Electrochemical-ferrate combined process iron mud-based environmental functional material as well as preparation method and application thereof
By transforming the iron sludge produced by the electrochemical-ferrate combined process into an environmentally functional material with both oxidation and adsorption functions, the problem of iron sludge being regarded as hazardous waste has been solved, realizing resource utilization and efficient pollutant removal, and reducing operating costs.
Patent Information
- Application Number
- CN202610210523.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-02-13
- Publication Date
- 2026-04-28
AI Technical Summary
Iron sludge produced by the electrochemical-ferrate combined process is considered hazardous waste, causing environmental risks and resource waste. Moreover, the efficiency of single electrochemical oxidation is limited and it is difficult to completely mineralize stubborn pollutants.
Iron sludge produced by the electrochemical-ferrate combined process is transformed into an environmental functional material with an amorphous nanofibrillated structure through the synergistic effect of electrochemical oxidation and ferrate. The material utilizes the dual-functionality of oxidation and adsorption of the intermediate valence iron active sites to remove pollutants such as arsenic, antimony and phosphate from water.
It realizes the resource utilization of iron sludge, reduces the overall operating cost of the process, and the material can efficiently remove a variety of anionic pollutants within a wide pH range, simplifying the treatment process and possessing good environmental and economic benefits.
Smart Images

Figure CN121927581A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of environmental functional materials and water treatment technology, specifically relating to an iron mud-based environmental functional material prepared by an electrochemical-ferrate combined process, its preparation method, and its application. Background Technology
[0002] Electrochemical advanced oxidation technology generates active species in situ through electrode reactions, effectively degrading recalcitrant organic pollutants in water and has become an important means of advanced industrial wastewater treatment. However, single electrochemical oxidation has limitations such as limited current efficiency and incomplete mineralization of certain stubborn pollutants. Combining it with ferrates can exert a synergistic oxidation effect, significantly improving treatment efficiency.
[0003] The electrochemical-ferrate combined process inevitably generates iron sludge during operation. This iron sludge originates from the reduction products of ferrate, but its formation environment differs from that of conventional systems where ferrate is added alone. Its potential activity is not recognized, and it is currently treated as hazardous waste and disposed of in landfills, increasing environmental risks and compliance costs, as well as wasting iron resources. In the electrochemical system, the BDD anode continuously generates strong oxidizing species such as hydroxyl radicals, while the cathode undergoes a reduction reaction that may generate H₂O₂. Simultaneously, an electric field and a local pH gradient exist within the system. Under this unique environment, the Fe(VI)→Fe(V)→Fe(IV)→Fe(III) reduction pathway of ferrate may be modulated, allowing intermediate valence iron to be retained in the iron sludge or forming an active structure different from conventional trivalent iron oxides.
[0004] Currently, this type of iron sludge is typically disposed of as waste, and its unique composition and structure have not yet received sufficient attention. In fact, iron-based materials containing intermediate-valence iron or special active sites often exhibit superior oxidation activity and adsorption performance compared to conventional trivalent iron oxides, demonstrating potentially high-efficiency removal capabilities for typical pollutants in water, such as arsenic, antimony, and phosphates. Converting the iron sludge produced by the electrochemical-ferrate combined process into environmentally functional materials for utilization can both achieve waste-to-waste treatment and reduce the overall operating costs of the combined process. Summary of the Invention
[0005] This invention addresses the problem of iron sludge generated by the electrochemical-ferrate combined process being disposed of as waste and a waste of resources. It provides a method for converting this iron sludge into an environmentally functional material and its application in water pollution control. This invention discloses an iron sludge-based environmentally functional material based on the synergistic effect of electrochemical-ferrate processes, its preparation method, and its application. The material originates from iron sludge byproducts generated during the co-treatment of wastewater by electrochemical oxidation and ferrate. Under the synergistic effect of an electrochemical field (such as hydroxyl radicals and electric field) and ferrate, the formation mechanism of this iron sludge differs from conventional chemical precipitation. The resulting material possesses an amorphous or low-crystallinity nanofibrillated structure, high specific surface area, and exhibits unique oxidation-adsorption dual-functionality. The material of this invention can efficiently remove anionic pollutants such as arsenic (including As(III) and As(V)), antimony (including Sb(III) and Sb(V)), and phosphates from water, especially through an "in-situ oxidation-simultaneous adsorption" mechanism to deeply purify highly toxic As(III) and Sb(III). This invention transforms solid waste generated from advanced oxidation processes into high-performance adsorbent materials, realizing the resource utilization of "waste treatment," effectively reducing the overall operating cost of the process, and demonstrating good environmental and economic benefits and application prospects.
