A method for preparing a light-cured 3D printed PU prosthesis

Through the light-curing 3D printing PU prosthesis preparation method, CT scan data and specific raw materials are used to prepare light-curing PU printing ink, which solves the problems of traditional palatine fistula prosthesis production complexity and insufficient material performance, and achieves high precision and low cost. Palatal fistula repair options.

CN116198113BActive Publication Date: 2024-10-22SOUTHERN MEDICAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310205761.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-06
Publication Date
2024-10-22
Estimated Expiration
2043-03-06

AI Technical Summary

Technical Problem

The manufacturing process of traditional palatal fistula prostheses is complicated and costly, and the materials are expensive. Moreover, the existing materials have insufficient mechanical properties and biocompatibility, making it difficult to meet clinical needs.

Method used

A light-curing 3D printing PU prosthetic preparation method was used to obtain the palatal defect model through CT scan data. Polytetramethylene ether glycol PTMEG and isophorone diisocyanate and other raw materials were used to prepare light-curing PU printing ink for 3D printing. Print to simplify the production process and improve accuracy and performance.

Benefits of technology

It achieves simple synthesis, good mechanical properties and biocompatibility of the prosthesis, reduces the difficulty and time of production, significantly improves the accuracy and mechanical properties of the prosthesis, and is suitable for palatal fistula repair.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116198113B_ABST
    Figure CN116198113B_ABST
Patent Text Reader

Abstract

A method for preparing a light-cured 3D printed PU prosthesis comprises the following steps: step (1), collecting CT scan data of a maxillary defect; step (2), obtaining a prosthesis printing model according to the CT scan data obtained in step (1); step (3), using a pre-prepared light-cured PU printing ink to perform 3D light-curing printing on the prosthesis printing model to obtain a prosthesis; the raw materials of the light-cured PU printing ink contain polytetramethylene ether glycol (PTMEG) and isophorone diisocyanate (IPDI). The prosthesis prepared by the light-cured 3D printed PU prosthesis preparation method is simple to synthesize, has good mechanical properties, good biocompatibility and strong mechanical properties, and the present invention reduces the difficulty of clinical operation of the impression before prosthesis production, shortens the production time and can greatly improve the accuracy of the prosthesis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oral medical materials, and in particular relates to a method for preparing a light-cured 3D printed PU prosthesis. Background Art

[0002] Palatal fistula is an abnormal communication between the oral and nasal cavities of patients with cleft palate after surgery. It is the most common complication after cleft palate surgery. Congenital developmental abnormalities, tumors, trauma, radiotherapy and chemotherapy can also cause palatal fistula. Large palatal fistulas can produce obvious clinical symptoms and cause functional disorders such as nasal leakage, dysarthria, and hearing loss. The communication between the oral and nasal cavities often causes a foul odor in the mouth, which seriously affects the patient's mental health and social activities. Due to various subjective and objective reasons, some cases do not undergo further surgery, but use prostheses for repair in order to restore complete function and improve the quality of life.

[0003] The production of traditional prostheses requires multiple steps such as molding, casting, and trimming. The process is complicated, the production cost and labor cost are high, the technology is highly sensitive, and it takes a long time. The computer-aided design and computer-aided manufacturing technology (CAD / CAM) that has emerged in recent years uses medical imaging technology such as CBCT to obtain the patient's three-dimensional data and then manufacture prostheses. Although this new method obtains a prosthesis that is closer to the desired shape through computer modeling, the materials available are limited and expensive. On the other hand, the materials currently used for palatal fistula prostheses are mainly medical-grade silicone rubber materials, which are expensive.

[0004] Therefore, in view of the shortcomings of the existing technology, it is necessary to provide a method for preparing a photocurable 3D printed PU prosthesis to solve the shortcomings of the existing technology. Summary of the invention

[0005] The purpose of the present invention is to avoid the shortcomings of the prior art and provide a method for preparing a light-cured 3D printed PU prosthesis. The light-cured 3D printed PU prosthesis preparation method has simple prosthesis synthesis, good mechanical properties, good biocompatibility and strong mechanical properties, and the present invention reduces the clinical operation difficulty of the impression before prosthesis production, shortens the production time and can greatly improve the accuracy of the prosthesis.

[0006] The above-mentioned purpose of the present invention is achieved by the following technical measures:

[0007] A method for preparing a light-cured 3D printed PU prosthesis is provided, comprising the following steps:

[0008] Step (1), collecting CT scan data of the maxillary defect;

[0009] Step (2), obtaining a prosthetic printed model based on the CT scan data obtained in step (1);

[0010] Step (3), using the pre-prepared light-curing PU printing ink to perform 3D light-curing printing on the prosthesis printing model to obtain the prosthesis;

[0011] The raw materials of light-curing PU printing ink contain polytetramethylene ether glycol PTMEG and isophorone diisocyanate IPDI.

[0012] Preferably, the raw materials of the above-mentioned photocurable PU printing ink further contain hydroxyethyl methacrylate HEMA and dibutyltin dilaurate DBTDL.

[0013] Preferably, the molecular weight of the polytetramethylene ether glycol (PTMEG) is in the range of 650 to 2000.

[0014] Preferably, the preparation method of the above-mentioned photocurable PU printing ink is divided into a single molecular weight PU polymer preparation process and a mixing process.

[0015] Preferably, the above-mentioned single molecular weight PU polymer preparation process steps include:

[0016] Step (A), adding isophorone diisocyanate IPDI and dibutyltin dilaurate DBTDL into a reaction container, and then adding a tetrahydrofuran solution of single molecular weight polytetramethylene ether glycol PTMEG into the reaction container, and stirring;

[0017] Step (B), adding hydroxyethyl methacrylate (HEMA) into a reaction container to obtain a PU solution;

[0018] Step (C), adding petroleum ether to the PU solution obtained in step (B) for layered extraction to obtain an extract;

[0019] Step (D), vacuum drying the extract obtained in step (C) to obtain a PU polymer.

[0020] Preferably, the mixing step is to mix the polyurethane elastomer, isooctyl acrylate, isobornyl acrylate and phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide to obtain the light-curable PU printing ink.

[0021] Preferably, the polyurethane elastomer is composed of at least one PU polymer obtained in step (D) with a molecular weight of 1.5 Å.

[0022] Preferably, the above step (A) is specifically to heat isophorone diisocyanate IPDI and dibutyltin dilaurate DBTDL to a temperature of 65°C to 72°C, and then add a tetrahydrofuran solution of single molecular weight polytetramethylene ether glycol PTMEG into a reaction container, heat to a temperature of 65°C to 72°C and stir for 2h to 4h.

[0023] Preferably, the above step (B) specifically comprises adding hydroxyethyl methacrylate HEMA into a reaction container, and stirring at a temperature of 65° C. to 72° C. for 2 h to 4 h to obtain a PU solution.

[0024] In the single molecular weight PU polymer preparation process, the raw material ratio is calculated by molar ratio:

[0025] Polytetramethylene ether glycol PTMEG: 0.01~0.03;

[0026] Isophorone diisocyanate IPDI: 0.02~0.06;

[0027] Hydroxyethyl methacrylate HEMA: 0.02~0.06;

[0028] Dibutyltin dilaurate DBTDL: 0.0010~0.0020.

