Silicon nitride powder precursor, silicon nitride powder and preparation method thereof
Through the inclined rotary fluidized bed technology and spray granulation process, the nitriding reaction conditions are optimized, and the problems of α-phase ratio and impurity content in silicon nitride powder are solved, and the continuous batching of high-purity and ultra-fine Si3N4 powder is achieved. Preparation improves the mechanical and thermal properties of the material.
Patent Information
- Application Number
- CN202410936523.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-07-12
AI Technical Summary
The prior art is difficult to increase the proportion of α phase in silicon nitride powder and reduce the impurity content, especially when preparing high-purity, ultra-fine Si3N4 powder, there is a problem of residual silicon and β phase generation.
Using inclined rotary fluidized bed technology, high-purity silicon powder and diluent silicon nitride powder are prepared by controlling the N2 flow rate, the rotation angle, the rotation rate and the temperature interval of the reaction chamber, combined with spray granulation and ball mill mixing technology, to form fluidity Good granulation powder is used and nitriding reaction is carried out in the fluidized bed to control the addition rate and temperature interval of the granulation powder, and optimize the nitriding reaction conditions.
The α-phase ratio in Si3N4 powder is improved, the impurity content is stable, and the production of high-purity and ultra-fine continuous batch preparation is achieved, which reduces the generation of residual silicon and β-phase, and improves the mechanical and thermal properties of the powder.
Smart Images

Figure CN119039007A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of ceramic powder preparation, in particular to a silicon nitride powder precursor, silicon nitride powder and a preparation method thereof. Background Art
[0002] IGBT modules have been widely used in the automotive industry, high-speed rail, smart grid and new energy fields due to their advantages such as low driving power, low saturation voltage drop and high current density. As traditional Si-based semiconductors are gradually replaced by wide-bandgap third-generation semiconductors (such as SiC and GaN), power electronic devices are rapidly developing in the direction of high voltage, high current, small size and high output power. High power density places higher requirements on the packaging materials of power modules. The ceramic substrate is located between the circuit equipped with semiconductor chips and the heat sink (metal), playing the role of insulation, heat dissipation and support protection. Commonly used ceramic substrate materials are mainly aluminum oxide (Al2O3), aluminum nitride (AlN) and silicon nitride (Si3N4). Among them, Si3N4 is recognized as the ceramic substrate material with the best comprehensive performance such as high thermal conductivity, high mechanics and high reliability, which makes it the first choice for high thermal conductivity substrate materials for high-power semiconductor devices.
[0003] High-quality Si3N4 powder is a prerequisite for the preparation of high-performance Si3N4 ceramic substrates. Its purity, phase composition (mainly including α and β phases), particle size, oxygen content and other impurity content have an important influence on the thermal conductivity of the prepared ceramic substrate and the subsequent sintering molding process. Usually, high-quality Si3N4 powder needs to meet the conditions of fine particle size, narrow distribution, high α phase content and low impurity content. At present, the main methods for preparing Si3N4 powder are: SiO2 carbon thermal nitridation, Si powder direct nitridation, chemical vapor synthesis, high-temperature thermal decomposition of silane precursor, combustion synthesis (high-temperature self-propagating), etc. [Xiang Maoqiao, Geng Yuqi, Zhu Qingshan. Research progress on preparation technology of silicon nitride powder and powder quality [J]. Journal of Chemical Industry, 2022, 73(1): 73-84].
[0004] 1.SiO2 carbon thermal nitriding method
[0005] The reaction principle of preparing Si3N4 powder by SiO2 carbon thermal nitridation is to activate the reducing property of C powder above 1400℃, reduce SiO2 powder and nitride it to Si3N4. The advantage of this method for preparing Si3N4 powder is that it is low cost, but it is difficult to synthesize high-quality Si3N4 powder with low oxygen content. The common difficulty is that it is difficult for Si-O bonds to be completely replaced by Si-N bonds in solid-phase reactions. To address this problem, the reaction path of the carbon thermal nitridation method can be further optimized, the nitridation path of gas-phase SiO2 can be separated, and a gas-phase carbon source can be used to first convert it into Si(g), and then nitrided into Si3N4, which is expected to reduce or eliminate lattice O impurities.
[0006] 2. Si powder direct nitridation method
[0007] Si powder direct nitridation method, that is, Si powder reacts with N2 to generate Si3N4 powder. The path for synthesizing Si3N4 by this reaction is relatively simple, and does not involve side reactions that generate impurities. This method is highly efficient and relatively low in cost, but it is difficult to synthesize Si3N4 powder with a high α-phase content and no free Si. The difficulty lies in strengthening solid-phase mass transfer and precisely controlling heat. Table 1 lists the main domestic and foreign companies with 100-ton production lines and the quality indicators of their respective optimal powders. It can be seen that although the α-phase content of the powders prepared by each company is relatively high, it is less than 95%, and still contains trace amounts of free Si, which makes it difficult to use them to prepare high thermal conductivity and high-strength ceramic substrates.
[0008] Table 1 Powder quality of Si3N4 produced by direct nitridation of Si powder at home and abroad
[0009]
[0010] Chinese patent CN202211087843.0 [Method for preparing high-purity Si3N4 powder by two-stage nitriding process assisted by high-energy ultrasonic pickling] uses silicon powder as raw material, and performs Si powder nitriding by a two-stage heating system. By adding halides and metal catalysts, low-energy consumption can be achieved to prepare uniform and stable Si3N4 powder. At the same time, the auxiliary ultrasonic pickling process improves the micromorphology of the powder to make the powder surface smooth, reduces free silicon, silicon oxynitride and metal impurities in the powder, and completes the stable preparation of high-purity Si3N4 powder. The invention uses a two-stage heating measure, and with the help of the halide molten salt environment, the uniform adsorption of nitrogen makes the silicon powder grow with equal probability in all directions, and finally prepares high-quality Si3N4 powder with an α-phase of 93% and a free silicon content of 0.5%. Since the patent includes a two-stage nitriding process stage and subsequent high-energy ultrasonic pickling, not only is the process more complicated, but the work section is also discontinuous.
