Flame-retardant modified thermal insulation foam and process for its preparation
By adding hydroxyl-terminated polydimethylsiloxane and 3,5-di-tert-butyl-4-hydroxyphenylacetic acid grafts to polyethylene foam, a silicon-phosphorus-boron composite carbon layer and chemically bonded antioxidant units are formed, which solves the flame retardancy and anti-oxidation problems of polyethylene foam and improves the safety and durability of the material.
Patent Information
- Application Number
- CN202610436547.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-04-03
- Publication Date
- 2026-06-23
AI Technical Summary
Polyethylene foam has insufficient flame retardant and oxidation resistance properties in automotive bumper and seat foam, making it easily combustible and prone to oxidation failure, which affects safety and durability.
Using low-density polyethylene as the base material, it incorporates hydroxyl-terminated polydimethylsiloxane grafts and 3,5-di-tert-butyl-4-hydroxyphenylacetic acid grafts, forming a dense, heat-insulating, and oxygen-barrier char layer through a ternary synergistic flame retardant of silicon, phosphorus, and boron. Combined with chemically bonded antioxidant units, it enhances flame retardant and antioxidant properties.
It achieves highly efficient flame retardant and antioxidant properties, improves the safety and durability of the material, and maintains the material's thermal insulation and mechanical properties.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of thermal insulation materials technology, specifically to a flame-retardant modified thermal insulation foam material and its preparation process. Background Technology
[0002] Polyethylene foam belongs to the category of polymer foam plastics. Its manufacturing process uses low-density polyethylene as the base material and employs physical foaming technology to create a massive number of independent air bubbles within the material. This material integrates multiple superior properties, possessing core advantages such as lightweight and environmental friendliness, thermal insulation, sound insulation and shock absorption, and water and moisture resistance. It also features outstanding toughness, strong plasticity, and excellent impact resistance. Composite products made by bonding polyethylene foam with various fabrics have become a preferred choice for vehicle interior decoration and high-quality materials due to their excellent comprehensive performance. Automotive foam bumpers and car seat foam bodies, based on low-density polyethylene foam, are among the core foam base materials for current automotive interior and exterior trims, thanks to their lightweight characteristics and excellent energy-absorbing properties. Bumpers are suitable for collision protection, and seats provide comfortable support.
[0003] However, the material's shortcomings in flame retardancy and oxidation resistance have severely limited its safety and durability in these two scenarios. In terms of flame retardancy, automotive foam bumpers need to cope with the risk of fire from contact with high-temperature components such as the engine after a collision, while seat foam is in a confined space inside the vehicle. Once it burns, it will spread rapidly and release toxic fumes. The molten dripping of low-density polyethylene during combustion will exacerbate the fire.
[0004] When polyethylene foam is used in automotive bumpers, it exhibits significant shortcomings in terms of oxidation resistance. The porous structure formed by foaming greatly increases the material's specific surface area, making it easier for oxygen, ultraviolet light, and moisture to permeate. Simultaneously, the pores easily accumulate heat, further accelerating oxidation. The application of antioxidants also has limitations. Small-molecule antioxidants are prone to migration and loss under conditions such as high temperatures and rain erosion. Reactive antioxidants have extremely low grafting rates due to the non-polar nature of polyethylene and the lack of active functional groups. Some antioxidants may also agglomerate due to poor compatibility with the foaming system, forming weak areas in terms of oxidation resistance. Combined with the synergistic effects of long-term exposure to high temperatures, ultraviolet light, acid rain, salt spray, and mechanical stress, this ultimately leads to oxidation failure phenomena such as yellowing, embrittlement, cracking, and decreased cushioning and resilience.
[0005] Therefore, it is of great significance to develop a heat-insulating foam material with flame retardancy and oxidation resistance. Summary of the Invention
[0006] The purpose of this invention is to provide a flame-retardant modified thermal insulation foam material and its preparation process.
[0007] The objective of this invention can be achieved through the following technical solutions: A flame-retardant modified thermal insulation foam material, comprising the following components by weight: 30-45 parts low-density polyethylene, 8-10 parts foaming agent, 7-10 parts anti-shrinkage agent, 3-5 parts hydroxyl-terminated polydimethylsiloxane graft, 3-5 parts 3,5-di-tert-butyl-4-hydroxyphenylacetic acid, 3-5 parts lubricant, and 1-2 parts coupling agent.
