Thermoplastic elastomer-based foaming composite material with excellent conductivity and electromagnetic shielding performance and preparation method thereof
The thermoplastic elastomer-based foaming composite material is prepared through the continuous extrusion process of composite foaming agent and double-step screw extruder, which solves the shrinkage problem during the foaming process and the residual problem of chemical foaming agent, and achieves excellent conductive and electromagnetic shielding performance, which is suitable for industrial production.
Patent Information
- Application Number
- CN202510956165.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-07-11
- Publication Date
- 2025-08-12
- Estimated Expiration
- 2045-07-11
AI Technical Summary
Existing thermoplastic elastomer-based foamed composite materials are prone to shrink during the foaming process, resulting in dimensional accuracy and appearance quality problems. The residue of chemical foaming agents affects product performance and safety, and it is difficult for physical foaming agents to achieve continuous production, which limits large-scale industrial applications.
The thermoplastic elastomer-based foaming composite material is prepared by a continuous extrusion process of a double-step screw extruder by using a composite foaming agent. The dispersion of conductive functional filler is improved by combining a photoinitiator and a cell stabilizer, and curing by electron radiation cross-linking to form a uniform conductive network and a stable cell structure.
It has realized a thermoplastic elastomer-based foamed composite material with excellent conductivity and electromagnetic shielding properties. The production process is continuous and stable, suitable for industrial scale production, with high product performance consistency and safety, and is suitable for aerospace, electronic equipment and other fields.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermoplastic elastomer-based electromagnetic shielding foam materials and relates to a thermoplastic elastomer-based foam composite material with excellent electrical conductivity and electromagnetic shielding properties and a preparation method thereof. Background Art
[0002] As a communication medium, electromagnetic waves have brought many benefits to the development of electronic technology and industry, but they also inevitably pose numerous safety risks, such as affecting the normal operation of various military and civilian electronic equipment, and even more seriously, harming people's health. The preparation of high-performance electromagnetic shielding materials is the main way to effectively prevent the propagation and diffusion of electromagnetic wave radiation. Currently, electromagnetic shielding materials mainly include metal materials, ferromagnetic materials, and conductive polymer composites (CPC). Among them, CPC has attracted much attention and is widely used in the preparation of electromagnetic shielding materials due to its advantages such as light weight, good flexibility, good corrosion resistance, and low processing cost. Thermoplastic elastomers are a preferred matrix material for preparing CPC.
[0003] Thermoplastic elastomer (TPE)-based CPC foam material is a novel functional material prepared by foaming a thermoplastic elastomer (TPE) matrix with conductive fillers. Its low density and lightweight properties make it an effective way to reduce structural weight and energy consumption in fields such as aerospace and automotive manufacturing. It not only inherits the flexibility of TPE and can recover its original shape after significant deformation, making it suitable for a variety of soft and elastic components such as cushioning and seals in electronic devices, but also the added conductive fillers form a conductive network within the matrix that reflects, absorbs, and dissipates electromagnetic waves, effectively blocking their propagation and providing reliable electromagnetic shielding for electronic devices, preventing signal interference and information leakage. It has broad application prospects in fields such as 5G communications and consumer electronics. Due to the properties of TPE, it can be formed using a variety of processing methods, such as extrusion, injection, and blow molding, offering high processing efficiency and short cycle times, making it easy to implement on a large scale. By adjusting the formulation and process parameters, the expansion ratio, cell structure, and performance can be flexibly controlled to meet the needs of different application scenarios. However, during the foaming process, the escape of gas and the cooling shrinkage of the polymer melt can easily lead to shrinkage of the material, affecting the dimensional accuracy and appearance quality of the product. In particular, for large or complex-shaped products, the shrinkage problem is more prominent and needs to be controlled by appropriate measures, such as optimizing the formula, adjusting the foaming process parameters, etc. CN118725282A discloses a thermoplastic polyether ester elastomer with strong microwave absorption and electromagnetic shielding in a wide band and a preparation method thereof. The elastomer involves a combination of one-dimensional conductive material liquid metal, high dielectric constant MXenes and its derivatives, and rare earth magnetic materials and their oxides. Although the electromagnetic shielding effect can be enhanced, the cost is relatively high. A multi-layer spatial structure shielding layer is used to form multiple heterogeneous interfaces, so that the electromagnetic interference field forms eddy currents in the shielding body and generates reflections at the interface between the shielding body and the protected space, thereby greatly weakening the field strength of the interference field in the protected space and curbing the influence of high-frequency electromagnetic fields to achieve the shielding effect. However, it adopts autoclave foaming, and the preparation process is relatively complicated, which is not suitable for industrial continuous production; CN115260735B discloses a wave-absorbing thermoplastic elastomer foam material and a preparation method thereof, which is made of thermoplastic resin, wave-absorbing powder, and additives. The wave-absorbing powder is used as a reinforcing phase and is added to the matrix under the action of a foaming additive, a cell regulator, and a plasticizer. After foaming and molding, the tensile strength, bending strength, and compressive strength of the foam are greatly improved, which is conducive to application in aviation, aerospace, trains, ships and other fields. However, the foaming additive used in this invention is mainly a chemical foaming agent, which is not conducive to cost reduction and environmental protection.
