A lithium ion battery
The use of LiCoO2/C3N4 and M2GeO4 composite materials solves the shortcomings of lithium cobalt oxide and graphite materials, improves the electrochemical performance and capacity of lithium-ion batteries, and is suitable for power batteries.
Patent Information
- Application Number
- CN202210594103.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-27
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-05-27
AI Technical Summary
The existing lithium-ion battery cathode material, lithium cobalt oxide, is expensive and has poor conductivity, while the anode material, graphite, is prone to failure during use, making it difficult to meet the requirements for high energy density and long lifespan.
The battery was prepared by using LiCoO2/C3N4 composite material as positive electrode active material and M2GeO4 (M=Zn, Mn, Co, Cd) as negative electrode active material through solid-phase molten salt method, combined with germanate as negative electrode active material, to improve the electrochemical performance of the battery.
It improves the reversible capacity and cycle performance of lithium-ion batteries, enhances the fast-charging performance of batteries, reduces costs, and is suitable for power batteries.
Smart Images

Figure CN114843486B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a lithium ion battery. Background Art
[0002] The development of green energy is an important topic at present. Lithium-ion batteries have the advantages of high energy density, long service life, and strong endurance, and are widely used in electronic portable devices and electric vehicles.
[0003] Currently, commercial positive electrode materials include lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, and high-nickel ternary lithium batteries. Among them, lithium cobalt oxide has relatively stable cycle performance, lithium manganese oxide has a lower cost, and lithium iron phosphate has better adaptability to conditions with large temperature differences. Although lithium cobalt oxide has good chemical stability and large capacity, it is expensive and has poor conductivity. Commercial negative electrode materials are mainly graphite, which has the advantages of high electronic conductivity, small volume change before and after charging and discharging, and low cost. However, graphite is already close to the theoretical value, and may fail during use, making it difficult to meet energy needs. Metal germanium has a higher theoretical specific capacity (1600mAh·g -1 ), excellent conductivity, low working potential and high ion diffusion rate, and is considered to be the most promising graphite in lithium-ion batteries (372mAh·g -1 ) is one of the alternatives.
[0004] Therefore, it is necessary to develop high-performance lithium-ion battery positive and negative electrode materials to improve the battery capacity of lithium-ion batteries. Summary of the invention
[0005] In order to solve the technical problem of improving the capacity of lithium ion batteries, a lithium ion battery is provided. The lithium ion battery of the present invention has a higher reversible capacity and better cycle performance and rate performance.
[0006] In order to achieve the above objectives, the present invention is implemented by the following technical solutions:
[0007] A lithium-ion battery comprises the following structure: a wound cell assembly, an electrolyte impregnated with the wound cell assembly, a metal shell loaded with the wound cell assembly and the electrolyte, and a sealing cover sealing the metal shell; the wound cell assembly comprises a positive electrode foil, a negative electrode foil and a separator separating the positive electrode foil from the negative electrode foil;
[0008] The positive electrode foil contains a positive electrode active material, which is a LiCoO2 / C3N4 composite material; the negative electrode foil contains a negative electrode active material, which is a M2GeO4 material, wherein M is selected from one or more of Zn, Mn, Co, and Cd, and the specific M2GeO4 material is Zn2GeO4, Mn2GeO4, Co2GeO4, Zn 1.8 Cd0.2 GeO4.
[0009] Furthermore, the preparation method of the LiCoO2 / C3N4 composite material comprises the following steps:
[0010] (1) Mixing lithium salt, cobalt salt and chloride salt uniformly, calcining at 540°C for 4 hours in an air atmosphere, and then washing and drying with water to obtain LiCoO2 after cooling;
[0011] Melamine was calcined at 550°C for 4 h to obtain C3N4;
[0012] (2) LiCoO2 and C3N4 were mixed and dispersed in an alcohol solvent and ball-milled. After drying, the mixture was calcined at 550°C for 4h to obtain a LiCoO2 / C3N4 composite material.
