Separator for lithium secondary battery having improved electrode adhesion strength and resistance characteristics, and lithium secondary battery including the separator for lithium secondary battery
By forming a porous coating of inorganic particles on the lithium secondary battery separator and adjusting the binder combination, the safety and resistance characteristics of the lithium secondary battery separator at high temperatures are solved, and the excellent adhesion and resistance of the electrode are achieved. The combination of characteristics improves the overall performance of the battery.
Patent Information
- Application Number
- CN202080054315.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-10-29
AI Technical Summary
Existing lithium secondary battery separators have safety issues due to thermal shrinkage at high temperatures, and there is a trade-off between the adhesion and resistance characteristics of PVDF-based polymers, making it difficult to meet the adhesion and resistance characteristics requirements of electrodes at the same time.
By forming a porous coating including inorganic particles on a porous polymer substrate, adjusting the viscosity and elastic rheological properties of the adhesive, using various types of adhesives such as PVDF-TFE, PVDF-HFP and PVDF-CTFE, combined A third adhesive is used to optimize the combination of adhesives to form separators with excellent adhesion and resistance properties.
It achieves both excellent adhesion and resistance characteristics of the electrode, improves the life, safety and high output characteristics of the lithium secondary battery, and avoids the risk of short circuit caused by separation of the electrode and separator.
Smart Images

Figure CN114175386B_ABST
Abstract
Description
Technical Field
[0001] This application claims priority to Korean Patent Application No. 10-2019-0135852 filed in Korea on October 29, 2019. The present disclosure relates to a separator for a lithium secondary battery having improved adhesion and resistance characteristics to an electrode, and a lithium secondary battery including the separator for a lithium secondary battery. Background Art
[0002] Lithium secondary battery is an energy storage device with a basic structure of positive electrode / negative electrode / separator / electrolyte, and is an electrochemical device that can be charged / discharged by reversible conversion between chemical energy and electrical energy and shows high energy density. These lithium secondary batteries are widely used in compact electronic devices, such as mobile phones, notebook computers or the like. Recently, the application of lithium secondary batteries has been rapidly expanded to hybrid electric vehicles (HEV), plug-in electric vehicles (plug-in EV), electric bicycles (e-bike), and energy storage systems (ESS) as a countermeasure for environmental problems, high oil prices, energy efficiency and energy storage.
[0003] Ensuring safety is an important issue to be solved in manufacturing and using these lithium secondary batteries. Specifically, the separators (separators) commonly used in lithium secondary batteries show severe thermal shrinkage behavior at high temperatures or under other conditions during their manufacturing process due to their material properties and characteristics, resulting in safety-related problems such as internal short circuits. Recently, an organic-inorganic composite porous separator has been proposed, which has a porous inorganic coating formed by coating a mixture of inorganic particles and a binder on a porous polymer substrate to ensure the safety of the lithium secondary battery. However, when an electrode assembly is formed by stacking electrodes and separators, interlayer adhesion is insufficient. Therefore, it is very likely that the electrode and separator are separated from each other. In this case, there is a problem that the inorganic particles detached during this separation may act as local defects in the device.
[0004] To solve the above-mentioned problem, a method of forming an adhesion layer has been used, in which a binder polymer is induced to migrate toward the surface of the separator through phase separation of a PVDF-based polymer such as poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP) or poly(vinylidene fluoride-co-chlorotrifluoroethylene) (PVDF-CTFE), so that the coating of the separator can have adhesion.
[0005] It is known that when such PVDF-based polymers are used in the adhesive layer of the separator, the adhesion of the PVDF-based polymer and its resistance characteristics have a trade-off relationship. That is, it is known that a PVDF-based polymer having excellent adhesion is disadvantageous in terms of resistance, while a PVDF-based polymer having superior resistance characteristics is disadvantageous in terms of adhesion. Summary of the invention
[0006] Technical issues
[0007] The present disclosure is designed to solve the problems of the prior art, and thus the present disclosure is directed to providing a separator for a lithium secondary battery having a porous coating layer including inorganic particles and having adhesion and resistance characteristics to an electrode simultaneously improved to a level sufficient to meet the requirements of the art.
[0008] The present disclosure is directed to providing a separator for a lithium secondary battery which satisfies both adhesion to an electrode and resistance characteristics by adjusting rheological properties such as viscosity and elasticity of a binder used for a porous coating layer.
[0009] These and other inventive purposes and advantages of the present disclosure can be understood from the following detailed description and become more fully apparent from the exemplary embodiments of the present disclosure. In addition, it is to be readily understood that the aspects of the present disclosure and advantages can be achieved by the means and methods and combinations thereof shown in the appended claims.
[0010] Technical Solution
[0011] According to a first embodiment of the present disclosure, there is provided a separator for a lithium secondary battery, including: a porous polymer substrate; and a porous coating layer formed on at least one surface of the porous polymer substrate and including a binder mixed with inorganic particles,
[0012] wherein the binder binds the inorganic particles to each other so that the inorganic particles can maintain their bonded state, and binds the inorganic particles to the porous polymer substrate so that the inorganic particles and the porous polymer substrate maintain their bonded state,
[0013] The inorganic particles form interstitial volumes while being substantially in contact with each other, and the interstitial volumes between the inorganic particles become vacant spaces to form pores of the porous coating layer, and
[0014] When the adhesive is pressurized at 190° C. to form an adhesive sample having a thickness of 0.4 mm, as measured by dynamic mechanical analysis (DMA), the adhesive sample includes a first adhesive having a tan δ peak at 15° C. to 27.6° C. and a second adhesive having a tan δ peak at 8° C. to 20.2° C.
[0015] According to a second embodiment of the present disclosure, there is provided a separator for a lithium secondary battery as defined in the first embodiment, wherein the binder of the porous coating layer includes the first binder and the second binder.
[0016] According to a third embodiment of the present disclosure, a separator for a lithium secondary battery as defined in the first embodiment or the second embodiment is provided, wherein the adhesive further includes a third adhesive, and when the third adhesive is pressurized at 190° C. to form an adhesive sample having a thickness of 0.4 mm, the adhesive sample has a tan δ peak at −12° C. to 0° C. as measured by dynamic mechanical analysis (DMA).
[0017] According to a fourth embodiment of the present disclosure, there is provided a separator for a lithium secondary battery as defined in the third embodiment, wherein the third binder is present in an amount of 8 wt % to 25 wt % based on 100 wt % of the total weight of the first binder, the second binder and the third binder.
[0018] According to a fifth embodiment of the present disclosure, there is provided a separator for a lithium secondary battery as defined in the third embodiment or the fourth embodiment, wherein the third binder includes PVDF-CTFE.
[0019] According to a sixth embodiment of the present disclosure, a separator for a lithium secondary battery as defined in any one of the first to fifth embodiments is provided, wherein the first adhesive is present in an amount of 5 wt % to 50 wt %, and the second adhesive is present in an amount of 50 wt % to 95 wt %, based on 100 wt % of the total weight of the first adhesive and the second adhesive.
[0020] According to a seventh embodiment of the present disclosure, a separator for a lithium secondary battery as defined in any one of the first to sixth embodiments is provided, wherein when the first adhesive is pressurized at 190° C. to form an adhesive sample having a thickness of 0.4 mm, the adhesive sample exhibits a behavior of a phase angle of less than 45° as measured by an Advanced Rheometric Expansion System (ARES) at 190° C.
[0021] According to an eighth embodiment of the present disclosure, a separator for a lithium secondary battery as defined in any one of the first to seventh embodiments is provided, wherein when the second adhesive is pressurized at 190° C. to form an adhesive sample having a thickness of 0.4 mm, the adhesive sample exhibits a behavior with a phase angle of 45° or greater as measured by an Advanced Rheological Expansion System (ARES) at 190° C.
[0022] According to a ninth embodiment of the present disclosure, a separator for a lithium secondary battery as defined in any one of the first to eighth embodiments is provided, wherein the first binder is present in an amount of 5 wt % to 15 wt %, and the second binder is present in an amount of 85 wt % to 95 wt %, based on 100 wt % of the total weight of the first binder and the second binder.