[0008] Furthermore, the preparation method of the hydroxyl-terminated polydimethylsiloxane graft includes the following steps: Step S1: Weigh 5-6g of hydroxyl-terminated polydimethylsiloxane and add it to 100-110ml of toluene. Stir well, then add 1.5-2.5g of [(6-oxo-6H-dibenzo[C,E][1,2]oxophosphoric acid-6-yl)methyl]succinic acid and 0.1-0.2g of p-toluenesulfonic acid. Heat to 80-90℃ and stir for 6-8 hours. After the reaction is complete, dry to obtain the hydroxyl-terminated polydimethylsiloxane intermediate. Step S2: Weigh 4-5g of hydroxyl-terminated polydimethylsiloxane intermediate and add it to 100-110ml of N,N-dimethylformamide. Stir well and then add 2-3g of benzoborazole. Heat and stir for 6-8 hours. After the reaction is complete, dry to obtain hydroxyl-terminated polydimethylsiloxane graft.
[0009] Further, in step S1, the molecular weight of the hydroxyl-terminated polydimethylsiloxane is 4000-5000.
[0010] Furthermore, in step S2, the heating temperature is 80-90℃.
[0011] Using the above technical solution, the hydroxyl groups on the hydroxyl-terminated polydimethylsiloxane react with the carboxyl groups on [(6-oxo-6H-dibenzo[C,E][1,2]oxophosphazenecyclo-6-yl)methyl]succinic acid to prepare the hydroxyl-terminated polydimethylsiloxane intermediate; the carboxyl groups on the hydroxyl-terminated polydimethylsiloxane intermediate react with the amino groups on benzoborazole to prepare the hydroxyl-terminated polydimethylsiloxane graft.
[0012] Furthermore, the preparation method of the 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft comprises the following steps: Step SS1: Weigh 5-6g of carboxyl-terminated polybutadiene and add it to 100-110ml of toluene. Stir well, add 1.5-2.5g of glycerol triglycidyl ether and 0.1-0.2g of catalyst, heat to 50-60℃, stir and react for 4-6h. After the reaction is complete, dry to obtain the carboxyl-terminated polybutadiene intermediate. Step SS2: Weigh 4-5g of carboxyl-terminated polybutadiene intermediate and add it to 100-110ml of toluene. Stir well, add 1.5-2.5g of 3,5-di-tert-butyl-4-hydroxyphenylacetic acid and 0.1-0.2g of p-toluenesulfonic acid, heat to 80-90℃, stir and react. After the reaction is complete, dry to obtain 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft.
[0013] Furthermore, in step SS1, the catalyst is triethylamine or diisopropylethylamine.
[0014] Furthermore, in step SS1, the molecular weight of the carboxyl-terminated polybutadiene is 2000-3000.
[0015] Furthermore, in step SS2, the stirring reaction time is 6-8 hours.
[0016] Furthermore, the foaming agent is azodicarbonamide; the anti-shrinkage agent is monoglyceride; the lubricant is zinc stearate or polyethylene wax; and the coupling agent is phthalate.
[0017] Using the above technical solution, the carboxyl group on the carboxyl-terminated polybutadiene reacts with the epoxy group on the glycerol triglycidyl ether to obtain a carboxyl-terminated polybutadiene intermediate; the hydroxyl group on the carboxyl-terminated polybutadiene intermediate reacts with the carboxyl group on 3,5-di-tert-butyl-4-hydroxyphenylacetic acid to obtain a 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft.
[0018] A method for preparing a flame-retardant modified thermal insulation foam material includes the following steps: Step A: Mix low-density polyethylene, anti-shrinkage agent, hydroxyl-terminated polydimethylsiloxane graft, 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft, lubricant, coupling agent, and foaming agent, and then granulate the mixture to obtain granulation masterbatch. Step B: The granulation masterbatch is extruded to obtain a molding master sheet, and then the molding master sheet is irradiated. Step C: Place the irradiated master sheet in a foaming furnace for foaming to obtain flame-retardant modified heat-insulating foam material.