[0006] An electrochemical-ferrate combined process for iron sludge-based environmental functional material is described. The material uses a boron-doped diamond electrode (BDD) or a metal oxide-coated titanium electrode as the anode and one of Ti plate, stainless steel, or graphite as the cathode. The iron sludge generated during the co-treatment of wastewater by the electrochemical system and ferrate is used to obtain the iron sludge-based environmental functional material.
[0007] The iron sludge contains intermediate valence iron active sites and has dual oxidation-adsorption properties.
[0008] A method for preparing an iron mud-based environmental functional material includes the following steps: Step (1) Electrochemical oxidation uses one of boron-doped diamond electrode or metal oxide coated titanium electrode as the anode, and one of Ti plate, stainless steel or graphite as the cathode. Ferrate is added to the wastewater to be treated to carry out electrochemical-ferrate combined oxidation treatment. After the reaction in step (2) is completed, collect the solid residue and separate the solid and liquid phases. Step (3) Wash and dry the solid residue to obtain iron mud-based environmental functional materials.
[0009] This invention also provides the application of the above-mentioned iron mud-based environmental functional materials in water pollution control, including but not limited to: (1) Used to remove arsenic or antimony from water; (2) Used to remove phosphates from water.
[0010] The technical solution of this invention has the following advantages compared with the prior art: 1. This invention transforms iron sludge, a byproduct of the electrochemical-ferrate combined process, into environmentally functional materials, thereby achieving waste treatment and reducing the overall operating cost of the process.
[0011] 2. In an environment where electrochemical oxidation and ferrates work together, the iron sludge byproducts produced have a unique amorphous nanofibrillated structure and high specific surface area, maintaining the strong adsorption capacity of iron (hydrogen) oxides for anionic pollutants.
[0012] 3. The iron mud-based environmental functional material prepared by this invention has both oxidation and adsorption functions. It can achieve "one-step" oxidation and adsorption of pollutants such as As(III) and Sb(III) without the need for additional pre-oxidation steps, thus simplifying the process.
[0013] 4. The iron mud-based environmental functional material prepared by this invention has a good removal effect on a variety of anionic pollutants such as arsenic, antimony, and phosphate. It maintains a stable and efficient removal capacity over a wide pH range and is suitable for the treatment of complex actual water bodies.
[0014] 5. The preparation method of this invention is simple, requires no complicated process, has a stable source of materials, and has good prospects for industrial application. Attached Figure Description
[0015] Figure 1 This is a morphological image of iron sludge produced after electrochemical activation of ferrate, observed using a scanning electron microscope (SEM).
[0016] Figure 2 This is an X-ray diffraction (XRD) diagram of the crystal structure of iron sludge produced after electrochemical activation of ferrate. Detailed Implementation
[0017] An electrochemical-ferrate combined process for iron sludge-based environmental functional material is disclosed. The material uses a boron-doped diamond electrode (BDD) or a metal oxide-coated titanium electrode as the anode and one of a Ti plate, stainless steel, or graphite as the cathode. The iron sludge produced during the electrochemical treatment of wastewater with ferrate is used to obtain the iron sludge-based environmental functional material. The iron sludge contains intermediate valence iron active sites and has oxidation-adsorption dual functional characteristics.