[0023] According to a tenth embodiment of the present disclosure, a separator for a lithium secondary battery as defined in any one of the first to ninth embodiments is provided, wherein the first binder satisfying the tan δ peak condition is poly(vinylidene fluoride-tetrafluoroethylene) (PVDF-TFE), poly(vinylidene fluoride-trifluoroethylene) (PVDF-TrFE), PVDF-HFP-acrylic acid graft copolymer (PVDF-HFP-acrylic acid graft copolymer, PVDF-HFP-AA), or a mixture thereof.
[0024] According to an eleventh embodiment of the present disclosure, there is provided a separator for a lithium secondary battery as defined in any one of the first to tenth embodiments, wherein the second binder satisfying the tan δ peak condition is poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP).
[0025] According to a twelfth embodiment of the present disclosure, there is provided a separator for a lithium secondary battery as defined in any one of the first to eleventh embodiments, wherein the porous coating layer further includes a dispersant.
[0026] In another aspect, according to a thirteenth embodiment of the present disclosure, there is provided a lithium secondary battery comprising a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein the separator is a separator for a lithium secondary battery as defined in any one of the first to twelfth embodiments.
[0027] Beneficial Effects
[0028] The separator for a lithium secondary battery according to the present disclosure uses two types of binders as binders for the porous coating layer, thereby making it possible to achieve preferred rheological properties such as viscosity and elasticity, and thus to satisfy both adhesion to an electrode and resistance characteristics.
[0029] Besides, fine and uniform pores are formed on the surface of the separator for a lithium secondary battery according to the present disclosure to provide an increased adhesion surface area to the electrode, resulting in improved adhesion to the electrode.
[0030] Further, a lithium secondary battery including the separator for a lithium secondary battery according to the present disclosure exhibits excellent lifespan, safety, and high output characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The accompanying drawings illustrate preferred embodiments of the present disclosure and are used together with the following disclosure to provide a further understanding of the technical features of the present disclosure, and therefore, the present disclosure should not be interpreted as being limited to the drawings. At the same time, the shapes, sizes, scales, or proportions of some components in the drawings may be exaggerated for the purpose of a clearer description.
[0032] Figure 1 is a graph illustrating the relationship between temperature and tan δ for each of the first adhesive and the second adhesive used in Example 1 and Example 2 as determined by Dynamic Mechanical Analysis (DMA).
[0033] Figure 2 : is a graph illustrating the relationship between the complex modulus and the phase angle at 190° C. measured for each of the first adhesive and the second adhesive used in Example 1 and Example 2.
[0034] Figure 3 1 is a graph illustrating the relationship between the angular frequency and the complex viscosity at 190° C. measured for each of the first adhesive and the second adhesive used in Example 1 and Example 2.
[0035] Figure 4: is a graph illustrating the relationship between temperature and storage modulus and the relationship between temperature and loss modulus measured for each of the first adhesive and the second adhesive used in Example 1 and Example 2.
[0036] Figure 5 and Figure 6 Scanning electron microscopic (SEM) images respectively illustrating a cross section of a separator for a lithium secondary battery according to Example 1 and a cross section of a separator according to Comparative Example 1 are shown.
[0037] Figure 7 is a graph illustrating the relationship between temperature and tan δ for the third adhesive used in each of Examples 3 to 6 as determined by Dynamic Mechanical Analysis (DMA). DETAILED DESCRIPTION
[0038] Hereinafter, preferred embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. Before the description, it should be understood that the terms used in the specification and the accompanying claims should not be interpreted as being limited to the common meaning and dictionary meaning, but should be interpreted based on the meaning and concept of the technical aspects of the corresponding present disclosure on the basis of the principle that the inventor is allowed to appropriately define the terms for the best interpretation. Therefore, the descriptions presented herein are only preferred examples for illustrative purposes and are not intended to limit the scope of the present disclosure, so it should be understood that other equivalents and improvements may be made thereto without departing from the scope of the present disclosure.
[0039] In one aspect of the present disclosure, a separator for a lithium secondary battery is provided, comprising: a porous polymer substrate; and a porous coating layer formed on at least one surface of the porous polymer substrate and comprising an adhesive mixed with inorganic particles, wherein the adhesive bonds the inorganic particles to each other so that the inorganic particles can maintain their combined state, and bonds the inorganic particles to the porous polymer substrate so that the inorganic particles and the porous polymer substrate can maintain their combined state, the inorganic particles form an interstitial volume while being substantially in contact with each other, and the interstitial volume between the inorganic particles becomes a vacant space to form pores of the porous coating layer, and when the adhesive is pressurized at 190° C. to form an adhesive sample with a thickness of 0.4 mm, as determined by dynamic mechanical analysis (DMA), the adhesive sample comprises a first adhesive having a tan δ peak at 15° C. to 27.6° C. and a second adhesive having a tan δ peak at 8° C. to 20.2° C.
[0040] In another aspect of the present disclosure, a lithium secondary battery is provided, including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein the separator is a separator for a lithium secondary battery according to an embodiment of the present disclosure.
[0041] Hereinafter, each constituent element will be explained in more detail.
[0042] 1. Porous polymer substrate
[0043] According to an embodiment of the present disclosure, the porous polymer substrate provides a lithium ion transmission channel while electrically insulating the negative electrode and the positive electrode from each other to prevent short circuit. Any material can be used without particular limitation as long as it is conventionally used as a material for a separator of a lithium secondary battery. Specific examples of porous polymer substrates include porous polymer substrates made of at least one polymer resin selected from polyolefins, polyethylene terephthalate, polybutylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide, and polyethylene naphthalate, but are not limited thereto.
[0044] Besides, the porous polymer substrate may be a sheet-like film formed by melting the polymer resin. Preferably, the porous polymer substrate is a porous polymer substrate provided in the form of a sheet-like film formed by melting the above-mentioned polymer resin.
[0045] Specifically, the porous polymer substrate may be any one of the following a) to c):
[0046] a) a porous membrane formed by melting and extruding a polymer resin;
[0047] b) a multilayer film formed by stacking two or more layers of the porous films of a); and
[0048] c) A porous composite membrane having a multilayer structure including both a) and b).
[0049] According to an embodiment of the present disclosure, the porous polymer substrate may have a thickness of 5 μm to 50 μm. The thickness of the porous polymer substrate is not limited to the range defined above. However, when the thickness is excessively less than the lower limit defined above, the separator exhibits poor mechanical properties and may be easily damaged during the use of the battery. At the same time, the size of the pores present in the porous polymer substrate and its porosity are not particularly limited, but may be 0.01 μm to 50 μm and 10% to 95%, respectively.
[0050] 2. Porous coating
[0051] According to an embodiment of the present disclosure, a porous coating is formed on one or both surfaces of a porous polymer substrate. The porous coating includes a mixture of multiple inorganic particles and a binder polymer, and the inorganic particles are combined to form a layer by the binder polymer. The binder of the porous coating allows the inorganic particles to adhere to each other to maintain their binding state (that is, the inorganic particles are connected to each other and fixed by the binder). In addition, the inorganic particles can maintain their binding state for the porous polymer substrate by the binder. The inorganic particles in the porous coating form interstitial volume while substantially contacting each other. Herein, interstitial volume refers to the space defined by the inorganic particles that are substantially facing each other in the close packing or dense packing (closed packed or densely packed) structure of the inorganic particles. The interstitial volume between the inorganic particles becomes a vacant space to form the pores of the porous coating.
[0052] When the surface of the porous polymer substrate is coated with a porous coating layer including inorganic particles as described above, heat resistance and mechanical properties can be further improved. That is, since the physical properties of the inorganic particles generally do not change even at a high temperature of 200° C., the separator for a lithium secondary battery has excellent heat resistance due to the porous coating layer.
[0053] According to an embodiment of the present disclosure, the porous coating layer has a thickness of 1 μm to 50 μm, 2 μm to 30 μm, or 2 μm to 20 μm. When the porous coating layer has a thickness within the above defined range, the separator can be formed into a thin film and can provide low resistance characteristics and high heat resistance.
