A kind of multi-twisted aluminum alloy cable and its preparation method and application

Through the structure of the corrugated aluminum alloy cable conductor and the optimized material formula, the problems of aluminum alloy single wire being easy to break and prone to mold breeding are solved, and the cable performance with high torsion resistance, salt spray and mold resistance are achieved, and it is suitable for offshore use. Wind power generation.

CN113871089BActive Publication Date: 2024-11-26JIANGSU HENGTONG POWER CABLE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111256058.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-27
Publication Date
2024-11-26
Estimated Expiration
2041-10-27

AI Technical Summary

Technical Problem

In the prior art, aluminum alloy single wire is prone to break wire during cable twisting, and offshore wind power cables are prone to breed mold, affecting product performance and aesthetics.

Method used

Using a composite twisted aluminum alloy cable conductor structure, a Class 5 aluminum alloy strands are obtained through right twisting, and a center unit and peripheral unit are obtained by left twisting. A wire rope is designed in the center unit to reduce the horizontal and vertical of the aluminum alloy conductor Force-bearing, combined with optimized insulation layer and sheath material formulation, improves torsion resistance and mildew resistance.

Benefits of technology

The resulting stranded aluminum alloy cable is not easy to break wire, has good torsion resistance, has a wide environmental temperature adaptation range, good flame retardant performance, and has significant salt spray and mildew resistance. It is suitable for wind power cables.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113871089B_ABST
    Figure CN113871089B_ABST
Patent Text Reader

Abstract

The present invention provides a multi-twisted aluminum alloy cable and its preparation method and application. The multi-twisted aluminum alloy cable includes a conductor, an insulating layer and a sheath in order from the inside to the outside in the radial direction; the conductor is obtained by left-twisting a central unit and 6 peripheral units, and the central unit is located at the center of the peripheral unit; the central unit is obtained by left-twisting a steel wire rope and 6 Class 5 aluminum alloy strands, and the steel wire rope is located at the center of the Class 5 aluminum alloy strands; the peripheral unit is obtained by left-twisting 7 Class 5 aluminum alloy strands; the Class 5 aluminum alloy strands are obtained by right-twisting 30 to 40 aluminum alloy monofilaments. The multi-twisted aluminum alloy cable provided by the present invention has good torsion resistance, flame retardant properties, salt spray resistance and mildew resistance, and is suitable for use as a cable for wind power generation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cables, and in particular relates to a multi-twisted aluminum alloy cable and a preparation method and application thereof. Background Art

[0002] With the development of society and economy and the enhancement of human environmental awareness, the world's energy structure is also undergoing tremendous changes. People's use of energy is gradually developing from non-renewable energy to renewable energy, and there is a trend of new energy such as solar energy and wind energy replacing traditional energy. Among them, wind energy, as a clean and renewable energy, is currently the largest, most technologically mature, and most commercially promising power generation model among many new energy sources. In recent years, it has received attention from many countries in the world. Since the development of offshore wind power does not occupy onshore land, and offshore wind energy resources are abundant and suitable for large-scale development, offshore wind power has become an inevitable trend in the future development of wind power.

[0003] Compared with onshore wind farms, the marine environment where offshore wind turbines are located is very complex and harsh, and they are subjected to a variety of random loads that vary with time and space, including wind, waves, currents, sea ice and tides, and are also threatened by earthquakes. Under such harsh environmental conditions, adverse factors such as environmental corrosion, marine biological attachment, foundation soil scouring and foundation dynamic softening, material aging, component defects and mechanical damage, fatigue and crack extension damage accumulation will lead to the attenuation of offshore wind turbine structural components and overall resistance, affecting the operational safety and durability of the wind turbine structure. As an important component for transmitting power in offshore wind turbine generator sets, offshore wind power cables are also affected by the harsh environment in which most wind turbines are located, seriously affecting the service life of the product. Therefore, offshore wind power cables have attracted widespread attention, and more and more technical means are used to prepare offshore wind power cables.

[0004] CN107033469A discloses a 5MW offshore wind turbine high current-carrying anti-torsion power cable, the cable comprises a copper conductor, an EPDM rubber insulation layer and a polyethylene rubber sheath layer, the EPDM rubber insulation layer is coated on the outer surface of the copper conductor, the polyethylene rubber sheath layer is coated on the outer surface of the EPDM rubber insulation layer, and the EPDM rubber insulation layer is prepared from the following components: EPDM Kep510, microcrystalline wax, paraffin oil 2280, antimony trioxide, titanium dioxide, white carbon black, zinc oxide, nano flame retardant reinforcing agent JP150, elastomer particles, adhesive, diisopropylbenzene peroxide DCP, trimethylolpropane trimethacrylate TMPTMA. The cable provided by this technical solution has a long service life, but it uses a copper conductor as a cable core, which makes the production cost of the cable high, which is not conducive to actual production and use, and when used at sea for a long time, it is easy to breed mold, affecting product performance and appearance.

[0005] CN110534244A discloses a low-voltage cable with a cold-resistant, corrosion-resistant, flame-retardant and water-resistant scandium aluminum alloy conductor for offshore wind power generation, the cable comprising a cable body, the cable body comprising a core and a protective layer arranged on the core, the protective layer comprising a water-blocking layer, an inner protective layer, a pressure-resistant layer and an outer sheath from the inside to the outside, the core is located on the surface of the inner protective layer and is provided with a rubber airbag at equal intervals along the length direction of the core, the outer surface of the rubber airbag is provided with a silicone tube at equal intervals, and the side wall of the pressure-resistant layer corresponds to the position where the rubber airbag is located. At least ten groups of air cavities are provided at equal intervals, each group of air cavities is composed of a plurality of strip air chambers, and each strip air chamber and the inner wall of the pressure-resistant layer are evenly provided with air ducts, each air duct is connected to the corresponding silicone tube, and the core comprises three power cores and one ground core. Although the cable prepared by this technical solution has good cold resistance and flame retardancy as well as good wear resistance and pressure resistance, its structure is relatively complex, and it is easy to breed mold when used at sea for a long time, affecting product performance and appearance.

[0006] CN205451902U discloses a cross-linked polyolefin cable for ultra-low temperature resistant and environmentally friendly wind power generation, the cable comprising: a cable core, a wrapping layer, and a sheath layer; the cable core comprises a plurality of conductors, each of which comprises a conductor, a semi-conductive layer, an insulating layer, and a shielding layer, the conductor is woven from a plurality of oxygen-free copper wires, the semi-conductive layer is coated on the outside of the conductor, the insulating layer is coated on the outside of the semi-conductive layer, the insulating layer is made of a cross-linked polyolefin insulating material, the shielding layer is coated on the outside of the insulating layer, the shielding layer is longitudinally wrapped with a copper tape, and a plurality of conductors are twisted to form a cable core; the wrapping layer is coated on the outside of the cable core, the sheath layer is coated on the outside of the wrapping layer, and the sheath layer is extruded with a polyolefin sheath material. The cable structure provided by the technical solution is complex, and copper wire is used as a conductor, which makes its production cost high. At the same time, when used at sea for a long time, it is easy to breed mold, affecting product performance and appearance.

