Binder and preparation method thereof, electrode plate and secondary battery

By using an elastic and flexible copolymer binder in lithium-ion batteries, combined with carboxylic acid, sulfonic acid groups and cyano groups, the problem of expansion and brittleness of the negative electrode material is solved, significantly improving the performance of the battery. Cycling performance and stability.

CN116404162BActive Publication Date: 2024-10-22SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310435510.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-21
Publication Date
2024-10-22
Estimated Expiration
2043-04-21

AI Technical Summary

Technical Problem

Existing lithium-ion battery negative electrode plate binders cannot effectively suppress the volume expansion and brittleness of silicon-based materials, affecting the cycle stability of the battery.

Method used

A binder composed of a copolymer and an organic substance containing more than two guanidine groups is used to form an elastic and flexible binder through the in-situ polymerization reaction of comonomer I and comonomer II, and combines carboxyl Groups such as acids, sulfonic acid groups and cyano groups form strong interfacial bonding and ionic bonds to inhibit the expansion of the pole piece material.

Benefits of technology

It effectively suppresses the expansion of the pole piece material, improves the cycle performance and fatigue resistance of the battery, maintains good adhesion between the active material and the pole piece, and improves the energy density and stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116404162B_ABST
    Figure CN116404162B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of secondary batteries, and in particular to a binder and a preparation method thereof, an electrode plate and a secondary battery. A binder comprises a copolymer and an organic substance containing two or more guanidine groups; the comonomer of the copolymer comprises comonomer I and comonomer II; the comonomer I comprises at least one of an unsaturated carboxylic acid, an unsaturated carboxylate, an unsaturated sulfonic acid and an unsaturated sulfonate; the structural formula of the comonomer II is as follows: #imgabs0#R is selected from at least one of H and methyl. The binder of the present invention is elastic and flexible, can effectively inhibit the expansion of the plate material, can maintain good adhesion with the active material during the battery cycle, and improve the battery cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of secondary batteries, and in particular to a binder and a preparation method thereof, an electrode plate and a secondary battery. Background Art

[0002] Lithium-ion batteries have excellent properties such as high capacity, long cycle, no memory effect, low self-discharge, and wide operating temperature range. They have been widely used in 3C products and electric vehicles. During the use of the battery, as lithium ions are inserted and removed, the positive and negative pole pieces will expand in volume, thereby destroying the internal structure of the pole pieces and affecting the performance of the lithium-ion battery. At present, how to effectively inhibit the expansion of the pole pieces and improve battery performance is one of the research hotspots.

[0003] The negative electrode sheet mainly contains graphite and silicon-based materials as negative electrode active materials, as well as binders and conductive agents. With the pursuit of high energy density lithium-ion batteries, silicon-based materials are increasingly valued. However, during the process of lithium insertion and extraction, silicon-based materials are accompanied by severe volume expansion, which leads to the crushing of material particles and repeated crushing and reconstruction of SEI film, seriously affecting battery performance and greatly limiting its commercial application. It is an economical and effective means to inhibit the expansion of silicon-based materials by structural design and modification of binders.

[0004] In the prior art, the binders used for negative electrode materials mainly include styrene-butadiene rubber (SBR), polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC), etc. However, the above binders have weak cohesive force and cannot effectively inhibit the expansion of silicon-based materials. Polyacrylic acid (PAA) binder can form a large number of intermolecular hydrogen bonds, which can effectively inhibit the large volume expansion of negative electrode materials. However, the excessively strong intermolecular hydrogen bonds of polyacrylic acid binder make the material brittle, which is not conducive to the processing and manufacturing of pole pieces, and lacks strong interfacial adhesion with carbon-based negative electrode active materials.

[0005] Therefore, existing binders either have weak cohesion and cannot effectively suppress the volume change of the negative electrode material during the charge and discharge process, or have excessive rigidity, resulting in brittleness of the electrode sheet, and it is difficult to maintain effective interface bonding with the active material, resulting in the inability to effectively improve the cycle stability of the battery.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] An object of the present invention is to provide an adhesive.

[0008] Another object of the present invention is to provide a method for preparing the binder.

