Polymeric compositions for optical fiber cable assemblies
By adding cross-linkable silanol functionalized polyolefin and hydroxyl-terminated poly(dimethylsiloxane) to the PBT-PE blend of the fiber optic buffer tube, the problem of kinking and dimensional stability of the fiber optic buffer tube is solved. Polymer compositions with high zero-shear viscosity and good mechanical properties are achieved.
Patent Information
- Application Number
- CN202080077241.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-11-03
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-11-03
AI Technical Summary
Existing fiber optic buffer tubes are prone to kinking during fiber installation, causing damage to the fiber. And after using injection-grade PBT to replace extrusion-grade PBT, the zero-shear viscosity decreases, affecting extrudability and dimensional stability.
A cross-linkable silanol functionalized polyolefin is added to the PBT-PE blend with a hydroxyl-terminated poly(dimethylsiloxane) and a condensation catalyst to form a polymer composition and cross-linked through an extrusion process , to improve zero-shear viscosity and maintain dimensional stability.
It achieves a zero-shear viscosity greater than 1000 PaS at 250°C, resists kink, and maintains good extrudability and dimensional stability. It is suitable for manufacturing buffer tubes with good mechanical properties.
Smart Images

Figure BDA0003629043920000061 
Figure BDA0003629043920000091 
Figure BDA0003629043920000251
Abstract
Description
Background Art Technical Field
[0002] The present disclosure relates generally to polymer compositions, and more particularly to polymer compositions comprising a blend of polybutylene terephthalate and polyethylene for use in fiber optic cable components. Background Art
[0003] Materials used in optical fiber buffer tubes need to exhibit a balance between rigidity, flexibility, extrudability, and kink resistance. Conventional buffer tubes are primarily composed of extruded polybutylene terephthalate ("PBT"), which provides rigidity, but is prone to kinking during optical fiber installation. Kinking of the buffer tube is undesirable because it may cause damage to the optical fiber within the buffer tube.
[0004] Traditional methods of increasing the flexibility of buffer tubes include blending PBT and polyethylene ("PE"). In such blends, PBT provides rigidity and resistance to telecommunication grease, while PE provides flexibility and kink resistance. Due to the polar nature of polyesters and the non-polar nature of polyolefins, PBT and PE blends incorporate compatibilizers to facilitate blending. An example of a conventional compatibilizer is maleic anhydride grafted polyethylene ("MAH-g-PE"). WO2019050627 discloses PBT and PE blends using MAH-g-PE as a compatibilizer.
[0005] Recently, attempts have been made to replace extrusion-grade PBT (i.e., PET having a melt flow index of less than 21 grams per 10 minutes (g / 10 min) at 250°C and 2.16 kg) with relatively inexpensive injection-grade PBT (i.e., PBT having a melt flow index of 21 g / 10 minutes (min) or more) in PBT-PE buffer tubes. The use of injection-grade PBT undesirably reduces the zero shear viscosity of the PBT-PE blend to less than 1000 Pascal*seconds (PaS) at 250°C, thereby reducing the extrudability and dimensional stability of the extruded tube. In addition, buffer tubes extruded from injection-grade PBT-PE blends may exhibit kinking and lower compressive resistance due to uneven tube wall thickness caused by reduced dimensional stability.
[0006] It is therefore surprising to find a PBT-PE blend that exhibits a zero shear viscosity greater than 1000 PaS at 250°C and resists kinking, but utilizes a PBT with a melt flow index greater than 21 g / 10 min. Summary of the invention
[0007] The present invention provides a solution to provide a PBT-PE blend containing PBT having a melt flow index greater than 21 g / 10 min and exhibiting a zero shear viscosity greater than 1000 PaS at 250°C and kink resistance.
[0008] The present invention is the result of the discovery that blending a crosslinkable silanol functionalized polyolefin with a hydroxyl terminated poly(dimethylsiloxane) and a condensation catalyst in an injection molding grade PBT produces a polymer composition having a zero shear viscosity sufficient to maintain dimensional stability when extruded. Unexpectedly, the crosslinking of the silanol functionalized polyolefin that occurs only due to blending and extrusion is sufficient to increase the zero shear viscosity of the polymer composition to maintain the dimensional stability of the polymer composition. It was also unexpectedly found that a polymer composition in which the crosslinkable silanol functionalized polyolefin is a minority component can still achieve a sufficiently high zero shear viscosity to provide a tube with good extrudability and dimensional stability. The inventors also found that despite the crosslinking of the silanol functionalized polyolefin, the MAH-g-HDPE is able to maintain the morphological stability of the mixed phase when the mixture is subjected to high shear events such as mixing, remelting and high speed extrusion. The stability of the mixed phase morphology resists phase separation, which would otherwise result in kinking and poor mechanical properties of the buffer tube. Therefore, relatively low cost injection molding grade PBT can be used to produce a stable mixture that can be used to make buffer tubes with good mechanical properties to resist kinking.
[0009] The present invention is particularly useful for buffer tubes in optical fiber devices.
[0010] According to at least one feature of the present invention, a method comprises the following steps:
[0011] (a) blending a polymer composition comprising:
[0012] (i) 5 wt % to 45 wt % of a silanol-functionalized polyolefin, based on the total weight of the polymer composition;
[0013] (ii) 55 wt% to 90 wt% of polybutylene terephthalate, based on the total weight of the polymer composition, the polymer composition having a melt flow index of 21 g / 10 min to 35 g / 10 min at 250° C. and 2.16 Kg;
[0014] (iii) a condensation catalyst; and
[0015] (iv) 0.5 wt% to 10 wt% of a hydroxyl-terminated poly(dimethylsiloxane), based on the total weight of the polymer composition; and
[0016] (b) extruding the polymer composition. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Reference is made to the accompanying drawings, in which:
[0019] Figure 1 A cross-sectional view of a loose buffer tube optical fiber cable is shown. DETAILED DESCRIPTION
[0020] As used herein, the term "and / or," when used in a list of two or more items, means that any one of the listed items can be used alone, or any combination of two or more of the listed items can be used. For example, if a composition is described as containing components A, B, and / or C, the composition can contain only A; only B; only C; a combination of A and B; a combination of A and C; a combination of B and C; or a combination of A, B, and C.
[0021] Unless otherwise indicated, all ranges are inclusive.Subscript values in polymer formulas refer to the molar average number of units per molecule of the designated component of the polymer.
[0022] Test methods refer to the most recent test methods as of priority purposes of this document unless the date is expressed as a two-digit number with a hyphen in the test method number. References to test methods contain references to the testing association and the test method number. Test method organizations are referenced by one of the following abbreviations: ASTM refers to ASTM International (formerly the American Society for Testing and Materials); EN refers to European Norm; DIN refers to the Deutsches Institut für Normung; and ISO refers to the International Organization for Standardization.
[0023] As used herein, "unimodal" means that a polymeric material has a molecular weight distribution ("MWD") such that its gel permeation chromatography ("GPC") curve exhibits only a single peak and no discernible second peak or even a shoulder or hump relative to this single peak. In contrast, as used herein, "bimodal" means that the MWD in the GPC curve exhibits the presence of two component polymers, such as by having two peaks or where one component may be indicated by a hump, shoulder or tail relative to the peak of the other component polymer.