[0019] The beneficial effects of this invention are: (1) The flame-retardant modified heat-insulating foam material prepared by the present invention is made of low-density polyethylene as the main material and hydroxyl-terminated polydimethylsiloxane graft and 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft as auxiliary materials, so that the flame-retardant modified heat-insulating foam material prepared by the present invention has flame-retardant, anti-oxidation and heat-insulating properties.
[0020] (2) The silicon-phosphorus-boron ternary synergistic flame retardant takes condensed phase flame retardancy as the core and gas phase flame retardancy as the auxiliary. It achieves high efficiency and halogen-free flame retardancy through the complementary synergistic effect of silicon, phosphorus and boron. Among them, the phosphorus component in [(6-oxo-6H-dibenzo[C,E][1,2]oxophosphorus-hexane-6-yl)methyl]succinic acid decomposes at high temperature to generate polyphosphoric acid, which catalyzes the dehydration and carbonization of the polymer matrix and forms the initial structure of phosphorus-oxygen carbon. The silicon component on the terminal hydroxyl polydimethylsiloxane crosslinks to form a rigid skeleton to support the carbon layer and prevent collapse. The decomposed boron component in benzoborazole fills the pores of the carbon layer in glassy state and reacts with silicon and phosphorus products to form a stable covalent bond network, constructing a dense, heat-insulating and oxygen-insulating silicon-phosphorus-boron composite carbon layer, while inhibiting melt dripping. At the same time, the inert small molecules and nano silica particles generated by the decomposition of silicon component dilute combustible gas and adsorb free radicals, further blocking the combustion chain reaction. Its flame retardant efficiency is much higher than that of the binary system, and it can take into account both the flame retardant performance and mechanical properties of the material.
[0021] (3) After grafting 3,5-di-tert-butyl-4-hydroxyphenylacetic acid onto carboxyl-terminated polybutadiene, the antioxidant units of 3,5-di-tert-butyl-4-hydroxyphenylacetic acid are chemically bonded to the flexible long chains of carboxyl-terminated polybutadiene. This process retains the antioxidant activity of 3,5-di-tert-butyl-4-hydroxyphenylacetic acid, inhibits its aggregation by utilizing the steric hindrance effect of carboxyl-terminated polybutadiene, and solves the problem of easy migration of 3,5-di-tert-butyl-4-hydroxyphenylacetic acid by covalently linking it to the molecular chain. At the same time, relying on the elastic properties of carboxyl-terminated polybutadiene, this product has both elasticity retention capability and multifunctional integration potential, and can be adapted to the antioxidant modification needs of various scenarios.
[0022] Of course, any product implementing this invention does not necessarily need to achieve all of the advantages described above at the same time. Detailed Implementation
[0023] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0024] Example 1
[0025] A flame-retardant modified thermal insulation foam material, by weight, comprises the following components: 30 parts low-density polyethylene, 8 parts foaming agent, 7 parts anti-shrinkage agent, 3 parts hydroxyl-terminated polydimethylsiloxane graft, 3 parts 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft, 3 parts lubricant, and 1 part coupling agent.
[0026] The preparation method of the flame-retardant modified thermal insulation foam material includes the following steps: Step A: Mix low-density polyethylene, anti-shrinkage agent, hydroxyl-terminated polydimethylsiloxane graft, 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft, lubricant, coupling agent, and foaming agent, and then granulate the mixture to obtain granulation masterbatch. Step B: The granulation masterbatch is extruded to obtain a molding master sheet, and then the molding master sheet is irradiated. Step C: Place the irradiated master sheet in a foaming furnace for foaming to obtain flame-retardant modified heat-insulating foam material.
[0027] The method for preparing the hydroxyl-terminated polydimethylsiloxane graft includes the following steps: Step S1: Weigh 5g of hydroxyl-terminated polydimethylsiloxane and add it to 100ml of toluene and stir well. Then add 1.5g of [(6-oxo-6H-dibenzo[C,E][1,2]oxophosphazenecyclo-6-yl)methyl]succinic acid and 0.1g of p-toluenesulfonic acid. Heat to 90℃ and stir for 8h. After the reaction is complete, dry to obtain the hydroxyl-terminated polydimethylsiloxane intermediate. Step S2: Weigh 4g of hydroxyl-terminated polydimethylsiloxane intermediate and add it to 100ml of N,N-dimethylformamide. Stir well and then add 2g of benzoborazole. Heat to 90℃ and stir for 6 hours. After the reaction is complete, dry to obtain hydroxyl-terminated polydimethylsiloxane graft.