[0018] The iron mud-based environmental functional materials prepared by this invention have an amorphous or low-crystallinity structure and a specific surface area of not less than 100 m². 2 / g.
[0019] The ferrate of the present invention is potassium ferrate or sodium ferrate; the valence state of iron in the iron mud-based environmental functional material includes +3 valence and intermediate valence iron.
[0020] A method for preparing an iron mud-based environmental functional material includes the following steps: Step (1) Electrochemical oxidation uses one of boron-doped diamond electrode or metal oxide coated titanium electrode as the anode, and one of Ti plate, stainless steel or graphite as the cathode. Ferrate is added to the wastewater to be treated to carry out electrochemical-ferrate combined oxidation treatment. After the reaction in step (2) is completed, collect the solid residue and separate the solid and liquid phases. Step (3) Wash and dry the solid residue to obtain iron mud-based environmental functional materials.
[0021] Furthermore, the amount of ferrate added is 1.0-4.0 g / L, calculated as Fe.
[0022] Furthermore, the current density of the electrochemical treatment is 10-40 mA / cm², and the treatment time is 120-180 min.
[0023] Furthermore, the pH of the wastewater needs to be adjusted to above 9.
[0024] Furthermore, the drying method is either forced air drying or vacuum drying, and the drying temperature is 45-60℃.
[0025] Application of an iron mud-based environmental functional material in water pollution control: (1) for removing phosphate ions from water, and (2) for removing arsenic or antimony from water.
[0026] Furthermore, the dosage of the iron mud-based environmental functional material is 0.5-1.0 g / L; the pH during the reaction is 3-12, and the reaction time is 5-20 min.
[0027] This invention discloses an iron sludge-based environmental functional material based on the synergistic effect of electrochemistry and ferrate, its preparation method, and its application. The material originates from iron sludge byproducts generated during the co-treatment of wastewater by electrochemical oxidation and ferrate. Due to the influence of reactive oxygen species, electric field, and local pH gradient in the electrochemical system, the formation process of this iron sludge differs from conventional chemical precipitation. The resulting material possesses a unique amorphous structure with a high specific surface area, endowing it with significant oxidation capacity and achieving synergistic oxidation and adsorption functions. The material of this invention can efficiently remove anionic pollutants such as arsenic (including As(III) and As(V)), antimony (including Sb(III) and Sb(V)), and phosphates from water. This invention transforms solid waste generated by the combined process into a high-performance adsorbent material, realizing the resource utilization of "waste-to-waste" treatment, effectively reducing the overall operating cost of this advanced oxidation process, and demonstrating good environmental and economic benefits and application prospects.
[0028] Example 1: Preparation of iron mud-based materials An electrochemical reactor was constructed using a BDD electrode as the anode and a Ti plate as the cathode, with a distance of 1.0 cm between the electrodes. The reactor contained 0.3 L of simulated wastewater. The pH was adjusted to 9-13, and potassium ferrate (1-4 g / L, calculated as Fe) was added. The power supply was turned on, and the current density at the anode was set to 10-40 mA / cm². 2 Under these conditions, an electrochemical-ferrate combined oxidation process was initiated and the reaction was continued for 120-180 min. After the reaction, the mixture was allowed to stand for 30 min to allow the solid product to settle completely. The precipitate at the bottom of the reactor was collected and washed at least three times with deionized water to remove residual soluble salts and impurities. The washed wet solid was placed in a drying device and dried at 60°C for 6 hours. Finally, the dried block material was ground and passed through a 100-mesh standard sieve to obtain the iron mud-based environmental functional material powder with dual oxidation-adsorption functions. Subsequently, at room temperature, 0.5 g / L of iron mud was added to 20 mg / L of phosphate and stirred for 20 min. The phosphate removal rate in the supernatant was then measured.
