A processing method for ultra-thick special-shaped reinforcement sheet of flexible circuit
Patent Information
- Application Number
- CN202010738574.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-07-28
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-07-28
AI Technical Summary
In the mass production of flexible circuit boards, it is difficult to achieve automated bonding of materials with a thickness of more than 0.35mm, resulting in difficult to ensure the bonding progress and efficiency.
The adhesive PET bearing sheet is cross-combined with the reinforcement sheet, and the automatic bonding of the coil is achieved through cutting, rolling and laser cutting technologies, and the acrylic adhesive layer and protective film are used to improve the bonding strength and accuracy.
The yield and mass production efficiency of special-shaped reinforcement sheets are improved, the separation between release paper and reinforcement sheets is avoided, and the reliability and consistency of fit is enhanced.
Smart Images

Figure CN112040630B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of flexible circuit board processing, and in particular to a method for processing an ultra-thick special-shaped reinforcement sheet of a flexible circuit. Background Art
[0002] Flexible Printed Circuit (FPC), also known as soft circuit board, has been widely used due to its excellent properties such as light weight, thin thickness, and free bending and folding.
[0003] As flexible printed circuit boards (FPCs) become thinner, quality requirements continue to rise, requiring local reinforcement, and the thickness of these reinforcements is also increasing. For irregularly shaped reinforcement sheets thicker than 0.35mm with small holes and slots, these sheets can be made of polyimide (PI), glass cloth substrate (FR4), or other materials. These thick sheets present numerous challenges during FPC production, ultimately requiring manual lamination of individual PCs, making it impossible to guarantee lamination progress and efficiency during mass production. Summary of the Invention
[0004] In view of the above, the present invention provides a method for processing ultra-thick special-shaped reinforcing sheets for flexible circuits. In order to solve this problem, the material preparation method is changed, and a single sheet of adhesive-coated PET carrier is cross-combined with the reinforcing sheet to achieve the purpose of automatic roll bonding.
[0005] A method for processing an ultra-thick special-shaped reinforcement sheet for a flexible circuit, comprising:
[0006] Step A. Cut the raw material of the reinforcing sheet into small pieces, and use a slotting knife to make grooves and / or holes on the cut reinforcing sheets according to the design requirements. The reinforcing sheet includes a reinforcing base layer, an adhesive layer, and a release paper layer. The thickness of the reinforcing base layer is ≥0.35 mm.
[0007] The raw material of the reinforcing sheet may be in the form of a roll or a sheet. We define reinforcing sheets with a thickness of ≥0.35mm as super-thick reinforcing sheets. Special-shaped refers to reinforcing sheets with a special shape, such as irregular or non-rectangular. Of course, the technical solution provided by the present invention can also be used to process reinforcing sheets of conventional shapes.
[0008] Step B. removing the release paper layer and bonding the reinforcing base layer after the release paper layer is removed to a PET sheet, wherein the PET substrate layer of the PET sheet is coated with an acrylic adhesive layer, and a portion of the PET substrate layer is left blank where the reinforcing base layer is not bonded;
[0009] The raw material of the PET sheet can also be in sheet or roll form, and can be coated with a strong acrylic adhesive before step B, or can be coated with an acrylic adhesive and provided with a release sheet material on the surface, and the release sheet material is removed before this step.
[0010] Step D: Bonding the PET sheets bonded to the reinforced base layer piece by piece onto the roll of protective film according to a set pattern, and bonding the protective film to the blank area of the acrylic adhesive layer.
[0011] Polyethylene terephthalate (PET), commonly known as polyester resin, is the most common type of thermoplastic polyester. It is a condensation polymer of terephthalic acid and ethylene glycol. Together with PBT, it is collectively referred to as thermoplastic polyester, or saturated polyester.
[0012] Acrylic adhesive can also be replaced by other adhesive materials.
[0013] Release paper is a commonly used consumable material in FPC production. Its important function is to isolate, fill, and protect finished products, semi-finished products, and raw materials. During FPC processing, it is often necessary to apply film to raw materials or semi-finished products, and then remove the film in another process.
