An activation-free heavy oil hydrogenation catalyst and preparation method thereof

Through the activation-free heavy oil hydrogenation catalyst preparation method, the use of inert gas drying and staged temperature sulfurization technology, combined with gradual passivation gas treatment, solves the problems of easy deactivation and environmental pollution of the catalyst, and achieves high sulfurization depth and stability of the catalyst. It is suitable for quick start-up and safe transportation.

CN113908887BActive Publication Date: 2024-10-01PETROCHINA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010656462.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-07-09
Publication Date
2024-10-01
Estimated Expiration
2040-07-09

AI Technical Summary

Technical Problem

Existing heavy oil hydrogenation catalysts need to be pre-sulfurized before starting work, which leads to problems such as easy deactivation of the catalyst, environmental pollution, and long start-up time. Catalysts that do not require on-site start-up activation have problems such as spontaneous combustion and difficulty in storage and transportation.

Method used

An activation-free heavy oil hydrogenation catalyst preparation method is adopted. Through inert gas drying, staged temperature sulfurization, and gradual passivation gas treatment, the hydrogen sulfide and oxygen contents are controlled to form a protective film to prevent the catalyst active metal from contacting oxygen and improve the stability of the catalyst. sex and transportation.

Benefits of technology

It significantly improves the sulfurization depth and uniformity of the catalyst, reduces the start-up time, and reduces environmental pollution. The catalyst exists stably in the air, making it suitable for quick start-up and safe transportation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113908887B_ABST
    Figure CN113908887B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing an activation-free heavy oil hydrogenation catalyst, comprising the following steps: S1, loading the heavy oil hydrogenation catalyst to be treated into a reactor, and purging and drying with an inert gas; S2, continuing to introduce a sulfiding gas for a sulfidation reaction, wherein the sulfiding gas is composed of 5-10v% hydrogen sulfide and the remainder of hydrogen, and controlling the pressure of the mixed gas to be 14-25.0MPa, and adopting a staged temperature rise sulfidation process; S3, after the sulfidation of step S2 is completed, gradually stop introducing the mixed sulfiding gas, and gradually introduce an inert gas at the same time, and ensure that the gas flow rate remains unchanged; S4, when the heavy oil hydrogenation catalyst to be sulfided is cooled to 60-90°C in an inert gas atmosphere, introduce a passivation gas with a gradually increasing oxygen content for catalyst passivation; then purge with cold air, and the passivation ends. The present invention also relates to an activation-free heavy oil hydrogenation catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a heavy oil hydrogenation catalyst free of activation, and in particular to an activation-free heavy oil hydrogenation catalyst particularly used for the conversion and modification of heavy oil products such as wax oil, deasphalted oil, residual oil, and the like, and a preparation method thereof. Background Art

[0002] Heavy oil hydroprocessing mainly refers to the hydrodemetallization, hydrodesulfurization, hydrodenitrogenation, aromatic saturation, olefin saturation and hydrocracking reactions on the residue and other fractions. Most of the metals in crude oil exist in the residue. Although the content of metals (mainly Ni, V, etc.) in the residue is very small, only in the order of parts per million, it is easy to permanently poison and deactivate the residue hydrodesulfurization catalyst, hydrodenitrogenation catalyst and catalytic cracking catalyst. Therefore, it is necessary to remove the trace metal compounds in the residue raw material. The residue hydrodemetallization reaction is also one of the important chemical reactions that occur in the residue hydroprocessing process. Under the action of the catalyst, various metal compounds react with hydrogen sulfide to form metal sulfides, which are then deposited on the catalyst and removed. In order to ensure the performance of the catalyst loaded in the subsequent reactor, the best way is to force the metal to deposit on the hydrodemetallization catalyst of the protective reactor to prevent the catalyst in the subsequent reactor from being deactivated prematurely, because the pores of these catalysts are very small, and the hydroprocessing and conversion reactions are mostly carried out in the subsequent reactor; the hydrodesulfurization reaction of residual oil is the most important chemical reaction that occurs during the hydroprocessing of residual oil. Under the action of catalysts and hydrogen, various sulfur-containing compounds are converted into sulfur-free hydrocarbons and hydrogen sulfide through the hydrodesulfurization reaction. Hydrocarbons remain in the product, while hydrogen sulfide is removed from the reactants; most of the nitrogen in crude oil is also present in the residual oil, and the nitrides in the residual oil can be divided into two categories: alkaline and non-alkaline. In the process of residue oil hydrogenation, various nitrogen-containing compounds generate ammonia and hydrocarbons under the action of catalysts. Ammonia is removed from the reactants, while hydrocarbons remain in the products. The hydrogenation saturation reaction of residue oil aromatics is mainly the hydrogenation of polycyclic aromatics. This type of reaction is the most difficult reaction among all hydrogenation reactions in the residue oil hydrogenation process. Monocyclic aromatics are difficult to hydrogenate and saturate, while polycyclic aromatics are hydrogenated and saturated ring by ring, and the difficulty of hydrogenation increases ring by ring. The hydrogenation reaction of each ring of polycyclic aromatics is a reversible reaction and is in a state of equilibrium. The depth of hydrogenation is often limited by chemical equilibrium. If there are substituents on the benzene ring, the hydrogenation saturation of aromatics is more difficult. The temperature of the residue hydrodenitrogenation catalyst should not be too high, and a high hydrogen partial pressure should be maintained as much as possible to facilitate the occurrence of aromatic hydrogenation saturation reaction; the olefin saturation reaction has a relatively fast reaction rate in all residue hydrotreating reactions, second only to the hydrodemetallization reaction rate, and at the hydrodesulfurization reaction temperature, the olefin hydrogenation reaction basically reaches complete saturation; the hydrocracking reaction is a reaction in which larger hydrocarbon molecules in the feed are converted into small molecules in the presence of hydrogen and a catalyst, and it occurs almost throughout the entire reaction process.

