Flexible plugging agent, preparation method thereof and GIS (Geographic Information System)

By modifying flexible sealant of epoxy POSS and other materials, the traditional GIS SF6 gas leakage sealing problem requires power outage and bubbling, achieving efficient sealing and stability, ensuring equipment safety and environmental protection.

CN118956325AActive Publication Date: 2024-11-15WUHAN ANYHEN TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411150433.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-15
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

The traditional GIS SF6 gas leakage sealing method requires power outage, which is complex and time-consuming. When sealing with pressure, the sealant is prone to bubbling due to gas pressure or impact, which cannot effectively prevent gas leakage, affecting equipment safety and environmental protection.

Method used

Modified epoxy POSS is used as the main component of flexible sealant, and by introducing materials such as benzene ring, polydicyclopentadiene and PAMAM, mechanical strength, impact resistance and adhesion are improved, and an efficient composite structure is formed. Reduce bubble phenomenon and promote cross-linking reactions through catalysts to form a stable network structure.

Benefits of technology

Efficient sealing is achieved in a high-pressure gas environment, reducing the occurrence of gas leakage and bubbles, improving the mechanical strength and stability of the sealant, ensuring the safe operation and environmental protection of GIS equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005003495520000021
    Figure BDA0005003495520000021
  • Figure BDA0005003495520000071
    Figure BDA0005003495520000071
  • Figure BDA0005003495520000081
    Figure BDA0005003495520000081
Patent Text Reader

Abstract

The invention relates to the technical field of sealants, and particularly provides a flexible blocking agent, a preparation method thereof and GIS (Geographic Information System), the formula of the blocking agent comprises 60-80 parts of polydimethylsiloxane, 10-20 parts of modified epoxy POSS (Polyhedral Oligomeric Silsesquioxane), 2-5 parts of a silane coupling agent, 5-10 parts of a plasticizer and 0.1-0.5 part of a catalyst, and the modified epoxy POSS is epoxy POSS grafted with a benzene ring. When the flexible plugging agent is applied to a high-pressure gas leakage scene, high-pressure gas impact can be effectively resisted, the high-pressure gas can be well plugged, and the bubbling problem is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sealants, and in particular to a flexible plugging agent and a preparation method thereof, and a GIS. Background Art

[0002] GIS (gas insulated switchgear) is widely used in modern power systems due to its small footprint, superior insulation performance, and high reliability. SF6 gas, as the main insulation and arc extinguishing medium in GIS, has excellent insulation performance and arc extinguishing ability. However, during the long-term operation of GIS, due to factors such as installation process, mechanical stress, and material aging, trace leakage of SF6 gas may occur.

[0003] SF6 gas leakage will not only reduce the insulation performance and safety of the equipment, but also have a serious impact on the environment, because SF6 is a strong greenhouse gas, and its greenhouse effect potential is thousands of times that of carbon dioxide. Therefore, timely and effective sealing of SF6 gas leakage in GIS is an important task to ensure the safe operation of the power system and environmental protection.

[0004] Traditional GIS SF6 gas leakage plugging methods usually require power outages, resulting in power supply interruptions and affecting users' normal electricity demand. At the same time, power outage operations are complicated and time-consuming, increasing maintenance costs and workload. In order to avoid power outages, the prior art has proposed some pressure plugging methods, but in actual applications, during the pressure plugging process, the sealant often produces bubbling due to the pressure or impact of the leaking gas, resulting in poor plugging effect and failure to effectively prevent SF6 gas leakage. Summary of the invention

[0005] In view of this, the present invention proposes an improved plugging agent capable of plugging SF6 gas leakage in GIS under pressure.

[0006] In a first aspect, the present invention provides a flexible plugging agent, wherein the raw material formula of the plugging agent is calculated by weight as follows:

[0007]

[0008] The modified epoxy POSS is an epoxy POSS grafted with a benzene ring.

[0009] In some embodiments, the preparation method of modified epoxy POSS includes: dissolving epoxy POSS in anhydrous ethanol, slowly adding phenyltrimethoxysilane, then adding APTES, heating to 40-50°C, stirring at this temperature for 2 hours, filtering and drying to obtain modified epoxy POSS, wherein the mass ratio of epoxy POSS: anhydrous ethanol: phenyltrimethoxysilane: APTES is 1: (5-10): (0.4-0.6): (0.04-0.06).