[0009] Another object of the present invention is to provide an electrode plate containing the above-mentioned binder.

[0010] Another object of the present invention is to provide a secondary battery containing the above-mentioned electrode plate.

[0011] In order to achieve the above-mentioned purpose of the present invention, the technical solution of the present invention is as follows:

[0012] The present invention provides a binder, which comprises a copolymer and an organic substance containing more than two guanidine groups;

[0013] The comonomers of the copolymer include comonomer I and comonomer II;

[0014] The comonomer I comprises at least one of an unsaturated carboxylic acid, an unsaturated carboxylate, an unsaturated sulfonic acid and an unsaturated sulfonate;

[0015] The structural formula of the comonomer II is as follows:

[0016] R is selected from at least one of H and methyl.

[0017] In a specific embodiment of the present invention, the comonomer I includes:

[0018] (a) at least one of a carboxylic acid group, a carboxylate group, a sulfonic acid group, and a sulfonate group; and,

[0019] (b) Alkenyl.

[0020] In a specific embodiment of the present invention, the unsaturated carboxylic acid includes at least one of acrylic acid, methacrylic acid, itaconic acid, maleic acid and fumaric acid; the unsaturated carboxylate includes at least one of lithium salt, potassium salt and sodium salt of the unsaturated carboxylic acid. Further, the unsaturated carboxylate includes at least one of lithium acrylate, potassium acrylate, sodium acrylate, lithium methacrylate, potassium methacrylate and sodium methacrylate.

[0021] In a specific embodiment of the present invention, the unsaturated sulfonate includes at least one of sodium styrene sulfonate, sodium 3-prop-2-enoyloxypropane-1-sulfonate, potassium methacrylate 3-sulfonate propyl ester, N,N-dimethyl-N-methylacrylamidopropyl-N,N-dimethyl-N-propane sulfonic acid inner salt, and 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt.

[0022] In a specific embodiment of the present invention, the organic substance containing more than two guanidine groups includes at least one of polyhexamethyleneguanidine hydrochloride, polyhexamethylenebiguanide hydrochloride, chlorhexidine gluconate, chlorhexidine acetate and biguanide octylamine.

[0023] In a specific embodiment of the present invention, the mass ratio of the sum of the mass of the comonomer I and the comonomer II to the mass ratio of the organic matter containing more than two guanidine groups is (1-50):1, preferably (5-20):1.

[0024] In a specific embodiment of the present invention, based on the total amount of the copolymer, the copolymer includes 40% to 80% of the comonomer I and 20% to 60% of the comonomer II by mass percentage. Further, the copolymer includes 60% to 70% of the comonomer I and 30% to 40% of the comonomer II by mass percentage.

[0025] The present invention also provides a method for preparing the above-mentioned binder, comprising the following steps:

[0026] The comonomer I and the comonomer II are subjected to in-situ polymerization reaction in a liquid system containing an organic substance containing more than two guanidine groups and an initiator.

[0027] In a specific embodiment of the present invention, the amount of the initiator is 1 wt% to 5 wt%, preferably 2 wt% to 4 wt%, of the total mass of the copolymer I and the comonomer II. Further, the initiator includes at least one of ammonium persulfate, potassium persulfate and sodium persulfate.

[0028] In a specific embodiment of the present invention, the liquid system comprises an aqueous system.

[0029] In a specific embodiment of the present invention, the preparation method comprises:

[0030] (a) dissolving an organic substance containing two or more guanidine groups in water to obtain an aqueous solution of the organic substance containing two or more guanidine groups;

[0031] (b) adding the comonomer I and the comonomer II to the aqueous solution and dispersing them uniformly; raising the temperature to the initiation temperature of the initiator under a protective atmosphere, adding the initiator, reacting for 2 to 6 hours, terminating the reaction, and drying to obtain a binder.

[0032] In a specific embodiment of the present invention, in step (a), in the aqueous solution of the organic matter containing more than two guanidine groups, the mass fraction of the organic matter containing more than two guanidine groups is 0.1% to 5%.

