Antistatic ink, preparation method and application thereof
By introducing a core-shell structure of carbon nanomaterials and polythiophene-based conductive polymers into the PEDOT:PSS coating, the problems of insufficient environmental stability and mechanical properties of the PEDOT:PSS coating are solved, enabling high stability and conductivity applications on a variety of substrates.
Patent Information
- Application Number
- CN202610347318.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-03-20
- Publication Date
- 2026-07-03
Smart Images

Figure CN122326045A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer materials, and more particularly to an antistatic ink. Background Technology
[0002] Poly(3,4-ethylenedioxythiophene)polystyrene sulfonate (PEDOT:PSS), a water-dispersible conductive polymer, is widely used in antistatic coatings due to its high light transmittance and good processability. However, long-term industrial applications have revealed two significant technical bottlenecks in antistatic coatings based on pure PEDOT:PSS:
[0003] (1) Insufficient environmental stability: PEDOT:PSS molecular chains are relatively sensitive to water vapor, oxygen and ultraviolet light. Long-term use in humid and light-exposed environments can easily damage its conductive pathways, leading to a significant increase in surface resistance and a decrease in antistatic performance, making it difficult to meet the requirements of permanent antistatic properties in outdoor or harsh storage environments.
[0004] (2) Poor mechanical deformation resistance: When coated on soft plastic substrates such as PET and PE and subjected to subsequent processing (such as thermoforming and stretching) or deformation during use, the pure PEDOT:PSS coating, due to its inherent brittleness, causes the conductive network to break at a low stretch ratio (usually 3-4 times), resulting in a decrease in surface resistance from the initial 10. 4 -10 6 Ω / □ jumps sharply to 10 7 When the current is above Ω / □, it loses its effective antistatic or electrostatic shielding function, severely limiting its application in scenarios such as flexible electronic packaging and dynamic protective films that require bending and stretching.
[0005] Therefore, developing an antistatic ink that combines excellent environmental stability (resistance to water, oxygen, and UV radiation) with outstanding mechanical deformation resistance (high tensile strength retention) has become a pressing technical problem to be solved in this field. Summary of the Invention
[0006] This invention provides an antistatic ink, its preparation method, and its application, to solve the technical problems of insufficient environmental stability and poor mechanical properties of existing PEDOT:PSS-based antistatic inks.
[0007] To solve the above problems, the technical solution proposed by this invention is as follows: An antistatic ink comprises carbon nanomaterials, a polythiophene-based conductive polymer, and a solvent; the polythiophene-based conductive polymer is adsorbed on the surface of the carbon nanomaterials and forms a core-shell structure.
[0008] The design concept of the above technical solution lies in the unique core-shell structure of conductive polymer-carbon materials. Carbon nanomaterials are encapsulated and interspersed between PEDOT:PSS aggregates, forming a dense physical barrier layer that effectively delays water and oxygen permeation. Simultaneously, carbon nanotubes, as highly efficient UV absorbers, protect the PEDOT:PSS molecular chains from photo-oxidative degradation, thus jointly ensuring the long-term stability of conductivity. Under tensile stress, the relatively brittle PEDOT:PSS phase may develop microcracks. However, the carbon nanotube network, with its high aspect ratio and excellent mechanical strength, can bridge these cracks, providing alternative electron transport paths after local conductive pathways in PEDOT:PSS are interrupted, thereby maintaining the overall conductivity stability of the coating on a macroscopic scale.
[0009] As a further preferred embodiment of the above technical solution, the mass ratio of the carbon nanomaterial to the polythiophene conductive polymer is 1:(1~15).
[0010] As a further preferred embodiment of the above technical solution, the carbon nanomaterial includes at least one of single-walled carbon nanotubes, multi-walled carbon nanotubes, graphene, and conductive carbon black, and is more preferably a single-walled carbon nanotube.
[0011] As a further preferred embodiment of the above technical solution, the polythiophene conductive polymer is PEDOT:PSS with an intrinsic conductivity of 300-650 S / cm.
[0012] As a further preferred embodiment of the above technical solution, the antistatic ink further includes additives, including at least one of conductive enhancers, pH adjusters, binders, leveling agents, wetting agents, coupling agents, lubricants, and defoamers.