[0029] In the mixing process, the weight ratio of the polyurethane elastomer, isooctyl acrylate and isobornyl acrylate is 4-8:1-3:1-3.

[0030] The amount of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide is 1% to 3% of the total weight percentage of the polyurethane elastomer, isooctyl acrylate and isobornyl acrylate.

[0031] The volume concentration of the tetrahydrofuran solution of the single molecular weight polytetramethylene ether glycol PTMEG is 10% to 30%.

[0032] The extracting liquid in the step (C) is petroleum ether, and the volume ratio of petroleum ether to PU solution is 5:1 to 15:1.

[0033] The polyurethane elastomer consists of 1000PU polymer, or the polyurethane elastomer consists of at least two of 650PU polymer, 1000PU polymer and 2000PU polymer.

[0034] Preferably, the 1000PU polymer is a single molecular weight PU polymer prepared from polytetramethylene ether glycol (PTMEG) having a molecular weight of 1000.

[0035] Preferably, the 650PU polymer is a single molecular weight PU polymer prepared from polytetramethylene ether glycol (PTMEG) having a molecular weight of 650.

[0036] Preferably, the 2000PU polymer is a single molecular weight PU polymer prepared from polytetramethylene ether glycol (PTMEG) having a molecular weight of 2000.

[0037] Further, in the single molecular weight PU polymer preparation process, the raw material ratio is calculated by molar ratio:

[0038] Polytetramethylene ether glycol PTMEG: 0.02;

[0039] Isophorone diisocyanate IPDI: 0.04;

[0040] Hydroxyethyl methacrylate HEMA: 0.04;

[0041] Dibutyltin dilaurate DBTDL: 0.0015.

[0042] In the mixing process, the weight ratio of the polyurethane elastomer, isooctyl acrylate and isobornyl acrylate is 6:2:2.

[0043] The amount of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide is 2% of the total weight percentage of the polyurethane elastomer, isooctyl acrylate and isobornyl acrylate.

[0044] The polyurethane elastomer is composed of 1000PU polymer, or the polyurethane elastomer is composed of at least two of 650PU polymer, 1000PU polymer and 2000PU polymer;

[0045] The 1000PU polymer is a single molecular weight PU polymer prepared from polytetramethylene ether glycol (PTMEG) having a molecular weight of 1000.

[0046] The 650 PU polymer is a single molecular weight PU polymer prepared from polytetramethylene ether glycol (PTMEG) having a molecular weight of 650.

[0047] The 2000 PU polymer is a single molecular weight PU polymer prepared from polytetramethylene ether glycol (PTMEG) having a molecular weight of 2000.

[0048] The volume concentration of the tetrahydrofuran solution of polytetramethylene ether glycol (PTMEG) with a single molecular weight is 20%.

[0049] The extracting liquid in step (C) is petroleum ether, and the volume ratio of petroleum ether to PU solution is 10:1.

[0050] Preferably, the above step (2) includes:

[0051] Step (2.1), importing the CT scan data obtained in step (1) into Mimics 21.0 software to perform three-dimensional reconstruction of the palate defect model, performing Thresholding selection on the CT scan data, deleting the frontal sinus, sphenoid sinus or ethmoid sinus cavity structure, and then using the Calculate 3D function to obtain a new mask, perform preliminary smoothing on it, and generate the first upper airway model before repair, the first palate defect animal skull model before repair, and the first palate mucosa model;

[0052] Step (2.2), importing the first upper airway model before repair, the first palate defect animal skull model before repair, and the first palate mucosa model obtained in step (2.1) into Geomagic 2017 for smooth optimization and surface filling, and obtaining the second upper airway model before repair, the second palate defect animal skull model before repair, and the second palate mucosa model accordingly;

[0053] Step (2.3), according to the spatial dimension data of the fistula at the palate defect of the second upper airway initial model before repair obtained in step (2.2), use Solidwork 2017 software to draw the prosthetic shape, and then perform smooth optimization processing on the prosthetic shape and surface filling to obtain a preliminary prosthetic model; then import the second upper airway initial model before repair obtained in step (2.2) and the preliminary prosthetic model into Geomagic 2017 software, align them, and obtain the upper airway model after repair;

[0054] Step (2.4), according to the animal skull model of the palate defect before the second repair and the second palate mucosa model, the edge of the preliminary prosthesis model is adjusted, and then according to the meshing and CFD analysis results of the upper airway initial model before the second repair and the upper airway model after the repair, the structure of the prosthesis model is adjusted to obtain the prosthesis printing model.

[0055] In step (2.4), the edge adjustment is specifically to merge the second animal skull model of the palate defect before repair and the second palate mucosa model into a merged model, and then import the preliminary prosthesis model and the merged model into Geomagic 2017 software, and perform fitting and preliminary alignment by manual registration through alignment, and set the mucosa and maxillary bone models as "test model", and set the prosthesis model as "reference model", and use the best fit alignment function to assemble the merged model and the prosthesis model, and then adjust the structure of the prosthesis model so that the edges of the prosthesis model and the merged model are sealed and aligned;

[0056] In step (2.4), data simulation and boundary condition definition are performed on the repaired upper airway model, and the airflow changes in the upper airway before and after the repair in a complete breathing cycle are calculated and simulated. CFD-Post is used to obtain gas flow data under the breathing state: three-dimensional airflow trajectory diagram, pressure cloud diagram, cross-sectional area of ​​each section and airflow velocity cloud diagram, and the structure of the prosthesis model is adjusted to obtain the prosthesis printing model.

[0057] Preferably, the repaired upper airway model corresponding to the above-mentioned prosthesis printed model has consistent pressure on the healthy side and the affected side and no abnormal vortex at the fistula.

[0058] The present invention discloses a method for preparing a light-cured 3D printed PU prosthesis, comprising the following steps: step (1), collecting CT scan data of a maxillary defect; step (2), obtaining a prosthesis printing model according to the CT scan data obtained in step (1); step (3), using a pre-prepared light-cured PU printing ink to perform 3D light-curing printing on the prosthesis printing model to obtain a prosthesis; the raw materials of the light-cured PU printing ink contain polytetramethylene ether glycol (PTMEG) and isophorone diisocyanate (IPDI). The prosthesis prepared by the light-cured 3D printed PU prosthesis preparation method is simple to synthesize, has good mechanical properties, good biocompatibility and strong mechanical properties, and the present invention reduces the difficulty of clinical operation of the impression before prosthesis production, shortens the production time and can greatly improve the accuracy of the prosthesis. BRIEF DESCRIPTION OF THE DRAWINGS

[0059] The present invention is further described with reference to the accompanying drawings, but the contents in the accompanying drawings do not constitute any limitation to the present invention.

[0060] Figure 1 The synthesis route of the photocurable PU printing ink of the present invention is

[0061] Figure 2 These are the rheological curves of the pure PU product and the photocurable PU printing ink of the present invention.

[0062] Figure 3 This is the rheological curve of the photocurable PU printing ink of the present invention.

[0063] Figure 4 It is the infrared image of polytetramethylene ether glycol PTMEG, the intermediate product of step (A) and the product of step (B).

[0064] Figure 5 This is a schematic diagram of the structure of the second animal skull model for repairing anterior palate defects.