[0028] The preparation method of the 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft includes the following steps: Step SS1: Weigh 5g of carboxyl-terminated polybutadiene and add it to 110ml of toluene. Stir well, add 1.5g of glycerol triglycidyl ether and 0.2g of triethylamine, heat to 60℃, stir and react for 6h. After the reaction is complete, dry to obtain the carboxyl-terminated polybutadiene intermediate. Step SS2: Weigh 5g of carboxyl-terminated polybutadiene intermediate and add it to 110ml of toluene. Stir well, add 1.5g of 3,5-di-tert-butyl-4-hydroxyphenylacetic acid and 0.1g of p-toluenesulfonic acid, heat to 80℃, stir and react for 8h. After the reaction is complete, dry to obtain 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft.
[0029] Example 2
[0030] A flame-retardant modified thermal insulation foam material, by weight, comprises the following components: 31 parts low-density polyethylene, 9 parts foaming agent, 8 parts anti-shrinkage agent, 4 parts hydroxyl-terminated polydimethylsiloxane graft, 4 parts 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft, 4 parts lubricant, and 1.5 parts coupling agent.
[0031] The preparation method of the flame-retardant modified thermal insulation foam material includes the following steps: Step A: Mix low-density polyethylene, anti-shrinkage agent, hydroxyl-terminated polydimethylsiloxane graft, 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft, lubricant, coupling agent, and foaming agent, and then granulate the mixture to obtain granulation masterbatch. Step B: The granulation masterbatch is extruded to obtain a molding master sheet, and then the molding master sheet is irradiated. Step C: Place the irradiated master sheet in a foaming furnace for foaming to obtain flame-retardant modified heat-insulating foam material.
[0032] The preparation methods of the terminal hydroxyl polydimethylsiloxane graft and the 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft are the same as those in Example 1.
[0033] Example 3
[0034] A flame-retardant modified thermal insulation foam material, by weight, comprises the following components: 45 parts low-density polyethylene, 10 parts foaming agent, 10 parts anti-shrinkage agent, 5 parts hydroxyl-terminated polydimethylsiloxane graft, 5 parts 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft, 5 parts lubricant, and 2 parts coupling agent.
[0035] The preparation method of the flame-retardant modified thermal insulation foam material includes the following steps: Step A: Mix low-density polyethylene, anti-shrinkage agent, hydroxyl-terminated polydimethylsiloxane graft, 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft, lubricant, coupling agent, and foaming agent, and then granulate the mixture to obtain granulation masterbatch. Step B: The granulation masterbatch is extruded to obtain a molding master sheet, and then the molding master sheet is irradiated. Step C: Place the irradiated master sheet in a foaming furnace for foaming to obtain flame-retardant modified heat-insulating foam material.
[0036] The preparation methods of the terminal hydroxyl polydimethylsiloxane graft and the 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft are the same as those in Example 1.
[0037] Comparative Example 1
[0038] A flame-retardant modified thermal insulation foam material, by weight, comprises the following components: 31 parts low-density polyethylene, 9 parts foaming agent, 8 parts anti-shrinkage agent, 4 parts 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft, 4 parts lubricant, and 1.5 parts coupling agent.
[0039] The preparation method of the flame-retardant modified thermal insulation foam material includes the following steps: Step A: Mix low-density polyethylene, anti-shrinkage agent, hydroxyl-terminated polydimethylsiloxane graft, 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft, lubricant, coupling agent, and foaming agent, and then granulate the mixture to obtain granulation masterbatch. Step B: The granulation masterbatch is extruded to obtain a molding master sheet, and then the molding master sheet is irradiated. Step C: Place the irradiated master sheet in a foaming furnace for foaming to obtain flame-retardant modified heat-insulating foam material.
[0040] The preparation method of the 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft is the same as that in Example 1.
[0041] Comparative Example 2
[0042] A flame-retardant modified thermal insulation foam material, by weight, comprises the following components: 31 parts low-density polyethylene, 9 parts foaming agent, 8 parts anti-shrinkage agent, 4 parts hydroxyl-terminated polydimethylsiloxane graft, 4 parts lubricant, and 1.5 parts coupling agent.
