A preparation process for mobile backfill material based on shield waste slurry
By combining multi-stage separation and flocculation conditioning with vacuum preloading and novel water-reducing and coagulant accelerator processes, the problems of resource utilization of tunnel boring machine waste mud and preparation of backfill materials have been solved. High-fluidity and high-strength flowable backfill material has been prepared, which is suitable for backfilling projects of pipe trenches and retaining walls.
Patent Information
- Application Number
- CN202211531512.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-01
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-12-01
AI Technical Summary
The disposal of waste slurry from tunnel boring machines is difficult to utilize as a resource, leading to land occupation and resource waste. Furthermore, existing methods for preparing backfill materials cannot guarantee strength and fluidity.
A combined process of multi-stage separation, flocculation conditioning-vacuum pre-compression, and novel water-reducing agent and coagulant accelerator is used to prepare flowable backfill material. This process includes drum screening, hydrocyclone separation, flocculant treatment, and vacuum pre-compression dewatering, combined with the mixing and stirring of cement, fly ash, water-reducing agent, and coagulant accelerator.
The project has achieved the resource utilization of waste slurry from tunnel boring machines. The prepared fluid backfill material has high fluidity and compressive strength, and is suitable for backfilling projects of pipe trenches and retaining walls, thus solving the problems of waste slurry treatment and backfill material preparation.
Smart Images

Figure CN116023080B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waste mud resource utilization and backfill material preparation, and more specifically, to a process for preparing flow backfill material based on shield waste mud. Background Art
[0002] With the rapid development of my country's economy, the scale of tunnel construction has continued to increase, and the output of waste mud from shield tunneling has increased year by year. In the construction of slurry shield tunneling, mud is an indispensable material to ensure the normal operation of the shield tunneling. It can balance the formation pressure, protect the shaft wall, clean the shaft bottom, and transmit power. At present, during the construction process, the mud participates in the cutting of soil and bedrock in the formation, mixed with rock debris and soil, forming a complex mixed system, and inevitably produces waste mud that cannot be reused. At present, shield tunneling mud usually uses bentonite mud, which mainly includes water, bentonite particles, clay particles, and admixtures such as polyacrylamide and carboxymethyl cellulose. The waste mud has the following characteristics: (1) The addition of admixtures leads to a higher pH value of the mud, which is generally alkaline; (2) The water content is high, generally 60%-90%, the viscosity is large, and it is difficult to settle naturally; (3) Fine particles such as clay minerals account for a large proportion, and also contain a certain proportion of coarse particles of gravel. At present, the main treatment method for shield waste mud is solid-liquid separation, which is to add flocculants to destabilize and settle the colloidal suspension, and then use mechanical filter presses to separate the solid and liquid, and finally transport the resulting mud cake to a landfill for disposal. This method results in the mud cake itself being used as a soil resource but not being effectively utilized, and transporting it to the landfill takes up more land, resulting in a waste of resources.
[0003] Flowing backfill is a new type of backfill material that is fluid and can be poured. It forms a suitable strength by adding solidifying materials. It is generally composed of cement, fly ash, coarse aggregate, fine aggregate, and water. It has the characteristics of self-leveling and self-compacting. It is mainly used for projects such as trench backfill and abutment backfill. The shield waste mud contains rich aggregates. The mud is prepared into flowing backfill for backfill projects through a series of treatments. It is a solution to solve the three problems of waste mud treatment and disposal, backfill material purchase and backfill construction at the same time. Summary of the invention
[0004] An object of the present invention is to provide a process for preparing mobile backfill material based on waste shield slurry, so as to realize resource utilization of waste shield slurry and solve the problem of preparing backfill material in engineering construction.
[0005] In order to achieve these purposes and other advantages according to the present invention, a process for preparing mobile backfill material based on waste slurry of shield tunneling is provided, which comprises the following three steps, specifically:
[0006] Step 1: Multi-stage separation of waste mud, screening the aggregate in the waste mud to obtain coarse aggregate, fine aggregate and mixed uniform mud;
[0007] Step 2: Mud flocculation and dehydration, using flocculation conditioning and vacuum preloading to treat the uniform mud after multi-stage separation to form a dehydrated mud cake, and the discharged water forms mud tail water;
[0008] Step 3: Preparation of mobile backfill material: the coarse aggregate and fine aggregate in step 1 are mixed with the dehydrated cement cake in step 2 to form an aggregate mixture; the mud tail water produced in step 2 is then mixed with cement, fly ash, water reducing agent and coagulant to form a gel mixture; the aggregate mixture and the gel mixture are stirred to prepare mobile backfill material.
