Pulse Width Multiplexing SNSPD Array Circuit, Chip, Fabrication Method and Application

By designing a pulse width multiplexed SNSPD array circuit and utilizing a series structure of nanowire detectors, inductors, and parallel resistors, the problem of insufficient scalability of existing SNSPD arrays is solved, and efficient readout with simultaneous response from multiple pixels is achieved.

CN116698203BActive Publication Date: 2026-11-10NANJING UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310699741.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-14
Publication Date
2026-11-10
Estimated Expiration
2043-06-14

AI Technical Summary

Technical Problem

Existing SNSPD array devices have insufficient scalability and cannot effectively cope with the problem of simultaneous response of multiple pixels. Furthermore, existing readout schemes are complex and lack scalability.

Method used

By employing a pulse width multiplexing (SNSPD) array circuit, and through the design of series nanowire detectors, inductors, and parallel resistors, as well as delay lines, the output response signal pulse widths differ when any number of nanowire detectors respond simultaneously. Current biasing and signal readout are achieved using a single coaxial line.

Benefits of technology

It achieves easily scalable multi-pixel simultaneous response, reduces system complexity, improves the accuracy and fidelity of signal readout, and avoids device latch-up.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116698203B_ABST
    Figure CN116698203B_ABST
Patent Text Reader

Abstract

This invention discloses a pulse width multiplexed (SNSPD) array circuit, chip, its fabrication method, and applications. The SNSPD array includes several detector units connected in series. The input terminal is connected to the output terminal via these series-connected detector units. Each detector unit includes a nanowire detector, an inductor, and a parallel resistor. The nanowire detector and the inductor are connected in series and then in parallel with the parallel resistor. The inductance increases sequentially according to the series order, ensuring that when any equal number of nanowire detectors respond simultaneously, the pulse width of the response signal output at the output terminal is not the same. This invention is easily scalable and can handle simultaneous responses from multiple pixels.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of photon detection, and more particularly to a pulse width multiplexed SNSPD array circuit, chip, its fabrication method, and its application. Background Technology

[0002] Superconducting nanowire single-photon detectors (SNSPDs) are high-performance single-photon detectors that have been applied in quantum information, long-range lidar, lunar-Earth laser communication, and biological imaging. However, most existing SNSPDs are single-pixel structures with small photosensitive areas, resulting in low coupling efficiency for free-space photons and an inability to distinguish spatial positions, making them unsuitable for many large-scale practical applications. Therefore, the development of large photosensitive area array devices is one of the important development directions in the field of SNSPDs, but the corresponding signal readout faces significant challenges.

[0003] Conventional readout uses coaxial cables to interconnect the device with the room-temperature readout circuit. As the number of arrays increases, the thermal load introduced by the coaxial cables becomes increasingly significant. The introduction of superconducting coding circuits can greatly reduce the number of coaxial cables required; however, the fabrication process for such devices is complex and large-scale scaling has not yet been achieved. Therefore, researchers have begun to employ multiplexed readout schemes to fully utilize information from all dimensions of the response signal. Row-column multiplexing is a practical readout scheme and has been used in kilopixel SNSPD arrays. The dual-layer thermally coupled readout method avoids the current redistribution effects of row-column multiplexing. Time-division multiplexing-based superconducting nanodelay lines have enabled single-photon imaging of approximately 590 effective pixels. Combining these methods can further improve array scalability and suppress crosstalk, but they generally suffer from the inability to handle simultaneous responses from multiple pixels.

[0004] Superconducting nanowire detectors based on timing logic can handle simultaneous four-photon incidence, but waveform analysis after large-scale expansion may be difficult. Pulse amplitude multiplexing requires only a single coaxial line to resolve the position and time of photon arrival, but the requirement of proportional resistance limits its scalability. Frequency division multiplexing readout and optical readout can both achieve simultaneous readout of multi-pixel responses, but they have high requirements for on-chip fabrication or external equipment, and currently their readout performance is not ideal and their scalability is limited. All current readout schemes have their own limitations; therefore, developing a readout method that is easily scalable and can handle simultaneous multi-pixel responses is a key focus of array SNSPD research. Summary of the Invention

[0005] Purpose of the invention: This invention addresses the problems existing in the prior art by providing a pulse width multiplexing (SNSPD) array circuit, chip, fabrication method, and application that is easily expandable and capable of handling simultaneous responses from multiple pixels.