[0024] As used herein, unless otherwise indicated, the term weight percent ("wt %") refers to the weight percent of a component based on the total weight of the polymer composition.
[0025] Polymer composition
[0026] The polymer composition of the present invention comprises a silanol functionalized polyolefin, polybutylene terephthalate, a condensation catalyst, and a hydroxyl terminated poly(dimethylsiloxane). As will be explained in more detail below, the polymer composition may also comprise a maleated ethylene-based polymer and a high density polyethylene. Such a polymer composition may be extruded to form a fiber optic cable protective component (e.g., a buffer tube).
[0027] Silanol functionalized polyolefins
[0028] The polymer composition comprises a silanol functionalized polyolefin. A "silane functionalized polyolefin" is a polymer containing a silane and a polymerized alpha-olefin equal to or greater than 50 wt% or a majority amount of the total weight of the silane functionalized polyolefin. "Polymer" means a macromolecular compound prepared by reacting (i.e., polymerizing) monomers of the same or different types. As described above, the polymer composition comprises a silanol functionalized polyolefin. The silanol functionalized polyolefin crosslinks and in doing so increases the viscosity of the polymer composition. The increased viscosity of the polymer composition enables extrusion of the polymer composition.
[0029] The silanol functionalized polyolefins may include α-olefin and silane copolymers, silane grafted polyolefins, and / or combinations thereof. "α-olefin and silane copolymers" are formed by copolymerization of an α-olefin (such as ethylene) and a hydrolyzable silane monomer (such as a vinyl silane monomer) such that the hydrolyzable silane monomer is incorporated into the backbone of the polymer, which is then incorporated into the polymer composition. "Silane grafted polyolefins" or "Si-g-PO" may be formed by the Sioplas process, in which a hydrolyzable silane monomer is grafted onto the backbone of a base polyolefin by a process such as extrusion before the polymer is incorporated into the polymer composition.
[0030] In the example where the silanol functionalized polyolefin is an α-olefin / silane copolymer, the silanol functionalized polyolefin is prepared by copolymerization of at least one α-olefin and a hydrolyzable silane monomer. In the example where the silanol functionalized polyolefin is a silanol grafted polyolefin, the silanol functionalized polyolefin is prepared by grafting one or more hydrolyzable silane monomers onto an α-olefin backbone.
[0031] As measured using Fourier transform infrared (FTIR) spectroscopy, the silanol functionalized polyolefin comprises 90 wt% or more, or 91 wt% or more, or 92 wt% or more, or 93 wt% or more, or 94 wt% or more, or 95 wt% or more, or 96 wt% or more, or 97 wt% or more, or 97.5 wt% or more, or 91 wt% or more, or 99 wt% or more, while 99.5 wt% or less, or 99 wt% or less, or 98 wt% or less, or 97 wt% or less, or 96 wt% or less, or 95 wt% or less, or 94 wt% or less, or 93 wt% or less, or 92 wt% or less, or 91 wt% or less of α-olefins. The α-olefins may include C2 or C3 to C4, or C6, or C8, or C9. 10 , or C 12 , or C 16 , or C 18 , or C 20 α-Olefins such as ethylene, propylene, 1-butene, 1-hexene, 4-methyl-1-pentene and 1-octene.
[0032] The silanol-functionalized polyolefin may contain 0.5 wt% or more, or 0.8 wt% or more, or 1.0 wt% or more, or 1.2 wt% or more, or 1.5 to 1.8 wt%, or 2.0 wt%, or 2.3 wt%, or 2.4 wt%, while at the same time 2.5 wt% or less, or 2.4 wt% or less, or 2.3 wt% or less, or 2.0 wt% or less, or 1.8 wt% or less, or 1.6 wt% or less, or 1.4 wt% or less, or 1.2 wt% or less, or 1.0 wt% or less, or 0.8 wt%, or 0.6 wt% or less of silane as measured using FTIR spectroscopy.
[0033] The silanol-functionalized polyolefin has a density of 0.910 grams per cubic centimeter (g / cc), or 0.915 g / cc, or 0.920 g / cc, or 0.921 g / cc, or 0.922 g / cc, or 0.925 g / cc to 0.930 g / cc, or 0.935 g / cc, while being 0.940 g / cc or less, or 0.935 g / cc or less, or 0.930 g / cc or less, or 0.925 g / cc or less, or 0.920 g / cc or less, or 0.915 g / cc or less, as measured by ASTM D-792.
[0034] A "hydrolyzable silane monomer" is a silane-containing monomer that will effectively copolymerize with an α-olefin (e.g., ethylene) to form an α-olefin / silane copolymer (e.g., an ethylene / silane reactor copolymer), or graft to an α-olefin polymer (i.e., a polyolefin) and crosslink therewith to form a reactor Si-g-polyolefin. A hydrolyzable silane monomer has structure (I):
[0035]
[0036] Where R 1 is a hydrogen atom or a methyl group; x is 0 or 1; n is an integer from 1 to 4 or 6 or 8 or 10 or 12; and each R 2 are independently hydrolyzable organic groups, such as alkoxy groups having 1 to 12 carbon atoms (e.g., methoxy, ethoxy, butoxy), aryloxy groups (e.g., phenoxy), aralkyloxy groups (e.g., benzyloxy), aliphatic acyloxy groups having 1 to 12 carbon atoms (e.g., formyloxy, acetoxy, propionyloxy), amino or substituted amino groups (e.g., alkylamino, arylamino), or lower alkyl groups having 1 to 6 carbon atoms, provided that the three R 2 No more than one of the groups is an alkyl group. The hydrolyzable silane monomer can be copolymerized with an α-olefin (e.g., ethylene) in a reactor (e.g., a high pressure process) to form an α-olefin-silane reactor copolymer. In the example where the α-olefin is ethylene, such copolymers are referred to herein as ethylene-silane copolymers. The hydrolyzable silane monomer can also be grafted onto a polyolefin (e.g., polyethylene) using an organic peroxide such as 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane to form a reactor Si-g-PO or an in-situ Si-g-PO.
[0037] Hydrolyzable silane monomers include silane monomers containing ethylenically unsaturated hydrocarbon groups, such as vinyl, allyl, isopropenyl, butenyl, cyclohexenyl or γ (meth) acryloxy allyl and hydrolyzable groups, such as hydrocarbonoxy, hydrocarbon acyloxy or hydrocarbon amino groups. Hydrolyzable groups may include methoxy, ethoxy, formyloxy, acetoxy, propionyloxy and alkyl or arylamino groups. In a specific example, the hydrolyzable silane monomer is an unsaturated alkoxysilane, which can be grafted onto a polyolefin or copolymerized with an α-olefin (e.g., ethylene) in a reactor. Examples of hydrolyzable silane monomers include vinyl trimethoxy silane (VTMS), vinyl triethoxy silane (VTES), vinyl triacetoxy silane and γ-(meth) acryloxy propyl trimethoxy silane.
[0038] Examples of suitable ethylene-silane copolymers are SI-LINK TM DFDA-5451 NT and SI-LINK TMACDFDB-5451NT is commercially available, each available from The Dow Chemical Company, Midland, Mich.