[0009] Preferably, the step 1 specifically comprises the following steps:
[0010] Step 1.1: The waste slurry from the shield tunnel in the slurry tank is transported to the drum screen through a slurry pump. The aperture of the drum screen is 5 mm. After the waste slurry is screened, coarse aggregate with a particle size of more than 5 mm is obtained;
[0011] Step 1.2: The waste mud remaining after screening is transported to the hydrocyclone, and the aggregates of 0.5-5 mm are separated by the hydrocyclone. The inner hydrocyclone mud with particle size below 0.5 mm is discharged from the upper part of the hydrocyclone, and the outer hydrocyclone mud with particle size within the range of 0.5-5 mm is discharged from the lower part of the hydrocyclone and enters the dewatering screen;
[0012] Step 1.3: The aperture of the dewatering screen is 0.5 mm. The dewatering screen can dewater and screen the aggregate in the external cyclonic mud to obtain fine aggregate with a particle size ranging from 0.5 to 5 mm;
[0013] Step 1.4: The mud screened by the dewatering screen is mixed with the internal cyclone mud to form a uniform mud with uniform components.
[0014] Preferably, the step 2 specifically comprises the following steps:
[0015] Step 2.1: The uniform slurry in the above step 1 is transported to a flocculation conditioning tank, and a flocculant is added thereto to make the suspended particles in the uniform slurry condense and settle. The flocculant used is anionic polyacrylamide, and the flocculant is added to make its mass concentration 0.02-0.03%. After adding the flocculant, the agitator in the flocculation conditioning tank is turned on for stirring and mixing. During the mixing stage, the agitator is stirred at a speed of 600-700 r / min for 2-3 minutes to make the flocculant and the solution evenly mixed. The flocculation and sedimentation time is 10-15 minutes;
[0016] Step 2.2: The flocculated and conditioned mud is transported to the vacuum preloading device through a mud pump for vacuum preloading to form a dehydrated water cake. The water discharged by the vacuum preloading is the mud tail water.
[0017] Preferably, the vacuum preloading device includes: a box body, a vacuum membrane is arranged on the top of which, the vacuum membrane isolates the interior of the box body as a closed space, and a mud input port is arranged at the lower part of the box body; a drain board, several of which are arranged in the closed space of the box body, the outer side of the drain board is wrapped by geotextile, and several water-permeable holes are arranged on the drain board; a drain pipe, which is correspondingly connected to the several water-permeable holes on the several drain boards, and the drain pipe is connected to the vacuum pump outside the box body.
[0018] Preferably, the step 3 specifically comprises the following steps:
[0019] Step 3.1: The coarse aggregate and fine aggregate produced in the above step 1 are mixed evenly with the dewatered cement cake formed in step 2, wherein the mixing mass ratio of the dewatered cement cake, the fine aggregate and the coarse aggregate is 1:1.7-2.8:2.5-4.5, and the three materials are mixed in proportion to form an aggregate mixture;
[0020] Step 3.2: the mud tail water produced in the above step 2 is mixed with cement, fly ash, water reducing agent and coagulant, the mixing mass ratio of cement, fly ash, water reducing agent, coagulant and mud tail water is 1:0.9-1.2:0.04-0.06:0.02-0.03:0.6-2.0, and the four materials and mud tail water are stirred into a gel mixture;
[0021] Step 3.3: Put the aggregate mixture formed in the above step 3.1 and the gel mixture formed in step 3.2 into a mortar mixer at a mass ratio of 1.5 to 1.9:1, and stir for 4 to 6 minutes to prepare a flowable backfill material.
[0022] Preferably, the water reducer in step 3.2 is composed of one or both of a phosphate-based water reducer and a polycarboxylate water reducer, and the coagulant is composed of one or both of sodium silicate and calcium formate.
