Method for improving hardness gradient of rail head section and rail head

Through the combined combination of the continuous casting speed control of the second cold electromagnetic stirring and solidification end electromagnetic stirring, the cross-sectional hardness gradient of the rail head is controlled, and the problem of uneven hardness in the existing technology is solved, and the significant reduction of the hardness gradient of the rail head and the tissue performance is achieved. The improvement extends the service life of the rail.

CN115488302BActive Publication Date: 2024-11-05PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211172001.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-26
Publication Date
2024-11-05
Estimated Expiration
2042-09-26

AI Technical Summary

Technical Problem

The prior art is difficult to effectively control the hardness gradient of the rail head cross section, resulting in uneven hardness and affecting the fatigue performance and service life of the rail.

Method used

The second-cold electromagnetic stirring and solidification end electromagnetic stirring combined with continuous casting speed control is used to regulate the macroscopic solute concentration and microstructure of the casting billet section. Through the dual-stage electromagnetic stirring control technology and continuous casting second-cold control, the hardness gradient of the rail rail head section is realized. Regulation.

Benefits of technology

It significantly reduces the hardness gradient of the rail head section, improves the uniformity of the structure performance of the material, extends the service life of the rail, and reduces the maintenance cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115488302B_ABST
    Figure CN115488302B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for improving the hardness gradient of a rail head section and a rail head. The hardness gradient of the rail head section is improved by controlling the parameters of the secondary cooling electromagnetic stirring and the electromagnetic stirring at the end of solidification, combined with the continuous casting speed control. The present invention innovatively solves the problem of the hardness gradient of the rail head section from the continuous casting stage. For the control of the hardness gradient of the heavy rail head section, the macroscopic solute concentration of the ingot section is systematically regulated, and a general heat treatment process is used to achieve the control of the hardness gradient of the heavy rail head section, providing continuous casting technical support for rail performance control.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of iron and steel metallurgy production, and in particular to a method for improving the cross-sectional hardness gradient of a rail head and a rail head. Background Art

[0002] As the main component of railway transportation construction, rails play an important role. On the one hand, they guide the train forward, and on the other hand, they bear the huge load of the train. Therefore, the quality of rails has an important impact on driving safety. In addition, with the continuous development of railway transportation, the transportation of passenger, high-speed and heavy-load freight has put forward higher requirements on the quality and performance of rails. The service performance of rails greatly determines the service life of rails and their maintenance costs.

[0003] It is necessary to improve the quality and performance of existing products and develop new high-performance products. Many scholars at home and abroad have carried out a lot of research. For example, many researchers have conducted in-depth research on the fatigue damage of rails. Their research usually homogenizes the hardness inside the rails, but actual product testing finds that the hardness inside the rails is not uniform. In addition, some scholars have pointed out that hardness is a very important influencing factor on the fatigue damage of rails. The researchers measured the cross-sectional hardness of rail heads of different varieties of rails, and the results showed that the cross-sectional hardness of the rail head gradually decreases from the surface to the inside. In addition, ASITHAC.ATHUKORALA studied the non-uniform hardness distribution, metallurgy and ratcheting behavior of Australian AS60HH rail steel. The results showed that the non-uniformity of the material will affect the ratcheting effect of the rail as the wear progresses, thereby affecting the service life of the rail.

[0004] Therefore, studying the distribution and control of rail hardness is of great significance to improving rail performance. Reducing the hardness gradient inside the rail head can reduce the difference in results produced by hardness homogenization research. Even for materials with small gradient hardness, the research within a smaller area can be simplified to hardness uniformity, thereby achieving the purpose of simplifying the research. For steel materials, the uniformity of organizational properties is a very important quality indicator. A large gradient of organizational properties will greatly weaken the comprehensive mechanical properties of the material, thereby reducing the reliability of the material performance.

[0005] A large number of scholars have conducted research on the hardness of steel, but most of them focus on heat treatment process research, analysis of the causes of incompatibility between hardness and structure, and the impact of hardness on other application performances. However, research on continuous casting control technology for the cross-sectional hardness distribution of heavy rail head has not yet been involved.

[0006] Based on this, the existing technology still needs to be improved. Summary of the invention

[0007] The main purpose of the present invention is to provide a method for improving the cross-sectional hardness gradient of a rail head and a rail head, so as to adjust the cross-sectional hardness gradient of a heavy rail head and provide continuous casting technical support for rail performance control.

[0008] According to one aspect of the present invention, a method for improving the hardness gradient of the rail head section is proposed, by controlling the parameters of the secondary cooling electromagnetic stirring and the electromagnetic stirring at the end of solidification, combined with the continuous casting speed control, to improve the hardness gradient of the rail head section.

