Electrode assembly and battery
By designing protrusions on the electrode sheets and using a softener, the problem of poor electrolyte wetting in the electrode assembly was solved, improving the charge-discharge cycle performance and safety of the battery while maintaining the battery's energy density.
Patent Information
- Application Number
- PCT/CN2025/119689
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-12-05
- Filing Date
- 2025-09-08
- Publication Date
- 2026-11-12
AI Technical Summary
Existing secondary battery electrode assemblies suffer from poor electrolyte wetting after winding, leading to deterioration of the electrode interface and affecting the battery's charge-discharge cycle performance and safety.
Multiple protrusions are designed on the electrode sheet, and the use of a softener ensures that the height of the protrusions and the content of the softener are within a specific range, thereby improving the wetting effect of the electrolyte and enhancing the flexibility and processing performance of the electrode sheet by increasing the adhesion between the current collector and the active material layer.
It effectively improves the electrolyte transport capability within the electrode assembly, enhances the charge-discharge cycle performance and safety of the battery, while maintaining the battery's energy density.
Smart Images

Figure CN2025119689_12112026_PF_FP_ABST
Abstract
Description
An electrode assembly and a battery
[0001] This application claims priority to Chinese Patent Application No. 202411786739.X, filed on December 5, 2024, entitled "An Electrode Assembly and a Battery", the entire contents of which are incorporated herein by reference. Technical Field
[0002] This application relates to the field of battery technology, and in particular to an electrode assembly and a battery. Background Technology
[0003] Currently, the electrode components inside secondary batteries use a wound structure. After winding, the electrode components need to be hot-pressed and fixed to prevent them from moving or puncturing the outer packaging. However, with wound electrode components, electrolyte cannot easily penetrate the interior of the electrode component, which can easily lead to problems such as insufficient electrolyte and poor wetting. Ultimately, this results in deterioration of the electrode interface, affecting the battery's charge-discharge cycle performance, and even causing lithium plating, thus compromising battery safety. Summary of the Invention
[0004] The inventors discovered that there is compression between the layers of the electrode assembly. Especially during the charging and discharging process of the battery, the expansion and compression of the electrode assembly will be further aggravated, resulting in insufficient electrolyte between the layers of the electrode assembly, poor wetting, and easy interface deterioration, or even abnormal situations such as poor wetting and cycle failure.
[0005] This application provides an electrode assembly and a battery that can improve the problem of poor electrolyte wetting in batteries.
[0006] In a first aspect, embodiments of this application provide an electrode assembly, which includes a plurality of electrodes and a separator disposed between two electrodes of opposite polarity, wherein at least one electrode has a plurality of first protrusions.
[0007] The electrode includes a current collector and an active material layer disposed on the surface of the current collector. A first protrusion is formed by a portion of the current collector and a portion of the active material layer protruding on the same side of the electrode. The height of the first protrusion is H1, and H1 satisfies: 20μm≤H1≤80μm. The active material layer includes a softener, which is selected from at least one of organosilicon, fatty acid salt, and quaternary ammonium salt. Based on the total weight of the active material layer, the weight percentage of the softener is A, and A satisfies: 0.01%≤A≤0.4%.
[0008] In the electrode assembly according to the embodiments of the present application, the height H1 of the first protrusion is in the range of 20μm≤H1≤80μm, and the first protrusion can provide good support to improve the wetting effect of the electrolyte. The weight percentage A of the softening agent is in the range of 0.01%≤A≤0.40%, and the softening agent can increase the flexibility of the active material layer, prevent the active material layer from being easily broken, and make the pole piece easy to bend and form the first protrusion.
[0009] In some embodiments, the electrode assembly satisfies one of the following conditions:
[0010] (1) When A satisfies: 0.01%≤A≤0.10%, then H1 satisfies: 20μm≤H1≤40μm;
[0011] (2) When A satisfies: 0.10%<A≤0.20%, then H1 satisfies: 40μm<H1≤60μm;
[0012] (3) When A satisfies: 0.20%<A≤0.40%, then H1 satisfies: 60μm<H1≤80μm.
[0013] Based on the above embodiments, the softening agent can improve the overall flexibility of the pole piece, so that the height of the first protrusion can be increased while reducing damage to the pole piece, preventing microcracks from occurring in the active material layer at the first protrusion, having no side effects on the processing process, thereby facilitating the fabrication of the electrode assembly that meets the use requirements and improving the electrolyte wetting effect.
[0014] In some embodiments, the organosilicon is selected from at least one of methyl silicone resin, phenyl silicone resin, vinyl silicone resin, and silicone rubber; the fatty acid salt is selected from at least one of aluminum stearate, magnesium stearate, aluminum isooctanoate, and magnesium isooctanoate; the quaternary ammonium salt is selected from at least one of long-chain quaternary ammonium salts, short-chain quaternary ammonium salts, aliphatic quaternary ammonium salts, and aromatic quaternary ammonium salts.
[0015] In some embodiments, the active material layer includes a first binder, and based on the total weight of the active material layer, the weight percentage of the first binder is B; the electrode assembly satisfies one of the following conditions:
[0016] (1) When B satisfies: 0.8%≤B≤1.6%, then H1 satisfies: 20μm≤H1≤40μm;
[0017] (2) When B satisfies: 1.6%<B≤2.4%, then H1 satisfies: 40μm<H1≤80μm.
[0018] Based on the above embodiments, during the process of bending the active material layer of the corner segment together with the current collector to form the first protrusion, the active material layer has good ductility and is not prone to cracking, thereby improving the yield during the electrode winding process and improving the safety of the battery. In addition, the content of the first binder is appropriate, preventing the excessive content of the first binder from reducing the energy density of the battery.
[0019] In some embodiments, the first adhesive is selected from at least one of polyvinylidene fluoride, polyvinylidene fluoride, polyvinyl alcohol, polystyrene, styrene-butadiene rubber, polyacrylic acid, polyacrylonitrile, polyvinyl acetate, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, and polytetrafluoroethylene.
[0020] In some embodiments, the compaction density of the active material layer is ρ, 3.6 g / cm³. 3 ≤ρ≤4.35g / cm 3 .
[0021] Based on the above embodiments, the active material layer can have good toughness and is not easily brittle, while enabling the battery to have a suitable energy density.
[0022] In some embodiments, the electrode further includes a base coating layer disposed between the active material layer and the current collector, the base coating layer comprising a primer material selected from at least one of inorganic oxides and carbon-containing materials.
[0023] In some embodiments, the unit weight of the primer layer is η, and the electrode assembly satisfies one of the following conditions:
[0024] (1) η satisfies: 0.5mg / 1540.25mm 2 ≤η≤2.0mg / 1540.25mm 2 Then H1 satisfies: 20μm≤H1≤40μm;
[0025] (2) η satisfies: 2.0 mg / 1540.25 mm 2 ≤η≤4.0mg / 1540.25mm 2 Then H1 satisfies: 40μm≤H1≤80μm.
[0026] Based on the above embodiments, the adhesion between the current collector and the active material layer can be improved, and thus, when processing the first protrusion, the adhesion between the active material layer of the first protrusion and the current collector is stronger, reducing the generation of microcracks and powder shedding.
[0027] In some embodiments, the flat portion has a second protrusion, which is formed by bending another portion of the current collector and another portion of the active material layer toward the same side of the electrode, and the height of the second protrusion is H2, 5μm≤H2≤40μm.
[0028] Based on the above embodiments, the second protrusion provided on the flat portion can also provide good support for the separator, allowing the electrolyte to smoothly enter the gap between the flat sections of the flat portion, thereby improving the electrolyte wetting effect and improving the electrolyte retention.
[0029] In some embodiments, the radius of the inner surface of the first protrusion is R1, and the radius of the inner surface of the second protrusion is R2, where R1 = R2, and 0.3 mm ≤ R2 ≤ 10.0 mm.
[0030] Based on the above embodiments, the height of the first and second protrusions that are easily processed and formed is within a suitable range, and the first and second protrusions can also have a suitable elongation, so that the first protrusion can provide good support for the separator and is not easily deformed.
[0031] In some embodiments, the straight portion has a first thickness L1 in a first direction; two corner portions are disposed at opposite ends of the straight portion in a second direction perpendicular to the first direction, and the corner portions have a second thickness L2 in the second direction; each electrode includes two straight segments disposed opposite each other in the first direction and two corner segments disposed at both ends of the straight segments in the second direction; the electrode has a terminal end corresponding to the straight segment of the outermost electrode, and all the straight segments and terminal ends stacked in the first direction form a straight portion; the first thickness L1 is the thickness of the straight portion passing through the terminal end in the first direction; all the corner segments located on the same side of the straight segments in the second direction form corner portions, and the second thickness L2 is the thickness of the corner portion passing through the midpoint of the line connecting the two ends of the innermost corner segment in the second direction. The electrode assembly satisfies one of the following conditions:
[0032] (1) The number of turns of the electrode sheet in the electrode body is even, and L1 and L2 satisfy: 1.5≤L1 / L2≤2.2; or,
[0033] (2) The number of turns of the electrode sheet of the electrode body is odd, and L1 and L2 satisfy: 1.5≤L1 / L2≤2.4.