[0033] The present invention also provides an electrode plate, comprising a current collector and an electrode membrane arranged on the current collector; the electrode membrane comprises the binder.

[0034] In a specific embodiment of the present invention, the electrode plate includes a negative electrode plate.

[0035] In a specific embodiment of the present invention, the amount of the binder is 1% to 5% of the mass of the electrode membrane, preferably 2% to 4%.

[0036] In a specific embodiment of the present invention, the active material in the electrode membrane includes a silicon-based material. Furthermore, the active material also includes a carbon material.

[0037] The present invention also provides a secondary battery, comprising a positive electrode plate, a negative electrode plate, a separator and an electrolyte; the negative electrode plate is the above-mentioned electrode plate.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] The binder of the present invention is elastic and flexible, can effectively inhibit the expansion of the pole piece material, can maintain good adhesion with the active material during the battery cycle, and has excellent fatigue resistance, so that the negative pole piece prepared based on it has excellent performance and improves the cycle performance of the battery. DETAILED DESCRIPTION

[0040] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0041] In the prior art, the electrode material binder cannot effectively inhibit the volume change of the active material during the charge and discharge process, and may induce the interface bonding contact failure between the binder and the active material and the current collector, thereby resulting in poor cycle stability of the battery.

[0042] The present invention provides a binder, which comprises a copolymer and an organic substance containing more than two guanidine groups;

[0043] The comonomers of the copolymer include comonomer I and comonomer II;

[0044] The comonomer I comprises at least one of an unsaturated carboxylic acid, an unsaturated carboxylate, an unsaturated sulfonic acid and an unsaturated sulfonate;

[0045] The structural formula of the comonomer II is as follows:

[0046] R is selected from at least one of H and methyl.

[0047] The comonomer I contained in the copolymer used in the binder of the present invention has water solubility and electronegativity, which can promote the stable dispersibility of the formed copolymer in the aqueous phase system and play a role in suspending and dispersing the slurry; and the carbonyl group contained in the comonomer I can complex lithium ions, thereby improving the dynamic performance of the battery. The comonomer II contained in the copolymer contains a strong polar group cyano, which can form a strong interface bond with the active material and the current collector, and improve the stability of the electrode structure during the charge and discharge process; and the coordination effect of the cyano group and lithium ions is also conducive to improving the lithium ion transmission dynamic performance.

[0048] The carboxylic acid group or sulfonic acid group contained in the monomers in the copolymer can form strong synergistic forces of ionic bonds and hydrogen bonds with the guanidine group, producing a strong physical cross-linking effect, thereby effectively inhibiting the expansion of the electrode material; and the existence of the physical cross-linking effect can dissipate the stress energy of the material through the breaking of the physical cross-linking hydrogen bonds and ionic bonds, thereby obtaining good flexibility.

[0049] In a specific embodiment of the present invention, the comonomer I includes:

[0050] (a) at least one of a carboxylic acid group, a carboxylate group, a sulfonic acid group, and a sulfonate group; and,

[0051] (b) Alkenyl.

[0052] The comonomer I of the present invention is at least one of alkenyl carboxylic acid, alkenyl carboxylate, alkenyl sulfonic acid and alkenyl sulfonate. The alkenyl group in the structure is used for polymerization reaction to form a copolymer, and the carboxylic acid, carboxylate, sulfonic acid and sulfonate groups provide water solubility and electronegativity, promote the stable dispersion of the copolymer in the aqueous phase, and achieve suspension and dispersion of the slurry, and the carbon group therein can complex lithium ions to improve the dynamic performance of the battery.

[0053] In a specific embodiment of the present invention, the unsaturated carboxylic acid includes at least one of acrylic acid, methacrylic acid, itaconic acid, maleic acid and fumaric acid; the unsaturated carboxylate includes at least one of lithium salt, potassium salt and sodium salt of the unsaturated carboxylic acid. Further, the unsaturated carboxylate includes at least one of lithium acrylate, potassium acrylate, sodium acrylate, lithium methacrylate, potassium methacrylate and sodium methacrylate.

[0054] In some specific embodiments of the present invention, the unsaturated carboxylate includes at least one of lithium acrylate, sodium acrylate, lithium methacrylate and sodium methacrylate.

