using a TEM. When the density of defects such as dislocations is sufficiently low, defects such as dislocations may not be observed in a specific 1 μm square of the observed sample. Dislocations are a type of crystal defect and are different from point defects. In addition, in powder evaluation of the second positive electrode active material 100y and other positive electrode active materials contained in the positive electrode active material composite 100α, it is preferable that defects including dislocations be few, as with the first positive electrode active material 100x.
[0080] <Crystallite Size> The crystallite size of the positive electrode active material of the positive electrode active material composite 100α will be described. The crystallite size is measured by XRD. Specifically, the crystallite size is preferably, for example, 300 nm or more. There is a relationship in which the fewer dislocations in the region observed by TEM described above, the larger the crystallite size measured by XRD.
[0081] The crystallite size is calculated using, for example, a Bruker D8 ADVANCE XRD device and CuKα as an X-ray source. 1 The diffraction pattern was acquired using a Lynxeye XE-T detector with a 2θ angle of 15° to 90° in increments of 0.005°, and the literature value for lithium cobalt oxide was ICSD Coll. Code 172909. Analysis can be performed using DIFFRAC. TOPAS ver. 6 crystal structure analysis software. It is preferable to use the LVol-IB value calculated by this method as the crystallite size.
[0082] When calculating the crystallite size, the diffraction pattern is preferably obtained using only the positive electrode active material as the measurement target. However, it may also be obtained for the positive electrode, which includes the positive electrode active material, a current collector, a binder, a conductive material, etc. However, in the positive electrode state, the positive electrode active material may be oriented due to the influence of pressure, etc., during the positive electrode fabrication process. Strong orientation may prevent accurate calculation of the crystallite size. Therefore, it is more preferable to obtain the pattern by removing the positive electrode active material layer from the positive electrode, removing some of the binder, etc., in the positive electrode active material layer using an organic solvent, etc., and then loading the sample into a sample holder. Alternatively, for powder samples, the diffraction pattern can be obtained by applying grease to a silicon anti-reflection plate and then adhering the powder.
[0083] <Differential Scanning Calorimetry> In differential scanning calorimetry (DSC), the positive electrode active material composite 100α is expected to have a smaller calorific value than when only the first positive electrode active material 100x is measured. The DSC measurement can be performed using a high-sensitivity differential scanning calorimeter (Thermo plus EVO2 DSC8231) manufactured by Rigaku.
[0084] A cathode active material layer according to one embodiment of the present invention may have a cathode active material composite 100α as shown in FIG. 1B . The cathode active material composite 100α shown in FIG. 1B shows a second cathode active material 100y having an average particle size and a maximum particle size that satisfy the average particle size range of 0.1 μm to 5 μm and a maximum particle size of less than 9 μm, respectively, and that is smaller than the second cathode active material 100y shown in FIG. 1A . It can be seen that as the average particle size and / or maximum particle size of the second cathode active material 100y decreases, the contact area with the first cathode active material 100x, i.e., the interface with the first cathode active material 100x, increases. The cathode active material composite 100α shown in FIG. 1B is a preferred embodiment that can further reduce the area of contact between the first cathode active material 100x and the electrolyte. The other configurations of FIG. 1B are similar to those described with reference to FIG. 1A .
[0085] A cathode active material layer according to one embodiment of the present invention may include a cathode active material composite 100α as shown in FIG. 2A . As shown in FIG. 2A , the cathode active material composite 100α according to one embodiment of the present invention may include a second cathode active material 100y covered with a carbon layer 102. The higher the electrical resistance of the material used for the second cathode active material 100y, the more improved its safety. Therefore, a structure in which the resistance is appropriately reduced by using the carbon layer 102 is desirable. Furthermore, the second cathode active material 100y covered with the carbon layer 102 is expected to further reduce the potential applied to the first cathode active material 100x. The other configurations in FIG. 2A are similar to those described with reference to FIGS. 1A and 1B .
[0086] A positive electrode active material layer of one embodiment of the present invention may include a positive electrode active material composite 100α as shown in FIG. 2B . As shown in FIG. 2B , the positive electrode active material composite 100α of one embodiment of the present invention may include a carbon layer 103 between a first positive electrode active material 100x and a second positive electrode active material 100y. The carbon layer 103 may include one or more materials selected from carbon black such as acetylene black and furnace black, graphite such as artificial graphite and natural graphite, carbon fibers such as carbon nanofibers and carbon nanotubes, and graphene compounds. Furthermore, the carbon layer 103 may include a binder in addition to the conductive material, as long as the conductive material has a higher mixing ratio than the binder. The carbon layer 103 is expected to further reduce the potential applied to the first positive electrode active material 100x. The other configurations of FIG. 2B are similar to those described with reference to FIGS. 1A to 2A .
[0087] A cathode active material layer of one embodiment of the present invention may include a cathode active material composite 100α as shown in FIG. 3A . As shown in FIG. 3A , the cathode active material composite 100α of one embodiment of the present invention may include a third cathode active material 100z in addition to a first cathode active material 100x and a second cathode active material 100y. The second cathode active material 100y has a small particle size within the ranges satisfying the average particle size and maximum particle size requirements, as shown in FIG. 1B . The third cathode active material 100z preferably has an average particle size of 5 μm to 9 μm and may have a medium particle size (also referred to as a medium particle size). The content of the third cathode active material 100z may be less than the content of the second cathode active material 100y. The content may be expressed in mass %. Adding two or more cathode active materials with different particle sizes to the first cathode active material 100x can also increase the density of the cathode active material contributing to the battery reaction in the cathode active material layer. The third positive electrode active material 100z may have the same composition as the second positive electrode active material 100y or the first positive electrode active material 100x. The other configurations of FIG. 3A are the same as those described with reference to FIGS. 1A to 2B.
[0088] The cathode active material layer of one embodiment of the present invention may include a cathode active material composite 100α as shown in FIG. 3B . As shown in FIG. 3B , the cathode active material composite 100α of one embodiment of the present invention may include a third cathode active material 100z in addition to a first cathode active material 100x and a second cathode active material 100y. The third cathode active material 100z may have the same composition as the second cathode active material 100y or the first cathode active material 100x. Furthermore, the third cathode active material 100z preferably includes a surface layer portion 100za and an interior portion 100zb. The surface layer portion 100za may have the same composition as the surface layer portion 100xa, and the interior portion 100zb may have the same composition as the interior portion 100xb. The content of the third cathode active material 100z may be less than the content of the second cathode active material 100y. The content may be expressed as a numerical value in mass %. Adding two or more positive electrode active materials with different particle sizes to the first positive electrode active material 100x can also increase the density of the positive electrode active material that contributes to the battery reaction in the positive electrode active material layer. The other configurations of FIG. 3B are the same as those described with reference to FIGS. 1A to 3A.
[0089] [Cathode Active Material Composite] Regarding the cathode active material composite of one embodiment of the present invention, a configuration including a first cathode active material 100x and a second cathode active material 100y and a configuration including a first cathode active material 100x, a second cathode active material 100y, and a third cathode active material 100z have been described. However, a desirable form of the cathode active material composite is a configuration in which at least a portion of the surface of the first cathode active material 100x, which has a smooth surface, is covered with the second cathode active material 100y. Alternatively, a desirable form of the cathode active material composite is a configuration in which at least a portion of the surface of the first cathode active material 100x, which has a smooth surface, is covered with the second cathode active material 100y and the third cathode active material 100z.
[0090] Here, "covering the first cathode active material 100x" preferably refers to a structure in which at least substantially the entire surface of the first cathode active material 100x is covered with the second cathode active material 100y, and "substantially covering the entire surface" refers to an ideal state in which the first cathode active material 100x does not come into direct contact with the electrolyte. Therefore, in the present invention, a portion of the surface of the first cathode active material 100x may be covered with the third cathode active material 100z. In other words, the above-described state is a state in which the second cathode active material 100y and / or the third cathode active material 100z covers 80% or more, preferably 90% or more, of the first cathode active material 100x in one cross section of the cathode active material composite.
[0091] By covering at least a portion of the surface of the first positive electrode active material 100x with the second positive electrode active material 100y and / or the third positive electrode active material 100z, the area of the first positive electrode active material 100x in direct contact with the electrolyte is reduced. This reduces the desorption of transition metal elements and / or oxygen from the first positive electrode active material 100x during high-voltage charging. Furthermore, this reduces the desorption of additive element X and / or oxygen from the first positive electrode active material 100x during high-voltage charging. This reduces capacity loss due to repeated charge / discharge.
[0092] Furthermore, when at least a portion of the surface of the first positive electrode active material 100x is covered with the second positive electrode active material 100y and / or the third positive electrode active material 100z, etc., there is a possibility that charge / discharge characteristics different from those obtained when the first positive electrode active material 100x and the second positive electrode active material 100y and / or the third positive electrode active material 100z are simply mixed together.
[0093] Furthermore, by using the second cathode active material 100y and / or the third cathode active material 100z, which have a stable crystal structure even in a high-voltage charging state, a secondary battery using the cathode active material composite of one embodiment of the present invention can achieve effects such as improved safety. In particular, by using, as the first cathode active material 100x, a material that has excellent stability in a high-voltage charging state, such as lithium cobalt oxide to which magnesium and fluorine are added, lithium cobalt oxide to which magnesium, fluorine, aluminum, and nickel are added, or a metal oxide-coated composite oxide in which secondary particles of nickel-cobalt-manganese lithium oxide having a ratio of nickel:cobalt:manganese=8:1:1 or nickel:cobalt:manganese=9:0.5:0.5 are coated with aluminum oxide, the durability and stability of the cathode active material composite during high-voltage charging can be further improved. Furthermore, the heat resistance and / or fire resistance of a secondary battery using the cathode active material composite can be further improved. Lithium cobalt oxide to which magnesium, fluorine, aluminum, and nickel are added has the characteristic that the surface layer of the positive electrode active material particles contains a large amount of magnesium, fluorine, and aluminum, and nickel is widely distributed throughout the particles. Therefore, when initial heating is performed as described below, the high-voltage charge / discharge cycle characteristics are significantly excellent. Therefore, the above-mentioned lithium cobalt oxide is a particularly preferred material for the first positive electrode active material 100x.
[0094] In the embodiment, a structure in which at least a part of the surface of the positive electrode active material composite is covered with the carbon layer 103 including a graphene compound or the like has also been described as a positive electrode of the present invention. However, the state in which the carbon layer 103 covers the first positive electrode active material 100x means a state in which the carbon layer 103 covers 80% or more, preferably 90% or more, of the first positive electrode active material 100x in one cross section of the positive electrode active material composite.
[0095] [Positive Electrode Active Material] The first positive electrode active material 100x is LiMO having a layered rock salt crystal structure. 2 (M1 is one or more selected from Fe, Ni, Co, Mn, and Al) can be used as the first positive electrode active material 100x. 2The first positive electrode active material 100x may contain one or more additive elements selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic. These elements may further stabilize the crystal structure of the first positive electrode active material 100x. Magnesium is a metal ion that acts as a catalyst for the formation of CoO in lithium cobalt oxide. 2 The first positive electrode active material 100x preferably uses lithium cobalt oxide doped with magnesium, which is an element capable of suppressing layer misalignment. Other examples of the first positive electrode active material 100x include lithium cobalt oxide doped with magnesium and fluorine, lithium cobalt oxide doped with magnesium, fluorine, aluminum, and nickel, lithium cobalt oxide doped with magnesium, fluorine, and titanium, lithium nickel-cobalt oxide doped with magnesium and fluorine, lithium cobalt-aluminate doped with magnesium and fluorine, lithium nickel-cobalt-aluminate doped with magnesium and fluorine, and lithium nickel-cobalt-manganate doped with magnesium and fluorine. Lithium cobalt oxide, lithium nickel-cobalt-aluminate, or lithium nickel-cobalt-manganate without the additional element X may also be used for the first positive electrode active material 100x. It is preferable that the transition metal ratio of nickel in the lithium nickel-cobalt-manganese oxide is high, and for example, materials with a ratio (weight ratio) of nickel:cobalt:manganese = 8:1:1 or nickel:cobalt:manganese = 9:0.5:0.5 are preferable. In the case of the above-mentioned lithium nickel-cobalt-manganese oxide, it is preferable to use calcium as the additive element X.
[0096] The first positive electrode active material 100x is LiMO 2Secondary particles of a composite oxide represented by the formula (M1 is one or more selected from Fe, Ni, Co, Mn, and Al) coated with a metal oxide may be used. The metal oxide may be an oxide of one or more metals selected from Al, Ti, Nb, Zr, La, and Li. For example, LiMO 2 A metal oxide-coated complex oxide in which secondary particles of a complex oxide represented by the formula (M1) (where M1 is one or more selected from Fe, Ni, Co, Mn, and Al) are coated with aluminum oxide can be used as the first positive electrode active material 100x. For example, a metal oxide-coated complex oxide in which secondary particles of nickel-cobalt-manganese lithium having a ratio (by weight) of nickel:cobalt:manganese = 8:1:1 or nickel:cobalt:manganese = 9:0.5:0.5 are coated with aluminum oxide can be used. Here, the coating layer is preferably thin, for example, 1 nm or more to 200 nm or less, more preferably 1 nm or more to 100 nm or less. In addition, in the case of the above-mentioned nickel-cobalt-manganese lithium, calcium is preferably used as the additive element X.
[0097] The first positive electrode active material 100x can be formed using a formation method described in an embodiment to be described later.
[0098] As the second positive electrode active material 100y, LiM2PO4 having an olivine-type crystal structure 4 (M2 is one or more selected from Fe, Ni, Co, and Mn). 4 As an example, LiFePO 4 , LiNiPO 4 , LiCoPO 4 , LiMnPO 4 , LiFe a Ni b P.O. 4 , LiFe a Co b P.O. 4 , LiFe a Mn b P.O. 4 , LiNi a Co b P.O. 4 , LiNi a Mn b P.O.4 (a+b is 1 or less, 0<a<1, 0<b<1), LiFe c Ni d Co e P.O. 4 , LiFe c Ni d Mn e P.O. 4 , LiNi c Co d Mn e P.O. 4 (c+d+e is 1 or less, 0<c<1, 0<d<1, 0<e<1), LiFe f Ni g Co h Mn i P.O. 4 (f+g+h+i is 1 or less, 0<f<1, 0<g<1, 0<h<1, 0<i<1), etc. In addition, carbon layer 102 may be provided on the particle surface of second positive electrode active material 100y.
[0099] The second positive electrode active material 100y can be formed by a known method.
[0100] [Carbon Layer] The carbon layer 103 of the positive electrode active material composite 100α will now be described. The carbon layer 103 may be made of one or more materials selected from carbon black such as acetylene black and furnace black, graphite such as artificial graphite and natural graphite, carbon fibers such as carbon nanofibers and carbon nanotubes, and graphene compounds.
[0101] In this specification and the like, graphene compounds include multilayer graphene, multigraphene, graphene oxide, multilayer graphene oxide, multi-graphene oxide, reduced graphene oxide, reduced multilayer graphene oxide, reduced multi-graphene oxide, etc. Graphene compounds contain carbon, have a shape such as a plate or sheet, and have a two-dimensional structure formed by six-membered carbon rings. They preferably have a curved shape. Graphene compounds having a shape such as a plate or sheet may also be called carbon sheets. They preferably have functional groups. Graphene compounds may also be rolled up into a shape like carbon nanofibers.
[0102] In this specification and the like, graphene oxide refers to, for example, a material that contains carbon and oxygen, has a sheet-like shape, and has a functional group, in particular, an epoxy group, a carboxy group, or a hydroxy group.
[0103] In this specification, reduced graphene oxide refers to, for example, a material containing carbon and oxygen, having a sheet-like shape, and having a two-dimensional structure formed by six-membered carbon rings. Reduced graphene oxide may also be referred to as a carbon sheet. A single reduced graphene oxide can function, but multiple sheets may be stacked. Reduced graphene oxide preferably has a portion where the carbon concentration is greater than 80 atomic % and the oxygen concentration is 2 atomic % or more and 15 atomic % or less. By achieving such carbon and oxygen concentrations, reduced graphene oxide can function as a highly conductive material even in small amounts. Furthermore, reduced graphene oxide preferably has an intensity ratio G / D of the G band to the D band in a Raman spectrum of 1 or more. Reduced graphene oxide with such an intensity ratio can function as a highly conductive material even in small amounts.
[0104] By reducing graphene oxide, it is sometimes possible to provide holes in the graphene compound. That is, it is preferable that the graphene compound has holes in parts of the carbon sheet. In the graphene compound, by providing holes in parts of the carbon sheet through which carrier ions such as lithium ions can pass, the insertion and desorption of carrier ions becomes easier on the surface of the active material covered with the graphene compound, and the rate characteristics of the secondary battery can be improved. The holes provided in parts of the carbon sheet are sometimes called vacancies, defects, or gaps.
[0105] A preferred method for reducing graphene oxide is to use graphene oxide as a graphene compound, mix it with an active material, and then reduce the graphene oxide to form an active material layer. In other words, the completed active material layer preferably contains reduced graphene oxide. By using graphene oxide, which has extremely high dispersibility in a polar solvent, to form the graphene compound, the graphene compound can be dispersed uniformly in the active material layer. The solvent is volatilized and removed from the dispersion medium containing uniformly dispersed graphene oxide, and the graphene oxide is reduced. The graphene compound remaining in the active material layer partially overlaps and is dispersed to such an extent that it is in surface contact with each other, thereby forming a three-dimensional conductive path. The graphene oxide may be reduced, for example, by heat treatment or by using a reducing agent.
[0106] The carbon layer 103 may also include a material in which the edges of graphene are terminated with fluorine.
[0107] The graphene compound described above is in a sheet form. Therefore, a state in which the sheet-like graphene compound is dispersed may be observed in a cross section of the active material layer. The plurality of graphene compounds are formed so as to partially cover the plurality of granular active materials or to be attached to the surfaces of the plurality of granular active materials, and are in surface contact with each other.
[0108] A mesh-like graphene compound sheet (hereinafter referred to as a graphene compound net or graphene net) can be formed by bonding multiple graphene compounds together. When an active material is covered with a graphene net, the graphene net can also function as a binder that bonds the active materials together. Therefore, the amount of binder can be reduced or no binder can be used, thereby improving the ratio of the active material to the electrode volume and electrode weight. In other words, the discharge capacity of a secondary battery can be increased.
[0109] Furthermore, by using a spray dryer, it is possible to form a coating of a graphene compound, which is a conductive material, covering the entire surface of the active material. Since the graphene compound is located between the active materials, the graphene compound electrically connects them to form a conductive path.
[0110] The graphene compound may also contain a catalyst used in forming the graphene compound. Examples of the catalyst used in forming the graphene compound include silicon oxide (SiO 2 , SiO x (x<2)), aluminum oxide, iron, nickel, ruthenium, iridium, platinum, copper, germanium, etc. The particles preferably have a D50 of 1 μm or less, more preferably 100 nm or less.
[0111] [Method for Producing Cathode Active Material Composite] The above-described cathode active material composite 100α can be obtained by subjecting the prepared cathode active materials to a composite treatment. Examples of the composite treatment include mechanical energy-based composite treatments such as mechanochemical, mechanofusion, and ball milling. Other examples of the composite treatment include liquid-phase reaction-based composite treatments such as coprecipitation, hydrothermal, and sol-gel. Other examples of the composite treatment include gas-phase reaction-based composite treatments such as barrel sputtering, atomic layer deposition (ALD), vapor deposition, and chemical vapor deposition (CVD). In other words, one or more of the above methods can be used for the composite treatment. Furthermore, a heat treatment may be performed after the composite treatment.
[0112] In this embodiment, a manufacturing method in which a first positive electrode active material 100x and a second positive electrode active material 100y are combined with each other by mechanical energy will be described with reference to FIGS. 4A and 4B. However, the present invention should not be construed as being limited to these descriptions.
[0113] In step S101 of FIG. 4A, a first positive electrode active material 100x is prepared, and in step S102, a second positive electrode active material 100y is prepared.
[0114] As the first positive electrode active material 100x, LiMO 2 (M1 is one or more selected from Fe, Ni, Co, Mn, and Al) is preferably used, and it is further preferable to use a composite oxide having an additive element X added thereto, such as lithium cobalt oxide to which magnesium and fluorine have been added, or lithium cobalt oxide to which magnesium, fluorine, aluminum, and nickel have been added. In particular, it is preferable to use lithium cobalt oxide that has been subjected to initial heating. Initial heating makes it possible to obtain lithium cobalt oxide with a smooth surface. Initial heating refers to heating of lithium cobalt oxide, and it is preferable to perform initial heating before introducing the additive element X in order to obtain a smooth surface.
[0115] Another example of the first positive electrode active material 100x is lithium nickel-cobalt-manganese oxide, in which a high nickel ratio is preferable as the transition metal ratio of the lithium nickel-cobalt-manganese oxide, such as nickel:cobalt:manganese=8:1:1 or nickel:cobalt:manganese=9:0.5:0.5.
[0116] As another example of the first positive electrode active material 100x, a metal oxide-coated composite oxide can be used, in which secondary particles of the nickel-cobalt-lithium manganese oxide are coated with a metal oxide, typically aluminum oxide. The thickness of the metal oxide is preferably small, for example, from 1 nm to 200 nm, more preferably from 1 nm to 100 nm.
[0117] The second positive electrode active material 100y is LiM2PO4 having an olivine-type crystal structure. 4 (M2 is one or more selected from Fe, Ni, Co, and Mn). 4 Materials mentioned above as, for example, LiFePO 4 , LiMnPO 4 , LiFe a Mn b P.O. 4 (a+b is 1 or less, 0<a<1, 0<b<1), LiFe a Ni bP.O. 4 (a+b is 1 or less, 0<a<1, 0<b<1) can be used. In addition, a carbon layer 102 may be provided on the surface of the second positive electrode active material 100y. Note that, since the second positive electrode active material 100y only needs to satisfy the small particle size requirement, it is possible to use the same composition as the positive electrode active material described for the first positive electrode active material 100x.
[0118] It is desirable to select a combination of the first positive electrode active material 100x and the second positive electrode active material 100y that is unlikely to produce a step in the charge / discharge curve, depending on the characteristics required of the secondary battery. Alternatively, it is desirable to select a combination of the first positive electrode active material 100x and the second positive electrode active material 100y that produces a step in the charge / discharge curve at a desired charge rate. If a step occurs in the charge / discharge curve, it is preferable that the step be located at a charge rate that does not affect the circuit design.
[0119] Next, in step S103, the first positive electrode active material 100x and the second positive electrode active material 100y are combined. When the combination is performed using mechanical energy, the combination can be performed by a mechanochemical method. Alternatively, the combination can be performed by a mechanofusion method.
[0120] Furthermore, when a ball mill is used in step S103, it is preferable to use, for example, zirconia balls as media. For the purpose of mixing, dry ball milling is preferable. When wet ball milling is used, acetone can be used. When wet ball milling is used, it is recommended to use dehydrated acetone with a moisture content of 100 ppm or less, preferably 10 ppm or less.
[0121] The composite treatment in step S103 makes it possible to create a state in which at least a portion, and preferably substantially the entire particle surface of first positive electrode active material 100x is covered with second positive electrode active material 100y.
[0122] Through the above steps, positive electrode active material composite 100α of one embodiment of the present invention can be produced (Step S104).
[0123] 4B is the same as the manufacturing method shown in FIG. 4A up to step S103, and after step S103, a heat treatment is performed as step S104. The heating in step S104 is preferably performed in an oxygen-containing or nitrogen-containing atmosphere at a temperature of 500° C. to 950° C., preferably 600° C. to 850° C., for 1 hour to 60 hours, preferably 2 hours to 20 hours. Heating at 600° C. to 850° C. in an oxygen-containing or nitrogen-containing atmosphere can increase the electrode density of the positive electrode active material composite 100α.
[0124] Through the above steps, the positive electrode active material composite 100α of one embodiment of the present invention can be produced (Step S105).
[0125] In order to obtain a good coating state in the composite treatment, the ratio of the particle diameter of the second positive electrode active material 100y to the particle diameter of the first positive electrode active material 100x (particle diameter of the second positive electrode active material 100y / particle diameter of the first positive electrode active material 100x) is preferably 1 / 50 or more and 1 / 2 or less, and more preferably 1 / 20 or more and 1 / 5 or less.
[0126] [Fluorination Treatment] The prepared positive electrode active materials may be subjected to a fluorination treatment. This can increase the fluorine concentration on the surface of each positive electrode active material. A positive electrode active material with a high fluorine concentration can suppress the elution of the additive element X and / or transition metal from the positive electrode active material.
