Glass for magnetic recording medium substrate, magnetic recording medium substrate, magnetic recording medium, glass spacer for magnetic recording / reproducing device, and magnetic recording / reproducing device

LAP742AUndetermined Publication Date: 2026-02-27HOYA CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
LAP742
Authority / Receiving Office
LA · LA
Patent Type
Applications
Current Assignee / Owner
Priority Date
2018-05-16
Filing Date
2019-05-14
Publication Date
2026-02-27

AI Technical Summary

Technical Problem

Conventional aluminum alloy substrates used in magnetic recording media are prone to deformation and have insufficiently smooth surfaces, and there is a need for magnetic recording medium substrates with higher heat resistance and rigidity to withstand high-temperature processing and reduce warping during spindle motor rotation.

Method used

Development of amorphous oxide glasses with specific compositions, such as SiO2, Li2O, B2O3, MgO, CaO, and ZrO2, which provide a glass transition temperature of 650°C or higher and a Young's modulus of 90 GPa or higher, enhancing heat resistance and rigidity.

Benefits of technology

The amorphous oxide glasses offer excellent heat resistance and rigidity, maintaining substrate flatness during high-temperature processing and reducing warping and deflection, thus improving the performance and reliability of magnetic recording media.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Provided is a glass for a magnetic recording medium substrate, the glass being an amorphous oxide glass having an SiO2 content of 56-80 mol%, an Li2O content of 1-10 mol%, a B2O3 content of 0-4 mol%, a total content (MgO + CaO) of MgO and CaO of 9-40 mol%, a specific gravity of 2.75 g / cm3 or lower, a glass transition temperature of 650°C or higher, and a Young's modulus of 90 GPa or higher.
Need to check novelty before this filing date? Find Prior Art

Description

Glass for magnetic recording medium substrate, magnetic recording medium substrate, magnetic recording medium, glass spacer for magnetic recording / reproducing device, and magnetic recording / reproducing device

[0001] The present invention relates to a glass for a magnetic recording medium substrate, a magnetic recording medium substrate, a magnetic recording medium, a glass spacer for a magnetic recording / reproducing device, and a magnetic recording / reproducing device.

[0002] Aluminum alloy substrates have traditionally been used as substrates for magnetic recording media such as hard disks (magnetic recording medium substrates). However, it has been pointed out that aluminum alloy substrates are prone to deformation and do not have sufficient surface smoothness after polishing. For this reason, glass magnetic recording medium substrates are now widely used (see, for example, Patent Document 1).

[0003] JP 2010-64921 A

[0004] In the process of forming a magnetic recording layer on a magnetic recording medium substrate, film formation is usually carried out at high temperatures, or a heat treatment is carried out at high temperatures after film formation. Therefore, glass for magnetic recording medium substrates is required to have high heat resistance that can withstand high-temperature treatment, specifically, a high glass transition temperature.

[0005] Furthermore, as magnetic recording media become thinner and their recording densities increase, there are growing demands for further reduction in warping and deflection of magnetic recording media during spindle motor rotation, as well as for magnetic recording media with higher practical strength. To meet these demands, it is desirable for glass for magnetic recording medium substrates to have high rigidity, specifically a high Young's modulus.

[0006] As described above, glass for use as a magnetic recording medium substrate is desired to have excellent heat resistance and rigidity.

[0007] Therefore, an object of one aspect of the present invention is to provide a glass for a magnetic recording medium substrate that is excellent in heat resistance and rigidity.

[0008] One aspect of the present invention is a method for producing a SiO 2 The content is 56 to 80 mol%, Li 2 O content is 1 to 10 mol %, B 2 O 3The total content of MgO and CaO (MgO + CaO) is 9 to 40 mol%, and the specific gravity is 2.75 g / cm 3 Hereinafter, the present invention relates to a glass for magnetic recording medium substrates (hereinafter also referred to as "glass A"), which is an amorphous oxide glass having a glass transition temperature of 650° C. or higher and a Young's modulus of 90 GPa or higher.

[0009] Another aspect of the present invention is a method for manufacturing a silicon dioxide film comprising: 2 The content is 56 to 80 mol%, Li 2 O content is 1 to 10 mol %, B 2 O 3 The total content of MgO and CaO (MgO+CaO) is 9 to 40 mol %, Al 2 O 3 SiO content 2 and ZrO 2 The molar ratio of the total content of (SiO 2 + ZrO 2 ) / Al 2 O 3 ) is 2 to 13, and the glass for a magnetic recording medium substrate is an amorphous oxide glass having a glass transition temperature of 650°C or higher and a Young's modulus of 90 GPa or higher (hereinafter also referred to as "glass B").

[0010] Glass A and glass B have the above glass composition, and have high heat resistance with a glass transition temperature of 650° C. or higher and high rigidity with a Young's modulus of 90 GPa or higher.

[0011] According to one aspect of the present invention, a glass for a magnetic recording medium substrate having excellent heat resistance and rigidity can be provided. Furthermore, according to another aspect, a magnetic recording medium substrate made of the above-mentioned glass for a magnetic recording medium substrate, and a magnetic recording medium including this substrate can also be provided. Furthermore, according to another aspect, a glass spacer for a magnetic recording device can be provided.

[0012] [Glasses for Magnetic Recording Medium Substrates] Glasses A and B are glasses for magnetic recording medium substrates that have the above glass composition and are amorphous oxide glasses with a glass transition temperature of 650° C. or higher and a Young's modulus of 90 GPa or higher.

[0013] Glasses A and B are amorphous glasses and oxide glasses. Unlike glass-ceramics, amorphous glasses are glasses that do not contain a crystalline phase and exhibit a glass transition phenomenon upon heating. Furthermore, oxide glasses are glasses in which the main network-forming component of the glass is an oxide. Glasses A and B are described in more detail below. Unless otherwise specified, the matters described apply to both glasses A and B.

[0014] <Glass Composition> In the present invention and this specification, the glass composition is expressed as a glass composition based on oxides. Here, "glass composition based on oxides" refers to a glass composition obtained by converting the glass raw materials into oxides present in the glass after they are all decomposed during melting. Unless otherwise specified, the glass composition is expressed on a molar basis (mol %, molar ratio). The glass composition in the present invention and this specification can be determined by a method such as ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). Quantitative analysis is performed for each element using ICP-AES. The analytical values ​​are then converted into oxide values. The analytical values ​​obtained by ICP-AES may contain a measurement error of, for example, about ±5% of the analytical value. Therefore, the oxide values ​​converted from the analytical values ​​may also contain an error of about ±5%. In the present invention and this specification, the expression "a component content of 0%, not containing, or not incorporating" means that the component is substantially not contained, and indicates that the content of the component is at or below the impurity level, for example, less than 0.01%.

[0015] The glass compositions of glasses A and B will be described below.

[0016] SiO 2 is a glass network forming component and has the function of improving glass stability. 2 is a component that also contributes to improving chemical durability. 2From the viewpoint of improving rigidity, the content is 80% or less, preferably 75% or less, more preferably 70% or less, even more preferably 66% or less, still more preferably 64% or less, even more preferably 63% or less, and still more preferably 62% or less. 2 From the viewpoint of maintaining chemical durability, the content is 56% or more, preferably 57% or more, more preferably 58% or more, even more preferably 59% or more, and still more preferably 60% or more.

[0017] Al 2 O 3 is a glass network forming component and has the function of improving heat resistance. 2 O 3 In glass B, Al also has the function of improving chemical durability. 2 O 3 is an essential component. From the viewpoint of improving heat resistance and chemical durability, the Al content in glasses A and B is 2 O 3 The content of Al in Glasses A and B is preferably 5% or more, more preferably 8% or more, even more preferably 10% or more, still more preferably 12% or more, and even more preferably 13% or more. 2 O 3 The content is preferably 20% or less, more preferably 18% or less, even more preferably 17% or less, still more preferably 16% or less, and even more preferably 15.5% or less.

[0018] In glasses A and B, SiO 2 and Al 2 O 3 The total content (SiO 2 +Al 2 O 3) is preferably 65% ​​or more, more preferably 67% or more, even more preferably 69% or more, still more preferably 70% or more, even more preferably 72% or more, and still more preferably 74% or more, from the viewpoint of maintaining chemical durability. 2 and Al 2 O 3 The total content (SiO 2 +Al 2 O 3 ) is preferably 80% or less, more preferably 78% or less, even more preferably 77% or less, even more preferably 76% or less, and even more preferably 75% or less.

[0019] B 2 O 3 is a component that forms a network of glass, a component that reduces the specific gravity of glass, and a component that improves meltability. 2 O 3 is easily volatilized during melting and tends to destabilize the glass component ratio. Moreover, excessive incorporation of B tends to reduce chemical durability. 2 O 3 The content of B is 0 to 4%. 2 O 3 The content of B is preferably 3.00% or less, more preferably 2.00% or less, even more preferably 1.50% or less, still more preferably 1.00% or less, even more preferably 0.50% or less, and still more preferably 0.30% or less. 2 O 3 The content of is preferably 0.00% or more, more preferably 0.05% or more, even more preferably 0.10% or more, and even more preferably 0.15% or more.

[0020] Among the alkaline earth metal oxides MgO, CaO, SrO, and BaO, MgO serves to increase the Young's modulus of glass, increase the thermal expansion coefficient, and improve the meltability and formability of glass. The specific elastic modulus will be described in detail later. In one embodiment, MgO is an essential component. From the viewpoint of achieving the above functions well, the content of MgO in Glasses A and B is preferably 3% or more, more preferably 5% or more, even more preferably 7% or more, still more preferably 8% or more, and even more preferably 9% or more. Furthermore, from the viewpoint of maintaining glass stability, the content of MgO in Glasses A and B is preferably 28% or less, more preferably 25% or less, still more preferably 22% or less, still more preferably 20% or less, even more preferably 18% or less, still more preferably 16% or less, still more preferably 15% or less, and even more preferably 14% or less.

