A post-treatment process for nylon microfiber leather dyed with sulfonate type acid dyes

By forming a cross-linked film after dyeing nylon superfiber, the color migration problem is solved, the color fixation and sun resistance of the dye are significantly improved, and higher wet fastness and sun fastness are achieved.

CN115874472BActive Publication Date: 2024-10-18JIANGSU HUAFON MICROFIBRE MATERIAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211669620.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-25
Publication Date
2024-10-18
Estimated Expiration
2042-12-25

AI Technical Summary

Technical Problem

Nylon superfiber is prone to color migration during the dyeing process, which is difficult to effectively solve with existing technology. Especially when using acidic dyes, the hydrolysis reactants of the dye and the dye that has not formed a chemical bond are difficult to tightly combine with the fiber molecular chain, resulting in color migration. serious.

Method used

The sulfonate acid dye dyeing process is used to form a cross-linked film to prevent the diffusion of the dye by rolling, pressing and baking after dyeing. The olefin-based sulfonate monomer and water-soluble cross-linking agent and initiator are used Form a macromolecular cross-linked film to enhance the binding force between dyes and fibers and reduce color migration.

Benefits of technology

The color fixation and sun resistance of nylon super fiber are significantly improved, and the color migration problem is improved. The wet fastness and sun fastness reach level 2 to 4, far exceeding the effects of traditional soaping and low-molecular anionic treatment solutions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004015791170000021
    Figure BDA0004015791170000021
  • Figure BDA0004015791170000061
    Figure BDA0004015791170000061
  • Figure BDA0004015791170000071
    Figure BDA0004015791170000071
Patent Text Reader

Abstract

The invention relates to a post-treatment process for nylon microfiber leather dyed with sulfonate acid dye, which comprises the steps of impregnating finishing liquid, rolling and pressing, and baking for finalizing in sequence; after rolling, the liquid carrying rate of the finishing liquid in the nylon microfiber leather dyed with sulfonate acid dye is not less than 30%; the finishing liquid is obtained by uniformly mixing the following raw materials in parts by mass: 100 parts of olefin sulfonate monomer; 60-100 parts of water-soluble crosslinking agent; 4-10 parts of initiator; 100-200 parts of water; after rolling, the liquid carrying rate of the finishing liquid in the nylon microfiber leather dyed with sulfonate acid dye is 30-70%, the rolling pressure is 0.1-0.3MPa; the baking temperature is 100-140°C, and the baking time is 3-10min; the ultrafine fiber in the nylon microfiber leather dyed with sulfonate acid dye is an ultrafine fiber with nylon as a fixed island or an unfixed island. The invention can significantly improve the color fixation of nylon microfiber leather dyed with sulfonate type acid dyes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nylon ultra-fine fiber dyeing and relates to a post-treatment process for nylon ultra-fine fiber leather dyed with sulfonate type acid dyes. Background Art

[0002] Fabrics with large deniers usually do not have color migration problems, but the finer the fiber, the easier it is for the dye inside the fiber to migrate to the fiber surface, resulting in poor color fastness. When ultrafine fibers are dyed, because the fineness of ultrafine fibers is extremely small, even smaller than the dye molecules, they often have color migration problems. Fabric color migration is when one color migrates to another color of fabric.

[0003] Polyester microfiber leather is usually dyed with disperse dyes, which can greatly reduce dye color migration through reduction cleaning. When nylon microfiber is dyed with disperse dyes, although it also has good dyeing properties, its wet fastness and light fastness are not ideal. Therefore, nylon microfiber is difficult to be dyed with disperse dyes and fixed by reduction cleaning. The dyes usually used are acid dyes. Acid dyes are a type of water-soluble dyes with acidic groups in the structure. During the dyeing process, the positively charged amino groups at the ends of nylon molecules under acidic conditions are combined with the sulfonic acid groups of the dyes and the intermolecular forces to form. However, for dyes that do not form chemical bonds and the hydrolysis reactants of the dyes, due to the lack of binding force with the nylon molecular chain, color migration is easily caused. Soap washing is generally performed after dark dyeing to reduce color migration, but it is not very helpful. At present, the problem of color migration of nylon microfiber dyeing is still a major technical difficulty.

[0004] Patent CN114808490A discloses a nylon acid dyeing one-bath fixing process, which uses a technical means to complete the complexation of the dye through a fixing agent, so that a compound with a larger molecular weight is formed between the dye molecules, thereby making it more difficult for the formed dye to escape from the gap. However, this technical means only slows down the time of color fastness degradation to a certain extent. In the subsequent use process, due to hydrolysis or ultraviolet light degradation, the large molecular dye molecules will still be converted into small molecular dye molecules.