[0029] Table 1 Effect of preparation pH on phosphate adsorption performance of materials
[0030] Table 2 Effect of ferrate dosage on phosphate adsorption performance of materials
[0031] Table 3 Effect of current density on phosphate adsorption performance of materials
[0032] Table 4 Effect of reaction time on the phosphate adsorption performance of the material
[0033] As shown in Table 1, the phosphate removal rate of the material gradually increased from 72.54% to 86.92% as the preparation pH increased from 9 to 13. This indicates that a strongly alkaline environment (pH ≥ 11) is conducive to the formation of a highly active iron sludge structure in the electrochemical-ferrate system, which may promote the formation of amorphous iron (hydride) oxides and intermediate valence iron species, thereby significantly enhancing the adsorption performance of the material. When the pH reaches above 12, the performance tends to stabilize.
[0034] As shown in Table 2, when the ferrate dosage (based on Fe) increased from 1 g / L to 4 g / L, the phosphate removal rate increased from 70.44% to 86.78%. This indicates that increasing the ferrate dosage helps to form more abundant surface active sites. However, when the dosage exceeds 3 g / L, the increase in removal rate slows down. Considering both performance and raw material costs, a ferrate dosage of 3–4 g / L is recommended.
[0035] As shown in Table 3, the current density is between 10-40 mA / cm². 2 As the range increases, the removal rate increases from 74.84% to 86.25%. Higher current density is beneficial for enhancing electrochemical activation, promoting the formation of intermediate valence iron, and optimizing the material structure. When the current density is ≥20 mA / cm², the removal rate increases. 2 When the current density is high, the performance improvement is particularly significant, but energy consumption control must be taken into account. Therefore, it is recommended that the current density be preferably 20–40 mA / cm².
[0036] As shown in Table 4, extending the reaction time from 120 min to 180 min only slightly increased the phosphate removal rate from 82.34% to 82.46%, a very small change. This indicates that in the system described, 120 min is sufficient to reach the reaction equilibrium for material formation and transformation, and further extending the time has limited effect on performance improvement. Therefore, controlling the reaction time to around 120 min is sufficient.
[0037] Example 2: Material Characterization 2.1 Morphology and Structure The morphology of the material was observed using scanning electron microscopy (SEM), and the results are as follows: Figure 1 As shown, the iron sludge produced after electrochemical activation of ferrate exhibits a typical amorphous flocculent structure composed of a large number of densely packed, porous fine particles, with a rough and porous surface. This morphology is beneficial for providing abundant surface active sites and material transport channels.
[0038] The crystal structure of the material was analyzed using X-ray diffraction (XRD), and the results are as follows: Figure 2 As shown in the figure, only broad and diffuse peaks are visible in the spectrum, with no sharp crystalline diffraction peaks. This indicates that the main body of the material is an amorphous or very low-crystallinity iron (hydrogen) oxide.
[0039] The specific surface area of the material, determined by BET nitrogen adsorption, was 113.5 m² / g. This high specific surface area further confirms its porous and amorphous structural characteristics, providing an ample interface for pollutant adsorption.
[0040] 2.2 Analysis of Iron in Intermediate Valence States To verify the existence of iron in the intermediate valence state, the PMSO probe method was used to indirectly demonstrate the oxidizing capacity of Fe(IV) / Fe(V) by measuring the ratio of PMSO to PMSO2. Iron sludge was added to a 20 mg / L PMSO solution and reacted with shaking at room temperature and 200 rpm for 20 min. The change in the PMSO / PMSO2 ratio before and after the reaction was measured.
[0041] Table 5. Changes in the proportion of PMSO oxidized to PMSO2 during the reaction process.
[0042] As shown in Table 5, after 20 min of reaction, the PMSO / PMSO2 ratio reached 0.108, indicating that PMSO was partially oxidized. This result demonstrates that the material has a certain oxidizing capacity, indirectly proving the presence of intermediate valence iron active species (Fe(IV) / Fe(V)) in the iron sludge.
[0043] Example 3: Phosphate Removal Experiment Prepare a phosphate-containing simulated wastewater solution with an initial concentration of 20 mg / L. Take 100 mL of the solution and place it in an Erlenmeyer flask. Add 0.3-1.0 g / L of iron mud-based material and adjust the pH to 3-12. Shake the solution at room temperature and 200 rpm for 20 min. After the reaction is complete, filter the solution and determine the phosphate concentration in the filtrate.