[0055] In actual operation, comonomer I may include more than two of the above substances. When it includes more than two substances, the ratio of various substances can be adjusted according to actual needs, and the total mass proportion of comonomer I can meet the requirements.

[0056] In a specific embodiment of the present invention, the unsaturated sulfonate includes at least one of sodium styrene sulfonate, sodium 3-prop-2-enoyloxypropane-1-sulfonate, potassium methacrylate 3-sulfonate propyl ester, N,N-dimethyl-N-methylacrylamidopropyl-N,N-dimethyl-N-propane sulfonic acid inner salt, and 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt.

[0057] In some specific embodiments of the present invention, the unsaturated sulfonate includes at least one of 3-sulfopropyl methacrylate potassium salt, N,N-dimethyl-N-methylacrylamidopropyl-N,N-dimethyl-N-propane sulfonic acid inner salt and 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt.

[0058] In actual operation, comonomer II may include more than two of the above substances. When more than two substances are included, the ratio of various substances can be adjusted according to actual needs, and the total mass proportion of comonomer II can meet the requirements.

[0059] In a specific embodiment of the present invention, the organic substance containing more than two guanidine groups includes at least one of polyhexamethyleneguanidine hydrochloride, polyhexamethylenebiguanide hydrochloride, chlorhexidine gluconate, chlorhexidine acetate and biguanide octylamine. Wherein, more than two includes 2 and more than 2.

[0060] In some specific embodiments of the present invention, the organic compound containing two or more guanidine groups includes polyhexamethyleneguanidine hydrochloride and / or polyhexamethylenebiguanidine hydrochloride.

[0061] In some specific embodiments of the present invention, the number average molecular weight of the polyhexamethyleneguanidine hydrochloride is 8000-12000; the number average molecular weight of the polyhexamethylene biguanidine hydrochloride is 2000-5000.

[0062] For example, in different embodiments, the number average molecular weight of the polyhexamethyleneguanidine hydrochloride can be 8000, 8500, 9000, 9500, 10000, 10500, 11000, 11500, 12000 or a range consisting of any two thereof; the number average molecular weight of the polyhexamethylene biguanide hydrochloride can be 2000, 2500, 3000, 3500, 4000, 4500, 5000 or a range consisting of any two thereof.

[0063] When R is H, the comonomer II is acrylonitrile; when R is methyl, the comonomer II is methacrylonitrile. That is, the comonomer II includes at least one of methacrylonitrile and acrylonitrile.

[0064] In a specific embodiment of the present invention, the mass ratio of the comonomer I and the comonomer II to the mass ratio of the organic matter containing more than two guanidine groups is (1-50) : 1, preferably (5-20) : 1. When the organic matter containing more than two guanidine groups is too much and the comonomer is too little, the suspension and dispersion effect of the binder on the slurry will be reduced, and the inhibitory effect on the expansion of the pole piece material will be weakened; when the organic matter containing more than two guanidine groups is too little and the comonomer is too much, a high elastic modulus can be provided, but the physical crosslinking effect between the copolymer and the guanidine group becomes weak, and the effect of dissipating the stress energy of the pole piece material through the breaking of the physical crosslinking hydrogen bonds and ionic bonds is weakened, and the flexibility is insufficient. The present invention further controls the mass ratio of the comonomer I and the comonomer II to the mass ratio of the organic matter containing more than two guanidine groups within the above range, taking into account the high elastic modulus and flexibility of the binder, effectively inhibiting the expansion of the pole piece material; and contributing to the uniform and stable dispersion of the active material, ensuring the interface adhesion to the active material and the current collector.

[0065] For example, in different embodiments, the mass ratio of the comonomer I and the comonomer II to the mass ratio of the organic matter containing more than two guanidine groups can be 1:1, 2:1, 5:1, 8:1, 10:1, 12:1, 15:1, 18:1, 20:1, 25:1, 30:1, 35:1, 40:1, 45:1, 50:1 or a range consisting of any two of them.