[0054] The weight ratio of inorganic particles to binder polymer in the porous coating is determined taking into account the thickness, pore size and porosity of the finished porous coating. According to an embodiment of the present disclosure, inorganic particles are used in an amount of 50wt% to 99.9wt% or 60wt% to 99.5wt%, and binder polymers are used in an amount of 0.1wt% to 50wt% or 0.5wt% to 40wt%. When the content of inorganic particles is less than 50wt%, the quality of the finished battery may be reduced due to the excessive content of the binder polymer, the reduction of the vacant space formed between the inorganic particles, and the reduction of the pore size and porosity. In contrast, when the content of inorganic particles is greater than 99.9wt%, the mechanical properties of the finished porous coating may be reduced due to the low content of the binder polymer and the reduction of the adhesion between the inorganic particles.
[0055] When the adhesive for the porous coating of the lithium secondary battery according to the present disclosure is pressurized at 190°C to form an adhesive sample with a thickness of 0.4 mm, as determined by dynamic mechanical analysis (DMA), the adhesive sample includes a first adhesive having a tan δ peak at 15°C to 27.6°C and a second adhesive having a tan δ peak at 8°C to 20.2°C. Herein, DMA is implemented by using DMA Q800 available from TA Instruments. In addition, the term "peak" used herein refers to a vertex, i.e., a point with a maximum height in a curve (curve) plotting the relationship between tan δ and temperature. Alternatively, "peak" may refer to an inflection point where the slope of the tangent line of the curve changes from a positive (+) value to a negative (-) value.
[0056] According to the present disclosure, the first adhesive generally tends to exhibit a large change in viscosity with temperature, high elasticity, low solubility in solvents, and solid-like rigid properties.
[0057] According to the present disclosure, the first adhesive satisfying the above-defined tan δ peak condition may be PVDF-TFE, PVDF-TrFE, PVDF-HFP-acrylic acid graft copolymer (PVDF-HFP-AA), or a mixture thereof.
[0058] According to the present disclosure, the second binder satisfying the above-defined tan δ peak condition may be PVDF-HFP.
[0059] According to an embodiment of the present disclosure, the porous coating layer includes a first binder and a second binder as binders. According to another embodiment of the present disclosure, the binder for the porous coating layer according to the present disclosure substantially includes the first binder and the second binder. According to yet another embodiment of the present disclosure, the binder for the porous coating layer according to the present disclosure consists of the first binder and the second binder.
[0060] According to an embodiment of the present disclosure, based on 100wt% of the total weight of the first adhesive and the second adhesive, the adhesive may include 5wt% to 50wt% of the first adhesive and 50 to 95wt% of the second adhesive. When the content of the first adhesive is less than the lower limit, a large number of microscopic pores (microvoid) exist in the coating to provide reduced resistance, but the porous coating density is reduced, which leads to a significant reduction in the thickness of the porous coating when laminated with the electrode for manufacturing a battery. In addition, in this case, the physical strength is reduced, resulting in reduced penetration strength or overcharge safety. At the same time, when the content of the first adhesive is greater than the upper limit, there is a problem of reduced adhesion. According to another embodiment of the present disclosure, based on 100wt% of the total weight of the first adhesive and the second adhesive, the adhesive may include 5wt% to 15wt% of the first adhesive and 85 to 95wt% of the second adhesive. According to another embodiment of the present disclosure, based on 100wt% of the total weight of the first adhesive and the second adhesive, the adhesive may include 14wt% to 50wt% of the first adhesive and 50 to 86wt% of the second adhesive.
[0061] According to an embodiment of the present disclosure, when the first adhesive is pressurized at 190° C. to form an adhesive sample having a thickness of 0.4 mm, the adhesive sample may exhibit a behavior with a phase angle of less than 45°, as measured by an Advanced Rheometric Expansion System (ARES) at 190° C., while the second adhesive may exhibit a phase angle of less than 10°. 5 The behavior of the phase angle of 45° or more at the complex modulus value of Pa or less. When the second adhesive shows a 5 When the phase angle behaves at a complex modulus value of Pa or less and is 45° or more, the second binder may show a softening property under the condition of laminating the electrode and the separator, that is, under heat pressing conditions.
[0062] Herein, the phase angle (δ) is measured by using an ARES instrument commercially available from TA Instruments under the model name ARES-G2.
[0063] Specifically, the phase angle (δ) is determined as follows:
[0064] (S1) The adhesive resin sample is loaded on the parallel plate of the ARES instrument and a gap of 1 mm is set with the 25 mm parallel plate.
[0065] (S2) The ratio of the viscosity modulus to the loss modulus is measured from an ARES instrument at a temperature of 190°C, a stress of 1%, and a shear rate of 0.05 rad / s to 5 rad / s. The measured value corresponds to the inverse tangent of the phase angle.
[0066] (S3) The arctangent value is converted into a tan δ (at shear rate = 100 rad / s) value. In this way, the phase angle is calculated.
[0067] According to an embodiment of the present disclosure, the 5 The phase angle of the first adhesive is measured at a complex modulus of Pa, and the first adhesive is about 10 5 Pa to 10 6 The first adhesive has a complex modulus of less than 45° only at a phase angle of less than 45°. The expression "the first adhesive has a complex modulus only at a phase angle of less than 45°" means that the first adhesive has a tan δ value of less than 1 (i.e., an inverse tangent value of greater than 1), and a ratio of the viscosity modulus to the loss modulus (viscosity modulus / loss modulus) of greater than 1.
[0068] According to an embodiment of the present disclosure, the second adhesive may be 5 Pa or less, especially at about 10 3 Pa to about 10 5 The expression "the second adhesive has a phase angle of 45° or greater at a complex modulus value of about 10 5 Pa or less complex modulus value with a phase angle of 45° or greater means that the second adhesive has a tan δ value of 1 or greater (i.e., an inverse tangent value of less than 1), and a ratio of the viscosity modulus to the loss modulus (viscosity modulus / loss modulus) of less than 1.
[0069] According to an embodiment of the present disclosure, when the complex viscosity of the adhesive is measured as a function of frequency, the first adhesive shows a greater complex viscosity than the second adhesive, which suggests that the first adhesive has a greater weight average molecular weight than the second adhesive. In addition, the first adhesive shows a relatively greater change in complex viscosity, while the second adhesive shows a relatively smaller change in complex viscosity.
[0070] According to an embodiment of the present disclosure, the first adhesive and the second adhesive can each be described in terms of storage modulus and loss modulus. In general, the storage modulus represents a polymer whose elasticity is dominant, while the loss modulus represents a polymer whose viscosity is dominant. The difference in hardness or viscosity of the rigidity or mobility of the main chain (mainchain) of each of the first adhesive and the second adhesive can be inferred from the measurement of the storage modulus and the loss modulus, wherein in the temperature range of the operation of the lithium secondary battery, for example, at a temperature of 0°C or higher, the first adhesive shows a higher storage modulus than the second adhesive, and the second adhesive shows a higher loss modulus than the first adhesive. That is, it can be inferred that in the temperature range of the operation of the lithium secondary battery, for example, at a temperature of 0°C or higher, the first adhesive shows a dominant elasticity compared to the second adhesive, and the second adhesive shows a dominant viscosity compared to the first adhesive.
[0071] Meanwhile, according to an embodiment of the present disclosure, the adhesive may further include a third adhesive. When the third adhesive is pressurized at 190° C. to form an adhesive sample having a thickness of 0.4 mm, as determined by dynamic mechanical analysis (DMA), the adhesive sample has a tan δ peak at -12° C. to 0° C., preferably -11° C. to -4° C., in the range of -12° C. to 50° C.
[0072] Non-limiting examples of the third binder include poly(vinylidene fluoride-co-chlorotrifluoroethylene) (PVDF-CTFE). Figure 7 As can be seen from , PVDF-CTFE (Solef 32008) used as the third adhesive according to the present disclosure has a tan δ at about -7.56°C.
[0073] Meanwhile, the third binder may be present in an amount of 8 wt % to 25 wt % based on 100 wt % of the total weight of the first binder, the second binder, and the third binder.
