An electrolyte containing a fluorinated solvent and a pyrazole additive
By using electrolyte containing fluorine solvents and pyrazole additives in lithium-ion batteries, the problems of poor circulation performance and insufficient thermal stability of lithium-ion batteries under high temperature and high pressure are solved, and higher battery life and safety are achieved performance.
Patent Information
- Application Number
- CN202210312896.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-28
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-03-28
AI Technical Summary
Existing lithium-ion batteries have poor cycling performance under high temperature and high pressure, and conventional electrolytes are easy to decompose at high voltage, resulting in insufficient battery life and thermal stability, and the inability to effectively improve the battery's energy density and range.
The electrolyte containing fluorine solvents and pyrazole additives is used to form a stable electrolyte system by reasonably combining fluorinated organic solvents and pyrazole compounds, thereby improving the cycling performance and thermal stability of the battery under high temperature and high pressure.
It significantly improves the high-voltage circulation capability and battery life of lithium-ion batteries, ensures the stability and safety performance of the battery in high and low temperature environments, avoids the problems of electrolyte decomposition and SEI film instability, and extends the service life of the battery.
Smart Images

Figure CN114665154B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion battery materials and relates to an electrolyte, in particular to an electrolyte containing a fluorine-containing solvent and a pyrazole additive. Background Art
[0002] Lithium-ion batteries have a series of advantages such as high operating voltage, high energy and power density, long cycle life, low self-discharge and environmental friendliness. They are currently widely used in mobile electronic devices and are widely used in electric vehicles. With the continuous upgrading of smartphone functions and the market's demand for improved mileage of electric vehicles, the requirements for batteries have been greatly increased, and improving the energy density of lithium batteries has become increasingly important and urgent. At present, the ester electrolyte of conventional lithium-ion batteries is easily decomposed under high voltage, resulting in relatively low charging and discharging efficiency and poor cycle performance of lithium-ion batteries; and the use of high-voltage additives to form a film on the surface of the positive electrode to prevent direct contact between the positive electrode and the electrolyte will lead to large battery polarization and rapid cycle decay.
[0003] For example, patent CN109786831A discloses an electrolyte containing a silicon solvent and a pyrazole additive and a lithium-ion battery using the electrolyte. The prepared high-voltage electrolyte for lithium-ion batteries can effectively improve the conductivity of lithium ions in the electrolyte under low temperature conditions and improve the low-temperature performance of the battery. However, there is no significant improvement in the cycle performance of the battery under high temperature and high voltage. Moreover, the external SEI film formed by the silicon solvent in a continuous cycle is unstable, which leads to further decomposition of the electrolyte and is accompanied by low Coulomb efficiency and capacity loss.
[0004] For example, CN111129664A discloses a lithium-ion battery electrolyte and a lithium-ion battery thereof. The electrolyte includes fluorinated ester compounds and cyanocyclic unsaturated hydrocarbon compounds, which are helpful for forming a stable SEI film at the negative electrode, and the cyanocyclic unsaturated hydrocarbon substances can improve the overcharge resistance and cyclability of the lithium cobalt oxide battery. However, such batteries often have a short cycle life at high temperatures and poor high-temperature storage performance.
[0005] Furthermore, although the above existing technologies have improved the safety performance of lithium-ion batteries to a certain extent, they cannot improve the high-voltage cycle performance, battery life and thermal stability of the battery when applied to ternary batteries. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the above-mentioned background technology and provide a lithium ion battery electrolyte and a lithium ion battery thereof containing a fluorinated solvent and a pyrazole additive, which have good room temperature and high temperature cycle stability and low battery impedance. The use of the electrolyte provided by the present invention can not only ensure the high-voltage cycle capability of the lithium ion battery, but also improve the battery life and thermal stability.
[0007] To achieve the above object, the technical solution adopted by the present invention is:
[0008] The present invention provides an electrolyte for a ternary lithium-ion battery, the electrolyte comprising a lithium salt, an organic solvent and an additive; the organic solvent comprises one or more of a chain carbonate organic solvent, a cyclic carbonate organic solvent and a fluorinated organic solvent, and the additive comprises a pyrazole compound; the mass proportion of the fluorinated organic solvent in the electrolyte is 10%-30%, and the mass proportion of the pyrazole compound is 1%-2%.