[0007] As the price of copper continues to rise, replacing copper with aluminum is an inevitable trend in the development of wires and cables. However, in the prior art, when aluminum alloy monofilaments are used as cable cores, they are prone to wire breakage during cable torsion. Therefore, how to solve the problem of aluminum alloy monofilaments being prone to wire breakage during cable torsion and provide a cable with good salt spray resistance and mildew resistance so that it is suitable for use as a wind power cable has become a technical problem that people are eager to solve. Summary of the invention

[0008] In view of the deficiencies of the prior art, the purpose of the present invention is to provide a multi-twisted aluminum alloy cable and its preparation method and application. The present invention further adopts a right-hand twisting method to obtain 5 types of aluminum alloy strands through the design of the conductor structure of the multi-twisted aluminum alloy cable, and a left-hand twisting method to obtain a central unit and a peripheral unit. The left-hand twisting method is used to twist the central unit and the peripheral unit to obtain a multi-twisted aluminum alloy cable conductor. The two opposite twisting methods can effectively reduce the horizontal torsional stress of the aluminum alloy conductor; at the same time, the design of the steel wire rope in the central unit can reduce the vertical stress of the aluminum alloy conductor, thereby preparing a multi-twisted aluminum alloy cable with good torsional resistance.

[0009] To achieve this object, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides a multi-twisted aluminum alloy cable, which comprises a conductor, an insulating layer and a sheath in order from inside to outside in radial direction;

[0011] The conductor is obtained by left-twisting one central unit and six peripheral units, wherein the central unit is located at the center of the peripheral units;

[0012] The central unit is obtained by left-twisting one steel wire rope and six Class 5 aluminum alloy strands, wherein the steel wire rope is located at the center of the Class 5 aluminum alloy strands;

[0013] The peripheral unit is obtained by left-twisting 7 Class 5 aluminum alloy strands;

[0014] The five types of aluminum alloy strands are obtained by right-handedly twisting 30 to 40 aluminum alloy single wires.

[0015] In the present invention, by designing the conductor structure of the multiple-twisted aluminum alloy cable, a right-hand twisting method is further adopted to obtain 5 types of aluminum alloy strands, a left-hand twisting method is adopted to obtain a central unit and a peripheral unit, and the central unit and the peripheral unit are twisted together by the left-hand twisting method to obtain a multiple-twisted aluminum alloy cable conductor. The horizontal torsional stress of the aluminum alloy conductor can be effectively reduced by the two opposite twisting methods; at the same time, the vertical stress of the aluminum alloy conductor can be reduced by the design of the steel wire rope in the central unit, thereby preparing a multiple-twisted aluminum alloy cable with good torsional resistance.

[0016] In the present invention, the 5 types of aluminum alloy strands are obtained by right-handedly twisting 30 to 40 aluminum alloy monofilaments, for example, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39 or 40 strands.

[0017] It should be noted that in the present invention, the conductors, the central unit and the peripheral unit are twisted using a 1+6 twist structure.

[0018] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the objectives and beneficial effects of the present invention can be better achieved and realized.

[0019] As a preferred technical solution of the present invention, the diameter of the aluminum alloy monofilament is 0.30-0.51 mm, for example, it can be 0.30 mm, 0.32 mm, 0.34 mm, 0.38 mm, 0.40 mm, 0.42 mm, 0.44 mm, 0.46 mm, 0.48 mm or 0.51 mm.

[0020] Preferably, the mass percentage of silicon element in the aluminum alloy monofilament is 0.03-0.15% (for example, it can be 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14% or 0.15%, etc.), the mass percentage of iron element is 0.40-1.00% (for example, it can be 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1.00%, etc.), and the mass percentage of zinc element is ≤0.10% (for example, it can be 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09% or 0.10%).

[0021] Preferably, the pitch diameter ratio of the 5 types of aluminum alloy strands is 16 to 18 times, for example, it can be 16 times, 16.2 times, 16.5 times, 16.7 times, 17 times, 17.3 times, 17.5 times, 17.8 times or 18 times.

[0022] Preferably, the diameter of the steel wire rope is 3.0-4.0 mm, for example, it can be 3.0 mm, 3.1 mm, 3.2 mm, 3.3 mm, 3.4 mm, 3.5 mm, 3.6 mm, 3.7 mm, 3.8 mm, 3.3 mm or 4.0 mm.

[0023] Preferably, the pitch-to-diameter ratio of the central unit is 14 to 16 times, for example, it may be 14 times, 14.2 times, 14.5 times, 14.7 times, 15 times, 15.3 times, 15.5 times, 15.8 times or 16 times.

[0024] Preferably, the pitch diameter ratio of the peripheral unit is 14 to 16 times, for example, it can be 14 times, 14.2 times, 14.5 times, 14.7 times, 15 times, 15.3 times, 15.5 times, 15.8 times or 16 times.

[0025] Preferably, the pitch diameter ratio of the conductor is 12 to 14 times, for example, it may be 12 times, 12.2 times, 12.5 times, 12.7 times, 13 times, 13.3 times, 13.5 times, 13.8 times or 14 times.

[0026] As a preferred technical solution of the present invention, the thickness of the insulating layer is 2.0-3.0 mm, for example, it can be 2.0 mm, 2.1 mm, 2.2 mm, 2.3 mm, 2.4 mm, 2.5 mm, 2.6 mm, 2.7 mm, 2.8 mm, 2.3 mm or 3.0 mm.

[0027] Preferably, the thickness of the sheath is 2.0-4.0 mm, for example, it may be 2.0 mm, 2.2 mm, 2.4 mm, 2.6 mm, 2.8 mm, 3.0 mm, 3.2 mm, 3.4 mm, 3.6 mm, 3.8 mm or 4.0 mm.

[0028] As a preferred technical solution of the present invention, the insulating layer is prepared from an insulating layer material;

[0029] The insulating layer material includes the following raw material components in parts by weight:

[0030] 45-55 parts of EPDM rubber, 20-30 parts of talc, 20-30 parts of modified calcined kaolin, 3-7 parts of white carbon black, 3-7 parts of rubber paraffin oil, 2-4 parts of nano zinc oxide, 2-4 parts of microcrystalline wax, 2-4 parts of titanium dioxide, 1-3 parts of vulcanizing agent, 0.7-1 parts of antioxidant RD and 0.8-1.2 parts of antioxidant MB.

[0031] In the present invention, by designing the raw material components of the insulating layer material and further by the synergistic effect of the antioxidant RD and the antioxidant MB, the prepared multi-twisted aluminum alloy cable has good anti-aging property.

[0032] In the present invention, the weight proportions of the EPDM rubber may be 45 parts, 46 parts, 47 parts, 48 ​​parts, 49 parts, 50 parts, 51 parts, 52 parts, 53 parts, 54 parts or 55 parts.

