Battery cell, battery device, electric device, and energy storage device

By adding phytate additives to battery cells, the spin mode of active oxygen is changed, the intensity of oxidation reaction is reduced, and the safety performance problem of high energy density battery cells is solved, achieving a balance between high energy density and high safety performance.

WO2026233203A1PCT designated stage Publication Date: 2026-11-12CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2026/093900
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-06
Filing Date
2026-04-29
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing high-energy-density battery cells are prone to catching fire and exploding during operation, resulting in poor safety performance and making it difficult to balance high energy density and high safety performance.

Method used

Adding phytate additives to battery cells can change the spin mode of active oxygen, converting it into inactive oxygen, reducing the intensity of the oxidation reaction, and catalyzing the conversion of active oxygen in the battery, thereby reducing the risk of thermal runaway, without affecting the normal electrical performance of the battery.

Benefits of technology

It effectively reduces the risk of battery thermal runaway, improves battery safety performance, and maintains high energy density and good electrical performance, making it suitable for lithium-ion and sodium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2026093900_12112026_PF_FP_ABST
    Figure CN2026093900_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of batteries, and provides a battery cell, a battery device, an electric device, and an energy storage device. The battery cell provided in the present application comprises a positive electrode sheet, a negative electrode sheet, a separator disposed between the positive electrode sheet and the negative electrode sheet, and an electrolyte. The positive electrode sheet comprises a positive electrode current collector and a positive electrode film layer disposed on at least one side of the positive electrode current collector. The positive electrode film layer comprises a positive electrode active material. The battery cell further comprises a phytate additive. The battery cell provided in the present application has both excellent energy density and low safety risks.
Need to check novelty before this filing date? Find Prior Art

Description

Battery cells, battery packs, electrical devices and energy storage devices

[0001] Cross-referencing

[0002] This application incorporates Chinese Patent Application No. 202510574648.8, filed on May 6, 2025, entitled “Battery Cell, Battery Device, Power Consumption Device and Energy Storage Device”, which is incorporated herein by reference in its entirety. Technical Field

[0003] This application relates to the field of battery technology, and in particular to a battery cell, battery device, power supply device, and energy storage device. Background Technology

[0004] In recent years, rechargeable batteries have been widely used in energy storage systems for hydropower, thermal power, wind power, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, and many other fields. With the increasing prevalence of battery applications in the industry, the demand for battery performance, especially energy density, is rising. However, high-energy-density battery cells have high internal activity, making them prone to fire and explosion during operation, resulting in poor safety performance. Therefore, there is an urgent need to provide a battery that balances high energy density and high safety performance. Summary of the Invention

[0005] This application is made in view of the above-mentioned issues, and its purpose is to provide a battery cell that combines high energy density and high safety performance.

[0006] An embodiment of the first aspect of this application provides a battery cell, which includes a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte. The positive electrode includes a positive current collector and a positive electrode film layer disposed on at least one side of the positive current collector. The positive electrode film layer includes a positive active material, and the battery cell also includes a phytate additive.

[0007] Phytate additives are a class of organic salt compounds formed by the esterification of all six hydroxyl groups on cyclohexanehexyl alcohol with phosphate groups and their combination with metal ions. They have a highly phosphorylated six-membered ring skeleton, which can change the spin mode of electrons in reactive oxygen species, so that the electron configuration in reactive oxygen species meets the principle of minimum energy, transforming them into inactive oxygen species. This effectively reduces the reactivity of reactive oxygen species, thereby reducing the intensity of the oxidation reaction of reactive oxygen species on the electrolyte / negative electrode, and effectively reducing the risk of thermal runaway of battery cells. At the same time, the addition of phytate to the battery can also reduce the intensity of battery thermal runaway, reduce the rate of thermal diffusion, reduce the risk of wider thermal runaway after battery cell failure, and prevent the occurrence of battery explosions and other risks.

[0008] Furthermore, phytate additives catalyze the conversion of reactive oxygen species into inactive oxygen species in the battery. They are not consumed during battery operation and do not affect the normal electrical performance of the battery. Therefore, they can maintain reliability over a long period of time during long-cycle operation. Adding phytate additives to battery cells can also reduce the polarization inside the battery, which is beneficial to improving the dynamic performance of the battery cells. This further enhances the capacity of the battery cells under the same charge and discharge rate, allowing the battery cells to have both high energy density and good safety performance.

[0009] In any embodiment, the phytate additive includes one or more of lithium phytate, sodium phytate, potassium phytate, zinc phytate, calcium phytate, and magnesium phytate.

[0010] When phytate additives include the above-mentioned substances, they can be adapted to the working voltage of the battery cell, ensuring that it does not decompose during battery operation, and improving the safety performance of the battery cell without affecting its electrical performance.

[0011] In any embodiment, the positive electrode active material includes nickel, and the molar proportion of nickel in the positive electrode active material is greater than or equal to 80% based on the total number of moles of transition metal elements in the positive electrode active material, and can be selected as 90%-96%.

[0012] The nickel content in the positive electrode active material meets the above-mentioned range, enabling the positive electrode active material to have a high specific capacity, which is beneficial for further improving the energy density of the battery cell. However, with the increase of nickel content, the oxygen release amount and oxygen release rate of the positive electrode under full charge also increase, leading to an increased probability of thermal runaway and a deterioration in the safety performance of the battery cell. The technical solution in the embodiments of this application is particularly suitable for this positive electrode sheet, which can further improve the energy density of the battery cell while reducing the probability of battery thermal runaway and improving safety performance, thus meeting performance requirements.

[0013] In any embodiment, the phytate additive is disposed in the electrolyte, and the mass content of the phytate additive is 0.1%-5% based on the total mass of the electrolyte, optionally 0.3%-1%.

[0014] The reactive oxygen released from the positive electrode active material undergoes an oxidation reaction with the electrolyte. Dissolving the phytate additive in the electrolyte allows it to contact the reactive oxygen, reducing its reactivity and thus the intensity of the oxidation reaction. This reduces the probability of thermal runaway in the battery cell and improves its safety performance. Controlling the phytate additive content in the electrolyte within the aforementioned range ensures its complete dissolution, allowing it to directly contact and reduce the activity of reactive oxygen, further enhancing the safety performance of the battery cell.

[0015] In any embodiment, the phytate additive is disposed in the positive electrode film layer, and the mass content of the phytate additive is 0.1%-2%, optionally 0.1%-1.5%, based on the total mass of the positive electrode film layer.

[0016] The active oxygen generated by the positive electrode active material enters the electrolyte from the positive electrode film. Placing phytate additives in the positive electrode film allows the active oxygen to interact with the phytate additives while active oxygen is being generated at the positive electrode, thereby reducing the activity of the active oxygen and the degree of oxidation reaction between active oxygen and the electrolyte / negative electrode, and improving the safety performance of the battery cell. However, the phytate additives occupy space in the positive electrode active material, which is not conducive to improving the energy density of the battery cell. Controlling the mass content of phytate additives in the positive electrode film to meet the above-mentioned range can improve the safety performance of the battery cell while also increasing its energy density.