[0011] Chinese patent application 202010673734.1 [A method for preparing silicon nitride powder] uses the difference in thermal expansion coefficients between Si and Si3N4 to prepare silicon nitride powder at 3°C min in a vacuum or inert atmosphere. -1The above heating rate rapidly heats up to more than 50°C and then cools down, so that the Si3N4 layer on the surface of the silicon powder is broken, thereby increasing the nitridation reaction rate and shortening the nitridation cycle; the entire preparation process of this invention will only be introduced with nitrogen or nitrogen-hydrogen mixed gas below 1350°C, and the silicon powder nitridation reaction will occur, which can prevent the formation of β-Si3N4, and is more conducive to the formation of α-Si3N4, and the obtained α-Si3N4 content is 93%-94%. This patent is based on the rapid heating of the heating equipment to achieve the surface of silicon nitride, and the particles with silicon inside have a significant temperature difference between the inside and the surface, causing the surface silicon nitride to "break", exposing the unreacted silicon inside to continue to react with nitrogen, thereby increasing the nitridation reaction rate, shortening the nitridation cycle, and reducing the residual silicon in the product, but it is limited to the uniform temperature zone of the equipment. This "breaking" phenomenon only occurs at a certain stage of the reaction or a certain area of the equipment.
[0012] Chinese patent 200510126334.4 [A method for continuously synthesizing silicon nitride powder at normal pressure using fluidized bed technology] belongs to the technical field of preparation of ultrafine silicon nitride powder. Using high-purity nitrogen as carrier gas at room temperature, silicon powder or a mixture of silicon powder and silicon nitride is rapidly fluidized and entrained away from the fast fluidized bed, and the gas-solid two-phase flow composed of powder and nitrogen enters the high temperature zone of the high temperature nitriding furnace, and continuously passes through the high temperature nitriding furnace in a dilute phase pneumatic conveying manner, so that a combustion synthesis reaction occurs at high temperature and normal pressure, and finally after cooling at the outlet using a heat exchanger, it is collected by a bag collector to obtain silicon nitride powder. The synthetic product is silicon nitride powder, and the main crystal phase can be amorphous, α phase, β phase or a mixture thereof.
[0013] 3 Chemical vapor synthesis
[0014] The principle of this method is to use a gas phase silicon source, such as SiCl4, SiH4, SiHCl3, SiBr4, etc., to react with NH3 or N2 and H2 to directly generate Si3N4 powder. Due to the high temperature of the plasma torch and the very large temperature gradient, the resulting powder is mainly β-phase Si3N4. In addition, the cost of plasma equipment is high and the production capacity is small. It is commonly used in laboratory research, and there has been no report on the industrial preparation of Si3N4 powder.
[0015] 4. High temperature thermal decomposition of silanamine precursor
[0016] The principle of the high-temperature thermal decomposition method of silicamine precursor is that SiCl4 and NH3 are first synthesized at low temperature (-80~100℃) to form silicamine precursor Si(NH2)4 or Si(NH)2, and then the silicamine precursor is crystallized at 1400~1600℃ to synthesize Si3N4 powder. This method can synthesize high-quality Si3N4 powder, but the cost is high. The difficulty lies in the precise control of the precursor synthesis reaction, the control of the hygroscopic protection cost in the preparation process and the continuous production.
[0017] 5 High temperature self-propagating method
[0018] Chinese patent CN201910700710.8 [A method for preparing α-phase silicon nitride ceramic powder] adopts a two-step reaction method, combining the traditional silicon powder direct nitridation method with the self-propagating process. The first step of the reaction controls the reaction speed by controlling the nitrogen introduction rate to prevent excessive reaction, local overheating, and the generation of silicon flow; the second step of the reaction is to introduce nitrogen at a relatively low temperature to promote the rapid combustion and reaction of the silicon powder that has not reacted completely in the first step. The mass content of the α phase in the generated Si3N4 ceramic powder is ≥96%, and the reaction time is short, the energy consumption is low, the production cost is saved, the output is large, and the output of a single furnace reaches 60-200kg. This patent has a complex process (two steps). Summary of the invention
[0019] The technical problem to be solved by the present invention is to provide a silicon nitride powder precursor, silicon nitride powder and a preparation method thereof, in view of the deficiencies in the prior art, so as to increase the proportion of α phase in the prepared silicon nitride powder and reduce the impurity content.
[0020] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0021] A method for preparing a silicon nitride powder precursor comprises the following steps:
[0022] S1, mixing Si powder, silicon nitride powder, triethyl phosphate, polyvinyl butyral and ethanol to obtain a precursor slurry;
[0023] S2. Spray granulate the precursor slurry to obtain a precursor.
[0024] A method for preparing silicon nitride powder comprises the following steps:
[0025] The prepared precursor is added into an inclined rotating fluidized bed reaction chamber, N2 is introduced into the rotating reaction chamber and the granulated powder is heated to obtain Si3N4 powder;
[0026] The flow rate of N2 is 0.010-0.019 g·s -1 ;
[0027] The inclination angle of the reaction chamber is 4-7°;
[0028] The rotation rate of the reaction chamber is 10 -19 r·min -1 ;
[0029] The temperature of the nitridation reaction is 1200-1500° C., and the time is 0.5-6 hours.
[0030] Preferably, the flow rate of N2 in the reaction chamber is 0.010-0.015 g·s -1 ;
[0031] The inclination angle of the fluidized bed reaction chamber is 4-6°;
[0032] The rotation rate of the fluidized bed reaction chamber is 10-15 r·min -1 .
[0033] S3 continuously adds granulated powder into the reaction chamber, and controls the continuous and high-stability preparation of Si3N4 powder by controlling the N2 flow rate, the reaction chamber rotation angle, the reaction chamber rotation rate and the reaction temperature, thereby increasing the proportion of α phase in the prepared silicon nitride powder.
