A method for preparing high-purity potassium fluorotitanate from hydrofluoric acid waste liquid

By using hydrofluoric acid waste liquid and titanic acid powder as raw materials, high-purity potassium fluorotitanate was prepared, solving the problems of resource waste and safety risks in the treatment of hydrofluoric acid waste liquid, and realizing the efficient and low-cost preparation of potassium fluorotitanate.

CN122276820APending Publication Date: 2026-06-26PERIC SPECIAL GASES CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202610512575.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-04-17
Publication Date
2026-06-26
Patent Text Reader

Abstract

This application belongs to the field of inorganic chemical waste recycling and fluoride preparation technology, specifically relating to a method for preparing potassium fluorotitanate from hydrofluoric acid waste liquid. The method includes: S1. Pretreatment of hydrofluoric acid waste liquid and titanic acid powder; S2. Adding the pretreated hydrofluoric acid waste liquid and titanic acid powder to a reaction vessel to generate a fluorotitanic acid solution; S3. Adding potassium carbonate to the fluorotitanic acid solution to generate potassium fluorotitanate, followed by purification of the reaction solution to obtain potassium fluorotitanate crystals; S4. Washing and drying the potassium fluorotitanate crystals to obtain a high-purity potassium fluorotitanate product. This application uses titanic acid powder as the titanium source and optimizes reaction parameters to achieve the dual goals of resource recovery from hydrofluoric acid waste liquid and low-cost preparation of high-purity potassium fluorotitanate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of inorganic chemical waste recycling and fluoride preparation technology, specifically relating to a method for preparing potassium fluorotitanate from hydrofluoric acid waste liquid. Background Technology

[0002] Hydrofluoric acid plays a crucial role in semiconductor manufacturing, glass etching, stainless steel pickling, and metal processing. However, its widespread use inevitably generates large quantities of hydrofluoric acid waste liquid. This waste liquid is characterized by high fluoride ion concentration, strong corrosiveness, and high toxicity. Existing hydrofluoric acid waste liquid treatment technologies mostly focus on preparing low-value-added calcium fluoride or recovering low-concentration hydrofluoric acid. Meanwhile, potassium fluorotitanate (K2TiF6), as a grain refiner for aluminum alloys, a raw material for ceramic glazes, and a polypropylene catalyst, faces challenges in its traditional preparation processes, including high raw material costs, significant safety risks, and low reaction efficiency.

[0003] The main methods for treating hydrofluoric acid wastewater include chemical precipitation, adsorption, and resource recovery. Among these, chemical precipitation is the most widely used traditional process in industry. This method involves adding lime or carbide slag to the wastewater, causing fluoride ions to precipitate as insoluble calcium fluoride. However, this process suffers from resource waste and secondary pollution, with a fluoride resource utilization rate of less than 30%. To address the shortcomings of the lime neutralization method, various resource recovery technologies for hydrofluoric acid wastewater have emerged in recent years.

[0004] The technical solution disclosed in CN1559931A is a high-concentration hydrofluoric acid waste liquid treatment system and method. However, it focuses on the treatment of waste liquid rather than its high-value utilization. In practical applications, this technology suffers from high heat release and a rapid increase in the temperature of the mixed liquid, which can easily lead to the volatilization and escape of hydrogen fluoride gas, resulting in the loss of fluorine resources.

[0005] The technical solution disclosed in CN117466250B is a method for the comprehensive utilization and recovery of hydrofluoric acid from fluorine-containing waste acid. Hydrofluoric acid is recovered from fluorine-containing waste acid through a specific separation process, achieving resource recycling. However, this type of method has high operating costs, and the recovered hydrofluoric acid often has a low concentration or contains impurities, making it difficult to directly use as a high-quality raw material for high-purity fluoride products.

[0006] The technical solution disclosed in announcement number CN107935008A is a method for treating hydrofluoric acid wastewater containing hydrochloric acid. This method involves adding an aluminum chloride solution to the wastewater, causing it to react and produce aluminum fluoride trihydrate and crystalline aluminum chloride. While this method achieves the resource recovery of the wastewater, the market value of the product, aluminum fluoride, is relatively low, and the process has limited adaptability to the hydrochloric acid content in the wastewater.