[0034] Based on the above embodiments, the tension and interlayer extrusion force on the straight section and the corner section are appropriate, so that the first convex part and the second convex part can play a good supporting role, are not easily deformed, and improve the electrolyte wetting effect.
[0035] In some embodiments, 1mm≤L1≤20mm, 0.5mm≤L2≤10mm.
[0036] Based on the above embodiments, it is convenient to select the first thickness L1 of the straight portion and the second thickness L2 of the corner portion to be appropriate relative to the height H1 of the first protrusion, so as to prevent the straight section of the straight portion from pulling on the corner section, thereby preventing excessive compression of the first protrusion, so as to maintain good support stability of the first protrusion, and to make the gap between the separator and the corner section appropriate, which can meet the electrolyte wetting requirements and prevent the overall size of the corner section from being too large due to the gap being too large.
[0037] Secondly, this application provides a battery, including a housing and the electrode assembly as described above, the electrode assembly being disposed within the interior space of the housing.
[0038] Based on the electrode assembly and battery of the embodiments of this application, by adding a softener to the active material layer, and selecting the height H1 of the first protrusion and the weight percentage A of the softener to satisfy 0.01% ≤ A ≤ 0.40% and 20μm ≤ H1 ≤ 80μm, the softener can improve the overall flexibility of the electrode sheet. For the structure at the first protrusion, it can achieve a higher height of the first protrusion while reducing damage to the electrode sheet, preventing microcracks from forming in the active material layer at the first protrusion, and having no side effects on the processing process. This facilitates the processing of electrode assemblies that meet the usage requirements, improves the electrolyte wetting effect, and improves the charge-discharge cycle performance of the battery when the electrode assembly is applied in the battery. Attached Figure Description
[0039] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0040] Figure 1 is a front view of a schematic diagram of the electrode sheet in an unfolded state according to an embodiment of this application;
[0041] Figure 2 is a cross-sectional view of an electrode assembly according to an embodiment of this application;
[0042] Figure 3 is a partial cross-sectional view of an embodiment of the present application showing a electrode sheet with a protrusion.
[0043] Figure 4 is a front view schematic diagram of an embodiment of the present application of an electrode sheet having an end clearance area;
[0044] Figure 5 is a front view schematic diagram of the electrode sheet having an electrode tab region according to an embodiment of this application;
[0045] Figure 6 is a schematic diagram of the front view of the electrode tab region penetrating the electrode sheet according to an embodiment of this application.
[0046] Reference numerals: 20, Electrode body; 21, Straight section; 22, Corner section; 40, Tab assembly; 50, Separating membrane; 201, Straight portion; 202, Corner portion; 300, Electrode sheet; 311, Protrusion; 3111, Inner surface; 3112, Outer surface; 301, First protrusion; 302, Second protrusion; 410, Positive electrode sheet; 420, Negative electrode sheet; 310, Protrusion area; 320, Tab area; 321, Tab mounting area; 322, Protective adhesive mounting area; 330, End clearance area; 3201, First side boundary; 3202, Second side boundary; 3203, Bottom boundary; 3204, Third side boundary; 3205, Fourth side boundary; 331, Head clearance area; 332, Tail clearance area; 3411, First edge; 3421, Second edge; 3431, Third edge; 3441, Fourth edge; 3101, First boundary; 3102, Second boundary; 3103, Third boundary; 3104, Fourth boundary; 341, First region; 342, Second region; X, Length direction; Y, Width direction; Z, Thickness direction. Detailed Implementation
[0047] To make the objectives, technical solutions, and advantages of this application clearer, the following detailed description is provided in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application.
[0048] The inventors discovered that the electrode assembly inside the secondary battery adopts a wound structure, which requires hot pressing after the electrode sheet and separator are alternately stacked and wound. There is internal stress inside the electrode assembly, resulting in poor electrolyte wettability. Furthermore, the electrode assembly expands during charging and discharging, further exacerbating the interlayer compression of the electrode assembly, leading to insufficient electrolyte, poor wettability, and ultimately, interface deterioration at weak points, and even lithium plating. To solve the above problems, gaps need to be created between battery layers. Currently, there are the following methods for creating gaps: (1) Applying adhesive paper to specific positions on the electrode to form gaps. This method currently improves the wetting ability, but the presence of adhesive paper increases the thickness of the electrode assembly and causes a certain loss in the energy density of the battery; (2) Applying soluble chemical substances to form gaps by uniformly applying some adhesive that is soluble in electrolyte to the electrode. However, the improvement effect is limited and there are other side effects on battery performance; (3) Thickening the separator. The separator has a stronger ability to store electrolyte and improves the wetting effect of electrolyte. However, this method will make the battery thicker and greatly reduce the energy density.
[0049] The inventors also discovered that by machining protrusions on the electrode sheets, which provide support during winding, gaps are formed between the electrode layers of the electrode assembly, thereby improving the electrolyte transport capacity within the electrode assembly and enhancing the battery's cycle performance. Based on this, embodiments of this application provide an electrode assembly and battery that design protrusions on the electrode sheets to effectively improve electrolytic wetting and electrode interface problems.
[0050] The battery provided in this application includes an outer packaging and an electrode assembly disposed within the inner space of the outer packaging, as well as an electrolyte filling the inner space of the outer packaging. The electrode assembly includes two electrodes with opposite polarities and a separator. As shown in FIG1, which is a front view of an embodiment of the present application with the electrode 300 in an unfolded state, the electrode 300 has a length direction X, a width direction Y, and a thickness direction Z that are perpendicular to each other. The length direction X, width direction Y, and thickness direction Z of the two electrodes 300 with opposite polarities of the electrode assembly are consistent. The separator 50 is disposed between the two electrodes 300 with opposite polarities in the thickness direction Z of the electrode 300. One of the two electrodes 300 with opposite polarities is a positive electrode 410 and the other is a negative electrode 420. The separator 50 has insulating properties to separate the positive electrode 410 and the negative electrode 420 to prevent the positive electrode 410 and the negative electrode 420 from short-circuiting.
[0051] At least one of the positive electrode 410 and the negative electrode 420 has a protrusion 311. Specifically, the electrode includes a current collector and an active material layer, which are stacked together along the thickness direction Z of the electrode 300, and the active material layer is disposed on the surface of the current collector. The protrusion 311 is formed by a portion of the current collector and a portion of the active material layer protruding along the thickness direction Z of the electrode 300 towards the same side of the electrode 300. The protrusion 311 provides support for the separator 50, creating a gap between the separator 50 and the electrode 300, thereby improving the electrolyte wetting effect.
[0052] The electrode 300 includes a first surface perpendicular to the thickness direction Z of the electrode 300. Referring again to Figure 1, the first surface includes a protrusion area 310, and multiple protrusions 311 are disposed in the protrusion area 310. There is a gap between the protrusion area 310 and the edge of the first surface. After the two electrodes 300 and the separator 50 are wound multiple times to form the electrode body 20, the protrusions 311 contact the separator 50 and provide support for the separator 50. When the electrode body 20 expands, the protrusions 311 can still support the separator 50. The contact area between the protrusions 311 and the separator 50 is small, so that there is space between the part of the electrode 300 corresponding to the protrusion area 310 and the separator 50 to accommodate the electrolyte. This prevents abnormal situations such as insufficient electrolyte or poor wetting between the electrode 300 and the separator 50 due to expansion and compression.
[0053] As shown in Figure 2, the separator 50 and two electrode plates 300 are wound multiple times along the length direction X of the electrode plates 300 to form the electrode body 20. The length direction X of the electrode plates 300 is the direction in which the electrode plates 300 are wound. The electrode body 20 is flat and includes a straight portion 201 and two corner portions 202. The two corner portions 202 are respectively located at opposite ends of the straight portion 201. Specifically, each turn of the electrode plate 300 in the electrode body 20 includes two straight sections 21 and two corner sections 22. The two straight sections 21 are arranged side by side in a direction perpendicular to the surface of the straight section 21, and the two straight sections 21 are arranged opposite each other in a direction perpendicular to the surface of the straight section 21. That is, the two straight sections 21 and the two corner sections 22 are connected end to end. The electrode body 20 has a terminal end, which is formed by a portion of the straight section 21 of the outermost electrode plate 300. All the straight sections 21 stacked in the first direction, the end points, and the isolation membrane 50 sandwiched between two adjacent straight sections 21 together form a straight portion 201; all the corner sections 22 located on the same side of the straight section 21 in the second direction and the isolation membrane 50 sandwiched between two adjacent corner sections 22 together form a corner portion 202.