[0034] Si powder is high-purity silicon powder, silicon nitride powder acts as diluent powder, triethyl phosphate acts as dispersant, and polyvinyl butyral acts as binder. Granulated powder with good fluidity is obtained by spray granulation.
[0035] In a preferred embodiment of the present invention, in S3, the temperature of the nitridation reaction is set to five temperatures, namely, the first temperature zone: 250-400°C, the second temperature zone: 700-850°C, the third temperature zone: 1100-1300°C, the fourth temperature zone: 1400-1500°C, and the fifth temperature zone: 1200-1300°C.
[0036] Preferably, the temperature of the nitridation reaction is: first temperature zone: 300-350°C, second temperature zone: 750-800°C, third temperature zone: 1200-1250°C, fourth temperature zone: 1400-1450°C, fifth temperature zone: 1200-1300°C.
[0037] This temperature range can significantly increase the proportion of α phase in the silicon nitride powder. The temperature in the fourth temperature zone is lower than 1400°C, which will lead to a decrease in the proportion of α phase in the silicon nitride powder and an increase in Si (residual). Because no matter how the temperature difference is used to break up the particles with an outer silicon nitride layer and an inner silicon structure, there is always a problem of reaction speed. Only when the temperature reaches the temperature in the fourth temperature range can the diffusion of nitrogen in the silicon nitride layer be increased to react with the silicon inside the particles, thereby promoting the complete conversion of silicon. The setting of the fifth temperature is also based on the difference in thermal expansion coefficients of silicon and silicon nitride after the temperature is lowered, which further breaks up the particles and uses high-purity nitrogen to react with the residual trace silicon, further increasing the yield and reducing residual silicon.
[0038] In a preferred embodiment of the present invention, in S3, the addition rate of the granulating powder is 10-80 g·min -1 .
[0039] Preferably, in S3, the granulation powder is added at a rate of 10-40 g·min -1Further preferably, in S3, the addition rate of the granulating powder is 10 -25g·min -1 .
[0040] S3 continuously adds granulation powder into the reaction chamber to further control the powder flow rate and the continuous and highly stable preparation of Si3N4 powder. By controlling the addition rate of granulation powder, the proportion of α phase in the prepared Si3N4 powder and the stability of impurity content are improved.
[0041] In a preferred embodiment of the present invention, the average particle size of the granulated powder, the diameter of the fluidized bed reaction chamber and the N2 flow rate have the following relationship:
[0042]
[0043] Where p1 is the atmospheric pressure in Pa, p2 is the pressure in the reaction chamber in Pa, and v1 is the N2 flow rate in g·s -1 , v2 is the powder flow rate in the reaction chamber, unit is g·s -1 , d1 is the diameter of the reaction chamber, in mm, d2 is the average particle size of the precursor granulation powder, in mm, and k is a constant ranging from 0.06 to 0.1.
[0044] In a preferred embodiment of the present invention, the N2 pressure in the reaction chamber is 1.1×10 5 -1.5×10 5 Pa;
[0045] The granulation powder flow rate in the reaction chamber is 0.2-1.0 g·s -1 ;
[0046] The reaction chamber has a diameter of 40-400 mm;
[0047] The average particle size of the granulated powder is 0.05-0.2 mm.
[0048] In a preferred embodiment of the present invention, the particle size of the Si powder is ≤5 μm and the purity is ≥99.99 wt %;
[0049] The silicon nitride powder has an average particle size of 500-900 nm and a purity of ≥99.99 wt %;
[0050] The purity of the triethyl phosphate is ≥99.5wt%;
[0051] The molecular weight of the polyvinyl butyral is 40,000-70,000 M.W., and the purity is ≥99.5wt%;
[0052] In a preferred embodiment of the present invention, in S1, by mass, 100 parts of Si powder, 10-60 parts of silicon nitride powder, 0.2-1.5 parts of triethyl phosphate, 0.2-10 parts of polyvinyl butyral, and 50-300 parts of ethanol are taken and ball-milled and mixed.
[0053] In a preferred embodiment of the present invention, ball milling is used in S1, and the ball milling rate of the ball milling is 20-60 r·min -1 , the time is 12-48h. When the ball milling time is less than 12h, shortening the ball milling time will lead to uneven mixing of the powder, uneven particle size and composition of the obtained granulated powder, and poor fluidity, which will lead to increased silicon content in the product and increased silicon nitride powder particle size. Prolonging the ball milling time will extend the production cycle and increase energy consumption.
[0054] The invention also discloses silicon nitride powder obtained by the preparation method.
[0055] The present invention also discloses a silicon nitride powder, wherein the α phase ratio in the silicon nitride powder is ≥96%, the residual silicon is 0.2-0.4wt%, and the D50 is 110-120nm;
[0056] Preferably, the impurity content is 0.19-0.45wt%;
[0057] Further preferably, the impurities include O, Fe, Al, and Ca;
[0058] The O content is 0.1-0.3wt%, the Fe content is 0.004-0.006wt%, the Al content is 0.001-0.003wt%, and the Ca content is 0.004-0.006wt%. When the purity is constant, the higher the proportion of the α phase in the powder, the more conducive it is to obtain a high-density silicon nitride ceramic green body or substrate green body, and then after sintering, it is conducive to obtaining a high-density silicon nitride ceramic or substrate material with excellent mechanical and thermal properties, because most of the α phase exists in the form of particles or sheets, which is conducive to the dense packing of the green body, while the β phase mainly exists in the form of columns and fibers. If the β phase content in the powder is high, due to the overlap of the columns or fibers, the green body density of the silicon nitride ceramic green body or substrate is low, which ultimately leads to a decrease in the mechanical and thermal properties of the sintered material.