[0065] Figure 6 This is a structural schematic diagram of the second palate mucosa model.

[0066] Figure 7A schematic diagram of the combined model.

[0067] Figure 8 Schematic diagram of the structure of the pseudocomplex model.

[0068] Fig. 9 Assembly diagram of the merged model and the pseudo-model.

[0069] Fig.10 These are five cross-sectional images of the upper airway before repair.

[0070] Fig.11 These are five cross-sectional images of the repaired upper airway.

[0071] Fig.12 It is a curve graph of the area of ​​each cross section of the prosthesis before and after repair.

[0072] Fig.13 Schematic diagram of the structure of the upper airway model before repair.

[0073] Fig.14 This is the air pressure, flow rate, and local pressure diagram before repair.

[0074] Fig.15 This is the air pressure, flow rate, and local pressure diagram after repair.

[0075] Fig.16 This is the flow velocity diagram of the healthy side before repair.

[0076] Fig.17 This is the flow velocity diagram of the affected side before repair.

[0077] Fig.18 This is the flow velocity diagram of the affected side after repair.

[0078] Fig.19 This is the flow velocity diagram of the healthy side after repair. DETAILED DESCRIPTION

[0079] The technical scheme of the present invention is further described in conjunction with the following examples. The experimental methods in the following examples are conventional methods unless otherwise specified. The raw materials, reagent materials, etc. used in the following examples, unless otherwise specified, can be purchased from conventional biochemical reagent stores or pharmaceutical companies. Among them, polytetramethylene ether glycol PTMEG and isooctyl acrylate with molecular weights of 650, 1000 and 2000 were purchased from Shanghai McLean Biochemical Technology Co., Ltd. Isobornyl acrylate was purchased from Shanghai Myrel Biochemical Technology Co., Ltd. Phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide was purchased from Shanghai Yuanye Biotechnology Co., Ltd. Hydroxyethyl methacrylate HEMA was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.

[0080] Example 1

[0081] A method for preparing a photocurable 3D printed PU pseudo-composite, wherein the raw materials of the photocurable PU printing ink contain polytetramethylene ether glycol (PTMEG), isophorone diisocyanate (IPDI), hydroxyethyl methacrylate (HEMA) and dibutyltin dilaurate (DBTDL).

[0082] Wherein, the molecular weight range of polytetramethylene ether glycol PTMEG is 650-2000.

[0083] The preparation method of the photocurable PU printing ink is divided into a single molecular weight PU polymer preparation process and a mixing process.

[0084] The steps of the single molecular weight PU polymer preparation process of the present invention are:

[0085] Step (A), adding isophorone diisocyanate IPDI and dibutyltin dilaurate DBTDL into a reaction container, and then adding a tetrahydrofuran solution of single molecular weight polytetramethylene ether glycol PTMEG into the reaction container, and stirring;

[0086] Step (B), adding hydroxyethyl methacrylate (HEMA) into a reaction container to obtain a PU solution;

[0087] Step (C), extracting the PU solution obtained in step (B) by layering and extracting to obtain an extract;

[0088] Step (D), vacuum drying the extract obtained in step (C) to obtain a PU polymer.

[0089] The mixing step is to mix polyurethane elastomer, isooctyl acrylate, isobornyl acrylate and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide to obtain a light-curable PU printing ink. The polyurethane elastomer is composed of at least one PU polymer obtained in step (D) with a molecular weight.

[0090] It should be noted that the national standard YY 0714.2-2016 stipulates the Shore hardness of the removable denture soft lining material, and the smaller the molecular weight of polytetramethylene ether glycol PTMEG, the harder the polyurethane elastomer obtained. Therefore, the polyurethane elastomer prepared by the present invention through PU polymers with different molecular weights can meet the national standard YY 0714.2-2016, and the prosthesis of the present invention can meet the hardness requirements of the national standard YY 0714.2-2016 and its tensile and compression values ​​are higher, so that the human body has good adaptability to it. And the flowability of the 3D printing of the obtained light-cured PU printing ink is in demand.

[0091] Step (A) is specifically to heat isophorone diisocyanate IPDI and dibutyltin dilaurate DBTDL to 65° C. to 72° C., then add a tetrahydrofuran solution of single molecular weight polytetramethylene ether glycol PTMEG into a reaction container, heat to 65° C. to 72° C. and stir for 2 h to 4 h;

[0092] Step (B) specifically comprises adding hydroxyethyl methacrylate HEMA into a reaction container, and stirring at a temperature of 65° C. to 72° C. for 2 h to 4 h to obtain a PU solution.

[0093] In the single molecular weight PU polymer preparation process, the raw material ratio is calculated by molar ratio:

[0094] Polytetramethylene ether glycol PTMEG: 0.01~0.03;

[0095] Isophorone diisocyanate IPDI: 0.02~0.06;

[0096] Hydroxyethyl methacrylate HEMA: 0.02~0.06;

[0097] Dibutyltin dilaurate DBTDL: 0.0010~0.0020.

[0098] In the mixing process, the weight ratio of the polyurethane elastomer, isooctyl acrylate and isobornyl acrylate is 4-8:1-3:1-3.

[0099] The volume concentration of the tetrahydrofuran solution of the single molecular weight polytetramethylene ether glycol PTMEG is 10% to 30%.

[0100] The extracting liquid in step (C) is petroleum ether, and the volume ratio of petroleum ether to PU solution is 5:1 to 15:1.

[0101] The amount of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide is 1% to 3% of the total weight percentage of the polyurethane elastomer, isooctyl acrylate and isobornyl acrylate.

[0102] The photocurable PU printing ink of the present invention has a C=C group in the system to obtain the photocurable properties of artificial synthetic polymers, and can be used to prepare a stable and high-precision prosthesis by initiating photocuring with ultraviolet light. Moreover, the prosthesis of the present invention has the advantages of good biocompatibility, strong mechanical properties, and is not easy to hydrolyze, and is suitable for long-term use in a moist oral environment.

[0103] The 3D printer parameter settings when using the photocurable PU printing ink of the present invention are specifically as follows: ultraviolet light irradiation is performed while printing, and the printed structure is photocross-linked layer by layer; the wavelength of the ultraviolet light used is 405nm, the layer thickness is 0.05mm, the exposure time is 2.5s, the bottom layer exposure time is 5s, the lifting distance is 7mm, and the lifting speed is 70mm / min.

[0104] The photocurable 3D printed PU prosthesis preparation method has simple prosthesis synthesis, good mechanical properties, good biocompatibility and strong mechanical properties. In addition, the present invention reduces the clinical operation difficulty of the impression before prosthesis production, shortens the production time and can greatly improve the accuracy of the prosthesis.

[0105] Example 2

[0106] A method for preparing a photocurable 3D printed PU prosthesis, the other features of which are the same as those of Example 1. In the preparation process of a single molecular weight PU polymer in this embodiment, the raw material ratio is calculated by molar ratio as follows:

[0107] Polytetramethylene ether glycol PTMEG: 0.02;

[0108] Isophorone diisocyanate IPDI: 0.04;

[0109] Hydroxyethyl methacrylate HEMA: 0.04;

[0110] Dibutyltin dilaurate DBTDL: 0.0015;

[0111] In the mixing process, the weight ratio of the polyurethane elastomer, isooctyl acrylate and isobornyl acrylate is 6:2:2.

