Co-BASE ALLOY MATERIAL AND Co-BASE ALLOY-MANUFACTURED PRODUCT

A Co-based alloy with controlled Ga and W compositions and microstructures addresses the high cost and interaction issues of FSW, providing superior mechanical properties and compatibility with Al-based materials.

JP2024141766AInactive Publication Date: 2024-10-10MITSUBISHI HEAVY IND LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023053586
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing Co-based alloy materials for friction stir welding (FSW) face high costs due to the use of expensive materials and methods, and there is a need for tools that can join Fe-based alloy materials with other metals like Al-based materials without negative interactions.

Method used

A Co-based alloy material with specific compositions of Ga, W, and other elements, along with controlled microstructures, is developed to provide mechanical properties comparable to Ni-based alloys while suppressing negative interactions with Al-based materials.

Benefits of technology

The Co-based alloy material achieves equivalent or better mechanical properties than conventional Ni-based alloys and prevents adverse interactions with Al-based metals, enabling effective FSW.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141766000001_ABST
    Figure 2024141766000001_ABST
Patent Text Reader

Abstract

To provide a Co-base alloy material and a Co-base alloy-manufactured product which have mechanical properties equal to or more than a Ni-base alloy-manufactured product, and can suppress negative interaction with an Al-base metallic material.SOLUTION: A Co-base alloy material has a chemical composition, wherein the material contains 0.26 to 26 mass% of Ga and 3 to 45 mass% of W, the total of Ga and W by less than 50 mass%, a component having one or more kinds selected from B, C, Y, La, misch metal by 2% or less in total and a component having one or more kinds selected from Cr, Fe, Ni, Mo, Ru, Re, Ir, Ti, Zr, Hf, V, Nb, Ta by 40 mass% or less in total, and the balance of Co with impurities. Segregation cells with average size of 0.15 to 1.5 μm are formed in a mother phase γ-phase crystal grains, γ'-phase particles which contain Co, Ga and W and has a particle diameter of 0.01 to 0.5 μm are dispersedly precipitated in the segregation cells, and μ-phase particles which contain Co and W and has a particle diameter of 0.005 to 2 μm are dispersedly precipitated on a particle boundary on a boundary region of the segregation cells and the γ-phase crystal grains.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a Co-based alloy material and a Co-based alloy product, and more particularly to a Co-based alloy material capable of suppressing negative interactions with Al-based metal materials, and a Co-based alloy product using said material. [Background technology]

[0002] Co (cobalt)-based alloy materials, along with Ni (nickel)-based alloy materials, are representative heat-resistant alloy materials, also called superalloys, and are widely used as components (heat-resistant components) that can be used in high-temperature environments. Co-based alloys have superior corrosion resistance and wear resistance compared to Ni-based alloys. For this reason, Co-based alloys have traditionally been used in turbine blades for gas turbines and steam turbines, combustor components, friction stir welding tools, and the like.

[0003] Friction stir welding (FSW) is a solid-state welding method in which a rotating welding tool is inserted into the area to be welded, stirring and flowing the materials to be welded. Since the heat input is smaller than that of arc welding, FSW has the advantage of being less susceptible to thermal effects (for example, thermal deformation and loss of mechanical strength). Since Al (aluminum)-based alloy materials and Cu (copper)-based alloy materials easily undergo plastic deformation at temperatures of around 600°C, tool steels can be used as welding tools, and FSW is becoming more and more practical.

[0004] On the other hand, when FSW is performed on Fe (iron)-based alloy materials, the temperature during joining is said to rise to 900-1200°C. Since mechanical properties (e.g., strength, toughness, and wear resistance) are required to withstand such temperatures, joining tools made of tool steel cannot be used, and there has been a problem in that practical application has not progressed very quickly.

[0005] To address the problem of FSW of Fe-based alloy materials, for example, Patent Document 1 (JP Patent Publication No. 2003-532543) has been proposed.

[0006] On the other hand, as shown in Patent Document 2 (Patent No. 4996468), research and development is also being conducted on Co-based alloy materials that exhibit heat resistance comparable to Ni-based alloy materials precipitation-strengthened by the γ' phase (e.g., Ni3(Al,Ti) phase) and also have excellent structural stability. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Special Publication No. 2003-532543 [Patent Document 2] Patent No. 4996468 [Patent Document 3] Patent application No. 2021-142631

[0008] Patent Document 3 will be described later. Summary of the Invention [Problem to be solved by the invention]

[0009] According to Patent Document 1, by using the FSW tool, MMCs, ferrous alloys, non-ferrous alloys and superalloys can be friction stir welded. However, the FSW tool of Patent Document 1 is very expensive because it uses high-cost materials and is manufactured by a high-cost method. Therefore, there is a strong demand for reducing the cost of FSW tools for Fe-based alloy materials.

[0010] Meanwhile, in recent years, in addition to FSW between Fe-based alloy materials, there has been a very strong demand for FSW between Fe-based alloy materials and other metal materials (for example, FSW between Fe-based alloy materials and Al-based metal materials).

[0011] According to Patent Document 2, a Co-based alloy in which an appropriate amount of γ' phase with an appropriate grain size is precipitated in the γ phase exhibits heat resistance comparable to that of precipitation-strengthened Ni-based alloy materials and good mechanical properties (e.g., 0.2% yield strength, tensile strength, Vickers hardness). For this reason, the Co-based alloy of Patent Document 2 may be applicable as a material for a tool for FSW between Fe-based alloy materials. In addition, if a tool for FSW is manufactured using this Co-based alloy, it is considered that a lower cost can be realized than the FSW tool of Patent Document 1.

[0012] However, when considering joining of an Fe-based alloy material and an Al-based metal material as the FSW of an Fe-based alloy material and another metal material, there is a concern that the Al component constituting the Co-based alloy of Patent Document 2 may negatively interact with the Al-based metal material being joined.

[0013] The present invention has been made in consideration of the above points, and its object is to provide a Co-based alloy material that has mechanical properties equal to or greater than those of conventional Ni-based alloy products and can suppress negative interactions with Al-based metal materials, and a Co-based alloy product using said material. [Means for solving the problem]

[0014] (I) One aspect of the present invention is a Co-based alloy material, Contains 0.26% by mass or more and 26% by mass or less of Ga (gallium) and 3% by mass or more and 45% by mass or less of W (tungsten), the sum of the Ga and the W being less than 50% by mass; An E1 component consisting of one or more selected from B (boron), C (carbon), Y (yttrium), La (lanthanum), and misch metals, the total amount of which is 2 mass% or less; and one or more E2 components selected from Cr (chromium), Fe, Ni, Mo (molybdenum), Ru (ruthenium), Re (rhenium), Ir (iridium), Ti (titanium), Zr (zirconium), Hf (hafnium), V (vanadium), Nb (niobium), and Ta (tantalum) in a total amount of 40 mass% or less, The present invention provides a Co-based alloy material having a chemical composition with the balance being Co and impurities.

