Method for online detection of failure of insulating pads for isolating galvanic connection of marine ship pipelines

By measuring the low-frequency real intercept value of the parallel AC impedance spectrum of the ship pipeline system online, combined with electrochemical parameters, the measurement inaccurate problem caused by parallel short circuit in seawater is solved, and the reliability evaluation of the failure degree of insulation pad is achieved, and the electricity is reduced The risk of corrosion and maintenance costs of occasional corrosion improve the safety and management efficiency of ship pipeline systems.

CN114384126BActive Publication Date: 2024-11-26SHANDONG ZHONGZHI CHEMICAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111651024.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-30
Publication Date
2024-11-26
Estimated Expiration
2041-12-30

AI Technical Summary

Technical Problem

When the prior art detects the failure degree of the insulating pad of the ship piping system, the measurement results are inaccurate due to the short circuit of the sea water in parallel, and the isolation resistance of the insulating pad cannot be reliably evaluated, resulting in misleading the maintenance plan and increasing the service risk.

Method used

By measuring the low-frequency real-part intercept value of the parallel AC impedance spectrum between ship pipelines, combining electrochemical parameters and impedance spectrum analysis, the failure degree of the insulating pad is accurately evaluated, and a two-electrode method and an electrochemical workstation with high accuracy is adopted. Perform measurements to separate the impedance of seawater and insulating pads to provide reliable maintenance decision data.

Benefits of technology

Early detection of the aging and installation damage of the insulation pad is achieved, and maintenance personnel are promptly reminded to replace the failed insulation pad, reducing the risk of galvanic corrosion, and improving the safety and efficiency management of the ship's pipeline system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114384126B_ABST
    Figure CN114384126B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for online detection of the failure of an insulating pad of an isolated galvanic connection of a marine ship pipeline. In order to prevent the occurrence of galvanic corrosion in a ship's multi-metal pipeline system due to the aging and failure of the insulating pad and the loss of isolation capability, the present invention relates to a method for quickly and reliably detecting / monitoring the degree of aging and failure of the isolated insulating pads between seawater pipelines of marine ships, including online measurement of the numerical value of the low-frequency real part intercept of the parallel AC impedance spectrum of the insulating pads between the ship's pipelines, thereby evaluating the degree of failure of the isolated insulating pads between the multi-metal pipelines, thereby reliably detecting the insulation performance of the insulating pads between the pipelines, and avoiding the occurrence of galvanic corrosion of the equipment to increase the risk of service.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a detection method for preventing galvanic corrosion from occurring in a multi-metallic piping system of a ship, and in particular to a method for rapidly detecting / monitoring the failure degree of an isolation insulating pad for preventing galvanic connection between seawater pipelines of a marine ship. Background Art

[0002] Large marine ships are equipped with complex seawater pipeline systems. Since the pipeline is composed of multiple metals and forms a galvanic corrosion system due to the short circuit of seawater, and the hull and various equipment are loaded with cathodic protection, the whole pipeline is coupled with seawater to form a complex galvanic corrosion system composed of multi-metal coupling current + cathodic protection current + stray current, which threatens the safe operation of the hull equipment. The detection and control of galvanic corrosion of marine ship pipelines has always been the most concerned service safety issue for ship operators. The most effective conventional method for controlling galvanic corrosion of pipelines is to use insulating gaskets between different metal pipelines to implement electrical insulation isolation technology, control the coupling between each local galvanic current and stray current, and eliminate / weaken various forms of galvanic corrosion current. However, due to the common reasons such as the long-term operation aging failure of the insulating gasket, which reduces the insulation capacity, and the complexity of many coupling equipment and imperfect construction that destroys the insulation performance of the gasket, the galvanic corrosion of the long-term operation of the ship pipeline system is difficult to avoid, and galvanic corrosion accidents often occur. Some new ships have galvanic corrosion pipeline perforation accidents within a few months, which reduces the service life of the equipment and increases the maintenance cost and the risk of major accidents.