[0059] Compared with the Chinese patent with application number 202211087843.0, this application is based on the inclined rotating fluidized bed and continuous feeding to achieve batch preparation of silicon nitride powder with stable composition, high purity and fine powder, etc., which is significantly different; at the same time, the preparation process of the Chinese patent with application number 202211087843.0 introduces halides and metal catalysts, which is not introduced in the preparation process of this application, resulting in certain advantages in product purity. As for the ability of this application to achieve continuous and highly stable preparation of silicon nitride powder, the Chinese patent with application number 202211087843.0 does not have it.
[0060] Compared with the Chinese patent application No. 202010673734.1, the present application utilizes the unique feeding and air intake method of the fluidized bed to achieve continuous contact between the lower temperature nitrogen and the higher temperature material during the entire reaction process. Since the nitridation reaction of silicon powder always starts from the surface of the powder, there is a difference between the surface layer (mainly Si3N4) and the internal composition (mainly Si) of the powder. By utilizing Si (about 2.5×10 -6 ℃ -1 ) and Si3N4 (about 3.2×10 -6 ℃ -1 ) The difference in thermal expansion coefficients causes the Si3N4 layer that has been formed on the surface of the silicon powder to "continue to break", exposing the unreacted silicon inside to continue to react with nitrogen, thereby greatly increasing the nitridation reaction rate and completely solving the problem of Si residue in the product. This is one of the main reasons why the present application is easy to obtain high-purity silicon nitride powder; at the same time, because the powder is always "broken" during the reaction process, this is why the present application is easy to obtain ultrafine powder. As for the ability of the present application to achieve continuous and highly stable preparation of silicon nitride powder, the comparative patent does not have it.
[0061] Compared with the Chinese patent with application number 200510126334.4, this application has the following differences: 1. The powder-airflow input method is different. The hot material and cold airflow proposed in this patent are input from both ends of the reaction chamber respectively; 2. The state of the reaction chamber is different. In this patent, the reaction chamber is always rotating during the material preparation process. These two differences are exactly the innovation points of this patent. The impact of the first difference on high-purity ultrafine silicon nitride powder can be seen in the description of Chinese patent application 202010673734.1; As for the second advantage, it is explained as follows: During the reaction process, the continuous flipping of the granulated powder in the reaction chamber is achieved through the rotation of the fluidized bed, and the effective release of the heat generated during the Si powder nitridation reaction process is achieved, thereby solving the problem of the difficulty of complete nitridation caused by the agglomeration and melting of silicon powder due to the excessive local temperature in the static bed, and the high residual Si content in the product. It can also effectively solve the problem of the product Si3N4 being easy to agglomerate and large particles, which is exactly what the comparative patent cannot solve.
[0062] In summary, compared with Chinese patents CN202211087843.0, 202010673734.1, and 200510126334.4, the core technical difference of this application lies in that the traditional static method is to improve the silicon conversion rate (because the raw silicon is accumulated, the reaction process starts from the surface and it takes a certain time to reach the bottom). For this reason, it is often necessary to extend the insulation time or add a catalyst to speed up the reaction progress, but the reaction temperature cannot generally be increased. On the one hand, if the temperature is too high, it is easy to cause the formation of β phase (high temperature stable phase). At the same time, silicon is easy to melt, resulting in an increase in the product particle size, and it is also easy to cause silicon residue.
[0063] Compared with the prior art, the present invention has the following beneficial effects:
[0064] 1. By controlling the addition rate of granulation powder, reaction temperature, rotation rate of fluidized bed reaction chamber and high-purity N2 flow rate, the target powder can be prepared in batches continuously; at the same time, the proportion of α phase in the prepared Si3N4 powder can be increased, and the impurity content can be stabilized;
[0065] 2 During the reaction, the rotation of the fluidized bed and the control of the N2 gas flow rate can realize the continuous turning of the granulated powder in the reaction chamber, and effectively release the heat generated in the Si powder nitridation reaction process, thereby solving the problem of difficulty in complete nitridation and high residual Si content in the product caused by the agglomeration and melting of silicon powder due to excessive local temperature in the static bed, which can also effectively solve the problem of large particles of Si3N4 in the product due to easy agglomeration;
[0066] 3 By controlling the inclination angle of the fluidized bed reaction chamber and the N2 gas flow rate, the residence time of the reaction materials in the reaction chamber is effectively controlled to improve the conversion rate of Si powder; in the same way, the greater the inclination of the pipeline, the faster the powder falls in the reaction chamber, which is equivalent to increasing the amount of powder added in disguise, and the thermal shock effect when nitrogen meets the powder, which is also conducive to the reduction of residual silicon and the formation of β phase. The design based on the nitrogen amount is sufficient, so in comparative example 2, the residual silicon is low, and the β phase content is higher,
[0067] 4. By adjusting the ratio of diluent to Si powder, the speed of the reaction chamber, and the type and amount of catalyst, the ratio of α and β phases in the product can be effectively controlled;
[0068] 5 Through the unique feeding and air intake method of the fluidized bed, the contact between cold N2 and hot materials is achieved, and the difference in thermal expansion coefficients between Si and Si3N4 is used to break the Si3N4 layer on the surface of silicon powder, thereby increasing the nitridation reaction rate, shortening the nitridation cycle, improving the utilization rate of Si powder, and reducing the residual Si content in the product
[0069] The present invention can realize continuous batch preparation of high-purity, ultrafine Si3N4 powder, and is easy to expand the production scale, and the powder composition is stable; the process has the advantages of simple equipment, fewer processes, simple operation, low cost, etc.
[0070] Calculated on the basis of a reaction chamber diameter of 200 mm, when a single tube continuously runs for 24 hours, the output of high-purity ultrafine powder can reach 15-40 kg, and once the system starts to run stably, it is only necessary to ensure that the process parameters such as the reaction chamber rotation speed, nitrogen flow rate, and temperature in different temperature zones are stable, and the target powder can be continuously obtained; at the same time, the present invention can further increase the output of high-purity, ultrafine Si3N4 powder by connecting multiple groups of reaction chambers in parallel. BRIEF DESCRIPTION OF THE DRAWINGS
[0071] Figure 1 This is a process technology roadmap for preparing high-purity Si3N4 powder in Example 1 of the present invention.