[0007] The technical solution disclosed in CN119874003A is a device and method for treating hydrofluoric acid waste liquid, which reacts concentrated hydrofluoric acid waste liquid with an aluminum source to generate anhydrous aluminum fluoride. Although this technology increases the added value of the product, it is still limited to the preparation of aluminum-based fluoride salts.

[0008] Potassium fluorotitanate is an important inorganic fluorine chemical product, appearing as a white crystalline powder, slightly soluble in cold water and soluble in hot water. Current production processes primarily focus on titanium dioxide or titanium tetrachloride as the titanium source: titanium tetrachloride is volatile and highly corrosive, requiring low-temperature, sealed storage; titanium dioxide reacts slowly with hydrofluoric acid, necessitating extended reaction time. Titanic acid powder (H₂TiO₃), however, offers advantages such as high stability, moderate reactivity, and lower cost than titanium tetrachloride. Furthermore, it produces no volatile byproducts in its reaction with hydrofluoric acid, making it more suitable for wastewater recycling applications. In summary, existing technologies exhibit two main problems: firstly, hydrofluoric acid wastewater treatment focuses on harmless or low-value utilization, lacking efficient technologies for producing high-value-added potassium fluorotitanate; secondly, potassium fluorotitanate preparation technologies mainly rely on pure hydrofluoric acid and traditional titanium sources, facing issues of high raw material costs or low reaction efficiency. Therefore, developing a process that uses titanic acid powder as the titanium source to directly produce high-purity potassium fluorotitanate from hydrofluoric acid wastewater is an urgent problem to be solved. Summary of the Invention

[0009] Existing technologies for treating hydrofluoric acid waste focus on harmless or low-value utilization, lacking efficient technologies for preparing high-value-added potassium fluorotitanate. Potassium fluorotitanate preparation technologies mainly rely on pure hydrofluoric acid and traditional titanium sources, facing problems of high raw material costs or low reaction efficiency. This application proposes a method for preparing potassium fluorotitanate from hydrofluoric acid waste. The technical solution of this application is as follows: A method for preparing potassium fluorotitanate from hydrofluoric acid waste liquid includes the following steps: S1. Pretreatment of hydrofluoric acid waste liquid and titanic acid powder; S2. Add the pretreated hydrofluoric acid waste liquid and titanic acid powder to the reaction vessel to generate fluorotitanic acid solution; S3. Potassium carbonate is added to the fluorotitanic acid solution to react and produce potassium fluorotitanate. The reaction solution is then purified to obtain potassium fluorotitanate crystals. S4. Wash and dry the potassium fluorotitanate crystals to obtain a high-purity potassium fluorotitanate product.

[0010] Preferably, in step S1, the hydrofluoric acid waste liquid contains 40-50% hydrofluoric acid by mass, and the titanic acid powder has a purity of ≥99.0%.

[0011] Preferably, the pretreatment of hydrofluoric acid waste liquid in step S1 is as follows: the hydrofluoric acid waste liquid is filtered through a 0.22μm polytetrafluoroethylene filter membrane.

[0012] Preferably, the titanate powder pretreatment in step S1 involves drying the titanate powder in an oven at 85°C for 2 hours.

[0013] Preferably, in step S2, the molar ratio of fluorine in the hydrofluoric acid waste liquid to titanium in the titanic acid is controlled to be 6-7:1; the reactor is made of polytetrafluoroethylene and its initial temperature before use is 15-20℃; the reaction temperature of the hydrofluoric acid waste liquid and the titanic acid powder is 30-35℃ and the reaction time is 2-3h.

[0014] Preferably, in step S3, the purity of potassium carbonate is ≥99.9%; the molar ratio of potassium carbonate to titanium in the fluorotitanic acid solution is controlled to be 2-3:1; the reaction temperature of the fluorotitanic acid solution and potassium carbonate is 30-40℃, and the reaction time is 1-3h.

[0015] Preferably, the purification process in step S3 involves first filtering with a 0.45 μm polytetrafluoroethylene filter membrane, followed by washing with deionized water.

[0016] Preferably, in step S4, the washing involves rinsing the crystal surface with anhydrous ethanol at 0-10°C, repeating the rinsing 2-3 times.

[0017] Preferably, in step S4, the drying process uses a polytetrafluoroethylene crucible, the drying temperature is 80-90℃, and the drying time is 2-3 hours.

