An electrolyte and its preparation method and application
By adding low-impedance additives and boron-containing compounds to the bis(fluorosulfonyl)imide lithium-based electrolyte, the problem of decreased electrolyte thermal stability was solved, and the high-temperature cycle stability and low-temperature discharge performance of the battery were improved, specifically manifested in a significant improvement in capacity retention and storage performance.
Patent Information
- Application Number
- CN202310150133.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-02-22
AI Technical Summary
When certain additives are added to existing high thermal stability bis(fluorosulfonyl)imide lithium-based electrolytes, the thermal stability decreases significantly, affecting electrolyte storage and battery performance, and limiting its application in battery cycling and high/low temperature performance.
Low-impedance additives and boron-containing compounds are added to bis(fluorosulfonyl)imide lithium-based electrolytes to optimize electrolyte composition and improve thermal stability and cycle performance. Specific additives include fluoroethylene carbonate, tris(trimethylsilane) phosphate, and boron-containing compounds such as benzylamine boron trifluoride complex.
It improves the battery's high-temperature cycle stability, high-temperature storage performance, and low-temperature discharge performance. The capacity retention rate is over 86% after 1500 cycles at 45℃, the capacity recovery rate is over 88% after 90 days of storage at 60℃, and the discharge capacity retention rate is over 66% at -20℃.
Smart Images

Figure BDA0004090471410000081 
Figure BDA0004090471410000091
Abstract
Description
Technical Field
[0001] The invention belongs to the field of lithium ion batteries and relates to an electrolyte and a preparation method and application thereof. Background Art
[0002] As the requirements for long cycles and high and low temperature performance of power batteries are increasing, electrode materials are undergoing technological upgrades. However, the matching electrolyte technology also needs to adapt to it. The successful application of high thermal stability lithium bis(fluorosulfonyl)imide has helped the battery to achieve excellent electrical and safety performance. However, in order to achieve both high and low temperature performance, when certain additives are added to the current high thermal stability lithium bis(fluorosulfonyl)imide-based electrolyte, there is a problem of significantly reduced thermal stability, which causes certain difficulties for electrolyte storage and battery performance.
[0003] Lithium bis(fluorosulfonyl)imide as the main salt electrolyte will become a development trend in the future. Its own thermal stability is better than that of lithium hexafluorophosphate, but when combined with certain unstable additives, its thermal stability will be lower than that of lithium hexafluorophosphate electrolyte. This greatly limits the application of lithium bis(fluorosulfonyl)imide as a high thermal stability lithium salt to improve battery cycle and high and low temperature performance.
[0004] CN113782833A discloses an electrolyte and its preparation method and application. The lithium salt is lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide, and the additives are phenyl vinyl sulfone and tri(2,2,2-trifluoroethyl) borate. CN109301324A discloses a high energy density lithium ion battery electrolyte, wherein the lithium salt includes lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide and lithium difluoroborate sulfate, and a lithium salt additive is used in combination. The additives added in the above two patents will affect the thermal stability of the lithium bis(fluorosulfonyl)imide electrolyte, causing certain difficulties for the storage of the electrolyte and the performance of the battery.
[0005] Therefore, how to improve the thermal stability and cycle performance of bis(fluorosulfonyl)imide lithium-based electrolytes is an important research direction in this field. Summary of the invention
[0006] In view of the deficiencies in the prior art, the present invention aims to provide an electrolyte and a preparation method and application thereof.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] One of the purposes of the present invention is to provide an electrolyte, the electrolyte comprising an additive and a lithium salt, the additive comprising a low impedance additive and a boron-containing compound, and the lithium salt comprising lithium bis(fluorosulfonyl)imide.
[0009] The present invention adds a low-impedance additive and a boron-containing compound to a bisfluorosulfonyl imide lithium-based electrolyte to improve the thermal stability and cycle performance of the electrolyte. When the low-impedance additive is added, the cycle performance of the battery is improved, but the problem of decreased thermal stability of the electrolyte is caused. The stability additive boron-containing compound is added to improve the thermal stability of the electrolyte. A lithium ion battery prepared by using the bisfluorosulfonyl imide lithium-based electrolyte, the low-impedance additive and the electrolyte containing the boron compound has excellent high-temperature cycle stability, high-temperature storage performance and low-temperature discharge performance compared with a traditional lithium hexafluorophosphate electrolyte.