[0010] In some embodiments, in the preparation method of modified epoxy POSS, heating to 40-50°C, keeping warm and stirring for 1-3 hours, after filtering and drying, further comprising adding toluene, polydicyclopentadiene and a catalyst, stirring and heating to 60-70°C, keeping warm and reacting for 5-7 hours, cooling to 25-35°C, filtering and drying to obtain modified epoxy POSS, wherein the catalyst is boron trifluoride ether complex.

[0011] In some embodiments, the mixture is heated to 40-50° C., kept warm and stirred for 1-3 hours, and the mass ratio of the solid material obtained after filtration and drying to the polydicyclopentadiene is 1:(1-3).

[0012] In some embodiments, the modified epoxy POSS is further subjected to a composite treatment, wherein the composite treatment comprises: dissolving the modified epoxy POSS in anhydrous ethanol, adding PAMAM, stirring for 3-5 hours, filtering and drying to obtain a composite-treated modified epoxy POSS.

[0013] In some embodiments, the PAMAM is a third generation polyamidoamine.

[0014] In some embodiments, the epoxy POSS is EP0408 produced by Hybrid Plastics.

[0015] In some embodiments, the silane coupling agent is methyltriethoxysilane, and / or; the plasticizer is silicone oil, and / or; the catalyst is dibutyltin dilaurate or a platinum catalyst.

[0016] In a second aspect, the present invention further provides a method for preparing the above-mentioned flexible plugging agent, comprising the following steps:

[0017] Step 1: mix polydimethylsiloxane, silane coupling agent and plasticizer, slowly add modified epoxy POSS under stirring, and stir mechanically to make it uniform;

[0018] Step 2: Add the catalyst, stir and disperse to obtain a flexible plugging agent.

[0019] In a third aspect, the present invention further provides a GIS device, which uses the above-mentioned flexible plugging agent for plugging treatment.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention generally provides a technical solution of a flexible plugging agent, which is particularly suitable for application in a high-pressure gas leakage environment, especially for plugging SF6 gas leakage in GIS. By introducing modified epoxy POSS, the mechanical strength and impact resistance of the material are significantly improved, ensuring an efficient sealing effect in a high-pressure gas environment, reducing gas leakage and the problem of bubbling during plugging. In addition, the low shrinkage and high mechanical properties of polydicyclopentadiene effectively reduce the bubbling phenomenon caused by pressure changes during use of the sealant, and the PAMAM high-score structure and multifunctional group in the composite treatment further enhance the adhesion and stability of the material, and reduce the probability of bubbling. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the embodiments of the present invention belong. If the definitions set forth in this section are contrary to or otherwise inconsistent with the definitions set forth in the patents, patent applications, published patent applications, and other publications incorporated herein by reference, the definitions listed in this section take precedence over the definitions incorporated herein by reference.

[0024] Unless otherwise specified, the methods used in the following examples are all conventional methods. Unless otherwise specified, the materials, reagents and instruments used are all conventional materials, reagents and instruments in the art, and can be obtained by those skilled in the art through commercial channels.

[0025] When an amount, concentration or other value or parameter is expressed as a range, a preferred range or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including the range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described herein, unless otherwise stated, the range is intended to include its end values ​​and all integers and fractions within the range. In the present specification and claims, range definitions can be combined and / or interchanged, and if not otherwise stated, these ranges include all subranges contained therein.

[0026] Conventional flexible silicone adhesives usually have insufficient mechanical strength before plugging. This results in the gas that continuously sprays outward exerting pressure on the adhesive film at the location where the high-pressure gas leaks, causing the adhesive film to be easily blown up and forming bubbles. The main reason is that the main matrix material in the flexible plugging adhesive has a soft and flexible molecular chain, lacks a rigid structure, and cannot provide high-strength support, such as polydimethylsiloxane (PDMS). In addition, inorganic fillers are generally used in these plugging adhesives. These fillers will form stress concentration points after uneven dispersion, making the plugging agent more likely to crack or deform under high pressure. Some plugging adhesive films have insufficient adhesion or cannot be tightly attached to the surface of the substrate. High-pressure gas can also easily form gaps between the adhesive film and the substrate, causing the adhesive film to be blown up. The lack of adhesion is mainly due to the large difference in surface energy between the silicone adhesive matrix and the adhered substrate, resulting in the poor chemical bond between the silicone adhesive matrix and the surface of the substrate. Some plugging adhesive films have insufficient mechanical strength and elasticity, cannot resist the impact of high-pressure gas, and are easily deformed or broken, forming bubbles. This bubbling problem seriously affects the sealing effect of the sealing glue on the leaking position.