[0006] Technical Solution: This invention provides a pulse width multiplexing (SNSPD) array circuit, including an input terminal, an output terminal, and a plurality of detector units connected in series. The input terminal is connected to the output terminal via the detector units connected in series. Each detector unit includes a nanowire detector, an inductor, and a parallel resistor. The nanowire detector and the inductor are connected in series and then in parallel with the parallel resistor. The inductance increases sequentially according to the series order, such that when any equal number of nanowire detectors respond simultaneously, the pulse width of the response signal output by the output terminal is different.

[0007] This invention also provides a pulse width multiplexing (SNSPD) array chip, including a substrate and an input electrode, an output electrode, a nanowire detector region, and a delay line region located on the substrate. The nanowire detector region includes a plurality of regularly arranged nanowire detectors formed by meandering nanowires. The delay line region includes a number of meandering delay lines equal to the number of meandering nanowires. Each nanowire detector is connected to a delay line and then connected in parallel with a parallel resistor to form a detector unit. A plurality of detector units are connected in series. The input electrode is connected to the output electrode through the sequentially connected detector units. The inductance value of the delay lines increases sequentially according to the series connection order, such that when any equal number of nanowire detectors respond simultaneously, the pulse width of the response signal output by the output electrode is different.

[0008] Furthermore, the meandering nanowire and the delay line are formed by etching the same superconducting thin film. The width of the delay line is greater than the width of the meandering nanowire. The length of the delay line satisfies:

[0009] d l =d w *L / L sq

[0010] d l L is the length of the delay line, and L is the inductance of the delay line. sq d is the inductance per unit area of ​​the material used. w This represents the width of the delay line.

[0011] Furthermore, the parallel resistor is a titanium resistor, which is connected in parallel with the nanowire detector through a delay line clamp-on contact point extending from the delay line region.

[0012] This invention also provides a method for fabricating a pulse width multiplexed SNSPD array chip, comprising the following steps:

[0013] (1) Superconducting thin films were deposited on a substrate by magnetron sputtering;

[0014] (2) The input and output electrodes were fabricated by photolithography and magnetron sputtering;

[0015] (3) Electron beam exposure and reactive ion etching are used to form the nanowire detector region, delay line region and clamp contact point;

[0016] The nanowire detection region includes several regularly arranged nanowire detectors formed by meandering nanowires. The delay line region includes an equal number of meandering delay lines. After each nanowire detector is connected to a delay line, the delay line extends a parallel clamp-shaped contact point. A nanowire detector, a delay line, and a parallel resistor form a detector unit. Several detector units are connected in series. The input electrode is connected to the output electrode via the sequentially connected detector units. The length of each delay line satisfies the following condition:

[0017] d l =d w *L / L sq

[0018] d l L is the length of the delay line. sq d is the inductance per unit area of ​​the superconducting thin film. w L is the width of the delay line, and L is the inductance of the delay line. The inductance increases sequentially in series, such that when any equal number of nanowire detectors respond simultaneously, the pulse width of the response signal output by the output electrode is different.

[0019] (4) Electron beam exposure and magnetron sputtering are used to deposit parallel resistors onto the contact points;

[0020] (5) Package and cool the substrate to form a pulse width multiplexed SNSPD array chip.

[0021] The inductance value of the delay line was obtained through simulation. The width of the delay line is greater than the width of the meandering nanowire.

[0022] The present invention also provides a data readout method based on a pulse width multiplexing (SNSPD) array chip, comprising the following steps:

[0023] (1) A single coaxial line is used to input a bias current to the input electrode of the pulse width multiplexed SNSPD array chip. The bias current is provided by a constant voltage source and a current-limiting resistor connected in series with the constant voltage source.

