Preparation method of self-aligned gate GaN HEMT device

By using etching and wet corrosion to form a T-shaped structure in GaN HEMT devices, the production of source and drain electrodes is simplified, the problem of complex processes and low yield in the prior art is solved, and higher frequency characteristics are achieved and lower parasitic resistance effects.

CN119008405AActive Publication Date: 2024-11-22XIDIAN UNIV

Patent Information

Application Number
CN202410999574.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-22
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

Existing GaN HEMT devices have complex device structures and processes in high-frequency applications, which are difficult to achieve mass production, and the yield of self-aligned gate technology is poor, which affects the improvement of frequency characteristics.

Method used

By stacking the substrate, gallium nitride layer, barrier layer and silicon nitride layer on the wafer, a T-shaped structure is formed by etching and wet etching to achieve selective growth when growing N+GaN, and simplifying the source and drain electricity The manufacturing process of electrodes and gate electrodes is used to etch the silicon nitride dielectric as a mask to expose the source and drain electrodes and reduce parasitic capacitance.

Benefits of technology

The selective growth of N+GaN is achieved, which reduces process complexity and cost, improves yield, reduces parasitic resistance, and improves the frequency characteristics of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008405A_ABST
    Figure CN119008405A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a self-aligned gate GaN HEMT device. The preparation method comprises the following steps: providing a wafer; forming a first regrowth region and a second regrowth region on the surface of the wafer; the silicon nitride layer in the middle area is used as a mask, and etching liquid is used for corroding the two sides of the silicon dioxide layer in the middle area, so that the silicon nitride layer and the silicon dioxide layer form a T-shaped structure; preparing a source electrode on the first N + GaN layer, and preparing a drain electrode on the second N + GaN layer; depositing a silicon nitride dielectric layer in the first region, the middle region and the second region, and polishing to flatten the upper surface of the device and expose the silicon dioxide layer in the middle region; corroding off the silicon dioxide layer in the middle region to form a groove, and preparing a gate electrode in the groove; and etching the silicon nitride dielectric layers of the first region and the second region of the device by using the gate electrode as a mask so as to expose the source electrode and the drain electrode. According to the invention, the performance of the GaN HEMT device can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of semiconductor technology, and in particular relates to a method for preparing a self-aligned gate GaN HEMT device. Background Art

[0002] GaN HEMT devices have become a key device technology for millimeter wave applications due to their excellent material properties. Driven by emerging fields such as 6G communications, automotive radar, and medical imaging, the demand for GaN RF devices is growing. Based on this, GaN HEMT devices need to continuously improve their frequency characteristics to meet the needs of RF applications. For example, in 6G wireless communications, the operating frequency of the equipment can reach the terahertz range, and GaN RF devices are required to achieve a characteristic frequency of more than 100G. Although there are scientific research literature reports on related high-frequency GaN HEMT devices, their device structure and process are very complex and have poor feasibility. There is no device technology that can be mass-produced at this frequency.

[0003] Improving the frequency characteristics of GaN millimeter wave devices requires scaling the lateral and longitudinal dimensions of the device. The longitudinal scaling shortens the distance from the gate to the channel by using AlN strong polarization thin barriers to reduce the short channel effect; the lateral scaling requires both the gate length and the source-drain spacing to be reduced. Simply reducing the gate length of the device will produce negative parasitic effects while increasing the frequency. For example, it will produce source-drain parasitic resistance. More importantly, the depletion region near the drain that stretches as the source-drain voltage increases blocks the enhancement of the lateral electric field under the gate, causing a decrease in the average drift velocity of electrons on a macro scale, increasing the drain delay, and thus hindering the improvement of the frequency characteristics. Therefore, it is necessary to reduce the contact resistance and reduce the spacing between the source and drain. Due to the difficulty of the GaN ion implantation doping process, the method of growing N+GaN is generally used to reduce the contact resistance. After the growth is completed, the N+GaN outside the source and drain regions is removed by etching or etching masking, and then the gate is made between the source and drain regions. Therefore, the distance between the source and drain is directly determined by the overlay accuracy of the lithography. In order to solve this problem, HRL Laboratory first proposed the self-aligned gate technology. However, the existing self-aligned gate technology is complex and has a poor yield rate. Summary of the invention