[0066] In a specific embodiment of the present invention, based on the total amount of the copolymer, the copolymer includes 40% to 80% of the comonomer I and 20% to 60% of the comonomer II by mass percentage. Further, the copolymer includes 60% to 70% of the comonomer I and 30% to 40% of the comonomer II by mass percentage. When the amount of comonomer I in the copolymer is too small, the stable dispersibility of the formed copolymer in the aqueous phase system is insufficient, the suspension and dispersion effect on the slurry is deteriorated, and the physical crosslinking effect formed with the guanidine group is weakened; when the amount of comonomer II in the copolymer is too small, the interfacial bonding effect between the formed copolymer and the active material and the current collector is insufficient, and it is not easy to maintain stability during the charge and discharge process. The present invention further controls the amount of comonomer I and comonomer II within the above range, taking into account the suspension and dispersion effect on the slurry, effectively inhibiting the expansion of the pole piece material, and ensuring the formation of a strong interfacial bonding with the active material and the current collector.

[0067] For example, in different embodiments, based on the total amount of the copolymer, in the copolymer, the mass percentage of the comonomer I can be 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80% or a range consisting of any two thereof; the mass percentage of the comonomer II can be 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60% or a range consisting of any two thereof.

[0068] The present invention also provides a method for preparing the above-mentioned binder, comprising the following steps:

[0069] The comonomer I and the comonomer II are subjected to in-situ polymerization reaction in a liquid system containing an organic substance containing more than two guanidine groups and an initiator.

[0070] The binder of the present invention is formed by in-situ polymerization, and the copolymer and the organic matter containing more than two guanidine groups can form an interpenetrating network, further improving the effect of inhibiting the expansion of the pole piece material.

[0071] In a specific embodiment of the present invention, the amount of the initiator is 1 wt% to 5 wt%, preferably 2 wt% to 4 wt%, of the total mass of the copolymer I and the comonomer II. Further, the initiator includes at least one of ammonium persulfate, potassium persulfate and sodium persulfate.

[0072] For example, in different embodiments, the amount of the initiator can be 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt% of the sum of the mass of the copolymer I and the comonomer II, or a range consisting of any two of them.

[0073] In a specific embodiment of the present invention, the liquid system comprises an aqueous system.

[0074] In a specific embodiment of the present invention, the preparation method comprises:

[0075] (a) dissolving an organic substance containing two or more guanidine groups in water to obtain an aqueous solution of the organic substance containing two or more guanidine groups;

[0076] (b) adding the comonomer I and the comonomer II to the aqueous solution and dispersing them uniformly; raising the temperature to the initiation temperature of the initiator under a protective atmosphere, adding the initiator, reacting for 2 to 6 hours, terminating the reaction, and drying to obtain a binder.

[0077] In actual operation, the protective atmosphere includes nitrogen; the initiation temperature refers to the temperature at which the initiator undergoes thermal decomposition to initiate monomer polymerization, and can be adjusted according to the conditions of the initiator.

[0078] In a specific embodiment of the present invention, the drying treatment method includes spray drying. The binder powder is obtained by conventional spray drying.

[0079] For example, in different embodiments, the reaction time can be 2 h, 3 h, 4 h, 5 h, 6 h, or a range consisting of any two of them. After the reaction is completed, the temperature of the reaction system is lowered to room temperature to terminate the reaction.

[0080] In a specific embodiment of the present invention, in step (a), in the aqueous solution of the organic matter containing more than two guanidine groups, the mass fraction of the organic matter containing more than two guanidine groups is 0.1% to 5%.

[0081] For example, in different embodiments, in the aqueous solution, the mass fraction of the organic matter containing more than two guanidine groups can be 0.1%, 0.2%, 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5% or a range consisting of any two of them.

[0082] The present invention also provides an electrode plate, comprising a current collector and an electrode membrane arranged on the current collector; the electrode membrane comprises the binder.

[0083] The binder of the present invention is elastic and flexible, can maintain good adhesion with the active material during the battery cycle, and has excellent fatigue resistance, so that the negative electrode sheet prepared based on the binder has excellent performance.

[0084] In a specific embodiment of the present invention, the electrode plate includes a negative electrode plate.

