Electrode assembly, secondary battery comprising same, and lamination roller for manufacturing same

The electrode assembly design with electrolyte flow regions and contact regions addresses incomplete impregnation issues, improving electrolyte penetration and maintaining adhesion and strength, thus enhancing battery performance and safety.

WO2026235254A1PCT designated stage Publication Date: 2026-11-12LG ENERGY SOLUTION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2026/000197
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-01-05
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing secondary batteries face issues with incomplete electrolyte impregnation, leading to increased resistance, reduced performance, and safety risks, while attempts to enhance impregnation often compromise adhesion and strength between the electrode and separator.

Method used

An electrode assembly design with alternating electrolyte flow regions and contact regions between the electrode and separator, allowing electrolyte flow paths while maintaining adhesion and strength, using a lamination roller to form these regions during manufacturing.

Benefits of technology

Maximizes electrolyte impregnation, minimizes adhesion reduction, and strengthens the electrode assembly, enhancing battery performance and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2026000197_12112026_PF_FP_ABST
    Figure KR2026000197_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to an electrode assembly, a secondary battery comprising same, and a lamination roller for manufacturing same and, more particularly, to an electrode assembly, a secondary battery comprising same, and a lamination roller for manufacturing same, in which an electrolyte flow region through which an electrolyte can flow is formed in a portion of an interface between an electrode and a separator to maximize an electrolyte impregnation degree of the electrode assembly, and at the same time, to minimize a decrease in adhesive strength between the electrode and the separator and a decrease in strength of the electrode assembly.
Need to check novelty before this filing date? Find Prior Art

Description

Electrode assembly, secondary battery including the same, and lamination roller for manufacturing the same

[0001] Cross-citation with related applications

[0002] This application claims the benefit of priority based on Korean Patent Application No. 10-2025-0059835 dated May 8, 2025, and all contents disclosed in the document of said Korean Patent Application are incorporated herein as part of this specification.

[0003] Technology field

[0004] The present invention relates to an electrode assembly, a secondary battery including the same, and a lamination roller for manufacturing the same. Specifically, the invention relates to an electrode assembly, a secondary battery including the same, and a lamination roller for manufacturing the same, wherein an electrolyte flow region is formed at a portion of the interface between the electrode and the separator to allow the electrolyte to flow, thereby maximizing the electrolyte impregnation of the electrode assembly while simultaneously minimizing the reduction in adhesion between the electrode and the separator and the weakening of the electrode assembly's strength.

[0005]

[0006] Secondary batteries are energy storage devices with high energy density that are capable of charging and discharging through the reversible conversion of chemical and electrical energy, and are widely used in small electronic devices such as mobile phones and laptops. Recently, in response to environmental issues, high oil prices, and the need for energy efficiency and storage, their applications are rapidly expanding into hybrid electric vehicles (HEV), plug-in hybrid electric vehicles (PHEV), electric bicycles (e-bike), and energy storage systems (ESS).

[0007] Examples of secondary batteries include a jellyroll (wound type) electrode assembly having a structure in which long sheet-type positive and negative electrodes are wound with a separator interposed therein, a stack type (stacked type) electrode assembly having a structure in which a plurality of positive and negative electrodes cut into units of a predetermined size are sequentially stacked with a separator interposed therein, and a stack-folding type electrode assembly having a structure in which unit cells, for example, bi-cells or full cells, are wound with a structure in which positive and negative electrodes of a predetermined unit are stacked with a separator interposed therein.

[0008] Meanwhile, in order for a secondary battery containing electrode assemblies as described above to have high capacity and high energy density and maintain a long lifespan, the electrode assembly contained within the battery must be completely immersed in the electrolyte so that the electrode reaction between the electrodes can occur actively.

[0009] In this case, if the electrode assembly is incompletely impregnated with the electrolyte, the reaction between the electrodes is not smooth, leading to increased resistance and a rapid decrease in output characteristics and battery capacity. Consequently, not only does this result in reduced battery performance and shortened lifespan, but the high resistance also exposes the battery to the risk of degradation or explosion.

[0010] Therefore, research on various methods to increase the electrolyte impregnation of electrode assemblies is continuously being conducted to improve the performance and safety of secondary batteries, and attempts are being made to ensure that other characteristics of the electrode assembly, such as the adhesion between the electrode and the separator or the strength of the electrode assembly, are not degraded while simultaneously increasing electrolyte impregnation.

[0011]

[0012] The present invention has been devised to solve the above-mentioned problems. The objective of the present invention is to provide an electrode assembly capable of maximizing the degree of electrolyte impregnation of the electrode assembly by forming an electrolyte flow region in which the electrolyte can flow at a part of the interface between the electrode and the separator, while simultaneously minimizing the reduction in adhesion between the electrode and the separator and the weakening of the electrode assembly's strength that may occur as a result of the formation of the electrolyte flow region; a secondary battery including the same; and a lamination roller for manufacturing the same.

[0013] The problems that the present invention aims to solve are not limited to those mentioned above, and other unmentioned problems will be clearly understood by those skilled in the art from the description below.

[0014]

[0015] To solve the above-mentioned problem, an electrode assembly according to a first embodiment of the present invention is an electrode assembly in which an electrode and a separator are alternately stacked, wherein a portion of the interface between the electrode and the separator is an electrolyte flow region in which an electrolyte flows, and the remainder is a contact region in which an electrolyte is in contact, and the electrolyte flow region includes a first region extending by a first length in a first direction from one edge of the interface toward the other edge of the interface, and a second region extending by a second length in a direction opposite to the first direction from the other edge of the interface toward one edge of the interface, wherein a first end in the extension direction of the first region and a second end in the extension direction of the second region are spaced apart from each other in a second direction intersecting the first direction, and the sum of the first length and the second length may be equal to the shortest distance between one edge of the interface and the other edge of the interface.

[0016] The first direction and the second direction may intersect perpendicularly to each other.

[0017] The above electrolyte flow region may further include a third region connecting the first end and the second end.

[0018] The third region may include a first communication region communicating with the first end, a second communication region communicating with the second end, and a third communication region communicating with the first communication region, the second communication region, the side of the first region, and the side of the second region.

[0019] A portion of the one edge of the interface may be opened by the first region, and a portion of the other edge of the interface may be opened by the second region.

[0020] The first region and the second region are each provided in multiple numbers, and the number of the second region may be greater than the number of the first region.

[0021] The first end and the second end may be alternately arranged along the second direction at a constant distance from each other.

[0022] Each of the above-mentioned first regions may be extended parallel to each other, and each of the above-mentioned second regions may be extended parallel to each other.

[0023] Each of the above first region and each of the above second region can be extended parallel to each other.

[0024] The first length may be longer than the third length, which is the second direction length of the first region.

[0025] The above third length may be 5mm or more and 10mm or less.

[0026] The second length may be longer than the fourth length, which is the second direction length of the second region.

[0027] The above fourth length may be 5mm or more and 10mm or less.

[0028] The first length and the second length may be the same as each other.

[0029] The adhesive force between the electrode and the separator in the above-mentioned contact area may be greater than the adhesive force between the electrode and the separator in the above-mentioned electrolyte flow area.

[0030] To solve the above-mentioned problem, a secondary battery according to a second embodiment of the present invention comprises an electrode assembly in which an electrode and a separator are alternately stacked, and an outer casing that accommodates the electrode assembly. A portion of the interface between the electrode and the separator is an electrolyte flow region in which an electrolyte flows, and the remainder is a contact region in which an electrolyte flows. The electrolyte flow region includes a first region extending by a first length in a first direction from one edge of the interface toward the other edge of the interface, and a second region extending by a second length in a direction opposite to the first direction from the other edge of the interface toward one edge of the interface. A first end, which is the end of the extension direction of the first region, and a second end, which is the end of the extension direction of the second region, are spaced apart from each other in a second direction that intersects the first direction. The sum of the first length and the second length is equal to the shortest distance between one edge of the interface and the other edge of the interface. An opening is formed in the outer casing for injecting an electrolyte. Each of the regions and the second region is provided in multiple numbers, and the distance between the multiple second regions and the opening is shorter than the distance between the multiple first regions and the opening, and the number of the multiple second regions may be greater than the number of the multiple first regions.