[0015] In the present invention, the following improvements and modifications can be freely combined in the above Co-based alloy material (I). (i) the chemical composition includes 2 mass% or more and 20 mass% or less of the Ga, 5 mass% or more and 35 mass% or less of the W, 40 mass% or less of the Ni, 20 mass% or less of the Cr, 15 mass% or less of the Ta, 1 mass% or less of the C, and 0.5 mass% or less of the B, The balance consists of Co and the impurities. (ii) the chemical composition includes 5% by mass or more and 15% by mass or less of the Ga, 10% by mass or more and 30% by mass or less of the W, 15% by mass or more and 35% by mass or less of the Ni, 3% by mass or more and 15% by mass or less of the Cr, 1% by mass or more and 10% by mass or less of the Ta, 0.05% by mass or more and 0.2% by mass or less of the C, and 0.001% by mass or more and 0.1% by mass or less of the B, The balance consists of Co and the impurities. (iii) The chemical composition contains 0.05 mass % or less of O (oxygen) as the impurity. (iv) segregation cells having an average size of 0.15 μm or more and 1.5 μm or less are formed in the γ (gamma) phase crystal grains which are the parent phase of the Co-based alloy material; In the segregation cells, γ' (gamma prime) phase particles containing the Co, the Ga, and the W and having a particle size of 0.01 μm or more and 0.5 μm or less are dispersed and precipitated, In the boundary regions of the segregation cells and on the grain boundaries of the γ-phase crystal grains, μ (mu) phase particles containing the Co and the W and having a grain size of 0.005 μm or more and 2 μm or less are dispersed and precipitated.

[0016] (II) Another aspect of the present invention is a Co-based alloy product, The Co-based alloy product is made of the above-mentioned Co-based alloy material, The Co-based alloy product has a γ-phase crystal grain as a parent phase, and segregation cells having an average size of 0.15 μm or more and 1.5 μm or less are formed in the γ-phase crystal grain. in the segregation cells, γ' phase particles containing the Co, the Ga, and the W and having a particle size of 0.01 μm or more and 0.5 μm or less are dispersed and precipitated, The present invention provides a Co-based alloy product, characterized in that μ-phase particles containing the Co and the W and having a particle size of 0.005 μm or more and 2 μm or less are dispersed and precipitated in the boundary regions of the segregation cells and on the grain boundaries of the γ-phase crystal grains.

[0017] (III) Another aspect of the present invention is a Co-based alloy product, The Co-based alloy product is made of the above-mentioned Co-based alloy material and is a polycrystalline body of γ-phase crystal grains having an average grain size of 10 μm or more and 100 μm or less, In the γ-phase crystal grains, γ'-phase particles containing the Co, the Ga, and the W and having a grain size of 0.01 μm or more and 1 μm or less are dispersed and precipitated in a range of 40 vol % or more and 85 vol % or less, The present invention provides a Co-based alloy product, characterized in that within the γ-phase crystal grains and on the grain boundaries, μ-phase particles containing the Co and the W and having a grain size of 0.005 μm or more and 20 μm or less are dispersed and precipitated with an average interparticle distance of 0.15 μm or more and 100 μm or less.

[0018] In the present invention, the sizes of the γ phase, γ' phase, μ phase, and segregation cells are measured using image processing software (e.g., ImageJ, public domain software developed by the National Institutes of Health, USA) on the microstructure observation image. In ImageJ, the shape of the measurement object is approximated to a circle, ellipse, rectangle, etc., and the size is calculated. In the present invention, after shape approximation is performed for each measurement object in the microstructure observation image, the maximum and minimum lengths of the measurement object are measured, and the average value of these is regarded as the size of the measurement object. The average size is the average value of the sizes of about 50 measurement objects in one observation image.

[0019] In the present invention, the average interparticle distance of the μ phase is determined by using image processing software on a microstructure observation image to search for μ phase particles radially from the coordinates of the center of gravity of a μ phase particle of interest, and averaging the distances between the centers of gravity of adjacent μ phase particles.

[0020] In the present invention, the above Co-based alloy products (II) and (III) can be improved or modified as follows. (v) The Co-based alloy product is a friction stir welding tool. Effect of the Invention

[0021] According to the present invention, it is possible to provide a Co-based alloy material that has mechanical properties equal to or greater than those of conventional Ni-based alloy products and can suppress negative interactions with Al-based metal materials, and a Co-based alloy product using said material. [Brief description of the drawings]

[0022] [Figure 1] FIG. 1 is a flow chart showing an example of a process for producing a Co-based alloy product according to the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an example of the microstructure of the Co-based alloy powder obtained in the starting material preparation step. [Diagram 3] FIG. 2 is a schematic diagram showing an example of the microstructure of a Co-based alloy product obtained in an aging treatment step. [Figure 4] FIG. 1 is a schematic perspective view showing an example of a Co-based alloy product according to the present invention, and shows a tool for FSW. [Diagram 5] FIG. 2 is a schematic perspective view showing another example of a Co-based alloy product according to the present invention, which is a turbine vane serving as a heat-resistant member. [Figure 6] 1 is a schematic cross-sectional view showing an example of a gas turbine equipped with a Co-based alloy product according to the present invention. [Figure 7] FIG. 2 is a schematic perspective view showing a heat exchanger as a heat-resistant member, which is another example of a Co-based alloy product according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] [Basic concept of the present invention] Co-based alloy materials generally have a melting point 50 to 100°C higher than Ni-based alloy materials, and the diffusion coefficient of substitutional elements is smaller than that of Ni-based alloys, so that there is little structural change during use at high temperatures. In addition, Co-based alloy materials have a higher ductility than Ni-based alloy materials, so that plastic processing such as forging, rolling, and pressing is easy. Furthermore, Co-based alloy materials have an elastic modulus of about 220 to 230 GPa, which is more than 10% larger than that of Ni-based alloy materials, which is about 200 GPa. Due to these characteristics, Co-based alloy materials are expected to be used in a wider range of applications than Ni-based alloy materials.