[0074] When a separator including a porous coating is manufactured and then applied to a battery, a loss of the adhesive may occur due to the dissolution of the adhesive included in the porous coating in the electrolyte, or the like. According to the present disclosure, the adhesive may include a predetermined amount of a third adhesive, and thus the separator according to the present disclosure may provide an effect of reducing the dissolution of the adhesive in the porous coating. Specifically, when the internal temperature of the battery rises, the problem of the adhesive dissolving in the electrolyte may become serious. Generally speaking, after the battery is manufactured, aging is performed at a temperature of 60° C. or higher for the purpose of accelerating the impregnation of the separator with the electrolyte. Despite the implementation of this aging, the adhesive resin in the porous coating is still dissolved by the electrolyte, resulting in a decrease in the bonding force of the porous coating. As a result, the porous coating may be removed from the porous substrate or the inorganic particles in the porous coating may be unexpectedly detached. Therefore, a third adhesive may be further introduced according to the present disclosure to reduce the dissolution of the adhesive in the electrolyte.
[0075] According to the embodiment of the present disclosure, although there is no particular restriction on the particle size of the inorganic particles of the porous coating, from the perspective of forming a coating with uniform thickness and appropriate porosity, the inorganic particles may have a particle size of 0.001 μm to 10 μm, 0.01 μm to 10 μm, 0.05 μm to 5 μm, or 0.1 μm to 2 μm. When the size of the inorganic particles meets the above-defined range, the inorganic particles maintain dispersibility to facilitate control of the physical properties of the separator for lithium secondary batteries. In addition, it is possible to avoid increasing the thickness of the porous coating to improve mechanical properties. Further, due to the excessive pore size, the possibility of internal short circuit during charge / discharge of the battery is less.
[0076] In this article, “particle size D 50 "D" refers to a particle diameter at a 50% point in a cumulative distribution of the number of particles depending on the particle diameter, and can be measured by using a laser diffraction method. Specifically, a powder to be analyzed is dispersed in a dispersion medium and introduced into a commercially available laser diffraction particle size analyzer (e.g., Microtrac S3500), and then a difference in a diffraction pattern depending on the particle diameter is measured when the particles pass through a laser beam, and then a particle diameter distribution is calculated. Subsequently, the particle diameter at a 50% point in the cumulative distribution of the number of particles depending on the particle diameter is calculated to determine D 50 .
[0077] There are no particular limitations on the inorganic particles as long as they are electrochemically stable. That is, there are no particular limitations on the inorganic particles as long as they are within the operating voltage range of the applicable electrochemical device (e.g., based on Li / Li +It is only necessary that oxidation and / or reduction are not caused in the 0 - 5V). Specifically, when using inorganic particles having ion transport ability, the ionic conductivity in the electrochemical device can be increased and the quality can be assisted in improving. In addition, when using inorganic particles having a high dielectric constant, the ionic conductivity of the electrolyte can be improved by increasing the dissociation degree of electrolyte salts such as lithium salts in the liquid electrolyte.
[0078] For the reasons mentioned above, the inorganic particles can be inorganic particles having a dielectric constant of 5 or greater, or 10 or greater, inorganic particles having lithium ion transport ability, or a mixture thereof. Non - limiting examples of inorganic particles having a dielectric constant of 5 or greater may include any one selected from the group consisting of BaTiO3, Pb(Zr,Ti)O3 (PZT), Pb 1-x La x Zr 1-y Ti y O3 (PLZT, where 0 < x < 1, 0 < y < 1), Pb(Mg3Nb 2 / 3 )O3PbTiO3 (PMN - PT), hafnium oxide (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, Y2O3, Al2O3, γ - AlOOH, SiC, and TiO2, or a mixture of two or more of them. In addition, when inorganic particles having lithium ion transport ability and inorganic particles having a high dielectric constant are used in combination, a synergistic effect can be provided.
[0079] Non - limiting examples of inorganic particles having lithium ion transport ability include lithium phosphate (Li3PO4), lithium titanium phosphate (Li x Ti y (PO4)3, 0 < x < 2, 0 < y < 3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, 0 < x < 2, 0 < y < 1, 0 < z < 3), (LiAlTiP) x O y - based glass (glass) (1 < x < 4, 0 < y < 13), lithium lanthanum titanate (Li x La y TiO3, 0 < x < 2, 0 < y < 3), lithium germanium thiophosphate such as Li 3.25 Ge 0.25 P 0.75 S4, etc. (Li x Ge y P z S w, where 0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5), lithium nitrides such as Li3N (Li x N y , where 0 < x < 4, 0 < y < 2), SiS2-based glasses such as Li3PO4-Li2S-SiS2 (Li x Si y S z , where 0 < x < 3, 0 < y < 2, 0 < z < 4), and P2S5-based glasses such as LiI-Li2S-P2S5 (Li x P y S z , where 0 < x < 3, 0 < y < 3, 0 < z < 7), or mixtures thereof.
[0080] According to an embodiment of the present disclosure, the porous coating may not use a dispersant.
[0081] According to another embodiment of the present disclosure, the porous coating may further include a dispersant. Based on 100 parts by weight of the solid content forming the porous coating, the dispersant is used in an amount of 1 to 3 parts by weight and is used to improve the dispersibility of the inorganic particles. Non-limiting examples of the dispersant include any one selected from polymer compounds such as acrylic copolymers, cyanoethylated polyvinyl alcohol; phenolic compounds including baicalin, luteolin, taxifolin, myricetin, quercetin, rutin, catechin, epigallocatechin gallate, butein, piceatannol, and tannic acid; pyrogallic acid; amylose; amylopectin; xanthan gum; and fatty acid compounds, or a mixture of two or more of them.
[0082] The acrylic copolymer may be a copolymer containing at least one functional group selected from the group consisting of OH, COOH, CN, amine, and amide groups.
[0083] Specific examples of these acrylic copolymers include, but are not limited to: ethyl acrylate-acrylic acid-N,N-dimethylacrylamide copolymer, ethyl acrylate-acrylic acid-2-(dimethylamino)ethyl acrylate copolymer, ethyl acrylate-acrylic acid-N,N-diethylacrylamide copolymer, ethyl acrylate-acrylic acid-2-(diethylamino)ethyl acrylate copolymer, or two or more of them.
[0084] The pore size and porosity of the porous coating mainly depend on the size of the inorganic particles. For example, when using inorganic particles with a particle size of 1 μm or less, the resulting pores also have a size of 1 μm or less. This porous structure is filled with the subsequently injected electrolyte, and the electrolyte is used to transport ions. Therefore, the pore size and porosity are important factors affecting the control of the ionic conductivity of the porous coating.
[0085] The porous coating layer according to an embodiment of the present disclosure may preferably have a pore size of 0.001 μm to 10 μm or 0.001 μm to 1 μm.
[0086] The porosity of the porous coating may have a porosity of 5% to 95%, 10% to 95%, 20% to 90%, or 30% to 80%. The porosity corresponds to a value obtained by subtracting the volume of the coating derived from the weight and density of each component of the coating from the volume of the porous coating calculated from its thickness, width, and length.
[0087] When the porous coating layer has a pore size and a porosity within the above-defined ranges, the separator for a lithium secondary battery according to an embodiment of the present disclosure may prevent a short circuit from occurring in an abnormal state and may be provided with appropriate resistance characteristics and air permeability at the same time.
[0088] 3. Method for forming a porous coating
[0089] According to an embodiment of the present disclosure, the porous coating layer may be formed by mixing inorganic particles and a binder in a solvent to prepare a composition for forming the porous coating layer, and applying the composition to a porous polymer substrate, followed by drying.
[0090] According to an embodiment of the present disclosure, the solvent is an organic solvent, and any organic solvent may be used without particular limitation as long as it can homogeneously disperse the inorganic particles and the binder.