[0018] The beneficial effects of this application are as follows: This application achieves efficient recovery of fluorine resources from hydrofluoric acid waste liquid, with a fluorine recovery rate of ≥95.5%. It solves the problem of complete waste of fluorine resources and secondary pollution caused by the generation of a large amount of fluorine-containing hazardous calcium slag when treating hydrofluoric acid waste liquid by the traditional lime neutralization method.

[0019] This application uses hydrofluoric acid waste liquid to replace high-purity hydrofluoric acid as the fluorine source, and titanic acid powder to replace the expensive titanium sources such as titanium tetrachloride and high-purity titanium dioxide in the traditional preparation process. This reduces the raw material cost of potassium fluorotitanate production from the raw material end, achieving cost reduction and hazardous waste resource utilization. In addition, the titanium source of titanic acid powder is stable, avoiding the production safety risks and chlorine impurity introduction problems caused by the volatility and strong corrosiveness of the traditional titanium tetrachloride titanium source. This further improves the economy and production safety of the process.

[0020] The method and process of this application are simple and controllable, easy to operate, with a maximum reaction temperature of only 40℃ and mild reaction conditions, requiring no special production equipment such as high-temperature and high-pressure equipment. This application can prepare high-purity potassium fluorotitanate through a full-process impurity control and purification process. The pretreatment stage involves precise filtration of hydrofluoric acid waste liquid through a 0.22μm polytetrafluoroethylene (PTFE) membrane to remove impurities, followed by constant-temperature drying pretreatment of titanate powder, controlling impurities at the source. After potassium fluorotitanate synthesis, it undergoes multi-stage filtration through a 0.45μm PTFE membrane and washing with deionized water to remove soluble impurities. It is then deeply washed with anhydrous ethanol at 0-10℃ to remove residual free acid and excess potassium salt impurities, effectively preventing product agglomeration and impurity residue. Detailed Implementation

[0021] To further illustrate the technical means and effects adopted by this application in order to achieve the intended purpose of the invention, the following detailed description of the specific implementation methods, structures, features and effects of this application, in conjunction with preferred embodiments, is provided below.

[0022] Unless otherwise specified, all methods described herein are conventional methods, and all raw materials described herein are obtainable from publicly available commercial sources. Example 1

[0023] Step S1. Raw material pretreatment Hydrofluoric acid pretreatment: Take 200 mL of 40% hydrofluoric acid waste liquid, filter it through a 0.22 μm polytetrafluoroethylene filter membrane, and collect the purified hydrofluoric acid waste liquid; Titanic acid pretreatment: Take 28g of titanium acid powder and dry it in an oven at 85℃ for 2 hours for later use.

[0024] Step S2. Preparation of fluorotitanic acid Add the refined hydrofluoric acid waste liquid to a 500mL polytetrafluoroethylene reactor and control the initial temperature at 15℃. Slowly add titanic acid powder according to the molar ratio of fluorine to titanium of 6:1 (after calculation: 200mL of 40% hydrofluoric acid contains about 36.2g of fluorine, corresponding to about 5.2g of titanium, and the titanium content in titanic acid is about 47.4%, so take 28g of titanic acid). After the addition is completed, raise the temperature to 30℃ and keep it at that temperature for 3h.

[0025] Step S3. Synthesis and purification of potassium fluorotitanate Potassium carbonate (99.9% purity) was added to the fluorotitanic acid solution, and the molar ratio of potassium carbonate to titanium was controlled at 2:1 (32g was calculated to be needed). The reaction temperature was 30℃ and the reaction was carried out for 3h. The reaction solution was filtered through a 0.45μm polytetrafluoroethylene filter membrane, and the filter cake was washed three times with 15mL of deionized water to obtain crude potassium fluorotitanic crystals.

[0026] Step S4. Washing and Drying The coarse crystals were slowly washed twice with anhydrous ethanol at 0°C (30 mL each time), and filtered until no droplets remained. The crystals were then transferred to a polytetrafluoroethylene crucible and dried under vacuum at 80°C for 3 hours to obtain 58 g of potassium fluorotitanate product.

[0027] The product has been tested and found to have a purity of 99.5% and a fluorine recovery rate of 95.0%, which meets the high-end product standard of GB / T 28652-2012 "Potassium Fluorotitanate". Example 2

[0028] Step S1. Raw material pretreatment Hydrofluoric acid pretreatment: Take 350 mL of 45% hydrofluoric acid waste liquid, filter it through a 0.22 μm polytetrafluoroethylene filter membrane, and collect the purified hydrofluoric acid waste liquid; Titanic acid pretreatment: Take 55g of titanium acid powder and dry it in an oven at 85℃ for 2 hours for later use.