[0017] In any embodiment, the negative electrode sheet includes a negative current collector and a negative electrode film layer disposed on at least one side of the negative current collector. The phytate additive is disposed in the negative electrode film layer, and the mass content of the phytate additive is 0.1%-2% based on the total mass of the negative electrode film layer, optionally 0.1%-1.5%.

[0018] Adding phytate additives to the negative electrode film can reduce the reactivity of active oxygen in contact with the negative electrode, reduce the degree of oxidation side reactions between active oxygen and the negative electrode material, and improve the safety performance of the battery cell.

[0019] In any embodiment, the phytate additive is disposed on the surface of the positive electrode film layer away from the positive electrode current collector; the phytate additive is disposed on the surface of at least one side of the separator; and / or, the phytate additive is disposed on the surface of the negative electrode film layer away from the negative electrode current collector.

[0020] In any embodiment, the phytate additive is disposed in the coating, and the thickness of the coating with the phytate additive is 1μm-10μm, optionally 2μm-4μm.

[0021] Incorporating phytate additives into the coating at the aforementioned locations on the battery cell can improve the safety performance of the battery cell. Controlling the coating thickness within the aforementioned range allows for both improved safety performance and high energy density in the battery cell.

[0022] In any embodiment, based on the total mass of the negative electrode film, the mass content of silicon in the negative electrode film is 5%-50%, and optionally 9%-45%.

[0023] High silicon content negative electrode active materials have higher theoretical specific capacity. Controlling the mass content of silicon in the negative electrode active material to meet the above-mentioned range is beneficial to improving battery capacity and can form a good match with high nickel content positive electrode active materials, ensuring effective insertion / extraction of cations between the positive and negative electrodes, and further improving the energy density of the battery cell. However, the active oxygen released from the positive electrode can react with the negative electrode active material to generate byproducts (such as silicates), and the heat generated can easily cause thermal runaway of the battery. The technical solution provided in this application is particularly suitable for this negative electrode sheet, which can improve the energy density of the battery cell while reducing the intensity of the oxidation side reaction and improving safety performance.

[0024] In any embodiment, the battery cell is a lithium-ion battery, and the positive electrode active material has the components shown in the following general formula: Li a1 Ni x1 Co y1 M1 z1 M2 w1 O 2-b1 Wherein, M1 includes one or more of Mn and Al, and M2 includes one or more of Zr, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, and K; 0.8≤a1≤1.2, 0.8≤x1≤1, 0≤y1≤0.2, 0≤z1≤0.2, 0≤w1≤0.1, and -0.1≤b1≤0.1.

[0025] Lithium-containing transition metal oxide ternary cathode active materials have high capacity and are the preferred materials for high energy density batteries. When the cathode active material includes the above-mentioned types of active materials, it is beneficial to further improve the energy density of the battery cell.

[0026] In any embodiment, the electrolyte in the lithium-ion battery includes a solvent and an electrolyte salt, and the solvent in the lithium-ion battery includes one or more of carboxylic acid ester solvents, carbonate solvents, and ether solvents.

[0027] In any embodiment, the electrolyte salt in the lithium-ion battery includes one or more of lithium hexafluorophosphate (LiPF6), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium dioxolaneborate (LiBOB), and lithium perchlorate (LiClO4).

[0028] The electrolyte of lithium-ion batteries contains the above-mentioned electrolyte salts, which can dissociate lithium ions in the electrolyte, improve the liquid phase dispersion ability of lithium ions, and help to further improve the energy density of the battery cell.

[0029] In any embodiment, the battery cell is a sodium-ion battery, and the positive electrode active material has the components shown in the following general formula: Na a2 Ni x2 Coy2 M3 z2 M4 w2 O 2-b2 M3 includes one or more of Mn and Al, and M4 includes one or more of Zr, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, and K; 0.8≤a2≤1.2, 0.8≤x2≤1, 0≤y2≤0.2, 0≤z2≤0.2, 0≤w2≤0.1, and -0.1≤b2≤0.1.

[0030] Sodium-ion batteries using sodium-containing transition metal oxides as positive electrode active materials have a high theoretical specific capacity, which is beneficial for improving the energy density of sodium-ion batteries.

[0031] In any embodiment, the electrolyte in the sodium-ion battery includes a solvent and an electrolyte salt, and the solvent includes one or more of carbonate solvents and ether solvents.

[0032] In any embodiment, the electrolyte salt in the sodium-ion battery includes one or more of sodium hexafluorophosphate (NaPF6), sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), sodium bis(fluorosulfonyl)imide (NaFSI), sodium di(oxalato)borate (NaBOB), and sodium perchlorate (NaClO4).

[0033] In any embodiment, the heat generation rate of the positive electrode in the battery cell is 60mW-100mW.

[0034] In any implementation, the combustion spread rate of the bare battery cell is less than or equal to 2.5 cm / s.

[0035] An embodiment of the second aspect of this application provides a battery device that includes the battery cell described in the above embodiments.

[0036] An embodiment of the third aspect of this application provides an electrical device that includes the battery device described in the above embodiments, wherein the battery is used to provide electrical energy.

[0037] An embodiment of the fourth aspect of this application provides an energy storage device, which includes the battery device in the above embodiments, the battery being used to store electrical energy.

[0038] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Attached Figure Description

[0039] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the various drawings denote the same or similar parts or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings depict only some embodiments disclosed in this application and should not be construed as limiting the scope of this application.

[0040] Figure 1 is an XRD characterization spectrum of phytate additive in a battery cell according to an embodiment of this application.

[0041] Figure 2 is a DSC heat generation rate curve of the positive electrode sheet of a single cell in an embodiment of this application and a comparative example.

[0042] Figure 3 is a schematic diagram of a battery cell according to an embodiment of this application;

[0043] Figure 4 is an exploded view of a battery cell according to an embodiment of this application shown in Figure 3;

[0044] Figure 5 is a schematic diagram of a battery module according to an embodiment of this application;

[0045] Figure 6 is a schematic diagram of a battery pack according to an embodiment of this application;

[0046] Figure 7 is an exploded view of the battery pack of one embodiment of this application shown in Figure 6;

[0047] Figure 8 is a schematic diagram of an electrical device using a secondary battery as a power source according to an embodiment of this application.

[0048] Explanation of reference numerals in the attached drawings: 1 Battery pack; 2 Upper housing; 3 Lower housing; 4 Battery module; 5 Battery cell; 51 Housing; 52 Electrode assembly; 53 Cover plate. Detailed Implementation

[0049] The following detailed description, with appropriate reference to the accompanying drawings, discloses embodiments of the battery cell, battery assembly, power consumption device, and energy storage device of this application. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.

[0050] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0051] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.

[0052] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.

[0053] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0054] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.