[0010] As a preferred technical solution of the present invention, the low-impedance additive includes any one of fluoroethylene carbonate, tris(trimethylsilyl)phosphate or vinyl sulfate, or a combination of at least two of them, wherein typical but non-limiting examples of the combination include: a combination of fluoroethylene carbonate and tris(trimethylsilyl)phosphate, a combination of tris(trimethylsilyl)phosphate and vinyl sulfate, or a combination of fluoroethylene carbonate and vinyl sulfate, etc.
[0011] Preferably, in the electrolyte, the mass fraction of the low-impedance additive is 1.5-10%, wherein the mass fraction can be 1.5%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0012] As a preferred technical solution of the present invention, the boron-containing compound includes any one of benzylamine boron trifluoride complex, pyridine boron trifluoride, 2-methylpyridine-3-boric acid pinacol ester, boron trifluoride butyl acetate or 3-methyl-5-cyano-phenylboric acid pinacol ester, or a combination of at least two of them, wherein typical but non-limiting examples of the combination include: a combination of benzylamine boron trifluoride complex and pyridine boron trifluoride, a combination of pyridine boron trifluoride and 2-methylpyridine-3-boric acid pinacol ester, a combination of 2-methylpyridine-3-boric acid pinacol ester and boron trifluoride butyl acetate, or a combination of boron trifluoride butyl acetate and 3-methyl-5-cyano-phenylboric acid pinacol ester, etc.
[0013] Preferably, in the electrolyte, the mass fraction of the boron-containing compound is 0.1-1%, wherein the mass fraction can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0014] As a preferred technical solution of the present invention, the concentration of the lithium bis(fluorosulfonyl)imide in the electrolyte is 0.5 to 1.0 mol / L, wherein the concentration may be 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L or 1.0 mol / L, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0015] Preferably, the lithium salt further includes lithium hexafluorophosphate.
[0016] Preferably, the concentration of the lithium salt in the electrolyte is 0.8 to 1.2 mol / L, wherein the concentration may be 0.8 mol / L, 0.9 mol / L, 1.0 mol / L, 1.1 mol / L or 1.2 mol / L, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0017] As a preferred technical solution of the present invention, the electrolyte also includes an organic solvent.
[0018] Preferably, the organic solvent includes a cyclic carbonate solvent and a linear carbonate solvent.
[0019] As a preferred technical solution of the present invention, the cyclic carbonate solvent includes ethylene carbonate.
[0020] Preferably, based on the volume of the organic solvent as 100%, the volume fraction of the cyclic carbonate solvent is 20-40%, wherein the volume fraction can be 20%, 22%, 24%, 26%, 28%, 30%, 32%, 34%, 36%, 38% or 40%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0021] Preferably, the linear carbonate solvent comprises any one of dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate or methyl propyl carbonate, or a combination of at least two thereof, wherein typical but non-limiting examples of the combination include: a combination of dimethyl carbonate and ethyl methyl carbonate, a combination of ethyl methyl carbonate and diethyl carbonate, or a combination of diethyl carbonate and methyl propyl carbonate, etc.
[0022] Preferably, based on the volume of the organic solvent as 100%, the volume fraction of the linear carbonate solvent is 60-80%, wherein the volume fraction can be 60%, 62%, 64%, 68%, 70%, 72%, 74%, 76%, 78% or 80%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0023] A second object of the present invention is to provide a method for preparing the electrolyte as described in the first object, the preparation method comprising:
[0024] The electrolyte is obtained by adding lithium salt into an organic solvent and mixing, and then adding additives.
[0025] As a preferred technical solution of the present invention, the organic solvent includes a cyclic carbonate solvent and a linear carbonate solvent.