[0021] The CaO content in Glasses A and B is 0% or more. CaO also has the functions of increasing the Young's modulus and specific elastic modulus of the glass, increasing the thermal expansion coefficient, and improving the meltability and formability of the glass. From the viewpoint of obtaining these functions well, the CaO content in Glasses A and B is preferably 2% or more, more preferably 3% or more, even more preferably 4% or more, and still more preferably 5% or more. Furthermore, from the viewpoint of maintaining chemical durability, the CaO content in Glasses A and B is preferably 18% or less, more preferably 15% or less, even more preferably 12% or less, even more preferably 10% or less, even more preferably 8% or less, and still more preferably 7% or less.

[0022] From the viewpoint of improving rigidity, the total content of MgO and CaO (MgO+CaO) in Glasses A and B is 9% or more, preferably 11% or more, more preferably 13% or more, even more preferably 15% or more, still more preferably 16% or more, and even more preferably 17% or more. From the viewpoint of glass stability, the total content of MgO and CaO (MgO+CaO) in Glasses A and B is 40% or less, preferably 35% or less, more preferably 30% or less, even more preferably 27% or less, even more preferably 25% or less, even more preferably 23% or less, even more preferably 21% or less, and still more preferably 20% or less.

[0023] The molar ratio of the CaO content to the MgO content (CaO / MgO) in Glasses A and B is, from the viewpoints of increasing Young's modulus and specific elastic modulus and improving glass stability, preferably 2.5 or less, more preferably 2.3 or less, even more preferably 2.1 or less, even more preferably 1.9 or less, still more preferably 1.6 or less, even more preferably 1.4 or less, even more preferably 1.1 or less, and still more preferably 1.0 or less. The molar ratio (CaO / MgO) is 0 or more, and, from the viewpoint of improving glass stability, is preferably 0.05 or more, more preferably 0.100 or more, even more preferably 0.120 or more, and even more preferably 0.150 or more.

[0024] SrO improves the meltability, formability, and glass stability of the glass, and functions to increase the thermal expansion coefficient. From the viewpoints of maintaining chemical durability, reducing the specific gravity, and reducing raw material costs, the SrO content in Glasses A and B is preferably 0 to 2%. The SrO content is more preferably in the range of 0 to 1.5%, even more preferably 0 to 1%, and even more preferably 0 to 0.5%. In one embodiment, it is preferable that no SrO is contained, i.e., the SrO content is 0%.

[0025] Both BaO and SrO are components that increase the specific gravity of the glass. From the viewpoint of reducing the specific gravity of the glass, the total content of BaO and SrO (BaO + SrO) in Glasses A and B is preferably 0 to 2%, more preferably 0 to 1.5%, even more preferably 0 to 1%, and even more preferably 0 to 0.5%. In one embodiment, it is preferable that neither BaO nor SrO is contained, that is, the total content of BaO and SrO (BaO + SrO) is 0%.

[0026] BaO also improves the meltability, formability, and glass stability of the glass, and functions to increase the thermal expansion coefficient. From the viewpoints of maintaining chemical durability, reducing the specific gravity, and reducing raw material costs, the BaO content in Glasses A and B is preferably 0 to 2%, more preferably 0 to 1.5%, even more preferably 0 to 1.0%, and even more preferably 0 to 0.5%. In one embodiment, it is preferable that no BaO is contained, that is, the BaO content is 0%.

[0027] The molar ratio of the BaO content to the total content of MgO, CaO, SrO, and BaO (BaO / (MgO+CaO+SrO+BaO)) is preferably 0.1 or less, more preferably 0.08 or less, even more preferably 0.06 or less, still more preferably 0.04 or less, still more preferably 0.03 or less, still more preferably 0.02 or less, and still more preferably 0.01 or less, from the viewpoints of improving rigidity, lowering specific gravity, increasing specific elastic modulus, and improving glass stability. In one embodiment, the molar ratio (BaO / (MgO+CaO+SrO+BaO)) is preferably 0.

[0028] The molar ratio of the MgO content to the total content of MgO, CaO, SrO, and BaO (MgO / (MgO+CaO+SrO+BaO)) is preferably 1 or less, more preferably 0.8 or less, and even more preferably 0.75 or less, from the viewpoint of improving glass stability. Furthermore, the molar ratio (MgO / (MgO+CaO+SrO+BaO)) is preferably 0.3 or more, more preferably 0.5 or more, even more preferably 0.6 or more, and even more preferably 0.65 or more, from the viewpoint of increasing Young's modulus and specific elastic modulus and improving glass stability.

[0029] The total content of alkaline earth metal oxides (MgO+CaO+SrO+BaO) in Glasses A and B is preferably 9% or more, more preferably 11% or more, even more preferably 13% or more, still more preferably 14% or more, and even more preferably 16% or more, from the viewpoint of improving the meltability and stability of the glass. Furthermore, from the viewpoint of the chemical durability of the glass, the total content of alkaline earth metal oxides (MgO+CaO+SrO+BaO) in Glasses A and B is preferably 40% or less, more preferably 35% or less, still more preferably 30% or less, even more preferably 28% or less, still more preferably 25% or less, even more preferably 22% or less, still more preferably 21% or less, and even more preferably 20% or less.

[0030] Among alkaline earth metal oxides, MgO functions to increase the Young's modulus and specific elastic modulus of glass and also contributes to suppressing an increase in specific gravity. Therefore, MgO is a very useful component for increasing the Young's modulus, specific elastic modulus, and specific gravity of glass, and is particularly effective for increasing the Young's modulus and specific gravity. CaO also functions to increase the Young's modulus and specific elastic modulus of glass, contributes to suppressing an increase in specific gravity, and is also an effective component for increasing the thermal expansion coefficient of glass. On the other hand, SrO and BaO increase the specific gravity and raw material costs. From the above perspectives, in Glasses A and B, the molar ratio of the total content of MgO and CaO to the total content of MgO, CaO, SrO, and BaO {(MgO + CaO) / (MgO + CaO + SrO + BaO)} is preferably 0.7 to 1. The lower limit of the molar ratio is more preferably 0.750 or more, even more preferably 0.800 or more, even more preferably 0.850 or more, even more preferably 0.900 or more, even more preferably 0.925 or more, even more preferably 0.950 or more, even more preferably 0.975 or more, and even more preferably 0.980 or more.

[0031] Li 2 Among alkali metal oxides, O has a strong effect of improving the melting property and moldability of glass, and is also a suitable component for increasing the Young's modulus and imparting suitable rigidity to the magnetic recording medium substrate. 2 O is also a component that plays a role in lowering the resistivity. The resistivity will be described in detail later. 2 O is also a component that increases the thermal expansion coefficient. When glasses A and B are used as glasses for chemical strengthening, O is also a component that plays a role in ion exchange during chemical strengthening. 2 O is also a component that lowers the glass transition temperature. 2 The content of O is 1 to 10%. 2The lower limit of the O content is preferably 2% or more, more preferably 3% or more, even more preferably 4% or more, and even more preferably 4.2% or more. 2 The upper limit of the O content is preferably 8% or less, more preferably 7% or less, even more preferably 6% or less, and even more preferably 5% or less.

[0032] Li relative to the total content of MgO and CaO 2 Molar ratio of O content (Li 2 From the viewpoint of suppressing a decrease in the glass transition temperature, the molar ratio (LiO / (MgO+CaO)) is preferably 0.4 or less, more preferably 0.37 or less, even more preferably 0.35 or less, even more preferably 0.32 or less, and even more preferably 0.30 or less. 2 From the viewpoints of improving the meltability of the glass, suppressing the generation of bubbles, and reducing the specific resistance, the ratio of MgO to CaO is preferably 0.03 or more, more preferably 0.05 or more, even more preferably 0.08 or more, still more preferably 0.10 or more, still more preferably 0.15 or more, even more preferably 0.20 or more, and still more preferably 0.21 or more.

[0033] Na 2 O is a component that improves the meltability and formability of the glass, increases the thermal expansion coefficient, and reduces the viscosity of the glass during fining, accelerating bubble removal. Furthermore, when glasses A and B are used as glasses for chemical strengthening, O is also a component responsible for ion exchange during chemical strengthening. Taking these functions into consideration, Na in glasses A and B was selected as the component for the following reasons: 2 The O content is preferably 0 to 10%, more preferably 0 to 8%, even more preferably 0 to 7%, still more preferably 0 to 6%, still more preferably 0 to 5%, even more preferably 0 to 3%, and still more preferably 0 to 1%.

[0034] Li 2 Na content relative to O content 2Molar ratio of O content (Na 2 O / Li 2 From the viewpoint of improving rigidity, the molar ratio (Na 2 O / Li 2 O) can be 0.

[0035] K 2 O also has the function of improving the meltability and formability of the glass, and is a component that increases the thermal expansion coefficient. On the other hand, if incorporated in excess, it tends to reduce chemical durability, especially acid resistance, and when used as a glass substrate, alkali elution from the substrate surface increases, and the precipitated alkali may affect the film properties of the magnetic recording layer, etc. In consideration of the above points, K in Glasses A and B was 2 The O content is preferably 0 to 5%, more preferably 0 to 3%, even more preferably 0 to 2%, and even more preferably 0 to 1%. 2 It is preferable that the material does not contain O.

[0036] Li 2 O content, Na 2 O content and K content 2 Regarding the O content, from the viewpoint of improving the meltability of the glass, 4 × Li 2 O content, 2×Na 2 O content and K content 2 Sum of O content (4Li 2 O + 2Na 2 O+K 2 O) is preferably 8% or more. 2 O + 2Na 2 O+K 2O) is preferably 8% or more in order to reduce the resistivity. From the above viewpoints, the above sum is more preferably 10% or more, even more preferably 12% or more, even more preferably 14% or more, even more preferably 16% or more, even more preferably 17% or more, even more preferably 17.3% or more, even more preferably 17.5% or more, and even more preferably 17.8% or more. Also, from the viewpoint of increasing the glass transition temperature, 4×Li 2 O content, 2×Na 2 O content and K content 2 Sum of O content (4Li 2 O + 2Na 2 O+K 2 O) is preferably 27% or less, more preferably 25% or less, even more preferably 23% or less, still more preferably 21% or less, even more preferably 20% or less, and even more preferably 19% or less.