[0127] Fluorination treatments include, for example, direct reaction with fluorine gas or a mixed gas of fluorine gas and an inert gas. For example, the cathode active material to be treated is left in fluorine gas or a mixed gas for a certain period of time. Alternatively, the cathode active material to be treated is subjected to plasma treatment using fluorine gas or a mixed gas. As a result, a cathode active material having fluorine on its surface is obtained. The fluorination treatment may also be performed using hydrofluoric acid. The fluorination treatment may result in partial substitution of fluorine for oxygen in magnesium oxide present in the surface layer 100xa. That is, partial substitution of fluorine for oxygen in the oxide containing the additive element X present in the surface layer 100xa. Fluorine has a high electronegativity and can substitute for oxygen. Furthermore, if the oxide containing the additive element X has oxygen vacancies, fluorine may bond to the vacancies. Preferably, the fluorine is present at least on the outermost surface of the cathode active material. Because this outermost surface is the region in contact with the electrolyte, it is generally the first to deteriorate, but the presence of fluorine can suppress deterioration. In other words, the fluorination treatment improves resistance to the electrolyte. This makes it possible to provide a secondary battery that is less likely to ignite in a nail penetration test and is highly safe.
[0128] 5A is the same as the manufacturing method shown in FIG. 4A up to step S102, and after step S101, the above-mentioned fluorination treatment is performed as step S203. Thereafter, step S103 is performed, and this step S103 is the same as the manufacturing method shown in FIG. 4A.
[0129] Through the above steps, positive electrode active material composite 100α of one embodiment of the present invention can be produced (Step S104).
[0130] 5B is the same as the manufacturing method shown in FIG. 5A up to step S203, and after step S102, the above-mentioned fluorination treatment is performed as step S204. Then, step S103 is performed, and this step S103 is the same as the manufacturing method shown in FIG. 4A.
[0131] Through the above steps, positive electrode active material composite 100α of one embodiment of the present invention can be produced (Step S104).
[0132] 5C is the same as the fabrication method shown in FIG. 4A up to step S102, and in a state in which first positive electrode active material 100x and second positive electrode active material 100y are mixed, the fluorination treatment described above is performed in step S203. Thereafter, step S103 is performed, which is the same as the fabrication method shown in FIG. 4A.
[0133] Through the above steps, positive electrode active material composite 100α of one embodiment of the present invention can be produced (Step S104).
[0134] Although the method using the first positive electrode active material 100x and the second positive electrode active material 100y has been described with reference to FIGS. 4 and 5, the same procedure can be followed when adding the third positive electrode active material 100z.
[0135] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0136] (Embodiment 2) In this embodiment, a nail penetration test will be described. The nail penetration test is one of the tests for verifying the safety of a secondary battery, in which a secondary battery is fully charged and a nail having a predetermined diameter selected from the range of 2 mm to 10 mm is thrust into the secondary battery at a predetermined speed.
[0137] <Nail Penetration Test Apparatus> First, the nail penetration test apparatus will be described. FIG. 6A shows a side view of the nail penetration test apparatus 1000, and FIG. 6B shows a perspective view of the stage of the nail penetration test apparatus 1000. The nail penetration test apparatus 1000 shown in FIG. 6A includes a stage 1001, a drive unit 1002, a nail 1003, a voltage measuring device 1015, a temperature measuring device 1016, and a control unit 1018. The drive unit 1002 includes a drive mechanism 1012 that moves the nail 1003 in the direction of the arrow in the figure, and the drive mechanism 1012 operates so that the nail 1003 penetrates a secondary battery 1004 placed on the stage 1001. At this time, the secondary battery 1004 is in a fully charged state (State of Charge: a state equivalent to 100% SOC), and this operation is called a nail penetration operation. The dashed line in FIG. 6A indicates a recess in the stage 1001 that is provided to accommodate the nail 1003 after penetration during the nail insertion operation.
[0138] The voltage measuring device 1015 transmits information about the voltage of the secondary battery during the nail penetration operation to the control unit 1018. Specifically, the amount of voltage change and the like are transmitted to the control unit 1018. Furthermore, the temperature measuring device 1016 transmits information about the temperature during the nail penetration operation to the control unit 1018. When controlling the operating conditions of the nail 1003, the control unit 1018 can transmit a control signal to the drive unit 1002.
[0139] FIG. 6B is a perspective view illustrating the vicinity of the upper portion of the stage 1001 of the nail penetration test device 1000. The secondary battery 1004 placed on the stage 1001 is electrically connected to wires 1005a and 1005b. The wires 1005a and 1005b belong to a voltage measuring device 1015, which are electrically connected to the positive and negative electrode tabs of the secondary battery 1004, respectively, to measure the voltage of the secondary battery 1004. The voltage of the secondary battery 1004 is simply referred to as voltage, voltage value between the positive and negative electrodes, battery voltage, cell voltage, or open-circuit voltage. When a temperature sensor is used as the temperature measuring device 1016, the temperature sensor is disposed so as to contact the surface of the exterior body of the secondary battery 1004.
[0140] 6B shows an example in which a first temperature sensor 1006a and a second temperature sensor 1006b are arranged, but one temperature sensor or three or more temperature sensors may be arranged. In FIG. 6B, the first temperature sensor 1006a is arranged on the side where the wiring 1005a and the wiring 1005b are not arranged, and the second temperature sensor 1006b is arranged on the side where the wiring 1005a and the wiring 1005b are arranged. Arranging two or more temperature sensors is preferable because even if one temperature sensor becomes unusable due to expansion of the exterior body or the like, the other temperature sensors can be used.
[0141] Furthermore, there is a welded region on the side where the wiring 1005a and the wiring 1005b are arranged, but there is no welded region on the side where the wiring 1005a and the wiring 1005b are not arranged because the exterior body is folded back. Therefore, even if the exterior body expands, expansion on the side where the wiring 1005a and the wiring 1005b are not arranged is suppressed, and the first temperature sensor 1006a is more unlikely to peel off than the second temperature sensor 1006b, which is preferable.
[0142] The dashed ellipse shown in Figure 6B is the area where the nail 1003 penetrates the secondary battery 1004 during the nail penetration operation. The first temperature sensor 1006a and the second temperature sensor 1006b are preferably provided in areas equidistant from the area where the nail 1003 penetrates. Typically, the first temperature sensor 1006a and the second temperature sensor 1006b are preferably provided within 5 cm, preferably within 2 cm, of the area where the nail 1003 penetrates. This is preferable because it allows for the detection of temperature changes in the vicinity of the area where the nail 1003 penetrates. When two or more temperature sensors are provided, it is preferable to start the nail penetration operation after confirming that the difference in temperature indicated by the temperature sensors is within ±5°C, preferably within ±2°C.
[0143] <Secondary Battery in Nail Penetration Test> Next, the state of a secondary battery in a nail penetration test will be described again with reference to FIG. 7 and other figures. The nail penetration test involves inserting a nail 1003 having a predetermined diameter selected from 2 mm to 10 mm into a fully charged secondary battery 1004 at a predetermined speed. FIG. 7 shows a cross-sectional view of the secondary battery 1004 with the nail 1003 inserted. The secondary battery 1004 has a structure in which a positive electrode 503, a separator 508, a negative electrode 506, and an electrolyte 530 are housed in an outer casing 541. The positive electrode 503 includes a positive electrode current collector 501 and positive electrode active material layers 502 formed on both sides thereof. It is preferable to apply the configuration described in the above embodiment to the positive electrode active material layer. The negative electrode 506 includes a negative electrode current collector 521 and negative electrode active material layers 512 formed on both sides thereof.
[0144] As shown in Figure 7, when a nail 1003 is inserted into a secondary battery 1004, specifically, the nail 1003 penetrates the positive electrode 503 and the negative electrode 506, causing an internal short circuit. Then, the potential of the nail 1003 becomes equal to the potential of the negative electrode 506, and electrons (e − ) flows to the positive electrode 503, and Joule heat is generated at the internal short circuit location and its vicinity. In addition, due to the internal short circuit, carrier ions, typically lithium ions (Li + ) are released into the electrolyte as indicated by the white arrow. However, before all the lithium ions are released from the negative electrode, the battery temperature rises rapidly due to Joule heat generated by the internal short circuit, causing the electrolyte to begin to reduce and decompose on the surface of the negative electrode. This is an electrochemical reaction, and is called the reduction reaction of the electrolyte by the negative electrode.
[0145] Furthermore, when the temperature of the secondary battery 1004 rises due to Joule heat, if lithium cobalt oxide is used as the positive electrode active material, the lithium cobalt oxide may undergo a phase change (i.e., a structural change) to an H1-3 type crystal structure or an O1 type crystal structure, which may further generate heat. The H1-3 type crystal structure and the O1 type crystal structure will be described later.
[0146] The electrons (e −) reduces the tetravalent Co in the charged lithium cobalt oxide to trivalent or divalent Co, and this reduction reaction releases oxygen from the lithium cobalt oxide, and the electrolyte 530 is decomposed by an oxidation reaction caused by the oxygen. This is one of the electrochemical reactions, and is called an oxidation reaction of the electrolyte by the positive electrode. The rate at which current flows into the first positive electrode active material 100x, etc., varies somewhat depending on the insulating properties of the positive electrode active material, and it is thought that the rate at which current flows affects the electrochemical reaction.
[0147] As mentioned above, when an internal short circuit occurs in a secondary battery, it is thought that the temperature will change as shown in the graph in Figure 8. Figure 8 is a partially modified version of the graph shown on page 70 [Figures 2-12] of Non-Patent Document 13, and is a graph of the temperature (specifically, the internal temperature) of the secondary battery versus time. When an internal short circuit occurs at (P0), the temperature of the secondary battery rises over time. As shown in (P1), when the temperature of the secondary battery rises to around 100°C due to Joule heat generated by the internal short circuit, it may exceed the reference temperature (Ts), which is the limit temperature at which the secondary battery will not go into thermal runaway. Then, at (P2), the negative electrode (when graphite is used, the negative electrode is C 6 In (P3), the electrolyte is oxidized by the positive electrode and heat is generated, and in (P4), heat is generated due to thermal decomposition of the electrolyte. This leads to thermal runaway in the secondary battery, resulting in fire or smoke.
[0148] At this time, the electrons that suddenly flow into the positive electrode active material convert the cobalt to Co 4+ From Co 2+ This reaction causes the cathode active material to be reduced to oxygen, releasing oxygen. Because this reaction is exothermic, it accelerates thermal runaway. In other words, if this reaction can be suppressed, a safe secondary battery can be made that is less susceptible to thermal runaway.
[0149] In order to suppress the above reaction, for example, the surface layer of the positive electrode active material preferably contains an additive element X that does not easily release oxygen, and further, the concentration of the additive element X is preferably higher than that of the inside. If oxygen is not released from the positive electrode active material, the above reduction reaction (for example, Co 4+ From Co 2+(reaction resulting in the following reaction) is also suppressed. Examples of the additive element X that does not easily release oxygen include magnesium and aluminum. Magnesium is suitable as the additive element X that does not easily release oxygen because the closer the oxygen is to the magnesium, the greater the energy required to desorb it. Nickel is also thought to have the effect of suppressing oxygen release when present at the lithium site.
[0150] Furthermore, even if cobalt or the like is reduced, if lithium ions can be inserted into the positive electrode active material before oxygen is released, electroneutrality is maintained and oxygen release does not occur. Therefore, even if electrons suddenly flow into the positive electrode active material, it is sufficient as long as the crystalline structure of the positive electrode active material is kept stable until the lithium ions are inserted into the positive electrode active material from the negative electrode via the electrolyte.
[0151] Furthermore, in order to prevent smoke generation, heat generation, and the like during a nail penetration test, it is considered effective to suppress the temperature rise of the secondary battery and to ensure that the anode, cathode, and / or electrolyte have stable properties at high temperatures. Specifically, it is preferable that the first cathode active material 100x has a stable structure that does not release oxygen, particularly when exposed to high temperatures. Alternatively, it is preferable that the first cathode active material 100x has a structure that slows the rate of current flow to the cathode active material. This is expected to have significant effects such as reduced thermal runaway and reduced risk of fire, etc. As will be described later, the first cathode active material 100x, which is one embodiment of the present invention, can have both the stable structure and a structure that slows the rate of current flow.
[0152] <Thermal Runaway of Secondary Batteries> Figure 9 shows a partially revised version of the graph shown on page 69 [Figures 2-11] of Non-Patent Document 13, which illustrates the principle of thermal runaway in secondary batteries. When the temperature (specifically, the internal temperature) of the above-mentioned secondary battery rises, for example, during charging, the secondary battery passes through several states and then goes into thermal runaway. Figure 9 is a graph of the temperature of the secondary battery against time. For example, when the temperature of the secondary battery reaches or is close to 100°C, (1) the SEI (Solid Electrolyte Interface) of the negative electrode collapses and heat is generated. Furthermore, when the temperature of the secondary battery exceeds 100°C, (2) the negative electrode (when graphite is used, the negative electrode becomes C 6(3) At or near 150°C, oxidation of the electrolyte by the positive electrode occurs, and heat is generated. When the temperature of the secondary battery reaches or near 180°C, (4) thermal decomposition of the electrolyte occurs, and (5) oxygen is released from the positive electrode and thermal decomposition of the positive electrode (this thermal decomposition includes a structural change in the positive electrode active material). When the temperature of the secondary battery then exceeds 200°C, (6) decomposition of the negative electrode occurs, and finally, (7) direct contact between the positive electrode and the negative electrode occurs. Through these states, particularly states (5), (6), or (7), the secondary battery reaches thermal runaway.
[0153] To prevent thermal runaway, it is considered effective to suppress the temperature rise of the secondary battery and to ensure that the negative electrode, positive electrode and / or electrolyte have stable characteristics at high temperatures.
[0154] <Characteristics of Secondary Battery in Nail Penetration Test> The characteristics of a secondary battery when a nail penetration test is carried out on the secondary battery including the positive electrode having the positive electrode active material composite described in the first embodiment and the like will be described.
[0155] The temperature rise of the secondary battery when subjected to a nail penetration test, i.e., the difference between the temperature before the nail penetration test and the maximum temperature reached after the nail penetration (also referred to as the temperature rise ΔT), is preferably 130°C or less, more preferably 100°C or less, more preferably 70°C or less, and even more preferably 50°C or less. The temperature is measured within 5 cm, preferably within 2 cm, of the nail hole, and specifically, the value is output by a temperature sensor located within 5 cm, preferably within 2 cm, of the nail hole. The temperature sensor is preferably provided so as to be in contact with the exterior body of the secondary battery.
[0156] The maximum temperature during the nail penetration test is preferably 250° C. or lower, more preferably 200° C. or lower, and even more preferably 180° C. or lower, and more preferably lower than the temperature at which oxygen is released from the positive electrode and thermal decomposition of the positive electrode occurs.
[0157] Furthermore, the maximum temperature during the nail penetration test is preferably 150°C or lower, more preferably 100°C or lower, and even more preferably 80°C or lower. More preferably, it is lower than the temperature at which oxidation of the electrolyte occurs due to the positive electrode. Even more preferably, the maximum temperature is lower than the flash point of the mixed solvent used in the electrolyte. If the flash point of the mixed solvent is unknown, the flash point of each solvent can be used as a reference. Even more preferably, it is lower than the softening point of the separator. For example, the softening point of polypropylene that can be used for the separator is approximately 155°C.
[0158] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0159] Embodiment 3 In this embodiment, a first positive electrode active material 100x will be described.
[0160] <Containing Elements> The first positive electrode active material 100x contains lithium, a transition metal M1, oxygen, and an additional element X. The first positive electrode active material 100x contains LiM1O 2 However, the positive electrode active material of one embodiment of the present invention is LiMO 2 The composition is not strictly limited to Li:M1:O=1:1:2.
[0161] The transition metal M1 contained in the first positive electrode active material 100x is preferably a metal capable of forming a layered rock-salt composite oxide belonging to the space group R-3m with lithium. For example, at least one of manganese, cobalt, and nickel can be used. That is, the transition metal contained in the first positive electrode active material 100x may be cobalt alone, nickel alone, a combination of cobalt and manganese, or a combination of cobalt and nickel, or three of cobalt, manganese, and nickel. That is, the first positive electrode active material 100x may have a composite oxide containing lithium and the transition metal M1, such as lithium cobalt oxide, lithium nickel oxide, lithium cobalt oxide in which some of the cobalt is substituted with manganese, lithium cobalt oxide in which some of the cobalt is substituted with nickel, or nickel-manganese-lithium cobalt oxide.
[0162] In particular, when cobalt is used as the transition metal M1 in the first positive electrode active material 100x in an amount of 75 atomic % or more, preferably 90 atomic % or more, and more preferably 95 atomic % or more, it has many advantages, such as being relatively easy to synthesize and handle, and having excellent cycle characteristics.
[0163] On the other hand, when nickel is used as the transition metal M1 in the first positive electrode active material 100x in an amount of 33 atomic % or more, preferably 60 atomic % or more, and more preferably 80 atomic % or more, the raw material may be cheaper than when a large amount of cobalt is used, and the discharge capacity per weight may be increased, which is preferable.
[0164] Furthermore, the inclusion of nickel as a transition metal M1 along with cobalt can suppress the shift in the layered structure of cobalt and oxygen octahedra. This is preferable because the crystal structure can be more stable, particularly in the charged state at high temperatures. This is because nickel easily diffuses deep into the lithium cobalt oxide, and while it is present at the cobalt site during discharge, it is thought to be located at the lithium site through cation mixing during charge. The nickel present at the lithium site during charge functions as a pillar supporting the layered structure of cobalt and oxygen octahedra, contributing to the stabilization of the crystal structure.
[0165] The transition metal M1 does not necessarily have to contain manganese, nickel, or cobalt.
[0166] It is preferable to use at least one of magnesium, fluorine, aluminum, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic as the additive element X. When phosphorus is used as the additive element X, it is possible to improve the continuous charge durability and to provide a secondary battery with high safety, which is preferable.
[0167] Furthermore, since manganese, titanium, vanadium, and chromium are materials that are stable and easily tetravalent, using them as the transition metal M1 of the first positive electrode active material 100x may enhance their contribution to structural stability.
[0168] These additional elements X may further stabilize the crystal structure of the first positive electrode active material 100x. That is, the first positive electrode active material 100x may include lithium cobalt oxide to which magnesium and fluorine have been added, lithium nickel-cobalt oxide to which magnesium and fluorine have been added, lithium cobalt-aluminate to which magnesium and fluorine have been added, nickel-cobalt-lithium aluminum oxide to which magnesium and fluorine have been added, nickel-cobalt-lithium aluminum oxide to which magnesium and fluorine have been added, lithium nickel-manganese-cobalt oxide to which magnesium and fluorine have been added, etc. In this specification and the like, the additional element X may be referred to as a mixture, a part of a raw material, an impurity, etc.
[0169] The additive element X in the first positive electrode active material 100x is LiMO 2 It is preferable that the amount of the compound added is such that the crystallinity of the composite oxide represented by the formula (1) is not significantly changed. For example, it is preferable that the amount is such that the Jahn-Teller effect is not exhibited.
[0170] The additional element X does not necessarily have to include magnesium, fluorine, aluminum, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, or arsenic.
[0171] <Inner portion 100xb> The inner portion 100xb includes lithium, a transition metal, and oxygen. It can be said that the inner portion 100xb includes a composite oxide including lithium and a transition metal. The inner portion 100xb may include the above-described lithium cobalt oxide doped with magnesium and fluorine, lithium nickel-cobalt oxide doped with magnesium and fluorine, lithium cobalt-aluminate doped with magnesium and fluorine, lithium nickel-cobalt-aluminate, lithium nickel-cobalt-aluminate doped with magnesium and fluorine, or lithium nickel-manganese-cobalt oxide doped with magnesium and fluorine.
[0172] The internal 100xb preferably has a layered rock-salt type crystal structure. A layered rock-salt type crystal structure is preferable for the internal 100xb because lithium easily diffuses two-dimensionally. Furthermore, if the internal 100xb has a layered rock-salt type crystal structure, the added element X, typically magnesium, is likely to segregate to the surface layer 100xa, which is preferable. However, the entire internal 100xb does not necessarily have a layered rock-salt type crystal structure. For example, a portion of the internal 100xb may have crystal defects, may be amorphous, or may have another crystal structure. The internal 100xb may be referred to as the first region.
[0173] <Surface Layer 100xa> The surface layer 100xa contains at least an additional element X. For example, when the surface layer 100xa contains magnesium as the additional element X, it may contain magnesium oxide having a rock-salt crystal structure. Some of the oxygen in the magnesium oxide may be substituted with fluorine. The magnesium oxide contained in the surface layer 100xa is an electrochemically stable material, and therefore is unlikely to deteriorate even with repeated charge and discharge, making it suitable as a coating layer.
[0174] If the surface layer 100xa is too thin, its function as a coating layer will be reduced, but if it is too thick, the capacity will be reduced. Therefore, the thickness of the surface layer 100xa is preferably 0.5 nm to 50 nm, more preferably 0.5 nm to 3 nm. The thickness of the surface layer 100xa can be measured using a cross section of the positive electrode active material.
[0175] The surface layer 100xa preferably has a rock salt crystal structure because the crystal orientation of the surface layer 100xa is more likely to match that of the inner layer 100xb, making it easier to function as a stable coating layer. However, the entire surface layer 100xa does not necessarily have to have a rock salt crystal structure. For example, a portion of the surface layer 100xa may be amorphous or may have another crystal structure.
[0176] The anions of layered rock salt crystals and rock salt crystals have a cubic close-packed structure (face-centered cubic lattice structure). When they contact, there is a crystal plane where the orientation of the cubic close-packed structure formed by the anions is aligned. However, the space group of layered rock salt crystals is R-3m, which is different from the space groups Fm-3m (space group of general rock salt crystals) and Fd-3m (space group of rock salt crystals with the simplest symmetry) of rock salt crystals, so the Miller indices of the crystal planes that satisfy the above conditions are different between layered rock salt crystals and rock salt crystals. In this specification, when the orientation of the cubic close-packed structure formed by the anions is aligned in layered rock salt crystals and rock salt crystals, it may be said that the crystal orientation is approximately the same.
[0177] The fact that the crystal orientations of the two regions roughly match can be determined from TEM (transmission electron microscope) images, STEM (scanning transmission electron microscope) images, HAADF-STEM (high-angle annular dark-field scanning transmission electron microscope) images, ABF-STEM (annular bright-field scanning transmission electron microscope) images, etc. X-ray diffraction (XRD), electron beam diffraction, neutron beam diffraction, etc. can also be used as materials for determination. When the crystal orientations roughly match, it can be observed in TEM images, etc. that the difference in direction between the rows of linearly alternating cations and anions is 5 degrees or less, more preferably 2.5 degrees or less. Note that light elements such as oxygen and fluorine may not be clearly observed in TEM images, etc., but in such cases, the alignment of the orientations can be determined from the arrangement of metal elements.
[0178] However, if the surface layer 100xa is composed only of MgO or a solid solution of MgO and CoO(II), it becomes difficult to insert and extract lithium. Therefore, the surface layer 100xa must contain at least cobalt and, in a discharged state, lithium, providing a path for lithium insertion and extraction. Furthermore, it is preferable that the concentration of cobalt be higher than that of magnesium.
[0179] Generally, as a positive electrode active material undergoes repeated charge and discharge, side reactions such as elution of transition metals such as cobalt and manganese into the electrolyte, elimination of oxygen, elution of the additive element X, and / or instability of the crystal structure occur, leading to deterioration. However, the first positive electrode active material 100x of one embodiment of the present invention has the surface layer portion 100xa, which allows the crystal structure of the composite oxide containing lithium and a transition metal contained in the inner portion 100xb to be more stable.
[0180] The surface layer 100xa of the first positive electrode active material 100x is CoO 2 In particular, when lithium ions are released from the first positive electrode active material 100x by charging, the surface layer 100xa is reinforced by the CoO 2 The surface layer 100xa has a reinforcing function to prevent the layer structure from being broken. The surface layer 100xa is called a barrier film of the first positive electrode active material 100x. The above-mentioned reinforcement includes suppressing oxygen desorption from the first positive electrode active material 100x. The above-mentioned reinforcement also includes suppressing oxygen desorption from the first positive electrode active material 100x. 2 The reinforcement described above includes suppressing the structural shift of the layer. The reinforcement described above also includes suppressing structural changes in the surface layer portion 100xa and the interior portion 100xb. The reinforcement described above also includes suppressing decomposition of the electrolyte on the surface of the first positive electrode active material 100x.
[0181] The surface layer 100xa is one of the regions that easily becomes unstable during charging and discharging, and where deterioration of the crystalline structure is likely to occur. Therefore, it is preferable that the surface layer 100xa have a composition and crystalline structure that are more stable at room temperature than the inner layer 100xb. For example, it is preferable that at least a portion of the surface layer 100xa has a rock salt-type crystalline structure. Alternatively, it is preferable that the surface layer 100xa has both a layered rock salt-type and a rock salt-type crystalline structure. In this way, the surface layer 100xa has a crystalline structure different from that of the inner layer 100xb, thereby significantly enhancing the reinforcing effect described above. Of course, the surface layer 100xa may have the same crystalline structure as the inner layer 100xb, as long as the reinforcing effect described above is achieved.