[0031] The above electrolyte flow region may further include a third flow region connecting the first end and the second end.

[0032] A degassing hole is formed in the exterior material to discharge internal gas, and the distance between the plurality of second regions and the degassing hole may be shorter than the distance between the plurality of first regions and the degassing hole.

[0033] To solve the above-mentioned problem, a lamination roller according to a third embodiment of the present invention is a lamination roller that presses an electrode assembly in which an electrode and a separator are alternately stacked, and comprises a roller member that presses the electrode assembly to bring the electrode and the separator into close contact, and a recess formed in the roller member, wherein the recess includes a first recess extending in the circumferential direction of the roller member and a second recess extending in the circumferential direction of the roller member, and the first recess and each of the second recesses are alternately arranged in an alternating manner along the circumferential direction of the roller member, and the end of the extension direction of the first recess and the end of the extension direction of the second recess may be spaced apart from each other in the longitudinal direction of the roller member.

[0034] It may further include a third recess connecting the end of the first recess in the extension direction and the end of the second recess in the extension direction.

[0035]

[0036] The electrode assembly according to the present invention, the secondary battery including the same, and the lamination roller for manufacturing the same have the effect of maximizing the degree of electrolyte impregnation of the electrode assembly by forming an electrolyte flow region in which the electrolyte can flow at a part of the interface between the electrode and the separator, while simultaneously minimizing the reduction in adhesion between the electrode and the separator and the weakening of the strength of the electrode assembly that may occur as a result of the formation of the electrolyte flow region.

[0037] The effects of the present invention are not limited to the effects described above, and unmentioned effects will be clearly understood by those skilled in the art from this specification and the attached drawings.

[0038]

[0039] FIG. 1 is an assembly diagram of a secondary battery according to a first embodiment of the present invention.

[0040] FIG. 2 is a side view of an electrode assembly according to a first embodiment of the present invention.

[0041] FIG. 3 is a plan view of the interface of an electrode assembly according to a first embodiment of the present invention.

[0042] Figure 4 is a plan view in which a third region is added to the electrolyte flow region shown in Figure 3.

[0043] Figure 5 is a magnified view of part A of Figure 4.

[0044] FIG. 6 is a drawing showing the electrolyte being injected through an opening into the outer material of a secondary battery according to a second embodiment of the present invention.

[0045] FIG. 7 is a drawing showing a degassing hole drilled in the outer material of a secondary battery according to a second embodiment of the present invention.

[0046] FIG. 8 is a drawing showing a lamination roller according to a third embodiment of the present invention manufacturing an electrode assembly.

[0047] FIG. 9 is a drawing showing the surface of a roller member of a lamination roller according to a third embodiment of the present invention.

[0048] Fig. 10 is an enlarged view of part B of Fig. 9.

[0049] Figure 11 is a photograph showing the result according to Comparative Example 1-1 of the present invention.

[0050] Figure 12 is a photograph showing the results according to Comparative Example 1-2 of the present invention.

[0051] Figure 13 is a photograph showing the result according to Manufacturing Example 1-1 of the present invention.

[0052] Figure 14 is a photograph showing the result according to Manufacturing Example 1-2 of the present invention.

[0053] Figure 15 is a photograph showing the results according to Manufacturing Example 1-3 of the present invention.

[0054] Figure 16 is a photograph showing the result according to Comparative Example 2-1 of the present invention.

[0055] Figure 17 is a photograph showing the result according to Comparative Example 2-2 of the present invention.

[0056] Figure 18 is a photograph showing the result according to Manufacturing Example 2-1 of the present invention.

[0057] Figure 19 is a photograph showing the result according to Manufacturing Example 2-2 of the present invention.

[0058]

[0059] Hereinafter, preferred embodiments of the present invention are described in detail with reference to the attached drawings so that those skilled in the art can easily implement the present invention. However, the present invention may be embodied in various different forms and is not limited or restricted by the following embodiments.

[0060] In order to clearly explain the present invention, detailed descriptions of related prior art that are irrelevant to the explanation or that may unnecessarily obscure the essence of the invention have been omitted. Furthermore, when assigning reference numerals to the components of each drawing in this specification, identical or similar reference numerals are assigned to identical or similar components throughout the entire specification.

[0061] Furthermore, terms and words used in this specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept consistent with the technical spirit of the invention, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention.

[0062]

[0063] First embodiment

[0064] FIG. 1 is an assembly diagram of a secondary battery according to a first embodiment of the present invention.

[0065] Referring to FIG. 1, the electrode assembly (10) according to the present invention may be formed in a form in which an electrode (100) and a separator (200) are alternately stacked. At this time, the electrode (100) may be composed of a positive electrode (110) and a negative electrode (120). Generally, the process of manufacturing a secondary battery involves first applying a slurry, which is a mixture of an electrode active material, a binder, and a plasticizer, to a positive electrode current collector and a negative electrode current collector to produce a positive electrode (110) and a negative electrode (120), and then stacking them on both sides of a separator (200) to form an electrode assembly (10) of a predetermined shape. Next, the electrode assembly (10) may be housed in an outer casing (20), and then sealed after injecting an electrolyte (E).

[0066] Additionally, as illustrated in FIG. 1, the electrode assembly (10) may include an electrode tab (400). The electrode tab (400) is connected to the positive electrode (110) and the negative electrode (120), respectively, and may protrude outside the electrode assembly (10) to form a path through which electrons can move between the inside and outside of the electrode assembly (10).

[0067] Additionally, an electrode lead (500) may be connected to the electrode tab (400) by spot welding or the like. Also, a portion of the electrode lead (500) may be surrounded by an insulating portion (600). The insulating portion (600) may be located in the sealing portion where the upper pouch (20a) and lower pouch (20b) of the outer material (20) are heat-fused, and the electrode lead (500) may be adhered to the outer material (20). Furthermore, it prevents electricity generated from the electrode assembly (10) from flowing to the outer material (20) through the electrode lead (500) and maintains the sealing of the outer material (20).

[0068] At this time, the electrode leads (500) may extend in the same direction or in different directions depending on the formation positions of the positive tab (410) and the negative tab (420). Additionally, a portion of the electrode leads (500) protruding outside the outer casing (20) may become a terminal portion and be electrically connected to an external terminal.

[0069] Meanwhile, the outer material (20) may be a pouch made of a flexible material. Additionally, the outer material (20) may accommodate and seal the electrode assembly (10) so that a part of the electrode lead (500), namely the terminal part (510, 520), is exposed. As shown in FIG. 1, this outer material (20) may include an upper pouch (20a) and a lower pouch (20b). The lower pouch (20b) is provided with a receiving space (S) capable of accommodating the electrode assembly (10), and the upper pouch (20a) covers the receiving space (S) from above so that the electrode assembly (10) does not escape from the outside of the outer material (20). At this time, a receiving space is also formed in the upper pouch (20a) so that a part of the electrode assembly (10) can be accommodated from above.

[0070] When an electrode lead (500) is connected to an electrode tab (400) of an electrode assembly (10) and a portion of the electrode lead (500) is surrounded by an insulating portion (600), the electrode assembly (10) is accommodated in a receiving space (S) formed in a lower pouch (20b), and the upper pouch (20a) can cover the receiving space (S) from above. Then, an electrolyte (E) is injected into the interior, and when the edges of the upper pouch (20a) and the lower pouch (20b) are sealed, a secondary battery (1) is manufactured.