[0039] Polybutylene terephthalate
[0040] As measured by ASTM D792, the density of PBT can range from 1.26 g / cc or greater, or 1.28 g / cc or greater, or 1.30 g / cc or greater, or 1.32 g / cc or greater, or 1.34 g / cc or greater, or 1.36 g / cc or greater, or 1.38 g / cc or greater, or 1.40 g / cc or greater, while 1.41 g / cc or less, 1.40 g / cc or less, or 1.38 g / cc or less, or 1.36 g / cc or less, or 1.34 g / cc or less, or 1.32 g / cc or less, or 1.30 g / cc or less, or 1.28 g / cc or less, or 1.26 g / cc or less.
[0041] PBT can be extrusion grade PBT or injection molding grade PBT. The typical feature of injection molding grade PBT is that the molecular weight is relatively low, as evidenced by a relatively high melt index. As measured according to ASTM method D1238, the melt index (I2) of PBT can be 10 g / 10 min or more, or 15 g / 10 min. or more, or 20 g / 10 min or more, or 25 g / 10 min or more, or 30 g / 10 min or more, or 35 g / 10 min or more, or 40 g / 10 min or more, or 45 g / 10 min or more, or 50 g / 10 min or more, or 55 g / 10 min or more, or 60 g / 10 min or more, or 65 g / 10 min or more. For PBT, the melt index is measured at 250°C and 2.16Kg (i.e., I2).
[0042] Examples of suitable commercially available extrusion grade PBT include, but are not limited to, PBT-61008 from Suzhou Yingmao Plastics Company, Jiangsu, China; ULTRADUR® from BASF, Ludwigshafen, Germany; TM BN6550; CRASTIN from DuPont, Wilmington, Delaware, USA TM 6129NC010; and PBT VALOX from Sabic Innovative Plastics, Pittsfield, Massachusetts, USA TM 176. Examples of suitable commercially available injection molding grade PBT include, but are not limited to, CRASTIN from DuPont, Wilmington, Delaware, USA. TM 6134.
[0043] The polymer composition comprises 50 wt % to 90 wt % PBT. The polymer composition may comprise 50 wt % or more, or 52 wt % or more, or 54 wt % or more, or 56 wt % or more, or 58 wt % or more, or 60 wt % or more, or 62 wt % or more, or 64 wt % or more, or 66 wt % or more, or 68 wt % or more, or 70 wt % or more, or 72 wt % or more, or 74 wt % or more, or 76 wt % or more, or 78 wt % or more, or 80 wt % or more, or 82 wt % or more, or 84 wt % or more, or 86 wt % or more, or 88 wt % or more % or less, or 64wt% or less, or 62wt% or less, or 60wt% or less, or 58wt% or less, or 56wt% or less, or 54wt% or less, or 52wt% or less of PBT.
[0044] Condensation catalyst
[0045] The polymer composition comprises a condensation catalyst. The condensation catalyst catalyzes the crosslinking of the silanol functionalized polyolefin. The condensation catalyst can be any compound that catalyzes the moisture crosslinking reaction with the hydrolyzable silane group. The condensation catalyst can include metals such as carboxylates of tin, zinc, iron, lead and cobalt; organic bases, inorganic acids and organic acids. Examples of such catalysts include, but are not limited to, dibutyltin dilaurate ("DBTDL"), dibutyltin diacetate, dioctyltin dilaurate, stannous acetate, stannous octoate, lead naphthenate, zinc octoate, cobalt naphthenate, ethylamine, dibutylamine, hexylamine, pyridine, inorganic acids (such as sulfuric acid and hydrochloric acid) and organic acids, such as sulfonic acids (such as toluenesulfonic acid), acetic acid, stearic acid and maleic acid. In various embodiments, the catalyst is selected from tin-based catalysts and sulfonic acids. In other embodiments, the catalyst can be a tin carboxylate. In addition, in certain embodiments, the catalyst is DBTDL. The catalyst can be used alone or as part of a masterbatch. Such a masterbatch may additionally comprise, for example, a polyolefin carrier (eg polyethylene), an antioxidant and / or a metal deactivator.
[0046] The polymer composition may contain 0.5 wt% or more, or 1.0 wt% or more, or 1.5 wt% or more, or 2.0 wt% or more, or 2.5 wt% or more, or 3.0 wt% or more, or 3.5 wt% or more, or 4.0 wt% or more, or 4.5 wt% or more, while 5.0 wt% or less, or 4.5 wt% or less, or 4.0 wt% or less, or 3.5 wt% or less, or 3.0 wt% or less, or 2.5 wt% or less, or 2.0 wt% or less, or 1.5 wt% or less, or 1.0 wt% or less of the condensation catalyst.
[0047] The condensation catalyst may be added to the polymer mixture as part of a catalyst masterbatch blend. An example of a suitable catalyst masterbatch is available under the trade name SI-LINK TM Commercially available from The Dow Chemical Company, including SI-LINK TM DFDA-5481Natural and SI-LINK TM AC DFDA-5488NT. SI-LINK TMAC DFDA-5488NT is a catalyst masterbatch containing a blend of a thermoplastic polymer, a phenolic compound antioxidant, and a hydrophobic acid catalyst (silanol condensation catalyst). The polymer composition can comprise 0 wt % or more, or 0.5 wt % or more, or 1.0 wt % or more, or 2.0 wt % or more, or 3.0 wt % or more, or 4.0 wt % or more, or 5.0 wt % or more, or 6.0 wt % or more, or 7.0 wt % or more, or 8.0 wt % or more, or 9.0 wt % or more, while 10.0 wt % or less, or 9.0 wt % or less, or 8.0 wt % or less, or 7.0 wt % or less, or 6.0 wt % or less, or 5.0 wt % or less, or 4.0 wt % or less, or 3.0 wt % or less, or 2.0 wt % or less, or 1.0 wt % or less of a catalyst masterbatch, based on the total weight of the polymer composition.
[0048] Hydroxyl terminated poly(dimethylsiloxane)
[0049] The polymer composition comprises a hydroxyl-terminated poly(dimethylsiloxane) (PDMS). The PDMS comprises units of formula R2SiO, wherein each group R is a methyl group. The PDMS may have structure (II):
[0050]
[0051] wherein Me is a methyl group and n is a number sufficient to impart to the PDMS a number average molecular weight (Mn) greater than or equal to (>) 4,000. The upper limit of n may be 100,000 or less, or 10,000 or less, or 1,000 or less, or 500 or less, as measured by gel permeation chromatography (GPC). Such polydimethylsiloxanes may be used as XIAMETER TM PMX-0156 silanol fluid was commercially available from The Dow Chemical Company, Midland, Michigan, USA.
[0052] Maleated ethylene-based polymers
[0053] As mentioned above, polymeric composition also comprises maleated ethylene-based polymer.As used herein, term "maleated " represents the polymer (for example, ethylene-based polymer) that has been modified to incorporate maleic anhydride monomer.Maleated ethylene-based polymer can be formed by copolymerization of maleic anhydride monomer with ethylene and other monomers (if present) to prepare the interpolymer with maleic anhydride incorporated in the polymer backbone.Additionally or alternatively, maleic anhydride can be graft polymerized to ethylene-based polymer.The above description of ethylene-based polymer is equally applicable to maleated ethylene-based polymer.