[0013] The coupling agent is selected from at least one of silane coupling agents and titanate coupling agents; specifically, it may include at least one of 3-glycidoxypropyltrialkoxysilane, 3-aminopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-methacryloyloxypropyltrimethoxysilane, vinyltrimethoxysilane, octyltriethoxysilane, and crosslinking agents, functional silanes (such as tetraethoxysilane), and alkoxysilane hydrolysates (such as tetraethoxysilane-based hydrolysates). For ink stability and adhesion considerations, 3-glycidoxypropyltrialkoxysilane is further preferred. In this invention, the coupling agent enhances the interaction between the components within the material, improves the overall performance and stability of the material, helps improve ink adhesion, and enhances the water resistance of the film.
[0014] The binder is selected from at least one of acrylic resin, polyurethane resin, and polyester resin. Preferably, it is an aqueous polyurethane dispersion. The leveling agent is selected from at least one of polyether-modified polysiloxane, acrylate polymer, and fluorocarbon polymer.
[0015] The wetting agent is selected from at least one of the following categories: (1) Ethynylene glycol and ethynylene alcohol surfactants; (2) Fluorinated surfactants; (3) Anionic surfactants, including at least one of alkylbenzene sulfonates, alkane sulfonates, sulfosuccinates, phosphate esters and alkyl ether carboxylates.
[0016] The defoamer is selected from at least one of mineral oil-based, polyether-based, and silicone-based defoamers; preferably a silicone-based defoamer, and more preferably a nonionic polysiloxane-polyether copolymer emulsion. The lubricant is selected from silicone-based hand-feeling agents.
[0017] The pH adjuster is selected from at least one of organic amines, inorganic bases, and organic acids; preferably, the pH adjuster is triethanolamine, ammonia, dimethylethanolamine, or imidazole, used to adjust the pH of the antistatic ink to the range of 2.0-7.0.
[0018] As a further preferred embodiment of the above technical solution, based on the total mass of the antistatic ink, the mass percentage of each component is as follows: Carbon nanomaterials: 0.06%~0.10%; Polythiophene conductive polymers: 0.30%~1.00%; Conductivity enhancers: 2.50%~5.00%; pH adjusters: 0.20%~0.50%; Binders: 5.00%~15.00%; Leveling agents: 0.50%~2.00%; Wetting agents: 0.50%~2.00%; Coupling agents: 0.50%~2.00%; Lubricants: 0.50%~2.00%; Defoamers: 0.50%~2.00%; Balance: Solvent.
[0019] As a further preferred embodiment of the above technical solution, the coating formed after the antistatic ink is cured has a surface resistivity ≤1.0×10⁻⁶ after being subjected to an 8-fold stretch. 8 Ω / □; The surface resistivity of the coating formed after curing the antistatic ink changes by ≤10 times after 500h of UV aging.
[0020] Based on the same technical concept, the present invention also provides a method for preparing the antistatic ink described in the above technical solution, comprising the following steps: S1. The carbon nanomaterial raw material is pre-dispersed, then diluted with solvent and dispersed again to obtain a carbon nanomaterial diluted solution. S2. The carbon nanomaterial dilution solution is mixed with the aqueous dispersion of polythiophene conductive polymer, so that the polythiophene conductive polymer is adsorbed on the surface of the carbon nanomaterial and forms a core-shell structure to obtain a pre-composite dispersion. S3. Add solvent and additives to the pre-composite dispersion, mix evenly, and obtain the antistatic ink.
[0021] To achieve the specific structure and the aforementioned antistatic ink effects, this invention particularly emphasizes the pre-composite step. Specifically, carbon nanotubes are first uniformly dispersed in an aqueous medium, and then this dispersion is thoroughly mixed and dispersed with a PEDOT:PSS aqueous dispersion. This step ensures sufficient contact and interaction between the carbon nanotubes and PEDOT:PSS at the nanoscale, a prerequisite for forming a stable, uniform composite conductive network and thus achieving optimal weather resistance and tensile properties. Through prolonged, stepwise shearing and stirring, the aggregated carbon nanotube bundles are physically opened, allowing each individual carbon nanotube or small bundle to be dispersed in the water to the maximum extent. When these fully dispersed nanounits are subsequently mixed with PEDOT:PSS, they can uniformly embed and support the flexible polymer network like tiny reinforcing bars. This uniform nanocomposite structure effectively disperses external stress, prevents crack propagation, and thus significantly improves the toughness, flexibility, and tensile strength of the film.