[0013] Preferably, the lithium salt is one or more of lithium carbonate, lithium acetate, and lithium nitrate, and more preferably, the lithium salt is lithium nitrate; the cobalt salt is one or more of cobalt nitrate, cobalt acetate, and cobalt carbonate, and more preferably, the cobalt salt is cobalt carbonate; the chloride salt is a mixture of potassium chloride and lithium chloride in a mass ratio of 6:1. All of the above are salt substances that are easily decomposed by high temperature and are easy to combine into target products in ions in molten salt (chloride salt).
[0014] Preferably, the ratio of the total amount of the lithium salt and the cobalt salt to the amount of the chloride salt is 2 mmol:(4-6) g; the mass ratio of the LiCoO2 to the C3N4 is (1-50):1.
[0015] Furthermore, the preparation method of the M2GeO4 material includes the following steps: grinding germanium salt, metal salt containing one or more elements of Cd, Cu, Zn, and Mn with chloride salt to mix evenly, calcining at 500-600°C for 4 hours in an air atmosphere, and soaking, cleaning, and drying with water after cooling to obtain the M2GeO4 material.
[0016] Preferably, the germanium salt is germanium nitrate and / or germanium oxide; the metal salt is one or more of carbonate, nitrate, acetate; the chloride salt is a mixture of potassium chloride and lithium chloride in a mass ratio of 6:1; the ratio of the total amount of the germanium salt and the metal salt to the amount of the chloride salt is 3mmol:(4-6)g.
[0017] Beneficial technical effects:
[0018] (1) The present invention adopts the solid-phase molten salt method to obtain the positive electrode active material LiCoO2 / C3N4 composite material and the negative electrode active material M2GeO4 (M=Zn, Mn, Co, Cd or one or more). The obtained products have good chemical stability and structuring. The solid-phase molten salt method is simple and easy to operate. Compared with the solvent thermal synthesis method, the present invention does not require experimental solvents, reducing the pollution caused by organic reagents. Compared with the solid-phase sintering method, the present invention uses salt as a solvent to make the material react fully, with better crystallinity and purer phase.
[0019] (2) The theoretical specific capacity of lithium cobalt oxide is 274 mAh / g, but only about 150 mAh / g can be used. The present invention uses C3N4 to compound the material on the basis of synthesizing LiCoO2 to increase the conductivity of LiCoO2, and uses cheap C3N4 to replace part of LiCoO2. On the basis of unchanged quality, it not only improves the performance of the raw materials, but also reduces the cost and improves the specific capacity of the battery.
[0020] (3) In the past, germanate was often used in the field of photocatalysis. In the present invention, germanate is used as the negative electrode active material of the battery in combination with the LiCoO2 / C3N4 composite material of the positive electrode, so that the assembled battery has higher electrochemical performance. Germanate can provide high capacity and strong ability for lithium ion insertion and extraction, thereby improving the electrochemical performance of the battery, and provides more active sites for the insertion and extraction of lithium ions on the positive electrode material. Compared with batteries made of other materials, the battery capacity is higher.
[0021] (4) Lithium-ion batteries made with LiCoO2 / C3N4 and M2GeO4 (M = one or more of Zn, Mn, Co, Cd) as electrode materials have high reversible capacity, good cycle performance and rate performance, and relatively stable fast charging performance, and can be used as power batteries.
[0022] (5) During the experiment of the present invention, the N / P ratio is preferably confirmed to be between 1 and 1.2 to ensure the compatibility of the positive and negative electrode materials and to maximize the electrochemical performance of the positive and negative electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The XRD graphs of the LiCoO2 / C3N4 (10%) composite material of Example 1 and the XRD graphs of the LiCoO2 / C3N4 (5%) composite material of Example 2 are shown.
[0024] Figure 2 This is the Zn2GeO4 (XRD) diagram.
[0025] Figure 3 This is the Mn2GeO4 (XRD) diagram.
[0026] Figure 4 It is Co2GeO4 (XRD).
[0027] Figure 5 Zn 1.8 Cd 0.2 GeO4 (XRD) pattern.
[0028] Figure 6 Cycling performance diagram of cylindrical cells assembled for LiCoO2 / C3N4(10%)-Zn2GeO4.
