An aqueous electrolyte for inhibiting zinc dendrites and a zinc-ion battery
By introducing indium chloride as an additive into aqueous zinc-ion batteries, a dynamic electrostatic shielding layer is formed, which solves the problem of battery life degradation caused by zinc dendrite growth and achieves improved cycle stability and coulombic efficiency of high-efficiency, low-cost zinc-ion batteries.
Patent Information
- Application Number
- CN202211563056.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-06
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-12-06
AI Technical Summary
In existing aqueous zinc-ion batteries, zinc dendrite growth leads to a decline in battery cycle life, polymer additives have weak bonding force, and metal ion additives are prone to side reactions and are costly.
An aqueous zinc-ion battery electrolyte containing indium chloride additive is used. By forming a dynamic electrostatic shielding layer on the surface of the zinc anode, uniform zinc ion deposition is induced, and dendrite growth is inhibited.
It significantly improves the cycle stability and coulombic efficiency of zinc metal electrodes, extends service life, reduces polarization voltage, and lowers costs.
Smart Images

Figure CN116259860B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of aqueous zinc-ion battery technology, and particularly relates to an aqueous electrolyte and zinc-ion battery that inhibit zinc dendrite formation. Background Technology
[0002] To achieve my country's strategic goal of "peak carbon and carbon neutrality," developing large-scale power storage systems to store electricity converted from new energy sources such as solar, wind, and tidal energy has become an effective approach. Commercially available lithium-ion batteries, due to their high energy density, flexibility, and scalability, have become one of the solutions for large-scale power storage; however, the scarcity of lithium and its increasing cost limit their large-scale application. In contrast, aqueous zinc-ion batteries have a high theoretical capacity (5854 mAh / cm³). -3 With its advantages such as high hydrogen evolution overpotential (1.2V vs. SHE), low cost, and high safety, it is gradually becoming a research hotspot in the field of large-scale power energy storage.
[0003] However, during charging and discharging, zinc metal anodes exhibit uncontrollable zinc ion deposition / dissolution on their surface, leading to the growth and deterioration of dendritic crystals, which severely reduces the battery's cycle life. Zinc dendrites, once they reach a certain size, will detach and form dead zinc, resulting in the loss of active material, low coulombic efficiency, and even puncture of the separator, causing internal short circuits. This significantly hinders the commercialization of aqueous zinc-ion batteries.
[0004] To address the problem of zinc dendrite growth and deterioration, introducing additives into the electrolyte is considered the simplest and most economical strategy. Electrolyte additives are mainly divided into two types: polymer additives and metal ion additives. Both types can adsorb onto the zinc anode surface, optimizing zinc ion deposition to inhibit dendrite growth. However, polymer additives have weaker adsorption and binding forces, while metal ion additives are prone to various side reactions. In addition, some additives can inhibit dendrite growth by optimizing the solvation structure of the electrolyte, but these additives require larger quantities and are more expensive. Therefore, there is an urgent need to develop a new additive to optimize the formulation of zinc-ion battery electrolytes, thereby controlling the zinc ion deposition / dissolution behavior and inhibiting the growth and deterioration of zinc dendrites.
[0005] Based on the above analysis, the existing technologies have the following problems and shortcomings: the polymer additives have weak adsorption and binding forces, and cannot be adsorbed on the zinc anode surface for a long time to inhibit the growth of zinc dendrites; metal ion additives are prone to various side reactions with the zinc anode, leading to accelerated corrosion of the zinc anode. In addition, some additives can inhibit dendrite growth by optimizing the solvation structure of the electrolyte, but these additives require large quantities and are costly, which cannot meet the low-cost requirement of zinc-ion batteries. Summary of the Invention
[0006] To address the thorny problem of zinc dendrite growth in the zinc metal anode during charge and discharge, which leads to a severe reduction in the cycle life of aqueous zinc-ion batteries, the primary objective of this invention is to provide an aqueous zinc-ion battery electrolyte containing indium chloride additive, which induces uniform deposition / dissolution of zinc ions, reduces polarization voltage, and inhibits the growth and deterioration of zinc dendrites.