[0055] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0056] As market demands for extended battery life increase, increasing the energy density of individual battery cells has become a common pursuit in the industry. Ternary cathode active materials, such as lithium nickel cobalt manganese oxide (LiCO), possess high discharge specific capacity, especially those with a high nickel content, which exhibit even greater discharge specific capacity. Batteries using LiCO as the cathode active material hold promise for meeting the industry's demand for high-energy-density batteries. However, in ternary materials, the Ni-O bond has poor stability and is prone to breakage, releasing oxygen. This oxygen release process easily generates various reactive oxygen species (such as free radical oxygen, singlet oxygen, and superoxide compounds), which exhibit stronger oxidation reactivity (especially singlet oxygen). 1 O2 directly oxidizes the electrolyte / negative electrode, causing severe oxidation and heat generation, which can lead to thermal runaway. As the Ni content increases, the oxygen release rate of the positive electrode increases under full charge conditions, further increasing the risk of battery thermal runaway. Safety has become the biggest bottleneck factor limiting the commercial application of high-nickel batteries.

[0057] To reduce oxidation heat generation during thermal runaway, modifications such as doping and coating of the positive electrode active material can be used to increase the oxygen release temperature or reduce the amount of oxygen released. However, elemental doping often reduces the specific capacity of the material, which is detrimental to improving the battery's energy density; while coating methods cannot change the intrinsic characteristics of oxygen release in the positive electrode material, failing to achieve the desired effect. Therefore, suppressing oxygen release and heat generation at the positive electrode through modifications to the positive electrode material has low effectiveness. Additionally, adding additives such as oxygen scavengers to the electrolyte can reduce electrolyte oxidation heat generation, but the oxygen scavengers themselves are also oxidized and generate heat, and they deactivate under high temperature and high voltage conditions, resulting in poor effectiveness in reducing thermal runaway. Besides the above improvements, existing technologies have shown that improving the oxidation resistance of the electrolyte / negative electrode can reduce oxidation heat generation after positive electrode oxygen release; however, these improvements reduce the battery's electrical performance. Although they increase the battery's energy density, they negatively impact other battery performance aspects (such as fast charging and cycle life), making large-scale use impossible. Therefore, there is an urgent need to provide a battery cell that balances high energy density and low safety risk.

[0058] Based on this, this application provides a battery cell, which includes a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte. The positive electrode includes a positive current collector and a positive electrode film disposed on at least one side of the positive current collector. The positive electrode film includes a positive active material, and the battery cell also includes a phytate additive.

[0059] Phytate additives are a class of organic salt compounds formed by the esterification of all six hydroxyl groups on cyclohexanehexyl alcohol with phosphate groups and their combination with metal ions. They have a highly phosphorylated six-membered ring skeleton, which can change the spin mode of electrons in reactive oxygen species, so that the electron configuration in reactive oxygen species meets the principle of minimum energy, transforming them into inactive oxygen species. This effectively reduces the reactivity of reactive oxygen species, thereby reducing the intensity of the oxidation reaction of reactive oxygen species on the electrolyte / negative electrode, and effectively reducing the risk of thermal runaway of battery cells. At the same time, the addition of phytate to the battery can also reduce the intensity of battery thermal runaway, reduce the rate of thermal diffusion, reduce the risk of wider thermal runaway after battery cell failure, and prevent the occurrence of battery explosions and other risks.

[0060] Furthermore, phytate additives catalyze the conversion of reactive oxygen species into inactive oxygen species in the battery. They are not consumed during battery operation and do not affect the normal electrical performance of the battery. Therefore, they can maintain reliability over a long period of time during long-cycle operation. Adding phytate additives to battery cells can also reduce the polarization inside the battery, which is beneficial to improving the dynamic performance of the battery cells. This further enhances the capacity of the battery cells under the same charge and discharge rate, allowing the battery cells to have both high energy density and good safety performance.

[0061] In this document, the phytate additives in the battery cell can be determined and characterized using methods and instruments known in the art. As an example, the following method can be used for testing: disassemble the battery cell, collect the electrolyte, wash and evaporate to obtain the sample powder to be tested, and perform characterization tests such as infrared and XRD. In the XRD test: Cu Kα X-rays are used, target voltage: 40 kV; target current: 40 mA. The Gonio method is used to scan at diffraction angles 2θ from 10° to 80°. The test results in one embodiment of this application are shown in Figure 1. Alternatively, the electrode components (such as positive electrode, negative electrode, separator, etc.) can be removed from the disassembled battery cell, powder is scraped off, washed and evaporated to obtain the sample powder to be tested, and the above-mentioned XRD test is performed.

[0062] In some embodiments, the phytate additive includes one or more of lithium phytate, sodium phytate, potassium phytate, zinc phytate, calcium phytate, and magnesium phytate.

[0063] When phytate additives include the above-mentioned substances, they can be adapted to the working voltage of the battery cell, ensuring that it does not decompose during battery operation, and improving the safety performance of the battery cell without affecting its electrical performance.

[0064] [Positive electrode plate]

[0065] The positive electrode includes a positive current collector and a positive electrode film layer disposed on at least one side of the positive current collector, the positive electrode film layer including a positive active material.

[0066] As an example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive current collector.

[0067] In some embodiments, the positive electrode active material includes nickel, and the molar percentage of nickel in the positive electrode active material is greater than or equal to 80% based on the total number of moles of transition metal elements in the positive electrode active material, and can be selected as 90%-96%.

[0068] As used herein, the molar percentage of transition metal elements in the positive electrode active material can be determined using instruments and methods known in the art. As an example, it can be determined as follows: 0.5 g of the test material is scraped from the positive electrode film and immersed in 100 mL of aqua regia for digestion at 50 °C. The completely dissolved solution is then subjected to inductively coupled plasma (ICP) testing to detect the content of transition metals (such as Ni, Co, Mn ions) in the solution. The molar percentage of nickel in the positive electrode active material is calculated by dividing the number of moles of nickel by the total number of moles of transition metal elements.

[0069] The nickel content in the positive electrode active material meets the above-mentioned range, enabling the positive electrode active material to have a high specific capacity, which is beneficial for further improving the energy density of the battery cell. However, with the increase of nickel content, the oxygen release amount and oxygen release rate of the positive electrode under full charge also increase, leading to an increased probability of thermal runaway and a deterioration in the safety performance of the battery cell. The technical solution in the embodiments of this application is particularly suitable for this positive electrode sheet, which can further improve the energy density of the battery cell while reducing the probability of battery thermal runaway and improving safety performance, thus meeting performance requirements.

[0070] In some embodiments, the phytate additive is disposed in the positive electrode film layer, and the mass content of the phytate additive is 0.1%-2% based on the total mass of the positive electrode film layer, optionally 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, or a range between any two of the above values. In some embodiments, the mass content of the phytate additive is 0.1%-1.5% based on the total mass of the positive electrode film layer.