[0043] The preparation method of the flame-retardant modified thermal insulation foam material includes the following steps: Step A: Mix low-density polyethylene, anti-shrinkage agent, hydroxyl-terminated polydimethylsiloxane graft, 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft, lubricant, coupling agent, and foaming agent, and then granulate the mixture to obtain granulation masterbatch. Step B: The granulation masterbatch is extruded to obtain a molding master sheet, and then the molding master sheet is irradiated. Step C: Place the irradiated master sheet in a foaming furnace for foaming to obtain flame-retardant modified heat-insulating foam material.
[0044] The preparation method of the hydroxyl-terminated polydimethylsiloxane graft is the same as that in Example 1.
[0045] Comparative Example 3
[0046] A flame-retardant modified thermal insulation foam material, by weight, comprises the following components: 31 parts low-density polyethylene, 9 parts foaming agent, 8 parts anti-shrinkage agent, 4 parts hydroxyl-terminated polydimethylsiloxane graft, 4 parts 3,5-di-tert-butyl-4-hydroxyphenylacetic acid, 4 parts lubricant, and 1.5 parts coupling agent.
[0047] The preparation method of the flame-retardant modified thermal insulation foam material includes the following steps: Step A: Mix low-density polyethylene, anti-shrinkage agent, hydroxyl-terminated polydimethylsiloxane graft, 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft, lubricant, coupling agent, and foaming agent, and then granulate the mixture to obtain granulation masterbatch. Step B: The granulation masterbatch is extruded to obtain a molding master sheet, and then the molding master sheet is irradiated. Step C: Place the irradiated master sheet in a foaming furnace for foaming to obtain flame-retardant modified heat-insulating foam material.
[0048] The preparation method of the hydroxyl-terminated polydimethylsiloxane graft is the same as that in Example 1.
[0049] Test case
[0050] The flame-retardant modified thermal insulation foam materials prepared in the embodiments and comparative examples of the present invention were made into test samples, and their thermal conductivity was tested in accordance with standard GB / T 10296-2008; their limiting oxygen index was tested in accordance with standard GB / T 2406-2008.
[0051] Based on the above experimental data, the thermal conductivity of the flame-retardant modified thermal insulation foam materials prepared in Examples 1-3 is ≤0.032W / (m·K), and the limiting oxygen index is ≥36.2%.
[0052] Comparing Comparative Example 1 and Example 2, the oxygen index of the thermal insulation foam material prepared without the addition of the terminal hydroxyl polydimethylsiloxane graft compound was lower than that of the thermal insulation foam material prepared with the addition of the terminal hydroxyl polydimethylsiloxane graft compound. The terminal hydroxyl polydimethylsiloxane graft compound achieves synergistic flame retardancy with silicon, phosphorus, and boron under high temperature, thus giving the thermal insulation foam material prepared by this invention flame-retardant properties.
[0053] The thermal insulation foam materials prepared in the embodiments and comparative examples of this invention were placed in an environment of 80°C for 48 hours to accelerate oxidation. At least five strip-shaped effective samples with a length of 50 mm and a width of 20 mm were cut from the defect-free parts of the finished foam product. Then, an electronic universal testing machine was used with a set speed of 500 ± 50 mm / min. After calibrating the instrument, the samples were coaxially clamped and stretched until fracture, and the maximum tensile force was recorded. The tensile strength was calculated using the formula α = F / bd, where α is the tensile strength in MPa; F is the maximum tensile force in N; b is the sample length in mm; and d is the sample width in mm. The rate of decrease in tensile strength before and after oxidation was tested. The smaller the rate of decrease, the better the oxidation resistance.
[0054]
[0055] Based on the above experimental data, the mechanical properties of the thermal insulation foam materials prepared in Examples 1-3 all decreased by ≤8.6%.
[0056] Comparing Comparative Examples 2, 3, and 2, the thermal insulation foam material prepared with the addition of 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft polymer showed a lower rate of mechanical property degradation after high-temperature aging than the thermal insulation foam material prepared with or without the addition of 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft polymer. Grafting carboxyl-terminated polybutadiene with 3,5-di-tert-butyl-4-hydroxyphenylacetic acid retains the antioxidant activity of 3,5-di-tert-butyl-4-hydroxyphenylacetic acid and inhibits its aggregation through the steric hindrance effect of the carboxyl-terminated polybutadiene, thus giving the thermal insulation foam material prepared by this invention antioxidant properties.