[0029] Step S2. Preparation of fluorotitanic acid Add the refined hydrofluoric acid waste liquid to a 1000mL polytetrafluoroethylene reactor and control the initial temperature at 18℃. Slowly add titanic acid powder at a fluorine to titanium molar ratio of 6.5:1. After the addition is complete, raise the temperature to 32℃ and keep it at that temperature for 2.5h.

[0030] Step S3. Synthesis and purification of potassium fluorotitanate Potassium carbonate (99.9% purity) was added to the fluorotitanic acid solution, and the molar ratio of potassium carbonate to titanium was controlled at 2.5:1 (68g was calculated to be needed). The reaction temperature was 35℃ and the reaction was carried out for 2 hours. The reaction solution was filtered through a 0.45μm polytetrafluoroethylene filter membrane, and the filter cake was washed three times with 25mL of deionized water to obtain crude potassium fluorotitanic crystals.

[0031] Step S4. Washing and Drying The coarse crystals were slowly washed three times with anhydrous ethanol at 5°C (50 mL each time), and filtered until no droplets remained. The crystals were then transferred to a polytetrafluoroethylene crucible and dried under vacuum at 85°C for 2.5 h to obtain 102 g of potassium fluorotitanate product.

[0032] The product has been tested and found to have a purity of 99.6% and a fluorine recovery rate of 96.3%, which meets the high-end product standard of GB / T 28652-2012 "Potassium Fluorotitanate". Example 3

[0033] Step S1. Raw material pretreatment Hydrofluoric acid pretreatment: Take 500 mL of 50% hydrofluoric acid waste liquid, filter it through a 0.22 μm polytetrafluoroethylene filter membrane, and collect the purified hydrofluoric acid waste liquid; Titanic acid pretreatment: Take 88g of titanium acid powder and dry it in an oven at 85℃ for 2 hours for later use.

[0034] Step S2. Preparation of fluorotitanic acid Add the refined hydrofluoric acid waste liquid to a 2000mL polytetrafluoroethylene reactor and control the initial temperature at 20℃. Slowly add titanic acid powder at a fluorine to titanium molar ratio of 7:1. After the addition is complete, raise the temperature to 35℃ and keep it at that temperature for 2 hours.

[0035] Step S3. Synthesis and purification of potassium fluorotitanate Potassium carbonate (99.9% purity) was added to the fluorotitanic acid solution, and the molar ratio of potassium carbonate to titanium was controlled at 3:1 (115g was required according to calculation). The reaction temperature was 40℃ and the reaction was carried out for 1h. The reaction solution was filtered through a 0.45μm polytetrafluoroethylene filter membrane, and the filter cake was washed three times with 40mL of deionized water to obtain crude potassium fluorotitanic crystals.

[0036] Step S4. Washing and Drying The coarse crystals were slowly washed three times with anhydrous ethanol at 10°C (80 mL each time), and filtered until no droplets remained. The crystals were then transferred to a polytetrafluoroethylene crucible and dried under vacuum at 90°C for 2 hours to obtain 165 g of potassium fluorotitanate product.

[0037] The product has been tested and found to have a purity of 99.7% and a fluorine recovery rate of 97.2%, which meets the high-end product standard of GB / T 28652-2012 "Potassium Fluorotitanate".

[0038] Comparative Example 1 The comparative example differs from Example 1 in that the raw material pretreatment step is omitted, i.e., the hydrofluoric acid waste liquid is not filtered through a 0.22μm polytetrafluoroethylene filter membrane, and the titanic acid powder is not dried in an 85°C oven. The remaining operations are the same as in Example 1.

[0039] In this comparative example, 51 g of potassium fluorotitanate with a purity of 98.1% was prepared, and the fluorine recovery rate was 89.2%.

[0040] Comparative Example 2 The difference between the comparative example and Example 2 is that the molar ratio of fluorine to titanium in the preparation step of fluorotitanic acid deviates from the preferred range, that is, it is adjusted from 6.5:1 in Example 2 to 5:1, while the rest of the operation is the same as in Example 2.

[0041] In this comparative example, 82 g of potassium fluorotitanate with a purity of 97.6% was prepared, and the fluorine recovery rate was 85.0%.