[0003] The goal of the residue oil hydrogenation unit is to provide high-quality raw materials for the downstream heavy oil catalytic cracking unit. For reactions such as residue oil hydrodemetallization, hydrodesulfurization, hydrodenitrogenation, aromatic saturation, olefin saturation and hydrocracking, the fixed-bed residue oil hydrogenation process generally includes multiple reactors (usually four or five reactors in series), which require the use of catalysts with different functions. When the unit is started, the catalyst needs to be pre-sulfurized to react the oxidized metal with the sulfur-containing compound to convert it into a sulfided metal to stimulate the catalyst activity.

[0004] The sulfidation process is mainly divided into two types: in-vessel sulfidation and ex-vessel sulfidation. In-vessel sulfidation refers to the in-situ sulfidation after the catalyst is loaded into the reactor. In-vessel sulfidation can be carried out in two ways: dry sulfidation and wet sulfidation. Dry sulfidation refers to mixing the sulfiding agent and hydrogen in a certain proportion and directly passing them into the catalyst bed, while wet sulfidation refers to sulfiding the catalyst with the sulfiding agent carried by oil products. The purpose of converting the oxidized metal into the sulfided metal is achieved by controlling the flow rate of the sulfide and adjusting the temperature and pressure of the bed. For the residual oil hydrogenation process, dimethyl disulfide is usually used as the sulfiding agent, and diesel and wax oil are used as solvents to perform the sulfidation operation on the catalyst. During the start-up sulfidation process of the residual oil unit, the temperature control is extremely strict. Because in the oxidized state, the residual oil hydrogenation catalyst contacts with pure hot H2 (without hydrogen sulfide), which will cause the active metal of the catalyst to undergo a reduction reaction, resulting in permanent deactivation of the catalyst. Generally, if the hydrogen temperature exceeds 260°C, the deactivation of the catalyst can occur within a few hours, so the hot H2 temperature must be controlled. Furthermore, during the sulfidation process, before hydrogen sulfide is detected in the circulating hydrogen, it is also necessary to control the maximum temperature of the catalyst bed to prevent reduction reactions from occurring.

[0005] In-vessel sulfidation has certain disadvantages. First, it is easy to cause the catalyst bed to overheat, resulting in temporary or permanent loss of catalyst activity. In-vessel sulfidation is also prone to incomplete catalyst sulfidation, affecting its activity. In addition, in-vessel sulfidation requires special equipment, and the sulfiding agent is generally toxic. Especially under high temperature conditions, the sulfiding agent will react with hydrogen to generate hydrogen sulfide and methane. Once leaked, it will pollute the environment and cause harm to operators. In order to ensure the degree of sulfidation, several reactors need to reach the optimal sulfidation temperature. The sulfidation time is very long, resulting in a long start-up time for industrial equipment, affecting the production progress of the refinery.

[0006] Ex-situ sulfurization is usually divided into two types: sulfur-carrying type and sulfurization type. The former mostly uses elemental sulfur or organic sulfides with different decomposition temperatures to load on the catalyst by impregnation technology, changing the active metal on the catalyst from an oxidized state to a partially sulfurized state. The metal components of the sulfurized catalyst are completely in a sulfurized state. When starting up, the temperature is directly raised and the oil is added without sulfurization or activation. The start-up time is very short and pollution-free. Refiners are willing to use this sulfurized hydrogenation catalyst that does not require on-site start-up and activation, but this catalyst also has problems such as the catalyst being prone to spontaneous combustion when exposed to air and being unable to be stored and transported for a long time, which affects the application of this technology. It is usually necessary to passivate the catalyst. Currently, the publicly available passivation technologies are roughly divided into gas phase passivation and liquid phase passivation. Gas phase passivation mainly uses an oxidizing gas to form an oxide film on the surface of the sulfurized catalyst at an appropriate temperature to protect the sulfurized catalyst. Liquid phase passivation mainly uses methods such as spraying and impregnation to load organic oxygen-containing hydrocarbons onto the surface of the sulfurized catalyst to form a protective film.