[0085] In a specific embodiment of the present invention, the amount of the binder is 1% to 5%, preferably 2% to 4%, of the mass of the electrode membrane, so as to ensure both the inhibitory effect of the binder on the volume expansion of the electrode material and the energy density of the battery.

[0086] For example, in different embodiments, the amount of the binder may be 1%, 2%, 3%, 4%, 5% of the mass of the electrode membrane, or a range consisting of any two of these.

[0087] In a specific embodiment of the present invention, the active material in the electrode membrane includes a silicon-based material. Furthermore, the active material also includes a carbon material.

[0088] For example, in different embodiments, the silicon-based material includes at least one of silicon-oxygen compounds, silicon-carbon compounds, silicon and silicon alloys; and the carbon material includes at least one of natural graphite, artificial graphite or mesophase carbon microbeads.

[0089] The present invention also provides a secondary battery, comprising a positive electrode plate, a negative electrode plate, a separator and an electrolyte; the negative electrode plate is the above-mentioned electrode plate.

[0090] Examples 1 to 15

[0091] Examples 1 to 15 provide binders and preparation methods thereof. The types and amounts of raw materials used in Examples 1 to 15 are specifically shown in Table 1. The specific preparation methods include:

[0092] (1) weighing an organic substance containing two or more guanidine groups, adding it to 2 kg of deionized water, stirring it to fully dissolve it to prepare a corresponding aqueous solution;

[0093] (2) Add comonomer I and comonomer II to the aqueous solution, stir to disperse them evenly, and form a dispersed system; under the protection of nitrogen atmosphere, slowly heat to 80°C, add ammonium persulfate (the amount of ammonium persulfate is 3% of the mass of comonomer I and comonomer II), stir evenly, and continue to react for 4 hours. Cool the reaction solution to room temperature to terminate the reaction, and spray dry the solution to obtain a binder.

[0094] Table 1 Types and amounts of raw materials of the binders of Examples 1 to 15

[0095]

[0096]

[0097] The preparation of lithium-ion batteries includes the following steps:

[0098] (1) Preparation of negative electrode sheets: Graphite, silicon oxide, carbon black and binder materials were mixed in a weight ratio of 72:24:1:3 and dispersed in deionized water to form a uniform slurry; the slurry was then cast on a copper foil by a doctor blade method, dried at 70°C, cold pressed, trimmed and cut into pieces, and then dried at 100°C under vacuum for 12 hours to obtain negative electrode sheets.

[0099] (2) A 2025-type button half-cell was assembled in a glove box filled with inert gas, wherein the contents of H2O and O2 were both less than 0.1 ppm. A metal lithium sheet was used as the counter electrode, PP / PE was used as the separator, and 1M LiPF6 (EC﹕EMC﹕DMC=1﹕1﹕1vol%) + 3% FEC (fluoroethylene carbonate) was used as the electrolyte.

[0100] Among them, lithium-ion batteries 1# to 15# respectively use the binder materials prepared in Examples 1 to 15.

[0101] Comparative Examples 1 to 4

[0102] Comparative Examples 1 to 4 provide binders and preparation methods thereof. The types and amounts of raw materials used in Comparative Examples 1 to 4 are specifically shown in Table 2. The specific preparation methods include:

[0103] (1) Weigh organic matter B and add it into 2 kg of deionized water, stirring to fully dissolve it to prepare the corresponding aqueous solution;

[0104] (2) Add comonomer I and comonomer II to the aqueous solution, stir to disperse them evenly, and form a dispersed system; under the protection of nitrogen atmosphere, slowly heat to 80°C, add ammonium persulfate (the amount of ammonium persulfate is 3% of the mass of comonomer I and comonomer II), stir evenly, and continue to react for 4 hours. Cool the reaction solution to room temperature to terminate the reaction, and spray dry the solution to obtain a binder.

[0105] Table 2 Raw material types and dosages of binders in comparative examples 1 to 4

[0106]

[0107] The preparation method of the lithium ion battery is referred to in the embodiment, except that:

[0108] Comparative 1# to 4# lithium ion batteries respectively use the binder materials prepared in Comparative Examples 1 to 4.