[0033] The weight proportions of the talc powder may be 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts or 30 parts, etc.

[0034] The weight proportions of the modified calcined kaolin may be 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts or 30 parts, etc.

[0035] The weight proportions of the white carbon black may be 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, 5.5 parts, 6 parts, 6.5 parts or 7 parts, etc.

[0036] The weight proportions of the rubber paraffin oil may be 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, 5.5 parts, 6 parts, 6.5 parts or 7 parts, etc.

[0037] The weight proportions of the nano zinc oxide can be 2 parts, 2.2 parts, 2.5 parts, 2.7 parts, 3 parts, 3.3 parts, 3.5 parts, 3.8 parts or 4 parts.

[0038] The weight proportions of the microcrystalline wax may be 2 parts, 2.2 parts, 2.5 parts, 2.7 parts, 3 parts, 3.3 parts, 3.5 parts, 3.8 parts or 4 parts, etc.

[0039] The weight proportions of the titanium dioxide can be 2 parts, 2.2 parts, 2.5 parts, 2.7 parts, 3 parts, 3.3 parts, 3.5 parts, 3.8 parts or 4 parts, etc.

[0040] The weight proportions of the vulcanizing agent may be 1 part, 1.2 parts, 1.5 parts, 1.7 parts, 2 parts, 2.3 parts, 2.5 parts, 2.8 parts or 3 parts, etc.

[0041] The weight proportion of the antioxidant RD can be 0.7 parts, 0.75 parts, 0.8 parts, 0.85 parts, 0.9 parts, 0.95 parts or 1 parts, etc.

[0042] The weight proportion of the antioxidant MB can be 0.8 parts, 0.85 parts, 0.9 parts, 0.95 parts, 1 parts, 10.5 parts, 1.1 parts, 1.15 parts or 1.2 parts, etc.

[0043] As a preferred technical solution of the present invention, the vulcanizing agent is selected from dicumyl peroxide and / or vulcanizing agent BIBP.

[0044] Preferably, the raw material components of the insulating layer material also include 0.8 to 1.5 parts of a vulcanizing agent, for example, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4 or 1.5 parts.

[0045] Preferably, the co-vulcanizing agent is selected from any one of triallyl isocyanurate, trimethylolpropane trimethacrylate or crosslinking agent TAC, or a combination of at least two thereof.

[0046] Preferably, the raw material components of the insulating layer material further include 0.4 to 0.7 parts of stearic acid, for example, 0.4 parts, 0.45 parts, 0.5 parts, 0.55 parts, 0.6 parts, 0.65 parts or 0.7 parts.

[0047] Preferably, the raw material components of the insulating layer material also include 0.3 to 0.8 parts of a coupling agent, for example, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75 or 0.8 parts.

[0048] Preferably, the coupling agent is selected from vinyltri(β-methoxyethoxy)silane and / or vinyltrimethoxysilane.

[0049] The present invention does not impose any particular limitation on the method for preparing the insulating layer material, which may exemplarily include the following steps:

[0050] (1) mixing EPDM rubber in an internal mixer at 105-115° C. for 1-2 minutes to obtain mixed EPDM rubber;

[0051] (2) mixing the mixed EPDM rubber obtained in step (1) with talcum powder, modified calcined kaolin, white carbon black, nano zinc oxide, microcrystalline wax, titanium dioxide, rubber paraffin oil, antioxidant RD, antioxidant MB, and optionally stearic acid and coupling agent at 105-115° C. for 4-5 minutes to obtain a mixture;

[0052] (3) kneading the mixture obtained in step (2) with a vulcanizing agent and an optional co-vulcanizing agent at 105 to 115° C. for 0.5 to 1 min to obtain a mixed rubber material;

[0053] (4) The mixed rubber material obtained in step (3) is thinned on a 660 open mill for 1 to 2 times and swung for 4 to 6 times, then input into a rubber filter, filtered through a 40+60+40 mesh rubber filter, turned over 2 to 3 times on a 550 open mill, and rolled, and finally slit into sheets on a three-roll calender. The output rubber sheet is cooled by a cooling roller and passed through a talcum powder box to obtain the insulating layer material.

[0054] As a preferred technical solution of the present invention, the sheath is prepared from a sheath material;

[0055] The sheath material comprises the following raw material components in parts by weight:

[0056] 45-55 parts of chlorinated polyethylene, 8-12 parts of POE, 15-25 parts of modified kaolin, 8-12 parts of white carbon black, 2-3 parts of carbon black, 5-10 parts of light magnesium oxide, 3-5 parts of calcium zinc stabilizer, 7-10 parts of flame retardant, 4-6 parts of mildewproof agent, 1-3 parts of red lead, 3-5 parts of chlorinated paraffin, 5-7 parts of cold-resistant plasticizer, 5-7 parts of trichloroethyl phosphate and 1-3 parts of vulcanizing agent.

[0057] In the present invention, by using a mildew-proof agent and controlling the weight percentage of the mildew-proof agent within a specific range, the prepared sheath material has good mildew resistance. If the weight percentage of the mildew-proof agent is too small, the mildew resistance effect of the prepared sheath material is poor; if the weight percentage of the mildew-proof agent is too large, the mechanical properties of the prepared sheath material are poor.

[0058] In the present invention, trichloroethyl phosphate is used as a flame retardant plasticizer and its weight fraction is controlled within a specific range, so that the prepared sheath material has good flame retardancy and excellent mechanical properties. If the weight fraction of trichloroethyl phosphate is too large, the flame retardancy of the prepared sheath material is poor; if the weight fraction of trichloroethyl phosphate is too small, the mechanical properties of the prepared sheath material are poor.

[0059] It should be noted that POE in the present invention is a polyethylene-octene co-elastomer.

[0060] In the present invention, the weight proportions of the chlorinated polyethylene can be 45 parts, 46 parts, 47 parts, 48 ​​parts, 49 parts, 50 parts, 51 parts, 52 parts, 53 parts, 54 parts or 55 parts.

[0061] The weight proportions of the POE may be 8 parts, 8.5 parts, 9 parts, 9.5 parts, 10 parts, 10.5 parts, 11 parts, 11.5 parts or 12 parts, etc.

[0062] The weight proportions of the modified kaolin may be 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts or 25 parts, etc.

[0063] The weight proportions of the white carbon black may be 8 parts, 8.5 parts, 9 parts, 9.5 parts, 10 parts, 10.5 parts, 11 parts, 11.5 parts or 12 parts, etc.

[0064] The weight proportions of the carbon black may be 2 parts, 2.1 parts, 2.2 parts, 2.3 parts, 2.4 parts, 2.5 parts, 2.6 parts, 2.7 parts, 2.8 parts, 2.9 parts or 3 parts, etc.

[0065] The weight proportions of the light magnesium oxide may be 5 parts, 6 parts, 7 parts, 8 parts, 9 parts or 10 parts, etc.