[0024] For example, Co-based alloy materials can be used not only for heat-resistant components, but also for applications requiring high strength and high elasticity, such as springs, wires, belts, cable guides, etc. Furthermore, since Co-based alloy materials are hard and have excellent wear resistance, they are also considered to be suitable as tool materials for FSW.

[0025] In Co-based alloy materials, Co3Ti phase, Co3Ta phase, Co3(Al,W) phase, etc. are known as precipitation strengthening phases corresponding to the γ' phase (e.g. Ni3Al phase) of the L12 structure in Ni-based alloy materials. However, the Co3Ti phase and Co3Ta phase have a lattice constant mismatch of 1% or more with the parent γ phase, which is disadvantageous in terms of creep resistance. In contrast, the Co3(Al,W) phase has a mismatch with the γ phase of about 0.5% or less, making it a suitable precipitation strengthening phase.

[0026] However, it is known that Co-based alloy materials are prone to the precipitation of undesired heterophases (e.g., the μ phase, a type of TCP [Topologically Close Packed phases]) when the alloy composition and / or manufacturing process deviate from the preferred range, and that when such heterophases coarsen, the mechanical properties of the alloy material are significantly impaired.

[0027] Patent Document 3 (Patent Application No. 2021-142631) studies a method for suppressing the precipitation and coarsening of unwanted heterogeneous phases, with the aim of obtaining mechanical properties equal to or better than conventional ones and suppressing the decline in manufacturing yield more than conventional ones. As a result of the study, it was found that although it is difficult to completely prevent the precipitation of unwanted heterogeneous phases, the precipitation of the heterogeneous phases can be finely dispersed by rapidly solidifying the molten alloy material, and the negative effects of the heterogeneous phases can be suppressed.

[0028] On the other hand, the inventors prepared an FSW tool made of a Co-based alloy material in which the Co3(Al,W) phase was finely dispersed and precipitated, and performed an FSW experiment between an Fe-based alloy material and an Al-based metal material. As a result, poor joining occurred and the expected level of joining was not achieved.

[0029] In addition, when an FSW tool made of a Ni-based alloy material in which the Ni3(Al,Ti) phase is finely dispersed and precipitated is used, the same results as above were obtained because the Ni-based alloy material contains Al components.

[0030] Therefore, we conducted extensive research into Co-based alloy materials that have mechanical properties equal to or greater than those of Ni-based alloy materials but do not contain Al components. As a result, we found that a Co-based alloy material in which the Co3(Ga,W) phase and its solid solution phase (a phase in which the A site and part of the B site of an A3B type compound are replaced with other elements) are finely dispersed and precipitated, and a product using the same, meets the desired properties. The present invention was completed based on this finding.

[0031] Hereinafter, the embodiments of the present invention will be described along with the manufacturing procedure of a Co-based alloy product with reference to the drawings. However, the present invention is not limited to the embodiments described here, and can be appropriately combined with known techniques or improved based on known techniques within the scope of the technical idea of ​​the invention. For example, the application and uses of the present invention are not limited to the following description.

[0032] [Method of manufacturing Co-based alloy] 1 is a flow diagram showing an example of a process for producing a Co-based alloy product according to the present invention. The process for producing a Co-based alloy product according to the present invention generally includes a starting material preparation step S1 for preparing a starting material for the Co-based alloy product (i.e., a Co-based alloy material), an alloy article formation step S2 for forming an alloy article of a desired shape using the prepared starting material, and an aging treatment step S3 for performing an aging treatment on the obtained alloy article to precipitate a desired amount of precipitation strengthening phase particles in the matrix crystal grains.

[0033] The starting material obtained in step S1 is one form of the Co-based alloy material according to the present invention, and the alloy article obtained in step S2 and the aged article obtained in step S3 are one form of the Co-based alloy product according to the present invention.

[0034] If necessary, the aged article obtained in step S3 may be further subjected to a surface treatment step S4 for surface finishing. Step S4 is not an essential step, but may be performed in consideration of the shape and use environment of the Co-based alloy product. The aged article subjected to step S4 is also one embodiment of the Co-based alloy product according to the present invention.

[0035] Each step will be described in more detail below.

[0036] (Starting material preparation process) The starting material preparation step S1 is a step of preparing a Co-based alloy material. Basically, conventional alloy manufacturing methods and techniques can be used as the method and technique for preparing the starting material. For example, a master alloy ingot preparation step S1a may be performed in which raw materials are mixed, melted, and cast to produce a master alloy ingot having a desired chemical composition, and an atomization step S1b may be further performed in which alloy powder is formed from the master alloy ingot.

[0037] The Co-based alloy material according to the present invention has a chemical composition comprising 0.26% by mass or more and 26% by mass or less of Ga, 3% by mass or more and 45% by mass or less of W, the total of Ga and W being less than 50% by mass, one or more selected from B, C, Y, La, and misch metals, totaling 2% by mass or less of E1 components, one or more selected from Cr, Fe, Ni, Mo, Ru, Re, Ir, Ti, Zr, Hf, V, Nb, and Ta, totaling 40% by mass or less of E2 components, with the balance being Co and impurities, including 0.05% by mass or less of O.

[0038] By having the above chemical composition, in the alloy article obtained in step S2, segregation cells having an average size of 0.15 μm or more and 1.5 μm or less are formed in the γ phase crystal grains that serve as the parent phase, and in the segregation cells, particles of the γ' phase (Co3(Ga,W) phase and its solid solution phase) having a grain size of 0.01 μm or more and 0.5 μm or less and having an L12 type structure are dispersed and precipitated as a precipitation strengthening phase, and a fine structure is obtained in which μ phase particles containing Co and W and having a grain size of 0.005 μm or more and 2 μm or less are dispersed and precipitated in the boundary regions of the segregation cells and on the grain boundaries of the γ phase crystal grains.

[0039] In addition, by having the above chemical composition, in the aging-treated article obtained in step S3, a fine structure is obtained in which the parent phase gamma phase crystal grains have an average grain size of 10 μm or more and 100 μm or less, and within the gamma phase crystal grains, particles of the L12 type structure gamma' phase (Co3(Ga,W) phase and its solid solution phase) having a grain size of 0.01 μm or more and 0.5 μm or less are dispersed and precipitated as a precipitation-strengthened phase in a range of 40 volume % or more and 85 volume % or less, and μ phase particles containing Co and W and having a grain size of 0.005 μm or more and 2 μm or less are dispersed and precipitated within and on the grain boundaries of the gamma phase crystal grains with an average interparticle distance of 0.15 μm or more and 100 μm or less.