[0037] Li 2 O, Na 2 O and K 2 SiO relative to the total content of O 2 Molar ratio of content (SiO 2 / (Li 2 O + Na 2 O+K 2 From the viewpoint of increasing the glass transition temperature, the molar ratio (SiO 2 / (Li 2 O + Na 2 O+K 2 From the viewpoint of improving the meltability and rigidity of the glass, O)) is preferably 22 or less, more preferably 20 or less, even more preferably 17 or less, still more preferably 15 or less, and still more preferably 14 or less.

[0038] Li 2 O, Na 2 O and K2 Li relative to the total content of O 2 Molar ratio of O content (Li 2 O / (Li 2 O + Na 2 O+K 2 From the viewpoint of increasing the Young's modulus and specific elastic modulus, improving solubility, and reducing specific resistance, the molar ratio (Li) is preferably 0.10 or more, more preferably 0.30 or more, even more preferably 0.50 or more, still more preferably 0.70 or more, even more preferably 0.80 or more, still more preferably 0.90 or more, and still more preferably 0.95 or more. In one embodiment, the molar ratio (Li 2 O / (Li 2 O + Na 2 O+K 2 O)) can be 1.

[0039] Li 2 O, Na 2 O and K 2 Na content relative to total O content 2 Molar ratio of O content (Na 2 O / (Li 2 O + Na 2 O+K 2 O)) can be 0 or more, and from the viewpoint of suppressing a decrease in Young's modulus and specific elastic modulus, is preferably 5 or less, more preferably 2 or less, still more preferably 1 or less, even more preferably 0.8 or less, and still more preferably 0.5 or less.

[0040] 5xLi 2 O content, 3×Na 2 O content, 3×K 2 O content, 2×B 2 O 3 content, MgO content, 2×CaO content, 3×SrO content, and BaO content (5Li 2 O + 3Na 2 O+3K 2 O+2B 2 O 3From the viewpoint of increasing the thermal expansion coefficient, the sum (5Li+MgO+2CaO+3SrO+BaO) is preferably 32% or more, more preferably 35% or more, even more preferably 38% or more, still more preferably 40% or more, even more preferably 42% or more, and still more preferably 44% or more. 2 O + 3Na 2 O+3K 2 O+2B 2 O 3 + 2MgO + 2CaO + 3SrO + BaO) is preferably 58% or less, more preferably 56% or less, even more preferably 54% or less, still more preferably 52% or less, even more preferably 51% or less, and even more preferably 50% or less.

[0041] MgO and Li 2 CaO and Na relative to the total content of O 2 Molar ratio of the total content of O ((CaO + Na 2 O) / (MgO+Li 2 From the viewpoint of improving the glass stability, the molar ratio ((CaO+Na 2 O) / (MgO+Li 2 From the viewpoint of suppressing a decrease in Young's modulus and specific elastic modulus, O)) is preferably 2.5 or less, more preferably 2 or less, even more preferably 1.5 or less, still more preferably 1.0 or less, even more preferably 0.8 or less, and still more preferably 0.6 or less.

[0042] Li 2 O, Na 2 O and K 2O is a component that improves the meltability and formability of the glass and increases the thermal expansion coefficient. From the viewpoint of obtaining the functions of these components well, the total content of alkali metal oxides in Glasses A and B (Li 2 O + Na 2 O+K 2 O) is preferably 2.5% or more, more preferably 3% or more, even more preferably 3.5% or more, and even more preferably 4% or more. On the other hand, from the viewpoint of maintaining the heat resistance and chemical durability of the glass, the total content of alkali metal oxides (Li 2 O + Na 2 O+K 2 O) is preferably 10% or less, more preferably 8% or less, even more preferably 7% or less, even more preferably 6% or less, and still more preferably 5% or less. When glass contains two or more alkali metal oxides, a mixed alkali effect can be obtained, which reduces or prevents alkali elution from the glass surface.

[0043] TiO 2 Although TiO has the function of improving the glass stability and chemical durability as well as improving rigidity, if incorporated in excess, the liquidus temperature of the glass may rise, leading to a deterioration in devitrification resistance and an increase in specific gravity. 2 The content is preferably 0 to 10%, more preferably 0 to 8%, even more preferably 0 to 6%, still more preferably 0 to 4%, even more preferably 0 to 3%, even more preferably 0 to 2%, and still more preferably 0 to 1%.

[0044] TiO relative to the total content of MgO and CaO 2 and Al 2 O 3 The molar ratio of the total content of (TiO 2 +Al 2 O 3From the viewpoints of suppressing bubble generation, improving chemical durability, and increasing the hardness of the glass, the molar ratio ((TiO 2 +Al 2 O 3 From the viewpoints of improving glass stability, increasing the specific elastic modulus, and decreasing the specific gravity, the ratio (MgO+CaO)) is preferably 2 or less, more preferably 1.800 or less, even more preferably 1.600 or less, still more preferably 1.400, even more preferably 1.200 or less, and still more preferably 1.000 or less.

[0045] ZrO 2 ZrO has the function of improving chemical durability and also the function of improving rigidity. However, excessive incorporation of ZrO may reduce the melting properties of the glass, resulting in unmelted raw materials. Therefore, ZrO in Glasses A and B is 2 The content of is preferably 0 to 5%, more preferably 0 to 3%, even more preferably 0 to 2%, still more preferably 0 to 1%, and even more preferably 0 to 0.5%. 2 The content can be 0.00%.

[0046] MgO content, 0.7×CaO content, Li 2 O content, TiO 2 Content and ZrO 2 Sum of contents (MgO+0.7CaO+Li 2 O+TiO 2 + ZrO 2 ) is preferably 16% or more, more preferably 18% or more, even more preferably 19% or more, even more preferably 20% or more, and even more preferably 21% or more, from the viewpoint of increasing the specific elastic modulus. 2 O+TiO 2 + ZrO 2) is preferably 40% or less, more preferably 35% or less, even more preferably 30% or less, still more preferably 28% or less, and even more preferably 25% or less, from the viewpoint of suppressing a decrease in glass stability and a decrease in glass transition temperature.

[0047] Al 2 O 3 SiO content 2 and ZrO 2 The molar ratio of the total content of (SiO 2 + ZrO 2 ) / Al 2 O 3 From the viewpoint of improving chemical durability, in glass B, the molar ratio ((SiO 2 + ZrO 2 ) / Al 2 O 3 From the viewpoint of improving rigidity and achieving a high specific elastic modulus, in glass B, Al is 13 or less, preferably 10 or less, more preferably 9 or less, even more preferably 8 or less, still more preferably 7 or less, and even more preferably 6 or less. 2 O 3 SiO content 2 and ZrO 2 The molar ratio of the total content of (SiO 2 + ZrO 2 ) / Al 2 O 3 ) is preferably 2 or more from the viewpoint of improving chemical durability, and is preferably 13 or less from the viewpoint of improving rigidity and achieving a high specific elastic modulus. 2 O 3 SiO content 2 and ZrO 2 The molar ratio of the total content of (SiO 2 + ZrO 2 ) / Al 2 O 3 For more preferred ranges of ), see the above description regarding glass B.

[0048] ZnO has the function of improving meltability and rigidity, but excessive incorporation raises the liquidus temperature. From the above viewpoints, the ZnO content in Glasses A and B is preferably 0 to 5%, more preferably 0 to 3%, even more preferably 0 to 2%, even more preferably 0 to 1%, and still more preferably 0 to 0.5%. In one embodiment, the ZnO content can be 0.00%.

[0049] P 2 O 5 Although P can be incorporated into glasses A and B, excessive incorporation tends to decrease chemical durability. 2 O 5 The content of P is preferably 0 to 2%. 2 O 5 The content of P is more preferably 0 to 1%, and further preferably 0 to 0.5%. 2 O 5 The content can be 0.00%.

[0050] SiO 2 Content, Al 2 O 3 Content, B 2 O 3 Content, P 2 O 5 Content, 1.5×Na 2 O content, 1.5×K 2 The sum of the O content, 2×SrO content, 3×BaO content and ZnO content (SiO 2 +Al 2 O 3 +B 2 O 3 +P 2 O 5 +1.5Na 2 O+1.5K 2 From the viewpoint of improving rigidity, the total content of SiO2 (2SrO+2SrO+3BaO+ZnO) is preferably 86% or less, more preferably 84% or less, even more preferably 82% or less, still more preferably 80% or less, even more preferably 78% or less, and still more preferably 77% or less.

[0051] SiO 2 Content, Al 2 O 3 Content, B 2 O 3 Content, P 2 O 5 Content, Na 2 O content, K 2 The sum of the O content, the CaO content, 2×SrO content, and 3×BaO content (SiO 2 +Al 2 O 3 +B 2 O 3 +P 2 O 5 +Na 2 O+K 2 From the viewpoint of achieving a high specific elastic modulus, the content of the SiO2 (2SrO+2CaO+2SrO+3BaO) is preferably 92% or less, more preferably 90% or less, even more preferably 88% or less, even more preferably 86% or less, and even more preferably 85% or less.

[0052] B 2 O 3 , SiO 2 , Al 2 O 3 and P 2 O 5 P relative to the total content of 2 O 5 Molar ratio of content (P 2 O 5 / (B 2 O 3 +SiO 2 +Al 2 O 3 +P 2 O 5 From the viewpoints of improving glass stability, improving rigidity, increasing the specific elastic modulus, and improving chemical durability, the molar ratio (P) is preferably 0.005 or less, more preferably 0.003 or less, even more preferably 0.002 or less, and even more preferably 0.001 or less. 2 O 5 / (B 2 O 3 +SiO 2 +Al2 O 3 +P 2 O 5 )) can be 0.

[0053] Glasses A and B contain SnO 2 , CeO 2 and Sb 2 O 3 In one embodiment, the composition may include one or more selected from the group consisting of SnO 2 and CeO 2 In another embodiment, the total content of glasses A and B can be 0%. 2 and / or CeO 2 and SnO 2 and CeO 2 The total content (SnO 2 + CeO 2 ) is preferably 0.05 to 2%. 2 and CeO 2 When the total content of SnO is 0.05% or more, a sufficient fining effect can be obtained, and residual bubbles can be reduced or suppressed. 2 + CeO 2 By making the total content (SnO ) 2% or less, it is possible to prevent the molten glass from blowing up during glass melting, thereby preventing a decrease in productivity. 2 + CeO 2 The lower limit of the total content (SnO 2 + CeO 2The upper limit of ) is preferably 1.5% or less, more preferably 1.2% or less, even more preferably 1.0% or less, still more preferably 0.70% or less, even more preferably 0.65% or less, still more preferably 0.60% or less, still more preferably 0.55% or less, and even more preferably 0.50% or less.

