Method for improving passivation contact performance of p region of TBC battery
By adopting ultra-low temperature PECVD process and nanosecond excimer laser treatment in TBC cells, combined with step-by-step etching technology, the problem of easy separation of B elements at the SiO2/c-Si interface is solved, significantly improving the p-zone passivation contact performance, and improving the open circuit voltage, filling factor and short-circuit current density of the battery.
Patent Information
- Application Number
- CN202510488213.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-18
- Publication Date
- 2025-07-22
AI Technical Summary
In the prior art, element B is easily separated at the interface of silicon oxide/crystalline silicon substrate, resulting in an increase in the interfacial defect density, limiting the passivation contact performance of the p-zone, and thus affecting the overall performance improvement of the TBC battery.
Ultra-low temperature PECVD process is used to deposit the tunneled oxide layer and boron-doped polycrystalline silicon, combined with nanosecond excimer laser treatment, ultra-high concentration doping is formed in the polycrystalline silicon layer through a non-equilibrium doping mechanism, and combined with step-by-step etching and laser processing technology to accurately control the geometric size and distribution of the p- and n-regions to build a double-doped structure.
The separation phenomenon of B element at the SiO2/c-Si interface is significantly suppressed, the carrier concentration gradient and energy band structure are improved, the interface state defect density is reduced, the open circuit voltage and filling factor is improved, the carrier collection efficiency is enhanced, and the short-circuit current density of the battery is improved.
Smart Images

Figure CN120358824A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of crystalline silicon solar cells, and in particular to a method for improving the passivation contact performance of a TBC cell p region. Background Art
[0002] TBC solar cells are crystalline silicon solar cells with a back contact structure, in which boron-doped and phosphorus-doped poly-Si serve as the emitter and back surface field (BSF) respectively. The cell deposits a tunneling oxide layer (SiO2) between the poly-Si and c-Si substrate to enhance carrier selectivity and inhibit the recombination of minority carriers, thereby increasing the open circuit voltage (V OC ). The main advantage of TBC solar cells is that the light-receiving surface is not blocked by metal, that is, the front electrode-free design maximizes the absorption of incident light and improves light utilization. In addition, the back side (non-light-receiving side) adopts an optimized metal grid line layout, which allows wider metal grid lines, thereby reducing series resistance and improving fill factor (FF). At the same time, the introduction of the front surface field (FSF) and high-quality passivation layer further improves the open circuit voltage, thereby improving the overall photoelectric conversion efficiency.
[0003] At present, in n-type c-Si TBC cells, the preparation of p-region poly-Si usually adopts a uniform emitter structure. + Compared with poly-Si structure, SiO2 / p + The passivation performance of poly-Si structure is relatively weak. For example, on n-type c-Si substrate, SiO2 / n + poly-Si structure OC Can easily reach 730mV, while SiO2 / p + iV of poly-Si structure OC Only about 710mV, which limits the overall passivation performance of TBC batteries. Studies have shown that the B element is prone to separation at the SiO2 / c-Si interface, resulting in an increase in the density of interface state defects, thereby reducing the quality of interface passivation and affecting the further improvement of battery performance.
[0004] Therefore, it is necessary to design a method to improve the passivation contact performance of the p-region of the TBC battery, so as to solve the problem that the B element in the prior art is easily separated at the silicon oxide / crystalline silicon substrate (SiO2 / c-Si) interface, resulting in an increase in the interface state defect density, thereby reducing the passivation ability of c-Si. Due to the limitation of the solid solubility of B in polycrystalline silicon, it is difficult to obtain a B-doped poly-Si film layer with a high doping concentration, which limits the passivation contact performance of the p-region and restricts the improvement of the overall performance of the TBC battery. Summary of the invention
[0005] In view of this, the present invention proposes a method for improving the passivation contact performance of the p-region of a TBC cell, aiming to solve the problem that in the prior art, boron (B)-doped polysilicon (poly-Si) is usually used in the p-region. However, the B element is prone to separation at the interface of silicon oxide / crystalline silicon substrate (SiO2 / c-Si), resulting in an increase in the density of interface state defects, thereby reducing the passivation ability for c-Si. Compared with phosphorus (P)-doped poly-Si, its passivation effect is weaker. In addition, the prior art, including plasma-enhanced chemical vapor deposition (PECVD) and low-pressure chemical vapor deposition (LPCVD), is limited by the solid solubility of B in polysilicon and it is difficult to obtain a B-doped poly-Si film layer with a high doping concentration, thus restricting the passivation contact performance of the p-region and restricting the improvement of the overall performance of the TBC cell.