[0040] The solid solution phase of Co3(Ga,W) can be expressed as (Co,X)3(Ga,W,Z), where X is Cr, Fe, Ru, Re and / or Ir, Z is Mo, Ti, Zr, Hf, V, Nb and / or Ta, and Ni can be both X and Z.

[0041] The chemical composition of Co-based alloy materials is explained.

[0042] Ga: 0.26 mass% or more and 26 mass% or less Ga is an essential component of the γ' phase, which is a precipitation strengthening phase, and also contributes to improving oxidation resistance. The Ga content is preferably 0.26% by mass or more and 26% by mass or less, more preferably 2% by mass or more and 20% by mass or less, and even more preferably 5% by mass or more and 15% by mass or less. If the Ga content is less than 0.26% by mass, the amount of precipitation of the γ' phase becomes insufficient and does not contribute to precipitation strengthening. On the other hand, if the Ga content exceeds 26% by mass, it promotes the formation of a hard and brittle heterophase.

[0043] W: 3% by mass or more and 45% by mass or less W is an essential component of the γ' phase and also has the effect of solid solution strengthening the γ phase. The W content is preferably 3% by mass or more and 45% by mass or less, more preferably 5% by mass or more and 35% by mass or less, and even more preferably 10% by mass or more and 30% by mass or less. If the W content is less than 3% by mass, the amount of precipitation of the γ' phase becomes insufficient and does not contribute to precipitation strengthening. On the other hand, if the W content exceeds 45% by mass, it promotes the formation of a hard and brittle heterophase.

[0044] Total of Ga and W: less than 50% by mass The total of Ga and W is preferably less than 50 mass%, more preferably 40 mass% or less, and even more preferably 35 mass% or less. If the total of Al and W exceeds 50 mass%, it promotes the formation of a hard and brittle heterogeneous phase.

[0045] E1 component: 2% by mass or less The E1 component is composed of one or more selected from B, C, Y, La, and misch metal, and is an optional component that can be added in a total amount of 2 mass% or less. If added, the total amount is preferably 0.001 mass% or more. Each E1 component will be described.

[0046] B: 0.5% by mass or less B is a component that contributes to improving the bonding of crystal grain boundaries (so-called grain boundary strengthening) and contributes to improving high-temperature strength. B is not an essential component, but when it is contained, it is preferably 0.001 mass% or more and 0.5 mass% or less, and more preferably 0.002 mass% or more and 0.1 mass% or less. If the B content exceeds 0.5 mass%, cracks are likely to occur during the formation of the additive manufacturing body.

[0047] C: 1% by mass or less C, like B, is a component that contributes to strengthening grain boundaries, and when it generates fine particles of MC type carbides (M is a transition metal, C is carbon) and disperses and precipitates, it contributes to improving mechanical strength. C is not an essential component, but when it is contained, it is preferably 0.001 mass% to 1 mass%, more preferably 0.01 mass% to 0.5 mass%, and even more preferably 0.05 mass% to 0.2 mass%. If the C content exceeds 1 mass%, carbides other than MC type carbides will be excessively precipitated or the alloy will be excessively hardened, reducing the toughness of the alloy material.

[0048] Y, La, Misch metal: 1% by mass or less each Y, La, and misch metal are all components that are effective in improving oxidation resistance. Y, La, and misch metal are not essential components, but when they are contained, their respective contents are preferably 0.01% by mass or more and 1% by mass or less, and more preferably 0.05% by mass or more and 0.5% by mass or less. If the content of these components exceeds 1% by mass, it may have a negative effect on the structural stability.

[0049] E2 component: 40% by mass or less The E2 component is an optional component that is composed of one or more selected from Cr, Fe, Ni, Mo, Ru, Re, Ir, Ti, Zr, Hf, V, Nb, and Ta, and can be added in a range of 0.1 mass% to 40 mass% in total. If added, it is preferable that the total amount is 0.1 mass% or more. Each E2 component will be explained.

[0050] The E2 component is a component that can dissolve in both the γ phase and the γ' phase. The distribution coefficient of the x element in the γ phase relative to the γ phase is "Kx γ’ / γ =Cx γ’ / Cxγ " " γ’ : atomic percent concentration of x element in γ' phase, Cx γ It is expressed as (x: atomic percent concentration of element x in the γ phase). A "distribution coefficient ≧1" means that the element stabilizes the γ' phase, and a "distribution coefficient <1" means that the element stabilizes the γ phase. For example, Mo, Ti, V, Nb, and Ta are elements with a "distribution coefficient ≧1" and contribute to the stabilization of the γ' phase.

[0051] Cr: 20% by mass or less Cr is a component with a "distribution coefficient <1" and forms an oxide film (Cr2O3) on the surface of the alloy product, contributing to improved corrosion resistance and oxidation resistance. Cr is not an essential component, but if it is contained, it is preferably 1% by mass to 20% by mass, more preferably 3% by mass to 15% by mass, and even more preferably 6% by mass to 10% by mass. If the Cr content exceeds 20% by mass, it promotes the formation of a σ phase, which is a type of heterophase, and mechanical properties (toughness, ductility, strength) decrease.

[0052] Fe: 10% by mass or less Fe is a component that contributes to improving workability by substituting Co. Fe is not an essential component, but if it is contained, it is preferably 1 mass% to 10 mass%, more preferably 2 mass% to 5 mass%. If the Fe content exceeds 10 mass%, it causes the structure to become unstable at high temperatures.

[0053] Ni: 40% by mass or less Ni is a component that improves the high-temperature stability of the γ' phase by substituting Co, Ga, and W that constitute the γ' phase, and also contributes to improving the heat resistance and / or corrosion resistance of the alloy material. Ni is not an essential component, but when it is contained, it is preferably 1 mass% to 40 mass%, more preferably 10 mass% to 38 mass%, and even more preferably 15 mass% to 35 mass%. If the Ni content exceeds 40 mass%, the wear resistance and resistance to local stress, which are characteristics of Co-based alloy materials, decrease.

[0054] Mo: 15% by mass or less Mo is a component with a "distribution coefficient ≧1", so it contributes to stabilizing the γ' phase and also has the effect of solid solution strengthening the γ phase. Mo is not an essential component, but if it is contained, it is preferably 1% by mass to 15% by mass, and more preferably 2% by mass to 10% by mass. If the Mo content exceeds 15% by mass, it promotes the formation of the σ phase, resulting in a decrease in mechanical properties (toughness, ductility, strength).

