A method for preparing high-molybdenum-high-silicon-cobalt-based thermal spray alloy powder

Through the prefabricated master alloy and ultrasonic gas atomization process, the problems of composition uniformity and impurity control of high molybdenum high silicon-cobalt-based alloy powder were solved, and high molybdenum high silicon-cobalt-based thermal spray alloy powder with excellent wear and corrosion resistance were prepared. Suitable for parts protection in high temperature environments.

CN114570933BActive Publication Date: 2024-11-22INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011382741.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-30
Publication Date
2024-11-22
Estimated Expiration
2040-11-30

AI Technical Summary

Technical Problem

Under high temperature environment, it is difficult for the prior art to effectively control the chemical composition and impurity content of high molybdenum, high silicon, cobalt-based alloy powder, resulting in insufficient wear and corrosion resistance of the coating, and large differences in the melting point of the raw materials make it difficult to ensure the uniformity of the alloy composition .

Method used

The prefabricated master alloy + ultrasonic gas atomization two-step process is adopted to prepare the master alloy ingot through vacuum induction smelting, and the ultrasonic gas atomization technology uses argon as the medium to control the atomization pressure and temperature to achieve the uniform composition of the alloy powder and Particle size screening ensures that the alloy composition and impurity content are within the specified range.

Benefits of technology

It realizes effective control of the chemical composition, impurity content and particle size of high molybdenum, high silicon, cobalt-based thermal spray alloy powder, improves the fluidity and loose density of the coating, provides high-quality wear-resistant and corrosion-resistant protection, and is suitable for Aviation, metallurgy, machinery and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114570933B_ABST
    Figure CN114570933B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of thermal spray coating materials, and specifically to a method for preparing a high-molybdenum, high-silicon, cobalt-based thermal spray alloy powder. A two-step process of "prefabricated master alloy + ultrasonic gas atomization" is adopted: (1) vacuum induction melting to prepare a master alloy ingot: heating when the vacuum degree is not greater than 5Pa, refining temperature 1550±50℃, refining time 8min~20min, and then pouring into an atomized alloy ingot. (2) ultrasonic gas atomization to prepare a powder: heating when the vacuum degree is not greater than 5Pa, stopping vacuuming when the melting temperature is 1460±50℃, filling argon gas into the furnace to normal pressure, and then adding silicon to continue melting for 2~5min before atomization, the atomization medium is argon gas, the atomization pressure is 8MPa~11MPa, and the alloy liquid flow rate is 3.5kg / min~5.5kg / min. The powder obtained by the present invention has uniform composition, low impurity content, good sphericity, and is conducive to the preparation of high-quality wear-resistant and corrosion-resistant coatings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of thermal spray coating materials, in particular to a method for preparing wear-resistant and corrosion-resistant high-molybdenum and high-silicon cobalt-based thermal spray alloy powder in a high-temperature environment. Background Art

[0002] With the continuous development of modern industry, technical equipment needs to operate under higher working parameters and harsher service environments, and parts are often in harsh working conditions such as high wear, high load, high temperature and corrosion. In order to extend the service life and improve the operating accuracy and stability, coating protection on the surface of parts is an effective means. High-molybdenum, high-silicon cobalt-based alloy coatings have excellent wear resistance, abrasion resistance, corrosion resistance, high-temperature oxidation resistance and abrasive wear resistance, and good high-temperature red hardness. They are used for surface protection of important parts such as landing gear, bearings, piston rings, and turbine casings. Therefore, it is necessary to develop a method for preparing high-molybdenum, high-silicon cobalt-based thermal spray alloy powder, effectively control the alloy composition and impurity content of the powder, and provide a basis and guarantee for the preparation of wear-resistant and corrosion-resistant coatings with excellent performance. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing wear-resistant and corrosion-resistant high-molybdenum, high-silicon, cobalt-based thermal spray alloy powder under high-temperature environment. The alloy powder material prepared by this method has uniform chemical composition, low impurity content and high powder yield, providing reliable material guarantee for the preparation of high-quality wear-resistant and corrosion-resistant protective coatings.