[0005] Therefore, it is urgent to study a post-treatment process that can effectively reduce the color migration of dyed nylon microfiber leather. Summary of the invention

[0006] The purpose of the present invention is to solve the above problems existing in the prior art and to provide a post-treatment process for dyeing nylon microfiber leather with sulfonate type acid dyes.

[0007] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] A post-treatment process for nylon microfiber leather dyed with sulfonate type acid dye (the base fabric is the previous state of the leather, and the base fabric becomes leather after some post-treatment, and the post-treatment process of the present invention is also applicable to the base fabric), which sequentially includes the steps of impregnating with finishing liquid, rolling and pressing, and baking and shaping;

[0009] After roller pressing, the liquid carrying rate of sulfonate acid dye dyed nylon microfiber leather is not less than 30%;

[0010] The finishing liquid is obtained by uniformly mixing the following raw materials in parts by mass:

[0011]

[0012] Since the dyes that do not generate chemical bonds and the hydrolysis reactants of the dyes are all small molecules or low-molecular organic substances, the small molecule substances have excellent molecular motion ability when not subject to external forces, and are easy to diffuse to the surface and produce discoloration / fading. The degree of diffusion is related to time and temperature parameters. The higher the temperature, the faster the diffusion, and the longer the time, the greater the degree of diffusion. During dyeing, the dye enters the interior of the fiber tissue and combines with the fiber in physical and chemical or chemical ways, and then removes the floating color, and enters the color fixation link after dyeing. The present invention forms a cross-linked film on the surface of the dyed object by impregnating the dyed object. The molecular structural unit of the cross-linked film contains sulfonate, which has anionic electronegativity, and forms sulfonate anion repulsion with the acid dye containing sulfonate groups, and the small molecules containing sulfonate groups are close to the cross-linked film when diffusing to the surface. The closer they are, the stronger the anion repulsion is, so that the small molecules containing sulfonate groups are difficult to cross the cross-linked film and precipitate to the surface.

[0013] The amount of water-soluble cross-linking agent will affect the amount of sulfonate ions in the final cross-linked macromolecule. Too little cross-linking agent will result in too few cross-linking sites and insufficient cross-linking degree, which will affect the film-forming effect of the polymer and lead to unclear improvement in color migration. Too much cross-linking agent will lead to excessive cross-linking and make the leather product feel hard. Too little initiator will cause water to be dried out during the baking process and the degree of cross-linking will be low. Too high a content will lead to too fast cross-linking, violent local reactions, and ultimately uneven distribution of the molecular film.

[0014] As the preferred technical solution:

[0015] A post-treatment process for nylon microfiber leather dyed with sulfonate acid dye as described above, the liquid carrying rate of the finishing liquid in the nylon microfiber leather dyed with sulfonate acid dye after roller pressing is 30-70%, and the roller pressure is 0.1-0.3MPa. The impregnation amount of the finishing liquid only needs to achieve sufficient wetting and coating instead of overfilling, otherwise the finishing liquid will produce crosslinking during the later baking and shaping, which will cause the microfiber leather to feel stiff. In the present invention, the liquid carrying rate of the finishing liquid in the dyed nylon microfiber leather needs to be controlled to be 30-70% (the percentage of the liquid weight of the microfiber leather after immersion and rolling to the dry weight of the microfiber leather). Too small a liquid carrying rate leads to insufficient coating of the finishing liquid on the surface of the dyed nylon microfiber, and an effective crosslinked film cannot be formed in the later stage, resulting in an insignificant effect of improving the dye color migration; too large a liquid carrying rate leads to excessive filling of the crosslinked macromolecules on the fiber net, which in turn leads to hardening of the leather material feel. The roller pressure is 0.1MPa-0.3MPa. If the roller force is too small, the impregnation will not be in place. If it is too high, it will easily cause the finishing liquid to excessively fill the internal gaps, which will easily cause the microfiber leather to become stiff.

[0016] In the above-mentioned post-treatment process for dyeing nylon microfiber leather with a sulfonate-type acid dye, the baking temperature is 100-140°C, the baking time is 2-11 min, and the baking time has the following relationship with the baking temperature: baking time = (10-(baking temperature - 100°C) / 5°C) min ~ (10-(baking temperature - 100°C) / 5°C+1) min. As the baking temperature increases, the baking time should be reduced to prevent the microfiber leather from being in a high temperature environment for a long time, resulting in deterioration of mechanical properties; as the baking temperature increases, the degree of reduction in color migration first increases and then decreases, and the best effect is achieved at 120-125°C.