[0007] To achieve the above objectives, the present invention adopts the following technical solution: an aqueous zinc-ion battery electrolyte containing indium chloride additive, the electrolyte being composed of additive, soluble zinc salt and deionized water; the additive is indium chloride, whose chemical formula is InCl3; the soluble zinc salt is zinc sulfate, whose chemical formula is ZnSO4·7H2O.
[0008] Furthermore, the concentration of zinc sulfate is 1–2 mol / L. -1 .
[0009] Furthermore, the concentration of indium chloride is 0.01–0.1 mol / L. -1 .
[0010] Furthermore, the pH value of the electrolyte is 4 to 6.
[0011] Furthermore, the indium chloride-containing electrolyte can form a dynamic electrostatic shielding layer on the zinc anode surface, inducing uniform deposition / dissolution of zinc ions, inhibiting dendrite growth and deterioration, and protecting zinc metal.
[0012] Another objective of this invention is to provide an aqueous zinc-ion battery constructed by the method for constructing an aqueous zinc-ion battery, wherein the battery comprises an electrolyte, a positive electrode, a negative electrode, and a separator, wherein the electrolyte is an aqueous zinc-ion battery electrolyte containing indium chloride additive, the positive electrode material is manganese dioxide, the negative electrode material is metallic zinc, and the separator is a glass fiber membrane.
[0013] Furthermore, the preparation method of the manganese dioxide positive electrode sheet is as follows:
[0014] 2.82 g of manganese acetate and 2.63 g of ammonium persulfate were weighed and dissolved in deionized water. The mixture was stirred until the aqueous solution turned pale yellow. This solution was transferred to a 100 mL reaction vessel and then hydrothermally reacted at 140 °C for 24 h. The reaction vessel was then allowed to cool naturally to room temperature. The sample was then collected by centrifugation and washed three times each with distilled water and anhydrous ethanol. The resulting product was dried at 80 °C for 12 h to obtain manganese dioxide powder.
[0015] Manganese dioxide, acetylene black, and polyvinylidene fluoride are mixed in a certain mass ratio, and N-methylpyrrolidone is added to make the three into a paste. The paste is repeatedly rolled into a thin sheet and pressed onto a cut stainless steel mesh to make an electrode sheet. Then, it is dried in a vacuum drying oven for 24 hours to obtain the manganese dioxide positive electrode sheet.
[0016] Furthermore, the preparation method of the zinc negative electrode sheet is as follows:
[0017] The zinc foil is cut to a suitable size, then cleaned with dilute sulfuric acid and deionized water, and finally vacuum dried at room temperature for 24 hours in a vacuum drying oven at 80°C to obtain the negative electrode sheet.
[0018] Furthermore, the assembly method for aqueous zinc-ion batteries is as follows:
[0019] An aqueous zinc-ion battery was assembled in a CR2032 coin cell casing. The assembly sequence was as follows: positive electrode casing, manganese dioxide positive electrode sheet, glass fiber separator, aqueous electrolyte, zinc negative electrode sheet, gasket, spring sheet, and negative electrode casing. The assembled battery was then placed on a coin cell sealing machine and sealed under pressure. After standing at room temperature for 10 hours, electrochemical performance tests were performed.
[0020] Based on the above technical solutions and the technical problems solved, the advantages and positive effects of the technical solution to be protected by this invention are as follows:
[0021] First, addressing the technical problems existing in the prior art and the difficulty in solving them, this paper closely analyzes, in conjunction with the technical solution to be protected by this invention and the results and data obtained during the research and development process, how the technical solution of this invention solves the technical problems, and the inventive technical effects brought about by solving these problems. The specific description is as follows:
[0022] (1) This invention introduces trace amounts of indium chloride additive into the aqueous electrolyte. 3+ In preferentially adsorbs onto the zinc anode surface due to the unique electrostatic shielding effect of rare earth metals. 3+ A dynamic electrostatic shielding layer is formed on the surface of the zinc anode, which reduces the polarization voltage, induces uniform deposition / dissolution of zinc ions, achieves dense metallic zinc deposition, inhibits the growth of zinc dendrites, and enables the zinc metal electrode to cycle stably for 3000 hours. This plays an important role in improving the cycle stability of aqueous zinc-ion batteries.