[0182] The surface layer portion 100xa contains the additive element X, and preferably also contains the same transition metal as the inner portion 100xb. Furthermore, when the surface layer portion 100xa and the inner portion 100xb contain the same transition metal, the valence of the transition metal in these two regions is preferably different. More specifically, the transition metal in the inner portion 100xb preferably contains more trivalent atoms than atoms with other valences, and the transition metal in the surface layer portion 100xa preferably contains more divalent atoms than atoms with other valences.
[0183] When the surface layer 100xa contains a large amount of divalent transition metals, typically divalent cobalt, the surface layer 100xa contains a large amount of metal oxides with a transition metal:oxygen ratio of 1:1 (atomic ratio), such as CoO(II), MnO(II), and Ni(II). These metal oxides tend to form stable solid solutions with magnesium oxide, which is also a divalent metal oxide. This allows the surface layer 100xa to become a more stable and excellent coating layer.
[0184] <Distribution of Added Element X> The added element X in the first positive electrode active material 100x is preferably appropriately distributed. In this specification and the like, the distribution of a certain element refers to the continuous presence of the element when the element is detected in a range that is not noise using any analytical method. Furthermore, the continuous change in the concentration of the element may be referred to as a concentration gradient. The maximum value in the distribution may be referred to as a peak. Note that when identifying a peak, a distribution limited to a certain region may be targeted. The above-mentioned distribution is not limited to a normal distribution. When the distribution corresponds to a normal distribution, the half-width of the distribution may also be determined.
[0185] The surface layer 100xa of the first positive electrode active material 100x preferably has a higher concentration of the additive element X than the internal portion 100xb and a different composition from the internal portion 100xb. Furthermore, it is preferable that the composition have a stable crystal structure at room temperature (25°C). Therefore, the surface layer 100xa may have a different crystal structure from the internal portion 100xb. For example, as described above, at least a portion of the surface layer 100xa of the first positive electrode active material 100x may have a rock salt crystal structure. Furthermore, when the surface layer 100xa and the internal portion 100xb have different crystal structures, it is preferable that the crystal orientations of the surface layer 100xa and the internal portion 100xb are approximately the same.
[0186] However, if the surface layer 100xa consists only of the additive element X and oxygen, for example, only MgO, or only a structure in which MgO and CoO(II) are solid-solved, it becomes difficult to insert and extract lithium. Therefore, the surface layer 100xa must contain at least a transition metal M1, and in the discharged state, it must also contain lithium, providing a path for lithium insertion and extraction. Furthermore, it is preferable that the concentration of the transition metal M1 be higher than that of each additive element X.
[0187] Note that the first positive electrode active material 100x of one embodiment of the present invention is not limited thereto and may include an additional element X that does not have a concentration gradient.
[0188] The distribution of the additive element X as described above can reduce deterioration of the first positive electrode active material 100x even after charge and discharge. That is, deterioration of the secondary battery can be suppressed. Furthermore, a highly safe secondary battery can be obtained.
[0189] [Types of Additional Element X] Magnesium can be used as the additional element X. Magnesium ions are divalent and are more stable at the lithium site than at the transition metal site in the layered rock-salt crystal structure, and therefore more likely to enter the lithium site. The presence of magnesium at an appropriate concentration at the lithium site in the surface layer 100xa makes it easier to maintain the layered rock-salt crystal structure. Furthermore, magnesium has a strong bond with oxygen, so it can suppress the desorption of oxygen around magnesium. Magnesium is preferable because, at an appropriate concentration, it does not adversely affect the intercalation and deintercalation of lithium during charge and discharge. However, excessive magnesium may adversely affect the intercalation and deintercalation of lithium.
[0190] Aluminum can be used as the additive element X. Aluminum ions are trivalent and can exist at transition metal sites in a layered rock salt crystal structure. Aluminum can suppress the elution of surrounding cobalt. Furthermore, aluminum has a strong bond with oxygen, so it can suppress the desorption of oxygen from around the aluminum. Therefore, when aluminum is included as the additive element X, a first positive electrode active material 100x can be obtained whose crystal structure is resistant to collapse even after repeated charge and discharge.
[0191] Fluorine can be used as the additive element X. Fluorine ions are monovalent anions, and when a portion of the oxygen in the surface layer portion 100xa is substituted with fluorine, the lithium desorption energy is reduced. This is because the valence of the cobalt ion changes with lithium desorption, from trivalent to tetravalent in the absence of fluorine, and from divalent to trivalent in the presence of fluorine, resulting in different oxidation-reduction potentials. Therefore, when a portion of the oxygen in the surface layer portion 100xa of the first positive electrode active material 100x is substituted with fluorine, it can be said that desorption and insertion of lithium ions near the fluorine is more likely to occur smoothly. Therefore, when used in a secondary battery, charge / discharge characteristics, rate characteristics, etc. are improved, which is preferable.
[0192] Titanium oxide is known to have superhydrophilic properties. Therefore, by providing a first positive electrode active material 100x having titanium oxide in the surface layer portion 100xa, wettability with highly polar solvents may be improved. In other words, titanium can be used as the additive element X. When a secondary battery is formed, good contact is achieved at the interface between the first positive electrode active material 100x and a highly polar electrolyte, which may suppress an increase in resistance. In this specification and the like, the term "electrolyte" may be used interchangeably with "electrolyte."
[0193] Phosphorus can be used as the additional element X. When phosphorus is used, the phosphorus reacts with hydrogen fluoride generated by decomposition of the electrolyte, which may result in a decrease in the concentration of hydrogen fluoride in the electrolyte.
[0194] The electrolyte is LiPF 6 In the case where the electrolyte contains PVDF, hydrogen fluoride may be generated by hydrolysis. Hydrogen fluoride may also be generated by the reaction of PVDF, which is used as a component of the positive electrode, with an alkali. By reducing the hydrogen fluoride concentration in the electrolyte, corrosion of the current collector and / or peeling of the coating may be suppressed. Furthermore, gelation and / or insolubilization of PVDF may be suppressed, which may result in a decrease in adhesion.
[0195] When first positive electrode active material 100x has cracks, the presence of phosphorus, more specifically, a compound containing phosphorus and oxygen, inside the cracks may inhibit the progression of the cracks.
[0196] As the charging voltage of a secondary battery increases, the voltage of the positive electrode generally increases. The positive electrode active material of one embodiment of the present invention has a stable crystal structure even at high voltages. The stable crystal structure of the positive electrode active material in a charged state can suppress a decrease in capacity due to repeated charge and discharge.
[0197] Furthermore, a short circuit in a secondary battery not only causes problems in the charging and / or discharging operations of the secondary battery, but may also lead to heat generation and fire. To achieve a safe secondary battery, it is preferable that a short circuit current be suppressed even at a high charging voltage. The first positive electrode active material 100x of one embodiment of the present invention suppresses a short circuit current even at a high charging voltage. Therefore, a secondary battery that achieves both high capacity and safety can be obtained.
[0198] A secondary battery using the first positive electrode active material 100x of one embodiment of the present invention preferably simultaneously satisfies high capacity, excellent charge / discharge cycle characteristics, and safety.
[0199] The concentration gradient of the added element X can be evaluated, for example, by using energy dispersive X-ray spectroscopy (EDX). Among EDX measurements, measuring while scanning an area and evaluating the area two-dimensionally is sometimes called EDX area analysis. Extracting data of a linear area from EDX area analysis and evaluating the distribution of atomic concentration within the positive electrode active material particles is sometimes called line analysis.
[0200] The EDX area analysis (e.g., element mapping) can quantitatively analyze the concentration of the additional element X in the surface layer portion 100xa, the interior portion 100xb, and the vicinity of the grain boundaries of the second positive electrode active material 100y. Furthermore, the EDX analysis can analyze the concentration peak of the additional element X.
[0201] When EDX ray analysis is performed on the first positive electrode active material 100x, the peak of the magnesium concentration in the surface layer portion 100xa is preferably present at a depth of up to 3 nm from the surface toward the center of the first positive electrode active material 100x, more preferably at a depth of up to 1 nm, and even more preferably at a depth of up to 0.5 nm.
[0202] The fluorine distribution of the first positive electrode active material 100x preferably overlaps with the magnesium distribution. Furthermore, the fluorine peak is preferably located closer to the surface of the first positive electrode active material 100x than the magnesium peak. When EDX-ray analysis is performed, the fluorine concentration peak of the surface layer 100xa preferably exists within a depth of 3 nm from the surface toward the center of the first positive electrode active material 100x, more preferably within a depth of 1 nm, and even more preferably within a depth of 0.5 nm.
[0203] It should be noted that not all of the additive elements X need have the same concentration distribution. For example, when the first positive electrode active material 100x contains aluminum as the additive element X, it is preferable that the distribution is slightly different from that of magnesium and fluorine. For example, when EDX-ray analysis is performed, it is preferable that the magnesium concentration peak is closer to the surface than the aluminum concentration peak in the surface layer portion 100xa. For example, the aluminum concentration peak is preferably present at a depth of 0.5 nm to 20 nm from the surface toward the center of the first positive electrode active material 100x, and more preferably at a depth of 1 nm to 5 nm.
[0204] Furthermore, when the first positive electrode active material 100x is subjected to linear or area analysis, the ratio (X / M1) of the additional element X to the transition metal M1 near the grain boundaries is preferably 0.020 or more and 0.50 or less. It is even more preferably 0.025 or more and 0.30 or less. It is even more preferably 0.030 or more and 0.20 or less. For example, when the additional element X is magnesium and the transition metal M1 is cobalt, the ratio of the number of magnesium atoms to the number of cobalt atoms (Mg / Co) is preferably 0.020 or more and 0.50 or less. It is even more preferably 0.025 or more and 0.30 or less. It is even more preferably 0.030 or more and 0.20 or less.
[0205] In this specification, the term "distributed unevenly" refers to the concentration of an element in a certain region being different from that in other regions, and being present at a higher concentration than in other regions. This term is synonymous with "bias." Distributed unevenly as a solid solution is called "segregation."
[0206] <Grain Boundaries> The additional element X contained in the first positive electrode active material 100x may be present randomly and dilutely inside the first positive electrode active material 100x, but it is more preferable that a portion of the additional element X segregates at the grain boundaries.
[0207] In other words, the concentration of the additional element X at and near the grain boundaries of the first positive electrode active material 100x is preferably higher than that in other regions inside the first positive electrode active material 100x.
[0208] Like the particle surface, the grain boundary is also a planar defect. Therefore, it is prone to become unstable and changes in the crystal structure are likely to occur. Therefore, if the concentration of the added element X at the grain boundary and its vicinity is high, changes in the crystal structure can be more effectively suppressed.
[0209] Furthermore, when the concentration of the additive element X is high at and near the grain boundaries, even if cracks occur along the grain boundaries of the particles of the first positive electrode active material 100x, the concentration of the additive element X becomes high near the surface where the cracks occur. Therefore, the corrosion resistance to hydrofluoric acid of the positive electrode active material after the cracks occur can be improved.
[0210] In this specification and the like, the vicinity of the grain boundary refers to the region up to about 10 nm from the grain boundary.
[0211] <Crystalline structure of positive electrode active material> Lithium cobalt oxide (LiCoO 2 Materials having a layered rock salt type crystal structure, such as LiCoO, are known to have a high discharge capacity and to be excellent as a positive electrode active material for secondary batteries. The crystal structures of lithium cobalt oxide in the discharged and charged states will be described with reference to FIGS. 10 and 11. FIG. 10 shows a first positive electrode active material 100x according to one embodiment of the present invention, and FIG. 11 shows a conventional positive electrode active material. The conventional positive electrode active material is lithium cobalt oxide (LiCoO) that does not contain any additional elements. 2 10 and 11 show that all the lithium sites are occupied by lithium ions, but in FIG. 10, an additional element X, typically a magnesium ion, may be located at some of the lithium sites.
[0212] <Li x CoO 2 When x is 1, the horizontal axis of Fig. 10 and Fig. 11 is Li x CoO 2Indicate x in (X in Li x CoO 2 ), and the discharge state is Li x CoO 2 When x is 1, lithium cobalt oxide has a layered rock-salt crystal structure belonging to the space group R-3m. In the layered rock-salt crystal structure, lithium ions occupy octahedral sites, and CoO is present in the unit cell. 2 There are three layers. For this reason, the layered rock salt type crystal structure belonging to the space group R-3m is sometimes called an O3 type crystal structure. 2 The layer refers to a structure in which octahedral structures in which cobalt is coordinated with six oxygen atoms are connected in a plane with edge sharing.
[0213] 10 and 11 show Li in a discharged state. x CoO 2 The crystal structure when x = 1 is shown in the figure, and is labeled R-3m(O3). The crystal structure represented by R-3m(O3) has a unit cell lattice constant of a = 2.81610 × 10 −10 (m), b=2.81610×10 −10 (m), c=14.05360×10 −10 (m), α = 90.0000, β = 90.0000, γ = 120.0000. The coordinates of lithium, cobalt, and oxygen in the unit cell are Li(0,0,0), Co(0,0,0.5), and O(0,0,0.23951). In other words, in the discharged state, the crystal structure of lithium cobalt oxide is the same regardless of the presence or absence of the added element X.
[0214] <Li x MO 2 Next, we will explain the crystal structure in the charged state. The state when charged at a high voltage is Li x CoO 2 The term "high voltage" means a voltage of 4.6 V or more, preferably 4.8 V or more, based on the lithium metal counter electrode.
[0215] First, the change in the crystal structure of a conventional positive electrode active material in a discharged state and in a charged state at a high voltage is shown in FIG. 11. Conventional lithium cobalt oxide has a structure similar to that of Lix CoO 2 It is known that when x = 0.5, the symmetry of lithium increases and the crystal structure belongs to the monoclinic space group P2 / m. This structure has CoO 2 There is one layer, so it is sometimes called O1 type or monoclinic O1 type.
[0216] In addition, conventional lithium cobalt oxide is Li x CoO 2 It is known that when x = 0, it has a crystal structure of the trigonal space group P-3m1. This structure also contains CoO in the unit cell. 2 There is one layer. Therefore, this crystal structure is sometimes called O1 type or trigonal O1 type. In addition, when the trigonal crystal is converted into a composite hexagonal lattice, it is sometimes called hexagonal O1 type.
[0217] In addition, conventional lithium cobalt oxide is Li x CoO 2 When x is about 0.12, the crystal structure has the space group R-3m. This structure is similar to CoO, such as trigonal O1 type. 2 and LiCoO such as R-3m(O3). 2 It can also be said that the structure of and the structure are stacked alternately. Therefore, this crystal structure is sometimes called an H1-3 type crystal structure. In fact, the number of cobalt atoms per unit cell in the H1-3 type crystal structure is twice that of other structures. In addition, the actual insertion and desorption of lithium ions does not necessarily occur uniformly in the positive electrode active material, and the lithium ions are unevenly distributed, that is, the lithium concentration becomes uneven. Therefore, in experiments, Li x CoO 2 In this case, an H1-3 type crystal structure is observed from about x=0.25.
[0218] As an example of the H1-3 type crystal structure, the coordinates of cobalt and oxygen in the unit cell can be expressed as Co (0,0,0.42150±0.00016), O1 (0,0,0.27671±0.00045), and O2 (0,0,0.11535±0.00045).
[0219] Which unit cell should be used to represent the crystal structure of the positive electrode active material can be determined, for example, by Rietveld analysis of the XRD diffraction pattern. For example, it is preferable to adopt a unit cell with a goodness of fit (GOF) value close to 1.
[0220] Li x CoO 2 When charging and discharging are repeated so that x is 0.24 or less (typically, charging at about x = 0.12), conventional lithium cobalt oxide alternates between an H1-3 type crystal structure and an R-3m(O3) crystal structure, and the crystal structure changes between these, i.e., non-equilibrium phase changes occur repeatedly. 2 The layer displacement increases. Such dynamic structural changes can adversely affect the stability of the crystal structure.
[0221] Furthermore, the difference in volume between these two crystal structures is large: when compared per equal number of cobalt atoms, the difference in volume between the H1-3 crystal structure and the R-3m(O3) crystal structure is greater than 3.5%, typically 3.9% or more.
[0222] In addition, the H1-3 type crystal structure has CoO, such as trigonal O1 type. 2 A structure with continuous layers is likely to be unstable.
[0223] For these reasons, the crystal structure of conventional lithium cobalt oxide breaks down when it is repeatedly charged and discharged so that x becomes 0.24 or less. When the crystal structure breaks down, the number of sites where lithium ions can exist stably decreases, and it becomes difficult to insert and extract lithium, causing a deterioration in cycle characteristics.
[0224] On the other hand, in the first positive electrode active material 100x shown in FIG. x CoO 2 The change in the crystal structure between the discharge state where x = 1 and the state where x is 0.24 or less is smaller than that of conventional lithium cobalt oxide. 2The layer misalignment is small. Furthermore, when compared per the same number of cobalt atoms, the difference in volume between the H1-3 type crystal structure and the R-3m(O3) type crystal structure can be reduced. Specifically, when the first cathode active material 100x having the same number of transition metal M1 atoms is compared with a conventional cathode active material, the volume change of the first cathode active material 100x is smaller than the volume change of the conventional cathode active material. Therefore, the crystal structure of the first cathode active material 100x is less likely to collapse even when repeatedly charged and discharged so that x is 0.24 or less, and sites where lithium ions can stably exist are maintained, thereby achieving excellent cycle characteristics.
[0225] Li x CoO 2 The crystal structure of the first positive electrode active material 100x when x = about 0.2 and x = about 0.15 is shown in Figure 10. Since the inner portion 100xb occupies most of the volume of the first positive electrode active material 100x, the crystal structure shown in Figure 10 can be said to be the crystal structure of the inner portion 100xb of the first positive electrode active material 100x. Since the inner portion 100xb is a portion that contributes greatly to charge and discharge, CoO 2 It is preferable that the layer displacement is small and the volume change of the inner 100xb is small.
[0226] As shown in FIG. 10 , the first positive electrode active material 100x has a crystal structure different from that of conventional lithium cobalt oxide when x is 0.24 or less, for example, when x is approximately 0.2 or 0.15, in which case the lithium cobalt oxide has an H1-3 type crystal structure.
[0227] <When x = Approximately 0.2> When x = approximately 0.2, the first positive electrode active material 100x has a crystal structure belonging to the trigonal space group R-3m. 2 The layer symmetry is the same as that of O3. Therefore, this crystal structure is called an O3'-type crystal structure. Although this crystal structure is not a spinel structure, it is sometimes called a pseudo-spinel structure because a pattern similar to a spinel structure may appear in the XRD pattern. This crystal structure is shown in Figure 10 with the notation R-3m(O3').
[0228] In the O3' type crystal structure, when M is cobalt, the coordinates of cobalt and oxygen in the unit cell can be expressed in the range of Co(0,0,0.5), O(0,0,x), 0.20≦x≦0.25. The lattice constant of the unit cell is 2.797×10 for the a-axis. −10 ≦a≦2.837×10 −10 (m) is preferred, and 2.807 × 10 −10 ≦a≦2.827×10 −10 (m) is more preferable, and typically a=2.817×10 −10 (m). The c-axis is 13.681 × 10 −10 ≦c≦13.881×10 −10 (m) is preferred, and 13.751 × 10 −10 ≦c≦13.811×10 −10 (m) is more preferable, and typically c=13.781×10 −10 (m).
[0229] <When x = Approximately 0.15> When x = approximately 0.15, the first positive electrode active material 100x has a crystal structure belonging to the monoclinic space group P2 / m. This is because CoO 2 There is one layer. Furthermore, when x = approximately 0.15, the lithium present in the first positive electrode active material 100x can be considered to be approximately 15 atomic % in the discharged state. Therefore, this crystal structure is referred to as a monoclinic O1(15) type crystal structure. This crystal structure is shown in Figure 10 with the P2 / m monoclinic O1(15) designation.
[0230] In the monoclinic O1(15) crystal structure, when M is cobalt, the coordinates of cobalt and oxygen in the unit cell are Co1(0.5,0,0.5), Co2(0,0.5,0.5), O1(X O1 , 0, Z O1 ), 0.23≦X O1 ≦0.24, 0.61≦Z O1 ≦0.65, O2(X O2 , 0.5, Z O2 ), 0.75≦X O2 ≦0.78, 0.68≦Z O2The lattice constants of the unit cell are a = 0.4880 ± 0.005 nm, b = 0.2817 ± 0.005 nm, c = 0.4839 ± 0.005 nm, α = 90°, β = 109.6 ± 0.1°, and γ = 90°.
[0231] In addition, this crystal structure can show the lattice constant even in the space group R-3m if a certain degree of error is allowed in the Rietveld analysis etc. In this case, the coordinates of cobalt and oxygen in the unit cell are Co(0,0,0.5), O(0,0,Z O ), 0.21≦Z O The lattice constants of the unit cell are a = 0.2817 ± 0.002 nm and c = 1.368 ± 0.01 nm.
[0232] In both the O3' and monoclinic O1(15) crystal structures, ions of cobalt, nickel, magnesium, etc. occupy hexacoordinated oxygen sites, although lighter elements such as lithium and magnesium may occupy tetracoordinated oxygen sites.
[0233] As shown in FIG. 10, the difference between R-3m(O3) in the discharged state and the O3′-type crystal structure is 2 There is almost no layer misalignment. In addition, the R-3m(O3) in the discharge state and the monoclinic O1(15) type crystal structure have a CoO 2 There is almost no layer misalignment.
[0234] The difference in volume per the same number of cobalt atoms between R-3m(O3) in a discharged state and the O3' type crystal structure is 2.5% or less, more specifically 2.2% or less, typically 1.8%.
[0235] The difference in volume per the same number of cobalt atoms between R-3m(O3) in a discharged state and the monoclinic O1(15) type crystal structure is 3.3% or less, more specifically 3.0% or less, typically 2.5%.
[0236] As described above, in the first positive electrode active material 100x of one embodiment of the present invention, Li x CoO 2When x is small, that is, when a large amount of lithium is released, the change in crystal structure is suppressed compared to conventional positive electrode active materials. Furthermore, the change in volume is also suppressed when compared per the same number of cobalt atoms. Therefore, the first positive electrode active material 100x is less likely to collapse in crystal structure even when repeatedly charged and discharged so that x is 0.24 or less, and the decrease in discharge capacity in charge-discharge cycle tests is suppressed. Furthermore, since more lithium ions can be stably utilized than in conventional positive electrode active materials, the first positive electrode active material 100x has a large discharge capacity per weight and per volume. Therefore, by using the first positive electrode active material 100x, a secondary battery with a high discharge capacity per weight and per volume can be fabricated.
[0237] It is not necessary for all particles in the interior 100xb of the first positive electrode active material 100x to have the O3′-type and / or monoclinic O1(15)-type crystal structure, but rather they may contain other crystal structures, or some of them may be amorphous.
[0238] Also Li x CoO 2 To make the value of x small, it is generally necessary to charge at a high charging voltage. x CoO 2 The state where x is small can be rephrased as a state where the battery is charged at a high charging voltage. For example, when CC / CV charging is performed at a voltage of 4.6 V or higher relative to the potential of lithium metal in an environment of 25°C, a H1-3 type crystal structure appears in conventional positive electrode active materials. Therefore, a charging voltage of 4.6 V or higher relative to the potential of lithium metal can be considered a high charging voltage.
[0239] Therefore, in other words, the first positive electrode active material 100x of one embodiment of the present invention is preferable because it can maintain the R-3m(O3) type crystal structure even when charged at a high charging voltage, for example, a voltage of 4.6 V or more at 25° C. In other words, it is preferable because it can adopt a monoclinic O1(15) type crystal structure when charged at an even higher charging voltage, for example, a voltage of 4.7 V or more and 4.8 V or less at 25° C.
[0240] Even in the first positive electrode active material 100x according to one embodiment of the present invention, when the charge voltage is further increased, the H1-3 type crystal structure may be finally observed. That is, depending on the charge / discharge conditions, the first positive electrode active material 100x may undergo the O3' type crystal structure to attain the H1-3 type crystal structure. However, even if the first positive electrode active material 100x undergoes the O3' type crystal structure to attain the H1-3 type crystal structure, it is estimated that the effect of suppressing oxygen release is still achieved.
[0241] Furthermore, as described above, since the crystal structure is affected by the number of charge / discharge cycles, charge / discharge current, temperature, electrolyte, and the like, the first positive electrode active material 100x may have an O3′-type crystal structure when the charge voltage is lower, for example, even when the charge voltage is 4.5 V or higher and lower than 4.6 V at 25° C. Similarly, when charged at a voltage of 4.65 V or higher and 4.7 V or lower at 25° C., the first positive electrode active material 100x may have a monoclinic O1(15)-type crystal structure.
[0242] In a secondary battery, for example, when graphite is used as the negative electrode active material, the voltage of the secondary battery is lower than the above by the potential of the graphite. The potential of graphite is about 0.05 V to 0.2 V with respect to the potential of lithium metal. Therefore, in the case of a secondary battery using graphite as the negative electrode active material, the battery has a similar crystal structure at a voltage obtained by subtracting the potential of graphite from the above voltage.