[0091] Specific examples of organic solvents include: alicyclic hydrocarbons such as cyclopentane and cyclohexane, for example, methylcyclohexane and ethylcyclohexane; aromatic hydrocarbons such as toluene, xylene, and ethylbenzene; ketones such as ethyl ketone, methyl ethyl ketone, diisopropyl ketone, cyclohexanone; chlorinated aliphatic hydrocarbons such as dichloromethane, chloroform, and carbon tetrachloride; esters such as ethyl acetate, butyl acetate, γ-butyrolactone, and ε-caprolactone; nitriles such as acrylonitrile, acetonitrile, and propionitrile; ethers such as tetrahydrofuran and ethylene glycol diethyl ether; alcohols such as methanol, ethanol, isopropanol, ethylene glycol, and ethylene glycol monomethyl ether; and amides such as N-methylpyrrolidone and N,N-dimethylformamide. According to an embodiment of the present disclosure, the solvent may include acetone in consideration of the advantages during the drying process.
[0092] These solvents can be used alone or in combination. Specifically, solvents with low boiling points and high volatility are preferred because they can be removed at low temperatures in a short time. Particularly preferred solvents include acetone, toluene, cyclohexanone, cyclopentanone, tetrahydrofuran, cyclohexane, dimethylbenzene, N-methylpyrrolidone or a mixed solvent comprising two or more of them.
[0093] Preferably, the ratio of the inorganic particles to the binder in the composition is the same as described above with respect to the porous coating layer.
[0094] There is no particular limitation on the method for forming a porous coating layer by applying the composition to a porous polymer substrate, and specific examples of the method include dip coating, die coating, roll coating, comma coating, blade coating, reverse roll coating, direct roll coating, or the like.
[0095] The coating process for forming the porous coating is preferably implemented under a certain range of humidity. After the composition for forming the porous coating is applied to any one surface or both surfaces of the porous polymer substrate, the binder polymer dissolved in the porous coating (composition) has a phase change property by the vapor-induced phase separation phenomenon known to those skilled in the art. Phase separation can be implemented by humidification phase separation or immersion phase separation.
[0096] Hereinafter, the humidification phase separation will be explained.
[0097] First, a non-solvent may be introduced in a gaseous state. The non-solvent is not particularly limited as long as it cannot dissolve the binder and has partial miscibility with the solvent. For example, the non-solvent may be at least one selected from the group consisting of water, methanol, ethanol, isopropanol, and butanol.
[0098] When the non-solvent is introduced and added in a gaseous state, there are advantages in that phase separation can be performed by using a small amount of the non-solvent and the inorganic composition can be easily dried.
[0099] Herein, the gaseous non-solvent may be added at a temperature of 15° C. to 70° C. When the temperature is lower than 15° C., the non-solvent can hardly maintain its gaseous state, and the inorganic composition is dried at a low rate, resulting in a decrease in productivity. When the temperature is higher than 70° C., the solvent and the non-solvent are dried at an excessively high rate, making it difficult to fully perform phase separation.
[0100] In addition, during phase separation, the non-solvent is added in such a manner that the vapor pressure of the non-solvent may be 15% to 80%, or 30% to 50% based on its saturated vapor pressure, and then the phase separation is sequentially performed. When the vapor pressure of the non-solvent is less than 15% based on its saturated vapor pressure, the amount of the non-solvent is too small to sufficiently perform the phase separation. When the vapor pressure of the non-solvent is greater than 80% based on its saturated vapor pressure, the phase separation occurs excessively, thereby making it difficult to form a uniform coating.
[0101] In order to perform phase separation by adding a non-solvent in a gaseous state, it is advantageous that the solvent has a low boiling point and thus evaporates easily. That is, when the solvent evaporates to lower the temperature, solvent exchange occurs easily, and the gaseous non-solvent is condensed. According to an embodiment, when a gaseous non-solvent is added, the solvent may have a boiling point of 30° C. to 80° C. In addition, the solvent of the inorganic composition to which the gaseous non-solvent is added may be at least one selected from the group consisting of acetone and methyl ethyl ketone.
[0102] Hereinafter, the impregnation phase separation will be explained.
[0103] After the composition for forming a porous coating is applied on at least one surface of a porous polymer substrate, the coated porous polymer substrate is immersed in a coagulation solution containing an appropriate non-solvent for a predetermined time. In this way, the binder resin solidifies, and phase separation occurs in the composition for forming a porous coating applied. In this process, the coating including the binder resin and the inorganic particles is converted into a porous layer. Then, the resulting product is washed with water to remove the coagulation solution, followed by drying, thereby forming a porous coating as a whole on the porous polymer substrate.
[0104] The solvent for dissolving the binder may be a solvent capable of dissolving the binder resin to 5 wt % or more, preferably 15 wt % or more, more preferably 25 wt % or more at 25° C. Non-limiting examples of the solvent include polar amide solvents such as N-methylpyrrolidone, dimethylacetamide, and dimethylformamide; acetone (propanone); cyclopentanone (cyclopentanone); methyl acetate (methylacetate); gamma-butyrolactone (gamma-butyrolactone); trimethylphosphate (trimethylphosphate); triethylphosphate (triethylphosphate); and dimethylethoxymethan (dimethylethoxymethan). When the solubility of the binder resin in the solvent is lower than the above-defined range, there is a problem that phase separation may be excessively performed.
[0105] The nonsolvent may be a nonsolvent providing a solubility of the binder resin of less than 5 wt % at 25° C. The nonsolvent may include at least one selected from water, methanol, ethanol, propanol, butanol, butanediol, ethylene glycol, propylene glycol, and tripropylene glycol.
[0106] As the coagulation solution, a non-solvent may be used alone, or a mixed solvent of a non-solvent and the above-mentioned solvent may be used. When a mixed solvent of a non-solvent and a solvent is used, the content of the non-solvent is 95wt% or more based on 100wt% of the coagulation solution from the perspective of forming a high-quality porous structure and improving productivity.
[0107] According to an embodiment of the present disclosure, the separator for a lithium secondary battery can be dried after phase separation. Drying can be implemented by a process known to those skilled in the art, and can be performed in a batch mode or a continuous mode by using an oven or a heating chamber in a temperature range taking into account the vapor pressure of the solvent used. Taking into account factors such as productivity, drying is preferably substantially removing the solvent present in the composition at a high rate. For example, drying can be implemented for 1 minute or shorter, preferably 30 seconds or shorter.
[0108] The porous coating layer may be formed on both surfaces of the porous polymer substrate, or selectively formed on one surface of the porous polymer substrate.
[0109] The separator for lithium secondary battery obtained as described above can be used as a separator of electrochemical device. Electrochemical device includes any device for implementing electrochemical reaction, and its specific example includes all types of primary battery, secondary battery, fuel cell, solar cell, or capacitor (capacitor) such as supercapacitor device. In particular, in secondary battery, lithium secondary battery including lithium metal secondary battery, lithium ion secondary battery, lithium polymer secondary battery, or lithium ion polymer battery is preferred.
[0110] According to an embodiment of the present disclosure, a lithium secondary battery can be obtained by conventional methods known to those skilled in the art. According to an embodiment of the present disclosure, a separator can be interposed between a positive electrode and a negative electrode to prepare an electrode assembly, the electrode assembly is introduced into a battery housing, and an electrolyte is injected therein to obtain the secondary battery.
[0111] According to an embodiment of the present disclosure, the electrode of the secondary battery can be obtained by combining an electrode active material with an electrode current collector by a method generally known in the art. In the electrode active material, non-limiting examples of positive electrode active materials include conventional positive electrode active materials that can be used for positive electrodes of conventional electrochemical devices. In particular, lithium intercalation materials such as lithium manganese oxide, lithium cobalt oxide, lithium nickel oxide, lithium iron oxide, or lithium composite oxides comprising a combination thereof are preferably used. Non-limiting examples of negative electrode active materials include conventional negative electrode active materials that can be used for negative electrodes of conventional electrochemical devices. In particular, lithium intercalation materials such as lithium metal or lithium alloys, carbon, petroleum coke, activated carbon, graphite, or other carbonaceous materials are preferably used. Non-limiting examples of positive electrode current collectors include foils made of aluminum, nickel, or a combination thereof. Non-limiting examples of negative electrode current collectors include foils made of copper, gold, nickel, nickel alloys, or a combination thereof.