[0071] The active oxygen generated by the positive electrode active material enters the electrolyte from the positive electrode film. Placing phytate additives in the positive electrode film allows the active oxygen to interact with the phytate additives while active oxygen is being generated at the positive electrode, thereby reducing the activity of the active oxygen and the degree of oxidation reaction between active oxygen and the electrolyte / negative electrode, and improving the safety performance of the battery cell. However, the phytate additives occupy space in the positive electrode active material, which is not conducive to improving the energy density of the battery cell. Controlling the mass content of phytate additives in the positive electrode film to meet the above-mentioned range can improve the safety performance of the battery cell while also increasing its energy density.

[0072] In some embodiments, the phytate additive is disposed on the surface of the positive electrode film layer away from the current collector side.

[0073] Phytate additives placed at the above-mentioned locations can come into contact with the generated reactive oxygen species, reducing the reactivity of the reactive oxygen species, decreasing the probability of oxidation reactions between the reactive oxygen species and the solvent in the electrolyte / active material in the negative electrode, reducing the heat of the reaction, and improving the safety performance of the battery cell.

[0074] In some embodiments, the phytate additive is disposed in the coating, and the thickness of the coating with the phytate additive is 1 micrometer (μm) to 10 μm, optionally 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, or any range between two of the above values. In some embodiments, the thickness of the coating with the phytate additive is 2 μm to 4 μm.

[0075] It is understandable that the thickness of the coating with phytate additives can be tested using instruments and methods known in the art, such as scanning electron microscopy.

[0076] Placing phytate additives in the coating at the aforementioned locations on the battery cell can improve the safety performance of the battery cell. However, the coating inevitably occupies internal space within the battery cell, and an excessively thick coating, in particular, will occupy space in the positive electrode film layer, which is detrimental to improving the energy density of the battery cell. Controlling the coating thickness to meet the above-mentioned range can improve the safety performance of the battery cell while also considering its energy density.

[0077] The types of positive electrode active materials used in this application can be selected by those skilled in the art based on the different types of battery cells.

[0078] In some embodiments, the battery cell is a lithium-ion battery, and the positive electrode active material has the components shown in the following general formula: Li a1 Ni x1 Co y1 M1 z1 M2 w1 O2-b1 Wherein, M1 includes one or more of Mn and Al, and M2 includes one or more of Zr, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, and K; 0.8≤a1≤1.2, 0.8≤x1≤1, 0≤y1≤0.2, 0≤z1≤0.2, 0≤w1≤0.1, and -0.1≤b1≤0.1.

[0079] In some embodiments, a1 can be selected as 0.8, 0.85, 0.9, 0.95, 1.0, 1.05, 1.1, 1.15, 1.2, or a range between any two of the above values. In some embodiments, x1 can be selected as 0.8, 0.82, 0.84, 0.86, 0.88, 0.90, 0.92, 0.94, 0.96, 0.98, 1.0, or a range between any two of the above values. In some embodiments, y1 can be selected as 0, 0.02, 0.04, 0.06, 0.08, 0.10, 0.12, 0.14, 0.16, 0.18, 0.2, or a range between any two of the above values. In some embodiments, z1 can be selected as 0, 0.02, 0.04, 0.06, 0.08, 0.10, 0.12, 0.14, 0.16, 0.18, 0.2, or a range between any two of the above values. In some embodiments, w1 can be selected as 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 1.0, or a range between any two of the above values. In some embodiments, b1 can be selected as -0.1, -0.08, -0.06, -0.04, -0.02, 0, 0.02, 0.04, 0.06, 0.08, 1.0, or a range between any two of the above values.

[0080] Lithium-containing transition metal oxide ternary cathode active materials have high capacity and are the preferred materials for high energy density batteries. When the cathode active material includes the above-mentioned types of active materials, it is beneficial to further improve the energy density of the battery cell.

[0081] In some embodiments, the battery cell is a sodium-ion battery, and the positive electrode active material has the components shown in the following general formula: Na a2 Ni x2 Co y2 M3 z2 M4 w2 O 2-b2M3 includes one or more of Mn and Al, and M4 includes one or more of Zr, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, and K; 0.8≤a2≤1.2, 0.8≤x2≤1, 0≤y2≤0.2, 0≤z2≤0.2, 0≤w2≤0.1, and -0.1≤b2≤0.1.

[0082] In some embodiments, a2 can be selected as 0.8, 0.85, 0.9, 0.95, 1.0, 1.05, 1.1, 1.15, 1.2, or a range between any two of the above values. In some embodiments, x2 can be selected as 0.8, 0.82, 0.84, 0.86, 0.88, 0.90, 0.92, 0.94, 0.96, 0.98, 1.0, or a range between any two of the above values. In some embodiments, y2 can be selected as 0, 0.02, 0.04, 0.06, 0.08, 0.10, 0.12, 0.14, 0.16, 0.18, 0.2, or a range between any two of the above values. In some embodiments, z2 can be selected as 0, 0.02, 0.04, 0.06, 0.08, 0.10, 0.12, 0.14, 0.16, 0.18, 0.2, or a range between any two of the above values. In some embodiments, w2 can be selected as 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 1.0, or a range between any two of the above values. In some embodiments, b2 can be selected as -0.1, -0.08, -0.06, -0.04, -0.02, 0, 0.02, 0.04, 0.06, 0.08, 1.0, or a range between any two of the above values.

[0083] Sodium-ion batteries using sodium-containing transition metal oxides as positive electrode active materials have a high theoretical specific capacity, which is beneficial for improving the energy density of sodium-ion batteries.

[0084] In some embodiments, the positive current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0085] In some embodiments, the positive electrode film layer may optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resin.

[0086] In some embodiments, the positive electrode film may optionally include a conductive agent. As an example, the conductive agent may include at least one selected from superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0087] In some embodiments, the positive electrode sheet can be prepared by dispersing the above-mentioned components for preparing the positive electrode film layer, such as positive electrode active material, conductive agent, binder and any other components, in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode film layer slurry; coating the positive electrode film layer slurry onto the surface of the base coating layer, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0088] [Negative electrode plate]

[0089] In some embodiments, the negative electrode includes a negative current collector and a negative electrode film layer disposed on at least one side of the negative current collector. A phytate additive is disposed in the negative electrode film layer. Based on the total mass of the negative electrode film layer, the mass content of the phytate additive is 0.1%-2%, optionally 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, or a range between any two of the above values. In some embodiments, based on the total mass of the negative electrode film layer, the mass content of the phytate additive is 0.1%-1.5%.

[0090] Adding phytate additives to the negative electrode film can reduce the reactivity of active oxygen in contact with the negative electrode, reduce the degree of oxidation side reactions between active oxygen and the negative electrode material, and improve the safety performance of the battery cell.

[0091] In some embodiments, based on the total mass of the negative electrode film, the silicon content in the negative electrode film is 5%-50%, selectable as 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, or any range between two of the above values. In some embodiments, based on the total mass of the negative electrode film, the silicon content in the negative electrode film is 9%-45%.