[0022] As a further preferred embodiment of the above technical solution, in step S1, the carbon nanomaterial raw material is first mechanically stirred and pre-dispersed for 30 minutes, then diluted with solvent at a 1:1 ratio, and dispersed for another 1 hour to obtain a diluted carbon nanomaterial solution. The dilution ratio aims to adjust the high-viscosity slurry to a suitable viscosity and concentration for further dispersion and subsequent mixing, ensuring effective shear force transfer while avoiding secondary agglomeration due to excessive concentration. This ensures the carbon nanomaterial is fully wetted and coated with water, forming a stable diluted dispersion, laying the foundation for the uniform and stable reaction with PEDOT:PSS in the next step. As a further preferred embodiment of the above technical solution, in step S2, the carbon nanomaterial dilution is slowly added to the aqueous dispersion of the polythiophene conductive polymer under stirring conditions. The polythiophene dispersion is pre-dispersed to form a stable colloidal system. After the carbon material is added stepwise, the polythiophene molecular chains can quickly adsorb onto the surface of the carbon material, forming a "polythiophene-carbon material" core-shell structure, preventing carbon material agglomeration and improving the uniformity of system dispersion. The carbon material, as a rigid reinforcing phase, is uniformly dispersed in the polythiophene matrix and can effectively transfer stress. When the cured film is subjected to tensile force, the carbon material particles can hinder crack propagation, while the flexibility of the polythiophene molecular chains can buffer stress, synergistically improving tensile strength and elongation at break. Carbon materials (especially graphene and carbon nanotubes) have excellent ultraviolet shielding properties, which can block ultraviolet light from damaging the polythiophene molecular chains. Simultaneously, the polythiophene coating of the carbon material reduces the contact between the carbon material and air and moisture, lowering the oxidation rate and thus improving overall weather resistance.
[0023] If polythiophene is added to a carbon material dispersion, the carbon material will agglomerate in advance to form a dense aggregate. The polythiophene molecular chains cannot penetrate into the interior of the aggregate and can only adhere to the surface. There are a large number of interfacial voids inside the cured film. When stretched, the stress is concentrated at the voids, resulting in a significant decrease in tensile strength and elongation at break. Ultraviolet light and humid and hot environments can easily penetrate into the interior of the film through the voids, accelerating the degradation of polythiophene and greatly reducing its weather resistance.
[0024] Based on the same technical concept, the present invention also provides an application of the antistatic ink described above in antistatic tape, electronic packaging film, protective film, release film or blister tray.
[0025] Compared with the prior art, the beneficial effects of the present invention are as follows: The antistatic ink of this invention exhibits strong dispersion uniformity and no significant agglomeration of internal components. After film formation, it has a smooth appearance, no mechanical defects, and excellent durability, with a tensile strength and elongation of 800%. It can meet the processing and usage requirements of various films and sheets, and has strong weather resistance. After 500 hours of ultraviolet aging, the surface resistivity change rate is less than 10 times, allowing for long-term application in outdoor or sunlight environments. The preparation process is simple and suitable for large-scale industrial production. Furthermore, it has a wide range of applications, including antistatic conductive films, antistatic tapes, electronic packaging films, protective films, release films, blister trays, and other substrates. Attached Figure Description
[0026] Figure 1 Here is a scanning electron microscope image of the morphology and structure of the antistatic ink in Example 1; Figure 2 The image shows the morphology and structure of the antistatic ink in Comparative Example 2 using a scanning electron microscope. Figure 3 The image shows the morphology and structure of the antistatic ink in Comparative Example 3 using a scanning electron microscope. Detailed Implementation
[0027] The following detailed description is based on embodiments of the present invention, but the present invention can be implemented in many different ways as defined and covered by the claims.
[0028] In the ink curing process of each embodiment and comparative example, the curing agent used can be selected from at least one of isocyanate compounds, aziridine compounds, carbodiimide compounds, oxazoline compounds, epoxy resin compounds, and amino resin compounds. The isocyanate curing agent is selected from at least one of hexamethylene diisocyanate, isophorone diisocyanate, toluene diisocyanate, and their trimers, prepolymers, or end-capped derivatives. The embodiments and comparative examples used a commercially available water-based blocked isocyanate curing agent from LANXESS, and the curing process was identical.
[0029] The table below shows an overview of the comparative experimental system in the specific implementation methods: Table 1. Overview of the comparative experimental system in the specific implementation methods
[0030] Series A: Verification of the Necessity of Core-Shell Structure Example 1: The antistatic ink of this embodiment has the following composition as shown in Table 2, and its morphological structure characterization results are as follows: Figure 1 As shown in the figure, the carbon nanotubes did not agglomerate, but were encapsulated by PEDOT:PSS to form a core-shell structure.
