Non-aqueous electrolyte secondary battery and battery pack

By using a separator and a reasonable number and thickness design of electrode plate stacking numbers and thicknesses in a nonaqueous electrolyte secondary battery, the problem of increasing reaction force caused by the relaxation of the battery is solved, and the combination of low reaction force and high output performance is achieved.

CN114156525BActive Publication Date: 2024-11-01PRIME PLANET ENERGY & SOLUTIONS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111047184.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-09-08
Filing Date
2021-09-07
Publication Date
2024-11-01
Estimated Expiration
2041-09-07

AI Technical Summary

Technical Problem

In the nonaqueous electrolyte secondary battery, the molding relaxation of the winding electrode body leads to an increase in reaction force, limiting the design freedom of the battery pack and the material selection of the constraint member.

Method used

By using a separator in the electrode body, the proportion limit is ensured to be below 10.2MPa, and creases are formed during the electrode body forming process to reduce rebound. Combined with the appropriate number and thickness relationship of positive and negative plates, the specific The thickness and stacking ratio are used to reduce the reaction force of the battery.

Benefits of technology

Effectively reduce the reaction force of the battery, allowing the use of low-rigid resin materials as the restraining member, improving the output performance of the battery and reducing the risk of poor welding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114156525B_ABST
    Figure CN114156525B_ABST
Patent Text Reader

Abstract

The present invention relates to a non-aqueous electrolyte secondary battery and a battery pack. The non-aqueous electrolyte secondary battery comprises an outer packaging body, an electrode body and an electrolyte. The outer packaging body contains the electrode body and the electrolyte. The electrode body is formed into a flat shape. The electrode body comprises a stack. The stack comprises a first separator, a positive electrode plate, a second separator and a negative electrode plate. The first separator, the positive electrode plate, the second separator and the negative electrode plate are stacked in sequence. The electrode body is formed by winding the stack into a spiral shape. The first separator and the second separator each have a proportional limit of less than 10.2 MPa. The proportional limit is measured in a compression test in the thickness direction of the first separator and the second separator.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a nonaqueous electrolyte secondary battery and a battery pack. Background Art

[0002] Japanese Patent Application Laid-Open No. 2004-214190 discloses a separator for lithium battery, characterized in that the elastic coefficient (elastic modulus) is 2.0 kgf / mm 2 the following. Summary of the invention

[0003] A non-aqueous electrolyte secondary battery (hereinafter referred to as a "battery") includes an electrode body. The electrode body is contained in an outer package. Generally, the electrode body includes a positive electrode plate, a separator, and a negative electrode plate. The electrode body may be a wound type. The wound electrode body is formed by winding a strip-shaped electrode plate and a separator into a spiral shape. Sometimes two separators are used. Sometimes the electrode body is formed into a flat shape after winding.

[0004] After molding, springback occurs in the electrode body, so that the electrode body sometimes loosens. This phenomenon is also referred to as "molding relaxation" below. If molding relaxation occurs, the reaction force of the battery increases. Here, "reaction force" refers to the reaction force relative to the force applied to the battery by the restraining member.

[0005] Batteries expand when charged. For example, in a battery pack, a casing is provided at the outer edge of the battery pack so that the outer dimensions of a single battery are within a predetermined range. The casing includes a restraining member. The restraining member restrains a single battery or a battery module. The restraining member includes, for example, an end plate and a band. If the reaction force of the battery increases, the restraining member is required to have high strength. That is, the design freedom of the battery pack is reduced.

[0006] An object of the present disclosure is to reduce the reaction force in a nonaqueous electrolyte secondary battery including a wound electrode body.

[0007] The technical structure and effects of the present disclosure are described below. However, the mechanism of action of the present disclosure includes assumptions. The correctness of the mechanism of action does not limit the claims.

[0008] [1] A non-aqueous electrolyte secondary battery comprises an outer packaging body, an electrode body and an electrolyte. The outer packaging body contains the electrode body and the electrolyte. The electrode body is formed into a flat shape. The electrode body comprises a laminate. The laminate comprises a first separator, a positive electrode plate, a second separator and a negative electrode plate. The first separator, the positive electrode plate, the second separator and the negative electrode plate are stacked in sequence. The electrode body is formed by winding the laminate into a spiral shape. The first separator and the second separator each have a proportional limit of less than 10.2 MPa. The proportional limit is measured in a compression test in the thickness direction of the first separator and the second separator.

[0009] Hereinafter, in the present disclosure, the "first separator" and the "second separator" may be simply collectively referred to as the "separator". The first separator and the second separator may have substantially the same "material, size, physical property value, etc.". The first separator and the second separator may also have different "materials, sizes, physical property values, etc." from each other.