[0092] High silicon content negative electrode active materials have higher theoretical specific capacity. Controlling the mass content of silicon in the negative electrode active material to meet the above-mentioned range is beneficial to improving battery capacity and can form a good match with high nickel content positive electrode active materials, ensuring effective insertion / extraction of cations between the positive and negative electrodes, and further improving the energy density of the battery cell. However, the active oxygen released from the positive electrode can react with the negative electrode active material to generate byproducts (such as silicates), and the heat generated can easily cause thermal runaway of the battery. The technical solution provided in this application is particularly suitable for this negative electrode sheet, which can improve the energy density of the battery cell while reducing the intensity of the oxidation side reaction and improving safety performance.

[0093] In some embodiments, the phytate additive is disposed on the surface of the negative electrode film layer away from the negative electrode current collector.

[0094] In some embodiments, the phytate additive is disposed in the coating, and the thickness of the coating with the phytate additive is 1 μm-10 μm, optionally 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, or any range between two of the above values. In some embodiments, the thickness of the coating with the phytate additive is 2 μm-4 μm.

[0095] Incorporating phytate additives into the coating at the aforementioned locations on the battery cell can improve the safety performance of the battery cell. Controlling the coating thickness within the aforementioned range allows for both improved safety performance and high energy density in the battery cell.

[0096] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0097] The types of negative electrode active materials used in this application can be selected by those skilled in the art based on the different types of battery cells.

[0098] In some embodiments, the negative electrode active material may be a negative electrode active material known in the art for use in batteries. As an example, the negative electrode active material may include at least one of the following materials: elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. However, this application is not limited to these materials, and other conventional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0099] In some embodiments, the negative electrode film layer may optionally include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0100] In some embodiments, the negative electrode film may optionally include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0101] In some embodiments, the negative electrode film may optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).

[0102] In some embodiments, the negative electrode sheet can be prepared by dispersing the components used to prepare the negative electrode sheet, such as the negative electrode active material, conductive agent, binder and any other components, in a solvent (e.g., deionized water) to form a negative electrode slurry; coating the negative electrode slurry onto the negative electrode current collector, and then obtaining the negative electrode sheet after drying, cold pressing and other processes.

[0103] Electrolyte

[0104] In some embodiments, the phytate additive is disposed in the electrolyte, and the mass content of the phytate additive is 0.1%-5% based on the total mass of the electrolyte, optionally 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, or a range between any two of the above values. In some embodiments, the mass content of the phytate additive is 0.3%-1% based on the total mass of the electrolyte.

[0105] The reactive oxygen released from the positive electrode active material undergoes an oxidation reaction with the electrolyte. Dissolving the phytate additive in the electrolyte allows it to contact the reactive oxygen, reducing its reactivity and thus the intensity of the oxidation reaction. This reduces the probability of thermal runaway in the battery cell and improves its safety performance. Controlling the phytate additive content in the electrolyte within the aforementioned range ensures its complete dissolution, allowing it to directly contact and reduce the activity of reactive oxygen, further enhancing the safety performance of the battery cell.

[0106] The composition of the electrolyte in this application can be selected by those skilled in the art based on the different types of battery cells.

[0107] In some embodiments, the battery cell is a lithium-ion battery, and the electrolyte in the lithium-ion battery includes a solvent and an electrolyte salt. The solvent in the lithium-ion battery includes one or more of carboxylic acid ester solvents, carbonate solvents, and ether solvents.

[0108] When used herein, the composition and components of the electrolyte can be determined using instruments and methods known in the art. As an example, the following methods can be used to characterize the composition and content of the electrolyte: gas chromatography-mass spectrometry (GC-MS), ion chromatography (IC), liquid chromatography (LC), nuclear magnetic resonance spectroscopy (NMR), and gas chromatography-mass spectrometry (GC-MS). For example, referring to GB / T-9722-2006 "General Rules for Gas Chromatography of Chemical Reagents" and / or GB / T6041-2002 "General Rules for Mass Spectrometry Analysis Methods," gas chromatography and mass spectrometry are coupled. After gas chromatography separates the components in the sample, the components are broken into ion fragments in mass spectrometry, separated according to their mass-to-charge ratio (m / z) to form specific mass spectra, obtaining qualitative analysis of each organic component in the electrolyte. Then, the organic components in the electrolyte are separated in the chromatographic column, generating detection signal spectra for each component. Component qualitative analysis is performed using retention time, and quantitative analysis is achieved by standardizing and correcting peak areas, obtaining quantitative analysis of the organic components in the electrolyte. Referring to JY / T-020, ion chromatography is used to detect and quantify the types of anions of electrolyte salts in the electrolyte. Referring to JY / T 0578-2020, nuclear magnetic resonance spectroscopy (NMR) is used to obtain qualitative and quantitative analysis of the components in the electrolyte.

[0109] In some embodiments, the electrolyte salt in the lithium-ion battery includes one or more of lithium hexafluorophosphate (LiPF6), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium dioxolaneborate (LiBOB), and lithium perchlorate (LiClO4).

[0110] The electrolyte of lithium-ion batteries contains the above-mentioned electrolyte salts, which can dissociate lithium ions in the electrolyte, improve the liquid phase dispersion ability of lithium ions, and help to further improve the energy density of the battery cell.

[0111] In some embodiments, the battery cell is a sodium-ion battery, and the electrolyte in the sodium-ion battery includes a solvent and an electrolyte salt. The solvent includes one or more of carbonate solvents and ether solvents.

[0112] In some embodiments, the electrolyte salt in the sodium-ion battery includes one or more of sodium hexafluorophosphate (NaPF6), sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), sodium bis(fluorosulfonyl)imide (NaFSI), sodium di(oxalato)borate (NaBOB), and sodium perchlorate (NaClO4).

[0113] In some embodiments, the electrolyte may optionally include additives. For example, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature or low-temperature performance, etc.

[0114] [Isolation membrane]

[0115] In some embodiments, the battery cell also includes a separator. This application does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be selected.

[0116] In some embodiments, the material of the separator can be selected from at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0117] In some embodiments, the phytate additive is disposed on the surface of the separator near the positive electrode side.

[0118] In some embodiments, the phytate additive is disposed in the coating, and the thickness of the coating with the phytate additive is 1 μm-10 μm, optionally 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, or any range between two of the above values. In some embodiments, the thickness of the coating with the phytate additive is 2 μm-4 μm.

[0119] Incorporating phytate additives into the coating at the aforementioned locations on the battery cell can improve the safety performance of the battery cell. Controlling the coating thickness within the aforementioned range allows for both improved safety performance and high energy density in the battery cell.

[0120] [Battery cell]

[0121] In some implementations, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly using a winding or stacking process.

[0122] In some embodiments, the battery cell may include an outer packaging. This outer packaging can be used to encapsulate the electrode assembly and electrolyte described above.

[0123] In some implementations, the heat generation rate of the positive electrode in the battery cell is 60 milliwatts (mW) to 100 mW.