[0066] The weight proportions of the calcium zinc stabilizer can be 3 parts, 3.3 parts, 3.6 parts, 3.9 parts, 4.2 parts, 4.4 parts, 4.6 parts, 4.8 parts or 5 parts, etc.

[0067] The weight proportions of the flame retardant may be 7 parts, 7.5 parts, 8 parts, 8.5 parts, 9 parts, 9.5 parts or 10 parts, etc.

[0068] The weight proportions of the mildew inhibitor may be 4 parts, 4.2 parts, 4.4 parts, 4.6 parts, 4.8 parts, 5 parts, 5.2 parts, 5.4 parts, 5.6 parts, 5.8 parts or 6 parts, etc.

[0069] The weight proportions of the red lead may be 1 part, 1.2 parts, 1.4 parts, 1.6 parts, 1.8 parts, 2 parts, 2.2 parts, 2.4 parts, 2.6 parts, 2.8 parts or 3 parts, etc.

[0070] The weight proportions of the chlorinated paraffin can be 3 parts, 3.2 parts, 3.4 parts, 3.6 parts, 3.8 parts, 4 parts, 4.2 parts, 4.4 parts, 4.6 parts, 4.8 parts or 5 parts, etc.

[0071] The weight proportions of the cold-resistant plasticizer may be 5 parts, 5.2 parts, 5.4 parts, 5.6 parts, 5.8 parts, 6 parts, 6.2 parts, 6.4 parts, 6.6 parts, 6.8 parts or 7 parts, etc.

[0072] The weight proportions of the trichloroethyl phosphate can be 5 parts, 5.2 parts, 5.4 parts, 5.6 parts, 5.8 parts, 6 parts, 6.2 parts, 6.4 parts, 6.6 parts, 6.8 parts or 7 parts, etc.

[0073] The weight proportions of the vulcanizing agent may be 1 part, 1.2 parts, 1.4 parts, 1.6 parts, 1.8 parts, 2 parts, 2.2 parts, 2.4 parts, 2.6 parts, 2.8 parts or 3 parts, etc.

[0074] As a preferred technical solution of the present invention, the flame retardant is a silicate flame retardant.

[0075] Preferably, the mildew preventer is dichlorophenol (2.2′-dihydroxy-5.5′-dichlorodiphenylmethane).

[0076] Preferably, the cold-resistant plasticizer is plasticizer DOS.

[0077] Preferably, the vulcanizing agent is selected from dicumyl peroxide and / or vulcanizing agent BIBP.

[0078] Preferably, the raw material components of the sheath material further include 0.8 to 1.2 parts of a vulcanizing agent, for example, 0.8 parts, 0.9 parts, 1.0 parts, 1.1 parts or 1.2 parts.

[0079] Preferably, the co-vulcanizing agent is selected from any one of triallyl isocyanurate, trimethylolpropane trimethacrylate or crosslinking agent TAC, or a combination of at least two thereof.

[0080] Preferably, the raw material components of the sheath material also include 0.3 to 0.7 parts of an antioxidant, for example, 0.3 parts, 0.35 parts, 0.4 parts, 0.45 parts, 0.5 parts, 0.55 parts, 0.6 parts, 0.65 parts or 0.7 parts.

[0081] Preferably, the antioxidant is selected from antioxidant RD and / or antioxidant MB.

[0082] Preferably, the raw material components of the sheath material also include 0.3 to 0.7 parts of a coupling agent, for example, 0.3 parts, 0.35 parts, 0.4 parts, 0.45 parts, 0.5 parts, 0.55 parts, 0.6 parts, 0.65 parts or 0.7 parts.

[0083] Preferably, the coupling agent is selected from γ-aminopropyltriethoxysilane.

[0084] The present invention does not impose any particular limitation on the method for preparing the sheath material, and an exemplary method may include the following steps:

[0085] (A) mixing chlorinated polyethylene and POE in an internal mixer at 105-115° C. for 1-2 minutes to obtain a mixture A;

[0086] (B) mixing the mixture A obtained in step (A) with modified kaolin, white carbon, carbon black, light magnesium oxide, calcium zinc stabilizer, flame retardant, mildew inhibitor, red lead, chlorinated paraffin, cold-resistant plasticizer, flame retardant plasticizer and optional antioxidant and coupling agent at 105-115° C. for 4-5 minutes to obtain a mixture B;

[0087] (C) mixing the mixture B obtained in step (B) with a vulcanizing agent and an optional co-vulcanizing agent at 105 to 115° C. for 0.5 to 1 min to obtain a mixed rubber material;

[0088] (D) The mixed rubber material obtained in step (C) is thinned on a 660 open mixing mill for 1 to 2 times and swung for 4 to 6 times, then inputted into a 550 open mixing mill and turned over for 2 to 3 times, and then cut into sheets on a three-roll calender. The output rubber sheets are cooled by cooling rollers and passed through a talcum powder box to obtain the sheath material.

[0089] In a second aspect, the present invention provides a method for preparing a multi-twisted aluminum alloy cable as described in the first aspect, the preparation method comprising the following steps:

[0090] After the insulating layer is extruded on the outer surface of the conductor, a sheath is extruded on the outer surface of the insulating layer to obtain the multi-twisted aluminum alloy cable.

[0091] As a preferred technical solution of the present invention, the extrusion method is extrusion molding through an extruder.

[0092] It should be noted that the basic method of extruding the insulating layer on the outer surface of the conductor and the basic method of extruding the sheath on the outer surface of the insulating layer in the present invention is extrusion molding through an extruder.

[0093] Preferably, the temperature of the extruder feeding port is 45-55°C, for example, it can be 45°C, 46°C, 47°C, 48°C, 49°C, 50°C, 51°C, 52°C, 53°C, 54°C or 55°C.

[0094] Preferably, the operating temperature of the extruder head is 75-85°C, for example, it can be 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C or 85°C.

[0095] Preferably, the extruder body comprises a first zone and a second zone connected.

[0096] Preferably, the operating temperature of the first zone is 65-75°C (for example, it may be 65°C, 66°C, 67°C, 68°C, 69°C, 70°C, 71°C, 72°C, 73°C, 74°C or 75°C, etc.), and the operating temperature of the second zone is 75-85°C (for example, it may be 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C or 85°C, etc.).

[0097] In a third aspect, the present invention provides an application of the multi-twisted aluminum alloy cable as described in the first aspect in wind power generation.