[0029] Figure 7 Cycling performance diagram of cylindrical batteries assembled for LiCoO2 / C3N4(5%)-Zn2GeO4.
[0030] Figure 8 Cycling performance diagram of cylindrical cells assembled for LiCoO2 / C3N4(20%)-Zn2GeO4.
[0031] Fig. 9 Cycling performance diagram of cylindrical cells assembled for LiCoO2 / C3N4(10%)-Mn2GeO4.
[0032] Fig.10 Cycling performance diagram of cylindrical battery assembled for LiCoO2 / C3N4(10%)-Co2GeO4
[0033] Fig.11 LiCoO2 / C3N4(10%)-Zn 1.8 Cd 0.2 Cycling performance diagram of GeO4 assembled cylindrical batteries. DETAILED DESCRIPTION
[0034] The technical solutions in the embodiments of the present invention will be described clearly and completely below in combination with the embodiments of the present invention and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. All other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention are within the scope of protection of the present invention.
[0035] Unless otherwise specifically stated, the numerical value set forth in these embodiments does not limit the scope of the present invention. The technology and method known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology and method should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values.
[0036] The experimental methods in the following examples without specifying specific conditions are usually measured according to national standards; if there is no corresponding national standard, it is carried out according to the general international standards or the standard requirements proposed by relevant enterprises. Unless otherwise specified, all parts are by weight and all percentages are by weight.
[0037] Example 1
[0038] A lithium-ion battery comprises the following structure: a wound cell assembly, an electrolyte impregnated with the wound cell assembly, a metal shell loaded with the wound cell assembly and the electrolyte, and a sealing cover sealing the metal shell; the wound cell assembly comprises a positive electrode foil, a negative electrode foil and a separator separating the positive electrode foil from the negative electrode foil; the substrate of the positive electrode foil is a carbon-coated aluminum foil, the carbon-coated aluminum foil contains a positive electrode active material, and the positive electrode active material is a LiCoO2 / C3N4 composite material; the substrate of the negative electrode foil is a copper foil, the copper foil contains a negative electrode active material, and the negative electrode active material is a Zn2GeO4 material.
[0039] The preparation of the positive electrode foil: the positive electrode active material LiCoO2 / C3N4 composite material, the conductive carbon black Super P, and the polymer binder polyvinylidene fluoride are stirred in a mass ratio of 8:1:1 for about 20 minutes until they are evenly mixed, an appropriate amount of N-methylpyrrolidone is added, and the mixing is continued until the mixture is evenly dispersed to form a mixed slurry. A carbon-coated aluminum foil is selected as the current collector, and the mixed slurry is evenly coated on the carbon-coated aluminum foil. The mixture is vacuum dried at 80°C for 12 hours to obtain the working electrode positive electrode foil.
[0040] The preparation method of the LiCoO2 / C3N4 composite material is as follows: 1mmol of cobalt nitrate and 1mmol of lithium carbonate are placed in 3.6g of potassium chloride and 0.6g of lithium chloride, 20mL of ethanol is added, and the mixture is ground in a mortar grinder at a speed of 300rpm for 2h to mix evenly, and then placed in a muffle furnace with a heating rate of 5℃ / min, heated to 540℃ in an air atmosphere, and calcined for 4h. After the calcination, it is naturally cooled to room temperature, and the product is soaked and washed with deionized water. After solid-liquid separation, it is dried in an oven at 80℃ to obtain LiCoO2; melamine is placed in a muffle furnace and heated to 55 The mixture was calcined at 0℃ for 4h, and after calcination, it was naturally cooled to room temperature to obtain C3N4 material; then LiCoO2 and C3N4 were mixed in a mass ratio of 10:1, alcohol was added and ultrasonicated for 30 minutes until uniform dispersion was achieved, the dispersed material was placed in an oven for drying, and finally the dried material was placed in a tubular furnace for calcination at 550℃ for 4h. After calcination, it was naturally cooled to room temperature to obtain LiCoO2 / C3N4 composite material. The positive electrode active material of this embodiment is recorded as LiCoO2 / C3N4 (10%), where 10% represents the mass fraction of carbon nitride relative to lithium cobalt oxide. The XRD pattern of the material is shown in the figure below: Figure 1 As shown, the composite C3N4 is an amorphous material, so no diffraction peak can be formed in the XRD test. The XRD pattern of the test is consistent with that of LiCoO2, the diffraction peaks can all correspond, and there are no other impurity peaks in the material.