[0055] Ru, Re: 10% by mass or less Ru and Re are components effective in improving oxidation resistance. Ru and Re are not essential components, but when they are contained, their respective contents are preferably 0.5% by mass or more and 10% by mass or less, and more preferably 1% by mass or more and 5% by mass or less. If the Ru content or Re content exceeds 10% by mass, it promotes the formation of heterogeneous phases.

[0056] Ir: 40% by mass or less Ir is a component that easily substitutes for Co in the γ' phase and contributes to improving corrosion resistance and oxidation resistance. Ir is not an essential component, but when it is contained, it is preferably 1 mass% to 40 mass%, more preferably 5 mass% to 35 mass%. If the Ir content exceeds 50 mass%, it promotes the formation of heterogeneous phases.

[0057] Ti, Zr, Hf, V: 10 mass% or less each, Nb, Ta: 20 mass% or less each Ti, Zr, Hf, V, Nb, and Ta are components with a "distribution coefficient ≧1", so they contribute to stabilizing the γ' phase and improving mechanical properties. Ti, Zr, Hf, V, Nb, and Ta are not essential components, but when Ti is contained, it is preferably 0.5% by mass to 10% by mass, and more preferably 1% by mass to 5% by mass. When Zr is contained, it is preferably 1% by mass to 10% by mass, and more preferably 2% by mass to 7% by mass. When Hf is contained, it is preferably 1% by mass to 10% by mass, and more preferably 2% by mass to 7% by mass. When V is contained, it is preferably 0.5% by mass to 10% by mass, and more preferably 1% by mass to 5% by mass. When Nb is contained, it is preferably 1% by mass to 20% by mass, more preferably 2% by mass to 15% by mass, and even more preferably 3% by mass to 8% by mass. When Ta is contained, it is preferably 1% by mass or more and 20% by mass or less, more preferably 1.5% by mass or more and 15% by mass or less, and even more preferably 2% by mass or more and 10% by mass or less. Ta has a higher effect of stabilizing the γ' phase than other components, so it is particularly preferable to contain Ta.

[0058] O: 0.05% by mass or less In alloy materials, O is usually an impurity component, but in the Co-based alloy material of the present invention, O is an allowable component in the range of 0.05 mass% or less from the viewpoint of microstructure control (for example, suppression of coarsening of γ-phase crystal grains). When O is intentionally contained, the O content is preferably 0.007 mass% (70 ppm) or more and 0.05 mass% or less (500 ppm), more preferably 0.009 mass% or more and 0.04 mass% or less, and even more preferably 0.011 mass% or more and 0.03 mass% or less. When suppression of coarsening of γ-phase crystal grains is performed by a method other than chemical composition control, the O content may be less than 0.007 mass%. On the other hand, if the O content exceeds 0.05 mass%, coarse oxide particles are formed, which causes deterioration of mechanical properties.

[0059] When the O component is intentionally contained, it is preferable to control the O content in the atomizing element step S1b. The atomizing method can be any conventional method or technique except for controlling the O content in the Co-based alloy material. For example, gas atomizing or centrifugal atomizing while controlling the amount of oxygen (O2 partial pressure) in the atomizing atmosphere can be preferably used. The element step S1b produces alloy powder with nearly spherical particles.

[0060] The alloy powder obtained in step S1 contains more O components as a chemical composition than conventional Co-based alloy materials (the O components are controlled to be more abundant). From this, it is considered that in the Co-based alloy powder according to the present invention, when the alloy melt solidifies into powder particles, the O atoms contained in the powder combine with the metal atoms of the alloy to form extremely small oxides locally. The heterogeneous interface resulting from the oxide generation is likely to become the starting point for solidification of the alloy melt (the nucleation site of γ-phase crystals). As a result, each particle of the alloy powder is basically a polycrystalline body of γ-phase fine crystals, and the average crystal grain size of the γ-phase fine crystals is about 5 to 50 μm. Note that the present invention does not deny the presence of particles consisting of single crystal bodies of γ-phase crystals in the alloy powder.

[0061] Here, the grain size of the alloy powder is preferably 0.3 μm to 90 μm, more preferably 1 μm to 70 μm, and even more preferably 5 μm to 50 μm, from the viewpoint of the handleability in the next alloy article forming step S2 and the shape precision of the alloy article. If the grain size of the alloy powder is less than 0.3 μm, the flowability of the alloy powder decreases in the next step S2, which causes a decrease in the moldability of the alloy article. On the other hand, if the grain size of the alloy powder exceeds 90 μm, this causes an increase in the surface roughness of the alloy article in the next step S2 and a decrease in the shape precision.

[0062] In view of the above, when the Co-based alloy material is powdered, it is preferable to carry out an alloy powder classification step S1c in which the particle size of the powder is classified into a range of 0.3 μm to 90 μm. In the present invention, this step S1c is also considered to have been carried out when the particle size distribution of the obtained alloy powder is measured with a laser diffraction / scattering type particle size distribution analyzer and confirmed to be within the desired range.

[0063] In the present invention, the particle size range of 0.3 to 90 μm is defined as 90 mass % or more of the alloy powder having a particle size in the range of 0.3 μm to 90 μm. When metal powder flow rate measurement (hole flow test) is performed on 50 g of classified powder having a particle size of 15 μm to 45 μm in accordance with JIS Z 2502:2012, the flow rate (the time required for the powder to flow out of a specified orifice) is preferably 15 seconds to 30 seconds.

[0064] (Microstructure of Co-based alloy powder) Fig. 2 is a schematic diagram showing an example of the microstructure of the Co-based alloy powder obtained in the starting material preparation step S1. The schematic diagram in Fig. 2 depicts a cross-section of an alloy powder particle observed with a scanning electron microscope-energy dispersive X-ray analyzer (SEM-EDX). From the microstructure observation, it was confirmed that the alloy powder particle is a polycrystalline body of γ-phase fine crystals with an average crystal grain size of 5 μm to 50 μm, and that extremely small cells with an average size of 0.15 μm to 1.5 μm are formed within the fine crystal grains of the polycrystalline body.