[0014] Preferably, in step B, bonding the reinforcing base layer after removing the release paper layer to the PET sheet comprises:
[0015] B1. Manual pre-pasting, at least on one side of the reinforcement base and PET sheet, the adhesive layer of the reinforcement plate and the acrylic adhesive layer of the PET sheet are bonded together;
[0016] B2. Peel off a portion of the PET substrate layer from the reinforcing base layer, leaving a local bonding portion of 10 to 20 mm or more;
[0017] Feed the locally bonded portion into a roller press with the reinforced base layer at the bottom;
[0018] Through the rolling and driving action of the upper and lower rollers, the PET base layer and the reinforcing base layer are closely fitted.
[0019] A knife cutter is used to cut the polyimide reinforcing sheet roll to a fixed size, using the pressure of the metal blade to quickly and sequentially sever the molecular connections between the polyimide reinforcing sheet and the release paper material. The reinforcing sheet has a theoretical thickness greater than 0.35mm, a large cross-sectional area, and high cohesion, resulting in high shear strength. This easily causes the release paper to peel, making it unsuitable for special-shaped processing, grooving, or drilling. Rapid cutting reduces peeling caused by the weak adhesive during the cutting process. The polyimide roll is covered with a release paper, which has poor flexibility, while the polyimide reinforcing sheet has a certain degree of flexibility. Due to uneven tension, the reinforcing sheet undergoes elastic deformation that is different from the elastic deformation of the release paper, which easily causes peeling.
[0020] Preferably, in step B, the linear speed of the upper roller and the lower roller is 20-50 m / h, the rolling pressure of the upper roller and the lower roller is 0.2-0.4 MPa, and the rolling temperature is 90-110° C.;
[0021] During the rolling process, the reinforcing base layer is set horizontally at the bottom, and the peeled PET substrate layer is gradually fed between the upper roller and the lower roller at an angle of 35° to 50° to the reinforcing base layer. During the feeding process, a traction force of 0.3 to 0.7 kN is applied to the PET substrate layer.
[0022] During the rolling process, the PCT substrate layer should be kept in a certain tension state to avoid wrinkles. After rolling, there should be no bubbles, delamination or warping.
[0023] Preferably, after step B and before step D, the method further comprises:
[0024] Step C. Using laser cutting to cut the bonded PET substrate layer and the reinforcing base layer into shape, positioning the edges during the cutting process using the grooves and / or holes formed in Step A; cutting the two sides of the PET substrate layer in the long direction into serrated edges;
[0025] In step D: each cut PET substrate layer is sequentially adhered to the rolled protective film, and the serrated edge on one side of each PET substrate layer can be aligned with the serrated edge of another PET substrate layer on the adjacent side.
[0026] Processing the special-shaped structure after pasting the PCT substrate layer can avoid the separation of the release paper and the reinforcement sheet and improve the yield rate.
[0027] Preferably, in step C: when laser cutting the PET substrate layer and the reinforcing base layer to perform outer shape cutting, the reinforcing base layer is on the upper side;
[0028] In step A, the reinforcing sheet raw material is cut into small pieces by punching, and the punching is performed by a rapid punching method.
[0029] Preferably, in step A, using a grooving knife to form grooves and / or holes on the cut reinforcement sheet according to design requirements includes:
[0030] Stack the reinforcement sheets to be cut together, and use a phenolic board as the drilling board for the bottom layer and the top layer respectively;
[0031] Then use tape to stick the four corners, and use tape to fix the gong groove and gong hole on the surrounding side of the phenolic board. One side of the tape is pasted on the edge of the phenolic board, and the other side of the tape is pasted on the table of the drilling machine.
[0032] Preferably, before step B, the following steps are further included:
[0033] An array of blind holes is created on the side of the PET substrate facing away from the acrylic adhesive layer. The depth of the blind holes is 30% or less of the PCT substrate layer, and the total area of the blind holes is 20% to 40% of the PCT substrate layer's surface area. The purpose of creating this array of blind holes is to increase the flexibility of the PET substrate and facilitate roll fabrication.