[0044] 3.1 Impact of Dosage With a fixed pH of 5 and an initial phosphate concentration of 20 mg / L, the effect of material dosage (0.5-1.0 g / L) on phosphate removal efficiency was investigated.
[0045] Table 6. Effect of material dosage on phosphate removal rate
[0046] As shown in Table 6, the removal rate increased from 50.45% to 86.38% as the dosage increased from 0.3 g / L to 1.0 g / L; it reached 82.34% at 0.5 g / L. The relatively low dosage provides sufficient effective adsorption sites to adsorb most of the phosphate in the water. This indicates that iron sludge, after simple drying treatment, has excellent and stable adsorption capacity for phosphate.
[0047] 3.2 Effect of pH With a fixed dosage of 0.5 g / L and an initial phosphate concentration of 20 mg / L, the effect of pH (3-11) on phosphate removal efficiency was investigated.
[0048] Table 7 Effect of solution pH on phosphate removal rate of materials
[0049] As shown in Table 7, the removal rate remained between 85.21% and 89.19% within the pH range of 3–11. The material exhibits excellent pH adaptability, maintaining high efficiency under both acidic and alkaline conditions, making it suitable for real-world water environments with fluctuating pH levels.
[0050] 3.3 Adsorption Kinetics With a fixed dosage of 0.5 g / L, pH=5, and an initial phosphate concentration of 20 mg / L, the changes in phosphate concentration at different time points were measured. Pseudo-first-order and pseudo-second-order kinetic models were used for fitting.
[0051] Table 8 Fitting parameters of the adsorption kinetic model for phosphate by the material
[0052] As shown in Table 8, the pseudo-second-order model has an R² of 0.992, which is higher than the pseudo-first-order model's 0.968. The pseudo-second-order qe is 35.64 mg / g, indicating that the adsorption process is more consistent with the pseudo-second-order kinetics, suggesting that it is mainly chemisorption and may involve surface complexation or ion exchange mechanisms.
[0053] Example 4: Arsenic Removal Experiment Prepare simulated wastewater containing As(III) or As(V) with an initial concentration of 20 mg / L, using the same experimental method as in Example 3.
[0054] 4.1 Removal of As(III) With a fixed dosage of 0.5 g / L and pH=5, the mixture was filtered after the reaction was completed, and the concentration of As(III) in the filtrate was measured. The results are shown in Table 9, and the material achieved a 100% removal rate of As(III).
[0055] 4.2 Removal of As(V) With a fixed dosage of 0.5 g / L and pH=5, the mixture was filtered after the reaction was completed, and the concentration of As(V) in the filtrate was measured. The results are shown in Table 9, and the material achieved a 100% removal rate of As(III).
[0056] 4.3 Verification of Oxidation-Adsorption Synergistic Effect By measuring the change in the As(III) / As(V) ratio before and after the reaction, the material was verified to have an oxidizing effect on As(III), which can play a certain role in detoxifying the adsorbed As(III). The results are shown in Table 10. After 20 min of reaction, about 62% of As(III) was oxidized to a higher valence state, indicating that the material has a significant oxidizing function, can realize the in-situ oxidation and transformation of pollutants, and enhance the overall removal efficiency.
[0057] Example 5: Antimony Removal Experiment Simulated wastewater containing Sb(III) or Sb(V) with an initial concentration of 20 mg / L was prepared, and the experimental method was the same as in Example 3. The results are shown in Tables 9 and 10. Under the same conditions, the removal rates of Sb(III) and Sb(V) both reached 100%. After 20 min of reaction, approximately 39% of Sb(III) was oxidized to a higher valence state.