[0017] In the above-mentioned post-treatment process for dyeing nylon microfiber leather with sulfonate-type acid dyes, the olefin sulfonate monomer is one or more of vinyl sulfonate, methyl propylene sulfonate and 2-acrylamide-2-methylpropane sulfonate.

[0018] In the above-mentioned post-treatment process for dyeing nylon microfiber leather with sulfonate-type acid dyes, the water-soluble crosslinking agent is polyethylene glycol diacrylate with a weight average molecular weight of 600 to 1000. It is soluble in water, and both end groups are vinyl. It can participate in free radical polymerization to link two macromolecular chains, eventually forming a network cross-linked structure and a polymer film on a macro scale. Polyethylene glycol diacrylate with a weight average molecular weight of 600 to 1000 is selected. Polyethylene glycol diacrylate with a too low molecular weight has poor water solubility and is not suitable for this reaction. Polyethylene glycol diacrylate with a too high molecular weight will result in a relatively low concentration of sulfonate groups in the same reaction system, too few cross-linking sites, insufficient cross-linking degree, and affect the polymer film-forming effect.

[0019] In the above-mentioned post-treatment process for dyeing nylon microfiber leather with sulfonate-type acid dyes, the initiator is a water-soluble free radical polymerization initiator.

[0020] In the above-mentioned post-treatment process for dyeing nylon microfiber leather with sulfonate type acid dyes, the initiator is sodium sulfite or sodium persulfate.

[0021] The principle of the present invention is as follows:

[0022] Impregnation is a key step, so that the finishing liquid after impregnation can properly wet and coat the surface of the microfiber leather and control not to over-impregnate. Under the temperature and treatment time of baking and shaping, the olefin sulfonate monomer and the water-soluble cross-linking agent, under the catalysis of the initiator, open the double bond, carry out free radical reaction, and form a cross-linked film on the surface of the microfiber leather through cross-linking and curing. The coating of the microfiber leather with the cross-linked film greatly improves the color migration of nylon microfiber leather dyed with sulfonate-type acid dyes; during cross-linking, the olefin sulfonate monomer is polymerized by free radicals to form a macromolecular chain containing a large number of sulfonate groups. Due to the presence of sulfonate groups in acid dyes, the high-density sulfonate groups in such characteristic macromolecular chains show negative electronegativity and form electrostatic repulsion with the sulfonate groups of acid dyes. During the impregnation process, the finishing liquid containing olefin sulfonate monomers, cross-linking agents and initiators is coated on the outside of the microfiber leather. After baking and shaping, it is equivalent to forming a cross-linked film on the surface of the microfiber leather. The mutual repulsion of sulfonate anions formed between the dye molecules and the dye molecules can hinder the acid dye molecules from migrating outward.

[0023] In the experiment, it was found that if small or low molecular weight sulfonates or anionic treatment liquids are used to load on the fiber surface, a certain improvement in color migration can be obtained. However, the effect in long-term wet fastness and sunlight fastness is general, because under wet fastness, the polarity of water molecules has a serious impact on the coating of small or low molecular weight anionic treatment liquids on the surface of the base fabric; and the sunlight fastness is due to the distribution of the treatment liquid is uncontrollable. After long-term sunlight exposure, more small molecules will be formed. Compared with larger molecules, small molecules are more likely to escape in places where there is no anion distribution. If a sulfonate-containing polymer is dissolved in water and used as a treatment liquid to fix the color of microfiber leather, the effect is worse than that of a small or low molecular weight anionic treatment liquid, because the content of sulfonate groups in the polymer is limited, and the sulfonates within or between molecular chains interact with each other, making the entire molecular chain into a milky ball, and the coating on the fiber surface is unsatisfactory. Polymer treatment solutions containing vinyl sulfonates can improve color migration to a certain extent, but due to the smaller number of sulfonate groups, the improvement effect is not as good as that of small molecule or low molecular weight sulfonate treatment solutions.

[0024] Therefore, according to research findings, the surface of the synthetic leather is first impregnated with a treatment solution of an olefin sulfonate monomer, a water-soluble crosslinking agent, and an initiator. After coating, the olefin sulfonate monomer reacts with the crosslinking agent to form a crosslinked film, so that the sulfonate group has a uniform distribution at the molecular level and an adjustable distribution density. Uniform distribution and high distribution density are important factors to prevent small molecules from escaping. The ratio of the finishing solution, the molecular weight of the crosslinking agent, and the impregnation amount determine the distribution density of the sulfonate group. Compared with polymers, coating first and then crosslinking can greatly improve the distribution density of the sulfonate group while achieving effective coating.