[0042] Comparative Example 3 The difference between the comparative example and Example 3 is that the purity of potassium carbonate in the potassium fluorotitanate synthesis step deviates from the preferred requirement; that is, the 99.9% analytical grade potassium carbonate in Example 3 is replaced with 98.0% industrial grade potassium carbonate (containing Na). + Impurities 0.6%, Ca 2+ (Impurities 0.4%), the remaining operations are the same as in Example 3.

[0043] In this comparative example, 162 g of potassium fluorotitanate with a purity of 98.3% was obtained, and the fluorine recovery rate was 94.8%. The above description is merely a preferred embodiment of this application and is not intended to limit this application in any way. Although this application has been disclosed above with reference to preferred embodiments, it is not intended to limit this application. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the technical solution of this application. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of this application without departing from the scope of the technical solution of this application shall still fall within the scope of the technical solution of this application.

Claims

1. A method for preparing potassium fluorotitanate from hydrofluoric acid waste liquid, characterized in that, Includes the following steps: S1. Pretreatment of hydrofluoric acid waste liquid and titanic acid powder; S2. Add the pretreated hydrofluoric acid waste liquid and titanic acid powder to the reaction vessel to generate fluorotitanic acid solution; S3. Potassium carbonate is added to the fluorotitanic acid solution to react and produce potassium fluorotitanate. The reaction solution is then purified to obtain potassium fluorotitanate crystals. S4. Wash and dry the potassium fluorotitanate crystals to obtain a high-purity potassium fluorotitanate product.

2. The method for preparing potassium fluorotitanate from hydrofluoric acid waste liquid according to claim 1, characterized in that, In step S1, the hydrofluoric acid waste liquid contains 40-50% hydrofluoric acid by mass, and the titanium acid powder has a purity of ≥99.0%.

3. The method for preparing potassium fluorotitanate from hydrofluoric acid waste liquid according to claim 1, characterized in that, The pretreatment of hydrofluoric acid waste liquid in step S1 is as follows: the hydrofluoric acid waste liquid is filtered through a 0.22μm polytetrafluoroethylene filter membrane.

4. The method for preparing potassium fluorotitanate from hydrofluoric acid waste liquid according to claim 1, characterized in that, In step S1, the titanate powder pretreatment involves drying the titanate powder in an oven at 85°C for 2 hours.

5. The method for preparing potassium fluorotitanate from hydrofluoric acid waste liquid according to claim 1, characterized in that, In step S2, the molar ratio of fluorine in the hydrofluoric acid waste liquid to titanium in the titanic acid is controlled to be 6-7:1; the reactor is made of polytetrafluoroethylene and its initial temperature before use is 15-20℃; the reaction temperature of the hydrofluoric acid waste liquid and the titanic acid powder is 30-35℃ and the reaction time is 2-3h.

6. The method for preparing potassium fluorotitanate from hydrofluoric acid waste liquid according to claim 1, characterized in that, In step S3, the purity of potassium carbonate is ≥99.9%; the molar ratio of potassium carbonate to titanium in the fluorotitanic acid solution is controlled to be 2-3:1; the reaction temperature of the fluorotitanic acid solution and potassium carbonate is 30-40℃, and the reaction time is 1-3h.

7. The method for preparing potassium fluorotitanate from hydrofluoric acid waste liquid according to claim 1, characterized in that, The purification process in step S3 involves first filtering with a 0.45μm polytetrafluoroethylene filter membrane, followed by washing with deionized water.

8. The method for preparing potassium fluorotitanate from hydrofluoric acid waste liquid according to claim 1, characterized in that, In step S4, the crystal surface is rinsed with anhydrous ethanol at 0-10°C, and the rinsing is repeated 2-3 times.

9. The method for preparing potassium fluorotitanate from hydrofluoric acid waste liquid according to claim 1, characterized in that, In step S4, the drying process uses a polytetrafluoroethylene crucible, the drying temperature is 80-90℃, and the drying time is 2-3 hours.

Citation Information

Patent Citations

  • Treatment method of hydrofluoric acid wastewater containing hydrochloric acid

    CN107935008A

  • A method for recovering hydrofluoric acid by comprehensive utilization of fluorine-containing waste acid

    CN117466250B

  • Treatment device and method for waste liquid containing hydrofluoric acid

    CN119874003A

  • System and process of treating fluorhydric acid

    CN1559931A