[0023] The present invention has at least the following beneficial effects:
[0024] In view of the problem that construction waste mud has complex components and is difficult to dispose and utilize, this application has developed a preparation process for mobile backfill material based on shield waste mud. The preparation process of this application has the following outstanding advantages:
[0025] (1) In terms of the recycling of waste mud from shield tunneling, compared with the traditional method of using mud as building materials, roadbed materials and agricultural soil, this application proposes a new method for recycling waste mud, which makes full use of aggregates of different sizes and tail water in the mud to achieve green disposal of waste;
[0026] (2) In terms of multi-stage separation of waste mud, coarse aggregate and fine aggregate are separated step by step by using a drum screen, a cyclone and a dewatering screen, and added in proportion when preparing the flowing backfill material. Compared with direct mixing of mud and curing agent, this method can better ensure the strength and fluidity of the backfill material;
[0027] (3) In terms of mud flocculation and dehydration, the flocculation conditioning-vacuum preloading method is used to treat the mud. The flocculation conditioning agent uses anionic polyacrylamide, which has a better mud flocculation effect. The vacuum preloading method commonly used in soft foundation reinforcement projects is applied to mud dehydration. The mud cake after dehydration will not be hardened, which is more conducive to subsequent stirring. The energy consumption of the vacuum preloading method is lower than that of the conventional plate and frame filter press.
[0028] (4) In the preparation of flowing backfill material, a new type of water reducer and coagulant is used, and the materials are mixed according to the optimal ratio. The prepared flowing backfill material has higher fluidity and compressive strength, and has better performance advantages than the backfill materials of general trench and retaining wall backfill projects.
[0029] The preparation process of flowing backfill material based on shield waste mud realizes the full utilization of particles of different sizes and tail water in the waste mud. The prepared flowing backfill material has a 28d unconfined compressive strength of more than 350kPa and a flow value of more than 200mm, and can be used in trench and retaining wall backfill projects.
[0030] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a process flow chart of preparing mobile backfill material based on waste slurry from shield tunneling according to the present invention;
[0032] Figure 2 It is a schematic diagram of the structure of the vacuum preloading device of the present invention.
[0033] Explanation of the reference numerals: 1-box, 2-vacuum membrane, 3-mud input port, 4-drainage board, 5-geotextile, 6-drainage pipe, 7-vacuum pump. DETAILED DESCRIPTION
[0034] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.
[0035] It should be noted that the experimental methods described in the following embodiments are conventional methods unless otherwise specified, and the reagents and materials are commercially available unless otherwise specified; in the description of the present invention, the terms "lateral", "longitudinal", "upper", "lower", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0036] like Figure 1 As shown, the present invention provides a process for preparing mobile backfill material based on waste slurry from shield tunneling, which mainly includes the following steps: (1) multi-stage separation of waste slurry; (2) flocculation and dehydration of slurry; (3) preparation of mobile backfill material. The specific operation steps of each process are as follows.
[0037] Step 1: Multi-stage separation of waste mud
[0038] The composition of shield waste mud is relatively complex, containing crushed stone, coarse sand, fine sand and clay particles. The waste mud is treated by multi-stage separation to obtain materials of different components and realize the screening of aggregates in the waste mud. To achieve the above purpose, the equipment used in this step includes a drum screening machine, a cyclone and a dewatering screen. The shield waste mud in the mud tank is transported to the drum screening machine through a mud pump. The aperture of the drum screening machine is 5mm. After the mud is screened, coarse aggregates with a particle size of more than 5mm are obtained. The screened mud is transported to the cyclone, which can separate aggregates of 0.5 to 5mm. The inner cyclone mud with a particle size of less than 0.5mm is discharged from the upper part of the cyclone, and the outer cyclone mud with a particle size of 0.5 to 5mm is discharged from the lower part of the cyclone and enters the dewatering screen. The aperture of the dewatering screen is 0.5mm. The dewatering screen can dewater and screen the aggregate in the external cyclone mud to obtain fine aggregate with a particle size range of 0.5-5mm. The mud screened by the dewatering screen is mixed with the internal cyclone mud to become a mud with uniform components. The waste mud is separated in multiple stages to obtain coarse aggregate, fine aggregate and uniform mud. After the aggregate is separated, the preparation of the mobile backfill material according to a certain ratio can ensure that it has good strength and fluidity.