[0054] The maleated ethylene-based polymer can have a density of 0.93 g / cc or greater, or 0.933 g / cc or greater, or 0.935 g / cc or greater, or 0.937 g / cc or greater, or 0.94 g / cc or greater, or 0.943 g / cc or greater, or 0.945 g / cc or greater, or 0.947 g / cc or greater, or 0.95 g / cc or greater, or 0.958 g / cc or greater, 0.965 g / cc or greater, while 0.97 g / cc or less, or 0.965 g / cc or less, as measured by ASTM D792.
[0055] The maleated ethylene-based polymer may have a melt index (I2) in the range of 0.1 to 10 g / 10 min, 0.2 to 8 g / 10 min, or 0.5 to 5 g / 10 min at 190° C. and 2.16 Kg.
[0056] The maleic anhydride content of the maleated ethylene-based polymer can be 0.25 wt% or more, or 0.50 wt% or more, or 0.75 wt% or more, or 1.00 wt% or more, or 1.25 wt% or more, or 1.50 wt% or more, or 1.75 wt% or more, or 2.00 wt% or more, or 2.25 wt% or more, or 2.50 wt% or more, or 2.75 wt% or more, while 3.00 wt% or less, 2.75 wt% or less, or 2.50 wt% or less, or 2.25 wt% or less, or 2.00 wt% or less, or 1.75 wt% or less, or 1.50 wt% or less, or 1.25 wt% or less, or 1.00 wt% or less, or 0.75 wt% or less, or 0.5 wt% or less, based on the total weight of the maleated ethylene-based polymer. The maleic anhydride concentration is determined by titrimetric analysis. By utilizing dry resin to carry out titrimetric analysis, and use 0.02N KOH titration, to determine the amount of maleic anhydride. The dry polymer is titrated by dissolving 0.3 to 0.5 grams of maleated polymer in the refluxing xylene of about 150mL. After dissolving completely, deionized water (four drops) is added to the solution and the solution is refluxed for 14 hours. Next, 1% thymol blue (several drops) is added to the solution and the 0.02N KOH in ethanol is used to over-titrate the solution, as indicated by the formation of purple. Then the solution is used for the 0.05N HCl in isopropanol back titration to the yellow end point.
[0057] The polymer composition can include 2.5wt% to 7.5wt% of the maleated ethylene-based polymer. For example, the polymer composition can include 2.5wt% or more, or 3.0wt% or more, or 3.5wt% or more, or 4.0wt% or more, or 4.5wt% or more, or 5.0wt% or more, or 5.5wt% or more, or 6.0wt% or more, or 6.5wt% or more, or 7.0wt% or more, while 7.5wt% or less, or 7.0wt% or less, or 6.5wt% or less, or 6.0wt% or less, or 5.5wt% or less, or 5.0wt% or less, or 4.5wt% or less, or 4.0wt% or less, or 3.5wt% or less, or 3.0wt% or less.
[0058] Examples of suitable commercially available maleated ethylene-based polymers include, but are not limited to, AMPLIFY TM TY1053H、AMPLIFY TM GR204 and AMPLIFY TM GR205; BYNEL purchased from DuPont, Wilmington, DE, USA TM 4000 Series and FUSABOND TM P series products; OREVAC purchased from Arkema, Colombes, France TM Grafted polyethylene; and POLYBOND purchased from Addivant, Danbury, CT, USA TM 3000 Series.
[0059] High-density polyethylene
[0060] The polymer composition may include high density polyethylene ("HDPE"). HDPE is an ethylene-based polymer having a density of at least 0.94 g / cc, or at least 0.94 g / cc to 0.98 g / cc, as measured by ASTM D792. The melt index of HDPE is 0.1 g / 10 min to 25 g / 10 min. HDPE may include ethylene and one or more C3-C 20α-olefin comonomers. The comonomers may be linear or branched. Non-limiting examples of suitable comonomers include propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene and 1-octene. HDPE can be prepared in slurry reactors, gas phase reactors or solution reactors using Ziegler-Natta, chromium-based, constrained geometry or metallocene catalysts. Ethylene / C3-C 20 The alpha-olefin comonomer includes at least 50 wt% of ethylene polymerized therein, or at least 70 wt%, or at least 80 wt%, or at least 85 wt%, or at least 90 wt%, or at least 95 wt% of ethylene in polymerized form. In one embodiment, the HDPE is an ethylene / alpha-olefin copolymer having a density of 0.95 g / cc to 0.98 g / cc and a melt index (I2) of 0.1 g / 10 min to 10 g / 10 min. In one embodiment, the HDPE has a density of 0.960 g / cc to 0.980 g / cc and a melt index of 0.1 g / 10 min to 10 g / 10 min. Non-limiting examples of suitable HDPE are available under the trade name ELITE TM 5960G, HDPE KT 10000UE TM 、HDPE KS 10100UE TM 、HDPE 35057E TM and AXELERON TM CX-A-6944NT is commercially available, each available from The Dow Chemical Company, Midland, Michigan, USA.
[0061] HDPE can be unimodal or bimodal. In other embodiments, the HDPE is bimodal. Exemplary methods for preparing unimodal HDPE can be found, for example, in U.S. Pat. Nos. 4,303,771 or 5,324,800. Examples of commercially available unimodal HDPE include, but are not limited to, DGDL-3364NT from The Dow Chemical Company of Midland, Michigan, USA. TM .
[0062] The polymer composition may include a bimodal HDPE. The bimodal HDPE includes a first polymer component and a second polymer component. The first component may be an ethylene-based polymer; for example, the first component may be a high molecular weight ethylene homopolymer or an ethylene / α-olefin copolymer. The first component may include any amount of one or more α-olefin copolymers. For example, the first component may include less than 10 wt% of one or more α-olefin comonomers, based on the total first component weight. The first component may include any amount of ethylene; for example, the first component may include at least 90 wt% ethylene or at least 95 wt% ethylene, based on the total first component weight. The α-olefin comonomer present in the first component of the bimodal HDPE typically has no more than 20 carbon atoms. For example, the α-olefin comonomer may have 3 to 10 carbon atoms or 3 to 8 carbon atoms. Exemplary α-olefin comonomers include, but are not limited to, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, and 4-methyl-1-pentene. In one embodiment, the α-olefin comonomer is selected from the group consisting of propylene, 1-butene, 1-hexene, and 1-octene. In other embodiments, the α-olefin comonomer is selected from the group consisting of 1-hexene and 1-octene.
[0063] The density of the first component of the bimodal HDPE may be in the range of 0.915 g / cc to 0.940 g / cc, 0.920 g / cc to 0.940 g / cc, or 0.921 g / cc to 0.936 g / cc. The melt index (I2) (190°C / 2.16 kg) of the first component may be in the range of 0.510 g / 10 min to 10 g / 10 min, 1.10 g / 10 min to 7 g / 10 min, or 1.310 g / 10 min to 5 g / 10 min. The molecular weight of the first component may be in the range of 150,000 grams per mole (g / mol) to 375,000 g / mol, 175,000 g / mol to 375,000 g / mol, or 200,000 g / mol to 375,000 g / mol.