[0109] Experimental example

[0110] Cyclic performance test

[0111] Take 3 batteries from each group prepared as above, and repeatedly charge and discharge the batteries through the following steps, and calculate the discharge capacity retention rate of the batteries.

[0112] First, in a 25°C environment, discharge at 0.5C to 5mV, 0.05C to 5mV, 0.02C to 5mV, 0.01C to 5mV, and finally charge at 0.1C to 1.5V, and record the charge capacity of the first cycle. Then perform 200 discharge and charge cycles, and record the charge capacity of the 200th cycle. According to the following formula:

[0113] Cycle capacity retention rate = 200th cycle charge capacity / first cycle charge capacity * 100%

[0114] The average capacity retention rate of each group of batteries after cycling is calculated, as shown in Table 3.

[0115] Thickness expansion rate test of negative electrode full embedding state

[0116] Measure the thickness of the negative electrode before assembling the battery, record it as D0. Discharge the assembled battery at 0.1C to 5mV and then 0.02C to 5mV in a 25℃ environment, so that the negative electrode is in a fully embedded state. Disassemble the battery and test the thickness of the negative electrode in the fully embedded state, record it as D1. According to the following formula:

[0117] Thickness expansion rate = (D1-D0) / D0*100%

[0118] The thickness expansion rate of the negative electrode sheet under the fully embedded state is calculated, as shown in Table 3.

[0119] Table 3 Performance test results of different batteries

[0120]

[0121]

[0122] It can be seen from the above results that, compared with the comparative example, the binder prepared in the embodiment of the present invention has both high elastic modulus and flexibility, and can effectively inhibit the expansion of the negative electrode active material. In addition, the binder in the embodiment also helps to evenly and stably disperse the negative electrode active material, and maintains good adhesion with the negative electrode active material, and has excellent fatigue resistance, thereby greatly improving the performance of the battery.

[0123] It can be seen from Examples 1 and 2 to 7 that the present invention can further balance the mechanical properties of the binder by further optimizing the comonomers constituting the copolymer and the organic matter containing more than two guanidine groups, so that the negative electrode sheet prepared based on it can obtain the optimal expansion inhibition effect, thereby further improving the performance of the battery.

[0124] It can be seen from Examples 1 and 8 to 15 that when the ratio of comonomer I to comonomer II of the synthetic copolymer is different, and the ratio of the total amount of comonomer to the organic matter containing more than two guanidine groups is different, the expansion inhibition of the pole piece and the influence on the cycle performance of the battery cell are also different. When the ratio of comonomer I to comonomer II and the ratio of the total amount of comonomer to the organic matter containing more than two guanidine groups are within a certain range, the prepared binder is used for the battery pole piece, which can further inhibit the expansion of the pole piece and improve the cycle performance.

[0125] It can be seen from Example 1 and Comparative Examples 1 to 2 that when the comonomer I in the preparation of the binder is replaced by methyl acrylate without carboxylic acid groups or sulfonic acid groups, or the organic matter containing more than two guanidine groups is replaced by 1,6-hexanediol without guanidine groups, the strong physical crosslinking between the carboxylic acid group or sulfonic acid group and the guanidine group cannot be formed, which will cause the binder to be unable to effectively suppress the rebound expansion of the pole piece. It can be seen from Example 1 and Comparative Examples 3 to 4 that when the organic matter containing more than two guanidine groups is replaced by diethylenetriamine and polyethyleneimine containing amino groups, the ability of the binder to suppress the rebound expansion of the pole piece is significantly reduced because the carboxylic acid group or sulfonic acid group can only form a weak physical crosslinking with the amino group.

[0126] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A binder, characterized in that: Including copolymers and organic substances containing more than 2 guanidine groups; The comonomers of the copolymer include comonomer I and comonomer II; The comonomer I comprises at least one of an unsaturated carboxylic acid, an unsaturated carboxylate, an unsaturated sulfonic acid and an unsaturated sulfonate; The structural formula of the comonomer II is as follows: ; R is selected from at least one of H and methyl.