[0003] Therefore, it is necessary to regularly detect / monitor the galvanic corrosion process of the hull-pipeline system, promptly discover and replace failed insulation components in the system, eliminate / weaken the galvanic corrosion process with potential risks, and ensure the safe operation of ship pipeline equipment. The simplest method for testing the insulation performance of insulating pads is to drain the water and test the insulation resistance of the insulating pads offline, which is not feasible when the offshore ship is in operation. Another simple method is to connect an ammeter in series in the pipeline loop to measure the coupling current. This is equivalent to short-circuiting the pipeline system, which is not feasible even for a short time.

[0004] In view of this, some zero-resistance galvanometers and insulation resistance testers that are directly connected in parallel to the two ends of the insulation pads between online metal pipelines to measure the insulation resistance have been developed at home and abroad to detect the degree of insulation resistance drop when the insulation pads fail. Summary of the invention

[0005] However, there is a problem with the prior art method for detecting the degree of insulation resistance drop of failed insulating gaskets, that is, during online measurement, the flowing seawater in the pipeline short-circuits the insulating gaskets between the metal pipes in parallel, so the measured value is not the isolation resistance of the insulating gasket, but the mixed resistance of the seawater in parallel. Because seawater is different from fresh water, it has a higher electrical conductivity. The parallel measurement result is significantly lower than the actual insulation resistance of the gasket, and it is impossible to reliably evaluate the failure degree of the gasket. It will also mislead the maintenance plan and replace the insulating gasket that has not failed. In addition, during online measurement, since seawater flows in the entire pipeline system, in addition to the insulating gasket to be tested, all other pipelines, hulls and cathodic protection systems are connected in parallel. The measured value will be smaller, and the protective performance of the insulating gasket cannot be accurately and reliably detected. Series measurement is not feasible, and parallel measurement is unreliable. The detection / monitoring method of the galvanic corrosion tendency of marine ship pipelines has been one of the difficult problems in the field of marine ship equipment corrosion detection for many years.

[0006] In order to reliably detect the insulation performance of insulating pads between pipelines and avoid galvanic corrosion of equipment to increase service risks, the present invention proposes a reliable method for detecting / monitoring the galvanic corrosion tendency of ship piping systems.

[0007] In order to solve the above technical problems, the present invention is achieved through the following technical solutions:

[0008] The present invention firstly proposes a method for online detection of failure of insulating pads of marine ship pipeline isolation couple connections, which is characterized by online measurement of the numerical value of the low-frequency real part intercept of the parallel AC impedance spectrum of the insulating pads between ship pipelines, so as to evaluate the failure degree of the isolation insulating pads between multi-metal pipelines.

[0009] Furthermore, in a specific embodiment, the method comprises the following steps:

[0010] 1) First, find out the metal material of the pipes at both ends of the insulating pad to be tested and the polarization curves and behavior rules of the cathode / anode electrode process in seawater in the literature to obtain relevant electrochemical parameters;

[0011] 2) Process an AC impedance connection measurement terminal on each of the metal pipes at both ends of the online insulation pad to be tested, for measuring the electrochemical impedance spectrum of the insulation pad;

[0012] 3) Select an electrochemical workstation with target accuracy and impedance spectrum measurement function, use a two-electrode method to connect the two terminals on both sides of the insulating pad to be measured to form an electrochemical impedance measurement circuit, then turn on the workstation and set impedance measurement parameters;

[0013] 4) Check that the circuit connection and measurement parameter settings are correct. When the seawater is flowing in the pipeline, start the measurement after the open circuit potential is stable. After completion, record the measurement results, turn off the machine, and remove the measurement terminals; and

[0014] 5) Analyze the reliability of the electrochemical impedance spectrum of the parallel insulating pad, including accuracy and noise level. If it is reliable, the next step of data analysis can be carried out; if it is wrong, find out the cause and re-measure; thus, the failure degree of the insulating pad can be evaluated based on the analysis and measurement results.

[0015] In a further preferred embodiment, the method of the present invention, when performing step 5) of "analyzing the reliability of the electrochemical impedance spectrum of the parallel insulating pad", specifically comprises the following steps:

[0016] 6) First, determine the number of capacitive reactance arcs and diffusion oblique lines in the impedance spectrum and their frequency range based on the Bode diagram of the impedance spectrum and the Nyquist diagram when necessary, and determine the variation range of the insulation pad impedance; and

[0017] 7) Then find out the shape of the low-frequency impedance spectrum. If it is an upward sloping line, it can be confirmed that the insulating pad still maintains sufficient insulation resistance and isolation performance and does not need to be replaced. If it is a downward capacitive reactance arc, fit the full-range capacitive reactance arc and obtain the low-frequency real axis intercept data, which is the insulation pad resistance value. Evaluate the failure degree of the insulation pad based on experience and decide whether it needs to be shut down for replacement.