[0243] CoO 2 The additive element X, for example, magnesium, which is present randomly and dilutely between the layers, i.e., at the lithium site, is 2 This has the effect of suppressing layer misalignment. 2 When magnesium is present between layers, the O3'-type crystal structure is easily formed. Therefore, magnesium is preferably distributed throughout the particles of the first positive electrode active material 100x of one embodiment of the present invention. In order to distribute magnesium throughout the particles, heat treatment is preferably performed in the manufacturing process of the first positive electrode active material 100x of one embodiment of the present invention.
[0244] However, if the heat treatment temperature is too high, cation mixing occurs, increasing the possibility that the additive element X, such as magnesium, will enter the cobalt site. Magnesium present at the cobalt site is ineffective in maintaining the R-3m structure during high-voltage charging. Furthermore, if the heat treatment temperature is too high, there are concerns about adverse effects such as cobalt being reduced to divalent and lithium evaporating.
[0245] Therefore, it is preferable to add a halogen compound such as a fluorine compound to the lithium cobalt oxide before the heat treatment to distribute magnesium throughout the particles. The addition of the halogen compound lowers the melting point of the lithium cobalt oxide. Lowering the melting point makes it easier to distribute magnesium throughout the particles at a temperature where cation mixing is unlikely to occur. Furthermore, the presence of a fluorine compound is expected to improve corrosion resistance to hydrofluoric acid produced by decomposition of the electrolyte.
[0246] Note that if the magnesium concentration is increased above a desired value, the effect on stabilizing the crystal structure may be reduced. This is thought to be because magnesium enters the cobalt site in addition to the lithium site. The number of magnesium atoms in the positive electrode active material of one embodiment of the present invention is preferably 0.001 to 0.1 times the number of cobalt atoms, more preferably more than 0.01 to less than 0.04, and even more preferably about 0.02. The magnesium concentration shown here may be, for example, a value obtained by performing elemental analysis of the entire particles of the positive electrode active material using ICP-MS or the like, or may be based on the value of the raw material composition in the process of producing the positive electrode active material.
[0247] In addition to cobalt, lithium cobalt oxide may contain one or more additive elements X selected from nickel, aluminum, manganese, titanium, vanadium, and chromium, with nickel and aluminum being particularly preferred. Manganese, titanium, vanadium, and chromium may be stable and easily tetravalent, which may contribute significantly to structural stability. Adding metal Z to the positive electrode active material of one embodiment of the present invention may result in a more stable crystal structure, for example, in a charged state at a high voltage. In the positive electrode active material of one embodiment of the present invention, metal Z is preferably added at a concentration that does not significantly change the crystallinity of lithium cobalt oxide. For example, the amount is preferably such that the aforementioned Jahn-Teller effect or the like is not exhibited.
[0248] The transition metals, such as nickel and manganese, and aluminum are preferably present at the cobalt site, but may be partially present at the lithium site. Magnesium is preferably present at the lithium site. Oxygen may be partially substituted with fluorine.
[0249] As the magnesium concentration increases, the capacity of the positive electrode active material may decrease. For example, one possible cause of this is the incorporation of magnesium into lithium sites, which may reduce the amount of lithium contributing to charge and discharge. Excessive magnesium may also produce magnesium compounds that do not contribute to charge and discharge. When the positive electrode active material of one embodiment of the present invention contains nickel as the additive element X in addition to magnesium, the capacity per weight and per volume may be increased. When the positive electrode active material of one embodiment of the present invention contains aluminum as the additive element X in addition to magnesium, the capacity per weight and per volume may be increased. When the positive electrode active material of one embodiment of the present invention contains nickel and aluminum in addition to magnesium, the capacity per weight and per volume may be increased.
[0250] Hereinafter, the concentration of an additional element X or the like contained in a positive electrode active material of one embodiment of the present invention will be expressed in terms of the number of atoms.
[0251] The number of nickel atoms in the positive electrode active material of one embodiment of the present invention is preferably 10% or less of the number of cobalt atoms, more preferably 7.5% or less, even more preferably 0.05% or more and 4% or less, and particularly preferably 0.1% or more and 2% or less. The nickel concentration shown here may be a value obtained by performing elemental analysis of the entire particles of the positive electrode active material using, for example, ICP-MS or the like, or may be based on a value obtained by mixing raw materials in the process of producing the positive electrode active material.
[0252] If the positive electrode active material 100x is charged at a high voltage for a long period of time, transition metals may leach out of the positive electrode active material into the electrolyte, causing the crystal structure to collapse. However, by including nickel in the above proportion, it may be possible to suppress the leach-out of transition metals from the first positive electrode active material 100x.
[0253] The number of aluminum atoms in the positive electrode active material of one embodiment of the present invention is preferably 0.05% to 4%, and more preferably 0.1% to 2%, of the number of cobalt atoms. The aluminum concentration shown here may be a value obtained by performing elemental analysis of the entire particles of the positive electrode active material using, for example, ICP-MS or the like, or may be based on a value obtained by mixing raw materials in the process of producing the positive electrode active material.
[0254] <Analysis Method> Whether a certain positive electrode active material is the first positive electrode active material 100x that exhibits an O3′-type crystal structure when charged at a high voltage can be determined by analyzing the positive electrode charged at a high voltage using XRD, electron diffraction, neutron diffraction, electron spin resonance (ESR), nuclear magnetic resonance (NMR), etc. XRD is particularly preferred in that it can analyze the symmetry of transition metals such as cobalt contained in the positive electrode active material with high resolution, it can compare the level of crystallinity and the orientation of the crystals, it can analyze the periodic distortion of the lattice and the crystallite size, and it can obtain sufficient accuracy even when measuring a positive electrode obtained by disassembling a secondary battery as is.
[0255] As described above, the first positive electrode active material 100x is characterized by minimal change in crystal structure between the high-voltage charged state and the discharged state. Materials in which a crystal structure that exhibits a large change between the high-voltage charged state and the discharged state accounts for 50 wt % or more are undesirable because they cannot withstand high-voltage charging and discharging. It should be noted that the desired crystal structure may not be achieved simply by adding an additive element X. For example, even if both materials share the common feature of being lithium cobalt oxide containing magnesium and fluorine, there are cases in which the O3'-type crystal structure accounts for 60 wt % or more when charged at a high voltage, and cases in which the H1-3-type crystal structure accounts for 50 wt % or more when charged at a high voltage. Furthermore, at a certain voltage, the O3'-type crystal structure may be nearly 100 wt %, and further increasing the certain voltage may result in the H1-3-type crystal structure. Therefore, to determine whether a material is the first positive electrode active material 100x, analysis of the crystal structure, including XRD, is required.
[0256] However, when a positive electrode active material is charged or discharged at a high voltage, its crystal structure may change when exposed to air. For example, it may change from an O3'-type crystal structure to an H1-3-type crystal structure. Therefore, it is preferable to handle all samples in an inert atmosphere such as an argon atmosphere.
[0257] <Charging Method> High-voltage charging for determining whether a certain composite oxide is the first positive electrode active material 100x can be performed by preparing a coin cell (CR2032 type, diameter 20 mm, height 3.2 mm) using a lithium counter electrode, for example.
[0258] More specifically, the positive electrode may be prepared by coating a positive electrode current collector made of aluminum foil with a slurry containing a positive electrode active material, a conductive additive, and a binder.
[0259] Lithium metal can be used for the counter electrode. When a material other than lithium metal is used for the counter electrode, the potential of the secondary battery differs from the potential of the positive electrode. Unless otherwise specified, voltages and potentials in this specification refer to the potential of the positive electrode.
[0260] The electrolyte contained in the electrolytic solution was 1 mol / L lithium hexafluorophosphate (LiPF 6) is used, and the electrolyte may be a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of EC:DEC=3:7 with 2 wt % vinylene carbonate (VC).
[0261] The separator can be made of polypropylene having a thickness of 25 μm.
[0262] The positive electrode can and the negative electrode can may be made of stainless steel (SUS).
[0263] The coin cell fabricated under the above conditions was charged at a constant current of 4.6 V and 0.5 C, followed by constant voltage charging until the current reached 0.01 C (CCCV charging). Here, 1 C corresponds to 200 mA / g of positive electrode active material weight. The temperature was 25°C. After charging in this manner, the coin cell was disassembled in an argon-atmosphere glove box and the positive electrode was removed, yielding a positive electrode active material charged at high voltage. When various analyses were subsequently performed, it was preferable to seal the cell in an argon atmosphere to prevent reactions with external components. For example, XRD could be performed by sealing the cell in an airtight container in an argon atmosphere.
[0264] <XRD> CuKα calculated from the O3' type crystal structure and H1-3 type crystal structure model 1 12 to 14 show ideal powder XRD patterns based on the line. For comparison, LiCoO 2 (O3) and CoO at charge depth 1 2 The ideal XRD pattern calculated from the crystal structure of LiCoO (O1) is also shown. 2 (O3) and CoO 2 The pattern of (O1) was created using Reflex Powder Diffraction, one of the modules of Materials Studio (BIOVIA), from crystal structure information obtained from the Inorganic Crystal Structure Database (ICSD) (see Non-Patent Document 5). The 2θ range was set to 15° to 75°, with a step size of 0.01 and a wavelength of λ1 of 1.540562 × 10. −10m and λ2 were not set, and the monochromator was single. The pattern of the H1-3 type crystal structure was similarly created from the crystal structure information described in Non-Patent Document 3. The crystal structure pattern of the O3' type crystal structure was estimated from the XRD pattern of the positive electrode active material of one embodiment of the present invention, and fitting was performed using TOPAS ver. 3 (crystal structure analysis software manufactured by Bruker), and an XRD pattern was created in the same manner as the others.
[0265] As shown in Figure 12, in the O3' type crystal structure, diffraction peaks appear at 2θ = 19.30 ± 0.20° (19.10° to 19.50°) and 2θ = 45.55 ± 0.10° (45.45° to 45.65°). More specifically, sharp diffraction peaks appear at 2θ = 19.30 ± 0.10° (19.20° to 19.40°) and 2θ = 45.55 ± 0.05° (45.50° to 45.60°). However, as shown in Figure 13, in the H1-3 type crystal structure and CoO 2 In the case of (P-3m1, O1), no peaks appear at these positions. Therefore, the appearance of peaks at 2θ = 19.30 ± 0.20° and 2θ = 45.55 ± 0.10° in a state charged at a high voltage can be said to be a characteristic of the first positive electrode active material 100x.
[0266] This can also be said to mean that the positions at which XRD diffraction peaks appear are close between the crystal structure at a charge depth of 0 and the crystal structure upon high-voltage charging. More specifically, the difference in the positions at which two or more, preferably three or more, of the main diffraction peaks of both structures appear is 2θ = 0.7 or less, more preferably 2θ = 0.5 or less.
[0267] Although the first positive electrode active material 100x has an O3'-type crystal structure when charged at a high voltage, not all of the particles need to have an O3'-type crystal structure. Other crystal structures may be included, or some may be amorphous. However, when Rietveld analysis is performed on the XRD pattern, the O3'-type crystal structure is preferably 50 wt% or more, more preferably 60 wt% or more, and even more preferably 66 wt% or more. If the O3'-type crystal structure is 50 wt% or more, more preferably 60 wt% or more, and even more preferably 66 wt% or more, a positive electrode active material with sufficiently excellent cycle characteristics can be obtained.
[0268] Furthermore, even after 100 or more charge / discharge cycles from the start of measurement, when Rietveld analysis is performed, the O3' type crystal structure is preferably 35 wt% or more, more preferably 40 wt% or more, and even more preferably 43 wt% or more.
[0269] The crystallite size of the O3'-type crystal structure of the positive electrode active material particles is 2 Therefore, even under the same XRD measurement conditions as the positive electrode before charging and discharging, a clear peak of the O3' type crystal structure can be confirmed after high voltage charging. On the other hand, 2 In this case, even if a part of the crystal structure resembles the O3'-type crystal structure, the crystallite size will be small and the peak will be broad and small. The crystallite size can be determined from the half-width of the XRD peak.
[0270] <EDX> Preferably, one or more selected from the additive elements X contained in the first positive electrode active material 100x have a concentration gradient. Furthermore, it is more preferable that the depth of the concentration peak from the surface of the first positive electrode active material 100x differs depending on the additive element X. The concentration gradient of the additive element X can be evaluated, for example, by analysis using energy dispersive X-ray spectroscopy (EDX). Among EDX measurements, EDX area analysis is performed by scanning an area and evaluating the area two-dimensionally. Linear analysis is performed by linear scanning and evaluating the distribution of atomic concentration within the positive electrode active material. Furthermore, linear analysis may be used to extract data from a linear area of EDX area analysis. Measurement of a certain area without scanning is called point analysis. More preferably, the concentration gradient of the added element is measured by exposing a cross section of the first positive electrode active material 100x using a focused ion beam (FIB) or the like and performing linear analysis on the cross section. The cross section of the first positive electrode active material 100x is preferably observed using a STEM, and this, together with EDX measurement, is called STEM-EDX line analysis.
[0271] The surface of the first positive electrode active material 100x in a cross-sectional STEM image or the like is the boundary between an area where an image derived from the crystalline structure of the positive electrode active material is observed and an area where it is not observed, and is the outermost area where atomic columns derived from the atomic nuclei of metal elements having atomic numbers larger than that of lithium among the metal elements constituting the positive electrode active material are observed. Alternatively, it is the intersection of a tangent drawn to the brightness profile from the surface to the bulk of the STEM image and the depth axis. The surface in a STEM image or the like may be determined in conjunction with an analysis with higher spatial resolution.
[0272] The reference point of the first positive electrode active material 100x in the STEM-EDX analysis or the like is the average value M of the detected amount of characteristic X-rays of the transition metal M1 inside the positive electrode active material. AVEWhen the left side of the reference point is described as the outside of the positive electrode active material and the right side of the reference point is described as the inside of the positive electrode active material, the reference point may be referred to as the position of the surface of the positive electrode active material. In addition, in STEM-EDX-ray analysis, if the amount of detected characteristic X-rays of the transition metal M1 does not decrease sufficiently to the left of the reference point, the amount of detected characteristic X-rays of the transition metal M1 to the left of the reference point is called background, and the average value M of the amount of detected characteristic X-rays of the transition metal M1 in the background is used. BG and the average detected amount of transition metal M1 inside AVE The reference point may be the point where the average value M of the detected amount of characteristic X-rays of oxygen inside the positive electrode active material is 50% of the sum of the transition metal M1 and the transition metal M1. However, since oxygen is an element that is easily affected by the outside of the positive electrode active material, the reference point is the average value M of the detected amount of characteristic X-rays of the transition metal M1. AVE It is preferable to calculate it from 50% of the average value M of the detected amount of characteristic X-rays of the transition metal M1 inside. AVE 50% of the average value of the detected amount of characteristic X-rays of oxygen inside M AVE If the difference is not 50% of the average value M of the detected amount of characteristic X-rays of the transition metal M1, it is considered to be due to the influence of metal oxides, carbonates, etc. containing oxygen attached to the surface. AVE In the case of a positive electrode active material having a plurality of transition metals M1, it is preferable to adopt the point where the amount of characteristic X-rays detected inside the element M1 is 50% of the amount of characteristic X-rays detected inside the element. AVE , or M AVE and M BG The reference point can be found using
[0273] The average value M of the detected amount of characteristic X-rays of the internal transition metal M1 AVE can be determined by averaging a range of 2 nm or more, preferably 3 nm or more, at a depth of 30 nm or more, preferably 50 nm or more, from a region where the detected amount of characteristic X-rays of the transition metal M1 saturates and stabilizes, for example, a region where the detected amount of characteristic X-rays of the transition metal M1 starts to increase. BGcan be obtained by averaging the amount of detected characteristic X-rays of the transition metal M1 over a range of 2 nm or more, preferably 3 nm or more, outside the area where the amount of detected characteristic X-rays of the transition metal M1 starts to increase. BG and the average value of the detected amount of characteristic X-rays of oxygen in the background O AVE can also be found in the same way.
[0274] The minimum spatial resolution of STEM-EDX is about 1 nm. Therefore, the maximum value of the additive element X profile may deviate by about 1 nm. For example, even if the maximum value of the additive element X profile of magnesium or the like is outside the surface obtained above, the difference between the maximum value and the surface can be considered an error if it is less than 1 nm.
[0275] The peak in STEM-EDX-ray analysis refers to the detected intensity in each element profile or the maximum value of the characteristic X-ray for each element. Note that noise in STEM-EDX-ray analysis may be a measured value with a half-width less than the spatial resolution (R), for example, R / 2 or less.
[0276] STEM-EDX analysis can be performed, for example, as follows: First, a protective film is vapor-deposited on the surface of the positive electrode active material. For example, carbon can be vapor-deposited using a carbon coating unit of an ion sputtering device (MC1000 manufactured by Hitachi High-Technologies).
[0277] Next, the positive electrode active material is sliced to prepare a STEM cross-section sample. For example, the slice processing can be performed using an FIB-SEM device (Hitachi High-Tech XVision 200TBS). Pickup is performed using an MPS (microprobing system), and the finishing conditions can be, for example, an acceleration voltage of 10 kV.
[0278] The STEM-EDX analysis can be performed using, for example, a STEM device (NEOARM manufactured by JEOL), and the EDX detector can be a Dual SDD detector manufactured by JEOL.
[0279] 15A and 15B show an example of STEM-EDX-ray analysis. This is an EDX-ray analysis of a cross-sectional STEM image of a surface layer portion having a plane other than the (001) plane. This is a case where magnesium, fluorine, and aluminum were detected as the added element X. As shown in FIGS. 15A and 15B, the magnesium concentration is preferably higher in the surface layer portion 100xa than in the interior portion 100xb. As shown in FIGS. 15A and 15B, the fluorine concentration is preferably higher in the surface layer portion 100xa than in the interior portion 100xb. Furthermore, when STEM-EDX-ray analysis is performed, the magnesium concentration peak in the surface layer portion 100xa preferably exists within a depth of 3 nm from the surface toward the center of the first positive electrode active material 100x0, more preferably within a depth of 1 nm, and even more preferably within a depth of 0.5 nm. Note that the concentration peak here refers to the maximum concentration value.
[0280] 15A and 15B, the fluorine distribution preferably overlaps with the magnesium distribution. For example, the difference in depth between the peak of the fluorine concentration and the peak of the magnesium concentration is preferably within 10 nm, more preferably within 3 nm, and even more preferably within 1 nm.
[0281] Furthermore, when STEM-EDX-ray analysis was performed, the fluorine concentration peak of the surface layer 100xa preferably exists at a depth of 3 nm from the surface toward the center of the first positive electrode active material 100x, more preferably at a depth of 1 nm, and even more preferably at a depth of 0.5 nm. As shown in FIGS. 15A and 15B, it is preferable that the fluorine concentration peak exists slightly closer to the surface than the magnesium concentration peak, as this increases resistance to hydrofluoric acid. For example, it is more preferable that the fluorine concentration peak be 0.5 nm or more closer to the surface than the magnesium concentration peak, and even more preferable that it be 1.5 nm or more closer to the surface. The maximum fluorine concentration shown in FIGS. 15A and 15B can be increased by undergoing the above-mentioned fluorination treatment.
[0282] Furthermore, when the first positive electrode active material 100x contains aluminum as the additive element X, as shown in FIGS. 15A and 15B , when STEM-EDX analysis is performed, the magnesium concentration peak and the fluorine concentration peak are preferably closer to the surface than the aluminum concentration peak in the surface layer portion 100xa. FIG. 15B is an example of STEM-EDX analysis in which the aluminum concentration peak is located deeper in the first positive electrode active material 100x than in FIG. 15A . As shown in FIGS. 15A and 15B , the aluminum distribution may not be a normal distribution. The aluminum concentration peak is preferably present at a depth of 0.5 nm to 50 nm, more preferably 5 nm to 50 nm, from the surface to the center of the first positive electrode active material 100x.
[0283] Although not shown, in the first positive electrode active material 100x having nickel as the additive element X, the nickel concentration peak in the surface layer 100xa is preferably present at a depth of 3 nm from the surface of the first positive electrode active material 100x toward the center, more preferably at a depth of 1 nm, and even more preferably at a depth of 0.5 nm. Furthermore, in the first positive electrode active material 100x containing magnesium and nickel, the nickel distribution preferably overlaps with the magnesium distribution. For example, the difference in depth between the nickel concentration peak and the magnesium concentration peak is preferably within 10 nm, more preferably within 3 nm, and even more preferably within 1 nm.
[0284] X-ray photoelectron spectroscopy (XPS) can analyze a region from the surface to a depth of about 2 to 8 nm (usually about 5 nm), so the concentration of each element can be quantitatively analyzed for about half of the surface layer 100xa. Furthermore, narrow scan analysis can be used to analyze the bonding state of elements. The quantitative accuracy of XPS is often about ±1 atomic %.
[0285] When XPS analysis was performed on the first positive electrode active material 100x, the number of atoms of the additive element X was preferably 0.3 to 1.6 times, more preferably 0.4 to less than 1.2 times, the number of atoms of the transition metal. When the additive element X is magnesium and the transition metal is cobalt, the number of atoms of magnesium is preferably 0.4 to 1.2 times, more preferably 0.4 to less than 1.0 times, the number of atoms of cobalt. Furthermore, the number of atoms of halogen such as fluorine is preferably 0.2 to 1.5 times, more preferably 0.4 to less than 1.0 times, the number of atoms of the transition metal.
[0286] When XPS analysis is performed, for example, a monochromated aluminum source can be used as the X-ray source, and the take-off angle is preferably set to, for example, 45°.
[0287] Furthermore, when the first positive electrode active material 100x is analyzed by XPS, the peak representing the bond energy between fluorine and other elements is preferably equal to or greater than 682 eV and less than 685 eV, and more preferably about 684.3 eV, which is different from both the bond energy of lithium fluoride (685 eV) and the bond energy of magnesium fluoride (686 eV).
[0288] Furthermore, when the first positive electrode active material 100x is analyzed by XPS, the peak indicating the bond energy between magnesium and other elements is preferably equal to or greater than 1302 eV and less than 1304 eV, and more preferably about 1303 eV, which is a different value from the bond energy of magnesium fluoride, 1305 eV, and is close to the bond energy of magnesium oxide.
[0289] The concentration of the additive element X, such as magnesium and aluminum, which is preferably present in large amounts in the surface layer portion 100xa, measured by XPS or the like is preferably higher than the concentration measured by ICP-MS (inductively coupled plasma mass spectrometry) or GD-MS (glow discharge mass spectrometry).
[0290] When a cross section of magnesium and aluminum is exposed by processing and analyzed using TEM-EDX, the concentration of the surface layer 100xa is preferably higher than the concentration of the inner layer 100xb. The processing can be performed using, for example, FIB.
[0291] In an XPS (X-ray photoelectron spectroscopy) analysis, the number of magnesium atoms is preferably 0.4 to 1.5 times the number of cobalt atoms, while in an ICP-MS analysis, the ratio of the number of magnesium atoms, Mg / Co, is preferably 0.001 to 0.06.
[0292] On the other hand, it is preferable that nickel contained in the transition metal is not unevenly distributed in the surface layer portion 100xa but is distributed throughout the first positive electrode active material 100x, unless there is a region where the excess additive element X is unevenly distributed as described above.
[0293] This embodiment can be used in combination with other embodiments.
[0294] 16A to 16C, a method 1 for manufacturing a first positive electrode active material 100x will be described. A smooth first positive electrode active material 100x can be provided by undergoing initial heating.
[0295] <Step S11> In step S11 shown in FIG. 16A, a lithium source (Li source) and a cobalt source (Co source) are prepared as starting materials for lithium and transition metal, respectively.
[0296] As the lithium source, it is preferable to use a compound containing lithium, such as lithium carbonate, lithium hydroxide, lithium nitrate, or lithium fluoride. It is preferable that the lithium source has high purity, and it is preferable to use a material with a purity of, for example, 99.99% or higher.
[0297] As the cobalt source, it is preferable to use a compound containing cobalt, for example, cobalt oxide such as tricobalt tetroxide, cobalt hydroxide, or the like.
[0298] <Step S12> Next, in step S12 shown in FIG. 16A, the lithium source and the cobalt source are pulverized and mixed to prepare a mixed material. The pulverization and mixing can be performed by a dry method or a wet method. The wet method is preferable because it allows for smaller pulverization. When performing the wet method, a solvent is prepared. Examples of solvents that can be used include ketones such as acetone, alcohols such as ethanol and isopropanol, ether, dioxane, acetonitrile, and N-methyl-2-pyrrolidone (NMP). It is more preferable to use an aprotic solvent that is less likely to react with lithium.
[0299] A ball mill, a bead mill, or the like can be used as a means for pulverizing and mixing. When using a ball mill, it is preferable to use aluminum oxide balls or zirconium oxide balls as media. Zirconium oxide balls are preferred because they emit less impurities. Furthermore, when using a ball mill, a bead mill, or the like, it is preferable to set the peripheral speed to 100 mm / s or more and 2000 mm / s or less in order to suppress contamination from the media.