[0004] Current research on thermoplastic elastomer-based foamed composites reveals that their preparation methods primarily rely on chemical foaming or physical foaming (primarily physical intermittent foaming). Chemical foaming agents inevitably leave residues in the finished product during the foam preparation process, impacting product performance and safety. Intermittent foaming, on the other hand, is difficult to achieve continuous production, making it difficult to ensure consistent and stable product quality, impacting subsequent processing and use. This not only reduces production efficiency but also increases production costs, limiting its application in large-scale industrial production. While physical foaming agents are often supercritical carbon dioxide or nitrogen, while environmentally friendly, the resulting foams can easily shrink. Therefore, the choice of foaming agent in the preparation of polymer foam materials directly influences the final foam's pore structure, leading to performance differences.
[0005] Based on this, the present invention adopts a composite foaming agent to continuously extrusion foam to prepare a thermoplastic elastomer-based foamed composite material with good mechanical properties, excellent electromagnetic shielding properties and conductive properties, which is of great significance for meeting the demand for electromagnetic shielding materials in modern electronic equipment, aerospace and other fields. Summary of the Invention
[0006] One objective of the present invention is to provide a novel thermoplastic elastomer-based foamed composite material exhibiting good mechanical properties, excellent electromagnetic shielding performance, electrical conductivity, and safety. Specifically, the foamed material is prepared by melt blending and continuous extrusion using a thermoplastic elastomer resin, a conductive functional filler, a coupling agent, a photoinitiator, a cell stabilizer, and a foaming agent as primary raw materials. This foamed material can be used in electronic equipment, communications equipment, transportation, aerospace, and medical devices.
[0007] Another object of the present invention is to provide a method for preparing the thermoplastic elastomer-based foamed composite material, wherein the production process is highly continuous and stable, the production process is safe and has no environmental pollution, and is suitable for industrial-scale production.
[0008] To achieve the above-mentioned purpose, the present invention provides a foamed composite material, which is mainly a thermoplastic elastomer-based foamed composite material prepared by continuous extrusion foaming of a composite foaming agent. Specifically, the foamed composite material is prepared by extruding and foaming the following components after being fully mixed in an extruder: 100 parts by weight of thermoplastic elastomer resin; 0.8-8 parts by weight of conductive functional filler; 0.1-10 parts by weight of coupling agent; 0.1-10 parts by weight of photoinitiator; 0.1-10 parts by weight of cell stabilizer; 0.2-8 parts by weight of composite foaming agent; In the thermoplastic elastomer-based foam composite material provided by the present invention, the thermoplastic elastomer resin is one or more of ethylene-vinyl acetate copolymer (EVA), polyolefin elastomer (POE), nylon elastomer (TPAE), polyurethane elastomer (TPU), thermoplastic vulcanizate (TPV), thermoplastic polyester elastomer (TPEE), and styrene block copolymer-type thermoplastic elastomers; the conductive functional filler is one or more of carbon nanotubes (CNTs), carbon black, graphene, and carbon fibers, or a mixture thereof with one or more of nano-ferrosoferric oxide, nano-silver particles, and copper powder, preferably a composite of multiple conductive fillers.