[0026] Preferably, the cyclic carbonate solvent and the linear carbonate solvent are mixed, and then purified to remove impurities and water to obtain an organic solvent.
[0027] The purification and impurity removal in the present invention uses any one of molecular sieves, calcium hydride or lithium hydride or a combination of at least two of them to perform purification and impurity removal.
[0028] Preferably, the mixing temperature is 15-30°C, wherein the temperature can be 15°C, 16°C, 17°C, 18°C, 19°C, 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C or 30°C, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0029] A third object of the present invention is to provide a lithium-ion battery, which comprises a positive electrode sheet, a negative electrode sheet and the electrolyte as described in one of the objects.
[0030] As a preferred technical solution of the present invention, the active material of the positive electrode sheet includes lithium iron phosphate.
[0031] Preferably, the active material of the negative electrode sheet includes graphite.
[0032] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] The electrolyte prepared by the present invention is used in 2.5-3.65V lithium iron phosphate / graphite system batteries, and the capacity retention rate after 1500 cycles at 45°C can be as high as over 86%, the capacity recovery rate after 90d storage at 60°C can be as high as over 88%, and the discharge capacity retention rate at -20°C can be as high as over 66%. DETAILED DESCRIPTION
[0035] The technical solution of the present invention is further illustrated below through specific implementation methods.
[0036] Example 1
[0037] This embodiment provides an electrolyte, which includes an organic solvent, a lithium salt and an additive.
[0038] Among them, the organic solvent includes ethylene carbonate and ethyl methyl carbonate in a volume ratio of 3:7, the lithium salt includes lithium bis(fluorosulfonyl)imide and lithium hexafluorophosphate in a concentration of 0.7 mol / L in the electrolyte, and the additives include 1.0% of vinyl sulfate, 0.5% of tris(trimethylsilyl) phosphate and 0.2% of pyridine boron trifluoride in a mass fraction in the electrolyte.
[0039] This embodiment also provides a method for preparing the above electrolyte, the preparation method comprising:
[0040] Cyclic carbonate solvent ethylene carbonate and linear carbonate solvent methyl ethyl carbonate are mixed in a volume ratio of ethylene carbonate: methyl ethyl carbonate = 3:7, and purified by molecular sieve, calcium hydride and lithium hydride to remove impurities and water to obtain an organic solvent. Under room temperature, conductive lithium salts lithium bis(fluorosulfonyl)imide and lithium hexafluorophosphate are dissolved in the organic solvent, wherein the concentration of lithium bis(fluorosulfonyl)imide is 0.7 mol / L, and the concentration of lithium hexafluorophosphate is 0.3 mol / L. After stirring evenly, low-impedance additives of 1.0% vinyl sulfate and 0.5% tris(trimethylsilyl)phosphate are added to the electrolyte by mass fraction, and a boron-containing compound of 0.2% pyridine boron trifluoride is further added to the electrolyte by mass fraction to obtain a high thermal stability lithium bis(fluorosulfonyl)imide electrolyte for lithium ion batteries.
[0041] The electrolyte prepared in this example is applied to 2.5-3.65V lithium iron phosphate / graphite system lithium ion batteries.
[0042] Example 2
[0043] This embodiment provides an electrolyte, which includes an organic solvent, a lithium salt and an additive.
[0044] Among them, the organic solvent includes ethylene carbonate and diethyl carbonate in a volume ratio of 4:6, the lithium salt includes lithium bis(fluorosulfonyl)imide and lithium hexafluorophosphate in a concentration of 0.5 mol / L in the electrolyte, and the additives include 1.0% of vinyl sulfate, 1.0% of fluoroethylene carbonate and 0.5% of boron trifluoride butyl acetate in a mass fraction in the electrolyte.