[0004] The technical solution of the present invention is:

[0005] A method for preparing high-molybdenum and high-silicon cobalt-based thermal spray alloy powder adopts a two-step process of "prefabricated master alloy + ultrasonic gas atomization". The chemical composition and impurity content of the alloy powder are as follows by weight percentage: Co balance; Cr: 16-19; Mo: 27-30; Si: 3-4; Fe≤1.50; O≤0.15; Ni≤1.00; C≤0.03; P≤0.03; S≤0.02.

[0006] The method for preparing the high-molybdenum-high-silicon-cobalt-based thermal spraying alloy powder comprises the following steps:

[0007] Step 1: Master alloy ingot preparation

[0008] The master alloy ingot is prepared by vacuum induction melting method, and the raw materials of cobalt, molybdenum and chromium are placed in a magnesium-aluminum crucible; vacuum is drawn, and heating is performed when the vacuum degree is not greater than 5Pa, the refining temperature is 1550±50℃, the refining time is 8min-20min, and then the alloy ingot is cast into an atomized alloy ingot;

[0009] Step 2: Powder gas atomization preparation

[0010] The powder material is prepared by ultrasonic gas atomization technology. The atomized alloy ingot is placed in a magnesium-aluminum crucible, and silicon is placed in a feeding hopper. Vacuum is drawn, and heating is performed when the vacuum degree is not greater than 5Pa. When the melting temperature is 1460±50℃, the vacuum is stopped, and argon is filled into the furnace body to normal pressure. Then silicon is added and smelted for 2 to 5 minutes before atomization. The atomization medium is argon, the atomization pressure is 8MPa to 11MPa, and the alloy liquid flow rate is 3.5kg / min to 5.5kg / min.

[0011] Step 3: The powder prepared in step 2 is screened for particle size.

[0012] The preparation method of the high-molybdenum, high-silicon, cobalt-based thermal spray alloy powder utilizes the Hartman shock tube principle to accelerate high-pressure gas and generate a pulsed airflow with an oscillation frequency of 10,000 to 100,000 Hz. The airflow directly impacts the liquid metal flow, causing it to be atomized into tiny droplets. Subsequently, the droplets quickly condense into alloy powder after heat exchange with the gas during flight.

[0013] The preparation method of the high-molybdenum-high-silicon-cobalt-based thermal spraying alloy powder comprises, by weight percentage, a particle size composition of the alloy powder of: +325 mesh ≤ 5%, -325 mesh to +800 mesh ≥ 85%, and -800 mesh ≤ 10%.

[0014] The preparation method of the high-molybdenum-high-silicon-cobalt-based thermal spraying alloy powder has a fluidity of ≤20s / 50g and a bulk density of ≥4.6g / cm 3 .

[0015] The method for preparing high-molybdenum, high-silicon, cobalt-based thermal spraying alloy powder is characterized in that the alloy powder particles are spherical or nearly spherical.

[0016] The method for preparing high-molybdenum, high-silicon, cobalt-based thermal spraying alloy powder has a finished product rate of 45-65%.

[0017] The design ideas and principles of the present invention are as follows:

[0018] The high-molybdenum-high-silicon cobalt-based thermal spray alloy powder of the present invention adds excessive molybdenum and silicon, and a hard phase Laves phase will precipitate during the solidification process and be evenly dispersed in the soft cobalt alloy matrix, so that the material has excellent wear resistance and corrosion resistance. However, the melting points of molybdenum and silicon are quite different (the melting point of molybdenum is 2620°C, and the melting point of silicon is 1410°C). How to ensure the uniformity of the alloy composition during the smelting and atomization process of the raw materials is a technical problem. The present invention adopts a two-step process of "prefabricated master alloy + ultrasonic gas atomization" to achieve effective control of the alloy composition; at the same time, ultrasonic gas atomization technology is adopted and the atomization process parameters are optimized to achieve effective control of the particle size and morphology of the alloy powder.

[0019] The advantages and beneficial effects of the present invention are:

[0020] The chemical composition, impurity content, morphology and particle size of the high-molybdenum, high-silicon cobalt-based thermal spraying alloy powder prepared by the method of the present invention are effectively controlled, and the powder has excellent fluidity and bulk density, providing material guarantee for the preparation of high-quality coatings. The powder can be widely used in aviation, metallurgy, machinery, electric power and other fields, and has significant social and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a scanning electron microscope photograph of the high-molybdenum, high-silicon, cobalt-based thermal spray alloy powder in Example 1.