[0009] According to a specific embodiment of the present invention, in the thermoplastic elastomer-based foamed composite material provided by the present invention, the composite foaming agent is preferably composed of 0 to 3 parts by weight of an air foaming agent, 0.2 to 2 parts by weight of a supercritical carbon dioxide foaming agent, and 0 to 3 parts by weight of a supercritical nitrogen foaming agent. More preferably, the air foaming agent in the composite foaming agent is not 0; the total amount of the composite foaming agent is controlled at 0.2 to 8 parts by weight, preferably 0.5 to 3 parts by weight. The present invention adopts a double-stage screw extruder, especially a twin-screw extruder in series with a single-screw extruder for continuous extrusion foaming process. The mixed extrusion equipment used has a strong shearing effect so that the materials can be fully mixed and dispersed. The extrusion foaming temperature is 80 to 120°C, the extrusion foaming pressure is 5 to 20 MPa, and the extrusion foaming time is 8 to 20 min. The temperature, pressure, and time of the foaming are important factors affecting gas diffusion, thereby affecting the final cell morphology.
[0010] In the present invention, the weight parts are based on the total amount of the thermoplastic elastomer resin being 100 weight parts. Unless otherwise specified, the ratios and contents in the present invention are all weight ratios and contents.
[0011] In the thermoplastic elastomer-based foamed composite material provided by the present invention, the conductive functional fillers need to be treated and modified with a coupling agent before being put into the extruder. The main function of these conductive functional fillers is to build a complete conductive network inside the matrix material, thereby improving the conductivity and electromagnetic shielding performance. In addition, these conductive functional fillers can also play a role in heterogeneous nucleation, thereby increasing the cell density.
[0012] In the thermoplastic elastomer-based foamed composite material provided herein, the coupling agent may be one or more of KH550, KH560, KH570, KH171, A-172, and A-174. The coupling agent primarily functions by dry-blending with the conductive functional filler to improve its dispersibility and interfacial compatibility in the matrix.
[0013] In the thermoplastic elastomer-based foamed composite material provided by the present invention, the photosensitive initiator is mainly used for cross-linking and curing after extrusion foaming. By rapidly absorbing electron radiation energy and converting it into chemical energy, it produces active centers that initiate cross-linking reactions, such as free radicals or cations, thereby greatly accelerating the cross-linking and curing rate of the thermoplastic elastomer, shortening the curing time, and improving production efficiency.
[0014] In the thermoplastic elastomer-based foamed composite material provided herein, the cell stabilizer is primarily used to increase the strength of the cell walls, prevent cell wall rupture, and stabilize the cells. The cell stabilizer employed may be one or a mixture of glycerol fatty acid ester cell stabilizers, propylene glycol fatty acid ester cell stabilizers, and isooctyl alcohol fatty acid ester cell stabilizers. Preferred cell stabilizers are glycerol fatty acid ester cell stabilizers, such as glyceryl monostearate (GMS). The preferred amount of the cell stabilizer is 0.1 to 2 parts by weight.
[0015] The thermoplastic elastomer-based foamed composite material provided by the present invention is prepared by continuously extruding and foaming the above raw materials through a double-stage screw extruder.
[0016] In another aspect, the present invention provides a method for preparing the thermoplastic elastomer-based foamed composite material, the method comprising the following steps: S1. vacuum drying the thermoplastic elastomer resin and the conductive functional filler; S2. Stirring the conductive functional filler and the coupling agent in a high-speed stirrer for dry mixing to obtain a pretreated conductive functional filler; S3, then uniformly mixing the thermoplastic elastomer resin, the pretreated conductive functional filler, the photoinitiator, and the cell stabilizer to obtain a mixed material; S4, adding the above-mentioned mixed material into a twin-screw extruder, injecting the composite foaming agent into the extruder at the same time, and after sufficient mixing, extruding and foaming molding; S5. Finally, the foamed sample is quickly subjected to electron radiation treatment to promote cross-linking and curing to obtain the foamed composite material.