[0054] SnO 2 has the function of promoting fining when the melting temperature of the glass is relatively high (temperature range of about 1400 to 1600°C). 2 O 3 In one embodiment, SnO is added to Glasses A and B in order to remove bubbles from glasses with high melting temperatures, while the use of fining agents that have an adverse effect on the environment, such as arsenic acid and arsenous acid, is restricted. 2 It is preferable to incorporate SnO. 2 From the viewpoint of obtaining a fining effect, the content of SnO is preferably 0.01% or more, more preferably 0.05% or more, even more preferably 0.10% or more, even more preferably 0.15% or more, and even more preferably 0.20% or more. 2 The content is preferably 2% or less, more preferably 1.5% or less, even more preferably 1.0% or less, even more preferably 0.8% or less, and even more preferably 0.5% or less.

[0055] CeO 2 is SnO 2 It is a component that has a fining effect on glass, similar to CeO 2 has the function of taking in oxygen and fixing it as a glass component when the melting temperature of the glass is relatively low (temperature range of about 1200 to 1400°C). Therefore, in one embodiment, CeO is added to glasses A and B as a fining agent. 2 It is preferable to incorporate CeO 2 From the viewpoint of obtaining a fining effect, the content of CeO is preferably 0.01% or more, more preferably 0.05% or more, even more preferably 0.08% or more, and even more preferably 0.10% or more. 2The content of SnO is preferably 2% or less, more preferably 1.5% or less, even more preferably 1.0% or less, still more preferably 0.8% or less, even more preferably 0.5% or less, and still more preferably 0.3% or less. 2 and CeO 2 By making the glass A and the glass B coexist with each other, a fining effect can be obtained in a wide temperature range. 2 and CeO 2 It is preferable to include both of the above.

[0056] Sb 2 O 3 From the viewpoint of reducing the environmental impact, it is desirable to refrain from using Sb. 2 O 3 The content of Sb is preferably in the range of 0 to 0.5%. 2 O 3 The content of Sb is more preferably 0.3% or less, further preferably 0.1% or less, even more preferably 0.05% or less, and even more preferably 0.02% or less. 2 O 3 It is particularly preferred that it does not contain

[0057] CeO 2 When it contains CeO 2 SnO content 2 Molar ratio of content (SnO 2 / CeO 2 ) can be 0 or more, preferably 0.1 or more, more preferably 0.3 or more, even more preferably 0.5 or more, even more preferably 0.7 or more, even more preferably 0.9 or more, even more preferably 1.0 or more, even more preferably 1.2 or more, and even more preferably 1.4 or more. 2 / CeO 2) is preferably 7 or less, more preferably 6 or less, even more preferably 5 or less, still more preferably 4 or less, even more preferably 3.5 or less, even more preferably 3.0 or less, even more preferably 2.5 or less, even more preferably 2.3 or less, and even more preferably 2.1 or less, 1.9 or less, 1.8 or less, or 1.7 or less. As will be described later with regard to resistivity, in embodiments in which electrical heating is performed during glass melting, glass with low resistivity is preferred. Glass with low resistivity can be melted by lowering the temperature inside the furnace during electrical heating. Lowering the temperature inside the furnace reduces the SnO 2 CeO, which can exert a better fining effect at low temperatures compared to 2 The content of SnO 2 In other words, the molar ratio (SnO 2 / CeO 2 ) is preferably small.

[0058] The Fe content of glasses A and B is expressed as Fe in the oxide-based glass composition expressed by mass. 2 O 3 In terms of the total iron content, the total iron content may be 1% by mass or less, 0.7% by mass or less, 0.5% by mass or less, 0.4% by mass or less, 0.3% by mass or less, 0.1% by mass or less, 0.07% by mass or less, 0.05% by mass or less, 0.04% by mass or less, or 0.03% by mass or less. In one embodiment, glasses A and B may contain no Fe (the content is 0% by mass). Glasses A and B may also contain one or more elements selected from the group consisting of Cu, Co, Yb, Mn, Nd, Pr, Nb, V, Cr, Ni, Mo, Ho, and Er.

[0059] Since Pb, Cd and As are substances that have a negative impact on the environment, it is preferable to avoid introducing them.

[0060] Glasses A and B can be produced by weighing, blending, and thoroughly mixing glass raw materials such as oxides, carbonates, nitrates, sulfates, and hydroxides so as to obtain a predetermined glass composition, heating and melting the mixture in a melting vessel, for example, at a temperature in the range of 1400 to 1600°C, refining, and stirring to form a homogenized glass melt that has been thoroughly defoamed. For example, it is preferable to heat and melt the glass raw materials in a melting vessel at 1400 to 1550°C, and then heat the resulting glass melt in a refining vessel and hold it at 1450 to 1600°C, and then lower the temperature to 1200 to 1400°C, at which point the glass flows out and is shaped. The glass may be heated by electrical heating or by a heating method other than electrical heating.

[0061] <Glass Physical Properties> Glasses A and B can have the various glass physical properties described below by adjusting the compositions as described above.

[0062] (Glass Transition Temperature) As described above, magnetic recording medium substrates are typically subjected to high-temperature treatment during the process of forming a magnetic recording layer on the substrate. For example, to form a magnetic recording layer containing a magnetic material with high magnetic anisotropy energy, which has been developed in recent years for higher-density recording in magnetic recording media, film formation is typically performed at high temperatures, or a heat treatment is performed at high temperatures after film formation. If the magnetic recording medium substrate does not have the heat resistance to withstand such high-temperature treatment, the substrate's flatness will be impaired by exposure to high temperatures during high-temperature treatment. In contrast, Glasses A and B have glass transition temperatures (hereinafter also referred to as "Tg"), which are an indicator of heat resistance, of 650°C or higher. A substrate made of a glass with high heat resistance, having a glass transition temperature of 650°C or higher, can maintain excellent flatness even after high-temperature treatment. However, Glasses A and B are not limited to glasses for use as substrates for magnetic recording media having a magnetic recording layer containing a magnetic material that requires high-temperature treatment, and can be used to produce magnetic recording media equipped with various magnetic materials. The glass transition temperature is preferably 660° C. or higher, more preferably 670° C. or higher, even more preferably 675° C. or higher, even more preferably 680° C. or higher, even more preferably 685° C. or higher, and even more preferably 687° C. or higher. The upper limit of the glass transition temperature is, for example, about 770° C. or about 750° C., but is not particularly limited because a higher glass transition temperature is preferable from the viewpoint of heat resistance.

[0063] (Young's Modulus) In order to meet the above-mentioned demand for improved rigidity of magnetic recording media, it is desirable for magnetic recording medium substrate glasses to have high rigidity. In this regard, Glasses A and B have a Young's modulus, which is an index of rigidity, of 90 GPa or more. Magnetic recording medium substrate glasses having high rigidity, showing a Young's modulus of 90 GPa or more, can suppress substrate deformation during rotation of a spindle motor, and therefore can also suppress warping and deflection of the magnetic recording medium due to substrate deformation. The Young's modulus of Glasses A and B is preferably 91 GPa or more, more preferably 92 GPa or more, even more preferably 93 GPa or more, even more preferably 94 GPa or more, and even more preferably 95 GPa or more. The upper limit of Young's modulus is, for example, about 120 GPa, but is not particularly limited, as a higher Young's modulus is preferable as a higher rigidity is higher.

[0064] (Specific Gravity) The specific gravity of glass A is 2.75 or less. Furthermore, the specific gravity of glass B is preferably 2.75 or less. The specific gravity of glasses A and B is more preferably 2.73 or less, even more preferably 2.70 or less, even more preferably 2.68 or less, even more preferably 2.64 or less, even more preferably 2.62 or less, and even more preferably 2.60 or less. By lowering the specific gravity of the glass for magnetic recording medium substrates, it is possible to reduce the weight of the magnetic recording medium substrate, and further reduce the weight of the magnetic recording medium, thereby enabling the reduction of power consumption of magnetic recording and reproducing devices (commonly called HDDs (hard disk drives)). The lower limit of the specific gravity is, for example, about 2.40, but is not particularly limited, as a lower specific gravity is preferable.

[0065] (Specific Elastic Modulus) The specific elastic modulus is the Young's modulus of glass divided by its density. Here, density refers to the specific gravity of the glass multiplied by the ratio of g / cm 3The specific elastic modulus of Glasses A and B can be thought of as a value with the unit "modulus of elasticity." From the viewpoint of providing a substrate that is less susceptible to deformation, the specific elastic modulus of Glasses A and B is preferably 30 MNm / kg or more, more preferably 32 MNm / kg or more, even more preferably 33 MNm / kg or more, even more preferably 34 MNm / kg or more, and even more preferably 35 MNm / kg or more. The upper limit of the specific elastic modulus is, for example, about 40 MNm / kg, but is not particularly limited, as a higher specific elastic modulus is more preferable.