[0018] In a further preferred embodiment, the method of the present invention is characterized in that when the method performs step 5), it also includes step 8):) according to actual needs and requirements, select repeated measurements until the measurement results meet the requirements, and save the measurement results for reference for the next measurement.

[0019] Furthermore, in a more preferred embodiment, the electrochemical parameters in step 1) include anode process polarization resistance, cathode process polarization resistance, diffusion process and solution resistance.

[0020] Further, in a more preferred solution, setting the impedance measurement parameters in step 3) includes setting impedance open circuit potential measurement, sine wave 10mV disturbance, frequency range of 1MHz-1mHz and octave of 10.

[0021] Beneficial effects of the present invention:

[0022] The method for online detection of failure of insulating pads for isolating galvanic connections of marine ship pipelines according to the present invention has the following effects.

[0023] 1) It can measure the early information of aging failure and installation damage of the insulation pad, and promptly remind the operator to pay attention to the performance changes of the insulation pad.

[0024] 2) The whole failure information of the insulation pad can be obtained, which can be used by operators to analyze the failure cause in order to improve the operation method or select insulation pad products with more stable performance;

[0025] 3) After accumulating long-term insulation pad aging data, a database of insulation pads in key parts of the ship is established. The potential values ​​on both sides of the insulation pads are measured using a simplified potential measurement method and compared with the impedance measurement data in the database to analyze and determine the performance changes of the insulation pads. This advantage can collect potential data on both sides of the key insulation pads and wirelessly transmit it back to the data center, realize remote monitoring of insulation pad performance, and efficiently manage the galvanic corrosion behavior of the ship's pipeline system. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The schematic diagram of the device structure of the ship pipeline formed by the seawater separated by the insulating pad and flowing through two different metal pipes and the insulating pad and seawater is described.

[0027] Figure 2 yes Figure 1 The simulated equivalent circuit diagram of the ship piping device structure is shown.

[0028] Figure 3 It describes the insulation pad resistance R m The Bode impedance spectrum response of the equivalent circuit measured when the value changes from 1E9 ohms to 1E2 ohms corresponds to the entire figure.

[0029] Figure 4a It describes the insulation pad resistance R m The full response graph of the Nyquist impedance spectrum of the equivalent circuit when the value changes from 1E9 ohms to 1E2 ohms;

[0030] Figure 4b It describes the insulation pad resistance R m Detail of the <1E6 response of the Nyquist impedance spectrum of the equivalent circuit when the value changes from 1E9 ohms to 1E2 ohms;

[0031] Figure 4c It describes the insulation pad resistance R m Detail of the <1E4 response of the Nyquist impedance spectrum of the equivalent circuit when the value changes from 1E9 ohms to 1E2 ohms;

[0032] Figure 4d It describes the insulation pad resistance R m Detail of the <1E3 response of the Nyquist impedance spectrum of the equivalent circuit when the value changes from 1E9 ohms to 1E2 ohms;

[0033] Figure 4e It describes the insulation pad resistance R m The Nyquist impedance spectrum of the equivalent circuit is measured when the value changes from 1E9 ohms to 1E2 ohms. 1E2 means 10exp(2), and so on.

[0034] Figure 5 It describes the actual insulation pad Rm Values ​​and calculated R m The fitted result graph of the values.

[0035] Description of Reference Numerals

[0036] 1-seawater, 2-pipeline, 3-flange, 4-bolt, 5-insulation pad DETAILED DESCRIPTION

[0037] The technical scheme of the method for detecting galvanic corrosion of a pipeline system of the present invention will be further described below in conjunction with the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only exemplary examples of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0038] As mentioned above, parallel measurement is the only feasible method for online measurement, but the DC resistance of the insulation pad cannot be measured due to the parallel shunting of seawater, and the true insulation resistance cannot be obtained, and the isolation performance of the insulation pad cannot be accurately evaluated. However, the AC impedance response of the insulation pad of the measuring pipeline can identify and separate the impedance of seawater and the impedance of the insulation pad, and can accurately judge the isolation performance of the insulation pad.