[0054] The electrode 300 has a plurality of protrusions 311, and at least one of the straight section 21 and the corner section 22 has a protrusion 311. Optionally, all the protrusions 311 provided on a single electrode 300 protrude toward the same side of the electrode 300 in the thickness direction Z of the electrode 300. For example, when both the straight section 21 and the corner section 22 have protrusions 311, the protrusions 311 provided on the straight section 21 protrude toward the side where the electrode body 20 is wound, and the protrusions 311 provided on the corner section 22 protrude toward the side where the electrode body 20 is wound; or, the protrusions 311 provided on the straight section 21 protrude toward the side away from the winding center of the electrode body 20, and the protrusions 311 provided on the corner section 22 protrude toward the side away from the winding center of the electrode body 20. Optionally, a portion of the protrusions 311 on a single electrode 300 protrude toward one side of the electrode 300 in the thickness direction Z, and another portion of the protrusions 311 protrude toward the other side of the electrode 300 in the thickness direction Z. For example, the protrusions 311 on the straight section 21 protrude toward the side facing the winding center of the electrode body 20, and the protrusions 311 on the corner section 22 protrude toward the side away from the winding center of the electrode body 20; or, the protrusions 311 on the straight section 21 protrude toward the side away from the winding center of the electrode body 20, and the protrusions 311 on the corner section 22 protrude toward the side facing the winding center of the electrode body 20.
[0055] The above is merely an illustrative description. This application does not limit the orientation of the protrusions 311 of each electrode 300, and the orientation can be selected according to actual needs.
[0056] Due to the presence of internal stress inside the electrode main body 20 and the expansion of the electrode main body 20 during the charge and discharge process of the battery, the two adjacent turns of the pole piece 300 are prone to extrusion, especially the extrusion at the corner sections 22 of the two adjacent turns of the pole piece 300 is relatively intense, which easily leads to insufficient gaps resulting in poor electrolyte wetting. Moreover, under the action of extrusion force and internal stress, when the corner section 22 is provided with the convex portion 311, the convex portion 311 located at the corner section 22 is prone to deformation, and cracks easily occur in the active material layer, which further affects the cycle performance of the battery.
[0057] The pole piece 300 is provided with a plurality of convex portions 311, a part of which are first convex portions 301, and the corner portion 202 is provided with the first convex portions 301 (specifically, each corner section 22 is provided with the first convex portion 301). Wherein, in the thickness direction Z of the pole piece 300, the height of the first convex portion 301 is H1, and 20μm ≤ H1 ≤ 80μm. Within this height range, the first convex portion 301 can provide good support to improve the wetting effect of the electrolyte.
[0058] The material of the active material layer includes a softening agent, which is selected from at least one of organosilicon, fatty acid salt, and quaternary ammonium salt. Based on the total weight of the active material layer, the weight percentage content of the softening agent is A, and 0.01% ≤ A ≤ 0.40%. Within this content range, the softening agent can increase the flexibility of the active material layer, prevent the active material layer from being easily broken, and make the pole piece 300 easy to be bent and formed with the convex portion 311.
[0059] Since the corner section 22 is a high-incidence area for bending deformation, when the height H1 of the first convex portion 301 at the corner section 22 is larger, the first convex portion 301 supports the separator 50 to make the gap between the separator 50 and the pole piece 300 larger, and the improvement effect on electrolyte wetting is better. However, the higher the height of the first convex portion 301, the larger the elongation of the pole piece 300 at the first convex portion 301 or the larger the area covered by the first convex portion 301, the more likely the pole piece 300 at the first convex portion 301 will be deformed, or cracks will occur in the active material layer. Based on this, in the implementation of the present application, it is selected that the height H1 of the first convex portion 301 at the corner section 22 and the weight percentage content A of the softening agent satisfy the following conditional expression:
[0060] (1) When A satisfies: 0.01% ≤ A ≤ 0.10%, then H1 satisfies: 20μm ≤ H1 ≤ 40μm.
[0061] (2) When A satisfies: 0.10% < A ≤ 0.20%, then H1 satisfies: 40μm < H1 ≤ 60μm.
[0062] (3) When A satisfies: 0.20% < A ≤ 0.40%, then H1 satisfies: 60μm < H1 ≤ 80μm.
[0063] By selecting H1 and A to satisfy the above ranges, the softening agent can improve the overall flexibility of the electrode sheet 300. For the structure at the first convex portion 301, while enabling the height of the first convex portion 301 to be higher, the damage to the electrode sheet 300 is reduced, so that no microcracks are generated in the active material layer at the first convex portion 301, and there are no side effects on the processing process, which further facilitates the fabrication of electrode assemblies that can meet usage requirements, improves the electrolyte wetting effect, and improves the charge-discharge cycle performance of the battery when the electrode assembly is applied to the battery. Wherein, when H1 is lower than the lower limit of 20 μm, the height of the first convex portion 301 is too low, and the supporting capability of the first convex portion 301 for the separator 50 is insufficient; when H1 is higher than the upper limit of 80 μm, the height of the first convex portion 301 is too high, and the first convex portion 301 is prone to deformation under the action of external force. In addition, when A satisfies 0.01% ≤ A ≤ 0.10% and H1 exceeds the upper limit of 40 μm, or when A satisfies 0.10% < A ≤ 0.20% and H1 exceeds the upper limit of 60 μm, cracks tend to occur in the active material layer at the first convex portion 301 due to insufficient content of the softening agent; when A satisfies 0.10% < A ≤ 0.20% and H1 is lower than the lower limit of 40 μm, or when A satisfies 0.20% < A ≤ 0.40% and H1 is lower than the lower limit of 60 μm, the selectable range of the height of the first convex portion 301 is narrow, and it is impossible to fabricate the first convex portion 301 with a sufficient height, resulting in an insufficient improvement effect on wetting, which easily leads to deteriorated charge-discharge cycle performance of the battery.
[0064] In some embodiments, the silicone is selected from at least one of methyl silicone resin, phenyl silicone resin, vinyl silicone resin, and silicone rubber.
[0065] In some embodiments, the fatty acid salt is selected from at least one of aluminum stearate, magnesium stearate, aluminum isooctanoate, and magnesium isooctanoate.
[0066] In some embodiments, the quaternary ammonium salt is selected from at least one of long-chain quaternary ammonium salts, short-chain quaternary ammonium salts, aliphatic quaternary ammonium salts, and aromatic quaternary ammonium salts. For example, the long-chain quaternary ammonium salt is selected from at least one of cetyl dimethyl ammonium bromide, octadecyl dimethyl ammonium bromide, dimethyl didecyl ammonium bromide, cetyl dimethyl benzyl ammonium chloride, and octadecyl dimethyl benzyl ammonium chloride; the short-chain quaternary ammonium salt is selected from at least one of sodium n-octoate, decyl trimethyl ammonium bromide, benzalkonium chloride, and benzalkonium bromide; the aliphatic quaternary ammonium salt is selected from at least one of dodecylamine, cetylamine, dodecylpropylamine, and cetylpropylamine; the aromatic quaternary ammonium salt is selected from at least one of aniline, aromatic amine, benzidine, and naphthylamine.
[0067] In some embodiments, the active material layer further includes a first binder. Based on the total weight of the active material layer, the weight percentage of the first binder is B, and the height H1 of the first convex portion 301 of the corner section 22 and the weight percentage B of the first binder satisfy the following conditional expression:
[0068] (1) When B satisfies: 0.8% ≤ B ≤ 1.6%, H1 satisfies: 20 μm ≤ H1 ≤ 40 μm.
[0069] (2) When B satisfies: 1.6% < B ≤ 2.4%, H1 satisfies: 40 μm < H1 ≤ 80 μm.
[0070] By selecting H1 and B to satisfy the above ranges, the active material layer has good toughness and ductility, so that the active material layer is less prone to microcracks. During the process in which the active material layer at the corner section 22 is bent together with the current collector to form the first convex portion 301, the active material layer has good ductility and is less prone to cracks, thereby improving the yield rate of the pole piece 300 during the winding process and improving the safety of the battery. In addition, the weight percentage B of the first binder satisfies the above range, its proportion in the active material layer is appropriate, which prevents the excessive content of the first binder from reducing the energy density of the battery.
[0071] In some embodiments, the first binder is selected from at least one of polyvinylidene difluoride, polyvinylidene fluoride, polyvinyl alcohol, polystyrene, styrene-butadiene rubber, polyacrylic acid, polyacrylonitrile, polyvinyl acetate, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, and polytetrafluoroethylene.