[0007] CN102041045B, CN1129609A and US2002000394A1 all belong to sulfur-carrying type off-site presulfurization methods. The selected vulcanizing agent is elemental sulfur or a sulfur-containing compound, and the organic solvent loaded on the catalyst together with the vulcanizing agent is an organic solvent containing an unsaturated bond. The method is simple in process and saves cost, but the method uses a large amount of organic solvents in the production process, which is not conducive to safety and environmental protection.

[0008] CN102284299A discloses a method for presulfiding an oxidized hydrogenation catalyst outside a hydrogenation reactor. In addition to presulfidation and passivation, the method has the added step of reactivation, i.e., the process of reactivating the passivated catalyst loaded in the hydrogenation reactor in an atmosphere containing a sulfiding agent. The presulfidation process of the method only involves the use of sulfiding gas (sulfur content 0.5-3%), does not require the sulfidation pressure, and the catalyst active metal is Mo and / or Ni.

[0009] US6294498B1 discloses a method for protecting active catalysts by spraying on the outer surface. The method sprays an inert material on the outer surface of the catalyst to form a protective film to protect the core and internal pores of the catalyst particles. The concentration of the protective material decreases gradually from the outer surface to the core, and the protective film disappears automatically under the reaction conditions. After passivation, the mechanical properties and wear resistance of the catalyst are improved, but the disclosed method of spraying the inert protective film is relatively complicated.

[0010] CN105233867B discloses a pre-sulfurized sulfur-resistant conversion catalyst and a preparation method. The surface of the sulfurized catalyst is coated with a surface layer formed by a polymer compound to prevent the active component from contacting with oxygen. The external coating compound is two or more of polyacrylamide, polystyrene acrylonitrile, polyamide, melamine or naphthalene, the mixing ratio is 1:1, and the compound can be gasified at 250-350°C. The preparation method of the catalyst is to pass the gasified coating compound through the sulfurized catalyst bed under vacuum conditions (0.2-1psi), and obtain a stable catalyst after cooling. The polymer compound film will not react chemically with the active center of the catalyst, will not affect the activity of the catalyst, and when the catalyst is used, the polymer compound film is discharged in the catalyst pore in a gaseous form, which has a secondary adjustment effect on the catalyst pore structure. The catalyst prepared by this method has high conversion activity and good stability, but it is difficult to evacuate in industrial applications. Summary of the invention

[0011] The present invention relates to a heavy oil hydrogenation catalyst preparation process without activation. The finished catalyst prepared by the process method has high activity, is easy to store and transport, and can meet the safe and rapid start-up requirements of refineries.

[0012] To this end, the present invention provides a method for preparing an activation-free heavy oil hydrogenation catalyst, comprising the following steps:

[0013] S1. Load the heavy oil hydrogenation catalyst to be treated into a reactor, purge it with inert gas, and dry it at 100-150° C. for 2-6 hours;

[0014] S2, continue to introduce the sulfiding gas for sulfidation reaction, the sulfiding gas is composed of 5-10v% hydrogen sulfide and the balance hydrogen, the pressure of the mixed gas is controlled to be 14-25.0MPa, and the temperature is increased by stage during the sulfidation process, starting from the drying temperature in step S11, the temperature is increased at a rate of 2-10°C / h, when the sulfidation temperature is 180-250°C, the temperature is kept constant for 1-15 hours, when the sulfidation temperature is 250-400°C, the temperature is kept constant for 1-10 hours, and the sulfidation is completed;

[0015] S3. After the vulcanization of step S2 is completed, the introduction of the mixed vulcanizing gas is gradually stopped, and the inert gas is gradually introduced, and the gas flow rate is kept constant;

[0016] S4. When the sulfurized heavy oil hydrogenation catalyst is cooled to 60-90° C. in an inert gas atmosphere, a passivation gas with gradually increasing oxygen content is introduced to passivate the catalyst; then cold air is blown to complete the passivation.

[0017] In the method for preparing the activation-free heavy oil hydrogenation catalyst of the present invention, it is preferred that the inert gas is nitrogen.

[0018] The preparation method of the activation-free heavy oil hydrogenation catalyst of the present invention is preferably that the heavy oil hydrogenation catalyst is a supported catalyst, the active metal thereof comprises at least one of Group VIB and / or Group VIII metals, and the carrier thereof comprises but is not limited to one or more of alumina, magnesium oxide, silicon aluminum oxide, and molecular sieve.

[0019] In the method for preparing the activation-free heavy oil hydrogenation catalyst of the present invention, the VIB group metal is more preferably molybdenum and / or tungsten, and the VIII group metal is more preferably cobalt and / or nickel.

[0020] In the method for preparing the activation-free heavy oil hydrogenation catalyst of the present invention, it is preferred that the oxygen content of the passivation gas is 0.05-10%.

[0021] The preparation method of the activation-free heavy oil hydrogenation catalyst of the present invention is preferably that in step S4, the passivation includes the following steps: the catalyst is first passivated in a passivation gas with an oxygen content of 0.05-0.5% for 0.5-6 hours; then, the passivation gas flow rate is kept unchanged and the oxygen content is increased, and the catalyst is passivated in a passivation gas with an oxygen content of 0.5-5% for 0.5-6 hours; the passivation gas flow rate is kept unchanged and the oxygen content is continuously increased, and the catalyst is passivated in a passivation gas with an oxygen content of 5-10% for 0.5-6 hours.

