Low-temperature chemical corrosion method and system for polycrystalline ceramic material

By using low-temperature chemical corrosion methods with KOH and NaOH, the safety hazards and high energy consumption of high-temperature corrosion of polycrystalline ceramic materials have been solved. The uniformity and controllability of the corrosion process have been achieved, improving the surface quality and performance consistency of polycrystalline ceramic materials, making it suitable for large-scale industrial production.

CN119043853APending Publication Date: 2024-11-29CHONGQING JIFENG TECHNOLOGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411371281.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing high-temperature thermal corrosion methods for polycrystalline ceramic materials are harsh and difficult to control, while traditional chemical corrosion methods pose safety hazards and consume a lot of energy, and the uneven corrosion affects product performance.

Method used

A low-temperature chemical etching method using KOH and NaOH is employed. After polishing, chemical etching is carried out at 100-250℃. The ratio and time of KOH and NaOH are controlled to ensure the uniformity and controllability of the etching process.

Benefits of technology

It enables effective etching of polycrystalline ceramic samples under low-temperature conditions, with clear grain boundaries and grains, reducing equipment costs and energy consumption, improving production efficiency, reducing thermal damage, and enhancing surface quality and performance consistency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119043853A_ABST
    Figure CN119043853A_ABST
Patent Text Reader

Abstract

The invention belongs to but not limited to the technical field of preparation of polycrystalline ceramic materials, and discloses a low-temperature chemical corrosion method and system for polycrystalline ceramic materials, and the method comprises the following steps: carrying out surface grinding and polishing on a prepared ceramic sample on a polishing machine by using a rough polishing disc until no macroscopic coarse particles exist on the surface of the sample; then, a rough polishing disc is replaced with fine polishing lint, and after 10000-mesh diamond polishing paste is coated, continuous polishing is conducted till the surface of the sample is in mirror surface brightness; kOH and NaOH are added into a metal nickel container according to the mass ratio of 51.5: 48.5, the polished ceramic sample is slowly put into the metal nickel container through tweezers, then the metal nickel container is put into a muffle furnace, and heat preservation is started after the temperature is increased to 100-250 DEG C; after chemical corrosion is carried out for 10-100 minutes, the sample is placed in a beaker containing a large amount of clear water through tweezers, ultrasonic cleaning is carried out, and the sample is wiped clean through dust-free cloth after being cleaned. The method is simple to operate, safe and low in energy consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to but is not limited to the technical field of polycrystalline ceramic material preparation, and in particular relates to a low-temperature chemical etching method and system for polycrystalline ceramic materials. Background Art

[0002] High-performance polycrystalline nano-ceramic materials are widely used in modern industry due to their excellent structural (high hardness, fracture toughness and bending strength, etc.) and functional (optical, electrical, magnetic, acoustic, thermal, etc.) properties. The microstructure of polycrystalline ceramic materials, such as grain size, grain shape, impurities, pores, etc., have a great influence on their performance. By observing the surface microstructure of ceramic samples, it is helpful to analyze their properties and optimize the preparation process. Before observing the surface microstructure of ceramics, it is usually necessary to perform surface treatment (such as high-temperature thermal corrosion or chemical corrosion, etc.) to reveal clear grains and grain boundaries.

[0003] Sun Kun and others from Jiangsu University used a high-temperature thermal corrosion method to corrode ceramics, under the condition of nitrogen atmosphere, 1800℃ for 1 hour. The thermal corrosion conditions of ceramics are relatively harsh, usually requiring high temperatures of >1000℃ and protection of inert gas, and the thermal corrosion process is difficult to control, which can easily lead to grain coarsening. The Chinese invention patent with publication number CN114804931A discloses a low-temperature chemical acid corrosion method for ceramics, which places the ceramic sample in a reaction vessel filled with concentrated phosphoric acid and begins heating and corrosion. Although the chemical corrosion method consumes less energy, the corrosion process is easy to control and the corrosion effect is also good, the concentrated phosphoric acid needs to be heated during the corrosion process, and the corrosion temperature usually needs to be above 300℃, which will bring considerable safety hazards to the operator or the environment. Summary of the invention

[0004] In response to the problems existing in the prior art, the present invention provides a low-temperature chemical etching method for polycrystalline ceramic materials (polycrystalline oxides, nitrides, carbides, nitrogen oxides and other ceramic materials), which simplifies the operation process and reduces the energy consumption required for the etching process while effectively etching the polycrystalline ceramics.