[0039] Step 2: Mud flocculation and dehydration
[0040] The flocculation conditioning-vacuum preloading method is used to treat the mud after multi-stage separation. After the mud is transported to the flocculation conditioning tank, flocculants are added to it to make the suspended particles in the mud coagulate and settle. The flocculant used is anionic polyacrylamide. The flocculant is added to make its mass concentration 0.02-0.03%. After adding the flocculant, turn on the agitator in the conditioning tank. During the mixing stage, stir at a speed of 600-700r / min for 2-3 minutes to allow the flocculant to mix quickly and evenly with the solution. The flocculation and sedimentation time is 10-15 minutes. Stop stirring during the flocculation stage to prevent the agitator from breaking the flocs. The flocculated and conditioned mud is transported to the vacuum preloading device through a mud pump, such as Figure 2 As shown, the vacuum preloading device is composed of a box 1, a vacuum membrane 2, a vacuum pump 7, a drain board 4, a drain pipe 6, a geotextile 5, and a mud input port 3. The box 1 and the vacuum membrane 2 form a closed space for storing mud. The surface of the drain board 4 has water-permeable holes. The geotextile 5 is wrapped on the outside of the drain board 4 to isolate the mud particles. The drain board 4 is connected to the drain pipe 6 to extract the water in the mud. When the vacuum pump 7 is turned on, the air pressure in the closed space formed by the box 1 and the vacuum membrane 2 gradually decreases. Under the action of atmospheric pressure, the water in the mud passes through the geotextile 5 and enters the drain board 4. The water in the drain board 4 flows out to the tailwater pool through the drain pipe 6. Compared with the traditional plate and frame filter press dehydration, the mud cake will not be hardened after dehydration by vacuum preloading, which is more conducive to the mixing of subsequent materials, and the energy consumption is lower than that of filter press dehydration.
[0041] Step 3: Mobile backfill preparation
[0042] The coarse aggregate and fine aggregate produced in step 1 are mixed evenly with the dewatered cement cake in step 2, and the mixing mass ratio of the dewatered cement cake, fine aggregate and coarse aggregate is 1:1.7-2.8:2.5-4.5. The three materials are mixed in proportion to form an aggregate mixture. The mud tail water produced in step 2 is mixed with cement, fly ash, water reducer and coagulant. The water reducer is mainly composed of one or two of phosphate-based water reducer and polycarboxylic acid water reducer. The coagulant is mainly composed of one or two of sodium silicate and calcium formate. The mixing mass ratio of cement, fly ash, water reducer, coagulant and mud tail water is 1:0.9-1.2:0.04-0.06:0.02-0.03:0.6-2.0. The four materials are mixed with the tail water to form a gel mixture. Then, the aggregate mixture and the gel mixture are put into a mortar mixer and stirred at a mass ratio of 1.5-1.9:1. After stirring for 4-6 minutes, a flowing backfill is prepared. Both the water reducing agent and the coagulant are made of new materials and are mixed according to the optimal ratio, so that the prepared flowing backfill material has better strength and fluidity.
[0043] Example 1
[0044] The waste mud of the shield tunnel was generated during the construction of a cross-river tunnel in Nanjing. The shield tunnel section is 3537m long and a circular slurry shield machine with a diameter of 14.93m was used for excavation. The construction process generated about 860,000m of waste mud. 3 The mud is made of bentonite, clay, sodium carbonate and water. The waste mud is highly alkaline and has a large volume, making it difficult to dispose of. A temporary mud storage pool is set up at the construction site to collect the waste mud and precipitate it to remove some of the water. The physical indicators of the shield waste mud are shown in Table 1.
[0045] Table 1 Physical indexes of shield waste slurry
[0046]
[0047] The method adopts three steps of waste mud multi-stage separation, mud flocculation dehydration and mobile backfill material preparation to treat the waste mud.
[0048] Step 1: The waste mud temporarily stored in the mud pool is introduced into the screening system (drum screen, cyclone and dewatering screen in sequence) through a delivery pump to separate coarse aggregates larger than 5 mm, fine aggregates of 0.5 to 5 mm and uniform mud.