[0010] The electrode body disclosed in the present invention is a winding type. A stacked body is formed by stacking a positive electrode plate, a separator and a negative electrode plate. A cylindrical electrode body is formed by winding the stacked body into a spiral shape. The electrode body is formed into a flat shape by extruding the cylindrical electrode body in the radial direction between two flat plates. The formed electrode body includes a flat portion and a curved portion. The curved portion is formed on both sides of the flat portion. In the curved portion, the separator is deformed. A crease is formed in the separator near the center of the electrode body (the inner layer side stack of the electrode body). The crease is considered to represent the plastic deformation of the separator. It is considered that the portion where the crease is formed is difficult to rebound. As the amount of deformation of the separator gradually decreases from the center of the electrode body to the outside (the outer layer side stack of the electrode body), the crease disappears eventually. It is considered that a curved portion is formed thereby. For the portion where no crease is formed in the separator and the separator is bent, it is considered that rebound is likely to occur. The wider the range of folds (plastic deformation) in the separator in the direction from the center of the electrode body toward the outside, that is, the greater the number of layers with folds, the less likely molding relaxation occurs, and the reaction force of the battery can be expected to decrease.

[0011] For example, in Japanese Patent Publication No. 2004-214190, it is recorded that the elastic modulus of the separator is below a specified value, thereby suppressing the increase in the thickness of the electrode body. The elastic modulus is a physical property value in the elastic deformation region. However, as described above, it is believed that the molding relaxation of the electrode body and the reaction force of the battery are associated with the deformation in the plastic deformation region exceeding the proportional limit.

[0012] In the present disclosure, the separator has a proportional limit of less than 10.2 MPa. The proportional limit is an indicator of the ease with which plastic deformation occurs. It is believed that the smaller the proportional limit, the easier the separator is to plastically deform. That is, it is believed that the smaller the proportional limit, the wider the range in which folds are formed in the separator in the electrode body. According to the new understanding of the present disclosure, when the proportional limit is less than 10.2 MPa, it can be expected that the reaction force of the battery is significantly reduced.

[0013] [2] The first separator and the second separator may each have a proportional limit of, for example, 4.5 MPa or more.

[0014] When the separator has a proportional limit of 4.5 MPa or more, an increase in output can be expected.

[0015] [3] In a cross section perpendicular to the winding axis of the electrode body, the electrode body includes a curved portion and a flat portion. In the curved portion, the positive electrode plate has a curved surface. In the flat portion, the positive electrode plate has a flat surface. For example, 54 or more layers and 110 or less layers of positive electrode plates may be stacked in the flat portion.

[0016] There is a tendency that the more the number of stacked electrode plates in the flat portion increases, the greater the reaction force of the battery. If the number of stacked positive plates is 54 or more, the increase in reaction force is significant. For electrode bodies with 54 or more positive plates, by applying the separator disclosed in the present invention, it can be expected that the reduction in reaction force will increase. If the number of stacked positive plates exceeds 110 layers, when welding the collector member to the electrode body, for example, it is likely that poor welding will occur.

[0017] [4] In the laminate, the following formula (1) may be satisfied:

[0018] x+y+z≦210 (1)

[0019] relationship.

[0020] In the above formula (1),

[0021] "x" represents the thickness of the positive electrode plate (μm).

[0022] "y" represents the thickness of the negative electrode plate (μm).

[0023] “z” represents the total of the thickness (μm) of the first separator and the thickness (μm) of the second separator.

[0024] When the relationship of the above formula (1) is satisfied, there is a tendency that molding relaxation becomes less likely to occur.

[0025] [5] The assembled battery includes a casing and one or more single cells. The single cell is a non-aqueous electrolyte secondary battery as described in any one of [1] to [4] above. The casing includes a restraining member. The restraining member restrains the single cell. The restraining member is made of a resin material.

[0026] In order to reduce the reaction force of the battery, the restraining member has been made of a metal material with high rigidity. In the present disclosure, the reaction force of the battery can be sufficiently reduced by the separator. Therefore, the restraining member can also be made of a resin material with low rigidity.

[0027] The foregoing and other objects, features, aspects and advantages of the present disclosure will become apparent from the following detailed description to which the present disclosure relates when read in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram showing an example of the nonaqueous electrolyte secondary battery in this embodiment.

[0029] Figure 2 This is a schematic diagram showing an example of an electrode body in this embodiment.

[0030] Figure 3 It is a schematic cross-sectional view showing an example of an electrode body.

[0031] Figure 4 It is a schematic plan view showing an example of a positive electrode plate in this embodiment.

[0032] Figure 5 It is a schematic plan view showing an example of a negative electrode plate in this embodiment.

[0033] Figure 6 This is a schematic diagram showing a method for measuring the reaction force.

[0034] Figure 7 Graph showing the relationship between the proportional limit of the separator and the reaction force.

[0035] Figure 8 is a graph showing the relationship between the proportional limit of the separator and the output.

[0036] Fig. 9 It is a graph showing the relationship between the number of stacked positive electrode plates and the reaction force.

[0037] Fig.10 This is a schematic diagram showing an example of a battery pack in this embodiment. DETAILED DESCRIPTION

[0038] Hereinafter, an embodiment of the present disclosure (hereinafter also referred to as “this embodiment”) will be described. However, the following description does not limit the claims.

[0039] The geometric terms (e.g., "vertical" etc.) in this embodiment may indicate that the state is basically the same. The geometric terms in this embodiment should not be interpreted in a strict sense. For example, "vertical" indicates a state that is basically vertical. That is, "vertical" may slightly deviate from the "vertical" state in the strict sense. "Substantially vertical" naturally includes tolerances, errors, etc. in design, operation, and manufacturing, for example.