[0041] Preparation of the negative electrode foil: Stir the negative electrode active material Zn2GeO4 material with the conductive carbon black Super P and the polymer binder polyvinylidene fluoride in a mass ratio of 7:2:1 for about 20 minutes until they are evenly mixed, add an appropriate amount of N-methylpyrrolidone, continue to mix until they are evenly dispersed to form a mixed slurry, use copper foil as the current collector, evenly coat the mixed slurry on the copper foil, and vacuum dry at 80°C for 12 hours to obtain the negative electrode foil of the working electrode;
[0042] The preparation method of Zn2GeO4 material is as follows: 1mmol germanium nitrate and 2mmol zinc acetate are placed in 3.6g potassium chloride and 0.6g lithium chloride, 20mL ethanol is added, and the mixture is placed in a mortar grinder and ground at 300rpm for 2h to mix evenly, and then placed in a muffle furnace with a heating rate of 5℃ / min, heated to 540℃ in an air atmosphere, and calcined for 4h. After calcination, the mixture is naturally cooled to room temperature, and the product is washed and soaked in deionized water. After solid-liquid separation, the material is placed in an oven at 80℃ until dried to obtain Zn2GeO4 material. The XRD pattern of the material is as shown in FIG. Figure 2 As shown, it is confirmed that the diffraction peaks of the Zn2GeO4 material synthesized by the one-pot method can all correspond, and there are no other impurity peaks in the material, confirming that this material is a pure phase.
[0043] The diaphragm adopts ordinary Celgard2400 diaphragm; the electrolyte is LiPF6+EC / DMC / DEC with a concentration of 1M (the volume ratio of the three is 1:1:1), and a cylindrical battery is made. For specific battery production, please refer to the description of Chinese patent 201911146515.1, paragraphs 0074-0080.
[0044] Example 2
[0045] The lithium ion battery of this embodiment is the same as that of Embodiment 1, except that the mass ratio of LiCoO2 and C3N4 in the positive electrode active material LiCoO2 / C3N4 composite material is 20:1, recorded as LiCoO2 / C3N4 (5wt%).
[0046] The XRD diffraction peak position of the positive electrode active material of this embodiment is the same as that of the positive electrode active material of Example 1.
[0047] Example 3
[0048] The lithium ion battery of this embodiment is the same as that of Embodiment 1, except that the mass ratio of LiCoO2 and C3N4 in the positive electrode active material LiCoO2 / C3N4 composite material is 5:1, recorded as LiCoO2 / C3N4 (20wt%).
[0049] The XRD diffraction peak position of the positive electrode active material of this embodiment is the same as that of the positive electrode active material of Example 1.
[0050] Example 4
[0051] The lithium ion battery of this embodiment is the same as that of embodiment 1, except that the amounts of potassium chloride and lithium chloride used in the preparation process of the positive electrode active material LiCoO2 / C3N4 composite material are 4.8 g and 0.8 g, respectively.
[0052] The XRD diffraction peak position of the positive electrode active material of this embodiment is the same as that of the positive electrode active material of Example 1.
[0053] Example 5
[0054] The lithium ion battery of this embodiment is the same as that of embodiment 1, except that during the preparation process of the negative electrode active material, manganese acetate and cobalt nitrate are used to replace zinc acetate, and the obtained negative electrode active materials are Mn2GeO4 and Co2GeO4 respectively.
[0055] Figure 3 and Figure 4 They are the X-ray diffraction patterns of manganese germanate and cobalt germanate of this embodiment. After comparison with the standard card, the synthesized materials are all pure phase.