[0031] The method for preparing the antistatic ink in this embodiment includes the following steps: S1. Add PEDOT:PSS polymer aqueous dispersion as a matrix to a non-metallic container (ceramic, plastic, glass, or polytetrafluoroethylene materials are all acceptable); S2. First, disperse and stir the PEDOT:PSS aqueous dispersion at high speed. Then, slowly add dimethyl sulfoxide and imidazole while stirring, and continue stirring until uniform to obtain the PEDOT:PSS dispersion. S3. First, mechanically stir and pre-disperse the single-walled carbon nanotube slurry for 30 minutes. Then, slowly add the pre-dispersed slurry to water at a mass ratio of 1:1 between the slurry and deionized water, and continue stirring for 1 hour to obtain a uniform carbon nanotube dilution. S4. Under stirring conditions, gradually add the PEDOT:PSS dispersion obtained in S2 to the carbon nanotube dilution obtained in S3 to mix and form a uniform pre-composite dispersion. S5. Add polyurethane resin DSM2202 to the pre-composite dispersion and stir thoroughly until the mixture is homogeneous; S6. Finally, add leveling agent MH4205, wetting agent Surfynol 465, coupling agent KH550, lubricant silok9146H, defoamer AC-810, and the remaining deionized water to the mixture in S5 in sequence, and continue stirring until the system is completely homogeneous to obtain the antistatic ink of this embodiment.
[0032] The antistatic ink of this embodiment was printed on the surface of a PET release film and baked at 90°C for 2 minutes to form an 8μm thick conductive layer. The surface resistance was tested to be 6.3E4Ω / □, the tensile strength elongation was 800%, and the surface resistance changed by 10 times after 500h of UV aging.
[0033] Table 2: Components and proportions of the antistatic ink in Example 1
[0034] Comparative Example 1: The inks of this comparative example have the following composition as shown in Table 3, and the preparation method includes the following steps: S1. Add PEDOT:PSS polymer aqueous dispersion to a non-metallic container; S2. Disperse and stir the PEDOT:PSS polymer aqueous dispersion at high speed until uniform, then slowly add the conductivity enhancer and pH adjuster, and continue stirring until uniform; S3. Add polyurethane resin DSM2202 to the mixture in S2 and stir until homogeneous; S4. Add leveling agent MH 4205, wetting agent Surfynol 465, coupling agent DC6400, lubricant DC51, defoamer AC-810S and the balance water to the mixture in S3, stir well to obtain the ink of this comparative example.
[0035] The ink of this comparative example was printed on the surface of a PET release film and baked at 90°C for 2 minutes to form an 8μm thick conductive layer. The surface resistance was tested to be 2E4Ω / □, the tensile strength and elongation were 800%, and the surface resistance basically disappeared after 500h of UV aging.
[0036] Table 3: Components and proportions of the ink in Comparative Example 1
[0037] Table 4: Performance test results of antistatic ink coatings in Example 1 and Comparative Example 1
[0038] Series B: Verification of Key Steps in the Preparation Process (Sequence of Carbon Material Addition) Example 2: The difference between the preparation method of the antistatic ink in this embodiment and that in Example 1 is that in S2, water is slowly added to the pre-dispersed carbon slurry at a mass ratio of 1:1 to deionized water. The coating formed after the antistatic ink is cured is then tested and compared with that in Example 1. The results are shown in Table 5.
[0039] Example 3: The difference between the preparation method of the antistatic ink in this embodiment and that in Example 1 is that in S3, the carbon nanotube dilution obtained in S3 is gradually added to the PEDOT:PSS dispersion obtained in S2 under stirring conditions to form a uniform pre-composite dispersion. The coating formed after the final antistatic ink is cured is tested and compared with that in Example 1. The results are shown in Table 5.
[0040] Table 5: Performance test results of antistatic ink coatings in Examples 1, 2, and 3
[0041] Series C: Validation of Component Synergistic Effect Comparative Example 2: The preparation method of the antistatic ink in this comparative example differs from that in Example 1 in that, in step S3, the single-walled carbon nanotube slurry was directly and slowly added to water at a mass ratio of 1:1 to obtain a carbon material dilution. The morphological and structural characterization results are as follows: Figure 2 As shown.