[0112] The amount of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide is 2% of the total weight percentage of the polyurethane elastomer, isooctyl acrylate and isobornyl acrylate.

[0113] The polyurethane elastomer of this embodiment is composed of 1000PU polymer, or the polyurethane elastomer is composed of at least two of 650PU polymer, 1000PU polymer and 2000PU polymer.

[0114] 1000PU polymer is a single molecular weight PU polymer prepared from polytetramethylene ether glycol PTMEG with a molecular weight of 1000. 650PU polymer is a single molecular weight PU polymer prepared from polytetramethylene ether glycol PTMEG with a molecular weight of 650. 2000PU polymer is a single molecular weight PU polymer prepared from polytetramethylene ether glycol PTMEG with a molecular weight of 2000.

[0115] The volume concentration of the tetrahydrofuran solution of polytetramethylene ether glycol (PTMEG) with a single molecular weight is 20%.

[0116] The extracting liquid in step (C) is petroleum ether, and the volume ratio of petroleum ether to PU solution is 10:1.

[0117] It should be noted that, the hardness of the composite prepared by using 650PU polymer alone is greater than 50, which exceeds the national standard YY 0714.2-2016, and the hardness of the composite prepared by using 2000PU polymer alone is within the range of the national standard YY 0714.2-2016, but its viscosity is relatively large and it is not suitable for use as a light-curable printing ink alone. Of course, according to actual needs, the polyurethane elastomer of the present invention can also be made of a variety of other molecular weights within the range of 650 to 2000 of polytetramethylene ether glycol PTMEG.

[0118] The prosthesis obtained in this embodiment within the scope of embodiment 1 has relatively good biocompatibility and relatively strong mechanical properties.

[0119] Example 3

[0120] A method for preparing a photocurable 3D printed PU prosthesis, the other features of which are the same as those of Example 1. In the photocurable PU printing ink of this embodiment, the molecular weight of polytetramethylene ether glycol PTMEG is 2000 and 650.

[0121] The steps of 650PU polymer preparation process are as follows:

[0122] Step (A), heating isophorone diisocyanate IPDI and dibutyltin dilaurate DBTDL to 70°C, then adding a tetrahydrofuran solution of polytetramethylene ether glycol PTMEG with a molecular weight of 650 into a reaction container, heating to 70°C and stirring for 3h;

[0123] Step (B), adding hydroxyethyl methacrylate HEMA into a reaction vessel, stirring at 68° C. for 3 h to obtain a PU solution;

[0124] Step (C), adding petroleum ether to the PU solution obtained in step (B) for layered extraction to obtain an extract;

[0125] Step (D), vacuum drying the extract obtained in step (C) to obtain 650 PU polymer.

[0126] In the 2000PU polymer preparation process, the raw material ratio is calculated by molar ratio:

[0127] Polytetramethylene ether glycol PTMEG: 0.02;

[0128] Isophorone diisocyanate IPDI: 0.04;

[0129] Hydroxyethyl methacrylate HEMA: 0.04;

[0130] Dibutyltin dilaurate DBTDL: 0.0015.

[0131] The volume concentration of the tetrahydrofuran solution of polytetramethylene ether glycol (PTMEG) with a single molecular weight is 10%.

[0132] The extracting liquid in step (C) is petroleum ether, and the volume ratio of petroleum ether to PU solution is 5:1.

[0133] The steps of 2000PU polymer preparation process are:

[0134] Step (A), heating isophorone diisocyanate IPDI and dibutyltin dilaurate DBTDL to 68°C, then adding a tetrahydrofuran solution of polytetramethylene ether glycol PTMEG with a molecular weight of 2000 into a reaction container, heating to 70°C and stirring for 3h;

[0135] Step (B), adding hydroxyethyl methacrylate HEMA into a reaction vessel, stirring at 68° C. for 3 h to obtain a PU solution;

[0136] Step (C), adding petroleum ether to the PU solution obtained in step (B) for layered extraction to obtain an extract;

[0137] Step (D), vacuum drying the extract obtained in step (C) to obtain 2000 PU polymer.

[0138] In the preparation process of PU polymer with a molecular weight of 2000, the raw material ratio is calculated by molar ratio:

[0139] Polytetramethylene ether glycol PTMEG: 0.02;

[0140] Isophorone diisocyanate IPDI: 0.04;

[0141] Hydroxyethyl methacrylate HEMA: 0.04;

[0142] Dibutyltin dilaurate DBTDL: 0.0015.

[0143] The volume concentration of the tetrahydrofuran solution of polytetramethylene ether glycol (PTMEG) with a single molecular weight is 15%.

[0144] The extracting liquid in step (C) is petroleum ether, and the volume ratio of petroleum ether to PU solution is 15:1.

[0145] The mixing process is to mix polyurethane elastomer, isooctyl acrylate, isobornyl acrylate and phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide to obtain a light-curable PU printing ink, wherein the mixing process is to mix the polyurethane elastomer, isooctyl acrylate and isobornyl acrylate in a weight ratio of 8:1:3, wherein the weight ratio of the PU polymer with a molecular weight of 2000 to the PU polymer with a molecular weight of 650 in the polyurethane elastomer is 1:1. The amount of phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide is 1% of the total weight percentage of the polyurethane elastomer, isooctyl acrylate and isobornyl acrylate.

[0146] Example 4

[0147] A method for preparing a photocurable 3D printed PU prosthesis, the other features of which are the same as those of Example 1. In the photocurable PU printing ink of this embodiment, the molecular weight of polytetramethylene ether glycol PTMEG is 1000.

[0148] The steps of 1000PU polymer preparation process are:

[0149] Step (A), heating isophorone diisocyanate IPDI and dibutyltin dilaurate DBTDL to 65°C, then adding a tetrahydrofuran solution of polytetramethylene ether glycol PTMEG with a molecular weight of 1000 into a reaction container, heating to 70°C and stirring for 2h;

[0150] Step (B), adding hydroxyethyl methacrylate HEMA into a reaction vessel, stirring at 66° C. for 2 h to obtain a PU solution;

[0151] Step (C), adding petroleum ether to the PU solution obtained in step (B) for layered extraction to obtain an extract;

[0152] Step (D), vacuum drying the extract obtained in step (C) to obtain 1000 PU polymer.

[0153] In the preparation process of PU polymer with a molecular weight of 1000, the raw material ratio is calculated by molar ratio:

[0154] Polytetramethylene ether glycol PTMEG: 0.02;

[0155] Isophorone diisocyanate IPDI: 0.04;

[0156] Hydroxyethyl methacrylate HEMA: 0.04;

[0157] Dibutyltin dilaurate DBTDL: 0.0015.

[0158] The volume concentration of the tetrahydrofuran solution of polytetramethylene ether glycol (PTMEG) of a single molecular weight is 8%.

[0159] The extracting liquid in step (C) is petroleum ether, and the volume ratio of petroleum ether to PU solution is 8:1.