[0034] Preferably, in step B, before bonding the reinforcing base layer after removing the release paper layer to the PET sheet, the process further comprises:
[0035] For viscosity reduction treatment, a clean release sheet is used to bond the adhesive layer on the surface of the reinforcing base layer after removing the release paper layer. Micro-synapses are formed on the surface of the release sheet, and nano-brush hairs are placed on the surface of the micro-synapses. The height of the micro-synapses is 10-50μm, the length of the nano-brush hairs is 50-300nm, and the diameter of the nano-brush hairs is 100-300nm. Relying solely on acrylic adhesive can ensure bonding strength. Removing the adhesive layer of the reinforcing base layer helps to strengthen the bonding between the acrylic adhesive and the reinforcing base layer, thereby improving the yield rate.
[0036] Preferably, the viscosity reducing treatment is performed twice or more, the first viscosity reducing treatment and the second viscosity reducing treatment are performed at different positions, and 50% to 75% of the surface area of the adhesive layer is subjected to the viscosity reducing treatment.
[0037] Preferably, the acrylic adhesive layer coated on the PET substrate layer is non-uniformly coated;
[0038] The acrylic adhesive layer applied at the positions corresponding to the gong groove and gong hole is blank to prevent the acrylic adhesive from sticking to dust;
[0039] The thickness of the acrylic adhesive layer where the reinforcing base layer is not attached is 1.1 to 1.3 times that of the layer where the reinforcing base layer is attached, thereby improving the bonding strength between the acrylic adhesive and the protective film.
[0040] The beneficial effects of the present invention are as follows: the present invention discloses a method for processing an ultra-thick special-shaped reinforcing sheet for a flexible circuit, comprising: step A. cutting the reinforcing sheet raw material into small pieces of reinforcing sheets, using a slotting knife to form grooves and / or holes on the cut reinforcing sheets according to design requirements, wherein the grooves and holes include functional holes and positioning holes, the reinforcing sheet includes a reinforcing base layer, an adhesive layer and a release paper layer, the thickness of the reinforcing base layer is ≥0.35 mm, and we define this thickness as an ultra-thick reinforcing sheet; step B. removing the release paper layer, and bonding the reinforcing base layer after the release paper layer is removed to a PET sheet, wherein the PET substrate layer of the PET sheet is coated with an acrylic adhesive layer, and a portion of the PET substrate layer is left There is a blank portion of the acrylic adhesive layer to which the reinforcing base layer is not adhered; the bonded PET substrate layer and the reinforcing base layer are cut into shape by laser cutting, and the grooves and / or holes formed in step A are used for positioning during the cutting process; both sides of the long direction of the PET substrate layer are cut into serrated edges; in step D: each cut PET substrate layer is sequentially adhered to a rolled protective film, and the serrated edge on one side of each PET substrate layer can be aligned with the serrated edge of another PET substrate layer on an adjacent side; the protective film is adhered to the blank portion of the acrylic adhesive layer, and the adhesive-attached PET carrier sheet and the reinforcing sheet are cross-bonded to achieve the purpose of automated roll bonding. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] The following further describes a method for processing an ultra-thick special-shaped reinforcement sheet for a flexible circuit according to the present invention with reference to the accompanying drawings.
[0042] Figure 1 The present invention is a schematic flow chart of a method for processing an ultra-thick special-shaped reinforcement sheet for a flexible circuit.
[0043] Figure 2 The present invention is a structural schematic diagram of a method for processing an ultra-thick special-shaped reinforcing sheet for a flexible circuit when punching out the raw material of the reinforcing sheet.
[0044] Figure 3 The present invention is a structural schematic diagram of a PET sheet for a method of processing an ultra-thick special-shaped reinforcement sheet for a flexible circuit.
[0045] Figure 4 The present invention is a structural schematic diagram of a rolling process of a method for processing an ultra-thick special-shaped reinforcement sheet for a flexible circuit.
[0046] Figure 5 This is a partial enlarged view of the unrolled reinforcing sheet roll produced by the processing method of the ultra-thick special-shaped reinforcing sheet for a flexible circuit of the present invention.