[0124] In this document, the heat generation rate of the positive electrode has a meaning known in the art. As an example, it can be determined using the following method: A fully charged battery is disassembled to obtain a fully charged positive electrode. The electrode is then cut into small circular pieces with a diameter of 5 mm and placed in a stainless steel sealed crucible commonly used in DSC (Differential Scanning Calorimetry) equipment. 1.5 μL of electrolyte is injected, and the threads of the sealed crucible are tightened. Finally, the crucible is placed in a DSC device for testing, with a heating rate of 10 °C / min and a temperature range of 30–460 °C. Based on the test results, the ordinate of the DSC curve represents the heat generation rate of the positive electrode, in mW.

[0125] In some implementations, the combustion spread rate of the bare battery cell is less than or equal to 2.5 cm / s.

[0126] In this paper, the combustion propagation rate of a bare battery cell can be determined using the following method: The battery cell is disassembled after full charging, and the positive and negative electrode plates in their fully charged state are obtained. These plates are cleaned with an organic solvent (such as dimethyl carbonate, DMC) and then cut to appropriate sizes. A separator is then placed between the positive and negative electrode plates to construct a single-layer stacked battery cell, which is then installed in a transparent stacked battery casing, and electrolyte is injected. On one side of the transparent stacked battery, the positive and negative electrode plates are ignited using laser heating. The propagation process of the ignited plates is recorded using a high-speed camera, and the propagation rate is calculated in cm / s.

[0127] In some embodiments, the outer packaging of the battery cell can be a rigid shell, such as a hard plastic shell, an aluminum shell, or a steel shell. The outer packaging of the battery cell can also be a flexible package, such as a pouch. The material of the flexible package can be plastic; examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0128] This application does not impose any particular limitation on the shape of the battery cell; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 3 shows a square battery cell 5 as an example.

[0129] In some embodiments, referring to FIG4, the outer packaging may include a housing 51 and a cover plate 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover plate 53 can be placed over the opening to close the receiving cavity. The positive electrode sheet, negative electrode sheet, and separator may be formed into an electrode assembly 52 by a winding process or a stacking process. The electrode assembly 52 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the battery cell 5 may be one or more, which can be selected by those skilled in the art according to specific practical needs.

[0130] [Battery Device]

[0131] This application also provides a battery device, which includes the battery cell provided in this application. In some embodiments, the battery device is one or more of a battery module, a battery pack, and an energy storage device.

[0132] In some implementations, individual battery cells can be assembled into a battery module. The number of individual battery cells contained in a battery module can be one or more, and the specific number can be selected by those skilled in the art based on the application and capacity of the battery module.

[0133] Figure 5 shows a battery module 4 as an example. Referring to Figure 5, in the battery module 4, multiple battery cells 5 can be arranged sequentially along the length of the battery module 4. Of course, they can also be arranged in any other manner. Furthermore, the multiple battery cells 5 can be fixed in place using fasteners.

[0134] Optionally, the battery module 4 may also include a housing with a receiving space in which multiple battery cells 5 are received.

[0135] In some embodiments, the battery modules described above can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be one or more, the specific number of which can be selected by those skilled in the art according to the application and capacity of the battery pack.

[0136] Figures 6 and 7 illustrate a battery pack 1 as an example. Referring to Figures 6 and 7, the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0137] [Electrical appliances]

[0138] In addition, this application also provides an electrical device, which includes at least one of the battery cell, battery module, or battery pack provided in this application. The battery cell, battery module, or battery pack can be used as the power source of the electrical device or as the energy storage unit of the electrical device. The electrical device may include, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.

[0139] As an electrical device, you can choose individual battery cells, battery modules, or battery packs according to your usage requirements.

[0140] Figure 8 shows an example of an electrical device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. To meet the high power and high energy density requirements of the individual battery cells, a battery pack or battery module can be used.

[0141] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use a single battery cell as their power source.

[0142] Example

[0143] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0144] I. Preparation Method

[0145] Example 1

[0146] 1) Preparation of positive electrode sheet

[0147] LiNi, the positive electrode active material 0.96 Co 0.03 Mn 0.01 O2, conductive carbon black, and polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 98:1:1, and then N-methylpyrrolidone solvent was added and stirred until homogeneous to obtain the positive electrode slurry. The positive electrode slurry was then prepared at a concentration of 30 mg / cm². 2 The coating quality is applied to both surfaces of the positive electrode current collector aluminum foil, and after drying, cold pressing, die cutting, and slitting, the positive electrode sheet is obtained.

[0148] 2) Preparation of negative electrode sheet

[0149] The negative electrode active materials silicon carbide, conductive carbon black, polystyrene-butadiene rubber (SBR), and carboxymethyl cellulose were mixed in a mass ratio of 97.7:0.7:1:0.6, then added to water and stirred until homogeneous to obtain a negative electrode slurry. The negative electrode slurry was coated onto both surfaces of the negative electrode current collector copper foil, and after drying and cold pressing, a negative electrode sheet was obtained.

[0150] 3) Preparation of the separating membrane

[0151] A 7μm polyethylene film was used as the base film. A slurry was formed by dissolving boehmite-ceramic binder PVDF in NMP solvent. The slurry was then applied to both sides of the base film using a gravure roller. The coating speed was set at 30 m / min, and the coating thickness was 1.5 μm on each side. After coating, the film was dried in an oven at 70℃ to obtain the release film.

[0152] 4) Preparation of electrolyte

[0153] Dimethyl carbonate and ethylene carbonate were mixed in a mass ratio of 7:3 to obtain a mixed solvent. Then, fully dried lithium salt LiPF6 was dissolved in the mixed organic solvent to prepare an electrolyte with a lithium salt concentration of 1 mol / L. Then, lithium phytate additive was added.

[0154] 5) Battery assembly

[0155] The negative electrode, separator, and positive electrode are arranged in sequence, with the separator positioned between the negative and positive electrodes to provide isolation. The electrodes are then stacked and the tabs are welded to obtain the electrode assembly. The electrode assembly is placed in a steel casing, and the prepared electrolyte is injected. After encapsulation, settling, formation, and capacity testing, a single battery cell is obtained.

[0156] Based on the total mass of the electrolyte, the phytate additive has a mass content of 1%; based on the total mass of the negative electrode film, the silicon content in the negative electrode film is 45%.

[0157] Example 2-10

[0158] The battery cells in Examples 2-10 are prepared in a similar manner to those in Example 1, except that the type and mass content of phytate additives and the type of positive electrode active material are changed. The specific preparation parameters are shown in Table 1.

[0159] Comparative Example 1

[0160] The preparation method of the battery cell in Comparative Example 1 is similar to that in Example 1, except that no phytate additive is added to the electrolyte. The specific preparation parameters are shown in Table 1.

[0161] Comparative Example 2

[0162] Comparative Example 2 is similar to the preparation method of the battery cell in Example 1, except that a non-phytate additive, triethylenediamine, is added to the electrolyte. The specific preparation parameters are shown in Table 1.