[0024] (2) The response signal is read from the output electrode using an analog-to-digital converter;

[0025] (3) Obtain the amplitude of the response signal. If the waveform amplitude is n times the amplitude of a single nanowire detector response, then determine that there are n nanowire detectors responding at the moment.

[0026] (4) Obtain the pulse width value of the response signal at a preset threshold, and find the current response nanowire detector combination from the pre-stored table according to the pulse width value. The preset threshold is set differently according to the number of nanowire detector responses. The pre-stored table stores the pulse width value of the response signal at the preset threshold when different numbers of nanowire detector combinations respond. The pulse width value is obtained through simulation or experiment.

[0027] Beneficial effects: Compared with the prior art, the significant advantages of this invention are:

[0028] 1. Compared with existing SNSPD arrays, this invention greatly reduces the complexity of the system, requiring only a single coaxial line to achieve current bias and signal readout, resulting in a simple circuit.

[0029] 2. It can handle situations where multiple detectors respond simultaneously and can read out with high fidelity, which is impossible to achieve with row-column multiplexing readout and other methods;

[0030] 3. Increasing the inductance will not cause device latch-up, so it has strong scalability. Attached Figure Description

[0031] Figure 1 A schematic diagram of the pulse width multiplexing SNSPD array circuit provided by the present invention;

[0032] Figure 2 An optical microscope image of the pulse width multiplexing SNSPD array chip provided by the present invention;

[0033] Figure 3 for Figure 2 Optical microscope detail of the parallel resistor and delay line in the middle;

[0034] Figure 4 This is a statistical histogram of pulse signals with different pixel responses and pulse widths at a fixed threshold. Detailed Implementation

[0035] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0036] Example 1

[0037] This embodiment provides a pulse width multiplexing (SNSPD) array circuit, such as Figure 1As shown, a detector unit comprises several detector units connected in series, including an input terminal (in), an output terminal (out), and an output terminal (out). The input terminal is connected to the output terminal via these connected detector units. Each detector unit includes a nanowire detector, an inductor (L1, L2, L3, L4), and a parallel resistor R. The nanowire detector and the inductor are connected in series, and then connected in parallel with the parallel resistor. The inductor is used to change the pulse width of the response signal from different detector units and can be any implementable device, such as a delay line. The parallel resistor is used to superimpose the response signals from different pixels.

[0038] The inductance value can be distributed using either arithmetic progressions or non-arithmetic progressions, increasing sequentially in series. The goal is to ensure that when any equal number of nanowire detectors respond simultaneously, the pulse width of the output signal is different for each detector. For example, assuming there are four nanowire detectors, labeled 1, 2, 3, and 4, there are six possible combinations of two detectors: (1, 2), (1, 3), (1, 4), (2, 3), (2, 4), and (3, 4). When these six combinations respond simultaneously, the pulse widths of the output signal are different for each combination. The same principle applies to combinations of three detectors. This ensures that the pulse widths of the output signal are different for each combination of nanowire detectors, allowing for differentiation of which nanowire detectors are responding.

[0039] In use, the constant voltage source V and the current-limiting resistor R connected in series... b The bias current for all detector units is provided by a single coaxial cable. The current flows sequentially through detector units 1, 2, 3, and 4, and is then output from the output terminal. The signals can be distinguished later by the difference in waveform peak value and pulse signal width.

[0040] Example 2

[0041] This embodiment provides a pulse width multiplexing (SNSPD) array chip, which is a concrete implementation of the circuit in Embodiment 1, such as... Figure 2 As shown, the image includes the substrate and the input electrode (input arrow), output electrode (output arrow), and nanowire detector region located on the substrate (within the black box; see enlarged view). Figure 2 (b) The delay line region (within the large white dashed box) comprises several regularly arranged nanowire detectors formed by meandering nanowires. Figure 2 As shown, there are four delay line regions, each containing the same number of meandering delay lines as the meandering nanowires. Each nanowire detector is connected to a delay line and then to a parallel resistor (within the small white dashed box) to form a detector unit. Several detector units are connected in series. The input electrode is connected to the output electrode via the series-connected detector units.