[0064] The second polymer component of the bimodal HDPE can be an ethylene-based polymer. For example, the second component can be a low molecular weight ethylene homopolymer. The ethylene homopolymer can contain trace amounts of contaminating comonomers, such as α-olefin comonomers. In various embodiments, the second component can contain less than 1 wt% of one or more α-olefin comonomers, based on the weight of the second component. For example, the second component can contain 0.0001 to 1.00 wt% of one or more α-olefin comonomers, or 0.001 to 1.00 wt% of one or more α-olefin comonomers. Based on the weight of the second component, the second component can contain at least 99 wt% of ethylene or ethylene in the range of 99.5 wt% to 100 wt%.
[0065] The density of the second component of the bimodal HDPE may be in the range of 0.965 g / cc to 0.980 g / cc or 0.970 g / cc to 0.975 g / cc. The melt index (I2) of the second component may be in the range of 50 g / 10 min to 1,500 g / 10 min, 200 g / 10 min to 1,500 g / 10 min, or 500 g / 10 min to 1,500 g / 10 min. The molecular weight of the second component may be in the range of 12,000 to 40,000 g / mol, 15,000 to 40,000 g / mol, or 20,000 to 40,000 g / mol.
[0066] A suitable method for making bimodal HDPE can be found, for example, in paragraphs
[0063] to
[0086] of U.S. Patent Application Publication No. 2009-0068429.
[0067] Examples of commercially available bimodal HDPE include, but are not limited to, DMDA-1250NT TM and DMDC 1250 TM , both available from The Dow Chemical Company, Midland, Michigan, USA.
[0068] The polymer composition can include 5 wt % or more, or 6 wt % or more, or 7 wt % or more, or 8 wt % or more, or 9 wt % or more, or 10 wt % or more, or 11 wt % or more, or 12 wt % or more, or 13 wt % or more, or 14 wt % or more, or 15 wt % or more, or 16 wt % or more, or 17 wt % or more, or 18 wt % or more, or 19 wt % or more, or 20 wt % or more, or 21 wt % or more, or 22 wt % or more, or 23 wt % or more, or 24 wt % or more, While at the same time 25wt% or less, or 24wt% or less, or 23wt% or less, or 22wt% or less, or 21wt% or less, or 20wt% or less, or 19wt% or less, or 18wt% or less, or 17wt% or less, or 16wt% or less, 15wt% or less, or 14wt% or less, or 13wt% or less, or 12wt% or less, or 11wt% or less, or 10wt% or less, or 9wt% or less, or 8wt% or less, or 7wt% or less, or 6wt% or less or less of HDPE.
[0069] additive
[0070] The polymer composition may include one or more particulate fillers, such as glass fibers or various mineral fillers, including nanocomposites. Fillers, especially fillers having elongated or plate-like particles that provide a higher aspect ratio (length / thickness), can improve modulus and post-extrusion shrinkage characteristics. The median size or d 50% The filler may be less than 20 μm, less than 10 μm or less than 5 μm. The filler may be surface treated to facilitate wetting or dispersion in the polymer composition. Specific examples of suitable fillers include, but are not limited to, calcium carbonate, silicon dioxide, quartz, fused quartz, talc, mica, clay, kaolin, wollastonite, feldspar, aluminum hydroxide, carbon black and graphite. Based on the total weight of the polymer composition, the filler may be included in the polymer composition in an amount ranging from 2 wt % to 30 wt % or from 5 wt % to 30 wt %.
[0071] The polymer composition may include a nucleating agent. Examples of suitable nucleating agents include ADK NA-11 nucleating agent commercially available from Asahi Denim Kokai and HYPERFORM HPN-20E commercially available from Milliken Chemical. TM Nucleating Agents. Nucleating agents can be included in the polymer composition in an amount ranging from 0.08 wt% to 0.3 wt%, 0.09 wt% to 0.25 wt%, or 0.1 to 0.22 wt%, based on total polymer composition weight.
[0072] The polymer composition may include additional additives in the form of antioxidants, crosslinking aids, curing accelerators and scorch retardants, processing aids, coupling agents, UV stabilizers (including UV absorbers), antistatic agents, additional nucleating agents, slip agents, lubricants, viscosity control agents, tackifiers, antiblocking agents, surfactants, extender oils, acid scavengers, flame retardants and metal deactivators. The polymer composition may include 0.01 wt% to 10 wt% of one or more additional additives.
[0073] UV light stabilizers may include hindered amine light stabilizers ("HALS") and UV light absorbers ("UVA") additives. Representative UVA additives include benzotriazole types such as TINUVIN 326 commercially available from Ciba, Inc. TM Light stabilizers and TINUVIN 328 TM Light Stabilizers: Blends of HAL and UVA additives are also effective.
[0074] The antioxidant may comprise hindered phenols such as tetrakis[methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)]methane; bis[(β-(3,5-di-tert-butyl-4-hydroxybenzyl)methylcarboxyethyl)]-sulfide, 4,4′-thiobis(2-methyl-6-tert-butylphenol), 4,4′-thiobis(2-tert-butyl-5-methylphenol), 2,2′-thiobis(4-methyl-6-tert-butylphenol) and thiodiethylenebis(3,5-di-tert-butyl-4-hydroxy)-hydrocinnamate; phosphites and phosphites Acid esters, such as tris(2,4-di-tert-butylphenyl) phosphite and di-tert-butylphenyl phosphite; thio compounds, such as dilauryl thiodipropionate, dimyristyl thiodipropionate and distearyl thiodipropionate; various siloxanes; polymerized 2,2,4-trimethyl-1,2-dihydroquinoline, n,n'-bis(1,4-dimethylpentyl-p-phenylenediamine), alkylated diphenylamine, 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, diphenyl-p-phenylenediamine, mixed diaryl-p-phenylenediamines and other hindered amine antidegradants or stabilizers.
[0075] Processing aids may include metal salts of carboxylic acids, such as zinc stearate or calcium stearate; fatty acids, such as stearic acid, oleic acid or erucic acid; fatty amides, such as stearamide, oleamide, erucamide or N,N′-ethylenebisstearamide; polyethylene waxes; oxidized polyethylene waxes; polymers of ethylene oxide; copolymers of ethylene oxide and propylene oxide; vegetable waxes; petroleum waxes; nonionic surfactants; silicone oils and polysiloxanes.
[0076] Compounding and extrusion
[0077] The components of the polymer composition other than PBT and the condensation catalyst can be added to a batch or continuous mixer to form a melt-blended composition. The components can be added in any order or one or more masterbatches can be prepared first to blend with the other components. Melt blending is carried out at a temperature higher than the highest molten polymer but lower than the maximum compounding temperature of 285°C. The melt-blended composition can then be transported to an extruder or injection molding machine, or formed into a desired article through a mold, or converted into pellets, tapes, strips or films or some other form for storage or preparation of materials supplied to the next forming or processing step. Optionally, if formed into pellets or some similar configuration, the pellets, etc. can be coated with a release agent to facilitate handling during storage.
[0078] Examples of compounding equipment used include internal batch mixers, such as BANBURY or BOLLING internal mixers. Alternatively, continuous single screw or twin screw mixers, such as FARRELL continuous mixers, WERNER and PFLEIDERER twin screw mixers or BUSS kneading continuous extruders, can be used. The type of mixer utilized and the operating conditions of the mixer will affect the properties of the composition, such as viscosity, volume resistivity and extruded surface smoothness.