[0017] In the process of preparing the foamed composite material of the present invention, the continuous extrusion foaming extruder used is a twin-stage screw extruder, which is a twin-screw extruder connected in series with a single-screw extruder or a single-screw extruder connected in series with a single-screw extruder, preferably a twin-screw extruder connected in series with a single-screw extruder. According to a preferred embodiment of the present invention, the processing temperature of the present invention is controlled to be 80-120°C, the extrusion foaming pressure is 5-20 MPa, and the extrusion foaming time is 8-20 minutes.
[0018] The die used in the extruder is an annular or sheet-shaped die that is electrically heated or oil-bathed for temperature control. Furthermore, a foaming stabilization device can be installed at the rear of the die to control melt uniformity. In the present invention, all raw materials are commercially available, and all mechanical equipment used is state-of-the-art. Steps not specifically described in the process described herein can be performed according to conventional procedures in the art.
[0019] The present invention mainly combines the components in a certain proportion to prepare a thermoplastic elastomer-based foamed composite material with excellent electrical conductivity and electromagnetic shielding properties, wherein the composite foaming agent used is a physical foaming agent, which has no effect on the performance and safety of the product. Utilizing the formula of the present invention, a thermoplastic elastomer-based foamed composite material with good mechanical properties, excellent electrical conductivity and electromagnetic shielding properties can be prepared, and the production process is highly continuous and stable, safe and has no environmental pollution, and is suitable for industrial-scale production. The thermoplastic elastomer-based foamed composite material product of the present invention has excellent comprehensive evaluation of foaming ratio, pore size distribution and mechanical properties, and the foaming ratio can be determined according to the application requirements of different fields, generally less than 10 times. The thermoplastic elastomer-based foamed composite material of the present invention can be used to process various types of sheets, plates, pipes and other products in order to be applied to aerospace, electronic equipment manufacturing, military and other fields.
[0020] In summary, the present invention provides a method for preparing a thermoplastic elastomer-based foamed composite material having good mechanical properties, excellent electrical conductivity and electromagnetic shielding properties. Compared with the prior art, the present invention has the following beneficial effects and advantages: 1. The present invention uses the method to prepare a thermoplastic elastomer foam material with excellent electrical conductivity, electromagnetic shielding and other properties on the basis of adding a relatively small amount of conductive functional filler. Specifically, it can achieve an electromagnetic shielding effectiveness of ≥65dB and an electrical conductivity of ≥75 S / cm with ≤10 parts of conductive functional filler, breaking through the limitation of the amount of conductive functional filler used in traditional CPC foam materials.
[0021] 2. Pre-treating the conductive filler with a coupling agent improves the uneven dispersion of the conductive filler in thermoplastic elastomer-based foam materials. The organic functional groups on the coupling agent can chemically react or physically adsorb with the surface of the conductive filler, forming a coating that reduces the filler's surface energy and makes it easier to disperse in the matrix. This improves filler utilization and the uniformity of the composite material's performance, thereby enhancing conductivity. For example, the vinyl group in the vinyl coupling agent molecule can copolymerize with the double bonds in the resin matrix, while the functional group at the other end can bind to the surface of the conductive filler, forming a chemically bonded bridge between the conductive filler and the matrix. This significantly enhances the interfacial bonding between the two, helps overcome stress concentration and interfacial debonding caused by poor interfacial compatibility between the filler and the matrix, and improves the mechanical properties of the composite material, such as tensile strength, flexural strength, and impact strength.
[0022] 3. The physical foaming agent used has no effect on the product's performance and safety, and improves the shrinkage problem of thermoplastic elastomer-based foam materials. Supercritical carbon dioxide has a high solubility and diffusion rate in polymers, which can increase the number of cells and reduce cell size, thereby improving the cell density and uniformity of the foamed material, making the material more elastic and less dense. Supercritical nitrogen is chemically stable, non-toxic, safe to use, and has strong solubility and diffusion ability in polymers. It is easy to control, forming a more uniform cell structure and high cell density during foaming, giving the foamed material better mechanical properties and dimensional stability. Air, as a foaming agent, is low-cost and easily available, relatively simple to operate during the foaming process, and can play a role in resisting shrinkage of thermoplastic elastomer foam.