[0056] Example 6
[0057] The lithium ion battery of this embodiment is the same as that of embodiment 1, except that the negative electrode active material is Zn 1.8 Cd 0.2 GeO4, wherein x represents the molar ratio, that is, 2 mmol of zinc acetate is replaced by 1.8 mmol of zinc acetate and 0.2 mmol of cadmium nitrate during the preparation process.
[0058] In this embodiment, the doping ratio of cadmium element is relatively small, so the X-ray diffraction pattern after doping will not change the peak position of Zn2GeO4, so the diffraction peak position does not change.
[0059] Comparative Example 1
[0060] The lithium ion battery of this embodiment is the same as that of embodiment 1, except that the positive electrode active material is pure LiCoO2 and the negative electrode active material is commercial graphite.
[0061] Comparative Example 2
[0062] The lithium ion battery of this embodiment is the same as that of embodiment 1, except that the positive electrode active material is a LiCoO2 / C composite material and the negative electrode active material is commercial graphite;
[0063] Preparation of LiCoO2 / C composite material as positive electrode active material: The prepared LiCoO2 was dispersed in 10wt% glucose solution, spray-dried and calcined at 540℃ for 4h to obtain LiCoO2 / C composite material, keeping the composite amount of C the same as that of the positive electrode active material in Example 1.
[0064] Comparative Example 3
[0065] The lithium ion battery of this embodiment is the same as that of Embodiment 1, except that the mass ratio of LiCoO2 and C3N4 in the positive electrode active material LiCoO2 / C3N4 composite material is 3.3:1, recorded as LiCoO2 / C3N4 (30wt%).
[0066] The specific capacity and capacity retention rate of the batteries made in the above embodiments and comparative examples after 100 cycles at different current densities are shown in Table 1.
[0067] Table 1 Electrochemical performance of batteries made in Examples and Comparative Examples
[0068]
[0069]
[0070] As can be seen from Table 1, compared with the current commercial negative electrode material graphite, at a current density of 0.5C, except for the LiCoO2 / C3N4 (10%)-Co2GeO4 assembled battery, the specific capacity after 100 cycles is about 77mAh / g, while the other LiCoO2 / C3N4 (5%)-Zn2GeO4 assembled batteries, LiCoO2 / C3N4 (10%)-Zn2GeO4 assembled batteries, LiCoO2 / C3N4 (20%)-Zn2GeO4 assembled batteries, LiCoO2 / C3N4 (10%)-Mn2GeO4 assembled batteries, LiCoO2 / C3N4 (10%)-Zn 1.8 Cd 0.2 The battery assembled with GeO4 has better performance, and the specific capacity can still reach above 95mAh / g after 100 cycles.
[0071] By comparing Examples 1-3, it can be seen that the carbon nitride compounding amount in the positive electrode active material composite material is increased from 5% to 20%, and the electrochemical performance of the battery shows a slightly declining trend with the increase in the carbon nitride compounding amount. Combined with the fact that the carbon nitride compounding amount in Comparative Example 3 is increased to 30%, the electrochemical performance of the battery has a smaller specific capacity at a larger current density, and is less than 70mAh / g after 100 cycles at a current density of 0.5C.
[0072] Compared with Example 1, Example 6 adds cadmium into the negative electrode zinc germanate active material, which helps to further improve the electrochemical activity of the battery.
[0073] Comparative Example 1 is a battery assembled with lithium cobalt oxide positive electrode active material and commercial graphite. Except that the battery assembled with LiCoO2 / C3N4 (10%)-Co2GeO4 has a slightly lower performance than that of the comparative example, the other batteries assembled with LiCoO2 / C3N4 (5%)-Zn2GeO4, LiCoO2 / C3N4 (10%)-Zn2GeO4, LiCoO2 / C3N4 (20%)-Zn2GeO4, LiCoO2 / C3N4 (10%)-Mn2GeO4, LiCoO2 / C3N4 (10%)-Zn 1.8 Cd 0.2 The performance of the batteries assembled with GeO4 is higher than that of Comparative Example 1.