[0025] Beneficial effects:

[0026] (1) Compared with traditional soap washing, the technical solution of the present invention can significantly improve the color fixation of nylon microfiber leather dyed with sulfonate type acid dyes.

[0027] (2) Compared with the use of a fixing agent that can complex dyes or a low-molecular anion treatment solution, the technical solution of the present invention is beneficial in terms of long-term wet fastness and light fastness.

[0028] (3) Compared with traditional soap washing, the color migration after treatment of the present invention can be improved by 1 to 2 levels, and the wet fastness reaches 2 to 3 levels; the light fastness after treatment of the present invention is 3 to 4 levels. DETAILED DESCRIPTION

[0029] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0030] The substances used in the present invention are as follows:

[0031] (1) Sodium vinyl sulfonate: purchased from Jinan Huijinchuan Chemical;

[0032] (2) Sodium methyl methacrylate sulfonate: purchased from Shandong Denno New Materials;

[0033] (3) 2-Acrylamide-2-methylpropanesulfonic acid: purchased from Dezhou Guorui Chemical Technology;

[0034] (4) Polyethylene glycol diacrylate (weight average molecular weight 600): purchased from Weikang Technology;

[0035] (5) Polyethylene glycol diacrylate (weight average molecular weight 1000): purchased from Weikang Technology;

[0036] (6) Polyethylene glycol diacrylate (weight average molecular weight 1200): purchased from Weikang Technology;

[0037] (7) Sodium polystyrene sulfonate (weight average molecular weight 70,000): purchased from Jinan Quanxing New Materials.

[0038] The sulfonate acid dye dyed nylon microfiber leather used in the following examples is prepared by the following method. Specifically, the EDGW0-100A12 brand microfiber base fabric of Shanghai Huafeng Microfiber Technology Co., Ltd. is used to dye it. The dyes are TX navy blue (dosage 1.8% owf) purchased from Hangzhou Tasi Chemical Co., Ltd. and black D-PA (0.5% owf) from Qingdao Yuzhen Trading Co., Ltd. Two sulfonate acid dyes. The dyeing process is to heat to 70°C at a rate of 5°C / min and keep warm for 10min, then heat to 98°C at a rate of 2°C / min and keep warm for 60min, then cool down and wash with water, soap and water, and the dyeing bath ratio is 1:15. The fineness of the nylon microfiber in the microfiber base fabric is 0.08dtex.

[0039] The testing method adopted by the present invention is as follows:

[0040] (1) Color migration: ISO 15701 test is used, specifically: the test sample is laminated with PVC, placed in a constant temperature oven at 50°C under a pressure of 50N, and kept at the constant temperature for 16 hours; the PVC is rated against a gray card and divided into 5 levels; the present invention can improve the color migration rating by 1 to 2 levels according to the amount of dye used;

[0041] (2) Wet fastness: ISO 105-X12 test is used, specifically, a wet pure cotton standard friction cloth (water evenly distributed, moisture content of 95-100%) is used to wrap the end of a round friction finger (diameter 16±0.1mm), the vertical pressure is 9±0.2N, and the linear reciprocation is 10 times, and the reciprocating stroke is 104±3mm. It is naturally air-dried at room temperature and rated against the gray card, which is divided into 5 levels;

[0042] (3) Light fastness: Tested using HG / T 3689-2013 (Method A), specifically:

[0043] ① Choose a spiral lamp socket solar bulb with a power of 300W and a voltage of 220V±10V. The wavelength of the ultraviolet light of the solar bulb is 280nm~400nm, and there is some visible light. The intensity of the ultraviolet light of the solar bulb is 25W / m 2 ±0.4W / m 2 ;

[0044] ②The temperature in the test chamber is specified to be 50℃±2℃;

[0045] ③ Cut two pieces of test specimens with a size of not less than 30mm×10mm, one piece is sent into the test box for yellowing resistance test, and the other piece is placed outside the box for test result evaluation;

[0046] ④ Place the sample on the tray (the area between two concentric circles with diameters of 75mm and 300mm), with the surface parallel to the bottom surface of the bulb, the distance is 250mm±2mm, and the irradiated surface faces the light source;

[0047] ⑤The tray rotates at a speed of 3r / min±1r / min, and the sample is exposed to light continuously for 24 hours;

[0048] ⑥ Under the standard light source, use the gray sample card to directly visually evaluate the yellowing degree corresponding to the test sample and the untested sample, which is divided into 5 levels.