[0023] 4. The thermoplastic elastomer-based foamed composite material prepared by continuous extrusion foaming using a two-stage screw extruder and then cross-linking and curing with electron radiation has good mechanical properties, excellent electrical conductivity and electromagnetic shielding properties. The production process is highly continuous and stable, safe and environmentally pollution-free, suitable for industrial-scale production, and the product has excellent comprehensive evaluation of foaming ratio, pore size distribution, electrical conductivity, electromagnetic shielding performance and mechanical properties. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention and are not intended to limit the present invention.
[0025] All test instruments and reagents are commercially available and can be purchased through commercial channels.
[0026] The preparation process of the thermoplastic elastomer-based foamed composite materials of Comparative Examples 1-10 and Examples 11-12 is as follows: S1. Drying the thermoplastic elastomer resin and the conductive functional filler in vacuum at 60° C. for 8 h; S2. Dry-mixing the conductive functional filler and the coupling agent in a high-speed mixer, i.e., pre-treating the conductive functional filler; S3, then uniformly mixing the thermoplastic elastomer resin, the pretreated conductive functional filler, the photoinitiator, and the cell stabilizer to obtain a mixed material; S4. The mixed material is then added to a twin-screw extruder, and the composite foaming agent is simultaneously injected into the extruder (air, supercritical carbon dioxide, and supercritical nitrogen are pumped into the air inlet of the extruder by a gas pressure pump at a rate of 0.6 kg / h, and the gas mass is converted by volume). Supercritical carbon dioxide or supercritical nitrogen is injected in the compression section, and air is injected in the homogenization section. In a second-stage twin-screw tandem single-screw extruder, the extruder conditions are set as follows: extrusion temperature of 100° C., extrusion foaming pressure of 15 MPa, and extrusion foaming time of 10 min. After sufficient mixing, extrusion foaming molding is performed; S5. Finally, the foamed sample is quickly subjected to electron radiation treatment, with an electron beam irradiation dose of 60 kGy and an irradiation time of 10 s at room temperature to promote cross-linking and curing to obtain the thermoplastic elastomer-based foamed composite material.
[0027] Effect test The foam density was measured using a density balance to calculate the expansion ratio; the compression rebound rate and tensile strength of the foam were measured using a universal testing machine; the electrical conductivity of the foam was measured using a four-probe method; and the electromagnetic shielding performance of the foam was measured using an electromagnetic shielding vector meter. Table 1 compares the components and test results of the thermoplastic elastomer-based foam composite materials prepared in the comparative examples and examples.
[0028] Table 1 Components and test results of Comparative Examples 1-10 and Examples 11-12
[0029] Note: The composite foaming agent in the table is a mixture of supercritical carbon dioxide and air at a weight ratio of 1:2, and the composite conductive functional filler is a mixture of CNTs and graphene at a weight ratio of 1:1.
[0030] Compatibility has an important influence on thermoplastic elastomer-based foaming. From Comparative Examples 1, 2, 3, and 4, it can be found that since POE and EVA are both polyolefin polymers, their molecular structures have certain similarities, making POE more compatible with the EVA matrix, forming a more uniform blending system, which can effectively improve foaming performance, compression rebound rate, and tensile strength. In contrast, the molecular structures of TPAE and TPU are quite different from those of EVA, and their compatibility with EVA is relatively poor, resulting in the possible presence of phase separation in the blending system, affecting the overall performance of the material.
[0031] The composition of the blowing agent also significantly impacts the material's performance. Comparative Examples 2 and 5 show that a single-component blowing agent (supercritical carbon dioxide) can achieve high expansion ratios but results in uneven pores, low tensile strength, poor compression rebound, rapid gas release, and prone to cell collapse. A composite blowing agent (supercritical carbon dioxide + air) achieves moderate expansion ratios, uniform and fine pores, high tensile strength, and excellent rebound resilience. Furthermore, the combination of air and slowed diffusion results in a more stable process.