[0098] Compared with the prior art, the present invention has the following beneficial effects:

[0099] (1) The present invention further adopts a right-hand twisting method to obtain 5 types of aluminum alloy strands through the design of the conductor structure of the multi-twisted aluminum alloy cable, and a left-hand twisting method to obtain a central unit and a peripheral unit. The central unit and the peripheral unit are twisted together by the left-hand twisting method to obtain a multi-twisted aluminum alloy cable conductor. The two opposite twisting methods can effectively reduce the horizontal torsional stress of the aluminum alloy conductor; at the same time, the vertical stress of the aluminum alloy conductor can be reduced through the design of the steel wire rope in the central unit, thereby preparing a multi-twisted aluminum alloy cable that is not easy to break and is soft. After the normal temperature torsional property test and the low temperature torsional property test, the aluminum alloy single wires in the conductor have no broken wire phenomenon;

[0100] (2) The present invention designs the insulating layer material and the sheath material to prepare a twisted aluminum alloy cable with a minimum environmental adaptability temperature of -40°C and a maximum operating temperature of 90°C. The cable has good flame retardant properties and can pass a single vertical combustion test. It also has good salt spray resistance and can pass a salt spray test. It also has good mildew resistance, and its mildew resistance effect can reach level 0. BRIEF DESCRIPTION OF THE DRAWINGS

[0101] Figure 1 It is a schematic structural diagram of a multi-twisted aluminum alloy cable provided in an embodiment of the present invention;

[0102] Among them, 1-central unit, 11-steel wire rope, 12-5 type aluminum alloy strand, 2-peripheral unit, 3-insulating layer, 4-sheath. DETAILED DESCRIPTION

[0103] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0104] It should be noted that all raw material components in the following examples and comparative examples are commercially available products, and the sources of some components are as follows:

[0105] Aluminum alloy monofilament: Jiangsu Guojia Conductor Technology Co., Ltd.;

[0106] Wire rope: Jiangyin Jiahua Rope Co., Ltd.;

[0107] EPDM rubber: KEP210, Kumho Corporation of Korea;

[0108] Talc: 1250 mesh, Shenzhen Lianhexin Technology Co., Ltd.;

[0109] Chlorinated polyethylene: CM135B, Shandong Riko Rubber & Plastic Technology Co., Ltd.;

[0110] POE: DF640, Mitsui Group;

[0111] Chlorinated paraffin: 52#, Shanghai Houhuang Chemical Trading Co., Ltd.;

[0112] Silicate flame retardant: GZRY, Hangzhou Longshang Chemical Co., Ltd.

[0113] Example 1

[0114] This embodiment provides a multi-twisted aluminum alloy cable, and its structural schematic diagram is as follows Figure 1 As shown, the multi-twisted aluminum alloy cable includes a conductor, an insulating layer and a sheath in sequence from the inside to the outside in the radial direction;

[0115] The conductor is obtained by left-twisting one central unit and six peripheral units, wherein the central unit is located at the center of the peripheral units;

[0116] The central unit is obtained by left-twisting one steel wire rope and six Class 5 aluminum alloy strands, wherein the steel wire rope is located at the center of the Class 5 aluminum alloy strands;

[0117] The peripheral unit is obtained by left-twisting 7 Class 5 aluminum alloy strands;

[0118] The five types of aluminum alloy strands are obtained by right-handedly twisting 35 aluminum alloy single wires;

[0119] The diameter of the aluminum alloy monofilament is 0.40 mm, and the diameter of the steel wire rope is 2.5 mm;

[0120] The pitch-diameter ratio of the five types of aluminum alloy strands is 16 times, the pitch-diameter ratio of the central unit is 15 times, the pitch-diameter ratio of the peripheral unit is 15 times, and the pitch-diameter ratio of the conductor is 12 times;

[0121] The thickness of the insulating layer is 2.5 mm, and the thickness of the sheath is 3.0 mm;

[0122] Wherein, the insulating layer is prepared from an insulating layer material, and the insulating layer material includes the following raw material components in parts by weight:

[0123] 50 parts of EPDM rubber, 25 parts of talc, 25 parts of modified calcined kaolin, 5 parts of white carbon black, 5 parts of rubber paraffin oil, 3 parts of nano zinc oxide, 3 parts of microcrystalline wax, 3 parts of titanium dioxide, 2 parts of dicumyl peroxide, 0.8 parts of antioxidant RD, 1 part of antioxidant MB, 1.2 parts of triallyl isocyanurate, 0.5 parts of stearic acid and 0.4 parts of vinyl tris(β-methoxyethoxy)silane;

[0124] The preparation method of the above insulating layer material is as follows:

[0125] (1) mixing ethylene propylene diene monomer rubber in an internal mixer at 110° C. for 1.5 minutes to obtain mixed ethylene propylene diene monomer rubber;

[0126] (2) mixing the mixed EPDM rubber obtained in step (1) with talcum powder, modified calcined kaolin, white carbon black, nano zinc oxide, microcrystalline wax, titanium dioxide, rubber paraffin oil, antioxidant RD, antioxidant MB, stearic acid and vinyl tri(β-methoxyethoxy)silane at 110° C. for 5 min to obtain a mixture;

[0127] (3) mixing the mixture obtained in step (2), dicumyl peroxide and triallyl isocyanurate at 110° C. for 1 min to obtain a mixed rubber material;

[0128] (4) The mixed rubber material obtained in step (3) is thinned twice on a 660 open mill and swung six times, then input into a rubber filter, filtered through a 40+60+40 mesh rubber filter, turned over three times on a 550 open mill and rolled, and finally slit into sheets on a three-roll calender. The output rubber sheet is cooled by a cooling roller and passed through a talcum powder box to obtain the insulating layer material.

[0129] The sheath is prepared from a sheath material, and the sheath material includes the following raw material components in parts by weight:

[0130] 50 parts of chlorinated polyethylene, 10 parts of POE, 20 parts of modified kaolin, 10 parts of white carbon black, 2.5 parts of carbon black, 7 parts of light magnesium oxide, 4 parts of calcium zinc stabilizer, 8.5 parts of silicate flame retardant, 5 parts of dichlorophenol (2.2'-dihydroxy-5.5'-dichlorodiphenylmethane), 2 parts of red lead, 4 parts of chlorinated paraffin, 5.5 parts of plasticizer DOS, 5.5 parts of trichloroethyl phosphate, 2 parts of diisopropyl peroxide, 1 part of triallyl isocyanurate, 0.5 parts of antioxidant RD and 0.5 parts of γ-aminopropyltriethoxysilane.

[0131] The preparation method of the above-mentioned multi-twisted aluminum alloy cable is as follows:

[0132] (A) mixing chlorinated polyethylene and POE in an internal mixer at 112° C. for 2 minutes to obtain a mixture A;

[0133] (B) mixing the mixture A obtained in step (A) with modified kaolin, white carbon, carbon black, light magnesium oxide, calcium zinc stabilizer, silicate flame retardant, dichlorophenol (2.2′-dihydroxy-5.5′-dichlorodiphenylmethane), red lead, chlorinated paraffin, plasticizer DOS, trichloroethyl phosphate, antioxidant RD and γ-aminopropyltriethoxysilane at 112° C. for 4 min to obtain a mixture B;

[0134] (C) mixing the mixture B obtained in step (B) with dicumyl peroxide and triallyl isocyanurate at 112° C. for 1 min to obtain a mixed rubber material;

[0135] (D) The mixed rubber material obtained in step (C) is thinned twice on a 660 open mixing mill and swung four times, then input into a 550 open mixing mill and turned twice, and then cut into sheets on a three-roll calender. The output rubber sheet is cooled by a cooling roller and passed through a talcum powder box to obtain the sheath material.