[0049] Step 2: transport the uniform mud to the flocculation conditioning tank, and treat it by flocculation conditioning-vacuum preloading method. Add anionic polyacrylamide to the conditioning tank, so that the flocculant promotes the mud particles to form flocs, and add the flocculant to make its mass concentration 0.02%. After adding the flocculant, turn on the agitator in the flocculation conditioning tank to stir and mix. Stir at a speed of 600r / min for 2min during the mixing stage. Then pump the mud into the vacuum preloading device through the mud input port 3. The box 1 and the vacuum membrane 2 form a closed space for storing mud. Run the vacuum pump 7 to form a negative pressure in the device. The water in the mud passes through the geotextile 5 and enters the drainage board 4. The particles in the mud will be intercepted by the geotextile 5. The water in the drainage board 4 is discharged through the drainage pipe 6. The discharged mud tail water is stored in the tail water tank. After the water is pumped to a certain extent, the dehydrated water cake in the device is taken out.
[0050] Step 3: The coarse aggregate and fine aggregate in step 1 and the dewatered cement cake in step 2 are stirred and mixed to form an aggregate mixture. The mud tail water in step 2 is mixed with cement, fly ash, water reducing agent, coagulant, etc. to form a gel mixture. The aggregate mixture and the gel mixture are stirred in a mortar mixer at a mass ratio of 1.6:1 for 5 minutes to prepare a mobile backfill. The composition of the mobile backfill is shown in Table 2.
[0051] Table 2 Mass fraction of each component in the mobile backfill
[0052] Components Mass fraction Components Mass fraction coarse aggregate 386 Fly ash 308 fine aggregate 209 Water reducing agent 15.2 Dewatering Cake 100 Coagulant 7.8 cement 330 Mud tail water 430
[0053] Example 2
[0054] The waste mud of the shield tunnel was generated during the construction of a lake bottom tunnel in Wuhan. The shield tunnel section is 5712m long and a circular slurry shield machine with a diameter of 15.06m was used for excavation. The construction process generated about 1.57 million m of waste mud. 3 The mud is made of bentonite, clay, sodium hydroxide and water. The waste mud is highly alkaline and large in volume, making it difficult to dispose of. A temporary mud storage pool is set up at the construction site to collect the waste mud and remove some of the water by sedimentation. The physical indicators of the shield waste mud are shown in Table 3.
[0055] Table 3 Physical indexes of shield waste slurry
[0056]
[0057] The method adopts three steps of waste mud multi-stage separation, mud flocculation dehydration and mobile backfill material preparation to treat the waste mud.
[0058] Step 1: The waste mud temporarily stored in the mud pool is introduced into the screening system through a delivery pump to separate coarse aggregates larger than 5 mm, fine aggregates of 0.5 to 5 mm, and uniform mud.
[0059] Step 2: transport the uniform mud to the flocculation conditioning tank, and treat it by flocculation conditioning-vacuum preloading method. Add anionic polyacrylamide to the conditioning tank, so that the flocculant promotes the mud particles to form flocs, and add the flocculant to make its mass concentration 0.03%. After adding the flocculant, turn on the agitator in the flocculation conditioning tank to stir and mix. Stir at a speed of 700r / min for 3min during the mixing stage. Then pump the mud into the vacuum preloading device through the mud input port 3. The box 1 and the vacuum membrane 2 form a closed space for storing mud. Run the vacuum pump 7 to form a negative pressure in the device. The water in the mud passes through the geotextile 5 and enters the drainage board 4. The particles in the mud will be intercepted by the geotextile 5. The water in the drainage board 4 is discharged through the drainage pipe 6. The discharged tail water is stored in the tail water tank. After the water is pumped to a certain extent, the dehydrated water cake in the device is taken out.
[0060] Step 3: The coarse aggregate and fine aggregate in step 1 and the dewatered cement cake in step 2 are stirred and mixed to form an aggregate mixture. The mud tail water in step 2 is mixed with cement, fly ash, water reducer, coagulant, etc. to form a gel mixture. The aggregate mixture and the gel mixture are stirred in a mortar mixer at a mass ratio of 1.9:1 for 5 minutes to prepare a mobile backfill. The composition of the mobile backfill is shown in Table 4.