[0066] (Thermal Expansion Coefficient) HDDs incorporating magnetic recording media are designed to rotate the magnetic recording media itself by holding down the central portion with the spindle and clamp of a spindle motor. Therefore, if there is a large difference in the thermal expansion coefficients of the magnetic recording media substrate and the spindle material that constitutes the spindle portion, a mismatch will occur between the thermal expansion and contraction of the spindle and the thermal expansion and contraction of the magnetic recording media substrate in response to ambient temperature changes during use, resulting in deformation of the magnetic recording media. If this occurs, the head will be unable to read the written information, causing a decrease in recording and playback reliability. Therefore, it is desirable for the glass for the magnetic recording media substrate to have an appropriate thermal expansion coefficient similar to that of the spindle material (e.g., stainless steel, etc.). Generally, HDD spindle materials have a thermal expansion coefficient of 70 x 10 in the temperature range of 100 to 300°C. -7 / °C or more, and the average linear expansion coefficient (thermal expansion coefficient) of the glass for a magnetic recording medium substrate at 100 to 300°C is 40 x 10 -7 / °C or more, the difference in thermal expansion coefficient with the spindle material is small, which can contribute to improving the reliability of the magnetic recording medium. The average linear expansion coefficient (hereinafter also referred to as "α") of Glasses A and B at 100 to 300°C is 40×10 -7 / °C or more, and -7 / °C or more, and more preferably 42 x 10 -7 / °C or more, and more preferably 43 x 10 -7 / °C or more, and more preferably 44 x 10 -7 / °C or more, and more preferably 45 x 10-7 / °C or more. The average linear expansion coefficient (α) of Glasses A and B at 100 to 300°C is 70×10 -7 / °C or less, and -7 / °C or less, and more preferably 65 x 10 -7 / °C or less, and more preferably 63 x 10 -7 / °C or less, and more preferably 60 x 10 -7 / °C or less, and more preferably 57 x 10 -7 / °C or less, and even more preferably 55 x 10 -7 / °C or less, and more preferably 53 x 10 -7 / °C or less, and even more preferably 50 x 10 -7 / °C or less. In one embodiment, the average linear expansion coefficient (α) of glasses A and B at 100 to 300°C is 48×10 -7 / °C, and can be less than 47 x 10 -7 / °C or less.

[0067] (Glass Stability) Glasses A and B can exhibit high glass stability. Methods for evaluating glass stability include a 1300°C 16-hour holding test and a 1250°C 16-hour holding test, which will be described in detail below. The evaluation result in the 1300°C 16-hour holding test is preferably A, more preferably the evaluation result in the 1300°C 16-hour holding test is A and the evaluation result in the 1250°C 16-hour holding test is A or B, and even more preferably the evaluation result in both holding tests is A.

[0068] (Bubble Density) Glasses A and B can also have reduced bubbles by adjusting their compositions as described above. Reducing bubbles is desirable in glasses for magnetic recording medium substrates. This is for the following reasons: With the recent trend toward higher density recording, there is a demand for a narrower distance (called the "flying height") between the head (magnetic head) used to write and read data and the surface of the magnetic recording medium. However, if irregularities due to bubbles exist on the surface of a glass substrate for a magnetic recording medium, these irregularities are reflected on the surface of the magnetic recording medium, reducing the surface smoothness of the magnetic recording medium. Bringing a magnetic head close to the surface of a magnetic recording medium with poor surface smoothness could result in contact with the surface of the magnetic recording medium and damage to the magnetic head. Therefore, a certain level of flying height must be maintained to prevent contact. For these reasons, it is desirable to reduce bubbles in glasses for magnetic recording medium substrates in order to narrow the flying height and produce magnetic recording media with high surface smoothness. Regarding bubbles in the glass, the density of bubbles per unit mass, as measured by an optical microscope (magnification of 40 to 100 times) and having a diameter of more than 0.03 mm, is preferably less than 50 bubbles / kg, more preferably less than 20 bubbles / kg, even more preferably less than 10 bubbles / kg, still more preferably 2 bubbles / kg or less, and most preferably 0 bubbles / kg.

[0069] (Specific Resistivity) The specific resistance of Glasses A and B can be reduced by adjusting the composition as described above. Glasses with low specific resistance are preferred in that they are less likely to corrode a melting furnace (e.g., made of brick) when electrical heating is performed during glass melting. When electricity flows into a melting furnace during electrical heating, the furnace is corroded. However, if the specific resistance of the glass in the furnace is high, electricity flows more easily through the furnace. Corrosion of the melting furnace can lead to glass leakage from the melting furnace or components resulting from the corrosion of the melting furnace being mixed into the glass. Therefore, it is preferable to be able to suppress the corrosion of the melting furnace. The natural logarithm lnρ of the specific resistance ρ can be used as an indicator of low specific resistance. In one embodiment, the natural logarithm lnρ (unitless) of the resistivity ρ (unit: Ω cm) at 1450°C of Glasses A and B is preferably 3.20 or less, more preferably 3.00 or less, even more preferably 2.90 or less, still more preferably 2.80 or less, still more preferably 2.70 or less, still more preferably 2.68 or less, and still more preferably 2.65 or less. Furthermore, the natural logarithm lnρ of the resistivity ρ at 1450°C can be, for example, 1 or more.

[0070] [Magnetic Recording Medium Substrate] A magnetic recording medium substrate according to one aspect of the present invention is made of Glass A or Glass B.

[0071] A magnetic recording medium substrate can be manufactured by heating glass raw materials to prepare a glass melt, forming the glass melt into a plate by any of the press molding, down-draw, and float processes, and then processing the resulting glass melt. For example, in the press molding process, the glass melt flowing out of a glass flow pipe is cut to a predetermined volume to obtain a desired glass melt lump, which is then press-molded in a press mold to produce a thin, disk-shaped substrate blank. Next, a center hole is formed in the resulting substrate blank, and the inner and outer peripheries are processed, and both main surfaces are lapped and polished. Next, a cleaning process including acid washing and alkali washing is performed to obtain a disk-shaped substrate.

[0072] In one embodiment, the magnetic recording medium substrate has a homogeneous surface and internal composition. Here, "homogeneous surface and internal composition" means that ion exchange has not been performed (i.e., the substrate does not have an ion exchange layer). For example, a magnetic recording medium substrate without an ion exchange layer can be used in cases where an HDD (hard disk drive) incorporating the magnetic recording medium is used in an environment that is unlikely to be subjected to external shocks. Furthermore, since a magnetic recording medium substrate without an ion exchange layer has not been subjected to an ion exchange process, manufacturing costs can be significantly reduced.

[0073] In one embodiment, the magnetic recording medium substrate has an ion-exchange layer on part or all of its surface. Because the ion-exchange layer exhibits compressive stress, the presence or absence of the ion-exchange layer can be confirmed by breaking the substrate perpendicular to the main surface and obtaining a stress profile on the fracture surface using the Babinet method. The "main surface" refers to the surface of the substrate on which the magnetic recording layer is provided or is provided. This surface is called the main surface because it has the largest area among the surfaces of the magnetic recording medium substrate. In the case of a disk-shaped magnetic recording medium, this corresponds to the circular surface of the disk (excluding the center hole, if any). The presence or absence of the ion-exchange layer can also be confirmed by measuring the concentration distribution of alkali metal ions in the depth direction from the substrate surface.

[0074] The ion exchange layer can be formed by contacting an alkali salt with the substrate surface at high temperature and exchanging the alkali metal ions in the alkali salt with the alkali metal ions in the substrate. Ion exchange (also called "strengthening treatment" or "chemical strengthening") can be performed using known techniques. For example, see paragraphs 0068 to 0069 of WO2011 / 019010A1.

[0075] The magnetic recording medium substrate has a thickness of, for example, 1.5 mm or less, preferably 1.2 mm or less, more preferably 1 mm or less, and the lower limit of the thickness is preferably 0.3 mm. The magnetic recording medium substrate is preferably in the shape of a disk having a center hole.

[0076] The magnetic recording medium substrate is made of amorphous glass, which can achieve superior surface smoothness when processed into a substrate compared to glass-ceramics.

[0077] [Magnetic Recording Medium] One aspect of the present invention relates to a magnetic recording medium having a magnetic recording layer on the above-described magnetic recording medium substrate.

[0078] Magnetic recording media are called magnetic disks, hard disks, etc., and are suitable for various magnetic recording and playback devices, such as internal storage devices (fixed disks, etc.) of desktop personal computers, server computers, notebook personal computers, mobile personal computers, etc., internal storage devices of portable recording and playback devices that record and play back images and / or audio, recording and playback devices for in-car audio, etc. In this invention and this specification, the term "magnetic recording and playback device" refers to a device that is capable of either or both of magnetically recording information and magnetically playing back information.

[0079] The magnetic recording medium has a structure in which, for example, at least an adhesive layer, an underlayer, a magnetic layer (magnetic recording layer), a protective layer, and a lubricating layer are laminated on the main surface of a magnetic recording medium substrate in order from the side closest to the main surface. For example, the magnetic recording medium substrate is introduced into a vacuum-drawn film-forming device, and films from the adhesive layer to the magnetic layer are sequentially formed on the main surface of the magnetic recording medium substrate using a DC (Direct Current) magnetron sputtering method in an Ar atmosphere. For example, CrTi can be used as the adhesive layer, and a material containing Ru or MgO can be used as the underlayer. Note that a soft magnetic layer and a heat sink layer may be added as appropriate. After the above-mentioned film formation, a C layer is formed by, for example, a CVD (Chemical Vapor Deposition) method. 2 H 4 A magnetic recording medium can be formed by forming a protective layer using a nitriding agent and then performing a nitriding process to introduce nitrogen into the surface in the same chamber. Thereafter, a lubricating layer can be formed by applying, for example, PFPE (polyfluoropolyether) onto the protective layer by a dip coating method.

[0080] To achieve even higher recording densities in magnetic recording media, the magnetic recording layer preferably contains a magnetic material with high magnetic anisotropy energy. From this perspective, preferred magnetic materials include Fe—Pt-based magnetic materials or Co—Pt-based magnetic materials. Here, "based" means "contained." That is, the magnetic recording medium preferably has a magnetic recording layer containing Fe and Pt, or Co and Pt. For magnetic recording layers containing such magnetic materials and methods for forming them, see paragraph 0074 of WO 2011 / 019010 A1 and the examples therein. Furthermore, magnetic recording media having such magnetic recording layers are preferably applied to magnetic recording devices using a recording method known as energy-assisted recording. Among energy-assisted recording methods, a recording method that assisted magnetization reversal by irradiation with near-field light or the like is called a thermally assisted recording method, and a recording method that assisted magnetization reversal by microwaves is called a microwave-assisted recording method. For details, see paragraph 0075 of WO 2011 / 019010 A1. As the magnetic material for forming the magnetic recording layer, a conventional CoPtCr-based material may be used.