[0300] 16A, the mixed material is heated at a temperature of preferably 800° C. to 1100° C., more preferably 900° C. to 1000° C., and even more preferably about 950° C.
[0301] After heating, the material may be crushed and sieved as necessary. The material after heating may be recovered by transferring it from the crucible to a mortar and then recovering it. The mortar is preferably an aluminum oxide mortar or a zirconium oxide mortar.
[0302] <Step S14> By the above steps, lithium cobalt oxide (LiCoO 2 ) can be synthesized.
[0303] Although an example of producing lithium cobalt oxide by a solid phase method as in steps S11 to S14 has been shown, lithium cobalt oxide may also be produced by a coprecipitation method or a hydrothermal method.
[0304] <Step S15> Next, in step S15 shown in Fig. 16A, the lithium cobalt oxide is heated. Because this is the first heating of the lithium cobalt oxide, the heating in step S15 is sometimes called initial heating. Alternatively, because this heating is performed before the next step S20, it is sometimes called preheating or pretreatment.
[0305] The crucible used for heating in step S15 is preferably an aluminum oxide crucible. An aluminum oxide crucible is a material that does not easily release impurities. In this embodiment, an aluminum oxide crucible with a purity of 99.9% is used. It is preferable to place a lid on the crucible when heating, as this can prevent volatilization or sublimation of the material. Placing a lid on the crucible means that it is sufficient to prevent volatilization or sublimation of the material from the time the temperature is increased to the time the temperature is decreased in this step, and it is not necessary to seal the crucible with a lid. For example, as described above, by filling the reaction chamber with oxygen, this step can be performed without sealing the crucible.
[0306] Furthermore, it is preferable to use a used crucible rather than a new one. In this specification, a new crucible refers to one that has undergone the process of heating with lithium cobalt oxide added thereto two or fewer times. A used crucible refers to one that has undergone the process of heating with lithium cobalt oxide and / or a material containing an additive element X added thereto three or more times. This is because when a new crucible is used, there is a risk that some of the materials, including lithium fluoride, may be absorbed, diffused, migrated, and / or adhered to the sheath during heating. If some of the materials are lost as a result of this, there is a growing concern that the distribution of elements, particularly in the surface layer of the positive electrode active material, may not fall within a preferred range. On the other hand, this risk is less likely with a used crucible.
[0307] The following effects are expected from the initial heating, but the initial heating is not essential for obtaining the positive electrode active material of one embodiment of the present invention.
[0308] The initial heating causes lithium to be desorbed from a portion of the surface layer 100xa of the lithium cobalt oxide. This is also expected to have the effect of improving the crystallinity of the interior 100xb. Furthermore, the lithium source and / or cobalt source prepared in step S11 or the like may contain impurities. The initial heating can reduce the amount of impurities in the lithium cobalt oxide completed in step S14.
[0309] Furthermore, initial heating has the effect of smoothing the surface of the lithium cobalt oxide. A smooth surface of lithium cobalt oxide means that there are few irregularities, the lithium cobalt oxide is rounded overall, and the corners are also rounded. A smooth surface of lithium cobalt oxide means that the surface of the composite oxide, which is the positive electrode active material particle, is smooth. Furthermore, a state in which there is little foreign matter adhering to the surface is called smooth. Foreign matter is thought to be a cause of irregularities, so it is preferable that it does not adhere to the surface.
[0310] For this initial heating, it is not necessary to prepare a lithium source, a source of an additional element, or a material that functions as a flux.
[0311] If the heating time in this step is too short, sufficient effects will not be obtained, but if it is too long, productivity will decrease. For example, the heating conditions can be selected from those described in step S13. Regarding the heating conditions, the heating temperature in this step is preferably lower than the temperature in step S13 in order to maintain the crystalline structure of the lithium cobalt oxide. Furthermore, the heating time in this step is preferably shorter than the time in step S13 in order to maintain the crystalline structure of the lithium cobalt oxide. For example, heating at a temperature of 700°C or higher and 1000°C or lower for 2 hours or higher and 20 hours or lower is recommended. Maintaining the crystalline structure of the lithium cobalt oxide means maintaining the crystalline structure of the composite oxide, which is the positive electrode active material particle.
[0312] The effect of increasing the crystallinity of the inner portion 100xb is, for example, the effect of alleviating distortion, displacement, etc. resulting from the difference in shrinkage of the lithium cobalt oxide produced in step S13.
[0313] The heating in step S13 may cause a temperature difference between the surface and the interior of the lithium cobalt oxide. This temperature difference may induce a shrinkage difference. It is also believed that the temperature difference causes a difference in fluidity between the surface and the interior, resulting in a shrinkage difference. The energy associated with the shrinkage difference causes an internal stress difference in the lithium cobalt oxide. This internal stress difference is also called strain, and this energy is sometimes called strain energy. It is believed that the internal stress is removed by the initial heating in step S15; in other words, the strain energy is homogenized by the initial heating in step S15. When the strain energy is homogenized, the strain in the lithium cobalt oxide is alleviated. This may result in a smoother surface for the lithium cobalt oxide. This is also referred to as an improved surface. In other words, it is believed that the shrinkage difference in the lithium cobalt oxide is alleviated and the surface of the composite oxide is smoother after step S15.
[0314] Furthermore, the shrinkage difference may cause microscopic deviations, such as crystal deviations, in the lithium cobalt oxide. It is preferable to carry out this step in order to reduce such deviations. This step makes it possible to equalize the deviations in the lithium cobalt oxide. Equalizing the deviations may result in a smooth surface of the lithium cobalt oxide. This is also referred to as crystal grain alignment. In other words, it is believed that step S15 alleviates deviations such as crystal deviations in the lithium cobalt oxide, resulting in a smooth surface of the lithium cobalt oxide. A smooth surface of the lithium cobalt oxide means that the surface of the composite oxide, which is the positive electrode active material particle, is smooth.
[0315] When a composite oxide with a smooth surface is used as a positive electrode active material, deterioration during charge and discharge in a secondary battery is reduced, and cracking of the positive electrode active material can be prevented.
[0316] The initial heating in step S15 causes lithium ions to be desorbed from a portion of the surface layer 100xa, resulting in a more favorable distribution of the additional element X. It is also believed that the initial heating facilitates the distribution of the additional element X to differ from one another due to the following mechanism. First, lithium ions are desorbed from a portion of the surface layer 100xa by the initial heating. Next, the lithium cobalt oxide having the lithium ion-deficient surface layer 100xa is mixed with an additional element source and heated. Magnesium, a typical element among the additional elements, becomes a divalent ion. Therefore, Mg is present in a portion of the surface layer 100xa. 2+ and Co reduced due to the lack of lithium ions. 2+ When these combine with oxygen, rock salt magnesium oxide and rock salt cobalt (II) oxide are formed.
[0317] Among the additive elements X, nickel is likely to dissolve and diffuse to the interior 100xb when the surface layer 100xa is a layered rock-salt lithium cobaltate, but when part of the surface layer 100xa is a rock-salt lithium cobaltate, nickel tends to remain in the surface layer 100xa. Therefore, initial heating can make it easier for divalent additive elements X, including nickel, to remain in the surface layer 100xa. This improves the distribution of the additive elements X. The effect of initial heating is particularly significant on the surface of the first positive electrode active material 100x other than the (001)-oriented surface and the surface layer 100xa.
[0318] Furthermore, in these rock salt types, the bond distance between the metal Me and oxygen (Me-O distance) tends to be longer than in the layered rock salt type.
[0319] For example, rock salt type Ni 0.5 Mg 0.5 The Me-O distance in O is 2.09 × 10 −10 m, and the Me-O distance in rocksalt MgO is 2.11 × 10 −10 m. Even if a spinel-type phase is formed in a part of the surface layer 100xa, the spinel-type NiAl 2 O 4 The Me-O distance is 2.0125 × 10 −10 m, spinel-type MgAl 2 O 4 The Me-O distance is 2.02 × 10−10 In both cases, the Me-O distance is 2 × 10 −10 Exceeds m.
[0320] On the other hand, in the layered rock salt type, the bond distance between metals other than lithium and oxygen is shorter than the above. For example, layered rock salt type LiAlO 2 The Al-O distance in −10 m (Li-O distance is 2.11 × 10 −10 m). Also, layered rock salt LiCoO 2 The Co-O distance in −10 m (Li-O distance is 2.0916 × 10 −10 m).
[0321] According to the Shannon ionic radius described in Non-Patent Document 15, the ionic radius of hexacoordinated aluminum is 0.535 × 10 −10 The ionic radius of hexacoordinated oxygen is 1.4 × 10 −10 m, and the sum of these is 1.935 × 10 −10 m.
[0322] From the above, it is considered that aluminum exists more stably in the non-lithium sites of the layered rock-salt type than in the rock-salt type, and therefore aluminum is more likely to be distributed in the deeper region having the layered rock-salt type and / or the interior 100xb than in the region close to the surface having the rock-salt type phase in the surface layer 100xa.
[0323] Note that pre-synthesized lithium cobalt oxide may be used in step S14. In this case, steps S11 to S13 can be omitted. By performing step S15 on pre-synthesized lithium cobalt oxide, lithium cobalt oxide with a smooth surface can be obtained.
[0324] <Step S20> Next, as shown in step S20, it is preferable to add the additional element A to the lithium cobalt oxide that has undergone the initial heating. When the additional element A is added to the lithium cobalt oxide that has undergone the initial heating, the additional element A can be added evenly. Therefore, it is preferable to add the additional element A after the initial heating. The step of adding the additional element A will be described with reference to FIGS. 16B and 16C.
[0325] 16B, a source of an additional element A (A source) to be added to lithium cobalt oxide is prepared. A lithium source may be prepared together with the additional element A source.
[0326] As the additional element A, one or more of the additional elements X described in the previous embodiment, specifically, magnesium, fluorine, nickel, aluminum, titanium, and phosphorus, can be used.
[0327] When magnesium is selected as the additive element, the source of the additive element can be called a magnesium source (Mg source). As the magnesium source, magnesium fluoride, magnesium oxide, magnesium hydroxide, magnesium carbonate, or the like can be used. Furthermore, a plurality of the above-mentioned magnesium sources may be used.
[0328] When fluorine is selected as the additive element, the source of the additive element can be called a fluorine source (F source). Examples of the fluorine source include lithium fluoride (LiF), magnesium fluoride (MgF 2 ), aluminum fluoride (AlF 3 ), titanium fluoride (TiF 4 ), cobalt fluoride (CoF 2 , CoF 3 ), nickel fluoride (NiF 2 ), zirconium fluoride (ZrF 4 ), vanadium fluoride (VF 5 ), manganese fluoride, iron fluoride, chromium fluoride, niobium fluoride, zinc fluoride (ZnF 2 ), calcium fluoride (CaF 2 ), sodium fluoride (NaF), potassium fluoride (KF), barium fluoride (BaF 2 ), cerium fluoride (CeF 3 , CeF 4 ), lanthanum fluoride (LaF 3 ), or sodium aluminum hexafluoride (Na 3 AlF 6 Among these, lithium fluoride is preferred because it has a relatively low melting point of 848° C. and is easily melted in the heating step described below.
[0329] Magnesium fluoride can be used as both a fluorine source and a magnesium source, and lithium fluoride can be used as both a fluorine source and a lithium source. Another lithium source that can be used in step S21 is lithium carbonate.
[0330] The fluorine source is preferably a gas, and fluorine (F 2 ), fluorocarbon, sulfur fluoride, or oxygen fluoride (OF 2 , O 2 F 2 , O 3 F 2 , O 4 F 2 , O 5 F 2 , O 6 F 2 , O 2 It is preferable to use a gas such as fluorine, and mix the gas into the atmosphere in the heating step described below.
[0331] In this embodiment, lithium fluoride (LiF) is prepared as the fluorine source, and magnesium fluoride (MgF) is prepared as the fluorine source and magnesium source. 2 Lithium fluoride and magnesium fluoride are prepared as LiF:MgF 2 The effect of lowering the melting point is greatest when the molar ratio of lithium fluoride and magnesium fluoride is about 65:35. On the other hand, if the amount of lithium fluoride is too high, there is a concern that the lithium will be excessive and the cycle characteristics will deteriorate. Therefore, the molar ratio of lithium fluoride and magnesium fluoride is set to LiF:MgF 2 =x:1 (0≦x≦1.9), and LiF:MgF 2 =x:1 (0.1≦x≦0.5) is more preferable, and LiF:MgF 2 = x: 1 (x = 0.33 or its vicinity) is more preferable. Here, "or its vicinity" refers to a value that is greater than 0.9 times and less than 1.1 times the value.
[0332] 16B, the magnesium source and the fluorine source are pulverized and mixed. This step can be performed under pulverization and mixing conditions selected from those described in step S12.
[0333] 16B, the pulverized and mixed materials are collected to obtain a source of the additional element A (A source). Note that the source of the additional element A shown in step S23 contains a plurality of starting materials and can be called a mixture.
[0334] The particle size of the mixture is preferably such that the median diameter (D50) is 600 nm or more and 10 μm or less, more preferably 1 μm or more and 5 μm or less. Even when a single material is used as the additive element source, the median diameter (D50) is preferably 600 nm or more and 10 μm or less, more preferably 1 μm or more and 5 μm or less.
[0335] Such a finely powdered mixture (including the case where only one kind of additive element is included) can be easily adhered to the surface of the lithium cobalt oxide when mixed with the lithium cobalt oxide in a later step. If the mixture is evenly adhered to the surface of the lithium cobalt oxide particles, it is preferable because the additive element can be easily distributed or diffused uniformly in the surface layer portion 100xa of the composite oxide after heating.
[0336] <Step S21a> A step different from that shown in Figure 16B will be described with reference to Figure 16C. In step S21a shown in Figure 16C, four types of additive element sources to be added to lithium cobalt oxide are prepared. That is, the types of additive element sources shown in Figure 16C are different from those shown in Figure 16B. A lithium source may be prepared together with the additive element sources.
[0337] As sources of four additive elements, a magnesium source (Mg source), a fluorine source (F source), a nickel source (Ni source), and an aluminum source (Al source) are prepared. The magnesium source and the fluorine source can be selected from the compounds described in FIG. 16B . Nickel oxide, nickel hydroxide, etc. can be used as the nickel source. Aluminum oxide, aluminum hydroxide, etc. can be used as the aluminum source.
[0338] <Steps S22 and S23> Steps S22 and S23 shown in FIG. 16C are similar to the steps described in FIG. 16B.
[0339] 16A , lithium cobalt oxide and a source of additional element A (A source) are mixed together. The ratio of the number of cobalt atoms Co in the lithium cobalt oxide to the number of magnesium atoms Mg in the source of additional element A is preferably Co:Mg=100:y (0.1≦y≦6), and more preferably Co:Mg=100:y (0.3≦y≦3).
[0340] The mixing conditions in step S31 are preferably milder than those in step S12 so as not to destroy the shape of the lithium cobalt oxide particles. For example, the mixing conditions are preferably lower in rotation speed or shorter in time than those in step S12. It can also be said that dry mixing provides milder conditions than wet mixing. For example, a ball mill, a bead mill, or the like can be used for mixing. When using a ball mill, it is preferable to use zirconium oxide balls as the media.
[0341] In this embodiment, dry mixing is performed in a ball mill using zirconium oxide balls with a diameter of 1 mm at 150 rpm for 1 hour in a dry room with a dew point of −100° C. or higher and −10° C. or lower.
[0342] <Step S32> Next, in step S32 of Fig. 16A, the mixed materials are collected to obtain a mixture 903. When collecting the materials, they may be crushed and then sieved, if necessary.
[0343] 16A to 16C illustrate a fabrication method in which the additive element X is added after initial heating, but the present invention is not limited to the above method. The additive element X may be added at a different timing or multiple times. The timing may be changed depending on the additive element X.
[0344] For example, as shown in Figures 17A to 17C, an additional element X may be added to the lithium source and the cobalt source in step S11, i.e., at the stage of the starting material for the composite oxide. Figure 17A shows a flow for adding a magnesium source to the lithium source and the cobalt source. Figure 17B shows a flow for adding a magnesium source and an aluminum source to the lithium source and the cobalt source. Figure 17C shows a flow for adding a magnesium source and a nickel source to the lithium source and the cobalt source. The additional element sources shown in Figures 17A to 17C are examples.
[0345] Subsequently, the process proceeds to step S12, then step S13, and finally step S14, where lithium cobalt oxide containing the additive element X can be obtained. It is also possible to control the distribution of the additive element X depending on the timing of adding the additive element X. The additive element X added as shown in FIGS. 17A to 17C is expected to be located inside the first positive electrode active material 100x. Furthermore, in the case of the flow shown in FIGS. 17A to 17C, the above-described steps S11 to S14 and steps S21 to S23 do not need to be separated, making this a simple and highly productive method. Of course, even in the flow shown in FIGS. 17A to 17C, a new additive element X may be added in step S20.
[0346] Alternatively, lithium cobalt oxide may be used that has already contained a portion of the additive element X. For example, if lithium cobalt oxide to which magnesium and fluorine have been added is used, it is possible to omit steps S11 to S14 and a portion of step S20. This method can be said to be simple and highly productive.
[0347] Alternatively, lithium cobalt oxide to which magnesium and fluorine have been added in advance may be heated in step S15, and then a magnesium source and a fluorine source, or a magnesium source, a fluorine source, a nickel source, and an aluminum source may be added as in step S20.
[0348] <Step S33> Next, in step S33 shown in Fig. 16A, the mixture 903 is heated. The heating can be performed under heating conditions selected from those described in step S15. The heating time is preferably 2 hours or more. At this time, the pressure inside the furnace may exceed atmospheric pressure in order to increase the oxygen partial pressure in the heating atmosphere. This is because if the oxygen partial pressure in the heating atmosphere is insufficient, cobalt and the like may be reduced, and the layered rock salt crystal structure of lithium cobalt oxide and the like may no longer be maintained.
[0349] Here, a supplementary note about the heating temperature will be provided. The lower limit of the heating temperature in step S33 must be equal to or higher than the temperature at which the reaction between the lithium cobalt oxide and the additive element source proceeds. The temperature at which the reaction proceeds is preferably a temperature at which interdiffusion between the lithium cobalt oxide and the elements contained in the additive element source occurs, and may be lower than the melting temperature of these materials. An oxide will be used as an example for explanation, but the melting temperature T m 0.757 times (Tammann temperature T d ) solid-phase diffusion occurs. Therefore, the heating temperature in step S33 is preferably 650° C. or higher.
[0350] Of course, the reaction is more likely to proceed if the temperature is equal to or higher than the melting point of one or more of the materials contained in the mixture 903. For example, LiF and MgF are used as the additive element source. 2 When LiF and MgF 2 Since the eutectic point of is around 742°C, the lower limit of the heating temperature in step S33 is preferably set to 742°C or higher.
[0351] Also, LiCoO 2 :LiF:MgF 2 In the mixture 903 obtained by mixing so that the molar ratio was 100:0.33:1, an endothermic peak was observed around 830° C. in DSC measurement. Therefore, the lower limit of the heating temperature is more preferably 830° C. or higher.
[0352] A higher heating temperature is preferable because the reaction proceeds more easily, the heating time is shorter, and productivity is higher.
[0353] The upper limit of the heating temperature is set to be lower than the decomposition temperature of lithium cobalt oxide (melting point 1130°C). At temperatures close to the decomposition temperature, there is a concern that lithium cobalt oxide may decompose, albeit only slightly. Therefore, the upper limit of the heating temperature is more preferably 1000°C or lower, even more preferably 950°C or lower, and even more preferably 900°C or lower.
[0354] In consideration of these, the heating temperature in step S33 is preferably 650°C or higher and 1130°C or lower, more preferably 650°C or higher and 1000°C or lower, even more preferably 650°C or higher and 950°C or lower, and even more preferably 650°C or higher and 900°C or lower. Also, it is preferably 742°C or higher and 1130°C or lower, more preferably 742°C or higher and 1000°C or lower, even more preferably 742°C or higher and 950°C or lower, and even more preferably 742°C or higher and 900°C or lower. Also, it is preferably 830°C or higher and 1130°C or lower, more preferably 830°C or higher and 1000°C or lower, even more preferably 830°C or higher and 950°C or lower, and even more preferably 830°C or higher and 900°C or lower. The heating temperature in step S33 is preferably lower than the heating temperature in step S13.
[0355] The cooling after heating in step S33 can be performed by natural cooling, but it is preferable that the time required for the temperature to drop from the specified temperature to room temperature is between 10 and 50 hours. For example, the temperature drop rate (hereinafter also referred to as the cooling rate) is preferably between 80°C / h and 250°C / h, and more preferably between 180°C / h and 210°C / h. The cooling rate in step S33 is preferably faster than that in step S13. A fast cooling rate is called rapid cooling. Rapid cooling after the melting allows for the appropriate production of a shell. Specifically, it is possible to produce a narrow shell. The temperature at the end of the temperature drop does not necessarily have to be room temperature; it is sufficient to cool to a temperature acceptable for the next step.
[0356] Furthermore, when heating the mixture 903, it is preferable to control the partial pressure of fluorine or a fluorine compound resulting from the fluorine source or the like within an appropriate range. The partial pressure can also be controlled by heating the crucible used in this step with a lid. As mentioned above, the lid can prevent the volatilization or sublimation of the material. Therefore, it is not necessary to seal the crucible with a lid, as long as the volatilization or sublimation of the material can be prevented from occurring during the temperature increase and decrease periods in this step. For example, by filling the reaction chamber in which the crucible is placed with oxygen, it is possible to perform this step without sealing the crucible. A positive electrode active material containing an appropriate amount of fluorine or a fluorine compound is preferable because it can suppress heat generation and smoke generation even in the event of an internal short circuit.
[0357] In the manufacturing method described in this embodiment, some materials, for example, LiF as a fluorine source, may function as a flux, which allows the heating temperature to be lowered below the decomposition temperature of lithium cobalt oxide, for example, to 742° C. or higher and 950° C. or lower, and allows the additive element X, such as magnesium, to be distributed in the surface layer, thereby enabling the manufacturing of a positive electrode active material with excellent characteristics.
[0358] However, since LiF has a lower specific gravity in a gaseous state than oxygen, there is a possibility that LiF may volatilize or sublime when heated, and if it volatilizes, the amount of LiF in the mixture 903 will decrease. This will weaken its function as a flux. Therefore, it is necessary to heat while suppressing the volatilization of LiF. Even if LiF is not used as a fluorine source, etc., LiCoO 2 There is a possibility that Li on the surface reacts with F in the fluorine source to produce LiF, which may then volatilize. Therefore, even if a fluorine compound with a higher melting point than LiF is used, it is still necessary to suppress volatilization.
[0359] Therefore, it is preferable to heat the mixture 903 in an atmosphere containing LiF, that is, to heat the mixture 903 in a state where the partial pressure of LiF is high in the heating furnace. By heating in this manner, it is possible to suppress the volatilization of LiF in the mixture 903. In order to suppress the volatilization of LiF, it is preferable to place a lid on the crucible.
[0360] The heating in this step is preferably performed so as not to cause particles of the mixture 903 to stick together. If the particles of the mixture 903 stick together during heating, the contact area with oxygen in the atmosphere will decrease and the route along which the additional element X (e.g., fluorine) diffuses will be blocked, which may result in poor distribution of the additional element X (e.g., magnesium and fluorine) in the surface layer. In order to promote the reaction with oxygen in the atmosphere, the crucible does not need to be sealed with a lid.
[0361] Furthermore, it is believed that uniform distribution of the additive element X (e.g., fluorine) in the surface layer portion results in a smooth cathode active material with few irregularities. Therefore, in order to maintain the smooth state of the surface after the heating in step S15 or to make it even smoother in this process, it is preferable that the particles of the mixture 903 do not stick to each other.
[0362] Furthermore, when heating in a rotary kiln, it is preferable to control the flow rate of the oxygen-containing atmosphere in the kiln during heating. For example, it is preferable to reduce the flow rate of the oxygen-containing atmosphere, or to first purge the atmosphere and then not flow the atmosphere after introducing the oxygen atmosphere into the kiln. Flowing oxygen may cause the fluorine source to evaporate, which is undesirable in terms of maintaining surface smoothness.
[0363] When heating is performed using a roller hearth kiln, the mixture 903 can be heated in an atmosphere containing LiF by placing a lid on a container containing the mixture 903, for example, in the same way as a lid placed on a crucible.
[0364] Regarding the heating time, the heating time varies depending on conditions such as the heating temperature, the size and composition of the lithium cobalt oxide obtained in step S14, etc. When the lithium cobalt oxide is small, a lower temperature or a shorter heating time may be more preferable than when the lithium cobalt oxide is large.
[0365] When the median diameter (D50) of the lithium cobalt oxide obtained in step S14 of Fig. 16A is about 12 µm, the heating temperature is preferably, for example, 650°C or more and 950°C or less. The heating time is preferably, for example, 3 hours or more and 60 hours or less, more preferably 10 hours or more and 30 hours or less, and even more preferably about 20 hours. The temperature-lowering time after heating is preferably, for example, 10 hours or more and 50 hours or less.