[0004] In order to solve the above problems existing in the prior art, the present invention provides a method for preparing a self-aligned gate GaN HEMT device. The technical problem to be solved by the present invention is achieved by the following technical solution:

[0005] In a first aspect, the present invention provides a method for preparing a self-aligned gate GaN HEMT device, comprising:

[0006] A wafer is provided, wherein the wafer comprises a substrate, a gallium nitride layer, a barrier layer, a silicon dioxide layer and a silicon nitride layer which are stacked in sequence;

[0007] The silicon nitride layer, the silicon dioxide layer, the barrier layer, and at least a portion of the gallium nitride layer in the first region and the second region of the device are etched away to form a first regrown region and a second regrown region, respectively;

[0008] Using the silicon nitride layer in the middle region of the device as a mask, etching liquid is used to etch both sides of the silicon dioxide layer in the middle region of the device, so that the silicon nitride layer and the silicon dioxide layer in the middle region of the device form a T-shaped structure;

[0009] Growing N+GaN in the first region, the middle region, and the second region of the device, forming a first N+GaN layer in the first regrown region, forming a second N+GaN layer in the second regrown region, and forming a polycrystalline GaN layer on the silicon nitride layer; preparing a source electrode on the first N+GaN layer, and preparing a drain electrode on the second N+GaN layer;

[0010] Depositing a silicon nitride dielectric layer on the first region, the middle region, and the second region of the device to cover the source electrode, the drain electrode, and the polycrystalline GaN layer, and polishing the first region, the middle region, and the second region of the device to flatten the upper surfaces of the first region, the middle region, and the second region of the device, and exposing the silicon dioxide layer in the middle region of the device;

[0011] The silicon dioxide layer in the middle area of ​​the device is etched away to form a groove, and a gate electrode is prepared in the groove and on the upper surface of the silicon nitride dielectric layer in the first area and the silicon nitride dielectric layer in the second area of ​​the device;

[0012] Using the gate electrode as a mask, etching the silicon nitride dielectric layer in the first region and the silicon nitride dielectric layer in the second region of the device to expose the source electrode and the drain electrode;

[0013] The middle region of the device is located between the first region and the second region.

[0014] Optionally, etching away the silicon nitride layer, the silicon dioxide layer, the barrier layer, and at least a portion of the gallium nitride layer in the first region and the second region of the device to form a first regrown region and a second regrown region, respectively, comprises:

[0015] Coating a layer of photoresist on the upper surface of the silicon nitride layer, and etching the photoresist, silicon dioxide layer and silicon nitride layer in the first region and the second region of the device using F-based plasma;

[0016] The photoresist in the middle area of ​​the device is removed by using a degumming solvent, the silicon dioxide layer and the silicon nitride layer in the middle area of ​​the device are used as masks, and the barrier layer and at least a portion of the gallium nitride layer in the first area of ​​the device are etched by using Cl-based plasma to form a first re-growth area, and the barrier layer and at least a portion of the gallium nitride layer in the second area of ​​the device are etched by using Cl-based plasma to form a second re-growth area.

[0017] Optionally, before forming a gate electrode in the groove and on the upper surface of the silicon nitride dielectric layer in the first region and the silicon nitride dielectric layer in the second region of the device, the method further includes:

[0018] A silicon nitride film is deposited in the groove and on the upper surface of the silicon nitride dielectric layer, and then the silicon nitride film on the upper surface of the silicon nitride dielectric layer is etched away, and the silicon nitride film at the bottom of the groove is etched away, leaving the silicon nitride film on the side wall of the groove.

[0019] Optionally, etching away the silicon nitride film on the upper surface of the silicon nitride dielectric layer and etching away the silicon nitride film at the bottom of the groove includes:

[0020] The silicon nitride film on the upper surface of the silicon nitride dielectric layer and the silicon nitride film at the bottom of the groove are etched away using F-based plasma.