[0023] (2) This invention proposes a method for regulating zinc deposition behavior using indium chloride as an electrolyte additive. The process is simple, the raw materials are readily available, and the cost is low. Adding a trace amount of indium chloride to an aqueous electrolyte can reduce the polarization voltage and increase the coulombic efficiency of the battery to over 98%. When combined with low-cost, high-capacity manganese dioxide cathode materials, this method helps to develop aqueous zinc-ion batteries with high energy density and long cycle life, thus promoting their industrialization.
[0024] Second, considering the technical solution as a whole or from a product perspective, the technical effects and advantages of the technical solution to be protected by this invention are specifically described as follows:
[0025] This invention provides an aqueous zinc-ion battery electrolyte containing indium chloride as an additive. By adding a trace amount of indium chloride to existing aqueous electrolytes, zinc dendrite growth can be significantly inhibited, thus improving the lifespan of the zinc metal anode. This method has the advantages of simple preparation process, low cost, and easy industrialization. Due to the unique electrostatic shielding effect of rare earth metals, In... 3+ A dynamic electrostatic shielding layer can be formed on the surface of the zinc anode, reducing the polarization voltage and inducing uniform deposition / dissolution of zinc ions, thereby achieving dense metallic zinc deposition.
[0026] Third, as supplementary evidence of the inventive step of the claims of this invention, it is also reflected in the following important aspects:
[0027] Does the technical solution of this invention overcome technical bias?
[0028] Existing polymer additives have weak adsorption and binding forces, making it impossible to control zinc dendrite growth over long periods; metal ion additives are prone to various side reactions with the zinc anode, leading to accelerated corrosion of the zinc anode. The electrolyte additive in this invention has strong adsorption and binding forces, which can inhibit dendrite growth over long periods and prevent various side reactions with the zinc anode, significantly improving the cycle life of the zinc anode and overcoming previous technological limitations. Attached Figure Description
[0029] Figure 1 This is a schematic diagram illustrating the mechanism of action of the indium chloride additive and the morphology of the zinc deposition layer provided in this embodiment of the invention.
[0030] Figure 2 This is the AC impedance spectrum of a zinc symmetric battery assembled using pure zinc sulfate electrolyte (a) and target electrolyte (b) according to an embodiment of the present invention;
[0031] Figure 3 The zinc symmetric battery assembled using pure zinc sulfate electrolyte (a) and target electrolyte (b) according to the embodiments of the present invention operates at 1 mA cm⁻¹. -2 Time-voltage curves at current density;
[0032] Figure 4 This is provided by the embodiments of the present invention. Figure 2 (b) Local time-voltage curves from 2998 to 3000 h;
[0033] Figure 5 These are scanning electron microscope images of the zinc electrode surface after 300h and 3000h cycles, respectively, of the zinc symmetric battery assembled using pure zinc sulfate electrolyte (a) and target electrolyte (b) provided in the embodiments of the present invention.
[0034] Figure 6 This is an X-ray diffraction pattern of manganese dioxide preparation provided in an embodiment of the present invention;
[0035] Figure 7 This is a scanning electron microscope image of the preparation of manganese dioxide provided in the embodiments of the present invention;
[0036] Figure 8 The zinc-ion battery assembled using pure zinc sulfate electrolyte (a) and target electrolyte (b) according to the embodiments of the present invention operates at 0.1 A g. -1 Cyclic curves at current density. Detailed Implementation
[0037] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0038] To enable those skilled in the art to fully understand how the present invention is specifically implemented, this section provides an explanatory description of the embodiments that expand upon the technical solutions of the claims.
[0039] This invention provides an aqueous zinc-ion battery electrolyte containing indium chloride as an additive. The electrolyte is composed of the additive, a soluble zinc salt, and deionized water. The additive is indium chloride, and the soluble zinc salt is zinc sulfate.
[0040] The concentration of zinc sulfate is 1–2 mol / L. -1 .
[0041] The concentration of indium chloride is 0.01–0.1 mol / L. -1 .
[0042] The electrolyte has a pH value of 4 to 6.
[0043] This invention provides a method for constructing an aqueous zinc-ion battery. The aqueous zinc-ion battery is constructed using the electrolyte, which can form a dynamic electrostatic shielding layer on the surface of the zinc anode, induce uniform deposition of zinc ions, inhibit dendrite growth and deterioration, and protect the zinc metal anode.