[0366] On the other hand, when the median diameter (D50) of the lithium cobalt oxide obtained in step S14 is about 5 μm, the heating temperature is preferably, for example, 650° C. or higher and 950° C. or lower. The heating time is preferably, for example, 1 hour or higher and 10 hours or lower, and more preferably about 5 hours. The temperature-lowering time after heating is preferably, for example, 10 hours or higher and 50 hours or lower.
[0367] <Step S34> Next, in step S34 shown in FIG. 16A , the heated material is recovered to obtain a first positive electrode active material 100x. The recovered particles may be further sieved. Through the above steps, a first positive electrode active material 100x according to one embodiment of the present invention can be produced. The positive electrode active material according to one embodiment of the present invention has a smooth surface.
[0368] 18 to 19C , a positive electrode active material preparation method 2, which is an embodiment of the present invention and differs from positive electrode active material preparation method 1, will be described. The positive electrode active material preparation method 2 differs from preparation method 1 mainly in the number of times the additive element X is added and the mixing method. For other details, the description of preparation method 1 can be referred to.
[0369] In FIG. 18, steps S11 to S15 are performed in the same manner as in FIG. 16A to prepare lithium cobalt oxide that has undergone initial heating.
[0370] <Step S20a> Next, as shown in step S20a, it is preferable to add an additional element A1 to the lithium cobalt oxide that has undergone the initial heating.
[0371] <Step S21> In step S21 shown in Fig. 19A, a first additive element source (A1 source) is prepared. The first additive element source can be selected from the additive elements described in step S21 shown in Fig. 16B and used. For example, one or more selected from magnesium and fluorine can be suitably used as the first additive element source. Fig. 19A illustrates an example in which a magnesium source (Mg source) and a fluorine source (F source) are used as the first additive element source.
[0372] Steps S21 to S23 shown in Fig. 19A can be performed under the same conditions as steps S21 to S23 shown in Fig. 16B, as a result of which the first additive element source can be obtained in step S23.
[0373] Furthermore, steps S31 to S33 shown in FIG. 18 can be performed in the same manner as steps S31 to S33 shown in FIG. 16A.
[0374] <Step S34a> Next, the material heated in step S33 is recovered to produce lithium cobalt oxide containing the first additive element source. To distinguish it from the composite oxide in step S14, this is also called a second composite oxide.
[0375] <Step S40> In step S40 shown in Fig. 18, a second additive element source (A2 source) is added. This will be described with reference to Figs. 19B and 19C.
[0376] <Step S41> In step S41 shown in Fig. 19B, a second additive element source is prepared. The second additive element source can be selected from the additive elements described in step S21 shown in Fig. 19A and used. For example, one or more selected from nickel, titanium, and aluminum can be suitably used as the second additive element source. Fig. 19B illustrates an example in which a nickel source (Ni source) and an aluminum source (Al source) are used as the second additive element source.
[0377] Steps S41 to S43 shown in Fig. 19B can be performed under the same conditions as steps S21 to S23 shown in Fig. 16B, as a result of which the second additive element source can be obtained in step S43.
[0378] 19C shows a modified example of the steps described with reference to FIG. 19B. In step S41 shown in FIG. 19C, a nickel source (Ni source) and an aluminum source (Al source) are prepared, and in step S42a, they are independently pulverized. As a result, in step S43, a plurality of second additive element sources are prepared. The steps in FIG. 19C differ from those in FIG. 19B in that the additive element X is independently pulverized in step S42a.
[0379] <Steps S51 to S54> Next, steps S51 to S54 shown in FIG. 18 can be performed under the same conditions as steps S31 to S34 shown in FIG. 16A. The conditions for step S53, which is a heating step, may be a lower temperature and a shorter time than those for step S33. Through the above steps, step S54 can produce a first positive electrode active material 100x according to one embodiment of the present invention. The positive electrode active material according to one embodiment of the present invention has a smooth surface.
[0380] 18 to 19C , in fabrication method 2, the additive element X to lithium cobalt oxide is introduced separately from a first additive element source and a second additive element source. By introducing the additive elements separately, the positions of the additive elements X in the depth direction can be changed. For example, it is possible to position the first additive element X so that it has a higher concentration in the surface layer portion than in the interior, and to position the second additive element X so that it has a higher concentration in the interior than in the surface layer portion.
[0381] The initial heating shown in this embodiment is performed on lithium cobalt oxide. Therefore, the initial heating is preferably performed under conditions that are lower than the heating temperature required to obtain lithium cobalt oxide and shorter than the heating time required to obtain lithium cobalt oxide. The step of adding the additive element X to the lithium cobalt oxide is preferably performed after the initial heating. This addition step can be performed in two or more steps. Following this order of steps is preferable because it maintains the surface smoothness obtained by the initial heating.
[0382] This embodiment mode can be freely combined with other embodiment modes.
[0383] Embodiment 4 In this embodiment, a lithium-ion secondary battery including a positive electrode active material according to one embodiment of the present invention will be described. The secondary battery includes at least an outer casing, a current collector, an active material (a positive electrode active material or a negative electrode active material), a conductive additive, and a binder. The secondary battery also includes an electrolyte solution containing a lithium salt or the like dissolved therein. In the case of a secondary battery using an electrolyte solution, a positive electrode, a negative electrode, and a separator are provided between the positive electrode and the negative electrode.
[0384] The positive electrode active material layer preferably includes the positive electrode active material composite 100α described in Embodiment 1, and may further include a binder, a conductive additive, and the like.
[0385] The current collector is a metal foil, and the positive electrode is formed by applying a slurry to the metal foil and drying it. After drying, the foil may be pressed further. The positive electrode is formed by forming an active material layer on the current collector.
[0386] The term "slurry" refers to a liquid material used to form an active material layer on a current collector, and includes at least an active material, a binder, and a solvent, preferably further containing a conductive additive. The slurry is also called an electrode slurry or an active material slurry. A positive electrode slurry is used to form a positive electrode active material layer, and a negative electrode slurry is used to form a negative electrode active material layer.
[0387] The conductive additive, also called a conductivity-imparting agent or conductive material, is made of a carbon material. By attaching the conductive additive between multiple active materials, the active materials are electrically connected to each other, thereby increasing their conductivity. Note that "attachment" does not only refer to physical adhesion between the active material and the conductive additive, but also encompasses cases where a covalent bond is formed, bonding due to van der Waals forces, the conductive additive covering part of the surface of the active material, the conductive additive fitting into the surface irregularities of the active material, and electrical connection even when not in contact with each other.
[0388] A typical carbon material used as a conductive additive is carbon black (furnace black, acetylene black, graphite, etc.).
[0389] A binder (resin) is mixed into the positive electrode of a secondary battery to bond the active material to a current collector such as a metal foil. The binder is also called a binding agent. The binder is a polymeric material, and adding too much binder reduces the ratio of active material in the positive electrode, reducing the discharge capacity of the secondary battery. Therefore, the amount of binder mixed is kept to a minimum.
[0390] Graphene is a carbon material that has amazing electrical, mechanical, and chemical properties and is expected to be applied in a variety of fields, including graphene-based field-effect transistors and solar cells.
[0391] Graphene or graphene compounds may have excellent electrical properties, such as high conductivity, and excellent physical properties, such as high flexibility and high mechanical strength. Graphene or graphene compounds may have a sheet-like shape. Graphene or graphene compounds may have a curved surface, enabling surface contact with low contact resistance. Even when thin, they may have very high conductivity, allowing a small amount to efficiently form a conductive path within an active material layer. Therefore, using graphene or graphene compounds as a conductive material can increase the contact area between the active material and the conductive material. It is preferable that the graphene compound clings to at least a portion of the active material particles. It is also preferable that the graphene compound overlaps at least a portion of the active material particles. It is also preferable that the shape of the graphene compound matches at least a portion of the shape of the active material particles. The shape of the active material particles refers, for example, to the unevenness of a single active material particle or the unevenness formed by multiple active material particles. It is also preferable that the graphene compound surrounds at least a portion of the active material particles. The graphene compound may also have holes.
[0392] By using the positive electrode active material composite 100α obtained in the first embodiment as a positive electrode, a secondary battery having a high energy density and high safety can be obtained.
[0393] Although the above configuration shows an example of a secondary battery using an electrolytic solution, the present invention is not particularly limited.
[0394] For example, a semi-solid battery or an all-solid battery can be manufactured using the positive electrode active material composite 100α shown in Embodiment 1.
[0395] In this specification, a semi-solid battery refers to a battery having a semi-solid material in at least one of the electrolyte layer, positive electrode, and negative electrode. Here, semi-solid does not mean that the ratio of solid material is 50%. Semi-solid means that while having solid properties such as small volume change, it also has some liquid-like properties such as flexibility. As long as these properties are met, the battery may be made of a single material or multiple materials. For example, a porous solid material may be impregnated with a liquid material.
[0396] In this specification, a polymer electrolyte secondary battery refers to a secondary battery having a polymer in the electrolyte layer between a positive electrode and a negative electrode. Polymer electrolyte secondary batteries include dry (or intrinsic) polymer electrolyte batteries and polymer gel electrolyte batteries. Polymer electrolyte secondary batteries are also sometimes called semi-solid batteries.
[0397] When a semi-solid battery is manufactured using the positive electrode active material composite 100α described in Embodiment 1, the semi-solid battery becomes a secondary battery with a large discharge capacity. Furthermore, the semi-solid battery can have a high charge / discharge voltage. Alternatively, a semi-solid battery with high safety or reliability can be realized.
[0398] Furthermore, the positive electrode active material composite 100α described in the first embodiment may be mixed with another positive electrode active material.
[0399] Other examples of the positive electrode active material include composite oxides having an olivine-type crystal structure, a layered rock salt-type crystal structure, or a spinel-type crystal structure. For example, LiFePO 4 , LiFeO 2 , LiNiO 2 , LiMn 2 O 4 , V 2 O 5 , Cr 2 O 5 , MnO2 and the like compounds.
[0400] Other positive electrode active materials include LiMn 2 O 4 Lithium-containing materials having a spinel-type crystal structure containing manganese, such as lithium nickel oxide (LiNiO 2 or LiNi 1−x M x O 2 It is preferable to mix (0<x<1) (M=Co, Al, etc.) This configuration can improve the characteristics of the secondary battery.
[0401] In addition, as another positive electrode active material, the composition formula Li a Mn b M c O d A lithium-manganese composite oxide that can be expressed by the formula (1) can be used. Here, element M is preferably a metal element selected from among lithium and manganese, or silicon or phosphorus, and more preferably nickel. Furthermore, when measuring the entire lithium-manganese composite oxide particle, it is preferable that 0<a / (b+c)<2, c>0, and 0.26≦(b+c) / d<0.5 are satisfied during discharge. The composition of metals, silicon, phosphorus, etc. in the entire lithium-manganese composite oxide particle can be measured, for example, using an inductively coupled plasma mass spectrometer (ICP-MS). The oxygen composition in the entire lithium-manganese composite oxide particle can be measured, for example, using energy dispersive X-ray spectroscopy (EDX). Furthermore, the composition can be determined by using valence evaluation of fused gas analysis and XAFS (X-ray absorption fine structure) analysis in combination with ICPMS analysis. The lithium manganese composite oxide refers to an oxide containing at least lithium and manganese, and may contain at least one element selected from the group consisting of chromium, cobalt, aluminum, nickel, iron, magnesium, molybdenum, zinc, indium, gallium, copper, titanium, niobium, silicon, phosphorus, and the like.
[0402] <Binder> As the binder, it is preferable to use a rubber material such as styrene-butadiene rubber (SBR), styrene-isoprene-styrene rubber, acrylonitrile-butadiene rubber, butadiene rubber, ethylene-propylene-diene copolymer, etc. Furthermore, as the binder, fluororubber can be used.
[0403] Furthermore, it is preferable to use, for example, a water-soluble polymer as the binder. Examples of the water-soluble polymer that can be used include polysaccharides. Examples of the polysaccharide that can be used include cellulose derivatives such as carboxymethyl cellulose (CMC), methyl cellulose, ethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, and regenerated cellulose, as well as starch. It is even more preferable to use these water-soluble polymers in combination with the above-mentioned rubber material.
[0404] Alternatively, it is preferable to use, as the binder, materials such as polystyrene, polymethyl acrylate, polymethyl methacrylate (polymethyl methacrylate, PMMA), sodium polyacrylate, polyvinyl alcohol (PVA), polyethylene oxide (PEO), polypropylene oxide, polyimide, polyvinyl chloride, polytetrafluoroethylene, polyethylene, polypropylene, polyisobutylene, polyethylene terephthalate, nylon, polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), ethylene propylene diene polymer, polyvinyl acetate, and nitrocellulose.
[0405] The binder may be used in combination with two or more of the above.
[0406] For example, a material with particularly excellent viscosity adjusting effect may be used in combination with other materials. For example, while rubber materials have excellent adhesive strength and elasticity, it may be difficult to adjust the viscosity when mixed with a solvent. In such cases, it is preferable to mix them with a material with particularly excellent viscosity adjusting effect. A material with particularly excellent viscosity adjusting effect is sometimes called a thickener. As a material with particularly excellent viscosity adjusting effect, for example, a water-soluble polymer may be used. Furthermore, as a water-soluble polymer with particularly excellent viscosity adjusting effect, the above-mentioned polysaccharides, for example, carboxymethyl cellulose (CMC), methyl cellulose, ethyl cellulose, hydroxypropyl cellulose, and diacetyl cellulose, cellulose derivatives such as regenerated cellulose, or starch may be used.
[0407] In addition, the solubility of cellulose derivatives such as carboxymethyl cellulose can be increased by converting them into salts such as sodium or ammonium salts of carboxymethyl cellulose, making them more effective as viscosity adjusters. Higher solubility can also improve dispersibility with the active material and other components when preparing electrode slurry. In this specification, the cellulose and cellulose derivatives used as electrode binders also include their salts.
[0408] Water-soluble polymers stabilize viscosity by dissolving in water, and can stably disperse active materials or other materials combined as binders, such as styrene-butadiene rubber, in aqueous solutions. Furthermore, their functional groups are expected to facilitate stable adsorption to the surface of active materials. Furthermore, many cellulose derivatives, such as carboxymethyl cellulose, contain functional groups, such as hydroxyl or carboxyl groups, and the functional groups are expected to allow interactions between polymers, resulting in widespread coverage of the active material surface.
[0409] When the binder covering or contacting the surface of the active material forms a film, it is expected to function as a passive film and have the effect of suppressing decomposition of the electrolyte. Here, the passive film is a film with no electrical conductivity or a film with extremely low electrical conductivity. For example, when a passive film is formed on the surface of the active material, it can suppress decomposition of the electrolyte at the battery reaction potential. Furthermore, it is more desirable that the passive film suppresses electrical conductivity while still allowing lithium ions to conduct.
[0410] <Positive Electrode Current Collector> As the positive electrode current collector, a highly conductive material such as a metal such as stainless steel, gold, platinum, aluminum, or titanium, or an alloy thereof, can be used. When aluminum is used for the positive electrode current collector, a thermite reaction between the positive electrode active material and aluminum may occur when the secondary battery becomes hot due to an abnormality such as an internal short circuit. Once the thermite reaction has begun, it is difficult to stop it midway, and there is a risk that the secondary battery may ignite and experience thermal runaway. The positive electrode active material composite 100α, which is one embodiment of the present invention, can suppress the thermite reaction with aluminum, i.e., suppress thermal runaway, even if an abnormality occurs.
[0411] The material used for the positive electrode current collector is preferably one that does not dissolve at the potential of the positive electrode. Aluminum alloys containing elements that improve heat resistance, such as silicon, titanium, neodymium, scandium, and molybdenum, can also be used. The positive electrode current collector may also be made of a metal element that reacts with silicon to form a silicide. Metal elements that react with silicon to form a silicide include zirconium, titanium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten, cobalt, and nickel.
[0412] The positive electrode current collector may be in any suitable shape, such as a foil, plate, sheet, mesh, punched metal, expanded metal, etc. The current collector preferably has a thickness of 5 μm to 30 μm.
[0413] [Negative Electrode] The negative electrode has a negative electrode active material layer and a negative electrode current collector. The negative electrode active material layer has a negative electrode active material, and may further have a conductive additive and a binder.
[0414] <Negative Electrode Active Material> As the negative electrode active material, for example, an alloy material, a carbon material, or a mixture thereof can be used.
[0415] Examples of the carbon material that can be used include graphite, easily graphitizable carbon (soft carbon), non-graphitizable carbon (hard carbon), carbon nanotubes, graphene, and carbon black.
[0416] Examples of graphite include artificial graphite and natural graphite, and one or more selected from these can be used. The interplanar spacing d(002) of the (002) plane of the graphite structure is preferably 0.335 nm or more and 0.337 nm or less, and the interplanar spacing d(002) can typically be determined by powder X-ray diffraction. Graphite that does not fall within this range may not provide good discharge capacity and / or charge capacity.
[0417] Examples of artificial graphite include mesocarbon microbeads (MCMB), coke-based artificial graphite, and pitch-based artificial graphite. Artificial graphite can be made to have a spherical shape, which is called spherical graphite. MCMB may have a spherical shape and is preferred as spherical graphite. MCMB is also relatively easy to reduce its surface area. If the specific surface area is large, the decomposition reaction with the electrolyte on the surface of the negative electrode active material becomes large, and good cycle characteristics may not be obtained. In order to suppress the decomposition reaction, the specific surface area of the carbon material, specifically, the specific surface area that MCMB satisfies as a powder characteristic, is 0.8 m as measured by the BET method (Brunauer Emmett Teller method). 2 / g or more 8m 2 / g, preferably 1m 2 / g or more 4.8m 2 / g is preferably satisfied. The BET method is an analytical technique that extends the Langmuir theory to multilayer adsorption of adsorbed gas molecules, and is the most common method for calculating specific surface area. The BET specific surface area can be measured using an automatic specific surface area measuring device, Tristar 2 3020.
[0418] If the particle diameter (D50) is small, the carbon material becomes bulky and may hinder the improvement of electrode density. Therefore, the median diameter (D50) of the carbon material, specifically, the median diameter (D50) that MCMB satisfies as a powder characteristic, should be 3 μm or more and 25 μm or less, preferably 5 μm or more and 10 μm or less. The median diameter (D50) is typically measured by laser diffraction.
[0419] Examples of natural graphite include flake graphite and spheroidized natural graphite. The flake graphite can be pulverized with a pulverizer to adjust the median diameter (D50). The median diameter (D50) is preferably 3 μm or more and 25 μm or less, and more preferably 5 μm or more and 10 μm or less. Natural graphite may also be subjected to a spheroidization treatment. If the specific surface area is large, the decomposition reaction with the electrolyte on the surface of the negative electrode active material may become large, and good cycle characteristics may not be obtained. The specific surface area that natural graphite satisfies as a powder characteristic to suppress the decomposition reaction is 0.8 m as measured by the BET method (Brunauer Emmett Teller method). 2 / g or more 8m 2 / g, preferably 1m 2 / g or more 4.8m 2 It is preferable that the above condition is satisfied.
[0420] When lithium ions are inserted into graphite (when a lithium-graphite intercalation compound is formed), the graphite exhibits a potential as low as that of metallic lithium (0.01 V to 0.3 V vs. Li / Li + This allows lithium-ion secondary batteries using graphite to exhibit high operating voltages. Graphite is also preferred because it has advantages such as a relatively high capacity per unit volume, relatively small volume expansion, low cost, and greater safety than metallic lithium.
[0421] As the alloying material, an element capable of undergoing a charge-discharge reaction by alloying / de-alloying reaction with lithium can be used. For example, a material containing at least one of silicon, tin, gallium, aluminum, germanium, lead, antimony, bismuth, silver, zinc, cadmium, indium, etc. can be used. Such elements have a larger capacity than carbon, and silicon in particular has a high theoretical capacity of 4200 mAh / g per active material weight. For this reason, it is preferable to use silicon as the negative electrode active material. Alternatively, a compound containing these elements may be used. For example, SiO, Mg 2 Si, Mg 2 Ge, SnO, SnO 2 , Mg 2 Sn, SnS 2 , V 2 Sn 3 , FeSn 2 , CoSn 2 , Ni 3 Sn 2 , Cu 6 Sn 5 , Ag 3 Sn, Ag 3 Sb, Ni 2 MnSb, CeSb 3 , LaSn 3 , La 3 Co 2 Sn 7 , CoSb 3 , InSb, SbSn, etc. Elements capable of undergoing charge-discharge reactions by alloying / dealloying reactions with lithium, and compounds containing such elements, are called alloy materials.
[0422] In this specification and the like, SiO refers to, for example, silicon monoxide. Alternatively, SiO refers to SiO x Here, x preferably has a value of 1 or close to 1. For example, x is preferably 0.2 or more and 1.5 or less, and more preferably 0.3 or more and 1.2 or less.
[0423] Titanium dioxide (TiO 2 ), lithium titanium oxide (Li 4 Ti 5 O 12 ), lithium-graphite intercalation compound (Lix C 6 ), niobium pentoxide (Nb 2 O 5 ), tungsten dioxide (WO 2 ), molybdenum dioxide (MoO 2 ) and other oxides can be used.
[0424] In addition, as the negative electrode active material, a nitride of lithium and a transition metal, Li 3 Li with N-type structure 3−x M x N (M=Co, Ni, Cu) can be used. For example, Li 2.6 Co 0.4 N has a large discharge capacity (900 mAh / g, 1890 mAh / cm per active material weight) 3 ) and is preferred.
[0425] When a nitride of lithium and a transition metal is used, lithium ions are contained in the negative electrode active material, so V, which does not contain lithium ions, is used as the positive electrode active material. 2 O 5 , Cr 3 O 8 It is preferable that the material can be combined with a material such as the above. Even when a material containing lithium ions is used as the positive electrode active material, it is possible to use a nitride of lithium and a transition metal as the negative electrode active material by first desorbing the lithium ions contained in the positive electrode active material.
[0426] Furthermore, a material that undergoes a conversion reaction can also be used as the negative electrode active material. For example, a transition metal oxide that does not form an alloy with lithium, such as cobalt oxide (CoO), nickel oxide (NiO), or iron oxide (FeO), can be used as the negative electrode active material. Further examples of materials that undergo a conversion reaction include Fe 2 O 3 ,CuO,Cu 2 O, RuO 2 , Cr 2 O 3 oxides such as CoS 0.89 , sulfides such as NiS and CuS, Zn 3 N 2 , Cu 3 N, Ge 3 N 4 Nitrides such as NiP2 , FeP 2 , CoP 3 Phosphides such as FeF 3 , BiF 3 This also occurs with fluorides such as
[0427] As the conductive additive and binder that can be contained in the negative electrode active material layer, the same materials as the conductive additive and binder that can be contained in the positive electrode active material layer can be used.
[0428] <Negative electrode current collector> In addition to the same materials as the positive electrode current collector, copper and the like can be used for the negative electrode current collector. However, aluminum cannot be used for the negative electrode current collector. It is preferable to use a material that does not alloy with carrier ions such as lithium for the negative electrode current collector.
[0429] [Separator] A separator is disposed between the positive electrode and the negative electrode. Examples of separators that can be used include those made of cellulose-containing fibers such as paper, nonwoven fabrics, glass fibers, ceramics, or synthetic fibers such as nylon (polyamide), vinylon (polyvinyl alcohol-based fibers), polyester, acrylic, polyolefin, and polyurethane. The separator is preferably processed into a bag shape and disposed so as to encase either the positive electrode or the negative electrode.
[0430] The separator may have a multilayer structure. For example, an organic film such as polypropylene or polyethylene may be coated with a ceramic material, a fluorine-based material, a polyamide material, or a mixture of these. Examples of ceramic materials include aluminum oxide particles and silicon oxide particles. Examples of fluorine-based materials include PVDF and polytetrafluoroethylene. Examples of polyamide materials include nylon and aramid (meta-aramid, para-aramid).
[0431] Coating with ceramic materials improves oxidation resistance, suppressing separator degradation during high-voltage charging and discharging and improving the reliability of secondary batteries. Coating with fluorine-based materials also improves adhesion between the separator and electrodes, improving output characteristics. Coating with polyamide-based materials, especially aramid, improves heat resistance, improving the safety of secondary batteries.
[0432] For example, both sides of a polypropylene film may be coated with a mixed material of aluminum oxide and aramid, or the surface of the polypropylene film that contacts the positive electrode may be coated with a mixed material of aluminum oxide and aramid, and the surface that contacts the negative electrode may be coated with a fluorine-based material.
[0433] When a separator with a multilayer structure is used, the safety of the secondary battery can be maintained even if the overall thickness of the separator is thin, and therefore the capacity per volume of the secondary battery can be increased.
[0434] [Electrolyte] As one form of electrolyte, an electrolytic solution having a solvent and an electrolyte dissolved in the solvent can be used. As the solvent, an aprotic organic solvent is preferable, and for example, ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, chloroethylene carbonate, vinylene carbonate, γ-butyrolactone, γ-valerolactone, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, 1,3-dioxane, 1,4-dioxane, dimethoxyethane (DME), dimethyl sulfoxide, diethyl ether, methyl diglyme, acetonitrile, benzonitrile, tetrahydrofuran, sulfolane, sultone, etc. can be used alone or in any combination and ratio of two or more of them.