[0061] Table 4 Mass fraction of each component in the mobile backfill
[0062] Components Mass fraction Components Mass fraction coarse aggregate 415 Fly ash 285 fine aggregate 237 Water reducing agent 15.4 Dewatering Cake 100 Coagulant 7.9 cement 306 Mud tail water 415
[0063] Comparative Example 1:
[0064] Waste mud from shield tunneling of a tunnel project (having the same physical index as the waste mud in Example 1) was selected, and the mud was directly poured into a mixer. After stirring for 2 minutes, cement, fly ash, water reducing agent, and coagulant were added, and stirred again to obtain a mobile backfill material. The composition of the mobile backfill material is shown in Table 5.
[0065] Table 5 Mass fraction of each component in the mobile backfill
[0066] Components Mass fraction Components Mass fraction Waste mud 950 Water reducing agent 4.3 cement 104 Coagulant 2.1 Fly ash 94
[0067] Comparative Example 2:
[0068] Waste mud from shield tunneling of a tunnel project (having the same physical indexes as the waste mud in Example 2) was selected, and the mud was directly poured into a mixer. After stirring for 2 minutes, cement, fly ash, water reducing agent, and coagulant were added, and stirred evenly again to obtain a mobile backfill material. The composition of the mobile backfill material is shown in Table 6.
[0069] Table 6 Mass fraction of each component in the mobile backfill
[0070] Components Mass fraction Components Mass fraction Waste mud 1080 Water reducing agent 4.2 cement 116 Coagulant 2.5 Fly ash 98
[0071] Comparative Example 3:
[0072] The coarse aggregate, fine aggregate and dehydrated cement cake in Example 1 were used as raw materials, and the flowable backfill material was prepared according to step 3 in Example 1. The composition of the flowable backfill material is shown in Table 7.
[0073] Table 7 Mass fraction of each component in the mobile backfill
[0074] Components Mass fraction Components Mass fraction coarse aggregate 280 Fly ash 308 fine aggregate 280 Water reducing agent 15.2 Dewatering Cake 140 Coagulant 7.8 cement 330 Mud tail water 430
[0075] Comparative Example 4:
[0076] The coarse aggregate, fine aggregate and dehydrated cement cake in Example 1 were used as raw materials, and the flowable backfill material was prepared according to step 3 in Example 1. The composition of the flowable backfill material is shown in Table 8.
[0077] Table 8 Mass fraction of each component in the mobile backfill
[0078] Components Mass fraction Components Mass fraction coarse aggregate 420 Fly ash 308 fine aggregate 140 Water reducing agent 15.2 Dewatering Cake 140 Coagulant 7.8 cement 330 Mud tail water 430
[0079] Comparative Example 5:
[0080] The coarse aggregate, fine aggregate and dehydrated cement cake in Example 1 were used as raw materials, and the flowable backfill material was prepared according to step 3 in Example 1. The composition of the flowable backfill material is shown in Table 9.
[0081] Table 9 Mass fraction of each component in the mobile backfill
[0082] Components Mass fraction Components Mass fraction coarse aggregate 350 Fly ash 308 fine aggregate 175 Water reducing agent 15.2 Dewatering Cake 175 Coagulant 7.8 cement 330 Mud tail water 430
[0083] Performance Test:
[0084] The performance of seven groups of flowing backfill materials was tested, and the test results are shown in Table 10.
[0085] Table 10 Performance test results of seven kinds of mobile backfill materials
[0086]
[0087] It can be seen from Table 10 that the 28d unconfined compressive strength of the flowable backfill prepared by the manufacturing process of Examples 1 and 2 of the present application is above 350 kPa, and the flow value is above 200 mm, and all aspects of the performance are much higher than those of the flowable backfill prepared by the manufacturing process of Comparative Examples 1, 2, 3, 4, and 5.
[0088] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.