2. The adhesive according to claim 1, characterized in that The unsaturated carboxylic acid comprises at least one of acrylic acid, methacrylic acid, itaconic acid, maleic acid and fumaric acid; the unsaturated carboxylic acid salt comprises at least one of a lithium salt, a potassium salt and a sodium salt of the unsaturated carboxylic acid; The unsaturated sulfonate includes at least one of sodium styrene sulfonate, sodium 3-prop-2-enoyloxypropane-1-sulfonate, potassium methacrylate 3-sulfonate propyl ester, N,N-dimethyl-N-methylacrylamidopropyl-N,N-dimethyl-N-propane sulfonic acid inner salt, and 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt.

3. The adhesive according to claim 2, characterized in that The unsaturated carboxylate includes at least one of lithium acrylate, sodium acrylate, lithium methacrylate and sodium methacrylate.

4. The adhesive according to claim 2, characterized in that The unsaturated sulfonate includes at least one of 3-sulfopropyl methacrylate potassium salt, N,N-dimethyl-N-methylacrylamidopropyl-N,N-dimethyl-N-propanesulfonic acid inner salt and 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt.

5. The adhesive according to claim 1, characterized in that The organic matter containing more than two guanidine groups includes at least one of polyhexamethyleneguanidine hydrochloride, polyhexamethylenebiguanide hydrochloride, chlorhexidine gluconate, chlorhexidine acetate and biguanide octylamine.

6. The adhesive according to claim 5, characterized in that The organic matter containing more than two guanidine groups includes polyhexamethyleneguanidine hydrochloride and / or polyhexamethylenebiguanidine hydrochloride.

7. The adhesive according to claim 1, characterized in that The mass ratio of the comonomer I and the comonomer II to the mass ratio of the organic matter containing more than two guanidine groups is (1-50):

1.

8. The adhesive according to claim 7, characterized in that The mass ratio of the comonomer I and the comonomer II to the mass ratio of the organic matter containing more than two guanidine groups is (5-20):

1.

9. The adhesive according to claim 1, characterized in that Based on the total amount of the copolymer, the copolymer includes 40% to 80% of the comonomer I and 20% to 60% of the comonomer II in terms of mass percentage.

10. The adhesive according to claim 9, characterized in that The copolymer comprises 60% to 70% of the comonomer I and 30% to 40% of the comonomer II in terms of mass percentage.

11. The method for preparing the binder according to any one of claims 1 to 10, characterized in that: The steps include: The comonomer I and the comonomer II are subjected to in-situ polymerization reaction in a liquid system containing an organic substance containing more than two guanidine groups and an initiator.

12. The method for preparing the adhesive according to claim 11, characterized in that: include: (a) dissolving an organic substance containing two or more guanidine groups in water to obtain an aqueous solution of the organic substance containing two or more guanidine groups; (b) adding the comonomer I and the comonomer II to the aqueous solution and dispersing them uniformly; raising the temperature to the initiation temperature of the initiator under a protective atmosphere, adding the initiator, reacting for 2 to 6 hours, terminating the reaction, and drying to obtain a binder.

13. The method for preparing the adhesive according to claim 12, characterized in that: In step (a), in the aqueous solution of the organic matter containing two or more guanidine groups, the mass fraction of the organic matter containing two or more guanidine groups is 0.1% to 5%.

14. An electrode plate, characterized in that: It comprises a current collector and an electrode membrane arranged on the current collector; the electrode membrane comprises the binder according to any one of claims 1 to 10 or the binder prepared by the preparation method according to any one of claims 11 to 13.

15. The electrode plate according to claim 14, characterized in that: The electrode plate includes a negative electrode plate.

16. The electrode plate according to claim 15, characterized in that: The amount of the binder used is 1% to 5% of the mass of the electrode membrane.

17. The electrode plate according to claim 15, characterized in that: The active material in the electrode membrane includes a silicon-based material.

18. The electrode plate according to claim 17, characterized in that: The active material also includes carbon materials.

19. A secondary battery, characterized in that: It comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte; the negative electrode sheet is the electrode sheet according to any one of claims 14 to 18.