[0072] Figure 2 This is a morphology photograph of the granulated powder of Example 1 of the present invention.
[0073] Figure 3 The XRD patterns of Si3N4 powders prepared in the examples and comparative examples of the present invention are shown in FIG.
[0074] Figure 4 These are SEM photos of Si3N4 powders prepared in the examples and comparative examples of the present invention.
[0075] Figure 4 In the examples, (a) Example 1; (b) Comparative Example 1; (c) Comparative Example 2; (d) Comparative Example 3; (e) Comparative Example 4; (f) Comparative Example 5; (g) Comparative Example 6.
[0076] Table 2 is the composition analysis of Si3N4 powder prepared in the examples and comparative examples of the present invention.
[0077] Figure 2 This indicates that the prepared precursor has good sphericity;
[0078] Figure 3 The XRD patterns of the powders obtained under different process conditions show that the powders are composed of a composite phase of α and β-Si3N4, with some residual silicon.
[0079] Figure 4 The SEM images of powders obtained under different process conditions show that the granules and flakes are mainly α phase, while the rods / columns and needles are mainly β phase. DETAILED DESCRIPTION
[0080] Example 1
[0081] Precursor slurry preparation process: In a 10L polyurethane ball mill, add 1000 parts of raw material Si powder, 400 parts of diluent Si3N4 powder, 2.0 parts of dispersant triethyl phosphate, 5.0 parts of binder polyvinyl butyral, 3000 parts of high-purity Si3N4 grinding balls with a diameter of about 2mm, and then add 2000 parts of ethanol for ball milling. The ball mill speed is 40r min -1 , ball milling time is 48h;
[0082] Precursor granulation process: The uniformly ground slurry is injected into the spray granulation tower through a diaphragm pump to prepare a precursor granulation powder with high sphericity and excellent fluidity. The injection pressure of the diaphragm pump is 0.75MPa, the inlet temperature in the granulation tower is 250℃, and the outlet temperature is 90℃.
[0083] The morphology of the granulated powder obtained is as follows Figure 2 As shown in the figure, it is spherical, complete in shape, has good fluidity, and an average particle size of about 150 μm.
[0084] Precursor granulation powder nitridation process: First, adjust the inclination angle of the fluidized bed reaction chamber to 4°, turn on the rotating device, adjust the reaction chamber speed to 10 rpm, then evacuate the reaction chamber to 15 Pa, maintain the pressure for 30 minutes, observe the air tightness of the reaction chamber, and after the air tightness is confirmed, slowly fill it with high-purity N2 until the pressure in the reaction chamber is slightly higher than the atmospheric pressure, open the outlet valve, and adjust the nitrogen flow value to 0.010 g·s -1 Then, the temperature of the reaction chamber is set in different zones, as follows: first temperature zone: 300-350°C, second temperature zone: 750-800°C, third temperature zone: 1200-1250°C, fourth temperature zone: 1400-1450°C (high temperature zone), fifth temperature zone: 1200°C. After the temperature of each temperature zone is stable, feed the material through the automatic feeder, and control the feed rate to 15g·min -1 , so that the precursor powder stays in the high temperature zone for 120 minutes, and the outlet powder temperature is close to room temperature.
[0085] The obtained Si3N4 powder is then ball-milled and vacuum-packed to obtain the product. The XRD pattern of the obtained powder is shown in Figure 3 , appearance see Figure 4 , component analysis and particle size test results are shown in Table 2.
[0086] Comparative Example 1 (different nitrogen flow rate value from Example 1)
[0087] Precursor slurry preparation process: In a 10L polyurethane ball mill, add 1000 parts of raw material Si powder, 400 parts of diluent Si3N4 powder, 2.0 parts of dispersant triethyl phosphate, 5.0 parts of binder polyvinyl butyral, 3000 parts of high-purity Si3N4 grinding balls with a diameter of about 2mm, and then add 2000 parts of ethanol for ball milling. The ball mill speed is 40r min -1 , ball milling time is 48h;
[0088] Precursor granulation process: The uniformly ground slurry is injected into the spray granulation tower through a diaphragm pump to prepare a precursor granulation powder with high sphericity and excellent fluidity. The injection pressure of the diaphragm pump is 0.75MPa, the inlet temperature in the granulation tower is 250℃, and the outlet temperature is 90℃.
[0089] The obtained granulated powder is spherical, has a complete shape, good fluidity, and an average particle size of about 150 μm.
[0090] Precursor granulation powder nitridation process: First, adjust the inclination angle of the fluidized bed reaction chamber to 4°, turn on the rotating device, adjust the reaction chamber speed to 10 rpm, then evacuate the reaction chamber to 15Pa, maintain the pressure for 30 minutes, observe the air tightness of the reaction chamber, and after the air tightness is confirmed, slowly fill it with high-purity N2 until the pressure in the reaction chamber is slightly higher than the atmospheric pressure, open the outlet valve, and adjust the nitrogen flow value to 0.020g·s -1 Then, the temperature of the reaction chamber is set by zones, as follows: first temperature zone: 300-350°C, second temperature zone: 750-800°C, third temperature zone: 1200-1250°C, fourth temperature zone: 1400-1450°C (high temperature zone); fifth temperature zone: 1200°C. After the temperatures of each temperature zone are stable, feed the material through the automatic feeder, and control the feed rate to 15g·min -1 , so that the precursor powder stays in the high temperature zone for 120 minutes, and the outlet powder temperature is close to room temperature.
[0091] The obtained Si3N4 powder is then ball-milled and vacuum-packed to obtain the product. The XRD pattern of the obtained powder is shown in Figure 3 , appearance see Figure 4 , component analysis and particle size test results are shown in Table 2.