[0021] Optionally, the etching solution is a buffered oxide etching solution.

[0022] Optionally, growing N+GaN in the first region, the middle region, and the second region of the device includes:

[0023] Using molecular beam epitaxy, N+GaN is grown in the first region, the middle region and the second region of the device.

[0024] Optionally, a silicon nitride dielectric layer is deposited in the first region, the middle region and the second region of the device, and the silicon nitride dielectric layer at least covers two sides of the silicon dioxide layer.

[0025] Optionally, polishing the first region, the middle region, and the second region of the device comprises:

[0026] The first region, the middle region and the second region of the device are polished by chemical mechanical polishing.

[0027] Optionally, using the gate electrode as a mask to etch the silicon nitride dielectric layer in the first region and the silicon nitride dielectric layer in the second region of the device includes:

[0028] The silicon nitride dielectric layer in the first region and the silicon nitride dielectric layer in the second region of the device are etched using F-based plasma.

[0029] Beneficial effects of the present invention:

[0030] 1. The selectivity of silicon nitride and silicon dioxide layers is different when wet-etched with a buffered oxide etchant. After the lateral width of silicon dioxide is reduced, a T-shaped structure is formed. During the growth of N+GaN, the silicon nitride layer shields the gate electrode area. The silicon nitride layer is subsequently removed during the planarization process to achieve selective growth of N+GaN, thereby overcoming the process complexity and difficulty of using wet etching to remove polycrystalline GaN on the mask surface.

[0031] 2. Use the gate electrode as a mask to etch the silicon nitride dielectric, exposing the source and drain electrodes while forming a support layer for the gate electrode, while reducing parasitic capacitance and avoiding the step of photolithography and etching holes. The formed gate electrode support is also conducive to improving the yield rate.

[0032] 3. Compatible with molecular beam epitaxy and metal organic chemical vapor deposition N+GaN processes; among them, molecular beam epitaxy is carried out in an ultra-high vacuum environment, the mean free path of molecules (atoms) is very large, and it is not easy to reach the inner side of the T-shaped structure; metal organic chemical vapor deposition is heteroepitaxial on silicon nitride and silicon dioxide, and it is not easy to attach to the T-shaped structure. Therefore, selective growth of N+GaN can be achieved using both processes.

[0033] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a flow chart of a method for preparing a self-aligned gate GaN HEMT device provided by an embodiment of the present invention;

[0035] FIG. 2( a ) to (i ) are schematic diagrams of a method for preparing a self-aligned gate GaN HEMT device provided in an embodiment of the present invention;

[0036] Figure 3(a) to 3(c) is another schematic diagram of a method for preparing a self-aligned gate GaN HEMT device provided by an embodiment of the present invention;

[0037] Figures 4(a) to 4(h) It is another schematic diagram of a method for preparing a self-aligned gate GaN HEMT device provided by an embodiment of the present invention. DETAILED DESCRIPTION

[0038] The present invention is further described in detail below with reference to specific embodiments, but the embodiments of the present invention are not limited thereto.

[0039] In order to improve the operating frequency of GaN HEMT (gallium nitride high electron mobility transistor) devices, reducing the device size is the most direct and important method. When the gate length is reduced to less than 100nm, severe short channel effect, large source-drain parasitic resistance, and drain delay that increases with the increase of source-drain voltage become important factors that limit the frequency characteristics of HEMT devices. Among them, the influence of short channel effect can be eliminated by using AlN (aluminum nitride) thin barrier layer materials, and the influence of parasitic resistance and drain delay needs to be solved by using N+GaN (N-type heavily doped GaN) and reducing the source-drain spacing. Compared with silicon-based MOSFET (metal oxide semiconductor field effect transistor) devices that use polysilicon gates and ion implantation doping to achieve source-drain self-alignment to reduce the source-drain spacing, the ion implantation doping activation temperature of GaN HEMT devices is high and the activation efficiency is low. At the same time, the mask materials used for implantation and activation have compatibility issues with subsequent processes, and are still difficult to apply. Usually, the parasitic resistance is reduced by growing N+GaN, but source and drain lithography selection and gate lithography are required before or after growth, and alignment and overlay are required between the two lithography. For example, taking a gate length of 150nm as an example, in order to successfully produce a device with a source-drain spacing of less than 250nm, the overlay error needs to be kept within 50nm. Due to the limitations of the current GaN process and the capacity of the mainstream production lines of III-V compound semiconductors, such conditions are difficult to achieve. In response to such difficulties, HRL Laboratory proposed a gate self-alignment technology that can effectively shorten the source-drain spacing. However, the process steps of this technology are complex, and the difficulty of production also brings problems of high cost and low yield for large-scale applications.