[0032] CNTs, as a conductive functional filler with excellent electrical conductivity and mechanical properties, have a significant effect on the performance of EVA thermoplastic elastomer-based foam materials. The addition of an appropriate amount of CNTs can act as a heterogeneous nucleation point, which helps to increase the foaming ratio, promote the formation of pores, and make the pore structure more uniform; the high elastic modulus of CNTs can improve the resilience of the foam material, so that it can recover to its original shape faster after compression, thereby improving the compression rebound rate; the interaction between CNTs and the polymer matrix can enhance the mechanical properties of the material and improve the tensile strength. In addition, the excellent electrical conductivity of CNTs can form a conductive network in the polymer matrix, thereby significantly improving the electrical conductivity of the material. At the same time, CNTs can reflect and absorb electromagnetic waves, thereby improving the electromagnetic shielding effectiveness of the foam material. It can be seen from Comparative Examples 5, 6, and 7 that the conductive filler modified with a coupling agent has a more significant effect on performance improvement.
[0033] It can be seen from Comparative Examples 8 and 9 that when CNTs are compounded and mixed with other conductive fillers, the electromagnetic shielding effect can be further enhanced, wherein the one-dimensional nanostructure of CNTs and the two-dimensional lamellar structure of graphene are combined to form a more complete conductive network, thereby improving the conductive properties and electromagnetic shielding effect of the material; in addition, according to Comparative Examples 9 and 10, increasing the amount of compounded conductive functional fillers also has an important influence on improving the various properties of thermoplastic elastomer-based foamed composite materials.
[0034] The addition of a photoinitiator to electron radiation crosslinking significantly improves tensile strength, compression rebound, and cell uniformity, although it slightly reduces the expansion ratio. Furthermore, the addition of a cell stabilizer, GMS, further enhances cell stability. Comparing the comparative examples and examples in Table 1, Example 12 is the optimal formulation, offering the best overall performance. During the electron radiation treatment after extrusion foaming, the photoinitiator in this invention rapidly absorbs the electron radiation energy and converts it into chemical energy, generating active centers that initiate the crosslinking reaction, thereby significantly accelerating the crosslinking and curing rate of the thermoplastic elastomer. This rapid crosslinking and curing process stabilizes the material's cell structure, preventing cell collapse and excessive expansion, and ensuring the material's dimensional accuracy and appearance quality. The vinyl acetate (VA) units in the EVA molecular chain contain highly reactive tertiary hydrogen atoms with low atomic bond energies. Under the action of the photoinitiator and electron radiation, they readily dehydrogenate to form carbon-centered free radicals, significantly accelerating the crosslinking reaction. Furthermore, the polar groups in VA enhance the initiator's compatibility with the matrix and its energy absorption efficiency. In contrast, pure polyolefins (such as POE) contain only secondary and primary hydrogen atoms with higher bond energies, resulting in slower crosslinking kinetics. Furthermore, electron radiation treatment not only promotes bonding between the matrix and the conductive functional filler but also enhances the matrix's crosslink density, improving the material's mechanical properties and thermal stability, thereby providing a strong foundation for achieving excellent electrical conductivity and electromagnetic shielding performance.
[0035] In addition, it should be noted that in the method of the present invention, different photosensitive initiators are suitable for different thermoplastic elastomer matrices, specifically: ① For EVA, acylphosphine oxides or benzophenone photoinitiators are usually selected. Benzophenones are excited after absorbing ultraviolet light, transitioning from the ground state to the excited state. The excited benzophenone molecules generate free radicals through energy transfer or electron-donating groups capturing hydrogen atoms. The free radicals trigger cross-linking reactions at the double bonds in the EVA molecular chain or the reactive sites in the vinyl acetate unit, forming a three-dimensional network structure between the EVA molecular chains, improving the material's cross-linking density and thermal stability.