[0040] In the present embodiment, the description of "consisting essentially of" indicates that additional components may be included in addition to the essential components, as long as the purpose of the present disclosure is not impaired. For example, components generally envisioned in the technical field (such as unavoidable impurities, etc.) may of course be included.

[0041] In the present embodiment, for example, "0.1 to 10 parts by mass" indicates a range including the boundary value unless otherwise specified. For example, "0.1 to 10 parts by mass" indicates a range of "0.1 parts by mass or more and 10 parts by mass or less".

[0042] In the present embodiment, when a stoichiometric composition formula such as "LiCoO2" is used to represent a compound, the stoichiometric composition formula is only a representative example. For example, when lithium cobalt oxide is represented as "LiCoO2", lithium cobalt oxide is not limited to a composition ratio of "Li / Co / O=1 / 1 / 2" and can contain Li, Co and O in any composition ratio.

[0043] <Non-aqueous electrolyte secondary battery>

[0044] Figure 1 It is a schematic diagram showing an example of the nonaqueous electrolyte secondary battery in this embodiment.

[0045] The battery 100 includes an outer package 90. The outer package 90 is in a square shape (a flat rectangular parallelepiped shape). The outer package 90 can be made of, for example, a metal material. The outer package 90 can be made of, for example, an aluminum (Al) alloy.

[0046] The outer package 90 contains the electrode body 50 and the electrolyte (not shown). That is, the battery 100 includes the electrode body 50 and the electrolyte. In the outer package 90, for example, the electrode body 50 can be held in a resin holder. The electrode body 50 is connected to the positive terminal 91 using the positive electrode collector member 81. The electrode body 50 is connected to the negative terminal 92 using the negative electrode collector member 82.

[0047] Electrode

[0048] Figure 2 This is a schematic diagram showing an example of an electrode body in this embodiment.

[0049] The electrode body 50 is of a wound type. The electrode body 50 is formed into a flat shape. The electrode body 50 includes a laminate 51 . The laminate 51 is wound in a spiral shape around a winding axis 52 , thereby forming the electrode body 50 .

[0050] The laminate 51 includes a first separator 31, a positive electrode plate 10, a second separator 32, and a negative electrode plate 20. The first separator 31, the positive electrode plate 10, the second separator 32, and the negative electrode plate 20 are laminated in this order. The thickness of the laminate 51 (the total thickness of the first separator 31, the thickness of the positive electrode plate 10, the thickness of the second separator 32, and the thickness of the negative electrode plate 20) can be, for example, 210 μm or less. Since the laminate 51 has a thickness of 210 μm or less, a fold is formed in the separator of the curved portion 53 during molding, and there is a tendency that molding relaxation is difficult to occur. That is, it is considered that in the direction from the center of the electrode body 50 to the outside, the range of the fold (plastic deformation) generated in the separator is widened (the number of layers with folds increased). When the laminate 51 has a thickness greater than 210 μm, it is difficult to form a fold in the separator of the curved portion 53 during molding, and there is a tendency that molding relaxation is easy to occur. That is, it is considered that the range of the fold (plastic deformation) in the separator is narrowed (the number of layers with folds is reduced) in the direction from the center of the electrode body 50 to the outside. The thickness of the stack 51 can be, for example, 135 μm to 200 μm from the viewpoint of ensuring the initial battery capacity.

[0051] That is, in the laminate 51, for example, the relationship of the following formula (1) may be satisfied:

[0052] x+y+z≦210 (1).

[0053] In the above formula (1),

[0054] “x” represents the thickness (μm) of the positive electrode plate 10 .

[0055] “y” represents the thickness (μm) of the negative electrode plate 20 .

[0056] "z" represents the total thickness (μm) of the first separator 31 and the thickness (μm) of the second separator 32. The thickness (μm) of the first separator 31 and the thickness (μm) of the second separator 32 may be substantially the same or different.

[0057] Alternatively, in the laminate 51, for example, the relationship of the following formula (2) may be satisfied:

[0058] 135≦x+y+z≦200 (2).

[0059] "x, y, z" in the above formula (2) are the same as "x, y, z" in the above formula (1).

[0060] Furthermore, in the above-mentioned formulas (1) and (2), for example, the following formulas (3) to (5) may be satisfied:

[0061] x≦80 (3)

[0062] y≦80 (4)

[0063] z≦50 (5)

[0064] By further satisfying the relationship between the above equations (3) to (5), it is expected that the reaction force will be reduced.

[0065] Figure 3 It is a schematic cross-sectional view showing an example of an electrode body.

[0066] exist Figure 3 The winding shaft 52 (see Figure 2 ) are perpendicularly intersected. The electrode body 50 includes a curved portion 53 and a flat portion 54. The curved portions 53 are formed on both sides of the flat portion 54. In the curved portion 53, the laminate 51 is curved in an arc shape. In the curved portion 53, the positive electrode plate 10, the negative electrode plate 20 and the separator have curved surfaces. In the flat portion 54, the positive electrode plate 10, the negative electrode plate 20 and the separator have flat surfaces. When the cross section of the curved portion 53 is regarded as an arc, the circle containing the arc has a radius of 0.5d. The flat portion 54 has a thickness of 1.0d.