[0040] In view of this, the present invention provides a method for preparing a self-aligned gate GaN HEMT device, which uses silicon nitride and silicon dioxide as masks, forms a T-shaped structure through etching and wet etching, and realizes selective growth when growing N+GaN; at the same time, it simplifies the manufacturing process steps of the source and drain electrodes and the gate electrode support, improves the yield and reduces the cost. At the same time, the process is in line with the current mainstream production line capabilities of GaN and III-V compound semiconductors, and can achieve lower parasitic resistance, higher gain and higher frequency characteristics of GaN HEMT devices.

[0041] See also Figure 1 , Figure 1 FIG. 2 is a flow chart of a method for preparing a self-aligned gate GaN HEMT device provided in an embodiment of the present invention. FIG. 2(a) to (i) are schematic diagrams of a method for preparing a self-aligned gate GaN HEMT device provided in an embodiment of the present invention. A method for preparing a self-aligned gate GaN HEMT device provided in the present invention includes:

[0042] S101, providing a wafer, wherein the wafer comprises a substrate, a gallium nitride layer, a barrier layer, a silicon dioxide layer and a silicon nitride layer stacked in sequence, as shown in FIG2(a).

[0043] Specifically, in this embodiment, a substrate is first provided, which includes a substrate, a gallium nitride layer and a barrier layer, and a silicon dioxide layer and a silicon nitride layer are deposited on the upper surface of the barrier layer to form a wafer; optionally, the substrate can be any one of a silicon carbide substrate, an aluminum oxide substrate or a silicon substrate, and the material of the barrier layer is AlN.

[0044] S102, etching away the silicon nitride layer, the silicon dioxide layer, the barrier layer, and at least a portion of the gallium nitride layer in the first region and the second region of the device to form a first regrown region and a second regrown region, respectively, as shown in FIG. 2(b).

[0045] Specifically, in this embodiment, the silicon nitride layer, the silicon dioxide layer, the barrier layer, and at least a portion of the gallium nitride layer in the first region and the second region of the device are etched away to form a first regrown region and a second regrown region, respectively, including:

[0046] A layer of photoresist is coated on the upper surface of the silicon nitride layer, and the photoresist in the middle area of ​​the device is used as a mask, and the photoresist, silicon dioxide layer and silicon nitride layer in the first area and the second area of ​​the device are etched using F-based plasma. Due to the lateral etching effect, the silicon nitride layer and the silicon dioxide layer shrink slightly in the lateral direction; it should be noted that due to the different material properties, the F-based plasma will not etch the barrier layer;

[0047] The photoresist in the middle area of ​​the device is removed by using a degumming solvent, the silicon dioxide layer and the silicon nitride layer in the middle area of ​​the device are used as masks, and the barrier layer and at least a portion of the gallium nitride layer in the first area of ​​the device are etched by using Cl-based plasma to form a first regrown area. The barrier layer and at least a portion of the gallium nitride layer in the second area of ​​the device are etched by using Cl-based plasma to form a second regrown area. The formed first regrown area and the second regrown area are provided for contact between the subsequently formed N+GaN and the two-dimensional electron gas channel.