[0009] As an embodiment of the present invention, the structural formula of the fluorinated organic solvent is as shown in formula (I) or formula (II):
[0010] (I) (II);
[0011] In formula (I), R1 and R2 represent an alkyl group or an alkoxy group containing 1 to 6 carbon atoms, or a fluoroalkyl group or a fluoroalkoxy group containing 1 to 6 carbon atoms, and at least one of R1 or R2 is a fluoroalkyl group or a fluoroalkoxy group containing 1 to 6 carbon atoms;
[0012] In formula (II), R3 and R4 represent an alkyl or alkoxy group containing 1 to 6 carbon atoms, or a fluoroalkyl or fluoroalkoxy group containing 1 to 6 carbon atoms, and at least one of R3 and R4 is a fluoroalkyl or fluoroalkoxy group containing 1 to 6 carbon atoms.
[0013] As an embodiment of the present invention, the compound represented by formula (I) is 2,2-difluoroethyl ethyl carbonate or 2,2-difluoroethyl methyl carbonate.
[0014] As an embodiment of the present invention, the compound represented by formula (II) is ethyl 3,3,3-trifluoropropionate or isopropyl 3,3,3-trifluoropropionate.
[0015] As an embodiment of the present invention, the additive further comprises FEC and DTD. The mass percentage of FEC in the electrolyte is 3-5%, and the mass percentage of DTD in the electrolyte is 1-2%.
[0016] As an embodiment of the present invention, the structural formula of the pyrazole compound is as shown in formula (III):
[0017] (III); wherein R5-R8 are each independently selected from a hydrogen atom, an ester group containing 1 to 6 carbon atoms, an alkyl group or a substituted alkyl group containing 1 to 6 carbon atoms, an alkoxy group or a substituted alkoxy group containing 1 to 6 carbon atoms, and the substituent in the substituted alkyl group or the substituted alkoxy group is selected from a phenyl group, a C1-C6 alkenyl group or an alkynyl group.
[0018] As an embodiment of the present invention, in the structural formula of the pyrazole compound, R5-R7 are independently selected from hydrogen atoms, alkyl groups containing 1 to 6 carbon atoms or alkoxy groups containing 1 to 6 carbon atoms, and R8 is selected from ester groups containing 1 to 6 carbon atoms.
[0019] As an embodiment of the present invention, the structural formula includes .
[0020] As an embodiment of the present invention, the lithium salt is selected from one or more of LiPF6, LiBF4, LiClO4, LiBOB, LiODFB, LiAsF6, LiN(SO2CF3)2, and LiN(SO2F)2.
[0021] As an embodiment of the present invention, the molar concentration of the lithium salt in the electrolyte is 1-1.5M.
[0022] The organic solvent in the present invention can be selected from chain carbonate organic solvents and cyclic carbonate organic solvents. Chain carbonate organic solvents can be selected from one or more of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and dipropyl carbonate (DPC). Cyclic carbonate organic solvents can be selected from one or more of ethylene carbonate, vinylene carbonate, and propylene carbonate.
[0023] As an embodiment of the present invention, the organic solvent contains, in addition to the fluorinated organic solvent, a mixed solvent consisting of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC) and vinylene carbonate in a weight ratio of 20-40:5-20:15-40:30-40:5-15.
[0024] As an embodiment of the present invention, the molar concentration of the lithium salt in the electrolyte is 1-1.5 M. The lithium salt is selected from one or more of LiPF6, LiBF4, LiClO4, LiBOB, LiODFB, LiAsF6, LiN(SO2CF3)2, and LiN(SO2F)2.
[0025] The present invention also provides a ternary lithium ion battery, which contains the aforementioned electrolyte.
[0026] As an embodiment of the present invention, the ternary lithium-ion battery comprises LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2、LiNi0.5 Co 0.2 Mn 0.3 O2、LiNi 0.8 Co 0.15 Al 0.05 O2, etc.
[0027] In the lithium battery of the present invention, preferably, the preparation method of the lithium ion battery is: injecting an electrolyte containing a fluorinated solvent and a pyrazole additive into a fully dried 4.45V LiNi 0.5 Co 0.2 Mn 0.3 The O2 / graphite soft-pack dry battery cell is then subjected to aging, high-temperature formation, secondary sealing and capacity separation processes.