[0044] The preparation method of manganese dioxide positive electrode sheet is as follows:
[0045] 2.82 g of manganese acetate and 2.63 g of ammonium persulfate were weighed and dissolved in deionized water. The mixture was stirred until the aqueous solution turned pale yellow. This solution was transferred to a 100 mL reaction vessel and then hydrothermally reacted at 140 °C for 24 h. The reaction vessel was then allowed to cool naturally to room temperature. The sample was then collected by centrifugation and washed three times each with distilled water and anhydrous ethanol. The resulting product was dried at 80 °C for 12 h to obtain manganese dioxide powder.
[0046] Manganese dioxide, acetylene black, and polyvinylidene fluoride are mixed in a certain mass ratio, and N-methylpyrrolidone is added to make the three into a paste. The paste is repeatedly rolled into a thin sheet and pressed onto a cut stainless steel mesh to make an electrode sheet. Then, it is dried in a vacuum drying oven for 24 hours to obtain the manganese dioxide positive electrode sheet.
[0047] The preparation method of the zinc negative electrode sheet is as follows:
[0048] The zinc foil is cut to a suitable size, then cleaned with dilute sulfuric acid and deionized water, and finally vacuum dried at room temperature for 24 hours in a vacuum drying oven at 80°C to obtain the negative electrode sheet.
[0049] The assembly method for aqueous zinc-ion batteries is as follows:
[0050] Assemble an aqueous zinc-ion battery in a CR2032 coin cell mold. The assembly sequence is as follows: positive electrode shell, manganese dioxide positive electrode sheet, glass fiber separator, aqueous electrolyte, zinc negative electrode sheet, gasket, spring sheet, and negative electrode shell. Place the assembled battery on a coin cell sealing machine for pressure sealing, and allow it to stand at room temperature for 10 hours before electrochemical performance testing.
[0051] To demonstrate the inventiveness and technical value of the technical solution of this invention, this section provides specific product or related technology application examples of the technical solution claimed.
[0052] This invention applies the method for constructing an aqueous zinc-ion battery to the construction of an aqueous zinc-ion battery, wherein the battery is composed of an electrolyte, a positive electrode, a negative electrode and a separator, wherein the electrolyte is an aqueous zinc-ion battery electrolyte containing indium chloride additive, the positive electrode material is manganese dioxide, the negative electrode material is metallic zinc, and the separator is a glass fiber membrane.
[0053] Zinc-ion batteries utilize zinc, an element widely distributed in the Earth's crust, resulting in lower costs and prices less affected by supply and demand. Abundant zinc reserves and low raw material costs give zinc-ion batteries significant resource and price advantages, making them more suitable for large-scale energy storage applications.
[0054] Zinc-ion batteries offer superior performance compared to lithium-ion batteries in both high and low temperatures. They can operate within a temperature range of -20°C to 50°C without requiring an additional air conditioning system. Zinc-ion batteries can be used in both hot and cold environments, as well as in high-altitude and low-temperature regions, making them suitable for a wider range of applications.
[0055] Zinc-ion battery aqueous electrolyte is non-toxic and harmless, with natural environmental protection properties. Even if it leaks, it will not affect human health, which is more in line with current environmental protection requirements. It can be widely used in various wearable electronic devices such as blood pressure sensors, breath sensors, Bluetooth headsets, and smart glasses.
[0056] The embodiments of the present invention have achieved some positive results during the research and development or use process, and have indeed great advantages compared with the prior art. The following content describes them in conjunction with the data, charts and other information of the experimental process.
[0057] Example 1
[0058] This embodiment describes an aqueous zinc-ion battery electrolyte containing indium chloride as an additive. The electrolyte is composed of indium chloride, soluble zinc sulfate, and deionized water, wherein the concentration of indium chloride is 0.02 mol / L. -1 The concentration of zinc sulfate is 2 mol / L. -1 .
[0059] This embodiment describes an aqueous zinc-ion battery electrolyte containing indium chloride additive, which is prepared using the following method, specifically including the following steps:
[0060] (1) Dissolve 16.145g of zinc sulfate in 50ml of deionized water and stir until completely dissolved to obtain an aqueous solution of zinc sulfate;
[0061] (2) Add 0.2212g of indium chloride to the above zinc sulfate aqueous solution and stir until completely dissolved to obtain the target electrolyte.