[0081] In recent years, magnetic heads have been equipped with a DFH (Dynamic Flying Height) mechanism, which significantly reduces the gap between the read / write element of the magnetic head and the surface of the magnetic recording medium (reducing the flying height), thereby achieving even higher recording densities. The DFH mechanism involves providing a heating element, such as a tiny heater, near the read / write element of the magnetic head, causing only the periphery of the element to protrude toward the surface of the medium. This reduces the distance (flying height) between the magnetic head and the magnetic recording layer of the medium, making it possible to pick up signals from smaller magnetic particles and achieving even higher recording densities. However, this also results in an extremely small gap (flying height) between the element of the magnetic head and the surface of the medium. If irregularities caused by bubbles exist on the surface of the magnetic recording medium substrate, these irregularities are reflected on the surface of the magnetic recording medium, reducing the surface smoothness of the magnetic recording medium. As described above, when a magnetic head is brought close to the surface of a magnetic recording medium with poor surface smoothness, there is a risk that the magnetic head may come into contact with the surface of the magnetic recording medium and be damaged, so a certain flying height must be maintained to prevent contact. For these reasons, it is desirable to reduce bubbles in the magnetic recording medium substrate in order to produce a magnetic recording medium with high surface smoothness. Reducing bubbles in the substrate makes it possible to narrow the flying height. Since the magnetic recording medium substrate preferably has reduced bubbles, the magnetic recording medium equipped with such a substrate is also suitable for a magnetic recording device equipped with a DFH mechanism that has an extremely narrow flying height.

[0082] There are no particular limitations on the dimensions of the magnetic recording medium substrate (e.g., magnetic disk substrate) and magnetic recording medium (e.g., magnetic disk). However, since high recording density is possible, the media and substrate can be miniaturized. For example, the nominal diameter can be 2.5 inches, and even smaller diameters (e.g., 1 inch, 1.8 inch), or even 3 inches or 3.5 inches can be used. Furthermore, the plate thickness can be, for example, 0.3 to 2 mm, but Glasses A and B are suitable for thin plates due to their excellent heat resistance and rigidity. Thinning the plate allows for an increased number of magnetic recording media to be mounted on a HDD, thereby increasing the recording capacity of the HDD. From this perspective, the plate thickness is preferably 0.635 mm or less in nominal value, more preferably 0.550 mm or less, even more preferably 0.500 mm or less, and even more preferably 0.400 mm or less.

[0083] [Glass spacer for magnetic recording / reproducing device] One aspect of the present invention is a glass spacer made of SiO 2 The content is 56 to 80 mol%, Li 2 O content is 1 to 10 mol %, B 2 O 3 The total content of MgO and CaO (MgO + CaO) is 9 to 40 mol%, and the specific gravity is 2.75 g / cm 3 The present invention relates to a glass spacer for a magnetic recording / reproducing device, which comprises an amorphous oxide glass having a glass transition temperature of 650° C. or higher and a Young's modulus of 90 GPa or higher.

[0084] Another aspect of the present invention is a method for manufacturing a silicon dioxide film comprising: 2 The content is 56 to 80 mol%, Li 2 O content is 1 to 10 mol %, B 2 O 3 The total content of MgO and CaO (MgO+CaO) is 9 to 40 mol %, Al 2 O 3 SiO content 2 and ZrO 2 The molar ratio of the total content of (SiO 2 + ZrO 2 ) / Al 2 O 3) is 2 to 13, and the glass spacer for a magnetic recording / reproducing device comprises an amorphous oxide glass having a glass transition temperature of 650° C. or higher and a Young's modulus of 90 GPa or higher.

[0085] Magnetic recording media can be used in magnetic recording and / or reproducing devices to magnetically record and / or reproduce information. Magnetic recording and reproducing devices typically include spacers for fixing the magnetic recording media to the spindle of a spindle motor and / or for maintaining a distance between multiple magnetic recording media. In recent years, the use of glass spacers as such spacers has been proposed. For reasons similar to those detailed above for the glass for magnetic recording medium substrates, these glass spacers are also desired to have excellent heat resistance and rigidity. In contrast, as detailed above for Glasses A and B, the above glasses can have excellent heat resistance and rigidity, making them suitable as glass spacers for magnetic recording and reproducing devices.

[0086] The spacer for a magnetic recording / reproducing device is a ring-shaped member, and details such as the structure and manufacturing method of the glass spacer are publicly known. Regarding the manufacturing method of the glass spacer, the above-mentioned descriptions regarding the manufacturing method of glass for a magnetic recording medium substrate and the manufacturing method of a magnetic recording medium substrate can be referenced. Regarding other details such as the glass composition and glass properties of the glass spacer for a magnetic recording / reproducing device according to one embodiment of the present invention, the above-mentioned descriptions regarding the glass for a magnetic recording medium substrate, the magnetic recording medium substrate, and the magnetic recording medium according to one embodiment of the present invention can be referenced. The glass spacer for a magnetic recording / reproducing device can be made of the above-mentioned glass, or can be configured with one or more layers, such as a conductive film, provided on the surface of the glass. For example, to remove static electricity generated during rotation of the magnetic recording medium, a conductive film such as a NiP alloy can be formed on the surface of the glass spacer by plating, immersion, vapor deposition, sputtering, or the like. Furthermore, the glass spacer can be polished to increase its surface smoothness (e.g., an average surface roughness of 1 μm or less), thereby strengthening the adhesion between the magnetic recording medium and the spacer and suppressing misalignment.

[0087] [Magnetic Recording and Reproducing Apparatus] One aspect of the present invention relates to a magnetic recording and reproducing apparatus including at least one of: a magnetic recording medium according to one aspect of the present invention; and a glass spacer according to one aspect of the present invention.

[0088] A magnetic recording and reproducing device includes at least one magnetic recording medium and at least one spacer, and typically further includes a spindle motor for rotating the magnetic recording medium and at least one magnetic head for recording and / or reproducing information on the magnetic recording medium. The magnetic recording and reproducing device according to one aspect of the present invention may include a magnetic recording medium according to one aspect of the present invention as at least one magnetic recording medium, or may include multiple magnetic recording media according to one aspect of the present invention. The magnetic recording and reproducing device according to one aspect of the present invention may include a glass spacer according to one aspect of the present invention as at least one spacer, or may include multiple glass spacers according to one aspect of the present invention. A small difference between the thermal expansion coefficients of the magnetic recording medium and the spacer is preferable from the viewpoint of suppressing the occurrence of phenomena that may arise due to the difference between the thermal expansion coefficients, such as distortion of the magnetic recording medium and reduced stability during rotation due to misalignment of the magnetic recording medium. From this viewpoint, the magnetic recording and reproducing device according to one aspect of the present invention preferably includes a magnetic recording medium according to one aspect of the present invention as at least one magnetic recording medium, or as more magnetic recording media if multiple magnetic recording media are included, and preferably includes a glass spacer according to one aspect of the present invention as at least one spacer, or as more spacers if multiple spacers are included. Furthermore, for example, in a magnetic recording and reproducing device according to one aspect of the present invention, the glass constituting the magnetic recording medium substrate included in the magnetic recording medium and the glass constituting the glass spacer can have the same glass composition.

[0089] A magnetic recording and reproducing device according to one embodiment of the present invention may include at least one of a magnetic recording medium according to one embodiment of the present invention and a glass spacer according to one embodiment of the present invention. Other aspects of the magnetic recording and reproducing device may be based on known techniques. In one embodiment, the magnetic head may be an energy-assisted magnetic recording head having an energy source (e.g., a heat source such as a laser light source, microwaves, etc.) for assisting magnetization reversal (assisting the writing of magnetic signals), a recording element, and a reproducing element. Such an energy-assisted magnetic recording head-equipped magnetic recording and reproducing device is useful as a magnetic recording and reproducing device with high recording density and high reliability. Furthermore, during the manufacture of magnetic recording media for use in energy-assisted magnetic recording and reproducing devices, such as thermally assisted magnetic recording devices equipped with a thermally assisted magnetic recording head having a laser light source, a magnetic recording layer containing a magnetic material with high magnetic anisotropy energy may be formed on a magnetic recording medium substrate. To form such a magnetic recording layer, a film is typically deposited at a high temperature, or a heat treatment is performed at a high temperature after deposition. A magnetic recording medium substrate according to one embodiment of the present invention is preferred as a magnetic recording medium substrate with high heat resistance that can withstand such high-temperature treatment. However, the magnetic recording and reproducing device according to one aspect of the present invention is not limited to an energy-assisted magnetic recording and reproducing device.

[0090] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the embodiments shown in the examples.

[0091] [Examples No. 1 to No. 76] Raw materials such as oxides, carbonates, nitrates, sulfates, and hydroxides were weighed and mixed to prepare blended raw materials so as to obtain glasses having the compositions shown in the tables below. These blended raw materials were charged into a melting tank and heated and melted in the range of 1400 to 1600°C. The resulting molten glass was then held in a refining tank at 1400 to 1550°C for 6 hours, after which the temperature was lowered (cooled down) and held in the range of 1200 to 1400°C for 1 hour, after which the molten glass was formed to obtain glasses (amorphous oxide glasses) for the evaluations described below. The heating can be performed using various heating methods, such as electrical heating.

[0092] [Evaluation Method] (1) Glass Transition Temperature (Tg) and Average Linear Expansion Coefficient (α) The glass transition temperature Tg and the average linear expansion coefficient α at 100 to 300° C. of each glass were measured using a thermomechanical analyzer (TMA).

[0093] (2) Young's Modulus The Young's modulus of each glass was measured by an ultrasonic method.

[0094] (3) Specific Gravity The specific gravity of each glass was measured by Archimedes' method.

[0095] (4) Specific Elastic Modulus The specific elastic modulus was calculated from the Young's modulus obtained in (2) above and the specific gravity obtained in (3) above.

[0096] (5) Glass Stability 100 g of each glass was placed in a platinum crucible, which was then placed in a heating furnace with the furnace temperature set to 1250°C or 1300°C. The crucible was then left for 16 hours while maintaining the furnace temperature (holding test). After 16 hours had elapsed, the crucible was removed from the heating furnace, and the glass in the crucible was transferred onto a refractory material and cooled to room temperature. The presence or absence of crystals in each glass was observed with an optical microscope and evaluated according to the following criteria: A: No crystals were observed when observed at a magnification with an optical microscope (40 to 100 times magnification). B: Crystals were observed when observed at a magnification with an optical microscope (40 to 100 times magnification), but no crystals were observed with the naked eye. C: Crystals were observed with the naked eye.