[0048] S103, using the silicon nitride layer in the middle region of the device as a mask, using an etching solution to etch both sides of the silicon dioxide layer in the middle region of the device, so that the silicon nitride layer and the silicon dioxide layer in the middle region of the device form a T-shaped structure, as shown in FIG. 2(c).

[0049] Specifically, in this embodiment, the etching solution is a buffered oxide etching solution, wherein the etching rate of silicon nitride by the buffered oxide etching solution is much lower than the etching rate of silicon dioxide, and therefore, silicon nitride is used as a mask.

[0050] S104, grow N+GaN in the first region, the middle region and the second region of the device, form a first N+GaN layer in the first regrown region, form a second N+GaN layer in the second regrown region, and form a polycrystalline GaN layer on the silicon nitride layer; prepare a source electrode on the first N+GaN layer, and prepare a drain electrode on the second N+GaN layer, as shown in Figure 2(d).

[0051] Specifically, in this embodiment, growing N+GaN in the first region, the middle region, and the second region of the device includes:

[0052] Using molecular beam epitaxy or metal organic chemical vapor deposition, N+GaN is grown in the first region, the middle region and the second region of the device.

[0053] It should be noted that, due to the lattice mismatch between N+GaN and the silicon nitride layer, polycrystalline GaN is grown on the silicon nitride layer.

[0054] S105. Depositing a silicon nitride dielectric layer in the first region, the middle region and the second region of the device to cover the source electrode, the drain electrode and the polycrystalline GaN layer, and polishing the first region, the middle region and the second region of the device to flatten the upper surfaces of the first region, the middle region and the second region of the device and expose the silicon dioxide layer in the middle region of the device, as shown in Figures 2(e) and (f).

[0055] Specifically, in this embodiment, a silicon nitride dielectric layer is deposited in the first region, the middle region, and the second region of the device, and the silicon nitride dielectric layer at least covers two sides of the silicon dioxide layer.

[0056] S106, etching away the silicon dioxide layer in the middle region of the device to form a groove, and preparing a gate electrode in the groove and on the upper surface of the silicon nitride dielectric layer in the first region and the silicon nitride dielectric layer in the second region of the device, as shown in FIGS. 2(g) and (h).

[0057] Specifically, in this embodiment, Figure 3(a) to 3(c) is another schematic diagram of a method for preparing a self-aligned gate GaN HEMT device provided by an embodiment of the present invention, such as Figure 3(a) and 3(b) As shown, before preparing the gate electrode in the groove and on the upper surface of the silicon nitride dielectric layer in the first region and the silicon nitride dielectric layer in the second region of the device, the method further includes:

[0058] A silicon nitride film is deposited in the groove and on the upper surface of the silicon nitride dielectric layer, and then the silicon nitride film on the upper surface of the silicon nitride dielectric layer is etched away, and the silicon nitride film at the bottom of the groove is etched away, leaving the silicon nitride film on the side wall of the groove.

[0059] It should be noted that silicon nitride has good conformal coverage and can cover the steps of the gate electrode groove;

[0060] A silicon nitride film is formed on the sidewalls of the groove, which can reduce the gate length.

[0061] Further, etching away the silicon nitride film on the upper surface of the silicon nitride dielectric layer and etching away the silicon nitride film at the bottom of the groove, including:

[0062] The silicon nitride film on the upper surface of the silicon nitride dielectric layer and the silicon nitride film at the bottom of the groove are etched away using F-based plasma.

[0063] In this embodiment, the first region, the middle region, and the second region of the device are polished, including:

[0064] The first region, the middle region and the second region of the device are polished by chemical mechanical polishing.

[0065] S107, using the gate electrode as a mask, etching the silicon nitride dielectric layer in the first region and the silicon nitride dielectric layer in the second region of the device to expose the source electrode and the drain electrode, as shown in FIG2(i);

[0066] The middle region of the device is located between the first region and the second region.

[0067] Specifically, in this embodiment, the silicon nitride dielectric layer in the first region and the silicon nitride dielectric layer in the second region of the device are etched using the gate electrode as a mask, including:

[0068] The silicon nitride dielectric layer in the first region and the silicon nitride dielectric layer in the second region of the device are etched using F-based plasma to reduce parasitic capacitance and form gate electrode support at the same time.