[0047] Figure 6 The present invention is a structural schematic diagram of an unrolled reinforcing sheet roll produced by a processing method of an ultra-thick special-shaped reinforcing sheet for a flexible circuit.
[0048] Figure 7 The present invention is a cross-sectional view of a reinforcing sheet produced by a processing method of an ultra-thick special-shaped reinforcing sheet for a flexible circuit.
[0049] In the picture:
[0050] 1- reinforcing sheet; 11- reinforcing base layer; 12- adhesive layer; 13- release paper layer; 2- the PET substrate layer 21 of the PET sheet 2 is coated with an acrylic adhesive layer 22 . DETAILED DESCRIPTION
[0051] The following is combined with Figures 1 to 7 The processing method of the ultra-thick special-shaped reinforcement sheet of a flexible circuit of the present invention is further described.
[0052] A method for processing an ultra-thick special-shaped reinforcement sheet for a flexible circuit, comprising:
[0053] Step A. Cut the reinforcing sheet raw material into small pieces of reinforcing sheets 1, and use a slotting knife to groove and / or punch holes on the cut reinforcing sheets 1 according to the design requirements. The reinforcing sheet 1 includes a reinforcing base layer 11, an adhesive layer 12, and a release paper layer 13. The thickness of the reinforcing base layer 11 is ≥ 0.35 mm.
[0054] Step B. Remove the release paper layer 13 and adhere the reinforcing base layer 11 after the release paper layer 13 is removed to the PET sheet 2. The acrylic adhesive layer 22 is coated on the PET substrate layer 21 of the PET sheet 2. A portion of the PET substrate layer 21 is left blank where the acrylic adhesive layer 22 is not attached to the reinforcing base layer 11.
[0055] Step D: The PET sheets 2 bonded with the reinforcing base layer 11 are bonded piece by piece to the rolled protective film 5 according to a predetermined rule, and the protective film 5 is bonded to the blank area of the acrylic adhesive layer 22 .
[0056] In this embodiment, in step B, bonding the reinforcing base layer 11 after removing the release paper layer 13 to the PET sheet 2 includes:
[0057] B1. Manual pre-pasting, at least one edge of the reinforcement base 11 and the PET sheet 2, the adhesive layer 12 of the reinforcement plate and the acrylic adhesive layer 22 of the PET sheet 2 are bonded together;
[0058] B2. The PET substrate layer 21 is peeled off from a portion of the reinforcing base layer 11, leaving a local bonding portion of 10 to 20 MM or more, the local bonding portion is a non-functional component portion, and can finally be cut off;
[0059] Feed the locally bonded portion into a roller press with the reinforcement base 11 at the bottom;
[0060] The upper roller 31 and the lower roller 32 roll and drive the PET substrate layer 21 to fit tightly with the reinforcing base layer 11 .
[0061] In this embodiment, in step B, the linear speed of the upper roller 31 and the lower roller 32 is 20-50 m / h, the rolling pressure of the upper roller 31 and the lower roller 32 is 0.2-0.4 MPa, and the rolling temperature is 90-110° C.;
[0062] During the rolling process, the reinforcing base layer 11 is arranged horizontally at the bottom, and the peeled PET substrate layer 21 is gradually fed into between the upper roller 31 and the lower roller 32 at an angle of 35° to 50° to the reinforcing base layer 11. During the feeding process, a traction force of 0.3 to 0.7 kN is applied to the PET substrate layer 21.
[0063] In this embodiment, after step B and before step D, the following steps are further included:
[0064] Step C. Using laser cutting to cut the bonded PET substrate layer 21 and the reinforcing base layer 11 into shape, the shape cutting may also include cutting and processing of special-shaped holes or special-shaped grooves. During the shape cutting process, the grooves and / or holes formed in Step A are used for positioning. The PET substrate layer 21 is cut into serrated edges 211 on both sides of the longitudinal direction.
[0065] In step D: each cut PET substrate layer 21 is sequentially adhered to the rolled protective film 5, and the serrated edge 211 of one side of each PET substrate layer 21 can be aligned with the serrated edge 211 of another PET substrate layer 21 on the adjacent side.