[0097] (6) Evaluation of bubble density rank A glass plate (substrate blank) with a thickness of approximately 1.2 mm was prepared from the glass melt obtained above. The surface of this glass plate was polished to be flat and smooth, and the interior of the glass was observed from the polished surface under an optical microscope at a magnification of 40 to 100 times, and the number of bubbles with a diameter of more than 0.03 mm (hereinafter simply referred to as "bubbles") was counted. The number of bubbles counted was divided by the mass of glass corresponding to the area observed under magnification, which was used to determine the bubble density. The bubble density rank was evaluated from rank S to rank F according to the bubble density determined by the above method. Specifically, a bubble density of 0 bubbles / kg was ranked S, a bubble density of 2 bubbles / kg or less was ranked A, a bubble density of more than 2 bubbles / kg but less than 10 bubbles / kg was ranked B, a bubble density of 10 bubbles / kg or more but less than 20 bubbles / kg was ranked C, a bubble density of 20 bubbles / kg or more but less than 50 bubbles / kg was ranked D, a bubble density of 50 bubbles / kg or more but less than 80 bubbles was ranked E, and a bubble density of 80 bubbles / kg or more was ranked F.

[0098] (7) Natural logarithm lnρ of resistivity ρ (1450°C) The glass to be measured for resistivity was melted to prepare a glass melt at a temperature of t°C, and the electrical conductivity σ (unit: S / cm) of this glass melt was measured using Pt-Rh ring electrodes (electrode distance 15 mm) at a voltage of 50 mV and a frequency of 20 kHz. The cell constant was measured using a reference solution with a concentration of 1 mol / dm 3 The electrical conductivity σ was determined using a KCl solution (temperature: 25°C). In the temperature range from about 1200°C to about 1600°C, the electrical conductivity σ was determined for each temperature t at temperature intervals of about 25 to 45°C, and the determined σ was plotted as an Arrhenius plot, from which the σ at 1450°C was determined from the straight line. From the σ at 1450°C thus determined, the resistivity ρ at 1450°C was determined using the equation resistivity ρ = 1 / σ, and the natural logarithm lnρ of the determined ρ was calculated.

[0099] The results are shown in the table below.

[0100]

[0101]

[0102]

[0103]

[0104]

[0105]

[0106]

[0107]

[0108]

[0109]

[0110] The results shown in the table above confirm that the magnetic recording medium substrate glasses of the examples all have excellent heat resistance and rigidity. Furthermore, the magnetic recording medium substrate glasses of the examples were also confirmed to have low specific gravity and a moderate thermal expansion coefficient. Regarding glass stability, in the retention test performed using the above method, the better the evaluation results at lower temperatures, the less likely the glass is to precipitate crystals in the molten state, and the glass can be molded at lower molding temperatures. Lowering the molding temperature extends the life of components of the molding equipment, such as heating elements, furnaces, and pipes. In particular, when producing substrate blanks by press molding, a lower molding temperature is preferable. Furthermore, lowering the molding temperature allows for increased glass viscosity during molding, thereby suppressing volatilization, striae, and molding bubble formation. Furthermore, the glass of the examples shown in the table above all had bubble density rankings of S, A, or B, confirming that bubble formation was suppressed.

[0111] [Preparation of Magnetic Recording Media Substrates] (1) Preparation of Substrate Blanks Next, a disk-shaped substrate blank was prepared by the following Method A or B. A similar method can also be used to prepare glass blanks for producing glass spacers for magnetic recording / reproducing devices. (Method A) The refined and homogenized glass melt of the above-described example was allowed to flow out of the flow pipe at a constant flow rate and received by a press-molding lower die. The flowed-out glass melt was then cut with a cutting blade to obtain a predetermined amount of glass melt gob on the lower die. The lower die bearing the glass melt gob was then immediately removed from the bottom of the pipe, and press-molded into a thin disk with a diameter of 66 mm and a thickness of 1.2 mm using an upper die and a barrel die facing the lower die. The press-molded product was cooled to a temperature at which it would not deform, then removed from the die and annealed to obtain a substrate blank. In the above-described molding process, multiple lower dies were used to successively mold the flowing glass melt into disk-shaped substrate blanks. (Method B) The clarified and homogenized glass melt of the above-described Examples was continuously poured from above into a heat-resistant mold having a cylindrical through-hole, formed into a cylindrical shape, and removed from below the through-hole. The removed glass was annealed, and then sliced ​​at regular intervals in a direction perpendicular to the cylindrical axis using a multi-wire saw to produce disk-shaped substrate blanks. While the above-described Methods A and B were employed in this Example, the following Methods C and D are also suitable for producing disk-shaped substrate blanks. Furthermore, the following Methods C and D are also suitable for producing glass blanks for producing glass spacers for magnetic recording / reproducing devices. (Method C) The glass melt of the above-described Examples can also be poured onto a float bath, formed into a glass sheet (forming by the float method), annealed, and then bored into a glass disk from the glass sheet to obtain a substrate blank. (Method D) The molten glass of the above-described Examples can be formed into a sheet of glass by the overflow downdraw method (fusion method), annealed, and then a disk of glass can be bored from the sheet of glass to obtain a substrate blank.

[0112] (2) Preparation of Glass Substrates. A through hole was drilled in the center of the substrate blank obtained by each of the above methods, and the outer and inner peripheries were ground. The main surfaces of the disk were then lapped and polished (mirror-polished) to produce a glass substrate for a magnetic disk with a diameter of 65 mm and a thickness of 0.8 mm. Using a similar method, a glass blank for producing a glass spacer for a magnetic recording / reproducing device can also be finished into a glass spacer for a magnetic recording / reproducing device. The glass substrate obtained above was cleaned using a 1.7% by weight aqueous solution of hydrofluorosilicic acid (HSiF) and then a 1% by weight aqueous solution of potassium hydroxide, followed by rinsing with pure water and drying. Magnified observation of the surface of the substrate prepared from the glass of the example revealed no surface roughness and a smooth surface.

[0113] [Preparation of Magnetic Recording Medium (Magnetic Disk)] An adhesive layer, an underlayer, a magnetic recording layer, a protective layer, and a lubricating layer were formed in this order on the main surface of a glass substrate obtained from the glass of the example by the following method, thereby obtaining a magnetic disk.

[0114] First, using a vacuum-drawn film-forming apparatus, an adhesive layer, an underlayer, and a magnetic recording layer were successively formed in an Ar atmosphere by DC magnetron sputtering.

[0115] The adhesive layer was formed using a CrTi target to form an amorphous CrTi layer with a thickness of 20 nm. A 10 nm thick MgO layer was then formed as an underlayer. The magnetic recording layer was formed using an FePtC or CoPtC target at a deposition temperature of 200 to 400°C to form a 10 nm thick granular layer of FePt or CoPt.

[0116] After the magnetic recording layer was formed, the magnetic disk was transferred from the film forming apparatus to a heating furnace and annealed. The temperature in the heating furnace during annealing was set to a range of 500 to 700°C. 10 Magnetic particles of CoPt-based alloy or FePt-based alloy with an ordered structure are formed. 10 Heating may be performed to create an ordered structure.

[0117] Next, a 3 nm protective layer made of hydrogenated carbon was formed by CVD using ethylene as the source gas. After this, a lubricating layer made of PFPE (perfluoropolyether) was formed by dip coating. The lubricating layer had a thickness of 1 nm. A magnetic disk was obtained through the above manufacturing process. The obtained magnetic disk was installed in a hard disk drive equipped with a DFH mechanism, and magnetic signals were recorded and reproduced in the recording area on the main surface of the magnetic disk at a recording density of 1000 gigabits per square inch. No collision between the magnetic head and the magnetic disk surface (crash failure) was observed.

[0118] Furthermore, a glass spacer obtained by the above manufacturing process using the glass of the example and having a NiP alloy conductive film formed on its surface (a glass spacer with a NiP alloy film) was mounted in a hard disk drive equipped with a DFH mechanism, and magnetic signals were recorded and reproduced at a recording density of 1000 gigabits per square inch in a recording area on the main surface of a magnetic disk separately prepared using a substrate made of a material different from the glass according to one embodiment of the present invention (Glass A or Glass B). No collision between the magnetic head and the magnetic disk surface (crash failure) was observed.

[0119] Furthermore, when the magnetic disk and the glass spacer with NiP alloy film manufactured as described above using the same glass material according to one embodiment of the present invention were mounted in a hard disk drive equipped with a DFH mechanism, and magnetic signals were recorded and reproduced in the recording area on the main surface of the magnetic disk at a recording density of 1000 gigabits per square inch, no collision between the magnetic head and the magnetic disk surface (crash failure) was observed. Here, since the glass substrate and the glass spacer included in the magnetic disk are made of the same glass material, it is clear that the phenomenon that can occur due to the difference in thermal expansion coefficient described above does not occur.

[0120] According to one aspect of the present invention, it is possible to provide a magnetic recording medium suitable for high-density recording.

[0121] Finally, the above-mentioned aspects will be summarized.

[0122] According to one embodiment, SiO 2 The content is 56 to 80 mol%, Li 2 O content is 1 to 10 mol %, B 2 O 3 The total content of MgO and CaO (MgO + CaO) is 9 to 40 mol %, and the specific gravity is 2.75 g / cm 3 Glass for magnetic recording medium substrates, which is an amorphous oxide glass having a glass transition temperature of 650° C. or higher and a Young's modulus of 90 GPa or higher; and SiO 2 The content is 56 to 80 mol%, Li 2 O content is 1 to 10 mol %, B 2 O 3 The content is 0 to 4 mol%, the total content of MgO and CaO (MgO + CaO) is 9 to 40 mol%, Al 2 O 3 SiO content 2 and ZrO 2 The molar ratio of the total content of (SiO 2 + ZrO 2 ) / Al 2 O 3 ) is 2 to 13, and is an amorphous oxide glass having a glass transition temperature of 650° C. or higher and a Young's modulus of 90 GPa or higher.