[0042] The inks of this comparative example have the following composition as shown in Table 6, and the preparation method includes the following steps: S1. In a non-metallic container, add carbon nanotube slurry. First, mechanically stir and pre-disperse the single-walled carbon nanotube slurry for 30 minutes. Then, slowly add water at a ratio of 1:1 between the slurry and deionized water and continue stirring for 1 hour to obtain a uniform carbon nanotube dilution. S2. In a non-metallic container, add polyurethane resin DSM2202 and stir until homogeneous. Then, slowly add leveling agent MH 4205, wetting agent Surfynol 465, coupling agent DC6400, lubricant silok9146H, defoamer AC-810, and the remaining deionized water to obtain a resin composite. S3. Add the single-walled carbon nanotube dilution from S1 to the resin composite from S2, and stir until homogeneous to obtain the ink.
[0043] The ink of this comparative example was printed on the surface of a PET release film and baked at 90°C for 2 minutes to form an 8μm thick conductive layer. The surface resistivity was measured to be 7E6Ω / □, the tensile strength elongation was 800%, and the surface resistivity changed by 0.08 times (the surface resistivity decreased) after 500 hours of UV aging. The coating formed after the antistatic ink was cured was tested and compared with that of Example 1. The results are shown in Table 7.
[0044] Table 6: Components and proportions of the ink in Comparative Example 2
[0045] Table 7: Performance test results of antistatic ink coatings in Example 1 and Comparative Example 2
[0046] Series D: Verification of the Necessity of Process Parameters (Pre-dispersion + Dilution) Comparative Example 3: The preparation method of the antistatic ink in this comparative example differs from that in Example 1 in that, in step S3, the single-walled carbon nanotube slurry was added slowly to water at a 1:1 mass ratio without pre-dispersion to obtain a carbon material dilution. Its morphological and structural characterization results are as follows: Figure 3 As shown, it can be seen that there is a clustering phenomenon in its wire diameter.
[0047] The ink used in this comparative example is prepared using the following steps: S1. Add PEDOT:PSS polymer aqueous dispersion as a matrix to a non-metallic container (ceramic, plastic, glass, or polytetrafluoroethylene materials are all acceptable); S2. First, disperse and stir the PEDOT:PSS aqueous dispersion at high speed. Then, slowly add dimethyl sulfoxide and imidazole while stirring, and continue stirring until uniform to obtain the PEDOT:PSS dispersion. S3. Add the single-walled carbon nanotube slurry to water at a mass ratio of 1:1 (slurry to deionized water) and stir for 30 minutes to obtain a carbon nanotube dilution. S4. Under stirring conditions, gradually add the PEDOT:PSS dispersion obtained in S2 to the carbon nanotube dilution obtained in S3 to mix and form a uniform pre-composite dispersion. S5. Add polyurethane resin DSM2202 to the pre-composite dispersion and stir thoroughly until the mixture is homogeneous; S6. Finally, add leveling agent MH4205, wetting agent Surfynol 465, coupling agent KH550, lubricant silok9146H, defoamer AC-810, and the remaining deionized water to the mixture in S5 in sequence, and continue stirring until the system is completely homogeneous to obtain the antistatic ink of this embodiment.
[0048] The antistatic ink of this embodiment was printed on the surface of a PET release film and baked at 90°C for 2 minutes to form an 8μm thick conductive layer. The surface resistance was tested to be 3E4Ω / □, the tensile strength elongation was 800%, and the surface sheet resistance after stretching could not be measured.
[0049] The coating formed after the antistatic ink was cured was tested and compared with that of Example 1. The results are shown in Table 8.
[0050] Table 8: Performance test results of antistatic ink coatings in Example 1 and Comparative Example 3
[0051] Performance Testing and Comparison To verify the effectiveness of the present invention, four sets of comparative experiments were set up: the experimental groups used Example 1, Example 3, Comparative Example 1, and Comparative Example 2. The raw material components of Example 1 and Example 3 were completely identical, but the premixing methods were different. Comparative Example 1 did not contain carbon materials, while Comparative Example 2 contained only carbon materials. The test results are shown in Table 9 below: (1) Comparison of tensile properties: Table 9: Comparison of tensile properties of some embodiments and comparative examples
[0052] (2) Weather resistance comparison Comparing stretched and unstretched film layers placed in an oven set to a temperature:humidity ratio of 85:85 or outdoors, Table 10 below shows the comparative data of unstretched antistatic film layers placed in a double 85 oven (temperature 85℃, humidity 85%): Table 10: Comparison of weather resistance performance of some embodiments and comparative examples (condition 1)
[0053] Table 11 below shows comparative data for unstretched antistatic film layers placed outdoors: Table 11: Comparison of weather resistance performance of some embodiments and comparative examples (condition 2)
[0054] Table 12 below shows comparative data on the stretching of the membrane when placed outdoors: Table 12: Comparison of weather resistance performance of some embodiments and comparative examples (condition 3)
[0055] The following conclusions can be drawn from the above data: Comparative Example 1, which only uses PEDOT:PSS, has significantly worse tensile and weather resistance properties than Examples 1 and 3.