[0067] (Number of layers)

[0068] The "number of stacking layers" of the present embodiment is counted at the flat portion 54. For example, when counting the number of stacking layers of the positive electrode plate 10, as long as a part of the positive electrode plate 10 covers (reaches) the flat portion 54, it is regarded as 1 layer. The number of stacking layers of the positive electrode plate 10 may be, for example, more than 54 layers and less than 110 layers. For the electrode body 50 in which the number of stacking layers of the positive electrode plate 10 is more than 54 layers, by applying the separator of the present embodiment, it is expected that the reduction of the reaction force will be greater. If the number of stacking layers of the positive electrode plate 10 exceeds 110 layers, poor welding may occur when the positive electrode current collecting component 81 is welded to the electrode body 50. The number of stacking layers of the positive electrode plate 10 may be, for example, more than 58 layers. The number of stacking layers of the positive electrode plate 10 may be, for example, more than 82 layers. The number of stacking layers of the positive electrode plate 10 may be, for example, less than 100 layers.

[0069] "Separator"

[0070] The electrode body 50 of the present embodiment includes a first separator 31 and a second separator 32. In the electrode body 50, at least a portion of the separator is interposed between the positive electrode plate 10 and the negative electrode plate 20. The separator separates the positive electrode plate 10 from the negative electrode plate 20.

[0071] The separator is a strip-shaped sheet. The separator may have a thickness of, for example, 25 μm or less. The separator has a thickness of 25 μm or less, so that molding relaxation is less likely to occur. The separator may have a thickness of, for example, 5 μm to 20 μm. The separator may have a thickness of, for example, 14 μm to 23 μm. The separator may have a thickness of, for example, 14 μm to 20 μm. The separator may have a thickness of, for example, 14 μm to 19 μm. The separator may have a thickness of, for example, 19 μm to 23 μm. The separator may have a thickness of, for example, 20 μm to 23 μm.

[0072] The separator is electrically insulating. The separator may be made of, for example, polyolefin. The separator may be made of, for example, polyethylene (PE). The separator may be made of, for example, polypropylene (PP). The separator may have, for example, a single-layer structure. The separator may be composed of, for example, a PE layer. The separator may have, for example, a laminated structure. The separator may include, for example, a PP layer, a PE layer, and a PP layer. The PP layer, the PE layer, and the PP layer may be laminated in sequence. For example, a ceramic particle layer may be formed on the surface of the separator.

[0073] The separator is porous. The separator may have a porosity of, for example, 40% to 60%. The separator may have a porosity of, for example, 50% to 60%. The porosity may be measured using a mercury porosimeter. The separator may have an air permeability of, for example, 200 s / 100 ml to 300 s / 100 ml. The air permeability may be measured using an Oken type air permeability meter.

[0074] (Proportional Limit)

[0075] "Proportional limit" means the limit of stress at which the proportional relationship between stress and strain (Hooke's law) holds when a solid is deformed by an external force. The separator of the present embodiment has a proportional limit of less than 10.2 MPa. By having a proportional limit of less than 10.2 MPa for the separator, it is expected that the reaction force will be reduced. For example, the separator may have a proportional limit of less than 9.7 MPa. For example, the separator may have a proportional limit of less than 8.8 MPa. For example, the separator may have a proportional limit of less than 7.8 MPa.

[0076] The separator may have a proportional limit of, for example, 4.5 MPa or more. When the separator has a proportional limit of 4.5 MPa or more, an increase in output is expected. The separator may have a proportional limit of, for example, 6.2 MPa or more.

[0077] (Method for determining proportional limit)

[0078] The proportional limit of the present embodiment is determined in a compression test in the thickness direction of the separator. First, prepare a test piece. Recover the electrode body 50 from the battery 100. Recover the separator from the electrode body 50. Cut a test piece from the separator. As for the test piece, it is recovered from the portion of the electrode body 50 corresponding to the curved portion 53. The portion corresponding to the flat portion 54 may undergo physical property changes due to the influence of the molding pressure. In addition, counting from the center of the electrode body 50, a test piece is taken from the outer portion of the 30th layer. The test piece is set to a rectangle with a length of one side of more than 1 cm (the test piece is set to be larger than the plane size of the indenter described later). Prepare 172 test pieces. 172 test pieces can be collected from a battery pack with the same specifications.

[0079] Prepare a compression tester. For example, Autograph "AG-50kNG W975" manufactured by Shimadzu Corporation can be used. A tester having equivalent functions can also be used.

[0080] The indenter is mounted on a compression tester. The indenter is a block made of stainless steel (SUS) and has a planar size of 1 cm×1 cm.

[0081] 172 test pieces were stacked to form a stacked body. The stacked body was placed on a sample stand of a compression tester. The indenter was pressed into the stacked body along the stacking direction of the stacked body (i.e., the thickness direction of the separator).

[0082] Manually press the indenter into the laminate until the compressive stress reaches 75N (0.075MPa). After the compressive stress reaches 75N, continue to press the indenter in such a way that the rate of increase of the compressive stress becomes 666.5N / s (0.6665MPa / s). At the moment when the compressive stress reaches 1500N (1.5MPa), stop pressing the indenter. Through the above operation, a stress-strain curve is obtained. In the stress-strain curve, the limit of stress at which the proportional relationship between stress and strain (Hooke's law) is established is determined. The proportional limit is valid to the first decimal place. Round off the decimal places below the second place.