[0071] FIG. 2 is a side view of an electrode assembly according to a first embodiment of the present invention. Specifically, FIG. 2 shows a unit cell according to a first embodiment of the present invention.

[0072] Referring to FIG. 2, some of the interface (300) between the electrode (100) and the separator (200) may be an electrolyte flow region (310) where the electrolyte (E) flows, and the rest may be a close contact region (320) where the electrolyte is close.

[0073] At this time, the adhesive force between the electrode (100) and the separator (200) in the contact area (320) may be greater than the adhesive force between the electrode (100) and the separator (200) in the electrolyte flow area (310). Specifically, the adhesive force between the electrode (100) and the separator (200) in the electrolyte flow area (310) may be non-existent, or even if present, it may be smaller than the adhesive force between the electrode (100) and the separator (200) in the contact area (320). Therefore, when the electrode assembly (10) is impregnated with the electrolyte (E), the electrolyte flow area (310) can function as an electrolyte flow path through which the electrolyte (E) can penetrate and move.

[0074] Specifically, in the electrolyte flow region (310) excluding the contact region (320) of the interface (300), the electrode (100) and the separator (200) are separated and not completely bonded to each other, so when the electrode assembly (10) is immersed in the electrolyte (E), a gap may be formed between the electrode (100) and the separator. This gap may function as an electrolyte flow path, allowing the electrolyte (E) to penetrate into the electrode assembly (10) through this part.

[0075] In addition, the electrolyte (E) can not only easily penetrate into the electrolyte flow region (310), but can also function as a passage for the gas to flow out when gas is generated inside the electrode assembly (10).

[0076] At this time, the area of ​​the electrolyte flow region (310) may be 10% to 50% of the total area of ​​the interface (300), preferably 20% to 40%. That is, if the electrode (100) and the separator (200) do not adhere to each other for more than 50%, the electrode (100) and the separator (200) may separate during the process of repeated charging and discharging of the secondary battery (1), and the resistance may increase. If the area of ​​the interface (300) that is not adhered to each other is less than 10%, it is not desirable because it is difficult to achieve the effect of improving electrolyte impregnation.

[0077] Meanwhile, the electrolyte flow region (310) and / or the contact region (320) may be formed using a pressurizing member such as a lamination roller (2) or a jig. The pressurizing member may have a protrusion protruding outwardly or a groove indented inwardly formed on its surface, so that a contact region (320) may be formed in a certain part of the electrode assembly (10) that is pressed by the protrusion, or an electrolyte flow region (310) may be formed in a certain part of the electrode assembly corresponding to the groove. In this regard, the lamination roller (2) for manufacturing the electrode assembly (10) according to the first embodiment of the present invention will be described later.

[0078] FIG. 3 is a plan view of the interface of an electrode assembly according to a first embodiment of the present invention.

[0079] Referring to FIG. 3, the electrolyte flow region (310) may include a first region (311) and a second region (312).

[0080] The first region (311) may be extended by a first length (L1) from one edge (300a) of the interface (300) toward the other edge (300b) of the interface (300). In this specification, the direction from one edge (300a) of the interface (300) toward the other edge (300b) of the interface may be defined as the first direction (+X-axis direction).

[0081] At this time, the first region (311) can function as an electrolyte flow path through which the electrolyte (E) can penetrate and move. That is, the electrolyte (E) can easily penetrate into the first region (311), and if gas is generated inside the electrode assembly (10), it can also function as an outlet for the gas.

[0082] In this way, for the penetration of the electrolyte (E) or the discharge of the generated gas, the first region (311) may be formed such that one end is open to the outside of the electrode assembly (10). That is, one end of the first region (311) may engage with a part of one side edge (300a) of the interface (300). Thus, a part of one side edge (300a) of the interface (300) may be opened by the first region (311).

[0083] The second region (312) may be extended by a second length (L2) from the other edge (300b) of the interface (300) toward the one edge (300a) of the interface (300). In this specification, the direction from the other edge (300b) of the interface (300) toward the one edge (300a) of the interface (300) may be defined as the opposite direction (-X-axis direction) of the first direction.

[0084] In addition, the second region (312), like the first region (311), can function as an electrolyte flow path through which the electrolyte (E) can penetrate and move. That is, the electrolyte (E) can easily penetrate into the second region (312), and if gas is generated inside the electrode assembly (10), it can also function as an outlet for the gas.

[0085] In this way, for the penetration of the electrolyte (E) or the discharge of the generated gas, the second region (312) may be formed such that one end is open to the outside of the electrode assembly (10). That is, one end of the second region (312) may engage with a part of the other edge (300b) of the interface (300). Thus, a part of the other edge (300b) of the interface (300) may be opened by the second region (312).

[0086] The first end (E1), which is the end of the extension direction of the first region (311), and the second end (E2), which is the end of the extension direction of the second region (312), may be spaced apart from each other in a second direction (Y-axis direction). At this time, the second direction may be a direction that intersects the first direction. Preferably, the second direction may intersect perpendicularly with the first direction.

[0087] Meanwhile, as illustrated in FIG. 3, the first region (311a, 311b) and the second region (312a, 312b, 312c) may each be provided in multiple numbers. Additionally, the number of the second region (312a, 312b, 312c) may be greater than the number of the first region (311a, 311b). For example, there may be two first regions (311a, 311b) and three second regions (312a, 312b, 312c). Through this, as described later, there is an effect of maximally improving the electrolyte impregnation of the peripheral area of ​​the second region (312a, 312b, 312c), where the electrolyte impregnation may be relatively poor.

[0088] In addition, the first end (E1) and the second end (E2) may each be provided in multiple numbers, and the first end (E1) and the second end (E2) may be arranged alternately along the second direction (Y-axis direction) at regular intervals from each other.

[0089] Each of the first regions (311a, 311b) can be extended parallel to each other, and each of the second regions (312a, 312b, 312c) can also be extended parallel to each other. Additionally, the first regions (311a, 311b) and the second regions (312a, 312b, 312c) can also be extended parallel to each other. Thus, the first end (E1) and the second end (E2) can be located in different regions without overlapping each other. Through this, the number of second regions (312a, 312b, 312c) can be greater than the number of first regions (311a, 311b).

[0090] Meanwhile, the longer the first length (L1) and / or the second length (L2), the better the electrolyte impregnation of the electrode assembly (10). However, if the third length (L3) and / or the fourth length (L3) is excessively long, the portion (adhesion area (320)) where the electrode (100) and the separator (200) adhere to each other may be reduced. In this case, the adhesion between the electrode (100) and the separator (200) is reduced, and the strength of the electrode assembly (10) is also weakened. Therefore, it may be necessary to set the first length (L1) and the second length (L2) to solve the above problem.

[0091] In this regard, the sum of the first length (L1) and the second length (L2) may be equal to the shortest distance (D) between one edge (300a) of the interface (300) and the other edge (300b) of the interface (300).

[0092] At this time, since the sum of the first length (L1) and the second length (L2) is equal to the shortest distance (D), the virtual line (VL) that passes through any point on the interface (300) and extends in the second direction (Y-axis direction) passes through the first region (311) and / or the second region (312). That is, since the virtual line (VL) passes through at least one electrolyte flow region (310), the electrolyte impregnation of the electrode assembly (10) can be maximized.

[0093] Additionally, the first region (311) and the second region (312) overlap only with the contact region (320) in the first direction (+X-axis direction) and the opposite direction of the first direction (-X-axis direction), respectively. At this time, the contact region (320) that overlaps with the first region (311) in the first direction (+X-axis direction) and the contact region (320) that overlaps with the second region (312) in the opposite direction of the first direction (-X-axis direction) can contribute to improving the adhesion between the electrode (100) and the separator (200) and the strength of the electrode assembly (10). Accordingly, compared to the case where there is no adhesion area (320) overlapping the first region (311) in the first direction (+X-axis direction) and no adhesion area (320) overlapping the second region (312) in the opposite direction (-X-axis direction) of the first direction, the electrode assembly (10) according to the first embodiment of the present invention has the effect of minimizing the reduction in adhesion between the electrode (100) and the separator (200) and the weakening of the strength of the electrode assembly (10).