[0022] Figure 2 This is a scanning electron microscope photograph of the high-molybdenum, high-silicon, cobalt-based thermal spray alloy powder in Example 2.

[0023] Figure 3 This is a scanning electron microscope photograph of the high-molybdenum, high-silicon, cobalt-based thermal spray alloy powder in Example 3. DETAILED DESCRIPTION

[0024] In the specific implementation process, the preparation method of the high-molybdenum-high-silicon-cobalt-based thermal spraying alloy powder of the present invention, the chemical composition and impurity content of the high-molybdenum-high-silicon-cobalt-based thermal spraying alloy powder are shown in Table 1.

[0025] Table 1 Chemical composition and impurity content of high-molybdenum and high-silicon cobalt-based thermal spray alloy powder

[0026]

[0027] The two-step process of "prefabricated master alloy + ultrasonic gas atomization" is adopted to achieve effective control of the chemical composition of the powder. The specific process is as follows:

[0028] Step 1: Master alloy ingot preparation

[0029] The master alloy ingot is prepared by vacuum induction melting method, and the raw materials of cobalt, molybdenum and chromium are placed in a magnesium-aluminum crucible. Vacuum is drawn, and heating is performed when the vacuum degree is not greater than 5Pa, the refining temperature is 1550±50℃, the refining time is 8min~20min, and then the atomized alloy ingot is cast.

[0030] Step 2: Powder gas atomization preparation

[0031] Ultrasonic gas atomization technology is used to prepare powder materials. The Hartman shock tube principle is used to accelerate high-pressure gas and generate a pulsed airflow with an oscillation frequency of 10,000 to 100,000 Hz. The airflow directly impacts the liquid metal flow, atomizing it into tiny droplets. The droplets then exchange heat with the gas during flight and quickly condense into alloy powder.

[0032] Place the atomized alloy ingot in a magnesium-aluminum crucible and silicon in a charging hopper. Evacuate the furnace, heat when the vacuum is not greater than 5Pa, stop vacuuming when the melting temperature reaches 1460±50℃, fill the furnace with argon to normal pressure, then add silicon and continue melting for 2 to 5 minutes before atomization. The atomization medium is argon, the atomization pressure is 8MPa to 11MPa, and the alloy liquid flow rate is 3.5kg / min to 5.5kg / min.

[0033] Step 3: The powder prepared in step 2 is sieved for particle size, and the particle size composition meets the requirements of Table 2.

[0034] Table 2 Particle size composition of high molybdenum and high silicon cobalt-based thermal spray alloy powder

[0035] granularity +325 mesh -325 mesh~+800 mesh -800 mesh Content (wt%) ≤5% ≥85% ≤10%

[0036] In order to ensure that the impurity content meets the requirements, the preferred raw materials are:

[0037] (1) Cobalt (Co): electrolytic cobalt meeting the grade Co9995 or equivalent or higher specifications;

[0038] (2) Molybdenum (Mo): molybdenum bars with grades Mo-1 or Mo-2;

[0039] (3) Chromium (Cr): metallic chromium meeting the grade JCr98.5A or equivalent or higher specifications;

[0040] (4) Silicon (Si): Grade 3303 or equivalent or higher industrial silicon.

[0041] The present invention is further described in detail below through examples and drawings.

[0042] Example 1

[0043] In this embodiment, the preparation method of high-molybdenum-high-silicon-cobalt-based thermal spraying alloy powder is as follows:

[0044] Step 1: Master alloy ingot preparation

[0045] The master alloy ingot was prepared by vacuum induction melting. The raw materials of cobalt, molybdenum and chromium were placed in a magnesium-aluminum crucible, evacuated, heated at a vacuum degree of 3 Pa, the refining temperature was 1550°C, the refining time was 10 min, and then cast into an atomized alloy ingot.

[0046] Step 2: Powder gas atomization preparation

[0047] The powder was prepared by ultrasonic gas atomization equipment. The master alloy ingot was placed in a magnesium-aluminum crucible and silicon was placed in a hopper. Heating was performed when the vacuum degree was 2Pa. When the melting temperature was 1460℃, the vacuum was stopped. Argon was filled into the furnace to normal pressure. Then silicon was added. After smelting for 3 minutes, the atomization was performed. The atomization medium was argon, the atomization pressure was 10MPa, and the alloy liquid flow rate was 5.5kg / min. When the liquid alloy flowed through the atomization nozzle, it was broken into small droplets by the high-pressure and high-speed airflow. Then, the droplets quickly condensed into alloy powder after heat exchange with the gas during flight.