[0435] <Organic Solvent> As a more preferred solvent, an organic solvent using an organic compound containing fluorine will be described. Specific examples of organic compounds containing fluorine include fluorinated cyclic carbonates (sometimes referred to as fluorinated cyclic carbonates). Another example of an organic compound containing fluorine is a fluorinated chain carbonate (sometimes referred to as fluorinated chain carbonate). Both fluorinated cyclic carbonates and fluorinated chain carbonates have electron-withdrawing substituents. Organic compounds containing electron-withdrawing substituents have lower solvation energy of lithium ions than organic compounds without electron-withdrawing substituents. For this reason, fluorine-containing organic compounds are suitable for organic solvents, and such organic solvents can provide secondary batteries exhibiting good initial characteristics. It is more preferred that the organic solvent contains both a fluorinated cyclic carbonate and a fluorinated chain carbonate.
[0436] Examples of fluorinated cyclic carbonates that can be used include fluoroethylene carbonate (also called fluorinated ethylene carbonate or fluoroethylene carbonate, abbreviated as FEC or F1EC), difluoroethylene carbonate (abbreviated as DFEC or F2EC), trifluoroethylene carbonate (abbreviated as F3EC), tetrafluoroethylene carbonate (abbreviated as F4EC), and pentafluoroethylene carbonate (abbreviated as F5EC). DFEC includes isomers such as cis-4,5 and trans-4,5. Since all of the fluorinated cyclic carbonates have electron-withdrawing substituents, the solvation energy of lithium ions in organic solvents containing the fluorinated cyclic carbonates is thought to be low.
[0437] The structural formula of FEC is shown below in (H11): In FEC, the electron-withdrawing substituent is an F group.
[0438]
[0439] The structural formula of 4,5-difluoroethylene carbonate is shown below in (H12): In 4,5-difluoroethylene carbonate, the electron-withdrawing substituent is an F group.
[0440]
[0441] The structural formula of 4,4-difluoroethylene carbonate is shown below as (H13): In 4,4-difluoroethylene carbonate, the electron-withdrawing substituent is an F group.
[0442]
[0443] The structural formula of F3EC is shown below in (H14): In F3EC, the electron-withdrawing substituent is an F group.
[0444]
[0445] The structural formula of F4EC is shown below in (H15): In F4EC, the electron-withdrawing substituent is an F group.
[0446]
[0447] The above-mentioned fluorinated cyclic carbonates are sometimes collectively referred to as cyclic molecules.
[0448] Methyl trifluoropropionate is an example of a fluorinated chain carbonate, and a typical example is methyl 3,3,3-trifluoropropionate. The structural formula of methyl 3,3,3-trifluoropropionate is shown below in (H21). The abbreviation for methyl 3,3,3-trifluoropropionate is "MTFP." In MTFP, the electron-withdrawing substituent is CF 3 It is the base.
[0449]
[0450] An example of a fluorinated chain carbonate is methyl 2,2-difluoropropionate. The structural formula of methyl 2,2-difluoropropionate is shown below in (H22). In methyl 2,2-difluoropropionate, the electron-withdrawing substituent is CF 2 It is the base.
[0451]
[0452] An example of a fluorinated chain carbonate is trifluoromethyl propionate. The structural formula of trifluoromethyl propionate is shown below (H23). In trifluoromethyl propionate, the electron-withdrawing substituent is CF 3 It is the base.
[0453]
[0454] Methyl pentafluoropropionate is an example of a fluorinated chain carbonate. The structural formula of methyl pentafluoropropionate is shown below (H24). The electron-withdrawing substituent in methyl pentafluoropropionate is CF 3 It is the base.
[0455]
[0456] An example of a fluorinated chain carbonate is trifluoromethyl 3,3,3-trifluoropropionate. The structural formula of trifluoromethyl 3,3,3-trifluoropropionate is shown below in (H25). In trifluoromethyl 3,3,3-trifluoropropionate, the electron-withdrawing substituent is CF 3 It is the base.
[0457]
[0458] The above-mentioned fluorinated chain carbonates are sometimes collectively referred to as chain molecules.
[0459] The organic solvent preferably contains one or more selected from the above-mentioned fluorinated cyclic carbonates and one or more selected from the fluorinated chain carbonates. This makes it possible to provide a secondary battery that exhibits good initial characteristics. More preferably, the organic solvent contains both FEC and MTFP. The reason for this will be explained below.
[0460] <FEC and MTFP> FEC is a cyclic carbonate and has a high dielectric constant. Therefore, when FEC is used in an organic solvent, it exhibits the effect of promoting the dissociation of lithium salts. On the other hand, since FEC has an electron-withdrawing substituent, it is more likely to desolvate with lithium ions than ethylene carbonate (abbreviated as "EC"). Specifically, the solvation energy of lithium ions in FEC is smaller than that of EC that does not have an electron-withdrawing substituent. Therefore, it is easier to separate lithium ions from the surface of the positive electrode active material and the surface of the negative electrode active material, thereby reducing the internal resistance of the secondary battery. Furthermore, FEC is thought to have a deep highest occupied molecular orbital (HOMO) level and / or a lowest unoccupied molecular orbital (LUMO) level. A deep HOMO level is preferable because it is less susceptible to oxidation and improves the oxidation resistance of the electrolyte. On the other hand, FEC has a somewhat high viscosity, and using FEC alone as an organic solvent could result in high impedance. Therefore, it is recommended to use a mixed organic solvent containing MTFP in addition to FEC in the electrolyte. MTFP is a chain carbonate that exhibits the effect of reducing or maintaining viscosity. Maintaining viscosity is particularly necessary when the operating temperature of a secondary battery is low, but is also important at room temperature. MTFP also has electron-withdrawing substituents. Therefore, MTFP has a lower solvation energy than methyl propionate (abbreviated as "MP"), which does not have electron-withdrawing properties, but it may still form solvates with lithium ions.
[0461] The blending ratio of FEC and MTFP will be explained. The total content of FEC and MTFP, i.e., the total volume, is 100 vol%, and the volume ratio should be FEC:MTFP = y:100-y (where 5≦y≦30, preferably 10≦y≦20). In other words, it is preferable that the amount of MTFP is greater than that of FEC. An organic solvent containing FEC and MTFP exhibits an appropriate viscosity as an electrolyte. This allows for the provision of a secondary battery with good initial characteristics. Furthermore, because FEC and MTFP can maintain an appropriate viscosity as an electrolyte, the low-temperature characteristics of the secondary battery are improved.
[0462] The above volume ratio is measured before mixing as an organic solvent. Even if some volatilization occurs during mixing, it is not a problem as long as good initial properties can be exhibited. The organic solvent should be mixed at room temperature.
[0463] Although FEC has been described as a representative example above, any of the organic compounds described as fluorinated cyclic carbonates has the effect of promoting dissociation of lithium salts, is easily desolvated with lithium ions, and has a high viscosity that does not result in an appropriate viscosity when used alone. Furthermore, although MTFP has been described as a representative example above, any of the organic compounds described as fluorinated chain carbonates can also exhibit the effect of reducing or maintaining the viscosity of the electrolyte. Therefore, if the organic solvent contains a fluorinated cyclic carbonate and a fluorinated chain carbonate, a secondary battery exhibiting good initial characteristics can be provided.
[0464] The organic solvent described above is free from granular dust or molecules other than the constituent molecules of the organic solvent (hereinafter simply referred to as "impurities"), and oxygen (O 2 ), water (H 2 The electrolyte preferably contains a low content of 0 or water, and is highly purified. Specifically, the amount of impurities in the electrolyte is 100 ppm or less, preferably 50 ppm or less, and more preferably less than 10 ppm. The water concentration can be detected by Karl Fischer titration.
[0465] Furthermore, by using one or more flame-retardant and non-volatile ionic liquids (room-temperature molten salts) as the solvent for the electrolyte, it is possible to prevent the electricity storage device from exploding or catching fire even if the internal temperature rises due to an internal short circuit or overcharging of the electricity storage device. The ionic liquid is composed of a cation and an anion, and includes an organic cation and an anion. Examples of organic cations used in the electrolyte include aliphatic onium cations such as quaternary ammonium cations, tertiary sulfonium cations, and quaternary phosphonium cations, and aromatic cations such as imidazolium cations and pyridinium cations. Examples of anions used in the electrolyte include monovalent amide anions, monovalent methide anions, fluorosulfonate anions, perfluoroalkylsulfonate anions, tetrafluoroborate anions, perfluoroalkylborate anions, hexafluorophosphate anions, and perfluoroalkylphosphate anions.
[0466] The electrolyte to be dissolved in the solvent is, for example, LiPF 6 , LiClO 4 , LiAsF 6 , LiBF 4 , LiAlCl 4 , LiSCN, LiBr, LiI, Li 2 SO 4 , Li 2 B 10 Cl 10 , Li 2 B 12 Cl 12 , LiCF 3 SO 3 , LiC 4 F 9 SO 3 , LiC(CF 3 SO 2 ) 3 , LiC(C 2 F 5 SO 2 ) 3 , LiN(CF 3 SO 2 ) 2 , LiN(C 4 F 9 SO 2 ) (CF 3 SO2 ), LiN(C 2 F 5 SO 2 ) 2 , lithium bis(oxalato)borate (Li(C) 2 O 4 ) 2 , LiBOB), or two or more of these can be used in any combination and ratio.
[0467] The electrolyte used in the electricity storage device is preferably a highly purified electrolyte with a low content of granular waste or elements other than the constituent elements of the electrolyte (hereinafter simply referred to as "impurities"). Specifically, the weight ratio of impurities to the electrolyte is preferably 1% or less, preferably 0.1% or less, and more preferably 0.01% or less.
[0468] Alternatively, a polymer gel electrolyte may be used in which a polymer is swollen with an electrolytic solution.
[0469] The use of a polymer gel electrolyte improves safety against leakage, etc. It also enables the secondary battery to be made thinner and lighter.
[0470] Examples of polymers that can be gelled include silicone gel, acrylic gel, acrylonitrile gel, polyethylene oxide gel, polypropylene oxide gel, and fluorine-based polymer gel. For example, polymers having a polyalkylene oxide structure such as polyethylene oxide (PEO), PVDF, polyacrylonitrile, and copolymers containing these can be used. For example, PVDF-HFP, a copolymer of PVDF and hexafluoropropylene (HFP), can be used. The polymer formed may also have a porous shape.
[0471] In addition, the electrolyte can be a solid electrolyte containing an inorganic material such as a sulfide or oxide, or a solid electrolyte containing a polymer material such as a polyethylene oxide (PEO)-based material. When a solid electrolyte is used, the installation of a separator or spacer is unnecessary. Furthermore, since the entire battery can be solidified, the risk of leakage is eliminated, dramatically improving safety.
[0472] Therefore, the positive electrode active material composite 100α obtained in the first embodiment can be applied to an all-solid-state battery. By applying the positive electrode slurry or electrode to an all-solid-state battery, an all-solid-state battery with high safety and excellent characteristics can be obtained.
[0473] <Additives> For the purpose of improving safety, it is preferable to mix an additive with the organic solvent. The additive is preferably one or more selected from vinylene carbonate (VC), propane sultone (PS), tert-butylbenzene (TBB), fluoroethylene carbonate (FEC), lithium bis(oxalate)borate (LiBOB), SUN (suberonitrile), or a dinitrile compound such as succinonitrile or adiponitrile. The concentration of the additive is preferably, for example, 0.1 wt% to 5 wt% of the total organic solvent. The electrolyte according to one embodiment of the present invention does not need to contain the additive. It is also preferable to select an organic compound different from the organic solvent as the additive.
[0474] [Exterior Body] The exterior body of the secondary battery can be made of a metal material such as aluminum or a resin material. Alternatively, a film-like exterior body can be used. Examples of the film include a three-layer structure film in which a thin, flexible metal film such as aluminum, stainless steel, copper, or nickel is provided on a film made of a material such as polyethylene, polypropylene, polycarbonate, ionomer, or polyamide, and an insulating synthetic resin film such as a polyamide resin or polyester resin is further provided on the thin metal film as the outer surface of the exterior body.
[0475] The contents described in this embodiment can be combined with the contents described in other embodiments.
[0476] Embodiment Mode 5 In this embodiment mode, examples of various shapes of secondary batteries each having a positive electrode or a negative electrode manufactured by the manufacturing method described in the previous embodiment will be described.
[0477] [Coin-Type Secondary Battery] An example of a coin-type secondary battery will be described. Fig. 20A is an exploded perspective view of a coin-type (single-layer flat) secondary battery, Fig. 20B is an external view, and Fig. 20C is a cross-sectional view thereof. Coin-type secondary batteries are mainly used in small electronic devices. In this specification, coin-type batteries include button-type batteries.
[0478] 20A is a schematic diagram that shows the overlapping of components (upper and lower relationships and positional relationships) for ease of understanding. Therefore, FIG. 20A and FIG. 20B are not completely identical corresponding views.
[0479] In Fig. 20A, a positive electrode 304, a separator 310, a negative electrode 307, a spacer 322, and a washer 312 are stacked. These are sealed by a negative electrode can 302 and a positive electrode can 301. Note that a gasket for sealing is not shown in Fig. 20A. The spacer 322 and the washer 312 are used to protect the inside or to fix the position inside the can when the positive electrode can 301 and the negative electrode can 302 are crimped together. The spacer 322 and the washer 312 are made of stainless steel or an insulating material.
[0480] A positive electrode 304 has a laminated structure in which a positive electrode active material layer 306 is formed on a positive electrode current collector 305 .
[0481] To prevent short-circuiting between the positive electrode and the negative electrode, a separator 310 and a ring-shaped insulator 313 are arranged so as to cover the side and top surfaces of the positive electrode 304. The separator 310 has a larger planar area than the positive electrode 304.
[0482] FIG. 20B is a perspective view of the completed coin-type secondary battery.
[0483] In the coin-type secondary battery 300, a positive electrode can 301, which also serves as a positive electrode terminal, and a negative electrode can 302, which also serves as a negative electrode terminal, are insulated and sealed by a gasket 303 made of polypropylene or the like. The positive electrode 304 is formed by a positive electrode current collector 305 and a positive electrode active material layer 306 provided in contact with the positive electrode current collector. The negative electrode 307 is formed by a negative electrode current collector 308 and a negative electrode active material layer 309 provided in contact with the negative electrode current collector. The negative electrode 307 is not limited to a laminated structure, and may be formed of lithium metal foil or a lithium-aluminum alloy foil.
[0484] It is preferable that the positive electrode 304 and the negative electrode 307 used in the coin-type secondary battery 300 each have an active material layer formed on only one surface.
[0485] The positive electrode can 301 and the negative electrode can 302 can be made of a metal such as nickel, aluminum, or titanium that is corrosion-resistant to the electrolyte, or an alloy of these metals, or an alloy of these metals with other metals (e.g., stainless steel). Furthermore, to prevent corrosion by the electrolyte, etc., it is preferable to coat them with nickel, aluminum, etc. The positive electrode can 301 is electrically connected to the positive electrode 304, and the negative electrode can 302 is electrically connected to the negative electrode 307.
[0486] These negative electrode 307, positive electrode 304, and separator 310 are immersed in an electrolyte solution, and as shown in FIG. 20C , the positive electrode 304, separator 310, negative electrode 307, and negative electrode can 302 are stacked in this order with the positive electrode can 301 facing downwards, and the positive electrode can 301 and the negative electrode can 302 are crimped together via a gasket 303, thereby producing a coin-type secondary battery 300.
[0487] The above-described configuration allows the coin-type secondary battery 300 to have a high capacity, a high discharge capacity, and excellent cycle characteristics. Note that, when a secondary battery having a solid electrolyte between the negative electrode 307 and the positive electrode 304 is used, the separator 310 may be unnecessary.
[0488] [Cylindrical Secondary Battery] An example of a cylindrical secondary battery will be described with reference to Fig. 21A. As shown in Fig. 21A, a cylindrical secondary battery 616 has a positive electrode cap (battery lid) 601 on the top surface and a battery can (external can) 602 on the side and bottom surfaces. The positive electrode cap 601 and the battery can (external can) 602 are insulated by a gasket (insulating packing) 610.
[0489] 21B is a schematic diagram showing a cross section of a cylindrical secondary battery. The cylindrical secondary battery shown in Fig. 21B has a positive electrode cap (battery lid) 601 on the top surface and a battery can (external can) 602 on the side and bottom surfaces. The positive electrode cap and battery can (external can) 602 are insulated by a gasket (insulating packing) 610.
[0490] A battery element is provided inside a hollow cylindrical battery can 602, in which a strip-shaped positive electrode 604 and a negative electrode 606 are wound with a separator 605 sandwiched between them. Although not shown, the battery element is wound around a central axis. One end of the battery can 602 is closed and the other end is open. The battery can 602 can be made of a metal, such as nickel, aluminum, or titanium, or an alloy thereof, or an alloy of these with another metal (e.g., stainless steel), which is corrosion-resistant to the electrolyte. Furthermore, it is preferable to coat the battery can 602 with nickel, aluminum, or the like to prevent corrosion by the electrolyte. Inside the battery can 602, the wound battery element, in which the positive electrode, negative electrode, and separator are wound, is sandwiched between a pair of opposing insulating plates 608 and 609. A nonaqueous electrolyte (not shown) is poured into the battery can 602, in which the battery element is provided. The nonaqueous electrolyte may be the same as that used in coin-type secondary batteries.
[0491] Since the positive and negative electrodes used in a cylindrical storage battery are wound, it is preferable to form active materials on both sides of the current collector. While the secondary battery 616 shown in Figures 21A to 21D has a cylinder whose height is greater than its diameter, this is not limiting. A secondary battery whose diameter is greater than its height may also be used. This configuration, for example, can reduce the size of the secondary battery.
[0492] By using the positive electrode active material composite 100α obtained in Embodiment 1 for the positive electrode 604, a cylindrical secondary battery 616 having a high capacity, a high discharge capacity, and excellent cycle characteristics can be obtained.
[0493] A positive electrode terminal (positive electrode current collecting lead) 603 is connected to the positive electrode 604, and a negative electrode terminal (negative electrode current collecting lead) 607 is connected to the negative electrode 606. The positive electrode terminal 603 can be made of a metal material such as aluminum, and the negative electrode terminal 607 can be made of a metal material such as copper. The positive electrode terminal 603 is resistance-welded to a safety valve mechanism 613, and the negative electrode terminal 607 is resistance-welded to the bottom of the battery can 602. The safety valve mechanism 613 is electrically connected to the positive electrode cap 601 via a PTC (Positive Temperature Coefficient) element 611. The safety valve mechanism 613 cuts off the electrical connection between the positive electrode cap 601 and the positive electrode 604 when the increase in internal pressure of the battery exceeds a predetermined threshold. The PTC element 611 is a thermosensitive resistor whose resistance increases when the temperature rises, and the increase in resistance limits the amount of current to prevent abnormal heat generation. 3 )-based semiconductor ceramics, etc. can be used.
[0494] 21C shows an example of a power storage system 615. The power storage system 615 has a plurality of secondary batteries 616. The positive electrodes of each secondary battery are in contact with and electrically connected to conductors 624 separated by insulators 625. The conductors 624 are electrically connected to a control circuit 620 via wiring 623. The negative electrodes of each secondary battery are electrically connected to the control circuit 620 via wiring 626. A protection circuit or the like that prevents overcharging or overdischarging can be used as the control circuit 620.
[0495] 21D shows an example of a power storage system 615. The power storage system 615 has a plurality of secondary batteries 616, which are sandwiched between a conductive plate 628 and a conductive plate 614. The plurality of secondary batteries 616 are electrically connected to the conductive plate 628 and the conductive plate 614 by wiring 627. The plurality of secondary batteries 616 may be connected in parallel, in series, or in parallel and then further connected in series. By configuring the power storage system 615 to have a plurality of secondary batteries 616, it is possible to extract a large amount of power.
[0496] A plurality of secondary batteries 616 may be connected in parallel and then further connected in series.
[0497] A temperature control device may be provided between the multiple secondary batteries 616. When the secondary batteries 616 are overheated, they can be cooled by the temperature control device, and when the secondary batteries 616 are too cold, they can be heated by the temperature control device. This makes it difficult for the performance of the power storage system 615 to be affected by the outside air temperature.
[0498] 21D , the power storage system 615 is electrically connected to a control circuit 620 via wiring 621 and wiring 622. The wiring 621 is electrically connected to the positive electrodes of the plurality of secondary batteries 616 via a conductive plate 628, and the wiring 622 is electrically connected to the negative electrodes of the plurality of secondary batteries 616 via a conductive plate 614.
[0499] [Another Structural Example of Secondary Battery] Structural examples of secondary batteries will be described with reference to FIGS. 22 and 23. FIG.
[0500] The secondary battery 913 shown in FIG. 22A has a wound body 950 provided with terminals 951 and 952 inside a housing 930. The wound body 950 is immersed in an electrolyte inside the housing 930. The terminal 952 contacts the housing 930, and the terminal 951 is not in contact with the housing 930 by using an insulating material or the like. Note that in FIG. 22A , for convenience, the housing 930 is shown separated, but in reality, the wound body 950 is covered by the housing 930, and the terminals 951 and 952 extend outside the housing 930. The housing 930 can be made of a metal material (e.g., aluminum) or a laminate of a metal material and a resin material.
[0501] 22B, the housing 930 shown in Fig. 22A may be formed from a plurality of materials. For example, the secondary battery 913 shown in Fig. 22B has a housing 930a and a housing 930b bonded together, and a wound body 950 is provided in the area surrounded by the housing 930a and the housing 930b.
[0502] The housing 930a can be made of a metal material (such as aluminum) or a laminate of a metal material and a resin material. By using a resin material on the surface on which the antenna is formed, it is possible to prevent the secondary battery 913 from blocking the electric field. Note that if the electric field blocking by the housing 930a is small, the antenna may be provided inside the housing 930a. The housing 930b can be made of a metal material (such as aluminum) or a laminate of a metal material and a resin material.
[0503] 22C shows the structure of the wound body 950. The wound body 950 has a negative electrode 931, a positive electrode 932, and a separator 933. The wound body 950 is a wound body in which the negative electrode 931 and the positive electrode 932 are stacked on top of each other with the separator 933 sandwiched therebetween, and the laminated sheet is wound. Note that multiple layers of the negative electrode 931, the positive electrode 932, and the separator 933 may be stacked.
[0504] 23A to 23C may be used as a secondary battery 913 having a wound body 950a. The wound body 950a shown in Fig. 23A includes a negative electrode 931, a positive electrode 932, and a separator 933. The negative electrode 931 includes a negative electrode active material layer 931a. The positive electrode 932 includes a positive electrode active material layer 932a.
[0505] By using the positive electrode active material composite 100α obtained in Embodiment 1 for the positive electrode 932, the secondary battery 913 can have a high capacity, a high discharge capacity, and excellent cycle characteristics.
[0506] The separator 933 has a width wider than the negative electrode active material layer 931 a and the positive electrode active material layer 932 a, and is wound so as to overlap the negative electrode active material layer 931 a and the positive electrode active material layer 932 a. From the standpoint of safety, it is preferable that the negative electrode active material layer 931 a be wider than the positive electrode active material layer 932 a. A wound body 950 a having such a shape is preferable due to its high safety and productivity.
[0507] As shown in Fig. 23B, the negative electrode 931 in Fig. 23A is electrically connected to a terminal 951. The terminal 951 is electrically connected to a terminal 911a. The positive electrode 932 in Fig. 23A is electrically connected to a terminal 952. The terminal 952 is electrically connected to a terminal 911b.
[0508] 23C , the wound body 950 a and the electrolyte are covered by the housing 930 to form the secondary battery 913. It is preferable to provide the housing 930 with a safety valve, an overcurrent protection element, etc. The safety valve is a valve that opens when the inside of the housing 930 reaches a predetermined internal pressure to prevent the battery from exploding.
[0509] As shown in Fig. 23B, the secondary battery 913 may have multiple wound bodies 950a. Using multiple wound bodies 950a can result in a secondary battery 913 with a larger discharge capacity. For other elements of the secondary battery 913 shown in Figs. 23A and 23B, refer to the descriptions of the secondary battery 913 shown in Figs. 22A to 22C.
[0510] 24A and 24B show examples of external views of a laminated secondary battery, which includes a positive electrode 503, a negative electrode 506, a separator 507, an outer casing 509, a positive electrode lead electrode 510, and a negative electrode lead electrode 511.