[0094] And, the first region (311) and the second region (312) overlap only with the contact region (320) in the second direction (Y-axis direction), except for the mutually extended ends (E1, E2). Therefore, the contact region (320) that overlaps with the first region (311) and the second region (312) in the second direction (Y-axis direction) can also contribute to improving the adhesion between the electrode (100) and the separator (200) and the strength of the electrode assembly (10).

[0095] Through this, the electrode assembly (10) according to the first embodiment of the present invention has the effect of maximizing electrolyte impregnation while simultaneously minimizing the reduction in adhesion between the electrode (100) and the separator (200) and the weakening of the strength of the electrode assembly (10).

[0096] Meanwhile, the first length (L1) and the second length (L2) may be the same. In this case, the first length (L1) may be half of the shortest distance (D), and the second length (L2) may also be half of the shortest distance (D). That is, by forming an electrolyte flow region (310) in which the electrode (100) and the separator (200) do not adhere to each other as uniformly as possible, the uneven reduction in adhesion between the electrode (100) and the separator (200) and the uneven weakening of strength of the electrode assembly (10) can be minimized.

[0097] Meanwhile, the first length (L1) may be longer than the third length (L3), which is the second direction (Y-axis direction) length of the first region (311). In this case, it is preferable that the first region (311) be a rectangular shape where the first length (L1) is longer than the third length (L3), but the shape is not particularly limited. Additionally, the second length (L2) may be longer than the fourth length (L3), which is the second direction (Y-axis direction) length of the second region (312). In this case, it is preferable that the second region (312) be a rectangular shape where the second length (L2) is longer than the fourth length (L3), but the shape is not particularly limited.

[0098] At this time, the longer the third length (L3) and / or the fourth length (L3), the better the electrolyte impregnation of the electrode assembly (10). However, if the third length (L3) and / or the fourth length (L3) is excessively long, the portion (adhesion area (320)) where the electrode (100) and the separator (200) adhere to each other may be reduced. In this case, the adhesion between the electrode (100) and the separator (200) is reduced, and the problem of weakening the strength of the electrode assembly (10) also occurs. Therefore, it is preferable that the third length (L3) and / or the fourth length (L3) be 5 mm or more and 10 mm or less. The optimal third length (L3) and / or the fourth length (L3) with specific numerical values ​​will be described later.

[0099] FIG. 4 is a plan view in which a third region is added to the electrolyte flow region shown in FIG. 3, and FIG. 5 is a magnified view of part A of FIG. 4.

[0100] Referring to FIGS. 4 and FIGS. 5, the electrolyte flow region (310) may further include a third region (313).

[0101] The third region (313) can connect the first region (311) and the second region (312) by connecting the first end (E1) and the second end (E2). At this time, the third region (313) can be extended in the second direction (Y-axis direction).

[0102] Additionally, the third region (313) can form a continuous electrolyte flow path connecting from one side edge (300a) to the other side edge (300b) of the interface (300) by connecting the first region (311) and the second region (312). Through this, the electrolyte impregnation of the electrode assembly (10) can be further improved.

[0103] The third region (313) may include a first communication region (313a), a second communication region (313b), and a third communication region (313c).

[0104] The first communication area (313a) may be in communication with the first end (E1). The second communication area (313b) may be in communication with the second end (E2). The third communication area (313c) may be in communication with the first communication area (313a), the second communication area (313b), the side (311aa) of the first area (311a), and the side (312ab) of the second area (312a).

[0105] At this time, in order to minimize the decrease in adhesion between the electrode (100) and the separator (200) and the weakening of the strength of the electrode assembly (10), the length of the first direction (+X-axis direction) of the third communication area (313c) can be formed to be as short as possible. Specifically, the length of the first direction (+X-axis direction) of the third communication area (313c) can be formed to be shorter than the length of the second direction (Y-axis direction) of the first area (311a) or the second area (312a).

[0106] In each third region (313), the sum of the first direction (+X-axis direction) length of the first communication region (313a) and the first direction (+X-axis direction) length of the second communication region (313b) may be equal to the first direction (+X-axis direction) length of the third communication region (313c). At this time, the first direction (+X-axis direction) length of the third communication region (313c) may be 2.5 mm or more and 5 mm or less.

[0107] The length of the first direction (+X-axis direction) of the first communication area (313a) and the length of the first direction (+X-axis direction) of the second communication area (313b) may be equal to each other. Specifically, the length of the first direction (+X-axis direction) of the first communication area (313a) may be half the length of the first direction (+X-axis direction) of the third communication area (313c), and the length of the first direction (+X-axis direction) of the second communication area (313b) may be half the length of the first direction (+X-axis direction) of the third communication area (313c).

[0108] Additionally, as shown in FIG. 5, a left portion (311aa) and a right portion (311ab) are formed in the first region (311a), and a third communication region (313c) can be in communication with the left portion (311aa) of the first region (311a). Also, a left portion (312aa) and a right portion (312ab) are formed in the second region (312a), and a third communication region (313c) can be in communication with the right portion (312ab) of the second region (312a).

[0109] The electrode assembly (10) according to the first embodiment of the present invention further includes a third region (313) connecting the first region (311) and the second region (312), thereby having the effect of further improving the electrolyte impregnation of the electrode assembly (10) compared to the case where the third region (313) is not formed.

[0110] Additionally, since the third region (313) extends in a direction (Y-axis direction) that intersects the direction (X-axis direction) in which the first region (311) and the second region (312) extend, the first region (311) and the second region (312) overlap only with the contact region (320) in the second direction (Y-axis direction), excluding the mutually extending ends (E1, E2) and the third region (313). Therefore, the third region (313) has the effect of securing an improved electrolyte impregnation effect of the electrode assembly (10) while minimizing the reduction in adhesion between the electrode (100) and the separator (200) and the weakening of the strength of the electrode assembly (10).

[0111]

[0112] 2nd embodiment

[0113] FIG. 6 is a drawing showing an electrolyte being injected through an opening into an outer material of a secondary battery according to a second embodiment of the present invention, and FIG. 7 is a drawing showing a degassing hole being drilled into an outer material of a secondary battery according to a second embodiment of the present invention.

[0114] Referring to FIGS. 6 and FIGS. 7, a secondary battery (1) according to the second embodiment of the present invention may include an electrode assembly (10) and an outer casing (20) according to the first embodiment of the present invention.

[0115] At this time, since the electrode assembly (10) of the secondary battery (1) according to the second embodiment of the present invention is the electrode assembly (10) according to the first embodiment of the present invention, the description of the electrode assembly (10) of the secondary battery (1) according to the second embodiment of the present invention may be based on the description of the electrode assembly (10) according to the first embodiment of the present invention.

[0116] The outer casing (20) of the secondary battery (1) according to the second embodiment of the present invention can accommodate an electrode assembly (10).

[0117] After the electrode assembly (10) is received in the receiving space (S) of the exterior material (20), at least one corner among the plurality of corners (21) of the exterior material (20) where the opening (22) is formed can be opened, and the remaining corners can be sealed. For example, as shown in FIG. 6, the first corner (211) can be opened, and the remaining second to fourth corners (212, 213, 214) can be sealed. At this time, the entire first corner (211) can be opened, but alternatively, only a part of the first corner (211) can be opened. In this way, the opening (22) can be formed by opening the first corner (211) of the exterior material (20).