[0079] The composition of melt blending is then mixed with PBT and condensation catalyst in forcing machine, so that polymer composition is blended.Due to the blended polymer composition comprising condensation catalyst and silanol functionalized polyolefin now, silanol functionalized polyolefin begins to crosslink and increase the viscosity of the blended polymer composition.The extrusion of polymer composition can begin immediately, or can delay 1 minute, or 5 minutes, or 10 minutes, or 30 minutes or 1 hour from beginning blending.Then polymer composition is extruded to form one or more components.
[0080] Polymer composition properties
[0081] The polymer composition may exhibit 1,000 MPa or more, or 1,100 MPa or more, or 1,200 MPa or more, or 1,300 MPa or more, or 1,400 MPa or more, or 1,500 MPa or more, or 1,600 MPa or more, or 1,700 MPa or more, or 1,800 MPa or more, or 1,900 MPa or more, or 2,000 MPa or more, or 2,100 MPa or more, or 2,200 MPa or more, or 2,300 MPa or more, or 2,400 MPa or more, or 2,500 MPa or more, or 2,600 MPa or more, or 2,700 MPa or more, or 2,800 MPa or more, or 2,900 MPa or more. , while having a flexural modulus of 3,000 MPa or less, or 2,900 MPa or less, or 2,800 MPa or less, or 2,700 MPa or less, or 2,600 MPa or less, or 2,500 MPa or less, or 2,400 MPa or less, or 2,300 MPa or less, or 2,200 MPa or less, or 2,100 MPa or less, or 2,000 MPa or less, or 1,900 MPa or less, or 1,800 MPa or less, or 1,700 MPa or less, or 1,600 MPa or less, or 1,500 MPa or less, or 1,400 MPa or less, or 1,300 MPa or less, or 1,200 MPa or less, or 1,100 MPa or less. The flexural modulus is determined according to the procedure described in the Test Methods section below.
[0082] In various embodiments, particularly those where the polymer composition is intended for use in a buffer tube containing a hydrocarbon filler compound, when immersed in INFOGEL TM LA 444 (fiber optic cable buffer tube filling compound), the polymer composition can exhibit a weight gain of less than 3 wt%, less than 2 wt%, less than 1 wt%, or less than 0.5 wt%. INFOGEL TM LA444 filling compound consists of at least about 70 wt% mineral oil and up to about 10 wt% styrene-butadiene-styrene block copolymer and is commercially available from Honghui Corp., China.
[0083] The polymer composition may exhibit a melt index (I2) of 4 to 11 g / 10 min at 250° C. and 2.16 Kg. For example, the melt flow index may be 4 g / 10 min or more, or 4.5 / 10 min or more, or 5 g / 10 min or more, or 5.5 / 10 min or more, or 6 g / 10 min or more, or 6.5 / 10 min or more, or 7 g / 10 min or more, or 7.5 / 10 min or more, or 8 g / 10 min or more, or 8.5 / 10 min or more, or 9 g / 10 min or more, or 9.5 / 10 min or more, or 10 g / 10 min or more, or 10.5 / 10 min or more. , while at the same time 11g / 10min or less, or 10.5g / 10min or less, or 10g / 10min or less, or 9.5g / 10min or less, or 9g / 10min or less, or 8.5g / 10min or less, or 8g / 10min or less, or 7.5g / 10min or less, or 7g / 10min or less, or 6.5g / 10min or less, or 6g / 10min or less, or 5.5g / 10min or less, or 5g / 10min or less, or 4.5g / 10min or less.
[0084] The polymer composition may exhibit a zero shear viscosity of 200 PaS or more, or 500 PaS or more, or 1,000 PaS or more, or 5,000 PaS or more, or 10,000 PaS or more, or 15,000 PaS or more, or 20,000 PaS or more, or 25,000 PaS or more, while 30,000 PaS or less, or 25,000 PaS or less, or 20,000 PaS or less, or 15,000 PaS or less, or 10,000 PaS or less, or 5,000 PaS or less, or 1,000 PaS or less, or 500 PaS or less at 250° C. The test method for zero shear viscosity is described in detail below.
[0085] The polymer composition may exhibit 22 MPa or more, or 23 MPa or more, or 24 MPa or more, or 25 MPa or more, or 26 MPa or more, or 27 MPa or more, or 28 MPa or more, or 29 MPa or more, or 30 MPa or more, or 31 MPa or more, or 32 MPa or more, or 33 MPa or more, or 34 MPa or more, or 35 MPa or more, or 36 MPa or more, or 37 MPa or more, or 38 MPa or more, or 39 MPa or more. Pa or more, while 40MPa or less, or 39MPa or less, or 38MPa or less, or 37MPa or less, or 36MPa or less, or 35MPa or less, or 34MPa or less, or 33MPa or less, or 32MPa or less, or 31MPa or less, or 30MPa or less, or 29MPa or less, or 28MPa or less, or 27MPa or less, or 26MPA or less, or 25MPa or less, or 24MPa or less of the breaking stress. The test method of breaking stress is as follows.
[0086] The polymer composition can exhibit 55 MPa or more, or 56 MPa or more, or 57 MPa or more, or 58 MPa or more, or 59 MPa or more, or 60 MPa or more, or 61 MPa or more, or 62 MPa or more, or 63 MPa or more, or 64 MPa or more, or 65 MPa or more, or 66 MPa or more, or 67 MPa or more, or 68 MPa or more, or 69 MPa or more, or 70 MPa or more, or 71 MPa or more, or 72 MPa or more, or 73 MPa or more, or 74 MPa or more. The test method for pipe crush strength is as follows: the pipe crush strength is 75 MPa or less, or 74 MPa or less, or 73 MPa or less, or 72 MPa or less, or 71 MPa or less, or 70 MPa or less, or 69 MPa or less, or 68 MPa or less, or 67 MPa or less, or 66 MPa or less, or 65 MPa or less, or 64 MPa or less, or 63 MPa or less, or 62 MPa or less, or 61 MPa or less, or 60 MPa or less, or 59 MPa or less, or 58 MPa or less, or 57 MPa or less, or 56 MPa or less. The test method for pipe crush strength is as follows.
[0087] Fiber Optic Cable
[0088] Reference now Figure 1 , depicts a cross-sectional view of an exemplary optical fiber cable 1. In the depicted example, the optical fiber cable 1 is a "loose buffer tube" design. In this cable design, the buffer tube 2 is radially positioned around the central strength member 4, and the buffer tube 2 is spirally rotated along the axial length of the optical fiber 1. The spiral rotation of the buffer tube 2 allows the cable to bend without significantly stretching the tube or the optical fiber 6. If a reduced number of buffer tubes 2 is required, a foamed filler rod can be used as a spacer to occupy one or more buffer tube positions 10, thereby maintaining the geometry of the cable 1. The cable jacket 14 is typically made of a polyethylene-based material. The buffer tube 2 can contain a polymer composition, consist of a polymer composition, or consist essentially of a polymer composition. The buffer tube 2 is optionally filled with a cable grease or gel 8. The gel and grease compounds can include hydrocarbon-based greases incorporated into hydrocarbon oils and / or polymer-based greases using low-viscosity polymers formulated with hydrocarbon oils. These greases and gels provide the required suspension and protection of the environment surrounding the optical fiber 6, including the elimination of air spaces. The gel and grease also provide a barrier to prevent water penetration that is harmful to the performance of the optical fiber 6.