[0072] In some embodiments, the compaction density of the active material layer is ρ, 3.6 g / cm 3 ≤ ρ ≤ 4.35 g / cm 3 , for example, ρ may be 3.6 g / cm 3 , 3.8 g / cm 3 , 4.00 g / cm 3 , 4.05 g / cm 3 , 4.08 g / cm 3 , 4.10 g / cm 3 , 4.18 g / cm 3 , 4.28 g / cm 3 , 4.35 g / cm 3 or any range between the above values. Within the above range, the active material layer can have good toughness, is not prone to brittle fracture, and at the same time enables the battery to have an appropriate energy density.
[0073] In some embodiments, the thickness of the active material layer is h1, and h1 satisfies: 10 μm ≤ h1 ≤ 500 μm.
[0074] In some embodiments, the electrode further includes a base coating layer disposed between the active material layer and the current collector. The base coating layer includes a primer material selected from at least one of inorganic oxides and carbon-containing materials. The base coating layer also includes an adhesive material mixed with the primer material. The base coating layer is bonded to the active material layer and the current collector by the adhesive material. By providing the base coating layer, the connection stability of the active material layer can be improved, preventing the active material layer from peeling off and shedding powder. The inorganic oxide is selected from at least one of alumina, titanium oxide, and magnesium oxide, and the carbon-containing material is selected from at least one of graphene, carbon nanotubes, and fluorocarbons. The adhesive material can be the same material as the first adhesive.
[0075] In some embodiments, the unit weight of the base coat is η, and the height H1 of the first protrusion 301 of the corner segment 22 and the unit weight η of the base coat satisfy the following condition:
[0076] (1) η satisfies: 0.5mg / 1540.25mm 2 ≤η≤2.0mg / 1540.25mm 2 Then H1 satisfies: 20μm≤H1≤40μm.
[0077] (2) η satisfies: 2.0 mg / 1540.25 mm 2 ≤η≤4.0mg / 1540.25mm 2 Then H1 satisfies: 40μm≤H1≤80μm.
[0078] By selecting H1 and η to satisfy the above range, the adhesion between the current collector and the active material layer can be improved. As a result, when processing the first protrusion 301, the adhesion between the active material layer of the first protrusion 301 and the current collector is stronger, reducing the generation of microcracks and powder shedding.
[0079] In some embodiments, the thickness of the base coating is h2, where h2 satisfies: 0.5μm≤h2≤4.0μm.
[0080] In some embodiments, a portion of the protrusions 311 are second protrusions 302, and the straight portion 201 has the second protrusions 302. Specifically, the straight section 21 has the second protrusions 302. Along the thickness direction Z of the electrode 300, the height of the second protrusion is H2, 5μm≤H2≤40μm. For example, H2 can be 5μm, 10μm, 20μm, 30μm, 5μm, 35μm, 40μm, or any range thereof. By selecting the height H2 of the second protrusion 302 to satisfy the above range, the second protrusion 302 can provide good support for the separator 50, allowing the electrolyte to smoothly enter the gap between the straight sections 21 of the straight portion 201, improving the electrolyte wetting effect and improving the electrolyte retention.
[0081] It should be noted that in the embodiments of this application, the material composition, thickness and compaction density of the active material layer corresponding to the straight section 21 and the corner section 22 are the same, and the material composition, thickness and unit weight of the primer layer corresponding to the straight section 21 and the corner section 22 are the same.
[0082] In some embodiments, the radius of the inner surface of the first protrusion 301 is R1, where R1 is the diameter of the inscribed sphere D1 on the inner surface of the first protrusion 301, and the radius of the inner surface of the second protrusion 302 is R2, where R2 is the diameter of the inscribed sphere D2 on the inner surface of the second protrusion 302. R1 = R2, and 0.3 mm ≤ R2 ≤ 10.0 mm. For example, R2 can be 0.3 mm, 2.3 mm, 5.5 mm, 7.3 mm, 8.5 mm, or 10.0 mm. By selecting the radii of both the first protrusion 301 and the second protrusion 302 to be within the above range, it is convenient to ensure that the heights of the first protrusion 301 and the second protrusion 302 are within a suitable range after processing, and to ensure that the first protrusion 301 and the second protrusion 302 have suitable elongation, so that the first protrusion 301 can provide good support for the separator 50 and is not easily deformed.
[0083] In some embodiments, referring again to FIG2, the straight portion 201 has a first thickness L1 in a first direction, the first thickness L1 being the thickness of the straight portion 201 passing through the end point in the first direction; the corner portion 202 has a second thickness L2 in a second direction, the second thickness L2 being the thickness of the corner portion 202 passing through the midpoint of the line connecting the two ends of the innermost corner segment 22 in the second direction. L1 and L2 satisfy the following conditional expression:
[0084] (1) The number of turns of the electrode sheet of the electrode body is even, and L1 and L2 satisfy: 1.5≤L1 / L2≤2.2.
[0085] (2) The number of turns of the electrode sheet of the electrode body is odd, and L1 and L2 satisfy: 1.5≤L1 / L2≤2.4.
[0086] By selecting the first thickness L1 of the straight portion 201 and the second thickness L2 of the corner portion 202 to satisfy the above-mentioned condition, the tension and interlayer extrusion force on the straight section 21 and the corner section 22 are appropriate, so that the first protrusion 301 and the second protrusion 302 can play a good supporting role, are not easily deformed, and improve the electrolyte wetting effect.
[0087] In some embodiments, the straight portion 201 has a first thickness L1 in the first direction satisfying: 1mm ≤ L1 ≤ 20mm. For example, L1 can be 1mm, 2mm, 5mm, 8mm, 10mm, 15mm, 20mm, or any range thereof. Within the above range, it is convenient to select the first thickness L1 of the straight portion 201 and the height H1 of the first protrusion 301 to be within a suitable range, preventing the straight section 22 of the straight portion 201 from pulling on the corner section 21 of the corner portion 202, thereby preventing excessive compression of the first protrusion 301, so as to maintain good support stability of the first protrusion 301.
[0088] In some embodiments, the corner portion 202 has a second thickness L2 in the second direction satisfying: 0.5mm ≤ L2 ≤ 10mm. For example, L2 can be 0.5mm, 1mm, 2mm, 5mm, 6mm, 8mm, 10mm, or any range thereof. Within this range, it is convenient to match the second thickness L2 of the corner portion 202 and the height H1 of the first protrusion 301 within a suitable range, so that the gap between the separator 50 of the corner portion 202 and the corner segment 21 is appropriate, which can meet the electrolyte wetting requirements and prevent the overall size of the corner portion 202 from being too large due to an excessively large gap.
[0089] In some embodiments, the surface of the active material layer facing away from the current collector forms a first surface. The first surface includes a bump region 310, and a protrusion 311 is disposed in the bump region 310. The bump region 310 is defined by a bump boundary line. The protrusion 311 of the bump region 310 may be located in the inner region defined by the bump boundary line, or the protrusion 311 may be internally connected to the bump boundary line. The first surface also includes an end clearance region 330 and an edge clearance region. The end clearance region 330 is connected to the end of the bump region 310 in the length direction X of the electrode 300 and extends to the edge of the electrode 300. The edge clearance region is disposed on one side of the bump region 310 in the width direction Y of the electrode 300 and extends to the edge of the electrode 300. Neither the edge clearance region nor the end clearance region 330 is provided with a protrusion 311. After the two electrodes 300 and the separator 50 are wound together, the surfaces of the electrodes 300 corresponding to the edge clearance region and the end clearance region 330 may be spaced apart from the separator 50.
[0090] The end clearance area 330 is located at the end of the protrusion area 310 in the length direction X of the electrode 300 and extends to the edge of the electrode 300. The end clearance area 330 also extends to the edge of the electrode 300 in the width direction Y of the electrode 300. As shown in FIG4, the end clearance area 330 includes at least one of the head clearance area 331 and the tail clearance area 332. Preferably, the end clearance area 330 includes both the head clearance area 331 and the tail clearance area 332. In the length direction X of the electrode 300, the head clearance area 331 is located at one end of the protrusion area 310 and the tail clearance area 332 is located at the other end of the protrusion area 310.
[0091] After the two electrodes 300 and the separator 50 are wound, the head clearance area 331 can be located in the innermost few turns of the electrode body 20, which facilitates the winding and forming of the electrode body 20 and helps to improve the structural stability of the central area of the electrode body 20. The tail clearance area 332 can be located in the outermost few turns of the electrode body 20. The tail clearance area 332 can serve as a buffer area between the protrusion 311 and the tail end of the electrode body 20, so that the portion of the clearance area 330 at the corresponding end of the electrode 300 can more smoothly bind the inner layer structure of the electrode body 20, which helps to improve the encapsulation stability of the electrode body 20. Especially when the electrode body 20 has a tendency to expand, using the tail clearance area 332 without the protrusion 311 to finish can prevent the tail end of the electrode body 20 from slipping due to expansion stress, thereby improving the structural stability of the electrode body 20.