[0118] At this time, the electrolyte (E) can be injected into the receiving space (S) through the opening (22). Specifically, the electrolyte (E) can be injected into the receiving space (S) through a liquid injection part (23) that communicates with the opening (22). For example, the liquid injection part (23) may be in the form of a nozzle through which the electrolyte (E) can flow. Thus, when the liquid injection part (23) is connected to the opening (22), the liquid injection part (23) can communicate with the receiving space (S), and the electrolyte (E) that flows through the liquid injection part (23) can be injected into the receiving space (S).

[0119] The electrolyte (E) flows from the top to the bottom due to gravity. Therefore, in order for the electrode assembly (10) to be sufficiently impregnated with the electrolyte and for the electrolyte (E) not to leak out, the outer casing (20) can be positioned upright so that the opening (136) faces upward (+X-axis direction). Subsequently, it is preferable to inject the electrolyte (E) from the top to the bottom of the outer casing (20).

[0120] Meanwhile, the first area (311) and the second area (312) may each be provided in multiple numbers. At this time, the distance between the second area (312) and the opening (22) may be shorter than the distance between the first area (311) and the opening (22). That is, the second area (312) may be positioned higher (+X-axis direction) than the first area (311). Specifically, as shown in FIGS. 6 and 7, the first area (311) may be positioned close to the inner bottom surface of the receiving space (S), and the second area (312) may be positioned close to the opening (22) located on the opposite side of the bottom surface.

[0121] Additionally, the number of second regions (312) may be greater than the number of first regions (311). In this regard, when an electrolyte (E) is introduced into the outer material (20) while the electrode assembly (10) is contained in the receiving space (S) of the outer material (20), the electrolyte (E) rising from the bottom surface of the receiving space (S) is drawn up from the lower side to the upper side (+X-axis direction) by capillary action, and the electrolyte impregnation in the peripheral area of ​​the second region (312) placed relatively higher is lower than that of the lower side. Therefore, the present invention has the effect of maximizing the electrolyte impregnation in the peripheral area of ​​the second region (312), which may have relatively lower electrolyte impregnation, by placing the second region (312), which has a greater number than the first region (311), in the upper side (+X-axis direction).

[0122] Meanwhile, after injecting the electrolyte (E) into the receiving space (S) of the exterior material (20), as shown in FIG. 7, the first heating part (not shown) can first seal the exterior material (20) to form a sealing part (24). Since a degassing hole (H) is subsequently drilled on the lower side of the sealing part (24), it is preferable that the sealing part (24) be formed as close as possible to the first corner (211).

[0123] After the sealing portion (24) is formed, a degassing hole (H) for discharging internal gas may be perforated in the exterior material (20). At this time, the distance between the plurality of second areas (312) and the degassing hole (H) may be shorter than the distance between the plurality of first areas (311) and the degassing hole (H). Through this, the number of second areas (312) can be positioned higher (+X-axis direction) than the first area (311).

[0124] Meanwhile, the electrolyte flow region (310) may further include a third region (313) connecting the first end (E1) and the second end (E2). Here, the third region (313) according to the second embodiment of the present invention may be described by reference to the third region (313) according to the first embodiment of the present invention.

[0125]

[0126] Third embodiment

[0127] FIG. 8 is a drawing showing a lamination roller according to a third embodiment of the present invention manufacturing an electrode assembly, FIG. 9 is a drawing showing the surface of a roller member of a lamination roller according to a third embodiment of the present invention, and FIG. 10 is a magnified view of part B of FIG. 9.

[0128] Referring to FIGS. 8 to 10, a lamination roller (2) according to the third embodiment of the present invention can be used to manufacture an electrode assembly (10) according to the first embodiment of the present invention.

[0129] Specifically, the lamination roller (2) according to the third embodiment of the present invention can press the electrode assembly (10) according to the first embodiment of the present invention during the lamination step in the secondary battery manufacturing process.

[0130] That is, as illustrated in FIG. 8, when the separator (200), anode (110), and cathode (120) unwound from the separator unwound roller (3), anode sheet unwound roller (4), and cathode sheet unwound roller (5), respectively, form a laminate in the shape of separator / anode (cathode) / separator / cathode (anode), the lamination roller (2) presses the laminate to form an electrolyte flow region (310) and a contact region (320) at the interface (300) between the electrode (100) and the separator (200).

[0131] At this time, since the electrode assembly (10) that is pressed by the lamination roller (2) according to the third embodiment of the present invention is the electrode assembly (10) according to the first embodiment of the present invention, the description of the electrode assembly (10) that is pressed by the lamination roller (2) according to the third embodiment of the present invention may be based on the description of the electrode assembly (10) according to the first embodiment of the present invention.

[0132] A lamination roller (2) according to a third embodiment of the present invention may include a roller member (1000) and a recess (2000).

[0133] Meanwhile, referring to FIG. 8, the surface of the roller member (1000) of the lamination roller (2) according to the third embodiment of the present invention may be divided into a plurality of unit planes (1110, 1120, 1130) having a certain spacing along the circumferential direction. Accordingly, each unit cell (S1, S2, S3) of the electrode assembly (10) according to the first embodiment of the present invention may be formed by a part of the roller member (1000) corresponding to each unit plane (1110, 1120, 1130) and a recess (2000) formed for each unit plane (1110, 1120, 1130).

[0134] The roller member (1000) can press the electrode assembly (10) while heated, thereby bringing the electrode (100) and the separator (200) into close contact through heat and pressure. At this time, the roller member (1000) is fixed to the roller rotation axis (2a) and can rotate together with the roller rotation axis (2a).

[0135] The recessed portion (2000) may be formed by being recessed in the roller member (1000). At this time, since the electrode assembly according to the first embodiment of the present invention is manufactured by the lamination roller (2) according to the third embodiment of the present invention, the shape in which the recessed portion (2000) according to the third embodiment of the present invention is formed in the roller member (1000) may correspond to the shape in which the electrolyte flow region (310) according to the first embodiment of the present invention is formed at the interface (300).

[0136] Specifically, the roller member (1000) forms a contact area (320) of the electrode assembly (10) according to the first embodiment of the present invention, and the recessed portion (2000) forms an electrolyte flow area (310) of the electrode assembly (10) according to the first embodiment of the present invention. Specifically, since the roller member (1000) is relatively protruding compared to the recessed portion (2000), the interface (300) pressed by the roller member (1000) is in close contact with each other to form a contact area (320), and the interface (300) pressed by the recessed portion (2000) is relatively less close to form an electrolyte flow area (310).

[0137] Meanwhile, the depression (2000) may include a first depression (2100) and a second depression (2200). The first depression (2100) may form a first region (311) of the electrolyte flow region (310), and the second depression (2200) may form a second region (312) of the electrolyte flow region (310).

[0138] The first recess (2100) may extend in the circumferential direction of the roller member (1000), and the second recess (2200) may extend in the circumferential direction of the roller member (1000). At this time, the first recess (2100) and the second recess (2200) may be arranged alternately along the circumferential direction of the roller member (1000).

[0139] The first recess (2100) may be extended by a predetermined length from one side edge (1100a) of the unit surface (1100) toward the other side edge (1100b) of the unit surface (1100). At this time, the first recess (2100) may form an electrolyte flow area (310) in which the electrolyte (E) can penetrate and move by applying less pressure to the electrode assembly (10) compared to the surface of the surrounding roller member (1000). Specifically, the first recess (2100) may form a first area (311).

[0140] The second recess (2200) may be extended by a predetermined length from the other edge (1100b) of the unit surface (1100) toward the one edge (1100a) of the unit surface (1100). At this time, the second recess (2200) may form an electrolyte flow area (310) in which the electrolyte (E) can penetrate and move by applying less pressure to the electrode assembly (10) compared to the surface of the surrounding roller member (1000). Specifically, the second recess (2200) may form a second area (312).

[0141] The extension direction end (E1') of the first recess (2100) and the extension direction end (E2') of the second recess (2200) may be spaced apart from each other in the longitudinal direction of the roller member (1000). At this time, the longitudinal direction of the roller member (1000) may be the same as the axial direction of the roller rotation axis (2a).