[0049] Example 1

[0050] A post-treatment process for dyeing nylon microfiber leather with sulfonate type acid dyes, the specific steps are as follows:

[0051] (1) preparing a finishing solution;

[0052] The following raw materials in parts by weight are mixed evenly to obtain a finishing liquid:

[0053]

[0054] (2) Impregnated with finishing fluid;

[0055] The sulfonate type acid dye dyed nylon microfiber leather is impregnated with the finishing liquid until the dyed nylon microfiber suede leather is completely soaked, and then the finishing liquid is pressed by a roller to control the liquid carrying rate of the sulfonate type acid dye dyed nylon microfiber leather to be 70%, wherein the roller pressure is 0.1MPa;

[0056] (3) Baking and shaping;

[0057] After being rolled and pressed, the product is baked and shaped in a tentering heat setting machine, wherein the baking temperature is 120°C and the baking time is 6 minutes.

[0058] The color migration rating of the post-treated sulfonate acid dyed nylon microfiber leather is 4.5, its wet fastness is 2.5, and its light fastness is 3.5.

[0059] Example 2

[0060] A post-treatment process for dyeing nylon microfiber leather with sulfonate type acid dyes, the specific steps are as follows:

[0061] (1) preparing a finishing solution;

[0062] The following raw materials in parts by weight are mixed evenly to obtain a finishing liquid:

[0063]

[0064] (2) Impregnated with finishing fluid;

[0065] The sulfonate type acid dye dyed nylon microfiber leather is impregnated with the finishing liquid until the dyed nylon microfiber suede leather is completely soaked, and then the finishing liquid is pressed by a roller to control the liquid carrying rate of the sulfonate type acid dye dyed nylon microfiber leather to be 70%, wherein the roller pressure is 0.1MPa;

[0066] (3) Baking and shaping;

[0067] After being pressed by rollers, the product is baked and shaped in a tentering heat setting machine, wherein the baking temperature is 140°C and the baking time is 2 minutes.

[0068] The color migration rating of the post-treated sulfonate acid dyed nylon microfiber leather is 3.5, its wet fastness is 2, and its light fastness is 3.

[0069] Example 3

[0070] A post-treatment process for dyeing nylon microfiber leather with sulfonate type acid dyes, the specific steps are as follows:

[0071] (1) preparing a finishing solution;

[0072] The following raw materials in parts by weight are mixed evenly to obtain a finishing liquid:

[0073]

[0074] (2) Impregnated with finishing fluid;

[0075] The sulfonate type acid dye dyed nylon microfiber leather is impregnated with the finishing liquid until the dyed nylon microfiber suede leather is completely soaked, and then the finishing liquid is pressed by a roller to control the liquid carrying rate of the sulfonate type acid dye dyed nylon microfiber leather to be 70%, wherein the roller pressure is 0.1MPa;

[0076] (3) Baking and shaping;

[0077] After being rolled and pressed, the product is baked and shaped in a tentering heat setting machine, wherein the baking temperature is 125°C and the baking time is 5 minutes.

[0078] The color migration rating of the post-treated sulfonate acid dyed nylon microfiber leather is 4.5, its wet fastness is 2.5, and its light fastness is 3.5.

[0079] Example 4

[0080] A post-treatment process for dyeing nylon microfiber leather with sulfonate type acid dyes, the specific steps are as follows:

[0081] (1) preparing a finishing solution;

[0082] The following raw materials in parts by weight are mixed evenly to obtain a finishing liquid:

[0083]

[0084] (2) Impregnated with finishing fluid;

[0085] The sulfonate type acid dye dyed nylon microfiber leather is impregnated with the finishing liquid until the dyed nylon microfiber suede leather is completely soaked, and then the finishing liquid is pressed by a roller to control the liquid carrying rate of the sulfonate type acid dye dyed nylon microfiber leather to be 30%, wherein the roller pressure is 0.3MPa;

[0086] (3) Baking and shaping;

[0087] After being rolled and pressed, the film is baked and shaped in a tentering heat setting machine, wherein the baking temperature is 100°C and the baking time is 11 minutes.

[0088] The color migration rating of the post-treated sulfonate acid dyed nylon microfiber leather is 3.5, its wet fastness is 2, and its light fastness is 3.