[0065] It was confirmed that there was a difference in brightness between the inside of the microcell and the boundary region between the cells (the outer peripheral region of the microcell, the region such as the cell wall) in the backscattered electron image of the SEM. This means that there is a difference in the average composition inside the cell and the average composition in the boundary region (for example, this means that some components are unevenly distributed in the boundary region and other components are unevenly distributed inside the cell). In this invention, such a microcell in which alloy components are unevenly distributed inside the cell or in the boundary region is called a "segregation cell."

[0066] It was also confirmed that γ'-phase particles (particles based on Co3(Ga,W)) with a grain size of 0.01 μm or more and 0.5 μm or less were dispersed and precipitated inside the segregation cells, and μ-phase particles (particles based on Co3W2) with a grain size of 0.005 μm or more and 2 μm or less were dispersed and precipitated on the boundary regions of the segregation cells and on the grain boundaries of the γ-phase microcrystals.

[0067] The amount of γ' phase particles precipitated was calculated by image analysis using image processing software (ImageJ) for the obtained electron microscope images, and was found to be less than 40% by volume, which was less than the amount estimated from the alloy composition. This is believed to be due to the fact that the alloy powder particles were formed by rapid solidification and that the components that make up the γ' phase segregated on the boundary regions of the segregation cells.

[0068] (Alloy article forming process) The alloy article forming step S2 is a step of forming an alloy article of a desired shape using the Co-based alloy material prepared in step S1. There is no particular limitation on the method of forming the alloy article, and for example, an AM elementary step S2a in which an alloy article is formed by an additive manufacturing (AM) method using an alloy powder, a HIP elementary step S2b in which an alloy article is formed by a hot isostatic pressing (HIP) method using an alloy powder, or a forging elementary step S2c in which an alloy article is formed by a forging method using an alloy ingot can be suitably used. As the AM method, a powder bed fusion (PBF) method and a directed energy deposition (DED) method can be suitably used.

[0069] (Microstructure of alloy article) The microstructure of the alloy article obtained by the PBF method in step S2 was observed using SEM-EDX. Although not shown in the figure, the microstructure observed was almost the same as that in Figure 2. This result is due to the fact that additive manufacturing by the PBF method is based on local melting and rapid solidification of the alloy powder bed.

[0070] The present invention involves controlling the microstructure of an alloy article that serves as a precursor to a final Co-base alloy product in step S2 to obtain a desired microstructure in the final Co-base alloy product, and controlling the chemical composition and microstructure of the Co-base alloy material in step S1 to control the microstructure of the alloy article.

[0071] (Aging treatment process) The aging treatment step S3 is a step of performing an aging treatment on the alloy article obtained in step S2 to precipitate a desired amount of γ' phase particles in the γ phase crystal grains. The temperature of the aging treatment is preferably 500°C or higher and lower than 1100°C, more preferably 500°C or higher and 1000°C or lower, and even more preferably 500°C or higher and 900°C or lower.

[0072] The aging treatment may be a single-stage heat treatment performed at one temperature within the temperature range, or a multi-stage heat treatment performed at multiple temperatures. For example, a preferred schedule is a first aging treatment performed at a temperature range of 500°C to 700°C, followed by a second aging treatment at a temperature range of 600°C to 800°C that is higher than the temperature of the first aging treatment. The holding time of the heat treatment may be appropriately set in consideration of the heat capacity of the heat-treated material. The Co-based alloy product according to the present invention is obtained by step S3.

[0073] (Microstructure of Co-based alloy products) FIG. 3 is a schematic diagram showing an example of the microstructure of the Co-based alloy product obtained in the aging treatment step S3. The schematic diagram of FIG. 3 is a diagram showing the cross section of the alloy product observed by SEM-EDX, similar to FIG. 2. From the microstructure observation, it was confirmed that the alloy product is composed of a polycrystalline body of γ-phase crystal grains having an average grain size of 10 μm to 100 μm, γ'-phase grains having a grain size of 0.01 μm to 1 μm are dispersed and precipitated in the γ-phase grains, and μ-phase grains having a grain size of 0.005 μm to 20 μm are dispersed and precipitated in the γ-phase grains and on the grain boundaries with an average interparticle distance of 0.15 μm to 100 μm. In addition, the boundary region of the segregation cells as shown in FIG. 2 was not visible.

[0074] The amount of γ'-phase particles precipitated was calculated by image analysis using ImageJ for the obtained electron microscope images, and was found to be 40% by volume or more, which was consistent with the amount of precipitation estimated from the alloy composition. This is due to a combination of factors including the fact that the components present in the boundary regions of the segregation cells diffused along the boundary regions to form γ'-phase particles as a result of the aging heat treatment in step S3, the fact that the γ-phase crystal grains grew due to the rearrangement of atoms (recrystallization of the γ-phase), and the fact that the heat treatment temperature was lower than the solid solution temperature of the γ' phase, which inhibited the growth of μ-phase particles.

[0075] (Effects of the embodiment) As described above, the Co-based alloy product and the manufacturing method of the present invention can be said to have mechanical properties equivalent to those of the conventional technology because γ'-phase particles are finely dispersed and precipitated in the γ-phase crystal grains. In addition, the μ-phase, which impairs mechanical properties and manufacturing yield, is finely dispersed without being coarsened, so that the manufacturing yield can be improved compared to the conventional technology.

[0076] [Co-based alloy products] 4 is a perspective schematic diagram showing an example of a Co-based alloy product according to the present invention, which is an FSW tool. By using the Co-based alloy material of the present invention, the FSW tool 100 can fully enjoy the advantages of the Co-based alloy, such as excellent heat resistance, high strength, hardness, and wear resistance, and can also suppress negative interactions with Al-based metal materials.

[0077] The Co-based alloy product according to the present invention is not limited to use in FSW tools, but can also be applied to members (heat-resistant members) used in high-temperature environments.

[0078] For example, Fig. 5 is a schematic perspective view showing a turbine vane as a heat-resistant member, which is another example of the Co-based alloy product according to the present invention. The turbine vane 200 is generally composed of an inner ring endwall 220, a blade portion 210, and an outer ring endwall 230. A cooling structure is often formed inside the blade portion. The Co-based alloy product according to the present invention may be used as a turbine blade.

[0079] Fig. 6 is a schematic cross-sectional view showing an example of a gas turbine equipped with the Co-based alloy product according to the present invention. The gas turbine 300 is generally composed of a compressor section 310 that compresses intake air and a turbine section 320 that blows fuel combustion gas against turbine blades to obtain rotational power. The heat-resistant member of the present invention can be suitably used as a turbine nozzle 321, a turbine vane 200, or a turbine rotor blade 322 in the turbine section 320. The heat-resistant member of the present invention is not limited to gas turbine use, and may be used for other turbines (for example, steam turbines), or may be a member used in a high-temperature environment in other machines / devices.