[0036] ② For POE, acylphosphine oxide photoinitiators are generally used. When acylphosphine oxides are exposed to ultraviolet light, double bonds or specific groups within the molecule absorb light energy and become excited, undergoing homolytic cleavage or generating free radicals through other pathways. These free radicals can initiate crosslinking and curing of the double bonds within the POE molecular chain. The presence of a small number of double bonds in POE improves material performance after crosslinking.
[0037] ③ For nylon elastomer (TPAE), choose iodonium salt photoinitiator. TPAE contains amide groups with lone pairs of electrons, which are suitable for cationic initiation. Ionium salts generate super acid (H + ), initiates the ring-opening polymerization of the amide group, and the generated HX protonates the amide group, triggering the ring-opening cross-linking.
[0038] ④ For polyurethane elastomers (TPU), choose aromatic diazonium salts as photoinitiators. TPU contains carbamate groups. Aromatic diazonium salts release nitrogen upon photolysis and generate carbon cations, which can initiate cationic polymerization of polyester segments and further cross-linking and curing.
[0039] Nitrobenzoxadiazole photoinitiators are often used for thermoplastic vulcanizates (TPVs). The rubber phase in TPVs contains allylic hydrogen atoms, resulting in low bond energy. Under ultraviolet light, electron-withdrawing groups such as nitro groups in the nitroxadiazole molecular structure absorb light and become excited. The excited initiator then abstracts hydrogen atoms from the allylic positions, generating free radicals in the rubber macromolecules that crosslink and form a crosslinked network.
[0040] ⑥ For thermoplastic polyester elastomer (TPEE), select benzophenone photoinitiators and amine co-initiators. Because TPEE contains ester and ether bonds, but no easily activated hydrogen, benzophenone (BP) needs to capture α-hydrogen from the amine co-initiator in the excited state to generate aminoalkyl free radicals to initiate crosslinking, that is, the aminoalkyl free radicals attack the ether bond or ester group of TPEE to initiate the crosslinking reaction.
[0041] ⑦ For styrene block copolymer thermoplastic elastomers, azo photoinitiators are more suitable. Styrene units contain benzylic hydrogen atoms, which are easily abstracted by free radicals. Upon photolysis, azo initiators (such as AIBN) generate cyanoisopropyl radicals that abstract the benzylic hydrogen atoms, forming a crosslinked network.
[0042] In summary, it can be seen that the present invention works together through the selection and regulation of components and ratios, as well as the optimization of the preparation process, by adopting multiple mechanisms, including: ① filler dispersion and interface effect: coupling agent pretreatment, forming an organic coating layer on the filler surface, reducing agglomeration; ② compound filler synergy: constructing a multidimensional conductive network; ③ pore structure optimization conduction path: composite foaming agent forms uniform micropores; ④ conductive fillers are distributed on the pore wall to increase the electromagnetic wave reflection / absorption interface; ⑤ radiation cross-linking stabilizes the pore structure: electron beam curing causes the pore wall to quickly cross-link, prevent collapse, and ensure the stability of the filler network; ultimately, the preparation of foamed composite materials with excellent comprehensive performance based on the application of a small amount of conductive functional fillers is achieved, especially with very excellent electrical conductivity and electromagnetic shielding performance.
[0043] The above description is merely a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Therefore, any modifications, equivalent changes, and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention shall still fall within the scope of the technical solution of the present invention.
Claims
1. A thermoplastic elastomer-based foamed composite material with excellent electrical conductivity and electromagnetic shielding properties, characterized in that: The foam composite material is prepared by fully mixing the following components in an extruder and then extruding and foaming: 100 parts by weight of thermoplastic elastomer resin; 0.8-8 parts by weight of conductive functional filler; 0.1-10 parts by weight of coupling agent; 0.1-10 parts by weight of photoinitiator; 0.1-10 parts by weight of cell stabilizer; 0.2-8 parts by weight of composite foaming agent; The conductive functional filler is one or more of carbon nanotubes, carbon black, graphene, and carbon fibers, or a mixture thereof with one or more of nano-ferroferric oxide, nano-silver particles, and copper powder. The composite foaming agent is composed of 0 to 3 parts by weight of an air foaming agent, 0.2 to 2 parts by weight of a supercritical carbon dioxide foaming agent, and 0 to 3 parts by weight of a supercritical nitrogen foaming agent, and the air foaming agent is not 0.