[0089] Example
[0090] Material
[0091] The following materials were used in the following examples.
[0092] The PBT is a PBT having a density of 1.30 g / cc and a melt index of 33.5 g / 10 min at 250°C (ie, injection molding grade), which is available under the trade name CRASTIN TM 6134 was commercially available from EI du Pont de Nemours, Wilmington, DE, USA.
[0093] LDPE is a high pressure low density polyethylene having a density of 0.921 g / cc and a melt index of 1.9 g / 10 min, which is available under the trade name DXM-446 TM Commercially available from The Dow Chemical Company, Midland, Michigan, USA.
[0094] The HDPE is a bimodal HDPE having a density of 0.955 g / cc and a melt index (I2) of 1.5 g / 10 min at 190°C, which is available under the trade name DMDC-1250NT TM Commercially available from The Dow Chemical Company, Midland, Michigan, USA.
[0095] MAH-g-HDPE is a maleic anhydride grafted HDPE having a density of 0.958 g / cc, a melt index of 2.0 g / 10 min, and a maleic anhydride content greater than 1.0 wt %, which can be obtained under the trade name AMPLIFY TY 1053H TM Commercially available from The Dow Chemical Company, Midland, Michigan, USA.
[0096] The silane copolymer is a copolymer of silane and ethylene having a density of 0.924 g / cc and a melt index of 1.5 g / 10 min at 190°C and 2.16 kg, which can be found under the trade name SI-LINK TM DFDB-5451NT is commercially available from The Dow Chemical Company, Midland, Michigan, USA.
[0097] M1 is a masterbatch containing less than 5 wt% of a sulfonic acid silanol condensation catalyst and less than 6 wt% of a phenolic antioxidant based on the total weight of the masterbatch, wherein the masterbatch has a density of 0.925 g / cc and a melt index of 1.5 g / 10 min at 190°C and 2.16 Kg. M1 is available under the trade name SI-LINK TM DFDA-5488NT is commercially available from The Dow Chemical Company, Midland, Michigan, USA.
[0098] M2 is a masterbatch containing less than 5 wt% of a tin-based silanol condensation catalyst and less than 6 wt% of a phenolic antioxidant based on the total weight of the masterbatch, wherein the masterbatch has a density of 0.930 g / cc and a melt index of 0.93 g / 10 min at 190°C and 2.16 Kg. M2 is available under the trade name SI-LINK TM DFDA-5481NT masterbatch was commercially available from The Dow Chemical Company, Midland, Michigan, USA.
[0099] The nucleating agent is a nucleating agent with the chemical name of 2,2′-methylene-bis-(4,6-di-tert-butylphenyl) sodium phosphate (CAS No. 85209-91-2), which can be obtained under the trade name NA-11A. TM The nucleating agent was commercially available from ADEKA Corporation, Tokyo, Japan.
[0100] AO1 is a sterically hindered phenolic antioxidant with the chemical name pentaerythritol tetrakis (3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate), which can be sold under the trade name IRGANOX 1010 TM Commercially available from BASF, Ludwigshafen, Germany.
[0101] AO2 is a hydrolysis-stable phosphite processing stabilizer with the chemical name tris(2,4-di-tert-butylphenyl)phosphite, which can be purchased under the trade name IRGAFOS 168 TM Commercially available from BASF, Ludwigshafen, Germany.
[0102] OH-PDMS is a hydroxyl-terminated poly(dimethylsiloxane) having a hydroxyl content of 2.5% or less and is available under the trade name XIAMETER TM PMX-0156 silanol fluid was commercially available from The Dow Chemical Company, Midland, Michigan, USA.
[0103] Tube sample preparation
[0104] Inventive Examples ("IE") and Comparative Examples ("CE") were prepared according to the following criteria. Master blends IE4-15 and CE3-7 were formed containing all designated sample ingredients except PBT, M1 and M2. Master blends were created using LDPE, HDPE, silane copolymer, MAH-g-HDPE, OH-PDMS and antioxidant components to ensure proper oil incorporation. TMThe main mix was produced in a mixing bowl apparatus with the cam mixing blade set at 30 rpm and a temperature of 160°C to 170°C. The main blend of IE4-15 and CE3-7 along with PBT and M1 and M2 were placed into the BRABENDER using a 42 mm screw according to the conditions provided in Table 1. TM Model D6 / 2 twin screw extruder.
[0105] The ingredients of IE1-3 and CE2 were placed into a ZSK 30 COPERION set to the mixing conditions given in Table 2. TM In a twin screw extruder.
[0106] Table 1
[0107] parameter condition Region 1 230℃ Area 2 240℃ Area 3 250℃ Region 4 253℃ Extruder (rpm) 60
[0108] Table 2
[0109] parameter condition Bucket 1 neutral Buckets 2 and 3 125℃ Buckets 4 and 5 235℃ Buckets 6 and 7 182℃ Buckets 8 and 9 201℃ Buckets 10 and 11 247℃ Mold adapter 252℃ Mould 232℃ RPM 350 Feed rate 30lb / h Discharge melting temperature 258℃
[0110] The samples were formed by coated wire extrusion. The coated wire extrusion molded the dimensions of the buffer tube and tested the extrusion properties of the polymer composition. The coated wire extrusion was performed using a BRABENDER mini wire line on 14 gauge copper wire. The BRABENDER mini wire line settings are provided in Table 3.
[0111] Table 3
[0112] parameter condition Region 1 230℃ Area 2 240℃ Area 3 250℃ Region 4 240℃ Melting temperature 254℃ RPM 40 Delivery speed 10ft / min
[0113] The final diameter of the Inventive and Comparative Examples was about 2.9 mm (0.114") and the wall thickness was about 0.635 mm (25 mils) on a 1.63 mm (0.064") diameter 14 AWG solid copper conductor. The conductor was removed from the wire to leave the Inventive and Comparative Examples tubes. The tubes were mechanically tested according to the following test methods.
[0114] Compression molded board samples
[0115] The examples of the present invention and the comparative examples were extruded into single stents with a diameter of 3.6 mm. TM The pellets were compression molded to form plaques for flexural modulus testing.
[0116] Test Method
[0117] The following test methods were used to determine the properties of the materials and the following Inventive and Comparative Examples.
[0118] density
[0119] Polymer density was determined according to ASTM D792 at 23°C.
[0120] Fracture stress
[0121] Cut the tube into 10.16 cm lengths. Clamp the tube into the INSTRON TM A 4202 tensile test unit with a jaw spacing of 2.54 cm and a 100 lb load cell was used. The crosshead speed was set to 10 mm / min and the stress at the point where the tube broke was measured. This was repeated five times and the average was taken.
[0122] Flexural modulus
[0123] Rectangular samples of 1.27 cm wide x 7.62 cm x 0.127 cm were die cut from the compression molded plaques. The samples were placed in the INSTRON TM Perform 3-point deflection in the flexure fixture of the 4202 tester. Determine the flexural modulus at the maximum flexural stress experienced during the test.
[0124] Kink
[0125] Wrapping Inventive and Comparative Example Sample 1 was completely wrapped around a 6 mm mandrel and held in place for 10 seconds. Any kinks that formed were observed.