[0112] The electrolyte that can be used in the electrochemical device according to the present disclosure is one having A + B - A salt of the structure + Including such as Li + 、Na + , K + , or a combination thereof such as an alkali metal cation, B - Including PF6 - 、BF4 - , Cl - Br - ,I - 、ClO4 - 、AsF6 - 、CH3CO2 - CF3SO3 - 、N(CF3SO2)2 - 、C(CF2SO2)3 - , or anions such as a combination thereof, the salt is dissolved or dissociated in an organic solvent including propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), gamma-butyrolactone (γ-butyrolactone), or a combination thereof. However, the present disclosure is not limited thereto.
[0113] Depending on the manufacturing process of the finished product and the properties required for the finished product, the injection of electrolyte can be implemented in a suitable step during the process for manufacturing the battery. That is, the injection of electrolyte can be implemented before assembling the battery or in the final step of assembling the battery. According to an embodiment of the present disclosure, as a process for applying an electrode assembly to a battery, in addition to a conventional winding process, lamination or stacking of a separator with an electrode, and folding can also be used.
[0114] Embodiments will be described more fully hereafter so that the present disclosure can be easily understood. However, the following embodiments can be embodied in a variety of different forms and should not be construed as being limited to the exemplary embodiments set forth herein. On the contrary, these exemplary embodiments are provided so that the present disclosure will be thorough and complete, and will fully convey the scope of the present disclosure to those skilled in the art.
[0115] Example
[0116] Example 1
[0117] Preparation of composition for forming porous coating layer
[0118] As inorganic particles, an average particle size D 50 It is 500nm Al2O3 powder.
[0119] As adhesive, two types of PVDF-based adhesives were prepared. Specifically, the first adhesive was a PVDF-TFE adhesive (available from Daikin's VT-475) with a rheological behavior dominated by elasticity, wherein when the adhesive was pressurized at 190°C and formed into an adhesive sample with a thickness of 0.4 mm, as determined by a dynamic mechanical analysis (DMA) using DMAQ800 available from TA Instruments, the adhesive sample had a tan δ peak at 15°C to 27.6°C. In addition, the second adhesive was a PVDF-HFP adhesive (available from Solvay's Solef 21510) with a rheological behavior dominated by viscosity, wherein when the adhesive was pressurized at 190°C and formed into an adhesive sample with a thickness of 0.4 mm, as determined by a dynamic mechanical analysis (DMA) using DMA Q800 available from TA Instruments, the adhesive sample had a tan δ peak at 8°C to 20.2°C.
[0120] Figure 1 is a graph illustrating the relationship between temperature and tan δ for each of the first adhesive and the second adhesive. Figure 1In the embodiment of the present invention, the first adhesive has a peak at about 19.44°C, and the second adhesive has a peak at about 11.45°C.
[0121] besides, Figure 2 is a graph illustrating the relationship between the complex modulus and the phase angle for each of the first adhesive and the second adhesive. Figure 2 The first adhesive is shown in about 10 5 Pa to 10 6 The second adhesive showed a rheological behavior with a phase angle of less than 30° at a complex modulus value of about 10 5 Pa or less, specifically about 10 3 Pa to 10 5 Rheological behavior with a phase angle of 45° or greater at a complex modulus value of Pa.
[0122] Herein, the relationship between the complex modulus and the phase angle of each of the first adhesive and the second adhesive is determined by forming each of the first adhesive and the second adhesive into an adhesive sample having a thickness of 0.4 mm by pressing at 190° C. and analyzing the adhesive sample using an Advanced Rheometric Expansion System (ARES) at 190° C.
[0123] besides, Figure 3 is a graph illustrating the relationship between the angular frequency and the complex viscosity for each of the first adhesive and the second adhesive. Figure 3 It can be inferred that the first adhesive has a larger weight average molecular weight than the second adhesive because the first adhesive has a higher complex viscosity than the second adhesive. In addition, the first adhesive shows a relatively larger change in complex viscosity, while the second adhesive shows a relatively smaller change in complex viscosity.
[0124] Further, Figure 4 is a graph illustrating the storage modulus and loss modulus of each of the first adhesive and the second adhesive as a function of temperature. Figure 4 It can be inferred that the first adhesive has higher elasticity than the second adhesive at a temperature of about 0°C or higher because the first adhesive shows a higher storage modulus than the second adhesive at a temperature of about 0°C or higher. Figure 4 It can also be inferred that the second adhesive shows a higher viscosity at a temperature of about -40°C to about 20°C compared to the first adhesive, while the first adhesive shows a lower viscosity (i.e., flowability) compared to the second adhesive because the second adhesive shows a higher loss modulus at a temperature of about -40°C to about 20°C compared to the first adhesive.
[0125] Al2O3 powder, a first binder, and a second binder were prepared in a ratio of 65wt%:5wt%:30wt%.
[0126] The first adhesive is mixed with the second adhesive, and the resulting mixture is dissolved in N-methylpyrrolidone (NMP) as a solvent for about 1 hour to prepare an adhesive composition at room temperature (23°C). Then, inorganic particles are added to the adhesive composition. By using a bead mill, the adhesive composition including inorganic particles is passed through a layer including beads having a diameter of 0.65mm three to five times so that the inorganic particles can be dispersed, thereby providing a composition for forming a porous coating. Herein, the composition for forming a porous coating is controlled to have a solid content of 20wt%.
[0127] Formation of porous coatings on porous polymer substrates
[0128] As the porous polymer substrate, a polyethylene porous polymer substrate (thickness 9 μm, porosity 43%, air permeation time 110 sec, resistance 0.45 Ω) having a size of 6 cm×15 cm was prepared.
[0129] The composition for forming a porous coating is applied to both surfaces of a polyethylene porous polymer substrate having a size of 6cm×15cm by a dip coating process. Then, the polyethylene porous polymer substrate coated with the composition for forming a porous coating is directly immersed in water as a non-solvent to implement phase separation by solvent / non-solvent exchange. After that, the substituted non-solvent, i.e., water, is dried to obtain a separator for a lithium secondary battery having a porous coating on both surfaces of the porous polymer substrate. The porous coating has a structure in which an adhesive bonds inorganic particles to each other so that the inorganic particles can maintain their binding state, and the inorganic particles are bonded to the porous polymer substrate so that the inorganic particles and the porous polymer substrate maintain their binding state, and the inorganic particles form interstitial volumes while substantially contacting each other, and the interstitial volumes between the inorganic particles become vacant spaces to form pores of the porous coating. In addition, the porous coating has a structure in which it also has pores generated during the exchange between the solvent and the non-solvent, i.e., water, in the adhesive layer. The total coating amount of the porous coating applied to both surfaces of the porous polymer substrate was 5.8 g / m 2 .
[0130] Example 2
[0131] A composition for forming a porous coating layer was prepared in the same manner as in Example 1, except that Al2O3 powder, the first binder, and the second binder were prepared in a weight ratio of 70:5:25. The composition was controlled to have a solid content of 20 wt%.
[0132] Then, a porous polymer substrate was prepared, and the composition was applied to one surface of the substrate to obtain a separator for a lithium secondary battery, the separator being provided with a porous coating layer formed on one surface of the porous polymer substrate and comprising a binder mixed with inorganic particles. The total coating amount of the porous coating layer was 5.6 g / m 2 .
[0133] Example 3
[0134] A composition for forming a porous coating was prepared in the same manner as in Example 1, except that Al2O3 powder, a first binder, a second binder, and a third binder were prepared in a weight ratio of 70:2:24:4, and the third binder was introduced together with the first binder and the second binder during the preparation of the binder composition. The composition was controlled to have a solid content of 20 wt%. Here, PVDF-CTFE (Solef 32008 available from Solvay) was used as the third binder.
[0135] Meanwhile, when the third adhesive, PVDF-CTFE (Solef 32008 available from Solvay), was formed into an adhesive sample having a thickness of 0.4 mm by pressing at 190° C., the adhesive sample was analyzed by dynamic mechanical analysis (DMA) using DMA Q800 available from TA Instruments. It was shown that the adhesive sample had a tan δ peak at −7.56° C.