[0083] In the stress-strain curve, the elastic modulus can be calculated based on the slope of the region where stress and strain have a proportional relationship. The separator can have an elastic modulus of, for example, 180 MPa to 210 MPa. The separator can have an elastic modulus of, for example, 188 MPa to 208 MPa.

[0084] Positive Plate

[0085] Figure 4 It is a schematic plan view showing an example of a positive electrode plate in this embodiment.

[0086] The positive electrode plate 10 is a strip-shaped sheet. The positive electrode plate 10 may have a thickness of, for example, 10 μm to 100 μm. The positive electrode plate 10 may have a thickness of, for example, 81 μm or less. The positive electrode plate 10 has a thickness of 81 μm or less, which tends to be less prone to molding relaxation. The positive electrode plate 10 may have a thickness of, for example, 50 μm to 81 μm. The positive electrode plate 10 may have a thickness of, for example, 50 μm to 75 μm. The positive electrode plate 10 may have a thickness of, for example, 75 μm to 81 μm.

[0087] The positive electrode plate 10 includes a positive electrode substrate 11 and a positive electrode active material layer 12. The positive electrode substrate 11 may be, for example, an aluminum (Al) alloy foil or the like. The positive electrode substrate 11 may have, for example, a thickness of 10 μm to 20 μm. The positive electrode active material layer 12 is arranged on the surface of the positive electrode substrate 11. The positive electrode active material layer 12 may be arranged only on one side of the positive electrode substrate 11. The positive electrode active material layer 12 may also be arranged on both the front and back sides of the positive electrode substrate 11. A portion of the positive electrode substrate 11 is exposed from the positive electrode active material layer 12. The exposed portion of the positive electrode substrate 11 is hereinafter also referred to as "positive electrode substrate exposed portion". The positive electrode substrate exposed portion is arranged in the horizontal direction ( Figure 4 The exposed portion of the positive electrode substrate is in the longitudinal direction ( Figure 4 The exposed portion of the positive electrode substrate can be used to connect the electrode body 50 and the positive electrode terminal 91.

[0088] The positive electrode active material layer 12 may have a thickness of 2 g / cm 3 Up to 3g / cm 3 The positive electrode active material layer 12 may have a density of, for example, 2.4 g / cm 3 Up to 2.6g / cm 3 The positive electrode active material layer 12 contains a positive electrode active material. The positive electrode active material layer 12 can be basically composed of a positive electrode active material.

[0089] The positive electrode active material may contain any component. For example, the positive electrode active material may contain at least one selected from LiCoO2, LiNiO2, LiMnO2, LiMn2O4, Li(NiCoMn)O2, Li(NiCoAl)O2, and LiFePO4. Among them, for example, the record of "(NiCoMn)" in the composition formula such as "Li(NiCoMn)O2" indicates that the total of the composition ratio in the brackets is 1. In addition to the positive electrode active material, the positive electrode active material layer 12 may further include a conductive material and a binder, etc. The conductive material may contain any component. The conductive material may include acetylene black, etc., for example. In terms of the amount of the conductive material, it may be, for example, 0.1 to 10 parts by mass relative to 100 parts by mass of the positive electrode active material. The binder may contain any component. The binder may include, for example, polyvinylidene fluoride (PVDF), etc. The amount of the binder to be blended may be, for example, 0.1 parts by mass to 10 parts by mass relative to 100 parts by mass of the positive electrode active material.

[0090] Negative Plate

[0091] Figure 5 It is a schematic plan view showing an example of a negative electrode plate in this embodiment.

[0092] The negative electrode plate 20 is a strip-shaped sheet. The negative electrode plate 20 may have a thickness of, for example, 10 μm to 100 μm. The negative electrode plate 20 may have a thickness of, for example, 83 μm or less. The negative electrode plate 20 has a thickness of 83 μm or less, which tends to be less prone to molding relaxation. The negative electrode plate 20 may have a thickness of, for example, 57 μm to 83 μm. The negative electrode plate 20 may have a thickness of, for example, 57 μm to 76 μm. The negative electrode plate 20 may have a thickness of, for example, 76 μm to 83 μm.

[0093] The negative electrode plate 20 includes a negative electrode substrate 21 and a negative electrode active material layer 22. The negative electrode substrate 21 may be, for example, a copper (Cu) alloy foil or the like. The negative electrode substrate 21 may have, for example, a thickness of 5 μm to 10 μm. The negative electrode active material layer 22 is arranged on the surface of the negative electrode substrate 21. The negative electrode active material layer 22 may be arranged only on one side of the negative electrode substrate 21. The negative electrode active material layer 22 may also be arranged on both the front and back sides of the negative electrode substrate 21. A portion of the negative electrode substrate 21 is exposed from the negative electrode active material layer 22. The exposed portion of the negative electrode substrate 21 is hereinafter referred to as "negative electrode substrate exposed portion". The negative electrode substrate exposed portion is arranged in the horizontal direction ( Figure 5 The exposed portion of the negative electrode substrate is in the longitudinal direction ( Figure 5 The exposed portion of the negative electrode substrate can be used for connection between the electrode body 50 and the negative electrode terminal 92.