[0136] The preparation method of the above-mentioned multi-twisted aluminum alloy cable is as follows:

[0137] Using an extruder, after extruding an insulating layer on the outer surface of the conductor, a sheath is extruded on the outer surface of the insulating layer to obtain the multi-twisted aluminum alloy cable;

[0138] When the insulating layer is extruded, the temperature of the feed port of the extruder is 50°C, the working temperature of the die head is 80°C, the extruder body includes a first zone and a second zone connected, the working temperature of the first zone is 70°C, and the working temperature of the second zone is 80°C;

[0139] When extruding the sheath, the temperature of the extruder feed port is 55°C, the working temperature of the die head is 85°C, and the extruder body includes a first zone and a second zone connected in sequence. The working temperature of the first zone is 75°C, and the working temperature of the second zone is 85°C.

[0140] Example 2

[0141] This embodiment provides a multi-twisted aluminum alloy cable, which is different from Embodiment 1 in that:

[0142] The five types of aluminum alloy strands are obtained by twisting 30 aluminum alloy single wires in a left-hand direction.

[0143] The diameter of the aluminum alloy monofilament is 0.51 mm, and the diameter of the steel wire rope is 3.0 mm;

[0144] The pitch diameter ratio of the five types of aluminum alloy strands is 18 times, the pitch diameter ratio of the central unit is 14 times, the pitch diameter ratio of the peripheral unit is 14 times, and the pitch diameter ratio of the conductor is 14 times;

[0145] The thickness of the insulating layer is 2.0 mm, and the thickness of the sheath is 2.0 mm;

[0146] The insulating layer material includes the following raw material components in parts by weight:

[0147] 45 parts of EPDM rubber, 20 parts of talc, 20 parts of modified calcined kaolin, 3 parts of white carbon black, 3 parts of rubber paraffin oil, 4 parts of nano zinc oxide, 4 parts of microcrystalline wax, 4 parts of titanium dioxide, 3 parts of vulcanizing agent BIBP, 0.7 parts of antioxidant RD, 0.8 parts of antioxidant MB, 1.5 parts of triallyl isocyanurate, 0.7 parts of stearic acid and 0.8 parts of vinyl tris(β-methoxyethoxy)silane;

[0148] The sheath material comprises the following raw material components in parts by weight:

[0149] 55 parts of chlorinated polyethylene, 12 parts of POE, 25 parts of modified kaolin, 12 parts of white carbon black, 3 parts of carbon black, 10 parts of light magnesium oxide, 3 parts of calcium zinc stabilizer, 7 parts of silicate flame retardant, 4 parts of dichlorophenol (2.2′-dihydroxy-5.5′-dichlorodiphenylmethane), 3 parts of red lead, 3 parts of chlorinated paraffin, 7 parts of plasticizer DOS, 5 parts of trichloroethyl phosphate, 3 parts of vulcanizing agent BIBP, 1.2 parts of triallyl isocyanurate, 0.7 parts of antioxidant RD and 0.3 parts of γ-aminopropyltriethoxysilane;

[0150] Other conditions are the same as in Example 1.

[0151] Example 3

[0152] This embodiment provides a multi-twisted aluminum alloy cable, which is different from Embodiment 1 in that:

[0153] The five types of aluminum alloy strands are obtained by twisting 40 aluminum alloy single wires in a left-hand direction;

[0154] The diameter of the aluminum alloy monofilament is 0.30 mm, and the diameter of the steel wire rope is 4.0 mm;

[0155] The pitch diameter ratio of the five types of aluminum alloy strands is 17 times, the pitch diameter ratio of the central unit is 16 times, the pitch diameter ratio of the peripheral unit is 16 times, and the pitch diameter ratio of the conductor is 13 times;

[0156] The thickness of the insulating layer is 3.0 mm, and the thickness of the sheath is 4.0 mm;

[0157] The insulating layer material includes the following raw material components in parts by weight:

[0158] 55 parts of EPDM rubber, 30 parts of talc, 30 parts of modified calcined kaolin, 7 parts of white carbon black, 7 parts of rubber paraffin oil, 2 parts of nano zinc oxide, 2 parts of microcrystalline wax, 2 parts of titanium dioxide, 1 part of dicumyl peroxide, 1 part of antioxidant RD, 1.2 parts of antioxidant MB, 0.8 parts of triallyl isocyanurate, 0.4 parts of stearic acid and 0.3 parts of vinyl tris(β-methoxyethoxy)silane;

[0159] The sheath material comprises the following raw material components in parts by weight:

[0160] 45 parts of chlorinated polyethylene, 8 parts of POE, 15 parts of modified kaolin, 8 parts of white carbon black, 2 parts of carbon black, 5 parts of light magnesium oxide, 5 parts of calcium zinc stabilizer, 10 parts of silicate flame retardant, 6 parts of dichlorophenol (2.2′-dihydroxy-5.5′-dichlorodiphenylmethane), 1 part of red lead, 5 parts of chlorinated paraffin, 5 parts of plasticizer DOS, 7 parts of trichloroethyl phosphate, 1 part of diisopropyl peroxide, 0.8 parts of triallyl isocyanurate, 0.3 parts of antioxidant MB and 0.7 parts of γ-aminopropyltriethoxysilane;

[0161] Other conditions are the same as in Example 1.

[0162] Example 4

[0163] This embodiment provides a twisted aluminum alloy cable, which is different from Embodiment 1 in that the raw material components of the insulating layer material do not contain antioxidant MB, the weight portion of antioxidant RD is 1.8 parts, and other conditions are the same as those of Embodiment 1.

[0164] Example 5

[0165] This embodiment provides a twisted aluminum alloy cable, which is different from Embodiment 1 in that the raw material components of the insulating layer material do not contain antioxidant RD, the weight portion of antioxidant MB is 1.8 parts, and other conditions are the same as Embodiment 1.

[0166] Example 6

[0167] This embodiment provides a twisted aluminum alloy cable. The difference from Embodiment 1 is that the weight proportion of dichlorophenol (2.2′-dihydroxy-5.5′-dichlorodiphenylmethane) in the raw material components of the sheath material is 4 parts, and other conditions are the same as those in Embodiment 1.

[0168] Example 7

[0169] This embodiment provides a double-twisted aluminum alloy cable, which is different from Example 1 in that the weight proportion of dichlorophenol (2.2′-dihydroxy-5.5′-dichlorodiphenylmethane) in the raw material components of the sheath material is 6 parts, and other conditions are the same as Example 1.

[0170] Example 8

[0171] This embodiment provides a twisted aluminum alloy cable. The difference from Embodiment 1 is that the weight proportion of dichlorophenol (2.2′-dihydroxy-5.5′-dichlorodiphenylmethane) in the raw material components of the sheath material is 3 parts, and other conditions are the same as those in Embodiment 1.