[0045] This embodiment also provides a method for preparing the above electrolyte, the preparation method comprising:
[0046] Cyclic carbonate solvent ethylene carbonate and linear carbonate solvent diethyl carbonate are mixed in a volume ratio of ethylene carbonate:ethyl methyl carbonate=4:6, and purified by molecular sieve, calcium hydride and lithium hydride to remove impurities and water, so as to obtain an organic solvent. Under room temperature, conductive lithium salts lithium bis(fluorosulfonyl)imide and lithium hexafluorophosphate are dissolved in the organic solvent, wherein the concentration of lithium bis(fluorosulfonyl)imide is 0.5 mol / L, and the concentration of lithium hexafluorophosphate is 0.5 mol / L. After stirring evenly, low-impedance additives of 1.0% vinyl sulfate and 1.0% fluoroethylene carbonate are added to the electrolyte by mass fraction, and a boron-containing compound of 0.5% boron trifluoride butyl acetate is further added to the electrolyte by mass fraction, so as to obtain a high thermal stability lithium bis(fluorosulfonyl)imide electrolyte for lithium ion batteries.
[0047] The electrolyte prepared in this example is applied to 2.5-3.65V lithium iron phosphate / graphite system lithium ion batteries.
[0048] Example 3
[0049] This embodiment provides an electrolyte, which includes an organic solvent, a lithium salt and an additive.
[0050] Among them, the organic solvent includes ethylene carbonate and ethyl methyl carbonate in a volume ratio of 2:8, the lithium salt includes lithium bis(fluorosulfonyl)imide with a concentration of 1.0 mol / L in the electrolyte, and the additives include 1.0% of vinyl sulfate, 0.5% of tris(trimethylsilyl) phosphate, 0.5% of fluoroethylene carbonate and 1% of 2-methylpyridine-3-boric acid pinacol ester in the electrolyte.
[0051] This embodiment also provides a method for preparing the above electrolyte, the preparation method comprising:
[0052] Cyclic carbonate solvent ethylene carbonate and linear carbonate solvent methyl ethyl carbonate are mixed in a volume ratio of ethylene carbonate: methyl ethyl carbonate = 2:8, and purified by molecular sieve, calcium hydride and lithium hydride to remove impurities and water to obtain an organic solvent. Under room temperature, a conductive lithium salt lithium bis(fluorosulfonyl)imide is dissolved in the organic solvent, wherein the concentration of the lithium bis(fluorosulfonyl)imide is 1.0 mol / L. After stirring evenly, a low-impedance additive of 1.0% vinyl sulfate, 0.5% fluoroethylene carbonate and 0.5% tris(trimethylsilyl)phosphate is added to the electrolyte by mass fraction, and a boron-containing compound of 2-methylpyridine-3-boric acid pinacol ester is further added to the electrolyte by mass fraction to obtain a high thermal stability lithium bis(fluorosulfonyl)imide electrolyte for lithium ion batteries.
[0053] The electrolyte prepared in this example is applied to 2.5-3.65V lithium iron phosphate / graphite system lithium ion batteries.
[0054] Example 4
[0055] Except that vinyl sulfate was not added, other conditions in this example were the same as those in Example 1.
[0056] Example 5
[0057] In this embodiment, except that the mass fraction of pyridine boron trifluoride in the electrolyte is replaced with 1.2%, other conditions are the same as those in Embodiment 1.
[0058] Example 6
[0059] In this embodiment, except that only ethylene carbonate is used as the organic solvent, other conditions are the same as those in embodiment 1.
[0060] Example 7
[0061] In this embodiment, except that the concentration of lithium bis(fluorosulfonyl)imide in the electrolyte is replaced with 0.3 mol / L, other conditions are the same as those in Embodiment 1.
[0062] Comparative Example 1
[0063] In this comparative example, except that pyridine boron trifluoride is not used, other conditions are the same as those in Example 1.
[0064] Comparative Example 2
[0065] In this comparative example, except that lithium bis(fluorosulfonyl)imide was not used as the lithium salt, and lithium hexafluorophosphate with a concentration of 1.0 mol / L in the electrolyte was used, other conditions were the same as those in Example 1.
[0066] The lithium ion batteries prepared in Examples 1-7 and Comparative Examples 1-2 were subjected to electrolyte thermal stability evaluation and battery performance testing. The test results are shown in Tables 1 and 2.