[0039] like Figure 1 As shown in FIG. 1 , it describes a schematic diagram of a device structure of a ship pipeline + insulating pad 5 + seawater 1 formed by seawater 1 separated by an insulating pad 5 flowing through two different metal pipes 2, wherein the insulating pad 5, flange 3 and bolt 4 isolate the direct connection of the two metal pipes 2, and the seawater in the two pipes 2 still maintains a flow connection. The analog equivalent circuit diagram of this structure is shown in FIG. Figure 2 As shown. Among them, the insulation pad equivalent circuit consists of resistor R m and C m Parallel representation; the equivalent circuit of seawater in the pipeline is shown in the figure, R ct,a Represents the anode process of the left pipeline, R ct,c represents the cathode process of the right pipeline; the double-layer capacitance of the left anode and the right cathode are represented by C dl,a and C dl,c ; The cathode process in the seawater of the right pipeline is oxygen reduction reaction, which is controlled by the diffusion of dissolved oxygen, and W O2 Indicates that the solution resistance of the seawater in the pipeline is R sol ; The anode process and cathode process in the seawater pipeline and the solution resistance are connected in series, and then connected with the insulation pad resistance R m and capacitor C m In addition, the rate-controlling step of the coupled anode and cathode processes in the pipeline seawater is the oxygen diffusion step W in the cathode process. O2 Therefore, the determining factor for the current density in the pipeline seawater loop is the oxygen diffusion step W O2.

[0040] Obviously, the equivalent circuit of the impedance response has not only resistance response but also capacitance response. These responses can be clearly expressed in the frequency domain to show the difference between the response of the insulation pad and the process response of the seawater electrode and the resistance response of the seawater solution. They can also be clearly identified and accurately analyzed and calculated in the frequency domain, thereby separating the change in the insulation pad resistance and the degree of failure, providing engineers with reliable maintenance decision-making data. The following is a simple analysis and evaluation of them.

[0041] like Figure 1-2 As shown in the figure, the equivalent circuit shows that the impedance spectrum response at both ends of A and B is composed of the insulation pad branch and the pipeline seawater branch in parallel. m The value should be above 1E8 ohms. At this time, the impedance of the seawater loop is lower and becomes the main loop, showing diffusion control characteristics. The low-frequency impedance will gradually move away from the real axis and will not intersect with the real axis. The insulation resistance R m will drop significantly, the resistive characteristics of the insulating pad loop will gradually increase, and have an increasing impact on the impedance spectrum, that is, it gradually approaches the real axis. Therefore, in the low-frequency region, the low-frequency impedances of the above two loops exist in two directions respectively, and the total impedance changes as the frequency decreases, depending on the parallel value of the impedance change of the seawater pipeline away from the real axis and the impedance change of the insulating pad loop gradually approaching the real axis. If the impedance of the insulating pad is greater than the impedance of the seawater pipeline, the total impedance depends on the impedance of the seawater loop; if the impedance of the insulating pad is less than the impedance of the seawater pipeline, the total impedance depends on the impedance of the insulating pad loop; the balance of the two depends on the average value of the two. Since the DC resistance of the seawater loop is R ct,a , R ct,c and R sol and W O2 The total resistance of the insulating pad R is usually much greater than 10k ohms. m When it decreases close to this value, its proportion in the parallel resistance will increase. When it is less than this value, it will become the main contributor to the parallel resistance, indicating that the degree of failure of the insulation pad has increased, thereby increasing the risk of galvanic corrosion of the pipeline and requiring maintenance measures.

[0042] Figure 3 and Figure 4a-4e Describes Figure 2 In the simulation equivalent circuit, other parameters are kept unchanged, R m Bode impedance spectrum measured when the value changes from 1E9 ohms to 1E2 ohms ( Figure 3 ) and Nyquist impedance spectroscopy ( Figure 4a-4e ) responds to changes in details. Its main features are as follows.