[0092] Specifically, the first surface of the electrode 300 includes a first edge 3411 and a second edge 3421 disposed opposite to each other in the length direction X of the electrode 300, and the convex boundary line of the convex region 310 includes a first boundary 3101 and a second boundary 3102 disposed opposite to each other in the length direction X of the electrode 300, with the first boundary 3101 corresponding to the first edge 3411 and the second boundary 3102 corresponding to the second edge 3421. The head clearance area 331 is formed between the first edge 3411 and the first boundary 3101, and the tail clearance area 332 is formed between the second edge 3421 and the second boundary 3102. One end of the separator 50 is flush with or extends out of the head clearance area 331 to be sandwiched between two electrodes 300 with opposite polarities. The electrode 300 is wound from the head clearance area 331 and the separator 50 along the length direction X of the electrode 300 to form a flat electrode body 20. That is, the head clearance area 331 is located in the inner circle of the electrode body 20, and the tail clearance area 332 is located in the outer circle of the electrode body 20. The other end of the separator 50 extends out of the tail clearance area 332 in the winding direction of the electrode 300 to prevent the separator 50 from shrinking and causing the two electrodes 300 with opposite polarities to short-circuit.
[0093] The first surface of the electrode 300 has an edge clearance area, which includes a first region 341 and a second region 342. In the width direction Y of the electrode 300, the first region 341 is connected to one side of the protrusion region 310, and the second region 342 is connected to the other side of the protrusion region 310. The first region 341 extends to the edge of the electrode 300 in a direction away from the second region 342, and the second region 342 extends to the edge of the electrode 300 in a direction away from the first region 341. That is, the two opposite boundaries of the protrusion region 310 in the width direction Y of the electrode 300 are respectively spaced from the corresponding edge of the electrode 300, so as to prevent the deformation stress when the protrusion 311 is processed in the protrusion region 310 from causing abnormal deformation such as wavy edges or wrinkles on the edge of the electrode 300.
[0094] Specifically, the electrode 300 includes a third edge 3431 and a fourth edge 3441 disposed opposite to each other in the width direction Y of the electrode 300. The convex boundary line of the convex region 310 includes a third boundary 3103 and a fourth boundary 3104 disposed opposite to each other in the width direction Y of the electrode 300. The third boundary 3103 corresponds to the third edge 3431, and the fourth boundary 3104 corresponds to the fourth edge 3441. A first region 341 is formed between the third boundary 3103 and the third edge 3431, and a second region 342 is formed between the fourth boundary 3104 and the fourth edge 3441. The first region 341 and the second region 342 extend in the length direction X of the electrode 300 to connect with the end clearance region 330. That is, the extension line of the first boundary 3101, the extension line of the second boundary 3102, the third boundary 3103 and the fourth edge 3441 are connected to the end clearance region 330. The first region 341 is defined by three edges 3431. The extension of the first boundary 3101, the extension of the second boundary 3102, the fourth boundary 3104 and the fourth edge 3441 define the second region 342. The extension of the first boundary 3101, the first edge 3411, the third edge 3431 and the fourth edge 3441 define the head clearance zone 331. The extension of the second boundary 3102, the second edge 3421, the third edge 3431 and the fourth edge 3441 define the tail clearance zone 332. The protrusion area 310 is located in the region defined by the first boundary 3101, the second boundary 3102, the third boundary 3103 and the fourth boundary 3104. The protrusion 311 can be internally connected to at least one of the first boundary 3101, the second boundary 3102, the third boundary 3103 and the fourth boundary 3104.
[0095] Optionally, the first boundary 3101, the second boundary 3102, the first edge 3411 and the second edge 3421 are parallel to the width direction Y of the electrode 300, and the third boundary 3103, the fourth boundary 3104, the third edge 3431 and the fourth edge 3441 are parallel to the length direction X of the electrode 300. In this case, the head clearance area 331 and the tail clearance area 332 are each independently rectangular or square, and the first region 341 and the second region 342 are rectangular.
[0096] Optionally, one of the first region 341 and the second region 342 is used to mount the electrode assembly tab 40. As shown in FIG4, exemplaryly, the second region 342 is used to mount the electrode assembly tab 40, and the protrusion region 310 is spaced apart from the tab assembly 40. In this case, the protrusion region 310 is defined by the first boundary 3101, the second boundary 3102, the third boundary 3103, and the fourth boundary 3104.
[0097] Optionally, as shown in FIG5, the first surface further includes a tab region 320, which extends from the third boundary 3103 toward the side where the fourth boundary 3104 is located. The tab region 320 is used to mount the tab assembly 40 of the electrode assembly, and the tab assembly 40 is spaced apart from the protrusion region 310. When mounting the tab assembly 40 onto the tab region 320, the processing method affects the mounting stability of the tab assembly 40 and the stability of the surrounding structure, which in turn affects the stability of the electrode 300 interface. For example, when the tab assembly 40 is pressed onto the electrode 300 using a roll forming method, the tab assembly 40 may be pressed together with the area where the protrusion 311 is located, or the distance between the tab assembly 40 and the protrusion 311 may be too close, which may result in deformation of the protrusion 311 or indentation. By planning the tab region 320 for mounting the tab assembly 40, the installation of the tab assembly 40 is facilitated, the process difficulty is reduced, the mounting stability of the tab assembly 40 is improved, and the interface stability near the tab assembly 40 is improved. It can also make the tab assembly 40 and the protrusion 311 misaligned in the thickness direction Z of the electrode 300, which helps to improve the energy density of the battery when the electrode assembly is used in the battery.
[0098] Each tab region 320 is used to provide at least one tab assembly 40. For example, the tab assembly 40 includes a tab and a protective adhesive, and the tab and the protective adhesive can be installed in the same tab region 320; or, the tab is installed in one tab region 320 and the protective adhesive is installed in another tab region 320, wherein the tab extends out of the edge of the electrode 300 along the width direction Y of the electrode, and the protective adhesive is flush with the edge of the electrode 300. The protective adhesive is used to separate the corresponding tab from the electrode 300 to prevent lithium deposition at the tab.
[0099] Optionally, as shown in Figure 5, the tab region 320 extends from the fourth boundary 3104 along the width direction Y of the electrode 300 to the side where the third boundary 3103 is located, and is spaced apart from the third boundary 3103; or, as shown in Figure 6, the tab region 320 extends from the fourth boundary 3104 along the width direction Y of the electrode 300 through the protrusion region 310.
[0100] The electrode 300 in this embodiment can form at least one of a positive electrode 410 and a negative electrode 420. The current collector of the negative electrode 420 is a negative current collector, and the active material layer is a negative active material layer. The current collector of the positive electrode 410 is a positive current collector, and the active material layer is a positive active material layer. The negative active material layer includes, in addition to the softener and the first adhesive as described above, a negative active material. The positive active material layer includes, in addition to the softener and the first adhesive as described above, a positive active material.
[0101] This application does not impose any particular limitations on the materials used for positive electrode active materials, positive electrode current collectors, negative electrode active materials, and negative electrode current collectors. Various materials known in the art that can be used as positive electrode active materials, positive electrode current collectors, negative electrode active materials, and negative electrode current collectors are applicable to this application.
[0102] Exemplarily, the negative electrode current collector can be at least one of copper foil, aluminum foil, nickel foil, or carbon-based current collector; the thickness of the negative electrode current collector can be from 1 μm to 200 μm. The negative electrode active material layer can be disposed on one or both opposing surfaces of the negative electrode current collector. Further, in the thickness direction Z of the negative electrode sheet 420, the negative electrode active material layer can be coated only on a portion of the negative electrode current collector. Exemplarily, the thickness of the negative electrode active material layer can be from 10 μm to 500 μm.
[0103] Exemplarily, the negative electrode active material includes at least one of lithium metal, natural graphite, artificial graphite, or silicon-based materials, wherein the silicon-based material includes at least one of silicon, silicon oxide, silicon carbide, or silicon alloy. The negative electrode active material layer may also include a conductive agent; exemplaryly, the conductive agent in the negative electrode active material layer may include at least one of carbon black, acetylene black, Ketjen black, sheet graphite, graphene, carbon nanotubes, carbon fibers, or carbon nanowires. The negative electrode active material layer may also include a second binder, which may include at least one of carboxymethyl cellulose (CMC), polyacrylate, polyacrylate, polyvinylpyrrolidone, polyaniline, polyimide, polyamide-imide, polysiloxane, epoxy resin, polyester resin, polyurethane resin, or polyfluorene.