[0123] According to one embodiment, SiO 2 The content is 56 to 80 mol%, Li 2 O content is 1 to 10 mol %, B 2 O 3 The total content of MgO and CaO (MgO + CaO) is 9 to 40 mol %, and the specific gravity is 2.75 g / cm 3 a glass spacer for a magnetic recording / reproducing device, comprising an amorphous oxide glass having a glass transition temperature of 650° C. or higher and a Young's modulus of 90 GPa or higher; and SiO 2 The content is 56 to 80 mol%, Li 2 O content is 1 to 10 mol %, B 2 O 3 The content is 0 to 7 mol%, the total content of MgO and CaO (MgO + CaO) is 9 to 40 mol%, Al 2 O 3SiO content 2 and ZrO 2 The molar ratio of the total content of (SiO 2 + ZrO 2 ) / Al 2 O 3 ) is 2 to 13, and the glass spacer for a magnetic recording / reproducing device comprises an amorphous oxide glass having a glass transition temperature of 650° C. or higher and a Young's modulus of 90 GPa or higher.

[0124] The glass for a magnetic recording medium substrate has excellent heat resistance and rigidity, as does the glass spacer for a magnetic recording / reproducing device.

[0125] In one embodiment, the average linear expansion coefficient of the oxide glass at 100 to 300°C is 40 x 10 -7 ~70 x 10 -7 / °C range.

[0126] In one embodiment, the CaO content of the oxide glass can be in the range of 0 to 18 mol %.

[0127] In one embodiment, the total content of BaO and SrO in the oxide glass can be in the range of 0 to 2 mol %.

[0128] In one embodiment, the Li of the oxide glass 2 O, Na 2 O and K 2 The total content of O (Li 2 O + Na 2 O+K 2 O) can range from 2.5 to 10 mole percent.

[0129] In one embodiment, the SnO 2 and CeO 2 The total content (SnO 2 + CeO 2 ) can range from 0.05 to 2 mole percent.

[0130] In one embodiment, the CeO of the oxide glass 2 SnO content 2 Molar ratio of content (SnO 2 / CeO 2 ) can be 1 or more.

[0131] In one embodiment, the oxide glass contains, in mol %, SiO 2 Content is 56-65%, Al 2 O 3 Content 5-20%, B 2 O 3 Content is 0-4%, MgO content is 3-28%, Li 2 O content 1-10%, SiO 2 and Al 2 O 3 The total content (SiO 2 +Al 2 O 3 ) is 65 to 80%, the total content of MgO and CaO (MgO + CaO) is 11 to 30%, the total content of MgO, CaO, SrO and BaO (MgO + CaO + SrO + BaO) is 12 to 30%, the MgO content, 0.7 × the CaO content, Li 2 O content, TiO 2 Content and ZrO 2 Sum of contents (MgO+0.7CaO+Li 2 O+TiO 2 + ZrO 2 ) is 16% or more, 5 × Li 2 O content, 3×Na 2 O content, 3×K 2 O content, 2×B 2 O 3 content, MgO content, 2×CaO content, 3×SrO content, and BaO content (5Li 2 O + 3Na 2 O+3K 2 O+2B 2 O 3 +MgO+2CaO+3SrO+BaO) is 32-58%, SiO 2 Content, Al 2 O 3 Content, B 2 O 3 Content, P 2 O 5 Content, 1.5×Na 2 O content, 1.5×K 2 The sum of the O content, 2×SrO content, 3×BaO content and ZnO content (SiO 2 +Al 2 O3 +B 2 O 3 +P 2 O 5 +1.5Na 2 O+1.5K 2 O + 2SrO + 3BaO + ZnO) is 86% or less, SiO 2 Content, Al 2 O 3 Content, B 2 O 3 Content, P 2 O 5 Content, Na 2 O content, K 2 The sum of the O content, the CaO content, 2×SrO content, and 3×BaO content (SiO 2 +Al 2 O 3 +B 2 O 3 +P 2 O 5 +Na 2 O+K 2 O + CaO + 2SrO + 3BaO) is 92% or less, the molar ratio of the CaO content to the MgO content (CaO / MgO) is 2.5 or less, Li 2 Na content relative to O content 2 Molar ratio of O content (Na 2 O / Li 2 O) is 5 or less, and the Li content relative to the total content of MgO and CaO 2 Molar ratio of O content (Li 2 O / (MgO+CaO)) is 0.03 to 0.4, Li 2 O, Na 2 O and K 2 SiO relative to the total content of O 2 Molar ratio of content (SiO 2 / (Li 2 O + Na 2 O+K 2 O)) is 4 to 22, Al 2 O 3 SiO content 2 and ZrO 2 The molar ratio of the total content of (SiO 2 + ZrO 2 ) / Al 2 O 3) is 2 to 10, and TiO relative to the total content of MgO and CaO 2 and Al 2 O 3 The molar ratio of the total content of (TiO 2 +Al 2 O 3 ) / (MgO+CaO)) is 0.35 to 2, the molar ratio of the total content of MgO and CaO to the total content of MgO, CaO, SrO and BaO ((MgO+CaO) / (MgO+CaO+SrO+BaO)) is 0.7 to 1, the molar ratio of the content of BaO to the total content of MgO, CaO, SrO and BaO (BaO / (MgO+CaO+SrO+BaO)) is 0.1 or less, B 2 O 3 , SiO 2 , Al 2 O 3 and P 2 O 5 P relative to the total content of 2 O 5 Molar ratio of content (P 2 O 5 / (B 2 O 3 +SiO 2 +Al 2 O 3 +P 2 O 5 )) can be 0.005 or less.

[0132] According to one embodiment, there is provided a magnetic recording medium substrate made of the above-mentioned glass for magnetic recording medium substrates.

[0133] In one embodiment, the magnetic recording medium substrate has a homogeneous composition on the surface and in the interior.

[0134] According to one embodiment, there is provided a magnetic recording medium having a magnetic recording layer on the above magnetic recording medium substrate.

[0135] According to one aspect, there is provided a magnetic recording and reproducing device including at least one of the above magnetic recording medium and the above glass spacer for a magnetic recording and reproducing device.

[0136] The embodiments disclosed herein should be considered to be illustrative in all respects and not restrictive. The scope of the present invention is defined by the claims, not by the above description, and is intended to include all modifications within the meaning and scope of the claims. For example, by adjusting the composition as described in the specification to the glass compositions exemplified above, it is possible to produce glass for magnetic recording medium substrates and glass spacers for magnetic recording / reproducing devices according to one aspect of the present invention. Furthermore, it is of course possible to arbitrarily combine two or more of the items described in the specification as examples or preferred ranges.

Claims

1. SiO 2 The content is 56 to 80 mol%, Li 2 O content is 1 to 10 mol %, B 2 O 3 The total content of MgO and CaO (MgO + CaO) is 9 to 40 mol%, and the specific gravity is 2.75 g / cm 3 Hereinafter, a glass for a magnetic recording medium substrate is an amorphous oxide glass having a glass transition temperature of 650° C. or higher and a Young's modulus of 90 GPa or higher.

2. SiO 2 The content is 56 to 80 mol%, Li 2 O content is 1 to 10 mol %, B 2 O 3 The total content of MgO and CaO (MgO+CaO) is 9 to 40 mol %, Al 2 O 3 SiO content 2 and ZrO 2 The molar ratio of the total content of (SiO 2 + ZrO 2 ) / Al 2 O 3 ) is 2 to 13, and the glass for a magnetic recording medium substrate is an amorphous oxide glass having a glass transition temperature of 650° C. or higher and a Young's modulus of 90 GPa or higher.

3. The average linear expansion coefficient at 100 to 300°C is 40 x 10 -7 ~70 x 10 -7 3. The glass for a magnetic recording medium substrate according to claim 1, wherein the glass has a viscosity of 1000 MPa or more.

4. The glass for a magnetic recording medium substrate according to any one of claims 1 to 3, wherein the CaO content is in the range of 0 to 18 mol %.

5. The glass for a magnetic recording medium substrate according to any one of claims 1 to 4, wherein the total content of BaO and SrO is in the range of 0 to 2 mol %.

6. Li 2 O, Na 2 O and K 2 The total content of O (Li 2 O + Na 2 O+K 2 6. The glass for a magnetic recording medium substrate according to claim 1, wherein O) is in the range of 2.5 to 10 mol %.

7. SnO 2 and CeO 2 The total content (SnO 2 + CeO 2 7. The glass for a magnetic recording medium substrate according to claim 1, wherein the content of ZnO is in the range of 0.05 to 2 mol %.

8. CeO 2 SnO content 2 Molar ratio of content (SnO 2 / CeO 2 8. The glass for a magnetic recording medium substrate according to claim 1, wherein the number of nuclei is 1 or more.

9. A magnetic recording medium substrate made of the glass for magnetic recording medium substrates according to any one of claims 1 to 8.

10. A magnetic recording medium having a magnetic recording layer on the magnetic recording medium substrate according to claim 9.

11. SiO 2 The content is 56 to 80 mol%, Li 2 O content is 1 to 10 mol %, B 2 O 3 The total content of MgO and CaO (MgO + CaO) is 9 to 40 mol%, and the specific gravity is 2.75 g / cm 3 Hereinafter, a glass spacer for a magnetic recording / reproducing device includes an amorphous oxide glass having a glass transition temperature of 650° C. or higher and a Young's modulus of 90 GPa or higher.

12. SiO 2 The content is 56 to 80 mol%, Li 2 O content is 1 to 10 mol %, B 2 O 3 The total content of MgO and CaO (MgO+CaO) is 9 to 40 mol %, Al 2 O 3 SiO content 2 and ZrO 2 The molar ratio of the total content of (SiO 2 + ZrO 2 ) / Al 2 O 3 ) is 2 to 13, and the glass spacer for a magnetic recording / reproducing device comprises an amorphous oxide glass having a glass transition temperature of 650° C. or higher and a Young's modulus of 90 GPa or higher.

13. A magnetic recording and reproducing device comprising at least one of the magnetic recording medium according to claim 10 and the glass spacer for a magnetic recording and reproducing device according to claim 11 or 12.