[0511] 25A shows an external view of a positive electrode 503 and a negative electrode 506. The positive electrode 503 has a positive electrode current collector 501, and a positive electrode active material layer 502 is formed on the surface of the positive electrode current collector 501. The positive electrode 503 also has a region where the positive electrode current collector 501 is partially exposed (hereinafter referred to as a tab region). The negative electrode 506 has a negative electrode current collector 504, and a negative electrode active material layer 505 is formed on the surface of the negative electrode current collector 504. The negative electrode 506 also has a region where the negative electrode current collector 504 is partially exposed, i.e., a tab region. The areas and shapes of the tab regions of the positive electrode and negative electrode are not limited to the example shown in FIG. 25A .
[0512] <Method of Manufacturing Laminated Secondary Battery> Here, an example of a method of manufacturing the laminated secondary battery whose external view is shown in FIG. 24A will be described with reference to FIGS. 25A to 25C.
[0513] First, the negative electrode 506, separator 507, and positive electrode 503 are stacked. FIG. 25B shows the stacked negative electrode 506, separator 507, and positive electrode 503. Here, an example is shown in which five pairs of negative electrodes and four pairs of positive electrodes are used. This can also be called a laminate consisting of a negative electrode, a separator, and a positive electrode. Next, the tab regions of the positive electrodes 503 are joined together, and the positive electrode lead electrode 510 is joined to the tab region of the outermost positive electrode. For example, ultrasonic welding or the like may be used for joining. Similarly, the tab regions of the negative electrodes 506 are joined together, and the negative electrode lead electrode 511 is joined to the tab region of the outermost negative electrode.
[0514] Next, the negative electrode 506 , the separator 507 and the positive electrode 503 are arranged on the outer casing 509 .
[0515] Next, as shown in Fig. 25C, the exterior body 509 is folded at the portion indicated by the dashed line. Thereafter, the outer periphery of the exterior body 509 is joined. For example, thermocompression bonding or the like may be used for joining. At this time, an area (hereinafter referred to as an inlet) that is not joined is provided in a part (or one side) of the exterior body 509 so that an electrolyte can be introduced later.
[0516] Next, an electrolyte solution (not shown) is introduced into the inside of the exterior body 509 through an inlet provided in the exterior body 509. The introduction of the electrolyte solution is preferably carried out under a reduced pressure atmosphere or an inert atmosphere. Finally, the inlet is joined. In this manner, the laminated secondary battery 500 can be produced.
[0517] By using the positive electrode active material composite 100α obtained in Embodiment 1 for the positive electrode 503, the secondary battery 500 can have a high capacity, a high discharge capacity, and excellent cycle characteristics.
[0518] [Example of Battery Pack] An example of a secondary battery pack according to one embodiment of the present invention that can be wirelessly charged using an antenna will be described with reference to FIGS. 26A to 26C.
[0519] Fig. 26A is a diagram showing the appearance of secondary battery pack 531, which has a thin rectangular parallelepiped shape (also called a thick flat plate shape). Fig. 26B is a diagram illustrating the configuration of secondary battery pack 531. Secondary battery pack 531 has circuit board 540 and secondary battery 513. Label 529 is affixed to secondary battery 513. Circuit board 540 is fixed with sticker 515. Secondary battery pack 531 also has antenna 517.
[0520] The interior of the secondary battery 513 may have a structure including a wound body or a laminated body.
[0521] 26B , the secondary battery pack 531 has a control circuit 590 on a circuit board 540. The circuit board 540 is electrically connected to the terminals 514. The circuit board 540 is also electrically connected to the antenna 517, one 551 of the positive electrode lead and the negative electrode lead of the secondary battery 513, and the other 552 of the positive electrode lead and the negative electrode lead of the secondary battery 513.
[0522] Alternatively, as shown in FIG. 26C, the device may have a circuit system 590 a provided on a circuit board 540 and a circuit system 590 b electrically connected to the circuit board 540 via a terminal 514 .
[0523] The antenna 517 is not limited to a coil shape, and is preferably a wire or plate shape, for example. It is also preferable to use an antenna such as a planar antenna, an aperture antenna, a traveling wave antenna, an EH antenna, a magnetic field antenna, or a dielectric antenna. Alternatively, it is preferable to use a flat conductor for the antenna 517. This flat conductor can function as one of the conductors for electric field coupling. In other words, the antenna 517 can function as one of the two conductors of a capacitor. This allows power to be exchanged not only by electromagnetic fields and magnetic fields, but also by electric fields.
[0524] The secondary battery pack 531 includes a layer 519 between the antenna 517 and the secondary battery 513. The layer 519 has a function of, for example, shielding an electromagnetic field generated by the secondary battery 513. The layer 519 can be formed using, for example, a magnetic material.
[0525] The content of this embodiment mode can be freely combined with the content of other embodiment modes.
[0526] Sixth Embodiment In this embodiment, an example of fabricating an all-solid-state battery using the positive electrode active material composite 100α obtained in the first embodiment will be described.
[0527] As shown in FIG. 27A , a secondary battery 400 of one embodiment of the present invention includes a positive electrode 410 , a solid electrolyte layer 420 , and a negative electrode 430 .
[0528] The positive electrode 410 includes a positive electrode current collector 413 and a positive electrode active material layer 414. The positive electrode active material layer 414 includes a positive electrode active material 411 and a solid electrolyte 421. The positive electrode active material 411 is formed using the positive electrode active material composite 100α obtained in Embodiment 1. The positive electrode active material layer 414 may include a conductive additive and a binder.
[0529] Solid electrolyte layer 420 includes solid electrolyte 421. Solid electrolyte layer 420 is located between positive electrode 410 and negative electrode 430, and is a region that does not include either positive electrode active material 411 or negative electrode active material 431.
[0530] The negative electrode 430 includes a negative electrode current collector 433 and a negative electrode active material layer 434. The negative electrode active material layer 434 includes a negative electrode active material 431 and a solid electrolyte 421. The negative electrode active material layer 434 may also include a conductive additive and a binder. Note that when metallic lithium is used as the negative electrode active material 431, it is not necessary to form the material into particles, and therefore the negative electrode 430 can be formed without the solid electrolyte 421, as shown in FIG. 27B . Using metallic lithium for the negative electrode 430 is preferable because it can improve the energy density of the secondary battery 400.
[0531] The solid electrolyte 421 of the solid electrolyte layer 420 may be, for example, a sulfide-based solid electrolyte, an oxide-based solid electrolyte, or a halide-based solid electrolyte.
[0532] The sulfide-based solid electrolytes include thiolithium-based (Li 10 GeP 2 S 12 , Li 3.25 Ge 0.25 P 0.75 S 4etc.), sulfide glass (70Li 2 S・30P 2 S 5 , 30Li 2 S・26B 2 S 3 ・44LiI, 63Li2 S ・36SiS 2 ・1Li 3 P.O. 4 , 57Li 2 S・38SiS 2 ・5Li 4 SiO 4 , 50Li 2 S・50GeS 2 etc.), sulfide crystallized glass (Li 7 P 3 S 11 , Li 3.25 P 0.95 S 4 Sulfide-based solid electrolytes have the advantages of being highly conductive, being able to be synthesized at low temperatures, and being relatively soft, which makes it easy to maintain conductive paths even after charging and discharging.
[0533] The oxide-based solid electrolyte includes a material having a perovskite crystal structure (La 2/3−x Li 3x TiO 3 etc.), materials having a NASICON type crystal structure (Li 1−Y Al Y Ti 2−Y (P.O. 4 ) 3 etc.), materials having a garnet-type crystal structure (Li 7 La 3 Zr 2 O 12 etc.), materials having a LISICON type crystal structure (Li 14 ZnGe 4 O 16 etc.), LLZO (Li 7 La 3 Zr 2 O 12 ), oxide glass (Li 3 P.O. 4 -Li 4 SiO 4 , 50Li 4 SiO 4 ・50Li3 BO 3 etc.), oxide crystallized glass (Li 1.07 Al 0.69 Ti 1.46 (P.O. 4 ) 3 , Li 1.5 Al 0.5 Ge 1.5 (P.O. 4 ) 3 Oxide-based solid electrolytes have the advantage of being stable in the atmosphere.
[0534] Halide-based solid electrolytes include LiAlCl 4 , Li 3 InBr 6 , LiF, LiCl, LiBr, LiI, etc. Composite materials in which these halide-based solid electrolytes are filled into the pores of porous aluminum oxide or porous silica can also be used as the solid electrolyte.
[0535] Also, different solid electrolytes may be mixed and used.
[0536] Among them, Li having a NASICON type crystal structure 1+x Al x Ti 2−x (P.O. 4 ) 3 (0<x<1) (hereinafter, LATP) is preferable because it contains aluminum and titanium, elements that may be contained in the positive electrode active material used in the secondary battery 400 of one embodiment of the present invention, and therefore a synergistic effect can be expected in improving cycle characteristics. In addition, productivity can be expected to be improved by reducing the number of steps. Note that in this specification and the like, the NASICON-type crystal structure refers to a structure having a NASICON-type crystal structure, which is a structure having a NASICON-type crystal structure, and which is ... 2 (XO 4 ) 3 (M: transition metal, X: S, P, As, Mo, W, etc.), 6 Octahedron and XO 4 It refers to a structure in which tetrahedrons are arranged three-dimensionally with their vertices shared.
[0537] [Exterior Body and Shape of Secondary Battery] The exterior body of the secondary battery 400 of one embodiment of the present invention can be made of various materials and has various shapes, but preferably has a function of applying pressure to the positive electrode, the solid electrolyte layer, and the negative electrode.
[0538] For example, FIG. 28 shows an example of a cell for evaluating materials for an all-solid-state battery.
[0539] 28A is a cross-sectional schematic diagram of the evaluation cell, which has a lower member 761, an upper member 762, and a fixing screw or wing nut 764 that fixes them together, and electrode plate 753 is pressed to fix the evaluation material by rotating a holding screw 763. An insulator 766 is provided between lower member 761 and upper member 762, both made of stainless steel. An O-ring 765 is also provided between upper member 762 and holding screw 763 to provide a tight seal.
[0540] The evaluation material is placed on electrode plate 751, surrounded by insulating tube 752, and pressed from above by electrode plate 753. Figure 28B is an enlarged perspective view of the evaluation material and its surroundings.
[0541] The evaluation material is an example of a laminate of a positive electrode 750a, a solid electrolyte layer 750b, and a negative electrode 750c, and its cross-sectional view is shown in Fig. 28C. Note that the same reference numerals are used for the same parts in Figs. 28A to 28C.
[0542] The electrode plate 751 and the lower member 761, which are electrically connected to the positive electrode 750a, can be said to correspond to a positive electrode terminal. The electrode plate 753 and the upper member 762, which are electrically connected to the negative electrode 750c, can be said to correspond to a negative electrode terminal. Electrical resistance and the like can be measured by applying pressure to the evaluation material via the electrode plates 751 and 753.
[0543] The secondary battery of one embodiment of the present invention preferably uses an airtight package for its exterior. For example, a ceramic package or a resin package can be used. Furthermore, the exterior is preferably sealed in a sealed atmosphere, such as in a glove box, while blocking external air.
[0544] Fig. 29A is a perspective view of a secondary battery of one embodiment of the present invention, which has an exterior body and a shape different from those in Fig. 28. The secondary battery in Fig. 29A has external electrodes 771 and 772 and is sealed in an exterior body having a plurality of package members.
[0545] 29B shows an example of a cross section taken along the dashed line in FIG. 29A. A stack including a positive electrode 750a, a solid electrolyte layer 750b, and a negative electrode 750c is enclosed and sealed by a package member 770a having a flat plate with an electrode layer 773a, a frame-shaped package member 770b, and a package member 770c having a flat plate with an electrode layer 773b. The package members 770a, 770b, and 770c can be made of insulating materials, such as resin materials and ceramics.
[0546] The external electrode 771 is electrically connected to the positive electrode 750a via the electrode layer 773a and functions as a positive electrode terminal, while the external electrode 772 is electrically connected to the negative electrode 750c via the electrode layer 773b and functions as a negative electrode terminal.
[0547] By using the positive electrode active material composite 100α obtained in the first embodiment, an all-solid-state secondary battery having high energy density and good output characteristics can be realized.
[0548] The content of this embodiment mode can be combined with the content of other embodiment modes as appropriate.
[0549] Seventh Embodiment This embodiment is an example different from the cylindrical secondary battery shown in Fig. 21D. Fig. 30C shows an example of application to a vehicle such as an electric vehicle (EV).
[0550] The electric vehicle is equipped with first batteries 1301a and 1301b as main driving secondary batteries, and a second battery 1311 that supplies power to an inverter 1312 that starts a motor 1304. The second battery 1311 is also called a cranking battery (also called a starter battery). The second battery 1311 only needs to have high output, and does not need to have a large capacity, and the capacity of the second battery 1311 is smaller than that of the first batteries 1301a and 1301b.
[0551] The internal structure of the first battery 1301a may be a wound type shown in Fig. 22A or 23C. The first battery 1301a may use the all-solid-state battery of Embodiment 5. By using the all-solid-state battery of Embodiment 5 for the first battery 1301a, a high capacity can be achieved, safety can be improved, and the battery can be made smaller and lighter.
[0552] In this embodiment, an example is shown in which two first batteries 1301a and 1301b are connected in parallel, but three or more batteries may be connected in parallel. Furthermore, if the first battery 1301a can store sufficient power, the first battery 1301b may be omitted. By configuring a battery pack having multiple secondary batteries, it is possible to extract large amounts of power. The multiple secondary batteries may be connected in parallel, in series, or in series after being connected in parallel. A plurality of secondary batteries is also called a battery pack.
[0553] In addition, in a secondary battery for vehicle use, a service plug or circuit breaker that can cut off high voltage without using tools is provided in the first battery 1301a in order to cut off power from multiple secondary batteries.
[0554] The power of the first batteries 1301a and 1301b is mainly used to rotate the motor 1304, but also supplies power to 42V in-vehicle components (such as an electric power steering 1307, a heater 1308, and a defogger 1309) via a DCDC circuit 1306. When a rear motor 1317 is provided for the rear wheels, the first battery 1301a is also used to rotate the rear motor 1317.
[0555] In addition, the second battery 1311 supplies power to 14V in-vehicle components (audio 1313, power windows 1314, lamps 1315, etc.) via the DCDC circuit 1310.
[0556] The first battery 1301a will be described with reference to FIG. 30A.
[0557] FIG. 30A shows an example in which nine prismatic secondary batteries 1300 are combined into one battery pack 1415. Furthermore, nine prismatic secondary batteries 1300 are connected in series, with one electrode fixed by a fixing portion 1413 made of an insulator and the other electrode fixed by a fixing portion 1414 made of an insulator. While this embodiment shows an example in which the batteries are fixed by the fixing portions 1413 and 1414, they may also be housed in a battery housing box (also called a casing). Because it is expected that a vehicle will be subjected to external vibrations or shaking (such as from the road surface), it is preferable to fix multiple secondary batteries using the fixing portions 1413 and 1414 and the battery housing box. Furthermore, one electrode is electrically connected to the control circuit unit 1320 by wiring 1421. The other electrode is electrically connected to the control circuit unit 1320 by wiring 1422.
[0558] A memory circuit including a transistor using an oxide semiconductor may be used for the control circuit portion 1320. A charge control circuit or a battery control system including a memory circuit including a transistor using an oxide semiconductor may be referred to as a battery operating system (BTOS) or a battery oxide semiconductor (BTOS).
[0559] It is preferable to use a metal oxide that functions as an oxide semiconductor. For example, a metal oxide such as In-M-Zn oxide (wherein element M is one or more selected from aluminum, gallium, yttrium, copper, vanadium, beryllium, boron, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten, and magnesium) may be used as the oxide. In particular, the In-M-Zn oxide that can be used as the oxide is preferably a C-Axis Aligned Crystal Oxide Semiconductor (CAAC-OS) or a Cloud-Aligned Composite Oxide Semiconductor (CAC-OS). Alternatively, an In—Ga oxide or an In—Zn oxide may be used as the oxide. A CAAC-OS is an oxide semiconductor having multiple crystalline regions, each with its c-axis aligned in a specific direction. The specific direction refers to the thickness direction of the CAAC-OS film, the normal direction to the surface where the CAAC-OS film is formed, or the normal direction to the surface of the CAAC-OS film. A crystalline region is a region with periodic atomic arrangement. If the atomic arrangement is considered as a lattice arrangement, a crystalline region is also a region with a uniform lattice arrangement. Furthermore, a CAAC-OS has a region where multiple crystalline regions are connected in the a-b plane direction, and the region may have distortion. Note that distortion refers to a portion where the lattice arrangement changes between a region with a uniform lattice arrangement and a region with another uniform lattice arrangement in a region where multiple crystalline regions are connected. In other words, a CAAC-OS is an oxide semiconductor with a c-axis aligned and no clear orientation in the a-b plane direction. CAC-OS is a material in which elements constituting a metal oxide are unevenly distributed in a size range of 0.5 nm to 10 nm, preferably 1 nm to 3 nm, or in the vicinity thereof. Note that hereinafter, a state in which one or more metal elements are unevenly distributed in a metal oxide and regions containing the metal elements are mixed in a size range of 0.5 nm to 10 nm, preferably 1 nm to 3 nm, or in the vicinity thereof, is also referred to as a mosaic or patch state.
[0560] FIG. 30B shows an example of a block diagram of the battery pack 1415 shown in FIG. 30A.
[0561] The control circuit 1320 includes a switch unit 1324 including at least a switch for preventing overcharging and a switch for preventing overdischarging, a control circuit 1322 for controlling the switch unit 1324, and a voltage measurement unit for the first battery 1301a. The control circuit 1320 sets upper and lower voltage limits for the secondary battery used and limits the upper limit of the external current and the upper limit of the output current. The range between the lower and upper voltage limits of the secondary battery is within the recommended voltage range, and when the secondary battery falls outside this range, the switch unit 1324 activates and functions as a protection circuit. The control circuit 1320 can also be called a protection circuit because it controls the switch unit 1324 to prevent overcharging and overdischarging. For example, if the control circuit 1322 detects a voltage that could cause overcharging, it turns off the switch unit 1324 to cut off the current. Furthermore, a PTC element may be provided in the charge / discharge path to provide a function for cutting off the current in response to an increase in temperature. The control circuit section 1320 also has an external terminal 1325 (+IN) and an external terminal 1326 (-IN).
[0562] The switch unit 1324 can be configured by combining an n-channel transistor and a p-channel transistor. The switch unit 1324 is not limited to a switch having a Si transistor using single crystal silicon, and may be, for example, Ge (germanium), SiGe (silicon germanium), GaAs (gallium arsenide), GaAlAs (gallium aluminum arsenide), InP (indium phosphide), SiC (silicon carbide), ZnSe (zinc selenide), GaN (gallium nitride), GaO xThe switch portion 1324 may be formed using a power transistor having, for example, gallium oxide (x is a real number greater than 0). Furthermore, a memory element using an OS transistor can be freely arranged by stacking it on a circuit using a Si transistor, and therefore integration can be easily achieved. Furthermore, an OS transistor can be manufactured using the same manufacturing equipment as a Si transistor, and therefore can be manufactured at low cost. That is, a control circuit portion 1320 using an OS transistor can be stacked on the switch portion 1324 and integrated into a single chip. The volume occupied by the control circuit portion 1320 can be reduced, enabling miniaturization.
[0563] The first batteries 1301a and 1301b mainly supply power to in-vehicle devices of the 42V system (high voltage system), and the second battery 1311 supplies power to in-vehicle devices of the 14V system (low voltage system).
[0564] In this embodiment, an example in which lithium ion secondary batteries are used for both the first battery 1301a and the second battery 1311 is shown. A lead-acid battery, an all-solid-state battery, or an electric double layer capacitor may be used for the second battery 1311. For example, the all-solid-state battery of Embodiment 5 may be used. By using the all-solid-state battery of Embodiment 5 for the second battery 1311, high capacity can be achieved, and miniaturization and weight reduction are possible.
[0565] Furthermore, regenerative energy generated by the rotation of the tire 1316 is sent to the motor 1304 via the gear 1305, and is then charged into the second battery 1311 from the motor controller 1303 and the battery controller 1302 via the control circuit unit 1321. Alternatively, the first battery 1301a is charged from the battery controller 1302 via the control circuit unit 1320. Alternatively, the first battery 1301b is charged from the battery controller 1302 via the control circuit unit 1320. In order to efficiently charge the regenerative energy, it is desirable that the first batteries 1301a and 1301b be capable of rapid charging.
[0566] The battery controller 1302 can set the charging voltage and charging current of the first batteries 1301a and 1301b. The battery controller 1302 can set charging conditions in accordance with the charging characteristics of the secondary battery used, and can perform rapid charging.
[0567] Although not shown, when an external charger is connected, the charger's outlet or the charger's connection cable is electrically connected to the battery controller 1302. Power supplied from the external charger is charged to the first batteries 1301a and 1301b via the battery controller 1302. Some chargers are provided with a control circuit, and although the functions of the battery controller 1302 may not be used, it is preferable to charge the first batteries 1301a and 1301b via the control circuit unit 1320 to prevent overcharging. The control circuit unit 1320 may also be provided in the connection cable or the charger's connection cable. The control circuit unit 1320 is sometimes called an ECU (Electronic Control Unit). The ECU is connected to a CAN (Controller Area Network) provided in the electric vehicle. CAN is one of the serial communication standards used as an in-vehicle LAN. The ECU includes a microcomputer. The ECU uses a CPU or a GPU.
[0568] External chargers installed at charging stations and the like come in a variety of types, including 100V outlets, 200V outlets, and three-phase 200V and 50kW outlets. Charging can also be performed by receiving power from external charging equipment using a wireless power supply system or the like.
[0569] When rapid charging is performed, a secondary battery that can withstand high voltage charging is desired in order to charge in a short time.
[0570] The secondary battery of the present embodiment described above uses the positive electrode active material composite 100α obtained in Embodiment 1. Furthermore, by using graphene as a conductive additive, a secondary battery with significantly improved electrical characteristics can be realized, as a synergistic effect of suppressing capacity reduction and maintaining high capacity even when the electrode layer is thickened and the loading amount is increased. This is particularly effective for secondary batteries used in vehicles, and a vehicle with a long cruising range, specifically a cruising range of 500 km or more per charge, can be provided without increasing the ratio of the weight of the secondary battery to the total weight of the vehicle.
[0571] In particular, the secondary battery of the present embodiment described above can increase the operating voltage of the secondary battery by using the cathode active material composite 100α described in Embodiment 1, and can increase the usable capacity as the charging voltage increases. Furthermore, by using the cathode active material composite 100α described in Embodiment 1 for the cathode, a secondary battery for vehicles with excellent cycle characteristics can be provided.
[0572] Next, an example in which a secondary battery according to one embodiment of the present invention is mounted on a vehicle, typically a transportation vehicle, will be described.
[0573] Furthermore, when the secondary battery described in th...
Claims
A positive electrode, a negative electrode, and an electrolyte, The positive electrode has a first positive electrode active material and a second positive electrode active material, The first positive electrode active material is LiMO 2 (M1 represents one or more selected from F, Ni, Co, Mn, and Al), The second positive electrode active material is LiM2PO 4 (M2 represents one or more selected from Fe, Ni, Co, and Mn), the first positive electrode active material has an additive element X (X is one or more selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic) in a surface layer portion; The negative electrode comprises graphite, The graphite has a specific surface area of 0.8 m as measured by the BET method. 2 / g or more 8m 2 / g. A positive electrode, a negative electrode, and an electrolyte, The positive electrode has a first positive electrode active material and a second positive electrode active material, The first positive electrode active material is LiMO 2 (M1 represents one or more selected from Fe, Ni, Co, Mn, and Al), The second positive electrode active material is LiM2PO 4 (M2 represents one or more selected from Fe, Ni, Co, and Mn), the first positive electrode active material has an additive element X (X is at least one selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic) in a surface layer portion; The negative electrode comprises graphite, The graphite has a median diameter (D50) of 3 μm or more and 50 μm or less as measured by a laser diffraction method. In claim 1 or 2, The electrolyte comprises a fluorinated cyclic carbonate and a fluorinated chain carbonate as a solvent. In claim 1 or 2, The electrolyte contains fluoroethylene carbonate and methyl trifluoropropionate as a solvent, and when the total volume of the fluoroethylene carbonate and the methyl trifluoropropionate is 100 vol%, a volume ratio of the fluoroethylene carbonate to the methyl trifluoropropionate is y:100-y (where 5≦y≦30). In claim 1 or 2, The additional element X includes at least magnesium and fluorine, a secondary battery, wherein, when a cross section of the first positive electrode active material is subjected to STEM-EDX ray analysis, a fluorine concentration peak is located on a surface side of a magnesium concentration peak. A vehicle comprising the secondary battery according to claim 1 or 2.
3. An electronic device comprising the secondary battery according to claim 1.
Citation Information
Patent Citations
Lithium ion secondary battery
JP2010251060A
Lithium ion secondary battery
JP2023009361A
Manufacturing method for positive electrode active material and manufacturing method for lithium ion secondary battery
JP2023076432A
Nonaqueous electrolytic solution including ester having 3,3,3-trifluoropropionate group and nonaqueous electrolyte battery using same
WO2016006315A1
Lithium ion secondary battery
WO2017013827A1