[0172] Example 9

[0173] This embodiment provides a twisted aluminum alloy cable. The difference from Embodiment 1 is that the weight proportion of dichlorophenol (2.2′-dihydroxy-5.5′-dichlorodiphenylmethane) in the raw material components of the sheath material is 8 parts, and other conditions are the same as those in Embodiment 1.

[0174] Example 10

[0175] This embodiment provides a twisted aluminum alloy cable. The difference from Embodiment 1 is that the weight proportion of trichloroethyl phosphate in the raw material components of the sheath material is 5 parts, and other conditions are the same as those in Embodiment 1.

[0176] Embodiment 11

[0177] This embodiment provides a twisted aluminum alloy cable. The difference from Embodiment 1 is that the weight proportion of trichloroethyl phosphate in the raw material components of the sheath material is 7 parts, and other conditions are the same as those in Embodiment 1.

[0178] Example 12

[0179] This embodiment provides a double-twisted aluminum alloy cable. The difference from Embodiment 1 is that the weight proportion of trichloroethyl phosphate in the raw material components of the sheath material is 3 parts, and other conditions are the same as those in Embodiment 1.

[0180] Embodiment 13

[0181] This embodiment provides a double-twisted aluminum alloy cable. The difference from Embodiment 1 is that the weight proportion of trichloroethyl phosphate in the raw material components of the sheath material is 9 parts, and other conditions are the same as those in Embodiment 1.

[0182] Embodiment 14

[0183] This embodiment provides a twisted aluminum alloy cable. The difference from Embodiment 1 is that trichloroethyl phosphate in the raw material components of the sheath material is replaced by trioctyl trimellitate, and other conditions are the same as those in Embodiment 1.

[0184] Comparative Example 1

[0185] This comparative example provides an aluminum alloy cable, which is different from Example 1 in that the Category 5 aluminum alloy strands are obtained by left-handedly twisting 35 aluminum alloy monofilaments, and other conditions are the same as those in Example 1.

[0186] Comparative Example 2

[0187] This comparative example provides an aluminum alloy cable, which is different from Example 1 only in that the central unit and the peripheral unit are both obtained by left-twisting 7 Class 5 aluminum alloy strands; other conditions are the same as Example 1.

[0188] The performance of the aluminum alloy cables provided in the above embodiments and comparative examples was tested, and the testing method is as follows:

[0189] Flame retardancy: GB / T 18380-2008;

[0190] Mechanical properties: GB / T 29631-2013;

[0191] Anti-aging performance: GB / T 29631-2013;

[0192] Torsion resistance at room temperature: At 25°C, a torsion test was carried out in accordance with GB / T 29631-2013 standard, with a torsion angle of 120° / m and a test cycle of 10,000 times. The surface of the aluminum alloy cable was observed for cracks and distortion after the torsion resistance test at room temperature, and the aluminum alloy monofilament in the conductor was observed for broken wires. At the same time, a breakdown test was carried out under the condition of 6.5kV / 5min. If there were no cracks or distortion on the surface of the aluminum alloy cable, and no broken wires in the aluminum alloy monofilament in the conductor, and the cable withstands the voltage without breakdown after torsion, it is considered qualified.

[0193] Low temperature torsion resistance: at -40℃, according to GB / T 29631-2013 standard, a torsion test is carried out, where the torsion angle is 120° / m and the test cycle is 2000 times. The surface of the aluminum alloy cable after the normal temperature torsion resistance test is observed for cracks and distortion, and the aluminum alloy monofilament in the conductor is observed for broken wires. At the same time, a breakdown test is carried out under the condition of 6.5kV / 5min. If there are no cracks or distortion on the surface of the aluminum alloy cable, and no broken wires in the aluminum alloy monofilament in the conductor, and the withstand voltage does not break down after torsion, it is considered qualified.

[0194] Salt spray resistance: The salt spray resistance test is carried out in accordance with GB / T 2423.17-2008 standard, where the test time is 336h. If the change rate of tensile strength and elongation at break of the insulation layer and sheath before and after the salt spray test does not exceed ±30%, it is considered qualified;

[0195] Mildew resistance: GJB 150.10A.

[0196] The test results of the aluminum alloy cable performance provided by the above embodiments and comparative examples are shown in Table 1 below:

[0197] Table 1

[0198]

[0199]

[0200] As can be seen from Table 1, the present invention designs the single structure of the multi-twisted aluminum alloy cable and designs the steel wire rope in the central unit, so that after the normal temperature torsional resistance test and the low temperature torsional resistance test, the aluminum alloy monofilaments in the conductor have no broken wire phenomenon; at the same time, the present invention designs the insulating layer material and the sheath material to prepare the multi-twisted aluminum alloy cable, which has good flame retardant properties and can pass the single vertical burning test, and has good salt spray resistance and can pass the salt spray test, and has good mildew resistance, and its mildew resistance effect can reach level 0.

[0201] Compared with Example 1, if only antioxidant RD (Example 4) or only antioxidant MB (Example 5) is selected as the antioxidant in the raw material components of the insulating layer material, the anti-aging effect of the prepared multi-twisted aluminum alloy cable is poor. It can be seen that in the present invention, a multi-twisted aluminum alloy cable with good anti-aging performance can be prepared through the synergistic effect of antioxidant RD and antioxidant MB.

[0202] Compared with Example 1, if the content of mildew inhibitor in the raw material components of the sheath material is too little (Example 8), the mildew resistance of the prepared multi-twisted aluminum alloy cable is poor; if the content of mildew inhibitor in the raw material components of the sheath material is too much (Example 9), the mechanical properties and anti-aging properties of the prepared multi-twisted aluminum alloy cable are poor, and the cost is high, which is not conducive to actual production.

[0203] Compared with Example 1, if the content of trichloroethyl phosphate in the raw material components of the sheath material is too little (Example 12), the mechanical properties of the prepared sheath are poor; if the content of trichloroethyl phosphate in the raw material components of the sheath material is too much (Example 13), the flame retardancy of the prepared sheath is poor, and it cannot pass the single vertical flame retardant test, and its mechanical properties and mildew resistance are poor; if the flame retardant plasticizer trichloroethyl phosphate in the raw material components of the sheath material is replaced with other plasticizers (Example 14), the flame retardant properties of the prepared twisted aluminum alloy cable are poor.

[0204] Compared with Example 1, if the twisting direction of the 5 types of aluminum alloy strands is the same as the twisting direction of the central unit and the peripheral unit (Comparative Example 1), the torsional properties of the prepared multi-twisted aluminum alloy cable are poor and cannot pass the normal temperature torsional properties test and the low temperature torsional properties test; if no steel wire rope is arranged in the central unit (Comparative Example 2), the torsional properties of the prepared multi-twisted aluminum alloy cable are also poor.

[0205] In summary, the present invention designs the conductor structure of the multi-twisted aluminum alloy cable and designs the steel wire rope in the central unit, so that the multi-twisted aluminum alloy cable has good torsional resistance and no broken aluminum alloy monofilaments in the conductor; at the same time, the present invention designs the insulating layer material and the sheath material, so that the multi-twisted aluminum alloy cable has good flame retardant properties, salt spray resistance and mildew resistance.