[0066] In this embodiment, in step C: when the PET substrate layer 21 and the reinforcing base layer 11 are laser cut to perform the outer shape cutting, the reinforcing base layer 11 is on the upper side;
[0067] In step A, the raw material of the reinforcing sheet 1 is cut into small pieces of the reinforcing sheet 1 by punching.
[0068] In this embodiment, in step A, using a grooving knife to form grooves and / or holes on the cut reinforcement sheet 1 according to design requirements includes:
[0069] Stack the reinforcement sheets 1 to be cut together, and use a phenolic board as the drilling board for the bottom layer and the top layer respectively;
[0070] Then use tape to stick the four corners, and use tape to fix the gong groove and gong hole on the surrounding side of the phenolic board. One side of the tape is pasted on the edge of the phenolic board, and the other side of the tape is pasted on the table of the drilling machine.
[0071] In this embodiment, before step B, the following steps are also included:
[0072] An array of blind holes is made on the side of the PET substrate layer 21 facing away from the acrylic adhesive layer 22. The depth of the blind holes is less than or equal to 30% of the PCT substrate layer, and the total area of the array of blind holes is 20% to 40% of the surface area of the PCT substrate layer.
[0073] In this embodiment, in step B, before bonding the reinforcing base layer 11 after removing the release paper layer 13 to the PET sheet 2, the following steps are further included:
[0074] The viscosity-reducing treatment uses a clean release sheet to bond the adhesive layer 12 on the surface of the reinforcing base layer 11 after removing the release paper layer 13. Micro synapses are set on the surface of the release sheet, and nano-brush is set on the surface of the micro-synapses. The height of the micro-synapses is 10 to 50 μm, the length of the nano-brush is 50 to 300 nm, and the bristle diameter of the nano-brush is 100 to 300 nm.
[0075] In this embodiment, the viscosity reducing treatment is performed more than twice, the first viscosity reducing treatment and the second viscosity reducing treatment are staggered, and 50% to 75% of the surface area of the adhesive layer 12 is subjected to the viscosity reducing treatment.
[0076] The role of the viscosity-reducing treatment is to make the acrylic adhesive layer adhere to the reinforcement base as closely as possible, thereby improving the yield of the reinforcement base.
[0077] In this embodiment, the acrylic adhesive layer 22 coated on the PET substrate layer 21 is non-uniformly coated;
[0078] At the positions corresponding to the gong groove and the gong hole, the coated acrylic adhesive layer 22 is blank;
[0079] The thickness of the acrylic adhesive layer 22 where the reinforcing base layer 11 is not attached is 1.1 to 1.3 times that of the portion where the reinforcing base layer 11 is attached.
[0080] The above description is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements can be made without departing from the principles of the present invention. These improvements should also be regarded as the scope of protection of the present invention.
Claims
1. A method for processing an ultra-thick special-shaped reinforcement sheet for a flexible circuit, characterized in that: include: Step A. Cut the raw material of the reinforcing sheet into small pieces of reinforcing sheets, and use a slotting knife to make grooves and / or holes on the cut reinforcing sheets according to design requirements, wherein the reinforcing sheet comprises a reinforcing base layer, an adhesive layer and a release paper layer, and the thickness of the reinforcing base layer is ≥0.35 mm; Step B. removing the release paper layer, and bonding the reinforcing base layer after the release paper layer is removed to a PET sheet, wherein an acrylic adhesive layer is coated on the PET substrate layer of the PET sheet, and a blank portion of the acrylic adhesive layer where the reinforcing base layer is not bonded is left on the PET substrate layer; manually pre-bonding, aligning at least one edge of the reinforcing base layer and the PET sheet, and bonding the adhesive layer of the reinforcing sheet to the acrylic adhesive layer of the PET sheet; Step C. cutting the bonded PET substrate layer and the reinforcing base layer into shape by laser cutting, positioning the gong grooves and / or gong holes formed in step A during the cutting process; cutting the two sides of the PET substrate layer in the long direction into serrated edges; Step D: Each of the cut PET substrate layers is sequentially bonded to the rolled protective film, with the jagged edge of one side of each PET substrate layer being aligned with the jagged edge of another PET substrate layer on the adjacent side, and the protective film being bonded to the blank area of the acrylic adhesive layer.