[0080] 7 is a perspective schematic diagram showing a heat exchanger as a heat-resistant member, which is another example of the Co-based alloy product according to the present invention. The heat exchanger 400 is an example of a plate-fin type heat exchanger, and basically has a structure in which a separation layer 410 and a fin layer 420 are alternately laminated. Both ends of the fin layer 420 in the flow path width direction are sealed with a side bar portion 430. By alternately circulating a high-temperature fluid and a low-temperature fluid through the adjacent fin layers 420, heat exchange is performed between the high-temperature fluid and the low-temperature fluid.

[0081] When the heat exchanger 400 is manufactured by additive manufacturing, the components of a conventional heat exchanger (e.g., a separate plate, a corrugated fin, a side bar) are integrally formed without brazing or welding, so that the heat exchanger 400 can be more heat resistant and lighter than conventional heat exchangers. In addition, by forming an appropriate uneven shape on the flow path surface, the fluid can be made turbulent, improving the heat transfer efficiency. The improvement in heat transfer efficiency leads to a reduction in the size of the heat exchanger. EXAMPLES

[0082] The present invention will now be described more specifically with reference to examples and comparative examples.

[0083] [Experiment 1] (Preparation of the invented alloy material IA-1 and the comparative alloy material CA-1) In the preparation of the inventive alloy material IA-1 and the comparative alloy material CA-1, the raw materials of the Co-based alloy were mixed, melted, and cast to prepare a master ingot (100 kg). Melting was performed by vacuum induction heating melting. Next, the obtained master ingot was remelted, and alloy powder was produced by gas atomization while controlling the O2 partial pressure in the atomization atmosphere.

[0084] The chemical composition of IA-1 was Ga: 8.8 mass% (9.0 atomic %), W: 20.4 mass% (7.9 atomic %), Ni: 25.6 mass% (30.9 atomic %), Cr: 7.5 mass% (10.3 atomic %), Ta: 5.1 mass% (2.0 atomic %), C: 0.10 mass% (0.62 atomic %), B: 0.009 mass% (0.062 atomic %), O: 0.014 mass% (0.060 atomic %), balance: Cr and other impurities. The chemical composition of CA-1 was Al: 3.6 mass%, W: 21.5 mass%, Ni: 27.0 mass%, Cr: 8.0 mass%, Ta: 5.4 mass%, C: 0.11 mass%, B: 0.010 mass%, O: 0.014 mass%, balance: Cr and other impurities. CA-1 is an alloy material according to Patent Document 3, and the chemical compositions of IA-1 and CA-1, when converted into atomic percentages, have the same ratios except that Al and Ga are interchanged.

[0085] The particle sizes of the prepared IA-1 powder and CA-1 powder were measured using a laser diffraction / scattering particle size distribution analyzer (SYNC, manufactured by Microtrack Bell Co., Ltd.), and it was confirmed that the particle sizes of each were in the range of 0.3 μm to 90 μm. In addition, a part of the IA-1 powder and CA-1 powder was classified into a particle size range of 15 μm to 45 μm, and a hole flow test was performed on 50 g of the classified IA-1 powder and 50 g of CA-1 powder in accordance with JIS Z 2502:2012, and it was confirmed that the flow rate was in the range of 15 seconds to 30 seconds.

[0086] [Experiment 2] (Preparation of the invention alloy product IP-1 and the comparative alloy product CP-1) Using IA-1 and CA-1 prepared in experiment 1, alloy articles were fabricated by the PBF method in the shape of an FSW tool (see Fig. 4). The PBF conditions were as follows: alloy powder bed thickness h was 100 μm, laser beam output P was 100 W, and the laser beam scanning speed S (mm / s) was variously changed to control the local heat input P / S (unit: W·S / mm = J / mm) so that the average grain size of the gamma phase crystal grains was in the range of 10 μm to 100 μm. Controlling the local heat input corresponds to controlling the cooling rate.

[0087] Next, the prepared alloy articles were subjected to a first aging treatment at 650°C for 24 hours and a second aging treatment at 760°C for 16 hours to produce the inventive alloy product IP-1 and the comparative alloy product CP-1.

[0088] [Experiment 3] (Preparation of comparative alloy material CA-2 and comparative alloy product CP-2) A commercially available Ni-based alloy material (Pearl® Micro ABD®-900AM, manufactured by Aubert & Duval, France) was prepared, and an alloy article was produced by shaping the shape of an FSW tool (see Figure 4) using the PBF method under conditions suitable for the Ni-based alloy material. In addition, the prepared alloy article was subjected to solution and aging treatment under conditions suitable for the Ni-based alloy material to produce a comparative alloy product CP-2.

[0089] [Experiment 4] (Microstructural observation and mechanical property testing) The microstructures of the inventive alloy material IA-1, an alloy article using IA-1, the inventive alloy product IP-1, and the comparative alloy products CP-1 and CP-2 were observed.

[0090] As explained in FIG. 2, IA-1 and alloy articles using it are polycrystalline bodies of fine γ-phase crystals with an average grain size of 5 μm or more and 50 μm or less, and it has been confirmed that extremely small cells with an average size of 0.15 μm or more and 1.5 μm or less are formed within the fine grains of the polycrystalline body.

[0091] As explained in FIG. 3, IP-1 is composed of a polycrystalline body of γ-phase grains having an average grain size of 10 μm or more and 100 μm or less, and γ'-phase grains having grain sizes of 0.01 μm or more and 1 μm or less are dispersed and precipitated within the γ-phase grains, and μ-phase grains having grain sizes of 0.005 μm or more and 20 μm or less are dispersed and precipitated within the γ-phase grains and on the grain boundaries, with an average interparticle distance of 0.15 μm or more and 100 μm or less.

[0092] Although not shown in the figures, a microstructure similar to that of IP-1 (see FIG. 3) was confirmed in CP-1. In other words, IP-1 can finely disperse the precipitation of undesired different phases, as in Patent Document 3, and can suppress the negative effects of the different phases. In CP-2, a microstructure similar to that of the conventional technology in Ni-based alloy products was confirmed.