[0104] For example, the positive current collector can be aluminum foil, or other positive current collectors commonly used in the art can be used. The thickness of the positive current collector can be from 1 μm to 200 μm. The positive active material layer can be disposed on one or both opposite surfaces of the positive current collector. Furthermore, in the thickness direction Z of the positive electrode 410, the positive active material layer can be coated only on a portion of the positive current collector, and the thickness of the positive active material layer can be from 10 μm to 500 μm.
[0105] For example, the positive electrode active material includes LiCoO2, LiNiO2, LiMn2O4, and LiCo. 1-y M y O2, LiNi 1-y M y O2, LiMn 2-y M y O4, LiNi x Co y Mn z M 1-x-y-zO2, wherein M is selected from at least one of Fe, Co, Ni, Mn, Mg, Cu, Zn, Al, Sn, B, Ga, Cr, Sr, V, or Ti, and 0≤y≤1, 0≤x≤1, 0≤z≤1, x+y+z≤1. Exemplarily, the positive electrode active material may include at least one of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, or lithium nickel manganese oxide, and the above positive electrode active material may be doped and / or coated. The positive electrode active material layer also includes a conductive agent; exemplaryly, the conductive agent in the positive electrode active material layer may include at least one of conductive carbon black, acetylene black, Ketjen black, sheet graphite, graphene, carbon nanotubes, or carbon fibers. The positive electrode active material layer may further include a third adhesive, which may include at least one of the following: a copolymer of vinylidene fluoride and hexafluoropropylene, a copolymer of styrene and acrylate, a copolymer of styrene and butadiene, polyamide, polyacrylonitrile, polyacrylate, polyacrylate, sodium carboxymethyl cellulose, polyvinyl acetate, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, or polyhexafluoropropylene.
[0106] This application does not impose any particular limitation on the separator 50, and various materials known in the art that can be used as the separator 50 are applicable to this application. Exemplarily, the separator 50 includes at least one selected from polyethylene, polypropylene, polyvinylidene fluoride, polyethylene terephthalate, polyimide, or aramid. For example, polyethylene includes at least one selected from high-density polyethylene, low-density polyethylene, or ultra-high molecular weight polyethylene. Polyethylene and polypropylene, in particular, have good short-circuit prevention properties and can improve the stability of the electrode assembly through a turn-off effect. The thickness of the separator 50 is in the range of about 3 μm to 500 μm. The positive and negative tabs are made of a metallic conductive material.
[0107] The tabs in this application embodiment include positive tabs and negative tabs. The positive tab is disposed on the positive electrode plate, and the negative tab is disposed on the negative electrode plate. This application embodiment does not have any particular limitations on the positive tab, negative tab and protective adhesive. Various materials known in the art that can be used as positive tabs, negative tabs and protective adhesives are applicable to this application.
[0108] This application does not impose any particular limitation on the electrolyte. Various materials known in the art that can be used as electrolytes are applicable to this application. Electrolytes include lithium salts and non-aqueous organic solvents.
[0109] For example, lithium salts include lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium nitrate, and lithium methyl sulfite.
[0110] By way of example, the non-aqueous organic solvent may also contain at least one of a carboxylic acid ester compound, an ether compound, or other organic solvent. The aforementioned carbonate compound may include, but is not limited to, at least one of a chain carbonate compound and a cyclic carbonate compound. The aforementioned chain carbonate compound may include, but is not limited to, at least one of dipropyl carbonate (DPC) or ethyl methyl carbonate (EMC). The aforementioned cyclic carbonate compound may include, but is not limited to, at least one of butyl carbonate (BC) or vinyl ethylene carbonate (VEC). The aforementioned carboxylic acid ester compound may include, but is not limited to, at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, or propyl propionate. The aforementioned ether compound may include, but is not limited to, at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, 2-methyltetrahydrofuran, or tetrahydrofuran. The other organic solvents mentioned above may include, but are not limited to, at least one of dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolium ketone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, trimethyl phosphate, triethyl phosphate, trioctyl phosphate, or phosphate esters. This application does not impose any particular limitation on the mass percentage of non-aqueous organic solvents in the electrolyte, as long as the purpose of this application is achieved. For example, based on the total mass of the electrolyte, the mass percentage of non-aqueous organic solvents may be from 10% to 70%.
[0111] This application does not impose any particular restrictions on the packaging bag for the battery; it can be any packaging bag known in the art, as long as it can achieve the purpose of this application.
[0112] This application does not impose any particular limitation on the type of battery, which may include any device in which an electrochemical reaction occurs. In this application, the battery may include, but is not limited to, lithium metal batteries, lithium-ion batteries, lithium polymer batteries, or lithium-ion polymer batteries.
[0113] The battery manufacturing process described in this application is well known to those skilled in the art, and this application does not impose any particular limitations. For example, it may include, but is not limited to, the following steps: after installing the positive electrode tab on the positive electrode sheet and the negative electrode tab on the negative electrode sheet, stacking the positive electrode sheet, the separator, and the negative electrode sheet in sequence, and performing operations such as winding and folding as needed to obtain a wound electrode assembly; placing the electrode assembly in a packaging bag; injecting electrolyte into the packaging bag and sealing it to obtain a battery; or, stacking the positive electrode sheet, the separator, and the negative electrode sheet in sequence, and then fixing the four corners of the entire stacked structure with tape to obtain a stacked electrode assembly; placing the electrode assembly in a packaging bag; injecting electrolyte into the packaging bag and sealing it to obtain a battery.
[0114] The battery described in this application can be used in electrical devices. This application does not specifically limit the type of electrical device; it can be any electrical device known in the prior art. In some embodiments, the electrical device may include, but is not limited to, laptops, pen-based computers, mobile computers, e-book players, portable telephones, portable fax machines, portable copiers, portable printers, stereo headphones, video recorders, LCD TVs, portable cleaners, portable CD players, mini CDs, transceivers, electronic notebooks, calculators, memory cards, portable recorders, radios, backup power supplies, motors, automobiles, motorcycles, electric bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries, and lithium-ion capacitors, etc.
[0115] The present application will be further illustrated below using a lithium-ion battery as an example and with specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the present application.
[0116] The performance of lithium-ion batteries in the embodiments and comparative examples of this application is tested using the following methods:
[0117] (1) Test method for capacity retention during 1C charging / 0.7C discharging at 25℃
[0118] In an environment of 25°C, the lithium-ion battery was charged at a constant current of 1C to its full charge voltage (the maximum designed voltage of the lithium-ion battery is 4.5V). Then, it was charged at the maximum voltage at a constant voltage until the current reached 0.02C. Finally, it was discharged at a constant current of 0.7C until the final voltage reached 3.0V. The discharge capacity of the first cycle was recorded. This process was repeated for 1000 charge-discharge cycles, and the discharge capacity of the lithium-ion battery after 1000 charge-discharge cycles was recorded.
[0119] The cycle capacity retention rate at 25℃ with 1C charging and 0.7C discharging is calculated as (discharge capacity of the 1000th cycle / discharge capacity of the first cycle) × 100%.
[0120] (2) 25℃ Cyclic Lithium Plating Test Method
[0121] In an environment of 25°C, the lithium-ion battery was charged at a constant current of 1C to its full charge voltage (the battery's maximum design voltage is 4.5V). Then, it was charged at the maximum voltage at a constant voltage until the current reached 0.02C. Finally, it was discharged at a constant current of 0.7C until the final voltage reached 3.0V. The discharge capacity of the first cycle was recorded. This process was repeated for 1000 charge-discharge cycles, and the discharge capacity of the lithium-ion battery after 1000 charge-discharge cycles was recorded.
[0122] After testing at 25℃ and 1000 charge-discharge cycles, the battery was disassembled while fully charged (maximum design voltage 4.5V) to observe whether lithium plating was present at the negative electrode interface, tabs, or protective adhesive.
[0123] (3) Method for testing the processing yield during the winding process
[0124] The separator is placed between two electrodes 300 with opposite polarities (positive electrode 410 and negative electrode 420) and wound in an integrated winding machine to form an electrode body 20. The distance M (M>0.1mm is acceptable) of the edge of the negative electrode 420 in the width direction of the positive electrode 410 is measured using an X-ray device. Samples are continuously prepared, and the total number of samples T (total number is 100) and the number of qualified products N are counted.
[0125] Winding yield = N / T × 100%.