[0005] The present invention is implemented as follows: a low temperature chemical etching method for polycrystalline ceramic material comprises the following steps:

[0006] Step 1, polishing of ceramic samples: rough polishing of the prepared ceramic samples first, and then fine polishing;

[0007] Step 2: Chemical etching of ceramic samples: Chemical etching is performed using KOH and NaOH.

[0008] Further, rough polishing: the prepared ceramic sample is firstly ground and polished on the surface of the polishing machine with a rough polishing disc until there are no coarse particles visible to the naked eye on the surface of the sample.

[0009] Further, fine polishing: replace the rough polishing disc with the fine polishing polishing velvet cloth, apply 10000 mesh diamond polishing paste and polish continuously until the sample surface becomes mirror-bright.

[0010] Furthermore, KOH and NaOH were added into a metal nickel container in a mass ratio of 51.5:48.5, and the polished ceramic sample was slowly placed into it with tweezers, and then placed into a muffle furnace, heated to 100-250°C and then kept warm.

[0011] Furthermore, after the chemical corrosion is carried out for 10-100 minutes, the sample is placed in a beaker containing a large amount of clean water using tweezers, and is cleaned using ultrasound, and then wiped clean with a dust-free cloth.

[0012] Another object of the present invention is to provide a low-temperature chemical etching system for polycrystalline ceramic materials of a low-temperature chemical etching method for polycrystalline ceramic materials, comprising:

[0013] A polishing module, used for rough polishing and then fine polishing the prepared ceramic sample;

[0014] Chemical etching module, using KOH and NaOH for chemical etching.

[0015] In combination with the above technical solutions and the technical problems solved, the advantages and positive effects of the technical solutions to be protected by the present invention are as follows:

[0016] First, the present invention is simple to operate, safe and has low energy consumption. The ceramic samples etched by this method have obvious grain shapes and clear grain boundaries. The microstructure of the ceramic and the distribution of defects such as internal impurities and pores can be effectively observed, which is convenient for researchers to analyze and judge the preparation process and performance of the material.

[0017] The technical solution of the present invention solves the technical problem that people have been eager to solve but have never succeeded in solving: compared with the traditional thermal corrosion method, which usually requires surface corrosion of the sample under high temperature conditions, the present invention realizes surface chemical corrosion of the sample under low temperature conditions. The grain boundaries and grain states of the polycrystalline ceramic sample after corrosion are clearly visible, which is conducive to our observation and analysis of the surface state of the polycrystalline ceramic sample.

[0018] Second, the technical solution of the present invention solves multiple technical problems existing in the existing polycrystalline ceramic material corrosion method in industrial applications and has achieved significant technical progress, as follows:

[0019] 1. Reduce the corrosion temperature and equipment cost: The traditional chemical corrosion method of polycrystalline ceramic materials usually requires a higher temperature (such as above 500°C) to achieve effective corrosion, which places higher requirements on the heat resistance and energy consumption of the equipment. The present invention uses a chemical corrosion method of KOH and NaOH to complete the corrosion process at a relatively low temperature (100-250°C), effectively reducing the heat resistance requirements for the equipment, saving energy costs, and is suitable for large-scale industrial production.

[0020] 2. Improve corrosion efficiency and shorten process time: The chemical corrosion process in the prior art is usually time-consuming and inefficient, which affects production efficiency. The present invention can complete corrosion within 10-100 minutes by optimizing the ratio of KOH and NaOH and temperature control, greatly shortening the corrosion time and improving the overall production efficiency.

[0021] 3. Improve surface quality and reduce subsequent processing steps: Traditional polycrystalline ceramic corrosion methods often lead to rough sample surfaces, which require multiple grinding and polishing processes to improve surface quality. The present invention performs fine polishing before corrosion, and uses a fine polishing disk and high-mesh diamond polishing paste to make the sample surface reach a mirror effect, thereby reducing subsequent processing steps and further improving production efficiency.

[0022] 4. Enhance process controllability and improve corrosion uniformity: Traditional chemical corrosion methods are prone to uneven corrosion, local over-corrosion or under-corrosion, which affects product performance. The present invention ensures the uniformity and controllability of the corrosion process by controlling the ratio of KOH and NaOH, temperature and corrosion time, and ensures the surface quality and performance consistency of polycrystalline ceramic materials.

[0023] 5. Reduce damage to ceramic materials and improve material performance: During high-temperature corrosion, ceramic materials are prone to thermal damage, resulting in a decrease in their mechanical properties. The present invention reduces thermal damage to ceramic materials by performing chemical corrosion under relatively low temperature conditions, maintains their excellent mechanical properties, and prolongs the service life of the product, making it suitable for ceramic products with high performance requirements.