[0206] The applicant declares that the present invention illustrates the detailed structural features and detailed process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed structural features and detailed process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed structural features and detailed process flow to be implemented. Those skilled in the art should understand that any improvement to the present invention, the equivalent replacement of the components selected by the present invention, the addition of auxiliary components, the selection of specific methods, etc., as well as the equivalent replacement of the raw materials of the product of the present invention, the addition of auxiliary components, the selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A multi-twisted aluminum alloy cable, characterized in that: The multi-twisted aluminum alloy cable comprises a conductor, an insulating layer and a sheath in sequence from the inside to the outside in radial direction; The conductor is obtained by left-twisting one central unit and six peripheral units, wherein the central unit is located at the center of the peripheral units; The central unit is obtained by left-twisting one steel wire rope and six Class 5 aluminum alloy strands, wherein the steel wire rope is located at the center of the Class 5 aluminum alloy strands; The peripheral unit is obtained by left-twisting 7 Class 5 aluminum alloy strands; The five types of aluminum alloy strands are obtained by twisting 30 to 40 aluminum alloy single wires in the right direction; The diameter of the aluminum alloy monofilament is 0.30 to 0.51 mm; The mass percentage of silicon in the aluminum alloy monofilament is 0.03-0.15%, the mass percentage of iron is 0.40-1.00%, and the mass percentage of zinc is ≤0.10%; The pitch diameter ratio of the five types of aluminum alloy strands is 16 to 18 times; The diameter of the steel wire rope is 3.0-4.0 mm; The pitch-to-diameter ratio of the central unit is 14 to 16 times; The pitch-diameter ratio of the peripheral unit is 14 to 16 times; The conductor has a pitch diameter ratio of 12 to 14 times; The thickness of the insulating layer is 2.0 to 3.0 mm; The thickness of the sheath is 2.0-4.0 mm.

2. The multi-twisted aluminum alloy cable according to claim 1, characterized in that: The insulating layer is prepared from an insulating layer material; The insulating layer material includes the following raw material components in parts by weight: 45-55 parts of EPDM rubber, 20-30 parts of talc, 20-30 parts of modified calcined kaolin, 3-7 parts of white carbon black, 3-7 parts of rubber paraffin oil, 2-4 parts of nano zinc oxide, 2-4 parts of microcrystalline wax, 2-4 parts of titanium dioxide, 1-3 parts of vulcanizing agent, 0.7-1 part of antioxidant RD and 0.8-1.2 parts of antioxidant MB.

3. The multi-twisted aluminum alloy cable according to claim 2, characterized in that: The vulcanizing agent is selected from dicumyl peroxide and / or vulcanizing agent BIBP.

4. The multi-twisted aluminum alloy cable according to claim 2, characterized in that: The raw material components of the insulating layer material also include 0.8 to 1.5 parts of a vulcanizing agent.

5. The multi-twisted aluminum alloy cable according to claim 4, characterized in that: The co-vulcanizing agent is selected from any one of triallyl isocyanurate, trimethylolpropane trimethacrylate and crosslinking agent TAC, or a combination of at least two thereof.

6. The multi-twisted aluminum alloy cable according to claim 2, characterized in that: The raw material components of the insulating layer material also include 0.4 to 0.7 parts of stearic acid.

7. The multi-twisted aluminum alloy cable according to claim 2, characterized in that: The raw material components of the insulating layer material also include 0.3 to 0.8 parts of a coupling agent.

8. The multi-twisted aluminum alloy cable according to claim 7, characterized in that: The coupling agent is selected from vinyl tri(β-methoxyethoxy) silane and / or vinyl trimethoxy silane.

9. The multi-twisted aluminum alloy cable according to claim 1, characterized in that: The sheath is prepared from a sheath material; The sheath material comprises the following raw material components in parts by weight: 45-55 parts of chlorinated polyethylene, 8-12 parts of POE, 15-25 parts of modified kaolin, 8-12 parts of white carbon black, 2-3 parts of carbon black, 5-10 parts of light magnesium oxide, 3-5 parts of calcium zinc stabilizer, 7-10 parts of flame retardant, 4-6 parts of mildewproof agent, 1-3 parts of red lead, 3-5 parts of chlorinated paraffin, 5-7 parts of cold-resistant plasticizer, 5-7 parts of trichloroethyl phosphate and 1-3 parts of vulcanizing agent.

10. The multi-twisted aluminum alloy cable according to claim 9, characterized in that: The flame retardant is a silicate flame retardant.

11. The multi-twisted aluminum alloy cable according to claim 9, characterized in that: The mildew preventer is dichlorophenol.

12. The multi-twisted aluminum alloy cable according to claim 9, characterized in that: The cold-resistant plasticizer is plasticizer DOS.

13. The multi-twisted aluminum alloy cable according to claim 9, characterized in that: The vulcanizing agent is selected from dicumyl peroxide and / or vulcanizing agent BIBP.

14. The multi-twisted aluminum alloy cable according to claim 9, characterized in that: The raw material components of the sheath material also include 0.8 to 1.2 parts of a vulcanizing agent.

15. The multi-twisted aluminum alloy cable according to claim 14, characterized in that: The co-vulcanizing agent is selected from any one of triallyl isocyanurate, trimethylolpropane trimethacrylate and crosslinking agent TAC, or a combination of at least two thereof.

16. The multi-twisted aluminum alloy cable according to claim 9, characterized in that: The raw material components of the sheath material also include 0.3 to 0.7 parts of an antioxidant.

17. The multi-twisted aluminum alloy cable according to claim 16, characterized in that: The antioxidant is selected from antioxidant RD and / or antioxidant MB.

18. The multi-twisted aluminum alloy cable according to claim 9, characterized in that: The raw material components of the sheath material also include 0.3 to 0.7 parts of a coupling agent.

19. The multi-twisted aluminum alloy cable according to claim 18, characterized in that: The coupling agent is selected from γ-aminopropyltriethoxysilane.

20. A method for preparing a multi-twisted aluminum alloy cable according to any one of claims 1 to 19, characterized in that: The preparation method comprises the following steps: After the insulating layer is extruded on the outer surface of the conductor, a sheath is extruded on the outer surface of the insulating layer to obtain the multi-twisted aluminum alloy cable.

21. The preparation method according to claim 20, characterized in that: The extrusion method is extrusion molding through an extruder.

22. The preparation method according to claim 21, characterized in that: The temperature of the feed port of the extruder is 45-55°C.

23. The preparation method according to claim 21, characterized in that: The working temperature of the extruder head is 75-85°C.

24. The preparation method according to claim 21, characterized in that: The extruder body includes a first region and a second region connected.

25. The preparation method according to claim 24, characterized in that: The working temperature of the first zone is 65-75°C, and the working temperature of the second zone is 75-85°C.

26. Use of the multi-twisted aluminum alloy cable according to any one of claims 1 to 19 in wind power generation.