[0093] To confirm the mechanical properties, creep tests were conducted on IP-1 and CP-2. The test conditions were a test in which a stress of 600 MPa was applied in a temperature environment of 750°C, and a test in which a stress of 200 MPa was applied in a temperature environment of 840°C, and the time to fracture was measured for each. The results are shown in Table 1.

[0094] [Table 1]

[0095] As shown in Table 1, it is confirmed that the inventive alloy product IP-1 has mechanical properties equal to or greater than those of the comparative alloy product CP-2.

[0096] [Experiment 5] (FSW Examination) A commercially available high-tensile steel plate (H-SA700A) and an Al-based metal plate (A1050) were prepared as the samples to be joined (each 3 mm thick), and a test was conducted to butt-join them by FSW using the products IP-1 and CP-1 to CP-2 prepared in Experiments 2 and 3. The FSW conditions were a tool rotation speed of 1000 rpm, a tool feed speed of 400 mm / min, and a joint length of 1000 mm.

[0097] After the FSW test, the condition of the joints was visually inspected. Those that were judged to have a good joint were judged to be "passed", and those with poor joints such as unjoined areas or burrs were judged to be "failed".

[0098] As a result, the FSW using product IP-1 produced a good joint over the entire joint length and was judged to be "passed." On the other hand, the FSW using products CP-1 to CP-2 produced burrs in places and were judged to be "failed." When products CP-1 to CP-2 were inspected after the FSW test, small pieces of the Al-based metal plate were found to have adhered, which is believed to have caused a negative interaction between the Al component in alloy materials CA-1 to CA-2 and the Al-based metal plate being joined.

[0099] As shown above, the results of microstructural observation, mechanical property testing, and FSW testing confirmed that Co-based alloy products using the Co-based alloy material of the present invention have mechanical properties equal to or greater than those of conventional Ni-based alloy products, and can suppress negative interactions with Al-based metal materials. [Explanation of symbols]

[0100] 100...Friction stir welding tools, 200...turbine stator blade, 210...blade portion, 220: inner ring side end wall; 230: outer ring side end wall; 300... gas turbine, 310... compressor section, 320... turbine section, 321...turbine nozzle, 322...turbine blade, 400...heat exchanger, 410...separate layer, 420...fin layer, 430...side bar portion.

Claims

1. A Co-based alloy material, Contains 0.26% by mass or more and 26% by mass or less of Ga and 3% by mass or more and 45% by mass or less of W, the sum of the Ga and the W being less than 50% by mass; Component E1, which is one or more selected from B, C, Y, La, and misch metal, and is 2 mass% or less in total; and one or more E2 components selected from Cr, Fe, Ni, Mo, Ru, Re, Ir, Ti, Zr, Hf, V, Nb, and Ta in a total amount of 40 mass% or less, A Co-based alloy material having a chemical composition consisting essentially of Co and impurities.

2. The Co-based alloy material according to claim 1, The chemical composition is The Ga content is 2% by mass or more and 20% by mass or less, The W content is 5% by mass or more and 35% by mass or less; 40% by mass or less of the Ni; 20% by mass or less of the Cr; 15% by mass or less of the Ta; 1 mass % or less of the C; and 0.5 mass% or less of B; The remainder of the Co-based alloy material is Co and the impurities.

3. The Co-based alloy material according to claim 1, The chemical composition is The Ga content is 5% by mass or more and 15% by mass or less, 10% by mass or more and 30% by mass or less of W; 15% by mass or more and 35% by mass or less of the Ni; The Cr content is 3% by mass or more and 15% by mass or less, The Ta content is 1 mass % or more and 10 mass % or less, The C content is 0.05% by mass or more and 0.2% by mass or less; B is 0.001 mass% or more and 0.1 mass% or less, The remainder of the Co-based alloy material is Co and the impurities.

4. The Co-based alloy material according to any one of claims 1 to 3, The Co-based alloy material is characterized in that the chemical composition contains 0.05 mass % or less of O as the impurity.

5. The Co-based alloy material according to any one of claims 1 to 3, The Co-based alloy material has a γ-phase crystal grain as a parent phase, and segregation cells having an average size of 0.15 μm or more and 1.5 μm or less are formed in the γ-phase crystal grain as a parent phase of the Co-based alloy material. in the segregation cells, γ' phase particles containing the Co, the Ga, and the W and having a particle size of 0.01 μm or more and 0.5 μm or less are dispersed and precipitated, A Co-based alloy material, characterized in that μ-phase particles containing Co and W and having a particle size of 0.005 μm or more and 2 μm or less are dispersed and precipitated in the boundary regions of the segregation cells and on the grain boundaries of the γ-phase crystal grains.

6. A Co-based alloy product, The Co-based alloy product is made of the Co-based alloy material according to any one of claims 1 to 3, The Co-based alloy product has a γ-phase crystal grain as a parent phase, and segregation cells having an average size of 0.15 μm or more and 1.5 μm or less are formed in the γ-phase crystal grain. in the segregation cells, γ' phase particles containing the Co, the Ga, and the W and having a particle size of 0.01 μm or more and 0.5 μm or less are dispersed and precipitated, A Co-based alloy product, characterized in that μ-phase particles containing Co and W and having a particle size of 0.005 μm or more and 2 μm or less are dispersed and precipitated in the boundary regions of the segregation cells and on the grain boundaries of the γ-phase crystal grains.

7. The Co-based alloy product according to claim 6, The Co-based alloy product is a tool for friction stir welding.

8. A Co-based alloy product, The Co-based alloy product is made of the Co-based alloy material according to any one of claims 1 to 3, and is made of a polycrystalline body of γ-phase crystal grains having an average grain size of 10 μm to 100 μm, In the γ-phase crystal grains, γ'-phase particles containing the Co, the Ga, and the W and having a grain size of 0.01 μm or more and 1 μm or less are dispersed and precipitated in a range of 40 vol % or more and 85 vol % or less, A Co-based alloy product, characterized in that within the γ-phase crystal grains and on the grain boundaries, μ-phase particles containing the Co and the W and having a grain size of 0.005 μm or more and 20 μm or less are dispersed and precipitated with an average interparticle distance of 0.15 μm or more and 100 μm or less.

9. The Co-based alloy product according to claim 8, The Co-based alloy product is a tool for friction stir welding.

Citation Information

Patent Citations

  • JP1974096468A

  • Friction stir welding using high wear resistant tools

    JP2003532543A

  • Co-BASED ALLOY MATERIAL, Co-BASED ALLOY PRODUCT, AND PRODUCTION METHOD OF THE PRODUCT