[0163] Table 1

[0164] Examples 11-14

[0165] The battery cell in Example 11 is prepared in a similar manner to the battery cell in Example 1, except that no phytate additive is added to the electrolyte of the battery cell, and the preparation of the positive electrode is adjusted to the following steps: The positive electrode active material LiNi... 0.96 Co 0.03 Mn 0.01 O2, conductive carbon black, polyvinylidene fluoride (PVDF), and phytate additive lithium phytate are mixed in a mass ratio of 97:1:1:1, and then N-methylpyrrolidone solvent is added and stirred until homogeneous to obtain a positive electrode slurry. The positive electrode slurry is coated on both surfaces of the positive electrode current collector aluminum foil, and after drying, cold pressing, die cutting, and slitting, the positive electrode sheet is obtained.

[0166] The battery cells in Examples 12-14 are prepared in a similar manner to those in Example 11, except that the types of phytate additives are adjusted. The specific preparation parameters are shown in Table 2.

[0167] Table 2

[0168] Examples 15-17

[0169] The preparation method of the battery cell in Example 15 is similar to that in Example 1, except that the preparation steps of the positive electrode and electrolyte of the battery cell are adjusted as follows:

[0170] 1-1) Preparation of additive coating

[0171] Phytate additive lithium phytate and binder PVDF are mixed at a mass ratio of 9:1, and then N-methylpyrrolidone solvent is added and stirred evenly to obtain additive slurry.

[0172] 1-2) Preparation of positive electrode sheet

[0173] The positive electrode slurry from Example 1 was coated on both surfaces of the positive electrode current collector aluminum foil. After drying to form a positive electrode film, the additive slurry was coated on the surface of the positive electrode film. Then, after drying, cold pressing, die cutting, and slitting, a positive electrode sheet with an additive coating on the surface was obtained.

[0174] The thickness of the additive coating is 2μm.

[0175] 4-1) No phytate additives are added to the electrolyte.

[0176] The battery cells in Examples 16-17 are prepared in a similar manner to those in Example 15, except that the coating position of the additive coating is adjusted. The specific preparation parameters are shown in Table 3.

[0177] Table 3

[0178] Example 18

[0179] The battery cell in Example 18 is prepared using a similar method to the battery cell in Example 1, except that phytate additives are not added to the electrolyte, and the preparation of the negative electrode sheet is adjusted as follows: The negative electrode active material silicon carbide, conductive carbon black, polystyrene-butadiene rubber (SBR), carboxymethyl cellulose, and phytate additive lithium phytate are mixed in a mass ratio of 96.7:0.7:1:0.6:1 and then added to water. The mixture is stirred until homogeneous to obtain a negative electrode slurry. The negative electrode slurry is coated onto both surfaces of the negative electrode current collector copper foil, and after drying and cold pressing, a negative electrode sheet is obtained.

[0180] II. Performance Testing

[0181] 1. Test method for energy density of a single battery cell

[0182] (1) The formed battery was tested using the Xinwei CT-4016-5V30A charge-discharge instrument. First, it was left to stand for 5 hours at 25℃. (2) It was charged at a constant current of 0.33C to 4.3V. (3) The battery was charged at a constant voltage of 4.3V until the current was ≤0.05C, and the first charge capacity E0 (Ah) was obtained. (4) It was left to stand for 5 minutes at 25℃. (5) It was discharged at a constant current of 0.33C to 2.5V, and the first discharge capacity E1 (Ah) was obtained. (6) It was left to stand for 30 minutes at 25℃. (7) The median discharge voltage V0 of the battery in the instrument was read. The discharge capacity E1 in step (5) was multiplied by the median discharge voltage V0 to obtain the discharge energy W0 (Wh) of the battery. (8) The discharge energy W0 in step 7 was divided by the weight of the single cell to obtain the energy density of the battery (Wh / kg).

[0183] 2. Test method for heat generation rate of positive electrode in battery cell

[0184] The fully charged battery was disassembled to obtain the fully charged positive electrode sheet. The electrode sheet was then cut into small circular pieces with a diameter of 5 mm and placed in a stainless steel sealed crucible commonly used in DSC (Differential Scanning Calorimeter) equipment. 1.5 μL of the corresponding electrolyte was injected, and the threads of the sealed crucible were tightened. Finally, it was placed in a DSC device (Netzsch DSC300 Caliris Classic) for testing, with a heating rate of 10 °C / min and a temperature range of 30–460 °C. Based on the test results, the ordinate of the DSC curve represents the heat generation rate of the positive electrode sheet, in mW. The test results of the embodiment and comparative examples in this application are shown in Figure 2.

[0185] 3. Test method for the combustion spread rate of bare battery cells

[0186] The fully charged battery is disassembled to obtain the fully charged positive and negative electrode plates. After cleaning them with DMC (dimethyl carbonate) solution, they are cut into appropriate sizes. Then, the above-mentioned separator is placed between the positive and negative electrode plates to construct a single-layer stacked battery bare cell, which is then installed in a transparent stacked battery casing and injected with the corresponding electrolyte.

[0187] On one side of the transparent stacked battery, the positive and negative electrode sheets are ignited by laser heating. The spread process of the ignited electrode sheets is recorded by a high-speed camera, and the spread rate is calculated in cm / s.

[0188] 4. Test method for the termination of directional pressure relief time of a single battery cell

[0189] An internal heating film was added to the prepared aluminum-cased battery, and then the aluminum-cased battery cells were fully charged to 4.3V. The internal heating film was started with a constant power of 400W until the battery experienced thermal runaway and ignited. The time of flame ejection from the explosion-proof valve was recorded. The timing was stopped when the battery combustion ended or flames were ejected from other parts of the battery casing (such as the casing weld). This time was the battery's termination directional pressure relief time.

[0190] III. Analysis of Test Results for Each Embodiment and Comparative Example

[0191] Battery cells for each embodiment and comparative example were prepared according to the above method, and various performance parameters were measured. The results are shown in Table 4 below.

[0192] Table 4

[0193] As can be seen from the comparison of Examples 1-18 and Comparative Examples 1-2 in Table 4, the addition of phytate additives to the battery can reduce the heat generation rate and combustion spread rate of the electrode in the battery cell, and effectively prolong the orientation time after thermal runaway. This can effectively reduce the risk and intensity of thermal runaway, and reduce the risk of a larger-scale thermal runaway after battery cell failure. At the same time, it can also reduce the polarization inside the battery cell, which is beneficial to the capacity of the battery cell, so that the battery cell has both high energy density and good safety performance. As can be seen from the results of Comparative Example 2, compared with the non-phytate additive triethylenediamine, although it can reduce the heat generation rate of the electrode and the combustion spread rate of the bare cell, it cannot be practically applied to the battery cell. The termination orientation pressure relief time after battery thermal runaway cannot meet the requirements of practical applications. Phytate additives can reduce the risk of thermal runaway from three levels: positive electrode, bare cell, and battery cell, and improve the safety performance of the battery cell.