[0009] In some embodiments, the parameter control of the secondary cooling electromagnetic stirring includes: the central magnetic field strength of the stirring coil of the secondary cooling electromagnetic stirring is 50×10 -4 ~100×10 -4 T.

[0010] In some embodiments, the parameter control of the secondary cooling electromagnetic stirring includes: the secondary cooling electromagnetic stirring is installed in a region 4000 to 5000 mm away from the liquid surface of the crystallizer.

[0011] In some embodiments, the parameter control of the electromagnetic stirring at the end of coagulation includes: the central magnetic field strength of the stirring coil of the electromagnetic stirring at the end of coagulation is 410×10 -4 ~450×10 -4 T.

[0012] In some embodiments, the parameter control of the electromagnetic stirring at the end of solidification includes: the electromagnetic stirring at the end of solidification is installed in a region 8000 to 10000 mm away from the liquid surface of the crystallizer.

[0013] In some embodiments, the continuous casting speed is controlled at 0.7 m / min.

[0014] In some embodiments, the method further includes controlling the water content of the secondary cooling in continuous casting.

[0015] In some embodiments, the continuous casting secondary cooling water volume is controlled at 160-180 L / min.

[0016] In some embodiments, the superheat degree of the molten steel in the casting process is 25-35°C.

[0017] On the other hand, an embodiment of the present invention further discloses a rail head, which is manufactured by the above-mentioned continuous casting method.

[0018] By adopting the above technical solution, the present invention has at least the following beneficial effects:

[0019] The method for improving the hardness gradient of the rail head section and the rail head provided by the present invention innovatively solve the hardness gradient problem of the rail head section from the continuous casting stage. For the control of the hardness gradient of the heavy rail head section, the macroscopic solute concentration of the ingot section is systematically regulated, and a general heat treatment process is used to achieve the hardness gradient control of the heavy rail head section, providing continuous casting technical support for rail performance control. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 , Figure 2 A schematic diagram showing a method for improving the hardness gradient of a rail head section disclosed in an embodiment of the present invention to adjust the local macroscopic solute concentration of the rail to change the hardness value of a corresponding position point of the rail. DETAILED DESCRIPTION

[0022] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the embodiments of the present invention are further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.

[0023] It should be noted that all expressions using "first" and "second" in the embodiments of the present invention are for distinguishing two non-identical entities with the same name or non-identical parameters. It can be seen that "first" and "second" are only for the convenience of expression and should not be understood as limitations on the embodiments of the present invention. The subsequent embodiments will not explain this one by one.

[0024] Some embodiments of the present invention disclose a method for improving the hardness gradient of the rail head section. For the hardness gradient control of the heavy rail head section, the key technology lies in the systematic regulation of the macro solute concentration of the ingot section, and the general heat treatment process, so as to achieve the hardness gradient control of the heavy rail head section, and provide continuous casting technical support for the rail performance control. The macro solute concentration distribution of the alloy elements in the heavy rail steel ingot section is changed by the two-stage electromagnetic stirring control technology integrating the secondary cooling electromagnetic stirring and the solidification end electromagnetic stirring; the electromagnetic stirring action position is regulated by the continuous casting drawing speed, so as to interactively coordinate the macro solute concentration of the alloy elements in the ingot section by the drawing speed and electromagnetic stirring; the continuous casting secondary cooling control is performed, and the macro solute diffusion control and micro segregation control of the ingot section are comprehensively achieved by regulating the secondary cooling intensity. In this way, the macro solute concentration of the alloy elements in the ingot section is finely regulated, and the high-level control of the micro segregation of the ingot is taken into account, and finally the coordinated regulation of the hardness and micro (phase change) structure of the rail head section after the ingot is rolled into a rail is achieved.

[0025] like Figure 1 , Figure 2 As shown, the method of the present invention is used to control the local macroscopic solute concentration of the rail to change the hardness value of the corresponding position point of the rail. Specifically, after implementing secondary cooling electromagnetic stirring with a certain intensity, the macroscopic concentration of the solute element at 20mm from the tread of the rail is increased, thereby changing the hardness evolution trend of the rail from 15mm to 20mm from the tread, reducing the hardness difference between the two points from A to B, and thus reducing the hardness gradient of the local area.