[0006] On the one hand, the present invention proposes a method for improving the passivation contact performance of the p-region of a TBC cell, including:
[0007] Step 1: Use an n-type monocrystalline silicon wafer as the crystalline silicon substrate and use an alkaline solution to remove the cutting damage layer on the silicon surface;
[0008] Step 2: Polish the silicon wafer obtained in Step 1 with a KOH solution having a concentration of 1% - 2% and perform standard RCA cleaning to obtain a pretreated silicon wafer;
[0009] Step 3: Place the pretreated silicon wafer into a PECVD furnace, deposit a SiO2 layer and B-doped amorphous silicon at a temperature of 200 - 250 °C, and perform high-temperature annealing treatment in a nitrogen atmosphere;
[0010] Step 4: Etch the silicon wafer obtained in Step 3 to remove the borosilicate glass (BSG) on the front and side surfaces, use a laser to remove the BSG outside the p-region on the back surface, use an alkaline solution to remove the exposed poly-Si, and polish the back surface;
[0011] Step 5: Perform laser ablation on the p-region of the silicon wafer obtained in Step 4 with an excimer laser and place it in the air to cool;
[0012] Step 6: Deposit P-doped poly-Si on the back surface of the silicon wafer obtained in Step 5 by PECVD and perform annealing treatment;
[0013] Step 7: Perform etching treatment on the silicon wafer obtained in Step 6 to remove the phosphosilicate glass (PSG) on the front and side surfaces, use a laser to clean the PSG outside the n-region on the back surface, and perform cleaning and front surface texturing;
[0014] Step 8: Deposit an Al2O3 passivation layer using atomic layer deposition (ALD) equipment and deposit SiN using PECVD equipment x: H anti-reflection layer;
[0015] Step 9, the p and n regions on the back of the silicon wafer obtained in Step 8 are respectively covered with silver-aluminum paste (Ag / Al) and Ag paste by screen printing, and co-sintered through an infrared belt furnace.
[0016] Furthermore, the crystal orientation of the n-type monocrystalline silicon wafer is (100), the thickness of the silicon wafer is <150 μm, and the resistivity is 0.5 - 50 Ω·cm.
[0017] Furthermore, the deposition thickness of the SiO2 layer is 1 - 3 nm, the deposition thickness of the B-doped amorphous silicon is 100 - 350 nm, the precursors used for the SiO2 layer include SiH4, N2O and H2, the precursors used for the B-doped amorphous silicon include SiH4, H2 and a B source, and the B source is B2H6, TMB or BCl3;
[0018] The annealing deposition time in Step 3 is 30 min, and the annealing temperature is 900 - 1000 °C.
[0019] Furthermore, the laser in Step 4 is a 325 nm violet laser, and the width of the p region formed by the laser is 300 - 500 μm.
[0020] Furthermore, the wavelength of the laser in Step 5 is 248 nm, and the pulse duration is 22 ns.
[0021] Furthermore, the phosphorus doping concentration of the deposited P-doped poly-Si in Step 6 is 1×10 20 ~1×10 21 cm -3 , the thickness is 50 - 150 nm, and during the deposition process, silane, phosphine and hydrogen are introduced, and the flow ratio of the phosphine gas is 2% - 8%.
[0022] Furthermore, the laser in Step 7 is a 532 nm green laser, and the width of the n region formed by the laser is 100 - 300 μm, and the gap width between the p region and the n region is 30 - 100 μm.
[0023] Furthermore, the thickness of the Al2O3 passivation layer is 2 - 4 nm, and the thickness of the SiN x :H anti-reflection layer is 70 - 80 nm.
[0024] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0025] 1. The present invention deposits a tunneling oxide layer and boron-doped polysilicon in the p-region by using an ultra-low temperature PECVD process. Combining a specific precursor ratio (such as the reaction system of SiH4 and N2O), the compactness of the oxide layer at low temperature is effectively improved, and the segregation phenomenon of B element at the SiO2 / c-Si interface is significantly inhibited. This optimized interface structure can reduce the density of interface state defects, thereby improving the passivated contact performance of the p-region and significantly increasing the open-circuit voltage compared with the traditional structure.