[0142] The first recess (2100) and the second recess (2200) may each be provided in multiple numbers, and the number of the second recess (2200) may be greater than the number of the first recess (2100). Accordingly, the extension direction end (E1') of the first recess (2100) and the extension direction end (E2') of the second recess (2200) may also each be provided in multiple numbers, and the extension direction end (E1') of the first recess (2100) and the extension direction end (E2') of the second recess (2200) may be arranged alternately along the length direction of the roller member (1000) at a constant interval from each other.

[0143] Each first recess (2100) may be extended parallel to each other, and each second recess (2200) may also be extended parallel to each other. Additionally, the first recess (2100) and the second recess (2200) may also be extended parallel to each other.

[0144] In addition, as described above in the first embodiment of the present invention, in order to maximize the electrolyte impregnation of the electrode assembly (10) and at the same time minimize the decrease in adhesion between the electrode (100) and the separator (200) and the weakening of the strength of the electrode assembly (10), the sum of the extensional length of the first recess (2100) and the extensional length of the second recess (2200) may be equal to the circumferential length of the roller member (1000) of one unit surface (1110).

[0145] In addition, as described above in the first embodiment of the present invention, in order to minimize the uneven reduction in adhesion between the electrode (100) and the separator (200) of the electrode assembly (10) and the uneven weakening of strength of the electrode assembly (10), the extensional length of the first recess (2100) and the extensional length of the second recess (2200) may be the same as each other.

[0146] Meanwhile, the circumferential length of the roller member (1000) of the first recess (2100) may be longer than the length in the direction of the roller rotation axis (2a) of the first recess (2100). Additionally, the circumferential length of the roller member (1000) of the second recess (2200) may be longer than the length in the direction of the roller rotation axis (2a) of the second recess (2200).

[0147] At this time, since the shapes of the first recess (2100) and the second recess (2200) correspond to the shapes of the first region (311) and the second region (312) of the electrode assembly (10), the lengths of the first recess (2100) and the second recess (2200) in the direction of the roller rotation axis (2a) may each be 5mm or more and 10mm or less.

[0148] Additionally, the lamination roller (2) according to the third embodiment of the present invention may further include a third recess (2300). The third recess (2300) may form a third region (313) among the electrolyte flow regions (310).

[0149] The third recess (2300) can connect the extension direction end (E1') of the first recess (2100) and the extension direction end (E2') of the second recess (2200). By connecting the first recess (2100) and the second recess (2200), the third recess (2300) can connect the first recess (2100) and the second recess (2200). At this time, the third recess (2300) can be extended in the axial direction of the roller rotation axis (2a).

[0150] The third depression (2300) may include a third-1 depression (2300a), a third-2 depression (2300b), and a third-3 depression (2300c).

[0151] The 3-1 recess (2300a) may be connected to the extensional end (E1') of the 1st recess (2100a). The 3-2 recess (2300b) may be connected to the extensional end (E2') of the 2nd recess (2200a). The 3-3 recess (2300c) may be connected to the 1st recess (2100a), the 2nd recess (2200a), the side (2100ab) of the 1st recess (2100a), and the side (2200ab) of the 2nd recess (2200a).

[0152] At this time, as illustrated in FIG. 10, a left portion (2100aa) and a right portion (2100ab) are formed in the first recess (2100a), and the third recess (2300) can be in communication with the left portion (2100aa) of the first recess (2100a). Additionally, a left portion (2200aa) and a right portion (2200ab) are formed in the second recess (2200a), and the third recess (2300) can be in communication with the right portion (2200ab) of the second recess (220aa).

[0153] Accordingly, the lamination roller (2) according to the third embodiment of the present invention further includes a third recess (2300) connecting the first recess (2100) and the second recess (2200), thereby having the effect of further improving the electrolyte impregnation of the electrode assembly (10) manufactured compared to the case where the third recess (2300) is not formed.

[0154] Additionally, since the third recess (2300) extends in a direction that intersects the direction in which the first recess (2100) and the second recess (2200) extend (circumferential direction of the roller member (1000)) (axial direction of the roller rotation axis (2a)), the first recess (2100) and the second recess (2200) overlap only with the roller member (1000) in the axial direction of the roller rotation axis (2a), except for the mutual extension direction ends (E1', E2') and the third recess (2300). At this time, as described above, the roller member (1000) forms a contact area (320) and the recessed portion (2000) forms an electrolyte flow area (310). Therefore, as described in the first embodiment of the present invention, the electrode assembly (10) formed by the lamination roller (2) according to the third embodiment of the present invention has the effect of securing an improved electrolyte impregnation effect while minimizing the reduction in adhesion between the electrode (100) and the separator (200) and the weakening of the strength of the electrode assembly (10).

[0155]

[0156] Meanwhile, below, we will describe Experimental Example 1, which observes the electrolyte impregnation of an electrode assembly according to the shape or number of electrolyte flow regions, and Experimental Example 2, which observes the electrolyte impregnation of an electrode assembly according to the width of the electrolyte flow regions.

[0157]

[0158] Experimental Example 1 - Electrolyte impregnation of electrode assembly according to the shape or number of electrolyte flow regions

[0159]

[0160] Comparative Example 1-1

[0161] With the temperature of the lamination roller, which has no indentations formed at all, set to 70 degrees Celsius, an electrode assembly stacked in the form of a separator / anode / separator / cathode and having a width of 328 mm was pressed, and then the electrode assembly was cut at regular intervals to manufacture a mono cell. At this time, the pressure of the lamination roller pressing the mono cell was set to 693 kgf.

[0162]

[0163] Comparative Example 1-2

[0164] In Comparative Example 1-2, a mono cell was manufactured in the same manner as in Comparative Example 1-1, except that the electrode assembly was pressed with a lamination roller having only three first depressions formed therein. Accordingly, the electrolyte flow region formed in the mono cell manufactured according to Comparative Example 1-2 included only three first regions extending from one corner of the interface toward the other corner. At this time, the width of the plurality of first regions is all the same at 10 mm, and the spacing between each first region is all the same at 31 mm.

[0165]

[0166] Preparation Example 1-1

[0167] In Preparation Example 1-1, a mono cell was manufactured in the same manner as in Comparative Example 1-1, except that the electrode assembly was pressed with a lamination roller having three first indentations and two second indentations formed therein. Accordingly, the electrolyte flow region formed in the mono cell manufactured according to Preparation Example 1-1 includes three first regions extending from one corner of the interface toward the other corner, and two second regions extending from the other corner of the interface toward one corner. At this time, the width of the plurality of first regions and the plurality of second regions is all the same at 10 mm, and the spacing between adjacent first regions and second regions is all the same at 31 mm.

[0168]

[0169] Preparation Example 1-2

[0170] In Preparation Example 1-2, a mono cell was manufactured in the same manner as in Comparative Example 1-1, except that the electrode assembly was pressed with a lamination roller having three first depressions, two third depressions, and a third depression connecting the first and second depressions. Accordingly, the electrolyte flow region formed in the mono cell manufactured according to Preparation Example 1-2 includes three first regions extending from one corner of the interface toward the other corner, two second regions extending from the other corner of the interface toward one corner, and a third region connecting the first end of the plurality of first regions and the second end of the plurality of second regions. At this time, the width of the plurality of first regions, the plurality of second regions, and the plurality of third regions is all the same at 10 mm, and the spacing between adjacent first regions and second regions is all the same at 31 mm.