[0067] Among them, the method for evaluating the thermal stability of the electrolyte includes DSC; the method for testing the battery performance includes cycle and storage tests.
[0068] Table 1
[0069]
[0070] Table 2
[0071]
[0072] The above table shows that the low impedance additive and the boron-containing compound can be used together to improve the thermal stability and cycle performance of the electrolyte. In Example 4, no vinyl sulfate is added, and the cycle performance and thermal stability of the battery are significantly reduced. In Example 5, the amount of pyridine boron trifluoride added is too much, and the cycle performance and thermal stability of the battery are significantly reduced. In Example 6, only vinyl carbonate is used as the organic solvent, and the cycle performance and thermal stability of the battery are significantly reduced. In Example 7, the concentration of lithium bis(fluorosulfonyl)imide is too low, and the cycle performance and thermal stability of the battery are significantly reduced.
[0073] In Comparative Example 1, pyridine boron trifluoride is not used, and the cycle performance and thermal stability of the battery are significantly reduced. In Comparative Example 2, only lithium hexafluorophosphate is used as the lithium salt, and lithium bis(fluorosulfonyl)imide is not used, and the cycle performance and thermal stability of the battery are significantly reduced.
[0074] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. An electrolyte, characterized in that: The electrolyte includes an additive and a lithium salt, wherein the additive includes a low impedance additive and a boron-containing compound, and the lithium salt includes lithium bis(fluorosulfonyl)imide with a concentration of 0.5 to 1.0 mol / L; In the electrolyte, the mass fraction of the low-impedance additive is 1.5 to 10%; In the electrolyte, the mass fraction of the boron-containing compound is 0.1 to 1%; The low impedance additive is any one of fluoroethylene carbonate, tris(trimethylsilyl)phosphate or vinyl sulfate, or a combination of at least two thereof; The boron-containing compound is any one of benzylamine boron trifluoride complex, pyridine boron trifluoride, 2-methylpyridine-3-boric acid pinacol ester, boron trifluoride butyl acetate or 3-methyl-5-cyano-phenylboric acid pinacol ester or a combination of at least two thereof.
2. The electrolyte according to claim 1, characterized in that The lithium salt also includes lithium hexafluorophosphate.
3. The electrolyte according to claim 1, characterized in that The concentration of the lithium salt in the electrolyte is 0.8 to 1.2 mol / L.
4. The electrolyte according to claim 1, characterized in that The electrolyte also includes an organic solvent.
5. The electrolyte according to claim 4, characterized in that The organic solvent includes a cyclic carbonate solvent and a linear carbonate solvent.
6. The electrolyte according to claim 5, characterized in that The cyclic carbonate solvent includes ethylene carbonate.
7. The electrolyte according to claim 5, characterized in that Based on the volume of the organic solvent being 100%, the volume fraction of the cyclic carbonate solvent is 20-40%.
8. The electrolyte according to claim 5, characterized in that The linear carbonate solvent includes any one of dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate or methyl propyl carbonate, or a combination of at least two thereof.
9. The electrolyte according to claim 5, characterized in that Based on the volume of the organic solvent being 100%, the volume fraction of the linear carbonate solvent is 60-80%.
10. A method for preparing an electrolyte according to any one of claims 1 to 9, characterized in that: The preparation method comprises: The electrolyte is obtained by adding lithium salt into an organic solvent and mixing, and then adding additives.
11. The preparation method according to claim 10, characterized in that: The organic solvent includes a cyclic carbonate solvent and a linear carbonate solvent.
12. The preparation method according to claim 11, characterized in that: The cyclic carbonate solvent and the linear carbonate solvent are mixed, and then purified to remove impurities and water to obtain an organic solvent.
13. The preparation method according to claim 10, characterized in that: The mixing temperature is 15-30°C.
14. A lithium ion battery, characterized in that: The lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet and the electrolyte according to any one of claims 1 to 9.
15. The lithium ion battery according to claim 14, characterized in that: The active material of the positive electrode sheet includes lithium iron phosphate.
16. The lithium ion battery according to claim 15, characterized in that: The active material of the negative electrode sheet includes graphite.