2. The foamed composite material according to claim 1, characterized in that The thermoplastic elastomer resin is one or more of ethylene-vinyl acetate copolymer, polyolefin elastomer, nylon elastomer, polyurethane elastomer, thermoplastic vulcanized rubber, thermoplastic polyester elastomer, and styrene block copolymer thermoplastic elastomer.
3. The foamed composite material according to claim 1, characterized in that The conductive functional filler needs to be pretreated before being put into the extruder. The pretreatment is to use the coupling agent to dry blend with the conductive functional filler to improve the dispersibility and interface compatibility of the conductive functional filler in the matrix. The coupling agent is one or more of KH550, KH560, KH570, KH171, A-172, and A-174.
4. The foamed composite material according to claim 1, characterized in that The photoinitiator is one or more of benzophenones, acylphosphine oxides, aromatic diazonium salts, nitrobenzoxadiazoles, iodonium salts, and azo groups.
5. The foamed composite material according to claim 1, characterized in that The cell stabilizer is one or a mixture of glycerol fatty acid ester cell stabilizers, propylene glycol fatty acid ester cell stabilizers and isooctyl alcohol fatty acid ester cell stabilizers.
6. The foamed composite material according to claim 1, characterized in that The extruder is a double-stage screw extruder, which is a double-screw extruder connected in series with a single-screw extruder or a single-screw extruder connected in series with a single-screw extruder.
7. The method for preparing the foamed composite material according to claim 1, characterized in that: The following steps are involved: S1. vacuum drying the thermoplastic elastomer resin and the conductive functional filler; S2. Stirring the conductive functional filler and the coupling agent in a high-speed stirrer for dry mixing to obtain a pretreated conductive functional filler; S3, then uniformly mixing the thermoplastic elastomer resin, the pretreated conductive functional filler, the photoinitiator, and the cell stabilizer to obtain a mixed material; S4, adding the above-mentioned mixed material into a twin-screw extruder, injecting the composite foaming agent into the extruder at the same time, and after sufficient mixing, extruding and foaming molding; S5. Finally, the foamed sample is quickly subjected to electron radiation treatment to promote cross-linking and curing to obtain the foamed composite material.
8. The method according to claim 7, characterized in that In a first-stage extruder of a twin-stage screw extruder, all the mixed materials are melt-blended, and the processing temperature is controlled at 80-120° C.; after uniform mixing, the materials are conveyed to a second-stage extruder, and the extrusion foaming temperature is controlled at 80-120° C., the extrusion foaming pressure is 5-20 MPa, and the extrusion foaming time is 8-20 minutes, for continuous extrusion foaming; and the foamed product is rapidly subjected to electron radiation treatment, with an electron beam irradiation dose of 40-80 kGy and an irradiation time of 5-30 seconds at room temperature, to promote cross-linking and curing, thereby obtaining the thermoplastic elastomer-based foamed composite material.
Citation Information
Patent Citations
A microwave-absorbing thermoplastic elastomer foam material and preparation method thereof
CN115260735B
Thermoplastic polyether ester elastomer with broadband microwave strong absorption electromagnetic shielding and preparation method thereof
CN118725282A
Microcellular foam conductive thermoplastic elastomer material having pressure-sensitive characteristic, and production method thereof
CN107629443A
Method for synergistically improving polystyrene supercritical foaming performance by multi-nanometer fillers
CN108384134A
Ethylene-vinyl acetate copolymer foaming material and preparation method thereof
CN109734992A
Cited By
Microporous high-magnification polyethersulfone foam material for electromagnetic shielding and mould pressing foaming preparation method of microporous high-magnification polyethersulfone foam material
CN120988477A
Microporous high-void polyether sulfone foam for electromagnetic shielding and its compression molding foaming preparation method
CN120988477B