[0094] The negative electrode active material layer 22 may have a thickness of, for example, 1.05 g / cm 3 Up to 1.2g / cm3 The negative electrode active material layer 22 may have a density of, for example, 1.1 g / cm 3 Up to 1.12g / cm 3 The negative electrode active material layer 22 contains a negative electrode active material. The negative electrode active material layer 22 may be substantially composed of a negative electrode active material.

[0095] The negative electrode active material may contain any component. For example, the negative electrode active material may contain a material selected from graphite, soft carbon, hard carbon, silicon, silicon oxide, silicon-based alloy, tin, tin oxide, tin-based alloy, and Li4Ti5O 12 At least one of. In addition to the negative electrode active material, the negative electrode active material layer 22 may further include, for example, a conductive material and a binder. The conductive material may include any component. The conductive material may include, for example, at least one selected from acetylene black, vapor-grown carbon fiber, and carbon nanotubes. In terms of the amount of the conductive material, it may be, for example, 0.1 to 10 parts by mass relative to 100 parts by mass of the negative electrode active material. The binder may include any component. The binder may include, for example, at least one selected from styrene butadiene rubber (SBR), carboxymethyl cellulose (CMC), and polyacrylic acid (PAA). In terms of the amount of the binder, it may be, for example, 0.1 to 10 parts by mass relative to 100 parts by mass of the negative electrode active material.

[0096] Electrolyte

[0097] At least a portion of the electrolyte is impregnated in the electrode body 50. The entire electrolyte may be impregnated in the electrode body 50. A portion of the electrolyte may also be impregnated in the electrode body 50. A portion of the electrolyte may be stored outside the electrode body 50. The electrolyte is a liquid electrolyte. The electrolyte contains a solvent and a supporting electrolyte. The solvent is aprotic. The solvent may contain any component. For example, the solvent may contain at least one selected from ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC) and diethyl carbonate (DEC). The supporting electrolyte is dissolved in the solvent. The supporting electrolyte may contain any component. For example, the supporting electrolyte may contain at least one selected from LiPF6, LiBF4, LiN(FSO2)2 and LiB(C2O4)2. In addition to the solvent and the supporting electrolyte, the electrolyte may further contain any additives.

[0098] <Battery pack>

[0099] Fig.10 This is a schematic diagram showing an example of a battery pack in this embodiment.

[0100] The assembled battery 300 includes one or more single cells 310 and a casing. The single cells 310 are the non-aqueous electrolyte secondary batteries of the present embodiment described above. The assembled battery 300 may include, for example, 1 to 100 single cells 310. The assembled battery 300 may include, for example, 2 to 20 single cells 310. When the assembled battery 300 includes a plurality of single cells 310, the plurality of single cells 310 are arranged in a predetermined direction. Fig.10 In the embodiment, a plurality of cells 310 are arranged in the y-axis direction. The direction in which the cells 310 are arranged is also referred to as the "arrangement direction". A plurality of cells 310 may be electrically connected in series. A plurality of cells 310 may also be electrically connected in parallel. A group of electrically connected cells 310 is also referred to as a "battery module".

[0101] The housing includes, for example, a storage box (not shown) and a restraining member 320. The storage box accommodates the single cell 310 and the restraining member 320. The restraining member 320 includes, for example, two end plates 321 and a belt 322. The end plates 321 are respectively arranged at both ends of the arrangement direction. The belt 322 connects the two end plates 321 to each other so that the distance between the two end plates 321 converges within a predetermined range. Thus, the single cell 310 clamped between the two end plates 321 is restrained. That is, the restraining member 320 restrains the single cell 310.

[0102] The restraining member 320 in this embodiment may be formed of a material with low rigidity. This is because the single cell 310 can exhibit a small reaction force. The restraining member may be made of, for example, a resin material. For example, at least one of the end plate 321 and the belt 322 may be made of a resin material.

[0103] Example

[0104] Hereinafter, an embodiment of the present disclosure (hereinafter also referred to as "this embodiment") will be described. However, the following description does not limit the claims.

[0105] <Manufacturing of test batteries>

[0106] No.1

[0107] The test cell of this example was manufactured by the following steps.

[0108] The positive electrode active material [Li(NiCoMn)O2], the conductive material (acetylene black), the binder (PVDF) and the dispersion medium (N-methyl-2-pyrrolidone) are mixed to prepare a positive electrode slurry. The positive electrode slurry is applied to the surface of the positive electrode substrate (Al alloy foil, thickness 15 μm) and dried to form a positive electrode active material layer. Thus, the original positive electrode is manufactured. The original positive electrode is compressed and cut into a specified size to manufacture a positive electrode plate. The positive electrode plate has the following planar dimensions.

[0109] Width of exposed portion of positive electrode substrate (W11 , reference Figure 4 ): 10mm

[0110] The width of the positive electrode active material layer (W 12 , reference Figure 4 ): 110mm

[0111] The negative electrode active material (natural graphite), binder (CMC, SBR) and dispersion medium (water) are mixed to prepare the negative electrode slurry. The negative electrode slurry is applied to the surface of the negative electrode substrate (Cu alloy foil, thickness 8 μm) and dried to form a negative electrode active material layer. The original negative electrode is thus manufactured. The original negative electrode is compressed and cut into a specified size to manufacture a negative electrode plate. The negative electrode plate has the following planar dimensions.