[0028] Alternative implementations:
[0029] The positive electrode active material may also be selected from LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2、LiNi 0.8 Co 0.15 Al 0.05 O2、LiNi 0.5 Co 0.2 Mn 0.3 The negative electrode active material may also be selected from one or more of natural graphite, artificial graphite, silicon, and silicon-carbon composites.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] 1) The fluorinated solvent and pyrazole compound with specific structure in the ternary lithium-ion battery electrolyte of the present invention have wider oxidation stability, which can solve the problem that the external SEI film formed by the silicon-containing solvent in the electrolyte system of the prior art is unstable during continuous circulation, thereby causing further decomposition of the electrolyte and accompanied by low Coulomb efficiency and capacity loss;
[0032] 2) In the ternary lithium-ion battery electrolyte of the present invention, pyrazole compound additives and other functional additives (fluorinated solvents, etc.) are used in a reasonable combination, which can solve the problems of the electrolyte system containing fluorinated ester compounds and cyanocyclic unsaturated hydrocarbon compounds in the prior art, such as short cycle life at high temperature and poor high temperature storage performance;
[0033] 3) By improving the interface between the positive and negative electrodes, the battery can have better cycle performance in extreme high and low temperature environments, thereby improving the battery life and safety performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:
[0035] Figure 1 It is a schematic diagram for comparing 1C cycles of lithium-ion batteries using the electrolytes of various embodiments and comparative examples under high temperature conditions of 45°C. DETAILED DESCRIPTION
[0036] The present invention is described in detail below in conjunction with embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, some adjustments and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0037] The structural formulas of the fluorinated organic solvents and pyrazole compounds involved in the following examples are as follows:
[0038]
[0039] Fluorinated compounds (1) Pyrazole compounds (1)
[0040] The structural formula of the cyanocyclic unsaturated hydrocarbon compound involved in Comparative Example 3 is: ; The structural formula of the silicon-containing solvent involved in Comparative Example 4 is: ; The fluorine-containing pyrazole compound involved in Comparative Example 5 is .
[0041] Example 1
[0042] In a glove box, solvents ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), and vinylene carbonate are mixed in a weight ratio of EC / PC / EMC / DEC / vinylene carbonate = 25 / 5 / 40 / 30 / 10 to obtain a mixed solvent, and then a fluorine compound (1) is added to the mixed solvent, and then a lithium salt LiPF6 is added to dissolve to prepare a solution containing lithium salt LiPF6. Thereafter, other additives such as FEC, DTD, and a pyrazole compound (1) are added to the prepared solution containing lithium salt LiPF6 to obtain a lithium ion battery electrolyte product. The molar concentration of the lithium salt in the electrolyte is 1M, the mass percentage of the fluorine compound in the electrolyte is 10%, the mass percentage of the pyrazole compound in the electrolyte is 2%, the mass percentage of FEC in the electrolyte is 5%, and the mass percentage of DTD in the electrolyte is 2%.
[0043] The prepared lithium-ion battery electrolyte was injected into the fully dried 4.45V LiNi 0.5 Co 0.2 Mn 0.3 The O2 / graphite soft-pack dry cell is subjected to processes such as 45°C storage, high-temperature fixture formation and secondary sealing to obtain a lithium-ion battery.
[0044] Embodiment 2-3:
[0045] The electrolyte formulation components of Examples 2-3 are shown in Table 1, and the preparation method is the same as that of Example 1.
[0046] The prepared lithium-ion battery electrolyte was injected into the fully dried 4.45V LiNi 0.5 Co 0.2 Mn 0.3 The O2 / graphite soft-pack dry cell was placed at 45°C, formed in a high-temperature fixture, and sealed for the second time to obtain the lithium-ion battery of Example 2-3.
[0047] Comparative Examples 1-5:
[0048] The electrolyte formulation components of Comparative Examples 1-5 are shown in Table 2, and the preparation method is the same as that of Example 1.
[0049] The prepared lithium-ion battery electrolyte was injected into the fully dried 4.45V LiNi 0.5 Co 0.2 Mn 0.3 The O2 / graphite soft-pack dry battery cell is placed at 45°C, formed in a high-temperature fixture, and sealed twice to obtain the lithium-ion battery of Comparative Example 1-5.