[0026] The fundamental principle is to intervene in the macroscopic concentration distribution of solute elements in the cross section of the ingot by electromagnetic stirring in advance during continuous casting, and based on its genetic characteristics after rolling into rails, to increase or decrease the concentration of solute elements at specific positions of the rails in a targeted manner, thereby achieving the cross-sectional hardness control of the rails under specific heat treatment process conditions. For example, generally speaking, assuming that the solute concentration of the ingot cross section is uniformly distributed, the corresponding cross-sectional solute element concentration of the rails is also uniformly distributed. Under this condition, the inevitable difference in cooling rate inside and outside the rails during heat treatment will directly affect the characteristics of the microstructure of the phase change process, thereby leading to performance differences between the inside and outside of the rails. Generally, the farther from the surface of the rail, the slower the cooling, the coarser the grains, and the lower the hardness. As a result, the hardness of the rails changes from high to low when moving from the surface to the center, thereby generating a hardness gradient. The improvement of the hardness gradient of the rail cross section is conducive to improving the performance of the rails. For example, if the hardness gradient needs to be reduced in a certain area, the solute concentration at the point farther from the surface of the rails can be increased to compensate for the hardness drop caused by the lower actual cooling rate, thereby reducing the hardness gradient in the area and achieving rail performance improvement control.

[0027] In some embodiments, specific main process parameter requirements are:

[0028] (1) Secondary cooling electromagnetic stirring: Installed in the area 4000-5000 mm away from the liquid surface of the crystallizer, the magnetic field strength at the center of the stirring coil is 50×10 -4 ~100×10 -4 T;

[0029] (2) Electromagnetic stirring at the end of solidification: Installed in the area 8000-10000 mm away from the liquid surface of the crystallizer, the magnetic field strength at the center of the stirring coil is 410×10 -4 ~450×10 -4 T;

[0030] (3) The overall water volume of the secondary cooling system of continuous casting is controlled at 160-180 L / min.

[0031] In addition to the above-mentioned key process technology requirements, general technical parameters are also required for implementation, such as the continuous casting section of 280mm×380mm, the superheat of the molten steel during the casting process of 25-35°C; the overall continuous casting speed is controlled at 0.70m / min, and the resulting ingot is heat treated using conventional rolling and cooling systems.

[0032] Example 1

[0033] This embodiment is a steel mill using the method of the present invention to continuously cast and produce large square billets of U75V heavy rail steel with a cross-section of 280mm×380mm.

[0034] The specific implementation of this embodiment is as follows: (1) Secondary cooling electromagnetic stirring: Installed in the area 4000-5000 mm away from the liquid surface of the crystallizer, the magnetic field strength at the center of the stirring coil is 50×10 -4 T; (2) Electromagnetic stirring at the end of solidification: installed in the area 8000-10000 mm away from the liquid surface of the crystallizer, the magnetic field strength at the center of the stirring coil is 450×10 -4 T; (3) The water volume of the secondary cooling of continuous casting is controlled at 170L / min. In addition to the above key process and technical requirements, general technical parameters are also required for implementation, such as the continuous casting section of 280mm×380mm, the superheat of the steel liquid during the casting process is 25-35℃; the continuous casting speed is controlled at 0.70m / min, and the obtained ingot is heat treated by conventional rolling and cooling system; there is no need to assemble the crystallizer electromagnetic stirring.

[0035] Then, the cast billet is rolled and heat treated by conventional process to obtain rails, and the obtained rails are tested for hardness of the iron standard A line (A1-A4 with a distance of 5mm, 10mm, 15mm, and 20mm from the tread), and the microstructure of the 5mm×5mm area of ​​each hardness test point of the rail is further identified. After testing the hardness value of each position point, the absolute value of the hardness difference between adjacent positions and the hardness extreme difference value (maximum value max-minimum value min) of all test positions in the standard area are calculated to determine the hardness gradient of the entire region and the hardness gradient of the local area.

[0036] The results show that the maximum value of the hardness gradient of adjacent positions of the rail obtained in this embodiment is 0.24HRC / mm, which is significantly better than the 0.40HRC / mm of the rail obtained by the conventional production process; the hardness range of all test positions in the standard area of ​​the rail is 2.20HRC, which is equivalent to the rail obtained by the conventional production process. Further microstructure identification of the 5mm×5mm area of ​​each hardness test point of the rail shows that no abnormal structure appears in each area of ​​the rail.