[0048] Step 3: The powder prepared in step 2 was sieved and the particle size composition is shown in Table 3.

[0049] Table 3 Particle size composition of alloy powder in Example 1

[0050] granularity +325 mesh -325 mesh~+800 mesh -800 mesh Content (wt%) 0.5% 95.3 4.2%

[0051] The high-molybdenum and high-silicon cobalt-based thermal spray alloy powder prepared in step 3 was characterized:

[0052] (1) The chemical composition and impurity content of high-molybdenum and high-silicon cobalt-based thermal spray alloy powder are shown in Table 4.

[0053] Table 4 Chemical composition and impurity content of the powder of Example 1

[0054]

[0055] (2) The fluidity of high-molybdenum and high-silicon cobalt-based thermal spray alloy powder is 16.0s / 50g, and the bulk density is 4.89g / cm 3 .

[0056] (3) The high-molybdenum and high-silicon cobalt-based thermal spray alloy powder particles are spherical or nearly spherical (such as Figure 1 ).

[0057] (4) The yield rate of high-molybdenum, high-silicon, cobalt-based thermal spraying alloy powder is 48.5%.

[0058] Example 2

[0059] The difference from Example 1 is that, in step 2: when preparing the powder by gas atomization, an ultrasonic gas atomization device is used to prepare the powder, the master alloy ingot is placed in a magnesium-aluminum crucible, and silicon is placed in a hopper. Heating is performed when the vacuum degree is 3Pa, and the vacuum is stopped when the melting temperature is 1450°C. Argon is filled into the furnace to normal pressure, and then silicon is added. After continuing to melt for 5 minutes, atomization is performed. The atomization medium is argon, the atomization pressure is 9MPa, and the alloy liquid flow rate is 4kg / min. When the liquid alloy flows through the atomization nozzle, it is broken into small droplets by the high-pressure and high-speed airflow, and then the droplets quickly condense into alloy powder after heat exchange with the gas during flight.

[0060] The powder prepared in Example 2 was subjected to particle size screening, and the particle size composition is shown in Table 5.

[0061] Table 5 Powder particle size composition of Example 2

[0062] granularity +325 mesh -325 mesh~+800 mesh -800 mesh content(%) 0.4% 92.8 6.8%

[0063] The high-molybdenum and high-silicon cobalt-based thermal spray alloy powder prepared in Example 2 was characterized:

[0064] (1) The chemical composition and impurity content of high-molybdenum and high-silicon cobalt-based thermal spray alloy powder are shown in Table 6.

[0065] Table 6 Chemical composition and impurity content of powder of Example 2

[0066]

[0067] (2) The high-molybdenum, high-silicon cobalt-based thermal spray alloy powder has a fluidity of 16.2s / 50g and a bulk density of 4.90g / cm 3 .

[0068] (3) The high-molybdenum and high-silicon cobalt-based thermal spray alloy powder particles are spherical or nearly spherical (such as Figure 2 ).

[0069] (4) The yield rate of high-molybdenum, high-silicon, cobalt-based thermal spraying alloy powder is 56.3%.

[0070] Example 3

[0071] The difference from Example 1 is that, in step 2: when preparing the powder by gas atomization, an ultrasonic gas atomization device is used to prepare the powder, the master alloy ingot is placed in a magnesium-aluminum crucible, and silicon is placed in a hopper. Heating is performed when the vacuum degree is 1Pa, and the vacuum is stopped when the melting temperature is 1470°C. Argon gas is filled into the furnace body to normal pressure, and then silicon is added. After continuing to melt for 4 minutes, atomization is performed. The atomization medium is argon gas, the atomization pressure is 8MPa, and the alloy liquid flow rate is 3.5kg / min. When the liquid alloy flows through the atomization nozzle, it is broken into small droplets by the high-pressure and high-speed airflow, and then the droplets quickly condense into alloy powder after heat exchange with the gas during flight.

[0072] The powder prepared in Example 3 was subjected to particle size screening, and the particle size composition is shown in Table 7.