[0160] The mixing process is to mix polyurethane elastomer, isooctyl acrylate, isobornyl acrylate and phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide to obtain a light-curable PU printing ink, wherein the mixing process is to mix the polyurethane elastomer, isooctyl acrylate and isobornyl acrylate in a weight ratio of 6:2:2. The amount of phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide is 2% of the total weight percentage of the polyurethane elastomer, isooctyl acrylate and isobornyl acrylate.

[0161] Example 5

[0162] A method for preparing a photocurable 3D printed PU prosthesis, the other features of which are the same as those of Example 1. In the photocurable PU printing ink of this embodiment, the molecular weight of polytetramethylene ether glycol PTMEG is 1000 and 650.

[0163] The steps of 650PU polymer preparation process are as follows:

[0164] Step (A), heating isophorone diisocyanate IPDI and dibutyltin dilaurate DBTDL to 65°C, then adding a tetrahydrofuran solution of polytetramethylene ether glycol PTMEG with a molecular weight of 650 into a reaction container, heating to 72°C and stirring for 4 hours;

[0165] Step (B), adding hydroxyethyl methacrylate HEMA into a reaction vessel, stirring at 72° C. for 4 hours to obtain a PU solution;

[0166] Step (C), adding petroleum ether to the PU solution obtained in step (B) for layered extraction to obtain an extract;

[0167] Step (D), vacuum drying the extract obtained in step (C) to obtain 650 PU polymer.

[0168] In the 650PU polymer preparation process, the raw material ratio is calculated by molar ratio:

[0169] Polytetramethylene ether glycol PTMEG: 0.01;

[0170] Isophorone diisocyanate IPDI: 0.02;

[0171] Hydroxyethyl methacrylate HEMA: 0.02;

[0172] Dibutyltin dilaurate DBTDL: 0.0010.

[0173] The volume concentration of the tetrahydrofuran solution of polytetramethylene ether glycol (PTMEG) of a single molecular weight is 12%.

[0174] The extracting liquid in step (C) is petroleum ether, and the volume ratio of petroleum ether to PU solution is 10:1.

[0175] The steps of 1000PU polymer preparation process are:

[0176] Step (A), heating isophorone diisocyanate IPDI and dibutyltin dilaurate DBTDL to 72° C., then adding a tetrahydrofuran solution of polytetramethylene ether glycol PTMEG with a molecular weight of 1000 into a reaction container, heating to 71° C. and stirring for 2 hours;

[0177] Step (B), adding hydroxyethyl methacrylate HEMA into a reaction vessel, stirring at 65° C. for 2 h to obtain a PU solution;

[0178] Step (C), adding petroleum ether to the PU solution obtained in step (B) for layered extraction to obtain an extract;

[0179] Step (D), vacuum drying the extract obtained in step (C) to obtain 1000 PU polymer.

[0180] In the 1000PU polymer preparation process, the raw material ratio is calculated by molar ratio:

[0181] Polytetramethylene ether glycol PTMEG: 0.03;

[0182] Isophorone diisocyanate IPDI: 0.06;

[0183] Hydroxyethyl methacrylate HEMA: 0.06;

[0184] Dibutyltin dilaurate DBTDL: 0.0020.

[0185] The volume concentration of the tetrahydrofuran solution of polytetramethylene ether glycol (PTMEG) of a single molecular weight is 9%.

[0186] The extracting liquid in step (C) is petroleum ether, and the volume ratio of petroleum ether to PU solution is 6:1.

[0187] The mixing process is to mix polyurethane elastomer, isooctyl acrylate, isobornyl acrylate and phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide to obtain a light-curable PU printing ink, wherein the mixing process is to mix the polyurethane elastomer, isooctyl acrylate and isobornyl acrylate in a weight ratio of 4:3:1, wherein the weight ratio of the PU polymer with a molecular weight of 1000 to the PU polymer with a molecular weight of 650 in the polyurethane elastomer is 1:1. The amount of phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide is 3% of the total weight percentage of the polyurethane elastomer, isooctyl acrylate and isobornyl acrylate.

[0188] Example 6

[0189] A method for preparing a photocurable 3D printed PU prosthesis, the other features of which are the same as those of Example 1. In the photocurable PU printing ink of this embodiment, the molecular weight of polytetramethylene ether glycol PTMEG is 2000.

[0190] The steps of 2000PU polymer preparation process are:

[0191] Step (A), heating isophorone diisocyanate IPDI and dibutyltin dilaurate DBTDL to 68°C, then adding a tetrahydrofuran solution of polytetramethylene ether glycol PTMEG with a molecular weight of 2000 into a reaction container, heating to 71°C and stirring for 3h;

[0192] Step (B), adding hydroxyethyl methacrylate HEMA into a reaction vessel, stirring at 68° C. for 3 h to obtain a PU solution;

[0193] Step (C), adding petroleum ether to the PU solution obtained in step (B) for layered extraction to obtain an extract;

[0194] Step (D), vacuum drying the extract obtained in step (C) to obtain 2000 PU polymer.

[0195] In the 2000PU polymer preparation process, the raw material ratio is calculated by molar ratio:

[0196] Polytetramethylene ether glycol PTMEG: 0.02;

[0197] Isophorone diisocyanate IPDI: 0.05;

[0198] Hydroxyethyl methacrylate HEMA: 0.05;

[0199] Dibutyltin dilaurate DBTDL: 0.0018.

[0200] The volume concentration of the tetrahydrofuran solution of polytetramethylene ether glycol (PTMEG) of a single molecular weight is 13%.

[0201] The extracting liquid in step (C) is petroleum ether, and the volume ratio of petroleum ether to PU solution is 15:1.

[0202] The mixing process is to mix polyurethane elastomer, isooctyl acrylate, isobornyl acrylate and phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide to obtain a light-curable PU printing ink, wherein the mixing process is to mix the polyurethane elastomer, isooctyl acrylate and isobornyl acrylate in a weight ratio of 6:2:2. The amount of phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide is 1.5% of the total weight percentage of the polyurethane elastomer, isooctyl acrylate and isobornyl acrylate.

[0203] Example 7

[0204] A method for preparing a photocurable 3D printed PU prosthesis, the other features of which are the same as those of Example 1. In the photocurable PU printing ink of this embodiment, the molecular weight of polytetramethylene ether glycol PTMEG is 650.

[0205] The steps of 650PU polymer preparation process are as follows:

[0206] Step (A), heating isophorone diisocyanate IPDI and dibutyltin dilaurate DBTDL to 68°C, then adding a tetrahydrofuran solution of polytetramethylene ether glycol PTMEG with a molecular weight of 650 into a reaction container, heating to 68°C and stirring for 3h;

[0207] Step (B), adding hydroxyethyl methacrylate HEMA into a reaction vessel, stirring at 68° C. for 3 h to obtain a PU solution;

[0208] Step (C), adding petroleum ether to the PU solution obtained in step (B) for layered extraction to obtain an extract;

[0209] Step (D), vacuum drying the extract obtained in step (C) to obtain 650 PU polymer.

[0210] In the 650PU polymer preparation process, the raw material ratio is calculated by molar ratio:

[0211] Polytetramethylene ether glycol PTMEG: 0.02;

[0212] Isophorone diisocyanate IPDI: 0.04;

[0213] Hydroxyethyl methacrylate HEMA: 0.04;

[0214] Dibutyltin dilaurate DBTDL: 0.0018.