[0057] The above description is merely an example and illustration of the concept of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described or use similar methods to replace them, as long as they do not deviate from the concept of the invention or exceed the scope defined in the claims, they should all fall within the protection scope of the present invention.
Claims
1. A flame-retardant modified insulating foam material, characterized in that, By weight, it includes the following components: 30-45 parts low-density polyethylene, 8-10 parts foaming agent, 7-10 parts anti-shrinkage agent, 3-5 parts hydroxyl-terminated polydimethylsiloxane graft, 3-5 parts 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft, 3-5 parts lubricant, and 1-2 parts coupling agent.
2. A flame-retardant modified insulating foam material according to claim 1, characterized in that, The method for preparing the hydroxyl-terminated polydimethylsiloxane graft includes the following steps: Step S1: Add hydroxyl-terminated polydimethylsiloxane to toluene and stir until homogeneous. Then add [(6-oxo-6H-dibenzo[C,E][1,2]oxophosphazenecyclo-6-yl)methyl]succinic acid and p-toluenesulfonic acid. Heat to 80-90℃ and stir for 6-8 hours. After the reaction is complete, dry to obtain the hydroxyl-terminated polydimethylsiloxane intermediate. Step S2: Add the hydroxyl-terminated polydimethylsiloxane intermediate to N,N-dimethylformamide, stir until homogeneous, then add benzoborazole, heat and stir for 6-8 hours. After the reaction is complete, dry to obtain the hydroxyl-terminated polydimethylsiloxane graft.
3. A flame-retardant modified insulating foam material according to claim 2, characterized in that, In step S1, the molecular weight of the hydroxyl-terminated polydimethylsiloxane is 4000-5000.
4. A flame-retardant modified insulating foam material according to claim 2, characterized in that, In step S2, the heating temperature is 80-90℃.
5. The flame-retardant modified insulating foam material according to claim 1, wherein The preparation method of the 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft includes the following steps: Step SS1: Add carboxyl-terminated polybutadiene to toluene, stir until homogeneous, add glycerol triglycidyl ether and catalyst, heat to 50-60℃, stir for 4-6 hours until the reaction is complete, and dry to obtain carboxyl-terminated polybutadiene intermediate. Step SS2: Add the carboxyl-terminated polybutadiene intermediate to toluene, stir until homogeneous, add 3,5-di-tert-butyl-4-hydroxyphenylacetic acid and p-toluenesulfonic acid, heat to 80-90℃, stir to react, and after the reaction is complete, dry to obtain the 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft.
6. The flame-retardant modified thermal insulation foam material according to claim 5, characterized in that, In step SS1, the catalyst is triethylamine or diisopropylethylamine.
7. The flame-retardant modified thermal insulation foam material according to claim 5, characterized in that, In step SS1, the molecular weight of the carboxyl-terminated polybutadiene is 2000-3000.
8. The flame-retardant modified thermal insulation foam material according to claim 5, characterized in that, In step SS2, the stirring reaction time is 6-8 hours.
9. The flame-retardant modified thermal insulation foam material according to claim 1, characterized in that, The foaming agent is azodicarbonamide; the anti-shrinkage agent is monoglyceride; the lubricant is zinc stearate or polyethylene wax; and the coupling agent is phthalate.
10. A preparation process for the flame-retardant modified thermal insulation foam material as described in claim 1, characterized in that, Specifically, the following steps are included: Step A: Mix low-density polyethylene, anti-shrinkage agent, hydroxyl-terminated polydimethylsiloxane graft, 3,5-di-tert-butyl-4-hydroxyphenylacetic acid graft, lubricant, coupling agent, and foaming agent, and then granulate the mixture to obtain granulation masterbatch. Step B: The granulation masterbatch is extruded to obtain a molding master sheet, and then the molding master sheet is irradiated. Step C: Place the irradiated master sheet in a foaming furnace for foaming to obtain flame-retardant modified heat-insulating foam material.