[0024] In summary, the technical solution of the present invention has achieved significant technical progress in reducing corrosion temperature, improving corrosion efficiency, enhancing surface quality and process controllability, etc. It is suitable for large-scale production and high-demand polycrystalline ceramic material processing scenarios, and has broad industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a flow chart of a low-temperature chemical etching method for polycrystalline ceramic materials provided by an embodiment of the present invention;

[0026] Figure 2It is a structural diagram of a low-temperature chemical etching system for polycrystalline ceramic materials provided by an embodiment of the present invention;

[0027] Figure 3 is an optical microscope picture of the sample provided in Example 1 of the present invention;

[0028] Figure 4 is a SEM picture of the sample provided in Example 2 of the present invention;

[0029] Figure 5 This is a SEM picture of the sample provided in Example 3 of the present invention. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0031] like Figure 1 As shown, a low-temperature chemical etching method for polycrystalline ceramic materials provided by an embodiment of the present invention includes the following steps:

[0032] Step 1, polishing of ceramic samples: rough polishing of the prepared ceramic samples first, and then fine polishing;

[0033] Step 2: Chemical etching of ceramic samples: Chemical etching is performed using KOH and NaOH.

[0034] (1) Polishing of ceramic samples: The prepared ceramic samples were first polished with a rough polishing disc on a polishing machine until there were no coarse particles visible to the naked eye on the sample surface. Then the rough polishing disc was replaced with a fine polishing velvet cloth, and after applying 10,000 mesh diamond polishing paste, the sample surface was polished continuously until it became mirror-bright.

[0035] (2) Chemical corrosion of ceramic samples: Add KOH and NaOH in a metal nickel container with a mass ratio of 51.5:48.5, and slowly place the polished ceramic sample in it with tweezers, and then place it in a muffle furnace, heat it to 100-25℃ and start to keep it warm. After chemical corrosion for 10-100 minutes, place the sample in a beaker filled with a large amount of clean water with tweezers, clean it with ultrasound, and wipe it clean with a dust-free cloth.

[0036] Finally, the corroded ceramic samples were placed under a microscope to observe the microstructure. It was found that the grain shape of the ceramic samples corroded by this method was obvious and the grain boundaries were clearly visible.

[0037] like Figure 2As shown, a low-temperature chemical etching method for polycrystalline ceramic materials provided by an embodiment of the present invention includes a low-temperature chemical etching system for polycrystalline ceramic materials, comprising:

[0038] A polishing module, used for rough polishing and then fine polishing the prepared ceramic sample;

[0039] Chemical etching module, using KOH and NaOH for chemical etching.

[0040] Example 1

[0041] Step 1) Polishing of Al2O3 ceramic sample: The prepared Al2O3 ceramic sample is first polished on a polishing machine with a rough polishing disc until the required thickness is reached. Then the rough polishing disc is replaced with a fine polishing velvet cloth, and after applying 10000 mesh diamond polishing paste, the sample is continuously polished until the surface is mirror-bright.

[0042] Step 2) Chemical etching of Al2O3 transparent ceramics: Add KOH and NaOH in a metal nickel container with a mass ratio of 51.5:48.5, then put it into a muffle furnace and heat it to 200°C and start to keep it warm. Use tweezers to slowly put the AlON transparent ceramic sample into the metal nickel container with molten alkali, and immerse the sample completely in the molten alkali. After 60 minutes of chemical etching, use tweezers to place the sample in a beaker containing a large amount of hydrophilic, and clean it with ultrasound, and wipe it clean with a dust-free cloth.

[0043] Example 2

[0044] Step 1) Polishing of ZrO2 ceramic sample: The prepared ZrO2 ceramic sample is first polished on a polishing machine with a rough polishing disc until the required thickness is reached. Then the rough polishing disc is replaced with a fine polishing velvet cloth, and after applying 10000 mesh diamond polishing paste, the sample is continuously polished until the surface is mirror-bright.

[0045] Step 2) Chemical corrosion of ZrO2 transparent ceramics: Add KOH and NaOH in a metal nickel container with a mass ratio of 51.5:48.5, then put it into a muffle furnace and heat it to 200°C and start to keep it warm. Use tweezers to slowly put the AlON transparent ceramic sample into the metal nickel container with molten alkali, and immerse the sample completely in the molten alkali. After 60 minutes of chemical corrosion, use tweezers to place the sample in a beaker containing a large amount of hydrophilic, and clean it with ultrasound, and wipe it clean with a dust-free cloth.