[0215] The volume concentration of the tetrahydrofuran solution of polytetramethylene ether glycol (PTMEG) of a single molecular weight is 12%.

[0216] The extracting liquid in step (C) is petroleum ether, and the volume ratio of petroleum ether to PU solution is 10:1.

[0217] The mixing process is to mix polyurethane elastomer, isooctyl acrylate, isobornyl acrylate and phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide to obtain a light-curable PU printing ink, wherein the mixing process is to mix the polyurethane elastomer, isooctyl acrylate and isobornyl acrylate in a weight ratio of 6:2:2. The amount of phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide is 2% of the total weight percentage of the polyurethane elastomer, isooctyl acrylate and isobornyl acrylate.

[0218] Example 8

[0219] A method for preparing a photocurable 3D printed PU prosthesis, the other features of which are the same as those of Example 7, except that in the mixing step, polyurethane elastomer, isooctyl acrylate, and isobornyl acrylate are mixed in a weight ratio of 5:3:2 to obtain a photocurable PU printing ink.

[0220] Example 9

[0221] A method for preparing a photocurable 3D printed PU prosthesis, the other features of which are the same as those of Example 4, except that in the mixing step, polyurethane elastomer, isooctyl acrylate, and isobornyl acrylate are mixed in a weight ratio of 5:3:2 to obtain a photocurable PU printing ink.

[0222] Example 10

[0223] A method for preparing a photocurable 3D printed PU prosthesis, the other features of which are the same as those of Example 6, except that in the mixing step, polyurethane elastomer, isooctyl acrylate, and isobornyl acrylate are mixed in a weight ratio of 5:3:2 to obtain a photocurable PU printing ink.

[0224] Rheology, Shore hardness and infrared analysis

[0225] 1. Rheology

[0226] The rheological properties of the cured PU printing inks prepared in Examples 4 and 6 to 10 were tested. Figure 2 and Figure 3 .from Figure 2 and Figure 3It can be seen that the viscosity of the photocurable PU printing ink obtained by 2000PU polymer is too high, so it is not suitable for use as a photocurable printing ink alone. The viscosity of the 1000PU polymer alone, the 6500PU polymer alone, the 1000PU polymer and the 6500PU polymer, the 2000PU polymer and the 6500PU polymer is moderate and suitable for use as a photocurable printing ink.

[0227] 2. Shore hardness

[0228] The photocurable printing inks prepared in Examples 3 to 7 were used to print the same composite under the printing conditions of step (3) of Example 1, and the Shore hardness thereof was tested, as shown in Table 1.

[0229] Table 1, Shore hardness

[0230] As can be seen from the table, the photocurable PU printing ink of Example 7 is composed of a single 650 PU polymer.

[0231] The obtained pseudocomposite has a Shore hardness greater than 50 at different points, while the Shore hardness of the pseudocomposite obtained in Example 3 composed of 650PU polymer and 2000PU polymer, Example 5 composed of 650PU polymer and 1000PU polymer, Example 4 composed of 650PU polymer alone, and Example 6 composed of 650PU polymer alone are all within the range of 37 to 42. Considering the rheological properties and Shore hardness of the photocurable printing ink, the photocurable printing ink obtained by the polyurethane elastomer composed of 1000PU polymer alone, or composed of two of 650PU polymer, 1000PU polymer and 2000PU polymer is the most suitable.

[0232] 3. Infrared analysis

[0233] The polytetramethylene ether glycol PTMEG and the intermediate product of step (A) and the product of step (B) of Examples 4, 6 and 7 were subjected to infrared detection, as shown in FIG. Figure 4 .in Figure 4The PU solution-1 is the product of step (A) of Example 6, the intermediate product-1 is the product of step (B) of Example 6, the PU solution-2 curve is the product of step (A) of Example 4, the intermediate product-2 is the product of step (B) of Example 4, the PU solution-3 is the product of step (A) of Example 7, and the intermediate product-3 is the product of step (B) of Example 7. For intermediate product-1, intermediate product-2 and intermediate product-3, it is shown that the NCO group has been connected, and the curves of Example 4, Example 6 and Example 7 in the figure show that the synthetic product after the reaction of step (B) has a C=C group. This C=C group is the key to the photocurable printing ink, and the photocuring effect can be achieved after adding a photoinitiator. Therefore, the preparation method of the photocurable printing ink of the present invention is effective and feasible.

[0234] Embodiment 11

[0235] A method for preparing a light-cured 3D printed PU prosthesis comprises the following steps:

[0236] Step (1), collecting CT scan data of the maxillary defect;

[0237] Step (2), obtaining a prosthetic printed model based on the CT scan data obtained in step (1);

[0238] Step (3), using the light-curable PU printing ink prepared in Examples 1 to 10 to perform 3D light-curing printing on the prosthesis printing model to obtain a prosthesis.

[0239] Step (2) includes:

[0240] Step (2.1), import the CT scan data obtained in step (1) into Mimics 21.0 software for three-dimensional reconstruction of the palate defect model, perform Thresholding selection on the CT scan data, delete the frontal sinus, sphenoid sinus or ethmoid sinus cavity structure, and then use the Calculate 3D function to obtain a new mask, perform preliminary smoothing on it, and generate the first upper airway model before repair, the first palate defect animal skull model before repair, and the first palate mucosa model. It should be noted that the CT scan data format of the present invention is Dicom format, and Thresholding is used to adjust and select the threshold of the CT scan data according to the required tissue density. Moreover, because the bone surface and the airway surface are prone to unevenness during the three-dimensional reconstruction process, it will cause the unit quality to be difficult to guarantee during the meshing process. Therefore, the present invention performs appropriate and necessary simplification on the unaffected parts. Specifically, by editing the mask, manually select and delete the suspected frontal sinus, sphenoid sinus, ethmoid sinus and other cavities that have no correlation with this experiment.

[0241] Step (2.2): import the first upper airway model before repair, the first animal skull model of palate defect before repair and the first palate mucosa model obtained in step (2.1) into Geomagic 2017 for smooth optimization and surface filling, and obtain the second upper airway model before repair, the second animal skull model of palate defect before repair and the second palate mucosa model accordingly. It should be noted that the first upper airway model before repair is obtained by setting the threshold range within the gas range, and the first animal skull model of palate defect before repair is obtained by setting the threshold range within the bone density range. The above three models are processed by smooth optimization in Geomagic 2017 by using tools such as "delete features" and "fill holes". This operation will delete the holes left by unnecessary features on the surface and perform surface filling, and obtain the second upper airway model before repair, the second animal skull model of palate defect before repair and the second palate mucosa model accordingly.

[0242] Step (2.3), according to the spatial dimension data of the fistula at the palate defect of the second upper airway initial model before repair obtained in step (2.2), use Solidwork 2017 software to draw the prosthetic shape, and then smooth and optimize the prosthetic shape and fill the surface to obtain a preliminary prosthetic model; then import the second upper airway initial model before repair obtained in step (2.2) and the preliminary prosthetic model into Geomagic 2017 software, align them, and obtain the upper airway model after repair. It should be noted that in this step, tools such as "delete features" and "fill holes" are used to smooth and optimize the second upper airway initial model before repair, and the holes left by deleting unnecessary surface features are filled with the surface.