[0022] The method for preparing the activation-free heavy oil hydrogenation catalyst of the present invention preferably further comprises the following steps: coating the outer surface of the passivated heavy oil hydrogenation catalyst with an oxide film, wherein the oxide film disappears after heating.

[0023] In the method for preparing the activation-free heavy oil hydrogenation catalyst of the present invention, it is preferred that, in step S1, the heavy oil hydrogenation catalyst to be treated is a calcination-free heavy oil hydrogenation catalyst or a calcined oxidized heavy oil hydrogenation catalyst.

[0024] The method for preparing the activation-free heavy oil hydrogenation catalyst of the present invention is suitable for preparing a series of heavy oil hydrogenation catalysts, which include hydrodemetallization catalysts, hydrodesulfurization catalysts and hydrodenitrogenation catalysts.

[0025] To this end, the present invention also provides an activation-free heavy oil hydrogenation catalyst, which is prepared by the above-mentioned preparation method. The heavy oil hydrogenation catalyst is a heavy oil hydrodemetallization catalyst, a heavy oil hydrodenitrogenation catalyst or a heavy oil hydrodesulfurization catalyst.

[0026] The activation-free heavy oil hydrogenation catalyst of the present invention is preferably such that when the active metal comprises a Group VIII metal, the content thereof is 1.0 to 10.0 wt % calculated as Group VIII metal sulfide; and when the active metal comprises a Group VIB metal, the content thereof is 3.0 to 35.0 wt % calculated as Group VIB metal sulfide.

[0027] Taking nickel and molybdenum as active metals for example, the Group VIII metal sulfide is Ni3S2, and its content is 1.0-10.0 wt%; the Group VIB metal sulfide is MoS2, and its content is 3.0-35.0 wt%.

[0028] The activation-free heavy oil hydrogenation catalyst of the present invention preferably has a specific surface area greater than 10 m 2 .g -1 , pore volume greater than 0.1cm 3 .g -1 .

[0029] The activation-free heavy oil hydrogenation catalyst of the present invention preferably has a specific surface area of ​​20-500 m 2 .g -1 , pore volume is 0.2-3.0cm 3 .g -1 .

[0030] In the activation-free heavy oil hydrogenation catalyst of the present invention, the passivating gas includes but is not limited to one or two of oxygen and air.

[0031] The preparation method of the activation-free heavy oil hydrogenation catalyst of the present invention has the following specific process:

[0032] (1) Catalyst sulfurization: The oxidized heavy oil hydrogenation catalyst or the calcination-free heavy oil hydrogenation catalyst (which has been impregnated and dried) is loaded into the reactor and purged with an inert gas. The reactor is dried at a temperature of 100 to 150°C for 2 to 6 hours. A sulfurizing gas is continuously introduced at a temperature of 100 to 250°C for sulfurization reaction. The sulfurizing gas is composed of 5 to 10% by volume of hydrogen sulfide and the remainder of hydrogen. The pressure of the sulfurizing gas is controlled at 14 to 25.0 MPa. The sulfurization process adopts staged temperature rise sulfurization. The catalyst sulfurization temperature rise rate is 5 to 10°C / h. When the sulfurization temperature rises to 180 to 250°C, the temperature is kept constant for 1 to 8 hours. When the sulfurization temperature rises to 250 to 500°C, the temperature is kept constant for 1 to 8 hours. The sulfurization is then completed.

[0033] (2) Catalyst passivation: After the catalyst is completely vulcanized, the injection of the sulfiding gas is gradually stopped, and nitrogen is introduced to replace it, and the total gas flow rate is ensured to remain unchanged during the replacement process. When the fully vulcanized catalyst is cooled to 60-90°C in a nitrogen atmosphere, an oxygen-containing passivation gas is introduced to perform a catalyst passivation operation, and the passivation gas flow rate is kept constant, and the oxygen content (oxygen concentration) therein is gradually increased within the range of 0.05-0.5v%. Specifically, the catalyst is first passivated in a passivation gas with an oxygen content of 0.05-0.5% for 0.5-6 hours; then, the passivation gas flow rate is kept constant, and the oxygen content is increased, and the catalyst is passivated in a mixed gas with an oxygen content of 0.5-5% for 0.5-6 hours; the mixed gas flow rate is kept constant, and the oxygen content is continued to be increased, and the catalyst is passivated in a mixed gas with an oxygen content of 5-10% for 0.5-6 hours; finally, cold air is introduced for purging. After the passivation is completed, the catalyst can be barreled and sealed.