[0136] Then, a porous polymer substrate was prepared, and the composition was applied to one surface of the substrate to obtain a separator for a lithium secondary battery, the separator being provided with a porous coating layer formed on one surface of the porous polymer substrate and including a binder mixed with inorganic particles. The total coating amount of the porous coating layer was 6.48 g / m 2 .
[0137] Example 4
[0138] A composition for forming a porous coating was prepared in the same manner as in Example 1, except that Al2O3 powder, a first binder, a second binder, and a third binder were prepared in a weight ratio of 72:2:22:4, and the third binder was introduced together with the first binder and the second binder during the preparation of the binder composition. The composition was controlled to have a solid content of 20 wt%. Here, PVDF-CTFE (Solef 32008 available from Solvay) was used as the third binder.
[0139] Then, a porous polymer substrate was prepared, and the composition was applied to one surface of the substrate to obtain a separator for a lithium secondary battery, the separator being provided with a porous coating layer formed on one surface of the porous polymer substrate and including a binder mixed with inorganic particles. The total coating amount of the porous coating layer was 6.8 g / m 2 .
[0140] Example 5
[0141] A composition for forming a porous coating was prepared in the same manner as in Example 1, except that Al2O3 powder, a first binder, a second binder, and a third binder were prepared in a weight ratio of 70:2:22:6, and the third binder was introduced together with the first binder and the second binder during the preparation of the binder composition. The composition was controlled to have a solid content of 20 wt%. Here, PVDF-CTFE (Solef 32008 available from Solvay) was used as the third binder.
[0142] Then, a porous polymer substrate was prepared, and the composition was applied to one surface of the substrate to obtain a separator for a lithium secondary battery, the separator being provided with a porous coating layer formed on one surface of the porous polymer substrate and comprising a binder mixed with inorganic particles. The total coating amount of the porous coating layer was 6.96 g / m 2 .
[0143] Example 6
[0144] A composition for forming a porous coating layer was prepared in the same manner as in Example 5, except that PVDF-HFP (Solef 20808 available from Solvay) was used as a second binder. The composition was controlled to have a solid content of 20 wt%.
[0145] Then, a porous polymer substrate was prepared, and the composition was applied to one surface of the substrate to obtain a separator for a lithium secondary battery, the separator being provided with a porous coating layer formed on one surface of the porous polymer substrate and comprising a binder mixed with inorganic particles. The total coating amount of the porous coating layer was 6.96 g / m 2 .
[0146] Meanwhile, when the second adhesive, PVDF-HFP (Solef 20808 available from Solvay), was formed into an adhesive sample having a thickness of 0.4 mm by pressing at 190° C., the adhesive sample was analyzed by dynamic mechanical analysis (DMA) using DMA Q800 available from TA Instruments. It was shown that the adhesive sample had a tan δ peak at 11.95° C.
[0147] Comparative Example 1
[0148] A composition for forming a porous coating layer was prepared in the same manner as in Example 1, except that the first binder was not used, and the PVDF-HFP (Solef 21510 available from Solvay) used as the second binder in Example 1 was used alone as a binder for the composition for forming a porous coating layer. Then, the composition was applied to both surfaces of a porous polymer substrate using the same materials and methods as in Example 1 to obtain a separator for a lithium secondary battery, the separator being provided with a porous coating layer comprising a binder mixed with inorganic particles.
[0149] Comparative Example 2
[0150] A composition for forming a porous coating was prepared in the same manner as in Example 3, except that the first binder was not used, and Al2O3 powder, the second binder, and the third binder were prepared in a weight ratio of 65:30:5. The composition was controlled to have a solid content of 20 wt%. Then, the composition was applied to both surfaces of a porous polymer substrate using the same materials and methods as in Example 1 to obtain a separator for a lithium secondary battery, the separator being provided with a porous coating comprising a binder mixed with inorganic particles.
[0151] Comparative Example 3
[0152] A composition for forming a porous coating was prepared in the same manner as in Example 3, except that the first binder was not used, and Al2O3 powder, the second binder, and the third binder were prepared in a weight ratio of 65:25:10. The composition was controlled to have a solid content of 18 wt%. Then, the composition was applied to both surfaces of a porous polymer substrate using the same materials and methods as in Example 1 to obtain a separator for a lithium secondary battery, the separator being provided with a porous coating comprising a binder mixed with inorganic particles.
[0153] Comparative Example 4
[0154] A composition for forming a porous coating was prepared in the same manner as in Example 1, except that PVDF-HFP-AA (Solef 75130 available from Solvay) was used as the first binder, and Al2O3 powder, the first binder, and the second binder were prepared in a weight ratio of 70:15:15. The composition was controlled to have a solid content of 20wt%. Then, the composition was applied to both surfaces of a porous polymer substrate using the same materials and methods as in Example 1 to obtain a separator for a lithium secondary battery, the separator being provided with a porous coating comprising a binder mixed with inorganic particles.
[0155] When the first adhesive, PVDF-HFP-AA (Solef 75130 available from Solvay), was formed into an adhesive sample having a thickness of 0.4 mm by pressing at 190° C., the adhesive sample was analyzed by dynamic mechanical analysis (DMA) using DMA Q800 available from TA Instruments. It was shown that the adhesive sample had a tan δ peak at 20.5° C.
[0156] evaluate
[0157] The separators for lithium secondary batteries obtained from Examples 1 to 6 and Comparative Examples 1 to 4 were evaluated for bulk density D of the porous coating layer, air permeability, adhesion to the electrode, peel strength, high-temperature shrinkage, and resistance by the following methods. The results are shown in Tables 2 and 3 below. In addition, scanning electron microscope (SEM) images of the surface and cross section of each separator for lithium secondary batteries are shown in Figure 5 and Figure 6 middle.
[0158] (1) Bulk density D of porous coating
[0159] The packing density D of the porous coating is defined as the 2 ) of the porous polymer substrate to a density of the porous coating layer at a height of 1 μm and can be calculated as follows:
[0160] D=(S g -F g ) / (S t -E t ),
[0161] Where S g Indicates per unit area (m 2 ) of a separator for a lithium secondary battery having a porous coating layer formed on a porous polymer substrate (g),
[0162] F g Indicates per unit area (m 2 )’s weight (g),
[0163] S t represents the thickness (μm) of a separator for a lithium secondary battery having a porous coating layer formed on a porous polymer substrate, and
[0164] F t Indicates the thickness of the porous polymer substrate (μm)
[0165] (2) Air permeability of separators for lithium secondary batteries
[0166] The air permeability (Gurley) was measured according to the method of ASTM D726-94. Herein, Gurley type air permeability refers to the resistance against air flow and is measured by using a Gurley densometer. Each air permeability value defined herein is shown as 100cc of air passing through 1in of each separator according to Examples 1 and 2 and Comparative Example at a pressure of 12.2in of water column. 2 The time required for the cross section to be filled (i.e., air penetration time).
[0167] (3) Adhesion to the electrode
[0168] A negative electrode slurry was prepared by mixing artificial graphite as a negative electrode active material, denka black (carbon black) as a conductive material, and polyvinylidene fluoride (PVdF) as a binder in a weight ratio of 75:5:25, and adding N-methylpyrrolidone (NMP) as a solvent to the resulting mixture.
[0169] The negative electrode slurry was coated on a copper current collector to a concentration of 3.8 mAh / cm 2 The negative electrode is prepared by drying the negative electrode layer.
[0170] Each separator for lithium secondary battery obtained from Examples 1 to 6 and Comparative Examples 1 to 4 was stacked on the negative electrode in such a manner that the surface of the porous coating layer of each separator could face the negative electrode active material layer, and the resulting structure was laminated with a laminating device. Then, the resulting sample was introduced into a UTM instrument to measure the force required to peel off the electrode-separator (porous coating) adhesion surface at a rate of 100 mm / min.