[0171]

[0172] Preparation Examples 1-3

[0173] In Preparation Example 1-3, a mono cell was manufactured in the same manner as in Comparative Example 1-1, except that the electrode assembly was pressed with a lamination roller having two first depressions, three second depressions, and a third depression connecting the first and second depressions. Accordingly, the electrolyte flow region formed in the mono cell manufactured according to Preparation Example 1-3 includes two first regions extending from one corner of the interface toward the other corner, three second regions extending from the other corner of the interface toward one corner, and a third region connecting the first end of the plurality of first regions and the second end of the plurality of second regions. At this time, the width of the plurality of first regions, the plurality of second regions, and the plurality of third regions is all the same at 10 mm, and the spacing between adjacent first regions and second regions is all the same at 31 mm.

[0174]

[0175] measurement method

[0176] One stack of mono cells according to Comparative Example 1-1, Comparative Example 1-2, Preparation Example 1-1, Preparation Example 1-2, and Preparation Example 1-3 prepared above was each immersed in 3.67 g (= 3.06 mL) of electrolyte for 6 hours. Then, they were removed, and the anode and separator were peeled off, and a photograph of the separator attached to the anode was taken. Meanwhile, the amount of electrolyte required for the experiment was minimized by testing the electrolyte impregnation using a mono cell corresponding to a single stack rather than an electrode assembly consisting of multiple stacks.

[0177]

[0178] Measurement results

[0179] FIG. 11 is a photograph showing the result according to Comparative Example 1-1 of the present invention, FIG. 12 is a photograph showing the result according to Comparative Example 1-2 of the present invention, FIG. 13 is a photograph showing the result according to Manufacturing Example 1-1 of the present invention, FIG. 14 is a photograph showing the result according to Manufacturing Example 1-2 of the present invention, and FIG. 15 is a photograph showing the result according to Manufacturing Example 1-3 of the present invention. The photograph located at the top of each figure is a photograph of a monocell before being impregnated with an electrolyte, and the photograph located at the bottom of each figure is a photograph of one side of a separator peeled off from the anode after the monocell has been impregnated with an electrolyte. In the photograph located at the bottom of each figure, the area showing a relatively dark brightness is the area impregnated with the electrolyte, and the area showing a relatively bright brightness is the area not impregnated with the electrolyte.

[0180]

[0181] When comparing Preparation Examples 1-1 to 1-3 with Comparative Examples 1-1 and 1-2, it was confirmed that the electrolyte impregnation of the monocell improved as the electrolyte flow region at the interface of the monocell increased. In addition, it was confirmed that the electrolyte impregnation of the monocell improved further when the electrolyte flow region was placed on both the lower and upper sides rather than only on the lower side. Furthermore, it was confirmed that the electrolyte impregnation of the monocell improved further when the number of electrolyte flow regions placed on the upper side was greater than the number of electrolyte flow regions placed on the lower side.

[0182] Specifically, when comparing Comparative Example 1-1 and Comparative Example 1-2, it was confirmed that Comparative Example 1-2 had a wider electrolyte impregnation region than Comparative Example 1-1. In other words, it was confirmed that the electrolyte impregnation of the monocell is improved when there is at least a first region at the interface of the monocell compared to when there is no electrolyte flow region at all.

[0183] In addition, when comparing Comparative Example 1-2 with Preparation Example 1-1, it was confirmed that Preparation Example 1-1 had a wider electrolyte impregnation area than Comparative Example 1-2. That is, it was confirmed that the electrolyte impregnation of the monocell is further improved when the electrolyte flow area includes both the first and second regions rather than including only the first region.

[0184] In addition, when comparing Preparation Example 1-1 and Preparation Example 1-2, it was confirmed that Preparation Example 1-2 had a wider electrolyte impregnation area than Preparation Example 1-1. That is, it was confirmed that the electrolyte impregnation of the monocell is further improved when the electrolyte flow area includes the first, second, and third regions, rather than including only the first and second regions.

[0185] In addition, when comparing Preparation Example 1-2 and Preparation Example 1-3, it was confirmed that Preparation Example 1-3 had a wider electrolyte impregnation area than Preparation Example 1-2. That is, it was confirmed that the electrolyte impregnation of the monocell was improved when the number of the second area was greater than the number of the first area, compared to when the number of the first area was greater.

[0186]

[0187] Experimental Example 2 - Electrolyte impregnation of electrode assembly according to the width of the electrolyte flow region

[0188]

[0189] Comparative Example 2-1

[0190] With the temperature of the lamination roller, which has no indentations formed at all, set to 70 degrees Celsius, an electrode assembly stacked in the form of a separator / anode / separator / cathode and having a width of 328 mm was pressed, and then the electrode assembly was cut at regular intervals to manufacture a mono cell. At this time, the pressure of the lamination roller pressing the mono cell was set to 693 kgf.

[0191]

[0192] Comparative Example 2-2

[0193] In Comparative Example 2-2, a mono cell was manufactured in the same manner as in Comparative Example 2-1, except that the electrode assembly was pressed with a lamination roller having three first depressions with a width of 2.5 mm and four second depressions with a width of 2.5 mm. Accordingly, the electrolyte flow region formed in the mono cell manufactured according to Comparative Example 2-2 includes three first regions extending from one corner of the interface toward the other corner, and four second regions extending from the other corner of the interface toward one corner. At this time, the width of the plurality of first regions and the plurality of second regions is all the same at 2.5 mm.

[0194]

[0195] Preparation Example 2-1

[0196] In Preparation Example 2-1, a mono cell was manufactured in the same manner as in Comparative Example 2-1, except that the electrode assembly was pressed with a lamination roller having three first depressions with a width of 5 mm and four second depressions with a width of 5 mm. Accordingly, the electrolyte flow region formed in the mono cell manufactured according to Preparation Example 2-1 includes three first regions extending from one edge of the interface toward the other edge, and four second regions extending from the other edge of the interface toward one edge. At this time, the width of the plurality of first regions and the plurality of second regions is all the same at 5 mm.

[0197]

[0198] Preparation Example 2-2

[0199] In Preparation Example 2-2, a mono cell was manufactured in the same manner as in Comparative Example 2-1, except that the electrode assembly was pressed with a lamination roller having three first depressions with a width of 10 mm and four second depressions with a width of 10 mm. Accordingly, the electrolyte flow region formed in the mono cell manufactured according to Preparation Example 2-2 includes three first regions extending from one corner of the interface toward the other corner, and four second regions extending from the other corner of the interface toward one corner. At this time, the width of the plurality of first regions and the plurality of second regions is all the same at 10 mm.

[0200]

[0201] measurement method

[0202] One stack of mono cells prepared according to Comparative Example 2-1, Comparative Example 2-2, Preparation Example 2-1, and Preparation Example 2-2 was each immersed in 3.67 g (= 3.06 mL) of electrolyte for 6 hours. Then, they were removed, and the anode and separator were peeled off, and a photograph of the separator attached to the anode was taken. Meanwhile, the amount of electrolyte required for the experiment was minimized by using a mono cell corresponding to a single stack, rather than an electrode assembly consisting of multiple stacks, to test the electrolyte impregnation.

[0203]

[0204] Measurement results

[0205] FIG. 16 is a photograph showing the result according to Comparative Example 2-1 of the present invention, FIG. 17 is a photograph showing the result according to Comparative Example 2-2 of the present invention, FIG. 18 is a photograph showing the result according to Manufacturing Example 2-1 of the present invention, and FIG. 19 is a photograph showing the result according to Manufacturing Example 2-2 of the present invention. The photograph located at the top of each figure is a photograph of a monocell before being impregnated with an electrolyte, and the photograph located at the bottom of each figure is a photograph of one side of a separator peeled off from the anode after the monocell has been impregnated with an electrolyte. In the photograph located at the bottom of each figure, the area showing a relatively dark brightness is the area impregnated with the electrolyte, and the area showing a relatively bright brightness is the area not impregnated with the electrolyte.