[0034] The preparation method provided by the present invention can reduce the catalyst sulfurization time by more than 50% compared with conventional off-site presulfurization, effectively improve the sulfurization rate of the metal in the small pore part of the catalyst, and then improve the overall sulfurization rate of the catalyst. The catalyst prepared by this method has a high sulfurization depth, uniform sulfurization, good activity, can exist stably in the air, and is convenient for storage, transportation and loading. In addition, when the device is started, the temperature is increased, oil is added, and the reaction conditions are adjusted to directly enter the industrial production operation of the device without sulfurization, which can significantly improve the start-up efficiency and reduce the start-up time, reduce the environmental problems caused by the sulfurization process, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 The present invention is a process flow chart of an evaluation device for an activation-free heavy oil hydrogenation catalyst obtained by the preparation method of the present invention.

[0036] in:

[0037] 1- Buffer tank,

[0038] 2- the first hydrogenation reactor,

[0039] 3- The second hydrogenation reactor,

[0040] 4- the third hydrogenation reactor,

[0041] 5-Gas-liquid separator (including high-pressure separator and low-pressure separator). DETAILED DESCRIPTION

[0042] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions.

[0043] Example 1

[0044] (1) Sulfidation of Residue Hydrodemetallization Catalyst

[0045] The residue hydrodemetallization catalyst is an oxidized catalyst prepared by the method described in Example 1 of CN101928593A, and its properties are shown in Table 1.

[0046] The oxidized catalyst is added into the hydrogenation reactor, sealed and purged with nitrogen, and dried for 4 hours at a catalyst bed temperature of 130°C. After the catalyst bed is heated to 200°C at a rate of 10°C / h, sulfiding gas is introduced. The sulfiding gas consists of 5v% hydrogen sulfide and the remainder hydrogen, and the sulfiding gas pressure is ensured to be 14MPa during the entire sulfidation process.

[0047] The temperature is increased at a rate of 5°C / h. When the bed temperature reaches 230°C, the temperature is kept constant for 2 hours. The temperature is then increased to 400°C and kept constant for 2 hours, and the vulcanization is completed.

[0048] (2) Passivation of residue hydrodemetallization catalyst

[0049] After the catalyst is completely sulfided, the sulfiding gas is gradually replaced with nitrogen, ensuring that the gas flow rate remains unchanged until the catalyst bed temperature drops to 60°C. After the reactor temperature stabilizes, the passivation operation begins, and the bed temperature is kept constant at 60°C throughout the passivation process.

[0050] First, a passivation gas with an oxygen content of 0.05v% was introduced for 2 hours, and the passivation gas consisted of oxygen and the remainder of nitrogen; secondly, the passivation gas flow rate was kept constant, and the oxygen content of the passivation gas was gradually increased to 0.5v%, and the passivation was carried out for 2 hours; thirdly, the passivation gas flow rate was kept constant, and the oxygen content of the passivation gas was further increased to 5v%, and the passivation was carried out for 1 hour; finally, the heating was stopped, the hydrogenation reactor was cooled naturally, and cold air was gradually introduced to replace the passivation gas, and the cold air was used to purge the hydrogenation reactor until the bed temperature dropped to room temperature, and the passivation was completed. The catalyst was sealed in a barrel.

[0051] Example 2

[0052] (1) Sulfidation of residue hydrodesulfurization catalyst

[0053] The residue hydrodesulfurization catalyst was prepared by the method described in Example 1 of CN101928593A. The properties of the oxidized catalyst are shown in Table 1.

[0054] The oxidized catalyst is added into the hydrogenation reactor, sealed and purged with nitrogen, and dried for 4 hours at a catalyst bed temperature of 130°C. After the catalyst bed is heated to 200°C at a rate of 10°C / h, sulfiding gas is introduced. The sulfiding gas consists of 5v% hydrogen sulfide and the remainder hydrogen, and the sulfiding gas pressure is ensured to be 18MPa during the entire sulfidation process.

[0055] The temperature was raised at a rate of 8°C / h. After the bed temperature reached 230°C, it was kept constant for 3 hours. The temperature was further raised to 360°C and kept constant for 2 hours. Then, the vulcanization was completed.

[0056] (2) Passivation of residue hydrodesulfurization catalyst

[0057] After the catalyst is completely sulfided, nitrogen is gradually used to replace the sulfidation gas, ensuring that the gas flow rate remains unchanged until the catalyst bed temperature drops to 60°C. After the reactor temperature stabilizes, the passivation operation begins, and the bed temperature is kept constant at 60°C throughout the passivation process.

[0058] First, a passivation gas with an oxygen content of 0.1v% was introduced for 2 hours, and the passivation gas consisted of oxygen and nitrogen; secondly, the passivation gas flow rate was kept constant, and the oxygen content of the passivation gas was increased to 1v%, and the passivation was carried out for 2 hours; thirdly, the passivation gas flow rate was kept constant, and the oxygen content of the passivation gas was further increased to 7.5v%, and the passivation was carried out for 1 hour; finally, the heating was stopped, the hydrogenation reactor was cooled naturally, and cold air was gradually introduced to replace the passivation gas, and the reactor was purged with cold air until the bed temperature dropped to room temperature, and the passivation was completed. The catalyst was sealed in a barrel.