[0171] (4) Evaluation of high temperature shrinkage
[0172] The high temperature shrinkage of the separator was calculated by preparing a sample of the separator for lithium secondary batteries according to each of Examples 1 to 6 and Comparative Examples 1 to 4 into a size of 50 mm (length) × 50 mm (width), allowing each sample to stand in an oven heated to 150° C. for 30 minutes, recovering the sample, and then calculating the high temperature shrinkage from the change in length in the longitudinal direction (MD) and the transverse direction (TD) according to the following formula:
[0173] High temperature shrinkage rate (%) = [(length before shrinkage - length after shrinkage) / length before shrinkage] × 100
[0174] (5) Evaluation of the electrical resistance of the separator
[0175] The resistance of the separator for lithium secondary batteries according to each of Examples 1 to 6 and Comparative Examples 1 to 4 was measured as follows. A coin cell was obtained by using each separator, the coin cell was allowed to stand at room temperature for 1 day, and then the resistance of each coin cell was measured by using electrochemical impedance spectroscopy. The coin cell was manufactured as follows.
[0176] Negative electrode manufacturing
[0177] First, artificial graphite as a negative electrode active material, denka black (carbon black) as a conductive material, and polyvinylidene fluoride (PVdF) as a binder were mixed in a weight ratio of 75:5:25, and N-methylpyrrolidone (NMP) as a solvent was added to the resulting mixture to prepare a negative electrode slurry.
[0178] The negative electrode slurry was coated on a copper current collector to a concentration of 3.8 mAh / cm 2 The negative electrode was obtained by drying.
[0179] Cathode Manufacturing
[0180] First, LiCoO2 as a positive electrode active material, denka black as a conductive material, and polyvinylidene fluoride (PVDF) as a binder were mixed in a weight ratio of 85:5:15, and the resulting mixture was added to N-methylpyrrolidone (NMP) as a solvent to prepare a positive electrode active material slurry. The positive electrode active material slurry was coated on a sheet-like aluminum current collector and then dried to form a positive electrode active material layer until the final positive electrode molecular weight was 3.3 mAh / cm 2 .
[0181] Coin Cell Battery Manufacturing
[0182] The separator for lithium secondary batteries according to Examples 1 to 6 and Comparative Examples 1 to 4 was inserted between the negative electrode and the positive electrode obtained as described above, and a non-aqueous electrolyte (1M LiPF6, ethylene carbonate (EC) / propylene carbonate (PC) / diethyl carbonate (DEC), volume ratio = 3:3:4) was injected therein to obtain a coin battery.
[0183] (6) Evaluation of peel strength
[0184] Each of the separator samples obtained from Examples 1 to 6 and Comparative Examples 1 to 4 was cut into a size of 100 mm (length) × 15 mm (width). A double-sided tape was adhered to glass and the sample was adhered to the opposite surface of the double-sided tape to prepare a structure. Then, the resulting structure was fixed to an instrument for measuring adhesion strength, i.e., LFplus available from LLOYD Instrument, and the separator sample of the upper portion was peeled off at a rate of 300 mm / min at an angle of 180°, and the peel strength was measured.
[0185] Table 1 below shows the content ratios of the first binder, the second binder, and the third binder in the binder resin used in each of Examples 1 to 6 and Comparative Examples 1 to 4.
[0186] [Table 1]
[0187]
[0188] [Table 2]
[0189]
[0190]
[0191] [Table 3]
[0192]
[0193] As can be seen from Tables 2 and 3, each separator according to Examples 1 to 6 of the present disclosure has excellent electrical properties compared to the separators of Comparative Examples 1 to 4. When Examples 1 and 2 are compared with Comparative Examples 1 and 2 using the same amount of binder, each separator according to Examples 1 and 2 ensures the peel strength required for battery operation, does not generate microvoids, unlike Comparative Example 1, and shows excellent resistance characteristics. In addition, in terms of negative electrode / separator adhesion, Examples 1 and 2 show higher adhesion than Comparative Example 1.
[0194] Meanwhile, Examples 3 to 6 using a smaller amount of binder than Comparative Examples 1 to 4 each ensured negative electrode / separator adhesion and peel strength required for battery operation, and showed better results in terms of generation of microvoids and resistance characteristics than Comparative Examples 1 to 4.
[0195] Meanwhile, in the case of Comparative Example 4, Comparative Example 4 used a reduced amount of the second binder, resulting in a decrease in negative electrode / separator adhesion compared to Examples 1 to 3.
[0196] (5) Scanning electron microscope (SEM) images
[0197] A cross section of the separator for a lithium secondary battery obtained from each of Example 1 and Comparative Example 1 was photographed by SEM. Figure 5 and Figure 6 The cross-sectional images of Example 1 and Comparative Example 1 are shown respectively. Figure 5 and Figure 6 When compared, it can be seen that the porous coating layer forming the separator for a lithium secondary battery according to Example 1 is thicker than the porous coating layer forming the separator for a lithium secondary battery according to Comparative Example 1, resulting in no generation of microvoids and thus showing improved safety.
Claims
1. A separator for a lithium secondary battery, comprising: porous polymer substrate; and a porous coating layer formed on at least one surface of the porous polymer substrate and comprising a binder mixed with inorganic particles, wherein the binder binds the inorganic particles to each other so that the inorganic particles can maintain their bonded state, and binds the inorganic particles to the porous polymer substrate so that the inorganic particles and the porous polymer substrate maintain their bonded state, The inorganic particles form interstitial volumes while being substantially in contact with each other, and the interstitial volumes between the inorganic particles become vacant spaces to form pores of the porous coating layer, wherein the adhesive comprises a first adhesive, a second adhesive and a third adhesive, When the adhesive is pressed at 190° C. to form an adhesive sample having a thickness of 0.4 mm, the adhesive sample includes the first adhesive having a tan δ peak at 15° C. to 27.6° C. and the second adhesive having a tan δ peak at 8° C. to 11.95° C., as determined by dynamic mechanical analysis, When the third adhesive is pressed at 190° C. to form an adhesive sample having a thickness of 0.4 mm, the adhesive sample has a tan δ peak at −12° C. to 0° C. as determined by dynamic mechanical analysis, Based on 100 wt % of the total weight of the first binder and the second binder, the first binder is present in an amount of 5 wt % to 14.3 wt %, and the second binder is present in an amount of 85.7 wt % to 95 wt %, The third binder is present in an amount of 8 wt % to 25 wt % based on 100 wt % of the total weight of the first binder, the second binder and the third binder, wherein the first binder satisfying the tan δ peak condition is poly(vinylidene fluoride-tetrafluoroethylene), poly(vinylidene fluoride-trifluoroethylene), PVDF-HFP-acrylic acid graft copolymer, or a mixture thereof, wherein the second binder satisfying the tan δ peak condition is poly(vinylidene fluoride-hexafluoropropylene), and The third adhesive comprises PVDF-CTFE.
2. The separator for a lithium secondary battery according to claim 1, wherein when the first adhesive is pressurized at 190°C to form an adhesive sample having a thickness of 0.4 mm, the adhesive sample exhibits a behavior with a phase angle of less than 45° as measured by an advanced rheological expansion system at 190°C.
3. A separator for a lithium secondary battery according to claim 1, wherein when the second adhesive is pressurized at 190°C to form an adhesive sample having a thickness of 0.4 mm, the adhesive sample exhibits a behavior with a phase angle of 45° or greater as measured by an advanced rheological expansion system at 190°C. 4 . The separator for a lithium secondary battery according to claim 1 , wherein the porous coating layer further comprises a dispersant. 5 . A lithium secondary battery comprising a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein the separator is a separator for a lithium secondary battery as defined in any one of claims 1 to 4 .
Citation Information
Patent Citations
Method for interworking messenger service
KR1020190135852A
Lithium secondary battery containing high energy density positive electrode materials and organic / inorganic composite microporous separator membrane
CN102341939A
Separator for secondary battery and lithium secondary battery comprising same
CN108463904A
Separator for electrochemical device and manufacturing method thereof
CN111615761A
Separator for lithium secondary battery having enhanced electrode adhesive strength and improved resistance characteristics, and
CN114144931A