[0074] Comparative Example 2 is based on Comparative Example 1. Carbon material is composited on lithium cobalt oxide, which is the positive electrode active material. Although the electrochemical activity of the battery is increased to a certain extent, the specific capacity after 100 cycles at a current density of 0.5C reaches 92.41 mAh / g, but compared with the batteries assembled with LiCoO2 / C3N4(5%)-Zn2GeO4, LiCoO2 / C3N4(10%)-Zn2GeO4, LiCoO2 / C3N4(20%)-Zn2GeO4, LiCoO2 / C3N4(10%)-Mn2GeO4, LiCoO2 / C3N4(10%)-Zn 1.8 Cd 0.2 As for the battery assembled with GeO4, the battery assembled in the present invention has better performance, and the specific capacity can still reach more than 95mAh / g after 100 cycles at a current density of 0.5C.
[0075] Depend on Figure 6-Figure 11 It can be seen that the charge and discharge curves overlap well under high current density 2C, indicating that the electrochemical performance of the assembled battery is relatively stable and the coulomb efficiency is relatively high. By doping Zn2GeO4 with Cd to modify the negative electrode active material, the electrochemical energy of the assembled battery can be further improved. Even when running at 2C current, after 100 cycles, except for the battery assembled with LiCoO2 / C3N4 (10%)-Co2GeO4, the others can maintain a specific capacity of more than 70mAh / g, and have good electrochemical performance in the field of power battery applications.
[0076] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A lithium-ion battery, It is characterized in that The invention comprises the following structures: a wound battery cell assembly, an electrolyte impregnated with the wound battery cell assembly, a metal shell loaded with the wound battery cell assembly and the electrolyte, and a sealing cover sealing the metal shell; the wound battery cell assembly comprises a positive electrode foil, a negative electrode foil and a separator separating the positive electrode foil from the negative electrode foil; The positive electrode foil contains a positive electrode active material, and the positive electrode active material is LiCoO 2 / C 3 N 4 Composite material, the LiCoO 2 With the C 3 N 4 The mass ratio is 10:1; The negative electrode foil contains a negative electrode active material, and the negative electrode active material is Zn 1.8 Cd 0.2 GeO 4 ; Zn 1.8 Cd 0.2 GeO 4 Preparation of materials: 1mmol germanium nitrate, 1.8mmol zinc acetate, and 0.2mmol cadmium nitrate were placed in 3.6g potassium chloride and 0.6g lithium chloride, and 20mL ethanol was added. The mixture was placed in a mortar grinder and ground at 300rpm for 2h to mix evenly. Then, the mixture was placed in a muffle furnace with a heating rate of 5℃ / min. The temperature was raised to 540℃ in an air atmosphere and the mixture was kept warm and roasted for 4h. After the roasting, the mixture was naturally cooled to room temperature. The product was washed with deionized water. After solid-liquid separation, the material was placed in an oven at 80℃ until it was dried to obtain Zn 1.8 Cd 0.2 GeO 4 Material.
2. A lithium ion battery according to claim 1, It is characterized in that The LiCoO 2 / C 3 N 4 The preparation method of the composite material comprises the following steps: (1) Lithium salt, cobalt salt and chloride salt were mixed evenly and calcined at 540°C for 4 h in an air atmosphere. After cooling, they were soaked in water, cleaned and dried to obtain LiCoO 2 ; Melamine was calcined at 550℃ for 4h to obtain C 3 N 4 ; (2) LiCoO 2 With C 3 N 4 The mixture was dispersed in an alcohol solvent and ball-milled, and then dried and calcined at 550 °C for 4 h to obtain LiCoO 2 / C 3 N 4 Composite materials.
3. A lithium ion battery according to claim 2, It is characterized in that The lithium salt is one or more of lithium carbonate, lithium acetate, and lithium nitrate; the cobalt salt is one or more of cobalt nitrate, cobalt acetate, and cobalt carbonate; the chloride salt is a mixture of potassium chloride and lithium chloride in a mass ratio of 6:1; The ratio of the total amount of the lithium salt and the cobalt salt to the amount of the chloride salt is 2 mmol:(4-6) g.