2. The method for processing the ultra-thick special-shaped reinforcement sheet of the flexible circuit as claimed in claim 1, characterized in that: In the step B, bonding the reinforcing base layer after removing the release paper layer to the PET sheet also includes: B2. Peeling off a portion of the PET substrate layer from the reinforcing base layer, leaving a local bonding portion of more than 20MM; Send the local bonding part into the roller press with the reinforced base layer at the bottom; Through the rolling and driving action of the upper and lower rollers, the PET substrate layer and the reinforcing base layer are closely fitted.
3. The method for processing the ultra-thick special-shaped reinforcement sheet of the flexible circuit as claimed in claim 2, characterized in that: In the step B2, the linear speed of the upper roller and the lower roller is 20-50 m / h, the rolling pressure of the upper roller and the lower roller is 0.2-0.4 MPa, and the rolling temperature is 90-110° C.; During the rolling process, the reinforcing base layer is arranged horizontally at the bottom, and the partially peeled PET substrate layer is gradually fed between the upper roller and the lower roller at an angle of 35° to 50° with the reinforcing base layer. During the feeding process, a traction force of 0.3 to 0.7 KN is applied to the PET substrate layer.
4. The method for processing the ultra-thick special-shaped reinforcement sheet of the flexible circuit as claimed in claim 3, characterized in that: In the step C: when laser cutting the PET substrate layer and the reinforcing base layer to perform shape cutting, the reinforcing base layer is on the upper side; In the step A, the raw material of the reinforcing sheet is cut into small pieces of reinforcing sheet by punching.
5. The method for processing the ultra-thick special-shaped reinforcing sheet of the flexible circuit as claimed in claim 4, characterized in that: In the step A, using a groove cutter to make grooves and / or holes on the cut reinforcement sheet according to design requirements includes: Stack the cut reinforcement sheets together, and use a phenolic board as the drill plate for the bottom layer and the top layer respectively; Then use tape to stick the four corners, and also use tape to fix the gong groove and gong hole on the surrounding side of the phenolic board. One side of the tape is pasted on the edge of the phenolic board, and the other side of the tape is pasted on the table of the drilling machine.
6. The method for processing the ultra-thick special-shaped reinforcement sheet of the flexible circuit as claimed in claim 5, characterized in that: The step B also includes: An array of blind holes is made on the side of the PET substrate layer away from the acrylic adhesive layer. The depth of the blind holes is less than or equal to 30% of the thickness of the PET substrate layer. The total area of the array of blind holes is 20% to 40% of the surface area of the PET substrate layer.
7. The method for processing the ultra-thick special-shaped reinforcing sheet of the flexible circuit as claimed in claim 6, characterized in that: In the step B, before the reinforcing base layer after removing the release paper layer is bonded to the PET sheet, the step further includes: The viscosity reducing treatment uses a clean release sheet to bond the adhesive layer on the surface of the reinforcing base layer after removing the release paper layer, and micro synapses are arranged on the surface of the release sheet, and nano-brush is arranged on the surface of the micro-synapses, the height of the micro-synapses is 10 to 50 μm, the length of the nano-brush is 50 to 300 nm, and the bristle diameter of the nano-brush is 100 to 300 nm.
8. The method for processing the ultra-thick special-shaped reinforcing sheet of the flexible circuit as claimed in claim 7, characterized in that: The viscosity reducing treatment is performed more than twice, the first viscosity reducing treatment and the second viscosity reducing treatment are performed at different positions, and 50% to 75% of the surface area of the adhesive layer is subjected to the viscosity reducing treatment.
9. The method for processing the ultra-thick special-shaped reinforcing sheet of the flexible circuit as claimed in claim 8, characterized in that: The acrylic adhesive layer coated on the PET substrate layer is non-uniformly coated; At the positions corresponding to the gong groove and the gong hole, the coated acrylic adhesive layer is blank; The thickness of the acrylic adhesive layer at a location where the reinforcing base layer is not attached is 1.1 to 1.3 times that of the location where the reinforcing base layer is attached.