[0092] Comparative Example 2 (different inclination angle of the fluidized bed reaction chamber from that in Example 1)
[0093] Precursor slurry preparation process: In a 10L polyurethane ball mill, add 1000 parts of raw material Si powder, 400 parts of diluent Si3N4 powder, 2.0 parts of dispersant triethyl phosphate, 5.0 parts of binder polyvinyl butyral, 3000 parts of high-purity Si3N4 grinding balls with a diameter of about 2mm, and then add 2000 parts of ethanol for ball milling. The ball mill speed is 40r min -1 , ball milling time is 48h;
[0094] Precursor granulation process: The uniformly ground slurry is injected into the spray granulation tower through a diaphragm pump to prepare a precursor granulation powder with high sphericity and excellent fluidity. The injection pressure of the diaphragm pump is 0.75MPa, the inlet temperature in the granulation tower is 250℃, and the outlet temperature is 90℃.
[0095] The morphology of the granulated powder obtained is as follows Figure 2 As shown in the figure, it is spherical, complete in shape, has good fluidity, and an average particle size of about 150 μm.
[0096] Precursor granulation powder nitridation process: First, adjust the inclination angle of the fluidized bed reaction chamber to 8°, turn on the rotating device, adjust the reaction chamber speed to 10 rpm, then evacuate the reaction chamber to 15Pa, maintain the pressure for 30 minutes, observe the air tightness of the reaction chamber, and after the air tightness is confirmed, slowly fill it with high-purity N2 until the pressure in the reaction chamber is slightly higher than the atmospheric pressure, open the outlet valve, and adjust the nitrogen flow value to 0.010g·s -1 Then, the temperature of the reaction chamber is set by zones, as follows: first temperature zone: 300-350°C, second temperature zone: 750-800°C, third temperature zone: 1200-1250°C, fourth temperature zone: 1400-1450°C (high temperature zone); fifth temperature zone: 1200°C. After the temperatures of each temperature zone are stable, feed the material through the automatic feeder, and control the feed rate to 15g·min -1 , so that the precursor powder stays in the high temperature zone for 120 minutes, and the outlet powder temperature is close to room temperature.
[0097] The obtained Si3N4 powder is then ball-milled and vacuum-packed to obtain the product. The XRD pattern of the obtained powder is shown in Figure 3 , appearance see Figure 4 The component analysis results are shown in Table 2.
[0098] Comparative Example 3 (different reaction chamber speed from that in Example 1)
[0099] Precursor slurry preparation process: In a 10L polyurethane ball mill, add 1000 parts of raw material Si powder, 400 parts of diluent Si3N4 powder, 2.0 parts of dispersant triethyl phosphate, 5.0 parts of binder polyvinyl butyral, 3000 parts of high-purity Si3N4 grinding balls with a diameter of about 2mm, and then add 2000 parts of ethanol for ball milling. The ball mill speed is 40r min -1 , ball milling time is 48h;
[0100] Precursor granulation process: The uniformly ground slurry is injected into the spray granulation tower through a diaphragm pump to prepare a precursor granulation powder with high sphericity and excellent fluidity. The injection pressure of the diaphragm pump is 0.75MPa, the inlet temperature in the granulation tower is 250℃, and the outlet temperature is 90℃.
[0101] The morphology of the granulated powder obtained is as follows Figure 2 As shown in the figure, it is spherical, complete in shape, has good fluidity, and an average particle size of about 150 μm.
[0102] Precursor granulation powder nitridation process: First, adjust the inclination angle of the fluidized bed reaction chamber to 4°, turn on the rotating device, adjust the reaction chamber speed to 20 rpm, then evacuate the reaction chamber to 15 Pa, maintain the pressure for 30 minutes, observe the air tightness of the reaction chamber, and after the air tightness is confirmed, slowly fill it with high-purity N2 until the pressure in the reaction chamber is slightly higher than the atmospheric pressure, open the outlet valve, and adjust the nitrogen flow value to 0.010 g·s -1 Then, the temperature of the reaction chamber is set by zones, as follows: first temperature zone: 300-350°C, second temperature zone: 750-800°C, third temperature zone: 1200-1250°C, fourth temperature zone: 1400-1450°C (high temperature zone); fifth temperature zone: 1200°C. After the temperatures of each temperature zone are stable, feed the material through the automatic feeder, and control the feed rate to 15g·min -1 , so that the precursor powder stays in the high temperature zone for 120 minutes, and the outlet powder temperature is close to room temperature.
[0103] The obtained Si3N4 powder is then ball-milled and vacuum-packed to obtain the product. The XRD pattern of the obtained powder is shown in Figure 3 , appearance see Figure 4 , component analysis and particle size test results are shown in Table 2.
[0104] Comparative Example 4 (different temperatures from the fourth and fifth temperature zones in Example 1)
[0105] Precursor slurry preparation process: In a 10L polyurethane ball mill, add 1000 parts of raw material Si powder, 400 parts of diluent Si3N4 powder, 2.0 parts of dispersant triethyl phosphate, 5.0 parts of binder polyvinyl butyral, 3000 parts of high-purity Si3N4 grinding balls with a diameter of about 2mm, and then add 2000 parts of ethanol for ball milling. The ball mill speed is 40r min -1 , ball milling time is 48h;
[0106] Precursor granulation process: The uniformly ground slurry is injected into the spray granulation tower through a diaphragm pump to prepare a precursor granulation powder with high sphericity and excellent fluidity. The injection pressure of the diaphragm pump is 0.75MPa, the inlet temperature in the granulation tower is 250℃, and the outlet temperature is 90℃.
[0107] The morphology of the granulated powder obtained is as follows Figure 2 As shown in the figure, it is spherical, complete in shape, has good fluidity, and an average particle size of about 150 μm.