Claims
1. A process for preparing mobile backfill material based on shield waste mud. It is characterized in that It includes the following three steps, specifically: Step 1: Multi-stage separation of waste mud, screening the aggregate in the waste mud to obtain coarse aggregate, fine aggregate and mixed uniform mud; Step 2: Mud flocculation and dehydration, using flocculation conditioning and vacuum preloading to treat the uniform mud after multi-stage separation to form a dehydrated mud cake, and the discharged water forms mud tail water; Step 3: preparing a mobile backfill material, mixing the coarse aggregate and fine aggregate in step 1 with the dewatered cement cake in step 2 to form an aggregate mixture, then mixing the mud tail water produced in step 2 with cement, fly ash, water reducing agent and coagulant to form a gel mixture, and stirring the aggregate mixture and the gel mixture to prepare a mobile backfill material; The step 1 specifically includes the following steps: Step 1.1: The waste slurry from the shield tunnel in the slurry tank is transported to the drum screen through a slurry pump. The aperture of the drum screen is 5 mm. After the waste slurry is screened, coarse aggregate with a particle size of more than 5 mm is obtained; Step 1.2: The remaining waste mud after screening is transported to the hydrocyclone, and the aggregates of 0.5~5mm are separated by the hydrocyclone. The inner hydrocyclone mud with particle size below 0.5mm is discharged from the upper part of the hydrocyclone, and the outer hydrocyclone mud with particle size within the range of 0.5~5mm is discharged from the lower part of the hydrocyclone and enters the dewatering screen; Step 1.3: The aperture of the dewatering screen is 0.5 mm. The dewatering screen dehydrates and screens the aggregate in the external cyclonic mud to obtain fine aggregate with a particle size ranging from 0.5 to 5 mm; Step 1.4: The mud screened by the dewatering screen is mixed with the internal cyclone mud to form a uniform mud with uniform components; The step 3 specifically includes the following steps: Step 3.1: The coarse aggregate and fine aggregate produced in the above step 1 are mixed evenly with the dewatered cement cake formed in step 2, wherein the mixing mass ratio of the dewatered cement cake, the fine aggregate and the coarse aggregate is 1:1.7-2.8:2.5-4.5, and the three materials are mixed in proportion to form an aggregate mixture; Step 3.2: the mud tail water produced in the above step 2 is mixed with cement, fly ash, water reducing agent and coagulant, the mixing mass ratio of cement, fly ash, water reducing agent, coagulant and mud tail water is 1:0.9~1.2:0.04~0.06:0.02~0.03:0.6~2.0, and the four materials and mud tail water are stirred into a gel mixture; Step 3.3: Put the aggregate mixture formed in the above step 3.1 and the gel mixture formed in step 3.2 into a mortar mixer at a mass ratio of 1.5 to 1.9:1, and stir for 4 to 6 minutes to prepare a flowable backfill material.
2. The process for preparing mobile backfill material based on shield waste mud according to claim 1, It is characterized in that The step 2 specifically includes the following steps: Step 2.1: The uniform slurry in the above step 1 is transported to a flocculation conditioning tank, and a flocculant is added thereto to make the suspended particles in the uniform slurry coagulate and settle. The flocculant used is anionic polyacrylamide, and the flocculant is added to make its mass concentration 0.02-0.03%. After adding the flocculant, the agitator in the flocculation conditioning tank is turned on for stirring and mixing. During the mixing stage, the agitator is stirred at a speed of 600-700 r / min for 2-3 minutes to make the flocculant and the solution evenly mixed. The flocculation and sedimentation time is 10-15 minutes; Step 2.2: The flocculated and conditioned mud is transported to the vacuum preloading device through a mud pump for vacuum preloading to form a dehydrated water cake. The water discharged by the vacuum preloading is the mud tail water.
3. The process for preparing mobile backfill material based on shield waste mud according to claim 2, It is characterized in that The vacuum preloading device comprises: A box body, a vacuum membrane is arranged on the top of the box body, the vacuum membrane isolates the inside of the box body into a closed space, and a mud input port is arranged at the bottom of the box body; Drainage boards, several of which are arranged in the closed space of the box, the outer side of the drainage boards is wrapped with geotextiles, and the drainage boards are provided with several water-permeable holes; A drainage pipe is connected to the plurality of water-permeable holes on the plurality of drainage plates, and the drainage pipe is connected to a vacuum pump outside the box.
4. The process for preparing mobile backfill material based on shield waste mud according to claim 1, It is characterized in that The water reducer in step 3.2 is composed of one or two of phosphate-based water reducer and polycarboxylate water reducer, and the coagulant is composed of one or two of sodium silicate and calcium formate.
Citation Information
Cited By
Preparation method and application of modified shield soil recycled coarse aggregate
CN121270131A