[0026] 2. The present invention innovatively uses a nanosecond-level excimer laser to locally process the p-region. Through the non-equilibrium doping mechanism, the B element breaks through the conventional solid solubility limit, and a super-high concentration doping is formed in the poly-Si layer. This doping method not only enhances the carrier concentration gradient but also improves the energy band structure at the interface, further enhancing the carrier selective transport efficiency, thereby increasing the open-circuit voltage and fill factor of the battery.
[0027] 3. The present invention precisely controls the geometric dimensions and distributions of the p-region and n-region through step-by-step etching and laser processing techniques (such as backside laser selective removal of the BSG / PSG layer), effectively reducing the back surface parasitic resistance. At the same time, by optimizing the gap width between the p-region and n-region, the lateral leakage phenomenon is suppressed, and the reverse breakdown characteristics of the battery are improved. The present invention constructs a double-doped structure on the back surface and forms an effective back surface field (BSF) by combining a high-temperature annealing process. This structural design can significantly reduce the recombination probability of minority carriers at the back surface, improve the carrier collection efficiency, and thus increase the short-circuit current density of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] By reading the detailed description of the preferred embodiments below, various other advantages and benefits will become clear to those of ordinary skill in the art. The drawings are only for the purpose of showing the preferred embodiments and are not considered to be a limitation of the present invention. Moreover, throughout the drawings, the same reference numerals are used to represent the same components. In the drawings:
[0029] Figure 1 is a flowchart of the method for improving the passivated contact performance of the p-region of the TBC battery according to the embodiment of the present invention;
[0030] Figure 2 is a schematic diagram after the silicon wafer is cleaned and polished;
[0031] Figure 3 is the tunneling oxide layer and boron-doped polysilicon deposited by PECVD;
[0032] Figure 4 is the laser ablation treatment of the p-region by a nanoscale pulsed laser;
[0033] Figure 5Schematic diagram of the final TBC crystalline silicon solar cell structure of the present invention, where 1 is an n-type crystalline silicon substrate, 2 is a tunneling oxide layer, 3 is boron-doped polysilicon, 4 is a phosphorus-doped polysilicon layer, 5 and 6 are aluminum oxide passivation layers, 7 and 8 are hydrogenated silicon nitride antireflection layers, and 9 is a metal electrode. Detailed implementation manners
[0034] Exemplary embodiments of the present invention will be described in more detail below with reference to the drawings. Although the exemplary embodiments of the present invention are shown in the drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided so that the present invention can be more thoroughly understood and the scope of the present invention can be completely conveyed to those skilled in the art. It should be noted that, without conflict, the embodiments in the present invention and the features in the embodiments can be combined with each other. The present invention will be described in detail below with reference to the drawings and in combination with the embodiments.
[0035] In the drawings, components with the same structure are denoted by the same numeral labels, and components with similar structures or functions everywhere are denoted by similar numeral labels. The size and thickness of each component shown in the drawings are arbitrarily shown, and the present invention does not limit the size and thickness of each component. In order to make the drawings clearer, the thickness of some components in the drawings is appropriately exaggerated.
[0036] Referring to Figure 1 As shown, in some embodiments of the present application, a method for improving the passivated contact performance of the p region of a TBC cell includes:
[0037] Step 1: Use an n-type monocrystalline silicon wafer as the crystalline silicon substrate, and use an alkaline solution to remove the silicon surface cutting damage layer;
[0038] Step 2: Polish the silicon wafer obtained in Step 1 with a KOH solution having a concentration of 1% - 2%, and perform a standard RCA cleaning to obtain a pretreated silicon wafer;
[0039] Step 3: Place the pretreated silicon wafer in a PECVD furnace, deposit a SiO2 layer and B-doped amorphous silicon at a temperature of 200 - 250 °C, and perform an annealing treatment in a nitrogen atmosphere at a temperature of 900 - 1000 °C;
[0040] Step 4: Etch the silicon wafer obtained in Step 3 to remove the boron-silicate glass (BSG) on the front and side surfaces, use a laser to remove the BSG outside the p region on the back surface, use an alkaline solution to remove the exposed poly-Si, and polish the back surface;
[0041] Step 5: Perform laser ablation on the p region of the silicon wafer obtained in Step 4 through an excimer laser, and place it in the air to cool;
[0042] Step 6: Deposit P-doped poly-Si on the back side of the silicon wafer obtained in Step 5, and perform annealing treatment.