[0089] Example 5

[0090] A post-treatment process for dyeing nylon microfiber leather with sulfonate type acid dyes, the specific steps are as follows:

[0091] (1) preparing a finishing solution;

[0092] The following raw materials in parts by weight are mixed evenly to obtain a finishing liquid:

[0093]

[0094] (2) Impregnated with finishing fluid;

[0095] The sulfonate type acid dye dyed nylon microfiber leather is impregnated with the finishing liquid until the dyed nylon microfiber suede leather is completely soaked, and then the finishing liquid is pressed by a roller to control the liquid carrying rate of the sulfonate type acid dye dyed nylon microfiber leather to be 70%, wherein the roller pressure is 0.1MPa;

[0096] (3) Baking and shaping;

[0097] After being rolled and pressed, the film is baked and shaped in a tentering heat setting machine, wherein the baking temperature is 110° C. and the baking time is 8.5 min.

[0098] The color migration rating of the post-treated sulfonate acid dyed nylon microfiber leather is 4, its wet fastness is 2.5, and its light fastness is 3.5.

[0099] Example 6

[0100] A post-treatment process for dyeing nylon microfiber leather with sulfonate type acid dyes, the specific steps are as follows:

[0101] (1) preparing a finishing solution;

[0102] The following raw materials in parts by weight are mixed evenly to obtain a finishing liquid:

[0103]

[0104] (2) Impregnated with finishing fluid;

[0105] The sulfonate type acid dye dyed nylon microfiber leather is impregnated with the finishing liquid until the dyed nylon microfiber suede leather is completely soaked, and then the finishing liquid is pressed by a roller to control the liquid carrying rate of the sulfonate type acid dye dyed nylon microfiber leather to be 50%, wherein the roller pressure is 0.2MPa;

[0106] (3) Baking and shaping;

[0107] After being rolled and pressed, the product is baked and shaped in a tentering heat setting machine, wherein the baking temperature is 130°C and the baking time is 4 minutes.

[0108] The color migration rating of the post-treated sulfonate acid dyed nylon microfiber leather is 4, its wet fastness is 2.5, and its light fastness is 3.5.

[0109] Example 7

[0110] A post-treatment process for dyeing nylon microfiber leather with sulfonate type acid dyes, the specific steps are as follows:

[0111] (1) preparing a finishing solution;

[0112] The following raw materials in parts by weight are mixed evenly to obtain a finishing liquid:

[0113]

[0114] (2) Impregnated with finishing fluid;

[0115] The sulfonate type acid dye dyed nylon microfiber leather is impregnated with the finishing liquid until the dyed nylon microfiber suede leather is completely soaked, and then the finishing liquid is pressed by a roller to control the liquid carrying rate of the sulfonate type acid dye dyed nylon microfiber leather to be 30%, wherein the roller pressure is 0.3MPa;

[0116] (3) Baking and shaping;

[0117] After being rolled and pressed, the film is baked and shaped in a tentering heat setting machine, wherein the baking temperature is 135° C. and the baking time is 3.5 min.

[0118] The color migration rating of the post-treated sulfonate acid dyed nylon microfiber leather is 3.5, its wet fastness is 2, and its light fastness is 3.

[0119] Comparative Example 1

[0120] A post-treatment process for dyeing nylon microfiber leather with sulfonate type acid dyes, the specific steps are as follows:

[0121] (1) preparing a finishing solution;

[0122] The following raw materials in parts by weight are mixed evenly to obtain a finishing liquid:

[0123] 100 parts of sodium vinyl sulfonate;

[0124] 150 parts water;

[0125] (2) Impregnated with finishing fluid;

[0126] The sulfonate type acid dye dyed nylon microfiber leather is impregnated with the finishing liquid until the dyed nylon microfiber suede leather is completely soaked, and then the finishing liquid is pressed by a roller to control the liquid carrying rate of the sulfonate type acid dye dyed nylon microfiber leather to be 70%, wherein the roller pressure is 0.1MPa;

[0127] (3) Baking and shaping;

[0128] After being rolled and pressed, the product is baked and shaped in a tentering heat setting machine, wherein the baking temperature is 120°C and the baking time is 6 minutes.

[0129] The color migration rating of the post-treated sulfonate acid dyed nylon microfiber leather is 4, its wet fastness is 1.5, and its light fastness is 2.5.