[0108] Precursor granulation powder nitridation process: First, adjust the inclination angle of the fluidized bed reaction chamber to 4°, turn on the rotating device, adjust the reaction chamber speed to 10 rpm, then evacuate the reaction chamber to 15 Pa, maintain the pressure for 30 minutes, observe the air tightness of the reaction chamber, and after the air tightness is confirmed, slowly fill it with high-purity N2 until the pressure in the reaction chamber is slightly higher than the atmospheric pressure, open the outlet valve, and adjust the nitrogen flow value to 0.010 g·s -1 Then, the temperature of the reaction chamber is set in different zones, as follows: the first temperature zone: 300-350°C, the second temperature zone: 750-800°C, the third temperature zone: 1200-1250°C, the fourth temperature zone: 1370-1390°C (high temperature zone), the fifth temperature zone: 1200°C. After the temperature of each temperature zone is stable, the material is fed through the automatic feeder, and the feed rate is controlled to be 15g·min -1 , so that the precursor powder stays in the high temperature zone for 120 minutes, and the outlet powder temperature is close to room temperature.
[0109] Comparative Example 5 (different feed rate from Example 1)
[0110] Precursor slurry preparation process: In a 10L polyurethane ball mill, add 1000 parts of raw material Si powder, 400 parts of diluent Si3N4 powder, 2.0 parts of dispersant triethyl phosphate, 5.0 parts of binder polyvinyl butyral, 3000 parts of high-purity Si3N4 grinding balls with a diameter of about 2mm, and then add 2000 parts of ethanol for ball milling. The ball mill speed is 40r min -1 , ball milling time is 48h;
[0111] Precursor granulation process: The uniformly ground slurry is injected into the spray granulation tower through a diaphragm pump to prepare a precursor granulation powder with high sphericity and excellent fluidity. The injection pressure of the diaphragm pump is 0.75MPa, the inlet temperature in the granulation tower is 250℃, and the outlet temperature is 90℃.
[0112] Precursor granulation powder nitridation process: First, adjust the inclination angle of the fluidized bed reaction chamber to 4°, turn on the rotating device, adjust the reaction chamber speed to 10 rpm, then evacuate the reaction chamber to 15 Pa, maintain the pressure for 30 minutes, observe the air tightness of the reaction chamber, and after the air tightness is confirmed, slowly fill it with high-purity N2 until the pressure in the reaction chamber is slightly higher than the atmospheric pressure, open the outlet valve, and adjust the nitrogen flow value to 0.010 g·s -1 Then, the temperature of the reaction chamber is set in different zones, as follows: first temperature zone: 300-350°C, second temperature zone: 750-800°C, third temperature zone: 1200-1250°C, fourth temperature zone: 1400-1450°C (high temperature zone), fifth temperature zone: 1200°C. After the temperature of each temperature zone is stable, feed the material through the automatic feeder, and control the feed rate to 30g·min -1 , so that the precursor powder stays in the high temperature zone for 120 minutes, and the outlet powder temperature is close to room temperature.
[0113] The obtained Si3N4 powder is then ball-milled and vacuum-packed to obtain the product. The XRD pattern of the obtained powder is shown in Figure 3 , appearance see Figure 4 , component analysis and particle size test results are shown in Table 2.
[0114] Comparative Example 6 (Different diluent ratio from Example 1)
[0115] Precursor slurry preparation process: In a 10L polyurethane ball mill, add 1000 parts of raw material Si powder, 200 parts of diluent Si3N4 powder, 2.0 parts of dispersant triethyl phosphate, 5.0 parts of binder polyvinyl butyral, 3000 parts of high-purity Si3N4 grinding balls with a diameter of about 2mm, and then add 2000 parts of ethanol for ball milling. The ball mill speed is 40r min -1 , ball milling time is 48h;
[0116] Precursor granulation process: The uniformly ground slurry is injected into the spray granulation tower through a diaphragm pump to prepare a precursor granulation powder with high sphericity and excellent fluidity. The injection pressure of the diaphragm pump is 0.75MPa, the inlet temperature in the granulation tower is 250℃, and the outlet temperature is 90℃.
[0117] Precursor granulation powder nitridation process: First, adjust the inclination angle of the fluidized bed reaction chamber to 4°, turn on the rotating device, adjust the reaction chamber speed to 10 rpm, then evacuate the reaction chamber to 15 Pa, maintain the pressure for 30 minutes, observe the air tightness of the reaction chamber, and after the air tightness is confirmed, slowly fill it with high-purity N2 until the pressure in the reaction chamber is slightly higher than the atmospheric pressure, open the outlet valve, and adjust the nitrogen flow value to 0.010 g·s -1 Then, the temperature of the reaction chamber is set in different zones, as follows: first temperature zone: 300-350°C, second temperature zone: 750-800°C, third temperature zone: 1200-1250°C, fourth temperature zone: 1400-1450°C (high temperature zone), fifth temperature zone: 1200°C. After the temperature of each temperature zone is stable, feed the material through the automatic feeder, and control the feed rate to 15g·min -1 , so that the precursor powder stays in the high temperature zone for 120 minutes, and the outlet powder temperature is close to room temperature.
[0118] The obtained Si3N4 powder is then ball-milled and vacuum-packed to obtain the product. The XRD pattern of the obtained powder is shown in Figure 3 , appearance see Figure 4 , component analysis and particle size test results are shown in Table 2.
[0119] Table 2 Composition and particle size analysis results of Si3N4 powder obtained from different results (D 50 )
[0120]
[0121] The main test methods consist of:
[0122] Si element: gravimetric test;
[0123] N / O element: nitrogen instrument test;
[0124] Fe / Al / Ca elements: tested by ICP;
[0125] The "K value method" in XRD quantitative analysis is used to analyze the percentage of α-Si3N4, β-Si3N4 and free silicon in the product (this has been reported in numerous literatures).
[0126] Powder particle size: tested by nano laser particle size analyzer.