[0243] Step (2.4), according to the second pre-repair palatal defect animal skull model and the second palatal mucosa model, the edge of the preliminary prosthesis model is adjusted, and then according to the second pre-repair upper airway initial model and the repaired upper airway model, meshing and CFD analysis results are performed to adjust the structure of the prosthesis model to obtain a prosthesis printing model. It should be noted that the present invention needs to import the second pre-repair upper airway initial model and the repaired upper airway model into the Ansys 2021 software to divide the CFD model mesh, in order to improve the similarity and accuracy of the model, and the mesh quality is required to be above 0.35.

[0244] In step (2.4), the edge adjustment is specifically to merge the second animal skull model of the palate defect before repair and the second palate mucosa model into a merged model, and then import the preliminary prosthesis model and the merged model into Geomagic 2017 software, manually register through alignment, fit them, and align them preliminarily, set the mucosa and maxillary models as "test model", set the prosthesis model as "reference model", use the best fit alignment function, assemble the merged model and the prosthesis model, and then adjust the structure of the prosthesis model to make the edges of the prosthesis model and the merged model sealed and aligned. It should be noted that the role of edge alignment is to prevent the edge from being too long, and edge sealing is to prevent edge leakage.

[0245] In step (2.4), data simulation and boundary condition definition are performed on the repaired upper airway model, and the airflow changes in the upper airway before and after the repair in a complete breathing cycle are calculated and simulated. CFD-Post is used to obtain gas flow data under the breathing state: three-dimensional airflow trajectory diagram, pressure cloud diagram, cross-sectional area of ​​each section and airflow velocity cloud diagram, and the prosthesis model is adjusted to obtain the prosthesis printing model.

[0246] The pressure of the repaired upper airway model corresponding to the prosthesis printed model was consistent on the healthy side and the affected side, and there was no abnormal vortex at the fistula.

[0247] The light-cured 3D printed PU prosthesis preparation method of the present invention obtains a personalized prosthesis printing model through reverse design, and finally obtains a real prosthesis. The present invention can reduce the clinical operation difficulty of the impression before prosthesis production, shorten the production time, and the obtained personalized prosthesis can reduce the patient's clinical discomfort and greatly improve the accuracy of the prosthesis.

[0248] Example 12

[0249] A method for preparing a light-cured 3D printed PU prosthesis, such as Figures 5 to 19 , and other features are the same as those of Example 11. This example illustrates the present invention using a palate defect animal model.

[0250] 1. Establishment of animal model of palate defect

[0251] Under general and local anesthesia, the mucosa and hard palate bone plate were cut with a scalpel and a dental turbine ball drill on the right side of the rabbit's upper palate midline to create a fistula connecting the oral cavity and the nasal cavity, which was an ellipse of about 8mm*6mm. The palatal mucosa and the nasal floor mucosa were sutured to construct an animal model of palate defect. After 2 weeks, the fistula was checked, and a CT scan of the rabbit's maxillofacial region was performed to obtain imaging data to confirm that the animal model was successfully established.

[0252] 2. Data simulation and boundary condition definition

[0253] The calculation software of this embodiment is FLUENT 21.0. The calculation domain is from the anterior nares to the pharynx. The pressure field and velocity field are solved. The momentum equation is discretized with second-order accuracy. The medium is air, and the density is ρ = 1.225 kg / m 3 , dynamic viscosity coefficient μ=1.7894×10 -5 kg / m·s.

[0254] Normally, rabbits breathe 20 ml of tidal volume each time, breathe about 46 times a minute, and have a cycle of about 1.3 seconds. This experiment uses an effective ventilation volume of 20 ml and a respiratory frequency of 46 times per minute, that is, a respiratory cycle of 1.3 seconds (t = 1.3s). Generally speaking, the respiratory wave can be regarded as a sine wave, and the ratio of exhalation to inhalation time is 1:1.

[0255] In order to eliminate the influence of boundary effect on the experimental results, the definition of inhalation is: the anterior nares of the upper respiratory tract are the inlet; the lower edge of the throat is set as the outlet. The definition of exhalation is: the positions of the inlet and outlet are set to be reversed, and the inlet and outlet are exactly opposite to those during inhalation; the calculation formula regards the wall of the upper airway as a no-slip boundary (V = 0m / s), and the upper airway as a whole is regarded as an instantaneous rigid body. The internal fluid is regarded as an incompressible fluid with steady flow. During the simulation process, the influence of gravity is considered, and the changes in the temperature field, the cilia on the mucosa, and the influence of the maxillary sinus cavity are ignored. The flow is regarded as steady state. The wall of the upper airway is set as a no-slip boundary (V = 0). This experiment uses the standard k-ε turbulence model to calculate and simulate the changes in the airflow in the upper airway before and after repair in a complete respiratory cycle under the set flow rate.

[0256] It should be noted that for human data simulation and boundary condition definition, general values ​​can be calculated based on existing literature and replaced with these values. The boundary condition refers to setting an exit and an entrance in CFD analysis. The applicant analyzed the effect of palate defects on breathing. When inhaling, the entrance is the two nostrils, and the exit is set to the airway behind the palate defect.

[0257] 3. Gas flow data analysis

[0258] After calculating the transient solution of the corresponding breathing process by computer, CFD-Post is used to obtain the gas flow data under the breathing state: three-dimensional airflow trajectory diagram, pressure cloud diagram, cross-sectional area of ​​each section and airflow velocity cloud diagram.

[0259] The positions of the sections selected in the experiment are as follows: the repaired upper airway model is cut using the section method, and the coordinate axis perpendicular to the section is set as the Y axis. The first section after entering the anterior nares is designated as Section 1, and the section corresponding to the palate defect is designated as Section 2. In addition, three typical sections of the airway model after the defect are selected and set as Sections 3, 4, and 5. A total of five sections are taken for each model. Because the data comes from the same animal model, for the convenience of comparison, the five sections at the same position of the upper airway before and after repair are named Sections 1-5, and are distinguished by marking "Before Repair" and "After Repair", such as Figures 9 to 11 .

[0260] The three-dimensional image of the post-processing result shows the airflow conditions in all areas of the upper airway model before and after prosthetic repair in a color atlas, including: flow rate, pressure, direction, etc. Fig.14 and 15 . Analyze and compare the area and velocity values ​​of each cross section before and after prosthesis repair. When the pressure of the repaired upper airway model corresponding to the prosthesis printing model is inconsistent on the healthy side and the affected side or there is an abnormal vortex at the fistula, adjust the prosthesis model until the pressure on the healthy side and the affected side is consistent and there is no abnormal vortex at the fistula. Figures 16 to 19 , the corresponding pseudo-complex model is the pseudo-complex printing model.