[0126] (4) Battery energy density testing method
[0127] In an environment of 25°C, the lithium-ion battery was charged to full charge voltage (the battery's maximum design voltage is 4.5V) at a constant current of 0.5C. Then, it was charged at the maximum voltage at a constant voltage until the current was 0.02C. Finally, it was discharged at a constant current of 0.2C until the final voltage was 3.0V. The discharge capacity of the first cycle was recorded.
[0128] Battery energy density = First 0.2C discharge capacity * First 0.2C discharge plateau voltage / Lithium-ion battery volume
[0129] (5) Test methods for fabric softeners
[0130] The fabric softener content is obtained by measuring the content of specific elements in the sample using ICP (inductively coupled plasma atomic emission spectrometry). These specific elements include, but are not limited to, the content of silicon in organosilicon, metal elements in fatty acid salts, and nitrogen in quaternary ammonium salts.
[0131] (6) Test method for the height H1 of the convex part
[0132] The height of the protrusion of the electrode at the corner of the battery cell is tested.
[0133] Example 1-1
[0134] (1) Preparation of positive electrode sheet
[0135] Sodium carboxymethyl cellulose binder and alumina primer were mixed at a mass ratio of 3:97, with water added as a solvent. The mixture was stirred evenly under vacuum to obtain a primer slurry with a solid content of 40 wt%. The primer slurry was then uniformly coated onto one surface of a 9 μm thick aluminum foil for the positive electrode current collector. After drying at 85°C, the coating was cold-pressed to obtain a single-sided primer layer with a thickness of 1 μm. The unit weight η of the primer layer was 2 mg / 1540.25 mm. 2 .
[0136] Lithium cobalt oxide (LiCoO2) as the positive electrode active material, conductive carbon black as the conductive agent, polyvinylidene fluoride (PVDF) as the first binder, and methyl silicone resin as the softener were mixed at a mass ratio of 97.5:1.69:0.8:0.01. N-methylpyrrolidone (NMP) was added as a solvent, and the mixture was stirred evenly under vacuum to obtain a positive electrode slurry with a solid content of 75 wt%. The positive electrode slurry was uniformly coated on the surface of the base coating layer, dried at 85°C, and cold-pressed to obtain a positive electrode sheet with a single-sided coating thickness of 95 μm for the positive electrode active material layer.
[0137] Then, the above steps are repeated on the other surface of the aluminum foil to obtain a positive electrode sheet with a double-sided coating of positive active material layer. After cutting, a positive electrode sheet with dimensions of 74mm × 851mm is obtained for use. The compaction density of the positive active material layer is 4.20 g / cm³. 3 .
[0138] (2) Preparation of negative electrode sheet
[0139] Artificial graphite (negative electrode active material), styrene-butadiene rubber (SBR) binder, and sodium carboxymethyl cellulose (CMC) secondary binder were mixed at a mass ratio of 97.4:1.4:1.2. Deionized water was then added as a solvent, and the mixture was stirred evenly under vacuum to obtain a negative electrode slurry with a solid content of 50 wt%. This negative electrode slurry was uniformly coated onto one surface of a 10 μm thick copper foil used as a negative electrode current collector. The foil was then dried at 85°C and cold-pressed to obtain a negative electrode sheet with a single-sided coating of 130 μm thick negative electrode active material. The above steps were repeated on the other surface of the same copper foil to obtain a negative electrode sheet with a double-sided coating of negative electrode active material. After cutting, negative electrode sheets with dimensions of 76 mm × 867 mm were obtained for later use. The compaction density of the negative electrode active material layer was 1.80 g / cm³. 3 .
[0140] (3) Preparation of the separating membrane
[0141] A porous polyethylene (PE) membrane with a thickness of 5 μm was used.
[0142] (4) Preparation of electrolyte
[0143] In an argon-atmospheric glove box with a water content of less than 10 ppm, ethylene carbonate (EC), propylene carbonate (PC), and diethyl carbonate (DEC) were mixed in a mass ratio of 1:1:2 to obtain a base solvent. Lithium hexafluorophosphate (LiPF6) was then dissolved in the base solvent to obtain the electrolyte. The mass percentage of LiPF6 in the electrolyte was 12.5%.
[0144] (5) Assembly of lithium-ion batteries
[0145] The positive electrode aluminum tab is installed on the edge area of the positive electrode sheet 410 by rolling, and the protective adhesive is pasted on the edge area of the positive electrode sheet 410. The negative electrode nickel tab is installed on the edge area of the negative electrode sheet 420 by rolling.
[0146] The positive electrode 410 with positive tabs, the separator 50, and the negative electrode 420 with negative tabs are stacked sequentially, with the separator 50 positioned between the positive electrode 410 and the negative electrode 420 to provide insulation. The electrode body 20 is then formed by winding the separator. The electrode assembly is placed in an outer aluminum-plastic film package and dried in an 85°C vacuum oven for 12 hours to remove moisture. Electrolyte is then injected, and the lithium-ion battery is obtained through vacuum sealing, settling, formation, capacity testing, degassing, and edge trimming.
[0147] In Example 1-1, the positive electrode sheet has a protrusion. The protrusion is rolled out on the positive electrode sheet by rolling. The electrode sheet shown in Figure 4 is used as the positive electrode sheet. In the electrode body 20 formed by winding, the corner section 21 of each turn of the electrode sheet 300 has a first protrusion 301 and the straight section 22 has a second protrusion 302. The parameters of the lithium-ion battery are shown in Table I.
[0148] Table I
[0149] Examples 1-2 to 1-25 and Comparative Examples 1-1 to 1-6 are the same as in Example 1-1, except that the height H1 of the first protrusion 301 and the weight percentage A of the softener are adjusted according to Table 1 in the preparation of the positive electrode sheet.
[0150] Examples 1-26 to 1-35 are the same as in Example 1-1, except that the type of softener is adjusted as shown in Table 1 during the preparation of the positive electrode sheet.
[0151] Examples 1-36 to 1-39 are the same as in Example 1-1, except that the compaction density ρ of the active material layer is adjusted as shown in Table 1 during the preparation of the positive electrode sheet.
[0152] The parameters and performance test results of the lithium-ion batteries of Examples 1-1 to 1-39 and Comparative Examples 1-1 to 1-6 are shown in Table 1.
[0153] Table 1
[0154] As can be seen from Examples 1-1 to 1-39 and Comparative Examples 1-1 to 1-6 in Table 1, by adding a softener to the active material layer and selecting a height H1 of the first protrusion 301 of the corner segment 22 that satisfies 20μm≤H1≤80μm, and a softener weight percentage A that satisfies 0.01%≤A≤0.40%, the lithium-ion battery exhibits good charge-discharge cycle performance, with no lithium plating during the charge-discharge cycle, and good processing yield during the winding process. When H1 is below the lower limit of 20μm, the height of the first protrusion 301 is too low, resulting in insufficient support capacity and insufficient gap between the positive electrode 410 and the separator 50, leading to poor charge-discharge cycle performance of the lithium-ion battery. When H1 is above the upper limit of 50μm, the height of the first protrusion 301 is too high, making the active material layer prone to microcracks, which reduces the processing yield during the winding process.
[0155] According to Examples 1-1 to 1-25 and Comparative Examples 1-1 to 1-6 in Table 1, the height H1 of the first protrusion 301 of the corner segment 22 and the weight percentage A of the fabric softener satisfy (1) 0.01% ≤ A ≤ 0.10%, 20 μm ≤ H1 ≤ 40 μm, or satisfy (2) 0.10%. <A≤0.20%,40μm
[0156] Examples 2-1 to 2-16 and Comparative Examples 2-1 to 2-4 are the same as Examples 1-4, except that the height H1 of the first protrusion 301 and the weight percentage B of the first adhesive are adjusted according to Table 1 in the preparation of the positive electrode sheet.
[0157] The parameters and performance test results of the lithium-ion batteries of Examples 2-1 to 2-14 and Comparative Examples 2-1 to 2-6 are shown in Table 2.
[0158] Table 2
[0159] According to Examples 1-4, Examples 2-1 to 2-16, and Comparative Examples 2-1 to 2-4 in Table 2, it can be seen that the height H1 of the first protrusion 301 of the corner segment 22 and the weight percentage B of the first adhesive satisfy (1) 0.8% ≤ B ≤ 1.6% and 20 μm ≤ H1 ≤ 40 μm, or satisfy (2) 1.6%. <B≤2.4%、40μm
[0160] Examples 3-1 to 3-16 and Comparative Examples 3-1 to 3-4 are the same as Examples 1-4, except that the height H1 of the first protrusion 301 and the unit weight η of the base coating are adjusted according to Table 1 in the preparation of the positive electrode sheet.
[0161] The parameters and performance test results of the lithium-ion batteries of Examples 3-1 to 3-16 and Comparative Examples 3-1 to 3-4 are shown in Table 3.