[0043] Step 7: Etch the silicon wafer obtained in Step 6 to remove the phosphosilicate glass (PSG) on the front and side surfaces, clean the PSG other than the n-region on the back side using a laser, and then perform cleaning and front-side texturing.
[0044] Step 8: Deposit an Al2O3 passivation layer using an atomic layer deposition (ALD) device, and deposit a SiN x :H antireflection layer using a PECVD device.
[0045] Step 9: Cover the p-region and n-region on the back side of the silicon wafer obtained in Step 8 with silver-aluminum paste (Ag / Al) and Ag paste respectively by screen printing, and perform co-sintering using an infrared belt sintering furnace.
[0046] Specifically, prepare an n-type single-crystalline silicon wafer with an industrial-grade crystal orientation of (100) as the crystalline silicon substrate. The thickness of the silicon wafer is 100 - 150 μm, and the resistivity is 0.5 - 50 Ω·cm; use an alkaline solution to remove the cutting damage layer on the silicon surface.
[0047] It can be understood that by optimizing the concentration of the alkaline solution and the treatment time, while ensuring the removal of the damage layer, over-corrosion is avoided. This operation eliminates the defect states introduced by surface mechanical damage and provides a high-quality substrate for subsequent interface engineering.
[0048] Specifically, as shown in Figure 2 , polish the n-type silicon wafer obtained in Step 1 with a KOH solution having a concentration of 1% - 2%, and then perform standard RCA cleaning to obtain a pre-treated silicon wafer.
[0049] It can be understood that by controlling the chemical ratio and treatment duration of the polishing solution, the surface of the silicon wafer reaches atomic-level flatness, and metal ions and organic contaminants are thoroughly removed through multiple-step cleaning. This process significantly reduces the surface roughness and provides excellent interface bonding conditions for subsequent deposited layers.
[0050] Specifically, as shown in Figure 3 , place the n-type silicon wafer obtained in Step 2 into a PECVD furnace and deposit a SiO2 layer with a thickness of 1.5 - 2 nm and a B-doped amorphous silicon layer with a thickness of 200 - 300 nm at a temperature of 200 - 250 °C. The precursors used for depositing the SiO2 layer include SiH4, N2O, and H2, while the precursors used for depositing the B-doped amorphous silicon include SiH4, H2, and a B source. The B source is B2H6. Then, perform annealing deposition for 30 min in a nitrogen atmosphere, and control the annealing temperature at 900 - 1000 °C.
[0051] It is understandable that by precisely controlling the flow rate of the precursor gas and the deposition parameters, a tunneling oxide layer with an ideal thickness is formed, and the crystallization process of amorphous silicon is promoted through high-temperature annealing. This structure constructs an effective carrier selective contact, inhibits the recombination of minority carriers, and reduces the segregation of B element at the interface.
[0052] Specifically, as shown in Figure 4 , the silicon wafer obtained in step 3 is etched with an HF solution to remove the BSG on the front and side surfaces, while the BSG outside the p-region on the back surface is removed by laser. The laser is 325nm violet light, and the width of the formed p-region is 300 - 500μm. Then, the exposed poly-Si is removed with an alkaline solution, and then the back surface is polished.
[0053] It is understandable that by optimizing the ratio of the etching solution and the laser energy density, the borosilicate glass layer in the local area is precisely removed, and the exposed polysilicon is selectively removed with an alkaline solution. This step eliminates the parasitic conductive channels on the side surface, forms a clear PN junction boundary, and effectively reduces the leakage loss.
[0054] Specifically, the p-region of the silicon wafer obtained in step 4 is subjected to laser ablation by an excimer laser. The wavelength of the laser is 248nm, and the pulse duration is 22ns (based on the full width at half maximum). After the laser treatment, it is placed in the air for rapid cooling. The doping concentration of the treated p-region can reach 5×10 20 ~8×10 20 cm -3 .
[0055] It is understandable that by adjusting the laser wavelength, pulse parameters, and scanning path, the microstructure control of doping is achieved. This operation promotes the defect reconstruction at the interface, forms a gradient doping distribution, and significantly improves the electrical properties of the passivated contact.
[0056] Specifically, P-doped poly-Si is deposited on the back surface of the silicon wafer obtained in step 5 by PECVD, and then annealing treatment is carried out. The P doping concentration is 5×10 20 ~1×10 21 cm -3 , and the thickness is 100 - 150nm. During the deposition process, silane, phosphine, and hydrogen gases need to be introduced, and the flow ratio of the phosphine gas is 8%.