[0069] In summary, the method for preparing a self-aligned gate GaN HEMT device provided by the present invention has the following beneficial effects:

[0070] 1. The selectivity of silicon nitride and silicon dioxide layers is different when wet-etched with a buffered oxide etchant. After the lateral width of silicon dioxide is reduced, a T-shaped structure is formed. During the growth of N+GaN, the silicon nitride layer shields the gate electrode area. The silicon nitride layer is subsequently removed during the planarization process to achieve selective growth of N+GaN, thereby overcoming the process complexity and difficulty of using wet etching to remove polycrystalline GaN on the mask surface.

[0071] 2. Use the gate electrode as a mask to etch the silicon nitride dielectric, exposing the source and drain electrodes while forming a support layer for the gate electrode, while reducing parasitic capacitance and avoiding the step of photolithography and etching holes. The formed gate electrode support is also conducive to improving the yield rate.

[0072] 3. Compatible with molecular beam epitaxy and metal organic chemical vapor deposition N+GaN processes; among them, molecular beam epitaxy is carried out in an ultra-high vacuum environment, the mean free path of molecules (atoms) is very large, and it is not easy to reach the inner side of the T-shaped structure; metal organic chemical vapor deposition is heteroepitaxial on silicon nitride and silicon dioxide, and it is not easy to attach to the T-shaped structure. Therefore, selective growth of N+GaN can be achieved using both processes.

[0073] In an optional embodiment of the present invention, see Figures 4(a) to 4(h) , Figures 4(a) to 4(h) is another schematic diagram of a method for preparing a self-aligned gate GaN HEMT device provided by an embodiment of the present invention. The GaN HEMT device is prepared by the following process, specifically:

[0074] Providing a wafer, the wafer comprising a substrate, a gallium nitride layer, a barrier layer and a silicon dioxide layer stacked in sequence;

[0075] The silicon dioxide layer, the barrier layer, and at least a portion of the gallium nitride layer in the first region and the second region of the device are etched away to form a first regrown region and a second regrown region, respectively; it should be noted that the first regrown region and the second regrown region are formed by etching the regrown region using silicon dioxide as a mask;

[0076] N+GaN is grown in the first region, the middle region and the second region of the device, a first N+GaN layer is formed in the first regrown region, a second N+GaN layer is formed in the second regrown region, and a polycrystalline GaN layer is formed on the silicon dioxide layer; a source electrode is prepared on the first N+GaN layer, and a drain electrode is prepared on the second N+GaN layer, as shown in FIG4(a);

[0077] A silicon nitride dielectric layer is deposited on the first region, the middle region and the second region of the device to cover the source electrode, the drain electrode and the polycrystalline GaN layer, and the first region, the middle region and the second region of the device are polished to flatten the upper surfaces of the first region, the middle region and the second region of the device and expose the silicon dioxide layer in the middle region of the device, as shown in FIGS. 4(b) and (c);

[0078] After the polycrystalline GaN is etched away by Cl-based plasma, BOE removes silicon dioxide to form a gate groove; a silicon nitride film is deposited to cover the groove, and the silicon nitride at the bottom is etched to form a sidewall to isolate the source and drain, and finally the gate is made, as shown in Figure 4 (d), (e), and (f);

[0079] Using the gate electrode as a mask, the silicon nitride dielectric layer in the first region and the silicon nitride dielectric layer in the second region of the device are etched to expose the source electrode and the drain electrode, as shown in FIG. 4( h ).