[0043] (1) See Appendix Figure 3 , Figure 3The insulation pad resistance is shown to be 1E2-1E9ohm / cm 2 (Ohm / cm 2 )hour, Figure 2 The electrochemical impedance spectrum (Bode diagram) of the equivalent circuit corresponds to the full diagram. Obviously, the impedance spectrum details are difficult to see when the insulation pad resistance Rm is low. Figure 3 The Bode diagram shows that all impedance spectra have two time constants and a diffusion process; obviously Figure 3 In the situation shown, it is difficult to find out the detailed changes. It is necessary to further check the Nyquist diagram and calculate the low-frequency real axis intercept data to obtain the changes in the insulation pad resistance Rm.

[0044] (2) See Appendix Figure 4a , Figure 4a The insulation pad resistance is shown to be 1E2-1E9ohm / cm 2 (Ohm / cm 2 )hour, Figure 2 The electrochemical impedance spectrum (Nyquist diagram) of the equivalent circuit corresponds to the full diagram. When the insulation pad resistance Rm is low, the impedance spectrum details are still difficult to see clearly; that is to say, it can be seen that the diffusion process increases with Rm. m The decrease gradually weakens and m Almost disappears at <1E4 ohms;

[0045] (3) See Appendix Figure 4b , Figure 4b The insulation pad resistance is shown to be 1E2-1E5ohm / cm 2 hour, Figure 2 EIS (Nyquist plot) of the equivalent circuit, local detail response, medium insulation pad resistance Rm = 1E5 ohm / cm 2 When Rm can be accurately measured and calculated; R m >1E7 low frequency impedance spectrum is far away from the real axis; R m The impedance spectrum in the low-frequency region <1E7 ohms begins to approach the real axis;

[0046] (4) See Appendix Figure 4c , Figure 4c The insulation pad resistance is shown to be 1E2-1E4ohm / cm 2 hour, Figure 2 EIS (Nyquist plot) of the equivalent circuit, local detail response, medium insulation pad resistance Rm = 1E4 ohm / cm 2 When Rm can be accurately measured and calculated; R m <1E5 ohm low frequency impedance spectrum close to the real axis, diffusion control and R m The capacitive reactance response is controlled together, and another capacitive reactance arc appears at high frequency; R mThe impedance spectrum in the low-frequency region of <1E4 ohms is close to the real axis, and a capacitive reactance arc appears at high frequencies. The original diffusion process and the insulating pad capacitive reactance process are mixed and controlled, and the latter gradually becomes dominant.

[0047] (5) See Appendix Figure 4d , Figure 4d The insulation pad resistance is shown to be 1E2-1E3 ohm / cm 2 hour, Figure 2 The local detail response of the electrochemical impedance spectroscopy (Nyquist plot) of the equivalent circuit. The medium insulation pad resistance value Rm = 1E3 ohm / cm 2 When Rm is , it can be accurately determined and calculated. m <1E3 ohm low frequency impedance spectrum is close to the real axis; there are two time constants, low frequency R m The impact of capacitive arc is getting bigger and bigger;

[0048] (6) See Appendix Figure 4e , Figure 4e The insulation pad resistance is shown to be 1E2-1E2ohm / cm 2 hour, Figure 2 The local details of the electrochemical impedance spectrum (Nyquist plot) of the equivalent circuit show that the resistance of the insulation pad is very low, Rm = 1E2 ohm / cm. 2 When Rm<1E2 ohm, the impedance spectrum in the low frequency region is close to the real axis; there are two time constants; the influence of high frequency capacitive reactance arc is getting bigger and bigger, but the low frequency R m The capacitive reactance arc is still the main impedance response.

[0049] See attached Figure 4a-4e , it is more clearly seen in the detailed Nyquist plot that R m >1E7, the low-frequency impedance spectrum still gradually moves away from the real axis, showing that the impedance response is mainly controlled by seawater diffusion; m <1E7 gradually decreases, and the low-frequency impedance spectrum becomes closer and closer to the real axis; below 1E5, the diffusion effect of the seawater pipeline gradually weakens, and the impedance spectrum is mainly the insulation pad resistance R m The main low-frequency capacitive reactance arc response.

[0050] Therefore, the Rm value calculated by the capacitive reactance arc of the fitted impedance spectrum is shown in Table 1.