[0037] Comparative Example

[0038] A domestic factory continuously casts large square billets of U75V, U71Mn and U78CrV heavy rail steel with a cross section of 280mm×380mm. The electromagnetic stirring coil of the crystallizer has a central magnetic field strength of 50×10 -4 ~60×10 -4 T, with the magnetic field strength of the secondary cooling electromagnetic stirring coil at the center of 200×10 -4 ~250×10 -4 The combined electromagnetic stirring of T and the implementation of strong secondary cooling to improve the macroscopic homogeneity achieved the improvement of the macroscopic homogeneity of the rail head. The extreme difference of C segregation in the rail head area was controlled at 0.03-0.06. However, due to the influence of the heat transfer characteristics of the heat treatment, the harder the rail is, the farther it is from the tread. The hardness of the rail section was tested at a spacing of 5mm. The maximum value of the hardness gradient of adjacent positions was 0.30-0.77HRC / mm, and the extreme difference of hardness of all test positions in the standard area was 4.23-7.10HRC.

[0039] Further, the process of the present invention is implemented by setting: (1) Secondary cooling electromagnetic stirring: installed in the area 4000-5000 mm away from the liquid surface of the crystallizer, the magnetic field strength at the center of the stirring coil is 50×10 -4 ~100×10 -4 T; (2) Electromagnetic stirring at the end of solidification: installed in the area 8000-10000 mm away from the liquid surface of the crystallizer, the magnetic field strength at the center of the stirring coil is 410×10 -4 ~450×10 -4T; (3) The overall water volume of the secondary cooling of continuous casting is controlled at 160-180L / min. In addition to the above-mentioned key process technical requirements, general technical parameters are also required for implementation, such as the continuous casting section of 280mm×380mm, the superheat of the molten steel during the casting process is 25-35℃; the continuous casting speed is controlled at 0.70m / min as a whole, and the resulting ingot is heat treated by conventional rolling and cooling system. The segregation degree range of the obtained rail head area C is controlled at 0.05-0.06, and the hardness of the rail section is tested at a spacing of 5mm. The maximum value of the hardness gradient of adjacent positions is 0.32-0.68HRC / mm, and the hardness range of all test positions in the standard area is 3.44-5.27HRC. The hardness gradient in the area is significantly reduced, and the hardness gradient of the rail head section is significantly improved.

[0040] Example 2

[0041] This embodiment is a steel mill using the method of the present invention to continuously cast and produce large square billets of U71Mn heavy rail steel with a cross-section of 280mm×380mm.

[0042] The specific implementation of this embodiment is as follows: (1) Secondary cooling electromagnetic stirring: Installed in the area 4000-5000 mm away from the crystallizer liquid surface, the magnetic field strength at the center of the stirring coil is 100×10 -4 T; (2) Electromagnetic stirring at the end of solidification: installed in the area 8000-10000 mm away from the liquid surface of the crystallizer, the magnetic field strength at the center of the stirring coil is 410×10 -4 T; (3) The water volume of the secondary cooling of continuous casting is controlled at 180L / min. In addition to the above key process and technical requirements, general technical parameters are also required for implementation, such as the continuous casting section of 280mm×380mm, the superheat of the steel liquid during the casting process is 25-35℃; the continuous casting speed is controlled at 0.70m / min, and the obtained ingot is heat treated by conventional rolling and cooling system.

[0043] Then, the cast billet is rolled and heat treated by conventional process to obtain rails, and the obtained rails are tested for hardness of the iron standard A line (A1-A4 with a distance of 5mm, 10mm, 15mm, and 20mm from the tread), and the microstructure of the 5mm×5mm area of ​​each hardness test point of the rail is further identified. After testing the hardness value of each position point, the absolute value of the hardness difference between adjacent positions and the hardness extreme difference value (maximum value max-minimum value min) of all test positions in the standard area are calculated to determine the hardness gradient of the entire region and the hardness gradient of the local area.

[0044] The results show that the maximum value of the hardness gradient of adjacent positions of the rail obtained in this embodiment is 0.23HRC / mm, which is significantly better than the 0.43HRC / mm of the rail obtained by the conventional production process; the hardness range of all test positions in the standard area of ​​the rail is 2.13HRC, which is equivalent to the rail obtained by the conventional production process. Further microstructure identification of the 5mm×5mm area of ​​each hardness test point of the rail shows that no abnormal structure appears in each area of ​​the rail.

[0045] Example 3

[0046] This embodiment is a steel mill using the method of the present invention to continuously cast and produce large square billets of U78CrV heavy rail steel with a cross-section of 280mm×380mm.