[0206]

[0207] When comparing Preparation Examples 2-1 and 2-2 with Comparative Examples 2-1 and 2-2, it was confirmed that the wider the width of the electrolyte flow region formed at the interface of the mono cell, the more the electrolyte impregnation of the mono cell is improved. However, it was also confirmed that when the width exceeds a certain limit, the degree of improvement in electrolyte impregnation decreases.

[0208] Specifically, when comparing Comparative Example 2-1 and Comparative Example 2-2, it was confirmed that Comparative Example 2-2 had a wider electrolyte impregnation area than Comparative Example 2-1. In other words, it was confirmed that the electrolyte impregnation performance of the monocell was improved when there was an electrolyte flow area with a width of 2.5 mm compared to when there was no electrolyte flow area at all.

[0209] In addition, when comparing Comparative Example 2-2 with Preparation Example 1-1, it was confirmed that Preparation Example 1-1 had a wider electrolyte impregnation area than Comparative Example 2-2. That is, it was confirmed that the electrolyte impregnation performance of the monocell was improved when the width of the electrolyte flow area was 5 mm compared to when it was 2.5 mm.

[0210] In addition, when comparing Preparation Example 1-1 and Preparation Example 1-2, it was confirmed that although the electrolyte impregnation area of ​​Preparation Example 1-2 was slightly wider than that of Preparation Example 1-1, the degree of this was smaller than the degree to which the electrolyte impregnation area of ​​Preparation Example 1-1 was wider than that of Comparative Example 2-2. That is, it was confirmed that when the width of the electrolyte flow area was 10 mm compared to 5 mm, the electrolyte impregnation of the monocell improved, but the degree of improvement was lower than when the width was increased from 2.5 mm to 5 mm.

[0211] In this regard, as the width of the electrolyte flow region increases, the space available for the electrolyte to flow increases; thus, while the electrolyte impregnation of the electrode assembly increases, the adhesion between the electrode and the separator and the strength of the electrode assembly may decrease. Therefore, it is necessary not to increase the width of the electrolyte flow region from the point where the degree of improvement in electrolyte impregnation decreases. That is, since the reduction in adhesion between the electrode and the separator and the weakening of the strength of the electrode assembly must be minimized while maximizing electrolyte impregnation, it is preferable that the width of the electrolyte flow region of the electrode assembly according to the present invention be 5 mm or more and 10 mm or less.

[0212]

[0213] Although the present invention has been described above by limited embodiments and drawings, the present invention is not limited thereto, and various implementations are possible within the scope of the technical spirit of the present invention and the equivalent scope of the claims described below by those skilled in the art to which the present invention belongs.

[0214]

[0215] [Explanation of the symbol]

[0216] 1: Secondary battery 10: Electrode assembly

[0217] 100: Electrode 110: Anode

[0218] 120: Cathode 200: Separator

[0219] 300: Interface 310: Electrolyte flow region

[0220] 311: Area 1 312: Area 2

[0221] 313: Third Zone 313a: First Communication Zone

[0222] 313b: Second communication area 313c: Third communication area

[0223] 320: Contact area 300a: One side corner

[0224] 300b: Other edge E1: First end

[0225] E2: Second end 400: Electrode tab

[0226] 500: Electrode lead 600: Insulation part

Claims

1. An electrode assembly in which electrodes and separators are alternately stacked, A portion of the interface between the electrode and the separator is an electrolyte flow region where the electrolyte flows, and the remainder is a close contact region where the electrolyte is in close contact. The above electrolyte flow region is, A first region extending by a first length in a first direction from one edge of the interface toward the other edge of the interface; and It includes a second region extending by a second length in the opposite direction of the first direction, from the other edge of the interface toward the one edge of the interface. The first end, which is the end of the extension direction of the first region, and the second end, which is the end of the extension direction of the second region, are spaced apart from each other in a second direction that intersects the first direction, and The sum of the first length and the second length is equal to the shortest distance between one edge of the interface and the other edge of the interface, in an electrode assembly.

2. In Paragraph 1, The first direction and the second direction are electrode assemblies that intersect perpendicularly to each other.

3. In Paragraph 1, The above electrolyte flow region is, An electrode assembly further comprising a third region connecting the first end and the second end.

4. In Paragraph 3, The above third area is, A first communication area communicating with the first end; A second communication area communicating with the second end; and An electrode assembly comprising the first communication region, the second communication region, the side of the first region, and the third communication region communicating with the side of the second region.

5. In Paragraph 1, A portion of the one-sided edge of the above interface is opened by the first region, and An electrode assembly in which a portion of the other edge of the above interface is opened by the second region.

6. In Paragraph 1, The first region and the second region are each provided in multiple numbers, and The number of the second region is greater than the number of the first region in the electrode assembly.

7. In Paragraph 6, The first end and the second end are electrode assemblies arranged alternately along the second direction at a constant distance from each other.

8. In Paragraph 6, Each of the above-mentioned first regions extends parallel to each other, and Each of the above-mentioned second regions is an electrode assembly extending parallel to each other.

9. In Paragraph 6, Each of the above-mentioned first region and each of the above-mentioned second region is an electrode assembly extending parallel to each other.

10. In Paragraph 1, The above first length is, An electrode assembly longer than the third length, which is the second direction length of the first region.

11. In Paragraph 10, The above third electrode assembly has a length of 5 mm or more and 10 mm or less.

12. In Paragraph 1, The above second length is, An electrode assembly longer than the fourth length, which is the second direction length of the second region.

13. In Paragraph 12, The above-mentioned fourth electrode assembly, having a length of 5 mm or more and 10 mm or less.

14. In Paragraph 1, The first length and the second length are electrode assemblies that are identical to each other.

15. In Paragraph 1, An electrode assembly in which the adhesion force between the electrode and the separator in the above-mentioned adhesion region is greater than the adhesion force between the electrode and the separator in the above-mentioned electrolyte flow region.

16. An electrode assembly in which electrodes and separators are alternately stacked; and Includes an outer casing that accommodates the electrode assembly; A portion of the interface between the electrode and the separator is an electrolyte flow region where the electrolyte flows, and the remainder is a close contact region where the electrolyte is in close contact. The above electrolyte flow region is, A first region extending by a first length in a first direction from one edge of the interface toward the other edge of the interface; and It includes a second region extending by a second length in the opposite direction of the first direction, from the other edge of the interface toward the one edge of the interface. The first end, which is the end of the extension direction of the first region, and the second end, which is the end of the extension direction of the second region, are spaced apart from each other in a second direction that intersects the first direction, and The sum of the first length and the second length is equal to the shortest distance between one edge of the interface and the other edge of the interface, and The above exterior material has an opening formed therein for injecting an electrolyte into the interior, and The first region and the second region are each provided in multiple numbers, and The distance between the plurality of second regions and the opening is shorter than the distance between the plurality of first regions and the opening, and A secondary battery in which the number of the plurality of second regions is greater than the number of the plurality of first regions.

17. In Paragraph 16, The above electrolyte flow region is, A secondary battery further comprising a third region connecting the first end and the second end.

18. In Paragraph 16, The above exterior material has a degassing hole formed therein for discharging internal gas, and A secondary battery in which the distance between the plurality of second regions and the degassing hole is shorter than the distance between the plurality of first regions and the degassing hole.

19. A lamination roller that presses an electrode assembly in which electrodes and separators are alternately laminated, A roller member that presses the electrode assembly to bring the electrode and the separator into close contact; and It includes a recess formed by being recessed in the above roller member, and The above-mentioned depression is, A first recess extending in the circumferential direction of the roller member; and It includes a second recess extending in the circumferential direction of the roller member; and The first indentation and each of the second indentations are alternately staggered along the circumferential direction of the roller member, and A lamination roller in which the end of the first recess in the extension direction and the end of the second recess in the extension direction are spaced apart from each other in the longitudinal direction of the roller member.

20. In Paragraph 19, A lamination roller further comprising a third recess connecting the end of the first recess in the extension direction and the end of the second recess in the extension direction.