[0112] The width of the exposed portion of the negative electrode substrate (W 21 , reference Figure 5 ): 13mm

[0113] The width of the negative electrode active material layer (W 22 , reference Figure 5 ): 115mm

[0114] Prepare the first separator and the second separator. The first separator and the second separator of this embodiment have the same specifications. The physical property values ​​of the separators are shown in Table 1 below. In addition, the "proportional limit" in Table 1 below is a value measured using the separator recovered from the battery after measuring the output and the reaction force.

[0115] The first separator, the positive electrode plate, the second separator and the negative electrode plate are stacked in sequence to form a stack. The stack is wound into a spiral shape to form a cylindrical electrode body. The cylindrical electrode body is extruded in the radial direction using a flat plate press. Thus, the electrode body is formed into a flat shape. In the electrode body, the number of stacking layers of the negative electrode plate is set to 2 more than the number of stacking layers of the positive electrode plate. The total number of stacking layers of the first separator and the second separator is set to 8 more than twice the number of stacking layers of the positive electrode plate.

[0116] An outer package was prepared. The outer package was in a square shape. The outer package was made of Al alloy. The dimensions of the outer package are shown in Table 1 below. The "outer dimensions" in Table 1 below represent Figure 1 The "thickness" in the following Table 1 indicates the thickness (plate thickness) of the outer packaging material.

[0117] The outer packaging body is composed of a container and a cover. A positive terminal and a negative terminal are provided on the cover. The positive terminal is electrically connected to the electrode body through the positive electrode collector. The negative terminal is electrically connected to the electrode body through the negative electrode collector. The electrode body is inserted into a bag-shaped bracket. The bracket is formed of a resin film (material PP, thickness 0.15 mm). The electrode body and the bracket are housed in a container together. The cover and the container are joined by laser welding. The electrolyte is injected into the outer packaging body from the injection hole provided in the cover. The electrode body is impregnated with the electrolyte. The electrolyte contains the following components.

[0118] Solvent: EC / EMC / DEC=3 / 3 / 4 (volume ratio)

[0119] Supporting electrolyte: LiPF6 (concentration 1 mol / L)

[0120] The battery is manufactured by the above operation. After the electrolyte is injected, the battery is charged to a predetermined amount with the injection hole opened. During charging, the gas generated from the electrode body is discharged from the injection hole. After charging, the injection hole is plugged with a sealing plug.

[0121] "No.2 to No.12"

[0122] Test cells were produced in the same manner as in No. 1 except that the ratio limit of the separator and the number of positive electrode plates stacked were changed as shown in Table 1. The "air permeability" in Table 1 is a relative value when the air permeability of the separator in No. 1 is defined as 100%.

[0123] <Evaluation>

[0124] Determination of reaction force

[0125] Figure 6 This is a schematic diagram showing a method for measuring the reaction force.

[0126] Prepare a pressing jig 200. The pressing jig 200 includes a first plate 201, a second plate 202, a third plate 203, a fourth plate 204, a bolt 205, and a nut 206. Each plate may be made of SUS, for example. Each plate may have a thickness of, for example, 13 mm or more. A protrusion is formed on the surface of the first plate 201 and the second plate 202. The protrusion has a height of 2 mm. The bolt 205 penetrates the first plate 201, the second plate 202, the third plate 203, and the fourth plate 204. The first plate 201, the second plate 202, the third plate 203, and the fourth plate 204 are fastened by the bolt 205 and the nut 206. A load cell 210 is arranged between the third plate 203 and the fourth plate 204. The load cell 210 may be, for example, a model "CMP1-2T" manufactured by MinebeaMitsumi Inc. A load sensor having the same function as this device may also be used. The battery 100 is clamped by the first plate 201 and the second plate 202. That is, the battery 100 is constrained. The first plate 201 and the second plate 202 are fixed in such a manner that the outer dimensions of the battery 100 (the outer dimensions in the y-axis direction) become predetermined values, thereby outputting pressure to the load sensor 210. This pressure is regarded as a "reaction force (F)". The load sensor 210 is arranged in the horizontal direction relative to the battery 100 in such a manner that the weight of the compression jig 200 does not affect the value of the reaction force.

[0127] The outer dimensions of the battery 100 when the first plate 201 and the second plate 202 are fixed are also referred to as “constraint dimensions (D)”. The restraint dimensions of this embodiment are about 0.1 mm smaller than the original outer dimensions of the outer package.

[0128] After the battery 100 is constrained by the first plate 201 and the second plate 202, the battery 100 is charged from 3.4V to 4.2V by constant current (CC) charging of 1It. After reaching 4.2V, the battery 100 is charged for 15 minutes by constant voltage (CV) charging. The battery is thus fully charged. After charging, the reaction force is measured. The reaction force is shown in the following Table 1. It should be noted that "It" is a symbol indicating the hourly rate of current. Using a current of 1It, the full charge capacity is discharged in 1 hour.

[0129] 《Measurement of output》

[0130] The battery was charged to 3.699V in 90 minutes by constant current-constant voltage (CC-CV) charging at 25°C. After charging, the battery was rested for 10 minutes and discharged at a current of 40A for 10 seconds. The output was calculated according to the following equations (6) and (7). The output is shown in Table 1 below. The output in Table 1 below is a relative value when the output of No. 1 is defined as 100%.