[0056] A comparison of Examples 1 and 3 further confirms that the carbon material addition process significantly improves the durability and tensile properties of the composite material. The fundamental reason is that this process forms a denser "core-shell" composite structure, effectively blocking the erosion and damage of ultraviolet light.
[0057] While Comparative Example 2 (pure carbon nanotube scheme) showed good weather resistance and stability, its initial electrical properties and tensile properties were inferior to those of Examples 1 and 3. Example 1, with a lower amount of single-walled carbon nanotubes than Comparative Example 3, still achieved similar weather resistance to Comparative Example 3, while achieving a better overall performance balance (including initial electrical conductivity and mechanical properties) thanks to the synergistic effect of PEDOT:PSS and carbon materials.
[0058] The above are merely preferred embodiments of this application and are not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application. The above are merely preferred embodiments of the present invention, and the protection scope of the present invention is not limited to the above embodiments. For those skilled in the art, improvements and modifications obtained without departing from the technical concept of the present invention should also be considered within the protection scope of the present invention.
Claims
1. An antistatic ink, characterized by, It includes carbon nanomaterials, polythiophene-based conductive polymers, and solvents; the polythiophene-based conductive polymers are adsorbed on the surface of the carbon nanomaterials and form a core-shell structure.
2. The antistatic ink according to claim 1, characterized in that, The mass ratio of the carbon nanomaterial to the polythiophene conductive polymer is 1:(1~15).
3. The antistatic ink according to claim 1, characterized in that, The carbon nanomaterials include at least one of single-walled carbon nanotubes, multi-walled carbon nanotubes, graphene, and conductive carbon black.
4. The antistatic ink according to claim 1, characterized by The polythiophene conductive polymer is PEDOT:PSS with an intrinsic conductivity of 300-650 S / cm.
5. The antistatic ink according to any one of claims 1 to 4, characterized in that, The antistatic ink also includes additives, which include at least one of conductive enhancers, pH adjusters, binders, leveling agents, wetting agents, coupling agents, lubricants, and defoamers.
6. The antistatic ink according to claim 5, characterized in that, Based on the total mass of the antistatic ink, the mass percentage of each component is as follows: Carbon nanomaterials: 0.06%~0.10%; Polythiophene conductive polymers: 0.30%~1.00%; Conductivity enhancers: 2.50%~5.00%; pH adjusters: 0.20%~0.50%; Binders: 5.00%~15.00%; Leveling agents: 0.50%~2.00%; Wetting agents: 0.50%~2.00%; Coupling agents: 0.50%~2.00%; Lubricants: 0.50%~2.00%; Defoamers: 0.50%~2.00%; Balance: Solvent.
7. The antistatic ink according to any one of claims 1 to 4, characterized in that, The surface resistance of the coating formed after curing of the antistatic ink is ≤ 1.0 × 10 8 Ω / □; the change rate of the surface resistance of the coating formed after curing of the antistatic ink is ≤ 10 times after 500 h of ultraviolet aging.
8. A method of preparing the antistatic ink according to any one of claims 1 to 7, characterized in that, Includes the following steps: S1. The carbon nanomaterial raw material is pre-dispersed, then diluted with solvent and dispersed again to obtain a carbon nanomaterial diluted solution. S2. The carbon nanomaterial dilution solution is mixed with the aqueous dispersion of polythiophene conductive polymer, so that the polythiophene conductive polymer is adsorbed on the surface of the carbon nanomaterial and forms a core-shell structure to obtain a pre-composite dispersion. S3. Add solvent and additives to the pre-composite dispersion, mix evenly, and obtain the antistatic ink.
9. The preparation method according to claim 8, characterized in that, In step S2, the carbon nanomaterial dilution is added to the aqueous dispersion of the polythiophene conductive polymer under stirring conditions.
10. The application of the antistatic ink according to any one of claims 1-7 in antistatic tape, electronic packaging film, protective film, release film or blister tray.