[0073] Table 7 Powder particle size composition of Example 3

[0074] granularity +325 mesh -325 mesh~+800 mesh -800 mesh Content (wt%) 0.4% 92.9 6.7%

[0075] The high-molybdenum and high-silicon cobalt-based thermal spray alloy powder prepared in Example 3 was characterized:

[0076] (1) The chemical composition and impurity content of high-molybdenum and high-silicon cobalt-based thermal spray alloy powder are shown in Table 8.

[0077] Table 8 Chemical composition and impurity content of powder of Example 3

[0078]

[0079] (2) The high-molybdenum, high-silicon cobalt-based thermal spray alloy powder has a fluidity of 16.2s / 50g and a bulk density of 4.90g / cm 3 .

[0080] (3) The high-molybdenum and high-silicon cobalt-based thermal spray alloy powder particles are spherical or nearly spherical (such as Figure 3 ).

[0081] (4) The yield rate of high-molybdenum and high-silicon cobalt-based thermal spraying alloy powder is 60.3%.

[0082] The results of the examples show that the chemical composition, impurity content, fluidity, bulk density and particle morphology of the CoCrAlY alloy powder prepared by the method of the present invention are all within the required range, and the powder is uniform and dry. The powder obtained by the present invention has uniform composition, low impurity content and good sphericity, which is conducive to the preparation of high-quality wear-resistant and corrosion-resistant coatings.

Claims

1. A method for preparing high-molybdenum-high-silicon-cobalt-based thermal spraying alloy powder, characterized in that: The two-step process of "prefabricated master alloy + ultrasonic gas atomization" is adopted; the chemical composition and impurity content of the alloy powder are as follows by weight percentage: Co balance; Cr: 16-19; Mo: 27-30; Si: 3-4; Fe≤1.50; O≤0.15; Ni≤1.00; C≤0.03; P≤0.03; S≤0.02; The method for preparing the high-molybdenum-high-silicon-cobalt-based thermal spraying alloy powder comprises the following steps: Step 1: Master alloy ingot preparation The master alloy ingot is prepared by vacuum induction melting method, and the raw materials of cobalt, molybdenum and chromium are placed in a magnesium-aluminum crucible; vacuum is drawn, and heating is performed when the vacuum degree is not greater than 5Pa, the refining temperature is 1550±50℃, the refining time is 8min-20min, and then the alloy ingot is cast into an atomized alloy ingot; Step 2: Powder gas atomization preparation The powder material is prepared by ultrasonic gas atomization technology. The atomized alloy ingot is placed in a magnesium-aluminum crucible, and silicon is placed in a feeding hopper. Vacuum is drawn, and heating is performed when the vacuum degree is not greater than 5Pa. When the melting temperature is 1460±50℃, the vacuum is stopped, and argon is filled into the furnace body to normal pressure. Then silicon is added and smelted for 2 to 5 minutes before atomization. The atomization medium is argon, the atomization pressure is 8MPa to 11MPa, and the alloy liquid flow rate is 3.5kg / min to 5.5kg / min. Step 3: Screening the powder prepared in step 2; The Hartman shock tube principle is used to accelerate high-pressure gas and generate a pulsed airflow with an oscillation frequency of 10,000 to 100,000 Hz. The airflow directly impacts the liquid metal flow, atomizing it into tiny droplets. The droplets then exchange heat with the gas during flight and quickly condense into alloy powder.

2. The method for preparing high-molybdenum-high-silicon-cobalt-based thermal spraying alloy powder according to claim 1, characterized in that: Calculated by weight percentage, the particle size composition of the alloy powder is: +325 mesh ≤ 5%, -325 mesh to +800 mesh ≥ 85%, -800 mesh ≤ 10%.

3. The method for preparing high-molybdenum-high-silicon-cobalt-based thermal spraying alloy powder according to claim 1, characterized in that: The fluidity of the alloy powder is ≤20s / 50g and the bulk density is ≥4.6g / cm 3 .

4. The method for preparing high-molybdenum-high-silicon-cobalt-based thermal spraying alloy powder according to claim 1, characterized in that: The alloy powder particles are spherical or nearly spherical.

5. The method for preparing high-molybdenum-high-silicon-cobalt-based thermal spraying alloy powder according to claim 1, characterized in that: The alloy powder yield is 45-65%.