[0027] In the technical solution of the present application, modified epoxy POSS with grafted benzene rings is mainly used. The modified epoxy POSS improves the mechanical strength and rigidity of the film by introducing benzene rings, so that it can better resist the impact of high-pressure gas. The epoxy group provides better adhesion performance, so that the film can adhere tightly to the surface of the substrate, reducing the entry of high-pressure gas into the gap between the film and the substrate.

[0028] The introduction of the benzene ring structure enhances the rigidity and heat resistance of the modified POSS. At the molecular level, the benzene ring provides rigidity, making the overall material more resistant to deformation when subjected to high-pressure gas impact. The amino-containing APTES forms stronger chemical bonds by reacting with epoxy groups. These chemical bonds increase the cross-linking density between molecules and improve the mechanical strength and adhesion properties of the material.

[0029] By introducing the modified epoxy POSS and making it evenly dispersed in the PDMS matrix, a reinforced composite material structure is formed, making the material less likely to deform or break under high pressure environments.

[0030] In some specific technical schemes of the present application, polydicyclopentadiene is introduced into the modified epoxy POSS. Polydicyclopentadiene has excellent mechanical strength and impact resistance, which can enable the sealing film to withstand the impact of high-pressure gas without being blown away. At the same time, the low shrinkage and high chemical resistance of polydicyclopentadiene further enhance the stability of the film and reduce the risk of deformation and rupture.

[0031] The polymer chain of polydicyclopentadiene reacts with epoxy POSS, which increases the intermolecular interaction force inside the material and at the interface, and improves the overall adhesion performance.

[0032] In other specific technical solutions of the present application, modified epoxy POSS is also compounded with PAMAM, which has a high branching structure and multifunctional groups, which helps to further improve the adhesion and stability of the film. The multifunctional group can be combined with the modified POSS to make the film have better uniformity and consistency, avoid local stress concentration, and help to further enhance the ability to resist high-pressure gas impact.

[0033] Epoxy POSS has a large molecular weight and a complex molecular structure. Through the reaction of phenyltrimethoxysilane and APTES, functional groups such as benzene rings and amino groups are introduced. The amino groups in APTES can undergo a ring-opening reaction with epoxy groups, further increasing the reactivity and adhesion properties of epoxy POSS. The silane groups combine with the siloxane network through hydrolysis and condensation, which helps to improve the crosslinking density and stability of the material. Ultimately, the thermal stability, mechanical strength and adhesion properties of epoxy POSS are improved, making the modified epoxy POSS perform better under high temperature and mechanical stress. After a stirring and heating reaction at 40-50°C for 2h, the reaction is ensured to be fully carried out, and a relatively pure modified epoxy POSS is obtained after filtration and drying.

[0034] The mixture of PDMS, silane coupling agent and silicone oil provides basic flexibility and adhesion properties. The introduction of modified epoxy POSS enhances the mechanical properties and adhesion properties of the plugging agent, especially the sealing effect under high pressure environment. The addition of catalyst promotes the cross-linking reaction to form a stable network structure, among which modified epoxy POSS provides enhanced mechanical strength and adhesion properties. By slowly adding and mechanically stirring, it is ensured that the modified epoxy POSS is evenly dispersed in the PDMS matrix to form a stable composite material. It helps the plugging agent maintain the structural stability of the film under the impact of high-pressure gas, so as to achieve the purpose of leak prevention and plugging.

[0035] In some further improved schemes, PDCPD forms a three-dimensional network structure with a certain degree of crosslinking with modified epoxy POSS grafted with phenyltrimethoxysilane after catalytic reaction, which helps to improve the compactness and stability of the material and reduce the pores inside the material, thereby effectively preventing the generation of bubbles in a high-pressure gas environment. In addition, PDCPD itself has a relatively low shrinkage and will not shrink significantly during the curing and curing process, reducing the generation of internal stress in the material, so that the plugging agent can still maintain the consistency of the internal structure during and after curing. At the same time, it can also improve the thermal stability of the material, so that the plugging agent can still maintain mechanical properties in high temperature and chemical environments.