[0047] The specific implementation of this embodiment is as follows: (1) Secondary cooling electromagnetic stirring: Installed in the area 4000-5000 mm away from the crystallizer liquid surface, the magnetic field strength at the center of the stirring coil is 75×10 -4 T; (2) Electromagnetic stirring at the end of solidification: installed in the area 8000-10000 mm away from the liquid surface of the crystallizer, the magnetic field strength at the center of the stirring coil is 430×10 -4 T; (3) The water volume of the secondary cooling of continuous casting is controlled at 160L / min. In addition to the above key process and technical requirements, general technical parameters are also required for implementation, such as the continuous casting section of 280mm×380mm, the superheat of the steel liquid during the casting process is 25-35℃; the continuous casting speed is controlled at 0.70m / min, and the resulting ingot is heat treated by conventional rolling and cooling system.

[0048] Then, the cast billet is rolled and heat treated by conventional process to obtain rails, and the obtained rails are tested for hardness of the iron standard A line (A1-A4 with a distance of 5mm, 10mm, 15mm, and 20mm from the tread), and the microstructure of the 5mm×5mm area of ​​each hardness test point of the rail is further identified. After testing the hardness value of each position point, the absolute value of the hardness difference between adjacent positions and the hardness extreme difference value (maximum value max-minimum value min) of all test positions in the standard area are calculated to determine the hardness gradient of the entire region and the hardness gradient of the local area.

[0049] The results show that the maximum value of the hardness gradient of adjacent positions of the rail obtained in this embodiment is 0.19HRC / mm, which is significantly better than the 0.47HRC / mm of the rail obtained by the conventional production process; the hardness range of all test positions in the standard area of ​​the rail is 2.32HRC, which is equivalent to the rail obtained by the conventional production process. Further microstructure identification of the 5mm×5mm area of ​​each hardness test point of the rail shows that no abnormal structure appears in each area of ​​the rail.

[0050] The above implementation examples show that by adopting the technical solution disclosed in this aspect, the macroscopic solute concentration distribution of the ingot cross section is improved and controlled, the hardness gradient of the corresponding rail head cross section is significantly reduced after the ingot is rolled into a rail, the uniformity of the organizational performance in the local area is significantly improved, and the microstructure of the hardness detection point of the obtained rail is normal. This technology provides a new technical idea for improving and controlling the hardness gradient of the rail cross section under specific heat treatment process conditions.

[0051] It should be particularly pointed out that the various components or steps in the above-mentioned embodiments can be cross-linked, replaced, added, or deleted with each other. Therefore, the combinations formed by these reasonable arrangements and combinations should also fall within the scope of protection of the present invention, and the scope of protection of the present invention should not be limited to the embodiments.

[0052] The above are exemplary embodiments disclosed in the present invention. The order disclosed in the above embodiments of the present invention is only for description and does not represent the advantages and disadvantages of the embodiments. However, it should be noted that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope (including claims) disclosed in the embodiments of the present invention is limited to these examples. Various changes and modifications may be made without departing from the scope defined in the claims. The functions, steps and / or actions of the method claims according to the disclosed embodiments described herein do not need to be performed in any particular order. In addition, although the elements disclosed in the embodiments of the present invention may be described or required in individual form, they may also be understood as multiple unless explicitly limited to the singular.

[0053] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention (including the claims) is limited to these examples; under the concept of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the embodiments of the present invention as described above, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.

Claims

1. A method for improving the hardness gradient of a rail head section, characterized in that: By controlling the parameters of electromagnetic stirring during secondary cooling and electromagnetic stirring at the end of solidification, combined with continuous casting speed control, the hardness gradient of the rail head section can be improved. The parameter control of the secondary cooling electromagnetic stirring includes: the central magnetic field strength of the stirring coil of the secondary cooling electromagnetic stirring is 50×10 -4 ~100×10 -4 T; The parameter control of the secondary cooling electromagnetic stirring includes: the secondary cooling electromagnetic stirring is installed in an area 4000-5000mm away from the crystallizer liquid surface; The parameter control of the electromagnetic stirring at the end of coagulation includes: the central magnetic field strength of the stirring coil of the electromagnetic stirring at the end of coagulation is 410×10 -4 ~450×10 -4 T; The parameter control of the electromagnetic stirring at the end of solidification includes: the electromagnetic stirring at the end of solidification is installed in an area 8000-10000 mm away from the liquid surface of the crystallizer; The continuous casting speed is controlled at 0.7 m / min; It also includes the control of the water ratio of the secondary cooling in continuous casting; The continuous casting secondary cooling water volume is controlled at 160-180 L / min; During the casting process, the superheat of the steel liquid is 25~35℃; The cross section of the rail head is 280mm×380mm.

2. A rail head, characterized in that: The method according to claim 1 is adopted to prepare the

Citation Information

Cited By

  • Method for improving hardness of position 5-10 mm below tread of steel rail and steel rail

    CN121046713A