[0126] Tube crush
[0127] Place the tube into the INSTRON TM The crosshead was placed between the upper movable plate (dimensions 50 mm x 100 mm) and the lower fixed plate (dimensions 50 mm x 100 mm) connected to the crosshead in the 4202. The tube was aligned with the longer dimension of the plates and the top plate was moved so that it just touched the top of the tube. The crosshead speed was set to 0.127 cm / min and the compressive force at the yield point of the tube was recorded.
[0128] Zero shear viscosity
[0129] Use a RHEOMETRICS equipped with a 25 mm parallel plate TM The SR-200 controlled stress rheometer was used to apply a stress of 500 Pa for 3 minutes at 250°C. The zero shear viscosity was calculated over the range of data where the time rate of change of the measured stress was constant. A recovery time of 15 minutes was allowed.
[0130] Test Results
[0131] Table 4 provides the composition and mechanical property data of CE1-CE7.
[0132] Table 4
[0133]
[0134]
[0135] As can be seen from Table 4, CE1-CE7 each exhibited kinking or breaking. Kinking and breaking are believed to be the result of dimensional and morphological instabilities during extrusion. In addition, dimensional and morphological instabilities generally lead to lower fracture stress values in Comparative Examples CE2-CE7 (Examples containing polyolefins) compared to IE1-IE15. Therefore, IE1-IE15 exhibit improved kink resistance compared to pure PBT (CE1) and samples without a silanol functionalized polyolefin component (CE2).
[0136] IE1 replaces approximately the same amount of LDPE used in CE2 with a silane copolymer while maintaining the same amount of MAH-g-HDPE. IE1 shows improved kink resistance and higher tube break stress compared to CE2. The HDPE component is removed in IE2, and the amount of MAH-g-HDPE is approximately twice that of IE1. IE2 shows similar improved tube break stress and higher flexural modulus compared to IE1, and no kinking. It is believed that increasing the concentration of MAH-g-HDPE increases morphological stability, resulting in improved flexural modulus. IE3 is similar to IE2, except that the amount of silane copolymer is increased by approximately 4wt%. The results for IE3 are not significantly changed compared to IE2. IE4 is similar in composition to IE1, except that IE4 has 1wt% OH-PDMS instead of 4.9wt%. The tube break stress and flexural modulus of IE4 are only slightly higher compared to IE1, IE2, and IE3. This result indicates that 1wt% OH-PDMS is sufficient to achieve crosslinking of the silane copolymer IE samples. CE3 is similar in composition to IE4, except that it does not contain MAH-g-HDPE. CE3 failed the kink test and also had lower values for stress at break and flexural modulus compared to IE1-IE4. This result is believed to occur due to morphological instability caused by the lack of compatibilization of MAH-g-HDPE between PBT and HDPE. IE9 does not contain HDPE and has a higher wt% silane copolymer compared to IE6, IE7, and IE8. The level of OH-PDMS was also increased compared to IE8 to accommodate the higher level of silane copolymer. The results for IE9 indicate that acceptable mechanical properties can be obtained without the HDPE component compared to IE6, IE7, and IE8. IE10 is similar in composition to IE9, except that it does not contain MAH-g-HDPE and HDPE. The amount of silane copolymer was increased to 24 wt% in IE10. Compared with IE5-IE9, the tube rupture stress and flexural modulus of IE10 decreased significantly, but the zero shear viscosity increased and did not exhibit kinking, indicating that sufficiently high levels of silane copolymer were able to maintain morphological stability and provide sufficient viscosity to maintain dimensional stability during extrusion.
[0137] The results demonstrate the ability to produce a composition that can be melt mixed and immediately used for extrusion while providing acceptable mechanical properties. In addition, the composition can use lower cost and lower viscosity injection molding grade PBT materials while maintaining dimensional stability.
Claims
1. A method wherein The following steps are involved: A polymer composition is blended, the polymer composition comprising: (a) 5 wt % to 45 wt % of a silanol-functionalized polyolefin, based on the total weight of the polymer composition; (b) 50 wt% to 74 wt% of polybutylene terephthalate, based on the total weight of the polymer composition, having a melt flow index of 21 to 35 g / 10 min at 250° C. and 2.16 Kg, measured according to ASTM method D1238; (c) a condensation catalyst, wherein the condensation catalyst comprises dibutyltin dilaurate, dibutyltin diacetate, dioctyltin dilaurate, stannous acetate, stannous octoate, lead naphthenate, zinc octoate, cobalt naphthenate, ethylamine, dibutylamine, hexylamine, pyridine, sulfuric acid, hydrochloric acid, acetic acid, stearic acid or maleic acid; and (d) 0.5 wt% to 10 wt% of a hydroxyl-terminated poly(dimethylsiloxane), based on the total weight of the polymer composition; and extruding the polymer composition; Wherein the blending step further comprises blending 0.1 wt % to 10 wt % of a maleated ethylene-based polymer into the polymer composition, based on the total weight of the polymer composition.
2. The method of claim 1, wherein the silanol functionalized polyolefin comprises 0.5 wt% to 2.5 wt% silane based on the weight of the silanol functionalized polyolefin.
3. The method of any one of claims 1-2, wherein the silanol functionalized polyolefin has a density in the range of 0.91 g / cc to 0.94 g / cc as measured according to ASTM D792.
4. The method of any one of claims 1-2, wherein the polymer composition comprises 2 wt% to 5 wt% of the maleated ethylene-based polymer, based on the total weight of the polymer composition.
5. The method of claim 4, wherein the maleated ethylene-based polymer has a density of 0.958 g / cc as measured according to ASTM D792.
6. The method of any one of claims 1-2, wherein the blending step further comprises blending 5 wt% to 25 wt% of a high density polyethylene into the polymer composition, based on the total weight of the polymer composition, and wherein the high density polyethylene has a density of 0.94 g / cc to 0.98 g / cc as measured according to ASTM D792.
7. The method of claim 1, wherein the polymer composition comprises 5 wt% to 25 wt% of a silanol-functionalized polyolefin, 60 wt% to 74 wt% of polybutylene terephthalate, 1 wt% to 6 wt% of a maleated ethylene-based polymer, and 0.5 wt% to 5 wt% of a hydroxyl-terminated poly(dimethylsiloxane).
8. The method of claim 1 wherein the silanol functionalized polyolefin is an ethylene-silane copolymer.
9. The method according to any one of claims 1-2, wherein extruding the polymer composition is extruding the polymer composition into an optical fiber buffer tube.
10. The method according to any one of claims 1-2, wherein the condensation catalyst comprises dibutyltin dilaurate, dibutyltin diacetate, dioctyltin dilaurate, stannous acetate or stannous octoate.
Citation Information
Patent Citations
High-density polyethylene compositions, method of making the same, wire and cable jackets made therefrom, and method of making such wire and cable jackets
US20090068429A1
Process for the preparation of high density ethylene polymers in fluid bed reactor
US4303771A
Process and catalyst for polyolefin density and molecular weight control
US5324800A
Polymeric compositions for optical fiber cable components
WO2019050627A1
Polymer articles made from a blend of a copolyester elastomer and an alpha-olefin vinyl acetate copolymer
CN104540893A