[0036] In other further improved schemes, PAMAM is composited with modified epoxy POSS grafted with phenyltrimethoxysilane, wherein PAMAM has a high-branched structure and multifunctional groups. PAMAM and modified epoxy POSS are evenly mixed by dissolving in ethanol and stirring for a certain period of time to form a high-performance composite material. This composite material has improved adhesion and mechanical strength, provides good cross-linking density through the high-branched structure, reduces internal voids and micropores, helps prevent gas penetration and diffusion, reduces bubbling, and enables the material to perform better under high-pressure environments.

[0037] The performance of the flexible plugging agent of the present application is tested through specific examples below.

[0038] In the following examples and comparative examples, the epoxy POSS used is produced by Hybrid Plastics Company, model EP0408.

[0039] Example 1

[0040] This embodiment provides a method for preparing a flexible plugging agent, and the weight proportion of the formula is as follows:

[0041]

[0042]

[0043] Preparation of modified epoxy POSS:

[0044] 10 g of epoxy POSS was dissolved in 50 g of anhydrous ethanol, and 5 g of phenyltrimethoxysilane was slowly added dropwise. After the addition was completed, 0.5 g of APTES was added, and then stirred and heated to 45°C. The mixture was stirred and reacted for 2 h, and then filtered and dried to obtain modified epoxy POSS.

[0045] Preparation of flexible plugging agent:

[0046] Polydimethylsiloxane, methyltriethoxysilane and silicone oil are mixed and stirred evenly. Under stirring, modified epoxy POSS is slowly added and mechanically stirred evenly. Then, dibutyltin dilaurate is added and stirred evenly to obtain a flexible plugging agent.

[0047] Example 2

[0048] This embodiment provides a method for preparing a flexible plugging agent, and the weight proportion of the formula is as follows:

[0049]

[0050] Preparation of modified epoxy POSS:

[0051] 10 g of epoxy POSS was dissolved in 70 g of anhydrous ethanol, and 4 g of phenyltrimethoxysilane was slowly added dropwise. After the addition was completed, 0.4 g of APTES was added, and then stirred and heated to 40°C. The mixture was stirred and reacted for 2 h, and then filtered and dried to obtain modified epoxy POSS.

[0052] Preparation of flexible plugging agent:

[0053] Polydimethylsiloxane, methyltriethoxysilane and silicone oil are mixed and stirred evenly. Under stirring, modified epoxy POSS is slowly added and mechanically stirred evenly. Then, dibutyltin dilaurate is added and stirred evenly to obtain a flexible plugging agent.

[0054] Example 3

[0055] This embodiment provides a method for preparing a flexible plugging agent, and the weight proportion of the formula is as follows:

[0056]

[0057] Preparation of modified epoxy POSS:

[0058] 10 g of epoxy POSS was dissolved in 100 g of anhydrous ethanol, and 6 g of phenyltrimethoxysilane was slowly added dropwise. After the addition was completed, 0.6 g of APTES was added, and then stirred and heated to 50°C. The mixture was stirred and reacted for 2 h, and then filtered and dried to obtain modified epoxy POSS.

[0059] Preparation of flexible plugging agent:

[0060] Polydimethylsiloxane, methyltriethoxysilane and silicone oil are mixed and stirred evenly. Under stirring, modified epoxy POSS is slowly added and mechanically stirred evenly. Then, dibutyltin dilaurate is added and stirred evenly to obtain a flexible plugging agent.

[0061] Example 4

[0062] This embodiment provides a method for preparing a flexible plugging agent, and the weight proportion of the formula is as follows:

[0063]

[0064] Preparation of modified epoxy POSS:

[0065] Dissolve 10g of epoxy POSS in 50g of anhydrous ethanol, slowly add 5g of phenyltrimethoxysilane, after the addition is completed, add 0.5g of APTES, then stir and heat to 45°C, keep stirring and react for 2h, then filter and dry, mix the obtained material with toluene, polydicyclopentadiene and boron trifluoride ether complex in a mass ratio of 1:1:0.1, heat to 65°C, keep warm and react for 6h, then cool to 30°C, filter and dry to obtain modified epoxy POSS.