[0051] Table 1 Actual insulation pad R m R calculated by fitting the capacitive reactance arc 拟合 Value comparison

[0052] <![CDATA[Actual R m value]]> <![CDATA[Fitting calculation of R 拟合 value]]> 1E7 9.5272E6 1E6 9.7919E5 1E5 99200 1E4 10023 5E3 5024.3 1E3 990.03 5E2 485.56 2E2 185.91 1E2 87.51

[0053] Figure 5 According to Table 1 and Figure 2Equivalent circuit, fitting comparison results of calculated and actual values ​​of pipeline insulation pad resistance Rm. The figure shows that the actual insulation pad R m Values ​​and calculated R 拟合 The value fitting degree is close to 1, so the measured coupling capacitive reactance arc fitting result R 拟合 Speculation R m value.

[0054] In addition, according to Figure 2 The equivalent circuit diagram shows that the insulation pad circuit and the seawater circuit are completely connected in parallel, and there are no shared components. m The small high-frequency capacitive reactance arc seen in the case is also the joint contribution of the solution resistance / insulating pad resistance in parallel with the insulating pad. Therefore, it is more reliable to obtain Rm by directly calculating the low-frequency intercept of the impedance spectrum.

[0055] Based on the above analysis, the patent proposes a method and implementation process for online measurement of the isolation resistance of the insulation pad of the running pipeline, which includes the following steps:

[0056] 1. First, find out the metal material of the pipes at both ends of the insulation pad to be tested and the steady-state polarization curves and behavior laws of the cathode / anode electrode process in seawater in the literature to obtain the polarization resistance R of the anode process of the seawater branch. ct,a , cathode process polarization resistance R ct,c and the diffusion process impedance W O2 and solution resistance R sol Electrochemical data (anode double layer capacitance C dl,a and cathode double layer capacitance C dl,c , for the insulation pad resistance R m The measurement has little impact and can be ignored), which is used to determine the seawater impedance data range of the branch parallel to the insulation pad to be tested, as well as the expected change range of the resistance of the intact insulation pad and the failure insulation pad and their proportion in the total impedance, so as to determine the failure degree of the insulation pad;

[0057] 2. Process an AC impedance connection measurement terminal on the metal pipes at both ends of the online insulation pad to be tested, for measuring the electrochemical impedance spectrum of the insulation pad;

[0058] 3. Select an electrochemical workstation with suitable accuracy and impedance spectrum measurement function (Gamrry, Ametek, Wan Tong, etc. can be used), and use the two-electrode method (working electrode at one end, auxiliary electrode and reference electrode short-circuited at the other end) to connect the two terminals of the insulation pad to be tested to form an electrochemical impedance measurement circuit. Then turn on the machine and set the impedance measurement parameters, such as open circuit potential measurement, sine wave 10mV disturbance, frequency range of 1MHz-1mHz, octave 10, etc.;

[0059] 4. Check that the circuit connection and measurement parameter settings are correct. When the seawater is flowing in the pipeline, start the measurement after the open circuit potential is stable. After completion, record the measurement results, turn off the machine, and remove the measurement terminals.

[0060] 5. Open the electrochemical impedance analysis software such as ZView on the computer, call in the measured electrochemical impedance spectrum of the parallel insulating pad, and first analyze the reliability of the measured impedance spectrum, including accuracy and noise level. If it is reliable, the next step of data analysis can be carried out; if it is wrong, find out the cause and re-measure;

[0061] 6. First, determine how many capacitive reactance arcs and diffusion oblique lines exist in the impedance spectrum based on the Bode diagram and further combine the Nyquist diagram as needed, and determine the frequency range in which they are located to determine the impedance variation range of the insulating pad;

[0062] 7. Then find out whether the low-frequency impedance spectrum is an upward sloping line or a downward capacitive reactance arc. If it is the former, it can be confirmed that the insulating pad still maintains sufficient insulation resistance and isolation performance and does not need to be replaced; if it is the latter, use impedance analysis software such as Zview from high frequency to low frequency to fit a single capacitive reactance arc to obtain the parallel DC resistance value, that is, R 拟合 =1 / (1 / R m +1 / (R ct,a +R ct,c +R sol +W O2 )). From this formula, we can see that R m The smaller the R ct,a +R ct,c +R sol +W O2 As shown in Table 1, R 拟合 The closer the value is to the true value of the insulation pad resistance R m .