[0059] Example 3

[0060] (1) Preparation of residue hydrodenitrogenation catalyst

[0061] Take 500g (dry basis) of silicon-containing pseudo-boehmite dry rubber powder (SiO2 content is 39%), add 15g of sesbania powder, and mix well. Add 395g of acetic acid solution with a concentration of 3.5wt% to the above materials, knead for 40 minutes, and then extrude into a cylindrical shape with a diameter of 2.0mm on a single screw extruder. Dry in a 120℃ oven for 3 hours, then place in a roasting furnace, heat to 780℃ at a heating rate of 100-150℃ / h, and roast for 3 hours.

[0062] Weigh 150g of the above-mentioned carrier with a water absorption rate of 1.10ml / g, and spray it with a measured ammonia solution containing ammonium molybdate (containing 82.0wt% MoO3) and nickel nitrate (containing 25.2wt% NiO) according to the amount of saturated absorption solution. Homogenize in the spraying equipment for 5 minutes, dry at 60℃ for 2 hours, then heat to 120℃ and dry for 3 hours to obtain a nickel-molybdenum-containing non-calcined hydrodenitrogenation catalyst.

[0063] To facilitate the characterization of the catalyst, the prepared nickel-molybdenum-containing calcination-free hydrodenitrogenation catalyst was calcined in air at 500°C for 3 hours. After cooling, the catalyst properties were analyzed. The results are shown in Table 1.

[0064] (2) Sulfidation of Residue Hydrodenitrogenation Catalyst

[0065] The calcination-free hydrodenitrogenation catalyst prepared in (1) was added to a hydrogenation reactor, sealed, purged with nitrogen, and dried for 4 hours at a catalyst bed temperature of 130°C. After the catalyst bed was heated to 200°C at a rate of 10°C / h, sulfiding gas was introduced, the sulfiding gas containing 5% by volume of hydrogen sulfide and the remainder of hydrogen, and the sulfiding gas pressure was ensured to be 21 MPa during the entire sulfiding process.

[0066] The temperature was raised at a rate of 3°C / h. After the bed temperature reached 230°C, the temperature was kept constant for 3 hours. The temperature was further raised to 330°C and kept constant for 3 hours. Then the vulcanization was completed.

[0067] (3) Passivation of residue hydrodenitrogenation catalyst

[0068] After the catalyst is completely sulfided, nitrogen is gradually used to replace the sulfiding gas, ensuring that the total gas flow remains unchanged until the catalyst bed temperature drops to 70°C. After the temperature of the hydrogenation reactor stabilizes, the passivation operation begins, and the bed temperature is kept constant at 70°C throughout the passivation process.

[0069] First, a passivation gas with an oxygen content of 0.2v% was introduced for 2 hours, and the passivation gas consisted of oxygen and nitrogen; secondly, the passivation gas flow rate was kept constant, and the oxygen content of the passivation gas was increased to 2v%, and the passivation was carried out for 2 hours; thirdly, the passivation gas flow rate was kept constant, and the oxygen content of the passivation gas was further increased to 10%, and the passivation was carried out for 1 hour; finally, the heating was stopped, the hydrogenation reactor was cooled naturally, and cold air was gradually introduced to replace the passivation gas, and the reactor was purged with cold air until the bed temperature dropped to room temperature, and the passivation was completed. The catalyst was sealed in a barrel.

[0070] Example 4

[0071] This example uses the activation-free heavy oil hydrogenation catalyst prepared by the present invention to test its activity and stability. The activation-free hydrodemetallization catalyst, hydrodesulfurization catalyst, and hydrodenitrogenation catalyst prepared in Examples 1-3 are added to a hydrogenation reaction device (3×300ml small test evaluation device, see Figure 1 The addition ratios were 30wt%, 43wt% and 27wt% respectively. The properties of the tested feedstock oil are shown in Table 2. The process conditions and the 2000-hour reaction results are shown in Table 4.

[0072] See also Figure 1As shown, the evaluation process of the present invention is as follows: the feedstock oil and hydrogen for hydrogenation evaluation are mixed in the buffer tank 1, and then sequentially enter the first hydrogenation reactor 2, the second hydrogenation reactor 4, and the third hydrogenation reactor 4 for reaction, and then pass through the gas-liquid separator 5 combination (pass through the high-pressure separator and the low-pressure separator in sequence), and finally obtain gas and hydrogenated full-fraction oil. The first hydrogenation reactor 2, the second hydrogenation reactor 3, and the third hydrogenation reactor 4 are arranged in series, and the reaction conditions are consistent.

[0073] Comparative Example 1

[0074] This comparative example uses the oxidized hydrodemetallization catalyst, oxidized hydrodesulfurization catalyst and calcination-free hydrodenitrogenation catalyst prepared in Examples 1-3 to compare and evaluate the sulfurization rate. The oxidized and calcination-free catalyst sulfurization device is the same as the evaluation device in Example 4. The catalyst bed is heated to 200°C at 10°C / h and then the sulfurization gas is introduced. The sulfurization gas contains 5v% hydrogen sulfide and the remainder of hydrogen, and the sulfurization gas pressure is ensured to be 2MPa during the entire sulfurization process. The temperature is raised at a heating rate of 5°C / h. After the bed is heated to 230°C, the temperature is kept constant for 3 hours; the temperature is continued to be raised to 330°C and kept constant for 3 hours, the sulfurization is completed, and the passivation is the same as in Example 1. The sulfurization rate of the catalyst is shown in Table 1.