[0162] Table 3
[0163] According to Examples 1-4, Examples 3-1 to 3-16, and Comparative Examples 3-1 to 3-4 in Table 3, it can be seen that the height H1 of the first protrusion 301 of the corner segment 22 and the unit weight of the primer coating η satisfy (1) 0.5mg / 1540.25mm 2 ≤η≤2.0mg / 1540.25mm 2 20μm≤H1≤40μm, or satisfy (2)2.0mg / 1540.25mm 2 ≤η≤4.0mg / 1540.25mm 2 With a diameter of 40μm≤H1≤80μm, lithium-ion batteries exhibit better charge-discharge cycle performance and do not experience lithium plating during charge-discharge cycles, resulting in excellent processing yield during the winding process.
[0164] Examples 4-1 to 4-10 are the same as in Example 1-1, except that the number of turns of the electrode is adjusted according to Table 1 during the assembly of the lithium-ion battery, and the first thickness L1 and the second thickness L2 of the electrode body 20 are adjusted.
[0165] The parameters and performance test results of the lithium-ion batteries in Examples 4-1 to 4-10 are shown in Table 4.
[0166] Table 4
[0167] According to Examples 1-1, 4-1 to 4-3, and 4-9 to 4-10 in Table 4, when the number of turns of the electrode sheet 300 of the electrode body is even, L1 and L2 satisfy: 1.5≤L1 / L2≤2.2, the lithium-ion battery has good charge-discharge cycle performance, and there is no lithium plating during the charge-discharge cycle.
[0168] According to Examples 4-4 to 4-6 and Examples 4-7 to 4-8 in Table 4, when the number of turns of the electrode sheet 300 of the electrode body is odd, L1 and L2 satisfy: 1.5≤L1 / L2≤2.4, the lithium-ion battery has good charge-discharge cycle performance, and there is no lithium plating during the charge-discharge cycle.
[0169] Examples 5-1 to 5-7 are the same as in Example 1-1, except that the height H1 of the first protrusion 301 and the height H2 of the second protrusion 302 are adjusted according to Table 1 in the preparation of the positive electrode sheet.
[0170] The parameters and performance test results of the lithium-ion batteries in Examples 5-1 to 5-7 are shown in Table 5.
[0171] Table 5
[0172] As can be seen from Examples 1-1, 5-1 to 5-7 in Table 5, when the height H1 of the first protrusion 301 satisfies 20μm≤H1≤80μm and the height H2 of the second protrusion 302 satisfies 5μm≤H2≤40μm, the heights of the first protrusion 301 and the second protrusion 302 are matched, so that there is a suitable gap between the straight part and the corner part for accommodating the electrolyte, and the first protrusion 301 and the second protrusion 302 are not easily deformed, thereby improving the charging cycle performance of the lithium-ion battery and having a good winding advantage during the winding process of the electrode 300.
[0173] In the accompanying drawings of this embodiment, the same or similar reference numerals correspond to the same or similar components. In the description of this application, it should be understood that if terms such as "upper," "lower," "left," and "right" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, they are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, the terms used to describe positional relationships in the accompanying drawings are only for illustrative purposes and should not be construed as limiting this patent. For those skilled in the art, the specific meaning of the above terms can be understood according to the specific circumstances.
[0174] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. An electrode assembly, wherein, The electrode assembly includes a plurality of pole pieces and a separator disposed between two pole pieces of opposite polarities, the pole pieces and the separator are wound for multiple turns to form a flat electrode main body, the electrode main body includes a straight portion and two corner portions, the two corner portions are respectively disposed at two opposite ends of the straight portion, and the pole pieces at the corner portions have first protrusions; The pole piece includes a current collector and an active material layer disposed on the surface of the current collector, the first protrusion is formed by a part of the current collector and a part of the active material layer protruding toward the same side of the pole piece, and the height of the first protrusion is H1; The active material layer includes a softening agent, the softening agent is selected from at least one of organosilicon, fatty acid salt and quaternary ammonium salt, and based on the total weight of the active material layer, the weight percentage of the softening agent is A; Wherein, A satisfies: 0.01%≤A≤0.4%, and H1 satisfies: 20μm≤H1≤80μm.
2. The electrode assembly according to claim 1, wherein, The electrode assembly satisfies one of the following conditions: (1) A satisfies: 0.01%≤A≤0.10%, and H1 satisfies: 20μm≤H1≤40μm; (2) A satisfies: 0.10%<A≤0.20%, and H1 satisfies: 40μm<H1≤60μm; (3) A satisfies: 0.20%<A≤0.40%, and H1 satisfies: 60μm<H1≤80μm.
3. The electrode assembly according to claim 1, wherein, The organosilicon is selected from at least one of methyl silicone resin, phenyl silicone resin, vinyl silicone resin and silicone rubber; The fatty acid salt is selected from at least one of aluminum stearate, magnesium stearate, aluminum isooctanoate and magnesium isooctanoate; The quaternary ammonium salt is selected from at least one of aliphatic quaternary ammonium salts and aromatic quaternary ammonium salts.
4. The electrode assembly according to claim 3, wherein, The aliphatic quaternary ammonium salt is selected from at least one of long-chain quaternary ammonium salts and short-chain quaternary ammonium salts.
5. The electrode assembly according to claim 1, wherein, The active material layer includes a first binder, and based on the total weight of the active material layer, the weight percentage of the first binder is B; the electrode assembly satisfies one of the following conditions: (1) B satisfies: 0.8%≤B≤1.6%, and H1 satisfies: 20μm≤H1≤40μm; (2) B satisfies: 1.6%<B≤2.4%, and H1 satisfies: 40μm<H1≤80μm.
6. The electrode assembly according to claim 5, wherein, The first binder is selected from at least one of polyvinylidene difluoride, polyvinylidene fluoride, polyvinyl alcohol, polystyrene, styrene-butadiene rubber, polyacrylic acid, polyacrylonitrile, polyvinyl acetate, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate and polytetrafluoroethylene.
7. The electrode assembly according to claim 1, wherein, The compaction density of the active material layer is ρ, 3.6 g / cm³. 3 ≤ρ≤4.35g / cm 3 .
8. The electrode assembly according to claim 1, wherein, The pole piece further includes a primer layer, the primer layer is disposed between the active material layer and the current collector, the primer layer includes a primer material, and the primer material is selected from at least one of inorganic oxides and carbon-containing materials; The unit primer weight of the primer layer is η; the electrode assembly satisfies one of the following conditions: (1) η satisfies: 0.5mg / 1540.25mm 2 ≤η≤2.0mg / 1540.25mm 2 H1 satisfies: 20μm≤H1≤40μm; (2) η satisfies: 2.0 mg / 1540.25 mm 2 ≤η≤4.0mg / 1540.25mm 2 H1 satisfies: 40μm <H1≤80μm。 9. The electrode assembly according to claim 1, wherein, The straight portion is provided with a second protrusion, and the second protrusion is formed by another part of the current collector and another part of the active material layer protruding toward the same side of the pole piece; The height of the second protrusion is H2, where 5μm≤H2≤40μm.
10. The electrode assembly according to claim 9, wherein, The radius of the inner surface of the first protrusion is R1, and the radius of the inner surface of the second protrusion is R2, where R1 = R2 and 0.3 mm ≤ R2 ≤ 10.0 mm.
11. The electrode assembly according to claim 1, wherein, The straight portion has a first thickness L1 in the first direction; The two corner portions are respectively disposed at opposite ends of the straight portion in a second direction perpendicular to the first direction, and the corner portions have a second thickness L2 in the second direction; Each of the electrode plates includes two straight sections arranged opposite each other along the first direction, and two corner sections disposed at both ends of the straight sections along the second direction. The electrode has a terminal end corresponding to the straight segment of the outermost electrode. All the straight segments and the terminal end stacked in the first direction form the straight portion. The first thickness L1 is the thickness of the straight portion passing through the terminal end in the first direction. All the corner segments located on the same side of the straight segments in the second direction form a corner portion. The second thickness L2 is the thickness of the corner portion passing through the midpoint of the line connecting the two ends of the innermost corner segment in the second direction. The electrode assembly satisfies one of the following conditions: (1) The number of turns of the electrode sheet in the electrode body is even, and L1 and L2 satisfy: 1.5 ≤ L1 / L2 ≤ 2.2; or, (2) The number of turns of the electrode sheet of the electrode body is odd, and L1 and L2 satisfy: 1.5≤L1 / L2≤2.
4.
12. The electrode assembly according to claim 11, wherein, 1mm≤L1≤20mm, 0.5mm≤L2≤10mm.
13. A battery, wherein, include: shell; and, The electrode assembly as described in any one of claims 1-12 is disposed within the interior space of the housing.