[0066] Preparation of flexible plugging agent:

[0067] Polydimethylsiloxane, methyltriethoxysilane and silicone oil are mixed and stirred evenly. Under stirring, modified epoxy POSS is slowly added and mechanically stirred evenly. Then, dibutyltin dilaurate is added and stirred evenly to obtain a flexible plugging agent.

[0068] Example 5

[0069] This embodiment provides a method for preparing a flexible plugging agent, and the weight proportion of the formula is as follows:

[0070]

[0071]

[0072] Preparation of modified epoxy POSS:

[0073] Dissolve 10g of epoxy POSS in 50g of anhydrous ethanol, slowly add 5g of phenyltrimethoxysilane, after the addition is completed, add 0.5g of APTES, then stir and heat to 45°C, keep stirring and react for 2h, then filter and dry, mix the obtained material with toluene, polydicyclopentadiene and boron trifluoride ether complex in a mass ratio of 1:3:0.1, heat to 65°C, keep warm and react for 6h, then cool to 30°C, filter and dry to obtain modified epoxy POSS.

[0074] Preparation of flexible plugging agent:

[0075] Polydimethylsiloxane, methyltriethoxysilane and silicone oil are mixed and stirred evenly. Under stirring, modified epoxy POSS is slowly added and mechanically stirred evenly. Then, dibutyltin dilaurate is added and stirred evenly to obtain a flexible plugging agent.

[0076] Example 6

[0077] This embodiment provides a method for preparing a flexible plugging agent, and the weight proportion of the formula is as follows:

[0078]

[0079]

[0080] Preparation of modified epoxy POSS:

[0081] Dissolve 10g of epoxy POSS in 50g of anhydrous ethanol, slowly add 5g of phenyltrimethoxysilane, after the addition is completed, add 0.5g of APTES, then stir and heat to 45°C, keep stirring and react for 2h, then filter and dry, mix the obtained material with toluene, polydicyclopentadiene and boron trifluoride ether complex in a mass ratio of 1:2:0.1, heat to 65°C, keep warm and react for 6h, then cool to 30°C, filter and dry to obtain modified epoxy POSS.

[0082] Preparation of flexible plugging agent:

[0083] Polydimethylsiloxane, methyltriethoxysilane and silicone oil are mixed and stirred evenly. Under stirring, modified epoxy POSS is slowly added and mechanically stirred evenly. Then, dibutyltin dilaurate is added and stirred evenly to obtain a flexible plugging agent.

[0084] Example 7

[0085] This embodiment provides a method for preparing a flexible plugging agent, and the weight proportion of the formula is as follows:

[0086]

[0087] Preparation of modified epoxy POSS:

[0088] Dissolve 10 g of epoxy POSS in 50 g of anhydrous ethanol, slowly add 5 g of phenyltrimethoxysilane, add 0.5 g of APTES after the addition is complete, then stir and heat to 45 ° C, keep stirring and react for 2 hours, then filter and dry, mix the obtained material with toluene, polydicyclopentadiene and boron trifluoride ether complex in a mass ratio of 1:2:0.1, heat to 65 ° C, keep warm and react for 6 hours, then cool to 30 ° C, filter and dry, then dissolve the dried modified epoxy POSS in anhydrous ethanol, then add the third-generation PAMAM, stir for 4 hours, filter and dry to obtain a composite-treated modified epoxy POSS, wherein the mass ratio of modified epoxy POSS: anhydrous ethanol: third-generation PAMAM is 1:10:0.15.

[0089] Preparation of flexible plugging agent:

[0090] Polydimethylsiloxane, methyltriethoxysilane and silicone oil are mixed and stirred evenly. Under stirring, the composite-treated modified epoxy POSS is slowly added and mechanically stirred evenly. Then, dibutyltin dilaurate is added and stirred evenly to obtain a flexible plugging agent.

[0091] Example 8

[0092] This example is based on Example 7, keeping other conditions the same, except that the PAMAM used is the second generation.

[0093] Example 9

[0094] This embodiment is based on the embodiment 7, keeping other conditions the same, except that the PAMAM used is the fourth generation.