[0080] In an optional embodiment of the present invention, a GaN HEMT device is prepared by the following process, specifically:

[0081] The wafer material uses a silicon carbide substrate, the barrier layer is composed of aluminum nitride, and the barrier layer thickness is 3 to 5 nm;

[0082] Plasma-enhanced chemical vapor deposition was used to deposit 250nm of silicon dioxide and 50nm of silicon nitride on the wafer surface;

[0083] A negative photoresist is coated on the surface of the wafer, and a photoresist mask with a length of 200 nm is formed on the surface by photolithography and development;

[0084] Using F-based inductively coupled plasma etching, with carbon tetrafluoride and oxygen as etching gases, both sides of the photoresist mask are etched to form silicon nitride and silicon dioxide patterns with a height of 300 nm and a length of 200 nm;

[0085] Use a stripping solution to clean and remove the remaining photoresist mask;

[0086] The barrier layer and the gallium nitride layer are etched using Cl-based gas inductively coupled plasma, the etching gases are chlorine and boron trichloride, and the etching depth is about 50nm;

[0087] Use BOE to etch silicon dioxide, shrinking both sides of silicon dioxide by 60nm. At this time, the length of silicon oxide is 80nm and the length of silicon nitride is about 200nm.

[0088] Use metal organic chemical vapor deposition to deposit 80nm of N+GaN to make the N+GaN contact the two-dimensional electron gas channel under the barrier layer;

[0089] Photolithography of source and drain patterns on both sides of the middle area, evaporation of Ti and Au, stripping of metal, and production of source and drain electrodes;

[0090] 500nm silicon nitride was deposited using plasma enhanced chemical vapor deposition;

[0091] Use chemical mechanical polishing to flatten the wafer surface while exposing the silicon dioxide;

[0092] Use BOE to etch silicon dioxide to form a gate groove;

[0093] Photolithography of the gate pattern is performed above the gate groove, Ni and Au are evaporated, and the metal is stripped to produce the gate, which has a T-shaped structure, with the top length of 600nm and the bottom length of 80nm;

[0094] F-based inductively coupled plasma etching is used, and the etching gases are carbon tetrafluoride and oxygen to expose the source and drain electrodes.

[0095] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. Moreover, the term "include", "comprise" or any other variant is intended to cover non-exclusive inclusion, so that the article or device including a series of elements includes not only those elements, but also other elements that are not explicitly listed. In the absence of more restrictions, the elements defined by the sentence "including one..." do not exclude the existence of other identical elements in the article or device including the elements. "Connect" or "connected" and similar words are not limited to physical or mechanical connections, but can include electrical connections, whether direct or indirect. The orientation or position relationship indicated by "up", "down", "left", "right", etc. is based on the orientation or position relationship shown in the accompanying drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention.

[0096] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification.

[0097] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.

Claims

1. A method for preparing a self-aligned gate GaN HEMT device, characterized in that: include: A wafer is provided, wherein the wafer comprises a substrate, a gallium nitride layer, a barrier layer, a silicon dioxide layer and a silicon nitride layer which are stacked in sequence; The silicon nitride layer, the silicon dioxide layer, the barrier layer, and at least a portion of the gallium nitride layer in the first region and the second region of the device are etched away to form a first regrown region and a second regrown region, respectively; Using the silicon nitride layer in the middle region of the device as a mask, etching liquid is used to etch both sides of the silicon dioxide layer in the middle region of the device, so that the silicon nitride layer and the silicon dioxide layer in the middle region of the device form a T-shaped structure; Growing N+GaN in the first region, the middle region, and the second region of the device, forming a first N+GaN layer in the first regrown region, forming a second N+GaN layer in the second regrown region, and forming a polycrystalline GaN layer on the silicon nitride layer; preparing a source electrode on the first N+GaN layer, and preparing a drain electrode on the second N+GaN layer; Depositing a silicon nitride dielectric layer in the first region, the middle region, and the second region of the device to cover the source electrode, the drain electrode, and the polycrystalline GaN layer, and polishing the first region, the middle region, and the second region of the device to flatten the upper surfaces of the first region, the middle region, and the second region of the device, and exposing the silicon dioxide layer in the middle region of the device; The silicon dioxide layer in the middle area of ​​the device is etched away to form a groove, and a gate electrode is prepared in the groove and on the upper surface of the silicon nitride dielectric layer in the first area and the silicon nitride dielectric layer in the second area of ​​the device; Using the gate electrode as a mask, etching the silicon nitride dielectric layer in the first region and the silicon nitride dielectric layer in the second region of the device to expose the source electrode and the drain electrode; The middle region of the device is located between the first region and the second region.