[0130] Comparing Comparative Example 1 with Example 1, it can be found that the wet fastness and light fastness of Comparative Example 1 are significantly lower than those of Example 1. This is because Comparative Example 1 is treated with small molecule sulfonate, without adding crosslinking agent and initiator, and there is no reaction in the baking process, only the water is dried, which is equivalent to dispersing the small molecule sulfonate on the surface of the material. Although the treated products can also obtain good color migration ratings, the effects shown in long-term wet fastness and light fastness are average, because the polarity of water molecules in wet fastness has a serious impact on the coating of small molecule or low molecular weight anion treatment liquid on the surface of the base fabric; and the light fastness is due to the fact that the distribution of the treatment liquid is uncontrollable, and there are inevitably dense and loose distribution areas. After long-term sunlight exposure, more small molecule dyes with extremely small sizes will be formed, and they are easy to come out in places where no anions are distributed.

[0131] Comparative Example 2

[0132] A post-treatment process for dyeing nylon microfiber leather with sulfonate type acid dyes, the specific steps are as follows:

[0133] (1) preparing a finishing solution;

[0134] The following raw materials in parts by weight are mixed evenly to obtain a finishing liquid:

[0135] 200 parts of sodium polyvinyl sulfonate;

[0136] 150 parts water;

[0137] (2) Impregnated with finishing fluid;

[0138] The sulfonate type acid dye dyed nylon microfiber leather is impregnated with the finishing liquid until the dyed nylon microfiber suede leather is completely soaked, and then the finishing liquid is pressed by a roller to control the liquid carrying rate of the sulfonate type acid dye dyed nylon microfiber leather to be 70%, wherein the roller pressure is 0.1MPa;

[0139] (3) Baking and shaping;

[0140] After being rolled and pressed, the product is baked and shaped in a tentering heat setting machine, wherein the baking temperature is 120°C and the baking time is 6 minutes.

[0141] The color migration rating of the post-treated sulfonate acid dyed nylon microfiber leather is 2.5, its wet fastness is 1.5, and its light fastness is 2.5.

[0142] By comparing Comparative Example 2 with Example 1, it can be found that the color migration rating, wet fastness and light fastness of Comparative Example 2 are significantly lower than those of Example 1. This is because Comparative Example 2 is directly treated with an aqueous solution of the sulfonate polymer, and there is no reaction during the baking process, which only dries the water, which is equivalent to dispersing the sulfonate polymer on the surface of the material. Compared with small molecular sulfonate compounds, the content of sulfonate groups in the polymer containing sulfonate is relatively greatly reduced, so the color migration rating, wet fastness and light fastness are significantly reduced.

[0143] Comparative Example 3

[0144] A post-treatment process for dyeing nylon microfiber leather with sulfonate type acid dyes, the specific steps are as follows:

[0145] (1) preparing a finishing solution;

[0146] The following raw materials in parts by weight are mixed evenly to obtain a finishing liquid:

[0147]

[0148] (2) Impregnated with finishing fluid;

[0149] The sulfonate type acid dye dyed nylon microfiber leather is impregnated with the finishing liquid until the dyed nylon microfiber suede leather is completely soaked, and then the finishing liquid is pressed by a roller to control the liquid carrying rate of the sulfonate type acid dye dyed nylon microfiber leather to be 70%, wherein the roller pressure is 0.1MPa;

[0150] (3) Baking and shaping;

[0151] After being rolled and pressed, the product is baked and shaped in a tentering heat setting machine, wherein the baking temperature is 120°C and the baking time is 6 minutes.

[0152] The color migration rating of the post-treated sulfonate acid dyed nylon microfiber leather is 3, its wet fastness is 2, and its light fastness is 3.

[0153] Comparing Comparative Example 3 with Example 1, it can be seen that the amount of cross-linking agent polyethylene glycol diacrylate used in Comparative Example 3 is relatively small, and the final color migration rating of Comparative Example 3 is significantly lower than that of Example 1. This is because Comparative Example 3 contains too little cross-linking agent, too few cross-linking sites, and insufficient cross-linking degree, which affects the film-forming effect of the polymer and results in an insignificant improvement in color migration.

[0154] Comparative Example 4

[0155] A post-treatment process for dyeing nylon microfiber leather with sulfonate type acid dyes, the specific steps are as follows:

[0156] (1) preparing a finishing solution;

[0157] The following raw materials in parts by weight are mixed evenly to obtain a finishing liquid:

[0158]

[0159] (2) Impregnated with finishing fluid;

[0160] The sulfonate type acid dye dyed nylon microfiber leather is impregnated with the finishing liquid until the dyed nylon microfiber suede leather is completely soaked, and then the finishing liquid is pressed by a roller to control the liquid carrying rate of the sulfonate type acid dye dyed nylon microfiber leather to be 70%, wherein the roller pressure is 0.1MPa;

[0161] (3) Baking and shaping;

[0162] After being rolled and pressed, the product is baked and shaped in a tentering heat setting machine, wherein the baking temperature is 120°C and the baking time is 6 minutes.