[0062] Prepare a pure zinc sulfate electrolyte according to the above steps as a control electrolyte. The concentration of the zinc sulfate is 2 mol / L. -1 .
[0063] The target electrolyte and the control electrolyte prepared above were used to assemble an aqueous zinc-ion battery.
[0064] The aqueous zinc-ion battery consists of a positive electrode, a negative electrode, a separator, and an electrolyte. The positive electrode material is manganese dioxide, the negative electrode is a zinc sheet, the separator is a glass fiber membrane, and the electrolyte is the target electrolyte and the comparative electrolyte prepared above.
[0065] The aqueous zinc-ion battery of this embodiment is configured using the following method, specifically including the following steps:
[0066] (1) Preparation of manganese dioxide positive electrode sheet
[0067] 2.82 g of manganese acetate and 2.63 g of ammonium persulfate were weighed and dissolved in deionized water. The mixture was stirred until the aqueous solution turned pale yellow. This solution was transferred to a 100 mL reaction vessel and then hydrothermally reacted at 140 °C for 24 h. The reaction vessel was then allowed to cool naturally to room temperature. The sample was then collected by centrifugation and washed three times each with distilled water and anhydrous ethanol. The resulting product was dried at 80 °C for 12 h to obtain manganese dioxide powder.
[0068] Manganese dioxide, acetylene black, and polyvinylidene fluoride are mixed in a certain mass ratio, and N-methylpyrrolidone is added to make the three into a paste. The paste is repeatedly rolled into a thin sheet and pressed onto a cut stainless steel mesh to make an electrode sheet. Then, it is dried in a vacuum drying oven for 24 hours to obtain the manganese dioxide positive electrode sheet.
[0069] (2) Preparation of zinc negative electrode sheet
[0070] The zinc foil is cut into appropriate sizes, then cleaned with dilute sulfuric acid and deionized water, and finally vacuum dried at room temperature for 24 hours in a vacuum drying oven at 80°C to obtain the negative electrode sheet.
[0071] (4) Assembly of aqueous zinc-ion batteries
[0072] An aqueous zinc-ion battery was assembled in a CR2032 coin cell casing. The assembly sequence was as follows: positive electrode casing, manganese dioxide positive electrode sheet, glass fiber separator, aqueous electrolyte, zinc negative electrode sheet, gasket, spring sheet, and negative electrode casing. The assembled battery was placed on a sealing machine and sealed under pressure. After standing at room temperature for 10 hours, electrochemical performance was tested.
[0073] (5) Assembly of zinc symmetric cells
[0074] A zinc symmetric battery was assembled in a CR2032 coin cell casing. The assembly sequence was as follows: positive electrode casing, zinc electrode sheet, glass fiber separator, aqueous electrolyte, zinc electrode sheet, gasket, spring sheet, and negative electrode casing. The assembled symmetric battery was placed on a sealing machine and sealed under pressure. After standing at room temperature for 10 hours, electrochemical performance was tested.
[0075] Electrochemical performance tests were conducted on the zinc-symmetric battery and zinc-ion battery of this embodiment. The tests were performed on the Chenhua electrochemical workstation and the Xinwei battery testing system at room temperature (25°C). Additionally, the manganese dioxide sample prepared in this embodiment was characterized by X-ray diffraction and scanning electron microscopy.
[0076] Figure 1 This is a schematic diagram illustrating the mechanism of action of indium chloride additives in aqueous zinc-ion batteries, showing that In... 3+ Preferential adsorption on the zinc anode surface forms a dynamic electrostatic shielding layer, inducing zinc ions to preferentially grow along the Zn(002) plane, reducing the nucleation and growth rate of zinc dendrites, and inducing uniform deposition of zinc ions, which can effectively regulate the morphology of the zinc deposition layer.
[0077] Figure 2 The figures show the AC impedance spectra of zinc symmetric cells assembled using pure zinc sulfate electrolyte (a) and the target electrolyte in Example 1 (b). The values in Figures a and b are 730 Ω and 85 Ω, respectively, indicating that the indium chloride additive in the target electrolyte can effectively reduce the charge transfer impedance of the zinc surface.