[0057] It is understandable that by optimizing the flow ratio of the phosphine gas and the deposition temperature, a polysilicon layer with a suitable doping concentration is formed. This structure constructs an effective back surface field, reduces the recombination of minority carriers on the back surface, and improves the carrier collection efficiency at the same time.
[0058] Specifically, the silicon wafer obtained from step 6 is etched with an HF solution to remove the PSG on the front and side surfaces, and then the PSG other than the n-region is removed by laser cleaning on the back surface, followed by cleaning. The laser is a 532 nm green light. The width of the formed n-region is 100 - 300 μm, and the width of the Gap region is 30 - 100 μm. Then, texturing is performed on the front surface.
[0059] It can be understood that by optimizing the etching process parameters and the laser energy density, an ideal surface structure is formed. This step improves the light absorption efficiency while ensuring the insulation of the electrode region and reducing the surface recombination loss.
[0060] Specifically, an Al2O3 passivation layer and a SiN x :H antireflection layer are deposited using an ALD device and a PECVD device respectively, with thicknesses of 2 - 4 nm and 70 - 80 nm.
[0061] It can be understood that by precisely controlling the deposition cycle and the precursor flow rate, a composite film layer with the optimal thickness is formed. This combined structure simultaneously achieves the dual optimization of surface chemical passivation and optical antireflection, effectively improving the short-circuit current density of the battery.
[0062] Specifically, the p-region and n-region on the back surface of the silicon wafer obtained in step 8 are respectively covered with Ag / Al paste and Ag paste by screen printing, and finally co-sintered in an infrared belt furnace.
[0063] It can be understood that by optimizing the sintering temperature curve and the paste formulation, a metal electrode with a low contact resistance is formed. This process ensures the ohmic contact between the metal and the semiconductor layer, significantly reducing the series resistance and improving the fill factor of the battery.
[0064] Refer to Figure 5 As shown, an alumina passivation layer 5 and a hydrogenated silicon nitride antireflection layer 7 are sequentially formed on the front surface of the n-type crystalline silicon substrate 1; a tunneling oxide layer 2, a boron-doped polysilicon layer 3, a phosphorus-doped polysilicon layer 4, an alumina passivation layer 6, a hydrogenated silicon nitride passivation layer 8, and a metal electrode 9 are sequentially formed on the back surface of the n-type crystalline silicon substrate 1.
[0065] It is understandable that in the present invention, by depositing a tunneling oxide layer and boron-doped polysilicon in the p-region using an ultra-low temperature PECVD process and combining a specific precursor ratio (such as the reaction system of SiH4 and N2O), the compactness of the oxide layer at low temperatures is effectively improved, and the segregation phenomenon of B elements at the SiO2 / c-Si interface is significantly inhibited. This optimized interface structure can reduce the interface state defect density, thereby improving the passivation contact performance of the p-region and significantly increasing the open-circuit voltage compared with the traditional structure. The present invention innovatively uses a nanosecond excimer laser to locally process the p-region, enabling B elements to break through the conventional solid solubility limit through a non-equilibrium doping mechanism and forming a super-high concentration doping in the poly-Si layer. This doping method not only enhances the carrier concentration gradient but also improves the energy band structure at the interface, further enhancing the carrier selective transport efficiency, thereby increasing the open-circuit voltage and fill factor of the battery.
[0066] In the present invention, through stepwise etching and laser processing techniques (such as selectively removing the BSG / PSG layer by backside laser), the geometric dimensions and distributions of the p-region and n-region are precisely controlled, effectively reducing the back surface parasitic resistance. At the same time, by optimizing the gap width between the p-region and n-region, the lateral leakage phenomenon is suppressed, and the reverse breakdown characteristics of the battery are improved. The present invention constructs a double-doped structure on the back surface and forms an effective back surface field (BSF) in combination with a high-temperature annealing process. This structural design can significantly reduce the recombination probability of minority carriers at the back surface, improve the carrier collection efficiency, and thus increase the short-circuit current density of the battery.
[0067] It should be noted that:
[0068] In the specification provided herein, a large number of specific details are described. However, it can be understood that the embodiments of the present application can be practiced without these specific details. In some instances, well-known structures and technologies are not shown in detail so as not to obscure the understanding of this specification.