[0095] Example 10

[0096] This embodiment provides a method for preparing a flexible plugging agent, and the weight proportion of the formula is as follows:

[0097]

[0098]

[0099] Preparation of modified epoxy POSS:

[0100] Dissolve 10 g of epoxy POSS in 50 g of anhydrous ethanol, slowly add 5 g of phenyltrimethoxysilane, add 0.5 g of APTES after the addition is complete, and then stir and heat to 45°C, keep stirring and react for 2 hours, then filter and dry, then dissolve the modified epoxy POSS after drying in anhydrous ethanol, then add the third-generation PAMAM, stir for 4 hours, filter and dry to obtain a composite-treated modified epoxy POSS, wherein the mass ratio of modified epoxy POSS: anhydrous ethanol: third-generation PAMAM is 1:10:0.15.

[0101] Preparation of flexible plugging agent:

[0102] Polydimethylsiloxane, methyltriethoxysilane and silicone oil are mixed and stirred evenly. Under stirring, the composite-treated modified epoxy POSS is slowly added and mechanically stirred evenly. Then, dibutyltin dilaurate is added and stirred evenly to obtain a flexible plugging agent.

[0103] Embodiment 11

[0104] This example is based on Example 10, keeping other conditions the same, except that the PAMAM used is the second generation.

[0105] Example 12

[0106] This embodiment is based on the embodiment 10, keeping other conditions the same, except that the PAMAM used is the fourth generation.

[0107] Comparative Example 1

[0108] This comparative example provides a method for preparing a flexible plugging agent using conventional epoxy POSS, and the weight proportion of the formula is as follows:

[0109]

[0110]

[0111] Preparation of flexible plugging agent:

[0112] Polydimethylsiloxane, methyltriethoxysilane and silicone oil are mixed and stirred evenly. Under stirring, epoxy POSS is slowly added and mechanically stirred evenly. Then, dibutyltin dilaurate is added and stirred evenly to obtain a flexible plugging agent.

[0113] Comparative Example 2

[0114] This comparative example provides a preparation method using conventional fillers, and the weight proportion of the formula is as follows:

[0115]

[0116] Preparation of flexible plugging agent:

[0117] Polydimethylsiloxane, methyltriethoxysilane and silicone oil are mixed and stirred evenly. Under stirring, silicon dioxide is slowly added and mechanically stirred evenly. Then, dibutyltin dilaurate is added and stirred evenly to obtain a flexible plugging agent.

[0118] The performance of the plugging agents prepared in the above examples and comparative examples was verified respectively, and the verification method was as follows:

[0119] A 40mm*40mm square plane area is processed on the surface of the container, and a circular hole with a diameter of 0.5mm is drilled in the center of the square plane area with a micro drill bit. The plugging agents prepared in the above embodiments and comparative examples are evenly coated and filled in the square area, and the coating thickness is 3mm. After coating, nitrogen is flushed into the container, and the nitrogen pressure is timed from 0.3MPa, maintained at 0.3MPa for 1min, and then increased to 0.4MPa and maintained for 1min, and so on, until the pressure is increased to 0.9MPa and maintained for 1min. The height change of the plugging agent film in the square plane area is observed by a camera. When the height change exceeds 1mm, the corresponding gas pressure value and the corresponding pressure holding time are recorded. If it exceeds 1mm during the pressure increase process, it is recorded as 0s of the pressure value after the pressure increase. The specific recorded data are shown in the following table:

[0120] Grouping Pressure when exceeding 1mm / MPa When the pressure exceeds 1mm, the corresponding holding time / s Example 1 0.5 12 Example 2 0.4 34 Example 3 0.5 6 Example 4 0.7 15 Example 5 0.7 44 Example 6 0.7 57 Example 7 0.9 >60 Example 8 0.9 22 Example 9 0.8 49 Example 10 0.6 54 Embodiment 11 0.5 31 Example 12 0.6 25 Comparative Example 1 0.3 22 Comparative Example 2 0.3 0