[0058] Table 9. Removal rates of arsenic and antimony in different valence states by the materials
[0059] Table 10 Changes in the ratio of As(III) / Sb(III) oxidized to As(V) / Sb(V) during the reaction process
[0060] Example 6: Comparison with conventional iron-based materials The following control materials were prepared respectively: (a) Iron sludge produced by adding potassium ferrate alone (without electrochemistry) (b) Ferric hydroxide precipitate produced by conventional FeCl3 hydrolysis (c) Commercial iron oxide adsorbent (d) Iron sludge produced by adding sulfite to activate potassium ferrate A comparative experiment on phosphate removal was conducted under the same conditions (dosage 0.5 g / L, pH=5, initial phosphate concentration 20 mg / L).
[0061] Table 11 Comparison of phosphate removal performance of different iron-based materials
[0062] Table 11 shows that, under the same adsorption conditions, the electrochemical-ferrate iron sludge prepared in this invention achieves a phosphate removal rate of 87.59%, significantly surpassing the adsorption efficiency of control materials produced by simple chemical precipitation: including simple ferrate iron sludge (Fe(VI), 52.426%), commercially available iron oxide (Fe2O3, 74.15%), iron hydroxide prepared by FeCl3 hydrolysis (Fe(OH)3, 50.52%), and iron sludge produced by sulfite-activated potassium ferrate (71.54%). This result strongly indicates that the synergistic effect of the electrochemical field and ferrate is not a simple additive effect, but rather induces the formation of a novel iron (hydrogen) oxide structure with higher surface activity and adsorption capacity. This not only verifies the technical feasibility of directionally converting this process byproduct into a high-value adsorbent, but also supports the requirement of this invention regarding the "special activity" of the material from a performance perspective.
Claims
1. An iron sludge-based environmental functional material produced by an electrochemical-ferrate combined process, characterized in that: Using boron-doped diamond electrodes or metal oxide-coated titanium electrodes as anodes, and one of Ti plates, stainless steel, or graphite as cathodes, iron sludge generated during the co-treatment of wastewater with ferrates via an electrochemical system is used to obtain an iron sludge-based environmental functional material. The iron sludge contains intermediate valence iron active sites and has dual oxidation-adsorption properties.
2. The iron mud-based environmental functional material according to claim 1, characterized in that: The iron mud-based environmental functional material has an amorphous or low-crystallinity structure with a specific surface area of not less than 100 m². 2 / g.
3. The iron mud-based environmental functional material according to claim 1, characterized in that: The ferrate is potassium ferrate or sodium ferrate; the valence state of iron in the iron mud-based environmental functional material includes +3 valence and intermediate valence iron.
4. A method for preparing the iron mud-based environmental functional material according to any one of claims 1-3, characterized in that, Includes the following steps: Step (1) Electrochemical oxidation uses one of boron-doped diamond electrode or metal oxide coated titanium electrode as the anode, and one of Ti plate, stainless steel or graphite as the cathode. Ferrate is added to the wastewater to be treated to carry out electrochemical-ferrate combined oxidation treatment. After the reaction in step (2) is completed, collect the solid residue and separate the solid and liquid phases. Step (3) Wash and dry the solid residue to obtain iron mud-based environmental functional materials.
5. The preparation method according to claim 4, characterized in that: The dosage of the ferrate, calculated as Fe, is 1.0-4.0 g / L.
6. The preparation method according to claim 4, characterized in that: The current density of the electrochemical treatment is 10-40 mA / cm², and the treatment time is 120-180 min.
7. The preparation method according to claim 4, characterized in that: The pH of the wastewater needs to be adjusted to above 9.
8. The preparation method according to claim 4, characterized in that: The drying method is either forced air drying or vacuum drying, and the drying temperature is 45-60℃.
9. The application of the material according to claim 1 in water pollution control, characterized in that: Iron mud-based environmental functional materials are used to remove phosphate ions, arsenic, or antimony from water.
10. The application of the material according to claim 1 in water pollution control, characterized in that: The dosage of iron mud-based environmental functional materials is 0.5-1.0 g / L; the pH during the reaction is 3-12, and the reaction time is 5-20 min.