[0131] Ip =40×(V0-3) / (V0-V 10 ) (6)

[0132] Q=3×I p (7)

[0133] “I p ” indicates the current when the voltage reaches 3V after 10 seconds of discharge.

[0134] "V0" indicates the voltage at the start of discharge.

[0135] “V 10 ” indicates the voltage when 10 seconds have passed from the start of discharge.

[0136]

[0137] <Results>

[0138] 《Relationship between the proportional limit of a separator and the reaction force》

[0139] Figure 7 Graph showing the relationship between the proportional limit of the separator and the reaction force.

[0140] exist Figure 7 The results of No. 1 to No. 5 and No. 12 are shown in FIG. 1. When the proportional limit of the separator is 10.2 MPa or less, the reaction force is significantly reduced. When the proportional limit is 9.7 MPa or less, the reaction force gradually decreases as the proportional limit decreases.

[0141] When the proportional limit was 10.7 MPa (No. 12), the reaction force became extremely large, and it is considered that molding relaxation occurred.

[0142] 《Relationship between the proportional limit of the separator and the output》

[0143] Figure 8 is a graph showing the relationship between the proportional limit of the separator and the output.

[0144] exist Figure 8 The results of No. 1 to No. 5 and No. 12 are shown in FIG. 1. As the proportional limit increases, the output tends to increase gradually. When the proportional limit is 4.5 MPa or more, the output is expected to increase.

[0145] 《Relationship between the number of positive plate layers and reaction force》

[0146] Fig. 9 It is a graph showing the relationship between the number of stacked positive electrode plates and the reaction force.

[0147] exist Fig. 9The results of No. 1, No. 4, No. 6 to No. 9 are shown in FIG. 1. It was found that the more the number of positive electrode plates stacked, the greater the reaction force. In addition, it was found that the smaller the proportional limit, the smaller the reaction force.

[0148] The first curve (C1) reflects the result when the proportional limit is 9.7 MPa. The second curve (C2) reflects the result when the proportional limit is 6.2 MPa. The difference (C1-C2) between the first curve (C1) and the second curve (C2) increases as the number of stacking increases. In other words, it is believed that the reduction in the reaction force due to the adjustment of the proportional limit increases as the number of stacking increases.

[0149] In the range where the number of stacked layers is 54 or more, the difference (C1-C2) is large. Therefore, in the range where the number of stacked layers is 54 or more, it is expected that the reduction of the reaction force will be greater. However, if the number of stacked layers exceeds 110, for example, when welding the electrode body and the positive electrode current collector, poor welding may occur.

[0150] The present embodiment and the present example are illustrative in all respects. The present embodiment and the present example are not restrictive. For example, it is also possible to extract any configuration from the present embodiment and the present example and to combine them arbitrarily as originally intended.

[0151] The technical scope determined by the description of the claims includes all modifications within the meaning equivalent to the description of the claims. Furthermore, the technical scope determined by the description of the claims also includes all modifications within the scope equivalent to the description of the claims.

Claims

1. A non-aqueous electrolyte secondary battery, comprising an outer packaging body, an electrode body and an electrolyte, wherein the outer packaging body contains the electrode body and the electrolyte, the electrode body is formed into a flat shape, the electrode body comprises a laminate, the laminate comprises a first separator, a positive electrode plate, a second separator and a negative electrode plate, the first separator, the positive electrode plate, the second separator and the negative electrode plate are sequentially laminated, the electrode body is formed by winding the laminate into a spiral shape, the first separator and the second separator each have a proportional limit of 4.5 MPa or more and 10.2 MPa or less, the proportional limit being measured in a compression test in a thickness direction of the first separator and the second separator, The first separator and the second separator respectively include a porous sheet made of polyolefin and a ceramic particle layer, wherein the ceramic particle layer is formed on the surface of the porous sheet and the ceramic particle layer is in direct contact with the surface of the positive electrode plate or the negative electrode plate. In a cross section perpendicular to the winding axis of the electrode body, the electrode body includes a curved portion and a flat portion, wherein the positive electrode plate has a curved surface in the curved portion, and the positive electrode plate has a flat surface in the flat portion, and 54 or more and 110 or less layers of the positive electrode plates are stacked in the flat portion, At the center of the electrode body, a fold is formed in the first separator and the second separator, and as the deformation of the first separator and the second separator decreases from the center of the electrode body toward the outside, the fold disappears to form the curved portion, wherein the center of the electrode body refers to the inner layer side stack of the electrode body, and the outside of the electrode body refers to the outer layer side stack of the electrode body.

2. The nonaqueous electrolyte secondary battery according to claim 1, wherein In the laminate, the following relationship (1) is satisfied: x+y+z≤210 (1) In the formula (1), x represents the thickness of the positive electrode plate, y represents the thickness of the negative electrode plate, and z represents the total thickness of the first separator and the second separator. The unit of thickness here is μm.

3. A battery pack comprising a casing and one or more single cells, wherein the single cells are the nonaqueous electrolyte secondary batteries according to claim 1 or 2, wherein the casing comprises a restraining member, the restraining member restrains the single cells, and the restraining member is made of a resin material.