[0046] Example 3

[0047] Step 1) Polishing of AlON transparent ceramic sample: The prepared AlON ceramic sample is first polished on a polishing machine with a rough polishing disc until the required thickness is reached. Then the rough polishing disc is replaced with a fine polishing velvet cloth, and after applying 10000 mesh diamond polishing paste, the sample is continuously polished until the sample surface is mirror-bright.

[0048] Step 2) Chemical corrosion of AlON transparent ceramics: KOH and NaOH were added to a metal nickel container in a mass ratio of 51.5:48.5, and the AlON transparent ceramic sample was slowly placed into the metal nickel container with molten alkali using tweezers, and then placed in a muffle furnace and heated to 180°C and then kept warm. After 30 minutes of chemical corrosion, the sample was placed in a beaker containing a large amount of hydrophilic material using tweezers, and cleaned with ultrasound, and then wiped clean with a dust-free cloth.

[0049] The present invention can be successfully applied to the surface state analysis of polycrystalline ceramic products. At present, it has a good effect on the low-temperature corrosion of oxide and oxynitride ceramic surfaces, and can be extended to the low-temperature corrosion of carbide and nitride ceramic surfaces.

[0050] The following are two specific application embodiments of the present invention in the field of polycrystalline ceramic materials:

[0051] Application Example 1: Surface Treatment of Polycrystalline Ceramic Electronic Components

[0052] In the electronics industry, polycrystalline ceramic materials are widely used in the manufacture of key components such as high-frequency devices, semiconductor packaging, and insulating substrates. The low-temperature chemical etching method of the present invention can effectively improve the surface finish and uniformity of these electronic components, and reduce problems such as signal interference and poor heat dissipation caused by rough surfaces. The low-temperature etching process can avoid high-temperature damage to the material while maintaining its excellent electrical insulation properties. The surface of the ceramic electronic component after fine polishing and chemical etching treatment is smoother, which is suitable for the manufacture of high-precision electronic components, and improves the stability and service life of the device.

[0053] Application Example 2: Surface modification of ceramic dental materials

[0054] Polycrystalline ceramics are often used to make dental implants and denture restoration materials due to their biocompatibility and corrosion resistance. However, untreated ceramic surfaces may have microscopic roughness, which affects the bonding strength with teeth or bone tissue. Through the low-temperature chemical corrosion method of the present invention, the surface of ceramic dental materials can be modified, the corrosion depth can be accurately controlled, and tiny defects and impurities on the surface can be removed to make the surface smoother and enhance the affinity with biological tissues. This not only improves the stability and long-term use effect of the implant, but also reduces the discomfort of patients after surgery.

[0055] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.

Claims

1. A low temperature chemical etching method for polycrystalline ceramic materials, characterized in that: The following steps are involved: Step 1, polishing of ceramic samples: rough polishing of the prepared ceramic samples first, and then fine polishing; Step 2: Chemical etching of ceramic samples: Chemical etching is performed using KOH and NaOH.

2. The low temperature chemical etching method of polycrystalline ceramic material according to claim 1, characterized in that: Rough polishing: The prepared ceramic sample is first polished with a rough polishing disc on a polishing machine until there are no coarse particles visible to the naked eye on the surface of the sample.

3. The low temperature chemical etching method for polycrystalline ceramic material according to claim 1, characterized in that: Fine polishing: Replace the rough polishing disc with the fine polishing polishing velvet cloth, apply 10000 mesh diamond polishing paste and polish continuously until the sample surface becomes mirror-bright.

4. The low temperature chemical etching method for polycrystalline ceramic material according to claim 1, characterized in that: Add KOH and NaOH in a metal nickel container with a mass ratio of 51.5:48.5, and slowly put the polished ceramic sample into it with tweezers, then put it into a muffle furnace, heat it to 100-250℃ and start keeping it warm.

5. The low temperature chemical etching method for polycrystalline ceramic material according to claim 4, characterized in that: After chemical etching for 10-100 minutes, place the sample in a beaker filled with a large amount of clean water using tweezers and clean it using ultrasound. After cleaning, wipe it clean with a dust-free cloth.

6. A low-temperature chemical etching system for polycrystalline ceramic materials according to any one of claims 1 to 5, characterized in that: include: A polishing module, used for rough polishing and then fine polishing the prepared ceramic sample; Chemical etching module, using KOH and NaOH for chemical etching.

Citation Information

Patent Citations

  • AlON transparent ceramic low-temperature corrosion method

    CN114804931A