[0078] Figure 3 This refers to the zinc symmetric battery assembled using pure zinc sulfate electrolyte (a) and the target electrolyte in Example 1 (b) at 1 mA cm⁻¹. -2 The current density and 0.5 mAh cm⁻¹ -2 Time-voltage curves at a fixed capacity; in Figure a, the zinc in this battery failed in less than 300 hours, while in Figure b, the zinc in this battery could operate for a limited time of 3000 hours, indicating that the indium chloride additive in the target electrolyte can significantly improve the cycle stability of the zinc electrode.
[0079] Figure 4 yes Figure 2 (b) The local time-voltage curves from 2998 to 3000 hours show that the polarization voltage of the zinc symmetric cell assembled with the target electrolyte is still very small (about 0.027V) after 3000 hours of operation, indicating that the indium chloride additive can significantly reduce the polarization voltage of the zinc symmetric cell.
[0080] Figure 5 The images show scanning electron microscope (SEM) images of the zinc electrode surface after 300 h and 3000 h of cycling using pure zinc sulfate electrolyte (a) and the target electrolyte in Example 1 (b), respectively. A large number of zinc dendrites and disordered stacking can be observed in Figure a, while the morphology in Figure b is still relatively smooth and no obvious dendrites are found. This indicates that the indium chloride additive can effectively induce the uniform deposition of zinc ions and effectively control the deposition / dissolution of zinc.
[0081] Figure 6 The image shows the X-ray diffraction pattern of manganese dioxide prepared in Example 1. Its diffraction characteristic peaks are completely consistent with the standard PDF card of manganese dioxide (No. PDF#44-0141), indicating that a manganese dioxide material has been successfully prepared and can be applied to zinc-ion batteries.
[0082] Figure 7 This is a scanning electron microscope image of manganese dioxide prepared in Example 1. As can be seen from the image, its morphology is a linear structure with uniform particle size at the nanoscale.
[0083] Figure 8 The zinc-ion battery assembled using pure zinc sulfate electrolyte (a) and the target electrolyte from Example 1 (b) was tested at 0.1 A g. -1 As shown in Figure a, the cycling curves at current density indicate that the zinc-ion battery assembled with pure zinc sulfate electrolyte operates at 0.1 A g. -1 The initial capacity was 280mAh g. -1 After 100 charge-discharge cycles, the capacity is approximately 121 mAh g. -1 The capacity retention rate was 43.2%, which is not conducive to practical applications. However, for the zinc ion battery assembled with the target electrolyte (b) in Example 1, at 0.1 A g...-1 The initial capacity was 313 mAh g. -1 After 150 charge-discharge cycles, the performance reaches its optimal capacity of approximately 330mAh g. -1 There is no capacity decay. Therefore, the electrolyte additive (indium chloride) of the present invention can effectively inhibit the growth and deterioration of dendrites on the zinc anode surface, improve charge and discharge efficiency, and greatly enhance the cycle stability of zinc-ion batteries.
[0084] The above examples demonstrate that the indium chloride-containing electrolyte of the present invention can effectively inhibit dendrite growth and significantly improve the service life of zinc metal from less than 300 hours to 3000 hours, a tenfold increase. The aqueous zinc-ion battery assembled with the indium chloride-containing electrolyte achieves its optimal capacity of approximately 330 mAh g after 150 charge-discharge cycles. -1 It has no capacity decay and has greater application advantages.
[0085] Example 2
[0086] In Example 2, a solution containing 0.05 mol L was prepared. -1 The target electrolyte for the indium chloride additive still contains zinc sulfate at a concentration of 2 mol / L. -1 The other processes and steps are the same as in Example 1.
[0087] The zinc-ion battery assembled using the target electrolyte in Example 2 was tested at 0.1 A g. -1 Cyclic testing was performed using current density, and its initial capacity was 316 mAh g. -1 After 150 charge-discharge cycles, the capacity is approximately 310 mAh g. -1 The capacity retention rate is 98.1%, with almost no capacity decay. Therefore, the target electrolyte in Example 2 can also effectively suppress the growth and deterioration of dendrites on the zinc anode surface, improve charge and discharge efficiency, and enhance the cycle stability of zinc-ion batteries.
[0088] Example 3
[0089] In Example 3, a solution containing 0.08 mol L was prepared. -1 The target electrolyte for the indium chloride additive still contains zinc sulfate at a concentration of 2 mol / L. -1 The other processes and steps are the same as in Example 1.