[0042] The substrate can be a silicon / silicon oxide substrate or other types of substrate.

[0043] The meandering nanowires and the delay lines are formed by etching the same superconducting thin film. For example... Figure 3 As shown in (b), the width of the delay line is greater than the width of the meandering nanowire, which can reduce interference, and the length of the delay line satisfies:

[0044] d l =d w *L / L sq

[0045] d l L is the length of the delay line. sq d is the inductance per unit area of ​​the material used. w The width of the delay line is given by , and the inductance of the delay line is given by L. These values ​​are obtained through simulation. The simulation method specifically involves using... Figure 1 Through various combinations and experiments, the circuit shown was tested to obtain inductance values ​​that meet the following requirements: the inductance values ​​increase sequentially in series, and when any equal number of nanowire detectors respond simultaneously, the pulse widths of the response signals output by the output electrodes are all different.

[0046] The parallel resistor is a titanium resistor, which is connected through the clamp-on contact point of the delay line extending from the delay line region (e.g., Figure 3 (a) shown) is connected in parallel with the nanowire detector.

[0047] Example 3

[0048] This embodiment provides a method for fabricating a pulse width multiplexing (SNSPD) array chip according to Embodiment 2, including the following steps:

[0049] (1) Superconducting thin films were deposited on a substrate by magnetron sputtering;

[0050] (2) The input and output electrodes were fabricated by photolithography and magnetron sputtering using a lift-off process;

[0051] (3) Electron beam exposure and reactive ion etching are used to form the nanowire detector region, delay line region and clamp contact point;

[0052] The nanowire detection region includes several regularly arranged nanowire detectors formed by meandering nanowires. The delay line region includes an equal number of meandering delay lines, the width of which is greater than that of the meandering nanowires. Each nanowire detector, after being connected to a delay line, extends a parallel clamp-shaped contact point. A nanowire detector, a delay line, and a parallel resistor form a detector unit. Several detector units are connected in series. The input electrode is connected to the output electrode via these series-connected detector units. The length of each delay line satisfies the following condition:

[0053] d l =d w *L / L sq

[0054] d l L is the length of the delay line. sq d is the inductance per unit area of ​​the superconducting thin film. w L is the width of the delay line, and L is the inductance of the delay line. Through simulation, the inductance value increases sequentially in series, and when any equal number of nanowire detectors respond simultaneously, the pulse width of the response signal output by the output electrode is different.

[0055] (4) Electron beam exposure and magnetron sputtering are used to deposit parallel resistors onto the contact points;

[0056] (5) The substrate is packaged and cooled to 2.1K to form a pulse width multiplexed SNSPD array chip.

[0057] Example 4

[0058] The present invention also provides a data readout method based on the pulse width multiplexing SNSPD array chip described in Embodiment 2, comprising the following steps:

[0059] (1) A single coaxial line is used to input a bias current to the input electrode of the pulse width multiplexed SNSPD array chip. The bias current is provided by a constant voltage source and a current-limiting resistor connected in series with the constant voltage source.

[0060] (2) The response signal is read from the output electrode using an analog-to-digital converter;

[0061] (3) Obtain the amplitude of the response signal. If the waveform amplitude is n times the amplitude of a single nanowire detector response, then determine that there are n nanowire detectors responding at the moment.

[0062] (4) Obtain the pulse width value of the response signal at a preset threshold, and find the current response nanowire detector combination from the pre-stored table according to the pulse width value. The preset threshold is set differently according to the number of nanowire detector responses. The pre-stored table stores the pulse width value of the response signal at the preset threshold when different numbers of nanowire detector combinations respond. The pulse width value is obtained through simulation or experiment.