[0075] The results show that the average sulfur uptake rate of the activation-free desulfurization, demetallization and denitrification catalysts prepared in Examples 1-3 is 88%; under roughly the same sulfurization time, the average sulfur uptake rate of the catalyst in Comparative Example 1 is only 64%, indicating that high-pressure sulfurization can significantly increase the catalyst sulfurization rate, shorten the sulfurization time, and increase the sulfur uptake rate.

[0076] Comparative Example 2

[0077] This comparative example uses the oxidized hydrodemetallization catalyst, oxidized hydrodesulfurization catalyst and calcination-free hydrodenitrogenation catalyst prepared in Examples 1-3 to compare and evaluate the sulfurization rate. The oxidized and calcination-free catalyst sulfurization device is the same as the evaluation device in Example 4. The catalyst bed is heated to 200°C at 10°C / h and then the sulfurization gas is introduced. The sulfurization gas contains 5v% hydrogen sulfide and the remainder of hydrogen, and the sulfurization gas pressure is ensured to be 2MPa during the entire sulfurization process. The temperature is raised at a heating rate of 3°C / h. After the bed is heated to 230°C, the temperature is kept constant for 10 hours; the temperature is continued to be raised to 330°C and kept constant for 6 hours, the sulfurization is completed, and the passivation is the same as in Example 2. The sulfurization rate of the catalyst is shown in Table 1.

[0078] The results show that the sulfur uptake rates of the activation-free desulfurization, demetallization and denitrification catalysts prepared in Examples 1-3 are all above 86%; the sulfurization time of Comparative Example 2 is roughly twice the average sulfurization time of Examples 1-3, but the sulfur uptake rate of the catalyst is only above 82%, indicating that high-pressure sulfurization can significantly shorten the sulfurization time, increase the sulfur uptake rate, and thus help improve the catalyst performance.

[0079] Comparative Example 3

[0080] This comparative example uses the oxidized hydrodemetallization catalyst, oxidized hydrodesulfurization catalyst and calcination-free hydrodenitrogenation catalyst prepared in Examples 1-3 to compare and evaluate the sulfurization rate. The oxidized and calcination-free catalyst sulfurization device is the same as the evaluation device in Example 4. The catalyst bed is heated to 200°C at 10°C / h and then the sulfurization gas is introduced. The sulfurization gas contains 5v% hydrogen sulfide and the remainder of hydrogen, and the sulfurization gas pressure is ensured to be 8MPa during the entire sulfurization process. The temperature is raised at a heating rate of 3°C / h. After the bed is heated to 230°C, the temperature is kept constant for 3 hours; the temperature is continued to be raised to 330°C and kept constant for 3 hours, the sulfurization is completed, and the passivation is the same as in Example 1. The sulfurization rate of the catalyst is shown in Table 1.

[0081] The results show that the average sulfur uptake rate of the activation-free desulfurization, demetallization and denitrification catalysts prepared in Examples 1-3 is 88%; under roughly the same sulfurization time, the average sulfur uptake rate of the catalyst in Comparative Example 3 is only 69%, indicating that high-pressure sulfurization can significantly increase the catalyst sulfurization rate, shorten the sulfurization time, and increase the sulfur uptake rate.

[0082] Comparative Example 4

[0083] This comparative example uses the oxidized hydrodemetallization catalyst, oxidized hydrodesulfurization catalyst and calcination-free hydrodenitrification catalyst prepared in Examples 1-3 to compare and evaluate the catalyst performance. The evaluation device is the same as that in Example 4. The oxidized hydrodemetallization agent, oxidized hydrodesulfurization agent and calcination-free hydrodenitrification agent are added in order. Figure 1 The reaction device shown in the figure has the addition ratios of 30wt%, 43wt% and 27wt% respectively. The catalyst is vulcanized by wet vulcanization in the vessel, the vulcanization pressure is 10MPa, the vulcanizing agent is carbon disulfide, the addition amount is 2.0wt%, the vulcanization is carried out at 240℃ for 3 hours using sulfurized diesel, and at 300℃ for 2 hours using sulfurized wax oil. The properties of the tested raw oil are shown in Table 2. The properties of the sulfurized oil are shown in Table 3. The process conditions and the 2000-hour reaction results are shown in Table 4.

[0084] Table 1

[0085]

[0086] Note: The upper sulfur rate is the ratio of the amount of sulfur actually consumed by the catalyst active metal to the amount of sulfur required for the catalyst active metal to be completely sulfurized in theory.