[0063] During the test, the Bode diagram is measured first. If the low-frequency impedance spectrum is an upward sloping line, there is no need to test the Nyquist diagram. This can confirm that the insulation pad still maintains sufficient insulation resistance and isolation performance and does not need to be replaced. If the measured low-frequency impedance spectrum is a downward capacitive reactance arc, the Nyquist diagram needs to be further measured and fitted. Figure 4a-4e The method can accurately calculate the resistance value Rm of the insulation pad with different degrees of damage from the fine Nyquist impedance spectrum, and determine whether it needs to be replaced. Figure 5 According to Table 1 and Figure 2 Comparison results of the calculated and true values ​​of the pipe insulation pad resistance Rm in the equivalent circuit. It can be seen that the pipe insulation pad resistance Rm measured and calculated using the above method are highly linearly correlated, and the results are reliable.

[0064] During the fitting process, the data with excessive noise deviation is usually deleted first to avoid affecting the fitting accuracy; then the data fitting range is selected and the low-frequency real axis intercept data R is calculated by fitting. 拟合 , which is the parallel resistance value of the seawater branch and the insulation pad branch resistance. The failure degree of the insulation pad can be evaluated according to the value and it can be decided whether it needs to be shut down for replacement.

[0065] 8. If you are not satisfied with the result, you can repeat the measurement until you are satisfied. If you are satisfied, save the measurement result for reference next time.

[0066] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for online detection of failure of insulating pads of isolated galvanic connections of marine ship pipelines, characterized in that: A method for evaluating the failure degree of isolation insulation pads between multi-metal pipelines by online measuring the low-frequency real intercept value of the parallel AC impedance spectrum of the insulation pads between ship pipelines; The method comprises the following steps: 1) First, find out the metal material of the pipes at both ends of the insulating pad to be tested and the polarization curves and behavior rules of the cathode / anode electrodes in seawater to obtain relevant electrochemical parameters; Wherein, the electrochemical parameters in step 1) include anode process polarization resistance, cathode process polarization resistance and diffusion process and solution resistance; 2) Process an AC impedance connection measurement terminal on each of the metal pipes at both ends of the online insulation pad to be tested, for measuring the electrochemical impedance spectrum of the insulation pad; 3) Select an electrochemical workstation with target accuracy and impedance spectrum measurement function, use a two-electrode method to connect the two terminals on both sides of the insulating pad to be measured to form an electrochemical impedance measurement circuit, then turn on the workstation and set impedance measurement parameters; 4) Check that the circuit connection and measurement parameter settings are correct. When the seawater is flowing in the pipeline, start the measurement after the open circuit potential is stable. After completion, record the measurement results, turn off the machine, and remove the measurement terminals; and 5) Analyze the reliability of the electrochemical impedance spectrum of the parallel insulation pad. If it is reliable, proceed to the next step of data analysis; if it is wrong, find out the cause and re-measure; thus, evaluate the failure degree of the insulation pad based on the analysis and measurement results; Wherein, when performing step 5) of "analyzing the reliability of the electrochemical impedance spectrum of the parallel insulating pad", the following steps are specifically included: 6) First, determine the number of capacitive reactance arcs and diffusion oblique lines existing in the impedance spectrum and the frequency range in which they are located based on the Bode diagram and / or Nyquist diagram of the impedance spectrum, and determine the variation range of the insulation pad impedance; and 7) Then find out the shape of the low-frequency impedance spectrum. If it is an upward sloping line, it is confirmed that the insulating pad still maintains sufficient insulation resistance and isolation performance and does not need to be replaced. If it is a downward capacitive reactance arc, fit the full-range capacitive reactance arc and obtain the low-frequency real axis intercept data, which is the insulation pad resistance value. Evaluate the failure degree of the insulation pad based on experience and decide whether it needs to be shut down for replacement.

2. The method according to claim 1, characterized in that When the method performs step 5), it also includes step 8): according to actual needs and requirements, repeat the measurement until the measurement result meets the requirements, and save the measurement result for reference for the next measurement.

3. The method according to claim 1 or 2, characterized in that: Setting the impedance measurement parameters in step 3) includes setting the impedance open circuit potential measurement, the sine wave 10mV disturbance, the frequency range of 1MHz-1mHz and the octave of 10.