[0069] In addition, those skilled in the art can understand that although some embodiments described herein include certain features included in other embodiments rather than other features, the combination of the features of different embodiments means that it is within the scope of the present application and forms different embodiments.
[0070] As mentioned above, the above are only the preferred specific embodiments of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed in the present application should be covered by the protection scope of the present application. Therefore, the protection scope of the present application should be subject to the protection scope of the claims.
Claims
1. A method for improving the passivation contact performance of the p-region of a TBC cell, characterized in that, Including: Step 1: Use an n-type monocrystalline silicon wafer as the crystalline silicon substrate, and use an alkaline solution to remove the cutting damage layer on the silicon surface; Step 2: Polish the silicon wafer obtained in Step 1 with a KOH solution having a concentration of 1% - 2%, and perform standard RCA cleaning to obtain a pretreated silicon wafer; Step 3: Place the pretreated silicon wafer in a PECVD furnace, deposit a SiO2 layer and B-doped amorphous silicon at a temperature of 200 - 250 °C, and perform high-temperature annealing treatment in a nitrogen atmosphere; Step 4: Etch the silicon wafer obtained in Step 3 to remove the borosilicate glass (BSG) on the front and side surfaces, use a laser to remove the BSG outside the p-region on the back surface, use an alkaline solution to remove the exposed poly-Si, and polish the back surface; Step 5: Perform laser ablation on the p-region of the silicon wafer obtained in Step 4 through an excimer laser, and place it in the air to cool; Step 6: Deposit P-doped poly-Si on the back surface of the silicon wafer obtained in Step 5 by PECVD, and perform annealing treatment; Step 7: Perform etching treatment on the silicon wafer obtained in Step 6 to remove the phosphosilicate glass (PSG) on the front and side surfaces, use a laser to clean the PSG outside the n-region on the back surface, and perform cleaning and front surface texturing; Step 8, deposit an Al2O3 passivation layer using an atomic layer deposition (ALD) apparatus, and deposit a SiN x :H antireflection layer; Step 9: Cover the p and n regions on the back surface of the silicon wafer obtained in Step 8 with silver-aluminum paste (Ag / Al) and Ag paste respectively by screen printing, and perform co-sintering through an infrared belt sintering furnace.
2. A method for improving the passivation contact performance of the p-region of a TBC cell according to claim 1, characterized in that The crystal orientation of the n-type monocrystalline silicon wafer is (100), the thickness of the silicon wafer is <150 μm, and the resistivity is 0.5 - 50 Ω·cm.
3. A method for improving the passivation contact performance of the p-region of a TBC cell according to claim 1, characterized in that The deposition thickness of the SiO2 layer is 1 - 3 nm, the deposition thickness of the B-doped amorphous silicon is 100 - 350 nm, the precursors used for the SiO2 layer include SiH4, N2O and H2, the precursors used for the B-doped amorphous silicon include SiH4, H2 and a B source, and the B source is B2H6, TMB or BCl3; The annealing deposition time in Step 3 is 30 min, and the annealing temperature is 900 - 1000 °C.
4. A method for improving the passivation contact performance of the p-region of a TBC cell according to claim 1, characterized in that The laser in Step 4 is 325 nm violet light, and the width of the p-region formed by the laser is 300 - 500 μm.
5. A method for improving the passivation contact performance of the p-region of a TBC cell according to claim 1, characterized in that The wavelength of the laser in Step 5 is 248 nm, and the pulse duration is 22 ns.
6. A method for improving the passivation contact performance of the p-region of a TBC cell according to claim 1, characterized in that The phosphorus doping concentration of the deposited P-doped poly-Si described in step 6 is 1×10 20 ~1×10 21 cm -3 , and the gases introduced are silane, phosphine and hydrogen, where the phosphine gas flow ratio is 2% - 8%.
7. A method for improving the passivation contact performance of the p-region of a TBC cell according to claim 1, characterized in that The laser described in step 7 is green light with a wavelength of 532 nm, and the width of the n-region formed by the laser is 100 to 300 μm, and the gap width between the p-region and the n-region is 30 to 100 μm.
8. A method for improving the passivated contact performance of the p-region of a TBC battery according to claim 1, wherein The thickness of the Al2O3 passivation layer is 2 to 4 nm, and the thickness of the SiN x :H antireflection layer is 70 to 80 nm.
Citation Information
Cited By
TBC battery, preparation method thereof and photovoltaic module
CN121038426A
TBC battery and preparation method thereof
CN121194548A