[0087] Table 2 Evaluation indexes of crude oil properties

[0088] project Hydrogenated feedstock oil <![CDATA[Density at 20 °C (g / cm -3 )]]> 0.9785 Carbon residue (w%) 12.2 S(w%) 3.44 N(w%) 0.36 Ni+V(wppm) 55.19

[0089] Table 3 Properties of sulfurized oil used in Comparative Example 4

[0090]

[0091] Table 4 2000 hours evaluation results

[0092] Example 4 Comparative Example 4 Reaction conditions Reaction temperature (℃) 380 380 Pressure(MPa) 17.0 17.0 Hydrogen to oil ratio (v / v) 759 759 <![CDATA[Air speed (h -1 )]]> 0.20 0.20 product Desulfurization rate (wt%) 85.2 86.3 Demetallization rate (wt%) 71.4 71.4 Residual carbon removal rate (wt%) 50.6 49.2

[0093] *Note: The operating conditions of the three reactors are the same

[0094] From the data in Table 1 and Table 4 above, it can be seen that the performance of the catalyst prepared by the present invention is comparable to that of the catalyst prepared by conventional in-situ sulfidation in the comparative example. This indicates that the performance of the activation-free catalyst prepared by the present method meets the use requirements and does not require reactivation during use, effectively reducing the start-up time of the device (2-4 days).

[0095] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the present invention.

Claims

1. A method for preparing an activation-free heavy oil hydrogenation catalyst, characterized in that: The following steps are involved: S1. Load the heavy oil hydrogenation catalyst to be treated into a reactor, purge it with inert gas, and dry it at 100-150° C. for 2-6 hours; S2, continue to introduce sulfiding gas for sulfiding reaction, the sulfiding gas is composed of 5-10 v% hydrogen sulfide and the balance hydrogen, the pressure of the sulfiding gas is controlled to be 14-25.0 MPa, and the temperature is increased by stage during the sulfiding process, starting from the drying temperature in step S1, and the heating rate is 2-10°C / h. When the sulfiding temperature is 180-250°C, the temperature is kept constant for 1-15 hours, and when the sulfiding temperature is 250-400°C, the temperature is kept constant for 1-10 hours, and the sulfiding is completed; S3. After the vulcanization in step S2 is completed, the introduction of the vulcanizing gas is gradually stopped, and the inert gas is gradually introduced, and the gas flow rate is kept constant; S4, when the temperature of the sulfurized heavy oil hydrogenation catalyst is lowered to 60-90° C. in an inert gas atmosphere, a passivation gas with gradually increasing oxygen content is introduced to passivate the catalyst; Then cold air is blown and the passivation is finished; In step S4, the passivation includes the following steps: the catalyst is first passivated in a passivation gas with an oxygen content of 0.05 to 0.5 v% for 0.5 to 6 hours; then, the passivation gas flow rate is kept unchanged and the oxygen content is increased, and the catalyst is passivated in a passivation gas with an oxygen content of 0.5 to 5 v% for 0.5 to 6 hours; the passivation gas flow rate is kept unchanged and the oxygen content is continued to be increased, and the catalyst is passivated in a passivation gas with an oxygen content of 5 to 10 v% for 0.5 to 6 hours.

2. The method for preparing the activation-free heavy oil hydrogenation catalyst according to claim 1, characterized in that: The heavy oil hydrogenation catalyst is a supported catalyst, and the active metal thereof comprises at least one of Group VIB and / or Group VIII metals.

3. The method for preparing the activation-free heavy oil hydrogenation catalyst according to claim 1, characterized in that: The following steps are also included: An oxide film is coated on the outer surface of the passivated heavy oil hydrogenation catalyst, and the oxide film can disappear after heating.

4. The method for preparing an activation-free heavy oil hydrogenation catalyst according to claim 1, characterized in that: In step S1, the heavy oil hydrogenation catalyst to be treated is a non-calcined heavy oil hydrogenation catalyst or a calcined oxidized heavy oil hydrogenation catalyst.

5. An activation-free heavy oil hydrogenation catalyst, which is prepared by the preparation method according to any one of claims 1 to 4, characterized in that: The heavy oil hydrogenation catalyst is a heavy oil hydrogenation demetallization catalyst, a heavy oil hydrogenation denitrogenation catalyst or a heavy oil hydrogenation desulfurization catalyst.

6. The activation-free heavy oil hydrogenation catalyst according to claim 5, characterized in that: When the active metal comprises a Group VIII metal, the content thereof is 1.0 to 10.0 wt % calculated as the Group VIII metal sulfide; when the active metal comprises a Group VIB metal, the content thereof is 3.0 to 35.0 wt % calculated as the Group VIB metal sulfide.

7. The activation-free heavy oil hydrogenation catalyst according to claim 5, characterized in that: The specific surface area of ​​the activation-free heavy oil hydrogenation catalyst is greater than 10 m 2 .g -1 , pore volume greater than 0.1 cm 3 .g -1 .

8. The activation-free heavy oil hydrogenation catalyst according to claim 7, characterized in that: The specific surface area of ​​the activation-free heavy oil hydrogenation catalyst is 20-500 m 2 .g -1 , pore volume is 0.2-3.0 cm 3 .g -1 .