[0194] As can be seen from the comparison of Examples 1-4 in Table 4, when the phytate additive in the battery cell includes phytates such as lithium phytate, sodium phytate, zinc phytate, and calcium phytate, it can improve the safety performance of the battery cell without affecting its electrical performance. As can be seen from the comparison of Examples 1 and 5-9 in Table 4, when the phytate additive is placed in the electrolyte, the mass content of the phytate additive is 0.1-5% based on the total mass of the electrolyte, which can ensure that the phytate is fully dissolved in the electrolyte and effectively reduce the probability of thermal runaway of the battery cell. Furthermore, controlling the mass content of the phytate additive to 0.3%-1% can further reduce the intensity of the oxidation reaction in the electrolyte, so that the battery cell can have both high energy density and good safety performance.

[0195] As can be seen from the comparison of Examples 1 and 10 in Table 4, the nickel content in the positive electrode active material is greater than or equal to 80%, and further 90%-96%, which enables the positive electrode active material to have a high specific capacity. This is beneficial to improving the energy density of the battery cell while reducing the probability of battery thermal runaway and improving safety performance.

[0196] As can be seen from the comparison of Examples 11-14 in Table 4, the phytate additive can also effectively reduce the intensity of thermal runaway reaction and improve the safety performance of the battery cell when it is placed in the positive electrode film layer. Further controlling the mass content of the phytate additive in the positive electrode film layer to meet 0.1%-1.5% can improve the safety performance of the battery cell while also increasing the energy density of the battery cell.

[0197] As can be seen from the comparison of Examples 1, 11, and 15-18 in Table 4, placing phytate additives in the electrolyte, in the positive electrode film layer, and preparing coatings that are placed on the surface of the positive electrode sheet, the surface of the negative electrode sheet, and at least one side of the separator can enable the battery cell to have high energy density and good safety performance.

[0198] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.

Claims

1. A battery cell, the battery cell comprising a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte, wherein the positive electrode comprises a positive current collector and a positive electrode film disposed on at least one side of the positive current collector, the positive electrode film comprising a positive active material, characterized in that, The battery cell also includes phytate additives.

2. The battery cell according to claim 1, characterized in that, The phytate additive includes one or more of lithium phytate, sodium phytate, potassium phytate, zinc phytate, calcium phytate, and magnesium phytate.

3. The battery cell according to claim 1 or 2, characterized in that, The positive electrode active material includes nickel. Based on the total number of moles of transition metal elements in the positive electrode active material, the molar percentage of nickel in the positive electrode active material is greater than or equal to 80%, and can be selected as 90%-96%.

4. The battery cell according to any one of claims 1 to 3, characterized in that, The phytate additive is disposed in the electrolyte, and the mass content of the phytate additive is 0.1%-5% based on the total mass of the electrolyte, optionally 0.3%-1%.

5. The battery cell according to any one of claims 1 to 3, characterized in that, The phytate additive is disposed in the positive electrode film layer, and the mass content of the phytate additive is 0.1%-2%, optionally 0.1%-1.5%, based on the total mass of the positive electrode film layer.

6. The battery cell according to any one of claims 1 to 3, characterized in that, The negative electrode sheet includes a negative current collector and a negative electrode film layer disposed on at least one side of the negative current collector. The phytate additive is disposed in the negative electrode film layer. Based on the total mass of the negative electrode film layer, the mass content of the phytate additive is 0.1%-2%, optionally 0.1%-1.5%.

7. The battery cell according to any one of claims 1 to 3, characterized in that, The phytate additive is disposed on the surface of the positive electrode film layer away from the positive electrode current collector; The phytate additive is disposed on the surface of at least one side of the separator membrane; and / or, The phytate additive is disposed on the surface of the negative electrode film layer away from the negative electrode current collector.

8. The battery cell according to claim 7, characterized in that, The phytate additive is disposed in the coating, and the thickness of the coating with the phytate additive is 1μm-10μm, optionally 2μm-4μm.

9. The battery cell according to any one of claims 1 to 8, characterized in that, Based on the total mass of the negative electrode film, the mass content of silicon in the negative electrode film is 5%-50%, and can be selected as 9%-45%.

10. The battery cell according to any one of claims 1 to 9, characterized in that, The battery cell is a lithium-ion battery, and the positive electrode active material has the following components represented by the general formula: Li a1 Ni x1 Co y1 M1 z1 M2 w1 O 2-b1 Wherein, M1 includes one or more of Mn and Al, and M2 includes one or more of Zr, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, and K; 0.8≤a1≤1.2, 0.8≤x1≤1, 0≤y1≤0.2, 0≤z1≤0.2, 0≤w1≤0.1, and -0.1≤b1≤0.

1.

11. The battery cell according to claim 10, characterized in that, The electrolyte in the lithium-ion battery includes a solvent and an electrolyte salt. The solvent in the lithium-ion battery includes one or more of carboxylic acid ester solvents, carbonate solvents, and ether solvents.

12. The battery cell according to claim 10 or 11, characterized in that, The electrolyte salt in the lithium-ion battery includes one or more of lithium hexafluorophosphate (LiPF6), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium dioxaborate (LiBOB), and lithium perchlorate (LiClO4).

13. The battery cell according to any one of claims 1 to 9, characterized in that, The battery cell is a sodium-ion battery, and the positive electrode active material has the following components represented by the general formula: Na a2 Ni x2 Co y2 M3 z2 M4 w2 O 2-b2 M3 includes one or more of Mn and Al, and M4 includes one or more of Zr, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, and K; 0.8≤a2≤1.2, 0.8≤x2≤1, 0≤y2≤0.2, 0≤z2≤0.2, 0≤w2≤0.1, and -0.1≤b2≤0.

1.

14. The battery cell according to claim 13, characterized in that, The electrolyte in the sodium-ion battery includes a solvent and an electrolyte salt, wherein the solvent includes one or more of carbonate solvents and ether solvents.

15. The battery cell according to claim 13 or 14, characterized in that, The electrolyte salt in the sodium-ion battery includes one or more of sodium hexafluorophosphate (NaPF6), sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), sodium bis(fluorosulfonyl)imide (NaFSI), sodium di(oxalato)borate (NaBOB), and sodium perchlorate (NaClO4).

16. The battery cell according to any one of claims 1 to 15, characterized in that, The heat generation rate of the positive electrode in the battery cell is 60mW-100mW.

17. The battery cell according to any one of claims 1 to 16, characterized in that, The combustion spread rate of the bare battery cell is less than or equal to 2.5 cm / s.

18. A battery device, characterized in that, The battery device comprises the battery cell according to any one of claims 1 to 17.

19. An electrical appliance, characterized in that, The electrical device includes a battery cell as described in any one of claims 1 to 18 or a battery device as described in claim 18.

20. An energy storage device, characterized in that, The energy storage device includes a battery cell as described in any one of claims 1 to 18 or a battery device as described in claim 18.