2. The method for preparing a self-aligned gate GaN HEMT device according to claim 1, characterized in that: The step of etching the silicon nitride layer, the silicon dioxide layer, the barrier layer, and at least a portion of the gallium nitride layer in the first region and the second region of the device to form a first regrown region and a second regrown region, respectively, comprises: Coating a layer of photoresist on the upper surface of the silicon nitride layer, and etching the photoresist, the silicon dioxide layer and the silicon nitride layer in the first region and the second region of the device using F-based plasma; The photoresist in the middle area of ​​the device is removed by using a degumming solvent, the silicon dioxide layer and the silicon nitride layer in the middle area of ​​the device are used as masks, the barrier layer and at least a portion of the gallium nitride layer in the first area of ​​the device are etched by using Cl-based plasma to form a first re-growth area, and the barrier layer and at least a portion of the gallium nitride layer in the second area of ​​the device are etched by using Cl-based plasma to form a second re-growth area.

3. The method for preparing a self-aligned gate GaN HEMT device according to claim 1, characterized in that: Before preparing the gate electrode in the groove and on the upper surface of the silicon nitride dielectric layer in the first region and the second region of the device, the method further includes: A layer of silicon nitride film is deposited in the groove and on the upper surface of the silicon nitride dielectric layer, and then the silicon nitride film on the upper surface of the silicon nitride dielectric layer is etched away, and the silicon nitride film at the bottom of the groove is etched away, leaving the silicon nitride film on the side wall of the groove.

4. The method for preparing a self-aligned gate GaN HEMT device according to claim 3, characterized in that: The etching of the silicon nitride film on the upper surface of the silicon nitride dielectric layer and the etching of the silicon nitride film at the bottom of the groove include: The silicon nitride film on the upper surface of the silicon nitride dielectric layer is etched away using F-based plasma, and the silicon nitride film at the bottom of the groove is etched away.

5. The method for preparing a self-aligned gate GaN HEMT device according to claim 1, characterized in that: The etching solution is a buffered oxide etching solution.

6. The method for preparing a self-aligned gate GaN HEMT device according to claim 1, characterized in that: The method of growing N+GaN in the first region, the middle region and the second region of the device comprises: Using molecular beam epitaxy, N+GaN is grown in the first region, the middle region and the second region of the device.

7. The method for preparing a self-aligned gate GaN HEMT device according to claim 1, characterized in that: A silicon nitride dielectric layer is deposited in the first region, the middle region and the second region of the device, and the silicon nitride dielectric layer at least covers two sides of the silicon dioxide layer.

8. The method for preparing a self-aligned gate GaN HEMT device according to claim 1, characterized in that: The polishing of the first region, the middle region and the second region of the device comprises: The first region, the middle region and the second region of the device are polished by chemical mechanical polishing.

9. The method for preparing a self-aligned gate GaN HEMT device according to claim 1, characterized in that: The method of using the gate electrode as a mask to etch the silicon nitride dielectric layer in the first region and the silicon nitride dielectric layer in the second region of the device comprises: The silicon nitride dielectric layer in the first region and the silicon nitride dielectric layer in the second region of the device are etched using F-based plasma.

Citation Information

Patent Citations

  • GaN HEMT device based on self-aligning process and manufacture method thereof

    CN107170809A

  • Method for producing grooved gate enhanced HEMT device based on CMP etching technology

    CN114068329A

  • Structure and process method for improving grid etching damage of GaN heterojunction device

    CN117198878A

  • Inverted T-shaped composite gate dielectric structure gallium nitride HEMT device and preparation method thereof

    CN118173595A

  • High-electron-mobility transistor structure as well as fabricating method and use thereof

    US20240186405A1

Cited By

  • Full-self-alignment method for gate source, gate drain and short gate length and application of full-self-alignment method

    CN119767717A