[0050] Functional testing:
[0051] Under high temperature (45°C), the above lithium-ion battery was charged to 4.45V at 1C constant current and constant voltage, and then discharged to 2.8V at 1C constant current. The discharge capacity of the first cycle was taken as 100%, and the discharge capacity retention rate was calculated. The results are as follows:
[0052] like Figure 1 , compared with the comparative example 1 in which only pyrazole compounds were added without adding fluorine compounds. After a certain number of high-temperature cycles, the cycle trend is still maintained without diving. The comparative example 1 without adding fluorine compounds has obvious diving. This is because its SEI film is unstable during the cycle, which leads to further decomposition of the electrolyte and is accompanied by low Coulomb efficiency and capacity loss.
[0053] Compared with Comparative Example 2 in which fluorine compounds are added but no pyrazole compounds are added, the high temperature capacity retention rate is always higher than that of Comparative Example 2. Since the pyrazole compounds can form a film on the surface of the positive electrode and protect the active sites of the positive electrode, the high temperature cycle performance of the battery is greatly improved.
[0054] Comparative Example 3 in which a fluorine compound and a cyanocyclic unsaturated hydrocarbon compound are added. Figure 1 It can be seen that the capacity retention rate of Example 3 decreases rapidly after the start of the cycle and then gradually slows down after about 80 weeks. Example 1 always maintains a good cycle trend. This shows that the additive in Example 1 has a significant effect on the stability of the graphite anode at high temperature and high voltage. The graphite anode can be protected from the beginning of the cycle and the reversible Li + De-embedding.
[0055] Comparative Example 4 in which a silicon-containing solvent and a pyrazole additive are added. Figure 1 It can be seen that the decay trend of Comparative Example 4 after the cycle starts is worse than that of Example 1, but it basically maintains linear decay. It can be seen that fluorinated solvents are more helpful for the stability of the battery at high temperatures. This may be because fluorinated solvents and co-solvents have a wider oxidation stability than ordinary organic solvents.
[0056] Comparative Example 5 in which a fluorine compound and a fluorine-containing pyrazole additive are added. Figure 1 It can be seen that after the cycle starts, the decay trend of Comparative Example 5 is significantly worse than that of Example 1. It can be seen that the silicon-containing solvent has poor stability at high temperatures, generates more gas and heat, and has an irreversible effect on the battery interface during the cycle.
[0057] Example and comparative example ratio:
[0058] Table 1
[0059]
[0060] Table 2
[0061]
[0062] Comparison of capacity retention rates of three groups of embodiments ( Figure 1 ), the cycle trends of Examples 1, 2, and 3 are all better than those of Comparative Examples 1-6, which basically confirms the above speculation. Example 2 has an obvious diving trend in the later stage of the cycle, which may be due to the addition of more fluorine compounds, and the reversible Li in the graphite anode cannot be maintained in the later stage of the cycle. + Disembedding creates a dead zone which results in a sharp dive.
[0063] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.
Claims
1. An electrolyte for a ternary lithium-ion battery, characterized in that: The electrolyte comprises a lithium salt, an organic solvent and an additive; the organic solvent comprises a fluorinated organic solvent, and further comprises one or more of a chain carbonate organic solvent and a cyclic carbonate organic solvent; the additive comprises a pyrazole compound; the mass proportion of the fluorinated organic solvent in the electrolyte is 10%-30%, and the mass proportion of the pyrazole compound is 1%-2%; the structural formula of the fluorinated organic solvent is: ; The pyrazole compound structural formula is: .
2. The electrolyte according to claim 1, characterized in that The chain carbonate organic solvent is selected from one or more of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, and dipropyl carbonate; the cyclic carbonate organic solvent is selected from one or more of ethylene carbonate, vinylene carbonate, and propylene carbonate.
3. The electrolyte according to claim 1, characterized in that The organic solvent contains, in addition to the fluorinated organic solvent, a mixed solvent consisting of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate and vinylene carbonate in a weight ratio of 20-40:5-20:15-40:30-40:5-15.
4. The electrolyte according to claim 1, characterized in that The lithium salt is selected from one or more of LiPF6, LiBF4, LiClO4, LiBOB, LiODFB, LiAsF6, LiN(SO2CF3)2, and LiN(SO2F)2; the molar concentration of the lithium salt in the electrolyte is 1-1.5M.
5. A ternary lithium-ion battery, characterized in that: The lithium ion battery contains the electrolyte according to any one of claims 1 to 4.
6. The ternary lithium-ion battery according to claim 5, characterized in that: The ternary lithium-ion battery includes LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2、LiNi 0.5 Co 0.2 Mn 0.3 O2、LiNi 0.8 Co 0.15 Al 0.05 One or more of O2.