[0261] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a light-cured 3D printed PU prosthesis, characterized in that: The steps include: Step (1), collecting CT scan data of the maxillary defect; Step (2), obtaining a prosthetic printed model based on the CT scan data obtained in step (1); Step (3), using the pre-prepared light-curing PU printing ink to perform 3D light-curing printing on the prosthesis printing model to obtain the prosthesis; The raw materials of light-curable PU printing ink contain polytetramethylene ether glycol PTMEG and isophorone diisocyanate IPDI; Step (2) includes: Step (2.1), importing the CT scan data obtained in step (1) into Mimics 21.0 software to perform three-dimensional reconstruction of the palate defect model, performing Thresholding selection on the CT scan data, deleting the frontal sinus, sphenoid sinus or ethmoid sinus cavity structure, and then using the Calculate 3D function to obtain a new mask, which is preliminarily smoothed to generate the first upper airway model before repair, the first palate defect animal skull model before repair, and the first palate mucosa model; Step (2.2), importing the first upper airway model before repair, the first palate defect animal skull model before repair, and the first palate mucosa model obtained in step (2.1) into Geomagic 2017 for smooth optimization and surface filling, and obtaining the second upper airway model before repair, the second palate defect animal skull model before repair, and the second palate mucosa model accordingly; Step (2.3), according to the spatial dimension data of the fistula at the palate defect of the second upper airway preliminary model before restoration obtained in step (2.2), the prosthesis shape is drawn using Solidwork 2017 software, and then the prosthesis shape is smoothed and optimized and the surface is filled to obtain a preliminary prosthesis model; then the second upper airway preliminary model before restoration obtained in step (2.2) and the preliminary prosthesis model are imported into Geomagic 2017 software for alignment to obtain a repaired upper airway model; Step (2.4), adjusting the edge of the preliminary prosthesis model according to the animal skull model of the palate defect before the second repair and the second palate mucosa model, and then performing meshing and CFD analysis results according to the upper airway initial model before the second repair and the upper airway model after the repair, adjusting the structure of the prosthesis model, and obtaining a prosthesis printing model; In step (2.4), the edge adjustment is specifically to merge the second animal skull model of the palate defect before repair and the second palate mucosa model into a merged model, and then import the preliminary prosthesis model and the merged model into Geomagic 2017 software, manually register them through alignment, fit them, and align them preliminarily. The mucosa and maxillary bone models are set as "test model", and the prosthesis model is set as "reference model". The merged model and the prosthesis model are assembled using the best fit alignment function, and then the structure of the prosthesis model is adjusted to make the edges of the prosthesis model and the merged model sealed and aligned; In step (2.4), the data simulation and boundary condition definition of the repaired upper airway model are performed, and the airflow changes in the upper airway before and after the repair in a complete breathing cycle are calculated and simulated. CFD-Post is used to obtain the gas flow data under the breathing state: three-dimensional airflow trace diagram, pressure cloud diagram, cross-sectional area of ​​each section and airflow velocity cloud diagram, and the prosthesis model is adjusted to obtain the prosthesis printing model; The pressure of the repaired upper airway model corresponding to the prosthesis printed model was consistent on the healthy side and the affected side, and there was no abnormal vortex at the fistula.

2. The method for preparing a light-cured 3D printed PU prosthesis according to claim 1, characterized in that: The raw materials of light-curable PU printing ink also contain hydroxyethyl methacrylate HEMA and dibutyltin dilaurate DBTDL.

3. The method for preparing a light-cured 3D printed PU prosthesis according to claim 1, characterized in that: The molecular weight range of polytetramethylene ether glycol PTMEG is 650-2000.

4. The method for preparing a light-cured 3D printed PU prosthesis according to claim 2, characterized in that: The preparation method of the light-curable PU printing ink is divided into a single molecular weight PU polymer preparation process and a mixing process; The steps for preparing single molecular weight PU polymer are: Step (A), adding isophorone diisocyanate IPDI and dibutyltin dilaurate DBTDL into a reaction container, and then adding a tetrahydrofuran solution of polytetramethylene ether glycol PTMEG of a single molecular weight into the reaction container, and stirring; Step (B), adding hydroxyethyl methacrylate (HEMA) into a reaction container to obtain a PU solution; Step (C), extracting the PU solution obtained in step (B) by layering and extracting to obtain an extract; Step (D), vacuum drying the extract obtained in step (C) to obtain a PU polymer; The mixing process is to mix polyurethane elastomer, isooctyl acrylate, isobornyl acrylate and phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide to obtain a light-curable PU printing ink; The polyurethane elastomer is composed of at least one PU polymer obtained in step (D) with a molecular weight of 1.

5. The method for preparing a light-cured 3D printed PU prosthesis according to claim 3, characterized in that: Step (A) is specifically to heat isophorone diisocyanate IPDI and dibutyltin dilaurate DBTDL to 65°C to 72°C, then add a tetrahydrofuran solution of single molecular weight polytetramethylene ether glycol PTMEG into a reaction container, heat to 65°C to 72°C and stir for 2h to 4h; Step (B) specifically comprises adding hydroxyethyl methacrylate HEMA into a reaction container, and stirring at a temperature of 65° C. to 72° C. for 2 h to 4 h to obtain a PU solution.

6. The method for preparing a light-cured 3D printed PU prosthesis according to claim 4, characterized in that: In the single molecular weight PU polymer preparation process, the raw material ratio is calculated by molar ratio: Polytetramethylene ether glycol PTMEG: 0.01~0.03; Isophorone diisocyanate IPDI: 0.02~0.06; Hydroxyethyl methacrylate HEMA: 0.02~0.06; Dibutyltin dilaurate DBTDL: 0.0010~0.0020; In the mixing process, the weight ratio of polyurethane elastomer, isooctyl acrylate and isobornyl acrylate is 4-8:1-3:1-3, and the weight of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide is 1%-3% of the total weight of polyurethane elastomer, isooctyl acrylate and isobornyl acrylate; The volume concentration of the tetrahydrofuran solution of single molecular weight polytetramethylene ether glycol PTMEG is 10% to 30%; The extracting liquid in step (C) is petroleum ether, and the volume ratio of petroleum ether to PU solution is 5:1 to 15:

1.

7. The method for preparing a light-cured 3D printed PU prosthesis according to claim 4, characterized in that: In the single molecular weight PU polymer preparation process, the raw material ratio is calculated by molar ratio: Polytetramethylene ether glycol PTMEG: 0.02; Isophorone diisocyanate IPDI: 0.04; Hydroxyethyl methacrylate HEMA: 0.04; Dibutyltin dilaurate DBTDL: 0.0015; In the mixing process, the weight ratio of polyurethane elastomer, isooctyl acrylate and isobornyl acrylate is 6:2:2, and the weight of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide is 2% of the total weight of polyurethane elastomer, isooctyl acrylate and isobornyl acrylate; The polyurethane elastomer is composed of 1000PU polymer, or the polyurethane elastomer is composed of at least two of 650PU polymer, 1000PU polymer and 2000PU polymer; 1000PU polymer is a single molecular weight PU polymer prepared from polytetramethylene ether glycol PTMEG having a molecular weight of 1000; 650PU polymer is a single molecular weight PU polymer prepared from polytetramethylene ether glycol PTMEG having a molecular weight of 650; 2000PU polymer is a single molecular weight PU polymer prepared from polytetramethylene ether glycol PTMEG with a molecular weight of 2000; The volume concentration of the tetrahydrofuran solution of single molecular weight polytetramethylene ether glycol PTMEG is 20%; The extracting liquid in step (C) is petroleum ether, and the volume ratio of petroleum ether to PU solution is 10:1.