[0090] The zinc-ion battery assembled using the target electrolyte in Example 3 was tested at 0.1 A g. -1 Current density was used for cycling tests, and its initial capacity was 318 mAh g. -1 After 150 charge-discharge cycles, the capacity is approximately 315 mAh g. -1The capacity retention rate is 99.1%, with almost no capacity decay. Therefore, the target electrolyte in Example 3 can also effectively suppress the growth and deterioration of dendrites on the zinc anode surface, improve charge and discharge efficiency, and enhance the cycle stability of zinc-ion batteries.
[0091] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any modifications, equivalent substitutions, and improvements made by those skilled in the art within the scope of the technology disclosed in the present invention, and within the spirit and principles of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. An aqueous zinc-ion battery electrolyte containing indium chloride additive, characterized in that, The electrolyte is composed of additives, soluble zinc salts, and deionized water; the additive is indium chloride with the chemical formula InCl3, and the soluble zinc salt is zinc sulfate with the chemical formula ZnSO4·7H2O. The concentration of zinc sulfate is 1–2 mol / L. -1 ; The concentration of indium chloride is 0.01–0.1 mol / L. -1 .
2. The aqueous zinc-ion battery electrolyte according to claim 1, characterized in that, The electrolyte has a pH value of 4 to 6.
3. A method for constructing an aqueous zinc-ion battery, characterized in that, An aqueous zinc-ion battery is constructed using the electrolyte described in any one of claims 1 to 2. The electrolyte can form a dynamic electrostatic shielding layer on the surface of the zinc anode, induce uniform deposition of zinc ions, inhibit dendrite growth and deterioration, and protect the zinc anode.
4. The method for constructing an aqueous zinc-ion battery as described in claim 3, characterized in that, The preparation method of manganese dioxide positive electrode sheet is as follows: 2.82 g of manganese acetate and 2.63 g of ammonium persulfate were weighed and dissolved in deionized water. The mixture was stirred until the aqueous solution turned light yellow. This solution was then transferred to a 100 mL reaction vessel and subjected to hydrothermal reaction at 140 °C for 24 h. The reaction vessel was then allowed to cool naturally to room temperature. The sample was then collected by centrifugation and washed three times each with distilled water and anhydrous ethanol. The resulting product was dried at 80 °C for 12 h to obtain manganese dioxide powder. Manganese dioxide, acetylene black, and polyvinylidene fluoride are mixed in a certain mass ratio, and N-methylpyrrolidone is added to make the three into a paste. The paste is repeatedly rolled into a thin sheet and pressed onto a cut stainless steel mesh to make an electrode sheet. Then, it is dried in a vacuum drying oven for 24 hours to obtain the manganese dioxide positive electrode sheet.
5. The method for constructing an aqueous zinc-ion battery as described in claim 3, characterized in that, The preparation method of the zinc negative electrode sheet is as follows: The zinc foil is cut to a suitable size, then cleaned with dilute sulfuric acid and deionized water, and finally vacuum dried in a vacuum drying oven at 80°C for 24 hours to obtain the negative electrode sheet.
6. The method for constructing an aqueous zinc-ion battery as described in claim 3, characterized in that, The preparation method for assembling an aqueous zinc-ion battery is as follows: Assemble an aqueous zinc-ion battery in a button cell casing. The assembly sequence is as follows: positive electrode casing, manganese dioxide positive electrode sheet, glass fiber separator, aqueous electrolyte, zinc negative electrode sheet, gasket, spring sheet, and negative electrode casing. Place the assembled battery on a button cell sealing machine and seal it under pressure.
7. An aqueous zinc-ion battery constructed using the method of claim 3, characterized in that, The battery comprises an electrolyte, a positive electrode, a negative electrode, and a separator, wherein the electrolyte is the electrolyte according to any one of claims 1 to 2, the positive electrode material is manganese dioxide, the negative electrode material is metallic zinc, and the separator is a glass fiber membrane.
Citation Information
Patent Citations
High-specific-capacitance manganese-dioxide conducting polymer composite electrode material with core-shell structure and manufacturing method thereof
CN103151179A
Battery
CN104752681A
Aqueous zinc ion battery electrolyte containing additive, preparation method of aqueous zinc ion battery electrolyte and battery
CN113161631A