[0127] The larger the nitrogen flow rate, the three aspects of influence: 1. The more nitrogen there is, the faster the silicon nitridation rate is, and the faster the crystal growth rate of silicon nitride powder is. Of course, it is also easy to introduce inclusions, such as lattice oxygen, because the solid solubility of O in the β-Si3N4 lattice can reach 0.26wt%, while the solid solubility in the α-Si3N4 lattice is only 0.9-1.48wt%, which is conducive to the formation of β-Si3N4; 2. The larger the nitrogen flow rate, the better the thermal shock generated by the cold air flow and the hot air flow will be on the surface of silicon nitride, The core is silicon The particle crushing effect is better, which is conducive to increasing the reaction rate of silicon. At the same time, the nitrogen flow value in Comparative Example 1 is higher, and the nitrogen is sufficient, which will also lead to a more thorough reaction between silicon and nitrogen, so the less residual silicon is, and Comparative Example 1 has less residual silicon than the embodiment; the combined effect of the above two factors leads to less residual silicon in Comparative Example 1, but the α phase content is lower than that in Example 1. The inclination angle of the reaction chamber in Comparative Example 2 is larger, and the α phase content is lower than that in Example 1. In Comparative Example 3, the rotation rate of the reaction chamber is relatively high, and the α-phase content is lower than that in Example 1. In Comparative Example 4, the temperatures in the fourth and fifth temperature zones are relatively low, and the α-phase content is lower than that in Example 1. In Comparative Example 5, the feed rate is relatively high, and the α-phase content is lower than that in Example 1. In Comparative Example 6, the diluent ratio is relatively low, and the α-phase content is lower than that in Example 1.
Claims
1. A method for preparing a silicon nitride powder precursor, It is characterized in that The steps include: S1, mixing Si powder, silicon nitride powder, triethyl phosphate, polyvinyl butyral and ethanol to obtain a precursor slurry; S2. Spray granulate the precursor slurry to obtain a precursor.
2. A method for preparing silicon nitride powder, It is characterized in that The steps include: The precursor prepared in claim 1 is added into the inclined rotating fluidized bed reaction chamber, and N 2 and heating the granulated powder to make it 2 Nitriding reaction occurs to obtain Si 3 N 4 pink; The N 2 The flow rate is 0.010-0.019 g·s -1 ; The inclination angle of the reaction chamber is 4-7°; The rotation rate of the reaction chamber is 10-19 r·min -1 ; The temperature of the nitridation reaction is 1200-1500° C., and the time is 0.5-6 hours.
3. The method for preparing silicon nitride powder according to claim 1, It is characterized in that In S3, the temperature of the nitridation reaction is set to five temperatures, namely, the first temperature zone: 250-400°C, the second temperature zone: 700-850°C, the third temperature zone: 1100-1300°C, the fourth temperature zone: 1400-1500°C, and the fifth temperature zone: 1200-1300°C.
4. The method for preparing silicon nitride powder according to claim 1, It is characterized in that In S3, the granulation powder is added at a rate of 10-80 g·min -1 .
5. The method for preparing silicon nitride powder according to any one of claims 2 to 4, Features: The average particle size of the granulated powder, the diameter of the fluidized bed reaction chamber and N 2 The flow rate has the following relationship: In the formula, p 1 is atmospheric pressure, unit is Pa, p 2 is the pressure in the reaction chamber, in Pa, v 1 N 2 Flow rate, in g·s -1 , v 2 is the powder flow rate in the reaction chamber, in g·s -1 , d 1 is the diameter of the reaction chamber, in mm, d 2 is the average particle size of the precursor granulated powder, in mm, and k is a constant ranging from 0.06 to 0.
1.
6. The method for preparing silicon nitride powder according to any one of claims 2 to 4, Features: N in the reaction chamber 2 The air pressure is 1.1×10 5 -1.5×10 5 Pa; The granulation powder flow rate in the reaction chamber is 0.2-1.0 g·s -1 ; The reaction chamber has a diameter of 40-400 mm; The average particle size of the granulated powder is 0.05-0.2 mm.
7. The method for preparing silicon nitride powder according to any one of claims 2 to 4, Features: The particle size of the Si powder is ≤5 μm and the purity is ≥99.99 wt %; The silicon nitride powder has an average particle size of 500-900 nm and a purity of ≥99.99 wt %; The purity of the triethyl phosphate is ≥99.5wt%; The molecular weight of the polyvinyl butyral is 40,000-70,000 M.W., and the purity is ≥99.5wt%.
8. The method for preparing silicon nitride powder according to any one of claims 2 to 4, Features: In S1, by weight, 100 parts of Si powder, 10-60 parts of silicon nitride powder, 0.2-1.5 parts of triethyl phosphate, 0.2-10 parts of polyvinyl butyral, and 50-300 parts of ethanol are taken and mixed by ball milling.
9. The method for preparing silicon nitride powder according to any one of claims 2 to 4, Features: S1 adopts ball milling mixing, and the ball milling rate of the ball milling mixing is 20-60r·min -1 , time is 12-48h.
10. A silicon nitride powder obtained by the preparation method according to any one of claims 2 to 9, It is characterized in that The α phase ratio of the silicon nitride powder is ≥96%, the residual silicon is 0.2-0.4wt%, and the D50 is 110-120nm; Preferably, the impurity content is 0.19-0.45wt%; Further preferably, the impurities include O, Fe, Al, and Ca; The O content is 0.1-0.3wt%, the Fe content is 0.004-0.006wt%, the Al content is 0.001-0.003wt%, and the Ca content is 0.004-0.006wt%.
Citation Information
Patent Citations
Production method of high-content silicon nitride (Si3N4) powder
CN102173397A
Preparation method of high-thermal-conductivity silicon nitride ceramic substrate
CN115028460A
Preparation method of silicon nitride
CN115072678A
Process for ordinary pressure continuous synthesizing silicon nitride powder by fluidized bed tech.
CN1792774A
Process for the continuous treatment of very finely divided substances with gases in fluidized beds, and reactor for the implementation of this process
EP0449398A2