[0163] The color migration rating of the post-treated sulfonate acid dyed nylon microfiber leather is 3, its wet fastness is 2, and its light fastness is 3.

[0164] Comparing Comparative Example 4 with Example 1, it can be seen that the molecular weight of the polyethylene glycol diacrylate used in Comparative Example 4 is relatively high, and the color migration rating of Comparative Example 4 is significantly lower than that of Example 1. This is because the excessively high molecular weight of the polyethylene glycol diacrylate in Comparative Example 4 will result in the same number of reaction systems, where the relative concentration of sulfonate groups is too low, the number of cross-linking sites is too small, and the degree of cross-linking is insufficient, which affects the film-forming effect of the polymer and results in an insignificant improvement in color migration.

[0165] Comparative Example 5

[0166] A post-treatment process for dyeing nylon microfiber leather with sulfonate type acid dyes, the specific steps are as follows:

[0167] (1) preparing a finishing solution;

[0168] The following raw materials in parts by weight are mixed evenly to obtain a finishing liquid:

[0169]

[0170] (2) Impregnated with finishing fluid;

[0171] The sulfonate type acid dye dyed nylon microfiber leather is impregnated with the finishing liquid until the dyed nylon microfiber suede leather is completely soaked, and then the finishing liquid is pressed by a roller to control the liquid carrying rate of the sulfonate type acid dye dyed nylon microfiber leather to be 25%, wherein the roller pressure is 0.4MPa;

[0172] (3) Baking and shaping;

[0173] After being rolled and pressed, it was baked and set in a tentering heat setting machine, wherein the baking temperature was 120°C and the baking time was 6 minutes. The color migration rating of the post-treated sulfonate acid dyed nylon microfiber leather was 3, its wet fastness was 2, and its light fastness was 3.

[0174] Comparing Comparative Example 5 with Example 1, it can be seen that the color migration rating of Comparative Example 5 is significantly lower than that of Example 1. This is because the excessively small liquid carrying rate in Comparative Example 5 results in insufficient coating of the surface of the dyed nylon microfiber by the finishing liquid, and an effective cross-linked film cannot be formed in the later stage, resulting in an insignificant effect in improving the color migration of the dye.

Claims

1. A post-treatment process for dyeing nylon microfiber leather with sulfonate type acid dyes, characterized in that The process includes the steps of impregnation with finishing liquid, roller pressing and baking for shaping; The liquid carrying rate of sulfonate acid dye-dyed nylon microfiber leather after roller pressing is not less than 30%; The finishing liquid is obtained by uniformly mixing the following raw materials in parts by mass: 100 parts of olefin sulfonate monomer; 60-100 parts of water-soluble cross-linking agent; 4-10 parts of initiator; 100~200 parts of water; The olefin sulfonate monomer is one of vinyl sulfonate, methyl propylene sulfonate and 2-acrylamide-2-methyl propane sulfonate; The water-soluble crosslinking agent is polyethylene glycol diacrylate with a weight average molecular weight of 600-1000.

2. The post-treatment process for dyeing nylon microfiber leather with sulfonate type acid dyes according to claim 1, characterized in that: After roller pressing, the liquid carrying rate of sulfonate type acid dye dyed nylon microfiber leather is 30~70%, and the roller pressure is 0.1~0.3MPa.

3. The post-treatment process for dyeing nylon microfiber leather with sulfonate type acid dyes according to claim 1, characterized in that: The baking temperature is 100~140℃, and the baking time is 2~11min.

4. The post-treatment process for dyeing nylon microfiber leather with sulfonate type acid dyes according to claim 1, characterized in that: The initiator is a water-soluble free radical polymerization initiator.

5. A post-treatment process for dyeing nylon microfiber leather with sulfonate type acid dyes according to claim 4, characterized in that: The initiator is sodium sulfite or sodium persulfate.

Citation Information

Patent Citations

  • Nylon acid dyeing one-bath color fixing process

    CN114808490A

  • Method for dyeing polyester-type superfine fiber synthetic leather

    CN108360187A

  • Rapid dyeing method for superfine fiber suede leather

    CN109594362A

  • Manufacturing method of high-color-fastness superfine fiber synthetic leather

    CN113802386A

  • Method of dyeing nylon fiber with acid dye: sulfamic acid

    US5364417A