[0063] by Figure 2 Taking the four-pixel (nanowire detector) SNSPD array shown as an example, all its possible response scenarios are as follows: Figure 4 As shown, there are four possible responses from a single pixel. Setting the threshold to 25mV and measuring the pulse width at this threshold, the statistical histogram of pulse widths reveals four different distributions, corresponding to responses from pixels 1, 2, 3, and 4, respectively. There are six possible responses from two pixels simultaneously: pixel 1 + pixel 2, pixel 1 + pixel 3, pixel 1 + pixel 4, pixel 2 + pixel 3, pixel 2 + pixel 4, and pixel 3 + pixel 4. Their pulse widths increase sequentially, and the pulse amplitude is twice that of the single-pixel response signal. Setting the threshold to 35mV, the statistical histogram of pulse widths reveals six different distributions. There are four possible scenarios for simultaneous responses from three pixels: pixel 1 + pixel 2 + pixel 3, pixel 1 + pixel 2 + pixel 4, pixel 1 + pixel 3 + pixel 4, and pixel 2 + pixel 3 + pixel 4. The pulse widths increase sequentially, and the pulse amplitude is three times that of a single-pixel response signal. With a threshold set to 85mV, the pulse width histogram shows four different distributions. There is also one scenario for simultaneous responses from four pixels: pixel 1 + pixel 2 + pixel 3 + pixel 4. The pulse width is fixed, and the pulse amplitude is four times that of a single-pixel response signal. With a threshold set to 100mV, the pulse width histogram shows only one distribution. These scenarios are stored in a pre-stored table, allowing the current pixel combination to be retrieved during data acquisition.

Claims

1. A method for fabricating a pulse width multiplexed SNSPD array chip, characterized in that, Includes the following steps: (1) Superconducting thin films are deposited on a substrate by magnetron sputtering; (2) The input and output electrodes were fabricated using photolithography and magnetron sputtering; (3) Electron beam exposure and reactive ion etching are used to form the nanowire detector region, delay line region and clamp contact point; The nanowire detection region includes several regularly arranged nanowire detectors formed by meandering nanowires. The delay line region includes an equal number of meandering delay lines. After each nanowire detector is connected to a delay line, the delay line extends a parallel clamp-shaped contact point. A nanowire detector, a delay line, and a parallel resistor form a detector unit. Several detector units are connected in series. The input electrode is connected to the output electrode via the sequentially connected detector units. The length of each delay line satisfies the following condition: d l =d w *L / L sq , d l L is the length of the delay line. sq d is the inductance per unit area of ​​the superconducting thin film. w L is the width of the delay line, and L is the inductance of the delay line. The inductance increases sequentially in series, such that when any equal number of nanowire detectors respond simultaneously, the pulse width of the response signal output by the output electrode is different. (4) Electron beam exposure and magnetron sputtering are used to deposit parallel resistors onto the contact points; (5) The substrate is packaged and cooled to form a pulse width multiplexed SNSPD array chip.

2. The method for fabricating a pulse width multiplexed SNSPD array chip according to claim 1, characterized in that: The inductance value of the delay line was obtained through simulation.

3. The method for fabricating a pulse width multiplexed SNSPD array chip according to claim 1, characterized in that: The width of the delay line is greater than the width of the meandering nanowire.

4. A data readout method for a pulse width multiplexed SNSPD array chip prepared according to any one of claims 1-3, characterized in that... Includes the following steps: (1) A single coaxial cable is used to input a bias current to the input electrode of the pulse width multiplexed SNSPD array chip. The bias current is provided by a constant voltage source and a current-limiting resistor connected in series with the constant voltage source. (2) The response signal is read from the output electrode using an analog-to-digital converter; (3) Obtain the amplitude of the response signal. If the waveform amplitude is n times the amplitude of a single nanowire detector response, then determine that there are n nanowire detectors responding at the moment. (4) Obtain the pulse width value of the response signal at a preset threshold, and find the current response nanowire detector combination from the pre-stored table according to the pulse width value. The preset threshold is set differently according to the number of nanowire detector responses. The pre-stored table stores the pulse width value of the response signal at the preset threshold when different numbers of nanowire detector combinations respond. The pulse width value is obtained through simulation or experiment.

Citation Information

Patent Citations

  • Superconductive nanowire single-photon detector capable of distinguishing photon number and preparation method thereof

    CN102353464A

  • High-speed superconducting nanowire single-photon detector structure

    CN110487402A