[0121] The above embodiments 1-3 respectively adopt raw materials of different proportions, and the modified epoxy POSS is the epoxy POSS modified by benzene ring grafting. Compared with Comparative Example 1, the pressure resistance is significantly improved, and the maximum 12S can be kept without bubbling under 0.5MPa pressure. Embodiments 4-6 adopt a further improvement scheme. Under the premise of adopting benzene ring grafting modification, polydicyclopentadiene is also introduced for grafting modification, which further improves

[0122] The pressure resistance of the plugging agent is that after coating, the coating surface can maintain no deformation under a pressure of 0.7 MPa. Examples 7-9 further introduce PAMAM on the basis of Example 6, wherein Example 7 introduces the third generation, and Examples 8-9 introduce the second and fourth generations respectively. It can be seen that the comprehensive performance of the third generation is significantly better than that of the second and fourth generations. Similarly, Examples 10-12 introduce PAMAM on the basis of Example 1, and the comprehensive performance of the third generation is also better than that of the second and fourth generations, and compared with Example 1, there is a significant performance improvement.

[0123] In summary, the present application provides a flexible plugging agent using modified epoxy POSS, which has good performance in the scenario of plugging high-pressure gas leakage, especially in resisting gas shock and bubbling risk problems.

[0124] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A flexible plugging agent, characterized in that: The raw material formula is calculated by weight: The modified epoxy POSS is an epoxy POSS grafted with a benzene ring.

2. The flexible plugging agent according to claim 1, characterized in that: The preparation method of the modified epoxy POSS comprises: dissolving the epoxy POSS in anhydrous ethanol, slowly dropping phenyltrimethoxysilane, then adding APTES, heating to 40-50° C., keeping warm and stirring for 2 hours, filtering and drying to obtain the modified epoxy POSS, wherein the mass ratio of the epoxy POSS: anhydrous ethanol: phenyltrimethoxysilane: APTES is 1: (5-10): (0.4-0.6): (0.04-0.06).

3. The flexible plugging agent according to claim 2, characterized in that: In the preparation method of modified epoxy POSS, the process comprises heating to 40-50°C, keeping warm and stirring for 1-3 hours, and after filtering and drying, adding toluene, polydicyclopentadiene and a catalyst, stirring and heating to 60-70°C, keeping warm and reacting for 5-7 hours, cooling to 25-35°C, filtering and drying to obtain modified epoxy POSS, wherein the catalyst is boron trifluoride ether complex.

4. The flexible plugging agent according to claim 3, characterized in that: Heat to 40-50°C, keep warm and stir for 1-3h, and after filtering and drying, the mass ratio of the obtained solid material to polydicyclopentadiene is 1:(1-3).

5. The flexible plugging agent according to claim 1, characterized in that: The modified epoxy POSS is further subjected to a composite treatment, wherein the steps of the composite treatment include: dissolving the modified epoxy POSS in anhydrous ethanol, adding PAMAM, stirring for 3-5 hours, filtering and drying to obtain the composite-treated modified epoxy POSS.

6. The flexible plugging agent according to claim 5, characterized in that: The PAMAM is a third generation polyamidoamine.

7. The flexible plugging agent according to claim 1, characterized in that: The epoxy POSS is EP0408 produced by Hybrid Plastics.

8. The flexible plugging agent according to claim 1, characterized in that: The silane coupling agent is methyltriethoxysilane, and / or; the plasticizer is silicone oil, and / or; the catalyst is dibutyltin dilaurate or a platinum catalyst.

9. The method for preparing the flexible plugging agent according to any one of claims 1 to 8, characterized in that: The steps include: Step 1: mix polydimethylsiloxane, silane coupling agent and plasticizer, slowly add modified epoxy POSS under stirring, and stir mechanically to make it uniform; Step 2: Add the catalyst, stir and disperse to obtain a flexible plugging agent.

10. A GIS device, characterized in that: The GIS equipment is sealed using the flexible organic sealing agent described in any one of claims 1-8.

Citation Information

Patent Citations

  • High-modulus and high-toughness epoxy structural adhesive and preparation method and application thereof

    CN113444457A

  • Epoxy adhesive, encapsulation layer and application thereof

    CN114196357A

  • Silicone adhesive for sealing electronic product and preparation method thereof

    CN114921221A

  • High-thixotropy single-component room temperature vulcanized silicone adhesive and preparation method thereof

    CN115895586A

Cited By

  • Plugging material as well as preparation method and application thereof

    CN121517647A